Composite fiber nonwoven fabric using composite fiber web, and apparatus and method for manufacturing composite fiber web

The composite fiber nonwoven fabric, manufactured using a novel apparatus that mixes meltblown and electrospun fibers, addresses the challenges of uneven distribution and mechanical strength by achieving uniform fiber distribution and enhanced performance in sound absorption and filtration.

WO2024228569A1PCT designated stage expired Publication Date: 2024-11-07SNT CO LTD
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
PCT/KR2024/005978
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2024-05-03
Filing Date
2024-05-03
Publication Date
2024-11-07

AI Technical Summary

Technical Problem

Conventional methods for manufacturing composite nonwoven fabrics using meltblown and electrospun fibers face challenges such as uneven fiber distribution, peeling of nanofiber layers, and reduced mechanical strength due to differential pressure and post-processing damage, leading to non-uniform performance and structural issues.

Method used

A composite fiber nonwoven fabric is created using a manufacturing apparatus that uniformly mixes meltblown and electrospun fibers in a single-layer structure, where the electrospun fibers are randomly distributed between meltblown fibers, with a specific nozzle configuration and thermal entanglement to improve mixing and penetration, resulting in enhanced mechanical strength and uniform performance.

Benefits of technology

The solution achieves a uniform distribution of fibers across the thickness direction, improving mechanical strength and performance consistency, while minimizing fiber scattering and post-processing damage, leading to improved sound absorption and filtration capabilities.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure KR2024005978_07112024_PF_FP_ABST
    Figure KR2024005978_07112024_PF_FP_ABST
Patent Text Reader

Abstract

The present invention relates to a composite fiber nonwoven fabric using a composite fiber web, and to an apparatus and a method for manufacturing a composite fiber web. The present invention provides a manufacturing apparatus and a manufacturing method which are capable of manufacturing a composite fiber manufactured by mixing fibers spun by electrospinning and fibers spun by melt blowing. Accordingly, a composite fiber web, in which the fiber spun by electrospinning penetrates into the inside of the fiber spun by melt blowing, can be manufactured, and a composite fiber nonwoven fabric using same can be provided.
Need to check novelty before this filing date? Find Prior Art

Description

Composite fiber nonwoven fabric using a composite fiber web, manufacturing device for a composite fiber web, and manufacturing method thereof

[0001] The present invention relates to a composite fiber nonwoven fabric, and more particularly, to a composite fiber nonwoven fabric in which fibers spun by a melt-blown method and fibers spun by an electrospinning method are uniformly mixed to form a web in a single-layer structure.

[0002] (Description of government-supported research and development)

[0003] In addition, this study was conducted with the support of the Ministry of Trade, Industry and Energy and the Korea Industrial Technology Evaluation and Planning Institute's Research and Development Project on Machinery and Equipment Industry Technology Development (Research Project Name: Development of Roll-to-Roll Continuous Production Equipment for Ultrafine Nanofiber and Melt-blown Integrated Composite Nonwoven Fabric, Project Identification Number: 1415184294, Subproject Number: 20018393).

[0004] In general, nonwoven fabric refers to a textile product made by forming and combining a web in the shape of a sheet (fabric) by intertwining various fibers according to their mutual characteristics through chemical or mechanical action or appropriate moisture and heat treatment without a process such as spinning, weaving, or knitting.

[0005] Nonwoven fabrics are manufactured by manufacturing a web of thin sheets of fiber aggregates, typically made from staple fibers or filaments, and then imparting dimensional stability through the bonding of the fibers themselves. Any fiber-like material can be used to make nonwoven fabrics, including natural fibers, synthetic fibers, regenerated fibers, and inorganic fibers such as glass or carbon fibers. Fibers can range in length from a few millimeters to 100 millimeters, or from infinitely long fibers to virtually any type.

[0006] Nonwoven fabrics have traditionally been used for a variety of purposes because they can be imparted with various functions by appropriately combining the constituent fibers, the method of forming the fiber web, or the method of bonding the fiber web. Furthermore, because the smaller the fiber diameter of the fibers constituting the nonwoven fabric, the superior performance of various properties such as separation performance, liquid retention performance, odor control, hiding performance, insulation performance, and flexibility is expected, there is a growing demand for nonwoven fabrics made from fibers with the smallest possible fiber diameter.

[0007] These nonwoven fabrics are formed in various ways and are used in various industrial fields, such as sound-absorbing materials, filtration materials, various types of filters, masks or sanitary products, batteries and electronic devices such as secondary battery separators, biosensor substrates, scaffolds, medical applications such as pharmaceutical packaging materials or test containers, and optical applications such as lenses or optical films. Here, nonwoven fabrics are provided with different characteristics depending on the usage environment or purpose, and for example, nonwoven sound-absorbing materials are used for the purpose of absorbing sound to reduce noise.

[0008] This type of non-woven sound-absorbing material is mainly used in the automotive and construction fields, and as a large number of fibers intersect on the surface and inside of the non-woven fabric, small bubbles or tube-shaped holes are formed, and as the air inside the holes vibrates due to sound waves, sound energy is absorbed due to friction, reducing noise.

[0009] In the past, to manufacture nonwoven sound-absorbing materials, a device was used to form a fiber web using the melt-blown method. In other words, a single layer of melt-blown web was used as a nonwoven for sound-absorbing materials.

[0010] The meltblown spinning device for manufacturing such single-layer meltblown web-type nonwoven fabrics can manufacture ultra-fine fibers with diameters from sub-micron to several microns, but there are limitations on the applicable polymers and the miniaturization of fiber diameters for high-performance materials. The method for manufacturing nanofibers using electrospinning, one of various fiber manufacturing methods, can achieve such fiber miniaturization and high-performance filter materials. However, the conventional electrospinning device has the disadvantage of an electrical short phenomenon occurring due to the application of high voltage because it uses an electric heater to apply high-temperature heat for polymer melting.

[0011] To overcome these problems, efforts have been made to manufacture blended nonwoven fabrics made of heterogeneous fibers with different properties or fiber diameter sizes.

[0012] Accordingly, a laminated mixed nonwoven fabric has been proposed by laminating and mixing electrospun nanofibers on a meltblown web. However, the conventional laminated mixed nonwoven fabric has an electrospun nanofiber layer, and the sound absorption efficiency is improved compared to the conventional single-layer meltblown nonwoven fabric due to the fine and uniform pore characteristics of the nanofiber layer. However, since the nanofiber layer is simply laminated and bonded to the meltblown nonwoven layer, there is a phenomenon of delamination, and a high pressure difference is generated before and after the nanofiber layer, and the nanofiber layer is damaged by this pressure difference, so there is a disadvantage that the function of the sound-absorbing material or filter material is reduced.

[0013] Furthermore, conventional laminated mixed nonwoven fabrics require post-processing such as high-pressure pressing, heat bonding, and chemical bonding using resin to laminate the nanofiber layer and the substrate layer, which can cause damage or structural deformation of the nanofiber layer during post-processing. Furthermore, since the nanofiber layer, which has low mechanical strength, can be exposed and damaged, there is a disadvantage in that the number of processes increases, such as adding a spunbond nonwoven layer or a meltblown nonwoven layer to protect the nanofiber layer.

[0014] Accordingly, in order to supplement these problems, a technology for manufacturing a single-layer composite nonwoven fabric in which meltblown fibers and electrospun fibers are mixed is introduced in Japanese Patent Registration No. 5305960 (Method for manufacturing ultra-fine fiber nonwoven fabric and manufacturing apparatus therefor, hereinafter referred to as “prior art”). According to the manufacturing technology of the prior art, a meltblown spinning unit and a collector are arranged to be spaced apart from each other, forming a structure in which meltblown fibers are radiated toward the collector, and an electrospinning unit is arranged between the meltblown spinning unit and the collector so as to have a spinning direction orthogonal to the meltblown spinning flow, thereby forming mixed fibers by electrospinning.

[0015] However, even if manufacturing technology according to these prior arts is used, it is difficult to penetrate the fibers spun by electrospinning, which is a relatively low-velocity manufacturing environment, into the interior of the meltblown fibers, and the mechanical strength and other properties of the composite nonwoven fabric are inherently insufficient for use as a sound-absorbing material.

[0016] That is, the manufacturing technology of the prior art has a problem in that the electrospinning flow is generated in the middle of the meltblown spinning flow moving toward the collector by placing an electrospinning section between the meltblown spinning section and the collector, so that the electrospinning flow is captured on the collector in a state in which only the outer surface of the meltblown spinning flow is wrapped, and the electrospinning fibers are not smoothly mixed with the meltblown fibers. In particular, in the conventional case, there was a problem in that there was a large difference in the level of fiber mixing between the outer surface and the inner surface (the surface in contact with the collector) of the nonwoven fabric captured and formed on the collector due to the flow in which the fibers were accumulated on the outer surface.

[0017] In other words, according to the manufacturing technology of the prior art, since the electrospun fibers are not introduced into the inside of the meltblown spinning flow, they are mainly formed only on the outer surface side of the nonwoven fabric, and in reality, only a very small amount of fibers are formed on the inside and back of the nonwoven fabric, which has a significant problem in terms of the distribution and uniformity of the fibers along the thickness direction, and such products are not much different from a laminated structure in which the electrospun nonwoven fabric is laminated on the outer surface.

[0018] In addition, according to the prior art, during the mixing process of meltblown fibers and electrospun fibers, since each fiber is spun in a different direction, there is a problem that the fibers are scattered, the two fibers are not uniformly mixed, or the scattered fibers settle on the nozzle or other components of the spinning section located adjacent to the spinning stream.

[0019] In particular, according to conventional manufacturing equipment, there was a problem in that the degree of fiber mixing was different depending on the thickness direction position of the nonwoven fabric as the flying fibers fell on the outer surface layer of the nonwoven fabric being produced and were captured or mixed.

[0020] Ultimately, conventional manufacturing equipment had the problem of making it difficult to manufacture nonwoven fabrics with a uniform distribution.

[0021] (Prior art literature)

[0022] (Patent Document)

[0023] (Patent Document 1) Japanese Patent No. 5305960 (registered on June 8, 2012)

[0024] (Patent Document 2) Republic of Korea Patent No. 10-2115206 (registered on May 20, 2020)

[0025] Accordingly, the purpose of the present invention is to provide a manufacturing device and a manufacturing method capable of manufacturing a composite fiber manufactured by mixing fibers spun by an electrospinning method and fibers spun by a meltblown method.

[0026] In particular, the purpose of the present invention is to provide a manufacturing device and a manufacturing method for minimizing the scattering phenomenon of radiated fibers and improving the mixing action of composite fibers.

[0027] In addition, an object of the present invention is to provide a composite fiber manufactured using the above-described manufacturing device or manufacturing method.

[0028] The present invention has been devised to solve the above-described problems, and an object of the present invention is to provide a composite fiber nonwoven fabric in which heterogeneous fibers of different diameter sizes or different materials are mixed.

[0029] In particular, the present invention provides a composite fiber nonwoven fabric having a single-layer structure in which electrospun fibers are uniformly distributed between meltblown fibers.

[0030] In order to achieve the above-described object, the composite fiber nonwoven fabric of the present invention comprises a single-layer fiber sheet made of a fiber web in which meltblown fibers formed by a meltblown spinning method and electrospun fibers formed by an electrospinning method are irregularly mixed, and the fiber sheet comprises a first surface area portion provided on one side along the thickness direction of the fiber sheet, a second surface area portion provided on the other side of the fiber sheet opposite the first surface area portion, and an internal area portion located between the first surface area portion and the second surface area portion, and is characterized in that a first difference in each area according to the number of electrospun fibers among the total number of measured fibers in the first surface area portion, the second surface area portion, and the internal area portion is 50%P (percentage point) or less in the first surface area portion, the second surface area portion, and the internal area portion.

[0031] According to the present embodiment, the fiber sheet may be formed such that each of the first surface area portion, the second surface area portion, and the inner area portion is at least 15% or more.

[0032] According to the present embodiment, the meltblown fibers can be formed to have a diameter size of more than 1.5 μm and less than or equal to 5 mm, and the electrospun fibers can be formed to have a diameter size of more than 0.001 μm and less than or equal to 1.5 μm.

[0033] According to the present embodiment, the pore size of the fiber sheet formed between the meltblown fiber and the electrospun fiber is characterized by being 0.1 ㎛ to 3.0 ㎛.

[0034] According to the present embodiment, the fiber sheet may be formed from 1 to 50 wt% of the second electrospun fiber within the fiber web according to the measured weight, out of 100 wt% of the total measured weight.

[0035] According to the present embodiment, the fiber sheet can be formed with a surface area ratio of 20% to 55% by electrospun fibers measured in the first surface area portion, the second surface area portion, and the internal area portion, respectively.

[0036] According to this embodiment, the fiber sheet has a specific surface area of ​​1 m by meltblown fibers. 2 / g to 3 m 2 / g, and the specific surface area of ​​the electrospun fiber is about 5 m 2 / g to 7 m 2 / g can be.

[0037] Meanwhile, in order to achieve the aforementioned purpose, the composite fiber web of the present invention comprises first fibers formed by a melt-blown spinning method; and second fibers formed by an electrospinning method and randomly mixed with the first fibers.

[0038] According to the present embodiment, the first fiber is characterized in that it has a diameter size exceeding 1.5 ㎛ and not more than 5 cm, and the second fiber is characterized in that it has a diameter size of not less than 0.001 ㎛ and not more than 1.5 ㎛.

[0039] According to the present embodiment, the mixing ratio of the first fiber and the second fiber is characterized by being formed as 60% to 75%: 40% to 25% based on the measured number.

[0040] According to the present embodiment, the device for manufacturing the composite fiber web includes a first spinning unit including a first nozzle for discharging a first spinning solution to one side by a melt-blown method; a collecting unit arranged to be spaced apart from the first spinning unit to one side and for collecting the first spinning solution discharged from the first spinning unit; and a second spinning unit including a second nozzle installed between the first spinning unit and the collecting unit for discharging a second spinning solution to cross the first spinning solution by an electrospinning method, wherein the flow of the second spinning solution discharged from the second nozzle is formed to be opposite to the flow direction of the first spinning solution.

[0041] According to the present embodiment, the second radiating portion is characterized in that the second nozzle is arranged to be inclined toward the first nozzle.

[0042] According to the present embodiment, the second nozzle includes: a body part having a space formed inside; a first discharge pipe provided in the body part and discharging a first fluid supplied to the space; and a second discharge pipe having a constant outer diameter and discharging a second fluid while being inserted into the first discharge pipe.

[0043] According to the present embodiment, a method for manufacturing the composite fiber web includes the steps of forming a first stream by ejecting a first spinning solution to one side by a melt-blown method using a first nozzle of a first spinning unit; forming a second stream by ejecting a second spinning solution toward the first stream by an electrospinning method using a second nozzle of a second spinning unit; intersecting the first stream and the second stream and mixing the first spinning solution and the second spinning solution in a web structure; and capturing the mixed stream in a capturing unit.

[0044] According to the present embodiment, a nonwoven fabric having a web structure in which first fibers produced by a melt-blown spinning method and second fibers produced by an electrospinning method are randomly mixed is provided.

[0045] According to the present embodiment, a laminate is provided, which includes a hybrid layer in which first fibers formed by a melt-blown spinning method and second fibers formed by an electrospinning method are randomly mixed; and a connecting layer connected in a laminated state to at least one surface of the nonwoven fabric layer.

[0046] According to the present embodiment, a laminate is provided, characterized in that the connecting layer is provided in a multi-layer structure in which a plurality of identical or different layers are provided.

[0047] According to the present embodiment, the nonwoven fabric or laminate is characterized by nanofibers being mixed throughout the cross-section. Flame-retardant polyimide (PI) can be used. Based on the cross-section of the nonwoven fabric, the number of pores per unit area can be distributed in various ways.

[0048] According to the present embodiment, the composite fiber manufacturing device using the heat bridge of the present invention includes a first spinning unit including a first nozzle that discharges a first spinning solution to one side by a melt blown method, a collecting unit that is arranged to be spaced apart from the first spinning solution to one side and collects the first spinning solution discharged from the first spinning solution, and a second nozzle that is installed between the first spinning unit and the collecting unit to be spaced apart from the flow of the first spinning solution and discharges a second spinning solution to cross the first spinning solution by an electrospinning method, and a second spinning unit that forms the flow of the second spinning solution discharged from the second nozzle to be opposite to the flow direction of the first spinning solution.

[0049] According to the present embodiment, the second radiating portion is characterized in that the second nozzle is arranged to be inclined toward the first nozzle.

[0050] According to the present embodiment, the second radiating portion is characterized in that the installation angle of the second nozzle through which the second radiating solution is discharged is tilted by 38 to 52 degrees from the vertical discharge position with respect to the first stream.

[0051] According to the present embodiment, the second radiation unit is characterized in that the second nozzle is positioned so as to be able to reach the flow of the first radiation solution at a position adjacent to the first nozzle so that the second radiation solution is thermally mixed with the first radiation solution.

[0052] According to the present embodiment, the second radiating portion is characterized in that the distance between the installation position of the second nozzle and the collecting portion is shorter than the distance between the installation position of the second nozzle and the first nozzle.

[0053] Here, the first and second radiating units may be configured as a single module in which the nozzles are arranged in a row. Furthermore, each radiating unit may have multiple modules arranged in series or adjacently. Furthermore, each radiating unit may have multiple modules arranged at different positions. That is, for example, the radiating unit may be configured with an upper module that provides a flow of the second radiating solution at a position above the flow of the first radiating solution, and a lower module that provides another flow of the second radiating solution at a position below the flow of the first radiating solution, thereby forming a uniform distribution on the composite fiber web.

[0054] According to this embodiment, a composite fiber manufactured by the composite fiber manufacturing device described above can be provided.

[0055] The composite fiber nonwoven fabric according to the present invention as described above is provided as a single-layer structured fiber web in which electrospun fibers are uniformly distributed between meltblown fibers, so that it can be utilized as a product having uniform performance.

[0056] Meanwhile, according to the composite fiber manufacturing device and manufacturing method of the present invention, it is possible to manufacture a composite fiber in which fibers spun by an electrospinning method penetrate into the interior of fibers spun by a meltblown method.

[0057] In particular, according to the composite fiber manufacturing device and manufacturing method of the present invention, the phenomenon of fiber scattering occurring during the manufacturing process can be minimized, and the mixing action of the composite fiber can be improved to manufacture a uniform composite fiber product.

[0058] In addition, the composite fiber manufactured by the composite fiber manufacturing device and manufacturing method can improve the mechanical strength of the composite fiber by improving the fiber volume content.

[0059] FIG. 1 is a cross-sectional view of a composite fiber nonwoven fabric according to one embodiment of the present invention.

[0060] FIG. 2 is an electron microscope image of the surface of a composite fiber nonwoven fabric according to one embodiment of the present invention.

[0061] FIG. 3 is an electron microscope image of a cross-section of a composite fiber nonwoven fabric according to one embodiment of the present invention.

[0062] FIG. 4 is a schematic drawing of a composite fiber manufacturing device according to one embodiment of the present invention.

[0063] FIG. 5 is a drawing for explaining the structure of a composite fiber manufacturing device according to one embodiment of the present invention.

[0064] Figure 6 is a schematic drawing of a composite fiber manufacturing device according to one embodiment of the present invention.

[0065] FIG. 7 shows a flow chart of a method for manufacturing a composite fiber web using a composite fiber manufacturing device according to one embodiment of the present invention.

[0066] FIG. 8 is a schematic drawing of an electrospinning section of a composite fiber manufacturing device according to another embodiment of the present invention.

[0067] FIG. 9 is a graph showing the fiber composition ratio according to the fiber diameter analysis results for a composite fiber web nonwoven fabric manufactured according to one embodiment of the present invention.

[0068] The advantages and features of the present invention, and the methods for achieving them, will become clearer with reference to the embodiments described below in detail, along with the accompanying drawings. However, the present invention is not limited to the embodiments disclosed below and may be implemented in various different forms.

[0069] Hereinafter, the technical features of the present invention will be described in detail with reference to the attached drawings.

[0070] Fig. 1 is a cross-sectional view schematically illustrating an example of a composite fiber nonwoven fabric according to one embodiment of the present invention. In addition, Figs. 2 and 3 are electron microscope images showing the fiber web of the composite fiber nonwoven fabric. Here, Fig. 2 is an SEM image photographing the surface fiber web of the composite fiber nonwoven fabric of the present invention. In addition, Fig. 3 is an SEM image photographing the fiber web in the first surface area of ​​a cut cross-section of the composite fiber nonwoven fabric of the present invention, as an example.

[0071] Referring to FIGS. 1 and 2, a composite fiber nonwoven fabric using a composite fiber web according to one embodiment of the present invention is characterized in that meltblown fibers (1a) formed by a meltblown spinning method and electrospun fibers (1b) formed by an electrospinning (or electrostatic spinning) method are mixed in a fiber form.

[0072] Here, the resin constituting each of these fibers is a resin that can be spun by melt-blown spinning or electrospinning, and there is no particular limitation on the material or type of the resin.

[0073] For example, the melt-blown spinning solution used to form the melt-blown fiber (1a) can be used without limitation as long as it is a melt-spinnable thermoplastic resin. Such a thermoplastic polymer resin can be, for example, at least one selected from the group consisting of polypropylene (PP), polypropylene copolymer, nylon, polyester (PE), polyurethane (PUR), polyimide (PI), polyacrylonitrile (PAN), polyolefin (PO), pitch, and cellulose.

[0074] And, the electrospinning spinning solution used to form the electrospun fiber (1b) may include at least one selected from the group consisting of, for example, polypropylene (PP), polyethylene terephthalate (PET), polyvinylidene fluoride (PVdF), polyvinylacetate (PVAc), polymethyl methacrylate (PMMA), polyacrylonitrile (PAN), polyurethane (PUR), polybutylene terephthalate (PBT), polyvinyl butyral (PVB), polyvinyl chloride (PVC), polyolefin (PO), polylactic acid (PLA), polyethylene naphthalate (PEN), polyimide (PI), polyamide (PA), polyvinyl alcohol (PVA), polyethylene imide (PEI), pitch, polycaprolactone (PCL), polylactic acid glycolic acid (PLGA) resin, silk solution, cellulose solution, and chitosan solution.

[0075] The process by which these meltblown spinning solutions and electrospinning spinning solutions are produced into fibers will be described later.

[0076] In this way, the melt-blown spinning solution can be formed into micro-sized fibers by the melt-blown spinning method, and can be formed to have a diameter size that mainly exceeds 1.5 μm, preferably exceeds 1.5 μm and is 30 μm or less. In one embodiment, depending on the manufacturing conditions, the melt-blown spinning solution can also be formed into fibers having a diameter of 1.5 μm or less. The micro-sized fibers measured in this way can be classified as melt-blown fibers (1a).

[0077] In addition, the electrospinning solution can be formed into micro- or nano-sized fibers by the electrospinning method, and can be formed to have a diameter of mainly 1.5 μm or less, preferably 0.001 μm to 1.5 μm (1 to 1,500 nm). In one embodiment, depending on the manufacturing conditions, the electrospinning solution can also be formed into fibers having a diameter exceeding 1.5 μm. The nano-sized fibers measured in this way can be classified as electrospun fibers (1b).

[0078] Here, the diameter of each fiber refers to the diameter size of the fiber that can be confirmed in the electron microscope photograph of the composite fiber nonwoven fabric of Fig. 2, and specifically, can be obtained by measuring the diameter size of each fiber for a case of 90 or more fibers. Related experimental examples are described below.

[0079] That is, in the fiber web constituting the composite fiber nonwoven fabric of the present invention, the meltblown fibers (1a) may be formed mainly of micro-sized fibers, and the electrospun fibers (1b) may be formed mainly of nano-sized fibers.

[0080] At this time, among the meltblown fibers (1a), there may be nano-sized fibers of 1.5㎛ or less, and among the electrospun fibers (1b), there may be micro-sized fibers exceeding 1.5㎛. However, in this embodiment, these are classified and distinguished according to the standard measurement size, which is a set value of 1.5㎛, through the experimental examples described below. The diameter size of each fiber will be described below.

[0081] In other words, the composite fiber nonwoven fabric of the present invention is a mixture of meltblown fibers (1a) having a fiber diameter exceeding 1.5 ㎛ and electrospun fibers (1b) having a fiber diameter of 0.001 to 1.5 ㎛. In this embodiment, the meltblown fibers (1a) can be classified as microfibers, and the electrospun fibers (1b) can be classified as nanofibers. In this case, the diameter size for distinguishing between microfibers and nanofibers is generally divided based on 1 ㎛, but in this embodiment, the two fibers are distinguished based on a size of 1.5 ㎛.

[0082] Here, the fiber sheet (1) can be divided into a first surface area portion provided on one side along the thickness direction, a second surface area portion on the other side opposite the first surface area portion, and an internal area portion located between the two surface areas. In this embodiment, the distinction between one side and the other side of the fiber sheet (1) can be divided into the surface (one side) and the back side (the other side) of a general non-woven fabric. Such a fiber sheet (1) is typically manufactured by being spun by a spinning device and captured by a capturing device to form a fiber web. The side that is arranged to face the spinning device is referred to as the surface, and the side that is arranged to face the capturing device (collector) is referred to as the back side.

[0083] In this way, the first surface area refers to one surface area, which is the upper layer of the fiber sheet (1), and can be provided as an area including the outer surface, which is the outer part of the fiber layer formed by collecting it on the collector during the manufacture of the fiber web.

[0084] The second surface area refers to the other surface area, which is the lower layer of the fiber sheet (1), and can be provided as an area including the inner surface, which is the inner part of the fiber layer.

[0085] The inner region refers to the middle region of the fiber sheet (1) located between the two surface regions, and includes a portion excluding the first surface region and the second surface region.

[0086] For example, the first surface area portion may be formed as an upper area of ​​the upper layer of the fiber sheet (1) including the outer surface layer, which is at most 40% of the total 100% thickness of the fiber sheet (1), and the second surface area portion may be formed as a lower area of ​​the lower layer of the fiber sheet (1) including the inner surface layer, which is at most 40% of the total 100% thickness of the fiber sheet (1). The inner area portion may be formed as an intermediate area other than the first surface area portion and the second surface area portion. This inner area portion may be formed as an intermediate area of ​​1 to 99% of the total 100% thickness of the fiber sheet (1). In the present embodiment, the inner area portion is divided into three areas, but the entire thickness may be divided into four or more areas, and may be formed within the range of a measurable area. That is, when the thickness of the fiber sheet (1) is thin, it is limited to measure by dividing it into multiple areas, but when the thickness is thick, measurement is possible in each area even if it is divided into multiple areas, so it will be possible to divide it in detail as needed in response to the application field to which the nonwoven fabric is applied or the thickness of the product produced.

[0087] In one embodiment, the fiber sheet (1) may have a first surface area that is measured within a section of about 10% of the total thickness from the outer surface, a second surface area that is measured within a section of about 10% of the total thickness from the inner surface, and an internal area that is measured within a section of about 80%. For example, when the fiber sheet (1) is formed to have a thickness of about 10 mm, the first surface area may be formed to have a thickness of 0 mm to 1 mm from the surface, the second surface area may be formed to have a thickness of 0 mm to 1 mm from the back surface, and the internal area may be formed to have a thickness of 8 mm to 10 mm. In this case, 0 mm refers to the surface layer itself of the front or back surface.

[0088] For ease of explanation, this fiber sheet (1) is described as having each region roughly divided into three regions, upper, middle, and lower, based on the thickness direction. In other words, it can be formed at a ratio in which each region is divided into approximately 1 / 3 based on the thickness direction.

[0089] Specifically, the composite fiber nonwoven fabric of the present invention includes a single-layer structured fiber sheet (1) made of a fiber web in which different types of fibers are mixed.

[0090] The fiber sheet (1) is formed to a predetermined thickness due to its volume due to the fiber web structure, and meltblown fibers (1a) and electrospun fibers (1b) are irregularly entangled and mixed over the entire surface area and cross-sectional thickness direction.

[0091] At this time, the existing composite fiber nonwoven fabrics of composite radiation type had problems such as the fibers not being smoothly mixed during the manufacturing process due to the radiation structure that was discharged from different materials and environments, and the degree of fiber mixing occurring differently (distribution deviation occurring) depending on the location in the direction of the entire surface and cross-sectional thickness of the nonwoven fabric, resulting in non-uniform characteristic differences and deterioration of performance.

[0092] Accordingly, the composite fiber nonwoven fabric of the present invention has as its main feature that electrospun fibers (1b) are uniformly distributed within the fiber web of the fiber sheet (1).

[0093] According to this embodiment, the degree to which the electrospun fibers (1b) are uniformly distributed can be expressed by the first mixing ratio, which is the ratio of the number of fibers mixed.

[0094] In this embodiment, the first mixing ratio means the ratio according to the number of electrospun fibers (1b) among the total number of fibers of the fiber sheet (1). To elaborate, the first mixing ratio is expressed as a ratio (percentage; %) calculated from the number of electrospun fibers (1b) to the total number counted from 90 or more fibers that can be confirmed from the electron microscope image of the composite fiber nonwoven fabric of FIG. 2. That is, the first mixing ratio can be calculated by an equation regarding the ratio of the number of electrospun fibers to the total number of fibers, and P, which derives the first mixing ratio as a value, EF can be expressed by the following mathematical formula.

[0095]

[0096] In the above equation, TF is the total number of fibers that can be confirmed and counted in the image, and EF is the number of electrospun fibers (1b) having a diameter size of 1.5 μm or less among the fibers.

[0097] According to the present embodiment, the fiber sheet (1) of the present invention has a first mixing ratio P based on the measured number of electrospun fibers (1b) among the total number of fibers measured in the fiber web. EF The value can be formed by more than 15%.

[0098] At this time, the fiber sheet can be formed so that each of the first surface area portion, the second surface area portion, and the internal area portion has a first mixing ratio of at least 15%.

[0099] And, according to the present embodiment, the meltblown fiber (1a) can be formed to have a diameter size exceeding 1.5 ㎛ and not more than 5 mm, and the electrospun fiber (1b) can be formed to have a diameter size of not less than 0.001 ㎛ and not more than 1.5 ㎛.

[0100] In addition, according to the present embodiment, the pore size of the fiber sheet (1) formed between the meltblown fiber (1a) and the electrospun fiber (1b) can be provided to be 0.001 µm to 3.0 µm.

[0101] In addition, according to the present embodiment, the fiber sheet can be formed with a second mixing ratio of electrospun fibers in the fiber web according to the measured weight of 1 to 50 wt% of the total measured weight.

[0102] Moreover, according to the present embodiment, the fiber sheet (1) can be formed with a surface area ratio of 20% to 55% by electrospun fibers measured in the first surface area portion, the second surface area portion, and the internal area portion, respectively.

[0103] In addition, according to the present embodiment, the fiber sheet (1) has a specific surface area of ​​1 m by meltblown fibers. 2 / g to 3 m 2 / g, and the specific surface area of ​​the electrospun fiber is about 5 m 2 / g to 7 m 2 / g can be formed.

[0104] Hereinafter, the present invention will be described in more detail based on experimental examples of composite fiber nonwoven fabrics according to embodiments of the present invention.

[0105] The nonwoven fabric of the experimental example was a nonwoven fabric formed by simultaneously spinning a melt-blown spinning solution of polypropylene (PP) and an electrospinning spinning solution of nylon (NY) / polyvinyl alcohol (PVA) and a fiber web formed by composite spinning. Here, the nonwoven fabric was a mixture of melt-blown fibers and electrospun fibers, and a sample size of 300 mm in length, 22 mm in width, a weight of about 80 g / ㎡, and a thickness of about 8 mm was used.

[0106] According to the main requirements according to the manufacturing process of the composite fiber nonwoven fabric of the present invention, the specification standards of the fiber sheet may vary depending on the thickness, weight, etc., and the fiber composition within the fiber web may be classified into the weight (%) mixing ratio of meltblown fibers (MF) and electrospinning fibers (EF), diameter size, mixing number ratio (overall average, surface, middle, back), surface area ratio, specific surface area, etc. In addition, as manufacturing requirements, there may exist the nozzle diameter size, number, set temperature, spinning solution (material), distance from the collector (DCD), hourly discharge amount, etc. for the meltblown spinning device, and there may exist the assistant air discharge amount, distance from the meltblown spinning stream, hourly discharge amount, voltage, etc. for the electrospinning device. The measured values ​​or conditions may be configured differently depending on the use of the fiber nonwoven fabric to be manufactured.

[0107] In this example, the SEM analysis device used for measurement was the JSM7600F model. The sample according to the experimental example was requested to the Korea Quality Testing Institute (www.kqti.co.kr), and the diameter size of each fiber was measured and recorded from 90 fibers counted in the image using the Eyeview diameter analysis tool at an analysis magnification of x1,000.

[0108] In this measurement experiment, images taken from each of the first surface area, the internal area, and the second surface area of ​​the fiber sheet (1) were used based on the cross-section.

[0109] In this way, the diameter size of the fibers included in the composite fiber nonwoven fabric of the present invention refers to the diameter of the fibers that can be confirmed by an electron microscope photograph, and was measured from all measurable fibers, and as an example, it could be obtained by measuring a number of 90 fibers.

[0110] In these measurement experiments, the recorded total fibers were classified by diameter size into meltblown fibers (1a) if they exceeded the standard measurement size (1.5㎛) and electrospun fibers (1b) if they were smaller than the standard measurement size. Then, the ratio of meltblown fibers and electrospun fibers among the total fibers was quantified and compared and analyzed.

[0111] The following table shows the distribution by region, categorized by fiber diameter size.

[0112] Fiber distribution by size 1st surface area internal area 2nd surface area division fiber diameter fiber number ratio fiber number ratio fiber number ratio unit nm EA% EA% EA% 1750 33.3% 44.4% 55.6% 2850 55.6% 22.2% 44.4% 31,000 66.7% 55.6% 44.4% 41,250 1011.1% 77.8% 88.9% 51,500 88.9% 1011.1% 44.4% 62,000 1415.6% 1516.7% 1617.8% 7 3,0001314.4%1213.3%1516.7%85,0001213.3%1921.1%1314.4%97,00077.8%88.9%33.3%1010,00044.4%55.6%88.9%1120,00077.8%33.3%1011.1%1230,00011.1%00.0%00.0%Total90100.0%90100.0%90100.0%

[0113] And, the following table shows the analysis results by number of fibers classified by diameter size in each area of ​​the fiber.

[0114] EF-MF classification standard (1,500 nm) Area-by-area measurement values ​​1st surface internal area 2nd surface fiber count 909090 average diameter (nm) 3,6983,1784,045 dispersion distribution (CV) 118.19% 85.89% 106.52% EF count 322825 EF ratio 35.56% 31.11% 27.78% MF ratio 64.44% 68.89% 72.22% EF mixing effect (based on 1st surface) 100.00% 87.50% 78.13%

[0115] Looking at the measurement results, fibers of various diameter sizes were measured as shown in Table 2 above, and showed a wide distribution from fibers of sizes less than 750 nm to fibers of sizes less than 30,000 nm. In addition, the status of fiber measurement in each area is explained with reference to Table 2 above.

[0116] In the first surface area, the overall average diameter size of 90 measured fibers was 3,698 nm, and the standard deviation was 4,370 nm. The maximum diameter size of the fibers was 29,786 nm, and the minimum diameter size was 712 nm. In addition, the number of electrospun fibers (EF) classified based on 1,500 nm (1.5 μm) was counted as 32, accounting for 35.6% of the total mixing ratio. The relative number of meltblown fibers (MF) was 58, and the mixing ratio was 64.4%.

[0117] In the internal region, the overall average diameter size of 90 measured fibers was 3,178 nm, and the standard deviation was 2,730 nm. The maximum diameter size of the fibers was 13,595 nm, and the minimum diameter size was 619 nm. In addition, the number of electrospun fibers (EF) classified based on 1,500 nm (1.5 μm) was counted as 28, accounting for 31.1% of the total mixing ratio. The relative number of meltblown fibers (MF) was 62, and the mixing ratio was 68.9%.

[0118] In the second surface area, the overall average diameter size of 90 measured fibers was 4,045 nm, and the standard deviation was 4,309 nm. The maximum diameter size of the fibers was 17,339 nm, and the minimum diameter size was 559 nm. In addition, the number of electrospun fibers (EF) classified based on 1,500 nm (1.5 μm) was counted as 25, accounting for 27.8% of the total mixing ratio. The relative number of meltblown fibers (MF) was 65, and the mixing ratio was 72.2%.

[0119] In this way, according to the present embodiment, it was confirmed that the composite fiber nonwoven fabric was formed as a single-layer structured fiber web in which meltblown fibers (1a) and electrospun fibers (1b) were irregularly mixed.

[0120] Here, according to one embodiment, the fiber sheet (1) of the present invention has a first mixing ratio P based on the measured number of electrospun fibers (1b) among the total number of fibers measured in the fiber web. EF The value can be formed by more than 15%.

[0121] That is, according to the present embodiment, the fiber sheet (1) can be formed so that the first mixing ratio in each of the first surface area, the second surface area, and the internal area is 15% or more. Preferably, the fiber sheet can be formed in a first mixing ratio range of 20 to 50%, and for example, the mixing ratio in each area can be 25 to 37%.

[0122] At this time, the fiber sheet (1) may have different first mixing ratios in each region, but since the electrospun fibers (1b) are provided to have a uniform distribution within the fiber web, the deviation can be formed without being large. In other words, since the composite fiber nonwoven fabric of the present invention is formed to have the electrospun fibers have a uniform distribution within the fiber web, the difference between the first mixing ratios in each region is not large.

[0123] Here, the value of the first mixing ratio by the first surface area is SP EF , the value of the first mixing ratio by the second surface area is MP EF , the value of the first mixing ratio by the internal area is CP EF can be expressed as , respectively.

[0124] According to this embodiment, the fiber sheet (1) has a first mixing ratio value SP in the first surface area, the second surface area, and the internal area. EF , MP EF , and CP EFThe deviation of the first mixing ratio in each region can be formed to be 50%P (percentage point) or less. That is, the difference in the first mixing ratio in each region can be a deviation of 0.1 to 50%P, preferably 0.1 to 30%P or less, and more preferably 0.1 to 15%P or less. In particular, it can be understood that the smaller the deviation between ratios, the more uniformly the electrospun fibers (1b) are distributed relatively throughout the entire thickness direction of the sheet, and as an example, can be formed with a deviation of about 10%P or less.

[0125] According to the experimental example described above, when the composite fiber nonwoven fabric of the present invention is measured for each area, the first mixing ratio value in the first surface area is SP EF is about 36%, and the first mixing ratio in the internal area is MP EF CP, which is the first mixing ratio in the second surface area, is about 31% EF was detected at approximately 28%.

[0126] That is, in this embodiment, the fiber sheet (1) was found to have a maximum difference of 8%P per region. In this way, it was confirmed through measurement experiments that each region had a deviation of less than 10%.

[0127] In particular, in the case of conventional nonwoven fabrics manufactured by conventional composite spinning, the fibers produced by electrospinning do not smoothly penetrate into the interior of the fiber web, but are mixed near the surface and formed with an uneven distribution. Therefore, although the outer surface of the nonwoven fabric contains a large amount of nano-sized fibers produced by electrospinning, the middle region or the inner surface contains only a very small amount of nano-sized fibers. Due to this uneven distribution, the actual micro-sized fiber layer and the nano-sized fiber layer tend to exist as separate regions. At this time, in the case of conventional nonwoven fabrics, there is a problem that actual layer separation occurs in the cross-sectional thickness direction, and there is a problem that the performance difference occurs in each region of the nonwoven fabric due to the uneven distribution in the surface portion according to the width direction or length direction.

[0128] On the other hand, since the composite fiber nonwoven fabric of the present invention is formed to have a uniform distribution even when the fiber content is adjusted to suit the usage environment or purpose required for each industrial field, the electrospun fibers (1b) can be present at an appropriate mixing ratio with little deviation in the positions of each region in the cross-sectional thickness direction of the fiber sheet (1). Accordingly, the present invention can be utilized as a nonwoven fabric product exhibiting uniform characteristics.

[0129] In this way, the present invention can provide a nonwoven fabric having a high content of meltblown fibers (1a) in the fiber sheet (1) or a nonwoven fabric having a relatively high content of electrospun fibers (1b), and in this case, the present invention can be formed so that the first mixing ratio of electrospun fibers (1b) is uniformly distributed throughout the nonwoven fabric, regardless of the content of the electrospun fibers (1b).

[0130] In this way, the composite fiber nonwoven fabric of the present invention has mechanical strength and functionality according to the respective characteristics of the meltblown fiber (1a) and the electrospun fiber (1b).

[0131] For purposes of appropriately imparting these properties, the nonwoven fabric of the present invention can be used, for example, in sound-absorbing materials, filtering materials, medical materials, etc. For example, when the composite fiber nonwoven fabric according to the present embodiment is used as an NVH material for automobiles, each spinning solution may be composed of polypropylene (PP) or polyethylene terephthalate (PET). Additionally, polyimide (PI) may be used as a suitable material.

[0132] When the nonwoven fabric of the present invention is used as an NVH material for automobiles to absorb vibration or noise, it is designed to prevent various vibration noises transmitted from the engine or motor, drive system, and body of the vehicle.

[0133] According to this embodiment, the composite fiber nonwoven fabric of the present invention can have sound absorption properties at a specific frequency.

[0134] The following is an example of a characteristic experiment conducted on sound-absorbing materials.

[0135] The composite fiber nonwoven fabric of the present invention was prepared as a sound-absorbing material of a specific size, and sound-absorbing characteristics were compared with existing products using a sound-absorbing performance measuring device commonly known as Alpha Cabin. The sound-absorbing materials used in this example are a combined sound-absorbing material having a structure in which the nonwoven fabric of the present invention is laminated to a base pad by heat bonding (Example A), and a base pad in its original state (Example B).

[0136] Table 3 below shows the sound absorption characteristics of samples utilizing composite fiber nonwoven fabric as an absorbent material, as measured through experimental examples. Data from 400 to 4,000 Hz were selectively used among the entire measurement range. This band is included in the ranges distinguished during human hearing tests, and can be included in the low-frequency range of 400 to 1,000 Hz, the mid-frequency range of 1,000 to 3,150 Hz, and the high-frequency range of 2,000 to 5,000 Hz, which are included in the audible frequency range.

[0137] FrequencySound Absorption CoefficientHzExample AExample BComparative Example AComparative Example BComparative Example CComparative Example DComparative Example E4000.5130.4800.0000.1900.4600.4100.2404500.6980.6250.0000.2560.5650.4800.3205000.8960.7730.0300.3250.6830.5500.4005650.9870.8380.0700.4300.7800.6250.4306301.0820.9050.1200.5450.8780.7000.4607151.1170.95 00.1520.6340.9700.7700.5208001.1571.0100.1840.7161.0650.8400.5809001.1901.0830.1860.7821.1350.9500.66510001.2231.1700.1900.8521.2001.0600.75011251.2111.2300.2000.9421.2301.1300.79012501.2061.2830.2021.01 61.2501.2000.83014251.1871.2400.1721.0161.2501.2750.91516001.1731.1880.1461.0161.2451.3501.00018001.1601.1530.1301.0781.2301.2701.01520001.1431.1230.1101.1501.2201.1901.03022501.1631.0350.1161.1901.1801. 1701.01525001.1850.9530.1201.2151.1451.1501.00028251.0850.9080.0841.1461.1051.2001.05031500.9890.8650.0501.1001.0651.2501.10035750.9780.8880.0301.0681.0601.2201.07540000.9670.9170.0001.0501.0401.1901.050

[0138] Referring to Table 3 above, it can be seen that the sound-absorbing material using the nonwoven fabric according to the present invention (Example A) shows excellently improved sound-absorbing characteristics across the entire range compared to the general sound-absorbing pad (Comparative Example A). That is, it can be confirmed that the sound-absorbing performance is improved in the audible frequency band including the low-frequency and high-frequency bands by using the sound-absorbing material having a single-layer structure according to the present invention. Meanwhile, according to the present embodiment, the pore size of the fiber sheet (1) of the present invention can be formed to be 0.001 ㎛ to 3.0 ㎛. That is, the pore size refers to the gap formed between the meltblown fiber (1a) and the electrospun fiber (1b). Depending on the pore size, different filtration or sound-absorbing characteristics can be exhibited.

[0139] These composite fiber nonwoven fabrics have various porosities formed by randomly distributing relatively thin-diameter electrospun fibers (1b) between relatively thick-diameter meltblown fibers (1a).

[0140] Accordingly, when the composite fiber nonwoven fabric of the present invention is used as a sound-absorbing material, it can provide an excellent sound-insulating effect, and when used as an air filter, it can remove particles of various particle sizes, thereby providing excellent filter performance.

[0141] In addition, the composite fiber nonwoven fabric of the present invention can provide a predetermined air layer through each pore of the fiber sheet (1).

[0142] For example, in a vehicle environment where sound-absorbing materials are used, the characteristics of nonwoven fabrics are designed to be different in consideration of air-borne noise, which is gas noise, and structure-borne noise, which is solid noise. The present invention requires noise-blocking characteristics due to the air layer structure described above.

[0143] In addition, the composite fiber nonwoven fabric of the present invention can be formed such that the second mixing ratio (weight%) of the electrospun fiber (1b) in the fiber web according to the measured weight of the fiber sheet (1) is 1 to 50 weight% of the total measured weight of 100 weight%.

[0144] The composite fiber nonwoven fabric of the present invention contains a mixture of meltblown fibers (1a) and electrospun fibers (1b). A method for separating these fibers and measuring their weight includes a method of separating them by dissolving the electrospun fibers (1b) in a solvent. Through this method, the weight of the electrospun fibers (1b) (in addition to the weight of the meltblown fibers) can be confirmed within the total weight of the fiber sheet (1).

[0145] The following shows the average diameter (Table 4) and density (Table 5) according to the surface area of ​​the electrospun fibers (EF).

[0146] EF Surface Area RatioNanofiberAverage Diameter(um)32.1%300400500600700800Nanofiber Incorporation Ratio(wt.%)527.1%21.8%18.3%15.7%13.8%12.3%1044.0%37.1%32.1%28.2%25.2%22.8%1555.5%48.4%42.8%38.4%34.9%31.9%2063.9%57.0%51.5%46.9%43.1%39.9%2570.2%63.9%58.6%54.1%50.3%46.9%3075.2%69.5%64.5%60.3%56.5%53.2%

[0147] EF Surface Area RatioNanofiberPolymer Density32.1%0.80.91.01.11.21.3Microfiber Diameter(㎛)2,50039.0%36.2%33.8%31.7%29.9%28.2%3,00043.4%40.5%38.0%35.8%33.8%32.1%3,50047.2%44 .3%41.7%39.4%37.4%35.5%4,00050.5%47.6%45.0%42.6%40.5%38.6%4,50053.5%50.5%47.9%45.5%43.4%41.4%5,00056.1%53.2%50.5%48.2%46.0%44.0%

[0148] At this time, the present invention can form a second mixing ratio (weight %) between each region within an appropriate range. For example, the second mixing ratio, similar to the first mixing ratio described above, can have a deviation of 0.1 to 50%P or less for each region. Preferably, it can be formed to be 0.1 to 30%P or less, and more preferably 0.1 to 15%P or less. That is, since the present invention forms the electrospun fiber (1b) to have a uniform distribution, the mixing ratio according to weight appears within a range where the deviation is not large for each region. Accordingly, a product utilizing the composite fiber nonwoven fabric of the present invention can stably exhibit uniform performance.

[0149] In addition, in this embodiment, the fiber sheet (1) can be formed so that the surface area ratio by the electrospun fibers (1) measured in the first surface area, the second surface area, and the internal area, respectively, is 20% to 55% of the total area. In this case, the specific surface area by the meltblown fibers (1a) is 1 m 2 / g to 3 m 2 / g, and the specific surface area by electrospun fiber (1b) is about 5 m 2 / g to 7 m 2 / g may be.

[0150] (Surface area ratio calculation example 1)

[0151] For example, in a state where the electrospun fiber is 10 wt% of the total weight of the fiber sheet (1), the meltblown fiber is a PP material with a density of 0.92 g / cm. 3 , the average diameter is 3㎛, and the electrospun fiber is made of PI material and has a density of 1.3 g / cm. 3 And when the average diameter is 0.5㎛, the surface area ratio of the meltblown fiber and the electrospun fiber is 67.9%: 32.1%.

[0152] And, when the average diameter of the melt-blown fiber (1a) of the fiber sheet (1) is 3 ㎛ and the average diameter of the electrospun fiber (1b) is 0.5 ㎛, the specific surface area by the melt-blown fiber (1b) is about 1.45 m 2 / g, and the specific surface area by electrospun fiber (1b) is about 6.15 m 2 / g can be formed.

[0153] Each surface area ratio and specific surface area are calculated results based on the image size measured from the electron microscope image of Fig. 2.

[0154] Generally, a larger specific surface area results in a larger surface area, enhancing the interactivity of the nonwoven fabric. This, in turn, enhances material absorption, energy storage, filtration, chemical reactions, and thermal conductivity. Furthermore, a higher specific surface area tends to decrease dimensional stability, while a lower specific surface area can improve dimensional stability. The specific surface area can be controlled by varying the fiber diameter.

[0155] Here, the surface area ratio increases by increasing the incorporation rate of electrospun fibers or decreasing the average fiber diameter. This can also be achieved by adjusting the density of the electrospun fiber raw material (increasing the ratio when the density decreases). The following explains the change in surface area ratio according to changes in the average fiber diameter.

[0156] (Surface area ratio calculation example 2)

[0157] Under the same conditions as in the above calculation example 1, when the average diameter of the electrospun fibers is measured as 0.2 ㎛, the surface area ratio of the meltblown fibers and the electrospun fibers is 45.9%: 54.1%. The specific surface area of ​​the electrospun fibers at this time is approximately 15.4 m 2 / g can be formed.

[0158] (Surface area ratio calculation example 3)

[0159] Under the same conditions as in the above calculation example 1, when the average diameter of the electrospun fibers is measured as 0.3 ㎛, the surface area ratio of the meltblown fibers and the electrospun fibers is 56.0%: 44.0%. At this time, the specific surface area of ​​the electrospun fibers is approximately 10.3 m 2 / g can be formed.

[0160] (Surface area ratio calculation example 4)

[0161] Under the same conditions as in the above calculation example 1, when the average diameter of the electrospun fibers is measured to be 0.7 ㎛, the surface area ratio of the meltblown fibers and the electrospun fibers is 74.8%:25.2%. The specific surface area of ​​the electrospun fibers at this time is approximately 4.4 m 2 / g can be formed.

[0162] (Surface area ratio calculation example 5)

[0163] Under the same conditions as in the above calculation example 1, if the average diameter of the electrospun fibers is 0.5 ㎛ and the average diameter of the meltblown fibers is measured as 2 ㎛, the surface area ratio of the meltblown fibers and the electrospun fibers is 76.1%: 23.9%. At this time, the specific surface area of ​​the meltblown fibers is approximately 2.2 m 2 / g can be formed.

[0164] (Surface area ratio calculation example 6)

[0165] Under the same conditions as the above calculation example 1, if the average diameter of the electrospun fibers is 0.5 ㎛ and the average diameter of the meltblown fibers is measured as 4 ㎛, the surface area ratio of the meltblown fibers and the electrospun fibers is 61.4%: 38.6%. At this time, the specific surface area of ​​the meltblown fibers is approximately 1.1 m 2 / g can be formed.

[0166] Furthermore, while the surface area ratio can be controlled by fiber diameter as described above, it can also be achieved by controlling the amount of electrospun fibers incorporated. This can be achieved by controlling the amount of assist air or by changing manufacturing conditions.

[0167] The composite fiber nonwoven fabric according to one embodiment of the present invention configured as described above can be provided as a single-layer structured fiber web in which electrospun fibers are uniformly distributed between meltblown fibers, and as a result, both fibers are uniformly distributed and mixed at all locations according to the overall area and thickness direction of the fiber sheet (1), thereby preventing performance degradation due to distribution deviation and providing uniform performance at each location.

[0168] In other words, the composite fiber nonwoven fabric of the present invention is manufactured by the manufacturing device or manufacturing method described below, and at this time, conditions are set so that meltblown fibers and electrospun fibers can be distributed in a preset ratio depending on the product to which the nonwoven fabric is applied, and since the present invention has a small distribution deviation by area, it is possible to configure a fiber web within the required specifications, and thus it is possible to provide a nonwoven fabric that exhibits uniform performance.

[0169] The composite fiber nonwoven fabric of the present invention can be utilized as a filter material. The functional characteristics of the present invention related to filtration efficiency will now be described. For example, different characteristics may be exhibited depending on the amount of electrospun fiber incorporated.

[0170] First, in the case where a large amount of nano-sized fibers are mixed and distributed in the fiber web of the nonwoven fabric (for example, when most of the fibers are composed of nano-sized fibers), it has the characteristic of high dust collection performance, that is, high filtration efficiency, because it can provide a relatively small pore size compared to micro-sized fibers. However, due to the small pore size, the basic differential pressure is high, and the area where the introduced particles are captured increases, so there is a disadvantage in that the flow rate of the filter is greatly reduced, and because the differential pressure is high, the filter replacement cycle is relatively shortened, and because the strength is weak, it is limited in using it alone.

[0171] In contrast, when a large number of micro-sized fibers are mixed and distributed, the pressure differential is less restrictive, but filter performance is relatively degraded. This often requires special processing to improve performance. In particular, nonwoven fabrics subjected to special processing, such as electrostatic treatment, exhibited a significant decline in filter performance over time.

[0172] Accordingly, the present invention provides a composite fiber nonwoven fabric composed of a fiber web in which micro-sized and nano-sized fibers are mixed.

[0173] Meanwhile, a composite fiber manufacturing device according to one embodiment of the present invention is for forming a composite fiber web, which is a fiber aggregate, and may be configured to include a first spinning unit (10), a second spinning unit (20), and a collecting unit (30), as illustrated in FIGS. 4 to 6. That is, the composite fiber manufacturing device of the present invention includes a first spinning unit (10) that discharges a first spinning solution in a meltblown manner, a second spinning unit (20) that discharges a second spinning solution in an electrospinning manner to the first spinning solution discharged from the first spinning unit (10), and a collecting unit (30) in which the first spinning solution and the second spinning solution are collected together.

[0174] Specifically, the first radiation unit (10) is provided to discharge the first radiation solution by a melt-blown radiation method. This first radiation unit (10) includes a first nozzle (11) for discharging the first radiation solution, and the first nozzle (11) is arranged in a first direction (F1) to discharge the first radiation solution along the first direction (F1).

[0175] Here, the first radiation unit (10) may include a configuration of a typical meltblown radiation system, and may be provided as a vertical type system that is arranged perpendicular to the ground or a horizontal type system that is arranged in a direction parallel to the ground. Accordingly, the first radiation unit (10) may have a different first direction (F1) in which the solution is to be discharged depending on whether the radiation system is formed as a vertical or horizontal structure, but may be determined as a direction that is arranged perpendicular to the surface side of the collecting unit (30). For example, as an exemplary form in the present embodiment, the first radiation unit (10) may be provided as a structure of a horizontal meltblown radiation system, and at this time, the first nozzle (11) of the first radiation unit (10) is arranged perpendicular to the collecting unit (30), so that the solution can be discharged in a horizontal discharge direction by being arranged in a horizontal installation direction in the drawing. That is, the first direction (F1) means the direction placed along the X-axis toward the capturing unit (30) arranged in the Y-axis direction in the drawing.

[0176] In this way, the first radiation unit (10) is provided to have a flow in a vertical direction with respect to the collection unit (30) and functions to discharge the first radiation solution, and the first radiation solution discharged from the first radiation unit (10) is discharged in a melt-blown manner. Accordingly, the first radiation unit (10) can provide a first stream (12) in which the first radiation solution is discharged in the first direction (F1).

[0177] The first radiation unit (10) forms a fiber by passing a polymer melt that has been melted at a high temperature through a first nozzle (11) composed of fine holes, and then applies a high-temperature, high-pressure process gas to discharge the fibers so that they are captured in the form of a web in a collection unit (30). That is, the melt-blown method used in the first radiation unit (10) relates to a method of melting a thermoplastic polymer and extruding and spinning it through a nozzle, and since it is a well-known technique that can be easily implemented by those skilled in the art, a detailed description thereof is omitted in one embodiment of the present invention so as not to obscure the gist of the invention.

[0178] The second radiation unit (20) is provided to discharge the second radiation solution by electrospinning. This second radiation unit (20) includes a second nozzle (21) for discharging the second radiation solution, and the second nozzle (21) is arranged in a direction crossing the flow in the first direction (F1) to discharge the second radiation solution. As will be described later, for example, the second nozzle (21) may be arranged in the second direction (F2) to discharge the second radiation solution along the second direction (F2). At this time, the second radiation unit (20) can directly set the discharge direction of the second radiation solution by the angle at which the second nozzle (21) is installed, but an air supply (not shown) that supplies separate assistant air may be arranged adjacent to the second nozzle (21) to indirectly guide and control the flow of the second radiation solution by air. For example, the air supply unit may be provided as a dual-nozzle structure integral with the second nozzle (21) to control the flow of the second radiation solution. That is, in the present embodiment, the direction or angle at which the second nozzle (21) of the second radiation unit (20) is installed refers to the direction or angle with respect to the radiation flow discharged through the second nozzle (21).

[0179] Here, the second radiation unit (20) may include a configuration of a typical electrospinning system, and may be installed between the first radiation unit (10) and the collection unit (30) to be spaced apart from the flow of the first radiation solution. That is, the second radiation unit (20) functions to discharge the second radiation solution by electrospinning to the first radiation solution discharged from the first radiation unit (10), and in particular, functions to discharge the second radiation solution in a direction intersecting with the flow of the first radiation solution. Accordingly, the second radiation unit (20) may provide a second stream (22) in which the second radiation solution is discharged in a direction intersecting with the first direction (F1).

[0180] The second radiation unit (20) applies a high voltage when the second radiation solution, which is a polymer solution, is spun into fibers, thereby discharging nanofibers having a fiber diameter of less than micrometers to be captured in the collection unit (30). That is, the electrospinning method used in the second radiation unit (20) refers to a method of generating a liquid material into micro- or nano-sized fibers through an electric field generated at a high voltage, and is a well-known technique that can be easily implemented by those skilled in the art. Therefore, in one embodiment of the present invention, a detailed description thereof is omitted in order to avoid obscuring the gist of the invention.

[0181] The collecting unit (30) relates to a device for collecting the first and second spinning solutions, and may be provided as a flat-plate collector or a cylindrical collector. Since the collecting unit (30) is a well-known technology that can be easily implemented by those skilled in the art, a detailed description thereof is omitted in one embodiment of the present invention so as not to obscure the gist of the invention. For example, the collecting unit (30) in this embodiment may be provided as a flat-plate collector, and a suction is provided on the lower surface of the collector so that the collected spinning solutions can settle on the surface of the collector. The collecting unit (30) may be configured to transport the fiber layer collected on one side while the collector is circulated in one direction by a conveyor. The fiber layer collected on the surface of the collector is formed as a non-woven fabric layer.

[0182] According to the present embodiment, the second radiation unit (20) may be set at a position for discharging the second radiation solution so that the second radiation solution can intersect with the first radiation solution before the first radiation solution reaches the collection unit (30). At this time, the installation position is a word encompassing the angle and height of the second radiation unit (20). It is preferable that the angle of the second radiation unit (20) be arranged toward the first stream (12) so that the second radiation solution discharged from the second radiation unit (20) intersects with the first radiation solution.

[0183] In this way, the meltblown fibers and electrospun fibers can go through a mixing process where they are evenly mixed through cross flow.

[0184] Finally, according to the present embodiment, since the electrospun fiber stream can be appropriately mixed into the meltblown stream by the double nozzle applying the assistant air, it is possible to manufacture a nonwoven fabric in which the electrospun fibers are uniformly distributed.

[0185] These composite fibers, with relatively fine electrospun nanofibers randomly distributed among relatively thick meltblown fibers, form a variety of porosities, enabling them to provide superior sound-insulating properties when used as sound-absorbing materials. Furthermore, when used as air filters, they can remove particles of various sizes, offering superior filtration performance.

[0186]

[0187]

[0188]

[0189]

[0190] Hereinafter, a method for manufacturing a composite fiber nonwoven fabric using a composite fiber web according to one embodiment of the present invention will be exemplarily described. Fig. 7 illustrates a flow chart of a method for manufacturing a composite fiber web using a composite fiber manufacturing apparatus according to one embodiment of the present invention.

[0191] This manufacturing method is described in a series of steps with reference to FIGS. 6 and 7 as follows.

[0192] In the first step (S110), the first nozzle of the first radiation unit (10) may be used to form a first stream by discharging the first radiation solution to one side using a melt-blown method.

[0193] In the second step (S120), the second nozzle of the second radiation unit (20) may be used to form a second stream by ejecting the second radiation solution toward the first stream using an electrospinning method.

[0194] In the third step (S130), the first stream and the second stream may be crossed and the first spinning solution and the second spinning solution may be mixed in a web structure.

[0195] In the fourth step (S140), the mixed stream may be captured in a capture unit (30).

[0196] According to the present invention, by applying assistant air to the second stream by the second radiation unit (20) in the second and third steps, the second stream, which has relatively weak straightness, is given straightness, thereby solving the existing problem of difficulty in penetrating into the interior of the first stream, thereby enabling the second spinning solution to be smoothly mixed with the first spinning solution, and thus the fiber sheet (1) is characterized in that the electrospun fibers (1b) can be mixed with a uniform distribution.

[0197] Specifically, according to the present invention, the first radiation section (10) and the second radiation section (20) of the above-described manufacturing device are compositely arranged to form a fiber sheet (1).

[0198] The raw material used as the spinning solution of the first radiator (10) may be provided as PP or PET. The first radiator (10) may have a plurality of nozzles (e.g., 501) arranged with a diameter size of 0.3 mm. At this time, the first radiator (10) may provide the temperature of the spin beam under a set condition of about 280°C. The discharge amount by the first radiator (10) is 100 g / min on average, has an air discharge amount of 6 CMM (㎥ / min), and the hot air temperature may be set to a maximum of about 300°C. The first radiator (10) may be arranged so that the distance between the nozzle and the collecting unit (30) is about 890 mm. This first radiator (10) may discharge the spinning solution by a melt-blown method under the condition of a line speed of 1.6 m / min.

[0199] And, the raw material used as the spinning solution of the second spinning unit (20) can be provided as PVA. The second spinning unit (20) can be set to have an average discharge amount of 1 g / min (regulator: 6 kgf / ㎠). Here, the second spinning unit (20) can be arranged so that the stream and nozzle of the first spinning unit (10) are spaced apart by an interval of about 500 mm. This second spinning unit (20) discharges the solution by an electrospinning method under a high voltage condition of 45 KV.

[0200] At this time, the second radiation unit (20) can discharge the electrospinning solution in a straight line by an air supply unit that supplies assistant air. In the second radiation unit (20), the assistant air can be discharged at a condition of about 200 LPM (l / min).

[0201] In this way, according to the manufacturing method of the present invention, as meltblown fibers (1a) formed by meltblown spinning through the first spinning unit (10) and electrospun fibers (1b) formed by electrospinning (or electrostatic spinning) through the second spinning unit (20) are spun while crossing each other, heterogeneous fibers (different in size or material) can be mixed and mixed in a fiber form.

[0202] Meanwhile, unlike the above, the second radiating unit (20) may emit assistant air under the condition of about 400 LPM, and the setting range of the assistant air may be set to 100 LPM to 700 LPM. Preferably, it may be set to a range of 200 LPM to 500 LPM. Here, if the setting value of the air of the second radiating unit (20) is less than 100 LPM, the straightness of the electrospinning solution is not properly provided, so there is a problem that it is not actually injected into the inside of the first stream by the first radiating unit (10), and if it exceeds 700 LPM, a problem that affects the flow or direction of progress of the first stream may occur, so it is preferable to set it within an appropriate range.

[0203] Meanwhile, according to the present embodiment, the second radiation unit (20) can be formed so that the flow of the second radiation solution is opposite to the flow direction of the first radiation solution. That is, the second radiation unit (20) can be arranged so that the discharge direction of the second nozzle (21) has a directionality opposite to the first direction (F1), thereby forming a second stream (22) that intersects the first stream (12) and is opposite to the first direction (F1), which is the direction in which the first stream (12) is traveling.

[0204] For example, the second nozzle (21) may be arranged so that its end faces the second direction (F2). Accordingly, the present invention can increase the mixing action between the spinning solutions by causing resistance to the first stream (12) compared to the existing vertical cross flow.

[0205] For this purpose, the second radiator (20) can be arranged so that the second nozzle (21) is inclined at a predetermined angle toward the first nozzle (11) of the first radiator (10).

[0206] Although not shown, the second radiation unit (20) is characterized in that it is arranged to be inclined at a predetermined angle toward the nozzle end of the first radiation unit (10) at a position perpendicular to the flow of the first radiation solution, so as to discharge the second radiation solution. That is, the second radiation unit (20) can be arranged along the second direction (F2) by tilting at a predetermined angle (α°) in the direction toward the first nozzle (11) of the first radiation unit (10) from a discharge position in the vertical direction with respect to the first stream (12).

[0207] That is, referring again to FIGS. 4 and 5, the second radiating portion (20) can be configured to allow the installation position or angle of the assistant air nozzle to be adjusted.

[0208] According to an exemplary form, when the installation position of the nozzle arranged corresponding to the first direction on the imaginary line (II) parallel to the imaginary line (I) for the discharge direction of the first stream (12) discharged in the first direction from the first nozzle (11) is 0°, and the discharge position in the vertical direction with respect to the first stream (12) at that point is at an angle of 90°, the second radiating portion (20) can be set so that the discharge angle of the second nozzle (21) is formed at 115° to 155°. Preferably, it can be set at 128° to 142°, and as an example, it can be set at a discharge angle of about 135°. That is, the second stream (22) is formed to be inclined at an angle of about 45° from the vertical position.

[0209] Here, the second radiator (20) may have somewhat reduced mixing properties due to mixing on the surface of the stream, similar to the existing vertical discharge structure, when the discharge angle of the second nozzle (21) is less than 115°, and when it exceeds 155°, the discharge distance to reach the first stream (12) increases, which causes structural limitations and may cause problems in that it may directly reach the first nozzle (11) depending on the installation location. Therefore, the discharge angle may be set within an appropriate range.

[0210] In this way, the second radiation unit (20) is placed in the opposite direction to the emission direction of the first radiation solution, and the nozzle is arranged in a diagonal direction intersecting with the first radiation solution rather than a direction intersecting perpendicularly to the first radiation solution, thereby emitting the second radiation solution.

[0211] At this time, the first radiation solution generally tends to scatter in the direction of travel of the second radiation solution after the second radiation solution reaches it, but since the discharge flow rate of the first radiation solution is relatively large, it can smoothly proceed in the original discharge direction of the first radiation solution, and the second radiation solution can be mixed into the first stream (12) that has a straight line, thereby reducing the occurrence of scattering.

[0212] By this discharge structure in the direction of the reverse line, the scattering of fibers is minimized, and the second spinning solution can go through a mixing process in which it is evenly mixed with the first spinning solution. In other words, rather than being discharged only on the outer surface of the first stream (12) as before, it is discharged in a direction opposite to the direction of travel of the first stream (12), thereby improving the internal penetration effect of the fibers.

[0213] Ultimately, the second stream (22) by the second radiation unit (20) is discharged in the direction of the history line and flows into the first stream (12), so that the second radiation solution can smoothly penetrate into the interior of the first stream (12), and the second radiation solution is uniformly mixed with the first radiation solution and captured together in the capture unit (30).

[0214] In this way, according to the composite fiber manufacturing device according to one embodiment of the present invention, the electrospinning stream is configured to have a discharge structure in a counter-clockwise direction rather than a direction orthogonal to the meltblown spinning stream, so that the second stream (22) is discharged in a direction opposite to the discharge direction of the first stream (12), thereby inducing smoother mixing than in the case of the conventional cross-direction vertical discharge direction, thereby improving the mixing property.

[0215] Therefore, according to the present invention, since the electrospun fibers can more smoothly penetrate between the meltblown fibers, the mechanical properties of the composite fiber nonwoven fabric used as a sound-absorbing material can be further improved.

[0216] In addition, according to the present embodiment, the second radiation unit (20) is characterized in that the second radiation solution discharged from the second nozzle (21) reaches the first radiation solution at a location adjacent to the first nozzle (11). Accordingly, the second radiation solution can be thermally entangled with the first radiation solution of the first radiation unit (10). Here, entanglement means a form in which fibers are entangled.

[0217] To elaborate, when the position of the intersection where the first and second radiation solutions meet in the existing vertically arranged radiation structure is referred to as the vertical intersection point (O), in the case of this embodiment, the first intersection point (A) is formed at a position retreating toward the nozzle side along the emission direction of the first radiation portion (10).

[0218] That is, the second stream (22) discharged by the second radiation unit (20) intersects at a position close to the first nozzle (11) from which the first radiation solution is discharged by the thermal melting method, thereby forming a first intersection point (A), thereby allowing the second radiation solution to be mixed with the first radiation solution, which is at a relatively high temperature compared to several points located in the entire length direction of the first stream (12).

[0219] Accordingly, according to the present invention, since the thermal entanglement phenomenon occurs at a higher temperature than in the structure of a conventional mixed fiber manufacturing device in the entanglement action of cross-spun fibers, the second spinning solution can be stably adsorbed and then cooled and solidified in the process of fiberizing and extruding the first spinning solution, which is a polymer material, thereby further improving the fixing force between the fibers. At this time, the second spinning solution is mixed at a relatively high temperature with respect to the first spinning solution that is extruded while retaining thermal energy due to thermal melting, so that stable mixing and fixing can be achieved over a sufficient period of time.

[0220] In other words, according to the present embodiment, the second radiation unit (20) forms a first intersection point (A) where the second stream (22) and the first stream (12) meet at a location close to the first nozzle (11), and ejects the second radiation solution in a reverse direction with a predetermined incline rather than a vertical direction with respect to the first stream (12), thereby simultaneously improving the fixing force and mixing property.

[0221] In this way, the present invention is such that the intersection point occurs at a position close to the first nozzle (11) of the first radiation unit (10), so that the stream directly discharged from the first radiation unit (10) can be mixed and smoothly proceed in the normal direction of progression of the first radiation solution.

[0222] At this time, the temperature at the intersection point may be formed differently depending on the discharge distance of the meltblown stream, and if it is formed close to 100% of the actual discharge temperature (melt radiation temperature) at a location close to the nozzle, mixing may be performed at a temperature that gradually decreases depending on the distance. For example, the mixed temperature may be formed in the range of 80% to 100% of the discharge temperature at a location close to the nozzle, in the temperature range of 20% to 80% near the middle position with the collector, and in the temperature range of 1% to 50% at a location close to the collector.

[0223] On the other hand, the second radiator (20) can be simply moved and arranged in a vertical cross state rather than a reverse cross state to form an intersection point adjacent to the first nozzle (11), but in this case, the problem of the existing vertical structure in which mixing occurs only on the outer surface is not solved, so there is a problem in that smooth mixing does not occur.

[0224] In particular, in such a conventional vertical discharge structure, even if the mixing action is increased by increasing the flow rate or moving the nozzle position, there is a problem that the stream flows in a specific direction when the flow rate increases, and since the discharge time and discharge distance are relatively shortened, there is a problem that the fiberization of the spinning solution by electrospinning is not completed normally, and since the separation distance between the nozzles on both sides is shortened, the flying fibers generated during the crossing of the streams can directly affect the nozzle, and in severe cases, the problem remains that they can block the nozzle hole.

[0225] The present invention provides a method to prevent this by appropriately maintaining the flow rate and mutual separation distance of each radiating section.

[0226] Therefore, according to this embodiment, even without increasing the flow rate, fiber scattering is minimized during manufacturing, and mixing is improved, so that composite fibers exhibiting a uniform fiber volume content can be manufactured.

[0227] In addition, the present invention can reduce the occurrence of flying fibers that fall without being captured by the capturing unit (30) due to a decrease in scattering.

[0228] According to this embodiment, the relative influence of the assistant air guiding the discharge direction of the second radiation solution varies depending on the location of the point where the first radiation solution and the second radiation solution intersect on the path of the first stream (12). In addition, the flow may also vary depending on the discharge power of the first radiation solution by the process gas of the first radiation unit (10).

[0229] For example, in the composite fiber manufacturing device of the present invention, when the first radiating section (10) and the capturing section (30) are arranged at a distance of about 1,000 mm, the distance (H) of the second radiating section (20) with respect to the first stream (12) can be arranged at about 300 mm. Referring to the drawing, the distance (H) is illustrated based on the rear end of the second nozzle (21), but may also be the distance from the front end of the second nozzle (21).

[0230] Accordingly, since the second stream (22) is formed with a discharge distance that is relatively short compared to the total length that the first stream (12) reaches from the first radiating portion (10) to the collecting portion (30), the second nozzle (21) is positioned at a distance where the assistant air affects part or a significant part of the first stream (12).

[0231] At this time, even if the second radiator (20) is arranged with the same distance as in the conventional vertical direction with respect to the first stream, the second nozzle (21) is installed at an angle so that the discharge distance of the second stream (22) is extended, thereby reducing the direct influence of the assistant air on the first stream (12).

[0232] In other words, the present invention has the advantage of reducing the influence of assistant air and increasing the flow rate while increasing the discharge distance relatively when the separation distance (H) is formed to the same length as the existing vertical structure, and even when installed to be spaced at a shorter distance compared to the vertical structure, it has the advantage of securing an appropriate discharge distance due to the inclined discharge direction.

[0233] Moreover, as described above, the present invention improves the flow rate discharged from the second radiation unit (20) by forming the first intersection point (A) close to the first radiation unit (10), or even if the second radiation solution is discharged at a position where the distance from the first stream (12) is shortened, the second radiation solution can be mixed at a position with a relatively high temperature and high discharge power among several points of the first stream (12), thereby inducing smooth mixing of the first radiation solution and the second radiation solution.

[0234] In addition, according to the present invention, since the two streams intersect at a position close to the first nozzle (11) as described above, the first stream (12) is introduced by the original discharge power of the straight-line stream, so that the second stream (22) can be prevented from affecting the direction of travel of the first stream (12) according to the flow rate or discharge distance set in the second radiating portion (20). That is, the present invention can solve the problem of not being able to increase the flow rate above a certain limit in order to prevent the stream from becoming disordered in the past.

[0235] Meanwhile, according to the present embodiment, the second radiating portion (20) may be formed such that the second length (L2) indicating the distance between the second nozzle (21) and the collecting portion (30) is shorter than the first length (L1) indicating the distance between the second nozzle (21) and the first nozzle (11) in the first direction. That is, the second nozzle (21) may be installed relatively closer to the collecting portion (30) than to the first radiating portion (10) based on the midpoint of the total length (L0) of the first stream (12) discharged in the first direction (F1) placed in the X-axis direction.

[0236] For example, as illustrated in FIG. 5, the position at which the second nozzle (21) of the second radiating portion (20) is installed can be expressed as a distance ratio of the distances L1 and L2 on both sides with respect to the total length (L0) of the first stream (12). The distance ratio (L1:L2) for the installation position can be formed at a ratio of 8 to 5.5: 2 to 4.5, and a preferable distance ratio can be between 6 to 6.5: 4 to 3.5.

[0237] According to this structure, the second radiation solution discharged in the direction of the history line from the second radiation unit (20) has an appropriate separation distance so as not to directly affect the first nozzle (11), and the distance reaching the first radiation solution is increased, so that an easy radiation distance can be secured for the time of fiber formation through electrospinning.

[0238] On the other hand, the composite fiber manufacturing device according to the present embodiment may be configured such that the discharge angle of the second nozzle (21) is variable. That is, the present invention may be configured to further include an angle adjusting unit (not shown) for adjusting the discharge angle of the second nozzle (21).

[0239] The angle adjustment unit may include a first adjustment means (not shown) that directly changes the discharge angle by adjusting the installation angle of the second nozzle (21) and a second adjustment means (not shown) that indirectly changes the discharge angle of the second nozzle (21) by adjusting the supply direction of auxiliary air.

[0240] According to an exemplary form, the first adjusting means may include a rotating shaft and a fixture fixedly installed on one side of the second nozzle (21), and the second nozzle (21) that is rotated by the rotating shaft is fixed at a specific angle by the fixture, thereby adjusting the installation angle to set the discharge angle of the radiation solution. The rotating shaft and the fixture fix the second nozzle (21) in a tiltable manner, but may also fix a part of the system of the second radiation unit (20) including the second nozzle (21) in a tiltable manner as a whole. Here, the rotating shaft and the fixture of the first adjusting means may be a simple hinge-type fixed structure, but may also be provided as a structure that requires a mechanical connection, such as a motor or a hydraulic device. In this way, the first adjusting means directly adjusts the installation angle of the second nozzle (21) to set the discharge angle of the second radiation solution.

[0241] As another exemplary form, the second control means may be configured as an air supply to control the discharge direction of the second nozzle (21). In this case, the second control means may function to set the discharge angle of the second nozzle (21) separately from the first control means (), but may be provided to perform an auxiliary function with respect to the first control means since excessive discharge angle control may be restricted.

[0242] In this way, the angle adjustment unit can tiltably set the discharge direction of the second radiation unit (20), thereby enabling adjustment at an angle to secure a smooth radiation distance corresponding to the relative nozzle spacing. In other words, the manufacturing device of the present invention can resolve installation space constraints and provide a compact structure due to its structure that tilts within a certain range.

[0243] According to the composite fiber manufacturing device according to the embodiment of the present invention configured as described above, a composite fiber can be manufactured in which fibers spun by the electrospinning method penetrate into the fibers spun by the melt blowing method.

[0244] In particular, according to the composite fiber manufacturing device of the present invention, the phenomenon of fiber scattering occurring during the manufacturing process can be minimized, and the mixing action of the composite fibers can be improved, so that a product of composite fibers mixed with a uniform distribution over the entire surface and interior can be manufactured.

[0245] Moreover, the present invention can reduce the occurrence of flying fibers that fall without being captured by the capturing unit (30) due to a decrease in scattering, thereby achieving the effects of cost reduction and increased production.

[0246] In addition, composite fibers manufactured using a composite fiber manufacturing device can improve the mechanical strength of the composite fibers by increasing the fiber volume content.

[0247] On the other hand, unlike the embodiment described above, the second radiating portion (20) may be tilted and arranged at an angle (β°) in the oblique direction opposite to the discharge angle (α°) of the first embodiment, and a product having a mixed shape and characteristics different from the structure in the reverse direction can be produced.

[0248] FIG. 8 is a schematic drawing of an electrospinning section of a composite fiber manufacturing device according to another embodiment of the present invention.

[0249] According to the present embodiment, as illustrated in FIG. 8, the electrospinning unit (120) may be configured such that each nozzle is arranged in a multi-row structure with respect to the base plate (120a). In addition, the electrospinning unit (120) may be configured such that the first flow path (121) and the second flow path (122) are arranged concentrically so as to simultaneously discharge the electrospinning solution and the assistant air. The second spinning unit of the composite fiber web manufacturing device according to this embodiment may be equipped with a flow dual nozzle according to Korean Patent No. 10-1762880.

[0250] Accordingly, interference by fluids discharged from two discharge pipes is prevented, and since both discharge pipes are formed with relatively different sized areas, there is an advantage in that fluids can be discharged while maintaining directivity.

[0251] Figure 9 is a graph showing the fiber composition ratio according to the fiber diameter analysis results for the composite fiber web nonwoven fabric manufactured above.

[0252] Specifically, to analyze the fiber diameter, the surface microstructure of the nanofiber nonwoven product was confirmed using a scanning electron microscope (SEM), and the diameter of 90 nanofibers was measured to determine the average fiber diameter.

[0253] The analysis was performed at the Korea Quality Testing Institute (www.kqti.co.kr), and the SEM analysis device was model JSM7600F.

[0254] In order to analyze the degree to which nanofibers are well distributed within the layer of microfibers, the cross-sectional microstructure of the composite nonwoven fabric was imaged at a magnification of x1,000 using SEM (JSM7600F), and the distribution of nanofibers was evaluated in the vertical direction from the top to the bottom of the cross-section of the composite nonwoven fabric. The total fiber diameter was measured in the cross-sectional microstructure of the upper (surface), middle, and lower (belt) sections, and among them, fibers with a fiber diameter of 1,500 nm or less were defined as nanofibers. The ratio of nanofibers among the total fibers was quantified and compared.

[0255] As exemplary fiber manufacturing conditions, the raw material for meltblown fiber was PP polymer, MI was manufactured under conditions of 800 g / 10 min, and the raw material for electrospun fiber was a solution of 25% nylon mixed with a formic acid solvent.

[0256] Table 6 below shows the results of this fiber diameter analysis. Figure 9 shows the fiber composition ratio graphically.

[0257] Standard (nm) S5B-Surface S5B-Middle S5B-C Surface Fiber Count (EA) 909090 Average Diameter (nm) 3,6983,1784,045 Variance Distribution (CV) 118.19% 85.89% 106.52% NF Count (EA) 322825 NF Ratio 35.56% 31.11% 27.28% MB Ratio 64.44% 68.89% 72.22% NF Incorporation Effect 100.00% 87.50% 78.13%

[0258] In Table 6 above, S5B refers to a composite fiber sample manufactured by mixing and manufacturing nanofibers with meltblown fibers using Process Air to impart straightness. The cross-sectional microstructure of the composite fiber sample was divided into the surface, middle, and C-surface (collector-side surface layer) and SEM analysis was performed. The composite fiber ratio is a value converted by comparing the fiber ratios of the middle and C-surface layers based on the fiber ratio of the surface layer. Based on this fiber diameter analysis, it was confirmed that the nanofibers imparted straightness using Process Air sufficiently penetrated to the opposite surface of the web. In addition, it was confirmed that the mixing ratio of the composite fibers by Process Air sequentially decreased from the surface to the opposite surface to 36%, 31%, and 28%. At this time, the degree and level of mixing of composite fibers in the composite fibers can be controlled by changing the flow rate and velocity of the process air and the amount of spinning discharge. Previously, when the nanofibers of the electrospinning section were mixed into the meltblown nonwoven fabric by the traditional needle-type electrospinning during composite spinning, the nanofibers formed by electrospinning were mixed according to the surrounding fluid flow in the spinning area during meltblown spinning, so it was impossible to give directionality to the nanofibers and they had to follow only the fluid flow of the meltblown spinning, and therefore there was a limitation that the tendency of mixing could not be directly designed, as the nanofibers mostly existed on the surface of the meltblown nonwoven fabric.

[0259] According to this embodiment, since the nanofibers formed by electrospinning in the nanofiber radiation section can be given directionality by using assistant air (or process air), and can be controlled to be mixed with the fluid flow of meltblown radiation at a desired position with a desired force, it was possible to obtain a result in which the nanofiber mixing ratios in the upper, middle, and lower portions of the cross-sectional structure of the composite nonwoven fabric were uniformly measured.

[0260] To ensure the reliability of fiber diameter measurement data, the number of fiber diameter measurements for each sample was measured at least 90, and if possible, at least 100, and the average value of the measured values ​​was used as data.

[0261] The measurement results showed that the ratio of nanofibers was 35.56% on the upper surface (surface) of the composite nonwoven fabric, 31.11% in the middle, and 27.78% in the lower surface (belt), showing a tendency for the content of nanofibers to gradually decrease from the upper surface to the lower surface.

[0262] In this process, which enables forced transport of nanofibers using process air, the nanofiber mixing ratios in both the middle and lower parts are 87% in the middle part and 78.13% in the lower part based on the nanofiber mixing ratio on the surface, confirming excellent penetration of nanofibers into the meltblown nonwoven fabric layer.

[0263] For example, the mixing ratio of the first fiber and the second fiber is characterized by being formed as 60% to 75%: 40% to 25% based on the number of measurements. That is, when the number of fiber diameter measurements is 90, 32 nano-sized fibers of about 1.5㎛ or less can be confirmed on the upper surface of the nonwoven fabric (20 to 45 depending on the measurement position), 28 on the middle surface (15 to 40 depending on the measurement position), and 25 on the lower surface (10 to 35 depending on the measurement position). In this way, the mixing effect of nano-fibers can be enhanced. That is, the meltblown fibers and the electrospun fibers can be present in an appropriately mixed state over the entire area of ​​the composite fiber web, and in particular, the electrospun fibers can be uniformly distributed between the meltblown fiber structures.

[0264] In other words, if air supply is not performed simultaneously during electrospinning, it cannot be stably mixed into the meltblown stream, but according to the present invention, air penetrates into the interior of the meltblown stream to achieve uniform distribution.

[0265] In this way, according to the present invention, it is possible to configure the nanofibers to excellently penetrate into the meltblown nonwoven fabric layer by the assistant air.

[0266] According to one embodiment, in the case of composite radiation, the flow rate may be different depending on the flow rate at the discharge port of each module of the meltblown radiation unit and the electrospinning unit.

[0267] For example, in the case of a meltblown radiation module, when the flow rate is 3,000 L / min, the flow rate is formed as 83.3 m / s, when the flow rate is 4,000 L / min, the flow rate is formed as 111.1 m / s, when the flow rate is 5,000 L / min, the flow rate is formed as 138.9 m / s, when the flow rate is 6,000 L / min, the flow rate can be formed as 166.7 m / s, and according to a preferred embodiment, when the flow rate is 5,000 L / min, the flow rate is formed as 138.9 m / s.

[0268] At this time, the compressed air pressure is 6.5 kgf / cm 2 and the passage area is 6.00 cm 2 , and the force of the fluid can be expressed as 39.0 kgf.

[0269] In addition, in the case of the electrospinning module, when the flow rate is 200 L / min, the flow rate is formed as 61.7 m / s, when the flow rate is 400 L / min, the flow rate is formed as 123.3 m / s, when the flow rate is 500 L / min, the flow rate is formed as 154.1 m / s, and when the flow rate is 600 L / min, the flow rate can be formed as 185.0 m / s. According to a preferred embodiment, when the flow rate is 500 L / min, the flow rate is 154.1 m / s.

[0270] At this time, the compressed air pressure is 6.5 kgf / cm 2 and the passage area is 0.54 cm 2 , and the fluid force can be expressed as 3.5 kgf.

[0271] In this way, the flow rate can be formed more quickly by the electrospinning module, the passage area by the electrospinning module can be formed very narrowly at about 9% of the passage area by the meltblown module, and the fluid force can also be provided in a relatively very weak state at about 9%.

[0272] Meanwhile, a fiber sheet (1) is manufactured by extruding the first and second radiation solutions, which are configured as described above, into fibers by a melt-blown method and an electrospinning method, and the manufactured fiber sheet (1) can be utilized as a biomaterial or a filter material.

[0273] The above description merely exemplifies the technical concept of the present invention. Those skilled in the art will appreciate that various modifications and variations can be made without departing from the essential characteristics of the present invention. Therefore, the embodiments disclosed herein are intended to illustrate, rather than limit, the technical concept of the present invention, and the scope of the present invention is not limited by these embodiments.

[0274] (Explanation of symbols)

[0275] 1: Fiber sheet 1a: Meltblown fiber

[0276] 1b: Electrospun fibers

[0277] 10: First radiator 11: First nozzle

[0278] 12: 1st stream 20: 2nd radiation unit

[0279] 21: Second nozzle 22: Second stream

[0280] 30: Capture Unit

Claims

1. A first fiber formed by a melt blown spinning method; and A composite fiber web comprising second fibers formed by electrospinning and randomly mixed with the first fibers.

2. In paragraph 1, A composite fiber web, characterized in that the first fiber has a diameter size exceeding 1.5 ㎛ and not more than 5 cm, and the second fiber has a diameter size of not less than 0.001 ㎛ and not more than 1.5 ㎛.

3. In paragraph 1, A composite fiber web characterized in that the mixing ratio of the first fiber and the second fiber is formed as 60% to 75%: 40% to 25% based on the measured number.

4. A composite fiber nonwoven fabric having a web structure in which first fibers produced by melt blowing and second fibers produced by electrospinning are randomly mixed.

5. A single-layer fiber sheet comprising a fiber web in which meltblown fibers formed by a meltblown spinning method and electrospun fibers formed by an electrospinning method are irregularly mixed, wherein the fiber sheet comprises: A first surface area portion positioned on one side along the thickness direction of the fiber sheet; A second surface area portion located on the other side of the fiber sheet opposite to the first surface area portion; and Including an internal area portion located between the first surface area portion and the second surface area portion, A first mixing ratio (P) according to the number of electrospun fibers among the total number of measured fibers in each of the first surface area, the second surface area, and the internal area EF ) Composite fiber nonwoven fabrics each having a deviation of 50 percentage points or less.

6. In paragraph 5, The above fiber sheet is a composite fiber nonwoven fabric in which the first mixing ratio of the first surface area portion, the second surface area portion, and the internal area portion is at least 15%.

7. In paragraph 5, A composite fiber nonwoven fabric characterized in that the meltblown fiber has a diameter size exceeding 1.5 ㎛ and not more than 5 mm, and the electrospun fiber has a diameter size of not less than 0.001 ㎛ and not more than 1.5 ㎛.

8. In paragraph 7, A composite fiber nonwoven fabric, characterized in that the pore size of the fiber sheet formed between the meltblown fiber and the electrospun fiber is 0.1 ㎛ to 3.0 ㎛.

9. In paragraph 5, The above fiber sheet is a composite fiber nonwoven fabric in which the second mixing ratio of the electrospun fibers in the fiber web according to the measured weight is 1 to 50 wt% of the total measured weight.

10. In paragraph 5, The above fiber sheet is a composite fiber nonwoven fabric having a surface area ratio of 20% to 55% by the electrospun fibers measured in the first surface area portion, the second surface area portion, and the internal area portion, respectively.

11. In paragraph 5, The above fiber sheet has a specific surface area of ​​1 m by the meltblown fiber. 2 / g to 3 m 2 / g, and the specific surface area of ​​the electrospun fiber is about 5 m 2 / g to 7 m 2 / g composite fiber nonwoven fabric.

12. A first radiation unit including a first nozzle that discharges a first radiation solution to one side by a melt-blown method; A collecting unit that is arranged to be spaced apart from the first radiation unit to one side and collects the first radiation solution discharged from the first radiation unit; and A composite fiber web manufacturing device comprising a second spinning unit, which is installed between the first spinning unit and the collecting unit and which ejects a second spinning solution in a cross-sectional manner to the first spinning solution by an electrospinning method, and which forms the flow of the second spinning solution ejected from the second nozzle to be opposite to the flow direction of the first spinning solution.

13. In the 7th paragraph, the second radiation unit, A composite fiber web manufacturing device characterized in that the second nozzle is arranged at an angle toward the first nozzle.

14. In the 7th paragraph, the second nozzle, A body part with a space formed on the inside; A first discharge pipe provided in the above body portion and discharging a first fluid supplied to the space portion; and A composite fiber web manufacturing device including a second discharge tube having a constant outer diameter, which discharges a second fluid while being inserted into the first discharge tube.

15. A step of forming a first stream by discharging a first radiation solution to one side using a melt-blown method using a first nozzle of a first radiation unit; A step of forming a second stream by ejecting a second spinning solution toward the first stream by an electrospinning method using a second nozzle of a second radiating unit; A step in which the first stream and the second stream intersect and the first spinning solution and the second spinning solution are mixed in a web structure; and A method for manufacturing a composite fiber web, comprising the step of capturing a mixed stream in a capture unit.

Citation Information

Patent Citations

  • Flow duel nozzle

    KR101762880B1

  • Composite nonwoven fabric comprising Meta Aramid and melt blown fiber and manufacturing thereof

    KR1020130030043A

  • Filter using electro-spinning and melt-blowing and method for manufacturing same

    KR1020150023960A

  • Air conditioner for vehicle

    KR1020210112777A

  • Composite nanofiber materials and methods for making same

    WO2006049664A1