Multilayer structure, molded body, container, food container, and method for producing multilayer structure
The multilayer structure with an extruded and uniaxially stretched EVOH resin layer and an inorganic vapor-deposited layer addresses the issue of insufficient oxygen barrier properties in existing multilayer structures, achieving improved gas barrier performance for applications like food packaging.
Patent Information
- Application Number
- PCT/JP2024/016399
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-05-01
- Filing Date
- 2024-04-26
- Publication Date
- 2024-11-07
AI Technical Summary
Existing multilayer structures with EVOH resin layers, especially those using biaxially stretched films or multiple EVOH resins with different ethylene unit contents, often exhibit insufficient gas barrier properties, particularly oxygen barrier properties.
A multilayer structure is developed with an extruded and uniaxially stretched EVOH resin layer having a single ethylene unit content, combined with an inorganic vapor-deposited layer made of inorganic oxide or nitride, which is laminated onto the EVOH resin layer to enhance barrier properties.
The solution significantly improves the oxygen barrier properties of the multilayer structure, making it suitable for various applications including food packaging, by ensuring the EVOH resin layer has a single ethylene unit content and an inorganic vapor-deposited layer is applied, resulting in enhanced gas barrier performance.
Smart Images

Figure JPOXMLDOC01-APPB-T000001
Abstract
Description
Multilayer structure, molded body, container, food container, and method for manufacturing multilayer structure
[0001] The present invention relates to a multilayer structure, and more particularly to a multilayer structure having excellent barrier properties.
[0002] Ethylene-vinyl alcohol copolymers (hereinafter sometimes referred to as "EVOH resins") have very strong intermolecular forces due to hydrogen bonds between hydroxyl groups present in polymer side chains. Therefore, they are highly crystalline, and the intermolecular forces are strong even in the amorphous portions. Therefore, films using EVOH resins are difficult for gas molecules to pass through, and exhibit excellent gas barrier properties. Therefore, EVOH resins are used as gas barrier layers to impart gas barrier properties to multilayer structures such as films and containers in a wide range of fields, such as food packaging.
[0003] For example, Patent Document 1 discloses an example of a gas barrier laminate in which a carbon-containing silicon oxide vapor-deposited film is formed on a biaxially stretched multilayer substrate having an EVOH resin surface resin layer, and Patent Document 2 discloses an example of a vapor-deposited multilayer film in which aluminum is vapor-deposited on a uniaxially stretched multilayer film made of two types of EVOH having different ethylene unit contents.
[0004] JP 2022-009162 A International Publication No. 2021 / 210606
[0005] In Patent Document 1, a carbon-containing silicon oxide vapor-deposited film is formed on a biaxially stretched multilayer substrate, but when a vapor-deposited film is formed using a biaxially stretched film or the like, the barrier property tends to be insufficient, leaving room for improvement. Also, in Patent Document 2, two types of EVOH resins with different ethylene unit contents are used, but vapor-deposited films using two types of EVOH resins with different ethylene unit contents tend to have insufficient barrier property, leaving room for improvement.
[0006] The present invention has been made in view of the above problems, and provides a multilayer structure having a layer containing an EVOH resin, which has excellent barrier properties, particularly oxygen barrier properties.
[0007] As a result of extensive research aimed at solving the above-mentioned problems, the present inventors have found that the barrier properties can be improved by laminating an inorganic vapor-deposited layer on a layer containing an extruded, uniaxially stretched EVOH resin having a single ethylene content.
[0008] That is, the present invention provides the following items [1] to [9]. [1] A multilayer structure comprising a layer (A) containing an EVOH resin and an inorganic vapor-deposited layer (B) adjacent to the layer (A), wherein the layer (A) is extrusion-molded and uniaxially stretched, and the EVOH resin has a single ethylene unit content. [2] The multilayer structure according to [1], wherein the inorganic vapor-deposited layer (B) comprises an inorganic oxide and / or an inorganic nitride. [3] The multilayer structure according to [1] or [2], wherein the stretching ratio of the layer (A) is 3 times or more. [4] The multilayer structure according to any one of [1] to [3], further comprising a layer (C) containing a thermoplastic resin. [5] The multilayer structure according to [4], wherein the thermoplastic resin comprises a polyolefin. [6] A molded article comprising the multilayer structure according to any one of [1] to [5]. [7] A container comprising the multilayer structure according to any one of [1] to [5]. [8] A food container comprising the multilayer structure according to any one of [1] to [5]. [9] A method for producing a multilayer structure, comprising the steps of uniaxially stretching an EVOH resin-containing layer (A) and laminating an inorganic vapor-deposited layer (B) on the layer (A).
[0009] According to the present invention, an inorganic vapor-deposited layer is laminated on a layer containing an extruded and uniaxially stretched EVOH resin having a single ethylene unit content, thereby making it possible to obtain a vapor-deposited film with excellent barrier properties.
[0010] The present invention will be described below based on examples of embodiments for carrying out the present invention, but the present invention is not limited to the embodiments described below.
[0011] Furthermore, in this specification, when the expression "X to Y" (X and Y are any numbers) is used, unless otherwise specified, it means "X or more and Y or less," as well as "preferably greater than X" or "preferably smaller than Y." Furthermore, when the expression "X or more" (X is any number) or "Y or less" (Y is any number) is used, it also means "preferably greater than X" or "preferably less than Y." Furthermore, "X and / or Y (X and Y are any configurations)" means at least one of X and Y, and can mean three possibilities: X only, Y only, or X and Y. For numerical ranges described in stages in this specification, the upper or lower limit of a numerical range in one stage can be arbitrarily combined with the upper or lower limit of a numerical range in another stage. Furthermore, in the numerical ranges described in this specification, the upper or lower limit of the numerical range can also be replaced with the values shown in the examples.
[0012] Hereinafter, a monomer unit contained in an EVOH resin or a thermoplastic resin may be simply referred to as a “unit.” For example, a monomer unit based on ethylene may be referred to as an “ethylene unit.”
[0013] A multilayer structure according to one embodiment of the present invention (hereinafter referred to as "the multilayer structure") comprises a layer (A) containing an EVOH resin (hereinafter sometimes referred to as "EVOH resin layer (A)") and an inorganic vapor-deposited layer (B) adjacent to the layer (A). Each component will be described below.
[0014] <EVOH Resin Layer (A)> The EVOH resin layer (A) is formed from an EVOH resin composition containing an EVOH resin. The EVOH resin can be obtained by saponifying an ethylene-vinyl ester copolymer. A representative vinyl ester is vinyl acetate, but other fatty acid vinyl esters (vinyl propionate, vinyl pivalate, etc.) can also be used. The ethylene-vinyl ester copolymer can be produced by any known polymerization method, such as solution polymerization, suspension polymerization, or emulsion polymerization, and the saponification of the ethylene-vinyl ester copolymer can also be carried out by a known method.
[0015] The ethylene unit content of the EVOH resin is usually 20 to 60 mol%, preferably 22 to 45 mol%, particularly preferably 25 to 35 mol%, and most preferably 25 mol% or more and less than 32 mol%, as measured in accordance with ISO 14663. When the ethylene unit content of the EVOH resin is within the above range, the transparency of the present multilayer structure tends to be improved.
[0016] Furthermore, the EVOH resin used in the present multilayer structure has a single ethylene unit content. In other words, the EVOH resin layer (A) does not contain two or more EVOH resins with different ethylene unit contents. If the EVOH resin layer (A) contains two or more EVOH resins with different ethylene unit contents, the barrier properties of the present multilayer structure will be reduced. In the present invention, "having a single ethylene unit content" means that the melting peak in differential scanning calorimetry (DSC) is a single peak having only one apex, and two points at half the height (H / 2) of the height (H) from the baseline to the apex of the peak are within ±10°C of the apex temperature. In the above definition, the DSC conditions are as follows:
[0017] DSC conditions: The temperature was increased from 30°C to 230°C at a rate of 10°C / min, held at 230°C for 1 minute, cooled to 30°C at a rate of 10°C / min, held at 30°C for 1 minute, and then increased again from 30°C to 230°C at a rate of 10°C / min. The vertical axis of the second heating chart represents heat capacity, and the horizontal axis represents temperature. The shape of the melting peak was confirmed, and the apex temperature of the melting peak was read. The baseline was a straight line connecting a point 20°C higher than the apex temperature of the melting peak (point a) and a point 80°C lower than the apex temperature of the melting peak (point b). Two or more EVOH resins with different vinyl ester types, physical properties, etc., may be mixed together as long as they have the same ethylene unit content.
[0018] The degree of saponification of the vinyl ester unit of the EVOH resin is a value measured in accordance with JIS K6726 (wherein the EVOH resin is a solution uniformly dissolved in a water / methanol solvent), and from the viewpoints of barrier property, thermal stability, and moisture resistance, is preferably 80 mol% or more, further preferably 90 mol% or more, even more preferably 98 mol% or more, particularly preferably 99 mol% or more, and may be 100 mol%.
[0019] The melt flow rate (MFR) of the EVOH resin (210°C, load 2160 g) is usually 0.5 to 100 g / 10 min, preferably 1 to 50 g / 10 min, and particularly preferably 3 to 35 g / 10 min. If the MFR is too high, film-forming properties tend to become unstable, whereas if it is too low, the viscosity tends to become too high, making melt extrusion difficult.
[0020] The EVOH resin may be copolymerized with a polymerizable monomer other than ethylene and vinyl ester within a range that does not impair the effects of the present invention, generally within a range of 5 mol % or less. Examples of such polymerizable monomers include α-olefins such as propylene, isobutene, α-octene, α-dodecene, and α-octadecene; hydroxyl-containing α-olefins such as 3-buten-1-ol, 4-penten-1-ol, and 3-butene-1,2-diol, and hydroxyl-containing α-olefin derivatives such as esters and acylates thereof; hydroxymethylvinylidene diacetates such as 1,3-diacetoxy-2-methylenepropane, 1,3-dipropionyloxy-2-methylenepropane, and 1,3-dibutyronyloxy-2-methylenepropane; unsaturated carboxylic acids or salts thereof, partial alkyl esters, complete alkyl esters, nitriles, amides, or anhydrides; unsaturated sulfonic acids or salts thereof; vinylsilane compounds; vinyl chloride; and styrene. These may be used alone or in combination of two or more.
[0021] Furthermore, as the EVOH resin, a "post-modified" EVOH resin such as urethanized, acetalized, cyanoethylated, or oxyalkylened can also be used.
[0022] The content of EVOH contained in the EVOH resin layer (A) is not particularly limited, but it is preferable that the EVOH resin is the main component (i.e., the content of the EVOH resin contained in the EVOH layer resin (A) is 50% by mass or more), more preferably 60% by mass or more, still more preferably 70% by mass or more, particularly preferably 80% by mass or more, 90% by mass or more, 95% by mass or more, or 100% by mass or more.
[0023] The EVOH resin layer (A) may contain other components besides the EVOH resin, such as antiblocking agents, processing aids, resins other than the EVOH resin, carboxylic acid compounds, phosphoric acid compounds, boron compounds, metal salts, stabilizers, antioxidants, ultraviolet absorbers, plasticizers, antistatic agents, lubricants, colorants, fillers, surfactants, desiccants, crosslinking agents, reinforcing agents such as various fibers, etc., within a range that does not impair the effects of the present invention, generally within a range of 20 mass % or less. These may be used alone or in combination of two or more.
[0024] The thickness of the EVOH resin layer (A) is not particularly limited, but is preferably 0.5 μm or more, more preferably 0.8 μm or more, and may be 1 μm or more. When the thickness of the EVOH resin layer (A) is 0.5 μm or more, the gas barrier property tends to be improved. Furthermore, the thickness of the EVOH resin layer (A) is preferably 20 μm or less, more preferably 10 μm or less, and may be 5 μm or less. When the thickness of the EVOH resin layer (A) is 20 μm or less, the appearance characteristics (film surface) tend to be good. The thickness of the EVOH resin layer (A) means the thickness after stretching. Furthermore, when a plurality of EVOH resin layers (A) are provided in the present multilayer structure, the total thickness of all the EVOH resin layers (A) is preferably within the above range.
[0025] <Inorganic vapor-deposited layer (B)> The present multilayer structure includes an inorganic vapor-deposited layer (B) adjacent to the EVOH resin layer (A). By including the inorganic vapor-deposited layer (B) adjacent to the EVOH resin layer (A), the present multilayer structure has excellent barrier properties.
[0026] The inorganic vapor-deposited layer (B) may be adjacent to the EVOH resin layer (A), and for example, the inorganic vapor-deposited layer (B) may be provided on only one side of the EVOH resin layer (A), or on both sides of the EVOH resin layer (A). Among these, from the viewpoints of productivity and cost, it is preferable to provide the inorganic vapor-deposited layer (B) on only one side of the EVOH resin layer (A).
[0027] The inorganic vapor deposition layer (B) is preferably made of an inorganic oxide and / or an inorganic nitride from the viewpoint of barrier properties. Examples of the inorganic oxide and / or inorganic nitride include inorganic oxides and inorganic nitrides of aluminum, silicon, magnesium, calcium, zirconium, titanium, boron, hafnium, barium, etc. Specific examples include inorganic oxides such as aluminum oxide (alumina), silicon oxide (silica), magnesium oxide, calcium oxide, zirconium oxide, titanium oxide, boron oxide, hafnium oxide, and silicon carbide oxide (oxygen-containing silicon oxide), and inorganic nitrides such as silicon nitride and aluminum nitride. Among these, inorganic oxides are preferred, and aluminum oxide (alumina) and silicon oxide (silica) are particularly preferred.
[0028] The thickness of the inorganic vapor deposition layer (B) (thickness of one layer) is usually 1 to 100 nm, preferably 3 to 50 nm, and more preferably 5 to 20 nm. If the thickness of the inorganic vapor deposition layer (B) is less than 1 nm, the barrier property tends to be insufficient, while if the thickness exceeds 100 nm, the barrier property is not improved and the flex resistance and production costs tend to increase.
[0029] [Layer (C) Containing Thermoplastic Resin] The present multilayer structure preferably has a layer (C) containing a thermoplastic resin [hereinafter referred to as "thermoplastic resin layer (C)"]. By having the present multilayer structure have the thermoplastic resin layer (C), the mechanical strength and barrier properties against water vapor of the present multilayer structure tend to be further improved. In addition, properties such as heat sealability and mechanical strength can be imparted depending on the type of thermoplastic resin constituting the thermoplastic resin layer (C).
[0030] Examples of the thermoplastic resins are those other than the EVOH resins, and include polyolefins such as polyethylenes such as linear low-density polyethylene, low-density polyethylene, very low-density polyethylene, medium-density polyethylene, and high-density polyethylene, ethylene-vinyl acetate copolymers, ionomers, ethylene-propylene (block or random) copolymers, ethylene-(meth)acrylic acid copolymers, ethylene-(meth)acrylic acid ester copolymers, polypropylene, propylene-α-olefin copolymers, polybutene, and polypentene, as well as polyolefins graft-modified with unsaturated carboxylic acids or esters thereof; polyesters; polyamides (including copolymerized polyamides); polyvinyl chloride; polyvinylidene chloride; acrylic resins; polystyrene; polyvinyl esters; polyester elastomers; polyurethane elastomers; chlorinated polystyrene; chlorinated polypropylene; aromatic polyketones or aliphatic polyketones, and polyalcohols obtained by reducing these; polyacetals; and polycarbonates. Among these, polyolefins are preferred from the viewpoint of excellent heat-sealing properties and mechanical properties, with polypropylene and polyethylene being more preferred, and polyethylene being particularly preferred. These may be used alone or in combination of two or more.
[0031] When polyethylene is used as the thermoplastic resin, the melt flow rate (MFR) of the polyethylene, measured (190°C, 2160 g load) in accordance with JIS K 7210: 2014, is preferably 0.10 to 7.5 g / 10 min, more preferably 0.15 to 5.0 g / 10 min, and particularly preferably 0.2 to 2.5 g / 10 min. When the MFR of the polyethylene is within the above range, molding stability tends to be better.
[0032] The content of the thermoplastic resin in the thermoplastic resin layer (C) is not particularly limited, but it is preferable that the thermoplastic resin is the main component (i.e., the content of the thermoplastic resin contained in the thermoplastic resin layer (C) is 50% by mass or more). The content of the thermoplastic resin is more preferably 60% by mass or more, even more preferably 70% by mass or more, particularly preferably 80% by mass or more, 90% by mass or more, 95% by mass or more, or 100% by mass or more.
[0033] The thermoplastic resin layer (C) may contain other components besides the thermoplastic resin, such as antiblocking agents, processing aids, resins other than thermoplastic resins, carboxylic acid compounds, phosphoric acid compounds, boron compounds, metal salts, stabilizers, antioxidants, ultraviolet absorbers, plasticizers, antistatic agents, lubricants, colorants, fillers, surfactants, desiccants, crosslinking agents, reinforcing agents such as various fibers, etc., within a range that does not impair the effects of the present invention, generally within a range of 20 mass % or less. These may be used alone or in combination of two or more.
[0034] The thickness of the thermoplastic resin layer (C) is not particularly limited, but is usually 1 to 100 μm, preferably 2 to 80 μm, and more preferably 5 to 50 μm. The thickness of the thermoplastic resin layer (C) refers to the thickness after stretching, if the layer is stretched. Furthermore, when a plurality of thermoplastic resin layers (C) are provided in the multilayer structure, the total thickness of all the thermoplastic resin layers (C) is preferably within the above range.
[0035] [Layer (D) Containing Adhesive Resin] The present multilayer structure may have a layer (D) containing an adhesive resin (hereinafter referred to as "adhesive resin layer (D)"). By having the present multilayer structure have the adhesive resin layer (D), the appearance characteristics (film surface) of the present multilayer structure tend to be better.
[0036] The adhesive resin is not particularly limited, but is preferably a polyolefin having a carboxy group, a carboxylic anhydride group, or an epoxy group, and more preferably a polyolefin having a carboxylic anhydride group. Such adhesive resins tend to have excellent adhesion to the EVOH resin layer (A) and / or the thermoplastic resin layer (C).
[0037] Examples of polyolefins containing carboxyl groups include polyolefins copolymerized with acrylic acid or methacrylic acid. In this case, all or part of the carboxyl groups contained in the polyolefin may be present in the form of a metal salt, as typified by ionomers. Examples of polyolefins having carboxylic acid anhydride groups include polyolefins graft-modified with maleic anhydride or itaconic acid. Examples of polyolefins having epoxy groups include polyolefins copolymerized with glycidyl methacrylate. Among these, polyolefins having carboxylic acid anhydride groups such as maleic anhydride are preferred, and polyethylenes having carboxylic acid anhydride groups are particularly preferred. These may be used alone or in combination of two or more.
[0038] The melt flow rate (MFR) of the adhesive resin measured (190°C, 2160 g load) according to JIS K 7210: 2014 is not particularly limited, but is preferably 0.1 to 20.0 g / 10 min, more preferably 1.0 to 10.0 g / 10 min. When the MFR of the adhesive resin is in the above range, molding stability tends to be better.
[0039] The content of the adhesive resin in the adhesive resin layer (D) is not particularly limited, but it is preferable that the adhesive resin be the main component (i.e., the content of the adhesive resin contained in the adhesive resin layer (D) is 50% by mass or more). The content of the adhesive resin is more preferably 60% by mass or more, even more preferably 70% by mass or more, particularly preferably 80% by mass or more, 90% by mass or more, 95% by mass or more, or 100% by mass or more.
[0040] The adhesive resin layer (D) may contain other components besides the adhesive resin, such as antiblocking agents, processing aids, resins other than adhesive resins, carboxylic acid compounds, phosphoric acid compounds, boron compounds, metal salts, stabilizers, antioxidants, ultraviolet absorbers, plasticizers, antistatic agents, lubricants, colorants, fillers, surfactants, desiccants, crosslinking agents, reinforcing agents such as various fibers, etc., within a range that does not impair the effects of the present invention, generally within a range of 20 mass % or less. These may be used alone or in combination of two or more.
[0041] The thickness of the adhesive resin layer (D) (thickness of one layer) is not particularly limited, but is usually 0.1 to 20 μm, preferably 0.5 to 10 μm, and more preferably 1 to 5 μm. When the adhesive resin layer (D) is stretched, the thickness of the adhesive resin layer (D) means the thickness after stretching.
[0042] <Method for producing the present multilayer structure> The present multilayer structure can be obtained by a production method including the steps of uniaxially stretching the EVOH resin layer (A) and laminating the inorganic vapor deposition layer (B) on the EVOH resin layer (A).
[0043] [Step of uniaxially stretching the EVOH resin layer (A)] In the step of uniaxially stretching the EVOH resin layer (A), the EVOH resin composition forming the EVOH resin layer (A) may be extruded through a die, and then uniaxially stretched. Examples of the die that can be used include a circular die and a T-die.
[0044] The stretching ratio of the EVOH resin layer (A) is preferably 3 times or more, more preferably 4 times or more, and particularly preferably 5 times or more. If the stretching ratio is less than 3 times, thickness unevenness due to stretching tends to occur and gas barrier properties tend to deteriorate. The upper limit of the stretching ratio is preferably 12 times or less, more preferably 10 times or less, and particularly preferably 8 times or less. If the stretching ratio is more than 12 times, the film surface after stretching tends to deteriorate. Uniaxially stretching the EVOH resin layer (A) has advantages from the viewpoint of economy, ease of tearing the multilayer structure (making it easy to open packaging materials when used as packaging materials), and improved gas barrier properties. The stretching direction of the uniaxial stretching is not particularly limited and may be either the longitudinal direction (MD direction) or the transverse direction (TD direction), and is preferably uniaxial stretching in the longitudinal direction (MD direction). It is preferable that the film is not substantially stretched in a direction different from the stretching direction. The stretched state of the EVOH resin layer (A) can be confirmed by using a general method for analyzing the orientation of a resin (for example, wide-angle X-ray scattering (WAXS)).
[0045] The stretching method for the EVOH resin layer (A) is not particularly limited, and examples thereof include tenter stretching, tubular stretching, roll stretching, etc. Among these, uniaxial stretching by roll stretching is preferred from the viewpoint of production costs.
[0046] The stretching temperature when the EVOH resin layer (A) is uniaxially stretched is not particularly limited, but is generally 50 to 130°C.
[0047] Furthermore, when the present multilayer structure includes the thermoplastic resin layer (C) and the adhesive resin layer (D), the compositions forming the EVOH resin layer (A), the thermoplastic resin layer (C), and the adhesive resin layer (D) can be extruded into a film by a conventional coextrusion lamination method in which the respective compositions forming the EVOH resin layer (A), the thermoplastic resin layer (C), and the adhesive resin layer (D) are extruded and laminated through separate dies or a common die, and then uniaxially stretched to form a substrate film. The inorganic vapor deposition layer (B) can then be laminated on the EVOH resin layer (A) of this substrate film by the method described below. Alternatively, the present multilayer structure having the EVOH resin layer (A) and the inorganic vapor deposition layer (B) can be produced, and then the thermoplastic resin layer (C) and the adhesive resin layer (D) can be laminated thereon. Examples of the die that can be used include a circular die and a T-die.
[0048] In addition to the co-extrusion lamination method, the base film may be formed by extruding each resin layer and laminating these layers using various known manufacturing methods, such as dry lamination, sand lamination, extrusion lamination, and solution coating.
[0049] The base film may have the EVOH resin layer (A) as the outermost layer, and the other layer configurations are not particularly limited. Examples of the layer configuration of the base film include, where the EVOH resin layer (A) is referred to as "layer (A)," the thermoplastic resin layer (C) is referred to as "layer (C)," and the adhesive resin layer (D) is referred to as "layer (D)," layer configurations of the base film include layer (A) / layer (C), layer (A) / layer (D) / layer (C), layer (A) / layer (D) / layer (C) / layer (D) / layer (C), and layer (A) / layer (C) / layer (A) / layer (C). While the above examples illustrate layers other than layer (A), layer (C) and layer (D) are not limited thereto. Furthermore, the thermoplastic resin layer (C) preferably does not include a layer formed from a resin composition containing a polyamide resin as a main component (i.e., a resin composition containing 50% by mass or more of polyamide resin). In the above examples, " / " means that the layers on both sides of it are directly laminated.
[0050] The stretching method, stretching ratio, etc. of the base film are the same as those explained in the step of uniaxially stretching the EVOH layer (A).
[0051] The total thickness of the substrate film is not particularly limited and can be appropriately set depending on the application. The thickness of the substrate film is preferably 10 μm or more, more preferably 15 μm or more. When the thickness of the substrate film is 10 μm or more, industrial productivity and mechanical properties tend to be further improved. Furthermore, the thickness of the substrate film is preferably 100 μm or less, more preferably 50 μm or less. When the thickness of the substrate film is 100 μm or less, industrial productivity and economic efficiency tend to be further improved. The thickness of the substrate film means the thickness after stretching.
[0052] When the base film is a multilayer film, the ratio of the thickness of the EVOH layer (A) to the total thickness of all layers is not particularly limited, but from the viewpoints of industrial productivity and mechanical properties, it is preferably 30% or less, more preferably 20% or less, and may be 10% or less, or may be 5% or less.
[0053] The internal haze value of the EVOH resin layer (A) or the base film is preferably less than 0.4%, more preferably 0.3% or less, particularly preferably 0.2% or less, and can be measured in accordance with ASTM D1003 using a haze meter and an EVOH resin layer (A) or a base film having a thickness of 33 μm.
[0054] [Step of Laminating Inorganic Vapor Deposition Layer (B) on EVOH Resin Layer (A)] The method for laminating the inorganic vapor deposition layer (B) on the EVOH resin layer (A) is not particularly limited, and any known vapor deposition method may be appropriately employed, for example, a physical vapor deposition method (PVD method) such as a vacuum vapor deposition method, a sputtering method, or an ion plating method, or a chemical vapor deposition method (CVD method).
[0055] The oxygen permeability of the multilayer structure thus obtained at 20°C and 90% RH is 8 cc / m 2 ·day·atm or less, and 7cc / m 2·day·atm or less is more preferable, 5 cc / m 2 ·day·atm or less is particularly preferred.
[0056] The present multilayer structure can be suitably used as a molding for packaging general foods, as well as seasonings such as mayonnaise and dressings, fermented foods such as miso, oily foods such as salad oil, snacks, beverages, cosmetics, pharmaceuticals, etc., as well as packaging materials such as packaging films, or as part of a multilayer structure for forming these.
[0057] <Molded Article> Examples of the molded article include containers such as cups and trays, and food containers. When molding the containers and food containers, a drawing method is usually used, and specific examples include vacuum forming, pressure forming, vacuum pressure forming, and plug-assisted vacuum pressure forming. Furthermore, when using the present multilayer structure to obtain a tube- or bottle-shaped multilayer container (laminate structure) from a multilayer parison (a hollow tubular preform before blowing), a blow molding method is used. Specific examples include extrusion blow molding (double-head type, mold-moving type, parison shift type, rotary type, accumulator type, horizontal parison type, etc.), cold parison blow molding, injection blow molding, and biaxial stretch blow molding (extrusion type cold parison biaxial stretch blow molding, injection type cold parison biaxial stretch blow molding, injection molding in-line biaxial stretch blow molding, etc.). The resulting laminate may be subjected to heat treatment, cooling treatment, rolling treatment, printing treatment, dry lamination treatment, solution or melt coating treatment, bag making, deep drawing, box processing, tube processing, splitting processing, etc. as required.
[0058] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to the following examples as long as it does not depart from the gist of the invention. In the examples, "parts" and "%" refer to mass standards. Prior to the examples, the following materials were prepared.
[0059] <EVOH> EVOH resin 1: ethylene unit content 29 mol%, MFR (210°C, load 2160g): 3.8g / 10 minutes, saponification degree 99.9 mol% EVOH resin 2: ethylene unit content 32 mol%, MFR (210°C, load 2160g): 3.8g / 10 minutes, saponification degree 99.9 mol% EVOH resin 3: ethylene unit content 25 mol%, MFR (210°C, load 2160g): 4.0g / 10 minutes, saponification degree 99.9 mol% EVOH resin 4: ethylene unit content 44 mol%, MFR (210°C, load 2160g): 3.5g / 10 minutes, saponification degree 99.9 mol%
[0060] <Thermoplastic resin> Polyethylene: "Novatec HY540" manufactured by Mitsubishi Chemical Corporation, MFR (190°C, load 2160g): 1.0g / 10min
[0061] <Adhesive Resin> Acid-modified polyethylene resin: "Modic M545" manufactured by Mitsubishi Chemical Corporation, MFR (190°C, load 2160 g): 6.0 g / 10 min
[0062] Example 1 [Production of Substrate Film] EVOH resin 1, polyethylene, and acid-modified polyethylene resin were supplied to a multilayer cast film device (manufactured by Plastics Engineering Research Institute) and coextruded under the following multilayer coextrusion molding conditions to obtain a substrate film with a three-type, three-layer structure of EVOH resin layer / adhesive resin layer / polyethylene layer. The thicknesses (μm) of the layers of the obtained substrate film were 20 / 10 / 170. [Multilayer Coextrusion Molding Conditions] EVOH resin layer: 40 mmφ single-screw extruder (barrel temperature: 210°C) Polyethylene layer: 40 mmφ single-screw extruder (barrel temperature: 230°C) Adhesive resin layer: 32 mmφ single-screw extruder (barrel temperature: 200°C) Die: 4-type, 5-layer feedblock type T-die (die temperature: 230°C) Take-up speed: 5 m / min
[0063] The obtained substrate film was stretched 6 times in the machine direction (MD direction) using a stretching device (manufactured by MEC Techno Co., Ltd.) by passing it between a roll heated to a surface temperature (stretching temperature) of 120°C and another roll rotating at a different speed, thereby obtaining a uniaxially stretched substrate film. The thicknesses (μm) of the respective layers of the obtained substrate film were 3.3 / 1.7 / 28.3.
[0064] [Formation of inorganic vapor deposition layer] Using a batch-type vapor deposition facility manufactured by Showa Shinku K.K., an inorganic vapor deposition layer of alumina was formed on the EVOH resin layer surface of the substrate film while the film surface temperature was kept at 60°C or lower, thereby obtaining a multilayer structure of Example 1.
[0065] Example 2 A multilayer structure of Example 2 was obtained in the same manner as in Example 1, except that the EVOH resin used was changed to EVOH resin 2.
[0066] Example 3 A multilayer structure of Example 3 was obtained in the same manner as in Example 1, except that alumina was changed to silica.
[0067] Comparative Example 1 [Production of Substrate Film] EVOH resin 1, polyethylene, and adhesive resin were supplied to a multilayer cast film device (manufactured by Plastics Engineering Research Institute) and coextruded under the following multilayer coextrusion molding conditions to obtain a substrate film with a three-type, three-layer structure of EVOH resin layer / adhesive resin layer / polyethylene layer. The thicknesses (μm) of the layers of the obtained substrate film were 20 / 10 / 170. [Multilayer Coextrusion Molding Conditions] EVOH resin layer: 40 mmφ single-screw extruder (barrel temperature: 210°C) Polyethylene layer: 40 mmφ single-screw extruder (barrel temperature: 230°C) Adhesive resin layer: 32 mmφ single-screw extruder (barrel temperature: 200°C) Die: 4-type, 5-layer feedblock type T-die (die temperature: 230°C) Take-up speed: 5 m / min
[0068] The obtained multilayer film was stretched 2 times in the MD direction and 3 times in the TD direction using a tenter-type biaxial stretching machine (manufactured by Brukner) for a total of 6 times stretching to obtain a biaxially stretched substrate film.
[0069] [Formation of Metal Vapor Deposition Layer] Using a batch-type vapor deposition facility manufactured by Showa Shinku K.K., an alumina vapor deposition layer was formed on the EVOH resin layer surface of the substrate film while the film surface temperature was kept at 60°C or lower, thereby obtaining a multilayer structure of Comparative Example 1.
[0070] Comparative Example 2 A multilayer structure of Comparative Example 2 was obtained in the same manner as in Comparative Example 1, except that the EVOH resin used was changed to EVOH resin 2.
[0071] Comparative Example 3 A multilayer structure of Comparative Example 3 was obtained in the same manner as in Example 1, except that the EVOH resins used were changed to EVOH resin 3 and EVOH resin 4 in a mass ratio of 75:25.
[0072] The barrier properties were evaluated using the resulting vapor-deposited films of Examples 1 to 3 and Comparative Examples 1 to 3. The results are shown in Table 1 below.
[0073] [Barrier Property Evaluation] The oxygen permeability was measured using an oxygen permeability measuring device (Ox-tran 2 / 21, manufactured by Hitachi High-Technologies Corporation) under conditions of 20° C. and 90% RH, and the barrier property was evaluated.
[0074]
[0075] The results in Table 1 above show that the multilayer structures of Examples 1 to 3, which included an extruded, uniaxially stretched substrate film having an EVOH resin layer (A) formed using an EVOH resin having a single ethylene unit content, and an inorganic vapor-deposited layer (B) on the surface of the substrate film facing the EVOH resin layer (A), had excellent barrier properties. On the other hand, the multilayer structures of Comparative Examples 1 and 2, which used a substrate film having a biaxially stretched EVOH resin layer (A), and the multilayer structure of Comparative Example 3, which used two types of EVOH resins, had inferior barrier properties compared to the multilayer structures of Examples 1 and 2, in which the inorganic vapor-deposited layer was the same alumina.
[0076] Although the above examples show specific embodiments of the present invention, the examples are merely illustrative and should not be construed as limiting. Various modifications that are obvious to those skilled in the art are intended to fall within the scope of the present invention.
[0077] The present multilayer structure can be suitably used as a molding for packaging general foods, as well as seasonings such as mayonnaise and dressings, fermented foods such as miso, oily foods such as salad oil, snacks, beverages, cosmetics, pharmaceuticals, etc., as well as packaging materials such as packaging films, or as part of a multilayer structure for forming these.
Claims
1. A multilayer structure comprising a layer (A) containing an ethylene-vinyl alcohol copolymer and an inorganic vapor deposition layer (B) adjacent to the layer (A), wherein the layer (A) is extruded and uniaxially stretched, and the ethylene-vinyl alcohol copolymer has a single ethylene unit content.
2. The multilayer structure according to claim 1, wherein the inorganic vapor deposition layer (B) comprises an inorganic oxide and / or an inorganic nitride.
3. The multilayer structure according to claim 1, wherein the stretching ratio of said layer (A) is 3 times or more.
4. The multilayer structure according to claim 1 or 2, further comprising a layer (C) containing a thermoplastic resin.
5. The multi-layer structure of claim 4, wherein said thermoplastic resin comprises a polyolefin.
6. A molded article comprising the multilayer structure according to claim 1 or 2.
7. A container comprising the multilayer structure of claim 1 or 2.
8. A food container comprising the multilayer structure of claim 1 or 2.
9. A method for producing a multilayer structure, comprising the steps of uniaxially stretching a layer (A) containing an ethylene-vinyl alcohol copolymer, and laminating an inorganic vapor deposition layer (B) on the layer (A).
Citation Information
Patent Citations
Barrier laminate, heat-sealable laminate comprising said barrier laminate, and packaging container comprising said heat-sealable laminate
JP2022009162A
Packaging laminate film, and packaging bag
JP2009143033A
Resin composition, multilayer sheet, packaging material, and container
JP2015071694A
Laminate and high-capacity packaging bag
JP2020019209A
Laminate and packaging container
JP2021160262A