Cemented carbide comprising carbon nanomaterial and method for producing same
By doping carbon nanomaterials with heteroelements and integrating them into the bonding phase of cemented carbide alloys, the alloy achieves balanced hardness and toughness, addressing the trade-off issue and enhancing bending resistance for improved industrial performance.
Patent Information
- Application Number
- PCT/KR2024/005608
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-04-27
- Filing Date
- 2024-04-25
- Publication Date
- 2024-10-31
AI Technical Summary
Cemented carbide alloys face a trade-off between hardness and toughness, with reducing particle size and binder thickness improving hardness but decreasing toughness, and vice versa, limiting their performance in complex industrial environments.
Incorporating carbon nanomaterials doped with heteroelements like sulfur, nitrogen, and phosphorus into the bonding phase of cemented carbide alloys, along with tungsten carbide and binder metals, to enhance interfacial adhesion and prevent crack propagation, while maintaining hardness and improving bending resistance.
The approach results in cemented carbide alloys with enhanced hardness, toughness, and bending resistance, allowing for improved performance in machining tools and wear-resistant applications without the typical trade-off between hardness and toughness.
Smart Images

Figure KR2024005608_31102024_PF_FP_ABST
Abstract
Description
Superhard alloy containing carbon nanomaterials and method for manufacturing the same
[0001] The present invention relates to a superalloy containing carbon nanomaterials and a method for manufacturing the same, and more particularly, to a superalloy containing carbon nanomaterials doped with a different element, which can not only improve the strength of the bonding phase but also prevent the occurrence and propagation of cracks, thereby simultaneously securing hardness and toughness, and having excellent tensile strength, and a method for manufacturing the same economically and efficiently.
[0002] Cemented carbide is an alloy that combines hard particles of carbides (TiC, ZrC, HfC, VC, NbC, TaC, Cr3C2, Mo2C, WC) from groups IV, V, and VI of the periodic table with a tough binder metal, and has properties between those of high-hardness ceramic materials and high-toughness high-speed steel materials.
[0003] These superalloys have both hardness and a certain degree of toughness, which are important characteristics for tool materials, and have excellent mechanical properties from room temperature to high temperature, so they are widely used as machining tools, wear-resistant parts, and mold materials.
[0004] Cemented carbides contain hard particles and a binder metal that binds them together. The mechanical properties of cemented carbides are influenced by the size of the hard particles and the thickness of the bonding layer formed by the binder metal (mean free path). To achieve high hardness, it is necessary to reduce the size of the hard particles and thin the bonding layer formed by the binder metal.
[0005] However, using hard particles several hundred nanometers in size or reducing the thickness of the bonding layer between the hard particles increases hardness, but relatively reduces toughness, resulting in a decrease in rupture strength. In other words, hardness and toughness have opposing characteristics, and generally, as hardness increases, rupture strength decreases.
[0006] Therefore, there have been attempts to develop superalloys that can simultaneously secure hardness and toughness.
[0007] For example, Korean Patent Publication No. 10-2017-0093402 discloses that a cemented carbide alloy having optimal hardness and toughness can be provided by manufacturing a granular composite containing nano-sized hard particles and a binder metal in a specific content, dispersing the granular composite on a binder metal, molding it, and then sintering it.
[0008] However, with the development of the semiconductor industry, electronics industry, and precision industry, the environments in which they are used have become more complex and diverse, and there is a growing demand for the development of cemented carbide alloys with even better hardness and toughness.
[0009] The purpose of the present invention is to provide a super-hard alloy that can simultaneously secure hardness and toughness and has excellent tensile strength.
[0010] Another object of the present invention is to provide a method for manufacturing the above cemented carbide alloy economically and efficiently.
[0011] Meanwhile, the present invention provides a cemented carbide alloy comprising hard particles comprising carbon nanomaterials doped with a heterogeneous element in an amount of 0.01 to 2 wt%, a binder metal in an amount of 4 to 14 wt%, and tungsten carbide (WC) in an amount of 85 to 95 wt%.
[0012] In one embodiment of the present invention, the carbon nanomaterial may be at least one selected from the group consisting of graphene, carbon nanotubes (CNTs), fullerenes, graphite, and activated carbon.
[0013] In one embodiment of the present invention, the doped carbon nanomaterial may be doped with one or more heterogeneous elements selected from the group consisting of sulfur (S), nitrogen (N), and phosphorus (P).
[0014] In one embodiment of the present invention, the doped carbon nanomaterial may include one or more heterogeneous elements selected from the group consisting of sulfur (S), nitrogen (N), and phosphorus (P), and oxygen (O).
[0015] In one embodiment of the present invention, the doped carbon nanomaterial may have an atomic percent of one or more heterogeneous elements selected from the group consisting of sulfur (S), nitrogen (N), and phosphorus (P) of 0.1 to 15 at%, an atomic percent of oxygen (O) of 1 to 20 at%, and an atomic percent of carbon (C) of 65 to 98 at%.
[0016] In one embodiment of the present invention, the binder metal may include at least one selected from the group consisting of cobalt (Co), iron (Fe), and nickel (Ni).
[0017] According to one embodiment of the present invention, a superalloy may have a tensile strength of 400 kgf / mm2 or more at 25°C.
[0018]
[0019] On the other hand, the present invention
[0020] (i) a step of mixing graphene oxide powder and heterogeneous element doping raw material powder;
[0021] (ii) a step of heating the mixed powder to 90 to 300°C in a sealed container;
[0022] (iii) a step of washing and drying the heated mixed powder to obtain doped graphene;
[0023] (iv) a step of mixing and milling the doped graphene with hard particles and a binder metal;
[0024] (v) a step of pressure-molding the above-mentioned milled mixture to obtain a molded body; and
[0025] (vi) A method for manufacturing a cemented carbide alloy is provided, including a step of sintering the above-mentioned molded body.
[0026] In one embodiment of the present invention, the graphene oxide powder may have an atomic percentage of oxygen (O) element of 20 to 40 at%.
[0027] In one embodiment of the present invention, the heteroatom doping raw material may be at least one selected from the group consisting of sulfur, urea, thiourea dioxide, ammonium phosphate, and hydrazine.
[0028] In one embodiment of the present invention, the mixing in step (i) can be performed using a mixer, a ball mill or a three-roll mill.
[0029] In one embodiment of the present invention, the doped graphene may have an atomic percentage of 0.1 to 15 at% of one or more heterogeneous elements selected from the group consisting of sulfur (S), nitrogen (N), and phosphorus (P), an atomic percentage of oxygen (O) element of 1 to 20 at%, and an atomic percentage of carbon (C) element of 65 to 98 at%.
[0030] In one embodiment of the present invention, the sintering can be performed by first sintering at 500 to 1000°C and second sintering at 1000 to 1700°C.
[0031] The superhard alloy according to the present invention can not only improve the strength of the bonding phase by including carbon nanomaterials doped with different elements, but also prevent the occurrence and propagation of cracks, thereby simultaneously securing hardness and toughness and having excellent tensile strength.
[0032] In addition, according to the manufacturing method of the present invention, doped graphene can be mass-produced economically and efficiently by reacting graphene oxide powder and heterogeneous element doping raw material powder in a solid state without separate solvent dilution, and can be applied to the manufacturing of superhard alloys.
[0033] Figure 1 is a flow chart schematically showing a method for manufacturing a superhard alloy according to one embodiment of the present invention.
[0034] Figure 2 shows the XPS analysis results of the graphene oxide powder used in the above manufacturing examples and comparative manufacturing examples.
[0035] Figures 3 to 6 are XPS analysis results of doped graphene obtained in the above manufacturing examples 1 to 4.
[0036] Figure 7 is a graph showing the results of evaluating the tensile strength of the superhard alloy obtained in Example 1 and Comparative Example 1.
[0037] Figure 8 shows the results of hardness evaluation of the superhard alloy obtained in Example 1 and Comparative Example 1.
[0038] Hereinafter, the present invention will be described in more detail.
[0039]
[0040] One embodiment of the present invention relates to a superalloy comprising a carbon nanomaterial doped with a heterogeneous element.
[0041]
[0042] According to one embodiment of the present invention, a superalloy can improve the strength of the bonding phase by uniformly dispersing carbon nanomaterials doped with a different element within a bonding phase formed by a binder metal, thereby increasing the interfacial adhesion between the binder metals, and can effectively prevent the occurrence and propagation of cracks, thereby simultaneously securing hardness and toughness.
[0043] In particular, the super-hard alloy according to one embodiment of the present invention can maintain hardness while improving tensile strength.
[0044]
[0045] A cemented carbide alloy according to one embodiment of the present invention comprises hard particles comprising carbon nanomaterials doped with a heterogeneous element in an amount of 0.01 to 2 wt%, a binder metal in an amount of 4 to 14 wt%, and tungsten carbide (WC) in an amount of 85 to 95 wt%.
[0046]
[0047] In one embodiment of the present invention, the carbon nanomaterial doped with the heterogeneous element is uniformly dispersed between the binder metals in the bonding phase, thereby serving to increase the interfacial adhesion of the binder metals.
[0048] The above carbon nanomaterial refers to a material whose main component is carbon and has a particle, linear or plate-shaped form with a nano-scale size.
[0049] Examples of the above carbon nanomaterials include graphene, carbon nanotubes (CNT), fullerene, graphite, and activated carbon. Graphene is particularly preferable in that it is a plate-shaped material and increases the interfacial adhesion between binder metals through heterogeneous element doping, thereby improving hardness and toughness.
[0050] The above carbon nanomaterial may be doped with one or more heterogeneous elements selected from the group consisting of sulfur (S), nitrogen (N), and phosphorus (P) in terms of securing hardness and toughness, and preferably may include one or more heterogeneous elements selected from the group consisting of sulfur (S), nitrogen (N), and phosphorus (P) and an oxygen (O) element.
[0051] Preferably, the doped carbon nanomaterial may have an atomic percentage of at least one heterogeneous element selected from the group consisting of sulfur (S), nitrogen (N), and phosphorus (P) of 0.1 to 15 at%, an atomic percentage of oxygen (O) of 1 to 20 at%, and an atomic percentage of carbon (C) of 65 to 98 at% in terms of securing hardness and toughness.
[0052] More preferably, the doped carbon nanomaterial may have an atomic percentage of 3 to 15 at% of one or more heterogeneous elements selected from the group consisting of sulfur (S), nitrogen (N), and phosphorus (P), an atomic percentage of oxygen (O) element of 10 to 15 at%, and an atomic percentage of carbon (C) element of 75 to 85 at%.
[0053] The atomic percent of the above elements is a value measured using X-ray photoelectron spectroscopy (XPS) according to the method described in the experimental example described below.
[0054] In one embodiment of the present invention, the doped carbon nanomaterial may be included in an amount of 0.01 to 2 wt%, preferably 0.05 to 1 wt%, based on 100 wt% of the total weight of the cemented carbide alloy. When the doped carbon nanomaterial is included in the above content range, both hardness and toughness can be secured, and in particular, tensile strength can be increased.
[0055]
[0056] In one embodiment of the present invention, the binder metal forms a bonding phase that binds hard particles comprising tungsten carbide (WC).
[0057] The above binder metal includes an iron group element. That is, the binder metal may include one or more selected from the group consisting of cobalt (Co), iron (Fe), and nickel (Ni), and in particular, may include cobalt (Co) in terms of hardness and toughness.
[0058] The above-mentioned combination may further include unavoidable trace amounts of impurity elements in addition to the iron group elements and doped carbon nanomaterials. Such impurity elements include, for example, titanium (Ti).
[0059] In one embodiment of the present invention, the binder metal may be included in an amount of 4 to 14 wt%, preferably 6 to 12 wt%, based on 100 wt% of the total weight of the cemented carbide alloy. When the binder metal is included in the above content range, both hardness and toughness can be secured, and in particular, tensile strength can be increased.
[0060]
[0061] In one embodiment of the present invention, the hard particles form a hard phase of a superhard alloy and include tungsten carbide (WC) as a main component.
[0062] The above hard particles may contain, in addition to WC, unavoidable elements mixed in during the manufacturing process of WC, trace amounts of impurity elements, etc.
[0063] The content of WC among the above hard particles is preferably 99 wt% or more, and more preferably substantially 100 wt%.
[0064] Elements other than W and C that may be included in the above-mentioned hard particles include, for example, molybdenum (Mo) and chromium (Cr).
[0065] In one embodiment of the present invention, the hard particles may be included in an amount of 85 to 95 wt%, preferably 87 to 93 wt%, based on 100 wt% of the total weight of the cemented carbide. When the hard particles are included in the above content range, sufficient hardness can be secured.
[0066]
[0067] According to one embodiment of the present invention, the superalloy may have a tensile strength of 400 kgf / mm2 or more, for example, 400 to 500 kgf / mm2, at 25°C.
[0068]
[0069] One embodiment of the present invention relates to a method for manufacturing a superalloy including a carbon nanomaterial doped with a heterogeneous element.
[0070]
[0071] Figure 1 is a flow chart schematically showing a method for manufacturing a superhard alloy according to one embodiment of the present invention.
[0072]
[0073] As shown in Fig. 1, a method for manufacturing a cemented carbide alloy according to one embodiment of the present invention
[0074] (i) a step of mixing graphene oxide powder and heterogeneous element doping raw material powder;
[0075] (ii) a step of heating the mixed powder to 90 to 300°C in a sealed container;
[0076] (iii) a step of washing and drying the heated mixed powder to obtain doped graphene;
[0077] (iv) a step of mixing and milling the doped graphene with hard particles and a binder metal;
[0078] (v) a step of pressure-molding the above-mentioned milled mixture to obtain a molded body; and
[0079] (vi) a step of sintering the above molded body.
[0080]
[0081] According to one embodiment of the present invention, a manufacturing method can manufacture doped graphene by simultaneously performing partial reduction and doping of graphene oxide by mixing and heating graphene oxide powder and heterogeneous element doping raw material powder, and can manufacture a cemented carbide alloy having excellent hardness and toughness by mixing the doped graphene with hard particles and a binder metal, milling the mixed graphene, and then press-molding and sintering the mixed graphene.
[0082] In particular, the manufacturing method according to one embodiment of the present invention has the advantage of being able to economically and efficiently mass-produce doped graphene by reacting graphene oxide powder and heterogeneous element doping raw material powder in a solid state without separate solvent dilution, thereby being applicable to the manufacturing of superhard alloys.
[0083] Additionally, since no expensive equipment is required during the manufacturing process, cemented carbide alloys can be manufactured more economically.
[0084]
[0085] The above step (i) is a step of obtaining a mixed powder by mixing graphene oxide powder and a heterogeneous element doping raw material powder.
[0086] In the above step (i), the graphene oxide powder can be obtained by oxidizing graphite, and can be manufactured using a method known in the art or can be obtained and used as a commercially available product.
[0087] The above graphite may be pyrolytic graphite, natural graphite, synthetic graphite, etc.
[0088] Specifically, the method for producing the above graphene oxide powder may use the Hummers method (JA Chem. Soc. 1958, 80, 1339) or the modified Hummers method (Chem. Mater. 1999, 11(3), 771).
[0089] The above graphene oxide powder may have an atomic percentage of oxygen (O) element of 20 to 40 at%. If the atomic percentage of oxygen (O) element of the above graphene oxide powder is less than 20 at%, it may not be properly exfoliated, resulting in a multilayer graphene and low dispersibility. If it is more than 40 at%, the degree of defects may be high, making it difficult to control the intended heterogeneous element doping structure.
[0090] As the above heteroatom doping raw material, a doping raw material known in the relevant technical field can be used, and preferably, in terms of doping efficiency, one or more selected from the group consisting of sulfur, urea, thiourea dioxide, ammonium phosphate, and hydrazine can be used.
[0091] In one embodiment of the present invention, the mixing ratio of the graphene oxide powder and the heterogeneous element doping raw material powder can be appropriately adjusted by considering the atomic percentage of the element to be doped. For example, the mixing ratio of the graphene oxide powder and the heterogeneous element doping raw material powder can be 1:0.1 to 1:10 by weight.
[0092] In one embodiment of the present invention, the mixing in step (i) can be performed using a mixer, a ball mill or a three-roll mill.
[0093]
[0094] The above step (ii) is a step of performing partial reduction and doping of graphene oxide by heating a mixed powder of the graphene oxide powder obtained in the above step (i) and the heterogeneous element doping raw material powder.
[0095] In the above step (ii), the heating may be performed in a sealed container taking into account equipment contamination due to volume expansion.
[0096] The above heating temperature may be 90 to 300°C, preferably 150 to 250°C. Partial reduction and doping efficiency are excellent within the above heating temperature range.
[0097]
[0098] The above step (iii) is a step of washing and drying the heated mixed powder obtained in the above step (ii) to obtain doped graphene.
[0099] The above washing may be performed using an appropriate washing solvent, taking into account the type of the heterogeneous element doping raw material, etc. For example, the washing may be performed using toluene, water, ethanol, methanol, isopropanol, acetone, etc.
[0100] The above drying can be performed in air at a temperature of 30 to 200°C.
[0101] The above doped graphene may be doped with one or more heterogeneous elements selected from the group consisting of sulfur (S), nitrogen (N), and phosphorus (P) depending on the heterogeneous element doping raw material used, and preferably may include one or more heterogeneous elements selected from the group consisting of sulfur (S), nitrogen (N), and phosphorus (P), and an oxygen (O) element.
[0102] Preferably, the doped graphene may have an atomic percentage of at least one heterogeneous element selected from the group consisting of sulfur (S), nitrogen (N), and phosphorus (P) of 0.1 to 15 at%, an atomic percentage of oxygen (O) of 1 to 20 at%, and an atomic percentage of carbon (C) of 65 to 98 at%, in order to secure hardness and toughness through increased interfacial adhesion between binder metals.
[0103] More preferably, the doped graphene may have an atomic percentage of 3 to 15 at% of one or more heterogeneous elements selected from the group consisting of sulfur (S), nitrogen (N), and phosphorus (P), an atomic percentage of oxygen (O) element of 10 to 15 at%, and an atomic percentage of carbon (C) element of 75 to 85 at%.
[0104]
[0105] The above step (iv) is a step of mixing and milling the doped graphene with hard particles forming a hard phase and a binder metal forming a bonding phase.
[0106] The above doped graphene, hard particles and binder metal are the same as those described in the description of the above cemented carbide.
[0107] The above milling can be performed using a ball mill or an attritor mill.
[0108] Specifically, it is recommended that the ball mill use stainless steel, superalloy, silicon nitride, alumina or zirconia as the material of the reaction vessel and balls, the diameter of the balls is 5 to 30 mm, and the ratio of the mixed powder and balls charged into the reaction vessel is preferably 1:1 to 100 by weight.
[0109]
[0110] The above step (v) is a step of pressure-molding the milled mixture to obtain a molded body.
[0111] The above pressure forming method is not particularly limited, and a pressure forming method commonly used in the relevant technical field can be used.
[0112] For example, a mixed powder can be filled into a mold and molded into a desired shape under a predetermined pressure. Examples of molding methods include dry pressure molding, such as air pressing, and cold isostatic pressing. The pressure during pressure molding is preferably approximately 50 to 200 MPa. The shape of the molded body can be selected depending on the desired product shape.
[0113]
[0114] The above step (vi) is a step of sintering the molded body to obtain a sintered body.
[0115] It is preferable that the above sintering be performed by maintaining the molded body in a temperature range where the liquid phase is generated for a predetermined period of time.
[0116] At this time, it is preferable that sintering be performed by first sintering at 500 to 1000°C and second sintering at 1000 to 1700°C.
[0117] The holding time for each sintering may be 0.5 to 2 hours, preferably 1 to 1.5 hours.
[0118] It is preferable that the atmosphere during the above sintering be an inert gas atmosphere such as nitrogen or argon or a vacuum (about 0.5 ㎩ or less).
[0119]
[0120] The superhard alloy according to the present invention can be used, for example, in machining tools such as cutting tools, wear-resistant parts, mold materials, etc.
[0121]
[0122] Hereinafter, the present invention will be described in more detail through examples, comparative examples, and experimental examples. These examples, comparative examples, and experimental examples are intended solely to illustrate the present invention, and it will be apparent to those skilled in the art that the scope of the present invention is not limited thereto.
[0123]
[0124] Manufacturing Example 1: Preparation of oxygen / sulfur (O / S) doped graphene
[0125] 10 g of graphene oxide powder having an atomic percentage of oxygen (O) of 31.8 at% and 10 g of sulfur powder were mixed using a mixer. The mixed powder was placed in a sealed container and heated in an oven at 200°C for 3 hours.
[0126] The heated mixed powder was repeatedly washed with toluene to obtain doped graphene. Washing was repeated until the characteristic yellow color of sulfur disappeared. The washed doped graphene was dried in air at 80°C.
[0127]
[0128] Manufacturing Example 2: Manufacturing of Oxygen / Nitrogen (O / N) Doped Graphene
[0129] 10 g of graphene oxide powder having an atomic percentage of oxygen (O) of 31.8 at% and 10 g of urea powder were mixed using a mixer. The mixed powder was placed in a sealed container and heated in an oven at 200°C for 3 hours.
[0130] The above heated mixed powder was repeatedly washed with water to obtain doped graphene. The washed doped graphene was dried in air at 80°C.
[0131]
[0132] Manufacturing Example 3: Manufacturing of Oxygen / Nitrogen / Sulfur (O / N / S) Doped Graphene
[0133] 10 g of graphene oxide powder having an atomic percentage of oxygen (O) of 31.8 at% and 10 g of thiourea dioxide powder were mixed using a mixer. The mixed powder was placed in a sealed container and heated in an oven at 200°C for 3 hours.
[0134] The above heated mixed powder was repeatedly washed with water to obtain doped graphene. The washed doped graphene was dried in air at 80°C.
[0135]
[0136] Manufacturing Example 4: Manufacturing of Oxygen / Nitrogen / Phosphorus (O / N / P) Doped Graphene
[0137] 10 g of graphene oxide powder having an atomic percentage of oxygen (O) of 31.8 at% and 10 g of ammonium phosphate powder were mixed using a mixer. The mixed powder was placed in a sealed container and heated in an oven at 200°C for 3 hours.
[0138] The above heated mixed powder was repeatedly washed with water to obtain doped graphene. The washed doped graphene was dried in air at 80°C.
[0139]
[0140] Examples 1 to 4: Preparation of doped graphene-containing cemented carbide alloys
[0141] 90.5 wt% of WC powder having an average particle size of 800 nm, 9.4 wt% of Co powder having an average particle size of 800 nm, and 0.1 wt% of the doped graphene of each of the above examples were mixed and milled using an attrition milling machine. The milled WC / doped graphene-Co powder was pressurized at a pressure of 150 MPa using an air press to obtain a molded body. The molded body was first sintered at a temperature of 750°C in an air atmosphere, and then second sintered at a temperature of 1350°C to produce a cemented carbide.
[0142]
[0143] Comparative Example 1: Preparation of a doped graphene-free cemented carbide alloy
[0144] 90.6 wt% of WC powder having an average particle size of 800 nm and 9.4 wt% of Co powder having an average particle size of 800 nm were mixed and milled using an attrition milling machine. The milled WC / doped graphene-Co powder was pressurized at a pressure of 150 MPa using an air press to obtain a molded body. The molded body was first sintered at a temperature of 750°C in an air atmosphere, and then second sintered at a temperature of 1350°C to produce a cemented carbide.
[0145]
[0146] Experimental Example 1: Elemental Analysis of Graphene
[0147] Elemental analysis of the graphene oxide powder used in the above manufacturing examples and the doped graphene obtained in the above manufacturing examples 1 to 4 was performed using X-ray photoelectron spectroscopy (XPS).
[0148] The results are shown in Figures 2 to 6, respectively.
[0149] Figure 2 shows the XPS analysis results of the graphene oxide powder used in the above manufacturing example.
[0150] Through Figure 2, it can be seen that the atomic percentage of oxygen (O) element in the graphene oxide powder is at the level of 31.8 at%.
[0151] Figures 3 to 6 are XPS analysis results of doped graphene obtained in the above manufacturing examples 1 to 4.
[0152] Through FIGS. 3 to 6, it can be seen that the doped graphene obtained in the above manufacturing examples 1 to 4 is doped with one or more heterogeneous elements selected from the group consisting of sulfur (S), nitrogen (N), and phosphorus (P), and includes an oxygen (O) element.
[0153] Specifically, it can be seen that the doped graphene of Manufacturing Example 1 is composed of 3.27 at% sulfur (S), 14.79 at% oxygen (O), and 81.94 at% carbon (C), the doped graphene of Manufacturing Example 2 is composed of 13.02 at% nitrogen (N), 11.03 at% oxygen (O), and 75.95 at% carbon (C), the doped graphene of Manufacturing Example 3 is composed of 8.4 at% nitrogen (N), 1.26 at% sulfur (S), 13.99 at% oxygen (O), and 76.34 at% carbon (C), and the doped graphene of Manufacturing Example 4 is composed of 3.2 at% nitrogen (N), 0.47 at% phosphorus (P), 13.39 at% oxygen (O), and 82.94 at% carbon (C). there is.
[0154]
[0155] Experimental Example 2: Analysis of Mechanical Properties of Cemented Carbide
[0156] The mechanical properties of the superhard alloy obtained in the above examples and comparative examples were analyzed using the method described below, and the results are shown in Table 1 and Figures 7 to 8 below.
[0157]
[0158] (1) Evaluation of transverse strain (TRS)
[0159] The 25℃ tensile strength of the superhard alloy was evaluated as follows.
[0160] The transverse rupture strength was evaluated using a universal materials testing machine. A 3-Point Bendig Fixture was used as the test jig. The specimen size was 4 mm × 8 mm × 25 mm (thickness, width, length), and the evaluation was performed at a testing speed of 0.2 mm / min.
[0161]
[0162] (2) Hardness evaluation
[0163] The hardness of the cemented carbide alloy was evaluated as follows.
[0164] Rockwell A hardness was measured using a Rockwell hardness tester. The specimen size was 4 mm × 8 mm × 25 mm.
[0165]
[0166] Transverse tensile strength (kgf / ㎟) Hardness (HRA) Comparative Example 130092.4 Example 148692.7 Example 245792.4 Example 346292.5 Example 444892.3
[0167]
[0168] Through the above Table 1 and FIGS. 7 to 8, it can be confirmed that the superalloys obtained in Examples 1 to 4 have improved tensile strength and excellent hardness compared to the superalloys obtained in Comparative Example 1.
[0169] That is, the superalloys obtained in Examples 1 to 4 showed excellent hardness while improving the tensile strength by more than 50% compared to the superalloy obtained in Comparative Example 1.
[0170] Generally, there is a trade-off characteristic in which hardness decreases as tensile strength increases. However, it can be seen that the hardness of the cemented carbide alloy of the present invention does not decrease even when the tensile strength increases.
[0171] This appears to be because carbon nanomaterials doped with heterogeneous elements induce even dispersion of WC and Co powders and inhibit crack propagation by strengthening interfacial bonding.
[0172] In conclusion, it can be confirmed that when a superalloy is manufactured using carbon nanomaterials doped with heterogeneous elements according to the present invention, improved tensile strength and excellent strength can be secured.
[0173]
[0174] While specific aspects of the present invention have been described in detail above, it should be apparent to those skilled in the art that these specific descriptions are merely preferred embodiments and do not limit the scope of the present invention. Those skilled in the art will be able to make various applications and modifications within the scope of the present invention based on the above description.
[0175] Accordingly, the substantial scope of the present invention will be defined by the appended claims and their equivalents.
Claims
Carbon nanomaterials doped with 0.01 to 2 wt% of a heterogeneous element, 4 to 14 wt% of a binder metal, and A cemented carbide alloy comprising hard particles comprising 85 to 95 wt% of tungsten carbide (WC).
2. In the first paragraph, the superhard alloy is at least one selected from the group consisting of graphene, carbon nanotubes (CNT), fullerene, graphite, and activated carbon.
3. A superhard alloy according to claim 1, wherein the doped carbon nanomaterial is doped with one or more heterogeneous elements selected from the group consisting of sulfur (S), nitrogen (N), and phosphorus (P).
4. In the first paragraph, the doped carbon nanomaterial is a superalloy containing one or more heterogeneous elements selected from the group consisting of sulfur (S), nitrogen (N), and phosphorus (P), and an oxygen (O) element.
5. In the first paragraph, the doped carbon nanomaterial is a superalloy having an atomic percentage of at least one heterogeneous element selected from the group consisting of sulfur (S), nitrogen (N), and phosphorus (P) of 0.1 to 15 at%, an atomic percentage of oxygen (O) of 1 to 20 at%, and an atomic percentage of carbon (C) of 65 to 98 at%.
6. In the first paragraph, the binder metal is a super-hard alloy including at least one selected from the group consisting of cobalt (Co), iron (Fe), and nickel (Ni).
7. A cemented carbide alloy having a tensile strength of 400 kgf / mm2 or more at 25°C in the first paragraph. 8.(i) A step of mixing graphene oxide powder and heterogeneous element doping raw material powder; (ii) a step of heating the mixed powder to 90 to 300°C in a sealed container; (iii) a step of washing and drying the heated mixed powder to obtain doped graphene; (iv) a step of mixing and milling the doped graphene with hard particles and a binder metal; (v) a step of pressure-molding the above-mentioned milled mixture to obtain a molded body; and (vi) A method for manufacturing a cemented carbide alloy, comprising a step of sintering the above-mentioned molded body.
9. A manufacturing method in the 8th paragraph, wherein the graphene oxide powder has an atomic percentage of oxygen (O) element of 20 to 40 at%.
10. A manufacturing method according to claim 8, wherein the heterogeneous element doping raw material is at least one selected from the group consisting of sulfur, urea, thiourea dioxide, ammonium phosphate, and hydrazine.
11. A manufacturing method in which the mixing in step (i) is performed using a mixer, a ball mill or a 3-roll mill in the 8th paragraph.
12. A manufacturing method in accordance with claim 8, wherein the doped graphene has an atomic percentage of 0.1 to 15 at% of one or more heterogeneous elements selected from the group consisting of sulfur (S), nitrogen (N), and phosphorus (P), an atomic percentage of oxygen (O) element of 1 to 20 at%, and an atomic percentage of carbon (C) element of 65 to 98 at%.
13. A manufacturing method in which the sintering in the 8th paragraph is performed by first sintering at 500 to 1000°C and second sintering at 1000 to 1700°C.
Citation Information
Patent Citations
WC-Co hard alloy added with graphene / nanometer Al2O3 particles and preparation method
CN114277298A
High-performance superfine hard alloy and preparation method thereof
CN114990405A
Manufacturing method of super hard metal containing carbon nanotube, the super hard metal manufactured using the same and cutting tools comprising the super hard metal
KR1020150043276A
Air conditioning system for vehicle
KR102202311B1
Cited By
High-wear-resistance tungsten steel alloy and preparation method thereof
CN119571165A
High-wear-resistance and corrosion-resistance tungsten carbide coating on surface of alloy steel as well as preparation method and application thereof