Method for compounding shear thickening fluid and fabric
By adding ammonia to the shear thickening fluid and combining medium and high-frequency ultrasonic treatment, the problem of poor separation of solvent and nanoparticles and stabbing resistance in the composite of fluid and fabric is solved, and the strength and stabbing resistance of the composite material are significantly improved. The preparation of high-performance composite materials is realized.
Patent Information
- Application Number
- PCT/CN2024/086795
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-05-06
- Filing Date
- 2024-04-09
- Publication Date
- 2024-11-14
AI Technical Summary
In the existing method of composite shear thickening fluid and fabric, the solvent and nanoparticles of the fluid are easily separated, resulting in poor composite effect and poor stabbing resistance. The composite material produced by the traditional method is low in strength and cannot effectively resist GA68~2019 Standard D1 knife head stabbing.
The pre-mixing step adds ammonia water at pH = 7.1 to 9 to negatively charge the surface of the silica particles, and forms a uniform diluent through medium frequency ultrasonic dispersion, and uses high-frequency ultrasonic waves to eliminate micro bubbles during the impregnation process to ensure that the fluid is evenly dispersed in the fabric. In addition, the strength and stab resistance of composite materials are improved.
The uniform dispersion of shear thickening fluid in the fabric is achieved, which significantly improves the strength and stabbing resistance of the composite material, avoids solvent inhalation and particle agglomeration, and ensures the mechanical properties and stabbing resistance of the composite material.
Smart Images

Figure CN2024086795_14112024_PF_FP_ABST
Abstract
Description
A composite method of shear thickening fluid and fabric Technical Field
[0001] The invention relates to a composite method of a shear thickening fluid and a fabric, and belongs to the technical field of application of shear thickening fluid composite materials. Background Art
[0002] Shear-thickening fluids are highly stress-sensitive liquid materials composed of nanoparticles and a solvent. When subjected to external stress, the nanoparticles in the fluid instantly aggregate to form clusters, causing the fluid's concentration to increase dramatically, resulting in solid-like properties and resistance to external forces. This property makes shear-thickening fluids promising for widespread application in the field of protective equipment.
[0003] Shear thickening fluid can be applied to fabrics to make fully flexible bulletproof and stab-proof composites, which have broad application prospects. There are two commonly used composite processes: 1) the fluid is directly coated on the surface of the fabric and slowly penetrated into the interior of the fabric by hot pressing to form a composite; 2) the fluid is diluted with volatile solvents such as methanol and ethanol, and then the fabric is impregnated and dried to obtain a composite. Although both methods can produce composites, the composite effect and stab-proof performance are defective. Method 1 causes the solvent and nanoparticles of the fluid to separate, the solvent is absorbed into the fabric, and the particles agglomerate and deposit on the surface of the fabric, resulting in poor composite effect. The composite produced by method 2 has low strength and has basically no stab-proof effect on GA68~2019 standard D1 blades. Therefore, a method for preparing high-strength and high-performance composites is needed.
[0004] Summary of the Invention
[0005] The purpose of the present invention is to solve the problems in the prior art of poor shear thickening fluid composite fabric effect and poor stab resistance, and to provide a composite method of shear thickening fluid and fabric, which can evenly disperse the shear thickening fluid into the fabric and improve the strength and stab resistance of the composite fabric.
[0006] The purpose of the present invention is achieved through the following technical solutions:
[0007] A method for compounding a shear thickening fluid and a fabric, characterized by comprising the following steps:
[0008] a. Premixing: Add ammonia water with a pH of 7.1 to 9 to the shear thickening fluid and mix well to obtain a premixed liquid. The premixed liquid is milky white and contains clusters of millimeter and micron-sized particles.
[0009] b. Dispersion: Place the premixed solution in a sealed container and disperse it using medium-frequency ultrasound in a water bath to obtain a uniform dilution solution;
[0010] c. Impregnation: Immerse the fabric in the diluent and perform high-frequency ultrasonic treatment during the impregnation process. After impregnation, squeeze out the excess liquid and dry the fabric.
[0011] During the premixing process of the present invention, the mass ratio of the fluid to the ammonia water is 1:0.5-3. The ammonia water can make the surface of the silicon dioxide particles negatively charged, so that the particles are dispersed by charge repulsion, effectively avoiding agglomeration. In addition, the ammonia water can be completely removed by drying, and impurities that affect the rigid collision of the nanoparticles will not be introduced into the fluid, thereby avoiding affecting the mechanical properties of the final composite material.
[0012] During the dispersion process in step b, the ultrasonic power density is 50-100 W / gallon, the ultrasonic frequency is 30-40 kHzf, the ultrasonic temperature is 30-50°C, and the ultrasonic time is 10-30 minutes. Although low-frequency ultrasound (20-28 kHz) has a strong cavitation effect, it can cause local overheating of the liquid, which can lead to particle agglomeration and precipitation. Water bath ultrasound with an ultrasonic frequency of 30-40 kHz allows for continuous ultrasonic treatment and facilitates accurate temperature control. The treated dilution solution can be filtered through filter paper with a pore size of 1-3 μm, without any residue remaining on the filter paper surface.
[0013] The dispersed dilution solution does not produce precipitation after standing for 4 days, and separates into layers after standing for 2 to 3 weeks, that is, the bottom layer is milky white sediment and the upper layer is clear liquid. However, a well-uniform dilution solution can be obtained again by repeating steps 2 and 3.
[0014] During the impregnation process in step c of the present invention, the ultrasonic power density is 50 to 100 W / gallon, the ultrasonic frequency is 68 to 80 kHzf, and the ultrasonic treatment time is 10 to 30 seconds. The use of high-frequency ultrasonic waves can effectively remove microbubbles in the fabric during the impregnation liquid, making the composite more uniform and further dispersing any tiny particle clusters, thereby improving the mechanical properties of the composite material.
[0015] Compared with the traditional method, the advantages of the present invention are:
[0016] 1. During the dilution process, the fluid is in a closed container and no external impurities are introduced.
[0017] 2. Dilution uses medium frequency ultrasonic treatment. Ultrasonic waves in this frequency band can quickly dilute the fluid and will not cause particle agglomeration due to excessive cavitation.
[0018] 3. High-frequency ultrasonic oscillation is used during impregnation to eliminate micron-level and submicron-level bubbles in the fabric structure, increase the composite uniformity of the fluid and fabric, and increase the strength and puncture-proof performance of the composite material.
[0019] 4. Water bath ultrasound allows for precise temperature control because water has a large specific heat capacity and can absorb the heat generated by ultrasound without rapidly heating up. Therefore, precise temperature control is possible without the need for additional cooling devices.
[0020] 5. The dilution process is clean and green, without any toxic reagents. BRIEF DESCRIPTION OF THE DRAWINGS
[0021] Figure 1 is a diagram showing a single yarn extraction experiment;
[0022] FIG2 shows the relationship between the pulling force of a single yarn and the pulling displacement of the composite material of Example 1;
[0023] FIG3 shows the relationship between the pulling force of a single yarn and the pulling displacement of the composite material of Example 2;
[0024] FIG4 shows the relationship between the pulling force of a single yarn and the pulling displacement of the composite material of Example 3;
[0025] FIG5 shows the relationship between the pulling force of a single yarn and the pulling displacement of the composite material of Example 4;
[0026] FIG6 shows the relationship between the pulling force of a single yarn of the fabric of Comparative Example 1 and the pulling displacement;
[0027] FIG7 shows the relationship between the pulling force of a single yarn of the fabric of Comparative Example 2 and the pulling displacement;
[0028] FIG8 shows the relationship between the pulling force of a single yarn of the fabric of Comparative Example 3 and the pulling displacement;
[0029] FIG9 shows the relationship between the pulling force of a single yarn of the fabric of Comparative Example 4 and the pulling displacement. DETAILED DESCRIPTION
[0030] A method for compounding a shear thickening fluid and a fabric, characterized by comprising the following steps:
[0031] a. Premixing: Add ammonia water with a pH of 7.1 to 9 to the shear thickening fluid, with the mass ratio of fluid to ammonia water being 1:0.5 to 3, and mix well to obtain a pre-milky white mixed solution;
[0032] b. Dispersion: Place the premixed solution in a sealed container and ultrasonically disperse it in a water bath at an ultrasonic power density of 50-100 W / gallon, an ultrasonic frequency of 30-40 kHzf, and an ultrasonic temperature of 30-50°C for 10-30 minutes to obtain a uniform dilution solution that passes through a filter paper with a pore size of 1-3 μm and has no residual particulate matter.
[0033] c. Immersing: Immerse the fabric in the diluent and simultaneously perform ultrasonic treatment at a high frequency of 68 to 80 kHz for 10 to 30 seconds. After immersion, squeeze out excess liquid and dry the fabric. The present invention will be further described in detail below with reference to specific embodiments.
[0034] Example 1:
[0035] Polydisperse silica spheres with diameters of 86 nm to 117 nm were dispersed in polyethylene glycol 300 to obtain a shear thickening fluid with a silica sphere volume fraction of 0.48.
[0036] The fabric is aramid woven fabric, and the composite method of the shear thickening fluid and the fabric is:
[0037] a. Premixing: Add ammonia water with a pH of 8.5 to the shear thickening fluid, with the fluid and ammonia water mass ratio being 1:1, and mix well to obtain a pre-milky white mixed solution;
[0038] b. Dispersion: Place the premixed solution in a sealed container and ultrasonically disperse it in a water bath at an ultrasonic power density of 93 W / gallon, an ultrasonic frequency of 40 kHzf, and an ultrasonic temperature of 35 ± 2°C for 20 min to obtain a uniform dilution. Pass the dilution through a 1 μm filter paper. No particles are found on the filter paper.
[0039] c. Impregnation: Immerse the aramid woven fabric in the diluent, and simultaneously perform ultrasonic treatment at a high frequency of 75kHzf and an ultrasonic temperature of 35±2℃ for 30s during the impregnation process. After impregnation, extrude the fabric through a pressure roller with a roller pressure of 0.2MPa to squeeze out excess liquid, and dry the fabric at 80℃ for 30 minutes to obtain the nanocomposite material.
[0040] The strength of nanocomposites is primarily assessed through a "single yarn extraction" test. The nanocomposite is cut into a 20cm x 12cm rectangle, partially removed from the weft yarn, and mounted on a tensile testing machine, as shown in Figure 1. A single warp yarn is secured to a fixture and extracted along the warp direction at a constant speed of 100mm / min. The tensile testing machine's sensor head has a range of 300N. The induced force during the extraction process is recorded on a computer and displayed as the relationship between extraction force and displacement. The results are shown in Figure 2.
[0041] Example 2:
[0042] The shear thickening fluid and the woven fabric are the same as in Example 1, and the compounding method is as follows:
[0043] a. Premixing: Take an appropriate amount of fluid and place it in a wide-mouth bottle. Add an equal amount of water with a pH of 7.1. Prepare a uniform dilution according to steps a and b of the embodiment. Let it stand for 15 days to allow the dilution to separate into layers. The upper layer is a slightly yellow clear liquid, and the lower layer is a milky white sediment.
[0044] b. Dispersion: Place the jar containing the layered dilution in a water bath and ultrasonically disperse for 30 minutes at an ultrasonic power density of 52 W / gallon, an ultrasonic frequency of 30 kHzf, and an ultrasonic temperature of 50 ± 1°C to obtain a uniform dilution. Pass the dilution through filter paper, and no particles are found on the filter paper.
[0045] c. Impregnation: Immerse the aramid woven fabric in the diluent, and simultaneously perform ultrasonic treatment for 30 seconds at a high frequency of 80kHzf and an ultrasonic temperature of 50±1℃ during the impregnation process. After impregnation, extrude the fabric through a pressure roller with a roller pressure of 0.2MPa to squeeze out excess liquid, and dry the fabric at 80℃ for 30 minutes to obtain the nanocomposite material.
[0046] The warp yarn extraction force was tested according to the method of Example 1, and the results are shown in FIG3 .
[0047] Example 3:
[0048] The shear-thickening fluid is a highly concentrated suspension of nanosilica spheres (500 ± 25 nm in diameter) in polypropylene glycol, with a volume fraction of φ ≈ 0.52. The fabric is a plain weave blend of ultra-high molecular weight polyethylene and aramid, with aramid in the warp direction and ultra-high molecular weight polyethylene in the weft direction. The composite material is prepared as follows:
[0049] a. Premixing: Take an appropriate amount of fluid and place it in a wide-mouth bottle. Add ammonia water with a pH of 9 (the mass ratio of fluid to ammonia water is 1:3) and mix well to obtain a milky white premixed solution.
[0050] b. Dispersion: Place the premixed solution in a sealed container and ultrasonically disperse it in a water bath at an ultrasonic power density of 75 W / gallon, an ultrasonic frequency of 35 kHzf, and an ultrasonic temperature of 40 ± 1°C for 10 minutes to obtain a uniform dilution. Pass the dilution through filter paper, and no particles are found on the filter paper.
[0051] c. Impregnation: Immerse the blended plain woven fabric in the diluent, and simultaneously carry out ultrasonic treatment for 10 seconds at a high frequency of 68kHzf and an ultrasonic temperature of 42±2℃ during the impregnation process. After impregnation, extrude the fabric through a pressure roller at a turbid pressure of 0.15MPa, squeeze out the excess liquid, and dry the fabric at 80℃ for 30 minutes to obtain the nanocomposite material.
[0052] The warp yarn extraction force was tested according to the method of Example 1, and the results are shown in FIG4 .
[0053] Example 4:
[0054] The shear thickening fluid is a high-concentration suspension of nano-silica spheres (diameter 350±10nm) in polyethylene glycol 300, with a volume fraction of 0.57. The fabric is a plain woven high-strength polyester fabric. The composite material is compounded as follows:
[0055] a. Premixing: Place an appropriate amount of fluid in a wide-mouth bottle and add ammonia water with a pH of 8.0, so that the mass ratio of fluid to ammonia water is 2:1. Mix thoroughly to obtain a milky white premixed solution.
[0056] b. Dispersion: Place the premixed solution in a sealed container and ultrasonically disperse it in a water bath at an ultrasonic power density of 50 W / gallon, an ultrasonic frequency of 30 kHzf, and an ultrasonic temperature of 30°C for 15 minutes to obtain a uniform dilution. Pass the dilution through filter paper; no particulate residue is found on the filter paper.
[0057] c. Impregnation: The polyester fabric is immersed in the diluent, and the impregnation process is carried out simultaneously at a high frequency of 80kHzf and an ultrasonic temperature of 35°C for 20s. After impregnation, it is extruded through a pressure roller with a pressure between rollers of 0.18MPa to squeeze out excess liquid, and the fabric is dried at 90°C for 20 minutes to obtain a nanocomposite.
[0058] The warp yarn extraction force was tested using the method of Example 1, and the results are shown in FIG5 .
[0059] Comparative Example 1 (direct measurement of extraction force without treatment):
[0060] Without treating the fabric, the warp yarn extraction force was directly tested according to the method of Example 1, and the results are shown in FIG6 .
[0061] Comparative Example 2 (too alkaline water):
[0062] The shear thickening fluid and fabric were the same as those in Example 1. During the composite method, an equal mass of water with a pH value of 10 was added during premixing. Other steps were the same as those in Example 1 to prepare the nanocomposite material.
[0063] The warp yarn extraction force was tested according to the method of Example 1, and the results are shown in FIG7 .
[0064] Comparative Example 3 (too acidic water):
[0065] The shear thickening fluid and fabric were the same as those in Example 1. During the composite method, an equal mass of water with a pH value of 5.3 was added during premixing. Other steps were the same as those in Example 1 to prepare the nanocomposite material.
[0066] The warp yarn extraction force was tested according to the method of Example 1, and the results are shown in FIG8 .
[0067] Comparative Example 4 (no ultrasound, only premixing):
[0068] The shear thickening fluid and fabric are the same as in Example 1, and the compounding method is as follows:
[0069] An appropriate amount of fluid was mixed with an equal amount of ammonia water with a pH of ≈8.5 on a vortex shaker at 2500 rpm for 5 hours to obtain a milky white premix with essentially no stratification. Without water bath ultrasonic treatment, a nanocomposite material was prepared according to step c of Example 1, and the warp yarn pull-out force was tested. The results are shown in FIG9 .
[0070] Figure 6 shows that the maximum pull-out force for the untreated aramid woven warp yarn does not exceed 10 N. As the warp yarn is slowly pulled out, the pull-out force gradually decreases to 0 N. However, for the nanocomposite prepared with ammonia as the diluent, the shear-thickening fluid adheres well to the surface of the fabric yarn. During extraction, the mutual friction between the warp and weft yarns causes the fluid to be stressed and rapidly thickened. As a result, the maximum pull-out force exceeds 100 N, more than 10 times that of the untreated warp yarn. In contrast, the pull-out force of a single yarn in the composite prepared using conventional methods is only 60 N.
[0071] Nanocomposites prepared with ammonia as the diluent experience yarn breakage and a sudden drop in pullout force after yarn is pulled to a certain extent. This is because the nanoparticles in the shear-thickening fluid are extremely hard. After the fluid thickens, the rigid friction between the particles damages the yarn, causing it to break after being pulled to a certain extent. Furthermore, nanocomposites prepared with ammonia as the diluent exhibit extremely high pullout forces exceeding 100N. This is because ammonia molecules are small and have appropriate polarity, which easily helps the fluid fill the micropores of the fabric, making the composite more complete.
[0072] Although the diluted solution prepared by the method of the present invention will cause the nanoparticles to precipitate if left for a long time, a stable mixed solution can be reformed by repeating the water bath ultrasonication step, and the warp yarn extraction force of the prepared composite material will not be reduced, which can be demonstrated by comparing the test data of Examples 1 and 2.
[0073] Table 1 compares the pull-out forces of various fabric types before and after lamination in Examples 1, 3, and 4. The fabric types are aramid, aramid / polyethylene blended fabrics, and high-strength polyester fabrics. For all three fabric types, the pull-out forces were significantly improved after treatment (at least 10-fold), demonstrating both the significant strength improvement achieved by the composite materials produced by this method and its applicability to a wide variety of fabrics.
[0074] Table 1: Comparison of single yarn pull-out force test before and after different fabric treatments
Claims
1. A method for compounding a shear thickening fluid and a fabric, characterized in that The following steps are involved: a. Premixing: Add ammonia water with a pH of 7.1 to 9 to the shear thickening fluid and mix well to obtain a premixed liquid; b. Dispersion: Place the premixed solution in a sealed container and disperse it by medium-frequency ultrasound in a water bath to obtain a uniform diluted solution; c. Impregnation: Immerse the fabric in the diluent and perform high-frequency ultrasonic treatment during the impregnation process. After impregnation, squeeze out the excess liquid and dry the fabric.
2. A method for compounding a shear thickening fluid and a fabric according to claim 1, characterized in that The mass ratio of the fluid to the ammonia water is 1:0.5-3.
3. The method for compounding a shear thickening fluid and a fabric according to claim 1, characterized in that The instrument used for premixing is a vortex shaker.
4. A method for compounding a shear thickening fluid and a fabric according to claim 1, characterized in that The prepared premixed liquid is milky white and has agglomerated clusters of millimeter and micrometer-sized particles.
5. The method for compounding a shear thickening fluid and a fabric according to claim 1, characterized in that During the dispersion process, the ultrasonic power density is 50-100 W / gallon, the ultrasonic frequency is 30-40 kHzf, the ultrasonic temperature is 30-50° C., and the ultrasonic time is 10-30 min.
6. The method for compounding a shear thickening fluid and a fabric according to claim 1, characterized in that During the immersion process, the ultrasonic power density is 50-100 W / gallon, the ultrasonic frequency is 68-80 kHzf, the ultrasonic temperature is 30-40° C., and the ultrasonic treatment time is 10-30 s.
7. The method for compounding a shear thickening fluid and a fabric according to claim 1, characterized in that The diluted solution obtained in step b was left to stand for 4 days without generating precipitation.
8. The method for compounding a shear thickening fluid and a fabric according to claim 1, characterized in that The dilution obtained in step b passes through filter paper with a pore size of 1 to 3 μm and no particulate matter remains.
9. The method for compounding a shear thickening fluid and a fabric according to claim 1, characterized in that The fabric has a liquid content of 7-25% after drying.
Citation Information
Patent Citations
Preparing method of impact-resistant shear thickening liquid non-woven fabric composite
CN110541299A
Bulletproof material prepared from ultra-high molecular weight polyethylene fiber / shear thickening fluid composite fiber
CN112391691A
Dispersion phase particle for shear thickening fluid, preparation method and application
CN112695518A
Method for compounding shear thickening fluid and fabric
CN116590911A
Shear thickening fluid impregnated structure and astronaut protective garments having the same
KR1020150107987A