Low-refractive-index radiation-resistant glass material, method for preparing same, and use thereof
By developing low-refractive index radiation-resistant glass materials, the monopoly and localization of radiation-resistant fiber panels has been solved, and the preparation of high-performance fiber panels has been realized, which meets the needs of radiation environment applications and reduces production costs.
Patent Information
- Application Number
- PCT/CN2023/097222
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-05-11
- Filing Date
- 2023-05-30
- Publication Date
- 2024-11-14
AI Technical Summary
The existing radiation-resistant fiber panel industry has a serious monopoly, and it is difficult for domestic companies to master core technologies, resulting in core device supply problems and industrial chain safety issues in the fields of domestic production of digital CT systems and industrial flaw detection.
Developed a low refractive index radiation-resistant glass material, which includes 60-80% SiO2, 2-10% B2O3, 0.1-1% CeO2, 5-10% Na2O, 2-10% K2O, 1 ~8% Al2O3, 0-2% CaF2, 0-1% As2O3, and 1-5% alkaline earth metal oxides, with a refractive index of ≤1.47, with suitable thermal expansion coefficient and softening temperature properties, and are used as leather glass The material matches the core glass material with high refractive index to improve the performance of fiber panels and reduce production costs.
The preparation of low-refractive radiation-resistant glass materials has excellent X-ray absorption effect and radiation-resistant stability. It can effectively match the core glass materials with high-refractive index, improve the performance of fiber panels and reduce production costs, and solve the problem of X-rays. Problems in supplying core materials of detectors and industrial chain safety issues.
Smart Images

Figure CN2023097222_14112024_PF_FP_ABST
Abstract
Description
Low refractive index radiation-resistant glass material and its preparation method and application
[0001] This invention claims priority to the Chinese patent application filed with the Patent Office of China on May 11, 2023, with application number 202310540481.4 and invention name “Low refractive index radiation-resistant glass material, preparation method and application thereof”, the entire contents of which are incorporated by reference into the present invention and constitute a part of the present invention. Technical Field
[0002] The present invention relates to the technical field of glass materials, in particular to a low-refractive-index radiation-resistant glass material and a preparation method and application thereof. Background Art
[0003] Any discussion of the prior art throughout the specification should not be considered as an admission that such prior art is widely known or forms part of the common general knowledge in the field.
[0004] X-ray detectors are instruments that can see through and image the internal structures of the human body and other living organisms or materials. They are currently widely used in fields such as digital X-ray imaging, veterinary medicine, safety inspection, industrial non-destructive testing, and food safety testing. Fiber optic panels are core technical components in the field of X-ray radiology. They are fiber optic materials with special functions and are a common key technology in the development of modern industry and high-tech industries. The development of technical fields such as information, energy, defense, and advanced manufacturing is inseparable from the development of fiber optic functional materials and devices. Radiation-tolerant fiber optic panels with high X-ray absorption properties are a key component of digital CT-X-ray imaging systems. Radiation-tolerant fiber optic panels serve as the substrate for the scintillator in the detector system, while also reducing noise, protecting the sensor, and enhancing contrast. This allows the observer to observe real-time, high-definition images while also reducing the exposure of sensors such as CCDs (charge-coupled devices) and CMOS (complementary metal oxide semiconductors) to X-rays.
[0005] Since the 21st century, with the emergence of digital X-ray imaging systems, the demand for X-ray detection imaging has skyrocketed in high-end medical imaging digital CT diagnosis, food safety testing, lithium battery X-ray testing, etc., and there are high requirements for high-definition imaging while significantly increasing the radiation dose. The emergence of high-X-ray absorption, high-resolution, large-size radiation-resistant fiber optic panels has successfully solved the above problems. It has the characteristics of high X-ray stability, high resolution, and low cost.
[0006] However, the radiation-resistant fiber optic panel industry faces high barriers to entry. Currently, the market for glass materials used in radiation-resistant fiber optic panels is largely monopolized by a few companies, including Incom, Corning, and SCHOTT. These companies, having established early positions, have leveraged advantages in capital, technology, and customer base to secure a significant share of the global market over the years. The domestic industry, on the other hand, started relatively late. Although, after 20 years of development, domestic manufacturers have gradually mastered the core technologies of X-ray imaging systems, they still rely on imported components, hindering the localization of digital CT systems and industrial flaw detection.
[0007] In fiber optics, only light that enters the fiber along a specific cone angle can propagate along the fiber. This cone half angle is called the acceptance angle θ. The size of the acceptance angle depends only on the refractive index n of the core glass and the sheath glass, where The smaller the refractive index of the glass material, the larger the acceptance angle θ is, and more light can enter.
[0008] The present invention aims to overcome or improve at least one disadvantage of the prior art, or to provide a useful alternative. Unless the context clearly requires otherwise, throughout the specification and claims, words such as "include," "comprise," and "comprising" should be interpreted from an inclusive perspective, rather than an exclusive or exhaustive perspective; that is, from the perspective of "including, but not limited to."
[0009] Summary of the Invention
[0010] In response to the shortcomings of the existing technology, the present invention provides a low-refractive-index radiation-resistant glass material, its preparation method, and application. The low-refractive-index radiation-resistant glass material of the present invention has a refractive index of ≤1.47 and has a suitable thermal expansion coefficient and softening temperature performance. It can be used as a skin glass material for the production of optical glass fibers and optical fiber panels. At the same time, the glass material of the present invention can ensure that its viscosity matches that of the core glass material, especially the radiation-resistant core glass material with a refractive index of ≥1.8, which is conducive to the wire drawing process and has good process formability and process adaptability. The prepared optical fiber panel also has good radiation resistance, which can fundamentally meet the application of radiation environments and solve the core material supply problem and industrial chain security problems of X-ray detectors.
[0011] Specifically, the technical solution provided by the present invention is as follows:
[0012] In a first aspect of the present invention, a glass material is provided which can be used as skin glass, and which comprises, in molar percentage, 60-80% SiO2, 2-10% B2O3, 0.1-1% CeO2, 5-10% Na2O, 2-10% K2O, 1-8% Al2O3, 0-2% CaF2, 0-1% As2O3, and 1-5% alkaline earth metal oxide, wherein the alkaline earth metal oxide is selected from at least one of BaO, SrO, CaO and MgO.
[0013] The silica component in the glass composition has a relatively low refractive index. Increasing the silica content in the glass composition can reduce the refractive index of the glass to a certain extent. However, the increase in silica content will lead to an increase in the softening point temperature (viscosity) of the glass material, which is a major contradiction faced when preparing low-refractive-index glass materials. In addition, when used in the optical field, the requirements for radiation resistance and stability are also very high. Therefore, how to resolve the above contradictions and / or improve the radiation resistance and stability of the glass material and / or provide a glass material with good processing and process adaptability when preparing optical components or instruments such as optical fiber panels is a technical problem to be solved by the present invention. The glass material of the present invention is mainly composed of SiO2, B2O3, CeO2, alkali metals (Na2O and K2O), Al2O3 and alkaline earth metal oxides selected from BaO, SrO, CaO and MgO, and can optionally contain CaF2 and / or As2O3. The different combinations of these components not only make the glass material of the present invention have the advantages of: excellent X-ray absorption effect and radiation resistance stability; low refractive index (refractive index not higher than 1.47); while maintaining a low refractive index, it still has properties such as a suitable thermal expansion coefficient and a not too high softening point temperature. Such excellent properties enable it to be used as a skin glass material and well matched with the core glass material; good process formability and adaptability. For example, when it is used as a skin glass material and a core glass material, especially a core glass material with a high refractive index for the preparation of an optical fiber panel, it is not only beneficial to the wire drawing process, but also can improve the numerical aperture of the optical fiber panel, greatly improve the performance of the optical fiber panel, and at the same time can effectively reduce the production cost.
[0014] For example, in some embodiments of the present invention, the glass material is composed of the following components, measured by mole percentage: 60-80% SiO2, 2-10% B2O3, 0.1-1% CeO2, 5-10% Na2O, 2-10% K2O, 1-8% Al2O3, 0-2% CaF2, 0.1-1% As2O3, and 1-5% alkaline earth metal oxide, wherein the alkaline earth metal oxide is selected from at least one of BaO, SrO, CaO and MgO.
[0015] For example, in some embodiments of the present invention, the glass material is composed of the following components, measured by mole percentage: 60-80% SiO2, 2-10% B2O3, 0.1-1% CeO2, 5-10% Na2O, 2-10% K2O, 1-8% Al2O3, 0.1-2% CaF2, 0-1% As2O3, and 1-5% alkaline earth metal oxide, wherein the alkaline earth metal oxide is selected from at least one of BaO, SrO, CaO and MgO.
[0016] For example, in some embodiments of the present invention, the glass material is composed of the following components, measured by mole percentage: 60-80% SiO2, 2-10% B2O3, 0.1-1% CeO2, 5-10% Na2O, 2-10% K2O, 1-8% Al2O3, 0.1-2% CaF2, 0.1-1% As2O3, and 1-5% alkaline earth metal oxide, wherein the alkaline earth metal oxide is selected from at least one of BaO, SrO, CaO and MgO.
[0017] In embodiments of the present invention, SiO2 forms the basic framework of the glass structure and is the primary component of the radiation-resistant fiber optic faceplate sheath glass. The SiO2 content in the glass material of the present invention is 60-80% to maintain the glass's tensile strength, chemical stability, viscosity, and thermal expansion coefficient. In some embodiments of the present invention, this content, measured in mole percentage, can be selected from the following ranges: 60-75.1%, 60-70.5%, 60-69.8%, 60-65.8%, 65.8-80%, 65.8-75.1%, 65.8-70.5%, 65.8-69.8%, 69.8-80%, 69.8-75.1%, 69.8-70.5%, 70.5-80%, 70.5-75.1%, 75.1-80%, and the like. Preferably, the content of SiO2 is 65.8-75.1% or 65.8-70.5% or 65.8-69.8% or 70.5-75.1% or 69.8-75.1% or 69.8-70.5% in mole percentage.
[0018] B2O3 is a glass-forming oxide that can form glass on its own. In silicate glass, B can partially replace Si to form a network structure. Additionally, B2O3 acts as a flux in glass, reducing its high-temperature viscosity and facilitating production costs. However, increasing B2O3 content increases the range of glass devitrification, and B2O3 is volatile, causing environmental pollution. Therefore, its usage should be strictly controlled during production. Therefore, the glass material provided herein contains 2-10% B2O3. In some embodiments of the present invention, this content, expressed in molar percentage, can be selected from the following ranges: 2-9.2%, 2-8.9%, 2-7%, 2-5.2%, 5.2-10%, 5.2-9.2%, 5.2-8.9%, 5.2-7%, 7-10%, 7-9.2%, 7-8.9%, 8.9-10%, 8.9-9.2%, 9.2-10%, and the like. Preferably, the content of B2O3 is 5.2-9.2% or 5.2-8.9% or 7-9.2% or 5.2-7% or 8.9-9.2% or 9-9.2% in molar percentage.
[0019] CeO2 is used as a stabilizer in the present invention. 3+ The introduction of has the tendency to capture holes and be oxidized to form Ce 3+(+) , Ce 4+ It has a tendency to capture free electrons and be reduced to form Ce 4+(-) , so that the free electrons generated by irradiation cannot enter the defects in the glass structure, thereby preventing the formation of color centers and improving the radiation stability of the glass. However, the introduction of too much CeO2 will reduce the transmittance of the glass, especially in the near-ultraviolet band, and the addition of CeO2 will increase the refractive index of the glass. Therefore, the content of CeO2 in the glass material of the present invention is controlled to be 0.1-1% (molar percentage). In some embodiments of the present invention, the content is selected from the following ranges in molar percentage: 0.1-0.2, 0.1-0.3%, 0.1-0.5%, 0.1-0.6%, 0.2-0.3, 0.2-0.5, 0.2-0.6, 0.2-1, 0.3-0.5, 0.3-0.6, 0.3-1, 0.5-0.6, 0.5-1, 0.6-1, etc. The more preferred CeO2 content is 0.3-1% or 0.1-0.5% or 0.5-1% or 0.3-0.5% or 0.1-0.3% in molar percentage.
[0020] Na2O and K2O are network oxides in glass. Alkali metal ions easily migrate and diffuse within the glass, reducing the viscosity of the glass during high-temperature melting, making it easier to melt. They act as good fluxing agents. They also increase the thermal expansion coefficient of the glass, reducing its chemical stability and mechanical strength. In the glass material described herein, the Na2O content is 5-10% and the K2O content is 2-10%, measured in mole percentage. In some embodiments of the present invention, the combined content of Na2O and K2O is ≥10%, preferably 10-20% or 10-13%. In some embodiments of the present invention, the content of Na2O can be selected from the following ranges, calculated in mole percentage: 5-9%, 5-8%, 5-7%, 5-6%, 6-10%, 6-9%, 6-8%, 6-7%, 7-10%, 7-9%, 7-8%, 8-10%, 8-9%, 9-10%, etc., and the content of KO can be selected from the following ranges: 2-6.3%, 2-6%, 2-5%, 2-4.8%, 4.8-10%, 4.8-6.3%, 4.8-6%, 4.8-5%, 5-10%, 5-6.3%, 5-6%, 6-10%, 6-6.3%, 6.3-10%, etc.
[0021] Al2O3 is a network intermediate that forms the glass structure. Its content affects the thermal expansion coefficient and chemical and thermal stability of the glass. Al2O3 can increase the mechanical processing performance of the glass, but too much will reduce the material properties. In the glass material of the present invention, the content of Al2O3 is 1 to 8% by mole percentage. In some embodiments of the present invention, the content can be selected from the following ranges: 1 to 4.1%, 1 to 3.9%, 1 to 1.1%, 1.1 to 8%, 1.1 to 4.1%, 1.1 to 3.9%, 3.9 to 8%, 3.9 to 4.1% and 4.1 to 8%, etc. In some embodiments of the present invention, the preferred Al2O3 content is 1.1 to 4.1% or 4.1 to 8% by mole percentage.
[0022] CaF2 has unique dispersion properties and is commonly used as an important material for correcting chromatic aberration in optical systems. In the glass material of the present invention, the content of CaF2 is 0-2% by mole percentage. In some embodiments of the present invention, the content can be selected from the following ranges: 0, 0-1.5%, 0-0.5%, 0-0.3%, 0-0.2%, 0.2-2%, 0.2-1.5%, 0.2-0.5%, 0.2-0.3%, 0.3-2%, 0.3-1.5%, 0.3-0.5%, 0.5-2%, 0.5-1.5%, 1.5-2%, and the like. The preferred CaF2 content is 0-0.2% or 0-0.3% or 0-1.5% or 0.2-1.5% or 0.3-1.5% or 1.5-2% by mole percentage.
[0023] As2O3 is commonly used as a clarifier. Its characteristic is that it absorbs oxygen at low temperatures and releases oxygen at high temperatures, which can clarify the glass melt. In the present invention, the use of As2O3 can lower the melting temperature of the glass and improve the melting quality. In the present invention, the content of As2O3 is 0-1% by mole. In some embodiments of the present invention, the content can be selected from the following ranges: 0, 0-0.5%, 0-0.2%, 0-0.1%, 0.1-1%, 0.1-0.5%, 0.1-0.2%, 0.2-1%, 0.2-0.5%, 0.5-1%, etc. The preferred As2O3 content is 0.5-1% or 0.2-0.5% by mole.
[0024] In an embodiment of the present invention, the sum of the contents of CeO2 and As2O3 is ≥0.1% by mole percentage, preferably 0.2-1.5%. In some embodiments of the present invention, the sum of the contents can be selected from the following ranges: 0.2-1.3%, 0.2-0.7%, 0.2-0.5%, 0.2-0.4%, 0.4-1.5%, 0.4-1.3%, 0.4-0.7%, 0.4-0.5%, 0.5-1.5%, 0.5-1.3%, 0.5-0.7%, 0.7-1.5%, 0.7-1.3%, 1.3-1.5%, etc. Preferably, the sum of the contents of CeO2 and As2O3 is 0.2-1.3% or 0.2-0.5% or 0.5-1.5% or 0.5-1.3% or 1.3-1.5%.
[0025] In the present invention, the addition of at least one alkaline earth metal oxide selected from BaO, SrO, CaO and MgO can greatly reduce the phase separation tendency of the glass. Therefore, the glass material described in the present invention needs to contain at least one alkaline earth metal oxide selected from BaO, SrO, CaO and MgO, and its content is 1 to 5% (molar percentage).
[0026] For example, in some embodiments of the present invention, the alkaline earth metal oxide contains at least MgO, and its content in mole percentage can be selected from the following content ranges: 1-3.5%, 1-2.6%, 1-2.5%, 1-2.1%, 1-1.8%, 1.8-3.5%, 1.8-2.6%, 1.8-2.5%, 1.8-2.1%, 2.1-3.5%, 2.1-2.6%, 2.1-2.5%, 2.5-3.5%, 2.5-2.6%, 2.6-3.5%; the more preferred MgO content in mole percentage is 1-2.5% or 1.8-2.5% or 2.1-2.5% or 1.8-2.1%.
[0027] For example, in some embodiments of the present invention, the alkaline earth metal oxide contains at least BaO, and its content in mole percentage can be selected from the following content ranges: 0-1.5%, 0-1.2%, 0-1%, 0-0.5%, 0.5-1.5%, 0.5-1.2%, 0.5-1%, 1-1.5%, 1-1.2% and 1.2-1.5%; preferably, the more preferred BaO content in mole percentage is 0 or 0-1% or 1-1.2% or 0.5-1%.
[0028] For example, in some embodiments of the present invention, the alkaline earth metal oxide contains at least SrO, and its content in molar percentage can be selected from the following content ranges: 0-0.5%, 0-0.3%, 0-0.2%, 0.2-0.5%, 0.2-0.3% and 0.3-0.5%; the more preferred content is 0 or 0.2-0.5% or 0.3-0.5%.
[0029] For example, in some embodiments of the present invention, the alkaline earth metal oxide contains at least CaO, and its content is selected from the following in molar percentage: 0-1%, 0-0.4%, 0-0.2%, 0.2-1%, 0.2-0.4% and 0.4-1%; preferably 0 or 0.2-1% or 0.4-1% or 0.2-0.4%.
[0030] As preferred examples, in the above embodiments of the present invention, the alkaline earth metal oxide may be MgO, or a combination of BaO and MgO, or a combination of BaO, SrO, CaO, and MgO. In some embodiments, the content of the alkaline earth metal oxide is 3.5-5%, 4-5%, 1-4%, or 3.5-4% by mole.
[0031] In an embodiment of the present invention, the glass material of the present invention contains at least MgO and may or may not contain at least one selected from BaO, SrO, and CaO; when containing at least one selected from BaO, SrO, and CaO, the content of MgO in the total amount of alkaline earth metal oxides should be ≥50%, preferably 50-100% or 50-75%, more preferably 50-65%, and even more preferably 50-52.5%.
[0032] The various specific technical features described in the above embodiments of the present invention can be combined in any appropriate manner without contradiction. In order to avoid unnecessary repetition, the present invention will not further explain various possible combinations.
[0033] Unless otherwise specified, the numerical ranges described in the present invention include all values within this range, and include the range values formed by any two values within this range. For example, the numerical range of 0.1-1% CeO2 includes all values between 0.1-1%, and includes the range value (0.11-0.9%) formed by any two values within this range (for example, 0.11% and 0.9%). Different numerical values of the same indicator appearing in all embodiments of the present invention can be arbitrarily combined to form a range value.
[0034] In some embodiments of the present invention, the glass material is a low-refractive-index radiation-resistant glass material, whose refractive index is ≤1.47, or even ≤1.46, ≤1.45, ≤1.44, ≤1.43 or ≤1.42. The low refractive index increases the acceptance angle θ, and more light can enter the optical fiber, which has good refractive properties. In some embodiments, the refractive index of the glass material of the present invention is 1.42 to 1.47.
[0035] In some embodiments of the present invention, the glass material has a suitable glass transition temperature Tg, and / or expansion softening temperature Tf, and / or softening point temperature Ts, and / or thermal expansion coefficient, wherein more suitable parameters are Tg≤550°C, Tf≤645°C, Ts≤748°C, and the thermal expansion coefficient at 20°C to 300°C is (82 to 87)×10 -7 / ℃.
[0036] In some embodiments of the present invention, the glass material exhibits excellent radiation stability. Its transmittance at 560 nm before X-ray irradiation is higher than 90.8%. After irradiation with a dose of 4700 Gy of X-rays, the transmittance at 560 nm remains at least 89%, generally above 90%. The transmittance decreases before and after irradiation by ≤2%, preferably ≤1.8, or even ≤1.5 or ≤1.4. In some embodiments, the transmittance of the glass material of the present invention decreases before and after irradiation by 1.4% to 1.8%.
[0037] In a second aspect, the present invention provides a method for preparing the glass material described in the first aspect, comprising: mixing raw materials in appropriate proportions, melting them at high temperature, clarifying them with auxiliary stirring, cooling them to form them, and performing precision annealing. The forming method may be mechanical forming.
[0038] In some embodiments of the present invention, the high-temperature melting temperature is 1380-1520°C, the forming temperature is 1080-1320°C, and the annealing temperature is 580-610°C. According to the proportions of the components disclosed in the first aspect of the present invention, the glass material prepared within this temperature range has stable properties, including but not limited to good refractive properties, good heat resistance, good processing properties and good radiation stability. Of course, it can be understood that within this temperature range, higher temperatures can shorten the preparation process compared to lower temperatures. If it is necessary to shorten the time cost as much as possible, those skilled in the art can choose a relatively higher temperature within the temperature range disclosed in the present invention during operation.
[0039] The present invention provides a method for preparing a low-refractive-index radiation-resistant glass material. The raw materials include: quartz sand, boric acid, cerium oxide, sodium carbonate or sodium nitrate, potassium carbonate or potassium nitrate, aluminum hydroxide or aluminum oxide, fluorite, arsenic oxide, barium nitrate or barium carbonate, strontium carbonate, calcium carbonate and magnesium carbonate.
[0040] In a third aspect, the present invention provides an optical element made of the glass material described in the first aspect, wherein the optical element includes but is not limited to optical glass, optical fiber panel, etc.
[0041] In a fourth aspect, the present invention provides an optical glass fiber, the sheath of which comprises the glass material described in the first aspect.
[0042] In an embodiment of the present invention, the optical glass fiber comprises at least a sheath and a core. The glass material of the present invention serves as the sheath glass material constituting the sheath of the optical glass fiber. The core material may be a core glass material conventionally used in the art for preparing optical glass fibers. Of course, it is understood that when the glass material of the present invention is used in conjunction with the sheath glass material of the present invention, compatibility with the sheath glass material of the present invention in the drawing process is required. Such core glass materials generally have a relatively high refractive index, such as hard optical fiber-type core glass materials or radiation-resistant glass materials having a high refractive index.
[0043] The hard optical fiber core glass may be a common optical fiber panel core glass material, or may be as described in Chinese Patent CN201110378012.4. For example, in some embodiments of the present invention, the hard optical fiber core glass material has a refractive index of 1.850-1.86, a softening temperature of 590-632°C, and an expansion coefficient of (89±4)×10 at 300°C. -7 / °C. In some embodiments, the composition may be: in mass percentage, BaO content is 20-45%, La2O3 content is 18-27%, B2O3 content is 12-20%, Nb2O5+Y2O3+Ta2O5 content is 5-20%, ZrO2 content is 3-10%, Al2O3 content is 0-6%, CaO content is 0-5%, K2O content is 1-1.5%, and Na2O content is 0.5-0.8%.
[0044] For example, in some embodiments of the present invention, the refractive index of the radiation-resistant glass material with a high refractive index is ≥1.8, its transmittance decreases by ≤2% after irradiation with a total dose of 4700Gy of X-rays, its glass transition temperature is ≥560°C, its expansion softening temperature is ≥650°C, and its thermal expansion coefficient at 30°C to 300°C is (85 to 90)×10 -7 / ℃;
[0045] For example, in some embodiments, the radiation-resistant glass (core glass material) with a high refractive index is composed of the following components, in mass percentage: 20-40% SiO2, 0-10% Al2O3, 0-5% CaO, 5-20% BaO, 40-50% PbO, 1-5% CeO2, 0-5% La2O3, 0-2% Nb2O5, 0-2% Ta2O5, 0-1% Bi2O3, and 0-1% of an oxide selected from Na2O, K2O, Rb2O and Cs2O.
[0046] For example, in some other embodiments, the composition of the radiation-resistant glass (core glass material) with a high refractive index is: in mass percentage, 20-40% SiO2, 0-10% Al2O3, 0-5% CaO, 5-20% BaO, 40-50% PbO, 1-5% CeO2, 0-5% La2O3, 0-2% Nb2O5, 0-2% Ta2O5, 0-1% Bi2O3, wherein the total content of La2O3, Nb2O5, Ta2O5 and Bi2O3 is 1-8%, and the content of alkali metal oxide is 0-1%, and the alkali metal oxide is selected from at least one of Na2O, K2O, Rb2O and Cs2O.
[0047] For example, in some other embodiments, the radiation-resistant glass (core glass material) with a high refractive index is composed of, in percentage by mass, 20-40% SiO2, 2-10% Al2O3, 1-5% CaO, 5-20% BaO, 40-50% PbO, 1-5% CeO2, 0.5-5% La2O3, 0-2% Nb2O5, 0-2% Ta2O5, 0-1% Bi2O3, and 0-1% alkali metal oxide, wherein the alkali metal oxide is selected from Na2O, K2O, Rb2O and Cs2O.
[0048] For example, in some other embodiments, the composition of the radiation-resistant glass (core glass material) with a high refractive index is: in mass percentage, 20-40% SiO2, 0-10% Al2O3, 0-5% CaO, 5-20% BaO, 40-50% PbO, 1-5% CeO2, 0-5% La2O3, 0-2% Nb2O5, 0-2% Ta2O5, wherein the total content of La2O3, Nb2O5 and Ta2O5 is 1-8%, and the content of alkali metal oxide is 0-1%, and the alkali metal oxide is selected from Na2O, K2O, Rb2O and Cs2O.
[0049] For example, in some other embodiments, the radiation-resistant glass (core glass material) with a high refractive index has a composition of, by mass percentage, 20-40% SiO2, 0-10% Al2O3, 0-5% CaO, 5-20% BaO, 40-50% PbO, 1-5% CeO2, 0-5% La2O3, 0-2% Nb2O5, 0-2% Ta2O5, and 0-1% Bi2O3, wherein the total content of La2O3, Nb2O5, Ta2O5, and Bi2O3 is 1-8%;
[0050] In a fifth aspect, the present invention provides a fiber optic panel (optical glass fiber panel), the sheath of which comprises the glass material described in the first aspect above. For example, in some embodiments of the present invention, the glass material of the present invention may be nested with a core glass material (the material of which may be as described in the fourth aspect above, such as a hard fiber-type glass material or a radiation-resistant glass material with a high refractive index). The core glass material is drawn from a single filament or multiple multifilaments, and the multifilaments are regularly arranged and melt-pressed into blank plate segments. The fiber optic panel is then sliced, rounded, ground, and polished to produce the fiber optic panel. The fiber optic panel can be customized in size, up to the meter level.
[0051] The glass material of the present invention is used as a skin glass material in combination with a high refractive index (≥1.80) core glass material. The resulting optical fiber panel has a numerical aperture greater than 1, and theoretically, incident light at any angle can enter the optical fiber.
[0052] The glass material described in the present invention has a glass transition temperature Tg≤550°C, an expansion softening temperature Tf≤645°C, and a softening point temperature Ts≤748°C. Its expansion softening temperature is lower than that of the core glass material with a refractive index ≥1.8 described in the fourth aspect above. When the glass material described in the present invention is used as a skin glass material, its viscosity is lower than that of the core glass material, and it can be well matched during the preparation process, and has good process formability and process adaptability.
[0053] In addition, the optical fiber panel provided by the present invention also has good radiation resistance, which can fundamentally meet the application of radiation environment and solve the core material supply problem and industrial chain security problem of X-ray detectors.
[0054] Specifically, the core glass material that can perfectly match the glass material described in the present invention (as a skin glass material) for preparing optical glass fibers or optical fiber panels can be as described in Chinese patent application CN202310200621.3, the entire contents of which are incorporated by reference into the present invention and constitute a part of the present invention. The two can be perfectly matched during the drawing process, have good process formability and process adaptability, and the prepared optical fiber panel also has excellent radiation resistance.
[0055] In the sixth aspect of the present invention, the present invention provides the application of the glass material described in the first aspect above in the optical field, especially the application of the glass material in the preparation of optical elements or optical instruments; wherein the optical elements or optical instruments include but are not limited to optical glass and optical fiber panels, etc.
[0056] Compared with the prior art, the advantages of the present invention include:
[0057] The glass material provided by the present invention has excellent X-ray absorption effect and radiation resistance stability; has a low refractive index (refractive index is not higher than 1.47); while maintaining a low refractive index, it still has properties such as a suitable thermal expansion coefficient and a not too high softening point temperature. Such excellent properties enable it to be used as a skin glass material and well matched with the core glass material; has good process formability and adaptability. For example, when it is used as a skin glass material and a core glass material, especially a core glass material with a high refractive index for preparing an optical fiber panel, it is not only beneficial to the wire drawing process, but also can improve the numerical aperture of the optical fiber panel, greatly improve the performance of the optical fiber panel, and at the same time can effectively reduce the production cost. Of course, any product implementing the present invention does not necessarily need to achieve all of the advantages described above simultaneously, but the present invention is optimally capable of achieving all of the advantages described above simultaneously. For example, the glass material provided by the present invention has a low refractive index of ≤1.47, a transmittance drop of ≤2% after irradiation with a total dose of 4700Gy of X-rays, a glass transition temperature Tg ≤550°C, an expansion softening temperature Tf ≤645°C, and a softening point temperature Ts ≤748°C. It has good radiation resistance and can be used as skin glass, compatible with core glass materials, and a thermal expansion coefficient of (82-87)×10 -7 / ℃, has good thermal processing performance, is conducive to the molding and preparation of large-size devices, and its comprehensive performance is superior to similar materials at home and abroad. BRIEF DESCRIPTION OF THE DRAWINGS
[0058] The drawings constituting part of the present application are provided to provide a further understanding of the present application. The illustrative embodiments and their descriptions of the present application are provided to explain the present application and do not constitute an undue limitation on the present application. The following describes the implementation scheme of the present application in detail in conjunction with the drawings, wherein:
[0059] FIG1 shows a comparison of the transmittance (560 nm) of the glass material of Preparation Example 4 of the present invention before and after irradiation with X-rays (4700 Gy dose).
[0060] FIG2 shows a large size (140×90×2mm) made of the low refractive index radiation-resistant glass material of the present invention. 3 ) Actual image of the radiation-resistant fiber optic panel. DETAILED DESCRIPTION
[0061] The present application will be further described below in conjunction with specific examples. It should be understood that these examples are intended to illustrate the present application only and are not intended to limit the scope of the present application. The experimental methods in the following examples where specific conditions are not specified are generally performed under conventional conditions or as recommended by the manufacturer.
[0062] Unless otherwise defined, all professional and scientific terms used herein have the same meaning as those familiar to those skilled in the art. The reagents or raw materials used in this application can be purchased through conventional channels. Unless otherwise specified, the reagents or raw materials used in this application are used in a conventional manner in this area or in accordance with the product instructions. In addition, any methods and materials similar to or equivalent to those described herein can be applied to the present method. The preferred embodiments and materials described herein are for demonstration purposes only.
[0063] The present invention provides a low-refractive-index, radiation-resistant glass material, which comprises, by mole percentage, the following components: 60-80% SiO2, 2-10% B2O3, 0.1-1% CeO2, 5-10% Na2O, 2-10% K2O, 1-8% Al2O3, 0-2% CaF2, 0-1% As2O3, and 1-5% alkaline earth metal oxide, wherein the alkaline earth metal oxide is selected from at least one of BaO, SrO, CaO, and MgO. The glass material of the present invention has suitable thermal expansion coefficient and softening temperature properties, good process formability and process adaptability, and can be used as a sheath glass material for the production of optical glass fibers and optical fiber panels. The resulting optical fiber panels also have excellent radiation resistance, can fundamentally meet the needs of applications in radiation environments, and solve the core material supply problems and industrial chain security issues of X-ray detectors.
[0064] In particular, when the low-refractive-index radiation-resistant glass material of the present invention is composed of the above-mentioned components, in some embodiments of the present invention, the refractive index of the glass material of the present invention is ≤1.47; in some embodiments of the present invention, the glass transition temperature Tg of the glass material of the present invention is ≤550°C; in some embodiments of the present invention, the expansion softening temperature Tf of the glass material of the present invention is ≤645°C; in some embodiments of the present invention, the softening point temperature Ts of the glass material of the present invention is ≤748°C, which matches the core glass material; in some embodiments of the present invention, the thermal expansion coefficient of the glass material of the present invention is (82-87)×10 -7 / ℃; In some embodiments of the present invention, the 560nm transmittance of the glass material is above 91%, and after being irradiated with a dose of 4700Gy of X-rays, the 560nm transmittance can still be maintained above 90%, and the transmittance decreases by ≤2%. In addition, in some embodiments of the present invention, the glass material of the present invention has the above-mentioned excellent properties at the same time. These glass materials have a refractive index of ≤1.47, a glass transition temperature Tg ≤550℃, an expansion softening temperature Tf ≤645℃, a softening point temperature Ts ≤748℃, and a thermal expansion coefficient of (82~87)×10 -7 / ℃ and after irradiation with a dose of 4700Gy of X-rays, the transmittance decreases by ≤2%, or even ≤1.8%, ≤1.6% or ≤1.5%, showing more excellent comprehensive performance and being particularly suitable for the preparation of radiation-resistant optical elements or optical instruments.
[0065] Furthermore, the low-refractive-index, radiation-resistant glass material of the present invention can be prepared by the following method: after mixing the raw materials in proportion, the batch material is melted at a high temperature of 1380-1520°C, clarified with auxiliary stirring, mechanically drawn at 1080-1320°C, and annealed at 580-610°C to obtain the low-refractive-index, radiation-resistant glass material. This method has process stability, and the glass material prepared within this temperature range has stable properties, including but not limited to good refractive properties, good heat resistance, good processing properties, and good radiation resistance stability. Of course, it is understandable that within this temperature range, higher temperatures can shorten the preparation process compared to lower temperatures. If it is necessary to shorten the time cost as much as possible, those skilled in the art can choose a relatively higher temperature within the temperature range disclosed in the present invention when operating.
[0066] Furthermore, in a preparation method of a low-refractive-index radiation-resistant glass material provided by the present invention, the raw materials include: quartz sand, boric acid, cerium oxide, sodium carbonate or sodium nitrate, potassium carbonate or potassium nitrate, aluminum hydroxide or aluminum oxide, fluorite, arsenic oxide, barium nitrate or barium carbonate, strontium carbonate, calcium carbonate and magnesium carbonate.
[0067] Furthermore, in order to present the present invention more clearly, the present invention will be further described below with reference to specific examples.
[0068] Preparation Example 1
[0069] The low-refractive-index radiation-resistant glass material of this preparation example is composed of the following components in molar percentages: 75.1% SiO2, 7% B2O3, 0.1% CeO2, 9% Na2O, 6.3% K2O, 1.1% Al2O3, 0.3% CaF2, 0.1% As2O3, and 1% MgO.
[0070] The low-refractive-index radiation-resistant glass material of this preparation example is prepared by the following method: using quartz sand, boric acid, cerium oxide, sodium nitrate, potassium carbonate, aluminum hydroxide, fluorite, arsenic oxide, and magnesium carbonate as raw materials, mixing the various glass raw materials in proportion, melting the mixture at a high temperature of 1500°C, clarifying it with auxiliary stirring, mechanically drawing it at 1236°C, and annealing it at 605°C to obtain the glass material.
[0071] The refractive index of glass samples was measured using a Metricon Model 2010 / M prism coupling tester. When a beam of light enters the V-prism perpendicular to the incident surface, if the refractive index of the sample being tested is the same as that of the V-prism, the light will pass through the prism undeflected. If the refractive index of the sample being tested differs from that of the prism, the light will refract. The angle between the light and the incident beam is read, and the refractive index of the sample can be calculated according to the law of refractive index (GB / T7962.1-2010).
[0072] The thermal expansion coefficient of glass samples was measured using a NETZSCH DIL 402 thermal expansion coefficient tester. Sample preparation: Glass samples were ground and polished into cylindrical glass strips measuring Φ6 x 50 mm, with the two ends parallel. The heating rate was set at 5°C / min, and the data acquisition cycle was 20ms. The data were plotted against the linear expansion curve, and the glass transition temperature and dilatometric softening temperature were obtained using the tangent method. (GB / T 7962.16-2010)
[0073] The softening point temperature of the glass sample was tested using a Model PPV-1000 / 1200 plate viscometer manufactured by Orton. Sample preparation: The glass sample was ground and polished into a Φ6×6mm cylindrical glass strip, with both end faces parallel. The glass sample was placed on the top plate, and a heat-resistant metal alloy circular plate with a diameter of 44mm and a thickness of 6mm was connected to the bottom of the probe rod and the heat-resistant metal alloy circular plate below (also 44mm in diameter and 6mm thick). Two very thin platinum films (40mm in diameter and 0.001 inches thick) were placed between the sample and the upper and lower heat-resistant metal circular plates to facilitate sampling and sample placement. (GB / T 7962.16~2010)
[0074] The low-refractive-index radiation-resistant glass material prepared by the preparation method of this preparation example has a refractive index of 1.42, a transmittance of 90% (decreased by 1.4%) after irradiation with 4700Gy of X-rays, a glass transition temperature Tg of 543°C, an expansion softening temperature Tf of 632°C, a softening point temperature Ts of 740°C, and a thermal expansion coefficient of 83.8×10 -7 / ℃, it has good process formability and process adaptability, and can be used as skin glass material for the production of optical glass fiber and optical fiber panels. The prepared optical fiber panels also have good radiation resistance and can fundamentally meet the application needs of radiation environments.
[0075] Preparation Example 2
[0076] The low-refractive-index radiation-resistant glass material of this preparation example is composed of the following components in molar percentages: 70.5% SiO2, 5.2% B2O3, 0.3% CeO2, 8% Na2O, 2% K2O, 8% Al2O3, 1% As2O3, 1% BaO, 0.5% SrO, 1% CaO, and 2.5% MgO.
[0077] The low-refractive-index radiation-resistant glass material of this preparation example is prepared by using quartz sand, boric acid, cerium oxide, sodium nitrate, potassium carbonate, aluminum hydroxide, arsenic oxide, barium nitrate, strontium carbonate, calcium carbonate, and magnesium carbonate as raw materials, mixing the various glass raw materials in proportion, melting the mixture at a high temperature of 1508°C, clarifying it with auxiliary stirring, mechanically drawing it at 1289°C, and annealing it at 608°C to obtain the glass material.
[0078] The detection method is the same as that of Preparation Example 1. The refractive index of the low-refractive-index radiation-resistant glass material obtained by the preparation method of this preparation example is 1.43, and the transmittance after 4700Gy of X-ray irradiation is 91.2% (decreased by 1.5%), the glass transition temperature Tg is 550°C, the expansion softening temperature Tf is 639°C, the softening point temperature Ts is 745°C, and the thermal expansion coefficient is 82.9×10 -7 / ℃, it has good process formability and process adaptability, and can be used as skin glass material for the production of optical glass fiber and optical fiber panels. The prepared optical fiber panels also have good radiation resistance and can fundamentally meet the application needs of radiation environments.
[0079] Preparation Example 3
[0080] The low-refractive-index radiation-resistant glass material of this preparation example is composed of the following components in molar percentages: 80% SiO2, 2% B2O3, 0.6% CeO2, 6% Na2O, 4.8% K2O, 1% Al2O3, 0.5% CaF2, 0.1% As2O3, 1.5% BaO, and 3.5% MgO.
[0081] The low-refractive-index radiation-resistant glass material of this preparation example is prepared by the following method: using quartz sand, boric acid, cerium oxide, sodium nitrate, potassium carbonate, aluminum hydroxide, fluorite, arsenic oxide, barium nitrate, and magnesium carbonate as raw materials, mixing the various glass raw materials in proportion, melting the mixture at a high temperature of 1450°C, clarifying it with auxiliary stirring, mechanically drawing it at 1200°C, and annealing it at 601°C to obtain the glass material.
[0082] The detection method is the same as that of Preparation Example 1. The refractive index of the low-refractive-index radiation-resistant glass material obtained by the preparation method of this preparation example is 1.47, and the transmittance after 4700Gy of X-ray irradiation is 89% (decreased by 1.8%), the glass transition temperature Tg is 537°C, the expansion softening temperature Tf is 628°C, the softening point temperature Ts is 733°C, and the thermal expansion coefficient is 84.9×10 -7 / ℃, it has good process formability and process adaptability, and can be used as skin glass material for the production of optical glass fiber and optical fiber panels. The prepared optical fiber panels also have good radiation resistance and can fundamentally meet the application needs of radiation environments.
[0083] Preparation Example 4
[0084] The low-refractive-index radiation-resistant glass material of this preparation example is composed of the following components in molar percentages: 65.8% SiO2, 9.2% B2O3, 1% CeO2, 5% Na2O, 5% K2O, 8% Al2O3, 1.5% CaF2, 0.5% As2O3, 1% BaO, 0.5% SrO, 0.4% CaO, and 2.1% MgO.
[0085] The low-refractive-index radiation-resistant glass material of this preparation example is prepared by the following method: using quartz sand, boric acid, cerium oxide, sodium nitrate, potassium carbonate, aluminum oxide, fluorite, arsenic oxide, barium carbonate, strontium carbonate, calcium carbonate, and magnesium carbonate as raw materials, mixing the various glass raw materials in proportion, melting the mixture at a high temperature of 1520°C, clarifying it with auxiliary stirring, mechanically drawing it at 1320°C, and annealing it at 610°C to obtain the glass material.
[0086] The detection method is the same as that of Preparation Example 1. The refractive index of the low-refractive-index radiation-resistant glass material obtained by the preparation method of this preparation example is 1.44, and the transmittance after 4700Gy of X-ray irradiation is 91.8% (decreased by 1.4%), the glass transition temperature Tg is 550℃, the expansion softening temperature Tf is 645℃, the softening point temperature Ts is 748℃, and the thermal expansion coefficient is 82.0×10 -7 / °C, has good process formability and process adaptability, and can be used as a sheath glass material for the production of optical glass fibers and fiber optic panels. The prepared fiber optic panels also have good radiation resistance and can fundamentally meet the needs of applications in radiation environments. Figure 1 shows the comparison of the transmittance (560nm) of this glass material before and after X-ray irradiation (4700Gy dose).
[0087] Preparation Example 5
[0088] The low-refractive-index radiation-resistant glass material of this preparation example is composed of the following components in molar percentages: 60% SiO2, 10% B2O3, 0.2% CeO2, 10% Na2O, 10% K2O, 3.9% Al2O3, 2% CaF2, 0.2% As2O3, 0.5% BaO, 0.2% SrO, 0.4% CaO, and 2.6% MgO.
[0089] The low-refractive-index radiation-resistant glass material of this preparation example is prepared by the following method: using quartz sand, boric acid, cerium oxide, sodium nitrate, potassium nitrate, aluminum hydroxide, fluorite, arsenic oxide, barium carbonate, strontium carbonate, calcium carbonate, and magnesium carbonate as raw materials, mixing the various glass raw materials in proportion, melting the mixture at a high temperature of 1380°C, clarifying it with auxiliary stirring, mechanically drawing it at 1080°C, and annealing it at 580°C to obtain the glass material.
[0090] The detection method is the same as that of Preparation Example 1. The refractive index of the low-refractive-index radiation-resistant glass material obtained by the preparation method of this preparation example is 1.46, and the transmittance after 4700Gy of X-ray irradiation is 90.2% (decreased by 1.8%), the glass transition temperature Tg is 525℃, the expansion softening temperature Tf is 619℃, the softening point temperature Ts is 724℃, and the thermal expansion coefficient is 87×10 -7 / ℃, it has good process formability and process adaptability, and can be used as skin glass material for the production of optical glass fiber and optical fiber panels. The prepared optical fiber panels also have good radiation resistance and can fundamentally meet the application needs of radiation environments.
[0091] Preparation Example 6
[0092] The low-refractive-index radiation-resistant glass material of this preparation example is composed of the following components in molar percentages: 69.8% SiO2, 8.9% B2O3, 0.5% CeO2, 7% Na2O, 6% K2O, 4.1% Al2O3, 0.2% CaF2, 1.2% BaO, 0.3% SrO, 0.2% CaO, and 1.8% MgO.
[0093] The low-refractive-index radiation-resistant glass material of this preparation example is prepared by using quartz sand, boric acid, cerium oxide, sodium nitrate, potassium carbonate, aluminum oxide, fluorite, arsenic oxide, strontium carbonate, calcium carbonate, and magnesium carbonate as raw materials, mixing the various glass raw materials in proportion, melting the mixture at a high temperature of 1420°C, clarifying it with auxiliary stirring, mechanically drawing it at 1130°C, and annealing it at 588°C to obtain the glass material.
[0094] The detection method is the same as that of Preparation Example 1. The refractive index of the low-refractive-index radiation-resistant glass material obtained by the preparation method of this preparation example is 1.45, and the transmittance after 4700Gy of X-ray irradiation is 90.9% (decreased by 1.4%), the glass transition temperature Tg is 530°C, the expansion softening temperature Tf is 624°C, the softening point temperature Ts is 728°C, and the thermal expansion coefficient is 86.3×10 -7 / ℃, it has good process formability and process adaptability, and can be used as skin glass material for the production of optical glass fiber and optical fiber panels. The prepared optical fiber panels also have good radiation resistance and can fundamentally meet the application needs of radiation environments.
[0095] Comparative Example 1
[0096] The glass material of this comparative example is composed of the following components in molar percentages: 70% SiO2, 7.5% B2O3, 1.5% CeO2, 10% Na2O, 8.5% K2O, 1% Al2O3, 0.5% CaF2, and 1% MgO.
[0097] The glass material preparation method of this comparative example is: using quartz sand, boric acid, cerium oxide, sodium nitrate, potassium nitrate, aluminum hydroxide, fluorite, and magnesium carbonate as raw materials, mixing the various glass raw materials in proportion, and preparing the glass material according to the method of Preparation Example 1.
[0098] The detection method is the same as that of Preparation Example 1. The refractive index of the glass material of this comparative example is 1.55, and the transmittance after 4700Gy of X-ray irradiation is 82.3% (decreased by 3.7%), the glass transition temperature Tg is 538°C, the expansion softening temperature Tf is 626°C, the softening point temperature Ts is 727°C, and the thermal expansion coefficient is 88.1×10 -7 / ℃.
[0099] Comparative Example 2
[0100] The glass material of this comparative example is composed of the following components in molar percentages: 65% SiO2, 7.5% B2O3, 1% CeO2, 10% Na2O, 8.5% K2O, 1% Al2O3, 1% CaF2, 5% CaO, and 1% MgO.
[0101] The glass material preparation method of this comparative example is: using quartz sand, boric acid, cerium oxide, sodium nitrate, potassium carbonate, aluminum hydroxide, fluorite, calcium carbonate, and magnesium carbonate as raw materials, mixing the various glass raw materials in proportion, and preparing it according to the method of Preparation Example 1.
[0102] The detection method is the same as that of Preparation Example 1. The refractive index of the glass material of this comparative example is 1.67, the transmittance after 4700Gy of X-ray irradiation is 86.1% (decreased by 4.5%), the glass transition temperature Tg is 509°C, the expansion softening temperature Tf is 607°C, the softening point temperature Ts is 710°C, and the thermal expansion coefficient is 92.7×10 -7 / ℃.
[0103] Comparative Example 3
[0104] The glass material of this comparative example is composed of the following components in molar percentages: 82% SiO2, 8% B2O3, 3% CeO2, 1% K2O, 3% Al2O3, 1% As2O3, and 2% MgO.
[0105] The glass material preparation method of this comparative example is: using quartz sand, boric acid, cerium oxide, potassium nitrate, aluminum hydroxide fluorite, arsenic oxide, and magnesium carbonate as raw materials, mixing the various glass raw materials in proportion, and preparing the glass material according to the method of Preparation Example 1.
[0106] The detection method is the same as that of Preparation Example 1. The refractive index of the glass material of this comparative example is 1.6, the glass transition temperature Tg is 560°C, the transmittance after 4700Gy of X-ray irradiation is 79.5% (decreased by 4.7%), the expansion softening temperature Tf is 658°C, the softening point temperature Ts is 802°C, and the thermal expansion coefficient is 78.1×10 -7 / ℃.
[0107] Comparative Example 4
[0108] The glass material of this comparative example is composed of the following components in molar percentages: 73.2% SiO2, 7.3% B2O3, 7.0% NaO2, 3.0% K2O, 3.5% Al2O3, 1% CaF2, 2% CaO, and 3% MgO.
[0109] The glass material preparation method of this comparative example is: using quartz sand, boric acid, cerium oxide, sodium nitrate, potassium carbonate, aluminum hydroxide, fluorite, calcium carbonate, and magnesium carbonate as raw materials, mixing the various glass raw materials in proportion, and preparing it according to the method of Preparation Example 1.
[0110] The detection method is the same as that of Preparation Example 1. The refractive index of the glass material of this comparative example is 1.52, the transmittance after 4700Gy of X-ray irradiation is 78.7% (decreased by 9.4%), the glass transition temperature Tg is 552°C, the expansion softening temperature Tf is 647°C, the softening point temperature Ts is 766°C, and the thermal expansion coefficient is 82.5×10 -7 / ℃.
[0111] Example
[0112] The glass materials prepared in the above embodiments of the present invention can be used in the optical field to prepare optical components or optical instruments, such as optical glass and optical fiber panels, etc. The following embodiment illustrates the preparation of an optical fiber panel.
[0113] The glass material of the present invention can be nested with a core glass material (such as a hard optical fiber core glass material or a radiation-resistant glass material with a high refractive index), and drawn into a single filament or multiple multifilaments. The multifilaments are regularly arranged and melt-pressed into a blank plate segment, and then sliced, rounded, ground, and polished to produce an optical fiber panel. The size of the optical fiber panel can be customized, and the maximum size can reach the meter level. Figure 2 shows a large size (140×90×2mm) made of the low refractive index radiation-resistant glass material of the present invention as the skin glass. 3 ) Actual image of the radiation-resistant fiber optic panel.
[0114] Among them, the hard optical fiber core glass can be an ordinary optical fiber panel core glass material, or it can be as described in Chinese patent CN201110378012.4; the high refractive index radiation-resistant glass material is such as the glass material described in Chinese patent CN202310200621.3. In particular, when the glass material described in this patent is used as the core glass material and the glass material of the present invention (as skin glass) is used to prepare an optical fiber panel, the two can be perfectly matched during the drawing process, have good process formability and process adaptability, and the prepared optical fiber panel also has better radiation resistance.
[0115] Example 1
[0116] The core glass material composition is: 36% BaO, 25.2% La2O3, 14% B2O3, 5.9% Nb2O5, 6.3% Ta2O5, 5.1% ZrO2, 3.2% Al2O3, 2.2% CaO, 1.5% K2O, and 0.6% Na2O. The above proportions are by mass. Its refractive index is 1.864, and its transmittance after 4700Gy of X-ray irradiation is 80.83% (a decrease of 1.18%). The glass transition temperature is 619°C, and the thermal expansion coefficient is 92.4×10 -7 / ℃.
[0117] The glass material of Preparation Example 4 of the present invention is used as the skin glass material of the optical fiber panel, matched with the above-mentioned core glass material, and is drawn into single-filament and multiple-filament multifilaments. After the multifilaments are regularly arranged, they are melt-pressed into blank plate segments, and then sliced, rounded, ground and polished to prepare radiation-resistant optical fiber panels. The transmittance at a wavelength of 560nm is tested before and after 4700GyX-ray radiation, and the transmittance is 71.2% and 53.9% (a decrease of 17.3%) respectively.
[0118] Example 2
[0119] The core glass material composition is: 27.5% SiO2, 2% Al2O3, 5% CaO, 8% BaO, 50% PbO, 3% CeO2, 2% La2O3, 0.5% Nb2O5, 1% Ta2O5, 0.5% Rb2O, and 0.5% Cs2O. The above proportions are by mass. Its refractive index is 1.83, and its transmittance after 4700Gy of X-ray irradiation is 80.83% (a decrease of 1.18%). The glass transition temperature is 574°C, the expansion softening temperature is 680°C, and the thermal expansion coefficient is 86.2×10 -7 / ℃.
[0120] The glass material of Preparation Example 4 of the present invention is used as the skin glass material of the optical fiber panel, and the above-mentioned glass material is used as the core glass material. It is drawn into a single filament and multiple multifilaments, and the multifilaments are regularly arranged and melt-pressed into a blank plate segment. Then, it is sliced, rounded, ground and polished to prepare a radiation-resistant optical fiber panel. The transmittance at a wavelength of 560nm is tested to be 81.1% and 80.4% (a decrease of 0.7%) before and after 4700Gy X-ray radiation.
[0121] In addition, optical fiber panels prepared using the glass materials obtained in other embodiments of the present invention and the core glass material described above also have good radiation resistance, with the decrease in transmittance at 560nm being ≤0.89% before and after 4700Gy X-ray radiation.
[0122] Comparative Example 1
[0123] The core glass material composition is: 27.5% SiO2, 2% Al2O3, 5% CaO, 8% BaO, 50% PbO, 3% CeO2, 2% La2O3, 0.5% Nb2O5, 1% Ta2O5, 0.5% Rb2O, and 0.5% Cs2O. The above proportions are by mass. Its refractive index is 1.83, and its transmittance after 4700Gy of X-ray irradiation is 80.83% (a decrease of 1.18%). The glass transition temperature is 574°C, the expansion softening temperature is 680°C, and the thermal expansion coefficient is 86.2×10 -7 / ℃.
[0124] The composition of the skin glass material is: 78.2% SiO2, 1.8% Al2O3, 4.4% B2O3, 1.5% CaO, 1.5% Li2O, 5.0% Na2O, 7.0% K2O, 0.5% F2, 0.1% SnO2. The above proportions are molar percentages. Its refractive index is 1.46, its expansion softening temperature Tf is 688℃, its softening point temperature Ts is 759℃, and its thermal expansion coefficient is 78×10 -7 / ℃.
[0125] The above two glass materials are used as core and skin glass materials, and are drawn into single-filament and multiple-fiber filaments. The multifilaments are regularly arranged and melt-pressed into blank plate segments. Then, they are sliced, rounded, ground and polished to prepare radiation-resistant optical fiber panels. The transmittance at a wavelength of 560nm is tested before and after 4700GyX-ray radiation, and the results are 78.5% and 73.2% respectively (a decrease of 5.3%).
[0126] Comparative Example 2
[0127] The core glass material composition is: 36% BaO, 25.2% La2O3, 14% B2O3, 5.9% Nb2O5, 6.3% Ta2O5, 5.1% ZrO2, 3.2% Al2O3, 2.2% CaO, 1.5% K2O, and 0.6% Na2O. The above proportions are by mass. Its refractive index is 1.864, and its transmittance after 4700Gy of X-ray irradiation is 80.83% (a decrease of 1.18%). The glass transition temperature is 619°C, and the thermal expansion coefficient is 92.4×10 -7 / ℃.
[0128] The composition of the skin glass material is: 78.2% SiO2, 1.8% Al2O3, 4.4% B2O3, 1.5% CaO, 1.5% Li2O, 5.0% Na2O, 7.0% K2O, 0.5% F2, 0.1% SnO2. The above proportions are molar percentages. Its refractive index is 1.46, its expansion softening temperature Tf is 688℃, its softening point temperature Ts is 759℃, and its thermal expansion coefficient is 78×10 -7 / ℃.
[0129] The above two glass materials are used as core and skin glass materials, and are drawn into single-filament and multiple-fiber filaments. The multifilaments are regularly arranged and melt-pressed into blank plate segments. Then, they are sliced, rounded, ground and polished to prepare radiation-resistant optical fiber panels. The transmittance at a wavelength of 560nm is tested to be 66.6% and 23.3% (a decrease of 43.3%) before and after 4700GyX-ray radiation.
[0130] The following Tables 1 and 2 respectively summarize the glass sample compositions and glass properties of the above-listed illustrative preparation examples and comparative examples of the present invention.
[0131] Table 1 Composition of glass samples of Preparation Examples 1 to 6 and Comparative Examples 1 to 4
[0132] Table 2 Performance test results of glass samples of Preparation Examples 1 to 6 and Comparative Examples 1 to 4
[0133] As shown in Table 2, the low-refractive-index radiation-resistant glass material provided by the present invention has a refractive index of ≤1.47, a glass transition temperature Tg ≤550°C, an expansion softening temperature Tf ≤645°C, and a softening point temperature Ts ≤748°C. It has good process formability and process adaptability, and a thermal expansion coefficient of (82-87)×10- -7 / ℃, has good thermal processing performance, is conducive to the molding and preparation of large-size devices, matches the core glass material, and can be used as skin glass material for the production of optical glass fiber and optical fiber panels. After 4700Gy dose of X-ray irradiation, the transmittance drops by ≤2%. The prepared optical fiber panel also has good radiation resistance and can fundamentally meet the application of radiation environment.
[0134] The various specific technical features described in the above embodiments of the present invention can be combined in any appropriate manner without contradiction. In order to avoid unnecessary repetition, the present invention will not further explain various possible combinations.
[0135] The foregoing description is merely a preferred embodiment of the present invention and is not intended to limit the present invention. Those skilled in the art will readily appreciate that various modifications and variations of the present invention are possible. Any modifications, equivalent substitutions, or improvements made within the spirit and principles of the present invention are intended to be within the scope of protection of the present invention.
Claims
1. A glass material, which, by mole percentage, consists of the following components: 60-80% SiO2, 2-10% B2O3, 0.1-1% CeO2, 5-10% Na2O, 2-10% K2O, 1-8% Al2O3, 0-2% CaF2, 0-1% As2O3, and 1-5% alkaline earth metal oxide, wherein the alkaline earth metal oxide is selected from at least one of BaO, SrO, CaO and MgO.
2. The glass material according to claim 1, characterized in that The invention is composed of the following components by mole percentage: 60-80% SiO2, 2-10% B2O3, 0.1-1% CeO2, 5-10% Na2O, 2-10% K2O, 1-8% Al2O3, 0-2% CaF2, 0.1-1% As2O3, and 1-5% alkaline earth metal oxide, wherein the alkaline earth metal oxide is selected from at least one of BaO, SrO, CaO and MgO; Preferably, the present invention is composed of the following components by mole percentage: 60-80% SiO2, 2-10% B2O3, 0.1-1% CeO2, 5-10% Na2O, 2-10% K2O, 1-8% Al2O3, 0.1-2% CaF2, 0-1% As2O3, and 1-5% alkaline earth metal oxide, wherein the alkaline earth metal oxide is selected from at least one of BaO, SrO, CaO and MgO; Preferably, it is composed of the following components, measured by mole percentage: 60-80% SiO2, 2-10% B2O3, 0.1-1% CeO2, 5-10% Na2O, 2-10% K2O, 1-8% Al2O3, 0.1-2% CaF2, 0.1-1% As2O3, and 1-5% alkaline earth metal oxide, wherein the alkaline earth metal oxide is selected from at least one of BaO, SrO, CaO and MgO.
3. The glass material according to claim 1 or 2, characterized in that: The alkaline earth metal oxide contains at least MgO, and its content is 1 to 3.5% by mole percentage; Preferably, the alkaline earth metal oxide contains at least BaO, and its content is 0.5 to 1.5% by mole percentage; Preferably, the alkaline earth metal oxide contains at least SrO, and its content is 0.2-0.5% by mole percentage; Preferably, the alkaline earth metal oxide contains at least CaO, and its content is 0.2-1% by mole percentage; Preferably, the alkaline earth metal oxide is MgO, or a combination of BaO and MgO, or a combination of BaO, SrO, CaO and MgO; Preferably, when the alkaline earth metal oxide contains MgO and at least one selected from BaO, SrO and CaO, the content of MgO in the total amount of the alkaline earth metal oxide is ≥50%, preferably 50-75%; Preferably, the sum of the contents of Na2O and K2O is ≥ 10%, preferably 10-20%; Preferably, the total content of CeO2 and As2O3 is ≥ 0.1%, preferably 0.2-1.5%.
4. The glass material according to any one of claims 1 to 3, characterized in that Its refractive index is ≤1.47; Preferably, its glass transition temperature Tg≤550°C; Preferably, its expansion softening temperature Tf≤645°C; Preferably, its softening point temperature Ts≤748°C; Preferably, its thermal expansion coefficient at 20°C to 300°C is (82 to 87)×10 -7 / ℃; Preferably, the transmittance at 560 nm is ≥90.8%, and after irradiation with a dose of 4700 Gy of X-rays, the transmittance at 560 nm decreases by ≤2%.
5. A method for preparing the glass material according to any one of claims 1 to 4, comprising: The raw materials are mixed in proportion, melted at high temperature, clarified by auxiliary stirring, cooled to form, and annealed to obtain the product.
6. The method according to claim 5, characterized in that: The high temperature melting temperature is 1380-1520°C, the molding temperature is 1080-1320°C, and the annealing temperature is 580-610°C.
7. An optical element made of the glass material according to any one of claims 1 to 4.
8. An optical glass fiber, wherein the sheath portion of the optical glass fiber comprises the glass material according to any one of claims 1 to 4.
9. An optical fiber faceplate, wherein the skin portion thereof comprises the glass material according to any one of claims 1 to 4.
10. Use of the glass material according to any one of claims 1 to 4 in the field of optics, preferably use of the glass material in preparing optical elements or optical instruments; wherein: The optical element or optical instrument includes optical glass and an optical fiber panel.
Citation Information
Patent Citations
Low-refractive glass applied to drawing formation preparation of optical fiber faceplate and preparation method thereof
CN106517772A
Image intensifier with double-fiber light cone structure and image enhancement type detection imaging system
CN114171366A
Scintillation glass, scintillation glass panel and manufacturing method thereof
CN114988697A
Radiation shielding glass having an improved gamma irradiation browning and dielectric breakdown