Stretched film, metal laminated film using same, and film capacitor

A stretched film with a specific polypropylene and alicyclic structure composition maintains rigidity and electrical insulation at high temperatures, addressing the degradation issues in conventional films and improving passability through post-processing, making it suitable for high-temperature applications like automotive film capacitors.

WO2024228352A1PCT designated stage expired Publication Date: 2024-11-07OJI HLDG CORP

Patent Information

Application Number
PCT/JP2024/016112
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-10-25
Filing Date
2024-04-24
Publication Date
2024-11-07

AI Technical Summary

Technical Problem

Conventional stretched films made from polypropylene resin face challenges in maintaining rigidity and electrical insulation at high temperatures, especially above 110°C, due to degradation of physical properties, and are prone to breaking during post-processing steps such as metal vapor deposition, which affects their productivity and reliability in high-temperature applications like automotive film capacitors.

Method used

A stretched film with a specific composition comprising 55% to 99% polypropylene resin and 1% to 45% polymer with an alicyclic structure in its side chain, stretched in at least one direction, which maintains rigidity and electrical insulation even at high temperatures, and is designed to be more stretchable and passable through post-processing steps.

Benefits of technology

The solution effectively suppresses the deterioration of physical properties like rigidity and electrical insulation at high temperatures, enhances stretchability, and improves passability through post-processing steps, making the film suitable for high-temperature applications such as automotive film capacitors.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JPOXMLDOC01-APPB-T000001
    Figure JPOXMLDOC01-APPB-T000001
  • Figure JPOXMLDOC01-APPB-T000002
    Figure JPOXMLDOC01-APPB-T000002
Patent Text Reader

Abstract

The present invention provides a stretched film in which deterioration of physical properties such as a decrease in rigidity and a decrease in electric insulation properties is suppressed even in a high-temperature environment exceeding 110° C, and which is excellent in stretchability of itself and passability in post-processing steps. Specifically, the present invention provides a stretched film having at least an A layer, the stretched film being characterized in that (1) the A layer contains, per 100 mass%, 55-99 mass% of a polypropylene resin and 1-45 mass% of a polymer having an alicyclic structure in a side chain, and (2) the A layer is stretched in at least one direction.
Need to check novelty before this filing date? Find Prior Art

Description

Stretched film, metal laminated film using same, and film capacitor

[0001] The present invention relates to a stretched film, a metal laminated film using the same, and a film capacitor, and more particularly to a stretched film having excellent heat resistance suitable for use in a capacitor.

[0002] Stretched films made primarily of polypropylene are used in a variety of industrial applications, including packaging, due to their moisture-proof properties, rigidity, heat resistance, etc. In recent years, as their applications have expanded, higher performance has been required, and in particular, suppression of loss of rigidity at high temperatures is desired.

[0003] Furthermore, stretched films primarily composed of polypropylene are used in film capacitor applications due to their excellent electrical properties. Film capacitors made of stretched films primarily composed of polypropylene are used in electronic devices, electrical equipment, and the like, for example, as high-voltage capacitors; various switching power supplies; filter capacitors and smoothing capacitors for converters, inverters, and the like. Film capacitors are used, for example, in inverters and converters that control drive motors in automobiles such as electric vehicles and hybrid vehicles, which have seen increasing demand in recent years.

[0004] Film capacitors, particularly automotive film capacitors, are increasingly being used in high-temperature environments. For example, in devices (such as inverters and converters) that control automobile drive motors, the use of highly heat-resistant semiconductors (such as silicon carbide semiconductors) has increased in recent years. Accordingly, capacitors used in these devices are also required to have high heat resistance, for example, at 120°C or higher, preferably at 130°C or higher. Conventional capacitors using polypropylene film are said to have an upper limit of operating temperature of approximately 110°C, and it is extremely difficult to stably maintain electrical insulation in high-temperature environments exceeding this limit.

[0005] As one of the resin films with high heat resistance, a film made of a resin composition containing a polyolefin mainly composed of polypropylene and a hydrogenated block copolymer has been disclosed as a film having excellent heat resistance and particularly excellent water vapor impermeability (Patent Document 1).

[0006] Furthermore, as one of the resin films having high heat resistance, a film using a polypropylene resin and a resin having an alicyclic structure in the main chain of the polymer obtained by polymerizing a cyclic olefin monomer has been disclosed (Patent Document 2).

[0007] JP 2014-37532 A International Publication No. 2022 / 270577

[0008] Resin films containing polypropylene as a main component tend to show a decrease in physical properties such as a decrease in rigidity and a decrease in electrical insulation when their use temperature increases. Therefore, in general, a resin film containing polypropylene as a main component is stretched in at least one direction, preferably two directions, to form a stretched film, thereby improving the rigidity and electrical insulation and maintaining the rigidity and electrical insulation even at high use temperatures exceeding 110° C. However, when the use temperature reaches 120° C. or higher, or even 130° C. or higher, it is difficult for even a stretched film to maintain its rigidity and electrical insulation.

[0009] The film described in Patent Document 1 contains a hydrogenated block copolymer, which gives it excellent water vapor impermeability. However, because it is an unstretched film, its rigidity and electrical insulation properties are not high. Furthermore, when stretching a mixed resin, pores are often formed within the layer during stretching, resulting in a decrease in rigidity and electrical insulation. Therefore, special consideration is required to find stretching conditions that improve the physical properties while suppressing the formation of pores. However, Patent Document 1 does not disclose any findings regarding stretching conditions.

[0010] Furthermore, Patent Document 2 discloses a stretched film made of a mixed resin that has excellent electrical properties at high temperatures, but the mixed cyclic olefin resin has an alicyclic structure in the polymer main chain, making the resin rigid. As a result, pores are generated within the layer during stretching, making the film prone to breakage during post-processing (e.g., metal deposition in capacitor film applications), resulting in poor productivity.

[0011] In particular, for film capacitor applications, a thin film is required, for example, a thickness of 10 μm or less, preferably 5 μm or less, but within this thickness range, the film becomes more susceptible to fracture, which poses a production problem when the film formation speed and deposition speed are increased in order to reduce costs.

[0012] Therefore, an object of the present invention is to provide a stretched film that is inhibited from decreasing in physical properties such as rigidity and electrical insulation even in a high-temperature environment exceeding 110°C (particularly in a high-temperature environment of 120°C or higher), and that is excellent in its own stretchability and passability through post-processing steps.

[0013] As a result of intensive research into solving the above-mentioned problems, the present inventors have found that the above-mentioned problems can be solved by a stretched film having at least Layer A, which has a specific composition and is stretched in at least one direction. Based on this finding, the present inventors have conducted further research and have completed the present invention.

[0014] That is, the present invention relates to the following stretched film, and a metal laminated film and film capacitor using the same. 1. A stretched film having at least Layer A, characterized in that: (1) Layer A contains, based on 100 mass%, 55 to 99 mass% of a polypropylene-based resin and 1 to 45 mass% of a polymer having an alicyclic structure in its side chain; and (2) Layer A is stretched in at least one direction. 2. The stretched film according to item 1 above, in which Layer A contains, based on 100 mass%, 55 to 97 mass% of a polypropylene-based resin and 3 to 45 mass% of a polymer having an alicyclic structure in its side chain. 3. The stretched film according to item 1 or 2 above, in which the polymer has a glass transition temperature of 100°C to 180°C. 4. The stretched film according to any one of items 1 to 3 above, in which the alicyclic structure has a cyclohexane structure. 5. 5. The stretched film according to any one of items 1 to 4, wherein the stretched film has a thickness of 10 μm or less and a total light transmittance of 80% or more. 6. A metal laminated film comprising the stretched film according to any one of items 1 to 5 and a metal layer laminated on one or both sides of the film. 7. A film capacitor comprising the stretched film according to any one of items 1 to 5. 8. A film capacitor comprising the metal laminated film according to item 6.

[0015] According to the present invention, it is possible to provide a stretched film that is inhibited from suffering deterioration in physical properties such as deterioration in rigidity and electrical insulation even in a high-temperature environment exceeding 110°C, and that is excellent in its own stretchability and passability through post-processing steps.

[0016] In this specification, the expressions "contain" and "comprise" include the concepts of "contain," "comprise," "substantially consist of," and "consist only of." In this specification, when an upper limit and a lower limit are described for a preferred range, the combination thereof can be arbitrary. Furthermore, in this specification, a numerical range indicated as "A to B" includes the numerical values ​​at both ends, unless otherwise specified, and means "at least A and at most B."

[0017] 1. Stretched Film In one aspect, the present invention relates to a stretched film having at least Layer A, characterized in that: (1) Layer A contains, based on 100% by mass, 55% to 99% by mass of a polypropylene resin and 1% to 45% by mass of a polymer having an alicyclic structure in its side chain; and (2) Layer A is stretched in at least one direction (hereinafter also referred to as "the stretched film of the present invention"). This will be described below.

[0018] 1-1. Polypropylene Resin Layer A of the stretched film of the present invention contains 55% by mass or more and 99% by mass or less of a polypropylene resin, with the mass of Layer A being 100% by mass.

[0019] Examples of the polypropylene-based resin include propylene homopolymers such as isotactic polypropylene and syndiotactic polypropylene; copolymers of propylene and other olefins (e.g., ethylene, 1-butene, etc.) (the copolymer may be a random copolymer or a block copolymer having at least two polymer blocks); long-chain branched polypropylene; and polypropylene-based resins produced from plant-derived raw materials.

[0020] When the polypropylene resin is a copolymer of propylene and another olefin, the propylene content in the copolymer is 50% by mass or more, preferably 80% by mass or more, and more preferably 90% by mass or more, based on 100% by mass of the polypropylene resin. Note that the polypropylene resin does not include a polypropylene resin having an alicyclic structure in the side chain.

[0021] The polypropylene resin contained in the layer A may be one type or two or more types.

[0022] The content of the polypropylene resin in Layer A may be from 55% to 99% by mass, preferably from 55% to 97% by mass, more preferably from 60% to 90% by mass, and even more preferably from 65% to 85% by mass. In this case, the rigidity, electrical insulation, and stretchability of the stretched film of the present invention are improved. Note that, when the stretched film of the present invention is a multilayer film having other layers in addition to Layer A (for example, a skin layer described below), the effect of improving stretchability also includes a case where the entire multilayer film is stretched (the same applies hereinafter).

[0023] The melt mass flow rate (MFR) of the polypropylene resin contained in Layer A, measured at 230°C under a load of 2.16 kg, is preferably 0.5 g / 10 min to 6 g / 10 min, more preferably 1 g / 10 min to 5 g / 10 min, and even more preferably 1.5 g / 10 min to 4 g / 10 min, in this case, appropriate resin fluidity is obtained during stretching of the film, and stretchability is improved.

[0024] The melting point of the polypropylene resin contained in Layer A is preferably 155°C or higher. In this case, electrical insulation and stretchability at high temperatures are improved. The melting point is more preferably 160°C or higher and 180°C or lower, and even more preferably 163°C or higher and 170°C or lower.

[0025] The polypropylene resin contained in Layer A preferably has a mesopentad fraction of 95 mol% to 99.9 mol%. A mesopentad fraction of 95 mol% or more tends to improve the rigidity and electrical insulation of the stretched film of the present invention, while a mesopentad fraction of 99.9 mol% or less tends to improve the stretchability. The mesopentad fraction of the polypropylene resin is more preferably 96 mol% to 99.5 mol%, even more preferably 97 mol% to 99.2 mol%, and particularly preferably 98 mol% to 99 mol%.

[0026] The heptane insoluble matter (HI) of the polypropylene resin contained in Layer A is preferably 94% by mass or more and 99.9% by mass or less. At 94% by mass or more, the rigidity and electrical insulation of the stretched film are likely to be improved, while at 99.9% by mass or less, the stretchability is likely to be improved. The heptane insoluble matter of the polypropylene resin is more preferably 96% by mass or more and 99.5% by mass or less, even more preferably 97% by mass or more and 99.2% by mass or less, and particularly preferably 98% by mass or more and 99% by mass or less.

[0027] The number average molecular weight (Mn) of the polypropylene resin contained in Layer A is preferably from 30,000 to 70,000, and more preferably from 35,000 to 65,000. When Layer A contains a polypropylene resin with such a number average molecular weight (Mn), the rigidity, electrical insulation properties, and stretchability of the stretched film of the present invention are likely to be improved.

[0028] The weight-average molecular weight (Mw) of the polypropylene resin contained in Layer A is preferably from 250,000 to 500,000, and more preferably from 300,000 to 450,000. When Layer A contains a polypropylene resin with such a weight-average molecular weight (Mw), the rigidity, electrical insulation properties, and stretchability of the stretched film of the present invention are likely to be improved.

[0029] The polypropylene resin contained in Layer A preferably has a molecular weight distribution (Mw / Mn), calculated as the ratio of weight average molecular weight (Mw) to number average molecular weight (Mn), of 3 to 12, more preferably 5 to 10, and even more preferably 6 to 9.5. When Layer A contains a polypropylene resin with such a molecular weight distribution (Mw / Mn), the rigidity, electrical insulation, and stretchability of the stretched film of the present invention are likely to be improved.

[0030] The z-average molecular weight (Mz) of the polypropylene resin contained in Layer A is preferably from 700,000 to 3,000,000, and more preferably from 1,000,000 to 2,500,000. When Layer A contains a polypropylene resin with such a z-average molecular weight (Mz), the rigidity, electrical insulation properties, and stretchability of the stretched film of the present invention are likely to be improved.

[0031] The molecular weight distribution (Mz / Mw) of the polypropylene resin contained in Layer A, calculated as the ratio of the z-average molecular weight (Mz) to the weight-average molecular weight (Mw), is preferably from 2 to 7, more preferably from 2.5 to 6, and even more preferably from 3 to 5. When Layer A contains a polypropylene resin having such a molecular weight distribution (Mz / Mw), the rigidity, electrical insulation properties, and stretchability of the stretched film of the present invention are likely to be improved.

[0032] Polypropylene-based resins can be produced using conventionally known methods. Examples of polymerization methods include gas-phase polymerization, bulk polymerization, and slurry polymerization. The polymerization may be single-stage polymerization using one polymerization reactor, or multi-stage polymerization using two or more polymerization reactors. Furthermore, polymerization may be carried out by adding hydrogen or a comonomer to the reactor as a molecular weight modifier. Conventionally known Ziegler-Natta catalysts or metallocene catalysts can be used as the polymerization catalyst, and the polymerization catalyst may contain a cocatalyst component or a donor. The mesopentad fraction, melt mass flow rate, molecular weight, molecular weight distribution, and the like of the polypropylene-based resin can be controlled by appropriately adjusting the polymerization catalyst and other polymerization conditions.

[0033] 1-2. Polymer Having an Alicyclic Structure in a Side Chain Layer A of the stretched film of the present invention contains a polymer having an alicyclic structure in a side chain in an amount of 1% by mass to 45% by mass, based on 100% mass of Layer A. The polymer having an alicyclic structure in a side chain contained in Layer A may be one type, or two or more types.

[0034] The content of the polymer having an alicyclic structure in its side chain in Layer A may be from 1% by mass to 45% by mass, preferably from 3% by mass to 45% by mass, more preferably from 10% by mass to 40% by mass, and even more preferably from 15% by mass to 35% by mass, which improves the rigidity, electrical insulation, and stretchability of the stretched film of the present invention.

[0035] Here, the alicyclic structure includes one or more saturated and / or unsaturated carbon ring structures that do not have aromaticity. The carbon ring structures may have two or more carbon ring structures. The carbon ring structures may have a branched aliphatic hydrocarbon structure. The carbon ring structures are bonded to the hydrocarbon chain of the polymer main chain directly or via a hydrocarbon chain.

[0036] Examples of the carbocyclic structure include monocyclic structures such as cycloalkane structures such as cyclopropane, cyclobutane, cyclopentane, cyclohexane, cycloheptane, cyclooctane, cyclononane, cyclodecane, cycloundecane, and cyclododecane, and cycloalkene structures such as cyclopropene, cyclobutene, cyclopropene, cyclohexene, cycloheptene, and cyclooctene. Examples of bicyclic structures include bicyclic alkane structures such as bicycloundecane, and bicyclic alkene structures such as norbornene and norbornadiene, which can be suitably used. Of these, a carbocyclic structure having 4 to 8 carbon atoms is preferred from the viewpoint of stretchability, a monocyclic carbocyclic structure having 4 to 8 carbon atoms is more preferred, a carbocyclic structure that is a monocyclic cycloalkane structure having 4 to 8 carbon atoms is even more preferred, and a cyclohexane structure is particularly preferred.

[0037] The polymer main chain is mainly composed of aliphatic hydrocarbons. The polymer main chain may contain cyclic hydrocarbon structures and / or aromatic hydrocarbon structures as structural units, but preferably does not contain these. The aliphatic hydrocarbons of the polymer main chain may have branches of aliphatic hydrocarbon structures and / or aromatic hydrocarbon structures.

[0038] The polymer having an alicyclic structure in the side chain may be a homopolymer having a structure having an alicyclic structure in the side chain as a structural unit. For example, it may be polyvinylcycloolefin obtained by homopolymerizing vinylcycloolefin. Examples of polyvinylcycloolefin include polyvinylcyclopropane, polyvinylcyclobutane, polyvinylcyclopentane, polyvinylcyclohexane, polyvinylcycloheptane, polyvinylcyclooctane, polyvinylcyclononane, polyvinylcyclodecane, polyvinylcycloundecane, and polyvinylcyclododecane. Homopolymers are preferred because they tend to have high rigidity and electrical insulation properties in high-temperature environments. Among these, polyvinylcyclopentane, polyvinylcyclohexane, and polyvinylcycloheptane are preferred, with polyvinylcyclohexane being most preferred.

[0039] (Method for Producing Polymer Having an Alicyclic Structure in a Side Chain) The method for producing a polymer having an alicyclic structure in a side chain is not particularly limited, and the polymer can be produced using a known method such as a radical polymerization method, an ionic polymerization method (anionic polymerization method, coordination anionic polymerization method, etc.), for example, bulk polymerization, solution polymerization, suspension polymerization, etc.

[0040] Specifically, the polymer having an alicyclic structure in the side chain according to the present invention can be produced by carrying out a polymerization reaction using a known initiator such as an alkyllithium compound or a dilithium compound, followed by sequential polymerization of a monomer having an alicyclic structure (e.g., vinylcycloolefin); or a method in which a monomer having an alicyclic structure is sequentially polymerized and then a coupling agent is added to carry out coupling.

[0041] A polymer having an alicyclic structure in a side chain can be produced by polymerizing a monomer having an aromatic ring structure (e.g., styrene) by a known method, followed by a hydrogenation reaction. The hydrogenation reaction can be carried out, for example, by the method described later in the "Method for producing a hydrogenated block copolymer."

[0042] When produced by a hydrogenation reaction, the hydrogenation rate of the aromatic ring structure is preferably 50 mol% or more, more preferably 80 mol% or more, even more preferably 85 mol% or more, particularly preferably 90 mol% or more, and even more particularly preferably 95 mol% or more. The hydrogenation rate may be 100 mol%. By setting the hydrogenation rate within the above range, stretchability tends to be improved, which is preferable.

[0043] The polymer having an alicyclic structure in the side chain may be a copolymer having a structural unit having an alicyclic structure in the side chain and one or more other structural units. The copolymer may be a random copolymer or a block copolymer having at least two polymer blocks. From the viewpoint of stretchability, copolymers are preferred, and block copolymers are more preferred.

[0044] Examples of other structural units include ethylene, propylene, butene, pentene, hexene, heptene, and octene, and they may or may not have a side chain. Furthermore, the polymer may contain both structural units with a side chain and structural units without a side chain. Examples of structural units with a side chain include propylene, 1-butene, 1-pentene, 1-hexene, and 4-methyl-1-pentene. The other structural units may be unsaturated hydrocarbons, but saturated hydrocarbons are preferred from the viewpoint of electrical insulation.

[0045] Here, when the polymer having an alicyclic structure in a side chain (hereinafter also referred to as "the polymer") contains propylene as another structural unit, the content of propylene in the polymer is less than 50% by mass, preferably 20% by mass or less, and more preferably 10% by mass or less, based on 100% by mass of the polymer.

[0046] A polymer having an alicyclic structure in a side chain can be obtained, for example, by polymerizing a monomer having each structural unit by a known method. Alternatively, the polymer can be obtained by hydrogenating a polymer having an aromatic ring structure in a side chain. Hydrogenating a polymer having an aromatic ring structure in a side chain is preferred because it is easy to industrially obtain a polymer having an alicyclic structure in a side chain at low cost.

[0047] When a polymer having an aromatic ring structure in a side chain is hydrogenated, the polymer having an aromatic ring structure in a side chain may be a homopolymer or a copolymer. In the case of a copolymer, a block copolymer having at least a vinyl aromatic polymer block and a conjugated diene polymer block is preferred. By hydrogenating this, a hydrogenated block copolymer having at least a hydrogenated vinyl aromatic polymer block and a hydrogenated conjugated diene polymer block is obtained.

[0048] Hereinafter, a hydrogenated block copolymer having at least a hydrogenated vinyl aromatic polymer block and a hydrogenated conjugated diene polymer block will be described as one preferred embodiment.

[0049] (Hydrogenated vinyl aromatic polymer block) The hydrogenated vinyl aromatic polymer block contains structural units derived from a vinyl aromatic compound and hydrogenated therefrom. The hydrogenated vinyl aromatic polymer block contains structural units derived from a vinyl aromatic compound in an amount of 50% by mass or more, preferably 80% by mass or more, more preferably 90% by mass or more, and particularly preferably 100% by mass. By making the structural units derived from a vinyl aromatic compound 50% by mass or more, rigidity and electrical insulation properties in high-temperature environments are likely to be improved.

[0050] Examples of the vinyl aromatic compound include styrene, α-methylstyrene, 2-methylstyrene, 3-methylstyrene, 4-methylstyrene, 4-propylstyrene, 4-cyclohexylstyrene, 4-dodecylstyrene, 2-ethyl-4-benzylstyrene, 4-(phenylbutyl)styrene, vinyltoluene, 1-vinylnaphthalene, 2-vinylnaphthalene, etc. The vinyl aromatic compound is preferably selected from styrene and α-methylstyrene, and more preferably styrene.

[0051] The hydrogenated vinyl aromatic polymer block may be composed of only one type of the above vinyl aromatic compound, or may be composed of two or more types.

[0052] The hydrogenated vinyl aromatic polymer block may contain other structural units besides those derived from vinyl aromatic compounds, such as those derived from isoprene, butadiene, 2,3-dimethylbutadiene, 1,3-pentadiene, 1,3-hexadiene, etc.

[0053] The content of the hydrogenated vinyl aromatic polymer block is preferably 50% by mass or more but less than 100% by mass, based on 100% by mass of the total of the hydrogenated vinyl aromatic polymer block and the hydrogenated conjugated diene polymer block. By making it 50% by mass or more, rigidity and electrical insulation at high temperatures tend to be improved. It is more preferably 60% by mass or more, even more preferably 70% by mass or more, and particularly preferably 80% by mass or more.

[0054] (Hydrogenated Conjugated Diene Polymer Block) The hydrogenated conjugated diene polymer block contains structural units derived from a conjugated diene and hydrogenated from the conjugated diene. The hydrogenated conjugated diene polymer block contains 50% by mass or more, preferably 80% by mass or more, more preferably 90% by mass or more, and particularly preferably 100% by mass of structural units derived from the conjugated diene.

[0055] Examples of conjugated dienes include butadiene, 2-methyl-1,3-butadiene (isoprene), 2,3-dimethyl-butadiene, 1,3-pentadiene, 1,3-hexadiene, etc. The conjugated diene is preferably selected from butadiene and isoprene, and more preferably butadiene.

[0056] The hydrogenated conjugated diene polymer block may contain a structural unit derived from a conjugated diene having no side chain. Examples of the conjugated diene having no side chain include butadiene, 1,3-pentadiene, and 1,3-hexadiene. The conjugated diene having no side chain is preferably butadiene.

[0057] In the hydrogenated conjugated diene polymer block, the bonding form of the conjugated diene, i.e., the microstructure, is not particularly limited. For example, in the case of butadiene, bonding forms of 1,2-bonds and 1,4-bonds can be used. In addition, in the case of isoprene, bonding forms of 1,2-bonds, 3,4-bonds and 1,4-bonds can be used. Only one type of these bonding forms may be present, or two or more types may be present. When two or more types of bonding forms are present, the ratio of the bonding forms is not particularly limited.

[0058] The hydrogenated conjugated diene polymer block may contain other structural units besides those derived from conjugated dienes, such as structural units derived from styrene, α-methylstyrene, 2-methylstyrene, 3-methylstyrene, 4-methylstyrene, 4-propylstyrene, 4-cyclohexylstyrene, 4-dodecylstyrene, 2-ethyl-4-benzylstyrene, 4-(phenylbutyl)styrene, vinyltoluene, 1-vinylnaphthalene, and 2-vinylnaphthalene.

[0059] The content of the hydrogenated conjugated diene polymer block is preferably more than 0% by mass (e.g., 1% by mass or more) and 50% by mass or less, based on 100% by mass of the total of the hydrogenated vinyl aromatic polymer block and the hydrogenated conjugated diene polymer block. By setting it to 50% by mass or less, rigidity and electrical insulation at high temperatures tend to be improved, which is preferable. It is more preferably 40% by mass or less, even more preferably 30% by mass or less, and particularly preferably 20% by mass or less.

[0060] (Hydrogenation Rate) In the hydrogenated vinyl aromatic polymer block according to this embodiment, the hydrogenation rate of the aromatic rings in the hydrogenated vinyl aromatic polymer block is preferably 50 mol% or more, more preferably 80 mol% or more, even more preferably 85 mol% or more, particularly preferably 90 mol% or more, and even more particularly preferably 95 mol% or more. The hydrogenation rate may be 100 mol%. The hydrogenation rate of the carbon-carbon double bonds derived from the conjugated diene in the hydrogenated conjugated diene polymer block is preferably 90 mol% or more, more preferably 95 mol% or more. The hydrogenation rate may be 100 mol%.

[0061] By setting the hydrogenation rate of the aromatic ring of the hydrogenated vinyl aromatic polymer block and / or the hydrogenation rate of the carbon-carbon double bond derived from the conjugated diene of the hydrogenated conjugated diene polymer block within the above-mentioned range, stretchability tends to be improved, which is preferable.

[0062] (Bonding Pattern of Hydrogenated Block Copolymer) The bonding pattern of the polymer blocks in the hydrogenated block copolymer may be any of linear, branched, and radial, or a combination thereof.

[0063] For example, if the hydrogenated vinyl aromatic polymer block is represented by "X" and the hydrogenated conjugated diene polymer block is represented by "Y", examples of the bonding pattern include a diblock copolymer (X-Y), a triblock copolymer (X-Y-X), a tetrablock copolymer (X-Y-X-Y), a pentablock copolymer (X-Y-X-Y-X, or Y-X-Y-X-Y), etc. From the viewpoint of ease of production, the bonding pattern is preferably a diblock copolymer, a triblock copolymer, or a tetrablock copolymer.

[0064] Specific examples of hydrogenated block copolymers include hydrogenated block copolymers of styrene-isoprene diblock copolymer (SI), styrene-butadiene diblock copolymer (SB), styrene-isoprene-styrene triblock copolymer (SIS), styrene-butadiene / isoprene-styrene triblock copolymer (SB / IS), styrene-butadiene-styrene triblock copolymer (SBS), styrene-ethylene-butylene-styrene copolymer (SEBS), styrene-ethylene-propylene-styrene copolymer (SEPS), styrene-ethylene-ethylene-propylene-styrene copolymer (SEEPS), styrene-butylene-butadiene-styrene copolymer (SBBS), etc. Among these, hydrogenated block copolymers of styrene-butadiene diblock copolymer (SB) are particularly preferred.

[0065] (Method for Producing Hydrogenated Block Copolymer) The method for producing the hydrogenated block copolymer is not particularly limited, and known methods such as anionic polymerization can be used.

[0066] Specifically, the hydrogenated block copolymer according to the present invention can be produced by carrying out a polymerization reaction using, for example, a method of sequentially polymerizing a vinyl aromatic compound and a conjugated diene using an alkyllithium compound as an initiator; a method of sequentially polymerizing a vinyl aromatic compound and a conjugated diene using an alkyllithium compound as an initiator, followed by coupling by adding a coupling agent; or a method of sequentially polymerizing a conjugated diene and then a vinyl aromatic compound using a dilithium compound as an initiator, followed by carrying out a hydrogenation reaction.

[0067] Examples of the alkyllithium compound include methyllithium, ethyllithium, n-butyllithium, sec-butyllithium, tert-butyllithium, and pentyllithium.

[0068] Examples of coupling agents include divinylbenzene; polyfunctional epoxy compounds such as epoxidized 1,2-polybutadiene, epoxidized soybean oil, and 1,3-bis(N,N-glycidylaminomethyl)cyclohexane; halogen compounds such as dimethyldichlorosilane, dimethyldibromosilane, trichlorosilane, methyltrichlorosilane, tetrachlorosilane, and tetrachlorotin; ester compounds such as methyl benzoate, ethyl benzoate, phenyl benzoate, diethyl oxalate, diethyl malonate, diethyl adipate, dioctyl adipate, dimethyl phthalate, diethyl phthalate, dimethyl isophthalate, and dimethyl terephthalate; carbonate ester compounds such as dimethyl carbonate, diethyl carbonate, and diphenyl carbonate; and alkoxysilane compounds such as dimethyldimethoxysilane, methyltrimethoxysilane, methyltriethoxysilane, tetramethoxysilane, tetraethoxysilane, bis(trimethoxysilyl)hexane, and bis(triethoxysilyl)ethane.

[0069] Examples of dilithium compounds include naphthalenedilithium and dilithiohexylbenzene.

[0070] The polymerization reaction is preferably carried out in the presence of a solvent. The solvent is not particularly limited as long as it is inert to the initiator and does not adversely affect the reaction, and examples thereof include saturated aliphatic hydrocarbons such as hexane, cyclohexane, heptane, octane, and decane; and aromatic hydrocarbons such as toluene, benzene, and xylene. In addition, the temperature of the polymerization reaction is preferably 0 to 100°C, more preferably 30 to 90°C, even more preferably 40 to 80°C, and particularly preferably 50 to 80°C, from the viewpoint of microstructure control. The time of the polymerization reaction is preferably 0.5 to 50 hours, from the viewpoint of microstructure control.

[0071] Furthermore, a Lewis base may be used as a co-catalyst during the polymerization reaction. Examples of Lewis bases include ethers such as dimethyl ether, diethyl ether, and tetrahydrofuran; glycol ethers such as ethylene glycol dimethyl ether and diethylene glycol dimethyl ether; and amines such as triethylamine, N,N,N',N'-tetramethylethylenediamine, and N-methylmorpholine. These Lewis bases may be used alone or in combination of two or more.

[0072] The hydrogenation reaction may be carried out immediately after the polymerization reaction, or may be carried out after the block copolymer has been isolated after the polymerization reaction.

[0073] When the block copolymer is temporarily isolated after the polymerization reaction, the block copolymer can be isolated by pouring the polymerization reaction solution obtained after the polymerization reaction into a poor solvent for the block copolymer, such as methanol, to solidify the block copolymer, or by pouring the polymerization reaction solution together with steam into hot water to remove the solvent by azeotropy (steam stripping), followed by drying.

[0074] The hydrogenation reaction of the block copolymer can be carried out, for example, in the presence of a hydrogenation catalyst at a reaction temperature of 20 to 200° C. and a hydrogen pressure of 0.1 to 20 MPa for 0.1 to 100 hours.

[0075] Examples of the hydrogenation catalyst include Raney nickel; heterogeneous catalysts in which a metal such as platinum (Pt), palladium (Pd), ruthenium (Ru), rhodium (Rh), or nickel (Ni) is supported on a carrier such as carbon, alumina, or diatomaceous earth; Ziegler catalysts consisting of a combination of a transition metal compound (nickel octoate, nickel naphthenate, nickel acetylacetonate, cobalt octoate, cobalt naphthenate, or cobalt acetylacetonate) with an organoaluminum compound such as triethylaluminum or triisobutylaluminum, or an organolithium compound; and metallocene catalysts consisting of a combination of a bis(cyclopentadienyl) compound of a transition metal such as titanium, zirconium, or hafnium with an organometallic compound such as lithium, sodium, potassium, aluminum, zinc, or magnesium.

[0076] When the hydrogenation reaction is carried out subsequent to the polymerization reaction, the hydrogenated block copolymer can be isolated by pouring the hydrogenation reaction solution into a poor solvent for the hydrogenated block copolymer, such as methanol, to coagulate it, or by pouring the hydrogenation reaction solution together with steam into hot water to remove the solvent by azeotropy (steam stripping), followed by drying.

[0077] The glass transition temperature (Tg) of the polymer having an alicyclic structure in a side chain contained in Layer A of the present invention is preferably 100° C. or higher and 180° C. or lower. By setting the glass transition temperature to 100° C. or higher, rigidity and electrical insulation at high temperatures tend to be increased, and by setting it to 180° C. or lower, stretchability can be improved. The glass transition temperature is more preferably 120° C. or higher and 165° C. or lower, more preferably 130° C. or higher and 160° C. or lower, and particularly preferably 140° C. or higher and 155° C. or lower.

[0078] The Vicat softening point (1 kg, 50°C / hr) of the polymer having an alicyclic structure in a side chain contained in Layer A is preferably 100°C or higher and 170°C or lower. By setting the Vicat softening point to 100°C or higher, rigidity and electrical insulation at high temperatures tend to be increased, and by setting it to 170°C or lower, stretchability can be improved. The Vicat softening point is more preferably 120°C or higher and 165°C or lower, more preferably 130°C or higher and 160°C or lower, and particularly preferably 140°C or higher and 155°C or lower.

[0079] The glass transition temperature (Tg) and Vicat softening point of the polymer having an alicyclic structure in a side chain contained in Layer A can be adjusted by the type of structural unit having the above-mentioned structure having an alicyclic structure in a side chain, or the types and proportions of one or more other structural units.

[0080] The weight-average molecular weight (Mw) of the polymer having an alicyclic structure in a side chain contained in Layer A is not particularly limited, but is preferably from 50,000 to 400,000. When Layer A contains a polymer having an alicyclic structure with such a weight-average molecular weight (Mw), the rigidity, electrical insulation properties, and stretchability of the stretched film of the present invention are likely to be improved.

[0081] The melt mass flow rate (MFR) of the polymer having an alicyclic structure in a side chain contained in Layer A, measured at 260°C under a load of 2.16 kg, is preferably 1 g / 10 min to 40 g / 10 min, more preferably 2 g / 10 min to 20 g / 10 min, and even more preferably 3 g / 10 min to 15 g / 10 min, in which case adequate resin fluidity is obtained during stretching of the film, and stretchability is likely to be improved.

[0082] The polymer having an alicyclic structure in the side chain contained in Layer A may be produced by the method described above, or a commercially available product such as ViviOn (registered trademark) (manufactured by USI Corporation) may be used.

[0083] 1-3. Layer A The present invention has Layer A containing 55% by mass to 99% by mass of a polypropylene resin and 1% by mass to 45% by mass of a polymer having an alicyclic structure in a side chain, where the mass of Layer A is 100% by mass. Layer A is stretched in at least one direction.

[0084] Layer A may further contain other resins for the purposes of adjusting the low-temperature impact resistance of the film, adjusting the surface roughness, and adjusting various physical properties such as rigidity, strength, and elongation, as well as adjusting the mixability and stretchability of the polypropylene-based resin and the polymer having an alicyclic structure in the side chain.

[0085] The amount of the other resin added is preferably 20% by mass or less, more preferably 10% by mass or less, and even more preferably 5% by mass or less, based on 100% by mass of Layer A. The other resin is not particularly limited, and conventionally known resins suitable for stretched film applications can be used appropriately in the present invention. Examples include polyolefin resins such as polyethylene, poly(1-butene), polyisobutene, poly(1-pentene), and poly(4-methyl-1-pentene), and copolymer resins thereof, as well as copolymers of α-olefins such as ethylene-propylene copolymer, propylene-butene copolymer, ethylene-butene copolymer, and ethylene-(4-methyl-1-pentene) copolymer. Other examples include polystyrene resins, elastomers, polyvinyl resins, polyester resins, polyurethane resins, nylon resins, and copolymers thereof.

[0086] Here, when the other resin is a copolymer containing propylene, the propylene content is less than 50% by mass (for example, 40% by mass or less), preferably 20% by mass or less, and more preferably 10% by mass or less, based on 100% by mass of the other resin.

[0087] As the other resin, commercially available products may be used, for example, Tafmer (registered trademark) (manufactured by Mitsui Chemicals, Inc.) as a copolymer of α-olefins, which can be suitably used for the above-mentioned purpose.

[0088] Layer A can further contain particles such as inorganic particles and organic particles, either alone or in combination. By containing particles, the friction coefficient and surface roughness of the stretched film can be adjusted, allowing for a wrinkle-free wound film with a good appearance. Furthermore, when the stretched film is used for a capacitor, its electrical properties (self-healing properties) can be improved.

[0089] The inorganic particles are not particularly limited, and examples thereof include particles of metal oxides such as titanium oxide, zinc oxide, aluminum oxide, and magnesium oxide; and silicon compounds such as silica, which can be preferably used. In addition to these, examples of inorganic particles include particles of light calcium carbonate, heavy calcium carbonate, kaolin, calcined kaolin, talc, calcium sulfate, barium sulfate, zinc sulfide, zinc carbonate, satin white, aluminum silicate, diatomaceous earth, calcium silicate, magnesium silicate, alumina, colloidal alumina, boehmite, pseudoboehmite, aluminum hydroxide, magnesium carbonate, magnesium hydroxide, zeolite, and smectite. Examples of organic particles include resin particles made of crosslinkable resins and silicone resin particles.

[0090] The average particle size of the particles is, for example, 0.05 μm or more and 2.0 μm or less. The average particle size is preferably 0.1 μm or more and 1.5 μm or less, and more preferably 0.4 μm or more and 1.2 μm or less. The average particle size of the inorganic particles and organic particles is measured by the method described in the Examples below.

[0091] As the particles, commercially available products may be used, such as Seahoster (registered trademark) (manufactured by Nippon Shokubai Co., Ltd.), which can be suitably used for the above-mentioned purposes.

[0092] The particle content is, for example, 0.1% by mass or more and 2.0% by mass or less, preferably 0.2% by mass or more and 1.5% by mass or less, and more preferably 0.3% by mass or more and 1.2% by mass or less, with the mass of Layer A being 100% by mass.

[0093] Layer A can further contain an antioxidant. Antioxidants are mainly used for the following two purposes. One purpose is to suppress thermal and oxidative degradation of the resin in the film-forming extruder and / or melt kneader, and the other purpose is to suppress the deterioration of physical properties such as strength due to deterioration over long-term use of the stretched film. An example of the latter purpose is to contribute to suppressing deterioration over long-term use and maintaining the electrical properties of the capacitor when used in a capacitor. An antioxidant that mainly contributes to the former purpose is also called a "primary agent," and an antioxidant that mainly contributes to the latter purpose is also called a "secondary agent." Two or more types of antioxidants may be used for these two purposes, or one type of antioxidant may be used for both purposes.

[0094] An example of a primary agent is 2,6-di-tertiary-butyl-para-cresol (common name: BHT). This antioxidant is mostly oxidized, decomposed, or evaporated in the extruder, and almost none remains after the stretched film is formed. Therefore, when Layer A contains BHT after stretching, the content is usually less than 100 ppm by mass, with the mass of Layer A being 100%.

[0095] Examples of the secondary agent include hindered phenol-based antioxidants having a carbonyl group. Among the hindered phenol-based antioxidants, examples of the hindered phenol-based antioxidants having a carbonyl group include triethylene glycol-bis[3-(3-tert-butyl-5-methyl-4-hydroxyphenyl)propionate] (trade name: Irganox 245), 1,6-hexanediol-bis[3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate] (trade name: Irganox 259), pentaerythritol tetrakis[3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate] (trade name: Irganox 1010), 2,2-thiazolinone-2-one, ... Examples of suitable compounds include N,N'-hexamethylenebis(3,5-ditertiarybutyl-4-hydroxyphenyl)propionate (trade name: Irganox 1035), octadecyl-3-(3,5-ditertiarybutyl-4-hydroxyphenyl)propionate (trade name: Irganox 1076), and N,N'-hexamethylenebis(3,5-ditertiarybutyl-4-hydroxyhydrocinnamamide) (trade name: Irganox 1098), but pentaerythritol tetrakis[3-(3,5-ditertiarybutyl-4-hydroxyphenyl)propionate], which has excellent heat resistance, is particularly preferred. (Here, all Irganox (registered trademark) products are manufactured by BASF Japan Ltd.)

[0096] When Layer A contains one or more hindered phenol-based antioxidants, the total content thereof is preferably from 1,000 ppm by mass to 7,000 ppm by mass, and more preferably from 2,000 ppm by mass to 6,000 ppm by mass, based on 100% by mass of Layer A, from the viewpoint of achieving an appropriate effect. Note that the hindered phenol-based antioxidant is partially oxidized and decomposed during the extrusion process or the like during the production of a stretched film, and the remaining amount when the film is formed is generally 60 to 80% by mass of the aforementioned content.

[0097] Layer A may further contain additives. Examples of additives include nucleating agents, chlorine absorbers, lubricants, plasticizers, flame retardants, colorants, etc. The content of the additives in layer A is, for example, 0% by mass or more and 10% by mass or less, 0% by mass or more and 5% by mass or less, 0% by mass or more and 1% by mass or less, 0% by mass or more and 0.5% by mass or less, or 0% by mass or more and 0.1% by mass or less. The substantial lower limit is about 0.01% by mass.

[0098] The thickness of Layer A of the present invention is not particularly limited. The preferred thickness depends on the application; for example, for packaging applications, separator applications, etc., a thickness of 5 μm to 80 μm, or 10 μm to 50 μm, is preferably used. For capacitor applications, a thinner thickness is preferred from the viewpoint of reducing the volume of the capacitor and increasing the capacitance. From this viewpoint, the thickness is preferably 10 μm or less, more preferably 9 μm or less, even more preferably 8 μm or less, even more preferably 6 μm or less, particularly preferably 5 μm or less, especially more preferably 4 μm or less, and particularly preferably 3 μm or less. Furthermore, from the viewpoint of stretchability and the metal vapor deposition process, the thickness after stretching is, for example, 1 μm or more, preferably 1.5 μm or more, more preferably 1.8 μm or more, even more preferably 2 μm or more, and even more preferably 2.2 μm or more.

[0099] The stretched film of the present invention is a stretched film having Layer A containing 55% by mass or more and 99% by mass or less of a polypropylene resin and 1% by mass or more and 45% by mass or less of a polymer having an alicyclic structure in a side chain, where the mass of Layer A is 100% by mass, and the Layer A is stretched in at least one direction.

[0100] The stretched film of the present invention may be a single-layer stretched film consisting of Layer A, or may be a multilayer film obtained by laminating multiple layers and / or films using a conventionally known lamination method, such as coextrusion, lamination, heat sealing, coating, etc., either alone or in combination. The lamination may be carried out before or after stretching Layer A.

[0101] The multilayer film may have, for example, a three-layer structure (layer b / layer a / layer b) consisting of a surface layer (skin layer: layer b) and a core layer (layer a); a three-layer structure (layer b / layer a / layer c) in which one surface layer is further added with another layer (layer c); a four-layer structure (layer b / layer a / layer a / layer c) in which there are two core layers; a four-layer structure (layer b / layer a / layer a' / layer c) in which one core layer is replaced with another core layer (layer a'); a structure (layer b / layer d / layer a / layer d / layer b) in which an intermediate layer is also provided; or a so-called super multilayer film including a two-layer or more structure in which two or more layers of layer a are laminated, or a laminate structure in which ten or more layers of layer a are laminated. Each layer may be composed of a different resin or the same resin.

[0102] The Layer A of the present invention can be used as any of Layer a, Layer a', Layer b, Layer c, Layer d, etc. For example, when used as a surface layer, it tends to have excellent stretchability, and when used as a core layer, it tends to have excellent rigidity and insulating properties at high temperatures.

[0103] In order to facilitate the manifestation of the effects of the present invention, the thickness ratio of layer A to the stretched film of the present invention is preferably 50% or more, more preferably 60% or more, even more preferably 70% or more, and particularly preferably 80% or more, relative to 100% of the thickness of the stretched film.

[0104] When the layer A of the present invention is used as a core layer, a preferred surface layer to be laminated thereon is a layer containing a polypropylene-based resin as a main component and a pigment. The polypropylene-based resin and pigment may be the same as those used for the layer A.

[0105] The preferred layer structure depends on the application, but for example, in applications such as packaging and separators, two or more layers are preferred from the viewpoint of functional separation between the core layer and the skin layer. In applications such as capacitors, a single layer is preferred from the viewpoint of reducing the thickness, and two or more layers are preferred from the viewpoint of electrical insulation.

[0106] Specific examples of coextrusion methods include a pre-die lamination method in which molten resins are brought into contact in a feed block before a mold, an in-die lamination method in which they are brought into contact along a path inside a mold, and an out-of-die lamination method in which they are discharged from multiple concentric lips and brought into contact, etc. For example, in the in-die lamination method, a multi-layer die such as a three-layer multi-manifold die can be used.

[0107] The thickness of the stretched film of the present invention is not particularly limited. The preferred thickness depends on the application. For example, for packaging applications, separator applications, etc., a thickness of 5 μm to 80 μm, or 10 μm to 50 μm, is preferably used. For capacitor applications, a thinner thickness is preferred from the viewpoint of reducing the volume of the capacitor and increasing the capacitance. From this viewpoint, the thickness is preferably 10 μm or less, more preferably 9 μm or less, even more preferably 8 μm or less, even more preferably 6 μm or less, particularly preferably 5 μm or less, especially more preferably 4 μm or less, and particularly preferably 3 μm or less. Furthermore, from the viewpoint of stretchability and the metal vapor deposition process, the thickness after stretching is, for example, 1 μm or more, preferably 1.5 μm or more, more preferably 1.8 μm or more, even more preferably 2 μm or more, and even more preferably 2.2 μm or more.

[0108] The thickness of the film of the present invention, such as the unstretched film of the present invention or the biaxially stretched film of the present invention, is measured using an outside micrometer (high-precision digimatic micrometer MDH-25MB manufactured by Mitutoyo Corporation) in accordance with JIS K 7130:1999 Method A.

[0109] The stretched film of the present invention has high dielectric breakdown strength at high temperatures, which is measured at 120°C and 135°C according to the method described in the Examples below.

[0110] The stretched film of the present invention preferably has a dielectric breakdown strength of 450 V in a 120°C environment. DC / μm or more, more preferably 470V DC / μm or more, more preferably 490V DC / μm or more, particularly preferably 500V DC / μm or more, more particularly preferably 510V DC The upper limit of the dielectric breakdown strength at each of the above temperatures is not particularly limited, and is, for example, 700V DC / μm or less, 650V DC / μm or less.

[0111] The dielectric breakdown strength of the film of the present invention in an environment of 135°C is preferably 420V DC / μm or more, more preferably 440VDC / μm or more, more preferably 460V DC / μm or more, particularly preferably 480V DC / μm or more, more particularly preferably 490V DC The upper limit of the dielectric breakdown strength at each of the above temperatures is not particularly limited, and is, for example, 650 V DC / μm or less, 600V DC / μm or less.

[0112] The stretched film of the present invention is preferred because it exhibits little change in dielectric breakdown strength with increasing temperature. The dielectric strength retention rate (%), which is the ratio of the dielectric breakdown strength in a 135°C environment to the dielectric breakdown strength in a 120°C environment (dielectric breakdown strength in a 135°C environment / dielectric breakdown strength in a 120°C environment), is preferably 87% or more, more preferably 88% or more, even more preferably 89% or more, and particularly preferably 90% or more. The upper limit is not particularly limited, and may be, for example, 100%, 99%, or 98%. Note that the load related to dielectric breakdown strength differs significantly between a 120°C environment and a 135°C environment. Therefore, a typical polypropylene film is not preferred because it reduces the dielectric strength retention rate and reduces the temperature stability of the electrical properties of a capacitor using it. The stretched film of the present invention is preferred because it suppresses change in dielectric breakdown strength from a 120°C environment to a 135°C environment, improving the temperature stability of the electrical properties of a capacitor using it.

[0113] The rigidity of the stretched film of the present invention in a high-temperature environment is expressed as the elongation percentage measured using a thermomechanical analyzer (TMA) according to the method described in the Examples below. It is preferable that the rigidity of the stretched film changes little when heated from room temperature to 130°C, and the elongation percentage is preferably 4.5% or less, more preferably 4% or less, even more preferably 3.5% or less, and particularly preferably 3% or less. By setting the elongation percentage to 5% or less, the rigidity of the stretched film at high temperatures is maintained at a high level. Furthermore, excellent electrical insulation at high temperatures is also achieved, which is preferable because it improves the temperature stability of the electrical properties of capacitors using the film. The lower limit of the elongation percentage is, for example, 0.2% or more, 0.5% or more, or 1% or more. Setting the elongation percentage to 0.2% or more facilitates the improvement of the film's stretchability.

[0114] The stretched film of the present invention has high post-processing passability. When the stretched film of the present invention is used for capacitor applications, the post-processing passability is mainly a vapor deposition step for laminating a metal layer. The vapor deposition passability is measured according to the method described in the Examples below. The stretched film of the present invention can undergo vapor deposition without film breakage, even at a high deposition rate of, for example, 150 m / min.

[0115] The uses of the stretched film of the present invention are not particularly limited. For example, the film of the present invention can be used as a packaging film or separator with excellent heat resistance, taking advantage of its heat resistance. The stretched film of the present invention can also be suitably used as a film for capacitors. In particular, the film is extremely suitable for use in capacitors that are used in high-temperature environments of 120°C or higher, and that are small and have a high capacity (e.g., 5 μF or more, preferably 10 μF or more, and more preferably 20 μF or more).

[0116] 1-5. Method for Producing Stretched Film If the raw materials for the stretched film of the present invention (including at least the polypropylene resin and the polymer having an alicyclic structure in its side chain) contain a large amount of water, they are dried before use. The drying conditions are not particularly limited, but are, for example, 70 to 150°C, preferably 80 to 130°C. The drying time can be adjusted appropriately depending on the drying temperature, and is, for example, 2 to 30 hours, preferably 3 to 20 hours.

[0117] The raw materials may be individually fed into the film-forming extruder and mixed inside the film-forming extruder, or may be mixed before being fed into the film-forming extruder and then fed into the film-forming extruder as a raw material mixture.

[0118] The mixing method for preparing the raw material mixture is not particularly limited, but examples include a method in which a plurality of types of resin blocks (pellets, etc.) are dry-blended using a mixer or the like.

[0119] As a mixing method, melt kneading (melt blending) may be used. Melt kneading is preferred because if the resins can be kneaded uniformly, the rigidity, electrical insulation properties, stretchability, etc. of the stretched film are likely to be improved.

[0120] As a melt kneading method, a single-screw type, twin-screw type, or multi-screw type melt kneader having more than one screw can be used. Among these, twin-screw type melt kneaders are preferred because they are highly effective in improving the rigidity, electrical insulation, stretchability, etc. of the stretched film. In the case of twin-screw types, either co-rotating or counter-rotating kneading types can be used, but co-rotating is preferred from the viewpoint of suppressing resin degradation. The ratio of the screw diameter to length (L / D) of the melt kneader is preferably 20 or more, more preferably 25 or more, and even more preferably 28 or more. By setting L / D to 20 or more, the resin is thoroughly mixed, and the rigidity, electrical insulation, and stretchability of the stretched film are improved. There is no upper limit to L / D, but from the viewpoint of suppressing resin degradation, it is 80 or less, preferably 50 or less.

[0121] The temperature during melt kneading is preferably 200° C. to 300° C., more preferably 220° C. to 280° C., in order to balance the suppression of resin deterioration and kneadability. During melt kneading, it is preferable to purge the kneader with an inert gas such as nitrogen in order to suppress resin deterioration.

[0122] The raw materials and / or raw material mixture of the present invention are supplied to a film-forming extruder and extruded. The extrusion method is not particularly limited, and any known extrusion method can be used. For example, the solid raw materials or resin composition of the present invention supplied to the film-forming extruder are mixed in a heated molten state by a screw, filtered through a filter, extruded into a film form through a die such as a single-layer T-die, and solidified by contact with a cooling roll set at a predetermined surface temperature to form the unstretched film of the present invention.

[0123] Examples of film-forming extruders include single-screw types, twin-screw types, and multi-screw types with three or more screws. In the case of twin or more screws, the screw rotation type may be, for example, co-rotating or counter-rotating. The melt temperature is preferably 200 to 300°C, preferably 230 to 280°C, and more preferably 240 to 275°C. This allows the resin to be appropriately kneaded, which tends to improve the rigidity, electrical insulation, stretchability, etc. of the stretched film. In order to suppress deterioration of the resin during melt extrusion, it is preferable to purge the extruder with an inert gas such as nitrogen.

[0124] The filtration accuracy of the filter used to filter the molten resin of the present invention is not particularly limited, but is, for example, 2 to 30 μm, preferably 5 to 25 μm, and more preferably 10 to 25 μm.

[0125] The temperature of the die is not particularly limited, but is preferably 200 to 300°C, more preferably 210 to 280°C, more preferably 215 to 270°C, and even more preferably 220 to 260°C.

[0126] The method of contacting the molten resin of the present invention extruded from a die with a chill roll to solidify it is not particularly limited, and examples thereof include an air knife, electrostatic pinning, an elastic roll nip, a metal roll nip, an elastic metal roll nip, etc. The surface temperature of the chill roll is, for example, 30 to 130°C, preferably 35 to 120°C, and more preferably 40 to 110°C.

[0127] The draft ratio when the resin of the present invention in a molten state extruded from the die is brought into contact with a cooling roll is preferably 1 to 20, more preferably 1.1 to 16, more preferably 1.2 to 10, and even more preferably 1.3 to 8. By setting the draft ratio within this range, the longitudinal orientation of the stretched film can be set within an appropriate range, and the stretchability can be improved. The draft ratio is determined based on the density d (g / cm) of the molten resin. 3 The draft ratio is calculated by the following formula using the width W (cm) of the die lip outlet, the average slit gap t (cm) of the die lip outlet, the resin discharge rate Q (g / min), and the peripheral speed V (cm / min) of the cooling and molding roll.

[0128] The thickness of the unstretched film of the present invention is not particularly limited, but is, for example, 20 to 300 μm.

[0129] The method for stretching the unstretched film of the present invention is not particularly limited, and any known stretching method can be used. Examples include a method in which the unstretched film of the present invention is heated with a heated roll and stretched in the longitudinal direction (machine direction, MD) (longitudinal uniaxial roll stretching method), a method in which the unstretched film of the present invention is stretched in the transverse direction (width direction, TD) in an oven (generally called a tenter) at a predetermined temperature (transverse uniaxial stretching method), a method in which longitudinal uniaxial roll stretching is followed by transverse uniaxial stretching (sequential biaxial stretching method), a method in which longitudinal uniaxial roll stretching is followed by transverse uniaxial stretching and then longitudinal uniaxial (roll or tenter method) stretching (multistage sequential biaxial stretching method), a method in which the unstretched film of the present invention is longitudinally stretched and transversely stretched sequentially in a tenter at a predetermined temperature (tenter method sequential biaxial stretching method), and a method in which the unstretched film of the present invention is longitudinally stretched and transversely stretched simultaneously in a tenter (simultaneous biaxial stretching method). As a method for stretching the unstretched film of the present invention, a method of longitudinal uniaxial roll stretching followed by transverse uniaxial stretching (sequential biaxial stretching method) is preferred, as it provides a stretched film with excellent rigidity, electrical insulation, stretchability, etc.

[0130] In the longitudinal uniaxial roll stretching method, a plurality of heating rolls may be used. The stretching point may be one or two or more. When there is one stretching point, the temperature of the roll immediately before the stretching point (roll before stretching) (T MD ), when there are two or more stretching points, the surface temperature of the roll before stretching at the point where the stretching ratio is maximum (T MD ) is preferably 125°C or higher and 175°C or lower, more preferably 130°C or higher and 170°C or lower, even more preferably 135°C or higher and 168°C or lower, and particularly preferably 140°C or higher and 166°C or lower. The stretching ratio in the machine direction (the product of the stretching points when there are two or more stretching points) is preferably 1.5 times or higher and 5.0 times or lower, more preferably 2.0 times or higher and 4.6 times or lower, and even more preferably 2.2 times or higher and 4.2 times or lower. By setting the temperature and stretching ratio within these ranges, orientation in the machine direction is suppressed within an appropriate range, and a stretched film excellent in rigidity, electrical insulation, stretchability, etc. can be easily obtained.

[0131] The tenter used in the present invention preferably has three or more temperature zones, and more preferably five or more temperature zones, so that heating, stretching, and the later-described heat treatment, relaxation treatment, cooling treatment, etc. can be performed at different temperatures.

[0132] When longitudinal stretching is performed in a tenter, the oven temperature during stretching (T MD ) is preferably 125° C. or higher and 175° C. or lower, more preferably 130° C. or higher and 170° C. or lower, even more preferably 135° C. or higher and 168° C. or lower, and particularly preferably 140° C. or higher and 166° C. or lower. The draw ratio in the machine direction is preferably 1.5 times or higher and 5.0 times or lower, more preferably 2.0 times or higher and 4.6 times or lower, and even more preferably 2.2 times or higher and 4.2 times or lower.

[0133] When transverse stretching is performed in a tenter, the oven temperature during stretching (T TD ) is preferably 140°C or higher and 175°C or lower, more preferably 145°C or higher and 170°C or lower, even more preferably 150°C or higher and 168°C or lower, and particularly preferably 155°C or higher and 166°C or lower. The stretching ratio in the transverse direction is preferably 5.0 times or higher and 11.0 times or lower, more preferably 6.0 times or higher and 10.0 times or lower, and even more preferably 7.0 times or higher and 9.5 times or lower. By setting the temperature and stretching ratio within these ranges, orientation in the transverse direction is suppressed within an appropriate range, and a stretched film excellent in rigidity, electrical insulation, stretchability, etc. can be easily obtained.

[0134] The above-mentioned stretching temperature (T MD、 and T TD ) is more preferably adjusted depending on the glass transition temperature (Tg) of the polymer having an alicyclic structure in the side chain contained in the layer A of the present invention. MD is preferably Tg-10°C or higher and Tg+25°C or lower, more preferably Tg-5°C or higher and Tg+20°C or lower, and even more preferably Tg or higher and Tg+16°C or lower. TD is preferably Tg or higher and Tg+30° C. or lower, more preferably Tg+5° C. or higher and Tg+28° C. or lower, and even more preferably Tg+10° C. or higher and Tg+25° C. or lower. By setting the temperature within this range, the orientation of the stretched film is suppressed within an appropriate range, and a stretched film excellent in rigidity, electrical insulation, stretchability, etc. can be easily obtained.

[0135] In addition, the above-mentioned stretching temperature (T MD and T TD If the temperature is below the above-mentioned range, if the kneading properties during resin blending or extrusion are poor, or if the draft ratio during extrusion molding is inappropriate, pores may be formed in Layer A during stretching. If many pores are formed, the rigidity, electrical insulation properties, and stretchability of the stretched film tend to be easily reduced.

[0136] Since the total light transmittance of the stretched film is likely to decrease when many pores are formed, the total light transmittance of the stretched film of the present invention is preferably 80% or more, more preferably 85% or more, even more preferably 88% or more, and particularly preferably 90% or more. From the viewpoint of the electrical characteristics (safety) of the capacitor, the total light transmittance is preferably 99% or less, more preferably 98% or less, even more preferably 97% or less, and particularly preferably 96% or less.

[0137] The product of the longitudinal stretching ratio and the transverse stretching ratio of the stretched film (when a relaxation treatment described below is performed, the product is calculated using the longitudinal stretching ratio and the transverse stretching ratio before relaxation) is preferably 15 to 48, more preferably 17 to 42, even more preferably 19 to 38, particularly preferably 21 to less than 35, and more particularly preferably 22 to 34. By setting the temperature and stretching ratio within these ranges, a stretched film excellent in rigidity, electrical insulation, stretchability, etc. can be easily obtained.

[0138] Stretched films with an area ratio of 12% or less and unstretched films (with an area ratio of 1%) tend to have reduced rigidity and electrical insulation. Furthermore, if the area ratio at which a film can be stretched without breaking is 12% or less, the film's stretchability is not very good.

[0139] The stretched film of the present invention may be subjected to a relaxation treatment (a treatment of reducing the stretch ratio after stretching, for example, by up to 20% of the stretch ratio), a heating treatment, or a cooling treatment, as necessary. These treatments may be performed independently or in combination, for example, by performing the relaxation treatment and the heating treatment simultaneously, or by performing the relaxation treatment and the cooling treatment simultaneously. By appropriately performing the relaxation treatment, the heating treatment, and the cooling treatment, the flatness of the stretched film, the dimensional stability against temperature changes, the passability through the vapor deposition process, etc. can be improved.

[0140] The relaxation in the transverse direction is preferably 3% to 20% of the maximum stretching ratio in the transverse direction, more preferably 5% to 16%, and even more preferably 6.5% to 14%.

[0141] The heat treatment temperature is preferably 150° C. to 180° C., more preferably 155° C. to 175° C., and even more preferably 160° C. to 172° C. The heat treatment time is preferably 1 second to 20 seconds, and more preferably 2 seconds to 15 seconds.

[0142] The stretched film of the present invention may be subjected to corona treatment, static electricity removal treatment, heating treatment, etc. Appropriately performing corona treatment, static electricity removal treatment, heating treatment, etc. can improve the passability through the deposition process. The heating treatment temperature is preferably 20°C or higher and 80°C or lower, more preferably 25°C or higher and 60°C or lower, and even more preferably 30°C or higher and 55°C or lower. The heating treatment time is preferably 3 hours or higher and 50 hours or lower, and more preferably 6 hours or higher and 30 hours or lower.

[0143] 2. Metal Laminated Film In one aspect, the present invention relates to a metal laminated film (sometimes referred to herein as the "metal laminated film of the present invention") having the stretched film of the present invention and a metal layer laminated on one or both sides of the stretched film. This will be described below.

[0144] The stretched film of the present invention may have a metal layer on one or both sides thereof, for example, to adjust the permeability of gases such as oxygen and water vapor when used as a packaging film, or as an electrode when used as a capacitor.

[0145] Examples of methods for laminating a metal layer on the surface of the stretched film of the present invention include vacuum plating such as metal vapor deposition and sputtering, coating and drying of a metal-containing paste, and pressure bonding of a metal foil or metal powder. Among these, from the viewpoints of productivity and economy, vacuum vapor deposition and sputtering are more preferred, and vacuum vapor deposition is even more preferred. Examples of vacuum vapor deposition methods include the crucible method and the wire method, but are not particularly limited, and an optimal method can be selected as appropriate.

[0146] The metal used in the metal layer may be, for example, a single metal such as zinc, lead, silver, chromium, aluminum, copper, or nickel, a mixture of two or more of these metals, or an alloy of these metals. However, taking into consideration the environment, economy, performance, and the like, one or more of zinc and aluminum are preferred.

[0147] The film resistance of the metal layer is preferably about 0.5 to 10 Ω / □ from the viewpoint of permeability to gases such as oxygen and water vapor, and about 1 to 60 Ω / □ from the viewpoint of the electrical properties of the capacitor. From the viewpoint of the electrical properties of the capacitor, in order to exhibit self-healing properties, the film resistance is more preferably 5 Ω / □ or more, and even more preferably 10 Ω / □ or more, and from the viewpoint of safety as a capacitor, the film resistance is more preferably 50 Ω / □ or less, and even more preferably 30 Ω / □ or less.

[0148] When forming an electrode (metal vapor deposition film) by vacuum deposition, the film resistance can be measured during deposition, for example, by a non-contact eddy current method or light transmittance method known to those skilled in the art. The film resistance of the metal vapor deposition film can be adjusted, for example, by adjusting the output of the evaporation source to adjust the evaporation amount.

[0149] In capacitor applications, when a metal vapor deposition film is formed on one side of a stretched film, an insulating margin (vertical margin) of a certain width where no metal is laminated is formed so that it will become an insulating part when the film is rolled up to form a capacitor.

[0150] Furthermore, it is preferable to form a heavy edge portion to strengthen the bond between the metal layer of the metal layer-integrated film and the metallikon electrode. The film resistance of the heavy edge portion is usually about 1 to 8 Ω / □, and preferably about 1 to 5 Ω / □. The thickness of the metal film of the heavy edge portion is not particularly limited, but is preferably 1 to 200 nm.

[0151] In capacitor applications, there are no particular limitations on the deposition pattern (fuse pattern) of the metal deposition film to be formed, but from the viewpoint of improving the properties of the capacitor, such as safety, it is preferable to form fuses by pattern deposition, such as a fishnet pattern, a T-margin pattern, etc. Forming a metal deposition film with a deposition pattern including a fuse on at least one surface of the stretched film of the present invention is preferable because it improves the safety of the resulting capacitor and is effective in preventing breakdown and short circuits of the capacitor.

[0152] As a method for forming the fuse and the insulating margin, any known method can be used without any restrictions, such as a tape method in which masking is performed with tape during vapor deposition, or an oil method in which masking is performed by applying oil.

[0153] A protective agent may be applied to the metal laminated film of the present invention for the purposes of physical protection of the metal layer, prevention of moisture absorption, prevention of oxidation, etc. As the protective agent, silicone oil, fluorine oil, etc. can be preferably used. The protective agent may be provided as a layer on the metal layer, or may be impregnated into the metal layer.

[0154] The metal laminated film of the present invention can be processed into the capacitor of the present invention described below. The metal laminated film of the present invention can also be used for packaging purposes, for example, as a barrier film against oxygen and other gases.

[0155] 3. Film Capacitor In one aspect, the present invention relates to a film capacitor (sometimes referred to as the "capacitor of the present invention" in this specification) comprising the stretched film of the present invention or the metal-laminated film of the present invention. This will be described below.

[0156] In such capacitors, the stretched film of the present invention can be used as a dielectric film for a capacitor by, for example, (i) using the above-mentioned metal laminated film, (ii) laminating the stretched film of the present invention not provided with electrodes with a dielectric having metallized surfaces (the dielectric can be, for example, the stretched film of the present invention or another plastic film), or (iii) laminating the stretched film of the present invention not provided with electrodes with another conductor (for example, a metal foil).

[0157] In the process of producing a capacitor, a film winding process is performed. For example, a pair of metal laminated films of the present invention are overlapped and wound so that the metal layers of the metal laminated film of the present invention and the stretched film of the present invention are alternately stacked, and further, the insulating margins are on opposite sides. In this case, it is preferable to stack the pair of metal laminated films of the present invention with a 1 to 2 mm offset. The winding machine used is not particularly limited, and for example, an automatic winding machine 3KAW-N2 manufactured by Kaito Seisakusho Co., Ltd. can be used.

[0158] The film winding process is not limited to the above method, and other methods may be used. For example, a double-sided vapor-deposited stretched film of the present invention (in which case the heavy edges are positioned at the opposite ends of the front and back surfaces) and a non-vapor-deposited stretched film of the present invention (having a width 2 to 3 mm narrower than that of the double-sided vapor-deposited stretched film of the present invention) may be alternately laminated and wound.

[0159] When producing a flat capacitor, the resulting roll is usually pressed after winding. This press tightens the capacitor and promotes element formation. From the viewpoint of controlling and stabilizing the interlayer gap, the optimum pressure to be applied varies depending on the thickness of the stretched film of the present invention, but is generally 2 to 20 kg / cm. 2 is.

[0160] Next, metal is sprayed onto both end surfaces of the wound body to provide metallikon electrodes, thereby producing a capacitor.

[0161] The capacitor is then subjected to a predetermined heat treatment. That is, the present invention includes a step of subjecting the capacitor to heat treatment (hereinafter, sometimes referred to as "thermal aging"). The heat treatment temperature is not particularly limited, but is, for example, 80 to 190°C. The method for subjecting the capacitor to heat treatment may be appropriately selected from known methods, including, for example, a method using a thermostatic bath under a vacuum atmosphere or a method using high-frequency induction heating. The heat treatment time is preferably 1 hour or more, more preferably 5 hours or more, from the viewpoint of obtaining mechanical and thermal stability, but is more preferably 20 hours or less, from the viewpoint of preventing molding defects such as heat wrinkles and molding.

[0162] The heat treatment provides the effect of thermal aging. Specifically, the gaps between the films constituting the capacitor based on the stretched film of the present invention are reduced, corona discharge is suppressed, and the internal structure of the stretched film of the present invention is changed, promoting crystallization. As a result, it is believed that the electrical insulation properties are improved. If the heat treatment temperature is lower than the predetermined temperature, the above-mentioned effect of thermal aging cannot be fully obtained. On the other hand, if the heat treatment temperature is higher than the predetermined temperature, the stretched film of the present invention may undergo thermal decomposition, oxidative degradation, etc.

[0163] Lead wires or bus bars are usually welded to the metallikon electrodes of the heat-aged capacitor. To impart weather resistance, particularly to prevent humidity degradation, the capacitor is preferably encapsulated in a case and potted with epoxy resin.

[0164] The capacitor of the present invention using the stretched film of the present invention can be suitably used in high-temperature environments, and can be made into a small-sized capacitor with a high capacity (for example, 5 μF or more, preferably 10 μF or more, and more preferably 20 μF or more). Therefore, the capacitor of the present invention can be used as a high-voltage capacitor used in electronic devices, electrical devices, etc.; various switching power supplies; filter capacitors, smoothing capacitors for converters, inverters, etc. Furthermore, the capacitor of the present invention can be suitably used as an inverter capacitor, converter capacitor, etc. for controlling the drive motor of electric vehicles, hybrid vehicles, etc., which have seen increasing demand in recent years.

[0165] The present invention will be specifically described below with reference to examples and comparative examples, but the present invention is not limited to these examples.

[0166] (1) Measurement methods The various measurement methods are as follows.

[0167] (1-1) Number-average molecular weight (Mn), weight-average molecular weight (Mw), z-average molecular weight (Mz), molecular weight distribution (Mw / Mn), and molecular weight distribution (Mz / Mw) of polypropylene-based resins Using GPC (gel permeation chromatography) under the following conditions, the number-average molecular weight (Mn), weight-average molecular weight (Mw), z-average molecular weight (Mz), molecular weight distribution (Mw / Mn), and molecular weight distribution (Mz / Mw) of each resin were measured.

[0168] Specifically, a high-temperature GPC system with a built-in differential refractometer (RI), model HLC-8121GPC-HT, manufactured by Tosoh Corporation, was used. Three TSKgel GMHHR-H(20)HT columns manufactured by Tosoh Corporation were connected together and used. Measurements were performed at a column temperature of 140°C, with trichlorobenzene as the eluent at a flow rate of 1.0 ml / min. A calibration curve for the molecular weight M was created using standard polystyrene manufactured by Tosoh Corporation, and the measured values ​​were converted to the molecular weight of polypropylene using the Q-factor to obtain the number average molecular weight (Mn), weight average molecular weight (Mw), and z-average molecular weight (Mz). The molecular weight distribution (Mw / Mn) was obtained using the values ​​of Mw and Mn. The molecular weight distribution (Mz / Mw) was also obtained using the values ​​of Mz and Mw.

[0169] (1-2) Mesopentad Fraction of Polypropylene Resin A polypropylene resin was dissolved in a solvent and measured using a high-temperature Fourier transform nuclear magnetic resonance spectrometer (high-temperature FT-NMR) under the following conditions. High-temperature nuclear magnetic resonance (NMR) spectrometer: JNM-ECP500, high-temperature Fourier transform nuclear magnetic resonance spectrometer (high-temperature FT-NMR), manufactured by JEOL Ltd. Observation nucleus: 13C (125 MHz) Measurement temperature: 135°C Solvent: ortho-dichlorobenzene (ODCB: mixed solvent of ODCB and deuterated ODCB (mixing ratio = 4 / 1)) Measurement mode: single pulse proton broadband decoupling Pulse width: 9.1 μsec (45° pulse) Pulse interval: 5.5 sec Number of accumulations: 4,500 Shift reference: CH 3 (mmmm) = 21.7 ppm The mesopentad fraction, which indicates the degree of stereoregularity, was calculated as a percentage (%) from the integrated intensity values ​​of each signal derived from a combination of five pentads (pentads) consisting of meso (m) pentads arranged in the same direction and racemo (r) pentads arranged in the opposite direction (mmmm, mrrm, etc.). The assignment of each signal derived from mmmm, mrrm, etc. was based on the spectral descriptions in, for example, "T. Hayashi et al., Polymer, Vol. 29, p. 138 (1988)".

[0170] (1-3) Heptane-insoluble fraction (HI) of polypropylene-based resin: A polypropylene-based resin was press-molded to a size of 10 mm x 35 mm x 0.3 mm to prepare a measurement sample of approximately 3 g. Next, approximately 150 mL of heptane was added, and Soxhlet extraction was performed for 8 hours. The heptane-insoluble fraction was calculated from the sample mass before and after extraction.

[0171] (1-4) Melt Mass Flow Rate of Resin The melt flow rate (MFR) of each resin in the form of raw resin pellets was measured in accordance with JIS K 7210-1:2014 using a melt indexer manufactured by Toyo Seiki Co., Ltd. Specifically, 4 g of raw material was first inserted into a cylinder set to the test temperature (230 ° C for polypropylene resins, 260 ° C for polymers having an alicyclic structure in the side chain and polymers having an alicyclic structure in the main chain), and preheated for 3.5 minutes under a load of 2.16 kg. Thereafter, the weight of the raw material resin extruded from the bottom hole over 30 seconds was measured, and the MFR (g / 10 min) was calculated. The above measurement was repeated three times, and the average value was used as the measured MFR.

[0172] (1-5) Melting Point and Glass Transition Temperature of Resin Calculation was performed using a Perkin-Elmer Diamond DSC, an input compensation type DSC, according to the following procedure. 5 mg of each resin was weighed out, packed into an aluminum sample holder, and set in the DSC device. Under a nitrogen flow, the temperature was increased from 30°C to 230°C at a rate of 20°C / min, held at 230°C for 5 minutes, cooled to 30°C at 20°C / min, and held at 30°C for 5 minutes. The melting point and glass transition temperature were then determined from the DSC curve when the temperature was again increased to 230°C at 20°C / min. Specifically, the melting peak (the largest melting peak when multiple melting peaks are shown) defined in JIS-K7121 9.1(1) was used as the melting point, and the midpoint glass transition temperature defined in JIS-K7121 9.3(1) was used as the glass transition temperature.

[0173] (1-6) Average Particle Diameter The average particle diameter of the particles was measured as follows. The powder was scattered on a sample stage so that individual particles did not overlap as much as possible, and at least 100 particles were observed at 10,000 to 30,000 magnifications using an ultra-high resolution field emission scanning electron microscope (FE-SEM, S-5200, manufactured by Hitachi High-Technologies Corporation), and images were obtained. The longest diameter of each particle was measured from the observed image using image analysis software, and the measured values ​​were averaged to determine the average particle diameter.

[0174] (2) Preparation of resin composition and stretched film (2-1) Resins used, etc. [Polypropylene-based resins] Raw material A: Polypropylene-based resin A1: Isotactic polypropylene resin manufactured by Prime Polymer Co., Ltd. Prime Polypro (registered trademark) MFR: 3.5 g / 10 min (measurement temperature 230 ° C, 2.16 kg weight) Melting point: 164 ° C Mesopentad fraction: 98.6 mol % Heptane insoluble matter: 98.1 mass % Number average molecular weight (Mn): 49,000 Weight average molecular weight (Mw): 390,000 Z average molecular weight (Mz): 1,520,000 Molecular weight distribution (Mw / Mn): 8.0 Molecular weight distribution (Mz / Mw): 3.9 A2: Isotactic polypropylene resin manufactured by Prime Polymer Co., Ltd. Prime Polypro (registered trademark) MFR: 5.6 g / 10 min (measurement temperature 230°C, 2.16 kg weight) Melting point: 162°C Mesopentad fraction: 97.4 mol% Heptane insolubles: 97.8 mass% Number average molecular weight (Mn): 47,000 Weight average molecular weight (Mw): 270,000 Z average molecular weight (Mz): 750,000 Molecular weight distribution (Mw / Mn): 5.7 Molecular weight distribution (Mz / Mw): 2.8 Raw material B: Polymer having an alicyclic structure in the side chain B1: ViviOn (registered trademark) 0645 manufactured by USI Corporation Glass transition temperature: 146°C MFR: 5.5 g / 10 min (measurement temperature 260°C, 2.16 kg weight) Having a cyclohexane structure in the side chain (The cyclohexane structure is formed by hydrogenation of an aromatic ring structure, and the hydrogenation rate is 99 mol % or more.) B2: ViviOn (registered trademark) 1325 manufactured by USI Corporation Glass transition temperature: 128°C MFR: 13 g / 10 min (measurement temperature 260°C, weight 2.16 kg) Has a cyclohexane structure in the side chain(The cyclohexane structure is formed by hydrogenation of an aromatic ring structure, and the hydrogenation rate is 99 mol% or more.) Raw material C: Polymer having an alicyclic structure in the main chain C1: TOPAS (registered trademark) COC6013S-04 manufactured by Polyplastics Co., Ltd. Glass transition temperature: 138°C MFR: 14 g / 10 min (measurement temperature 260°C, 2.16 kg weight) Having a norbornene structure in the main chain Raw material D: Particles D1: Silica particles Seahoster (registered trademark) KE-S100 manufactured by Nippon Shokubai Co., Ltd. Average particle size: 1.0 μm

[0175] (2-2) Methods for Producing Resin Compositions and Stretched Films [Examples 1 to 6, Examples 8 to 10, Comparative Examples 1 to 2, Comparative Example 4] [Production of Unstretched Films] Raw materials A, B, C, and D were weighed out so that each raw material was in the proportions shown in Table 1, and the raw material mixture for layer A was obtained by dry blending using a tumbler. The raw materials were then charged into a single-screw film-forming extruder (GM-50, manufactured by GM Engineering Co., Ltd., L / D = 32). The raw materials were melted in the extruder, which was set to the melting temperature shown in Table 1, and then filtered through a filter with a filtration accuracy of 20 μm, and extruded from a T-die set to 235°C.

[0176] The molten resin was brought into contact with a mirror-finished metal roll (cooling roll) having a surface temperature of 90° C. using an air knife, solidified, and formed into a film to obtain a single-layer unstretched film.

[0177] The average slit gap t at the die lip outlet of the T-die was changed so that the draft ratio would be the value shown in Table 1.

[0178] The thickness of the unstretched film was finely adjusted by changing the extrusion rate and take-up speed so that the thickness after stretching would reach the target value.

[0179] [Preparation of Stretched Film] An unstretched film was introduced into a roll-type longitudinal stretching machine, heated sequentially by five preheating rolls, and then heated to the temperature (T MDThe film was heated with a pre-stretching roll whose surface temperature was adjusted to 100°C (T ), and uniaxially stretched in the machine direction (MD) at a stretching ratio shown in Table 1. The film was then introduced into a tenter, heated in a preheating zone whose furnace temperature was adjusted to the preheating temperature shown in Table 1, and then stretched at the temperature (T TD ), the film was stretched in the transverse direction (TD) at the stretching ratios listed in Table 1 in a stretching zone with an oven temperature adjusted to 170°C. The film was then relaxed in width (transverse direction) by 10% in a heating zone set at 170°C. The end of the stretched film emerging from the tenter was slit to a width of 620 mm, and the side where the air knife had been used was subjected to corona treatment and then wound up to obtain a roll of stretched film. The extrusion rate and take-up speed were finely adjusted to obtain a film thickness of 2.8 μm. The film stretchability was good in all of Examples 1 to 6, Examples 8 to 10, Comparative Example 1, and Comparative Example 4. On the other hand, the film of Comparative Example 2 broke when stretched to a ratio higher than the listed ratio, and its stretchability could not be said to be good.

[0180] [Example 7] [Production of Unstretched Film] 75 parts of raw material A1 and 25 parts of raw material B1 were weighed and dry-blended using a tumbler to obtain a raw material mixture for layer A. The raw materials were then charged into a single-screw film-forming extruder (GM-50, manufactured by GM Engineering Co., Ltd., L / D = 32). The raw materials were melted in the extruder set at 260°C, filtered through a filter with a filtration accuracy of 20 μm, and fed to the core layer (layer A) section of a three-layer multi-die set at 235°C.

[0181] 99.5 parts of raw material A1 and 0.5 parts of raw material D were weighed and dry-blended using a tumbler to obtain a raw material mixture for layer B, which was then charged into a single-screw film-forming extruder (GM-50, manufactured by GM Engineering Co., Ltd., L / D = 32). The raw materials were melted in the extruder, which was set to the melting temperature shown in Table 1, and then filtered through a filter with a filtration accuracy of 20 μm. The mixture was then branched into two flow paths and fed to the skin layer (layer B) sections on both sides of a three-layer multi-die set to 235°C.

[0182] The layers were laminated in the order of layer B / layer A / layer B in a three-layer multi-die and extruded from the multi-die.

[0183] The three-layer laminated molten resin was brought into contact with a mirror-finished metal roll (cooling roll) having a surface temperature of 90° C. using an air knife, solidified, and formed into a film to obtain a three-layer unstretched film.

[0184] The average slit gap t at the die lip outlet of the multi-die was changed so that the draft ratio was 4.0.

[0185] The thickness of the unstretched film was finely adjusted by changing the extrusion rate and take-up speed so that the thickness after stretching would reach the target value.

[0186] The extrusion rate was adjusted so that the thickness ratio of each layer of the unstretched film was layer B:layer A:layer B = 1:1.8:1.

[0187] [Preparation of Stretched Film] The unstretched film was introduced into a roll-type longitudinal stretching machine, heated sequentially by five preheating rolls, and then heated by a pre-stretching roll with a surface temperature adjusted to 150°C, followed by longitudinal uniaxial stretching at a ratio of 4.0 in the machine direction (MD). The film was then introduced into a tenter, heated in a preheating zone with an oven temperature adjusted to 170°C, and stretched in the transverse direction (TD) at a ratio of 10.0 in a stretching zone with an oven temperature adjusted to 167°C. The width (transverse direction) was then relaxed by 10% in a heating zone set at 170°C. The end of the stretched film emerging from the tenter was slit to a width of 620 mm, and the side where the air knife was used was subjected to corona treatment and then wound up to obtain a roll of stretched film. The extrusion rate and take-up speed were finely adjusted so that the film thickness was 2.8 μm. The stretchability of the film of Example 7 was good.

[0188] [Comparative Example 3] 75 parts of raw material A1 and 25 parts of raw material B1 were weighed and dry-blended using a tumbler to obtain a raw material mixture for layer A. The resulting mixture was then charged into a single-screw film-forming extruder (GM-50, manufactured by GM Engineering Co., Ltd., L / D = 32). The raw materials were melted in the extruder, which was set at 260°C, and then filtered through a filter with a filtration accuracy of 20 μm, and extruded from a T-die, which was set at 235°C.

[0189] The molten resin was brought into contact with a mirror-finished metal roll (cooling roll) having a surface temperature of 90° C. using an air knife, solidified, and formed into a film to obtain a single-layer unstretched film.

[0190] In this case, the average slit gap t at the die lip outlet of the T-die was changed so that the draft ratio would be 40.

[0191] The extrusion rate and take-up speed were changed and finely adjusted so that the thickness of the unstretched film would be 5 μm.

[0192] The unstretched film was slit at one end to a width of 620 mm, and the side on which the air knife had been used was subjected to a corona treatment, after which it was wound up to obtain a roll of unstretched film. In this way, a roll of unstretched film was obtained as a comparative product in Comparative Example 3.

[0193]

[0194] (3) Measurement and Evaluation of Physical Properties and Characteristics of Stretched Films (3-1) Measurement of Total Light Transmittance The total light transmittance of the stretched films obtained in the examples and comparative examples (however, Comparative Example 3 is a comparative product and is an unstretched film; the same applies hereinafter) was measured in accordance with JIS-K7361 using a haze meter NDH-5000 manufactured by Nippon Denshoku Industries Co., Ltd.

[0195] (3-2) Measurement of Dielectric Breakdown Strength and Dielectric Strength Retention Rate The dielectric breakdown strength of the stretched films obtained in the Examples and Comparative Examples at high temperatures was evaluated as follows. A measuring device conforming to 17.2.2 (Plate Electrode Method) of JIS C2151:2006 was prepared. However, as the lower electrode, a conductive rubber (E12S10 manufactured by Seiwa Electric Co., Ltd.) was used instead of the elastic body described in 17.2.2 of JIS C2151:2006, and aluminum foil was not wrapped around the electrode.

[0196] The measurement environment was a forced circulation oven set at a temperature of 120°C or 135°C, and the electrodes and films were used after 30 minutes of temperature adjustment in the oven. The voltage was increased from 0 V at a rate of 100 V / sec, and the voltage when the current value exceeded 5 mA was taken as the breakdown voltage. The breakdown voltage was measured 20 times, and each breakdown voltage value V DC is divided by the thickness (μm) of the stretched film, and the average of 16 points excluding the top 2 and bottom 2 points out of the 20 calculation results is calculated as the dielectric breakdown strength (V DC / μm).

[0197] The dielectric strength maintenance rate (%) was calculated as the ratio of the dielectric breakdown strength in a 135°C environment to the dielectric breakdown strength in a 120°C environment obtained by the above measurement (dielectric breakdown strength in a 135°C environment / dielectric breakdown strength in a 120°C environment).

[0198] (3-3) Measurement of Elongation Rate (Evaluation of Rigidity) Using a Thermo-Mechanical Measuring Apparatus (TMA) Model TMA / SS6000 manufactured by Seiko Instruments Inc., the stretched films of the Examples and Comparative Examples, which were sampled in the form of strips measuring 25 mm in the machine direction (MD) and 4 mm in the transverse direction (TD), were set on a quartz tensile probe. The stretched films were heated from 25°C at a heating rate of 10°C / min under a static load applied in the MD direction of the stretched film at a rate of 16.67 mN per 1 μm of thickness depending on the thickness of the stretched film, and the elongation rate (%) from the initial length (25°C) at a furnace temperature of 130°C was measured.

[0199] Measurement device: Seiko Instruments Inc., TMA / SS6000 type Measurement probe: Quartz tensile probe Measurement mode: F mode (load control mode) Static load: Depending on the thickness of the stretched film, the ratio is 16.67 mN per 1 μm of thickness Initial chuck distance: 15 mm Set temperature range: 25°C to 170°C Heating rate: 10°C / min Data sampling time: 0.5 sec

[0200] (3-4) Evaluation of Vapor Deposition Process Passability Using the rolls of the stretched films of the Examples and Comparative Examples, the vapor deposition process passability was evaluated by a vacuum vapor deposition method. Using a vacuum vapor deposition apparatus EWE-060 manufactured by ULVAC, Inc., aluminum was vapor-deposited on the corona-treated side of the stretched film at a tension of 40 N / m, a vapor deposition speed of 150 m / min, and an electron beam irradiation output of −3.5 KV for tightly contacting the stretched film with the cooling roll that holds the stretched film in close contact during vapor deposition, so that the surface resistivity of the metal film was 20 Ω / □.

[0201] In this case, in addition to both transverse ends of the stretched film, nine 4 mm wide insulating margins (vertical margins) where no metal was laminated were provided at equal intervals. The 11 areas where no metal was laminated, including two at both transverse ends and nine vertical margins, tend to be more difficult to peel from the cooling roll than the areas where metal was laminated.

[0202] This difference in peelability and the influence of heat from the metal during vapor deposition can cause breakage in the stretched film. Vapor deposition was performed on a 5,000 m length under these conditions, and the vapor deposition process passability was evaluated according to the following criteria: ◯: No breakage occurred in the stretched film (0 times). ×: Breakage occurred in the stretched film one or more times.

[0203] (4) Measurement and Evaluation Results Table 2 shows the measurement and evaluation results of the physical properties and characteristics of the stretched films of the Examples and Comparative Examples.

[0204] From the above evaluation results, it was found that the stretched films (Examples 1 to 10) having an A layer containing 55% by mass or more and 99% by mass or less of a polypropylene resin and 1% by mass or more and 45% by mass or less of a polymer having an alicyclic structure in a side chain, where the mass of the A layer is taken as 100%, and in which the A layer is stretched in at least one direction, suppress a decrease in rigidity and a decrease in electrical insulation even in a high-temperature environment exceeding 110°C, and are excellent in their own stretchability and passability through post-processing steps.

[0205]

Claims

1. A stretched film having at least Layer A, characterized in that: (1) Layer A contains, in 100% by mass, 55% to 99% by mass of a polypropylene-based resin and 1% to 45% by mass of a polymer having an alicyclic structure in its side chain; and (2) Layer A is stretched in at least one direction.

2. The stretched film described in claim 1, wherein the A layer contains, based on 100% by mass, 55% by mass or more and 97% by mass or less of a polypropylene-based resin and 3% by mass or more and 45% by mass or less of a polymer having an alicyclic structure in its side chain.

3. The stretched film according to claim 1, wherein the polymer has a glass transition temperature of 100°C or higher and 180°C or lower.

4. The stretched film according to claim 1, wherein the alicyclic structure has a cyclohexane structure.

5. The stretched film according to claim 1, wherein the thickness of the stretched film is 10 μm or less and the total light transmittance is 80% or more.

6. A metal laminated film comprising the stretched film according to any one of claims 1 to 5 and a metal layer laminated on one or both sides of the film.

7. A film capacitor comprising the stretched film according to any one of claims 1 to 5.

8. A film capacitor comprising the metal laminate film according to claim 6.

Citation Information

Patent Citations

  • Resin composition and film and container made of the resin composition

    JP2014037532A

  • Polyolefin-based film, metallized film including same, film capacitor, power control unit, electric vehicle, and electric aircraft

    WO2022270577A1

  • Highly rigid polypropylene composition

    JP1990135243A

  • Polypropylene drawn film

    JP1990135245A

  • Method for manufacturing capacitor element

    JP2015146374A

Cited By

  • Biaxially oriented polypropylene film

    JP7893388B1

  • Biaxially oriented polypropylene film

    WO2026140628A1