A fast response carbon nanotubes stretch sensor
A horizontally aligned single wall carbon nanotubes stretch sensor with a fast response time is achieved by aligning nanotubes between non-flexible substrates and layering a flexible substrate, addressing the challenge of achieving high-performance and fast-response strain sensors, resulting in a durable and quick-strain-detecting device.
Patent Information
- Application Number
- PCT/IN2024/050485
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-05-10
- Filing Date
- 2024-05-06
- Publication Date
- 2024-11-14
AI Technical Summary
Existing carbon nanotubes stretch sensors face challenges in achieving a highly aligned nanotube structure, which is crucial for producing high-performance and fast-response strain sensors, due to difficulties in deposition techniques that result in high production costs and complex engineering routes.
A carbon nanotubes stretch sensor is developed with a horizontally aligned single wall carbon nanotube layer, achieved by filling a single wall carbon nanotube solution in an acid between two non-flexible substrates, pressing one substrate while keeping the other stationary, and dipping it in a coagulant, followed by layering a flexible substrate and attaching electrodes, resulting in a fast response time of less than 5 milliseconds.
The solution provides a durable stretch sensor with high durability for over 70,000 cycles and a fast response time of less than 5 milliseconds, suitable for applications requiring quick strain detection.
Smart Images

Figure IN2024050485_14112024_PF_FP_ABST
Abstract
Description
[0001] A FAST RESPONSE CARBON NANOTUBES ST RETCH SENSOR
[0002] FIELD OF INVENTION
[0003] The invention relates generally to the field of stretch sensors and more particularly to a carbon nanotubes stretch sensor.
[0004] BACKGROUND
[0005] Stretch sensors are electronic sensors that produce a linear change in voltage, when they are stretched. The characteristics of high reliability, low maintenance and strain sensing capability make stretch sensors ideal for use in industries including but not limited to automotive, medical, biomedical, sports, aviation, robotics and consumerelectronics applications. More advanced application of the stretch sensors include body integrated electronic systems that can be embedded into clothing or attached directly to the body for measuring precise strain ranging from pulse rate, heart beat to bending of joints. Nanocarbon materials, such as graphene, carbon nanotubes and carbon nanofibers are being used for developing sensors due to their high electrical conductivity, mechanical flexibility and intrinsic carrier mobility. Predominantly, carbon nanotubes based stretch sensors are fabricated by preparing a composite of carbon nanotubes with a stretchable polymer. For preparing the carbon nanotubes-polymer composite, either multi-walled carbon nanotubes or single-walled carbon nanotubes are used. However, mixing carbon nanotubes directly with polymer substrates often suffers from a poor dispersion and requires high enough concentrations of carbon nanotubes to achieve a desired resistance value resulting in high production costs and complicated engineering routes. Deposition of individual carbon nanotubes solutions on the polymer surface is one of the more convenient techniques for fabricating carbon nanotubes networks by surface modification. Deposition technique play crucial role in forming a good conductive network of carbon nanotubes on a substrate while maintaining all the desirable performance parameters of the strain sensor. Various deposition techniques have been known for deposition of carbon nanotubes on the polymer surface. Yamada et’al 2011 , prepared a strain sensor by depositing single wall carbon nanotubes side by side with 1 mm overlap on a PDMS substrate with the alignment of the single wall carbon nanotubes arranged perpendicular to the strain axis. The strain sensor can withstand strain upto 280%, with a durability of 10,000 cycles at 150% strain and delay time of 14ms. Yulinati et’al 2021 , fabricated single wall carbon nanotubes by cyclic hydrothermal coating a flexible substrate with a thin polydopamine layer to form single wall carbon nanotubes-substrate interfacial bonding. The strain sensor has high sensitivity and good stretchability and can withstand extreme strains of up to 600%, a gauge factor (GF) of up to 28.5, and a response time of less than 1 s with low carbon nanotubes concentration. US 2014 / 0331793, discloses a strain sensor fabricated by layering a multi-wall carbon nanotubes fibre bundles on a flexible substrate and covering the carbon nanotubes fibre bundles with a resin layer. For preparing a high performance and fast response strain sensor, obtaining a highly aligned nanotube structure is a crucial step. From the techniques available in the art, it is difficult to form a highly aligned nanotube and hence the above mentioned techniques are not suitable for preparing a high performance strain sensor.
[0006] Hence, there is a need for a production technology that produces highly aligned nanotube structure for preparing a high performance and fast response strain sensor.
[0007] BRIEF DESCRIPTION OF DRAWINGS
[0008] So that the manner in which the recited features of the invention can be understood in detail, some of the embodiments are illustrated in the appended drawings. It is to be noted, however, that the appended drawings illustrate only typical embodiments of this invention and are therefore not to be considered limiting of its scope, for the invention may admit to other equally effective embodiments.
[0009] FIG. 1 is a schematic representation of a carbon nanotubes based stretch sensor, according to an embodiment of the invention.
[0010] FIG. 2 is a schematic representation of a carbon nanotubes based stretch sensor, according to another embodiment of the invention
[0011] FIG.3 shows the response of the carbon nanotubes based stretch sensor with respectto time, according to an embodiment of the invention. FIG. 4 shows response of the carbon nanotubes based stretch sensorwith respectto strain, according to an embodiment of the invention.
[0012] FIG. 5 shows the response time of the sensor, according to an embodimentof the invention.
[0013] SUMMARY OF THE INVENTION
[0014] One aspect of the invention provides a fast response carbon nanotubes stretch sensor. The stretch sensor includes a horizontally aligned single wall carbon nanotube layer, a flexible substrate layered on the horizontally aligned single wall carbon nanotube layer and a pair of electrodes on both the ends of the horizontally aligned single wall carbon nanotube layer. The horizontally aligned single wall carbon nanotube layer is obtained by filling a single wall carbon nanotube solution in an acid between two non flexible substrates; simultaneously pressing and pushing the upper non flexible substrate while keeping the lower non flexible substrate stationary and dipping the lower non flexible substrate layered with the single wall carbon nanotube solution in a coagulant. The response time of the carbon nanotubes stretch sensor is less than 5 milliseconds.
[0015] DETAILED DESCRIPTION OF INVENTION
[0016] The embodiments herein and the various features and advantageous details thereof are explained more fully with reference to the non-limiting embodiments that are illustrated in the accompanying drawings and detailed in the following description. Descriptions of well-known components and processing techniques are omitted so as to not unnecessarily obscure the embodiments herein. The examples used herein are intended merely to facilitate an understanding of ways in which the embodiments herein may be practiced and to further enable those of skill in the art to practice the embodiments herein. Accordingly, the examples should not be construed as limiting the scope of the embodiments herein.
[0017] The invention provides a fast response carbon nanotubes based stretch sensor. The stretch sensor includes a horizontally aligned single walled carbon nanotube layer, a flexible substrate layered on the horizontally aligned single wall carbon nanotube layer and a pair of electrodes on both the ends of the horizontally aligned single wall carbon nanotube layer. The horizontally aligned single walled carbon nanotube layer is prepared by filling a single wall carbon nanotube solution in an acid between two non flexible substrates. The upper non flexible substrate is then simultaneously pressed and pushed while the lower non flexible substrate is kept stationary. The lower non flexible substrate layered with the single wall carbon nanotube and acid solution is then dipped in a coagulant to obtain the horizontally aligned single wall carbon nanotube layer. FIG. 1 is a schematic representation of the carbon nanotubes stretch sensor, according to an embodiment of the invention. The carbon nanotubes stretch sensor includes a horizontally aligned single wall carbon nanotubes layer 101 , a flexible substrate 103 layered on the horizontally aligned single wall carbon nanotubes layer 101 and a pair of electrodes 105 on both the ends of the horizontally aligned single wall carbon nanotubes layer 101 . The horizontally aligned single wall carbon nanotubes layer 101 is obtained by filling a single wall carbon nanotube solution in an acid between two non flexible substrates. The single wall carbon nanotube solution in the acid is prepared by mixing a single wall carbon nanotube in an acid in weight percentage ranging from 1 % to 2.5%. The acid includes but is not limited to a chloro sulfonic acid (CSA), oleum, sulfuric acid, fuming sulfuric acid or a combination thereof. In one embodiment of the invention, single wall carbon nanotube solution is prepared in chlorosulfonic acid. The single wall carbon nanotube solution in chlorosulfonic acid is filled between two non flexible substrates. The non flexible substrate includes but is not limited to a glass substrate, a Teflon substrate, a quartz substrate. In one embodiment of the invention, a glass substrate is selected as the non flexible substrate. The upper non flexible substrate is then simultaneously pressed and pushed while the lower non flexible substrate is kept stationary. In one embodiment of the invention, the single wall carbon nanotube solution in CSA is filled between two glass substrates. The single wall carbon nanotube solution in CSA filled glass substrates is kept between a Polytetrafluoroethylene (PTFE) block. The upper glass substrate is then simultaneously pressed and pushed while the lower glass substrate is kept stationary. The lower glass substrate layered with single wall carbon nanotube in acid solution is then dipped in a coagulant to form a horizontally aligned single wall carbon nanotube layer. The coagulant includes but is not limited to diethyl ether, acetone, chloroform and water. In one embodiment of the invention, the lower glass substrate layered with single wall carbon nanotube in acid solution is dipped in diethyl ether bath to remove the acid and precipitate the horizontally aligned single wall carbon nanotube onto the glass substrate. The horizontally aligned single wall carbon nanotube layered on the glass substrate is dried at a temperature ranging from 20-30 °C for 24 hrs.
[0018] A flexible substrate 103 is then layered on the horizontally aligned single wall carbon nanotube layer 101. The flexible substrate includes but is not limited to polydimethylsiloxane (PDMS), polyurethane(PU) and ecoflex®. In one embodiment of the invention, polydimethylsiloxane (PDMS) is used as flexible substrate. The flexible substrate 103 is layered either by pouring the flexible substrate in liquid phase over the horizontally aligned single wall carbon nanotube layer 101 or by stamping the flexible substrate that is in semi-cured state on the horizontally aligned single wall carbon nanotube layer 101. In one embodiment of the invention, the flexible substrate 103 is layered by pouring PDMS in liquid phase over the horizontally aligned single wall carbon nanotube layer 101 on the glass substrate and allowed to cure at a temperature of 30 - 70 °C for 30 min to 2 hrs. In an alternate embodiment of the invention, the flexible substrate 103 is layered by stamping PDMS in semicured state on the horizontally aligned single wall carbon nanotube layer 101 on the glass substrate and allowed to cure at a temperature of 50-70 °C for 1 -2 hrs in vacuum. In another embodiment of the invention, the flexible substrate 103 is layered by stamping PDMS in semi-cured state on the horizontally aligned single wall carbon nanotube layer 101 on the glass substrate and allowed to cure at room temperature for 24- 48 hrs. The glass substrate is then removed to obtain a flexible substrate layered horizontally aligned carbon nanotube layer. A pair of electrodes 105 is then connected at both the ends of the horizontally aligned single wall carbon nanotube layer 101 to obtain carbon nanotube stretch sensor. In one embodiment of the invention, a spiral copper wire is attached at both the ends of the horizontally aligned single wall carbon nanotube layer 101. In one embodiment of the invention, a conductive metal epoxy is filled on the spiral copper wire and the horizontally aligned single wall carbon nanotube layer 101 and is cured at 100 °C in vacuum for 10- 12 hrs.
[0019] In one embodiment of the invention, the horizontally aligned single wall carbon nanotube layer 101 along with silver epoxy is sealed with another layer of the flexible substrate (Fig 2).
[0020] Example 1 : In one particular example of the invention, single wall carbon nanotube is mixed with chlorosulfonic acid to obtain 1 % w / v solution of single wall carbon nanotube in chlorosulfonic acid. The single wall carbon nanotube solution in chlorosulfonic acid is then filled between two glass substrates. The single wall carbon nanotube solution in chlorosulfonic acid filled glass substrates is kept between a Polytetrafluoroethylene (PTFE) block. The upper glass substrate is then simultaneously pressed and pushed while the lower glass substrate is kept stationary. The lower glass substrate layered with single wall carbon nanotube in chlorosulfonic acid solution is then dipped in di ethyl ether for coagulation and form horizontally aligned single wall carbon nanotube layer 101. The horizontally aligned single wall carbon nanotube layer 101 is then stamped with semi-cured PDMS 103 and allowed to cure at a temperature of 50-70°C for 1 -2 hrs. The glass substrate is then removed to obtain a PDMS layered horizontally aligned carbon nanotube layer. A spiral copper wire is attached at both the ends of the horizontally aligned single wall carbon nanotube layer 101 to obtain carbon nanotube stretch sensor. The obtained stretch sensor exhibits high durability for about 70,000 cycles and a fast response time of less than 5 milliseconds.
[0021] Example 2: In another example of the invention, single wall carbon nanotube is mixed with chlorosulfonic acid to obtain 2.5 % w / v solution of single wall carbon nanotube in chlorosulfonic acid. The single wall carbon nanotube solution in chlorosulfonic acid is then filled between two glass substrates. The single wall carbon nanotube solution in chlorosulfonic acid filled glass substrates is kept between a Polytetrafluoroethylene (PTFE) block. The upper glass substrate is then simultaneously pressed and pushed while the lower glass substrate is kept stationary. The lower glass substrate layered with single wall carbon nanotube in chlorosulfonic acid solution is then dipped in diethyl ether for coagulation and form horizontally aligned single wall carbon nanotube layer 101. The horizontally aligned single wall carbon nanotube layer 101 is then stamped with PDMS 103 and allowed to cure at room temperature for 24- 48 hrs. The glass substrate is then removed to obtain a flexible substrate layered horizontally aligned carbon nanotube layer. A spiral copper wire is attached at both the ends of the horizontally aligned single wall carbon nanotube layer 101 to obtain carbon nanotube stretch sensor. The obtained stretch sensor exhibits high durability for about 50,000 cycles and a fast response time of about less than 5 milliseconds.
[0022] The carbon nanotube stretch sensor is then tested for performance based on various standard parameters.
[0023] Response time: The response time of a resistive stretch sensor is the time it takes for the sensor's resistance to change in response to a change in strain. FIG.3 shows the response of the carbon nanotubes based stretch sensor with respect to time, according to an embodiment of the invention. The stretch sensor is connected in a Wheatstone bridge as one of the variable resistors to precisely measure the resistance. As the strain is applied, the resistance of the sensor changes, this change in resistance creates a voltage difference in the Wheatstone bridge and is recorded with the help of a microcontroller (data shown as sensor value). The figure shows the response of the sensor for the applied strain with time and shows the uniform behavior (repeatable) of the sensorfor multiple cycle of stretching and unstretching over the time. The obtained stretch sensor has a fast response time of less than 5 miliseconds.
[0024] Stretchability: Stretchability in resistive stretch sensors refers to the ability of the sensor to deform and recover its shape without affecting its electrical resistance. Tablei . shows the stretchability and change in resistance corresponding to the change in length.
[0025] Life Cycle:
[0026] FIG. 4 shows response of the carbon nanotubes based stretch sensorwith respectto strain, according to an embodiment of the invention. The data is plotted between the sensor value and the strain applied (the change in distance by the stretch sensor in 50 steps interval). The positive X- axis values are recorded during the stretching of the sensor and the negative X-axis values are recorded during the un-stretching of the sensor. The difference in the sensor value for a applied strain during stretching and unstretching shows hysteresis in the sensor. The plot indicates the sensor has a low hysteresis value. Further, the data plotted is for approximately 70,000 cycles and indicates that the sensor is following almost the same trajectory for all the 70,000 cycles. The plot reveals that the obtained stretch sensor has a high durability of more than 70,000 cycles.
[0027] FIG. 5 indicates the response time of the sensor, according to an embodiment of the invention. The graph shows: 1 ) The increase and decrease of the sensor length from 0% to 100% due to stretching and 2.) The resistance data collected from the sensor. Both sets of data are recorded independently. The stretch sensor is mounted on a test bench where one arm of the test bench is movable while the other arm is fixed. The test bench is then moved to a predefined distance along with the sensor. The red dots indicate the distance traveled by the test bench arm (where the sensor is held) for a predefined distance and step with the given time. The blue dots indicate the sensor value obtained as a result of the applied strain by the movement of the test bench arm. As shown(right side of the figure) for one instance, the red dot is at the 5062 ms and the corresponding blue dot is at 5065 ms indicating that the time taken by the sensorto respond to the applied strain is about 3 ms. The figure indicates that the sensor response was obtained within 5 milliseconds of the change in length. The same is repeatable.
[0028] The invention thus provides a carbon nanotube based stretch sensor that has high durability, high stretchability and a fast response time of less than 5 milliseconds. Fast response stretch sensors can detect changes in the stretch or deformation of a material almost instantaneously, making them ideal for applications that require a quick response time, such as in robotics or medical devices.
[0029] The foregoing description of the specific embodiments will so fully reveal the general nature of the embodiments herein that others can, by applying current knowledge, readily modify and / or adapt for various applications such specific embodiments without departing from the generic concept, and, therefore, such adaptations and modifications should and are intended to be comprehended within the meaning and range of equivalents of the disclosed embodiments. It is to be understood that the phraseology or terminology employed herein is for the purpose of description and not of limitation. Therefore, while the embodiments herein have been described in terms of preferred embodiments, those skilled in the art will recognize that the embodiments herein can be practiced with modification within the spirit and scope of the embodiments as described herein.
Claims
We Claim:
1. A fast response carbon nanotubes stretch sensor, the sensorcomprising : a horizontally aligned single wall carbon nanotube layer (101 ) characterized in that the layer is obtained by layering a single wall carbon nanotubes solution in an acid on a non flexible substrate; a flexible substrate (103) layered on the horizontally aligned carbon nanotube layer (101 ); and a pair of electrodes (105) on both the ends of the horizontally aligned carbon nanotube layer wherein the signal response time of the stretch sensor is less than 5 milliseconds.
2. The stretch sensor as claimed in claim 1 , wherein the horizontally aligned single wall carbon nanotube layer (101 ) on the non flexible substrate is obtained by filling the single wall carbon nanotube solution in the acid between two non flexible substrates; simultaneously pressing and pushing the upper non flexible substrate while keeping the lower non flexible substrate stationery; and dipping the lower non flexible substrate layered with the single wall carbon nanotube solution in a coagulant.
3. The stretch sensor as claimed in claim 1 , wherein the solution of single wall carbon nanotube in the acid is prepared by mixing single wall carbon nanotube in acid wherein the concentration of the single wall carbon nanotube ranges from 1 % to 2.5 % w / v of the acid.
4. The stretch sensor as claimed in claim 1 , wherein the acid is selected from chloro sulfonic acid, oleum, sulfuric acid, fuming sulfuric acid or a combination thereof.
5. The stretch sensor as claimed in claim 1 , wherein the nonflexible substrate is a glass substrate, a teflon substrate or a quartz substrate.
6. The stretch sensor as claimed in claim 1 , wherein the coagulant is diethyl ether, acetone, chloroform or water.
7. The stretch sensor as claimed in claim 1 , wherein the flexible substrate (103) is polydimethylsiloxane, polyurethane, or ecoflex.
Citation Information
Patent Citations
Strain sensor
US20140331793A1