Fluorine-containing compounds for use in high-frequency substrates
The fluorine-containing compound with a low degree of polymerization addresses the challenges of high-frequency substrate materials by providing excellent electrical and thermal stability, enabling the creation of substrates that can handle next-generation frequencies with reduced thermal expansion and improved crosslinking properties.
Patent Information
- Application Number
- PCT/US2024/026380
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-12-27
- Filing Date
- 2024-04-26
- Publication Date
- 2024-10-31
AI Technical Summary
Current high-frequency substrate materials, such as epoxy resins and fluororesins, face challenges in handling next-generation high frequencies exceeding 5 GHz due to inadequate electrical properties, dimensional stability, and high thermal expansion coefficients, making them unsuitable for advanced communication applications.
A fluorine-containing compound with a low degree of polymerization, specifically designed to have a low coefficient of thermal expansion and excellent crosslinking properties, is developed, which can be used to create prepregs for substrates that handle next-generation high frequencies, featuring a structure with a cyclopentylidene, cyclohexylidene, or cyclododecylidene group and a crosslinking agent, resulting in a cured product with a low thermal expansion coefficient and high gel fraction.
The fluorine-containing compound achieves excellent electrical properties, high dimensional stability, and efficient thermosetting properties, enabling reliable molding of prepregs for high-frequency substrates with a significantly reduced thermal expansion coefficient and high gel fraction, effectively addressing the limitations of existing materials.
Smart Images

Figure US2024026380_31102024_PF_FP_ABST
Abstract
Description
TITLE OF THE INVENTIONFLUORINE-CONTAINING COMPOUNDS FOR USE IN HIGH-FREQUENCY SUBSTRATESCROSS REFERENCE TO RELATED APPLICATIONS
[0001] This application claims the benefit of priority of Japanese Patent Application No. 2023-073742 filed April 27, 2023, and Japanese Patent Application No. 2023-221746 filed December 27, 2023, the disclosures of which are incorporated herein by reference in their entirety.FIELD OF THE INVENTION
[0002] The present invention relates to a fluorine-containing compound, and particularly relates to a fluorine-containing compound that can also be suitably used in next-generation high-frequency substrates.BACKGROUND OF THE INVENTION
[0003] In recent years, information and communication apparatuses such as smartphones, tablet terminals, and the like have been developed for nextgeneration high frequencies that enable high-speed and large-capacity transmission, and in response, substrate materials used are required to have a low dielectric constant and low dielectric tangent to reduce transmission loss.
[0004] Conventionally, materials such as epoxy resins, polyphenylene ether resins, and the like have been used as resin materials for high-speed communication and transmission (Patent Document 1 ). However, epoxy resins and polyphenylene ether resins have difficulty handling the high-speed and large-capacity transmissions of recent years.
[0005] In contrast, fluororesins are known as materials having excellent electrical properties. In particular, perfluororesins in which all of the hydrogens in a molecular chain are substituted with fluorine are known to exhibit particularly excellent electrical properties (dielectric constant, dielectric loss, and the like). However, fluororesins (perfluororesins) have issues such as ease of deformation (due to stress), a high coefficient of thermal expansion, and the like, making them difficult to use as substrate materials.
[0006] The use of fluorinated poly(arylene ether) and crosslinkable fluorinated poly(arylene ether) has been proposed as a dielectric body material in electronic components (Patent Documents 2 and 3). However, the electrical properties of the materials do not satisfy the current high-speed communication and transmission requirements. Furthermore, from the perspective of mass production and reducing manufacturing cost, there is a need to lower the crosslinking processing temperature such that manufacturing can be performed with existing substrate manufacturing devices.
[0007] As a solution to these problems, the present inventors and the like proposed the fluororesin described in Patent Document 4 below. The fluororesin described in Patent Document 4 is a resin material having excellent electrical properties (low dielectric constant and low dielectric loss), high solvent solubility for ease of thin film molding, and excellent crosslinking properties which allow a film to be formed by heating at approximately 200°C.PRIOR ART DOCUMENTS
[0008] [Patent Document 1] Japanese Unexamined Patent Application 2017-128718[Patent Document 2] U.S. Patent No. 5115082 Specification[Patent Document 3] U.S. Patent No. 5179188 Specification[Patent Document 4] Japanese Unexamined Patent Application 2022-89150SUMMARY OF THE INVENTION
[0009] However, even though the fluororesin specifically disclosed in the aforementioned Patent Document 4 satisfies electrical properties at 1 GHz, the electrical properties and dimensional stability (coefficient of thermal expansion) required to create a substrate that can handle next-generation high frequencies exceeding 5 GHz were unclear as well as whether or not a prepreg used to create the substrate can be reliably molded.
[0010] The present inventors and the like have discovered that a fluorine- containing compound with a low degree of polymerization, which was not thefocus in the Patent Document 4 above, has superior dimensional stability (coefficient of thermal expansion) and crosslinking properties as compared to the fluororesin specifically disclosed in Patent Document 4 above, and can reliably form prepregs for preparing a substrate that can handle nextgeneration high frequencies exceeding 5 GHz.
[0011] Therefore, an object of the present invention is to provide a fluorine- containing compound that has excellent electrical properties required for nextgeneration high frequencies, and in addition, has a significantly reduced coefficient of thermal expansion (thermal expansion coefficient) and can prepare a substrate with excellent thermosetting properties.DETAILED DESCRIPTION OF THE INVENTION
[0012] The present invention provides a fluorine-containing compound having a structure of the following Formula (I).Chem. Fig. 1In the formula, L represents a structure of the following Formula (II) or (III).Chem. Fig. 2where R1and R2each independently represent a group selected from a group consisting of a hydrogen atom, Ci to C10 alkyl groups, Ci to Cwhaloalkyl groups, and Ce to C aryl groups, or R1and R2may be combined together to form a ring structure that may include a substitution group,R3and R4each independently represent a group selected from a group consisting of a hydrogen atom, a fluorine atom, Ci to Cw saturated or unsaturated hydrocarbon groups in which some or all hydrogens may be substituted by a halogen and Ce to Cw aryl groups in which some or all hydrogens may be substituted by a halogen, n is in a range of 1 to 4, andX represents a group containing an olefinic carbon-carbon double bond or a carbon-carbon triple bond.
[0013] In the fluorine compound of the present invention preferably:(1 ) a coefficient of thermal expansion of the cured product at 240 to 290°C is 200 ppm / °C or less;(2) n is 1 ;(3) X includes at least one fluorine atom;(4) L is selected from a group consisting of cyclopentylidene groups that may have a substitution group, cyclohexylidene groups that may have a substitution group, and cyclododecylidene groups that may have a substitution group; and(5) the cured product has a gel fraction of 50% or more.
[0014] The present invention further provides a fluorine-containing composition containing: the fluorine-containing compound; and a crosslinking agent.
[0015] The present invention even further provides a prepreg containing: the fluorine-containing compound or the fluorine-containing composition; and a fibrous base material.
[0016] The present invention yet even further provides a copper clad laminated sheet including: a cured product of the prepreg; and at least one copper layer.
[0017] The present invention provides a printed circuit board including: a cured product of the prepreg; and a conductor pattern formed on a surface thereof.EFFECT OF THE INVENTION
[0018] The fluorine-containing compound of the present invention naturally has excellent electrical properties (low dielectric constant and low dielectric loss), sufficient heat resistance, suitable glass transition temperature (Tg), and sufficient solvent solubility, and by having a value of n in Formula (I) in a range of 1 to 4, particularly by having the value of n as 1 , the value of the coefficient of thermal expansion at 240°C or higher of a cured product cured under the conditions of 200°C for 120 minutes is 200 ppm / °C or less, which is very low, and thus it is possible to express extremely high dimensional stability. Furthermore, thermosetting (crosslinking) properties are also excellent, and the gel fraction of a cured product after curing is extremely high at 50% or higher.
[0019] This unexpected and unique effect of the present invention is evident in the results of the examples discussed later. In other words, in the case of the fluororesin (Comparative Example 1 ) in which the value of n in Formula (I) above is 30, the value of the thermal expansion coefficient measured under the conditions above is 274 ppm / °C. In contrast, in the case of a fluorine-containing compound (Example 1 ) having the same structure as the fluororesin above except that the value of n is 1 , the thermal expansion coefficient of the cured product was 128 ppm / °C, which clearly is unexpectedly low from the standpoint of a fluororesin with an n value of 30.
[0020] Similarly, in the fluororesin of Comparative Example 1 in which the value of n is 30, the gel fraction of the cured product cured under the conditions above is 16%. In contrast, in the fluorine-containing compound of Example 1 in which the value of n is 1 , the gel fraction of the cured product cured under the conditions above is 100%. Thus, it is clear that a remarkably high idealvalue is achieved, which is unexpected from the standpoint of a fluororesin with an n value of 30.
[0021] Furthermore, molding of a prepreg using thermosetting resin requires impregnation of glass fibers and curing to a semi-cured state. The fluorine-containing compound of the present invention can be easily composited with the glass fibers, enabling efficient molding of a prepreg for preparing a substrate that can handle next-generation high frequencies exceeding 5 GHz.
[0022] In other words, as is clear from the results of the gel fraction (crosslink density) described above, the fluorine-containing compound of the present invention has excellent curability. Therefore, even when pressing pressure is applied or a vacuum formed while the glass fibers are impregnated, compositing with the glass fibers can be reliably performed without the fluorine- containing compound protruding from the glass fibers (Examples 1 to 5). However, when the fluororesin of Comparative Example 1 with an n value of 30 was used, it was difficult to achieve uniform compositing with the glass fibers with the same method. With respect thereto, it is clear that the present invention has achieved unexpected effects from the standpoint of a fluororesin with an n value of 30.MODE FOR CARRYING OUT THE INVENTION(Fluorine-containing compound)
[0023] An important feature of the fluorine-containing compound of the present invention is that in Formula (I), n is in a range of 1 to 4, and preferably is 1. Accordingly, as described above, the fluorine-containing compound expressed by Formula (I) has sufficient heat resistance, an appropriate glass transition temperature (Tg), and sufficient solvent solubility. In comparison, when n is greater than 4, the compound has a reduced coefficient of thermal expansion, high gel fraction, and an unexpected effect of being easily composited with glass fibers and can achieve excellent electrical properties (low dielectric low dielectric loss) at a high frequency of 28 GHz.
[0024] In Formula (I) above, n represents the average degree of polymerization. The average degree of polymerization can be predicted from the stoichiometric ratio of the monomers and can also be measured by a conventionally known method such as nuclear magnetic resonance spectroscopy and the like. In the present invention, "n is 1" means that the average degree of polymerization of the compound is 0.5 to 1 .4.
[0025] In the fluorine-containing compounds of the present invention expressed by Formula (I) above, R1and R2in Formulas (II) and (III) above may each independently represent a group selected from a group consisting of hydrogen atoms, Ci to C10 alkyl groups, Ci to Cw haloalkyl groups, and Ce to C10 aryl groups. Examples of Ci to Cw alkyl groups include methyl groups, ethyl groups, propyl groups, 2-methylpropyl groups (isobutyl groups), butyl groups, pentyl groups, and the like. Examples of Ci to C haloalkyl groups include trifluoromethyl groups, pentafluoroethyl groups, perfluoropropyl groups, and the like. Examples of Ce to Cw aryl groups include phenyl groups and naphthyl groups (including 1-isomers and 2-isomers).
[0026] Alternatively, R1and R2together may be a group forming a ring structure which may have a substitution group. Examples of groups forming the ring structure include tetramethylene groups (forming a cyclopentane ring), pentamethylene groups (forming a cyclohexane ring), undecamethylene groups (forming a cyclododecane ring), 2-methyl-pentamethylene groups (forming a methylcyclohexane ring), 2,2,4-trimethyl-pentamethylene groups (forming a trimethylcyclohexane ring), biphenyl -2,2'-diyl groups (forming a fluorene ring), and the like.
[0027] In Formula (I) above, R3and R4may each independently represent a hydrogen atom, a fluorine atom, a Ci to Cw saturated or unsaturated hydrocarbon group in which some or all hydrogens may be substituted by a halogen or a Ce to Cw aryl group in which some or all hydrogens may be substituted by a halogen. Examples of Ci to Cw saturated or unsaturatedhydrocarbon groups in which some or all hydrogens may be substituted with a halogen include methyl groups, ethyl groups, propyl groups, 2-methylpropyl groups (isobutyl groups), butyl groups, pentyl groups, trifluoromethyll groups, pentafluoroethyl groups, perfluoropropyl groups, vinyl groups, allyl groups, 1- methylvinyl groups, 2-butenyl groups, 3-butenyl groups, and the like. Examples of Ce to Cw aryl groups in which some or all hydrogens may be substituted with a halogen include phenyl groups, naphthyl groups (including 1 -isomers and 2-isomers), perfluorophenyl groups, and the like.
[0028] In Formula (I) above, X represents a group containing an olefinic carbon-carbon double bond or carbon-carbon triple bond, preferably containing at least one fluorine atom. Examples of X include the following structures (X-1) to (X-10).Chem. Fig. 3
[0029] In the formula, p is an integer from 0 to 4. In some aspects, p is 4. In another aspect, p is 0. R represents a group selected from a group consisting of Ci to C alkyl groups and CB to C10 aryl groups. R' represents a hydrogen atom or a C 1 to C w alkyl group.
[0030] Preferably, X has one of the following structures (X-11 ) to (X-15).Chem. Fig. 4
[0031] Preferred fluorine-containing compounds in the present invention include, for example, resins having the following structure (in the formula, "n" is a value from 1 to 4 and "(*)" indicates the bonding position).Chem. Fig. 5Chem. Fig. 7
[0032] In the present invention, the fluorine-containing compound is preferably soluble in a solvent. The fluorine-containing compound being "soluble in a solvent" means 1 g or more, preferably 10 g or more, of the fluorine-containing compound is dissolved per 100 g of a solution obtained from a given solvent. The fluorine-containing compound of the present embodiment is preferably soluble in hydrocarbons described later. Furthermore, from the perspective of cost, the fluorine-containing compound of the present embodiment is particularly preferably soluble in toluene.
[0033] A cured product obtained by crosslinking the fluorine-containing compound of the present invention preferably has a gel fraction (crosslink density) of 50% or more as described above, but this is more preferably 80% or more, even more preferably 90% or more, and most preferably 100%.A large gel fraction (crosslink density) may have the effect of suppressing a reduction in durability due to the presence of unreacted crosslinking sites and reducing the coefficient of thermal expansion due to an increase in crosslink density.
[0034] Note that the gel fraction (crosslink density) of the cured product in the present specification is a value measured for the cured product after thermally curing the fluorine-containing compound at 200°C for 120 minutes. A method of measuring gel fraction is described later.
[0035] For a cured product obtained by crosslinking the fluorine-containing compound of the present invention, the glass transition temperature is preferably 200°C or higher. Furthermore, the coefficient of thermal expansion in a temperature environment above the glass transition temperature is preferably less than 200 ppm / °C, more preferably less than 180 ppm / °C, and even more preferably less than 150 ppm / °C. A glass transition temperature of 200°C or higher reduces the coefficient of thermal expansion (thermal expansion coefficient) under a normal use environment and improves durability when the cured product is used as an electronic substrate. In addition, the low coefficient of thermal expansion (thermal expansion coefficient) at high temperatures offers advantages such as use in high- temperature environments, easier soldering, and the like.
[0036] Note that the glass transition temperature and thermal expansion coefficient of the cured product in the present specification are values measured for the cured product after thermally curing the fluorine-containing compound at 200°C for 120 minutes. Methods for measuring the glass transition temperature and thermal expansion coefficient are described later.Preparation of Fluorine-containing Compound
[0037] As shown in the reaction formula below, the fluorine-containing compound of the present invention is manufactured by blending a bisphenol derivative (A), perfluorobiphenyl (B), and precursor of a substitution group X (C) in the presence of a base, either simultaneously or at a timing that does not cause a condensation reaction between the bisphenol derivative (A) and perfluorobiphenyl (B), and then heating and mixing.Chem. Fig. 8
[0038] Z in the precursor (C) in the reaction formula above is a leaving group, preferably selected from a group consisting of F, Cl, Br, and I, with F being more preferable.
[0039] The base to be used preferably includes an alkali metal carbonate, a hydrogen carbonate, and a hydroxide. Examples of preferred bases include sodium carbonate, potassium carbonate, sodium hydrogen carbonate, potassium hydrogen carbonate, sodium hydroxide, and potassium hydroxide. It is preferable to use a base having a normality of 2 Normal or more, and preferably 4 to 6 Normal, per 1 mol of the bisphenol derivative (A).
[0040] The heating and mixing described above are performed in an aprotic polar solvent or in a mixed solvent containing an aprotic polar solvent. Examples of preferred aprotic polar solvents include N, N-dimethylformamide (DMF), N,N-dimethylacetamide (DMAc), dimethyl sulfoxide (DMSO), sulfolane, and the like. The mixed solvent may contain a low polarity solvent, provided that the solubility of the fluorine-containing compound is not reduced and the reaction is not affected. Examples of low polarity solvents capable of being used include toluene, xylene, benzene, tetrahydrofuran, benzotrifluoride((trifluoromethyl)benzene), xylene hexafluoride(1 ,3-bis(trifluoromethyl)benzene), and the like. The polarity (dielectric constant) of the solvent mixture can be changed by the addition of a low polarity solvent to control the rate of the condensation reaction.
[0041] The heating and mixing are preferably performed under conditions of a reaction temperature of 10 to 200°C and a reaction time of 1 to 80 hours, preferably a reaction temperature of 20 to 180°C and a reaction time of 2 to 60 hours, and more preferably a reaction time of 50 to 160°C and a reaction time of 3 to 40 hours.(Fluorine-containing compositions)
[0042] Embodiment 2 of the present invention relates to a fluorine- containing composition containing fluorine-containing compound of Embodiment 1 and a crosslinking agent. The fluorine-containing compound of the present invention has excellent crosslinking properties itself, and therefore can exhibit excellent curability even without a crosslinking agent. However, by including a crosslinking agent, it is possible to obtain even superior curability and to impart sufficient hardness to a cured product containing the fluorine- containing composition.
[0043] The crosslinking agent used in the present embodiment includes a compound having two or more olefinic carbon-carbon double bonds in the molecule. Examples of crosslinking agents used in the present embodiment include: a polyfunctional methacrylate compound having two or more methacryl groups in a molecule, a polyfunctional acrylate compound having two or more acrylic groups in a molecule, triallyl isocyanurate (TAIC) and other trialkenyl isocyanurate compounds, divinylbenzene, and the like. Examples of polyfunctional acrylate / methacrylate compounds include: dicyclopentadiene type acrylate compounds such as tri cyclodecane dimethanol diacrylate and the like; and dicyclopentadiene type methacrylate compounds such as tricyclodecane dimethanol dimethacrylate and the like.
[0044] The fluorine-containing composition of the present embodiment may contain a crosslinking agent. Furthermore, in the fluorine-containingcomposition of the present embodiment, the mass ratio of the fluorine- containing compound to the crosslinking agent is preferably within a range of 9.5:0.5 to 5:5, and more preferably within a range of 7.5:2.5 to 5.5:4.5. The use of the mass ratio within this range can impart sufficient hardness to the cured product of the fluorine-containing composition.
[0045] The fluorine-containing composition of the present embodiment may further contain a solvent, a reaction initiator, and / or a filler. Furthermore, the fluorine-containing composition of the present embodiment may further contain any additives known in the art, such as antifoaming agents, thermal stabilizers, antistatic agents, ultraviolet absorbers, colorants (dyes or pigments), flame retardants, lubricants, dispersants, and the like.
[0046] The fluorine-containing composition of the present embodiment may be a varnish-like composition containing a solvent. In the present embodiment, various solvents can be used. From the perspective of solvent solubility, an aprotic solvent is preferably used in the present invention. The solvent used in the present embodiment may include: hydrocarbons such as benzene, toluene, xylene, heptane, cyclohexane, methylcyclohexane, mineral spirit, and the like; ketones such as acetone, methyl ethyl ketone (MEK), methyl isobutyl ketone (MIBK), diisobutyl ketone (DIBK), and the like; cyclic ketones such as cyclohexanone, cycloheptanone, cyclooctanone, and the like; esters such as ethyl acetate, butyl acetate, y-butyrolactone, and the like; cyclic ethers such as tetrahydrofuran (THF), 1 ,3-dioxolane, and the like; amides such as N,N-dimethylformamide (DMF), diethylformamide (DEF), N,N- dimethylacetamide (DMAc), N-methylpyrrolidone (NMP), N-cyclohexyl pyrrolidone, and the like; sulfones such as sulfolane, dimethylsulfone, and the like; and sulfoxides such as dimethylsulfoxide (DMSO). Preferable solvents for the present invention are hydrocarbons, and particularly preferably aromatic hydrocarbons.
[0047] The fluorine-containing composition of the present embodiment preferably includes a reaction initiator for a crosslinking reaction. Although crosslinking and curing by heating are possible in the absence of an initiator, ifa reaction initiator is present, more efficient crosslinking and curing is possible under milder conditions. Examples of the reaction initiators that can be used include benzoyl peroxide, di-t-butyl peroxide, t-butyl hydroperoxide, dicumyl peroxide, cumyl hydroperoxide, a,a'-di(t-butylperoxy)-diisopropylbenzene (Perbutyl P (registered trademark) available from NOP Corporation), bis(1 - methyl-1 -phenylethyl) peroxide (Percumyl D (registered trademark) available from NOF Corporation), t-butyl-a,a-dimethylbenzylperoxide (Perbutyl C (registered trademark) available from NOF Corporation), 2,5-dimethyl-2,5-di(t- butylperoxy)-3-hexene, 3,3',5,5'-tetramethyl-1 ,4-diphenaquinone, chloranyl, 2,4,6-tri-t-butylphenoxyl, t-butyl peroxyisopropyl monocarbonate, azobisisobutyronitrile, and the like.
[0048] The fluorine-containing composition of the present embodiment may further include one or a plurality of fillers. The filler may be an organic filler or an inorganic filler. Examples of organic fillers that can be used include: engineering plastics such as polyphenylene sulfide, polyether ether ketone (PEEK), polyamide, polyimide, polyamide-imide, and the like; and solventinsoluble fluororesins such as polytetrafluoroethylene (PTFE), perfluoroalkoxy alkane (PFA), and copolymer (FEP) of tetrafluoroethylene, hexafluoropropylene, and the like. Examples of inorganic fillers that can be used include: metals; aluminum oxide, zinc oxide, tin oxide, titanium oxide, and other metal oxides; metal hydroxides; titanic acid metal salts; zinc borate; zinc stannate; boehmite; silica; glass; silicon oxide; silicon carbide; boron nitride; calcium fluoride; carbon black; mica; talc; barium sulfate; molybdenum disulfide; and the like. Solvent-insoluble fluororesin is preferable in terms of improving the electrical properties (dielectric constant, dielectric loss, and the like) of the cured product of the fluorine-containing composition. Furthermore, silica is preferable in that the coefficient of thermal expansion can be reduced without impairing the electrical properties (dielectric constant, dielectric loss, and the like) of the cured product of the fluorine-containing composition.
[0049] The fluorine-containing composition of the present embodiment can be formed by mixing the fluorine-containing compound of Embodiment 1 , acrosslinking agent, and an optional component. Heating may be carried out during mixing. Mixing can also be carried out using an arbitrary mixing device known in the art, such as various stirrers, ball mills, bead mills, planetary mixers, roll mills, and the like.Prepreg
[0050] Embodiment 3 of the present invention relates to a prepreg including a semi-cured product of the fluorine-containing compound according to Embodiment 1 and a fibrous base material. The prepreg of the present embodiment may further include a reaction initiator for a crosslinking reaction. The reaction initiator that can be used in the present embodiment is the same as that of Embodiment 2.
[0051] Examples of fibrous base materials that can be used in the present embodiment include glass woven fabrics, aramid woven fabrics, polyester woven fabrics, carbon fiber woven fabrics, glass nonwoven fabrics, aramid nonwoven fabrics, polyester nonwoven fabrics, carbon fiber nonwoven fabrics, pulp paper, linter paper, and the like. A preferable fibrous base material is a glass woven fabric capable of achieving excellent mechanical strength. The fibrous base material desirably has a thickness of 0.01 mm to 0.3 mm.
[0052] The prepreg of the present embodiment can be formed by impregnating the fluorine-containing compound according to Embodiment 1 and an optional reaction initiator into the fibrous base material, which is then dried. Herein, the fluorine-containing compound to be impregnated is preferably in a varnish-like state containing a solvent. The solvent capable of being used is the same as in Embodiment 2. As a result of the drying process, the solvent in the varnish is at least partially removed and the fluorine- containing compound becomes semi-cured (so-called "B-stage"). The impregnating step can be performed by an arbitrary method known in the art, such as dipping, application, or the like. By impregnating the fluorine- containing compound and optional reaction initiator a plurality of times, the amount of fluorine-containing compound in the prepreg can be adjusted. Theconditions (temperature and time) of the drying step depend on the type of fluorine-containing compound and the type of optional reaction initiator and / or solvent. For example, the drying step can be performed by heating to a temperature of 80°C to 170°C for 1 to 60 minutes.
[0053] Embodiment 4 of the present invention relates to a prepreg including a semi-cured product of the fluorine-containing composition according to Embodiment 2 and a fibrous base material. The fibrous base material capable of being used in the present embodiment is the same as that of Embodiment 3.
[0054] The prepreg of the present embodiment can be formed by impregnating the fluorine-containing composition of Embodiment 2 into the fibrous base material and then drying. Herein, the fluorine-containing composition to be impregnated is preferably in a varnish-like state containing a solvent. As a result of the drying process, the solvent in the varnish is at least partially removed and the fluorine-containing composition becomes semicured (so-called "B-stage"). The impregnating step can be performed by an arbitrary method known in the art, such as dipping, application, or the like. By impregnating the fluorine-containing composition a plurality of times, the amount of fluorine-containing compound in the prepreg can be adjusted. The conditions (temperature and time) of the drying step depend on the type of fluorine-containing compound, crosslinking agent, and optional solvent included in the fluorine-containing composition. For example, the drying step can be performed by heating to a temperature of 80°C to 170°C for 1 to 60 minutes.Copper Clad Laminated Sheet
[0055] Embodiment 5 of the present invention relates to a copper clad laminated sheet, including a cured product of the prepreg according to Embodiment 3 or 4 and at least one copper layer.
[0056] The copper clad laminated sheet of the present embodiment can be formed by laminating one or a plurality of prepregs, laminating a copper foilon one or both surfaces thereof, and heating and pressing the obtained laminated product to integrate them. The fluorine-containing compound or composition in the copper clad laminated sheet is preferably in a state in which curing is complete (so-called "C stage"). The conditions of the heating and pressurizing process can be appropriately set based on the thickness of the copper clad laminated sheet to be manufactured, the composition of the fluorine-containing compound or composition in the prepreg, and the like. For example, the copper clad laminated sheet can be manufactured by heating to a temperature of 170°C to 220°Cfor60 to 150 minutes and applying a pressure of 1 .0 MPa to 10 MPa.Printed Circuit Board
[0057] Embodiment 6 of the present invention relates to a printed circuit board, including a cured product of the prepreg according to Embodiment 3 or 4 and a conductor pattern formed on the surface of the cured product.
[0058] The printed circuit board of the present embodiment can be manufactured by etching the copper layer of the copper clad laminated sheet of Embodiment 5 to form a conductor pattern. Alternatively, the printed circuit board can be manufactured via a method in which one or a plurality of prepregs are laminated, heated, and pressurized to form a laminated body, with the conductive material laminated in a pattern on the surface of the laminated body to form a conductor pattern.EXAMPLES(Example 1) (Synthesis of Fluorine-containing Compound, n = 1)
[0059] A glass reaction container was filled with 0.805 g (3.0 mmol) of 1 , 1- bis(4-hydroxyphenyl)cyclohexane (bisphenol Z), 0.501 g (1.5 mmol) of decafluorobiphenyl and 0.912 g (6.6 mmol) of potassium carbonate. The glass reaction container was decompressed to a vacuum and then substituted with nitrogen. Next, 10 mL of DMAc and 0.582 g (3.0 mmol) of 2, 3, 4,5,6- pentafluorostyrene were added to the glass reaction container. The reaction mixture was shielded from light, heated to 80°C with stirring, and then stirredfor 15 hours. Upon completion of heating, the reaction mixture was cooled to room temperature. The reaction mixture was subsequently poured into 0.5 L of pure water. The reaction mixture was suction filtered and the obtained solid was washed with pure water and methanol. After washing, the solid fraction was dried under reduced pressure to obtain 1.54 g of a fluorine-containing compound.
[0060] The average degree of polymerization calculated from a nuclear magnetic resonance spectrum (X-Plus, a nuclear magnetic resonance device manufactured by Oxford Instruments) was 1.0.(Example 2) (Synthesis of Fluorine-containing Compound, n = 2)
[0061] The procedure of Example 1 was repeated, except that 0.668 g (2.0 mmol) of decafluorobiphenyl and 0.388 g (2.0 mmol) of 2, 3, 4,5,6- pentafluorostyrene were used with respect to 0.805 g (3.0 mmol) of bisphenol Z to obtain 1 .50 g of a fluorine-containing compound.
[0062] The average degree of polymerization was calculated by nuclear magnetic resonance spectroscopy to be 1 .9.(Example 3) (Synthesis of Fluorine-containing Compound, n = 3)
[0063] The procedure of Example 1 was repeated, except that 0.752 g (2.3 mmol) of decafluorobiphenyl and 0.291 g (1.5 mmol) of 2, 3, 4,5,6- pentafluorostyrene were used with respect to 0.805 g (3.0 mmol) of bisphenol Z to obtain 1 .61 g of a fluorine-containing compound.
[0064] The average degree of polymerization was calculated by nuclear magnetic resonance spectroscopy to be 2.8.Example 4 Synthesis of Fluorine-containing Compound, n = 4
[0065] The procedure of Example 1 was repeated, except that 0.802 g (2.4 mmol) of decafluorobiphenyl and 0.233 g (1.2 mmol) of 2, 3, 4,5,6- pentafluorostyrene were used with respect to 0.805 g (3.0 mmol) of bisphenol Z to obtain 1 .58 g of a fluorine-containing compound.
[0066] The average degree of polymerization was calculated by nuclear magnetic resonance spectroscopy to be 3.5.(Example 5) (Synthesis of Fluorine-containing Compound, n = 1)
[0067] The procedure of Example 1 was repeated except that 0.889 g (3.0 mmol) of 1 ,1-bis(4-hydroxy-3-methylphenyl)cyclohexane was used instead of 0.805 g (3.0 mmol) of 1 ,1-bis(4-hydroxyphenyl) cyclohexane (bisphenol Z)to obtain 1.68 g of a fluorine-containing compound.
[0068] The average degree of polymerization was calculated by nuclear magnetic resonance spectroscopy to be 1 .0.Comparative Example 1 Synthesis of Fluororesin, n = 30
[0069] A fluororesin was obtained in accordance with a method described in Patent Document 4 (Japanese Unexamined Patent Application 2022- 89150).
[0070] In other words, a glass reaction container was filled with 0.805 g (3.0 mmol) of 1 , 1 -bis (4-hydroxyphenyl) cyclohexane (bisphenol Z) and 0.912 g (6.6 mmol) of potassium carbonate. The glass reaction container was decompressed to a vacuum and then substituted with nitrogen. 10 mL of DMAc was subsequently added to the glass reaction container. The reaction mixture was heated to 150°C while stirring, and then stirred for 3 hours. Upon completion of heating, the reaction mixture was cooled to room temperature. 0.802 g (2.4 mmol) of decafluoro biphenyl was subsequently added to the reaction mixture. The reaction mixture was heated to 70°C with stirring and stirred for 4 hours. The reaction mixture was subsequently shielded, after which 0.17 mL (0.233 g, 1.2 mmol) of 2, 3,4,5, 6-pentafluorostyrene was added thereto. Stirring was continued at a temperature of 70°C for 15 hours. Upon completion of stirring, the reaction mixture was cooled to room temperature. The reaction mixture was subsequently poured into 0.5 L of pure water. The reaction mixture was suction filtered and the obtained solid was washed with pure water and methanol. The washed solid fraction was decompressed and dried to obtain approximately 1 .14 g of a fluororesin.
[0071] The average degree of polymerization was determined by nuclear magnetic resonance spectroscopy to be 30.(Reference Example) Polyphenylene ether (PPE) resin
[0072] As a control for the performance of the fluorine-containing compounds of the present invention, various measurements were also performed on polyphenylene ether (PPE) resin (NORYL SA9000 available from SABIC), which is currently commonly used as a substrate material for high-frequency transmission.Evaluation 1 : Solvent solubility and thermosetting evaluation (gel fraction)
[0073] 0.5 g of each of the fluorine-containing compounds obtained inExamples 1 to 5, the fluororesin obtained in Comparative Example 1 , and the PPE resin of the Reference Example were weighed, toluene was added, and the mixture was heated to 80°C and mixed. If a solution of 50 mass% was obtained, the mixture was deemed to be toluene soluble.
[0074] All of the obtained solution was taken into aluminum cups and heated and dried at 200°C for 2 hours using a thermostatic oven (SPHH-102 available from ESPEC CORP.) to obtain a thermoset product. The thermoset product was removed from the aluminum cup and the weight was measured. A 9 mL sample tube was filled with 5 g of methyl ethyl ketone (MEK) and the cured product, and the cured product was immersed in MEK for 24 hours. Thereafter, the solvent was volatilized, washed with MEK, and the thermoset product was dried. The mass after drying was measured and the mass of the dried cured product after MEK immersion was calculated.
[0075] The gel fraction was calculated as mass of dried cured product after MEK immersion I mass of cured product before MEK immersion x 100 (%). The obtained results are shown in Table 1.Table 1
[0076] As shown in Table 1 , the fluorine-containing compounds of the present invention have a significantly larger gel fraction than the fluororesin of Comparative Example 1 , and it can be said that the gel fraction is as favorable as or superior to that of the PPE resin in terms of curability.Evaluation 2: Thermal expansion coefficient (coefficient of thermal expansion [CTE])
[0077] The fluorine-containing compounds obtained in Example 1 , the fluororesin obtained in Comparative Example 1 , and the PPE resin in the Reference Example were dissolved in toluene as described above to obtain a 50 mass% solution.
[0078] All of the obtained solution was taken in an aluminum cup and heated at 150°C for 1 hour using a thermostatic oven (SPHH-102 available from ESPEC CORP.) to remove the solvent, and then heated at 200°C for 2 hours to obtain a cured product. After cooling to room temperature, the cured product was peeled off and used as a test piece.
[0079] The thermal expansion coefficient was measured on the test piece using a dynamic viscoelasticity measurement device (DMAARES-G2 available from TA Instruments). The coefficient of thermal expansion between 240°C and 290°C is shown in Table 2.Table 2
[0080] Table 2 shows that the fluorine-containing compounds of the present invention have significantly lower thermal expansion coefficients than the Comparative Example and Reference Example, and have a unique characteristic of being resistant to expansion even in the high temperature region of 240°C to 290°C, which is at or above the glass transition temperature.(Evaluation 3: Electrical properties)[Preparation of varnish-like composition]
[0081] The fluorine-containing compounds obtained in Examples 1 to 5, the fluororesin obtained in Comparative Example 1 , and the PPE resin in the Reference Example were dissolved in toluene as described above to obtain a 50 mass% solution. Furthermore, Perbutyl (registered trademark) P (available from NOF Corporation) was added as a reaction initiator to 2 mass% with respect to the fluorine-containing compound to obtain a varnish-like composition.[Preparation of pre-preq]
[0082] Each varnish-like composition obtained by the method described above was dripped onto a 7 cm x 7 cm piece of glass cloth piece (L2-1078 available from Asahi Kasei Corporation) and then uniformly impregnated. Thereafter, the impregnated material was then dried at 110°C for 10 minutes to obtain a pre-preg.[Preparation of copper clad laminated sheet]
[0083] The pre-preg obtained by the method described above was cut into 5 cm x 5 cm pieces, and together with an electrolytic copper foil (thickness: 18pm) (HVLP available from FURUKAWA ELECTRIC CO., LTD.), the temperature was raised to 200°C while reducing the pressure using a vacuum hot press machine (manual hydraulic vacuum heating press IMC-4900 available from Imoto machinery Co., LTD.), and the pre-preg and copper foil were further adhered by pressing at 200°C for 120 minutes at 4 MPa.
[0084] The prepregs using the fluorine-containing compounds obtained in Examples 1 to 5 produced uniformly composited copper clad laminated sheets. However, when the fluororesin obtained in Comparative Example 1 was used, it could not be uniformly composited with the glass cloth, and a clean copper clad laminated sheet could not be obtained.
[0085] The copper foil of the copper clad laminated sheet prepared from the prepreg was peeled off with tweezers and cut into 4 cm x 4 cm test pieces, and the electrical properties (dielectric constant and dielectric tangent) were measured using a vector network analyzer (KEYSIGHT 5247B) using the split cylinder method under conditions of 28 GHz, 25°C.Table 3
[0086] Table 3 shows that the fluorine-containing compounds of the present invention are easy to process into copper clad laminated sheets, and furthermore, the dielectric tangent is greatly reduced in a very large frequency range of 28 GHz compared to PPE resin, which is currently commonly used as a substrate material for high-frequency transmission.(Evaluation 4: Glass transition temperature)
[0087] The copper-clad laminated sheets of Examples 1 and 5, Comparative Example 1 , and the reference example prepared for the aforementioned electrical characteristics evaluation were cut at an angle of 45 degrees to the mesh of the glass cloth, and test pieces 25 mm long x 25 mm wide were prepared.
[0088] Using these test pieces, the following temperature profiles were run using a dynamic viscoelasticity measurement device (DMA ARES-G2, available from TA Instruments) set to a frequency of 1.0 Hz and a strain of 0.1 %.(1 ) Hold at 25°C for 60 seconds and then heat from 25°C to 360°C at a rate of 5°C / min.(2) Maintain at a temperature of 360°C for 60 seconds, and end measurement.The temperature at the peak position of the loss coefficient (tan5) versus temperature in the calculated graph was assumed to be the glass transition temperature (Tg). The results are shown in Table 4.Table 4
[0089] The results in Table 4 show that the fluorine-containing compounds of the present invention have a higher glass transition temperature (Tg) than the Comparative Example. The higher Tg makes it less susceptible to thermal deformation and the like even when exposed to higher temperatures.
Claims
Claims1 . A fluorine-containing compound, comprising a structure according to the following Formula (I).[Chem. Fig. 1 ]In the formula, L represents a structure of the following Formula (II) or (HI).[Chem. Fig. 2]where R1and R2each independently represent a group selected from a group consisting of a hydrogen atom, Ci to Cw alkyl groups, Ci to Cw haloalkyl groups, and Ce to Cw aryl groups, or R1and R2may be combined together to form a ring structure that may include a substitution group,R3and R4each independently represent a group selected from a group consisting of a hydrogen atom, a fluorine atom, Ci to Cw saturated or unsaturated hydrocarbon groups in which some or all hydrogens may be substituted by a halogen and Ce to Cw aryl groups in which some or all hydrogens may be substituted by a halogen, n is in a range of 1 to 4, andX represents a group containing an olefinic carbon-carbon double bond or a carbon-carbon triple bond.
2. The fluorine-containing compound according to claim 1 , wherein the value of the thermal expansion coefficient of a cured product at 240°C to 290°C is 200 ppm / °C or less.
3. The fluorine-containing compound according to claim 1 or 2, wherein the n is 1 .
4. The fluorine-containing compound according to claim 1 or 2, wherein the X contains at least one fluorine atom.
5. The fluorine-containing compound according to claim 1 or 2, wherein the L is a group selected from a group consisting of cyclopentylidene groups that may have a substitution group, cyclohexylidene groups that may have a substitution group, and cyclododecylidene groups that may have a substitution group.
6. The fluorine-containing compound according to claim 1 or claim 2, wherein a gel fraction of a cured product is 50% or more.
7. A fluorine-containing composition, comprising: the fluorine-containing compound according to claim 1 ; and a crosslinking agent.
8. A prepreg, comprising: the fluorine-containing compound according to claim 1 ; and a fibrous base material.
9. A prepreg, comprising: the fluorine-containing composition according to claim 7; and a fibrous base material.
10. A copper clad laminated sheet, comprising: a cured product of the prepreg according to claim 8 or 9; and at least one copper layer.
11. A printed circuit board, comprising: a cured product of the prepreg according to claim 8 or 9; and a conductor pattern formed on a surface thereof.
Citation Information
Patent Citations
Polyphenylene ether resin composition, prepreg, metal-clad laminate, and printed wiring board
JP2017128718A
Fluorinated poly(arylene ether)
US5115082A
Crosslinkable fluorinated aromatic ether composition
US5179188A
Fluororesin
CN116685621A
Fluororesin
CN118159585A