Method for preparing monocrystalline silicon film based on laser interference technology
Through the combination of steady-state laser interference technology and magnetron sputtering, the problems of uneven surface, high roughness and low crystallinity in thin film preparation are solved, and the preparation of single crystal silicon film with high transmittance and crystallization is achieved, simplifying the It can reduce environmental pollution and is suitable for a wide range of applications.
Patent Information
- Application Number
- PCT/CN2023/134683
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-05-08
- Filing Date
- 2023-11-28
- Publication Date
- 2024-11-14
AI Technical Summary
In the prior art, there are problems such as uneven surface, high roughness, large film damage, poor density, complex process, difficult growth parameters, low film crystallinity and environmental pollution during the film preparation process.
Steady-state laser interference technology combined with magnetron sputtering method is used to prepare a single crystal silicon film with uniform surface, high transmittance and high crystallization on the substrate surface, and is generated by using a steady-state laser source during magnetron sputtering. The uniform thermal gradient induces the uniform deposition of target nanoparticles to form a dense and flat single crystal silicon thin film.
The film has achieved the preparation of single crystal silicon film with high transmittance, low roughness, flat surface and high crystallization rate, simplified the process steps, reduced environmental pollution, improved processing efficiency, and is suitable for large areas and low environmental conditions. film preparation.
Smart Images

Figure CN2023134683_14112024_PF_FP_ABST
Abstract
Description
A method for preparing single crystal silicon thin film based on laser interference technology Technical Field
[0001] The present invention relates to the technical field of nanomaterial film preparation, and in particular to a method for preparing single-crystal silicon films based on laser interference technology, which uses a steady-state laser irradiation combined with magnetron sputtering method to induce the preparation of single-crystal silicon films. Background Art
[0002] Due to its unique characteristics, laser processing technology has become a common materials processing technique in recent years, widely used in a wide range of fields. With the gradual development and continuous improvement of laser technology, the performance of high-power lasers has continued to improve. This technology offers significant advantages over traditional chemical and mechanical processing methods in terms of improving processing efficiency, accelerating production schedules, protecting the environment, reducing thermal damage to materials, and maintaining surface integrity. Consequently, laser processing technology has made rapid progress in recent years. Furthermore, laser processing can be combined with mechanical and chemical processing methods. For example, laser processing can be combined with chemical etching, electrochemical etching, liquid thin film technology, and liquid phase jet technology. The application of these methods significantly improves the processing efficiency of traditional technologies, addressing the time-consuming, costly, and polluting nature of traditional structural processing techniques, and expanding the application of laser processing technology in fields such as automotive manufacturing, aerospace, and biomedicine.
[0003] Traditional thin film preparation methods include sol-gel, molecular beam epitaxy (MBE), and metal-organic chemical vapor deposition (MOCVD). Each thin film preparation method has its own unique focus, characteristics, and advantages for the types of films produced.
[0004] Although the sol-gel method for preparing thin films can ensure uniformity at the molecular level, it has poor density and performance, and is prone to other reactions when preparing semiconductor devices, especially for Group IV elements. Molecular Beam Epitaxy (MBE) can precisely control and repeatedly grow ultra-thin epitaxial layer samples to form high-quality thin film samples. However, the MBE technology for coating films has too high requirements for process and equipment, making it impossible to produce on a large scale. Metal-organic Chemical Vapor Deposition (MOCVD) is often used to deposit compound semiconductor single crystal thin films. The disadvantage is that toxic gases may be generated during the MOCVD preparation process, and the preparation cost is high. Magnetron sputtering is a "high-speed, low-temperature sputtering technology." In comparison, magnetron sputtering technology can control the film area and has a higher deposition rate. At the same time, the thin films prepared by magnetron sputtering technology not only have good density, but also because the entire sputtering process takes place in a closed environment, the grown thin films have the advantages of high purity and no pollution.
[0005] Chinese patent CN113873738A discloses a self-supporting carbon-based capacitor target and its preparation method. The method utilizes photolithography, radio frequency magnetron sputtering, oxygen plasma etching, and wet etching to prepare a surface-structured α-C film. A DLC film is then formed on a polished copper foil using pulsed laser deposition. The polished copper foil of the DLC film is then melted away and rinsed multiple times in deionized water. The DLC film floating on the water surface is then removed using the surface-structured α-C film, and the copper film is then dissolved to obtain a carbon-based double-layer film. The carbon-based double-layer film is then rinsed multiple times in deionized water, removed using a target holder with circular holes, and allowed to evaporate naturally to dry, resulting in a self-supporting carbon-based capacitor target. The present invention effectively achieves a self-supporting carbon-based double-layer target with easy operation. The self-supporting carbon-based capacitor target is expected to achieve the desired results in physical experiments. However, the existing technology is somewhat insufficient in terms of film surface structure preparation, process steps, density, and environmental pollution. The present invention can prepare a high-precision thin film with uniform surface structure, flatness and smoothness through multi-beam laser interference induction combined with magnetron sputtering, thereby solving the problems of low surface structure accuracy, difficult to control structure size, complex process, poor density, environmental pollution and other problems of the thin film prepared by the etching process in the prior art.
[0006] Chinese patent CN105742407B discloses a method for preparing black silicon on a doped film layer. A doped silicon film layer is deposited on a clean silicon substrate using magnetron sputtering. The surface microstructure is then formed using femtosecond laser irradiation. After thermal annealing in an ambient environment, the resulting doped black silicon material exhibits consistent high absorption characteristics for light in the 400nm to 2400nm band: 95% absorptivity in the visible light band of 400-1100nm and 90% absorptivity in the near-infrared band of 1100-2400nm. This method lays a technical foundation for expanding the application of black silicon materials. Compared with existing technologies, solid film doping methods enrich the variety of doping elements, increase doping concentration, and reduce doping costs; they also reduce process steps and improve preparation efficiency. However, due to factors such as film damage, absorptivity, and roughness, existing technologies are somewhat insufficient. The single-crystal thin film produced by the present invention, deposited via steady-state laser induced deposition, exhibits advantages such as minimal damage, smooth surface, low roughness, and high absorptivity. The invention solves the problems of large film damage, uneven surface and low absorption rate caused by femtosecond laser ablation in the prior art.
[0007] Chinese patent CN102051589B discloses a method for preparing silicon carbide amorphous and epitaxial thin films at low temperatures. The method comprises growing a silicon carbide thin film on a substrate; cleaning the surfaces of the substrate and target material and placing them in a vacuum growth chamber, evacuating the chamber using a mechanical pump and a molecular pump; heating the substrate with a heater; and simultaneously adding an external light source to the substrate for direct illumination; growing the silicon carbide thin film using magnetron sputtering or laser pulses, with the deposition frequency controlling the crystal form of the grown silicon carbide; and annealing the substrate, which may be protected by an atmosphere during annealing. The method significantly reduces the growth temperature of the silicon carbide thin film, producing amorphous silicon carbide thin films or preferentially oriented crystalline films of 3C-SiC, 2H-SiC, 4H-SiC, and 15R-SiC structures. These films can be used in optoelectronics and microelectronics in semiconductor device manufacturing. However, the existing technology is somewhat insufficient in terms of film crystallinity. The present invention prepares a single-crystal silicon film with a high crystallization rate by inducing multi-beam steady-state laser interference, thereby solving the problem of insufficient crystallinity of thin films prepared by pulse laser in the prior art.
[0008] Chinese patent CN105039875B discloses a Ni-Nb metal film with ultra-low roughness and its preparation method. A target material synthesized from Ni and Nb metal raw materials is placed on the target position of a multi-target magnetron sputtering coating device. A single-sided polished silicon wafer is used as the substrate and mounted on a substrate holder, and the distance is adjusted. The chamber is evacuated and then filled with argon gas. The pressure in the chamber is adjusted for pre-sputtering. Sputtering is then performed. The single-sided polished silicon wafer is removed to obtain Ni-Nb metal films with different Ni and Nb compositions. The metal film material prepared by the present invention has a surface roughness of less than 1nm and an ultra-smooth surface. It can be used in fields such as magnetic high-energy laser reflectors, laser gyro reflectors, and optical windows. As a functional component, it has high reliability, high frequency response, and high sensitivity, and has broad application prospects. However, considering the film thickness, crystallinity, and transmittance, the existing technology is slightly insufficient. The present invention uses a laser-induced method to prepare a thin film with high transmittance and high crystallinity. This solves the problems of large film thickness, insufficient crystallinity, and low transmittance prepared in the existing technology.
[0009] Summary of the Invention
[0010] Technical problem to be solved: This application proposes a method for preparing single-crystal silicon thin films based on laser interference technology to solve the problems existing in the traditional thin film preparation process in the prior art, such as uneven surface, high roughness, large film damage, poor film density, complex process, difficult to control growth parameters, low film crystallinity, and easy environmental pollution. That is, a single-crystal silicon film with thin film, intact surface, uniform surface, high transmittance and high crystallization rate is prepared on the substrate surface by combining magnetron sputtering with laser interference induction. The inventive method has the advantages of large processing area, low environmental conditions, simple preparation process, safe and pollution-free, and small preparation structure size, realizing a thin film preparation technology that is suitable for most materials and has broad application prospects.
[0011] Technical solution:
[0012] A method for preparing a single crystal silicon thin film based on laser interferometry technology, the specific steps are as follows:
[0013] The first step is the preparation of silicon film: a pure silicon target with a purity of 99.999% is selected, a radio frequency magnetron sputtering source is used as the magnetron sputtering power source, and a SiO2 substrate is used as the substrate. The pure silicon target and the SiO2 substrate are placed in a vacuum chamber. When preparing the Si thin film sample, the initial temperature of the SiO2 substrate is room temperature, the target-substrate distance is set to 68 mm, and the sputtering gas used is 99.99% pure Ar. The working pressure during sputtering is 0.6 Pa, the sputtering power is 40-200 W, and the sputtering time is 10 minutes.
[0014] Step 2: At the beginning of sputtering, a steady-state laser source is used to uniformly distribute the light intensity on the surface of the SiO2 substrate using interference method to produce a uniform thermal gradient distribution, heat the SiO2 substrate, and induce the target Si nanoparticles to deposit on the surface of the SiO2 substrate to form a dense, flat, and highly transmittance single crystal silicon film with a film thickness of 800 to 990 nm.
[0015] As a preferred technical solution of the present application, the size of the pure silicon target in the first step is 48 mm in diameter and 3 mm in thickness.
[0016] As a preferred technical solution of the present application, the size of the SiO2 substrate in the first step is 10mm×10mm×1mm.
[0017] As a preferred technical solution of the present application, the magnetron sputtering power supply in the first step is a radio frequency AC power supply with a frequency of 10 to 35 MHz.
[0018] As a preferred technical solution of this application, the initial pressure in the vacuum chamber in the first step is 2.5*10 -4 Pa, the pressure during sputtering was maintained at 0.6Pa.
[0019] As a preferred technical solution of the present application, when a steady-state laser source is used for irradiation in the second step, the wavelength of the selected laser source is 475 nm, the power is 50 mW, and the irradiation time is 0 to 10 minutes.
[0020] As a preferred technical solution of the present application, during the second step of steady-state laser irradiation, the principle of multi-lens interference is utilized and a BS1 spectrometer is used to disperse the circular laser spot into an interference pattern of multiple beams of coherent light. The multiple beams of coherent light are converged on the substrate at an incident angle of 60° and an azimuth angle of 90° through the M1, M2, M3, and M4 plane mirrors, thereby generating a uniform thermal gradient so that the light intensity is evenly distributed on the substrate, inducing uniform growth of the silicon film.
[0021] The technical principle of this application is: laser processing technology has the advantages of high processing efficiency, fast production progress, environmental protection, and maintaining the integrity of the material surface. However, the laser processing in the existing technology will cause film damage by ablation on the film surface, and the transmittance and roughness of the film surface cannot be controlled. Magnetron sputtering is a "high-speed, low-temperature sputtering technology" that produces films with good density and high purity. However, magnetron sputtering requires heating at a heating rate of about 20°C / min, which is time-consuming and the uniformity of the film cannot be controlled. The present invention utilizes the principle of steady-state laser interference heating through multiple lenses. During magnetron sputtering, multiple beams of coherent light are irradiated on the substrate to generate a uniform thermal gradient distribution on the substrate, inducing the target particles to be evenly distributed on the substrate. At the same time, the photothermal effect generated by the interaction between photons and materials can greatly accelerate the deposition of induced nanoparticles to form a single crystal film with good density, low roughness, uniform surface, and high crystallization rate. Beneficial effects:
[0022] 1. This application combines laser processing technology with magnetron sputtering to form complementary advantages to meet the processing requirements of more fields. This processing method has the advantages of large processing area, low environmental conditions, simple preparation process, safety and pollution-free, and small preparation structure size, realizing a thin film preparation technology that is suitable for most materials and has broad application prospects.
[0023] 2. This method reduces the processing steps and can greatly improve the processing efficiency of traditional technology, solving the problems of high time consumption, high cost and serious pollution in structural processing by traditional technology.
[0024] 3. The thin film preparation technology of this application is more widely used in the fields of automobile manufacturing, aerospace, and biomedicine.
[0025] 4. The present application provides a new method for preparing thin films, namely, using steady-state laser induction combined with magnetron sputtering to prepare single-crystal silicon thin films. Compared with other thin film preparation technologies, this method requires a low ambient temperature, greatly shortens the processing time, and the prepared thin film has high transmittance, reaching 89.502% for the light band of 200-860nm, and the transmittance for the light band of 860-1200nm reaches 97.655%. The thin film has good surface uniformity, good density, low roughness, smooth surface, and high crystallization rate of single-crystal silicon film. BRIEF DESCRIPTION OF THE DRAWINGS
[0026] FIG1 is a schematic diagram of the principle of multi-beam laser interference heating in the method for preparing single-crystal silicon thin films based on laser interference technology of the present application, wherein Laser is a steady-state laser source, BS1 is a beam splitter, M1, M2, M3, and M4 are plane mirrors, the incident angle α is 60°, and the azimuth angle β is 90°;
[0027] FIG2 is a method for preparing a single-crystal silicon thin film based on laser interferometry technology of the present application, and a Raman spectrum of the silicon film;
[0028] FIG3 is a method for preparing a single-crystal silicon thin film based on laser interferometry technology of the present application, and an XRD pattern of the silicon film surface;
[0029] FIG4 is a SEM image of the surface of the silicon film according to the method for preparing a single-crystal silicon thin film based on laser interferometry technology of the present application;
[0030] FIG5 is a diagram showing the transmittance of a silicon film according to the method of the present application for preparing a single-crystal silicon thin film based on laser interference technology. DETAILED DESCRIPTION
[0031] The following is a detailed description of the embodiments of the present application. This embodiment is implemented based on the technical solution of the present application, and provides a detailed implementation method and specific operation process. The scope of protection of the present application is limited to the following examples.
[0032] Example 1:
[0033] A method for preparing a single crystal silicon thin film based on laser interferometry technology, the specific steps are as follows:
[0034] The first step is the preparation of silicon film: a pure silicon target with a purity of 99.999% is selected. The size of the pure silicon target is 48mm in diameter and 3mm in thickness. The magnetron sputtering power source uses an RF magnetron sputtering source. This is mainly because the Si target is a polycrystalline semiconductor with low conductivity. If a DC sputtering power source is used, its efficiency will be extremely low. The size of the SiO2 substrate used is 10mm×10mm×1mm. When preparing the Si thin film sample, the SiO2 substrate temperature is room temperature and the target-substrate distance is set to 68mm. The SiO2 substrate and target are placed in a vacuum chamber with an initial pressure of about 2.5*10 -4 Pa; the Ar flow rate is maintained at 20 sccm; the sputtering gas used is Ar with a purity of 99.99%. During the sputtering process, the working pressure in the vacuum chamber is maintained at 0.6 Pa, the sputtering power is 40 W, and the sputtering time is 10 min. The main reason for using 0.6 Pa is that when the working pressure is lower than 0.1 Pa, Ar is difficult to ionize and sputtering cannot be maintained; but when the working pressure is higher than 3.0 Pa, the quality of the deposited film is low, so the sputtering pressure is selected to be 0.6 Pa as the working pressure;
[0035] Step 2: Laser irradiation for 0 min, magnetron sputtering time for 10 min, no laser irradiation during the sputtering process until the sputtering time ends.
[0036] Example 2:
[0037] A method for preparing a single crystal silicon thin film based on laser interferometry technology, the specific steps are as follows:
[0038] The first step is the preparation of silicon film: a pure silicon target with a purity of 99.999% is selected. The size of the pure silicon target is 48mm in diameter and 3mm in thickness. The magnetron sputtering power source uses an RF magnetron sputtering source. This is mainly because the Si target is a polycrystalline semiconductor with low conductivity. If a DC sputtering power source is used, its efficiency will be extremely low. The size of the SiO2 substrate used is 10mm×10mm×1mm. When preparing the Si thin film sample, the SiO2 substrate temperature is room temperature and the target-substrate distance is set to 68mm. The SiO2 substrate and target are placed in a vacuum chamber with an initial pressure of about 2.5*10 -4 Pa; the Ar flow rate is maintained at 20 sccm; the sputtering gas used is Ar with a purity of 99.99%. During the sputtering process, the working pressure in the vacuum chamber is maintained at 0.6 Pa, the sputtering power is 40 W, and the sputtering time is 10 min. The main reason for using 0.6 Pa is that when the working pressure is lower than 0.1 Pa, Ar is difficult to ionize and sputtering cannot be maintained; but when the working pressure is higher than 3.0 Pa, the quality of the deposited film is low, so the sputtering pressure is selected to be 0.6 Pa as the working pressure;
[0039] Step 2: As shown in Figure 1, at the beginning of sputtering, a steady-state laser source Laser is used to use the interference method to split the steady-state laser through the beam splitter BS1, and then reflected to the center of the substrate surface through plane mirrors M1, M2, M3, and M4 at an incident angle of 60° and an azimuth angle of 90°. The light intensity is evenly distributed on the substrate surface to produce a uniform thermal gradient distribution, heat the substrate, and induce the target Si nanoparticles to form a dense and flat single-crystal silicon film on the substrate surface. The laser irradiation is 5 minutes, and the magnetron sputtering time is 10 minutes. The sputtering process maintains the laser irradiation for the first 5 minutes. The film produces single-crystal silicon and the surface roughness is reduced.
[0040] Example 3:
[0041] A method for preparing a single crystal silicon thin film based on laser interferometry technology, the specific steps are as follows:
[0042] The first step is the preparation of silicon film: a pure silicon target with a purity of 99.999% is selected. The size of the pure silicon target is 48mm in diameter and 3mm in thickness. The magnetron sputtering power source uses an RF magnetron sputtering source. This is mainly because the Si target is a polycrystalline semiconductor with low conductivity. If a DC sputtering power source is used, its efficiency will be extremely low. The size of the SiO2 substrate used is 10mm×10mm×1mm. When preparing the Si thin film sample, the SiO2 substrate temperature is room temperature and the target-substrate distance is set to 68mm. The SiO2 substrate and target are placed in a vacuum chamber with an initial pressure of about 2.5*10 -4Pa; the Ar flow rate is maintained at 20 sccm; the sputtering gas used is Ar with a purity of 99.99%. During the sputtering process, the working pressure in the vacuum chamber is maintained at 0.6 Pa, the sputtering power is 40 W, and the sputtering time is 10 min. The main reason for using 0.6 Pa is that when the working pressure is lower than 0.1 Pa, Ar is difficult to ionize and sputtering cannot be maintained; but when the working pressure is higher than 3.0 Pa, the quality of the deposited film is low, so the sputtering pressure is selected to be 0.6 Pa as the working pressure;
[0043] Step 2: During the sputtering process, a steady-state laser source Laser is used to use the interference method to split the steady-state laser through the beam splitter BS1, and then reflected to the center of the substrate surface through plane mirrors M1, M2, M3, and M4 at an incident angle of 60° and an azimuth angle of 90°. The light intensity is evenly distributed on the substrate surface to produce a uniform thermal gradient distribution, heat the substrate, and induce the target Si nanoparticles to form a dense and flat single-crystal silicon film on the substrate surface. The laser irradiation is 5 minutes, and the magnetron sputtering time is 10 minutes. The laser irradiation is maintained for the last 5 minutes of the sputtering process until the sputtering time ends. The film produces a single-crystal silicon film with a high crystallization rate.
[0044] Example 4:
[0045] A method for preparing a single crystal silicon thin film based on laser interferometry technology, the specific steps are as follows:
[0046] The first step is the preparation of silicon film: a pure silicon target with a purity of 99.999% is selected. The size of the pure silicon target is 48mm in diameter and 3mm in thickness. The magnetron sputtering power source uses an RF magnetron sputtering source. This is mainly because the Si target is a polycrystalline semiconductor with low conductivity. If a DC sputtering power source is used, its efficiency will be extremely low. The size of the SiO2 substrate used is 10mm×10mm×1mm. When preparing the Si thin film sample, the SiO2 substrate temperature is room temperature and the target-substrate distance is set to 68mm. The SiO2 substrate and target are placed in a vacuum chamber with an initial pressure of about 2.5*10 -4 Pa; the Ar flow rate is maintained at 20 sccm; the sputtering gas used is Ar with a purity of 99.99%. During the sputtering process, the working pressure in the vacuum chamber is maintained at 0.6 Pa, the sputtering power is 40 W, and the sputtering time is 10 min. The main reason for using 0.6 Pa is that when the working pressure is lower than 0.1 Pa, Ar is difficult to ionize and sputtering cannot be maintained; but when the working pressure is higher than 3.0 Pa, the quality of the deposited film is low, so the sputtering pressure is selected to be 0.6 Pa as the working pressure;
[0047] Step 2: At the beginning of sputtering, a steady-state laser source Laser is used to split the steady-state laser beam through the beam splitter BS1 by interference method, and reflected to the center of the substrate surface by plane mirrors M1, M2, M3, and M4 at an incident angle of 60° and an azimuth angle of 90°. The light intensity is evenly distributed on the substrate surface to produce a uniform thermal gradient distribution, heat the substrate, and induce the target material Si nanoparticles to form a dense and flat single crystal silicon film on the substrate surface. The laser irradiation lasts for 10 minutes, and the magnetron sputtering time is 10 minutes. The laser irradiation is maintained during the sputtering process until the sputtering time ends, and a film with good growth quality is obtained. It is measured by the instrument, as shown in Figure 2, and a characteristic peak of 522 cm is generated. -1 The single-crystal silicon film has a high peak and a narrow half-width at half-maximum, indicating good crystallinity and a high silicon content. The XRD pattern in Figure 3 shows a diffraction peak at 69.8°, corresponding to the Si(400) crystal plane, with a narrow half-width at half-maximum, indicating a high crystallinity rate. The SEM image in Figure 4 reveals a smooth surface with minimal roughness. As shown in Figure 5, the silicon film has a transmittance of 89.502% in the 200-860nm wavelength range and 97.655% in the 860-1200nm wavelength range, for a total average transmittance of 92.26%.
[0048] The above is only a preferred embodiment of the present application. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principles of the present application. These improvements and modifications should also be regarded as the scope of protection of the present application.
Claims
1. A method for preparing single crystal silicon thin film based on laser interference technology, It is characterized in that The specific steps are as follows: The first step is the preparation of silicon film: a pure silicon target with a purity of 99.999% is selected, a radio frequency magnetron sputtering source is used as the magnetron sputtering power source, and a SiO substrate is used. 2 Substrate, pure silicon target and SiO 2 The substrate is placed in a vacuum chamber and SiO 2 The initial temperature of the substrate was room temperature, the target-substrate distance was set to 68 mm, the sputtering gas used was 99.99% pure Ar, the working pressure during sputtering was 0.6 Pa, the sputtering power was 40-200 W, and the sputtering time was 10 min; Step 2: At the beginning of sputtering, a steady-state laser source is used to distribute the light intensity evenly on the SiO 2 A uniform thermal gradient is generated on the substrate surface, heating the SiO 2 substrate, inducing the target Si nanoparticles to form SiO 2 A dense, flat, high-transmittance single-crystal silicon film is deposited on the substrate surface, and the film thickness is 800 to 990 nm.
2. A method for preparing a single crystal silicon thin film based on laser interference technology according to claim 1, Features: The size of the pure silicon target in the first step is 48 mm in diameter and 3 mm in thickness.
3. The method for preparing a single crystal silicon thin film based on laser interference technology according to claim 1, Features: In the first step, SiO 2 The substrate size is 10 mm × 10 mm × 1 mm.
4. The method for preparing a single crystal silicon thin film based on laser interference technology according to claim 1, Features: In the first step, the magnetron sputtering power source is a radio frequency alternating current power source with a frequency of 10 to 35 MHz.
5. The method for preparing a single crystal silicon thin film based on laser interference technology according to claim 1, Features: In the first step, the initial pressure in the vacuum chamber is 2.5*10 -4 Pa, the pressure during sputtering was maintained at 0.6Pa.
6. The method for preparing a single crystal silicon thin film based on laser interference technology according to claim 1, It is characterized in that When a steady-state laser source is used for irradiation in the second step, the wavelength of the laser source selected is 475 nm, the power is 50 mW, and the irradiation time is 0 to 10 min.
7. The method for preparing a single crystal silicon thin film based on laser interference technology according to claim 1, Features: In the second step, when the steady-state laser source Laser is irradiated, the multi-lens interference principle is utilized and a BS1 beam splitter is used to disperse the circular laser spot into an interference pattern of multiple coherent light beams. The multiple coherent light beams are converged on the substrate at an incident angle of 60° and an azimuth angle of 90° through the M1, M2, M3, and M4 plane mirrors, thereby generating a uniform thermal gradient so that the light intensity is evenly distributed on the substrate, inducing uniform growth of the silicon film.
Citation Information
Patent Citations
Method for preparing monocrystalline silicon thin film and components thereof
CN101225543A
Method for preparing single crystal silicon film components
CN101582470A
Method for preparing amorphous silicon carbide film and epitaxial film at low temperature
CN102051589A
A method for depositing microcrystalline silicon thin films
CN102296363A
Preparation method of polysilicon thin film material
CN104392908A