Second-life material

The combination of cellulose acetate tow and stone powder with organic solvents creates a binder for requalifying waste materials from the stone and tobacco industries, resulting in sustainable composite products for construction and ceramics, addressing the challenge of waste reuse.

WO2024228635A1PCT designated stage expired Publication Date: 2024-11-07INST SUPERIOR TECH
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
PCT/PT2024/050015
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-05-04
Filing Date
2024-05-03
Publication Date
2024-11-07

AI Technical Summary

Technical Problem

The stone and tobacco industries generate substantial waste, with stone dust and unsuitable cigarette filters not being effectively reused, leading to a need for requalification into new materials.

Method used

A composition comprising cellulose acetate tow or its derivatives combined with stone powder, using organic solvents like acetone to create a binder that can be extruded or molded into composite materials for use in construction and ceramics, such as paving elements.

Benefits of technology

The solution effectively requalifies waste materials into new composite products that are resistant and suitable for various applications, reducing waste and costs while promoting sustainable reuse.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure PT2024050015_07112024_PF_FP_ABST
    Figure PT2024050015_07112024_PF_FP_ABST
Patent Text Reader

Abstract

The present disclosure refers to a new composition and composite material that arises from the combination of waste from two industries: 1) ornamental rock industry, and 2) cigarette filter industry. The composition developed comprises cigarette filters, specifically the component comprising cellulose acetate as a binder for stone powders, with the purpose of consolidation.
Need to check novelty before this filing date? Find Prior Art

Description

DESCRIPTION"SECOND -LIFE MATERIAL"FIELD OF THE INVENTION

[0001] The present disclosure is directed to compositions and composite materials comprising cigarette filters , more speci fically cellulose acetate , and stone dust .BACKGROUND OF THE INVENTION

[0002] Currently, the stone sector generates substantial amounts of stone dust , which is considered a waste . In turn, the tobacco sector, which includes the production of cigarette filters , generates products not approved for the market , as a result of high production rates . Filters for cigarettes that do not pass the quality control process , are discarded as waste .

[0003] There is thus a growing need to requali fy these two wastes into new materials .

[0004] Patent CN101081732A describes a type of brick produced from stone dust and a binding agent such as mud or clay .

[0005] Patent US 11028599B2 describes an arti ficial stone tile and construction method . It is made by layers of cement formulations separated by layers of metal mesh . The cement color batches are prepared and placed in the bottom of a mold, with the color batches becoming the visible face of the building tile .SUMMARY OF THE INVENTION

[0006] In one aspect of the disclosure , there is provided a composition comprising from 1 % to 50% weight per weight (w / w) of cellulose acetate tow or a derivative thereof and from 50% to 99% (w / w) of stone powder .

[0007] In some embodiments, the composition comprises from 0.1% to 10% (w / w) of triacetin.

[0008] In some embodiments, the composition comprises at least one organic solvent, preferably at least one low boiling point solvent, more preferably acetone.

[0009] In some embodiments, the cellulose acetate tow is a cigarette filter.

[0010] In some embodiments, the stone powder comprises limestone powder, marble powder, granite powder or any combination thereof.[Oil] In some embodiments, the stone powder comprises particles with a particle area of less than 50 pm2, preferably less than 30 pm2.

[0012] In some embodiments, the stone powder comprises particles with a particle area from 6 pm2to 50 pm2, preferably from 6 pm2to 30 pm2.

[0013] In some embodiments, the composition is an extrudable composition .

[0014] In another aspect of the disclosure, there is provided a composite material comprising the composition according to the present disclosure.

[0015] In another aspect of the disclosure, there is provided a method for producing the composition according to the present disclosure, the method comprising: a) contacting cellulose acetate tow with at least one organic solvent, preferably at least one low boiling point solvent, to form a saturated solution; and b) contacting from 50% to 99% (w / w) of a stone powder with the solution, thereby obtaining the composition according to the present disclosure.

[0016] In some embodiments, the method further comprises a step c) of extruding, molding and / or printing thecomposition, thereby obtaining a composite material.

[0017] In some embodiments, the printing comprises a pressure from 3 bar to 2 bar.

[0018] In some embodiments, the printing comprises a mixing time from 1 hour (h) and 23 minutes (min) to 1 h and 20 min.

[0019] In some embodiments, the printing comprises a feed rate from 40% to 10%.

[0020] In some embodiments, the composite material is the composite material according to the present disclosure.

[0021] In some embodiments, the method further comprises a step d) of contacting the composite material with at least one organic solvent, preferably at least one low boiling point solvent, thereby obtaining a mixture.

[0022] In some embodiments, the method comprises re-using the mixture in step c) .

[0023] In some embodiments, the method further comprises a step of drying and / or grinding a stone slurry, thereby obtaining the stone powder.

[0024] In another aspect of the disclosure, there is provided a use of the composition according to the present disclosure, in injection molding process.

[0025] In another aspect of the disclosure, there is provided a use of the composition according to the present disclosure, in construction sector, coatings, ceramics, or any combination thereof, preferably in the manufacture of a ceramic product, paving element selected from the group: block of pavement, curb or slab and / or element for draining rainwater and wastewater.

[0026] In another aspect of the disclosure, there is provided a use of the composite material according to the present disclosure, in construction sector, coatings, ceramics, or any combination thereof, preferably in the manufacture of a ceramic product, paving element selected from the group: block of pavement, curb or slab and / or element for draining rainwater and wastewater.BRIEF DESCRIPTION OF THE DRAWINGS

[0027] Some embodiments of the disclosure are herein described, by way of example only, with reference to the accompanying drawings . With speci fic reference now to the drawings in detail , it is stressed that the particulars shown are by way of example and for purposes of illustrative discussion of embodiments of the disclosure . In this regard, the description taken with the drawings makes apparent to those skilled in the art how embodiments of the disclosure may be practiced .

[0028] Figures 1A-B are scanning electron microscopy ( SEM) images of the particle si ze measurement of stone powder ;

[0029] Figures 2A-B are SEM images of stone powder without polymer ( cellulose acetate tow) ( Figure 2A) and stone powder with polymer ( Figure 2B ) ;

[0030] Figures 3A-B are energy-dispersive spectrometer (EDS ) pictures of calcium distribution of a control sample (powder without polymer ) ( figure 3A) and sample with polymer ( Figure 3B ) ;

[0031] Figure 4 is a graph presenting the influence of the percentage of cellulose acetate tow on the fragmentation point ; and

[0032] Figure 5 is a diagram of the process according to the present disclosure .DETAILED DESCRIPTION OF THE INVENTION

[0033] The present disclosure is directed to compositions comprising cigarette filter component derived from cellulose acetate as a binder for stone dust , requali fying these two waste materials , and resulting in a new material and / or product .

[0034] In one aspect of the disclosure , there is provided a composition comprising from 1 % to 50% weight per weight (w / w) of cellulose acetate tow or a derivative thereof and from 50% to 99% (w / w) of stone powder .

[0035] The present disclosure is based, in part, on the finding that cellulose acetate tow from cigarette filters (new or used) acts as a binder for stone dust.

[0036] The present disclosure is based, in part, on the finding that the amount of cellulose acetate tow can be adjusted according to the desired use and / or application of a composition as described herein.

[0037] In some embodiments, the composition comprises from 1% to 50% (w / w) , from 2% to 50% (w / w) , from 5% to 50% (w / w) , from 10% to 50% (w / w) , from 20% to 50% (w / w) , from 30% to 50% (w / w) , from 1% to 30% (w / w) , from 2% to 30% (w / w) , from 5% to 30% (w / w) , from 10% to 30% (w / w) , from 20% to 30% (w / w) , from 1% to 10% (w / w) , from 2% to 10% (w / w) , from 5% to 10% (w / w) , from 1% to 7% (w / w) , from 2% to 7% (w / w) , or from 5% to 7% (w / w) of cellulose acetate tow or a derivative thereof, including any range therebetween. Each possibility represents a separate embodiment of the present disclosure.

[0038] In some embodiments, the composition comprises from 50% to 99% (w / w) , from 60% to 99% (w / w) , from 70% to 99% (w / w) , from 80% to 99% (w / w) , from 90% to 99% (w / w) , 50% to 95% (w / w) , from 60% to 95% (w / w) , from 70% to 95% (w / w) , from 80% to 95% (w / w) , or from 90% to 95% (w / w) of stone powder, including any range therebetween. Each possibility represents a separate embodiment of the present disclosure.

[0039] In some embodiments, the stone powder comprises stone slurry waste. As used herein, stone slurry waste refers to waste derived from quarrying and stone cutting and stone polishing industry. In some embodiments, water content from slurry waste is removed remaining a stone powder.

[0040] The present disclosure is based, in part, on the finding that the two waste products [cigarette filters and stone powder (stone dust) ] can be requalified and used in new compositions and / or material composites.

[0041] The present disclosure is based, in part , on the finding that the composition is a homogeneous composition . As used herein "homogeneous" refers to compositions where the cellulose acetate polymer is evenly distributed in the composition . In some embodiments , the composition i s devoid of cellulose acetate agglomerates and stone powder agglomerates .

[0042] In some embodiments , the composition comprises at least one organic solvent . In some embodiments , the composition comprises at least one low boiling point solvent . In some embodiments , the composition comprises acetone .

[0043] The present disclosure is based, in part , on the finding that a minimum ammount of solvent can be used, thereby reducing costs , solvent waste and loss . The ammount of solvent of a composition according to the present disclosure , is the minimum ammount needed to disolve cellulose acetate tow ( saturation point of the solution of solvent and cellulose acetate tow) .

[0044] In some embodiments , the composition comprises from 3% (w / v) to 6% (w / v) , preferably from 4 % (w / v) to 6% (w / v) of an organic solvent , preferably a low boiling point solvent . It should be understood that a larger ammount of solvent can be used according to the present disclosure .

[0045] According to the present disclosure , an appropriate organic solvent is an organic solvent in which cellulose acetate tow is soluble . Non-limiting examples of organic solvent according to the present disclosure include acetone , methyl ethyl ketone , ethyl acetate , dichloromethane , and diethyl ether .

[0046] The present disclosure is based, in part , on the finding that choosing a low boil ing point solvent , allows for a better ef ficacy and an easier removal process . In some embodiments , the low boiling point solvent comprises acetone . The present disclosure is based, in part , on thefinding that acetone is used only to dissolve the cellulose acetate, and can be later easily evaporated from the composition .

[0047] In some embodiments, the cellulose acetate tow is a cigarette filter. In some embodiments, the cigarette filter is a waste product such as used cigarette filter or cigarette filter that didn't pass a quality test.

[0048] In some embodiments, the composition comprises from 0.1% to 10% (w / w) , from 0.2% to 10% (w / w) , from 0.3% to 10% (w / w) , from 0.5% to 10% (w / w) , from 0.9% to 10% (w / w) , from 1% to 10% (w / w) , from 2% to 10% (w / w) , from 0.1% to 7% (w / w) , from 0.2% to 7% (w / w) , from 0.3% to 7% (w / w) , from 0.5% to 7% (w / w) , from 0.9% to 7% (w / w) , from 1% to 7% (w / w) , from 2% to 7% (w / w) , from 0.1% to 5% (w / w) , from 0.2% to 5% (w / w) , from 0.3% to 5% (w / w) , from 0.5% to 5% (w / w) , from 0.9% to 5% (w / w) , from 1% to 5% (w / w) , from 2% to 5% (w / w) , from 0.1% to 2% (w / w) , from 0.2% to 2% (w / w) , from 0.3% to 2% (w / w) , from 0.5% to 2% (w / w) , from 0.9% to 2% (w / w) , or from 1% to 2% (w / w) of triacetin, including any range therebetween. Each possibility represents a separate embodiment of the present disclosure.

[0049] As used herein, the terms "stone powder" and "stone dust" are used interchangeably to refer to stone powder residues from stone slurry of ornamental rock industry processing. In some embodiments, stone powder is stone slurry that was dried and / or grinded into powder. Suitable rocks according to the present disclosure include igneous rocks, sedimentary rocks and metamorphic rocks. Non-limiting examples include marble, granite, sandstone, limestone, slate, travertine, onyx, flagstone, serpentine and soapstone. In some embodiments, the stone powder comprises limestone powder, marble powder, granite powder, or any combination thereof.

[0050] In some embodiments, the stone powder comprises particles with a particle area of less than 30 pm2, less than 25 pm2, less than 20 pm2, less than 15 pm2, or less than 10 pm2, including any range therebetween. Each possibility represents a separate embodiment of the present disclosure.

[0051] In some embodiments, the stone powder comprises particles with a particle area from 6 pm2to 30 pm2, from 6 pm2to 20 pm2, from 6 pm2to 15 pm2, from 6 pm2to 10 pm2, from 7 pm2to 20 pm2, from 7 pm2to 15 pm2, from 7 pm2to 10 pm2, from 8 pm2to 20 pm2, from 8 pm2to 15 pm2, from 8 pm2to 10 pm2, from 9 pm2to 20 pm2, from 9 pm2to 15 pm2, or from 9 pm2to 10 pm2, including any range therebetween. Each possibility represents a separate embodiment of the present disclosure .

[0052] In some embodiments, the composition is an extrudable composition. In some embodiments the composition is an extrudate. The term "extrudate" refers to a product in which the composition is heated and / or compressed to a molten (or softened) state and subsequently extruded. As used herein, the term "extrudable composition" refers to the ability of a composition to be extruded. "Extrudate" and "extrudable composition" are used herein to refer not only to a composition that contains properties similar to a thermoplastic, but also a composition that is readily extrudable by known techniques.

[0053] In one aspect of the disclosure, there is provided a use of the composition described hereinabove, in injection molding process.

[0054] In some embodiments, a composition for injection molding process comprises from 90% to 95% (w / w) of stone powder and from 5% to 10% (w / w) of cellulose acetate tow or a derivative thereof.

[0055] In one aspect of the disclosure, there is provided a use of the composition described hereinabove, inconstruction sector, coatings , ceramics , or any combination thereof . Non-limi tting examples of a use of the composition according to the present disclosure include manufacture of a ceramic product , paving element selected from the group : block of pavement , curb or slab and / or element for draining rainwater and wastewater .

[0056] In one aspect of the disclosure , there is provided a composite material comprising the composition described hereinabove .

[0057] In one aspect of the disclosure , there is provided a use of the composite material described hereinabove , in construction sector, coatings , ceramics , or any combination thereof . Non-limi tting examples of a use of the composition according to the present disclosure include manufacture of a ceramic product , paving element selected from the group : block of pavement , curb or slab and / or element for draining rainwater and wastewater . The present disclosure is based, in part , on the finding that composite materials according to the present disclosure are resistant and can be used in or as floors , coatings and coverings , chinaware market , or as an alternative to ceramic materials .

[0058] In one aspect of the disclosure , there is provided a method for producing the composition as described hereinabove , the method comprising : a ) contacting cellulose acetate tow with at least one organic solvent , preferably at least one low boiling point solvent , to form a saturated solution; and b ) contacting from 50% to 99% (w / w) of stone powder with the solution, thereby obtaining the composition as described hereinabove .

[0059] In some embodiments , step a ) comprises contacting cellulose acetate tow with from 3% (w / v) to 6% (w / v) , preferably from 4 % (w / v) to 6% (w / v) of an organic solvent , preferably a low boiling point solvent . In some embodiments , the low boiling point solvent comprises acetone .

[0060] In some embodiments, contacting comprises mixing, stirring, high shear mixing, ultrasonication, overhead stirring, homogenizing, or any combination thereof.

[0061] In some embodiments, the method further comprises a step c) of extruding, molding and / or printing the composition, thereby obtaining a composite material.

[0062] In some embodiments, the printing comprises a pressure from 3 bar to 2 bar.

[0063] In some embodiments, the printing comprises a mixing time from 1 hour (h) and 23 minutes (min) to 1 h and 20 min. In some embodiments, the printing comprises a feed rate from 40% to 10%, from 30% to 10%, or from 25% to 10%, including any range therebetween. Each possibility represents a separate embodiment of the present disclosure.

[0064] In some embodiments, the composite material is the composite material described hereinabove.

[0065] In some embodiments, the method further comprises a step d) of contacting the composite material with a low- boiling point solvent, thereby obtaining a mixture. In some embodiments, contacting the composite material with a low- boiling point solvent is during a period from 24 hours to 48 hours .

[0066] In some embodiments, the mixture is re-used in step c) . The present disclosure is based, in part, on the finding that such composite materials as described can be recycled and re-used in the process.

[0067] In some embodiments, the method further comprises a step of drying and / or grinding a stone slurry, thereby obtaining stone powder.

[0068] The terms "comprises", "comprising", "includes", "including", "having" and their conjugates mean "including but not limited to".

[0069] The term "consisting of" means "including and limited to" .

[0070] The term "consisting essentially of" means that the composition, method or structure may include additional ingredients, steps and / or parts, but only if the additional ingredients, steps and / or parts do not materially alter the basic and novel characteristics of the claimed composition, method or structure.

[0071] The word "exemplary" is used herein to mean "serving as an example, instance or illustration". Any embodiment described as "exemplary" is not necessarily to be construed as preferred or advantageous over other embodiments and / or to exclude the incorporation of features from other embodiments .

[0072] As used herein, the singular form "a", "an" and "the" include plural references unless the context clearly dictates otherwise. For example, the term "a polymer" or "at least one polymer" may include a plurality of polymers, including mixtures thereof.

[0073] Throughout this application, various embodiments of this disclosure may be presented in a range format. It should be understood that the description in range format is merely for convenience and brevity and should not be construed as an inflexible limitation on the scope of the disclosure. Accordingly, the description of a range should be considered to have specifically disclosed all the possible subranges as well as individual numerical values within that range. For example, description of a range such as from 1 to 6 should be considered to have specifically disclosed subranges such as from 1 to 3, from 1 to 4, from 1 to 5, from 2 to 4, from 2 to 6, from 3 to 6 etc., as well as individual numbers within that range, for example, 1, 2, 3, 4, 5, and 6. This applies regardless of the breadth of the range.

[0074] Whenever a numerical range is indicated herein, it is meant to include any cited numeral (fractional or integral) within the indicated range. The phrases "ranging / rangesbetween" a first indicate number and a second indicate number and "ranging / ranges from" a first indicate number "to" a second indicate number are used herein interchangeably and are meant to include the first and second indicated numbers and all the fractional and integral numerals therebetween .

[0075] It is appreciated that certain features of the disclosure , which are , for clarity, described in the context of separate embodiments , may also be provided in combination in a single embodiment . Conversely, various features of the disclosure , which are , for brevity, described in the context of a single embodiment , may al so be provided separately or in any suitable subcombination or as suitable in any other described embodiment of the disclosure . Certain features described in the context of various embodiments are not to be considered essential features of those embodiments , unless the embodiment is inoperative without those elements .EXAMPLES

[0076] Reference is now made to the following examples , which together with the above descriptions illustrate some embodiments of the disclosure in a non-limiting fashion .EXAMPLE 1 : Characterization of the residue materialStone slurry

[0077] Since the residue material ( stone dust ) comes out of the trans formation process as slurry, a test was performed to figure out how much time would be needed to remove the water and retain the stone powder . This test used as guidelines the European Standard NP EN 13755 .

[0078] For this procedure , 9 samples of stone slurry were collected over a four-week period . Since most of the samples were already dried out , each sample was diluted with tap water . The amount of water for each sample varied from sample to sample .

[0079] The samples were kept in an oven at 70°C for 12 days and the weight was registered every 24 hours.

[0080] After the first 24 hours all samples exhibited between 45 and 70 percent of weight loss.

[0081] In conclusion, after considering all results, it was found that a two-day period at 70° Celsius is sufficient and necessary to completely dry the mud past the point that the only humidity present is residual one. This result is regardless of the amount of water originally present.

[0082] The geometry, particle size and variations in composition was determined. An electron scanning microscopy (SEM) was used. This technique, when coupled with an energy- dispersive spectrometer (EDS) , allows for both quantitative and qualitive analysis.

[0083] It was observed that the particles showed uneven size, there was a size variation from particle to particle. Regarding the geometry, the particles presented an elliptical geometry. For this reason, the particles area was measured assuming an elliptical shape, and for each picture, on 15 particles, the main directions were measured using ImageJ (Figure 1) . For each pair of measurements, the area was calculated, the average area for each sample was calculated and finally, an average powder particle area calculated was 9.13 pm2. In addition, 75% of the particles had an area inferior to 10 pm2and 97,5% had an area inferior to 20 pm2.

[0084] The EDS analyses revealed that the powders being used were limestone powder, since all analyses performed pointed to the most common composition of Portuguese limestone. However, it must be pointed out that traces of Chlorine were found which were traced back to the water treatment performed on site, were the powder had been made.Cellulose Acetate Tow

[0085] To characterize the cigarette filters residue collected during this work, FTIR-ATR spectra were obtained using a Perkin Elmer, Spectrum Two, FTIR spectrometer equipped with a UATR Two accessory, at 4 cm-1 resolution, and eight scans of data accumulation.

[0086] The spectra obtained shows cellulose acetate's two distinctive peaks: 1,730 cm-1 (C=O) and 1,220 cm-1 (C-O-C) . Furthermore, when the results were compared with the available database, the best matches for the compound being analyzed were, in order of best match, cellulose triacetate, and cellulose acetate. This result is most likely explained by the presence of the plasticizer triacetin, whose acetyl groups are supposed to interact with the cellulose acetate via dipolar interactions and hydrogen boding.EXAMPLE 2: Preliminary Process for Materials' Consolidation

[0087] Since the two materials used were in the solid state, it was needed to change the state of matter (using a solvent) instead of using a binder. Since the filters were soluble in acetone with or without the presence of triacetin, the choice was to dilute them in acetone and study the saturation point, to minimize the amount of acetone required.

[0088] For this study, three grams of filters were placed in a cup with 50ml of acetone. The solution was considered saturated since the filters hadn't completely dissolved. From this point on, acetone was added 0,5ml at a time until all the filters were dissolved.

[0089] A saturation point of approximately 45,80 grams (g) per liter was reached, meaning that to completely dissolve 45, 80 g of acetate tow in the form of residue, it would require one liter of acetone.

[0090] Two simultaneous experiences were performed. First, it was made a cellulose acetate tow solution using 4 g of cellulose acetate and 100 ml of acetone. Then the solution was mixed with 150 g of stone powder, reaching a dense fluid.Finally, it was poured into a mold and left it to dry at 70 degrees Celsius .

[0091] At the same time , 100 ml of acetone were added to 150 g of stone powder, poured into a mold and left it out to dry at 70 degrees Celsius .

[0092] It was observed that the use of cellulose acetate promoted the aggregation of the stone powders . Cellulose acetate acts as a binder for the stone powders , while the acetone used is evaporated from the sample , showing that a new material made only of stone powder and cellulose acetate tow can exist .SEM & EDS Analyses

[0093] SEM analyzes were performed to analyze i f there is a homogenous distribution of polymer throughout the samples and i f there are polymer fibers present or i f the polymer has formed a film ( Figures 2A-B ) . The composition used to produce the composite samples was the same used for the previous test .

[0094] SEM analyses showed no maj or di f ferences in powder distribution between both samples . Additionally, there are no visible fibers present , leading to the conclusion that the polymer is spread as an even f ilm . Furthermore , since in both cases there are visible darker spots , these should not be mistaken for polymer aggregation sites .

[0095] EDS analyses ( Figures 3A-B) showed an even distribution of calcium indicating that there are no evident points of polymer or powder accumulation . This supports the idea that the polymer is evenly distributed throughout the sample . Additionally, EDS shows no signi ficant locali zed increase in carbon content between both samples which suggest once again that there are not points of polymer agglomeration .Influence of the binder composition

[0096] In further embodiments of the present disclosure, it was investigated how would the mechanical properties of this material, vary with the concentration of cellulose acetate tow .

[0097] For this study, it was defined that 10 samples would be produced for 2%, 3% and 4% of cellulose acetate tow. The samples were left to dry at 70 degrees Celsius.

[0098] The first 10 samples produced with 2% of cellulose acetate tow came out as expected, just showing some small holes, which were assumed to be gas bubbles, and some superficial cracks on the sides.

[0099] The same process was employed for the second set of samples but this time using 3% of acetate two. However, after drying, the samples displayed cracks and were stuck to the mold. These effects were so severe that, not one sample was taken out of the mold without breaking apart.Influence of Temperature

[0100] From the previous study, it was figured that the next step would be to study cellulose acetate tow percentage Vs. drying temperature relation.

[0101] For this study, it was defined that 4 samples would be produced for each concentration: 2%, 3% and 4% of cellulose acetate tow. However, this time one of each would be dried for a fix period of 24 hours at 100°C, 75°C, 50°C and 25°C. After being produced the paste, each sample, would be extruded using a syringe.

[0102] All samples produced were dried for at least 24 hours, using 100°C, 75°C, 50°C and 25°C as drying temperature. Samples were produced using a cellulose acetate tow concentration of 2%, 3% and 4%.

[0103] From the results a hypothesis was formulated: when drying, the structural integrity of each sample will be determined by two main variables I) cellulose acetate tow concentration and II) drying temperature.

[0104] It was observed that for a drying temperature of 100 ° C, the same phenomenon can be seen across all the results : bubbles and vacancies . As the temperature lowers , these fade out . However, as concentration varies , it can be seen that the last two phenomena are more pronounced as cellulose acetate tow concentration is increased . Before the sample can reach its ful ly dried state the celluloses acetate film that forms and binds the powder particles will form first in the outer regions . This will happen faster, i f the outer temperature is higher, however, the sample will be less porous i f the cellulose acetate tow concentration in lower .

[0105] These two factors , when seen together, lead to acetone entrapment in the mid-section of the sample , one might refer to it as encapsulation . Between two samples at the same temperature , i f one has a higher concentration of cellulose acetate tow, it will be more predi sposed to failure than the other . This is explained with the previous hypothesis but adding that higher cellulose acetate tow concentration will reenforce the gas encapsulation phenomenon, leading to higher internal pressure which results in failure of the structural integrity of the sample .EXAMPLE 3 : Mixture Consistency : Time Vs . Concentration

[0106] For the fragmentation point , of each batch of each composition, it was registered the mixing time required and the correspondent acetone percentage still present in the batch throughout the process .

[0107] Fragmentation point : when the mix loses its ' s consistency, and it is seen formation of separate bodies .

[0108] Desegregation point : all bodies desegregate into smaller bodies resembling gravel .Table 1 - Percentage of acetone still present , and duration of trial .

[0109] From the results summarized in Table 1, two things can be noticed: The time required decreases with batch size; and the fragmentation point will vary essentially with the percentage of cellulose acetate tow being used: the set of trials for a 2% composition seem irregular when compared to the others sets (however the average value is consistent) .

[0110] When a graphical analysis was made, it was not clear what is the exact behavior. To get a clearer picture it was decided to look for to more points, one for each extreme. The process was repeated for 1%, 6%, and 20%.

[0111] It was not possible to perform analysis for 1%, since the batch would go through its fragmentation point before a minute had gone by. Meanwhile, due to limitations of the equipment available in the laboratory, the set of tests for 6% was only done for a batch using 50g of stone powder and 100g of stone powder and for 20% using only 50g.

[0112] The results can be seen in table 2 and in Figure 4.Table 2 - Fragmentation points obtained in each trial.

[0113] As the acetone evaporates , the chains are losing the solvent . As the solvent disappears , chain mobility reduces , the chains regres s from being extended or partial extend to a state of being curled up, getting entangled . This step is what will entrap the stone powders and consolidate the material . I f at some point , when there is still acetone , mixing is stopped, then the acetone release will be slow allowing the material to conform . However, i f mixing continues , then the natural process of entanglement is being speeded up while the mixer keeps dragging the material . These two factors will put the polymer chains under tension . The polymer chains will only hold, as long as there is still enough solvent . When the fragmentation point is reached, the there is no longer enough solvent , which means the polymer chains are entangling . The continue loss of solvent , with the force being applied by the mixer will result in either the rupture of the chains or of the bonds between them . This will correspond to the point at which batch fragments , and the fragmentation point is crossed . As one keeps mixing, these ef fects continue and at the extreme lead to the desegregation of the batch, achieving the gravel-like state . In addition, as one increases the amount of polymer in the batch, one will get closer to the true properties of the polymer itsel f , j usti fying the presence of the asymptote . The polymer will be limited by its own natural properties .Example 4: the printing process: testing the technology

[0114] For every printing test done from this point on, a composition batch of 6% cellulose acetate and 94% of stone powder was fixed. This represents a batch size of approximately half a kilo.

[0115] All tests were performed using a nozzle with a diameter of 1,2 mm.

[0116] As object to be printed an inverted cone with 45 degrees of inclination was chosen to test for both printing continuity and structural limitations.

[0117] The first test performed used the following conditions: 1) pressure: 4,5 bar; 2) mixing time: 1:25:00,31 (hour: minutes: seconds) ; 3) feed rate: 100%.

[0118] During this test two problems arose, lack of adhesion to the printing base and lack of adhesion in between layers. These problems were attributed to the high volatility of acetone, meaning that at the moment of extrusion the batch was already to dry, lacking humidity. From this point mixing time was decreased as well as the pressure since the viscosity of the paste would be altering.

[0119] The second test performed used the following conditions: 1) pressure: 3 bar & 2 bar; 2) mixing time: 1:23:00, 00 (hour : minutes : seconds) ; and 3) feed rate: 100% .

[0120] During this test one managed to have good adhesion of the first layer to the printing base when pressure was lowered to two bars. However, one was still unable to achieve in between layer adhesion. Once again, the choice was to increase humidity. Additionally, the pressure was fixed at two bars and the feed rate decreased to 20% to account for the viscosity and elastic behavior of the paste.

[0121] The third test performed used the following conditions: 1) pressure: 2 bar; 2) mixing time: 1:22:00,00 (hour: minutes: seconds) ; 3) feed rate: 20%.

[0122] This test achieved both adhesion to the printing surface and in between layers. However, the adhesion in between layers was limited to the outer layers - the continuous circular layers. To solve the problem, it was once again opted to increase humidity.

[0123] The fourth test performed used the following conditions: 1) pressure: 2 bar; 2) mixing time: 1:21:30,00 (hour: minutes: seconds) ; 3) feed rate: 20%.

[0124] This test achieved the correction of the problems. However, glitches of feed were identifiable resulting in a fifth test to correct the pressure being applied.

[0125] The fifth test performed used the following conditions: 1) pressure: 2,2 bar; 2) mixing time: 1:21:30,00 (hour: minutes: seconds) ; 3) feed rate: 20%.

[0126] This test was considered successful in completing the printing job and allowed the comprehension that due the acetones high volatility one was able to print using the 45- degree angle, since the paste would dry only moments after being extruded allowing the printing body to maintain its shape, without collapsing.Example 5: Second life material characterization as a concept product Storage

[0127] For this study, the choice was to produce a batch containing 6% of cellulose acetate and store two samples sealed in a fridge and two sealed samples at room temperature. The four samples would be weighted at the beginning of the test and at the end of the storage period - 30 days. Two parameters would be of importance: weight variation (to test the seal) and components separation (Table 3) .Table 3 - Results of storage test.

[0128] From Table 3, the weight for all samples, varied less than 0,5%. In addition, the samples that were left at room temperature show a higher weight variation which is understandable. Since the temperature is higher, and acetone is highly volatile, the tendency for the acetone to escape should be higher at room temperature.

[0129] Regarding phase separation, for none of the samples this was a problem. All four samples presented no major visible alterations.

[0130] It was considered that the material will remain conserved, as long as it is properly sealed. Regarding storage temperature conditions one does not consider the difference between the four samples to be significant enough to justify the use of lower temperatures.Recycl ability

[0131] To test the recyclability of this material, 8 samples were prepared containing the same mass of processed material. By this it is meant, finished product. To each sample, acetone was added respecting the proportion established by the saturation point and sealed. Finally, the test was designed to evaluate the material every 24 hours. After 24,i f the material seemed as i f it had return to the paste state , i f there had already been full impregnation by the solvent , a second sample would be opened to confirm the previous result .

[0132] The first sample was opened after the first 24 hours had gone by . Even though the material body seemed to have maintained its form, after mixing the sample it retuned to paste state exhibiting only a few smaller bodies present .

[0133] The same result was obtained until the fourth day . At this moment it was figured that the results would not suf fer any maj or alterations and it was concluded that a period of 24 to 48 hours would be suf ficient to ensure full impregnation by the solvent , to return the material to its paste state and leave it ready to be reshaped .

[0134] The complete process can be seen in figure 5 .

[0135] The conceptual test performed showed that when using acetate tow as a binder, the mix of both materials would result in a consolidated material , with both components evenly distributed throughout . Thi s achievement allowed for the requali fication of both residues as new materials .

[0136] The research performed on this material uncovered the relations between the af fecting variables : drying temperature , mixing time and binder composition . With the data collected, using a DeltaWasp 2040 3D printer, a process for extrusion was standardi zed . From the printing process it was concluded that the material at hand showed promise for this particular technology, given that it tolerates complex geometry' s without collapsing .

[0137] Regarding this material as a product , the case study showed that the batch, when properly sealed will conserve its properties and the that the final product can be , having once been considered finished product , reinserted in the process .

[0138] In conclusion, it was possible to prove the proposed methodology and create a new perspective on how we should look at residues , attempting to requali fy them into the next generation of materials .

Claims

CLAIMS1. Composition comprising from 1% to 50% weight per weight (w / w) of cellulose acetate tow or a derivative thereof and from 50% to 99% (w / w) of stone powder.

2. Composition according to claim 1, comprising from 0.1% to 10% (w / w) of triacetin.

3. Composition according to any one of claims 1 to 2, comprising at least one organic solvent, preferably at least one low boiling point solvent, more preferably acetone.

4. Composition according to any one of claims 1 to 3, wherein said cellulose acetate tow is a cigarette filter.

5. Composition according to any one of claims 1 to 4, wherein said stone powder comprises limestone powder, marble powder, granite powder, or any combination thereof.

6. Composition according to any one of claims 1 to 5, wherein said stone powder comprises particles with a particle area of less than 50 pm2, preferably less than 30 pm2.

7. Composition according to any one of claims 1 to 6, wherein said stone powder comprises particles with a particle area from 6 pm2to 50 pm2, preferably between 6 pm2and 30 pm2.

8. Composition according to any one of claims 1 to 7, wherein said composition is an extrudable composition.

9. Composite material comprising the composition according to any one of claims 1 to 8.

10. Method for producing the composition according to any one of claims 1 to 9, the method comprising: a) contacting cellulose acetate tow with at least one organic solvent, preferably at least one low boiling point solvent, to form a saturated solution; and b) contacting from 50% and 99% (w / w) of a stone powder with the solution, thereby obtaining the composition of any one of claims 1 to 8.

11. Method according to claim 10, further comprising a step c) of extruding, molding and / or printing said composition, thereby obtaining a composite material.

12. Method according to claim 11, wherein said printing comprises a pressure between 3 bar and 2 bar.

13. Method according to any one of claims 11 to 12, wherein said printing comprises a mixing time from 1 hour (h) and 23 minutes (min) to 1 h and 20 min.

14. Method according to any one of claims 11 to 13, wherein said printing comprises a feed rate from 40% to 10%.

15. Method according to any one of claims 11 to 14, wherein said composite material is the composite material according to claim 9.

16. Method according to any one of claims 11 to 15, further comprising a step d) of contacting said composite material with at least one organic solvent, preferably at least one low boiling point solvent, thereby obtaining a mixture.

17. Method of claim 16, comprising re-using said mixture in step c) .

18. Method according to any one of claims 11 to 17, further comprising a step of drying and / or grinding a stone slurry, thereby obtaining said stone powder.

19. Use of the composition according to any one of claims 1 to 8, in injection molding process.

20. Use of the composition according to any one of claims 1 to 8, in construction sector, coatings, ceramics, or any combination thereof, preferably in the manufacture of a ceramic product, paving element selected from the group: block of pavement, curb or slab and / or element for draining rainwater and wastewater.

21. Use of the composite material according to claim 9, in construction sector, coatings, ceramics, or any combination thereof, preferably in the manufacture of a ceramic product, paving element selected from the group: block of pavement, curb or slab and / or element for draining rainwater and wastewater .

Citation Information

Patent Citations

  • Stone powder sludge sintering brick and method for making the same

    CN101081732A

  • Artificial stone construction material and method of making

    US11028599B2

  • Process and Method for Cellulose Acetate Manufacturing Waste Product Recycling

    US20140287144A1