Low-temperature sintered high-dielectric gyromagnetic ferrite material and preparation method therefor

WO2024230141A1PCT designated stage expired Publication Date: 2024-11-14HUAYANG TECH DEV
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
PCT/CN2023/136169
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-05-11
Filing Date
2023-12-04
Publication Date
2024-11-14

Smart Images

  • Figure CN2023136169_14112024_PF_FP_ABST
    Figure CN2023136169_14112024_PF_FP_ABST
Patent Text Reader

Abstract

The present invention relates to the technical field of electronic materials, in particular to a low-temperature sintered high-dielectric gyromagnetic ferrite material and a preparation method therefor. The molecular formula of said material is Bi1.45Ti0.1Y1.55-2x-yCa2x+yVxZry-0.1Fe5-y-xO12, wherein x is 0.6-0.65, y is 0.25-0.35, and 1.55-2x-y≥0. The provided preparation method not only can realize low-temperature sintering at 900℃, but also can realize good co-firing compatibility with silver electrodes of LTCC processes.
Need to check novelty before this filing date? Find Prior Art

Description

A low-temperature sintered high-medium-spin magnetic ferrite material and its preparation method Technical Field

[0001] The present invention relates to the technical field of electronic materials, and in particular to a low-temperature sintered high-meta-rotation magnetic ferrite material and a preparation method thereof. Background Art

[0002] Microwave gyromagnetic ferrite devices, such as circulators and isolators, play a crucial role in modern wireless communication systems. In recent years, with the rapid development of defense and civilian wireless communication technologies, the trend toward miniaturization, broadband, and multifunctionality has become increasingly evident in various communication electronics products. Consequently, the microwave gyromagnetic devices widely used in these devices must also continue to evolve towards miniaturization and integration. Because the wavelength of electromagnetic waves propagating through a medium is inversely proportional to the square root of the dielectric constant, increasing the dielectric constant of gyromagnetic ferrite materials has become a key approach to miniaturizing microwave ferrite devices.

[0003] LTCC (low-temperature co-fired ceramic) technology enables three-dimensional structural design and packaging of passive electronic components, facilitating not only the miniaturization and integration of electronic components but also providing new avenues for innovative structural design. While LTCC technology is widely used in many passive electronic components, it has been largely unused in gyromagnetic devices. This is primarily due to the high sintering temperatures of conventional gyromagnetic YIG ferrite materials. LTCC technology uses silver as a co-fired electrode material. To achieve compatibility with the LTCC process, the gyromagnetic material must be sintered to a density of 900°C or below. Currently available low-linewidth gyromagnetic YIG ferrite materials typically have a dielectric constant of only 13-15 and require sintering temperatures as high as 1300-1450°C. Therefore, achieving the desired combination of high dielectric constant, low sintering temperature, and low ferromagnetic resonance linewidth is challenging, requiring comprehensive innovations in material formulation and process.

[0004] In the development of high-dielectric gyromagnetic YIG ferrite materials, Transtech Corporation, in its 2016 US invention patent (Application No. US13484018), proposed using appropriate amounts of Bi to replace Y to effectively increase the dielectric constant of gyromagnetic YIG materials. However, the reported ferromagnetic resonance linewidth of the high-dielectric gyromagnetic YIG was still relatively high (over 50 Oe), and low-temperature sintering at or below 900°C was not achieved. Shenzhen Sunlord Electronics Co., Ltd.'s 2018 Chinese invention patent (Publication No. CN111285673A) employed a plasma co-replacement method with Bi, Ca, Zr, Al, and Mn to increase the dielectric constant of the material. However, the ferromagnetic resonance linewidth of the material was also relatively high (over 45 Oe), and low-temperature sintering was also not achieved. In 2021, Hengdian Group DMEGC Co., Ltd. also applied for a Chinese invention patent (publication number CN113896521 A). It adopted a method of co-substitution of 10 elements including Bi, Gd, Ca, Nb, and V to achieve a low-linewidth, high-dielectric gyromagnetic ferrite material with a ferromagnetic resonance linewidth of about 20 Oe and a dielectric constant of 25-28. However, this material only has a good balance between high dielectric constant and low linewidth, but the material system has not achieved low-temperature sintering. Combining all the relevant research reports at present, it can be found that there have been some research reports at home and abroad on improving the dielectric constant of gyromagnetic YIG materials, but there are no further research reports on how to achieve low-temperature sintering of high-dielectric gyromagnetic materials so that they can be combined with LTCC technology. Technical issues

[0005] In order to overcome the above-mentioned defects of the prior art, the technical problem to be solved by the present invention is to provide a gyromagnetic ferrite material having the characteristics of low-temperature sintering, high dielectric constant and low ferromagnetic resonance linewidth and a preparation method thereof. Technical Solutions

[0006] In order to solve the above technical problems, the technical solution adopted by the present invention is: a low temperature sintered high-medium rotation magnetic ferrite material with a molecular formula of Bi 1.45 Ti 0.1 Y 1.55-2x-y Ca 2x+y V x Zr y-0.1 Fe 5-y-x O 12 , where x is 0.6~0.65, y is 0.25~0.35, and 1.55-2x-y≥0.

[0007] Another technical solution adopted by the present invention is: a method for preparing the above-mentioned low-temperature sintered high-medium-rotation magnetic ferrite material, comprising the following steps:

[0008] S1: Using Bi2O3, Y2O3, TiO2, CaCO3, V2O5, ZrO2 and Fe2O3 as the initial raw materials, batching, mixing, ball milling, drying and pre-calcining are carried out in sequence according to the molecular formula of the gyromagnetic ferrite material to obtain a pre-calcined material;

[0009] S2: After the pre-sintered material is coarsely crushed, BBSZ (Bi2O3-H3BO3-SiO2-ZnO) glass and MoO3 are added, ball milled again, and then dried to obtain a second dried material;

[0010] S3: The dried material is granulated, pressed and sintered in sequence to obtain a gyromagnetic ferrite material. Beneficial effects

[0011] The present invention provides a high-K, low-temperature sintered gyromagnetic material with a 4πMs of approximately 780-830 Gs, a dielectric constant of approximately 26.5-27.5, and a ferromagnetic resonance linewidth ≤ 25 Oe. This material achieves a good balance of suitable saturation magnetization, high dielectric constant, low ferromagnetic resonance linewidth, and low-temperature sintering at 900°C. It is expected to promote the integrated development of LTCC technology and gyromagnetic devices, and find widespread application in new, small, integrated LTCC gyromagnetic devices. BRIEF DESCRIPTION OF THE DRAWINGS

[0012] FIG1 is a process flow chart showing a method for preparing a low-temperature sintered high-mesorotation magnetic ferrite material according to a specific embodiment of the present invention. Modes for Carrying Out the Invention

[0013] To illustrate the technical content, achieved objectives and effects of the present invention in detail, the following description is given in conjunction with the embodiments and accompanying drawings.

[0014] The key concept of the present invention is that the high-magnetic ferrite material has the molecular formula Bi 1.45 Ti 0.1 Y 1.55-2x-y Ca 2x+y V x Zr y-0.1 Fe 5-y-x O 12 It can not only achieve low-temperature sintering at 900°C, but also achieve good co-firing compatibility with the silver electrodes of the LTCC process.

[0015] The present invention is a low temperature sintered high mesorotation magnetic ferrite material, the molecular formula of which is Bi 1.45 Ti 0.1 Y 1.55-2x-y Ca 2x+y V x Zr y-0.1 Fe 5-y-x O 12, where x is 0.6~0.65, y is 0.25~0.35, and 1.55-2x-y≥0.

[0016] From the above description, it can be seen that the beneficial effects of the present invention are: the low-temperature sintered high-mesh ferrite material of the present invention can ultimately achieve a performance of 4πMs of about 780~830 Gs, a dielectric constant of about 26.5~27.5, and a ferromagnetic resonance linewidth of ≤25 Oe. It can not only achieve low-temperature sintering at 900°C, but also achieve good co-firing compatibility with the silver electrodes of the LTCC process.

[0017] The formula of the present invention first uses co-substitution of Ca and V ions to obtain the required 4πMs, then improves the dielectric constant by appropriate substitution of Bi ions, and finally further improves the dielectric constant by co-substitution of Ca and Ti ions. It has the following advantages:

[0018] (1) The substitution amount of Bi ions in the gyromagnetic ferrite is controlled at 1.45, which can maximize the comprehensive requirements of the material's high dielectric constant and low ferromagnetic resonance linewidth. At the same time, the sintering temperature of the material system is not too high, which is conducive to further reducing the sintering temperature to 900°C.

[0019] (2) The use of 0.1 mol of Ti ions for substitution is strictly controlled, which not only helps to improve the dielectric constant of the material system, but also can control the ferromagnetic resonance linewidth of the material from being too high. The combination of Ti ions and Ca ions can achieve valence balance.

[0020] (3) The co-replacement of Ca, V and Zr ions was adopted. On the one hand, the 4πMs of the material system can be controlled to about 780~830 Gs by appropriate substitution amount, thus meeting the needs of low-field gyromagnetic device design; on the other hand, the sintering temperature of the material system can be further reduced by large-dose V ion substitution, which is more conducive to the low-temperature sintering of the material system. The appropriate substitution of Bi and V ions not only improves the dielectric constant and adjusts the 4πMs value, but also reduces the sintering temperature of the material system as much as possible; in addition, the appropriate amount of Ca and Zr ion substitution is also beneficial to reducing the ferromagnetic resonance linewidth of the material system.

[0021] As shown in FIG1 , another technical solution adopted by the present invention is: a method for preparing the above-mentioned low-temperature sintered high-medium-rotation magnetic ferrite material, comprising the following steps:

[0022] S1: Using Bi2O3, Y2O3, TiO2, CaCO3, V2O5, ZrO2 and Fe2O3 as the initial raw materials, batching, mixing, ball milling, drying and pre-calcining are carried out in sequence according to the molecular formula of the gyromagnetic ferrite material to obtain a pre-calcined material;

[0023] S2: After the pre-sintered material is coarsely crushed, BBSZ glass and MoO3 are added, ball milled again, and then dried to obtain a second dried material;

[0024] S3: The dried material is granulated, pressed and sintered in sequence to obtain a gyromagnetic ferrite material.

[0025] As can be seen from the above description, the preparation method of the present invention first mixes the raw materials according to their composition, then conducts a primary ball milling and drying process before pre-calcining. During a secondary ball milling process, the pre-calcined materials are doped with BBSZ glass and MoO3. After a secondary ball milling and drying process, a PVA solution is added to form granules. Finally, sintering achieves full densification, resulting in a gyromagnetic ferrite material that combines low-temperature sintering, a high dielectric constant, and a low ferromagnetic resonance linewidth. Co-firing with Ag powder has been verified to produce no new phases. Not only can this material achieve low-temperature sintering at 900°C, but it also exhibits excellent co-firing compatibility with silver electrodes used in the LTCC process, making it suitable for the development and application of LTCC gyromagnetic devices.

[0026] By doping an appropriate amount of BBSZ glass and MoO3 during the secondary ball milling, on the one hand, the sintering temperature of the material system can be reduced to 900°C through further liquid phase flux sintering to achieve low-temperature sintering compatible with the LTCC process and improve the density. Secondly, the material performance can be improved by optimizing the micromorphology of the ferrite material, which is conducive to reducing the ferromagnetic resonance linewidth and improving the dielectric constant.

[0027] Furthermore, the pre-calcination is specifically as follows: the dried material obtained after drying is sieved, compacted and punched, heated to 750-850° C. and kept warm for 6-8 hours for pre-calcination, and cooled to obtain the pre-calcined material.

[0028] From the above description, it can be seen that during pre-firing, the diffusion of ions and vacancies completes the solid phase reaction and grain growth, thereby improving the material properties.

[0029] Furthermore, the addition amount of BBSZ glass is 0.2-0.3 wt % of the weight of the pre-sintered material.

[0030] Furthermore, the weight ratio of BBSZ glass to MoO3 is 2~3:1.

[0031] As can be seen from the above description, insufficient doping of BBSZ glass prevents the material from achieving sufficient densification during sintering at 900°C. Excessive doping of BBSZ glass leads to a decrease in magnetic properties, typically manifested by an increase in the ferromagnetic resonance linewidth. MoO3 doping helps improve the ferrite micromorphology, promoting more uniform grain growth and increasing the average grain size. Too little MoO3 doping fails to improve the micromorphology, while too much can easily lead to uneven grain growth, which in turn deteriorates the material's magnetic properties.

[0032] From the above description, it can be seen that the present invention uses a combined doping mode of BBSZ glass + MoO3, which can more effectively reduce the sintering temperature of the material system to 900°C, while the effect on the magnetic properties of the material is almost negligible.

[0033] Furthermore, the powder is ball-milled again until the average particle size is below 1 μm.

[0034] From the above description, it can be seen that the smaller the particles, the larger the specific surface area and the greater the activity, which is beneficial to lowering the sintering temperature and reducing the reaction time.

[0035] Furthermore, the preparation method of BBSZ glass is as follows: weigh Bi2O3, H3BO3, SiO2 and ZnO raw materials, add deionized water to ball mill and mix evenly, and then dry, then heat to 950~1050℃ and keep warm for 1h, then pour into deionized water for rapid quenching, and ball mill the glass slag obtained after rapid quenching to a particle size of 2~3um and then dry to obtain BBSZ glass.

[0036] Furthermore, a PVA (polyvinyl alcohol) solution accounting for 8% to 12% of the weight of the re-dried material is added during granulation.

[0037] Furthermore, the specific steps during sintering are: heating to 150-200°C at 2-3°C / min, keeping warm for 1-2 hours, and then draining the water; heating to 500-600°C at 2-3°C / min, keeping warm for 2-4 hours, and then debinding; finally heating to 900°C at 2-3°C / min, keeping warm for 4-6 hours, and completing sintering after cooling.

[0038] From the above description, it can be seen that sintering allows the particles inside the material to interact with each other, eliminate pores, increase density, and complete solid-phase reaction.

[0039] As shown in FIG1 , the first embodiment of the present invention is a method for preparing a low-temperature sintered high-medium-rotation magnetic ferrite material, comprising the following steps:

[0040] S1: Using Bi2O3, Y2O3, TiO2, CaCO3, V2O5, ZrO2 and Fe2O3 with purity of more than 99.5% as the initial raw materials, according to the molecular formula of the gyromagnetic ferrite material Bi 1.45 T i0.1 Y 1.55-2x-y Ca 2x+y V x Zr y-0.1 Fe 5-y-x O 12 The ingredients are precisely mixed, where x is 0.6~0.65, y is 0.25~0.35, and 1.55-2x-y≥0, and then mixed and ball-milled in a planetary ball mill for 6 hours and then dried.

[0041] S2. The dried material obtained after drying is passed through a 60-mesh sieve, compacted and punched, heated to 800° C. at a heating rate of 3° C. / min and kept warm for 6 h for pre-calcination, and then cooled to room temperature with the furnace to obtain a pre-calcined material.

[0042] S3: After the pre-sintered material is coarsely crushed, 0.25wt% of BBSZ glass and 0.1wt% of MoO3 are added to the pre-sintered material for trace doping; then, the pre-sintered material is ball-milled again in a planetary ball mill for 6 hours until the average particle size of the powder is less than 1μm, and then dried to obtain a second dried material;

[0043] The preparation method of BBSZ glass is as follows: Bi2O3, H3BO3, SiO2 and ZnO raw materials are weighed according to the molar fraction of 27%Bi2O3-35%H3BO3-6%SiO2-32%ZnO, deionized water is added to ball mill and mixed evenly, and then dried, and then the temperature is raised to 1000℃ and kept warm for 1 hour, and then poured into deionized water for rapid quenching, and the glass slag obtained after rapid quenching is ball milled to a particle size of 2.5um and then dried to obtain BBSZ glass.

[0044] S4: adding 10% of the weight of the PVA solution to the dried material again and pressing and molding to obtain a green embryo.

[0045] S5: The green sample is heated to 200°C at a rate of 2°C / min and kept at that temperature for 2 hours, then the water is drained, then the temperature is heated to 600°C at a rate of 2°C / min and kept at that temperature for 3 hours, then the binder is debonded, and finally the temperature is heated to 900°C at a rate of 2.5°C / min and kept at that temperature for 5 hours. The sample is then cooled to room temperature in the furnace and sintered to obtain a gyromagnetic ferrite material.

[0046] Table 1 shows the test results obtained when x and y in the formula molecular formula take different values.

[0047] Table 1

[0048]

[0049] As shown in Table 1, the low-temperature sintered high-magnetic-rotation ferrite material of the present invention can ultimately achieve a 4πMs performance of approximately 780-830 Gs, a dielectric constant of approximately 26.5-27.5, and a ferromagnetic resonance linewidth of ≤25 Oe. It can not only achieve low-temperature sintering at 900°C, but also achieve good co-firing compatibility with the silver electrodes of the LTCC process.

[0050] A second embodiment of the present invention is a method for preparing a low-temperature sintered high-medium-rotation magnetic ferrite material, comprising the following steps:

[0051] S1: Using Bi2O3, Y2O3, TiO2, CaCO3, V2O5, ZrO2 and Fe2O3 with purity of more than 99.5% as the initial raw materials, according to the molecular formula of the gyromagnetic ferrite material Bi 1.45 Ti0.1 Y 1.55-2x-y Ca 2x+y V x Zr y-0.1 Fe 5-y-x O 12 The ingredients were precisely proportioned, where x=0.6, y=0.25, and then mixed and ball-milled in a planetary ball mill for 6 hours before drying.

[0052] S2. The dried material obtained after drying is passed through a 60-mesh sieve, compacted and punched, heated to 750° C. at a heating rate of 3° C. / min and kept at this temperature for 8 h for pre-calcination, and then cooled to room temperature in the furnace to obtain a pre-calcined material.

[0053] S3: After the pre-sintered material is coarsely crushed, 0.2wt% of BBSZ glass and 0.1wt% of MoO3 are added to the pre-sintered material for trace doping; then, the pre-sintered material is ball-milled again in a planetary ball mill for 6h until the average particle size of the powder is less than 1μm, and then dried to obtain a second dried material;

[0054] The preparation method of BBSZ glass is as follows: Bi2O3, H3BO3, SiO2 and ZnO raw materials are weighed according to the molar fraction of 27%Bi2O3-35%H3BO3-6%SiO2-32%ZnO, deionized water is added to ball mill and mixed evenly, and then dried, and then the temperature is raised to 950℃ and kept warm for 1 hour, and then poured into deionized water for rapid quenching, and the glass slag obtained after rapid quenching is ball milled to a particle size of 2um and then dried to obtain BBSZ glass.

[0055] S4: adding 8% PVA solution by weight to the dried material again and pressing and molding to obtain a green embryo.

[0056] S5: The green sample was heated to 150°C at a rate of 2.5°C / min and kept at that temperature for 1.8 hours, then drained. The green sample was heated to 500°C at a rate of 2.5°C / min and kept at that temperature for 4 hours, then debinded. Finally, the green sample was heated to 900°C at a rate of 2°C / min and kept at that temperature for 4 hours. The green sample was cooled to room temperature in the furnace and sintered to obtain a gyromagnetic ferrite material.

[0057] The third embodiment of the present invention is a method for preparing a low-temperature sintered high-medium-rotation magnetic ferrite material, comprising the following steps:

[0058] S1: Using Bi2O3, Y2O3, TiO2, CaCO3, V2O5, ZrO2 and Fe2O3 with purity of more than 99.5% as the initial raw materials, according to the molecular formula of the gyromagnetic ferrite material Bi 1.45 Ti 0.1 Y 1.55-2x-y Ca 2x+y V x Zr y-0.1 Fe 5-y-x O12 The ingredients were precisely proportioned, where x=0.6 and y=0.25, and then mixed and ball-milled in a planetary ball mill for 6 hours before drying.

[0059] S2. The dried material obtained after drying is passed through a 60-mesh sieve, compacted and punched, heated to 850° C. at a heating rate of 3° C. / min and kept warm for 7 h for pre-calcination, and then cooled to room temperature in the furnace to obtain a pre-calcined material.

[0060] S3: After the pre-sintered material is coarsely crushed, 0.3wt% of BBSZ glass and 0.1wt% of MoO3 are added to the pre-sintered material for trace doping; then, the pre-sintered material is ball-milled again in a planetary ball mill for 6h until the average particle size of the powder is less than 1μm, and then dried to obtain a second dried material;

[0061] The preparation method of BBSZ glass is as follows: Bi2O3, H3BO3, SiO2 and ZnO raw materials are weighed according to the molar fraction of 27%Bi2O3-35%H3BO3-6%SiO2-32%ZnO, deionized water is added to ball mill and mixed evenly, and then dried, and then the temperature is raised to 1050℃ and kept warm for 1h, and then poured into deionized water for rapid quenching, and the glass slag obtained after rapid quenching is ball milled to a particle size of 3um and then dried to obtain BBSZ glass.

[0062] S4: adding 12% of the weight of the PVA solution to the dried material again and pressing and molding to obtain a green embryo.

[0063] S5: The green sample is heated to 170°C at a rate of 3°C / min and kept at this temperature for 1 hour, then the water is drained, then the temperature is heated to 550°C at a rate of 3°C / min and kept at this temperature for 2 hours, then the binder is debonded, and finally the temperature is heated to 900°C at a rate of 3°C / min and kept at this temperature for 6 hours. The sample is then cooled to room temperature in the furnace and sintered to obtain a spin-magnetic ferrite material.

[0064] In summary, the preparation method of the present invention provided by the present invention first pre-fires each raw material after being mixed into components and dried by ball milling once, and doped with pre-fired material BBSZ glass and MoO3 during the secondary ball milling. After the secondary ball milling and drying, PVA solution is added to form granules, and finally sintered to achieve full densification to obtain a gyromagnetic ferrite material with low temperature sintering, high dielectric constant and low ferromagnetic resonance linewidth characteristics. The material adopts the substitution of suitable Bi and V ions to improve the dielectric constant, adjust the 4πMs value, and reduce the sintering temperature of the material system as much as possible. Then, during the secondary ball milling, an appropriate amount of BBSZ glass and MoO3 is doped, and the sintering temperature of the material system is further liquid phase flux sintering to reduce it to 900°C to achieve low temperature sintering compatible with the LTCC process and improve density. The material is verified by co-firing with Ag powder, and no new phase is produced. It can not only achieve 900°C low temperature sintering, but also achieve good co-firing compatibility with the silver electrode of the LTCC process, and can be used for the research and development application of LTCC gyromagnetic devices.

[0065] The above descriptions are merely embodiments of the present invention and are not intended to limit the patent scope of the present invention. Any equivalent transformations made using the contents of the present invention's description and drawings, or directly or indirectly applied in related technical fields, are also included in the patent protection scope of the present invention.

Claims

1. A low temperature sintered high-medium rotation magnetic ferrite material, characterized in that: The molecular formula is Bi 1.45 Ti 0.1 Y 1.55-2x-y Ca 2x+y V x Zr y-0.1 Fe 5-y-x O 12 , where x is 0.6~0.65, y is 0.25~0.35, and 1.55-2x-y≥0.

2. A method for preparing a low temperature sintered high-medium rotation magnetic ferrite material according to claim 1, characterized in that: The following steps are involved: S1: Using Bi2O3, Y2O3, TiO2, CaCO3, V2O5, ZrO2 and Fe2O3 as initial raw materials, batching, mixing, ball milling, drying and pre-calcining are carried out in sequence according to the molecular formula of the gyromagnetic ferrite material to obtain a pre-calcined material; S2: After the pre-sintered material is coarsely crushed, BBSZ glass and MoO3 are added, ball-milled again, and then dried to obtain a second dried material; S3: The dried material is granulated, pressed and sintered in sequence to obtain a gyromagnetic ferrite material.

3. The method for preparing a low temperature sintered high-medium rotation magnetic ferrite material according to claim 2, characterized in that: The pre-burning is specifically as follows: the dried material obtained after drying is sieved, compacted and punched, heated to 750-850° C. and kept warm for 6-8 hours for pre-burning, and the pre-burned material is obtained after cooling.

4. The method for preparing a low temperature sintered high-medium rotation magnetic ferrite material according to claim 2, characterized in that: The added amount of the BBSZ glass is 0.2-0.3wt% of the weight of the pre-sintered material.

5. The method for preparing a low temperature sintered high-medium rotation magnetic ferrite material according to claim 2, characterized in that: The weight ratio of the BBSZ glass to MoO3 is 2-3:

1.

6. The method for preparing a low temperature sintered high-medium rotation magnetic ferrite material according to claim 2, characterized in that: The ball milling is repeated until the average particle size of the powder is below 1 μm.

7. The method for preparing a low temperature sintered high-medium rotation magnetic ferrite material according to claim 2, characterized in that: The preparation method of the BBSZ glass is as follows: weigh Bi2O3, H3BO3, SiO2 and ZnO raw materials, add deionized water to ball mill and mix them evenly, then dry them, then heat them to 950-1050°C and keep them warm for 1 hour, then pour them into deionized water for rapid quenching, ball mill the glass slag obtained after rapid quenching to a particle size of 2-3um, and then dry them to obtain BBSZ glass.

8. The method for preparing a low temperature sintered high-medium rotation magnetic ferrite material according to claim 2, characterized in that: During the granulation, a PVA solution accounting for 8% to 12% of the weight of the re-dried material is added.

9. The method for preparing a low temperature sintered high-medium rotation magnetic ferrite material according to claim 2, characterized in that: The specific steps of sintering are: heating to 150-200°C at 2-3°C / min, keeping warm for 1-2 hours, then draining the water; heating to 500-600°C at 2-3°C / min, keeping warm for 2-4 hours, then debinding; finally heating to 900°C at 2-3°C / min, keeping warm for 4-6 hours, and completing sintering after cooling.

Citation Information

Patent Citations

  • Compound low-temperature pre-sintering method of ferrite monoliths structure materials

    CN101700981A

  • Tunable resonator using high dielectric constant ferrite rods

    CN104795619A

  • Garnet ferrite material with high dielectric constant and preparation method thereof

    CN112456998A

  • Low-temperature sintered high-dielectric gyromagnetic ferrite material and preparation method thereof

    CN116496080A

  • High saturation magnetization and high dielectric constant ferrites containing indium

    US20230102155A1