Block copolymer and block copolymer modified silicon dioxide nanoparticles and preparation method therefor and use thereof

Through the addition reaction of block copolymer and amino surface modified silica nanoparticles, block copolymer modified silica nanoparticles with amphiphilicity and stability are formed, solving the difficulty of nanosilicon dioxide in regulating hydrophilicity and philia. The problem of oil performance has achieved the effect of reducing oil-water interface tension and improving crude oil recovery.

WO2024230156A1PCT designated stage expired Publication Date: 2024-11-14DAQING OILFIELD CO LTD +1

Patent Information

Application Number
PCT/CN2023/138065
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-05-10
Filing Date
2023-12-12
Publication Date
2024-11-14

AI Technical Summary

Technical Problem

Existing nanosilicon dioxide is difficult to accurately regulate hydrophilic and lipophilic properties, and its structure is unstable, resulting in an insignificant reduction in oil-water interface tension, affecting the recovery rate of low-permeability reservoirs.

Method used

Through the addition reaction of block copolymer and amino surface modified silica nanoparticles, block copolymer modified silica nanoparticles with -NHCONH-linking groups are formed, which has amphipathicity, stability and solvent responsiveness. , can reduce the tension of the oil-water interface, realize automatic oil search, capture and expand the volume of oil droplets.

Benefits of technology

It significantly improves the crude oil recovery rate and has a stable structure. It can automatically find oil, capture and expand the volume of oil droplets in the reservoir, and improves oil displacement efficiency.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN2023138065_14112024_PF_FP_ABST
    Figure CN2023138065_14112024_PF_FP_ABST
Patent Text Reader

Abstract

The present invention relates to the technical field of enhanced oil recovery for oil fields. Disclosed are a block copolymer and block copolymer modified silicon dioxide nanoparticles and a preparation method therefor and a use thereof. The block copolymer contains a structural unit A shown in formula I, a structural unit B shown in formula II or III, and a structural unit C shown in formula IV. In the present invention, -NCO contained in the structural unit B of the block copolymer and an amino contained in surface-modified silicon dioxide nanoparticles are subjected to an addition reaction so as to be connected by -NHCONH- to obtain the block copolymer modified silicon dioxide nanoparticles, and the block copolymer modified silicon dioxide nanoparticles are finally applied to an oil-displacing agent. The block copolymer modified silicon dioxide nanoparticles have amphipathicity, stability and solvent responsiveness, can reduce oil-water interfacial tension, and enhance oil recovery.
Need to check novelty before this filing date? Find Prior Art

Description

Block copolymer and block copolymer modified silica nanoparticles and preparation method and application thereof

[0001] CROSS-REFERENCE TO RELATED APPLICATIONS

[0002] This application claims the benefit of Chinese patent application No. 202310524776.2, filed on May 10, 2023, entitled “Block copolymers and block copolymer modified silica nanoparticles and their preparation methods and applications,” the contents of which are incorporated herein by reference. Technical Field

[0003] The present invention relates to the technical field of improving crude oil recovery in oil fields, and in particular to block copolymers and block copolymer-modified silicon dioxide nanoparticles, as well as preparation methods and applications thereof. Background Art

[0004] China's oil and gas resources are currently deteriorating significantly, manifesting in two key areas. First, as mature oilfields are developed further, low-grade reserves are rapidly increasing, making extraction increasingly difficult. For example, the Changyuan Oilfield in Daqing Oilfield, for example, has reached a "double-extremely high" development stage in terms of both water cut and recoverable reserves. Reservoirs have low remaining oil saturation and are highly fragmented, presenting a discontinuous phase. Mature and efficient post-reservoir recovery technologies are still lacking. Second, the majority of newly added reserves in China in recent years are in low- and ultra-low-permeability reservoirs. Due to the small pore radius, high pore tortuosity, and low liquid permeability of the rock, conventional development technologies offer poor economic benefits and low efficiency. Effectively improving the recovery of low-permeability reservoirs and achieving cost-effective development of low-permeability fields has become a key focus of oilfield development technology research both domestically and internationally. Consequently, existing tertiary oil recovery technologies are no longer sufficient to meet the current challenges of deteriorating oil and gas resource quality. There is an urgent need to develop new technologies for enhancing oil recovery, relying on technological innovation to address emerging challenges in oilfield development and meet the production and technical needs of oilfields.

[0005] In recent years, theoretical breakthroughs and technological innovations in nanotechnology have provided new avenues for the development of new technologies for enhancing oil recovery. An increasing number of research teams are applying the surface effects of nanomaterials to enhanced oil recovery technologies. Silica nanoparticles have become a preferred nanoscale oil displacement material due to their low cost, environmental friendliness, good compatibility with formations, high surface activity, high hydroxyl content, and ease of surface modification. Most of these methods utilize a "selective surface modification" method, which involves modifying the surface of the same nanoparticle to produce amphiphilic nanosilica particles. Because both hydrophilic and lipophilic modifications are performed on the same silica particle, the two modifications may affect each other, and the hydrophilic and lipophilic properties of the silica particles cannot be regulated independently, which can affect the optimization of the silica particles' amphiphilic properties. CN107416844B chemically couples hydrophilic and lipophilic nanosilica particles to produce bi-spherical amphiphilic nanosilica particles with a particle size of less than 100 nm. While these methods can regulate the hydrophilic and lipophilic properties separately, they are prone to causing stagnation and blockage during the migration of porous reservoir media.

[0006] Summary of the Invention

[0007] The purpose of the present invention is to overcome the problems of the existing technology that nano-silica is difficult to accurately control the hydrophilic and oleophilic properties, has unstable structure and insignificant reduction in oil-water interfacial tension, as well as low recovery rate of low permeability oil reservoirs. The present invention provides block copolymers and block copolymer-modified silica nanoparticles and their preparation methods and applications. The block copolymer-modified silica nanoparticles are obtained by an addition reaction of a block copolymer containing an -NCO structural unit with amino-surface-modified silica nanoparticles. The connecting group is -NHCONH-, and the block copolymer-modified silica nanoparticles have amphiphilicity, stability and solvent responsiveness, can reduce oil-water interfacial tension, and have oil displacement functions such as automatic oil search in the reservoir, capture and aggregate oil droplets, and intelligently expand the swept volume along the process, thereby significantly improving crude oil recovery rate.

[0008] In order to achieve the above object, the first aspect of the present invention provides a block copolymer, wherein the block copolymer comprises a structural unit A represented by formula I, a structural unit B represented by formula II or III, and a structural unit C represented by formula IV.

[0009] Wherein, R1, R3, R5 and R6 are each independently hydrogen or methyl; R2 is C1-C 12 R4 is a straight chain or branched chain alkyl or phenyl group; R7 is a straight chain or branched chain alkylene group of C1-C5; x, y and z are each independently an integer from 1 to 10.

[0010] A second aspect of the present invention provides a method for preparing a block copolymer, wherein the preparation method comprises the following steps:

[0011] (1) in a nitrogen atmosphere and in the presence of a first initiator, a chain transfer agent, and an organic solvent, subjecting the monomer represented by formula (1) and the monomer represented by formula (2) or methacryloyl isocyanate to a first polymerization reaction to obtain a first polymer product;

[0012] (2) conducting a second polymerization reaction on the first polymerization product and the monomer represented by formula (3) under a nitrogen atmosphere and in the presence of a second initiator to obtain the block copolymer;

[0013] Wherein, R1, R3 and R6 are each independently hydrogen or methyl; R2 is C1-C 12 R4 is a straight chain or branched chain alkyl or phenyl group; R7 is a straight chain or branched chain alkylene group of C1-C5; x, y and z are each independently an integer from 1 to 10.

[0014] A third aspect of the present invention provides a block copolymer modified silica nanoparticle, wherein the modified silica nanoparticle comprises: a core derived from a surface-modified silica nanoparticle, a coating layer derived from a block copolymer, and a linking group connecting the core and the coating layer, wherein the block copolymer comprises a structural unit A represented by formula I, a structural unit B represented by formula II or III, and a structural unit C represented by formula IV;

[0015] Wherein, the linking group is -NHCONH-, which is obtained by the addition reaction of -NCO contained in the structural unit B with the amino group contained in the surface-modified silica nanoparticles;

[0016] Wherein, R1, R3, R5 and R6 are each independently hydrogen or methyl; R2 is C1-C 12 R4 is a straight chain or branched chain alkyl or phenyl group; R7 is a straight chain or branched chain alkylene group of C1-C5; x, y and z are each independently an integer from 1 to 10.

[0017] A fourth aspect of the present invention provides a method for preparing block copolymer-modified silica nanoparticles, wherein the preparation method comprises the following steps:

[0018] reacting a block copolymer with silane coupling agent-modified silica nanoparticles to obtain block copolymer-modified silica nanoparticles; wherein the block copolymer is the block copolymer described above or a block copolymer prepared by the above preparation method;

[0019] Wherein, the mass ratio of the block copolymer to the silane coupling agent modified silica nanoparticles is 0.3-10:1.

[0020] The fifth aspect of the present invention provides block copolymer-modified silica nanoparticles prepared by the preparation method of the fourth aspect.

[0021] A sixth aspect of the present invention provides use of the block copolymer-modified silica nanoparticles according to the third aspect and / or the fifth aspect in enhancing crude oil recovery.

[0022] A seventh aspect of the present invention provides an oil-displacing agent, wherein the oil-displacing agent comprises: 99.5%-99.9% by mass of water and 0.1%-0.5% by mass of the block copolymer-modified silica nanoparticles of the third aspect and / or the fifth aspect.

[0023] The eighth aspect of the present invention provides use of the oil-displacing agent of the seventh aspect in improving crude oil recovery.

[0024] Through the above technical solution, the present invention can achieve the following beneficial effects:

[0025] (1) The present invention obtains block copolymer-modified silica nanoparticles having a connecting group of -NHCONH- by reacting a block copolymer containing -NCO structural units with surface-modified silica nanoparticles containing amino groups. The block copolymer-modified silica nanoparticles have a stable structure.

[0026] (2) The block copolymer modified silica nanoparticles prepared by the present invention connect the triblock copolymer with a hydrophilic segment and a lipophilic segment at both ends to the surface of the silica nanoparticles through the middle segment. It has a spontaneous conformational transformation function for water / oil solvents, which can greatly reduce the oil-water interfacial tension, thereby improving capillary action, increasing the oil washing efficiency of the oil displacement system and the ability to emulsify crude oil.

[0027] (3) The oil displacement agent provided by the present invention can further improve the recovery rate on the basis of water flooding, and has great application value in further improving the recovery rate in tertiary oil recovery of low permeability reservoirs and after chemical flooding. BRIEF DESCRIPTION OF THE DRAWINGS

[0028] FIG1 is an infrared spectrum (FTIR) diagram of silica nanoparticles before and after modification by the block copolymer in Example 1.

[0029] FIG2 is an infrared spectrum (FTIR) diagram of the silicon dioxide nanoparticles before and after modification of the block copolymer in Comparative Example 1. DETAILED DESCRIPTION

[0030] The endpoints of the ranges and any values ​​disclosed herein are not limited to the precise ranges or values, and these ranges or values ​​should be understood to include values ​​close to these ranges or values. For numerical ranges, the endpoints of each range, the endpoints of each range and individual point values, and the individual point values ​​can be combined with each other to obtain one or more new numerical ranges, which should be considered to be specifically disclosed herein.

[0031] The first aspect of the present invention provides a block copolymer, wherein the block copolymer comprises a structural unit A represented by formula I, a structural unit B represented by formula II or III, and a structural unit C represented by formula IV.

[0032] Wherein, R1, R3, R5 and R6 are each independently hydrogen or methyl; R2 is C1-C 12 R4 is a straight chain or branched chain alkyl or phenyl group; R7 is a straight chain or branched chain alkylene group of C1-C5; x, y and z are each independently an integer from 1 to 10.

[0033] In some embodiments, R2 is a C1-C8 straight chain or branched alkyl or phenyl group, preferably a methyl or ethyl group; R4 is a C1-C3 straight chain or branched alkylene group, preferably a methylene or ethylene group; x, y and z are integers from 1 to 6, and x, y and z are preferably 1 or 2.

[0034] In some embodiments, the molar ratio of the structural unit A, structural unit B and structural unit C is 1:0.02-3:0.05-20.

[0035] In some embodiments, the block copolymer has a weight average molecular weight of 15,000-160,000 g / mol, preferably 20,000-60,000 g / mol.

[0036] A second aspect of the present invention provides a method for preparing a block copolymer, wherein the preparation method comprises the following steps:

[0037] (1) in a nitrogen atmosphere and in the presence of a first initiator, a chain transfer agent, and an organic solvent, subjecting the monomer represented by formula (1) and the monomer represented by formula (2) or methacryloyl isocyanate to a first polymerization reaction to obtain a first polymer product;

[0038] (2) conducting a second polymerization reaction on the first polymerization product and the monomer represented by formula (3) under a nitrogen atmosphere and in the presence of a second initiator to obtain the block copolymer;

[0039] Wherein, R1, R3 and R6 are each independently hydrogen or methyl; R2 is C1-C12 R4 is a straight chain or branched chain alkyl or phenyl group; R7 is a straight chain or branched chain alkylene group of C1-C5; x, y and z are each independently an integer from 1 to 10.

[0040] In some embodiments, the molar ratio of the monomer represented by formula (1), the monomer represented by formula (2), and the monomer represented by formula (3) is 1:0.05-0.5:0.05-50.

[0041] In some embodiments, in step (1), the conditions of the first polymerization reaction include: reaction temperature of 60-80° C., and reaction time of 3-24 h.

[0042] In some embodiments, the first initiator is an azo initiator, preferably one of azobisisobutyronitrile, azobisisoheptanenitrile and dimethyl azobisisobutyrate.

[0043] In some embodiments, the chain transfer agent is benzyl dithiobenzoate or cumyl dithiobenzoate.

[0044] In some embodiments, R2 is a C1-C8 straight chain or branched alkyl or phenyl group, preferably a methyl or ethyl group; R4 is a C1-C3 straight chain or branched alkylene group, preferably a methyl or ethyl group; x, y and z are integers of 1-6, and x, y and z are preferably 1 or 2.

[0045] In some embodiments, the monomer represented by formula (1) is selected from methyl methacrylate, ethyl methacrylate, n-butyl methacrylate, tert-butyl methacrylate, hexyl methacrylate, 2-ethylhexyl methacrylate, isooctyl methacrylate, 2-ethylhexyl acrylate or styrene.

[0046] In some embodiments, the monomer represented by formula (2) is isocyanoethyl methacrylate or isocyanoethyl acrylate.

[0047] In some embodiments, the monomer represented by formula (3) is selected from methoxyethyl methacrylate, dimethylaminoethyl methacrylate, dimethylaminoethyl acrylate, poly(ethylene glycol) methacrylate, poly(ethylene glycol) acrylate, hydroxyethyl methacrylate, hydroxyethyl acrylate, hydroxypropyl methacrylate, hydroxypropyl acrylate, 4-hydroxybutyl 2-methacrylate, 4-hydroxybutyl acrylate or 2-methoxyethyl 2-acrylate.

[0048] In some embodiments, the organic solvent is benzene.

[0049] In some embodiments, the molar ratio of the initiator, the chain transfer agent and the monomer represented by formula (1) is 1:1-5:50-500.

[0050] In some embodiments, the volume ratio of the monomer represented by formula (1) to the monomer represented by formula (2) is 1:0.06-0.46.

[0051] In some embodiments, step (1) further comprises: dissolving the first polymer product in tetrahydrofuran, adding the first precipitant to precipitate, repeating 3-6 times, filtering and drying at 30-50° C. for 36-48 hours.

[0052] In some embodiments, the first precipitant is a mixed solution of toluene and petroleum ether in a volume ratio of 1:1-4.

[0053] In some embodiments, in step (2), the conditions of the second polymerization reaction include: reaction temperature of 60-80° C., and reaction time of 5-24 h.

[0054] In some embodiments, the second initiator is an azo initiator, preferably one of azobisisobutyronitrile, azobisisoheptanenitrile and dimethyl azobisisobutyrate.

[0055] In some embodiments, the molar ratio of the first polymer product, the monomer of formula (3), and the second initiator is 1:10-1000:0.5-1.

[0056] In some embodiments, step (2) further comprises: dissolving the block copolymer in tetrahydrofuran, adding a second precipitant to precipitate, repeating 3-6 times, filtering, and drying at 30-50° C. for 36-48 hours.

[0057] In some embodiments, the second precipitant is a mixed solution of toluene and petroleum ether in a volume ratio of 1:5-10.

[0058] A third aspect of the present invention provides a block copolymer modified silica nanoparticle, wherein the modified silica nanoparticle comprises: a core derived from a surface-modified silica nanoparticle, a coating layer derived from a block copolymer, and a linking group connecting the core and the coating layer, wherein the block copolymer comprises a structural unit A represented by formula I, a structural unit B represented by formula II or III, and a structural unit C represented by formula IV;

[0059] Wherein, the linking group is -NHCONH-, which is obtained by the addition reaction of -NCO contained in the structural unit B with the amino group contained in the surface-modified silica nanoparticles;

[0060] Wherein, R1, R3, R5 and R6 are each independently hydrogen or methyl; R2 is C1-C 12R4 is a straight chain or branched chain alkyl or phenyl group; R7 is a straight chain or branched chain alkylene group of C1-C5; x, y and z are each independently an integer from 1 to 10.

[0061] In some embodiments, R2 is a C1-C8 straight chain or branched alkyl or phenyl group, preferably a methyl or ethyl group; R4 is a C1-C3 straight chain or branched alkylene group, preferably a methylene or ethylene group; x, y and z are integers from 1 to 6, and x, y and z are preferably 1 or 2.

[0062] In some embodiments, the molar ratio of the structural unit A, structural unit B and structural unit C is 1:0.02-0.3:0.05-20.

[0063] In some embodiments, the content of the silica nanoparticles is 15-85 wt %, preferably 35-75 wt %, based on the total weight of the block copolymer-modified silica nanoparticles.

[0064] In some embodiments, the average particle size of the silica nanoparticles is 20-80 nm.

[0065] A fourth aspect of the present invention provides a method for preparing block copolymer-modified silica nanoparticles, wherein the preparation method comprises the following steps:

[0066] reacting a block copolymer with silane coupling agent-modified silica nanoparticles to obtain block copolymer-modified silica nanoparticles; wherein the block copolymer is the block copolymer described above or a block copolymer prepared by the above preparation method;

[0067] Wherein, the mass ratio of the block copolymer to the silane coupling agent modified silica nanoparticles is 0.3-10:1.

[0068] In some embodiments, the reaction conditions include: ultrasonically dispersing the block copolymer and the silane coupling agent-modified silica nanoparticles in toluene; reacting at 20-30° C. for 4-12 hours using a reflux method; separating the precipitate, washing it, and drying it at 60-100° C. for 12-36 hours to obtain block copolymer-modified silica nanoparticles.

[0069] In some embodiments, the silane coupling agent is selected from 3-aminopropyltriethoxysilane, 3-aminopropyltrimethoxysilane, N-(2-aminoethyl)-3-aminopropyltrimethoxysilane, N-(2-aminoethyl)-3-aminopropyltriethoxysilane, N-(2-aminoethyl)-3-aminopropylmethyldimethoxysilane, N-(2-aminoethyl)-3-aminopropylmethyldiethoxysilane, anilinemethyltrimethoxysilane or anilinemethyltriethoxysilane.

[0070] In some embodiments, the preparation method of the silane coupling agent modified silica nanoparticles includes: mixing anhydrous ethanol, deionized water, ammonia water and tetraethyl orthosilicate for a first reaction, and then adding a silane coupling agent for a second reaction for 2-5 hours to obtain the silane coupling agent modified silica nanoparticles.

[0071] In some embodiments, the molar ratio of anhydrous ethanol, deionized water, ammonia water and tetraethyl orthosilicate is 25-80:2-5:0.25-3.9:1; and the molar ratio of tetraethyl orthosilicate to silane coupling agent is 1:0.01-0.2.

[0072] In some embodiments, the conditions for the first reaction are: under stirring conditions, the reaction time is 12-24 hours; the reaction temperature is 20-30°C; the conditions for the second reaction are: under stirring conditions, the reaction time is 2-5 hours; the reaction temperature is 60-70°C.

[0073] In some embodiments, the preparation method further comprises: washing the silane coupling agent-modified silica nanoparticles in a dispersant, filtering, and drying at 70-90° C. for 12-24 hours, wherein the dispersant is deionized water and / or ethanol.

[0074] The fifth aspect of the present invention provides block copolymer-modified silica nanoparticles prepared by the preparation method of the fourth aspect.

[0075] A sixth aspect of the present invention provides use of the block copolymer-modified silica nanoparticles according to the third aspect and / or the fifth aspect in enhancing crude oil recovery.

[0076] A seventh aspect of the present invention provides an oil-displacing agent, wherein the oil-displacing agent comprises: 99.5%-99.9% by mass of water and 0.1%-0.5% by mass of the block copolymer-modified silica nanoparticles of the third aspect and / or the fifth aspect.

[0077] Compared with commercially available nano oil-displacing agents, the oil-displacing agent comprising the block copolymer-modified silica nanoparticles prepared in the present invention can significantly reduce oil / water interfacial tension, thereby improving crude oil recovery.

[0078] The eighth aspect of the present invention provides use of the oil-displacing agent of the seventh aspect in improving crude oil recovery.

[0079] The present invention will be described in detail below through examples.

[0080] In the following examples and comparative examples, if no specific conditions are specified, the experiments were carried out under conventional conditions or those recommended by the manufacturer. All reagents and instruments used, if no manufacturer is specified, are commercially available conventional products.

[0081] Water / crude oil interfacial tension reduction performance test, test method reference standard SY / T 5370-2018:

[0082] The test oil was a simulated oil prepared by combining crude oil from a block of Daqing Oilfield with aviation kerosene, and the test water was deep-treated sewage from the same block after being filtered through a filter membrane with a pore size of 0.45 μm.

[0083] A certain mass of the sample to be tested was added to the corresponding concentration of on-site water, ultrasonically dispersed for 30 minutes, and mechanically stirred for 30 minutes before use. The test instrument was a TEXAS-500 spinning drop interfacial tensiometer. The main test steps were as follows: start the constant temperature system and control the temperature between 45±0.2℃; fill the measuring tube with the nano-displacement oil system sample; use a microsyringe to draw simulated oil into the measuring tube to form a suitable droplet, and the measuring tube must not contain any bubbles; start the interfacial tensiometer and set the speed to 4500RPM; throughout the measurement process, try to keep the oil droplet in the middle of the capillary tube, and record the experimental data every 15 minutes; the entire measurement time is 2 hours.

[0084] The oil displacement experiment operation method refers to the standard SY / T 6424-2014, and the main steps are as follows:

[0085] 1. Vacuum a square-section 4.5 cm × 4.5 cm × 30 cm Bailey core continuously for more than 4 hours and saturate the core with filtered in situ water.

[0086] 2. Heat the core to 45°C, the formation temperature, and use the prepared simulated oil to displace water. The process ends when the amount of water in the outlet scale tube no longer changes. Measure the cumulative saturated oil volume to obtain the irreducible water saturation.

[0087] 3. Place the oil-saturated core in a 45°C constant temperature box for aging for 12 hours, then change the oil-saturated process to a water flooding process. Stop the water flooding when the water content reaches above 98% in the continuous water flooding 0.5 times the pore volume (0.5PV) stage.

[0088] 4. Switch to the nano-displacement agent injection process and continuously inject a 0.3 PV nano-displacement system slug at a rate of 0.3 mL / min, and record the oil and water production at each stage;

[0089] 5. Switch to subsequent water flooding until the water content of the produced fluid at the outlet reaches more than 98% for 0.5PV continuously. Then end the experiment and calculate the stage recovery factor and total recovery factor respectively.

[0090] Example 1

[0091] (1) Preparation of block copolymers

[0092] 0.05 g of azobisisobutyronitrile, 0.1 g of cumyl dithiobenzoate and 2.0 g of ethyl methacrylate (as shown in formula (1), R1 is methyl and R2 is ethyl) are added to 10 mL of benzene and reacted for 1.5 h at 65°C under a nitrogen atmosphere. Then, 1.2 g of isocyanoethyl methacrylate (as shown in formula (2), R3 is methyl and R4 is ethylene) is added and the reaction is continued for 1.5 h under a nitrogen atmosphere. The product is dissolved and diluted with tetrahydrofuran and slowly added dropwise to a first precipitant (toluene and petroleum ether in a volume ratio of 1:1) in an ice bath for precipitation. The reaction is repeated three times and then dried in vacuo to obtain a first polymer product.

[0093] 1.5 g of the first polymerization product and 9.1 g of dimethylaminoethyl acrylate (as shown in formula (3), R6 is hydrogen, R7 is x is 2) and 0.02 g of azobisisobutyronitrile were added to 15 mL of benzene, and the reaction was carried out under a nitrogen atmosphere at a temperature of 65°C for 5 h. The product was dissolved and diluted with tetrahydrofuran and slowly added dropwise to a second precipitant (toluene and petroleum ether in a volume ratio of 1:5) in an ice bath for precipitation. The reaction was repeated 3 times, and then vacuum dried to obtain a block copolymer, wherein the structural unit A (as shown in Formula I, R1 is methyl and R2 is ethyl), the structural unit B (as shown in Formula II, R3 is methyl and R4 is ethylene) and the structural unit C (as shown in Formula IV, R6 is hydrogen and R7 is The molar ratio of x being 2) is 1:0.29:3.9.

[0094] (2) Preparation of surface-modified silica nanoparticles

[0095] 200 g of ethanol, 5 g of deionized water, and 10 g of ammonia water (25 wt%) were mixed and stirred for 15 min. Then, 15 g of ethyl orthosilicate was added and stirred at room temperature for 12 h. The temperature was raised to 65° C., 1 g of 3-aminopropyltriethoxysilane was added dropwise, and the stirring reaction was continued for 2 h. The solid product was collected by centrifugation, dispersed and washed three times with ethanol and deionized water, and vacuum dried at 80° C. for 12 h to obtain surface-modified silica nanoparticles.

[0096] (3) Preparation of block copolymer modified silica nanoparticles

[0097] 1.5 g of the block copolymer and 0.5 g of surface-modified silica nanoparticles were ultrasonically dispersed in 20 mL of tetrahydrofuran solvent and refluxed at room temperature for 4 h. The solid product was separated by centrifugation, washed three times with tetrahydrofuran, and then vacuum-dried at 80°C for 24 h to obtain block copolymer-modified silica nanoparticles 1 (denoted as S1).

[0098] Example 2

[0099] Block copolymer modified silica nanoparticles were prepared according to the method of Example 1, except that the monomer represented by formula (2) was replaced by methacryloyl isocyanate to obtain block copolymer modified silica nanoparticles 2 (denoted as S2).

[0100] Example 3

[0101] Block copolymer modified silica nanoparticles were prepared according to the method of Example 1, except that the molar ratio of ethyl methacrylate, isocyanoethyl methacrylate and dimethylaminoethyl methacrylate was 1:0.25:0.33, to obtain block copolymer modified silica nanoparticles 3 (denoted as S3).

[0102] Example 4

[0103] Block copolymer modified silica nanoparticles were prepared according to the method of Example 1, except that the molar ratio of ethyl methacrylate, isocyanoethyl methacrylate and dimethylaminoethyl methacrylate was 1:0.03:0.67, to obtain block copolymer modified silica nanoparticles 4 (denoted as S4).

[0104] Example 5

[0105] Block copolymer modified silica nanoparticles were prepared according to the method of Example 1, except that the chain transfer agent was benzyl dithiobenzoate, to obtain block copolymer modified silica nanoparticles 5 (denoted as S5).

[0106] Comparative Example 1

[0107] Block copolymer-modified silica nanoparticles were prepared according to the method of Example 1, except that no silane coupling agent was used to modify the silica nanoparticles. The specific steps are as follows:

[0108] (1) preparing a block copolymer according to the method of Example 1;

[0109] (2) 1.2 g of the block copolymer and 0.4 g of silica nanoparticles were ultrasonically dispersed in 20 mL of tetrahydrofuran solvent and refluxed at room temperature for 5 h. The solid product was separated by centrifugation, washed three times with tetrahydrofuran, and then vacuum-dried at 80°C for 24 h to obtain block copolymer-modified silica nanoparticles (denoted as D1).

[0110] Comparative Example 2

[0111] Block copolymer modified silica nanoparticles were prepared according to the method of Example 1, except that the structural unit B was derived from glycidyl methacrylate, to obtain block copolymer modified silica nanoparticles (denoted as D2).

[0112] Comparative Example 3

[0113] Commercially available nano oil-displacing agent D3.

[0114] Test Case

[0115] The block copolymer modified silica nanoparticles S1-S5, D1, D2 and D3 prepared in the above examples and comparative examples were tested for their ability to reduce water / crude oil interfacial tension. The results are shown in Table 1.

[0116] Block copolymer-modified silica nanoparticles S1-S5, D1, D2, and D3 were used to prepare an oil displacement agent system, and core flooding experiments were carried out. The results are shown in Table 2.

[0117] Table 1

[0118] Table 2

[0119] It can be seen from the results in Table 1 that the interfacial tension of Examples 1-5 of the present invention is significantly reduced, and the interfacial tension of Example 1-3 can reach 10 when the mass concentration is higher than 0.3%. -2 The mN / m level indicates that the block copolymer modified silica nanoparticles provided by the present invention have good performance in reducing oil-water interfacial tension.

[0120] The results in Table 2 show that the core permeabilities of Examples 1-5 and Comparative Examples 1-2 are all less than or equal to 50 mD, indicating that they are natural Berea cores in the low permeability range. The water flooding recovery rate fluctuates within a normal range of ±2%. The nanoflooding recovery rates of Examples 1-5 of the present invention are significantly improved over water flooding, and the total recovery rate is also significantly improved. Moreover, the nanoflooding recovery rate of Example 1-3 can be increased by more than 8 percentage points over water flooding. Compared with commercially available nano oil-displacing agents, the block copolymer-modified silica nanoparticles provided by the present invention can significantly improve crude oil recovery.

[0121] FIG1 compares the infrared spectra of Example 1 with those of the silica nanoparticles not modified by the block copolymer of the present invention. It can be clearly seen that Example 1 has an infrared spectrum of 1600-1850 cm -1 The characteristic peak of carbon-oxygen double bond stretching vibration indicates that the block copolymer and the silica nanoparticles are connected through -NHCONH- in Example 1 to obtain block copolymer-modified silica nanoparticles.

[0122] FIG2 compares the infrared spectra of the silica nanoparticles of comparative example 1 with those of the silica nanoparticles. It can be seen that there is no obvious change in the characteristic peaks, and the silica nanoparticles of D1 are not modified by the block copolymer.

[0123] The preferred embodiments of the present invention have been described in detail above, but the present invention is not limited thereto. Within the technical concept of the present invention, various simple variations of the technical solution of the present invention may be made, including combining the various technical features in any other appropriate manner. These simple variations and combinations should also be regarded as disclosed in the present invention and fall within the scope of protection of the present invention.

Claims

1. A block copolymer, characterized in that The block copolymer contains a structural unit A shown in formula I, a structural unit B shown in formula II or III, and a structural unit C shown in formula IV. Wherein, R1, R3, R5 and R6 are each independently hydrogen or methyl; R2 is C1-C 12 R4 is a C1-C5 straight chain or branched chain alkylene; R7 is x, y and z are each independently an integer of 1-10.

2. The block copolymer according to claim 1, wherein R2 is a C1-C8 straight chain or branched alkyl or phenyl group; R4 is a C1-C3 straight chain or branched alkylene group; x, y and z are each independently an integer of 1 to 6; And / or, the molar ratio of the structural unit A, the structural unit B and the structural unit C is 1:0.02-0.3:0.05-20; And / or, the block copolymer has a weight average molecular weight of 15000-160000 g / mol.

3. A method for preparing a block copolymer, characterized in that: The preparation method comprises the following steps: (1) in a nitrogen atmosphere and in the presence of a first initiator, a chain transfer agent, and an organic solvent, subjecting the monomer represented by formula (1) and the monomer represented by formula (2) or methacryloyl isocyanate to a first polymerization reaction to obtain a first polymer product; (2) in a nitrogen atmosphere and in the presence of a second initiator, subjecting the first polymerization product to a second polymerization reaction with the monomer represented by formula (3) to obtain the block copolymer; Wherein, R1, R3 and R6 are each independently hydrogen or methyl; R2 is C1-C 12 R4 is a C1-C5 straight chain or branched chain alkylene; R7 is x, y and z are each independently an integer of 1-10.

4. The preparation method according to claim 3, wherein The molar ratio of the monomer represented by formula (1), the monomer represented by formula (2) and the monomer represented by formula (3) is 1:0.05-0.5:0.05-50.

5. The preparation method according to claim 3 or 4, wherein In step (1), the conditions of the first polymerization reaction include: reaction temperature of 60-80° C., reaction time of 3-24 h; And / or, the first initiator is an azo initiator, preferably one of azobisisobutyronitrile, azobisisoheptanenitrile and dimethyl azobisisobutyrate; And / or, the chain transfer agent is benzyl dithiobenzoate or cumyl dithiobenzoate; and / or, R2 is a C1-C8 straight chain or branched chain alkyl or phenyl; R4 is a C1-C3 straight chain or branched chain alkylene; x, y and z are each independently an integer of 1-6; And / or, the organic solvent is benzene; and / or, the molar ratio of the initiator, the chain transfer agent and the monomer represented by formula (1) is 1:1-5:50-500; And / or, the volume ratio of the monomer represented by formula (1) to the monomer represented by formula (2) is 1:0.06-0.

46.

6. The preparation method according to claim 5, wherein: The monomer represented by formula (1) is selected from methyl methacrylate, ethyl methacrylate, n-butyl methacrylate, tert-butyl methacrylate, hexyl methacrylate, 2-ethylhexyl methacrylate, isooctyl methacrylate, 2-ethylhexyl acrylate or styrene; and / or, the monomer represented by formula (2) is isocyanoethyl methacrylate or isocyanoethyl acrylate; And / or, the monomer represented by formula (3) is selected from methoxyethyl methacrylate, dimethylaminoethyl methacrylate, dimethylaminoethyl acrylate, poly(ethylene glycol) methacrylate, poly(ethylene glycol) acrylate, hydroxyethyl methacrylate, hydroxyethyl acrylate, hydroxypropyl methacrylate, hydroxypropyl acrylate, 4-hydroxybutyl 2-methacrylate, 4-hydroxybutyl acrylate or 2-methoxyethyl 2-acrylate.

7. The preparation method according to claim 3 or 4, wherein: Step (1) further comprises: dissolving the first polymer product in tetrahydrofuran, adding the first precipitant to precipitate, repeating 3-6 times, filtering and drying at 30-50° C. for 36-48 hours.

8. The preparation method according to claim 7, wherein: The first precipitant is a mixed solution of toluene and petroleum ether in a volume ratio of 1:1-4.

9. The preparation method according to claim 3 or 4, wherein: In step (2), the conditions of the second polymerization reaction include: reaction temperature of 60-80° C., reaction time of 5-24 h; And / or, the second initiator is an azo initiator; and / or, the molar ratio of the first polymer product, the monomer described in formula (3) and the second initiator is 1:10-1000:0.5-1; And / or, step (2) further comprises: dissolving the block copolymer in tetrahydrofuran, adding the block copolymer into a second precipitant for precipitation, repeating the process 3-6 times, filtering and drying at 30-50° C. for 36-48 hours.

10. The preparation method according to claim 9, wherein: The second precipitant is a mixed solution of toluene and petroleum ether in a volume ratio of 1:5-10.

11. A block copolymer modified silica nanoparticle, characterized in that: The modified silica nanoparticles comprise: a core from a surface-modified silica nanoparticle, a coating layer from a block copolymer, and a connecting group connecting the core and the coating layer, wherein the block copolymer comprises a structural unit A shown in formula I, a structural unit B shown in formula II or III, and a structural unit C shown in formula IV; Wherein, the connecting group is -NHCONH-, which is obtained by the addition reaction of -NCO contained in the structural unit B with the amino group contained in the surface-modified silica nanoparticles; Wherein, R1, R3, R5 and R6 are each independently hydrogen or methyl; R2 is C1-C 12 R4 is a C1-C5 straight chain or branched chain alkylene; R7 is x, y and z are each independently an integer of 1-10.

12. The block copolymer modified silica nanoparticles according to claim 11, wherein R2 is a C1-C8 straight chain or branched chain alkyl or phenyl; R4 is a C1-C3 straight chain or branched chain alkylene; x, y and z are integers of 1-6; Wherein, the molar ratio of the structural unit A, the structural unit B and the structural unit C is 1:0.02-0.3:0.05-20; and / or, based on the total weight of the block copolymer modified silica nanoparticles, the content of the silica nanoparticles is 15-85wt%; And / or, the average particle size of the silicon dioxide nanoparticles is 20-80 nm.

13. A method for preparing block copolymer modified silica nanoparticles, characterized in that: The preparation method comprises the following steps: The block copolymer is reacted with silane coupling agent modified silica nanoparticles to obtain block copolymer modified silica nanoparticles; wherein the block copolymer is the block copolymer according to claim 1 or 2 or the block copolymer prepared by the preparation method according to any one of claims 3-10.

14. The method for preparing block copolymer modified silicon dioxide nanoparticles according to claim 13, wherein: The mass ratio of the block copolymer to the silane coupling agent modified silicon dioxide nanoparticles is 0.3-10:

1.

15. The method for preparing block copolymer modified silicon dioxide nanoparticles according to claim 13 or 14, wherein: The reaction conditions include: ultrasonically dispersing the block copolymer and the silane coupling agent modified silica nanoparticles in tetrahydrofuran; reacting at 20-30° C. for 4-12 hours by reflux method; separating the precipitate, washing it, and drying it at 60-100° C. for 12-36 hours to obtain block copolymer modified silica nanoparticles.

16. The method for preparing block copolymer modified silicon dioxide nanoparticles according to claim 15, wherein: The silane coupling agent is selected from 3-aminopropyltriethoxysilane, 3-aminopropyltrimethoxysilane, N-(2-aminoethyl)-3-aminopropyltrimethoxysilane, N-(2-aminoethyl)-3-aminopropyltriethoxysilane, N-(2-aminoethyl)-3-aminopropylmethyldimethoxysilane, N-(2-aminoethyl)-3-aminopropylmethyldiethoxysilane, anilinemethyltrimethoxysilane or anilinemethyltriethoxysilane; And / or, the preparation method of the silane coupling agent modified silica nanoparticles comprises: mixing anhydrous ethanol, deionized water, ammonia water and tetraethyl orthosilicate for a first reaction, adding a silane coupling agent for a second reaction for 2-5 hours to obtain the silane coupling agent modified silica nanoparticles.

17. The method for preparing block copolymer modified silicon dioxide nanoparticles according to claim 16, wherein: The molar ratio of anhydrous ethanol, deionized water, ammonia water and tetraethyl orthosilicate is 25-80:2-5:0.25-3.9:1; And / or, the molar ratio of the tetraethyl orthosilicate to the silane coupling agent is 1:0.01-0.2; And / or, the conditions of the first reaction include: under stirring conditions, the reaction time is 12-24h and the reaction temperature is 20-30°C; And / or, the conditions of the second reaction include: under stirring conditions, the reaction time is 2-5h, and the reaction temperature is 60-70°C; And / or, the preparation method of the silane coupling agent modified silica nanoparticles further comprises: washing the silane coupling agent modified silica nanoparticles in a dispersant, filtering and drying at 70-90° C. for 12-24 hours, wherein the dispersant is deionized water and / or ethanol.

18. Block copolymer modified nano-silicon dioxide prepared by the preparation method described in any one of claims 13 to 17.

19. Use of the block copolymer modified silica nanoparticles according to any one of claims 11 to 12 and 18 in improving crude oil recovery.

20. An oil displacing agent, characterized in that: The oil displacing agent comprises: 99.5%-99.9% by weight of water and 0.1%-0.5% by weight of the block copolymer modified silicon dioxide nanoparticles according to any one of claims 11-12 and 18.

21. Use of the oil displacing agent according to claim 20 in improving crude oil recovery.

Citation Information

Patent Citations

  • Non-aqueous pigment ink

    CN101270245A

  • Preparation method of surface modified nano silicon dioxide colloid

    CN103160265A

  • Preparation method of amphiphilic acrylate copolymer surface grafting modified nano silicon dioxide

    CN103665269A

  • Modified silica nanoparticles and preparation method thereof and drilling fluid suitable for shale gas well

    CN105801783A

  • Acrylic-urethane composite resin particles

    CN105849142A