Polybutadiene latex and preparation method therefor, and ABS high rubber powder, preparation method therefor and use thereof
By controlling the preparation process of polybutadiene latex, the specific content of butadiene structure in ABS high glue powder is ensured, and the problem of insufficient horizontal combustion speed of ABS resin is solved, and the effect of low-level combustion speed is achieved. It is suitable for thin-wall flame retardant fields. .
Patent Information
- Application Number
- PCT/CN2023/115544
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-05-11
- Filing Date
- 2023-08-29
- Publication Date
- 2024-11-14
AI Technical Summary
The existing ABS resin is difficult to reach HB75 in terms of horizontal combustion speed, and cannot meet the high requirements of the home appliance industry for material performance stability.
By controlling the preparation process of polybutadiene latex, including adjusting the supplemental acceleration and replenishment timing, reaction temperature, and the amount of components added, ensuring Trans-1,4 butadiene and Cis in dry-based rubber -1,4 butadiene structure is within a specific range, thereby preparing ABS high glue powder with low level combustion speed.
The low-level combustion speed of ABS resin is achieved, which is particularly suitable for thin-wall flame retardant applications and reduces the flame spread speed.
Smart Images

Figure PCTCN2023115544-FTAPPB-I100001 
Figure PCTCN2023115544-FTAPPB-I100002 
Figure PCTCN2023115544-FTAPPB-I100003
Abstract
Description
A polybutadiene latex and its preparation method and an ABS high-rubber powder and its preparation method and application Technical Field
[0001] The present invention relates to the technical field of polymer materials, in particular to a polybutadiene latex and a preparation method thereof, and an ABS high-rubber powder and a preparation method and application thereof. Background Art
[0002] ABS resin boasts excellent heat resistance, impact resistance, rigidity, corrosion resistance, and dimensional stability, making it widely used in a wide range of fields, including household appliances, electronic products, industrial parts, and the automotive industry. ABS resin, one of the five major engineering plastics, possesses excellent mechanical and processing properties, and is widely used in automotive manufacturing, household appliance production, and other fields. ABS resin is a thermoplastic resin with an island-in-the-sea structure, formed by dispersing a polybutadiene rubber phase in a SAN resin (a copolymer of styrene and acrylonitrile). Currently, the two most widely used methods for preparing ABS resin are the continuous bulk method and the emulsion grafting-bulk SAN blending method.
[0003] The emulsion grafting-bulk SAN blending method has become the mainstream method for ABS resin production in the market due to its high equipment versatility, flexible formulation switching, wide product range, and high output per unit. This method involves polymerizing butadiene via emulsion to produce polybutadiene latex (PBL). Styrene and acrylonitrile are then grafted onto the polybutadiene latex particles. The resulting ABS grafted powder is then coagulated and dried to produce ABS resin. This is then blended with SAN resin and extruded into pellets to produce ABS resin.
[0004] The trend toward larger appliances and thinner walls in the OA industry is placing higher demands on material performance stability. ABS resin is typically used for housings, but currently available materials on the market struggle to achieve a horizontal burning velocity of HB75, failing to meet industry requirements.
[0005] Summary of the Invention
[0006] The object of the present invention is to provide a polybutadiene latex with a low horizontal burning speed and a preparation method thereof, and to provide ABS high-rubber powder obtained from the polybutadiene latex, which also has the advantage of a low horizontal burning speed.
[0007] The present invention is achieved through the following technical solutions:
[0008] A polybutadiene latex contains 7-10 g / L of vinyl structure, 18-30 g / L of Trans-1,4 butadiene structure, and 10-24 g / L of Cis-1,4 butadiene structure in dry base rubber.
[0009] The above parameters are characterized and measured according to SH / T 1727-2004. Preferably, the dry rubber in the polybutadiene latex contains 8-9 g / L of vinyl structure, 22-26 g / L of Trans-1,4 butadiene structure, and 10-16 g / L of Cis-1,4 butadiene structure.
[0010] The preparation method of the polybutadiene latex comprises the following steps: adding 85-95 parts of butadiene in an initial amount, 0.1-1 part of an initiator, 0.5-2 parts of an electrolyte, 1-5 parts of an emulsifier, 0.1-1 part of a chain transfer agent and 90-200 parts of water into a reactor, mixing them uniformly, heating the reactor to 55-85° C. and carrying out polymerization reaction; and when the butadiene conversion rate is 50% or less than or equal to 70%, starting to add the remaining butadiene monomer to 100 parts, controlling the addition to be completed within 2-4 hours, during which the temperature is controlled at 55-85° C., and when the total conversion rate of the butadiene monomers is greater than or equal to 95%, obtaining the polybutadiene latex.
[0011] Preferably, the process parameters of the preparation method are as follows: in parts by weight, an initial amount of 88-93 parts of butadiene, 0.2-0.8 parts of initiator, 0.8-1.5 parts of electrolyte, 1.5-4.5 parts of emulsifier, 0.2-0.8 parts of chain transfer agent, and 90-200 parts of water are added to a reactor and mixed uniformly, and the temperature is raised to 60-80° C. to carry out polymerization reaction; when the butadiene conversion rate is 55%≤≤65%, the remaining butadiene monomer is added to 100 parts, and the addition is completed within 2.5-3.5 hours, during which the temperature is controlled at 65-75° C.; when the total conversion rate of butadiene monomers is ≥95%, polybutadiene latex is obtained.
[0012] Optionally, the emulsifier is selected from anionic emulsifiers; the anionic emulsifier is selected from at least one of potassium oleate, potassium disproportionated rosinate, sodium lauryl sulfate, sodium dodecylbenzenesulfonate, and dioctyl sodium sulfosuccinate.
[0013] The electrolyte is selected from at least one of potassium bicarbonate, potassium carbonate, sodium bicarbonate, sodium carbonate, and sodium tripolyphosphate;
[0014] The chain transfer agent is selected from at least one of n-butyl mercaptan, n-octyl mercaptan, n-dodecyl mercaptan, and tert-dodecyl mercaptan;
[0015] The initiator includes (but is not limited to): hydrogen peroxide compounds, such as tert-butyl peroxide (which can be di-tert-butyl peroxide, tert-butyl hydroperoxide, 2,5-dimethyl-2,5-bis(tert-butylperoxy)hexane), p-menthane hydroperoxide, etc.; peroxyketal compounds, such as 1,1-bis-tert-butylperoxy-3,3,5-trimethylcyclohexane, 2,2-bis(4,4-bis(tert-butylperoxy)cyclohexyl)propane, Alkanes, etc.; peroxyester compounds, such as tert-butyl peroxypivalate, 2,5-dimethyl-2,5-di(2-ethylhexanol peroxy)hexane, etc.; peroxyketal compounds, such as 4,4-diperoxytert-butyl-n-butyl-valerate, etc.; peroxycarbonate compounds, such as 2-ethylhexyl tert-amyl peroxycarbonate, 2-ethylhexyl tert-butyl peroxycarbonate, etc.; or azo compounds with nitro and cyclohexane, etc.
[0016] An ABS high-rubber powder using the polybutadiene latex of the present invention comprises the following components by weight percentage: 20-80 wt% of the polybutadiene in the polybutadiene latex of the present invention; and 20-80 wt% of SAN grafted and blended on the surface of the polybutadiene.
[0017] The polybutadiene latex obtained by the preparation method of the polybutadiene latex of the present invention is further grafted with a styrene-acrylonitrile copolymer, coagulated, dehydrated, dried, and then blended with SAN to obtain ABS high-rubber powder.
[0018] The preparation method of ABS high-rubber powder is as follows: 60 parts of the above-mentioned polybutadiene latex are added to a reactor, and 2-4 parts of ferrous sulfate are added to the reactor and uniformly stirred. The reactor is heated to 65-70°C, and 0.1-0.5 parts of cumene hydroperoxide (initiator), 35-70 parts of acrylonitrile / styrene, 0.1-0.3 parts of tert-dodecyl mercaptan, 1-3 parts of sodium lauryl sulfonate, and 50-70 parts of deionized water are added. After heating is completed, the reaction is continued for 4-6 hours to obtain a grafted latex. The grafted latex is added to a coagulant reactor, stirred and heated to 70-80°C, and ethyl sulfuric acid is gradually added thereto over 1-4 hours. The temperature is then raised to 88-95°C and maintained at this temperature for 1-5 hours. The resulting coagulant latex is filtered, dried, and then blended with SAN through a twin-screw extruder to obtain ABS high-rubber powder.
[0019] The present invention has the following beneficial effects:
[0020] Butadiene polymerization is divided into tetrapolymerization and dipolymerization. The units obtained from tetrapolymerization contain cis / trans structures, while the units obtained from dipolymerization are vinyl. The present invention primarily controls the addition rate and timing of butadiene monomer addition (butadiene conversion rate), reaction temperature, and the amounts of each component in the polybutadiene latex preparation process to control the content of 1,2 and cis-1,4 structures in the backbone rubber to within a specific range. This results in the ABS high-density rubber powder prepared from the polybutadiene latex having a lower horizontal combustion velocity.
[0021] Through experiments, the inventors discovered that the 1,2-structure in the backbone butadiene rubber provides tertiary carbon atoms during combustion, making it highly active and reacting with oxygen to produce free radicals that promote polymer decomposition. The cis-1,4 structure also favors the formation of cyclic molecules during combustion. During horizontal combustion of ABS resin, polybutadiene preferentially decomposes, reducing the content of active tertiary carbon atoms and favoring the formation of cyclic molecules such as cyclohexene and polydipentene. This increases the molecular weight of organic molecules in the gas phase, allowing thermal radiation to dominate heat transfer, thereby reducing the flame spread rate. ABS resin prepared from the polybutadiene latex of the present invention exhibits a very low horizontal combustion velocity, making it particularly suitable for thin-wall flame-retardant applications. DETAILED DESCRIPTION
[0022] The present invention will be described in detail below with reference to specific embodiments. The following embodiments will help those skilled in the art to further understand the present invention, but are not intended to limit the present invention in any form. It should be noted that, for those skilled in the art, several variations and improvements can be made without departing from the scope of the present invention. These all fall within the scope of protection of the present invention.
[0023] The raw materials required for the preparation of the ABS high-rubber powder of the present invention are as follows:
[0024] Emulsifier:
[0025] A: Potassium disproportionate rosinate, purity 98%, Aladdin;
[0026] B: Potassium oleate, purity 98%, Aladdin;
[0027] Electrolytes:
[0028] A: Potassium carbonate, industrial grade, Uni-T;
[0029] B: Potassium bicarbonate, industrial grade, Uni-D;
[0030] Chain transfer agent:
[0031] A: tert-Dodecylmercaptan, purity 99.5%, Aladdin;
[0032] B: n-Dodecyl mercaptan, 98% purity, Chevron Phillips;
[0033] Initiator:
[0034] A: Tert-butyl peroxide, di-tert-butyl peroxide, purity 97%, Aladdin;
[0035] B: tert-butyl peroxypivalate, initiator LQ-TBPV, Lanzhou Auxiliary Agent Factory;
[0036] Preparation method of polybutadiene latex of Examples and Comparative Examples (addition of various raw materials is shown in the table): 130 parts by weight of butadiene, initiator, electrolyte, emulsifier, chain transfer agent and water are added to a reactor and mixed uniformly, and polymerization reaction is carried out at a specific temperature (specific temperature is shown in the table, note the reaction temperature of stage 1); when the butadiene conversion rate is 50%≤≤70% (specific conversion rate is shown in the table, the conversion rates of latex 17 / 18 are 46.2% and 74.1%, respectively), butadiene monomer is added, the time used for adding butadiene is (see the table), and the reaction temperature is controlled (specific temperature is shown in the table, note the reaction temperature of stage 2), and when the total conversion rate of butadiene monomers is ≥95%, polybutadiene latex is obtained.
[0037] Various test methods:
[0038] (1) Conversion Test: To test the residual butadiene monomer in latex, take a 0.1g sample into a 20ml headspace vial, dilute it to 2g with DMF, and analyze the sample using a PE TurboMatrix 40 headspace sampler and a Shimadzu GC 2010 gas chromatograph to determine the residual butadiene monomer content. The mass of the butadiene monomer remaining in the reactor is then calculated. Calculation of butadiene conversion: Butadiene conversion = (total mass of butadiene added to the reactor - mass of the butadiene monomer remaining in the reactor) / total mass of butadiene added to the reactor.
[0039] (2) The dry basis rubber structure determination method in polybutadiene latex is carried out in accordance with the test standard SH / T 1727-2004. 100 g of butadiene latex smear sample is taken, dried at 80°C to constant weight, extracted in ethanol / toluene (ETA), and then vacuum dried at 50-60°C; 100 mg of the extracted sample is dissolved in 20 mg of dichloromethane, and the latex solution is filtered; 3-4 drops of the latex solution are added to a horizontally placed salt plate, and the solvent is evaporated at room temperature; the infrared spectrometer is a BRUKER TENSOR 27, with a range of 2000-600 cm -1 Scan internally and draw the baseline. Measure 965 (A 965 )cm -1 、900(A 909 )cm -1 , and 728(A 728)cm -1 The absorbance of the wave number is used to characterize the content of trans (A965), vinyl (A909) and cis (A728). The absorbance is normalized to %A 965 =A 965 / (A 965 +A 909 +A 728 )×100; %A 909 =A 909 / (A 965 +A 909 +A 728 )×100; %A 728 =A 728 / (A 965 +A 909 +A 728 )×100;
[0040] The trans (A965), vinyl (A909) and cis (A728) contents are calculated according to the following formula, in g / L: Ccis = 1.7896 × %A 728 -0.0253×%A 965 -0.085×%A 909 ; C trans = 0.3971 × % A 965 -0.0502×%A 728 -0.0142×%A 909 ; C vinyl = 0.2954 × % A 909 -0.0075×%A 728 -0.0065×%A 965 .
[0041] (3) Horizontal burning rate (HB burning rate) test method: According to the test standard UL94-2000, the thickness of the ABS high rubber powder sample is 2.0 mm.
[0042] Table 1: Parameters (parts by weight) and test results of polybutadiene latex
[0043] It can be seen from Latexes 1 to 9 that the preferred process for polybutadiene latex can produce latex with a preferred structural polybutadiene composition.
[0044] Table 1 continued:
[0045] Table 1 continued:
[0046] It can be seen from Latexes 10 to 18 that without adopting the process of the present invention, it is impossible to obtain the latex composed of the polybutadiene with the specific structure applied for in the present invention.
[0047] Preparation of ABS high-density latex: 60 parts of polybutadiene latex obtained in the above experimental example according to the formulation in Table 2 were added to a reactor, and 3 parts of ferrous sulfate were added to the reactor and stirred uniformly. The reactor was heated to 67°C, and 0.2 parts of cumene hydroperoxide, acrylonitrile / styrene (the final SAN content by weight is shown in the table), 0.2 parts of tert-dodecyl mercaptan, 1 part of sodium lauryl sulfonate, and 50 parts of deionized water were added dropwise continuously for 2 hours. After heating, the reaction was continued for 5 hours to obtain a grafted latex. 1000 parts of the grafted latex were added to a coagulant reactor, stirred, and heated to 75°C. 450 parts of 5% sulfuric acid were gradually added over 2 hours, and the temperature was raised to 91°C and maintained for 3 hours. The resulting coagulant latex was filtered through a 325-mesh filter and dried in a fluidized bed dryer at 60°C for 6 hours. SAN was then blended through a twin-screw extruder (the final SAN content by weight is shown in the table) to obtain an ABS high-density latex with a moisture content of <1%.
[0048] Among them, the test results of the source of polybutadiene latex and the content of each unit (weight percentage) are as follows
[0049] Table 2:
[0050] Table 2:
[0051] Table 2:
[0052] From the above test examples, it can be seen that the ABS high-rubber powder prepared from the preferred latex containing polybutadiene with a specific structure has a slow horizontal combustion speed, while the horizontal combustion speed of the ABS high-rubber powder of ABS high-rubber powder -10 to 18 (comparative example) is too fast.
Claims
1. A polybutadiene latex, characterized in that: The dry base rubber in the polybutadiene latex contains 7-10 g / L of vinyl structure, 18-30 g / L of Trans-1,4 butadiene structure and 10-24 g / L of Cis-1,4 butadiene structure.
2. The polybutadiene latex according to claim 1, characterized in that The dry base rubber in the polybutadiene latex contains 8-9 g / L of vinyl structure, 22-26 g / L of Trans-1,4 butadiene structure and 10-16 g / L of Cis-1,4 butadiene structure.
3. The method for preparing the polybutadiene latex according to any one of claims 1 to 2, characterized in that: The method comprises the following steps: adding 85-95 parts of butadiene in an initial amount, 0.1-1.0 parts of initiator, 0.5-2 parts of electrolyte, 1-5 parts of emulsifier, 0.1-1 parts of chain transfer agent and 90-200 parts of water into a reactor by weight, mixing them evenly, heating to 55-85° C. to carry out polymerization reaction; when the butadiene conversion rate is 50%≤≤70%, starting to add the remaining butadiene monomer to 100 parts, controlling the addition to be completed within 2-4 hours, during which the temperature is controlled at 55-85° C., and when the total conversion rate of butadiene monomers is ≥95%, obtaining polybutadiene latex.
4. The method for preparing polybutadiene latex according to claim 3, characterized in that: The method comprises the following steps: adding 88-93 parts of butadiene in an initial amount, 0.2-0.8 parts of initiator, 0.8-1.5 parts of electrolyte, 1.5-4.5 parts of emulsifier, 0.2-0.8 parts of chain transfer agent and 90-200 parts of water into a reactor by weight, mixing them evenly, heating to 60-80 DEG C to carry out polymerization reaction; when the butadiene conversion rate is 55%≤≤65%, starting to add the remaining butadiene monomer to 100 parts, controlling the addition to be completed within 2.5-3.5 hours, during which the temperature is controlled at 65-75 DEG C, and when the total conversion rate of butadiene monomers is ≥95%, obtaining polybutadiene latex.
5. The method for preparing polybutadiene latex according to claim 3, characterized in that: The emulsifier is selected from anionic emulsifiers; the anionic emulsifier is selected from at least one of potassium oleate, potassium disproportionated rosin acid, sodium dodecyl sulfate, sodium dodecylbenzene sulfonate, and dioctyl sodium sulfosuccinate; the electrolyte is selected from at least one of potassium bicarbonate, potassium carbonate, sodium bicarbonate, sodium carbonate, and sodium tripolyphosphate; the chain transfer agent is selected from at least one of n-butyl mercaptan, n-octyl mercaptan, n-dodecyl mercaptan, and tert-dodecyl mercaptan; the initiator is selected from at least one of hydrogen peroxide compounds, peroxyketal compounds, peroxyester compounds, peroxyketal compounds, peroxycarbonate compounds, and azo compounds with nitro and cyclohexane.
6. An ABS high-rubber powder, characterized in that: By weight percentage, it includes the following components: 20-80 wt % of polybutadiene in the polybutadiene latex according to any one of claims 1 to 2; Polybutadiene surface grafted and blended SAN 20-80wt%.
7. The method for preparing the ABS high-rubber powder according to claim 6, characterized in that: The following steps are involved: The polybutadiene latex as claimed in any one of claims 1 to 2 is grafted with styrene and acrylonitrile, and then coagulated, dehydrated, dried, and then blended with SAN to obtain ABS high-rubber powder.
8. The use of the ABS high-rubber powder according to claim 6, characterized in that: Used for thin-wall flame retardant parts.
Citation Information
Patent Citations
Low cis-polybutadiene rubber as well as preparation method and application thereof
CN102532377A
Olefin polymer, preparation method and application thereof
CN105860406A
Low cis-polybutadiene rubber and preparing method and application thereof
CN106589247A
Preparation method of polybutadiene with greatly adjustable microstructure content and crystallinity
CN107266619A
Polybutadiene latex and preparation method thereof, ABS high rubber powder and preparation method and application thereof
CN116554376A
Cited By
Abs high rubber powder for pc / abs alloy and method for preparing the same
CN122790162A