Method for producing high-temperature coke, a high-temperature coke and use thereof
The thermal-oxidative coking method for producing high-temperature coke addresses the instability and low resistivity issues of existing cokes by achieving a coke with high structural strength and electrical resistivity, improving smelting performance and reducing energy consumption.
Patent Information
- Application Number
- PCT/EA2024/050008
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-05-02
- Filing Date
- 2024-04-27
- Publication Date
- 2024-11-07
AI Technical Summary
Existing high-temperature cokes used in electrothermal processes suffer from unstable structural strength and low electrical resistivity, leading to mechanical destruction during transportation and increased energy consumption, due to high volatile content and low specific electrical resistance.
A method for producing high-temperature coke through thermal-oxidative coking of coal at 900-1200°C with a heating rate of over 50°C/min, using a shaft furnace with controlled air flow, resulting in a product with less than 3.0% volatile substances and structural strength of at least 80%, suitable for use as a carbonaceous reducing agent in electrothermal processes.
The method produces a coke with improved structural strength and electrical resistivity, enhancing smelting performance, reducing raw material and electricity consumption, and improving the quality of smelted products by minimizing fine fraction formation and volatile-induced furnace issues.
Smart Images

Figure IMGF000015_0001 
Figure IMGF000016_0001 
Figure IMGF000018_0001
Abstract
Description
[0001] METHOD OF PRODUCING HIGH-TEMPERATURE COKE, HIGH-TEMPERATURE COKE AND ITS APPLICATION
[0002] Field of technology
[0003] The invention relates to the field of coal processing, in particular to the processing of low-grade non-caking coal, with the production of high-temperature coke as a product, which can be used in electrothermal production, namely in the production of various grades of ferroalloys, as well as silicon, calcium carbide, phosphorus and other products, where coke plays the role of a carbonaceous reducing agent.
[0004] The use of high-temperature coke as a reducing agent in electrothermal production does not exclude the possibility of its additional use as a fuel in various processes, for example, in the agglomeration and metallization of ore raw materials or in shaft and rotary kilns, as well as in the production of intermediate products of non-ferrous metallurgy.
[0005] State of the art
[0006] The following basic requirements are imposed on coke for electrothermal production:
[0007] • high carbon content (80-85%);
[0008] • minimum content of harmful elements (sulfur, phosphorus) in the mineral part, which worsen the quality of the product;
[0009] • developed porous structure;
[0010] • high electrical resistance;
[0011] • low yield of volatile substances without residual resin products;
[0012] • sufficiently high mechanical strength;
[0013] • optimal size (5-20 mm).
[0014] Numerous studies in the field of obtaining special types of coke - reducing agents that best meet the needs of electrothermal processes are aimed at satisfying the above requirements. As a result of the studies, it was established that the lower the caking of coals, the less dense the contact between the residual material of the original coal grains or petrographic microcomponents within one grain, the more defects in the structure of the coke substance and the higher its reactivity and electrical resistance.
[0015] Coking of non-caking coals or low-caking coals allows achieving increased indicators of chemical activity and electrical resistance of coke. Thus, the most promising for obtaining coke as a carbonaceous reducing agent in electrothermal processes may be non-caking or low-caking coals of a low stage of metamorphism of grades D, G, SS and T. (V.M. Strakhov, "Scientific and production aspects of obtaining special types of coke for electrothermal production", "Coke and Chemistry" No. 9, 2008, pp. 44-49).
[0016] In thermal-oxidative coking, the coke properties characterizing the volatile content and structural strength are affected by the parameters characterizing the coking temperature and the heating rate during coking. That is, the higher the coking temperature, the lower the volatile content in the coke, and the higher the heating rate, the higher the structural strength. For example, a product of high-speed thermal-oxidative coking obtained at high coking temperatures of 1000-1500°C is known from the prior art - this is the carbonizate "Rexil", disclosed in patent KZ23615, IPC: C01B57 / 00, published on 15.12.2010. The volatile content in the carbonizate Rexil is 0.1-3.5% with a structural strength of 70-85%. Additionally, we note that the carbon reducing agent "Rexil" is also disclosed in the Eurasian patent EA024335, IPC: C01B57 / 00, published on September 30, 2016. The carbonized Rexil is obtained from energy coals and is used as a basic reducing agent for smelting crystalline silicon.The specified carbonizate has the following composition and properties in total:.
[0017] Ash (Ad) 1.0 -5.0%,
[0018] Volatile matter (Vdaf) 0.1-3.5%,
[0019] Carbon (C) (91.5 - 98.9%),
[0020] Sulfur - 0.35 wt.%,
[0021] Reactivity 7-12 ml / g-s,
[0022] The specific electrical resistance at 1000°C is no more than 2.7 Ohm cm.
[0023] However, the above patent publications present a very large spread of values characterizing the heating rate during coking from 20 to 400 °C / min, which leads to general instability of the product properties, in particular to instability of the properties characterizing structural strength, the spread in the range of strength indicators is from 70 to 85%. In addition, we note that higher structural strength indicators were achieved under the conditions of processing a specific type of coal: grade "D" coal of the Kuznetsk coal basin, and from the energy coals of the Shubarkol open-pit mine, the strength of the same carbonizate was only 65-75%.
[0024] The disadvantages of Rexil carbonizate are the unstable structural strength of this product, which is the cause of partial mechanical destruction of this type of coke during transportation, dosing and transportation along the feeder tracts. The resulting fines of 0-10 mm fraction can cause sintering of the furnace throat, disruption of the electrode seating and increased consumption of electricity and reducing agent;
[0025] - the low specific electrical resistance of Rexil (at 1000°C it is less than 2.7 Ohm cm) can cause a violation of the electrode seating and an increased specific consumption of raw materials and electricity.
[0026] Eurasian patent EA030092, IPC: C10L5 / 12, published on 29.06.2018, contains the following information about the obtained product "HIGH-RESISTANCE COKE". High-resistance coke consists of a solid carbonaceous reducing agent impregnated with an aqueous emulsion based on gas cleaning dust - microsilica. In this quality of the solid carbonaceous reducing agent, it contains a product of high-speed thermal-oxidative pyrolysis of hard long-flame coal grade D, with a developed fine-porous structure and a specific surface area of 50-300 m 2 / g, of the following technical composition in wt.%: ash - 0.1-5.0%; volatile substances - 0.1-10.0%; sulfur - no more than 0.5%; phosphorus - no more than 0.04%, the rest is carbon, with the following ratio of components after impregnation (wt.%): carbon material: 75.0-99.0%; gas cleaning dust - microsilica: 1.0-25.0%.
[0027] The patent description also states that the structural strength of the carbonaceous reducing agent is 67-75%, the reactivity is 2.0-6.0 ml / g-s, and the specific electrical resistance (SER) at 1000°C is 2.7 ohm-cm.
[0028] From the given information on the properties of this product it follows that it is characterized by low structural strength with low values of the resistivity - at 1000 ° C, which is a disadvantage of this material. In addition, it should be noted that the presence of an additional feature characterizing the impregnation of a carbonaceous reducing agent with an aqueous emulsion based on gas cleaning dust (microsilica) in an amount of up to 25 wt.% turns this product into a composite material, therefore "High-Resistance Coke" is not a close analogue of the claimed invention, but refers to a different type of material compared to pure coke.
[0029] From the prior art for class IPC: C 10B 1 / 00, the publication of two patents RU2745271, IPC: C 10B 1 / 04, published on 03 / 22 / 2021 and RU2745272, IPC: C 10B 1 / 00, published on 03 / 22 / 2021, both under the title "Method and device for obtaining coal pyrolysis products", which also disclose a product in the form of a carbonizate introduced into civil circulation under the name "Carbosil E" (RF certificate for trademark No. 827224) were identified. The characteristics of this product are presented on the manufacturer's website: httDs: / / eDos-nsk.ru / tehnologii / karbosil-e-vosstanovitel-karbonizat-analog-koksa- i-polukoksa / /
[0030] The raw material for obtaining the Karbosil carbonizate is coal of the D, D(V), DG, DG(V), G, GZh, SS, T grades with a coal fraction size of no more than 50 mm. The Karbosil carbonizate is obtained by conducting high-temperature electric discharge roasting of lump carbon fractions in a hollow retort made of graphite, with the supply of an oxidizer - an air flow - to the heat treatment zone.
[0031] The resulting carbonizate is characterized by the following properties:
[0032] Porosity - 45-75 vol.%,
[0033] Reactivity - 4.00-8.00 cm 3 / g.s,
[0034] Ash - 5.3-14 wt.%,
[0035] Moisture - 1.5 - 4.7 wt.%,
[0036] Volatile - 7.3 - 8.5 wt.%,
[0037] Structural strength - 71%.
[0038] Specific electrical resistance at 1600K - 3.0-8.0 Ohm cm.
[0039] The disadvantages of the product "Carbosil E" include its low structural strength, high content of volatiles and high cost. The high cost is due to the increased energy costs for the production of this product, since electric discharge, high-temperature firing of lump, carbon fractions is used. Additionally, it should be noted that patents RU2745271 and RU2745272 indicate a retort made of graphite, which is a very expensive and non-technological material, for implementing the method for producing this carbonizate.
[0040] Thus, the product Karbosil cannot be called a close analogue of the claimed invention “High-temperature coke”, since it is produced by another industrial method, namely, electric discharge firing in graphite retorts, which does not apply to the technology used in the production of high-temperature coke.
[0041] The prior art includes the “Innovative carbon-containing product and method for producing it”, protected by patent RU2733610, MIC: C10B57 / 04, published on 05.10.2020.
[0042] The innovative carbon-containing product is an analogue of coal coke, which can be used in metallurgy. The innovative carbon-containing product is characterized by the fact that it is obtained in the process of layer coking of coal charge, consisting of 60-100% of coals of one or several grades, conditionally suitable for coking, and 0-40% of coking coals. The innovative carbon-containing product is characterized by the following properties:
[0043] Ash content - 11.5 wt.%,
[0044] Volatile yield - 0.9 - 1.0 wt.%,
[0045] Mass fraction of carbon 82.3 wt.%,
[0046] Strength index after reaction with carbon dioxide 25-40%,
[0047] The content of fractions not less than 25 mm is 92%.
[0048] Low structural strength of the product "Innovative carbon-containing product" prevents its successful use as a reducing agent in ferroalloy production, in particular in the production of ferrosilicon, since low structural strength is the cause of the formation of coke fines during the preparation, transportation and dosing of the charge. Low structural strength leads to deterioration of production indicators, causing sintering of the furnace throat and disruption of its gas permeability, to the loss of coke with dust removal as a result of combustion of small classes in the furnace throat. In terms of structural strength, the proposed high-temperature coke significantly exceeds the "Innovative carbon-containing product", therefore it cannot be considered a close analogue of the declared product.
[0049] From the description of patent RU2275407, MIC: 49 / 02, published on 27.04.2006, a method for producing metallurgical semi-coke and a product obtained by this method are known. The product of this method is a carbonizate, manufactured according to the example from Shubarkol coal grade D or from coal grade B2 of the Berezovskoye deposit, obtained by thermal-oxidative coking by heat treatment of a coal layer in a vertical shaft-type apparatus with ignition of the raw material from the side opposite to the air supply.
[0050] The product obtained under patent RU2275407 has the following properties:
[0051] Ash content, Ad, - 5.4-15%,
[0052] Structural strength of semi-coke is 60-74.8%,
[0053] Apparent density of semi-coke - 0.68 - 0.45 g / cubic meter,
[0054] It should be noted that the product of the method according to patent RU2275407 is semi-coke obtained at raw material heating temperatures below 900°C, characterized by low structural strength in the range of 60-74.8%, therefore it also cannot be considered a close analogue of the claimed invention.
[0055] It is also known to use petroleum coke and charcoal as carbon reducing agents for smelting silicon. For example, in the article by the authors O.I. Doshlov and M.I. Lubinsky "Highly reactive petroleum coke-carbon reducing agent for smelting chemically pure silicon" (BULLETIN OF Irkutsk State Technical University No. 6 (53), 2011, pp. 88-90) the properties of petroleum coke and charcoal are disclosed in relation to the possibility of their use in smelting silicon. The disadvantages of this type of reducing agents are their low structural strength and insufficient level of electrical resistance at high temperatures up to 1000 °C. Thus, the mechanical strength of petroleum coke is 20.4-26.8%, and charcoal - 77.0%. Low mechanical strength is the reason for partial destruction of this type of reducing agent during transportation, dosing and transportation along the batch feed paths.The resulting fines of 0-10 mm fraction can cause sintering of the furnace throat, disruption of the electrode seating and increased consumption of electricity and reducing agent.
[0056] The closest analogue of the claimed invention is carbonizate and the method for its production by thermal-oxidative coking, called Direxil, protected by the patent of the Republic of Kazakhstan KZ26466, IPC: C10B49 / 02, published on 14.12.2012, which can be used as a solid carbonaceous reducing agent in electrometallurgical processes for smelting pure metals, including smelting silicon by electrothermal method.
[0057] Direxil carbonizate is obtained from enriched non-caking coal by high-speed thermal-oxidative carbonization at a temperature of 950±50°C to obtain a product of the following composition:
[0058] Ash (Ad) 1.0-5.0%;
[0059] Volatile matter (Vdal) 3.6 - 15.0%;
[0060] Sulfur 0.20 -0.40%,
[0061] Phosphorus 0.010 - 0.040%.
[0062] The product Direxil is characterized by a structural strength of 65-75%, a reactivity of 7-12 ml / g-s and a specific electrical resistance (SER) at 1000°C of 2.9 ohm-cm.
[0063] The disadvantages of the prototype are the high content of volatile substances in the Direxil product up to 15%, which worsens the gas permeability of the furnace throat and complicates the operation of the gas cleaning of ore-reducing electric furnaces, as well as low structural strength (no more than 75%), which contributes to the formation of fines of the reducing agent during dosing and transportation and causes disruption of the electrode seating and increased specific consumption of raw materials and electricity.
[0064] The essence of the invention
[0065] The claimed invention is aimed at solving the problem of obtaining an effective solid carbonaceous reducing agent from coal using a thermal-oxidative method - "High-temperature coke" for electrothermal processes, containing no more than 3.0% volatile substances and having a structural strength of at least 80%.
[0066] In this application, thermal-oxidative coking is understood to mean the heat treatment of a layer of coal in a shaft-type apparatus, in particular a shaft furnace, with ignition of the raw material from the side opposite to the air supply.
[0067] The technical result of the invention is the production of a carbonaceous reducing agent with improved technological characteristics and stable physical and chemical properties, such as structural strength and high specific electrical resistance (SER) at 1000°C, which are necessary to increase the smelting performance in electrothermal processes, in particular, to increase the specific productivity of an electric smelting furnace, reduce the specific consumption of raw materials and electricity, and improve the quality of smelted products.
[0068] To solve the stated problem and achieve the technical result, a method for producing high-temperature coke for electrothermal processes is declared, as well as the product of this method - high-temperature coke and the use of the said product as a carbonaceous reducing agent in electrothermal processes.
[0069] The method for producing high-temperature coke for electrothermal processes by thermal-oxidative coking of coal is characterized by the fact that thermal-oxidative coking is carried out at a temperature of 900-1200°C, while heating of coal to the specified temperature is carried out at a heating rate of over 50°C / min, with the production of coke with a specific high-temperature electrical resistance of at least 3.5 Ohm-cm at 1000°C.
[0070] In a preferred embodiment, the method for producing high-temperature coke consists of thermal-oxidative coking of coal, which is carried out using a shaft furnace equipped with an air blast supplied to the furnace from below, while the ignition of the coal loaded into the shaft furnace is carried out from above, while the air consumption for the air blast is 150-400 m 3 per hour per 1 m 2cross-sectional area of the shaft furnace, preferably the air flow rate is 320 - 400 m3 per hour per 1 m3 of cross-sectional area of the shaft furnace.
[0071] In a more preferred embodiment, unenriched coal with a size of up to 100 mm, preferably with a size of 5-50 mm, and most preferably with a size of 10-30 mm is used for thermal-oxidative coking. The proposed method can process coals of various grades (D, G, GZh, SS, T, K, KO, B, etc.). However, high-quality coking coals are a scarce raw material, so the advantage of the claimed method is the possibility of processing low-grade unenriched non-caking coal, while thermal-oxidative coking is preferably carried out at a temperature of 950-1100 °C and a coal heating rate in the range of 50-90 °C / min, in particular, at a coal heating rate of at least 60 °C / min, most preferably, at a coal heating rate of 60-65 °C / min. After completion of the thermal-oxidative coking process, wet coke quenching is carried out.
[0072] High-temperature coke is produced using a shaft furnace. A shaft furnace is an industrial furnace with an upwardly elongated working space (shaft) of a round (cylindrical, conical) or rectangular shape. Shaft furnaces for coal coking are also called retorts.
[0073] The claimed method for producing high-temperature coke is carried out using a shaft furnace containing a body having an upper part and a lower part. A thermocouple is installed in the lower part, and before loading coal into the shaft furnace, the lower part is filled with coke in such a way that the coal-coke interface is at the level of the said thermocouple, so that when the combustion front reaches the said thermocouple, the air blast is automatically switched off. Preliminary loading of the lower part of the shaft furnace with coke allows for protection of the structural elements of the device from overheating. The location of the coal-coke interface at the level of the said thermocouple allows for more precise regulation of the furnace operation, ensuring energy and water savings.
[0074] The shaft furnace used in the claimed method preferably comprises an upper part of a substantially cylindrical shape, the lower part has a shape in the form of a truncated cone. In this case, the mentioned lower part of the furnace comprises a horizontal gas distribution ring, placed in such a way that at least part of the air blast can be directed under it. This ensures uniform air flow over the entire area of the furnace, which helps to increase the synchronicity and speed of movement of the combustion front, ensuring an increase in the specific productivity of the installation. The optimal vertical speed of movement of the combustion front is 0.16-0.4 cm / min, which ensures the stability of the coking process.
[0075] The product of the claimed method is high-temperature coke for electrothermal processes, obtained by thermal-oxidative coking of coal, characterized in that thermal-oxidative coking is carried out at a temperature of 900-1200°C, and the heating of the coal to the said temperature is carried out at a heating rate of over 50°C / min to obtain a carbonaceous reducing agent with a high-temperature specific electrical resistance of at least 3.5 Ohm-cm at 1000°C.
[0076] The declared high-temperature coke is characterized by a volatile content of no more than 3.0 wt.% with its structural strength of at least 76-80%. Moreover, a higher-quality product can be obtained using unenriched non-caking coal with a reduced content of sulfur and phosphorus.
[0077] High-temperature coke in the preferred embodiment is characterized by: structural strength of 80-83%, reactivity at 1000°C of at least 3.9 ml / (g-s), high-temperature specific electrical resistance at 1000°C of 3.5-3.8 Ohm-cm; with the following content of components of the carbonaceous reducing agent (in mass%): ash - 5.0-8.0, volatile substances 1.5-3.0, sulfur - no more than 0.3, phosphorus - no more than 0.035, the rest is carbon.
[0078] The use of the above-mentioned high-temperature coke as a carbonaceous reducing agent in electrothermal processes is also claimed.
[0079] Electrothermal processes include both electrometallurgical processes for smelting ferroalloys and electrothermal processes for smelting silicon, phosphorus and a number of carbides.
[0080] The scope of this invention includes the use of high-temperature coke as a carbonaceous reducing agent in electrometallurgical processes for smelting ferroalloys, in particular ferrosilicon.
[0081] The use of high-temperature coke as a carbonaceous reducing agent in electrothermal processes for smelting silicon and phosphorus is also claimed.
[0082] Implementation of the invention
[0083] The proposed solid carbonaceous reducing agent "High-temperature coke" is obtained by high-speed thermal-oxidative coking from unenriched, predominantly low-grade non-caking coal of fraction 5-50 mm at a temperature of 900-1200°C and a coal heating rate of over 50°C / min.
[0084] Coking coals are in short supply, and the traditional production of reducing agents for metallurgical processes from high-quality coking coals, for example, in the form of coke nut (GOST 8935-77) faces the problem of raw material shortage. Therefore, the problem of involving low-grade energy coals in the raw material base is relevant, which is also solved within the framework of the claimed invention. The method for producing high-temperature coke can be implemented using a mobile or stationary coking unit, which is a vertical shaft furnace (retort) of periodic action with a capacity of 20 to 60 tons of raw material in the form of coal with a size of up to 100 mm, preferably coal of fraction 5-50 mm.
[0085] The shaft furnace has a hollow, elongated top body, which has a discharge hatch at the bottom for unloading finished coke. In the upper part of the shaft furnace body there is a loading opening for filling raw materials, a branch pipe for removing coke gas and an automatic three-circuit coke quenching system. In this case, air blast is supplied to the furnace from below, from the side of the discharge hatch. Ignition of the coal charge is carried out from above. Air consumption for coking is from 150 to 400 m 3 / hour per 1 m 2 , preferably from 320 to 400 m 3 per hour per 1 m 2 cross-sectional area of the furnace, which helps to increase the speed of the combustion front, ensuring an increase in the specific productivity of the installation.
[0086] A thermocouple is installed in the lower part of the shaft furnace, and before loading coal into the shaft furnace, its lower part is filled with coke in such a way that the coal-coke interface is at the level of the said thermocouple, so that when the combustion front reaches the said thermocouple, the air blast can be automatically switched off. This ensures protection of the installation's structural elements from overheating. The location of the coal-coke interface at the level of the said thermocouple allows the furnace operation to be regulated, ensuring energy and water savings.
[0087] In this case, the said lower part of the furnace contains a horizontal gas distribution ring, placed in such a way that at least part of the air blast can be directed under it, which allows for uniform air flow over the entire area of the furnace, which helps to increase the speed of movement of the combustion front, ensuring an increase in the specific productivity of the installation in the range of 0.16-0.4 cm / min.
[0088] Thermal-oxidative coking is carried out at a temperature in the range of 900-1200°C, wherein the heating of the coal to the said temperature is carried out at a heating rate above 50°C / min with the production of a carbonaceous reducing agent with a high-temperature specific electrical resistance of at least 3.5-3.8 Ohm-cm at 1000°C. The said coal heating rate is preferably in the range of 50-90°C / min, wherein the carbonaceous reducing agent is characterized by a reduced content of volatile substances in the range of 1.5 - 3.0 wt.% with a structural strength of the product of at least 80%.
[0089] High-temperature coke can be obtained from various grades of coal, including non-caking coal.
[0090] The high-temperature coke obtained under the specified conditions is a loose lump material of silvery-black color with a lump size of 5 to 30 mm, with a bulk density of 0.37-0.42 t / m3. 3, which is characterized by the following properties: structural strength of 80-83%, reactivity at 1000°C of at least 3.9 ml / (g-s), high-temperature specific electrical resistance at 1000°C of 3.5-3.8 Ohm-cm; with the following content of components of the carbonaceous reducing agent (in mass%): ash - 5.0-8.0; volatile substances 1.5-3.05; sulfur - no more than 0.3; phosphorus - no more than 0.035; the rest is carbon.
[0091] This product can be used as a carbonaceous reducing agent in various electrothermal processes for smelting ferroalloys, such as ferrosilicon and ferromanganese, as well as in the smelting of pure silicon or phosphorus.
[0092] An essential feature of the product "High-temperature coke" and its difference from the prototype - carbonizate "Direxil" is the increased and stable structural strength, achieved in the range of 80-82% versus 65-75%, which allows to a significant extent to prevent the destruction of coke and the formation of small fractions (less than 10 mm) during transportation, dosing and transportation along the feed lines of ferroalloy enterprises.
[0093] In addition, in comparison with the prototype, high-temperature coke has a reduced content of volatile substances (1.5-3.0% versus 3.6-15.0%), i.e. it contains more solid (fixed) carbon, which is the leading useful element of any carbonaceous reducing agent. This is an important aspect, since the presence of excess volatile substances in the reducing agent leads to deterioration in the operation of furnaces due to sintering of the furnace throat and passivation of the reaction surface of the reducing agent due to deposits of pyrolytic carbon formed from high-molecular compounds contained in the volatile substances. In addition to low chemical activity, pyrolytic carbon is characterized by high electrical conductivity, which in turn contributes to a decrease in the high-temperature resistivity of the reducing agent and leads to disruptions in the operation of the electric furnace.
[0094] The invention is illustrated by the following examples.
[0095] Example 1.
[0096] The proposed carbonaceous reducing agent - "High-temperature coke" was obtained in a stationary coking unit, which includes a vertical shaft furnace of periodic action - a retort. At the bottom of the furnace there is a hatch for unloading finished coke. In the upper part of the furnace there is a loading opening for filling raw materials, a branch pipe for removing coke gas and an automatic three-circuit coke quenching system. In this case, air blast was supplied to the furnace from below, from the side of the unloading hatch. Ignition of the coal charge was carried out from above. Air consumption for coking was 340 - 350 m 3 per hour per 1 m 2 cross-sectional area of the furnace. High-speed thermal-oxidative coking of unenriched non-caking coal of grade D from the Kuznetsk coal basin with a grain size of 10-30 mm was carried out at a temperature of P50±50°C and a coal heating rate of 57°C per minute.
[0097] A comparison of the characteristics of the proposed carbonaceous reducing agent “High-temperature Coke” and the prototype Direxil is given in Table 1.
[0098] Table 1 When obtaining the high-temperature coke product, it was noted that in order to reduce harmful impurities in this product, sulfur below 0.27 wt.% and phosphorus below 0.03 wt.%, non-caking coals with a reduced content of sulfur, phosphorus and other impurities should be selected as the feedstock.
[0099] To test the possibility of using the new carbonaceous reducing agent in electrothermal and electrometallurgical processes, semi-industrial tests were conducted on smelting ferrosilicon grade FS75 (GOST 1415-93) in an experimental ore-thermal electric furnace with a transformer capacity of 300 kVA. Two smelting options were tested: a basic one using Direxil carbonizate as a reducing agent and an experimental one with a complete replacement of Direxil with the product High-temperature Coke. The test results are summarized in Table 2.
[0100] Table 2
[0101] From the data provided it is evident that the transition to high-temperature coke in the experimental smelting variant was accompanied by the following changes in technical and economic indicators:
[0102] - increase in specific furnace productivity by 3.5%;
[0103] - reduction of specific energy consumption by 1.8%;
[0104] - reduction of specific consumption of reducing agent by 2.7%;
[0105] - increase in silicon content in ferroalloy by 0.4%.
[0106] Thus, according to example 1, the advantage of the invention compared to the prototype is an increase in the quality characteristics of the carbon reducing agent and an improvement in the technical and economic indicators of smelting ferroalloys (ferrosilicon FS75).
[0107] The obtained carbonaceous reducing agent is characterized by stable physical and chemical properties, such as structural strength in a narrow range of 81.2-82.0% and high specific electrical resistance (SER) at 1000°C of 3.7 Ohm cm, which are necessary to increase the smelting indices in electrothermal processes, in particular, to increase the specific productivity of the electric smelting furnace, reduce the specific consumption of raw materials and electricity. An increase in the quality of the smelted ferrositium due to an increase in the Si content in the ferroalloy is also noted.
[0108] The carbonaceous reducing agent with the characteristics obtained in Example 1 also meets the technological requirements for its use as a reducing agent in the smelting of pure silicon and in the production of phosphorus in electric furnaces.
[0109] The process of phosphorus smelting is similar to the process of producing ferroalloys.
[0110] When smelting phosphorus, a carbonaceous reducing agent is also required; smelting is carried out in ore-thermal electric furnaces, which are practically no different from ferroalloy furnaces for smelting silicon, manganese, chromium and other ferroalloys. In obtaining phosphorus, coke plays the same role as in smelting ferroalloys, i.e. it reduces phosphorus from oxides under high-temperature conditions and serves as a conductor of electric current, providing heat for the necessary chemical reactions.
[0111] Example 2
[0112] The proposed carbonaceous reducing agent, "High-temperature coke", was obtained in the same way as in Example 1, in a stationary coking unit, including a vertical shaft furnace of periodic action. Air blast was supplied to the furnace from below, and the coal charge was ignited from above. Air consumption for coking was 260 - 270 m 3 per hour per 1 m 2 cross-sectional area of the furnace. High-speed thermal-oxidative coking of unenriched non-caking coal of grade D from the Kuznetsk coal basin with a size of 13-30 mm was carried out at a temperature of 960±30°C and a coal heating rate of 43°C per minute.
[0113] A comparison of the characteristics of the proposed carbonaceous reducing agent “High-temperature Coke” and the prototype Direxil is given in Table 3. Table 3
[0114] To evaluate the physicochemical and technological characteristics of high-temperature coke as a new carbonaceous reducing agent in the process of electrothermal production of technical silicon of the KrZ grade, semi-industrial tests were carried out in a large-scale single-electrode ore-thermal unit with a transformer capacity of 200 kVA. In this case, two smelting options were tested: a basic one using a mixture of charcoal and petroleum coke as a reducing agent, and an experimental one with a complete replacement of the reducing composition with the product "High-temperature coke". The test results are summarized in Table 4.
[0115] Table 4
[0116] From the data provided it is evident that the transition to high-temperature coke in the experimental smelting variant was accompanied by the following changes in technical and economic indicators:
[0117] - an increase in the specific productivity of the furnace (the ratio of the mass of the obtained alloy to the duration of the furnace operation) by 8%;
[0118] - reduction of specific energy consumption by 1.02%;
[0119] - increase in silicon extraction by 4.2%;
[0120] - increase in silicon content in metal by 0.47%.
[0121] Thus, according to example 2, the advantage of the invention compared to traditionally used reducing agents is the improvement of the technical and economic indicators of smelting technical silicon and an increase in the quality of the metal.
[0122] The obtained carbonaceous reducing agent is characterized by stable physical and chemical properties, such as structural strength in a narrow range of 76-79% and specific electrical resistance (SER) at 1000°C of at least 3.8 Ohm-cm, which are necessary to increase the smelting indices in electrothermal processes, in particular, to improve the electrode seating, increase the specific productivity of the electric smelting furnace, and increase the degree of extraction of the leading element. Also, despite the increased ash content of high-temperature coke in comparison with charcoal and petroleum coke (petroleum coke), an increase in the silicon content in the alloy was noted due to an increase in the degree of silicon extraction during smelting and a reduction in silicon losses caused by the escape of gaseous silicon monoxide.
[0123] The described embodiment examples are given solely for illustrative purposes. It will be obvious to a specialist that other embodiments are possible without changing the essence of the invention.
Claims
Invention formula 1. A method for producing high-temperature coke for electrothermal processes by thermal-oxidative coking of coal, characterized in that thermal-oxidative coking is carried out at a temperature of 900-1200°C, while heating of coal to the said temperature is carried out at a heating rate in excess of 50°C / min, with the production of high-temperature coke with a specific high-temperature electrical resistance of at least 3.5 Ohm-cm at 1000°C.
2. The method according to item 1, characterized in that the thermal-oxidative coking of coal is carried out using a shaft furnace equipped with an air blast, which is fed into the furnace from below, and the ignition of the coal loaded into the shaft furnace is carried out from above, while the air consumption for the air blast is 150-400 m 3 per hour per 1 m 2 cross-sectional area of the shaft furnace, preferably the air flow rate is 320 - 400 m 3 per hour per 1 m 2cross-sectional area of the shaft furnace.
3. The method according to item 1, characterized in that unenriched coal with a size of up to 100 mm, preferably with a size of 5-50 mm, and most preferably with a size of 10-30 mm, is used for thermal-oxidative coking.
4. The method according to claim 1, characterized in that unenriched, non-caking coal is used for thermal-oxidative coking, wherein thermal-oxidative coking is carried out at a temperature of 950-100°C and a coal heating rate in the range of 50-90°C / min, preferably at a coal heating rate of at least 60°C / min, most preferably at a coal heating rate of 60-65°C / min.
5. The method according to item 1, characterized in that after completion of the thermal-oxidative coking process, wet quenching of the coke is carried out.
6. The method according to item 2, characterized in that a shaft furnace is used, comprising an upper part and a lower part in which a thermocouple is installed, and before loading coal into the shaft furnace, the lower part is filled with coke in such a way that the coal-coke interface is at the level of said thermocouple, and when the combustion front reaches said thermocouple, the air blast is automatically turned off.
7. The method according to item 6, characterized in that the upper part of the shaft furnace is made essentially cylindrical in shape, and the lower part is made essentially in the shape of a truncated cone.
8. The method according to paragraph 6, characterized in that the lower part of the shaft furnace is provided with a horizontal gas distribution ring, positioned in such a way that at least part of the air blast can be directed underneath it.
9. The method according to paragraph 2, characterized in that during thermal-oxidative coking the vertical velocity of the combustion front is selected in the range of 0.16-0.4 cm / min.
10. High-temperature coke for electrothermal processes, obtained by thermal-oxidative coking of coal, characterized in that thermal-oxidative coking is carried out at a temperature of 900-1200°C, and the heating of the coal to the said temperature is carried out at a heating rate above 50°C / min to obtain high-temperature coke with a specific high-temperature electrical resistance of at least 3.5 Ohm-cm at 1000°C.
11. High-temperature coke according to clause 10, characterized in that it is characterized by a volatile substance content of no more than 3.05 wt.% with a structural strength of 76-83% and a reactivity at 1000°C of at least 3.9 ml / (g-s).
12. High-temperature coke according to item 10, characterized in that it is obtained using unenriched non-caking coal with a reduced content of sulfur and phosphorus.
13. High-temperature coke according to item 11, characterized in that it is characterized by: structural strength of 80-83%, reactivity at 1000°C of at least 4.6-5.7 ml / (g-s), high-temperature specific electrical resistance at 1000°C of 3.5-3.8 Ohm-cm; with the following content of components (in mass%): ash - 5.0-8.0 volatile substances - 1.5-3.05 sulfur - no more than 0.3 phosphorus - no more than 0.035 the rest is carbon.
14. Use of high-temperature coke according to I. 10 as a carbonaceous reducing agent in electrothermal processes.
15. Use of high-temperature coke according to I. 14 as a carbonaceous reducing agent in electrometallurgical processes for smelting ferroalloys.
16. The use of high-temperature coke according to paragraph 15 as a carbonaceous reducing agent in electrometallurgical processes for smelting ferrosilicon.
17. Use of high-temperature coke according to I. 14 as a carbonaceous reducing agent in electrothermal processes of silicon smelting.
18. Use of high-temperature coke according to I. 14 as a carbonaceous reducing agent in electrothermal processes of phosphorus smelting.
Citation Information
Patent Citations
Carbon reducing agent and method for obtaining the same
EA024335B1
Production of coke
JP1994184542A
Method for coal processing and device for its implementation
RU2673052C1
KZ26466B
Cited By
Industrial silicon smelting raw material proportioning method based on carbon content in reducing agent high-temperature coke