Method for cleaning semiconductor chip, and method for manufacturing semiconductor device

The method of using a chemical solution on semiconductor chips with a specific adhesive composition addresses the issue of foreign matter adherence during dicing, improving connection reliability by efficiently cleaning chips and maintaining adhesive strength, supporting advanced integration technologies.

WO2024228363A1PCT designated stage expired Publication Date: 2024-11-07RESONAC CORP
View PDF 10 Cites -1 Cited by

Patent Information

Application Number
PCT/JP2024/016315
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-05-01
Filing Date
2024-04-25
Publication Date
2024-11-07

AI Technical Summary

Technical Problem

In semiconductor manufacturing, foreign matter such as cutting debris adheres to semiconductor chips during the dicing process, which can cause reliability issues in hybrid bonding and other advanced integration technologies, as it can lead to poor connection reliability between devices.

Method used

A method for cleaning semiconductor chips using a chemical solution on an adhesive film with a specific adhesive composition that includes a resin represented by formula (1-1) and a photopolymerization initiator, allowing for efficient removal of foreign matter without compromising the adhesive strength, enabling high-level cleaning on-site during manufacturing.

Benefits of technology

This method effectively removes foreign substances from semiconductor chips, enhancing connection reliability in semiconductor devices by ensuring high cleanliness and maintaining adhesive strength, thus supporting advanced three-dimensional integration technologies.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JP2024016315_07112024_PF_FP_ABST
    Figure JP2024016315_07112024_PF_FP_ABST
Patent Text Reader

Abstract

This method for cleaning a semiconductor chip includes: (a) a step for cleaning, with a chemical liquid, a plurality of semiconductor chips arranged in a region which is on the surface of an adhesive film and within a dicing ring attached to the surface; and (b) a step for picking up the cleaned semiconductor chips from the surface. The adhesive film includes a base material film and an adhesive layer formed on the surface of the base material film. The adhesive layer contains an adhesive composition comprising a predetermined resin (A) and a photopolymerization initiator (B). The chemical liquid is one selected from the group consisting of a solvent-based chemical liquid, an acid-based chemical liquid, and an alkali-based chemical liquid.
Need to check novelty before this filing date? Find Prior Art

Description

Semiconductor chip cleaning method and semiconductor device manufacturing method

[0001] The present disclosure relates to a method for cleaning a semiconductor chip and a method for manufacturing a semiconductor device.

[0002] Conventionally, semiconductor devices are manufactured through the following steps: a semiconductor wafer is attached to a dicing adhesive sheet, and the semiconductor wafer is then diced into semiconductor chips (dicing process). Then, steps such as picking up the semiconductor chips and bonding the semiconductor chips to an adherend (e.g., a substrate) are carried out. As various devices become more multifunctional, stacked MCPs (multi-chip packages) that achieve high capacity by stacking semiconductor elements in multiple layers have become widespread. To achieve more advanced three-dimensional integration technology, for example, hybrid bonding, which connects different types of devices, has also been developed. Patent Document 1 discloses bonding multiple semiconductor chips to a substrate by hybrid bonding.

[0003] Japanese Patent Application Laid-Open No. 2001-197431

[0004] The present inventors have conducted research from various perspectives toward the practical application of advanced three-dimensional integration technologies such as hybrid bonding, and have found that it is useful to clean semiconductor chips more thoroughly than conventional methods before bonding them to an adherend. During the semiconductor device manufacturing process, for example, during the thinning and dicing steps of semiconductor wafers, foreign matter such as cutting debris is generated, and semiconductor chips with such foreign matter attached may be subjected to the next step. For example, hybrid bonding often involves bonding dissimilar devices together at their surfaces, and any foreign matter remaining between the two surfaces, even if it is very small, can reduce the connection reliability of the semiconductor device.

[0005] The present disclosure provides a semiconductor chip cleaning method capable of efficiently and thoroughly removing foreign matter adhering to semiconductor chips during the semiconductor device manufacturing process, and also provides a semiconductor device manufacturing method using semiconductor chips cleaned by this method.

[0006] One aspect of the present disclosure relates to a method for cleaning semiconductor chips. The method includes: (a) a step of cleaning, with a chemical solution, a plurality of semiconductor chips arranged in an area on the surface of an adhesive film, the area being within a dicing ring attached to the surface; and (b) a step of picking up the cleaned semiconductor chips from the surface. The adhesive film includes a substrate film and an adhesive layer formed on the surface of the substrate film. The adhesive layer contains an adhesive composition including a resin (A) represented by formula (1-1) and a photopolymerization initiator (B). The chemical solution is a type of chemical solution selected from the group consisting of solvent-based, acid-based, and alkaline-based chemical solutions. [In formula (1-1), k, l, m, and n represent the molar composition ratio when k + l + m + n = 100. k is greater than 0 and not greater than 92. l is 0 to 50. m is greater than 0 and not greater than 90. The sum of k, l, and m is 65 to 95. n is 5 to 35. R 1 , R 2 , R 3 , and R 4 is a hydrogen atom or a methyl group. 5 is an alkyl group having 1 to 16 carbon atoms. 6 is an alicyclic hydrocarbon group having 3 to 30 carbon atoms or an aromatic hydrocarbon group having 6 to 20 carbon atoms. 7 is a hydrogen atom or -(CH 2 ) j -COOH (wherein j is 1 or 2). 8 is a group represented by formula (1-2) or formula (1-3). [In formula (1-2) and formula (1-3), p and q are integers of 0 to 2. s is 0 when p is 0, and is 1 when p is 1 or 2. R 9 is a hydrogen atom or a methyl group.

[0007] Conventionally, semiconductor chips have been cleaned using water on the surface of an adhesive film (also called "dicing tape") to which a dicing ring is attached, but chemical solutions have not been used to clean the semiconductor chips. For example, when bonding a semiconductor chip to a substrate via bumps formed on the semiconductor chip, cleaning with water has not caused any problems. In contrast, according to the present invention, by cleaning the semiconductor chip on the adhesive film with chemical solutions, it is possible to thoroughly remove foreign matter that has adhered to the semiconductor chip through various processes up to that point. Using highly cleaned semiconductor chips can achieve excellent connection reliability in semiconductor devices manufactured using advanced three-dimensional integration technology.

[0008] Furthermore, the inventors have found that the resin contained in the adhesive composition is resistant to chemicals and is less likely to lose adhesive strength, so that the present invention can prevent the semiconductor chip from detaching from the surface of the adhesive film during the process of cleaning the semiconductor chip with chemicals.

[0009] The cleaning method described above is also useful in that it can be carried out efficiently in the semiconductor manufacturing process. That is, in the semiconductor device manufacturing process, it is not efficient to transport semiconductor chips to equipment for advanced cleaning of semiconductor chips and then return the cleaned semiconductor chips to the mounting equipment. In contrast, according to the present invention, advanced cleaning with chemicals is carried out on the surface of the adhesive film with the dicing ring attached to the adhesive film, so that the semiconductor chips after cleaning can be picked up and used directly in the next process.

[0010] One aspect of the present disclosure relates to a method for manufacturing a semiconductor device. This method includes a step of bonding a semiconductor chip that has been subjected to the above-described semiconductor chip cleaning method to an adherend. This method uses a highly cleaned semiconductor chip, making it possible to manufacture a semiconductor device with excellent connection reliability.

[0011] The present disclosure provides a semiconductor chip cleaning method capable of efficiently and highly removing foreign matter adhering to semiconductor chips during the semiconductor device manufacturing process, and also provides a semiconductor device manufacturing method using semiconductor chips cleaned by this method.

[0012] FIG. 1 is a cross-sectional view schematically showing a state in which preparations for carrying out the cleaning method according to the present disclosure are complete. FIG. 2 is a cross-sectional view schematically showing the state in which a semiconductor chip is being picked up after cleaning. FIGS. 3(a), 3(b), and 3(c) are cross-sectional views schematically showing the process of manufacturing a semiconductor device by the method according to the first embodiment. FIGS. 4(a), 4(b), and 4(c) are cross-sectional views schematically showing the process of manufacturing a semiconductor device by the method according to the first embodiment. FIG. 5 is a cross-sectional view schematically showing the state in which the spacing between two adjacent semiconductor chips is widened by applying tension to an adhesive film. FIG. 6 is a cross-sectional view schematically showing a state in which one semiconductor chip is bonded to a substrate. FIG. 7 is a cross-sectional view schematically showing a state in which multiple semiconductor chips are stacked on a substrate. FIG. 8 is a cross-sectional view schematically showing an example of a semiconductor device having a configuration in which multiple semiconductor chips are stacked. FIGS. 9(a) and 9(b) are cross-sectional views schematically showing the process of manufacturing a semiconductor device by the method according to the second embodiment. Figures 10(a) and 10(b) are cross-sectional views schematically showing the process of manufacturing a semiconductor device by the method according to the second embodiment. Figures 11(a) and 11(b) are cross-sectional views schematically showing the process of manufacturing a semiconductor device by the method according to the third embodiment. Figures 12(a) and 12(b) are cross-sectional views schematically showing the process of manufacturing a semiconductor device by the method according to the third embodiment. Figures 13(a) and 13(b) are cross-sectional views schematically showing the process of manufacturing a semiconductor device by the method according to the fourth embodiment. Figures 14(a), 14(b), and 14(c) are cross-sectional views schematically showing the process of manufacturing a semiconductor device by the method according to the fifth embodiment.

[0013] Hereinafter, embodiments of the present disclosure will be described in detail with reference to the drawings. However, the present disclosure is not limited to the following embodiments. In the following embodiments, components (including steps, etc.) are not essential unless otherwise specified. In the following description, identical or equivalent parts are given the same reference numerals, and duplicate explanations will be omitted. Furthermore, positional relationships such as up, down, left, and right will be based on the positional relationships shown in the drawings unless otherwise specified. The sizes of the components in each figure are conceptual, and the dimensional ratios of the drawings are not limited to the ratios shown.

[0014] The numerical values ​​and ranges in this specification do not limit the present disclosure. In this specification, numerical ranges indicated using "to" indicate ranges that include the numerical values ​​before and after "to" as the minimum and maximum values, respectively. In numerical ranges described in stages in this specification, the upper or lower limit value described in one numerical range may be replaced with the upper or lower limit value of another numerical range described in stages.

[0015] <Semiconductor Chip Cleaning Method> A semiconductor chip cleaning method according to this embodiment will be described with reference to FIGS. 1 and 2. FIG. 1 is a cross-sectional view schematically showing a state in which preparations are complete for carrying out the cleaning method according to this embodiment. A plurality of semiconductor chips C shown in FIG. 1 are to be cleaned. FIG. 2 is a cross-sectional view schematically showing a state in which the semiconductor chips C are being picked up after cleaning. The semiconductor chips C are obtained through a process of singulating the workpiece Pw shown in FIG. 3(a), and include a circuit layer C1 and a die C2. The circuit layer C1 is obtained by singulating the circuit layer Lc, and the die C2 is obtained by singulating the semiconductor wafer W (see FIG. 4(c)).

[0016] The cleaning method according to this embodiment includes the following steps: (a) a step of cleaning, with a chemical solution, a plurality of semiconductor chips C arranged in a region R on the surface 5 f of the adhesive film 5 and in a dicing ring DR attached to the surface 5 f, and (b) a step of picking up the semiconductor chips C from the surface after cleaning.

[0017] 1, a plurality of semiconductor chips C are arranged in a region R surrounded by a dicing ring DR. There are no particular limitations on the specific method for cleaning the semiconductor chips C, but, for example, the semiconductor chips C are cleaned by spraying a chemical solution from a nozzle toward the semiconductor chips C. The chemical solution is, for example, one type of chemical solution selected from the group consisting of solvent-based, acid-based, and alkaline-based chemical solutions.

[0018] The solvent-based chemical solution contains, for example, NMP (N-methyl-2-pyrrolidone), MEK (methyl ethyl ketone), PGMEA (propylene glycol monomethyl ether acetate), DMSO (dimethyl sulfoxide) or cyclopentanone, and can effectively remove foreign matter such as cutting chips, grinding chips, processing chips, and dust from the semiconductor chip C.

[0019] The acid-based chemical solution contains, for example, sulfuric acid, citric acid, or hydrofluoric acid, and can effectively remove foreign matter such as cutting chips, grinding chips, processing chips, and dust from the semiconductor chips C.

[0020] The alkaline chemical solution contains, for example, potassium hydroxide, sodium hydroxide, ammonium hydroxide, sodium bicarbonate, hydroxylamine, TMAH (tetramethylammonium hydroxide) or ammonia water, and can effectively remove foreign matter such as cutting chips, grinding chips, processing chips, and dust from the semiconductor chip C.

[0021] The adhesive film 5 includes a base film 1 and an adhesive layer 2 formed on the surface of the base film 1. Examples of the base film 1 include plastic films such as polytetrafluoroethylene film, polyethylene terephthalate film, polyethylene film, polypropylene film, polymethylpentene film, and polyimide film. Of these, a film that is resistant to chemicals used to clean the semiconductor chips C may be used. If necessary, the film may be subjected to a surface treatment such as primer application, UV treatment, corona discharge treatment, polishing treatment, or etching treatment.

[0022] The adhesive layer 2 contains an adhesive composition containing a resin (A) represented by formula (1-1) and a photopolymerization initiator (B). The adhesive composition may be resistant to chemical solutions used for cleaning the semiconductor chips C. The adhesive layer 2 is formed by a process of applying a coating liquid containing the adhesive composition to the surface of the substrate film 1, or by a process of preparing a film made of the adhesive composition using a coating liquid containing the adhesive composition and attaching this to the surface of the substrate film 1. The adhesive layer 2 may have the property of decreasing its adhesive strength when irradiated with activation energy (e.g., ultraviolet light (UV)).

[0023] The resin (A) is a compound (resin) represented by formula (1-1).

[0024]

[0025] In formula (1-1), k, l, m, and n represent the molar composition ratio when k + l + m + n = 100. k is greater than 0 and equal to or less than 92. l is 0 to 50. m is greater than 0 and equal to or less than 90. The sum of k, l, and m is 65 to 95. n is 5 to 35. R 1 , R 2 , R 3 , and R 4 is a hydrogen atom or a methyl group. 5 is an alkyl group having 1 to 16 carbon atoms. 6 is an alicyclic hydrocarbon group having 3 to 30 carbon atoms or an aromatic hydrocarbon group having 6 to 20 carbon atoms. 7 is a hydrogen atom or -(CH 2 ) j -COOH (wherein j is 1 or 2). 8 is a group represented by formula (1-2) or formula (1-3).

[0026] When the sum of k, l, and m is 65 or more, the adhesive composition exhibits sufficient adhesion to the adherend before irradiation with activation energy. The sum of k, l, and m is preferably 70 to 94, and more preferably 80 to 90.

[0027] In formula (1-1), the structural unit in parentheses around k (hereinafter referred to as "structural unit k") is an essential structural unit. The structural unit k contributes to the adhesive strength of the adhesive composition before irradiation with activation energy. The number of structural units in the structural unit k is more than 0 and 92 or less, preferably 45 to 90, and more preferably 60 to 88.

[0028] In formula (1-1), the structural unit in parentheses of l (hereinafter referred to as "structural unit l") is not necessarily an essential structural unit. In other words, the number of structural units of the structural unit l may be 0.

[0029] The structural unit 1 contributes to the heat resistance of the adhesive composition. The number of structural units in the structural unit 1 is 0 to 50, preferably 4 to 40, and more preferably 5 to 30.

[0030] In formula (1-1), the structural unit in parentheses of m (hereinafter referred to as "structural unit m") is an essential structural unit. The structural unit m contributes to the adhesive strength and heat resistance of the adhesive composition before irradiation with activation energy. Furthermore, when the adhesive composition contains a crosslinking agent having a functional group that reacts with a carboxy group, the structural unit m reacts with the crosslinking agent to improve the cohesive strength of the adhesive composition. The number of structural units m of the structural unit m is more than 0 and 90 or less, preferably 1 to 15, and more preferably 1 to 5.

[0031] In formula (1-1), the structural unit in parentheses of n (hereinafter referred to as "structural unit n") is an essential structural unit. The structural unit n contributes to the heat resistance of the adhesive composition. The number of structural units n in the structural unit n is 5 to 35, preferably 10 to 33, and more preferably 10 to 20. When the structural unit n is 35 or less, the unsaturated bonds in the resin (A) form a three-dimensional crosslinked structure upon irradiation with activation energy, and the adhesive composition is cured, resulting in an adhesive composition whose adhesive strength decreases to an appropriate range. Furthermore, when n is 5 or more, the heat resistance improvement effect resulting from the structure derived from the alicyclic compound is obtained.

[0032] Due to the synergistic effect of the functions contributed by each of these structural units, the adhesive composition containing resin (A) has an even better balance between the adhesive strength before and after activation energy irradiation. As a result, the adhesive composition has sufficient adhesive strength to the adherend before activation energy irradiation, and the adhesive strength decreases after activation energy irradiation, resulting in an adhesive composition with better releasability. Moreover, this adhesive composition does not have excessively high adhesive strength even when heated to a high temperature before activation energy irradiation and then returned to room temperature, and has excellent releasability after activation energy irradiation while also being less likely to leave adhesive residue on the adherend after peeling.

[0033] In the structural unit k, R 1 is a hydrogen atom (-H) or a methyl group (-CH 3 ), and preferably a hydrogen atom (—H). 5 is an alkyl group having 1 to 16 carbon atoms, preferably an alkyl group having 1 to 8 carbon atoms, and more preferably an alkyl group having 2, 4 or 8 carbon atoms.

[0034] The structural unit k is R 1 and R 5 When the structural unit k includes a plurality of structural units, the molar composition ratio of the structural unit k indicates the sum of the molar composition ratios of the plurality of structural units. For example, when the structural unit k includes R 1 and / or R 5 In the case where the molar composition ratio of the structural unit A is 2 mol % and the molar composition ratio of the structural unit B is 3 mol %, the molar composition ratio of the number of structural units k is "5" as the sum of the molar composition ratios of the structural unit A and the structural unit B.

[0035] In the structural unit l, R 2 is a hydrogen atom (-H) or a methyl group (-CH 3 ), and preferably a hydrogen atom (—H). 6 is an alicyclic hydrocarbon group having 3 to 30 carbon atoms or an aromatic hydrocarbon group having 6 to 20 carbon atoms, and is preferably an alicyclic hydrocarbon group having 6 to 20 carbon atoms or an aromatic hydrocarbon group having 6 to 10 carbon atoms.

[0036] The structural unit l is R 2 and R6 When the structural unit 1 includes a plurality of structural units, the molar composition ratio of the structural unit 1 represents the sum of the molar composition ratios of the plurality of structural units.

[0037] In the structural unit m, R 3 is a hydrogen atom (-H) or a methyl group (-CH 3 ), and preferably a hydrogen atom (—H). 7 is a hydrogen atom (-H) or -(CH 2 ) j It is —COOH (wherein j is 1 or 2), and preferably a hydrogen atom (—H).

[0038] The structural unit m is R 3 and R 7 In this case, the molar composition ratio of the structural unit m represents the sum of the molar composition ratios of the structural units.

[0039] In the structural unit n, R 4 is a hydrogen atom (-H) or a methyl group (-CH 3 ), and preferably a hydrogen atom (—H). 8 is a group represented by formula (1-2) or formula (1-3). The group represented by formula (1-2) or formula (1-3) both contains a structure derived from an alicyclic compound and has the function of improving the heat resistance of the adhesive composition.

[0040]

[0041] In formula (1-2) and formula (1-3), p and q are integers of 0 to 2. s is 0 when p is 0, and is 1 when p is 1 or 2. R 9 is a hydrogen atom or a methyl group.

[0042] The structural unit n is R 4 and R 8 In this case, the molar composition ratio of the structural unit n represents the sum of the molar composition ratios of the structural units.

[0043] Resin (A) represented by formula (1-1) may be any of a random copolymer, a block copolymer, or an alternating copolymer composed of structural units k, l, m, and n. Resin (A) represented by formula (1-1) may not contain structural unit l, and may be any of a random copolymer, a block copolymer, or an alternating copolymer composed of structural units k, m, and n.

[0044] The weight-average molecular weight (Mw) of the resin (A) is preferably 200,000 to 1,000,000, and more preferably 300,000 to 800,000. If the weight-average molecular weight of the resin (A) is 200,000 or more, when an adhesive layer containing the adhesive composition is attached to an adherend and then peeled off, the adhesive layer is less likely to remain on the adherend. If the weight-average molecular weight of the resin (A) is 1,000,000 or less, the viscosity of the resin (A) does not become too high, resulting in good workability. The weight-average molecular weight of the resin (A) means a value measured by gel permeation chromatography (GPC) and converted using a calibration curve based on standard polystyrene, and can be measured, for example, using the following equipment and conditions.

[0045] Measurement was performed at room temperature (25°C) using gel permeation chromatography (Shodex (registered trademark) GPC-101, manufactured by Resonac Co., Ltd.) and calculated in terms of polystyrene. Column: Shodex (registered trademark) LF-804, manufactured by Resonac Co., Ltd. Column temperature: 40°C Sample: 0.2% by mass solution of resin (A) in tetrahydrofuran Flow rate: 1 ml / min Eluent: tetrahydrofuran Detector: RI detector

[0046] The glass transition temperature (Tg) of the resin (A) is preferably −80 to 0°C, more preferably −60 to −10°C, and even more preferably −50 to −10°C. When the glass transition temperature of the resin (A) is in the range of −80 to 0°C, the adhesive strength of the adhesive composition before irradiation with activation energy is good. The Tg of the resin (A) refers to a value measured by the method described below. First, a 10 mg sample is taken from the resin (A). Next, differential scanning calorimetry is performed using a differential scanning calorimeter (DSC) by changing the temperature of the sample from −100 to 200°C at a heating rate of 10°C / min, and the endothermic onset temperature due to the observed glass transition is taken as the Tg. Note that when two Tg values ​​are observed, the simple average of the two Tg values ​​is taken as the Tg.

[0047] The acid value of the resin (A) is preferably greater than 0 and less than 20 mgKOH / g, and more preferably from 3 to 10 mgKOH / g. When the acid value of the resin (A) is in the range of greater than 0 and less than 20 mgKOH / g, there is no contamination of the adherend (adhesive residue) after heating, resulting in good adhesive properties. Furthermore, when the adhesive composition contains a crosslinking agent, when the acid value of the resin (A) is within the above range, the resin (A) and the crosslinking agent react with each other, resulting in good cohesive strength of the adhesive composition. The acid value of the resin (A) refers to the value measured in accordance with JIS K0070:1992.

[0048] Resin (A) can be produced, for example, by the following method. First, raw material monomers including a carboxyl group-containing ethylenically unsaturated monomer (a) and an ethylenically unsaturated monomer (d) are polymerized to produce a carboxyl group-containing resin (b). Here, the ethylenically unsaturated monomer (d) contains a monomer that provides structural unit k after polymerization, and may also contain a monomer that provides structural unit l. Next, resin (A) can be produced by an addition reaction between the carboxyl group-containing resin (b) and a specific alicyclic epoxy group-containing ethylenically unsaturated compound (c).

[0049] The carboxyl group-containing ethylenically unsaturated monomer (a) is a monomer that gives the structural unit m upon polymerization. The carboxyl group-containing ethylenically unsaturated monomer (a) has one carboxyl group.

[0050] Examples of the carboxy group-containing ethylenically unsaturated monomer (a) include (meth)acrylic acid, β-carboxyethyl (meth)acrylate, carboxypentyl (meth)acrylate, etc. Among these, it is preferable to use (meth)acrylic acid and / or β-carboxyethyl (meth)acrylate as the carboxy group-containing ethylenically unsaturated monomer (a) in terms of reactivity.

[0051] In this specification, (meth)acrylic means "acrylic" or "methacrylic", (meth)acrylate means "acrylate" or "methacrylate", and other similar expressions.

[0052] The carboxyl group-containing resin (b) is obtained by copolymerizing raw material monomers including at least a carboxyl group-containing ethylenically unsaturated monomer (a) and an ethylenically unsaturated monomer (d) copolymerizable with the carboxyl group-containing ethylenically unsaturated monomer (a).

[0053] The carboxyl group-containing resin (b) is a component that constitutes the main skeleton of the resin (A) represented by formula (1-1). The structural units k, l, and m are all structural units derived from the carboxyl group-containing resin (b).

[0054] As the ethylenically unsaturated monomer (d), one or more monomers that give the structural unit k upon polymerization are used. As the ethylenically unsaturated monomer (d), one or more monomers that give the structural unit l upon polymerization may be used together with the monomer that gives the structural unit k upon polymerization.

[0055] The ethylenically unsaturated monomer (d) that gives the structural unit k upon polymerization is an alkyl(meth)acrylate having 1 to 16 carbon atoms, and from the viewpoint of adjusting the peel strength of the adhesive composition, it preferably contains an alkyl(meth)acrylate having 2 to 16 carbon atoms, and more preferably contains an alkyl(meth)acrylate having 4 to 12 carbon atoms. Specific examples include methyl(meth)acrylate, ethyl(meth)acrylate, n-propyl(meth)acrylate, n-butyl(meth)acrylate, tert-butyl(meth)acrylate, isobutyl(meth)acrylate, 2-ethylhexyl(meth)acrylate, isodecyl(meth)acrylate, n-hexyl(meth)acrylate, isooctyl(meth)acrylate, lauryl(meth)acrylate, and the like. Among these, methyl (meth)acrylate, ethyl (meth)acrylate, n-butyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, or isooctyl (meth)acrylate is preferred.

[0056] Examples of the ethylenically unsaturated monomer (d) that gives the structural unit l upon polymerization include (meth)acrylates containing a cyclic alkyl group having 3 to 30 carbon atoms, and (meth)acrylates containing an aromatic group having 6 to 20 carbon atoms.

[0057] Examples of (meth)acrylates containing a cyclic alkyl group having 3 to 30 carbon atoms, which can be used as the ethylenically unsaturated monomer (d) that provides the structural unit l upon polymerization, include cyclohexyl (meth)acrylate, norbornyl (meth)acrylate, isobornyl (meth)acrylate, norbornanyl (meth)acrylate, dicyclopentenyl (meth)acrylate, dicyclopentenyloxyethyl (meth)acrylate, dicyclopentanyl (meth)acrylate, dicyclopentanyloxyethyl (meth)acrylate, and tricyclodecanedimethylol di(meth)acrylate. Among these, isobornyl (meth)acrylate is particularly preferred. When a cyclic alkyl (meth)acrylate is contained in the raw material monomer of the carboxyl group-containing resin (b), the heat resistance of an adhesive composition containing the resin (A) produced using the carboxyl group-containing resin (b) is improved.

[0058] Examples of aromatic group-containing (meth)acrylates having 6 to 20 carbon atoms that can be used as the ethylenically unsaturated monomer (d) that provides the structural unit l upon polymerization include benzyl (meth)acrylate, phenoxyethyl (meth)acrylate, phenoxypolyethylene glycol (meth)acrylate, phenoxypropyl (meth)acrylate, and phenoxypolypropylene glycol (meth)acrylate. Among these, benzyl (meth)acrylate is particularly preferred. When the carboxy group-containing resin (b) contains an aromatic group-containing (meth)acrylate as a raw material monomer, the heat resistance of an adhesive composition containing a resin (A) produced using the carboxy group-containing resin (b) is improved.

[0059] The raw material monomers of the carboxy group-containing resin (b) may contain, in addition to the carboxy group-containing ethylenically unsaturated monomer (a) and the ethylenically unsaturated monomer (d), a monomer copolymerizable with the carboxy group-containing ethylenically unsaturated monomer (a) other than the ethylenically unsaturated monomer (d).

[0060] Examples of the ethylenically unsaturated monomer copolymerizable with the carboxy group-containing ethylenically unsaturated monomer (a), other than the ethylenically unsaturated monomer (d), include alkoxyalkyl(meth)acrylates, alkoxy(poly)alkylene glycol (meth)acrylates, hydroxy group-containing (meth)acrylates, fluorinated alkyl(meth)acrylates, dialkylaminoalkyl(meth)acrylates, and (meth)acrylamides.

[0061] Examples of alkoxyalkyl (meth)acrylates include ethoxyethyl (meth)acrylate, methoxyethyl (meth)acrylate, butoxyethyl (meth)acrylate, 2-methoxyethoxyethyl (meth)acrylate, and 2-ethoxyethoxyethyl (meth)acrylate.

[0062] Examples of the alkoxy(poly)alkylene glycol (meth)acrylate include methoxydiethylene glycol (meth)acrylate, ethoxydiethylene glycol (meth)acrylate, and methoxydipropylene glycol (meth)acrylate.

[0063] Examples of hydroxy group-containing (meth)acrylates include 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, 4-hydroxybutyl (meth)acrylate, 1,3-butanediol (meth)acrylate, 1,4-butanediol (meth)acrylate, 1,6-hexanediol (meth)acrylate, and 3-methylpentanediol (meth)acrylate.

[0064] Examples of fluorinated alkyl (meth)acrylates include octafluoropentyl (meth)acrylate.

[0065] Examples of dialkylaminoalkyl (meth)acrylates include N,N-dimethylaminoethyl (meth)acrylate and N,N-diethylaminoethyl (meth)acrylate.

[0066] Examples of (meth)acrylamides include (meth)acrylamide, N-methyl(meth)acrylamide, N-ethyl(meth)acrylamide, N-propyl(meth)acrylamide, N-isopropylacrylamide, N-hexyl(meth)acrylamide, N,N-dimethyl(meth)acrylamide, N,N-diethyl(meth)acrylamide, (meth)acryloylmorpholine, and diacetone acrylamide.

[0067] Specific examples of the monomer other than the ethylenically unsaturated monomer (d) copolymerizable with the carboxy group-containing ethylenically unsaturated monomer (a) include acrylonitrile, methacrylonitrile, styrene, α-methylstyrene, vinyl acetate, vinyl propionate, vinyl stearate, vinyl chloride, vinylidene chloride, alkyl vinyl ethers, vinyl toluene, N-vinylpyridine, N-vinylpyrrolidone, itaconic acid dialkyl esters, fumaric acid dialkyl esters, allyl alcohol, hydroxybutyl vinyl ether, hydroxyethyl vinyl ether, 4-hydroxymethylcyclohexylmethyl vinyl ether, triethylene glycol monovinyl ether, diethylene glycol monovinyl ether, methyl vinyl ketone, allyl trimethylammonium chloride, and dimethylallyl vinyl ketone.

[0068] The method for producing the carboxyl group-containing resin (b) is not particularly limited. For example, the carboxyl group-containing resin (b) can be obtained by copolymerizing raw material monomers including the carboxyl group-containing ethylenically unsaturated monomer (a) and the ethylenically unsaturated monomer (d), which are components of the carboxyl group-containing resin (b), by a known polymerization method.

[0069] Specifically, the polymerization method may be a solution polymerization method, an emulsion polymerization method, a bulk polymerization method, a suspension polymerization method, an alternating copolymerization method, etc. Among these polymerization methods, in consideration of the addition reaction between the carboxy group-containing resin (b) obtained after polymerization and the alicyclic epoxy group-containing ethylenically unsaturated compound (c), it is preferable to use the solution polymerization method in terms of ease of reaction.

[0070] When the carboxyl group-containing resin (b) is produced by solution polymerization, a radical polymerization initiator and / or a solvent is used as necessary.

[0071] The radical polymerization initiator is not particularly limited and can be appropriately selected from known initiators. Examples of the radical polymerization initiator include 2,2'-azobis(isobutyronitrile), 2,2'-azobis(4-methoxy-2,4-dimethylvaleronitrile), 2,2'-azobis(2,4-dimethylvaleronitrile), 2,2'-azobis(2-methylbutyronitrile), 1,1'-azobis(cyclohexane-1-carbonitrile), 2,2'-azobis(2,4,4-trimethylpentane), and dimethyl-2,2'-azobis. and oil-soluble polymerization initiators such as azo-based polymerization initiators such as di-t-butyl peroxide, t-butyl hydroperoxide, di-t-butyl peroxide, t-butyl peroxybenzoate, dicumyl peroxide, 1,1-bis(t-butylperoxy)-3,3,5-trimethylcyclohexane, 1,1-bis(t-butylperoxy)cyclododecane, etc. These radical polymerization initiators may be used alone or in combination of two or more.

[0072] The amount of the radical polymerization initiator used is preferably 0.01 to 5 parts by mass, more preferably 0.02 to 4 parts by mass, and even more preferably 0.03 to 3 parts by mass, relative to 100 parts by mass of the total of the raw material monomers of the carboxy group-containing resin (b).

[0073] Various common solvents can be used as the polymerization solvent used in producing the carboxy group-containing resin (b). Examples of the solvent include esters such as ethyl acetate, n-propyl acetate, and n-butyl acetate; aromatic hydrocarbons such as toluene, xylene, and benzene; aliphatic hydrocarbons such as n-hexane and n-heptane; alicyclic hydrocarbons such as cyclohexane and methylcyclohexane; ketones such as methyl ethyl ketone and methyl isobutyl ketone; glycols such as ethylene glycol, propylene glycol, and dipropylene glycol; glycol ethers such as methyl cellosolve, propylene glycol monomethyl ether, and dipropylene glycol monomethyl ether; and glycol esters such as ethylene glycol diacetate and propylene glycol monomethyl ether acetate. These solvents may be used alone or in combination of two or more.

[0074] When producing the carboxy group-containing resin (b), the content of the carboxy group-containing ethylenically unsaturated monomer (a) in the raw material monomers containing the carboxy group-containing ethylenically unsaturated monomer (a), the ethylenically unsaturated monomer (d), and other monomers contained as needed is preferably 5 to 40 mass%, more preferably 7 to 30 mass%, and even more preferably 10 to 25 mass%. By setting the content of the carboxy group-containing ethylenically unsaturated monomer (a) in the raw material monomers within the above range, the adhesive strength of the adhesive layer obtained from the adhesive composition containing the resin (A) produced by the addition reaction of the carboxy group-containing resin (b) and the alicyclic epoxy group-containing ethylenically unsaturated compound (c) before irradiation with activation energy is improved.

[0075] The alicyclic epoxy group-containing ethylenically unsaturated compound (c) is an ethylenically unsaturated group-containing compound having an alicyclic epoxy group, and is a compound that provides a group represented by formula (1-2) or formula (1-3). Here, the alicyclic epoxy group means an epoxy group formed by bonding one oxygen atom to two adjacent carbon atoms on the ring of an alicyclic hydrocarbon compound.

[0076] The alicyclic epoxy group-containing ethylenically unsaturated compound (c) is used to add a group represented by formula (1-2') or formula (1-3'), which is a partial structure in the structural unit n of the resin (A) represented by formula (1-1). The group represented by formula (1-2') or formula (1-3') in the structural unit n in formula (1-1) is a group derived from the alicyclic epoxy group-containing ethylenically unsaturated compound (c).

[0077]

[0078] In formula (1-2') and formula (1-3'), q is an integer of 0 to 2. 9 is a hydrogen atom or a methyl group.

[0079] Examples of the alicyclic epoxy group-containing ethylenically unsaturated compound (c) include compounds represented by formula (1) or formula (2).

[0080]

[0081] In formula (1), R 9 is a hydrogen atom or a methyl group. q is an integer of 0 to 2. In formula (2), R 9 is a hydrogen atom or a methyl group. q is an integer of 0 to 2.

[0082] In formula (1), R 9 is a hydrogen atom (-H) or a methyl group (-CH 3 ) where q is an integer of 0 to 2, and q is preferably 1.

[0083] In formula (2), R 9 is a hydrogen atom (-H) or a methyl group (-CH 3 ) where q is an integer of 0 to 2, and q is preferably 1.

[0084] The alicyclic epoxy group-containing ethylenically unsaturated compound (c) is preferably a compound represented by formula (1), and more preferably 3,4-epoxycyclohexylmethyl(meth)acrylate. The alicyclic epoxy group-containing ethylenically unsaturated compound (c) may be used alone or in combination of two or more.

[0085] The resin (A) can be produced by subjecting the carboxy group of the carboxy group-containing resin (b) to an addition reaction with the alicyclic epoxy group of the alicyclic epoxy group-containing ethylenically unsaturated monomer (c).

[0086] Resin (A) is preferably produced by addition reaction of 0.2 to 0.99 mol, more preferably 0.3 to 0.95 mol, and even more preferably 0.6 to 0.95 mol of alicyclic epoxy group-containing ethylenically unsaturated compound (c) per mol of carboxy group in carboxy group-containing resin (b). An adhesive composition containing resin (A) obtained by using carboxy group-containing resin (b) and alicyclic epoxy group-containing ethylenically unsaturated compound (c) in the above ratio exhibits sufficient adhesion to adherends before activation energy irradiation, and exhibits reduced adhesion and superior removability after activation energy irradiation. Furthermore, this adhesive composition does not exhibit increased adhesion even when heated to a high temperature before activation energy irradiation and then returned to room temperature. It exhibits excellent removability after activation energy irradiation and effectively prevents adhesive residue on adherends after peeling.

[0087] The temperature of the addition reaction in producing Resin (A) is preferably 80 to 130°C, and more preferably 90 to 120°C. When the temperature of the addition reaction is 80°C or higher, a sufficient reaction rate can be obtained. When the temperature of the addition reaction is 130°C or lower, crosslinking of double bonds due to thermal radical polymerization can be prevented, preventing the formation of gelled products.

[0088] In the addition reaction in producing the resin (A), a known catalyst can be used as needed. Examples of the catalyst include tertiary amines such as triethylamine, tributylamine, dimethylbenzylamine, 1,8-diazabicyclo[5,4,0]undec-7-ene, 1,5-diazabicyclo[4,3,0]non-5-ene, and 1,4-diazabicyclo[2,2,2]octane; quaternary ammonium salts such as tetramethylammonium chloride, tetramethylammonium bromide, and tetrabutylammonium bromide; alkyl ureas such as tetramethylurea; alkyl guanidines such as tetramethylguanidine; and phosphine compounds such as triphenylphosphine, dimethylphenylphosphine, tricyclohexylphosphine, tributylphosphine, tris(4-methylphenyl)phosphine, tris(4-methoxyphenyl)phosphine, tris(2,6-dimethylphenyl)phosphine, tris(2,6-dimethoxyphenyl)phosphine, tris(2,4,6-trimethylphenyl)phosphine, and tris(2,4,6-trimethoxyphenyl)phosphine. Among these, it is preferable to use a phosphine compound as the catalyst in terms of reactivity.

[0089] The amount of the catalyst used in the addition reaction is preferably 0.01 to 30 parts by mass, more preferably 0.05 to 5 parts by mass, and even more preferably 0.1 to 2 parts by mass, per 100 parts by mass of the total of the carboxy group-containing resin (b) and the alicyclic epoxy group-containing ethylenically unsaturated monomer (c).

[0090] Furthermore, during the addition reaction, a gas having a polymerization-inhibiting effect may be introduced into the reaction system, or a polymerization inhibitor may be added. By introducing a gas having a polymerization-inhibiting effect into the reaction system, or by adding a polymerization inhibitor, gelation during the addition reaction can be prevented.

[0091] Examples of gases that have a polymerization-inhibiting effect include gases that contain oxygen to an extent that does not fall within the explosive range of the substances in the system, such as air.

[0092] As the polymerization inhibitor, known ones can be used, and there are no particular limitations, but examples thereof include 4-methoxyphenol, hydroquinone, methoquinone, 2,6-di-t-butylphenol, 2,2'-methylenebis(4-methyl-6-t-butylphenol), phenothiazine, etc. These polymerization inhibitors may be used alone or in combination of two or more.

[0093] The amount of polymerization inhibitor used is preferably 0.005 to 5 parts by mass, more preferably 0.03 to 3 parts by mass, and most preferably 0.05 to 1.5 parts by mass, per 100 parts by mass of the total of the carboxy group-containing resin (b) and the alicyclic epoxy group-containing ethylenically unsaturated monomer (c). If the amount of polymerization inhibitor is too small, the polymerization inhibitor effect may be insufficient. On the other hand, if the amount of polymerization inhibitor is too large, the exposure sensitivity of the resin (A) may decrease.

[0094] Furthermore, it is more preferable to use a gas having a polymerization inhibitor effect in combination with a polymerization inhibitor, since this allows the amount of polymerization inhibitor used to be reduced and the polymerization inhibitor effect to be enhanced.

[0095] The content of the resin (A) may be 70% by mass or more, 80% by mass or more, 90% by mass or more, 95% by mass or more, or 98% by mass or more based on the total amount of the adhesive composition (total amount of solids in the adhesive composition excluding the solvent).

[0096] Examples of the photopolymerization initiator (B) include benzophenone, benzil, benzoin, ω-bromoacetophenone, chloroacetone, acetophenone, 2,2-diethoxyacetophenone, 2,2-dimethoxy-2-phenylacetophenone, p-dimethylaminoacetophenone, p-dimethylaminopropiophenone, 2-chlorobenzophenone, 4,4'-dichlorobenzophenone, 4,4'-bisdiethylaminobenzophenone, Michler's ketone, benzoin methyl ether, benzoin isobutyl ether, and benzyl benzoate. carbonyl-based photopolymerization initiators such as benzoin-n-butyl ether, benzyl methyl ketal, 1-hydroxycyclohexyl phenyl ketone, 2-hydroxy-2-methyl-1-phenyl-propan-1-one, 1-(4-isopropylphenyl)-2-hydroxy-2-methylpropan-1-one, methyl benzoyl formate, 2,2-diethoxyacetophenone, 4-N,N'-dimethylacetophenone, and 2-methyl-1-[4-(methylthio)phenyl]-2-morpholinopropan-1-one.

[0097] Examples of the photopolymerization initiator (B) include sulfide-based photopolymerization initiators such as diphenyl disulfide, dibenzyl disulfide, tetraethylthiuram disulfide, and tetramethylammonium monosulfide; acylphosphine oxides such as 2,4,6-trimethylbenzoyldiphenylphosphine oxide and 2,4,6-trimethylbenzoylphenylethoxyphosphine oxide; quinone-based photopolymerization initiators such as benzoquinone and anthraquinone; sulfochloride-based photopolymerization initiators; and thioxanthone-based photopolymerization initiators such as thioxanthone, 2-chlorothioxanthone, and 2-methylthioxanthone.

[0098] Among these photopolymerization initiators (B), 1-hydroxycyclohexyl phenyl ketone and / or 2,4,6-trimethylbenzoyldiphenylphosphine oxide are preferably used in terms of solubility in the adhesive composition. The photopolymerization initiators (B) may be used alone or in combination of two or more.

[0099] The amount of photopolymerization initiator (B) is preferably 0.1 to 5.0 parts by mass, more preferably 0.5 to 2.0 parts by mass, per 100 parts by mass of resin (A). When the content of photopolymerization initiator (B) per 100 parts by mass of resin (A) is 0.1 part by mass or more, the adhesive composition cures at a sufficiently fast curing rate upon irradiation with activation energy, and the adhesive strength of the adhesive composition after irradiation with activation energy is sufficiently small, which is preferable. When the content of photopolymerization initiator (B) is 5.0 parts by mass or less, when an adhesive layer containing the adhesive composition is attached to an adherend and then peeled off, the adhesive layer is less likely to remain on the adherend.

[0100] The adhesive composition may contain a crosslinking agent (C) in addition to the resin (A) and the photopolymerization initiator (B). By containing the crosslinking agent (C), the adhesive composition has a better balance between the adhesive strength before and after irradiation with activation energy.

[0101] The crosslinking agent (C) is not particularly limited, but is preferably a compound having two or more functional groups reactive with the hydroxyl group of the structural unit n, or with the hydroxyl group of the structural unit n and the carboxyl group of the structural unit m.

[0102] Examples of the crosslinking agent (C) include isocyanate compounds such as 2,4-tolylene diisocyanate, 2,6-tolylene diisocyanate, hydrogenated tolylene diisocyanate, 1,3-xylylene diisocyanate, 1,4-xylylene diisocyanate, diphenylmethane-4,4-diisocyanate, isophorone diisocyanate, 1,3-bis(N,N'-diglycidylaminomethyl)cyclohexane, 1,3-bis(isocyanatomethyl)cyclohexane, an isocyanurate of hexamethylene diisocyanate, tetramethylxylylene diisocyanate, 1,5-naphthalene diisocyanate, a tolylene diisocyanate adduct of trimethylolpropane, a xylylene diisocyanate adduct of trimethylolpropane, triphenylmethane triisocyanate, and methylenebis(4-phenylmethane)triisocyanate; Epoxy compounds such as bisphenol A-epichlorohydrin type epoxy resins, N,N'-[1,3-phenylenebis(methylene)]bis[bis(oxiran-2-ylmethyl)amine], ethylene glycol diglycidyl ether, polyethylene glycol diglycidyl ether, glycerin diglycidyl ether, glycerin triglycidyl ether, 1,6-hexanediol diglycidyl ether, trimethylolpropane triglycidyl ether, sorbitol polyglycidyl ether, polyglycerol polyglycidyl ether, pentaerythritol polyglycidyl erythritol, and diglycerol polyglycidyl ether; Examples of the aziridine-based compounds include tetramethylolmethane-tri-β-aziridinylpropionate, trimethylolpropane-tri-β-aziridinylpropionate, N,N'-diphenylmethane-4,4'-bis(1-aziridinecarboxamide), and N,N'-hexamethylene-1,6-bis(1-aziridinecarboxamide); and melamine-based compounds such as hexamethoxymethylmelamine, hexaethoxymethylmelamine, hexapropoxymethylmelamine, hexaptoxymethylmelamine, hexapentyloxymethylmelamine, and hexahexyloxymethylmelamine.

[0103] Among these, it is preferable to use an epoxy compound and / or an isocyanate compound as the crosslinking agent (C) because they have good reactivity with the resin (A). The crosslinking agent (C) may be used alone or in combination of two or more kinds.

[0104] The content of the crosslinking agent (C) is preferably 0.05 to 10 parts by mass, more preferably 0.1 to 5 parts by mass, and even more preferably 0.1 to 1.0 parts by mass, per 100 parts by mass of the resin (A). When the content of the crosslinking agent (C) per 100 parts by mass of the resin (A) is 0.05 parts by mass or more, a three-dimensional crosslinked structure is sufficiently formed in the adhesive composition. As a result, the adhesive strength of the adhesive composition after irradiation with activation energy is sufficiently small, which is preferable. When the content of the crosslinking agent (C) per 100 parts by mass of the resin (A) is 10 parts by mass or less, the adhesive strength of the adhesive composition before irradiation with activation energy is good.

[0105] The adhesive composition may contain other components in addition to the resin (A), the photopolymerization initiator (B), and the crosslinking agent (C), as necessary. Examples of other components include an adhesion promoter and various additives.

[0106] Any conventionally known adhesion (tack)-imparting agent can be used without any particular limitation. Examples of adhesion-imparting agents include terpene resins, phenolic resins, rosin resins, aliphatic petroleum resins, aromatic petroleum resins, copolymerized petroleum resins, alicyclic petroleum resins, xylene resins, epoxy resins, polyamide resins, ketone resins, and elastomer resins. These adhesion-imparting agents may be used alone or in combination of two or more.

[0107] When the adhesive composition contains an adhesion promoter, the content thereof is preferably 30 parts by mass or less, and more preferably 5 to 20 parts by mass, per 100 parts by mass of the resin (A).

[0108] Examples of additives include plasticizers, surface lubricants, leveling agents, softeners, antioxidants, antiaging agents, light stabilizers, ultraviolet absorbers, polymerization inhibitors, benzotriazole-based light stabilizers, phosphate ester-based and other flame retardants, and antistatic agents such as surfactants.

[0109] The adhesive composition can be used as a coating liquid (adhesive varnish) containing a solvent for coating the adhesive composition.

[0110] Examples of the solvent that can be used include organic solvents such as methyl ethyl ketone, methyl isobutyl ketone, acetone, ethyl acetate, n-propyl acetate, tetrahydrofuran, dioxane, cyclohexanone, n-hexane, toluene, xylene, n-propanol, isopropanol, etc. These solvents may be used alone or in combination of two or more.

[0111] The adhesive composition can be produced by a conventionally known method, for example, by mixing and stirring the resin (A) and the photopolymerization initiator (B), and, if necessary, the crosslinking agent (C), the adhesion promoter, and various additives in a solvent using a conventionally known method.

[0112] The adhesive layer 2 can be produced, for example, by the following method. First, the adhesive composition described above is dissolved or dispersed in a solvent to prepare a coating liquid (adhesive varnish). Next, the coating liquid (adhesive varnish) is applied to a substrate film and dried by heating to form an adhesive layer. Another method for producing an adhesive layer involves applying the coating liquid (adhesive varnish) to a release film and drying by heating to form an adhesive layer. Thereafter, a release film having an adhesive layer is placed on a substrate film with the adhesive layer side facing the substrate, and the adhesive layer is transferred (transferred) onto the substrate.

[0113] The coating liquid (adhesive varnish) can be applied to the substrate film (or release film) by any known method, including, for example, a method using a conventional coater such as a gravure roll coater, a reverse roll coater, a kiss roll coater, a dip roll coater, a bar coater, a knife coater, a spray coater, a comma coater, or a direct coater.

[0114] The thickness of the adhesive layer 2 may be 1 to 100 μm, 2 to 80 μm, or 5 to 50 μm.

[0115] 2, the semiconductor chip C is pushed up by a push-up jig 42 to peel the semiconductor chip C from the adhesive layer 2, and then the semiconductor chip C is picked up by suction with a suction collet 44. If the adhesive layer 2 is one whose adhesive strength is reduced by irradiation with activation energy, the adhesive layer 2 is irradiated with activation energy rays prior to picking up. The irradiation dose is, for example, 10 to 1000 mJ / cm. 2 and 100 to 700 mJ / cm 2 or 200 to 500 mJ / cm 2 may be.

[0116] According to the cleaning method of this embodiment, cleaning the semiconductor chip C on the adhesive film 5 with a chemical solution can remove foreign matter adhering to the semiconductor chip C to a greater extent than cleaning with water. Furthermore, according to the cleaning method of this embodiment, detachment of the semiconductor chip from the surface of the adhesive film can be prevented during the cleaning process of the semiconductor chip with a chemical solution. By using a highly cleaned semiconductor chip C, a semiconductor device with excellent connection reliability can be manufactured. This cleaning method is also useful in that it can be efficiently implemented in the semiconductor manufacturing process. That is, according to this cleaning method, the highly cleaned chemical solution cleaning is performed on the surface 5f of the adhesive film 5 with the dicing ring DR attached to the adhesive film 5. Therefore, the semiconductor chip C can be picked up after cleaning and directly subjected to the next process. The semiconductor chip C may be cleaned with pure water before and / or after the chemical cleaning.

[0117] <Method of Manufacturing Semiconductor Device> [First Embodiment] A method of manufacturing a semiconductor device, including a step of carrying out the above-described cleaning method, will be specifically described. The method of manufacturing a semiconductor device according to the first embodiment includes the following steps: (1a) forming a photoresist Rp on a workpiece Pw including a semiconductor wafer W having a first surface f1 and a second surface f2, and a circuit layer Lc formed on the first surface f1, so as to cover the circuit layer Lc (see FIG. 3(a)); (2a) forming a groove G1 in the photoresist Rp that reaches the circuit layer Lc by exposing and developing the photoresist Rp (see FIG. 3(b)); (3a) cutting the circuit layer Lc through the groove G1 by plasma dicing and half-cutting the semiconductor wafer W to form a groove G2 (see FIG. 3(c)); (4a) peeling the photoresist Rp from the circuit layer Lc (see FIG. 4(a)); and (5a) applying a backgrinding tape T to cover the circuit layer Lc. BG (6a) A step of attaching the back-grinding tape T by grinding the semiconductor wafer W from the second surface f2 side (see FIG. 4(b)). BG (7a) A step of attaching a plurality of semiconductor chips C to the surface of the backgrind tape T (see FIG. 4(c)). BG (8a) A step of transferring the semiconductor chips C from the surface of the semiconductor chip C to the surface 5f of the adhesive film 5 and attaching a dicing ring DR to the surface 5f so as to surround the semiconductor chips C (see FIG. 1). (9a) A step of performing a method for cleaning the semiconductor chips C. (9b) A step of bonding the cleaned semiconductor chips C to an adherend (see FIG. 6).

[0118] The workpiece Pw shown in FIG. 3( a) includes a semiconductor wafer W and a circuit layer Lc. The thickness of the semiconductor wafer W is, for example, 5 to 775 μm and may be 50 to 300 μm. The diameter of the semiconductor wafer W is, for example, 50 to 300 mm and may be 150 to 300 mm. The circuit layer Lc has various electronic circuits (e.g., integrated circuits and power supply circuits) formed thereon depending on the application of the semiconductor device. The thickness of the circuit layer Lc is, for example, 0.01 to 50 μm and may be 0.1 to 10 μm. The photoresist Rp is made of a photosensitive insulating material, and a groove G1 can be formed in the photoresist Rp by a photolithography process ( FIG. 3( b)).

[0119] The groove G2 shown in FIG. 3(c) penetrates the circuit layer Lc and extends from the first surface f1 to the inside of the semiconductor wafer W. The groove G2 does not reach the second surface f2. The groove G2 is formed by plasma dicing. One known type of plasma dicing is a process called the Bosch process. In the Bosch process, C 4 F 8 A passivation step using plasma and SF 6 The silicon constituting the semiconductor wafer W is etched by alternating a passivation step with a plasma etching step. Specifically, in the passivation step, a fluorocarbon polymer film (hereinafter simply referred to as the "polymer film") is isotropically formed on the entire inner surface of the groove G1. Then, in the etching step, a bias is applied to the semiconductor wafer W, and the polymer film at the bottom of the groove G1 is removed by ion etching. Meanwhile, the polymer film on the sidewalls of the groove G1 remains and forms the sidewalls of the groove G1. Only the silicon exposed at the bottom of the groove G1 from which the polymer film has been removed is etched by fluorine radicals. By repeating these steps, the groove G2 is formed. The side surfaces of the groove G2 thus formed are covered with the polymer film. If the polymer film peels off in subsequent processes, it can become a foreign substance that reduces the reliability of the semiconductor device. The circuit layer Lc is divided by the groove G2, thereby forming multiple circuit layers C1.

[0120] After the step (6a), the thickness of the die C2 (the thickness of the semiconductor chip C excluding the circuit layer C1) is, for example, 5 to 775 μm, and may be 50 to 300 μm. Grinding debris generated in the step (6a) can also become foreign matter that reduces the reliability of the semiconductor device.

[0121] After the above step (7a), before carrying out the cleaning method for the semiconductor chips C, tension may be applied to the adhesive film 5 to widen the gap between two adjacent semiconductor chips C. That is, as shown in FIG. 5 , tension is applied to the adhesive film 5 by pushing up the inside of the dicing ring DR with the ring Ra from the base film 1 side of the adhesive film 5. This makes it easier to supply chemicals to the side surfaces of the semiconductor chips C in the above step (8a), allowing the polymer film adhering to the side surfaces to be sufficiently removed with the chemicals. To remove the polymer film, it is preferable to use an HFE (hydrofluoroether)-based or HAD (hydroxylamine)-based chemical. On the other hand, to remove grinding debris, it is preferable to use the above-mentioned solvent-based, acid-based, or alkaline-based chemicals.

[0122] Fig. 6 is a cross-sectional view schematically showing a state in which a semiconductor chip C is bonded to a substrate 10 (adherend) after cleaning. For example, a die bonding film (not shown) is used to bond the semiconductor chip C to the substrate 10. As shown in Fig. 7, when multiple semiconductor chips C are stacked, the object (adherend) to which the second and subsequent semiconductor chips C are bonded is the semiconductor chip C in the lower layer. A semiconductor device 30 shown in Fig. 8 is fabricated through a process of connecting the substrate 10 and the multiple semiconductor chips C with wires w, and a process of sealing the multiple semiconductor chips C with a resin material 20.

[0123] Second Embodiment A method for manufacturing a semiconductor device according to a second embodiment includes the following steps: (1b) placing a workpiece Pw in a region R within a dicing ring DR attached to the surface 5f of an adhesive film 5 (see FIG. 9(a)); (2b) forming a photoresist Rp to cover the circuit layer Lc (see FIG. 9(b)); (3b) forming grooves G3 in the photoresist that reach the circuit layer Lc by exposing and developing the photoresist Rp (see FIG. 10(a)); (4b) cutting the circuit layer Lc and the semiconductor wafer W through the grooves G3 by plasma dicing to obtain multiple semiconductor chips C on the surface 5f of the adhesive film 5 (see FIG. 10(b)); (5b) performing a method for cleaning the semiconductor chips C (see FIGS. 1 and 2); and (6b) bonding the cleaned semiconductor chips C to an adherend (see FIG. 6).

[0124] This embodiment will be described mainly with respect to the differences from the first embodiment. In this embodiment, steps (2b) to (5b) are performed on the surface of the adhesive film 5 to which the dicing ring DR is attached. After step (4b), as shown in FIG. 10(b), photoresist Rp remains on the upper surface of the semiconductor chip C. The photoresist Rp may be removed using a resist remover prior to step (5b), or may be removed using a chemical solution in step (5b). A solvent-based chemical solution (especially NMP) is preferably used to remove the photoresist Rp. The groove G4 shown in FIG. 10(b) penetrates the circuit layer Lc and the semiconductor wafer W and reaches the surface 5f of the adhesive film 5. Like the groove G2 described above, the groove G4 may be formed by plasma dicing. As with the first embodiment, the polymer film resulting from plasma dicing may be removed using an HFE-based or HDA-based chemical solution.

[0125] Third Embodiment A method for manufacturing a semiconductor device according to a third embodiment includes the following steps: (1c) placing a workpiece Pw in a region R within a dicing ring DR attached to the surface 5f of an adhesive film 5 (see FIG. 11(a)); (2c) forming a protective film Mp so as to cover the circuit layer Lc (see FIG. 11(b)); (3c) cutting the protective film Mp and the circuit layer Lc with a laser to form grooves G5 that reach the first surface f1 of the semiconductor wafer W (see FIG. 12(a)); (4c) cutting the semiconductor wafer W through the grooves G5 by plasma dicing to obtain multiple semiconductor chips C on the surface 5f of the adhesive film 5 (see FIG. 12(b)); (5c) performing a method for cleaning the semiconductor chips C (see FIGS. 1 and 2); and (6c) bonding the cleaned semiconductor chips C to an adherend (see FIG. 6).

[0126] This embodiment will be described mainly with respect to differences from the first and second embodiments. In this embodiment, a protective film Mp is formed in the above-described step (2c). The protective film Mp is intended to prevent damage to the circuit layer Lc. The protective film Mp is composed of, for example, a water-soluble resin and can be formed by applying a coating containing the resin to the surface of the workpiece Pw. The protective film Mp remains on the upper surface of the semiconductor chip C after the above-described step (4c) (see FIG. 12(b)). The protective film Mp is removed with pure water in the above-described step (5c). The groove G6 shown in FIG. 12(b) penetrates the semiconductor wafer W and reaches the surface 5f of the adhesive film 5. The groove G6 may be formed by plasma dicing, similar to the above-described groove G2. The polymer film resulting from plasma dicing may be removed using an HFE-based or HDA-based chemical solution, similar to the first embodiment.

[0127] In this embodiment, the grooves G6 may be formed by blade dicing instead of plasma dicing. For example, if the circuit layer Lc includes a low-k film, the grooves G5 are formed by cutting the circuit layer Lc with a laser to prevent peeling of the low-k film, which has relatively low mechanical strength. On the other hand, the subsequent process of cutting the semiconductor wafer W (the process of forming the grooves G6) may be performed by blade dicing. A low-k film is a film composed of a material with a low dielectric constant and is primarily used as an interconnect layer, i.e., an insulating material between metal wiring that electrically connects different electronic components within a chip. The use of a low-k film can reduce parasitic capacitance between wiring, thereby improving signal transmission speed and suppressing crosstalk between wiring. The process of forming grooves in the circuit layer Lc with a laser is called laser grooving.

[0128] [Fourth Embodiment] A method for manufacturing a semiconductor device according to a fourth embodiment includes the following steps: (1d) a step of placing a workpiece Pw in a region R within a dicing ring DR attached to the surface 5f of an adhesive film 5 (see FIG. 13(a)); (2d) a step of cutting the workpiece Pw by blade dicing to obtain a plurality of semiconductor chips C on the surface 5f of the adhesive film 5 (see FIG. 13(b)); (3d) a step of performing a method for cleaning the semiconductor chips C (see FIGS. 1 and 2); and (4d) a step of bonding the cleaned semiconductor chips C to an adherend (see FIG. 6).

[0129] This embodiment will be described mainly in terms of differences from the first, second, and third embodiments. In this embodiment, in step (2d) above, the workpiece Pw is divided into multiple semiconductor chips C by blade dicing. The grooves G7 formed by blade dicing penetrate the circuit layer Lc and the semiconductor wafer W and reach the surface 5f of the adhesive film 5. The grinding debris generated in step (2d) above can become foreign matter that reduces the reliability of the semiconductor device. The above-mentioned solvent-based, acid-based, or alkaline-based chemical solution is preferably used to remove the grinding debris generated by blade dicing. According to this embodiment, the steps of forming a photoresist or a protective film are not required, and the steps of removing them are also not required.

[0130] Fifth Embodiment A method for manufacturing a semiconductor device according to a fifth embodiment includes the following steps: (1e) placing a workpiece Pw in a region R within a dicing ring DR attached to the surface 5f of an adhesive film 5 (see FIG. 14(a)); (2e) cutting the circuit layer Lc with a laser to form grooves G8 that reach the first surface f1 of the semiconductor wafer W (see FIG. 14(b)); (3e) cutting the semiconductor wafer W through the grooves G8 with blade dicing to obtain multiple semiconductor chips C on the surface 5f of the adhesive film 5 (see FIG. 14(c)); (4e) performing a method for cleaning the semiconductor chips (see FIGS. 1 and 2); and (5e) bonding the cleaned semiconductor chips C to an adherend (see FIG. 6).

[0131] This embodiment will be described mainly in terms of differences from the fourth embodiment. In this embodiment, in step (2e), the circuit layer Lc is cut using a laser. Because a laser is used to cut the circuit layer Lc, peeling of the low-k film can be suppressed even if the circuit layer Lc includes a low-k film. Next, the semiconductor wafer W is cut using blade dicing. The groove G9 shown in FIG. 14(c) penetrates the semiconductor wafer W and reaches the surface 5f of the adhesive film 5. Grinding debris generated in steps (2e) and (3e) can become foreign matter that reduces the reliability of the semiconductor device. According to this embodiment, grinding debris generated in these steps can be removed in the subsequent step (4e). It is preferable to use the above-mentioned solvent-based, acid-based, or alkaline-based chemical solution as the chemical solution.

[0132] Although the embodiments of the present disclosure have been described in detail above, the present disclosure is not limited to the above embodiments. For example, in the second, third, fourth, and fifth embodiments, the semiconductor wafer W is used as is without backgrinding. However, the semiconductor wafer W may be backgrinded before being placed in the region R of the adhesive film 5. That is, in the above-described certain embodiments, before placing the workpiece Pw in the region R of the adhesive film 5, the semiconductor wafer W may be ground from the second surface f2 side with a backgrind tape attached to the workpiece Pw so as to cover the circuit layer Lc. In this case, the circuit layer Lc may also include a low-k film.

[0133] 1...base material film, 2...adhesive layer, 5...adhesive film, 5f...surface of adhesive film, 10...substrate (adherend), 20...resin material, 30...semiconductor device, 42...push-up jig, 44...suction collet, C...semiconductor chip, C1...(divided) circuit layer, C2...die, DR...dicing ring, f1...first surface, f2...second surface, G1, G2, G3, G4, G5, G6, G7, G8, G9...groove portion, Lc...circuit layer, Mp...protective film, Pw...workpiece, R...region, Rp...photoresist, T BG ...backgrinding tape, W...semiconductor wafer, w...wire.

Claims

1. A method for cleaning semiconductor chips, comprising: (a) a step of cleaning a plurality of semiconductor chips arranged in an area on the surface of an adhesive film and within a dicing ring affixed to the surface, with a chemical solution; and (b) a step of picking up the semiconductor chips from the surface after cleaning, wherein the adhesive film comprises a base film and an adhesive layer formed on the surface of the base film, the adhesive layer contains an adhesive composition comprising a resin (A) represented by the following formula (1-1) and a photopolymerization initiator (B), and the chemical solution is a type of chemical solution selected from the group consisting of solvent-based, acid-based, and alkaline-based chemical solutions. [In formula (1-1), k, l, m, and n represent the molar composition ratio when k+l+m+n=100. k is greater than 0 and equal to or less than 92. l is 0 to 50. m is greater than 0 and equal to or less than 90. The sum of k, l, and m is 65 to 95. n is 5 to 35. R 1 , R 2 , R 3 , and R 4 is a hydrogen atom or a methyl group. 5 is an alkyl group having 1 to 16 carbon atoms. 6 R is an alicyclic hydrocarbon group having 3 to 30 carbon atoms or an aromatic hydrocarbon group having 6 to 20 carbon atoms. 7 is a hydrogen atom or -(CH 2 ) j -COOH (wherein j is 1 or 2). 8 is a group represented by the following formula (1-2) or the following formula (1-3). [In formula (1-2) and formula (1-3), p and q are integers of 0 to 2. s is 0 when p is 0, and is 1 when p is 1 or 2. R 9 is a hydrogen atom or a methyl group.

2. A method for manufacturing a semiconductor device, comprising the steps of carrying out the method for cleaning a semiconductor chip according to claim 1, comprising the steps of: forming a photoresist on a workpiece comprising a semiconductor wafer having a first surface and a second surface, and a circuit layer formed on the first surface, so as to cover the circuit layer; exposing and developing the photoresist to form a groove in the photoresist that reaches the circuit layer; cutting the circuit layer through the groove by plasma dicing and half-cutting the semiconductor wafer; peeling the photoresist from the circuit layer; applying a backgrind tape so as to cover the circuit layer; obtaining a plurality of semiconductor chips on the surface of the backgrind tape by grinding the semiconductor wafer from the second surface side; transferring the plurality of semiconductor chips from the surface of the backgrind tape onto the surface of the adhesive film, and applying a dicing ring on the surface of the adhesive film so as to surround the plurality of semiconductor chips; carrying out the method for cleaning a semiconductor chip according to claim 1; and bonding the cleaned semiconductor chips to an adherend. A method for manufacturing a semiconductor device comprising the steps of:

3. A method for manufacturing a semiconductor device comprising the step of carrying out the method for cleaning semiconductor chips as defined in claim 1, the method for manufacturing a semiconductor device comprising the steps of: arranging a workpiece comprising a semiconductor wafer having a first surface and a second surface, and a circuit layer formed on the first surface, in an area on the surface of the adhesive film and within a dicing ring affixed to the surface; forming a photoresist so as to cover the circuit layer; forming grooves in the photoresist that reach the circuit layer by subjecting the photoresist to exposure and development treatments; cutting the circuit layer and the semiconductor wafer through the grooves by plasma dicing to obtain a plurality of semiconductor chips on the surface of the adhesive film; carrying out the method for cleaning semiconductor chips as defined in claim 1; and bonding the semiconductor chips after cleaning to an adherend.

4. A method for manufacturing a semiconductor device comprising the step of carrying out the method for cleaning semiconductor chips as defined in claim 1, the method for manufacturing a semiconductor device comprising the steps of: arranging a workpiece comprising a semiconductor wafer having a first surface and a second surface, and a circuit layer formed on the first surface, in an area on the surface of the adhesive film and within a dicing ring affixed to the surface; forming a protective film to cover the circuit layer; cutting the protective film and the circuit layer with a laser to form grooves reaching the first surface; cutting the semiconductor wafer through the grooves by plasma dicing to obtain a plurality of semiconductor chips on the surface of the adhesive film; carrying out the method for cleaning semiconductor chips as defined in claim 1; and bonding the cleaned semiconductor chips to an adherend.

5. The method for manufacturing a semiconductor device according to claim 4, wherein the step of carrying out said cleaning method includes removing said protective film.

6. A method for manufacturing a semiconductor device comprising the step of carrying out the method for cleaning a semiconductor chip described in claim 1, the method for manufacturing a semiconductor device comprising the steps of: arranging a workpiece comprising a semiconductor wafer having a first surface and a second surface, and a circuit layer formed on the first surface, in an area on the surface of the adhesive film and within a dicing ring affixed to the surface; cutting the workpiece by blade dicing to obtain a plurality of semiconductor chips on the surface of the adhesive film; carrying out the method for cleaning a semiconductor chip described in claim 1; and bonding the semiconductor chips after cleaning to an adherend.

7. A method for manufacturing a semiconductor device comprising the steps of: carrying out the method for cleaning a semiconductor chip according to claim 1; the method for manufacturing a semiconductor device comprising the steps of: arranging a workpiece comprising a semiconductor wafer having a first surface and a second surface, and a circuit layer formed on the first surface, in an area on the surface of the adhesive film and within a dicing ring affixed to the surface; dividing the circuit layer into a plurality of individual circuit layers by forming grooves in the circuit layer with a laser; cutting the semiconductor wafer through the grooves by blade dicing to obtain a plurality of semiconductor chips on the surface of the adhesive film; carrying out the method for cleaning a semiconductor chip according to claim 1; and bonding the semiconductor chips after cleaning to an adherend.

8. A method for manufacturing a semiconductor device comprising the step of carrying out the method for cleaning semiconductor chips as defined in claim 1, the method for manufacturing a semiconductor device comprising the steps of: arranging a workpiece comprising a semiconductor wafer having a first surface and a second surface, and a circuit layer formed on the first surface, in an area on the surface of the adhesive film and within a dicing ring affixed to the surface; forming a protective film to cover the circuit layer; cutting the protective film and the circuit layer with a laser to form grooves reaching the first surface; cutting the semiconductor wafer through the grooves by blade dicing to obtain a plurality of semiconductor chips on the surface of the adhesive film; carrying out the method for cleaning semiconductor chips as defined in claim 1; and bonding the cleaned semiconductor chips to an adherend.

9. The method for manufacturing a semiconductor device according to claim 8, wherein the step of carrying out the cleaning method includes removing the protective film.

10. The method for manufacturing a semiconductor device according to any one of claims 7 to 9, wherein the circuit layer formed on the first surface of the semiconductor wafer includes a low-k film.

11. A method for manufacturing a semiconductor device according to any one of claims 3 to 9, further comprising the step of grinding the semiconductor wafer from the second surface side with a backgrind tape attached to the workpiece so as to cover the circuit layer, before placing the workpiece in the region on the surface of the adhesive film.

Citation Information

Patent Citations

  • Method of manufacturing semiconductor device

    JP2010093273A

  • Semiconductor device manufacturing method

    JP2012169484A

  • Adhesive tape for semiconductor wafer processing, manufacturing method thereof, and method for processing semiconductor wafer

    JP2015185691A

  • Processing method for wafer

    JP2016039186A

  • Method for manufacturing element chip

    JP2018200957A