Carbon fiber bundle and method for producing carbon fiber bundle
The carbon fiber bundle with a controlled diameter and untwisted, unentangled structure, combined with precise manufacturing processes, achieves high strand strength and elastic modulus, addressing the challenges of previous methods and improving the mechanical properties of carbon fiber reinforced composites.
Patent Information
- Application Number
- PCT/JP2023/017522
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-05-10
- Publication Date
- 2024-11-14
AI Technical Summary
Existing carbon fiber bundles face challenges in achieving high strand strength and strand elastic modulus simultaneously, with previous methods either reducing productivity, causing fiber buckling, or resulting in insufficient resin impregnation, which affects the mechanical properties of carbon fiber reinforced composite materials.
A carbon fiber bundle with an average diameter of 5.7 μm to 6.5 μm and a substantially untwisted, unentangled structure, combined with specific heating and stretching processes, to achieve strand strengths of 4.7 GPa or more and strand elastic moduli of 320 GPa or more, while maintaining balanced physical properties.
The resulting carbon fiber bundle exhibits high strand strength, strand elastic modulus, and balanced physical properties, enhancing the mechanical performance of carbon fiber reinforced composite materials, particularly in applications requiring high bending strength and reduced weight.
Smart Images

Figure JPOXMLDOC01-APPB-T000001 
Figure JPOXMLDOC01-APPB-T000002 
Figure JPOXMLDOC01-APPB-T000003
Abstract
Description
Carbon fiber bundle and method for producing carbon fiber bundle
[0001] The present invention relates to a carbon fiber bundle and a method for producing a carbon fiber bundle.
[0002] To improve the mechanical properties of resin-based molded products, it is common to combine resins with fibers as reinforcing materials. Carbon fibers, among other materials, have excellent specific strength and specific modulus, and are lightweight. As a reinforcing fiber for high-performance resins, they are used in a wide range of applications, including aerospace and automotive applications, in addition to traditional sports and general industrial applications. In recent years, the advantages of carbon fiber-reinforced composite materials, which are obtained by integrating carbon fibers as reinforcing fibers with matrix resins, have become increasingly apparent, leading to growing demand for improved performance in carbon fiber-reinforced composite materials, particularly in automotive and aerospace applications.
[0003] These carbon fiber reinforced composite materials are formed, for example, from prepregs, which are intermediate products in which carbon fibers are impregnated with a matrix resin, through molding and processing steps such as heating and pressurization. In order to achieve high tensile strength in carbon fiber reinforced composite materials when combining carbon fibers with a matrix resin, the strand strength and strand modulus of the carbon fiber itself have been improved by reducing the diameter of the carbon fiber single fibers. Furthermore, it is important to increase the impregnation of the matrix resin into the carbon fiber bundles and suppress the generation of voids in the carbon fiber reinforced composite material.
[0004] Attempts have been made to obtain carbon fiber bundles that have high strand strength and strand modulus and also have excellent resin impregnation. Patent Document 1 describes carbon fibers that are obtained by twisting the fiber bundles in a flame-proofing process during the process of producing the carbon fiber bundles, thereby achieving excellent strand modulus while also being moldable into composite materials, and that easily maintain fiber length even when used as discontinuous fibers. Patent Document 2 describes carbon fiber bundles that are carbonized under high drawing tension in the carbonization process, thereby achieving both high levels of strand modulus and high levels of compressive strength of carbon fiber composite materials. Patent Document 3 describes a technology for increasing the strand strength and adhesive strength of carbon fibers by subjecting carbon fibers to an electrolytic surface treatment in an electrolyte solution having a specific range of nitrate ion concentration.
[0005] International Publication No. 2019 / 244830 International Publication No. 2019 / 203088 Japanese Patent Application Laid-Open No. 2002-327339
[0006] Through detailed studies by the present inventors, it has been found that Patent Documents 1 to 3 have the following problems. The carbon fiber bundles described in Patent Document 1 are produced by adding twisting, which not only reduces productivity due to an increase in the number of steps, but also causes excessive bundling in the fiber bundles, so that the carbon fibers remain helical even after untwisting after baking. Therefore, if the long fibers are used as they are, the impregnation with resin may be insufficient, or when they are made into a composite material with a matrix resin, the carbon fibers are prone to buckling when compressed in the fiber axis direction, resulting in low compressive strength in the fiber axis direction.
[0007] The carbon fiber bundles described in Patent Document 2 have a relatively large single fiber diameter. Among these, the carbon fibers with a smaller single fiber diameter are subjected to a strong entanglement treatment of the carbon fiber precursor fiber bundle in order to be carbonized at a high drawing tension. The strong entanglement treatment improves the bundle strength of the fiber bundle, resulting in less fuzz generation even when the drawing tension in the carbonization treatment is increased. However, due to the strong entanglement, the resulting carbon fiber bundle has insufficient resin impregnation. Furthermore, among these, the carbon fibers with a larger single fiber diameter are twisted to enable carbonization at a high drawing tension, resulting in carbon fibers with high strand strength and strand modulus. However, twisted carbon fiber bundles have poor matrix resin impregnation, resulting in poor mechanical properties of carbon fiber-reinforced composite materials, and the helical state remains even after untwisting, making the carbon fibers prone to buckling when the carbon fiber-reinforced composite material is compressed, resulting in low compressive strength.
[0008] The carbon fiber described in Patent Document 3 includes measurement results of strand strength and strand modulus, but because the measurements were performed using the old JIS method (JIS R-7601), the values are higher than those of the current JIS method (JIS R-7608:2007).In addition, Patent Document 3 does not describe a fiber having a good balance between strand strength and strand modulus, as in the present invention.
[0009] Furthermore, the market is demanding carbon fiber bundles with higher strand strength and strand modulus than ever before, but generally, increasing strand strength tends to decrease strand modulus, and vice versa. Thus, improving strand strength and improving strand modulus are contradictory, and it has been difficult to improve both physical properties.
[0010] Furthermore, with the recent advances in the development of flying cars and large drones, products using carbon fiber reinforced composite materials need to be even lighter. To reduce weight, carbon fiber reinforced composite materials need to be made thinner without reducing their bending strength. When a carbon fiber reinforced composite material is bent, tensile stress occurs on the outside of the bend and compressive stress occurs on the inside of the bend. This requires increasing the strand strength of the carbon fiber and the compressive strength in the fiber axis direction. The compressive strength of carbon fiber in the fiber axis direction depends on the modulus of elasticity and the diameter of the single fiber, so carbon fiber with a large single fiber diameter and a high modulus of elasticity is required.
[0011] The present invention has been made to solve the above problems, and an object of the present invention is to provide a carbon fiber bundle having well-balanced physical properties, such as high strand modulus and strand strength, even when the average diameter of the carbon fiber single fibers is large, and a method for producing the same.
[0012] The present invention has the following aspects. [1] A carbon fiber bundle having an average diameter of carbon fiber single fibers of 5.7 μm or more and 6.5 μm or less, which is substantially untwisted, and which has a strand strength of 4.7 GPa or more and a strand modulus of 320 GPa or more. [2] The carbon fiber bundle of [1] which is unentangled. [3] The carbon fiber bundle of [1] or [2], in which the average void length of the carbon fiber single fibers is 22.0 nm or less. [4] The carbon fiber bundle of any of [1] to [3], in which the crystallite size Lc of the carbon fiber single fibers is 3.7 nm or less. [5] The carbon fiber bundle of any of [1] to [4], in which the product of the strand strength (unit: GPa) and the strand modulus (unit: GPa) is 1650 or more. [6] The carbon fiber bundle according to any one of [1] to [5], having a strand strength of 4.9 GPa or more and a strand modulus of 385 GPa or more. [7] The carbon fiber bundle according to any one of [1] to [6], having a strand modulus of 390 GPa or more and 420 GPa or less. [8] The carbon fiber bundle according to any one of [1] to [7], having a strand strength of 5.4 GPa or more. [9] The knot strength is 400 N / mm 2
[10] The carbon fiber bundle according to any one of [1] to [8], wherein the knot strength is 415 N / mm or more. 2
[11] The carbon fiber bundle of any of [1] to
[10] , having a fracture surface generation energy of 19 N / m or more.
[12] The carbon fiber bundle of any of [1] to
[10] , having a fracture surface generation energy of 20.5 N / m or more.
[13] The carbon fiber bundle of any of [1] to
[10] , having a density of 1.79 g / cm 3
[14] A method for producing a carbon fiber bundle, comprising heating a carbon fiber precursor acrylic fiber bundle in an oxidizing atmosphere to form a flame-resistant fiber bundle, and heating the flame-resistant fiber bundle in a non-oxidizing atmosphere to form a carbon fiber bundle, wherein, in the heating in the non-oxidizing atmosphere, the temperature is increased from 1800°C to 2200°C at a rate of 200 to 500°C / min, and the average diameter of single carbon fibers contained in the obtained carbon fiber bundle is 6.5 μm or more and 8.5 μm or less.
[15] The method for producing a carbon fiber bundle according to
[14] , wherein the carbon fiber precursor acrylic fiber bundle and the flame-resistant fiber bundle are heated in an unentangled state.
[16] The method for producing a carbon fiber bundle according to
[14] or
[15] , wherein the carbon fiber precursor acrylic fiber bundle and the flame-resistant fiber bundle are heated in a substantially untwisted state.
[17] A method for producing a carbon fiber bundle according to any one of
[14] to
[16] , comprising the following steps (1) and (2): (1) a coagulation step in which an acrylonitrile-based polymer solution is extruded into air from an extrusion hole by using a dry-wet spinning method, and then coagulated in a coagulation bath containing an aqueous solution of an organic solvent at a temperature of 10°C or less and an organic solvent concentration of 79.3% by mass or more and 82.0% by mass or less to obtain a coagulated fiber bundle containing the organic solvent; (2) a second drawing step in which the coagulated fiber bundle obtained in the coagulation step is drawn at a draw ratio of 2.0 to 3.2 times in a warm aqueous solution at a temperature of 75°C or more and an organic solvent concentration of 40 to 65% by mass or less to obtain the carbon fiber precursor acrylic fiber bundle; and
[18] a method for producing a carbon fiber bundle according to any one of
[14] to
[17] , comprising, between the coagulation step and the second drawing step, a first drawing step in which the coagulated fiber bundle obtained in the coagulation step is drawn in air at a draw ratio of 1.00 to 1.20 times.
[19] The method for producing a carbon fiber bundle according to any one of
[14] to
[18] , wherein, in the second drawing step, after drawing the coagulated fiber bundle, the organic solvent is removed, and the coagulated fiber bundle is shrunk or drawn in warm water at a temperature of 90°C or higher at a draw ratio of 0.96 to 1.30, and then drawn in a pressurized water vapor atmosphere at a draw ratio of 3.7 to 4.2 to obtain the carbon fiber precursor acrylic fiber bundle.
[20] The method for producing a carbon fiber bundle according to any one of
[14] to
[19] , wherein a concentration of the organic solvent in the aqueous solution used in the coagulation step is 79.8 mass% or more and 81.2 mass% or less.
[21] The method for producing a carbon fiber bundle according to any one of
[14] to
[20] , wherein the organic solvent is dimethylformamide.
[22] The method for producing a carbon fiber bundle according to any one of
[14] to
[21] , comprising the following steps (3) to (6): (3) a flame-resistant step of heating a carbon fiber precursor acrylic fiber bundle or a carbon fiber precursor acrylic fiber bundle obtained in the second drawing step in an oxidizing atmosphere to obtain a flame-resistant fiber bundle. (4) a first carbonization step of heating the flame-resistant fiber bundle obtained in the flame-resistant step in a non-oxidizing atmosphere having a temperature gradient in an atmosphere temperature range of 300°C to 900°C at an elongation rate of 4.0% to 5.0%. (5) a second carbonization step of heating the fiber bundle after the first carbonization step in a non-oxidizing atmosphere having a temperature gradient in an atmosphere temperature range of 1000°C to 1800°C while applying a tension of 0.15 cN / dtex to the fiber bundle. (6) A third carbonization step, after the second carbonization step, of heating the fiber bundle while applying a tension of 0.15 cN / dtex or more and 0.23 cN / dtex or less to the fiber bundle in a non-oxidizing atmosphere having a temperature gradient in an atmospheric temperature range of 1700° C. or more and 2300° C.
[23] The flame-proofing step comprises heating the acrylic precursor fiber bundle of carbon fiber or the acrylic precursor fiber bundle of carbon fiber obtained in the second drawing step in an oxidizing atmosphere having a temperature gradient in an atmospheric temperature range of 220° C. or more and 280° C. at an elongation rate of 3.0% or more and 8.0% or less, and stretching the acrylic precursor fiber bundle to a density of 1.33 g / cm. 3 1.36g / cm or more 3 The method for producing a carbon fiber bundle according to
[22] , which is a step of obtaining the following flame-resistant fiber bundle:
[24] The method for producing a carbon fiber bundle according to
[22] or
[23] , wherein the difference between the maximum atmospheric temperature in the second carbonization step and the inlet atmospheric temperature in the third carbonization step is 700°C or less.
[25] The method for producing a carbon fiber bundle according to
[22] or
[23] , wherein the difference between the maximum atmospheric temperature in the second carbonization step and the inlet atmospheric temperature in the third carbonization step is 500°C or less.
[26] The method for producing a carbon fiber bundle according to any of
[14] to
[25] , wherein the maximum heating temperature in the heating in a non-oxidizing atmosphere is 2100 to 2300°C.
[0013] According to the present invention, it is possible to provide a carbon fiber bundle having well-balanced physical properties, such as high strand modulus and strand strength, even when the average diameter of the carbon fiber single fibers is large, and a method for producing the same. According to the present invention, it is possible to obtain a carbon fiber bundle suitable for a thin carbon fiber reinforced composite material having excellent bending strength.
[0014] FIG. 2 is an explanatory diagram illustrating a method for measuring the ultrasonic elastic modulus of a carbon fiber bundle.
[0015] [Carbon fiber bundle] The carbon fiber bundle of the present invention has an average diameter of carbon fiber single fibers of 5.7 μm or more and 6.5 μm or less, is substantially untwisted, has a strand strength of 4.7 GPa or more, and has a strand modulus of 320 GPa or more. Note that the term "carbon fiber bundle" means a bundle of a plurality of carbon fiber single fibers.
[0016] In the carbon fiber bundle of the present invention, the average diameter of the carbon fiber single fibers, i.e., the fiber diameter, is 5.7 μm or more and 6.5 μm or less. By setting the fiber diameter to 5.7 μm or more, it is possible to increase the gaps between the fibers, making it easier to uniformly impregnate the resin, and making it possible to suppress the generation of voids in the carbon fiber reinforced composite material obtained using the carbon fiber bundle of the present invention. By setting the fiber diameter to 6.5 μm or less, a cross-sectional double structure is less likely to become noticeable in the flame-proofing step (step (3)) described below, and it is easy to obtain a carbon fiber bundle with high strand strength without reducing the strand modulus. In order to achieve both uniformity of resin impregnation and high strand strength, the fiber diameter is preferably 5.7 μm or more and less than 6.5 μm, more preferably 5.8 μm or more and 6.4 μm or less, and even more preferably 5.9 μm or more and 6.3 μm or less. The measurement conditions for the average diameter of the carbon fiber single fibers are as described in the Examples described below. The strand strength is the strand tensile strength obtained by a tensile test, and the strand modulus is the strand tensile modulus obtained by a tensile test.
[0017] The carbon fiber bundle of the present invention is substantially untwisted. In the present invention, "substantially untwisted" means that there is no twist in the fiber bundle, or that there is localized twist, but S twist and Z twist are present equally. When S twist and Z twist are present equally in the fiber bundle, it is preferable that the net twist number in the entire carbonization process is 0.5 turns / m or less. When the carbon fiber bundle is substantially untwisted, the carbon fiber bundle has good openability, which makes it easier to improve the performance of the obtained carbon fiber reinforced composite material. It is also possible to include carbon fibers that are untwisted by performing baking in a twisted state. However, when untwisted, the carbon fibers are in a helical state, and when formed into a composite material with a matrix resin, they are prone to buckling when compressed, and the compressive strength in the fiber direction is likely to be low. From this point of view, it is preferable that the carbon fibers have straightness.
[0018] The compressive strength in the fiber direction can be measured by the following method.
[0019] [Method for measuring compressive strength in the fiber axis direction of a carbon fiber reinforced composite material] (Production of prepreg) A carbon fiber bundle unwound from a bobbin was placed on a release paper coated with epoxy resin #350 (manufactured by Mitsubishi Chemical Corporation) and impregnated with the epoxy resin. A protective film was then laminated on top of the carbon fiber bundle, resulting in a prepreg with a resin content of approximately 33% by mass and a carbon fiber density of 125 g / m. 2 A unidirectionally oriented prepreg (hereinafter referred to as "prepreg") is prepared.
[0020] (Production of unidirectional laminate material) Two plies of prepreg are laminated and bagged, and the pressure inside the bag is reduced using a vacuum pump. The resulting material is then placed in an autoclave, where the temperature is increased at a rate of 2°C / min, held at 80°C for 1 hour, then increased at a rate of 2°C / min, and held at 130°C for 1.5 hours to cure the material, yielding a carbon fiber reinforced composite material. The pressure inside the autoclave is increased to 0.6 MPa after being held at 80°C for 1 hour. The vacuum pump is stopped when the pressure inside the autoclave reaches 0.14 MPa, and the bag is opened to the atmosphere.
[0021] <Evaluation of Compressive Properties in the Fiber Axis Direction of Carbon Fiber Resin Composite Material> Six test specimens measuring 12.7 mm wide, 80 mm long, and 1 mm thick were prepared from the resulting unidirectional laminate. The length direction of the test specimen was the 0° fiber direction. The resulting test specimens were measured for compressive strength and compressive modulus in the fiber axis direction using an INSTRON 5882 measuring instrument equipped with a 100 kN load cell in accordance with SACMA SRM 1R at a temperature of 23°C, humidity of 50%, and a crosshead speed of 1.27 mm / min. The measured values were converted to a Vf (fiber volume fraction) of 56%. The same measurements were performed on six test specimens, and the average value was calculated. The measurements were performed by attaching tabs cut from the same plate to each test specimen.
[0022] The carbon fiber bundle of the present invention has a strand strength of 4.7 GPa or more and a strand modulus of 320 GPa or more. By setting the strand strength of the carbon fiber bundle to 4.7 GPa or more and the strand modulus to 320 GPa or more, a carbon fiber bundle with a balanced strand strength and strand modulus is obtained, making it easier to obtain a carbon fiber reinforced composite material with excellent mechanical properties. From these viewpoints, the lower limit of the strand strength is preferably 4.9 GPa or more, and more preferably 5.1 GPa or more. There is no particular restriction on the upper limit of the strand strength, but in terms of the balance with the strand modulus, it is preferably 6.5 GPa or less, and more preferably 6.0 GPa or less. The above upper and lower limits can be combined arbitrarily. For example, it may be 4.7 GPa or more and 6.5 GPa or less, 4.9 GPa or more and 6.5 GPa or less, or 5.1 GPa or more and 6.0 GPa or less. The lower limit of the strand elastic modulus is preferably 370 GPa or more, more preferably 380 GPa or more, and even more preferably 390 GPa or more. There is no particular restriction on the upper limit of the strand elastic modulus, but in consideration of the balance with strand strength, it is preferably 450 GPa or less, more preferably 420 GPa or less. The above upper and lower limits can be combined arbitrarily. For example, it may be 320 GPa or more and 450 GPa or less, 370 GPa or more and 450 GPa or less, 380 GPa or more and 420 GPa or less, or 390 GPa or more and 420 GPa or less. The measurement conditions for strand strength and strand elastic modulus are as described in the examples below.
[0023] The carbon fiber bundle of the present invention is preferably unentangled. "Unentangled" here means intentional entanglement using an entanglement device. Single fibers that naturally become entangled during the carbon fiber manufacturing process are considered unentangled. When the carbon fiber bundle is unentangled, the carbon fiber bundle has good openability when made into a carbon fiber reinforced composite material, and the impregnation with the matrix resin is likely to be good, making it easier to obtain a carbon fiber reinforced composite material with excellent mechanical properties. In this case, the hook drop value of the carbon fiber bundle is 500 mm or more, and preferably 1000 mm or more.
[0024] The hook drop value is measured by the following method. First, a 2000 mm carbon fiber bundle is arranged vertically and its upper end is fixed. Next, a hook with a total weight of 30 g and a weight attached is inserted into the carbon fiber bundle 1. The hook used here is made by molding a metal wire with a diameter of 1 mm, and the radius of the hook portion is 5 mm. Next, the hook is allowed to fall freely while still inserted into the carbon fiber bundle. As described above, a carbon fiber bundle is a thread in which many carbon fiber monofilaments are drawn in approximately the same direction and integrated with a sizing agent or the like. However, the carbon fiber monofilaments are often entangled at some point. The hook often stops at such a point. Therefore, the distance from the position where the hook was inserted into the carbon fiber bundle to the position where the hook stops can be measured. The falling distance of the hook from the insertion position to the stop position is the hook drop value.
[0025] In the carbon fiber bundle of the present invention, the average void length of the carbon fiber single fibers is preferably 22.0 nm or less. If the average void length of the carbon fiber bundle is 22.0 nm or less, the strand strength of the carbon fiber bundle is more likely to be maintained at a high level. From this viewpoint, it is more preferably 21.0 nm or less, and even more preferably 19.5 nm or less. If the lower limit of the average void length is 5.0 nm or more, the flexibility of the fiber is easily ensured, and it is more preferably 10 nm or more. The above upper and lower limits can be arbitrarily combined. For example, it may be 5.0 nm or more and 22.0 nm or less, 5.0 nm or more and 21.0 nm or less, or 10 nm or more and 19.5 nm or less. The average void length can be controlled by adjusting the heating temperature and temperature rise rate when the flame-resistant fiber bundle is heated for carbonization treatment. The measurement conditions for the average void length are as described in the Examples below.
[0026] In the carbon fiber bundle of the present invention, the crystallite size Lc of the carbon fiber single fibers is preferably 3.7 nm or less. If the crystallite size Lc of the carbon fiber bundle is 3.7 nm or less, it is easy to suppress the formation of defects and the decrease in strand strength of the carbon fiber bundle caused by the crystallite size of the carbon fiber becoming too large. From this viewpoint, the crystallite size Lc is more preferably 3.6 nm or less, and even more preferably 3.4 nm or less. Furthermore, the lower limit of the crystallite size Lc is preferably 3.0 nm or more, more preferably 3.1 nm or more, in order to obtain a high strand modulus. The above upper and lower limits can be arbitrarily combined. For example, it may be 3.0 nm or more and 3.7 nm or less, 3.0 nm or more and 3.6 nm or less, or 3.1 nm or more and 3.4 nm or less. The crystallite size Lc can be controlled by adjusting the heating temperature and temperature rise rate when the flame-resistant fiber bundle is heated for carbonization treatment. The measurement conditions for the crystallite size Lc are as described in the Examples below.
[0027] The carbon fiber bundle of the present invention preferably has a product of strand strength (unit: GPa) and strand modulus (unit: GPa) of 1650 or more. By setting the product of strand strength and strand modulus to 1650 or more, a carbon fiber bundle with a better balance between strand strength and strand modulus can be obtained, making it easier to obtain a carbon fiber reinforced composite material with better mechanical properties. The product of strand strength and strand modulus is more preferably 1700 or more, more preferably 1750 or more, and even more preferably 2000 or more. Furthermore, the product of strand strength and strand modulus is preferably 3000 or less, more preferably 2500 or less. The above upper and lower limits can be combined arbitrarily. For example, it may be 1650 or more and 3000 or less, 1700 or more and 3000 or less, 1750 or more and 2500 or less, or 2000 or more and 2500 or less.
[0028] From the viewpoint of the performance of the carbon fiber reinforced composite material to be obtained, the carbon fiber bundle of the present invention preferably has a strand strength of 4.9 GPa or more. From the viewpoint of the performance of the carbon fiber reinforced composite material to be obtained, the carbon fiber bundle of the present invention preferably has a strand modulus of 385 GPa or more. From the viewpoint of the performance of the carbon fiber reinforced composite material to be obtained, the carbon fiber bundle of the present invention may have a strand strength of 4.9 GPa or more and a strand modulus of 385 GPa or more.
[0029] The carbon fiber bundle of the present invention preferably has a strand modulus of 390 GPa or more and 420 GPa or less. By setting the strand modulus of the carbon fiber bundle to 390 GPa or more, the performance of the obtained carbon fiber reinforced composite material is likely to be further improved. Furthermore, by setting the strand modulus to 420 GPa or less, it is possible to prevent the graphite crystal size of the carbon fiber bundle from becoming excessively large and to prevent a decrease in compressive strength in the fiber axis direction, so it is likely to be possible to further improve the performance of the obtained carbon fiber reinforced composite material.
[0030] The carbon fiber bundle of the present invention preferably has a strand strength of 5.4 GPa or more. By making the strand strength of the carbon fiber bundle 5.4 GPa or more, the performance of the obtained carbon fiber reinforced composite material is likely to be improved. From these viewpoints, the strand strength of the carbon fiber bundle of the present invention is 4.7 GPa or more, preferably 4.9 GPa or more, more preferably 5.0 GPa or more, even more preferably 5.4 GPa or more, and particularly preferably 5.5 GPa or more. On the other hand, if the strand strength of the carbon fiber bundle is high, graphite crystals tend to develop, and the compressive strength in the fiber axis direction tends to decrease. In order to obtain a carbon fiber bundle having a good balance between the strand strength and the compressive strength in the fiber axis direction, the strand strength of the carbon fiber bundle is preferably 8.0 GPa or less, more preferably 7.5 GPa or less, even more preferably 7.0 GPa or less, particularly preferably 6.5 Pa or less, and most preferably 6.0 Pa or less. The above upper and lower limits can be combined arbitrarily. For example, it may be 4.7 GPa or more and 8.0 GPa or less, 4.9 GPa or more and 7.5 GPa or less, 5.0 GPa or more and 7.0 GPa or less, 5.4 GPa or more and 6.5 Pa or less, or 5.5 GPa or more and 6.0 Pa or less.
[0031] The carbon fiber bundle of the present invention has a knot strength of 400 N / mm 2 It is preferable that the knot strength is equal to or greater than 400 N / mm. The knot strength can be an index that reflects the mechanical performance of the fiber bundle in directions other than the fiber axis, and can easily evaluate performance in directions perpendicular to the fiber axis, in particular. Carbon fiber reinforced composite materials are often formed by quasi-isotropic lamination, which creates a complex stress field. In this case, in addition to tensile stress in the fiber axis direction and compressive stress in the fiber axis direction, stresses other than those in the fiber axis direction are also generated. Furthermore, when a relatively high-speed strain is applied, such as in an impact test, the stress state generated inside the material is quite complex, and strength in directions other than the fiber axis direction becomes important. Therefore, it is recommended to set the knot strength of the carbon fiber bundle to 400 N / mm. 2 By setting the knot strength of the carbon fiber bundle to 415 N / mm or more, it is easy to improve the performance of the obtained carbon fiber reinforced composite material. 2More preferably, it is 430 N / mm or more. 2 On the other hand, when the knot strength of the carbon fiber bundle is increased, the compressive strength in directions other than the fiber axis direction also increases, and the graphite crystal size tends to become smaller, resulting in a decrease in the modulus of elasticity. In order to obtain a carbon fiber bundle with a good balance between the strand modulus of elasticity and the knot strength, the knot strength of the carbon fiber bundle is preferably 600 N / mm 2 Preferably, it is 550 N / mm or less. 2 More preferably, it is 500 N / mm or less. 2 The upper and lower limits can be arbitrarily combined. 2 More than 600N / mm 2 may be less than or equal to 415 N / mm 2 550N / mm or more 2 may be less than or equal to 430 N / mm 2 More than 500N / mm 2 The conditions for measuring the knot strength are as described in the Examples below.
[0032] In the carbon fiber bundle of the present invention, the fracture surface generation energy is preferably 19 N / m or more. The fracture surface generation energy is determined by forming a hemispherical defect having a predetermined size range on the surface of a single fiber with a laser, breaking the fiber at the hemispherical defect site in a tensile test, and then using the following Griffith equation (F1) from the breaking strength of the fiber and the depth of the hemispherical defect: fracture surface generation energy = σ 2πC / 2E ... (F1) where σ is the breaking strength, E is the ultrasonic modulus of the carbon fiber bundle, and C is the depth of the hemispherical defect. The fracture initiation energy is an index of the resistance of the carbon fiber to breakage and represents the matrix strength. Carbon fiber is a material that exhibits brittle fracture, and its tensile strength is governed by defects. When carbon fibers have the same defects, the higher the matrix strength, the higher the fracture strength. Therefore, by setting the fracture surface initiation energy of the carbon fiber bundle to 19 N / m or more, it becomes easier to increase the strength without reducing the elastic modulus of the carbon fiber bundle, and it becomes easier to improve the performance of the resulting carbon fiber reinforced composite material. From these viewpoints, it is more preferable that the fracture surface initiation energy of the carbon fiber bundle is 20.5 N / m or more. On the other hand, when the fracture surface initiation energy of the carbon fiber bundle is high, the strength of the single fiber surface constituting the carbon fiber bundle increases, the graphite crystal size increases, and as a result, the compressive strength in the fiber axis direction tends to decrease. In order to obtain a carbon fiber bundle having a good balance between fracture surface generation energy and compressive strength in the fiber axis direction, the fracture surface generation energy of the carbon fiber bundle is preferably 30 N / m or less, more preferably 25 N / m or less. The above upper and lower limits can be arbitrarily combined. For example, it may be 19 N / m or more and 30 N / m or less, or 20.5 N / m or more and 25 N / m or less. The measurement conditions for the fracture surface generation energy are as described in the examples below.
[0033] The carbon fiber bundle of the present invention has a density of 1.79 g / cm 3 It is preferable that the density of the carbon fiber bundle is 1.79 g / cm or more. 3 From this viewpoint, the density of the carbon fiber bundle is 1.81 g / cm or more, and the strand strength and strand modulus are likely to be increased. 3 More preferably, 1.83 g / cm 3 The density of the carbon fiber bundle is more preferably 1.90 g / cm 3 Preferably, 1.88 g / cm or less 3 More preferably, 1.86 g / cm 3 The density of the carbon fiber bundle is more preferably 1.90 g / cm 3If the carbon fiber density is 1.79 g / cm or less, it is easy to prevent the graphite crystal size of the carbon fiber bundle from becoming excessively large, and it is easy to prevent a decrease in compressive strength in the fiber axis direction, so that the performance of the obtained carbon fiber reinforced composite material is easy to be further improved. The above upper and lower limits can be arbitrarily combined. For example, 1.79 g / cm 3 1.90g / cm or more 3 or less, 1.81 g / cm 3 1.88g / cm or more 3 or less, 1.83 g / cm 3 1.86g / cm or more 3 The density may be measured under the following conditions: The density may be measured under the following conditions:
[0034] [Method for producing carbon fiber bundle] The method for producing carbon fibers of the present invention is a method for producing a carbon fiber bundle by heating a carbon fiber precursor acrylic fiber bundle in an oxidizing atmosphere to form a flame-resistant fiber bundle, and heating the obtained flame-resistant fiber bundle in a non-oxidizing atmosphere to form a carbon fiber bundle, wherein, at the temperature for heating in the non-oxidizing atmosphere, the atmospheric temperature is raised from 1800°C to 2200°C at a temperature rise rate of 200 to 500°C / min, and the average diameter of carbon fiber single fibers is 6.5 μm or more and 8.5 μm or less. That is, the method for producing carbon fibers of the present invention is a method for producing a carbon fiber bundle including heating a carbon fiber precursor acrylic fiber bundle in an oxidizing atmosphere to form a flame-resistant fiber bundle, and heating the flame-resistant fiber bundle in a non-oxidizing atmosphere to form a carbon fiber bundle, wherein, in the heating in the non-oxidizing atmosphere, the temperature rise rate is 200 to 500°C / min to form a flame-resistant fiber bundle, and the average diameter of carbon fiber single fibers contained in the obtained carbon fiber bundle is 6.5 μm or more and 8.5 μm or less. By setting the temperature increase rate when the atmospheric temperature is increased from 1800°C to 2200°C to 200°C or more to 200°C / min, it is easy to produce a carbon fiber bundle with high productivity. By setting the temperature increase rate when the atmospheric temperature is increased from 1800°C to 2200°C to 500°C / min or less, it is easy to suppress a violent decomposition reaction that accompanies a sudden temperature increase, and it is easy to obtain a carbon fiber bundle having a high density, strand strength, and knot strength without reducing the strand modulus of the carbon fiber bundle having an average diameter of carbon fiber single fibers of 6.5 μm to 8.5 μm. From these viewpoints, the lower limit of the temperature increase rate when the atmospheric temperature is increased from 1800°C to 2200°C is preferably 210°C / min or more, more preferably 215°C / min or more, and most preferably 220°C / min. Furthermore, the upper limit of the temperature increase rate is preferably 490°C / min or less, more preferably 480°C / min or less, and most preferably 470°C / min or less. The above upper and lower limits can be combined arbitrarily. For example, the temperature may be 210 to 490°C / min, 215 to 480°C / min, or 220 to 470°C / min. The temperature rise rate when the atmospheric temperature is raised from 1800°C to 2200°C is the travel time of the fiber bundle at an atmospheric temperature of 1800°C to 2200°C divided by 400°C, which is the difference between 2200°C and 1800°C.
[0035] The carbon fiber precursor acrylic fiber bundle and the flame-resistant fiber bundle are preferably heated in an untangled state. By heating the fiber bundle in an untangled state, each single fiber of the fiber bundle is easily flame-resistant uniformly, and strand strength and strand strength are easily increased.
[0036] The carbon fiber precursor acrylic fiber bundle and the flame-resistant fiber bundle are preferably heated in a substantially untwisted state. By heating the fiber bundle in a substantially untwisted state, each single fiber of the fiber bundle is easily flame-resistant uniformly, and strand strength is easily increased.
[0037] The method for producing a carbon fiber of the present invention preferably includes the following steps (1) to (2). The method for producing a carbon fiber of the present invention preferably includes the following steps (3) to (6). The method for producing a carbon fiber of the present invention preferably includes the following steps (1) to (6).
[0038] (1) a coagulation step in which an acrylonitrile-based polymer solution is extruded into air from an extrusion hole by using a dry-wet spinning method, and then coagulated in a coagulation bath containing an aqueous solution of an organic solvent at a temperature of 10° C. or lower and having a concentration of 79.3% by mass or more and 82.0% by mass or less to obtain a coagulated fiber bundle containing the organic solvent. (2) a second drawing step in which the coagulated fiber bundle obtained in the coagulation step (1) is drawn at a draw ratio of 2.0 to 3.2 times in a warm aqueous solution at a temperature of 75° C. or higher and having a concentration of an organic solvent at a temperature of 40% by mass or more and 65% by mass or less to obtain a carbon fiber precursor acrylic fiber bundle.
[0039] (3) a flame-resistant step of heating a carbon fiber precursor acrylic fiber bundle or the carbon fiber precursor acrylic fiber bundle obtained in the second drawing step of (2) in an oxidizing atmosphere to obtain a flame-resistant fiber bundle. (4) a first carbonization step of heating the flame-resistant fiber bundle obtained in the flame-resistant step of (3) in a non-oxidizing atmosphere having a temperature gradient in an atmosphere temperature range of 300°C to 900°C at an elongation rate of 4.0% to 5.0%. (5) a second carbonization step of heating the fiber bundle after the first carbonization step of (4) in a non-oxidizing atmosphere having a temperature gradient in an atmosphere temperature range of 1000°C to 1800°C while applying a tension of 0.15 cN / dtex to the fiber bundle and 0.21 cN / dtex to the fiber bundle. (6) After the second carbonization step (5), a third carbonization step of heating the fiber bundle while applying a tension of 0.15 cN / dtex or more and 0.23 cN / dtex or less to the fiber bundle in a non-oxidizing atmosphere having a temperature gradient in an atmospheric temperature range of 1700°C or more and 2300°C or less.
[0040] <Coagulation Step> The coagulation step (1) is a step in which an acrylonitrile polymer solution is extruded into the air from an extrusion hole using a dry-wet spinning method, and then coagulated in a coagulation bath containing an aqueous solution (A) having an organic solvent concentration of 79.3% by mass or more and 82.0% by mass or less at a temperature of 10°C or less to obtain a coagulated fiber bundle containing the organic solvent. The temperature of the coagulation bath, i.e., the aqueous solution (A), is 10°C or less. By maintaining the temperature of the aqueous solution (A) at 10°C or less, dense coagulated fibers are easily formed, and the density of the fiber surface in particular can be increased, making it easy to obtain a carbon fiber bundle with high strand strength and knot strength without reducing the strand modulus. The temperature of the aqueous solution (A) is preferably 4°C or higher, more preferably 6°C or higher. By maintaining the temperature of the aqueous solution (A) at 4°C or higher, excessive densification of the coagulated fiber can be suppressed, making it easy to ensure stretchability in subsequent steps. For example, the temperature of the aqueous solution (A) may be 4 to 10°C, or 6 to 10°C.
[0041] The concentration of the organic solvent in the coagulation bath, i.e., the aqueous solution (A), is from 79.3% by mass to 82.0% by mass, and preferably from 79.8% by mass to 81.2% by mass, relative to the total mass of the aqueous solution (A). By setting the organic solvent concentration to from 79.3% by mass to 82.0% by mass, a coagulated yarn having a dense surface and a dense interior can be obtained, and as a result, the strand strength and knot strength of the obtained carbon fiber bundle can be easily increased without decreasing the strand modulus.
[0042] Examples of the organic solvent contained in the aqueous solution (A) include dimethylformamide, dimethylacetamide, and dimethylsulfoxide. Among these, dimethylformamide is preferred from the viewpoint of forming a denser structure.
[0043] <Second Drawing Step> The second drawing step (2) is a step of drawing the coagulated fiber bundle obtained in the coagulation step (1) at a temperature of 75°C or higher in a hot aqueous solution (B) having an organic solvent concentration of 40% by mass or higher and 65% by mass or lower at a draw ratio of 2.0 times to 3.2 times to obtain a carbon fiber precursor acrylic fiber bundle. The temperature of the hot aqueous solution (B) is 75°C or higher, and preferably 85°C or higher. By setting the temperature of the hot aqueous solution (B) to 75°C or higher, sufficient stretchability can be ensured, making stable drawing easy. The temperature of the hot aqueous solution (B) is preferably 98°C or lower, and more preferably 95°C or lower. By setting the temperature of the hot aqueous solution (B) to 98°C or lower, a sudden temperature change in the coagulated fiber bundle can be suppressed, making uniform drawing easy. The above upper and lower limits can be combined arbitrarily. For example, the temperature may be 75°C or higher and 98°C or lower, or 85°C or higher and 95°C or lower.
[0044] The concentration of the organic solvent in the hot aqueous solution (B) is from 40% by mass to 65% by mass, and preferably from 50% by mass to 60% by mass, relative to the total mass of the hot aqueous solution (B). By setting the concentration of the organic solvent in the hot aqueous solution (B) to from 40% by mass to 65% by mass, a dense structure can be formed on both the surface and the inside, and a carbon fiber bundle having high strand strength and knot strength can be easily obtained without decreasing the strand modulus.
[0045] Examples of the organic solvent contained in the hot aqueous solution (B) include dimethylformamide, dimethylacetamide, and dimethylsulfoxide. Among these, dimethylformamide is preferred from the viewpoint of forming a denser structure.
[0046] The draw ratio in the hot aqueous solution (B) is 2.0 times or more and 3.2 times or less, and preferably 2.7 times or more and 3.0 times or less. By setting the draw ratio in the hot aqueous solution (B) to 2.0 times or more, it is possible to produce a carbon fiber precursor acrylic fiber bundle having sufficient molecular orientation, and it is easy to obtain a carbon fiber bundle having high strand strength and knot strength without decreasing the strand modulus. By setting the draw ratio in the hot aqueous solution (B) to 3.2 times or less, excessive draw can be suppressed, and stable draw can be easily achieved.
[0047] In the second drawing step (2), after drawing the coagulated fiber bundle in the hot aqueous solution (B), for example, a step of removing the organic solvent, a step of drawing with hot water, a step of drawing by evaporation with pressurized steam, a step of drawing with dry heat, a step of applying an oil agent, and a drying step may be appropriately combined to obtain an acrylic fiber precursor for carbon fibers. Specifically, in the second drawing step (2), after drawing the coagulated fiber bundle, the organic solvent may be removed, and the coagulated fiber bundle may be shrunk or drawn in hot water (C) at a temperature of 90°C or higher at a draw ratio of 0.96 to 1.30, and then drawn at a draw ratio of 3.7 to 4.2 in a pressurized steam atmosphere to obtain an acrylic fiber precursor for carbon fibers. That is, the second drawing step (2) preferably includes, in order: step (2-1) of drawing the coagulated yarn bundle in a warm aqueous solution (B) at a draw ratio of 2.0 to 3.2 times; step (2-2) of removing the organic solvent; step (2-3) of shrinking or drawing the coagulated yarn bundle in warm water (C) at a temperature of 90°C or higher at a draw ratio of 0.96 to 1.30 times; and step (2-5) of drawing the coagulated yarn bundle in a pressurized steam atmosphere at a draw ratio of 3.7 to 4.2 times. The second drawing step (2) may further include step (2-4) of applying an oil composition. Step (2-4) can be carried out between steps (2-3) and (2-5).
[0048] Step (2-2) is a step of removing the organic solvent from the coagulated fiber bundle (hereinafter also referred to as "drawn fiber bundle") after drawing in the warm aqueous solution (B). Any method can be used to remove the organic solvent as long as it can remove the solvent. For example, the drawn fiber bundle can be washed and drawn in a multistage washing tank set at a temperature in the range of 50°C or higher and lower than 100°C.
[0049] In step (2-3), the drawn fiber bundle after removal of the organic solvent is shrunk or drawn at a draw ratio of 0.96 to 1.30 in hot water (C) having a temperature of 90°C or higher. Drawing strain can be alleviated by step (2-3). The temperature of the hot water (C) is 90°C or higher. Setting the temperature of the hot water (C) to 90°C or higher makes it possible to uniformly alleviate the drawing strain, thereby enabling a carbon fiber bundle having higher strand strength and knot strength to be obtained without decreasing the strand modulus. The temperature of the hot water (C) is preferably 97°C or lower. Setting the temperature of the hot water (C) to 97°C or lower makes it possible to suppress a rapid temperature change in the drawn fiber bundle, thereby enabling uniformly alleviating the drawing strain, thereby enabling a carbon fiber bundle having higher strand strength and knot strength to be obtained without decreasing the strand modulus. The shrinkage or draw ratio in the hot water (C) is 0.96 to 1.30. By setting the shrinkage or draw ratio to 0.96 times or more, poor take-up due to loosening of the fiber bundle can be prevented, and the strain due to drawing can be stably relaxed. By setting the shrinkage or draw ratio to 1.30 times or less, excessive load can be suppressed, and the strain due to drawing can be stably relaxed. In step (2-3), the stretched fiber bundle after removing the organic solvent is preferably shrunk (relaxed) in warm water (C) to a shrinkage ratio (relaxation ratio) of 0.96 times or more but less than 1.00 times, or stretched to a stretch ratio of 1.00 times or more but 1.30 times or less, more preferably shrunk (relaxed) to a shrinkage ratio (relaxation ratio) of 0.96 times or more but 1.09 times or less, or stretched to a stretch ratio of 1.05 times or more but 1.30 times or less, and even more preferably shrunk (relaxed) to a shrinkage ratio (relaxation ratio) of 0.96 times or more but 1.99 times or less.
[0050] Step (2-4) is a step of applying an oil composition to the drawn fiber bundle after shrinking or drawing in warm water (C). The oil composition can be determined taking into consideration the functions required of the carbon fiber precursor acrylic fiber bundle. For example, a silicone-based oil composition can be used. The oil composition can further contain additives such as antioxidants, antistatic agents, antifoaming agents, preservatives, antibacterial agents, and penetrating agents, as needed. As a method for applying the oil composition to the drawn fiber bundle, known methods such as a roller method, a guide method, a spray method, and a dipping method can be used. After applying the oil composition to the drawn fiber bundle, the bundle may be dried, as needed, by a conventionally known method.
[0051] In step (2-5), the drawn fiber bundle is shrunk or drawn in warm water (C), preferably after application of an oil composition, and dried as necessary, and then drawn at a draw ratio of 3.7 to 4.2 times in a pressurized steam atmosphere. The draw ratio in the pressurized steam atmosphere is 3.7 to 4.2 times. By setting the draw ratio in the pressurized steam atmosphere to 3.7 times or more, the molecular orientation of the resulting acrylic fiber bundle as a precursor to carbon fibers is improved, making it possible to obtain a carbon fiber bundle with higher strand strength and knot strength without reducing the strand modulus. By setting the draw ratio in the pressurized steam atmosphere to 4.2 times or less, excessive drawing can be suppressed, enabling stable drawing. The single fiber fineness of the acrylic fiber bundle as a precursor to carbon fibers is preferably in the range of 1.1 to 2.0 dtex. The single fiber fineness can be controlled by the amount of acrylonitrile polymer solution discharged from the discharge hole of the spinning nozzle and the draw ratio.
[0052] <Flaming-proofing step> The flame-proofing step (3) is a flame-proofing step in which the carbon fiber precursor acrylic fiber bundle or the carbon fiber precursor acrylic fiber bundle obtained in the second drawing step (2) is heated in an oxidizing atmosphere to obtain a flame-proofed fiber bundle. In the flame-proofing step, it is preferable to heat the carbon fiber precursor acrylic fiber bundle in an oxidizing atmosphere having a temperature gradient within a range of 220°C to 280°C. For example, it is more preferable to heat the carbon fiber precursor acrylic fiber bundle in an oxidizing atmosphere in a flame-proofing furnace having a linear temperature gradient within a range of 220°C to 280°C. In the flame-proofing step, a thermal cyclization reaction and an oxygen-induced oxidation reaction occur. It is important to balance these two reactions to obtain a carbon fiber bundle with high strand strength and knot strength without reducing the strand modulus. The atmospheric temperature in the flame-proofing step is preferably 220°C to 280°C. By setting the temperature of the atmosphere through which the carbon fiber precursor acrylic fiber bundle is passed in the flame-resistant treatment step to 220°C or higher, it is possible to reduce the number of areas where the oxidation reaction has not fully occurred and to suppress the occurrence of large structural irregularities in the cross-sectional direction of the single fiber, making it easy to obtain a carbon fiber bundle having high strand strength and knot strength without decreasing the strand modulus. By setting the temperature of the atmosphere through which the carbon fiber precursor acrylic fiber bundle is passed in the flame-resistant treatment step to 280°C or lower, it is possible to suppress the presence of a large amount of oxygen in areas close to the surface of the single fiber, and as a result, excess oxygen is eliminated by heat treatment in the first carbonization step or later described below, making it easy to suppress reactions that form defects, making it easy to obtain a carbon fiber bundle having high density and high strand strength and knot strength without decreasing the strand modulus.
[0053] In the flame-resistant process, the density of the obtained flame-resistant fiber bundle is 1.33 g / cm 3 1.36g / cm or more 3 It is preferable to heat the carbon fiber precursor acrylic fiber bundle until the density of the flame-resistant fiber bundle reaches 1.33 g / cm or less. 3By setting the density of the flame-resistant fiber bundle to 1.36 g / cm or more, it is possible to suppress the occurrence of portions where the flame-resistant treatment is insufficient, and as a result, it is possible to suppress the occurrence of a decomposition reaction due to the heat treatment in the first carbonization step or later described below, which would result in the formation of defects, and therefore it is easy to obtain a carbon fiber bundle having a high density and high strand strength and knot strength without decreasing the strand modulus. 3 By setting the above conditions, it is possible to suppress the presence of a large amount of oxygen in the flame-resistant fiber bundle, and as a result, the excess oxygen is eliminated by the heat treatment in the first carbonization step or later described below, and the reaction that forms defects is easily suppressed, and it is easy to obtain a carbon fiber bundle that has a high density and high strand strength and knot strength without decreasing the strand modulus.
[0054] In the flame-proofing step, the carbon fiber precursor acrylic fiber bundle is preferably elongated at an elongation rate of 3.0% or more and 8.0% or less to form a flame-proof fiber bundle. The elongation rate in the flame-proofing step is more preferably 4.0% or more and 7.0% or less, and even more preferably 5.0% or more and 6.5% or less. By setting the elongation rate in the flame-proofing step to 3.0% or more, the molecular orientation of the flame-proof fiber bundle can be improved, making it easy to obtain a carbon fiber bundle having high strand strength and knot strength without reducing the strand modulus. By setting the elongation rate in the flame-proofing step to 8.0% or less, excessive elongation can be suppressed, making it easy to obtain a stable flame-proof fiber bundle.
[0055] Examples of gases that form an oxidizing atmosphere include air, oxygen, and nitrogen dioxide, with air being preferred from the standpoint of economy. The treatment time in the flame-proofing furnace (the time of the flame-proofing treatment) can be, for example, 30 minutes or more and 100 minutes or less.
[0056] <First carbonization step> The first carbonization step (4) is a first carbonization step in which the flame-resistant fiber bundle obtained in the flame-resistant step (3) is heated in a non-oxidizing atmosphere having a temperature gradient in the atmospheric temperature range of 300°C to 900°C, at an elongation of 4.0% to 5.0%. In the first carbonization step, it is preferable to heat the flame-resistant fiber bundle in a non-oxidizing atmosphere in a first carbonization furnace having a linear temperature gradient in the atmospheric temperature range of 300°C to 900°C. The atmospheric temperature in the first carbonization step is 300°C to 900°C. By setting the atmospheric temperature in the first carbonization step to 900°C or less, it is possible to prevent the flame-resistant fiber bundle from becoming very brittle, and not only can the bundle be passed through the first carbonization step (first carbonization furnace) stably, but also the formation of defects is suppressed in the heat treatment in the second carbonization step and subsequent steps described below, and a carbon fiber bundle having high density and high strand strength and knot strength can be easily obtained without decreasing the strand modulus.
[0057] The elongation rate in the first carbonization step is 4.0% or more and 5.0% or less. By setting the elongation rate in the first carbonization step to 4.0% or more, the molecular orientation of the obtained carbon fiber bundle can be improved, and the strand strength and knot strength can be easily improved without decreasing the strand modulus. By setting the elongation rate in the first carbonization step to 5.0% or less, excessive elongation can be suppressed, and the fiber can be easily passed through the first carbonization step (first carbonization furnace) stably.
[0058] The treatment time in the first carbonization furnace (time of the first carbonization treatment) is preferably 1.0 minute or more and 3.0 minutes or less, and more preferably 1.2 minutes or more and 2.5 minutes or less. By setting the treatment time in the first carbonization furnace to 1.0 minute or more, it is possible to suppress a violent decomposition reaction accompanying a sudden rise in temperature, and it is easy to obtain a carbon fiber bundle having high density and high strand strength and knot strength without decreasing the strand modulus. By setting the treatment time in the first carbonization furnace to 3.0 minutes or less, it is possible to suppress a decrease in the degree of crystal orientation of the carbon fiber bundle, and it is easy to obtain a carbon fiber bundle having high strand strength and knot strength without decreasing the strand modulus.
[0059] Examples of gases that form a non-oxidizing atmosphere include nitrogen, argon, and helium, with nitrogen being preferred from the standpoint of economy.
[0060] <Second Carbonization Step> In the second carbonization step (5), after the first carbonization step (4), the fiber bundle is heated in a non-oxidizing atmosphere having a temperature gradient in the range of 1000°C to 1800°C while applying a tension of 0.15 cN / dtex to 0.21 cN / dtex to the fiber bundle. Note that the fiber bundle to be carbonized in the second oxygenation step (5) is the flame-resistant fiber bundle that has passed through the first carbonization step. In the second carbonization step, it is preferable to heat the fiber bundle that has passed through the first carbonization furnace (first carbonization step) in a non-oxidizing atmosphere in a second carbonization furnace having a linear temperature gradient in the range of 1000°C to 1800°C. The atmosphere temperature in the second carbonization step is 1000°C to 1800°C. By setting the atmospheric temperature in the second carbonization step to 1800°C or less, the formation of defects in the heat treatment in the third carbonization step described below is suppressed, and it is easy to obtain a carbon fiber bundle having high density and high strand strength and knot strength without decreasing the strand modulus.
[0061] Since the fiber bundle passing through the second carbonization step (second carbonization furnace) is subject to significant shrinkage, it is important to heat it under tension. In the second carbonization step, a tension of 0.15 cN / dtex or more and 0.21 cN / dtex or less is applied to the carbon fiber precursor acrylic fiber bundle with respect to the total fineness immediately before passing through the flame-proofing step (flame-proofing furnace), and preferably a tension of 0.17 cN / dtex or more and 0.20 cN / dtex or less is applied. By applying a tension of 0.15 cN / dtex or more to the fiber bundle passing through the second carbonization step (second carbonization furnace), it is possible to maintain a high molecular orientation in the obtained carbon fiber bundle, and it is easy to improve the strand strength and knot strength without decreasing the strand elastic modulus. By setting the tension applied to the fiber bundle passing through the second carbonization step (second carbonization furnace) to 0.21 cN / dtex or less, it becomes possible to suppress single fiber breakage in the carbon fiber bundle due to excessive tension, and it becomes easier to stably obtain a carbon fiber reinforced composite material.
[0062] The treatment time in the second carbonization furnace (time of the second carbonization treatment) is preferably 1.3 minutes or more and 5.0 minutes or less. By setting the treatment time in the second carbonization furnace to 1.3 minutes or more, it is possible to suppress a violent decomposition reaction accompanying a sudden rise in temperature, and it is easy to obtain a carbon fiber bundle having a high density and high strand strength and knot strength without decreasing the strand modulus. By setting the treatment time in the second carbonization furnace to 5.0 minutes or less, it is possible to sufficiently increase the degree of crystal orientation of the carbon fiber bundle while maintaining high productivity, and it is easy to efficiently obtain a carbon fiber bundle having high strand strength and knot strength without decreasing the strand modulus.
[0063] <Third Carbonization Step> The third carbonization step (6) is a third carbonization step that follows the second carbonization step (5), in which the fiber bundle is heated in a non-oxidizing atmosphere having a temperature gradient in the range of 1700°C to 2300°C while applying a tension of 0.15 cN / dtex to the fiber bundle and 0.23 cN / dtex to the fiber bundle. The fiber bundle to be carbonized in the third carbonization step (6) is the flame-resistant fiber bundle that has passed through the second carbonization step. In the third carbonization step, it is preferable to heat the fiber bundle that has passed through the second carbonization furnace (second carbonization step) in a non-oxidizing atmosphere in a third carbonization furnace having a linear temperature gradient in the range of 1700°C to 2300°C to obtain a carbon fiber bundle. The atmosphere temperature in the third carbonization step is 1700°C to 2300°C. Considering the temperature of the second carbonization step, it is preferable to set the atmospheric temperature in the third carbonization step higher than that in the second carbonization step, and more preferably to set it to 1800°C or higher. Setting the atmospheric temperature in the third carbonization step to 2300°C or lower not only prevents deterioration of the third carbonization furnace, but also suppresses the formation of defects in the resulting carbon fiber bundle, making it easier to obtain a carbon fiber bundle with high density and high strand strength and knot strength without reducing the strand modulus. The maximum heating temperature is preferably 2100 to 2300°C. A maximum temperature of 2100°C or higher makes it easier to increase the strand modulus, and a maximum temperature of 2300°C or lower can prevent deterioration of the third carbonization furnace.
[0064] Since the fiber bundle passing through the third carbonization step (third carbonization furnace) is subject to significant shrinkage, it is important to heat it under tension. In the third carbonization step, a tension of 0.15 cN / dtex or more and 0.23 cN / dtex or less is imparted to the carbon fiber precursor acrylic fiber bundle with respect to the total fineness immediately before passing through the flame-stabilization step (flame-stabilization furnace), and preferably a tension of 0.18 cN / dtex or more and 0.22 cN / dtex or less is imparted. By applying a tension of 0.15 cN / dtex or more to the fiber bundle passing through the third carbonization step (third carbonization furnace), it is possible to maintain a high molecular orientation in the obtained carbon fiber bundle, and it is easy to improve the strand strength and knot strength without decreasing the strand elastic modulus. By setting the tension applied to the fiber bundle passing through the third carbonization step (third carbonization furnace) to 0.23 cN / dtex or less, it becomes possible to suppress single fiber breakage in the carbon fiber bundle due to excessive tension, and it becomes easier to stably obtain a carbon fiber reinforced composite material.
[0065] The treatment time in the third carbonization furnace (time of the third carbonization treatment) is preferably 1.0 minute or more and 3.0 minutes or less. By setting the treatment time in the third carbonization furnace to 1.0 minute or more, it is possible to suppress a violent decomposition reaction accompanying a sudden rise in temperature, and it is easy to obtain a carbon fiber bundle having high density and high strand strength and knot strength without decreasing the strand modulus. By setting the treatment time in the third carbonization furnace to 3.0 minutes or less, it is possible to sufficiently increase the degree of crystal orientation of the carbon fiber bundle while maintaining high productivity, and it is easy to efficiently obtain a carbon fiber bundle having high strand strength and knot strength without decreasing the strand modulus.
[0066] In the third carbonization step (6), the temperature rise rate when the atmospheric temperature is raised from 1800°C to 2200°C is preferably 300°C / min or more and 600°C / min or less, more preferably 350°C / min or more and 550°C / min or less, and even more preferably 400°C / min or more and 500°C / min or less. By raising the atmospheric temperature from 1800°C to 2200°C at a temperature rise rate of 300°C / min or more, carbon fiber bundles can be easily produced with high productivity. By raising the atmospheric temperature from 1800°C to 2200°C at a temperature rise rate of 600°C / min or less, it is possible to suppress a violent decomposition reaction that accompanies a sudden temperature rise, and it is easy to obtain a carbon fiber bundle having high density and high strand strength and knot strength without reducing the strand modulus. The aforementioned temperature rise rate is the travel time of the fiber bundle at an atmospheric temperature of 1800°C to 2200°C divided by 400°C, which is the difference between 2200°C and 1800°C.
[0067] The difference between the maximum atmospheric temperature in the second carbonization step (5) and the inlet atmospheric temperature in the third carbonization step (6) is preferably 700°C or less, and more preferably 500°C or less. By setting the difference between the maximum atmospheric temperature in the second carbonization step (5) and the inlet atmospheric temperature in the third carbonization step (6) to 700°C or less, it is possible to suppress a violent decomposition reaction in the early stage of the third carbonization step (6), and it is easy to obtain a carbon fiber bundle having high density and high strand strength and knot strength without reducing the strand modulus. The difference between the maximum atmospheric temperature in the second carbonization step (5) and the inlet atmospheric temperature in the third carbonization step (6) is preferably 30°C or more, and more preferably 50°C or more. The above upper and lower limits can be combined arbitrarily. For example, it may be 30°C or more and 700°C or less, or 50°C or more and 500°C or less.
[0068] <Other Steps> The method for producing carbon fibers of the present invention may include the following (a) acrylonitrile-based polymer solution preparation step before the (1) coagulation step. The method for producing carbon fibers of the present invention may include the following (b) first drawing step between the (1) coagulation step and the (2) second drawing step. The method for producing carbon fibers of the present invention may include the following (c) surface oxidation treatment step and (d) sizing step after the (6) third carbonization step. (a) An acrylonitrile-based polymer solution preparation step of preparing an acrylonitrile-based polymer solution. (b) A first drawing step of drawing the coagulated fiber bundle obtained in the (1) coagulation step at a draw ratio of 1.00 to 1.20 in air. (c) A surface oxidation treatment step of surface-oxidizing the carbon fiber bundle obtained in the (6) third carbonization step. (d) A sizing step of sizing the surface-oxidized carbon fiber bundle obtained in the (c) surface oxidation treatment step.
[0069] (Acrylonitrile-based polymer solution preparation step) The acrylonitrile-based polymer solution preparation step (a) is a step of preparing an acrylonitrile-based polymer solution to be used in the coagulation step (1). The acrylonitrile-based polymer used in the present invention is a polymer obtained by polymerizing acrylonitrile as a main monomer. The acrylonitrile-based polymer may be a homopolymer obtained only from acrylonitrile, or may be a copolymer in which other monomers are copolymerized in addition to acrylonitrile as the main component.
[0070] The content of acrylonitrile-derived structural units (hereinafter also referred to as "acrylonitrile units") in the acrylonitrile-based polymer can be determined, for example, taking into consideration the quality desired for the resulting carbon fiber bundle, and is, for example, preferably 90% by mass or more and 100% by mass or less, more preferably 90% by mass or more and 99.5% by mass or less, and even more preferably 96% by mass or more and 99.5% by mass or less, relative to the total mass of the monomer units constituting the acrylonitrile-based polymer. When the content of acrylonitrile units is 90% by mass or more, fusion between single fibers can be suppressed in each of the flame-proofing and carbonization steps for converting the carbon fiber precursor acrylic fiber bundle into carbon fiber, and a decrease in the strand strength of the carbon fiber bundle can be easily prevented. Furthermore, adhesion between single fibers can be easily suppressed in treatments such as drawing with a heated roller or pressurized steam. When the content of acrylonitrile units is 100% by mass or less, preferably 99.5% by mass or less, the solubility in a solvent is less likely to decrease, and precipitation and solidification of the acrylonitrile-based polymer can be prevented, making it easier to stably produce a carbon fiber precursor acrylic fiber bundle.
[0071] When the acrylonitrile-based polymer contains a monomer unit other than an acrylonitrile unit, the monomer unit other than an acrylonitrile unit in the acrylonitrile-based polymer can be appropriately selected from vinyl-based monomers copolymerizable with acrylonitrile. A vinyl-based monomer unit that improves the hydrophilicity of the acrylonitrile-based polymer and a vinyl-based monomer unit that promotes the flame retardation reaction are preferred. Examples of suitable monomer units include acrylic acid, methacrylic acid, itaconic acid, methyl acrylate, methyl methacrylate, and other acrylic acid derivatives; acrylamide, methacrylamide, N-methylolacrylamide, N,N-dimethylacrylamide, and other acrylamide derivatives; and vinyl acetate. The acrylonitrile-based polymer may be synthesized by any polymerization method, and the present invention is not limited by the polymerization method. Examples of suitable solvents for the acrylonitrile-based polymer solution include organic solvents such as dimethylacetamide, dimethyl sulfoxide, and dimethylformamide; and aqueous solutions of inorganic compounds such as zinc chloride and sodium thiocyanate. Dimethylformamide is preferred due to its high dissolving power for acrylonitrile-based polymers.
[0072] The polymer concentration of the acrylonitrile-based polymer solution is preferably 20% by mass or more and 25% by mass or less, and more preferably 21% by mass or more and 24% by mass or less, relative to the total mass of the acrylonitrile-based polymer solution. By setting the polymer concentration to 20% by mass or more, voids inside the coagulated yarn are reduced, making it easier to increase the strand strength of the carbon fiber bundle. By setting the polymer concentration to 25% by mass or less, the acrylonitrile-based polymer solution can maintain appropriate viscosity and fluidity, making it easier to produce a carbon fiber precursor acrylic fiber bundle.
[0073] The temperature of the acrylonitrile-based polymer solution when used in the solidification step (1) is preferably adjusted to 50° C. or higher and 70° C. or lower, more preferably 55° C. or higher and 65° C. or lower. By adjusting the temperature of the acrylonitrile-based polymer solution to 50° C. or higher and 70° C. or lower, the acrylonitrile-based polymer solution can maintain appropriate viscosity and fluidity, which tends to facilitate the production of a carbon fiber precursor acrylic fiber bundle.
[0074] (First Drawing Step) The first drawing step (b) is a step of drawing the coagulated yarn bundle in air at a draw ratio of 1.00 to 1.20 times. The first drawing step (b) is preferably performed between the coagulation step (1) and the second drawing step (2). In the first drawing step (b), the coagulated yarn bundle taken up in the coagulation step (1) is drawn in air while still containing the coagulation liquid. The draw ratio in air is 1.00 to 1.20 times, and preferably 1.05 to 1.15 times. Setting the draw ratio in air to 1.00 times or more makes it possible to suppress non-uniform shrinkage, and as a result, it is easy to obtain a carbon fiber bundle with high strand strength and knot strength without reducing the strand modulus. Setting the draw ratio in air to 1.20 times or less makes it possible to suppress excessive drawing and facilitate stable drawing.
[0075] (Surface Oxidation Treatment Step) The surface oxidation treatment step (c) is a step of subjecting the carbon fiber bundle obtained in the third carbonization step (6) to a surface oxidation treatment. The surface oxidation treatment step (c) is preferably carried out after the third carbonization step (6). The carbon fiber bundle obtained by passing through the third carbonization step (third carbonization furnace) is preferably subjected to a surface oxidation treatment. Examples of the surface treatment method include known methods, namely oxidation treatments by electrolytic oxidation, chemical oxidation, air oxidation, etc., and any method may be used, but electrolytic oxidation treatment, which is widely practiced industrially, is preferred because it allows stable surface oxidation treatment. In the surface oxidation treatment, the IPA, which indicates the surface treatment state, is set to 0.05 μA / cm 2 0.25 μA / cm or more 2 It is preferable to set it to below 10 coulombs / g. A simple method for controlling it to such a range is to adjust the amount of electricity in the electrolytic oxidation treatment. In the electrolytic oxidation treatment, even with the same amount of electricity, the IPA varies greatly depending on the electrolyte used and its concentration. In an alkaline aqueous solution with a pH higher than 7, it is preferable to perform the oxidation treatment by passing an amount of electricity of 10 coulombs / g or more and 200 coulombs / g or less through the carbon fiber bundle as the anode. Examples of the electrolyte include ammonium carbonate, ammonium bicarbonate, ammonium sulfate, calcium hydroxide, sodium hydroxide, and potassium hydroxide.
[0076] (Sizing Step) The sizing step (d) is a step of sizing the carbon fiber bundles after the surface oxidation treatment step (c). The sizing step (d) is preferably performed after the surface oxidation treatment step (c). The surface-oxidized carbon fiber bundles obtained in the surface oxidation treatment step (c) are preferably subsequently subjected to a sizing treatment. The sizing treatment can be performed by applying a solution in which a sizing agent is dissolved in an organic solvent, or, for example, an emulsion in which a sizing agent is dispersed in water using an emulsifier, to the carbon fiber bundles by, for example, a roller immersion method or a roller contact method, and then drying the bundles. The amount of sizing agent attached to the surface of the carbon fiber can be adjusted by adjusting the concentration of the sizing agent solution or the amount of squeezing. Drying can be performed, for example, using hot air, a hot plate, a heated roller, or various infrared heaters. Known sizing agents can be used as the sizing agent. Examples include sizing agents mainly composed of epoxy resin, polyether resin, epoxy-modified polyurethane resin, and polyester resin.
[0077] The present invention will be described in detail below with reference to examples, but the present invention is not limited to the following description as long as it does not depart from the gist of the invention. Various measurement methods used in the examples are as follows.
[0078] [Method for measuring the average diameter of carbon fiber single fibers] Density of carbon fiber bundle (g / cm 3 The cross-sectional area per single carbon fiber was calculated from the mass per meter of the carbon fiber bundle, i.e., basis weight (g / m), and the number of filaments in the carbon fiber bundle. The diameter of a perfect circle having an area equal to the cross-sectional area was calculated and used as the average diameter of the single carbon fiber. The density of the carbon fiber bundle was measured in accordance with Method C (gradient density pipe method) described in JIS R 7063:1999.
[0079] [Method for measuring strand strength and strand modulus] The strand strength and strand modulus of the carbon fiber bundle were measured in accordance with JIS R 7608: 2007. The strand modulus was calculated by Method A of the same method.
[0080] [Method for measuring knot strength] The knot strength was measured as follows. A test specimen was prepared by attaching 25 mm long grips to both ends of a 150 mm long carbon fiber bundle. -3 The carbon fiber bundles were paralleled under a load of 100 N / denier. A knot was formed in the specimen at approximately the center, and the crosshead speed during tensioning was 100 mm / min. Twelve specimens were tested, and the minimum and maximum values were removed, and the average of the 10 specimens was used as the measured value.
[0081] [Method for Measuring Fracture Surface Creation Energy] Carbon fiber monofilaments were cut to 20 cm lengths, and the central portions of the monofilaments were attached and fixed to a single fiber tensile test mount for a 10 mm sample length as specified in JIS R 7606:2000. The excess portion protruding from the mount was then cut and removed to prepare samples. Next, these samples fixed to the mount were irradiated with a laser to form hemispherical defects. A Photonic Instruments Micropoint (pulse energy 300 uJ) was used as the laser interface system. A Nikon ECLIPSE LV100 optical microscope, required for focusing the laser, was used. The aperture stop of the optical microscope was set to the minimum, and the objective lens was set to 100x magnification. Under these conditions, a single pulse of a 435 nm laser, with the laser intensity attenuated by 10% using an attenuator, was irradiated to the central portion of the sample in the fiber axis direction and the central portion perpendicular to the fiber axis, to obtain a sample with a hemispherical defect. To prevent shrinkage fracture of the carbon fiber sample, the sample attached to the mount was sandwiched between films, which were then filled with a viscous liquid and subjected to a tensile test. Specifically, a film approximately 5 mm wide and 15 mm long was prepared, and the film was attached to the top of both sides of the sample mount with an adhesive. The sample was then sandwiched between the films so as to cover the mount. The space between the films was filled with a glycerin aqueous solution (1 part glycerin to 2 parts water by mass), and a tensile test was performed at a tensile speed of 0.5 mm / min to measure the breaking load. Next, the sample pair split into two pieces during the tensile test was removed from the mount, carefully washed with water, and allowed to air dry. Next, the sample was fixed with carbon paste to an SEM sample stage with the fracture surface facing up, and an SEM observation sample was prepared. The fracture surfaces of the obtained SEM observation samples were observed using a scanning electron microscope (manufactured by JEOL Ltd., product name "JSM6060") under conditions of an acceleration voltage of 10 kV to 15 kV and a magnification of 10,000 to 15,000 times. The obtained SEM images were imported into a personal computer and analyzed using image analysis software to measure the depth of the hemispherical defects and the cross-sectional area of the fiber. Here, the "depth of the hemispherical defects" was defined as the longest distance when a line was drawn from the circumference of a single fiber to the center.Next, the breaking load was divided by the fiber cross-sectional area (breaking load / fiber cross-sectional area) to calculate the breaking strength (σ). The fracture surface formation energy was calculated using the following formula (F2). The fracture surface formation energy was calculated for 30 single fibers, and the average value was used as the fracture surface formation energy of the carbon fiber bundle. Fracture surface formation energy = σ. 2 πC / 2E (F2) where σ is the breaking strength (GPa), E is the ultrasonic modulus of elasticity of the carbon fiber bundle (GPa), and C is the depth of the hemispherical defect (m). The ultrasonic modulus of elasticity of the carbon fiber bundle was measured in accordance with the measurement method described later.
[0082] <Method for measuring ultrasonic elastic modulus of carbon fiber bundle> The ultrasonic propagation velocity was measured according to the measurement method shown in Figure 1. The distance L1 between the transmitter and the first receiver was 0.20 m, the distance L2 between the transmitter and the second receiver was 0.25 m, and the tension applied to the carbon fiber bundle during measurement was 0.02 N / tex. A pulse was given from the pulse transmission circuit to the transmitter to drive it, propagating ultrasonic waves through the carbon fiber bundle, and the time from when the ultrasonic waves propagated from the carbon fiber bundle were detected by the first receiver was defined as reception time 1, and the time from when the ultrasonic waves propagated from the carbon fiber bundle were detected by the second receiver was defined as reception time 2. The ultrasonic elastic modulus of the carbon fiber bundle was calculated using the following formula (F3): ultrasonic elastic modulus (GPa) = ((0.25 m - 0.20 m) / (reception time 2 (sec) - reception time 1 (sec)) 2 × density of carbon fiber bundle (g / cm 3 ) x 10 -6 ... (F3)
[0083] [Crystallite Size Lc] Carbon fiber bundles were cut into 50 mm lengths, and 30 mg of each was precisely weighed and collected. The sample fiber axes were aligned so that they were precisely parallel, and then prepared into a fiber sample bundle with a width of 1 mm and a uniform thickness using a sample preparation jig. This fiber sample bundle was impregnated with a vinyl acetate / methanol solution to maintain its shape, and then fixed to a wide-angle X-ray diffraction sample stage. A Rigaku CuKα X-ray generator (using a Ni filter) was used as the X-ray source, and a Rigaku goniometer was used. The diffraction peak near 2θ = 25°, corresponding to the graphite plane index (002), was detected by a scintillation counter using a transmission method. The output was 40 kV-100 mA. The crystallite size Lc was calculated from the half-width of the diffraction peak using the following formula (F4): Lc = Kλ / (β0 cos θ) (F4) (where K is the Scherrer constant, 0.9; λ is the wavelength of the X-ray used (here, CuKα rays are used, so it is 1.5418 Å); θ is the Bragg diffraction angle; β0 is the true half-width; β0 = βE - β1 (βE is the apparent half-width; β1 is an instrument constant, here 1.05 × 10 -2 rad). The measurements were carried out with n=5.
[0084] [Method for calculating average void length] According to the Ruland method described in Macromolecules, Vol. 33, No. 5, 2000, the average void length was calculated by SAXS (small-angle X-ray scattering) as follows. Using an Anton Paar "SAXSpoint 2.0 system," CuKα (wavelength 1.54 Å) was used as X-rays, the exposure time was 30 minutes, the measurement environment was vacuum, and the distance from the sample to the detector was set to 610 mm. After aligning the carbon fiber bundles in one direction, the fiber axis direction was set vertically on the sample stage, and small-angle X-ray scattering measurement was performed. At this time, scattering originating from voids inside the carbon fibers was observed in a direction perpendicular to the fiber axis. Analysis by the Ruland method was performed using graphing software (Igor Pro 8.0). In this specification, the scattering vector q is defined as 4π sin θ / λ (θ: scattering angle, λ: X-ray wavelength). The two-dimensional scattering profile obtained according to the above measurement conditions was converted into polar coordinates by dividing the azimuth angle of 360° into 1000 parts, to obtain a scattering intensity map of azimuth angle vs. scattering vector q. Here, the carbon fiber axial direction is defined as an azimuth angle of 0°. The obtained scattering intensity map was analyzed by the Ruland method in the direction perpendicular to the carbon fiber axis (azimuth angle 90°) and in a range not including streaks resulting from total reflection of X-rays on the carbon fiber surface (q = 0.8 to 1.86 nm-1). Specifically, the scattering intensity map of azimuth angle vs. scattering vector q was averaged every five pixels in the q direction to obtain an azimuth angle vs. scattering intensity profile at each q. The range of azimuth angles of 0 to 180° of this profile was fitted with a Gaussian function to calculate the integral width B. q 2 B 2 q 2 The intercept and slope of the linear approximation were obtained, and the void length L of the voids present in the carbon fiber and the integral width of the void orientation distribution (scattering vector q) were calculated using the following formula (F5). 2 (Integral width B of scattering intensity distribution in the azimuthal direction) 2 = (scattering vector q) 2 (Integral width of void orientation distribution) 2 +(2π / L) 2 ... (F5)
[0085] [Method for measuring compressive strength in the fiber axis direction of a carbon fiber reinforced composite material] (Production of prepreg) A carbon fiber bundle unwound from a bobbin was placed on a release paper coated with epoxy resin #350 and impregnated with the epoxy resin. A protective film was laminated on top of the carbon fiber bundle, and a resin content of about 33 mass % and a carbon fiber density of 125 g / m 2 were obtained. 2 A unidirectionally oriented prepreg (hereinafter referred to as "prepreg") was prepared.
[0086] (Production of unidirectional laminate material) Two plies of prepreg were laminated and bagged, and the pressure inside the bag was reduced using a vacuum pump. The bag was then placed in an autoclave, and the temperature inside the autoclave was increased at a rate of 2°C / min, held at 80°C for 1 hour, and then increased at a rate of 2°C / min and held at 130°C for 1.5 hours to cure, thereby obtaining a carbon fiber reinforced composite material. The pressure inside the autoclave was increased to 0.6 MPa after holding at 80°C for 1 hour. The suction by the vacuum pump was stopped when the pressure inside the autoclave reached 0.14 MPa, and the bag was opened to the atmosphere.
[0087] <Evaluation of Compressive Properties in the Fiber Axis Direction of Carbon Fiber Reinforced Composite Materials> Six test specimens measuring 12.7 mm wide, 80 mm long, and 1 mm thick were prepared from the resulting unidirectional laminate. The length direction of the test specimen was the 0° fiber direction. The resulting test specimens were measured for compressive strength and compressive modulus in the fiber axis direction using an INSTRON 5882 measuring instrument equipped with a 100 kN load cell in accordance with SACMA SRM 1R at a temperature of 23°C, humidity of 50%, and a crosshead speed of 1.27 mm / min. The measured values were converted to a Vf (fiber volume fraction) of 56%. The same measurements were performed on six test specimens, and the average was calculated. The measurements were performed using tabs cut from the same plate and attached to each test specimen.
[0088] Example 1 Preparation of Carbon Fiber Precursor Acrylic Fiber Bundle An acrylonitrile-based polymer containing 98% by mass of acrylonitrile units and 2% by mass of methacrylic acid units was dissolved in dimethylformamide to prepare a 23.5% by mass acrylonitrile-based polymer solution. This acrylonitrile-based polymer solution was spun through a spinneret equipped with several 2,000 nozzles with a diameter of 0.15 mm and subjected to dry-wet spinning. That is, the acrylonitrile-based polymer solution was spun into air and passed through a space of approximately 5 mm, then coagulated in a coagulation solution filled with an aqueous solution (A) containing 80.4% by mass of dimethylformamide adjusted to 8°C, and a coagulated fiber bundle was obtained. The coagulated fiber bundle was then doubled into 12,000 filaments, withdrawn from the coagulation bath, stretched 1.1 times in air, and then stretched 2.9 times in a stretching tank filled with a warm aqueous solution (B) containing 55% by mass of dimethylformamide adjusted to 90°C. After stretching, the solvent-containing stretched fiber bundle was washed with clean water and then relaxed 0.98 times in warm water (C) at 96°C. Subsequently, an oil agent mainly composed of amino-modified silicone was added to the stretched fiber bundle to a concentration of 1.1 mass%, and the stretched fiber bundle was dried and densified. The stretched fiber bundle after drying and densification was stretched 4.0 times in a pressurized water vapor atmosphere to further improve orientation and densify, and then wound up to obtain an acrylonitrile-based precursor fiber bundle. The fineness of this fiber was 1.08 dtex.
[0089] <Preparation of Carbon Fiber Bundle> A plurality of carbon fiber precursor acrylic fiber bundles were aligned in parallel and introduced into a flame-resistant furnace having a linear temperature gradient with an inlet atmospheric temperature of 220° C. and a maximum atmospheric temperature of 280° C. Heated air was blown onto the carbon fiber precursor acrylic fiber bundles in the flame-resistant furnace, whereby the carbon fiber precursor acrylic fiber bundles were flame-resistant, and the density of the carbon fiber precursor acrylic fiber bundles was reduced to 1.345 g / cm. 3A flame-retardant fiber bundle of 1000 kJ / cm2 was obtained. The elongation rate was 6.0%, and the flame-retardant treatment time was 70 minutes. Next, the flame-retardant fiber bundle was passed through a first carbonization furnace in nitrogen with an inlet atmosphere temperature of 300°C, a maximum atmosphere temperature of 700°C, and a linear temperature gradient, while being elongated by 4.5%, to perform a first carbonization treatment. The treatment time was 2.0 minutes. Further, a second carbonization treatment was performed using a second carbonization furnace in a nitrogen atmosphere with an inlet atmosphere of 1100°C, a maximum atmosphere temperature of 1200°C, and a linear temperature gradient. The elongation rate was -2.0%, and the treatment time was 1.6 minutes. The tension applied to the yarn bundle during the treatment was 0.19 cN / dtex. Subsequently, a third carbonization treatment was performed using a third carbonization furnace in a nitrogen atmosphere with an inlet atmosphere of 1800°C, a maximum atmosphere temperature of 2300°C, and a linear temperature gradient, to obtain a carbon fiber bundle. The elongation rate was -2.0%, and the treatment time was 1.9 minutes. At this time, the tension applied to the yarn bundle during treatment was 0.21 cN / dtex. The difference between the maximum atmospheric temperature of the second carbonization furnace and the inlet atmosphere of the third carbonization furnace was 600°C, and the temperature increase rate when increasing the atmospheric temperature from 1800°C to 2200°C was 450°C / min. Subsequently, the carbon fiber bundle was run through a 10% by mass aqueous solution of ammonium bicarbonate at 30°C, and an electric current was applied between the carbon fiber bundle as the anode and the counter electrode so that the amount of electricity was 40 coulombs per gram of treated carbon fiber. The carbon fiber bundle was then washed with hot water at 90°C and dried. Next, 0.5% by mass of a sizing agent (manufactured by DIC Corporation, trade name "Hydran N320") was applied (sizing treatment), and the carbon fiber bundle was wound around a bobbin to obtain a carbon fiber bundle. The carbon fiber bundle after the sizing treatment was subjected to measurements of the average diameter, density, basis weight, knot strength, fracture surface formation energy, strand strength, and strand modulus of the single fibers. These results are shown in Table 3. In Table 3, "strength x elastic modulus" means strand strength x strand elastic modulus.
[0090] [Examples 2 to 5] Carbon fiber bundles were produced and various measurements were carried out in the same manner as in Example 1, except that the concentration of the coagulation bath and the maximum atmospheric temperature of the second carbonization furnace were changed as shown in Tables 1 and 2. The results are shown in Table 3.
[0091] [Comparative Example 1] An acrylic fiber precursor bundle for carbon fibers was produced in the same manner as in Example 1, except that the production conditions for the acrylic fiber precursor bundle for carbon fibers were changed as shown in Table 1 and the single fiber fineness of the acrylic fiber precursor bundle for carbon fibers was changed to 1.0 dtex. Using the obtained acrylic fiber precursor bundle for carbon fibers, a carbon fiber bundle was produced in the same manner as in Example 1, except that the production conditions for the carbon fiber bundle were changed as shown in Table 2, and various measurements were carried out. The results are shown in Table 3.
[0092] [Comparative Example 2] An acrylic fiber precursor bundle for carbon fibers was produced in the same manner as in Example 1, except that the production conditions for the acrylic fiber precursor bundle for carbon fibers were changed as shown in Table 1 and the single fiber fineness of the acrylic fiber precursor bundle for carbon fibers was changed to 0.77 dtex. Using the obtained acrylic fiber precursor bundle for carbon fibers, a carbon fiber bundle was produced in the same manner as in Example 1, except that the production conditions for the carbon fiber bundle were changed as shown in Table 2, and various measurements were carried out. The results are shown in Table 3.
[0093] [Reference Example 1] Various measurements were carried out on a commercially available carbon fiber bundle (manufactured by Toray Industries, Inc., product name "M40JB"). The results are shown in Table 3.
[0094]
[0095]
[0096]
[0097] As is clear from the results in Table 3, the carbon fiber bundles obtained in each Example had high strand strength and strand modulus, and were well-balanced. The carbon fiber bundles obtained in each Example were substantially untwisted. On the other hand, the carbon fiber bundles obtained in Comparative Examples 1 and 2 had lower fracture surface generation energy and lower strand strength and strand modulus than the carbon fiber bundles obtained in each Example. Furthermore, the commercially available carbon fiber bundle used in Reference Example 1 had a fracture surface generation energy comparable to that of the carbon fiber bundles obtained in each Example, but had a lower CF density and lower strand strength and strand modulus. Furthermore, since the diameter of the single fiber was also small, there is a concern that insufficient impregnation may occur due to the high viscosity of the matrix resin when a carbon fiber reinforced composite material is produced, resulting in a decrease in the tensile strength of the carbon fiber reinforced composite material.
[0098] The carbon fiber bundle of the present invention can exhibit high strand strength and knot strength without decreasing the elastic modulus, and the diameter of the single fiber is large, and therefore is useful in a wide range of applications requiring high mechanical properties, such as automotive components, aerospace materials, civil engineering and construction materials, sports and leisure materials, pressure vessels, wind turbine blades, and other industrial materials.
Claims
1. A carbon fiber bundle having an average diameter of carbon fiber single fibers of 5.7 μm or more and 6.5 μm or less, which is substantially untwisted, has a strand strength of 4.7 GPa or more, and has a strand elastic modulus of 320 GPa or more.
2. The carbon fiber bundle according to claim 1, which is unentangled.
3. The carbon fiber bundle according to claim 1 or 2, wherein the average void length of the carbon fiber single fiber is 22.0 nm or less.
4. The carbon fiber bundle according to any one of claims 1 to 3, wherein the crystallite size Lc of the carbon fiber single fiber is 3.7 nm or less.
5. A carbon fiber bundle according to any one of claims 1 to 4, in which the product of strand strength (unit: GPa) and strand modulus (unit: GPa) is 1650 or more.
6. The carbon fiber bundle according to any one of claims 1 to 5, having a strand strength of 4.9 GPa or more and a strand modulus of elasticity of 385 GPa or more.
7. The carbon fiber bundle according to any one of claims 1 to 6, wherein the strand elastic modulus is 390 GPa or more and 420 GPa or less.
8. The carbon fiber bundle according to any one of claims 1 to 7, having a strand strength of 5.4 GPa or more.
9. Knot strength 400N / mm 2 The carbon fiber bundle according to any one of claims 1 to 8.
10. Knot strength is 415N / mm 2 The carbon fiber bundle according to any one of claims 1 to 8.
11. The carbon fiber bundle according to any one of claims 1 to 10, having a breaking surface generation energy of 19 N / m or more.
12. The carbon fiber bundle according to any one of claims 1 to 10, having a breaking surface generation energy of 20.5 N / m or more.
13. Density is 1.79 g / cm 3 The carbon fiber bundle according to any one of claims 1 to 12.
14. A method for producing a carbon fiber bundle, comprising heating a carbon fiber precursor acrylic fiber bundle in an oxidizing atmosphere to form a flame-resistant fiber bundle, and heating the flame-resistant fiber bundle in a non-oxidizing atmosphere to form a carbon fiber bundle, wherein in the heating in the non-oxidizing atmosphere, the heating rate when heating from 1800°C to 2200°C is 200 to 500°C / min, and the average diameter of the carbon fiber single fibers contained in the obtained carbon fiber bundle is 6.5 μm or more and 8.5 μm or less.
15. The method for producing carbon fiber bundles according to claim 14, wherein the carbon fiber precursor acrylic fiber bundles and the flame-resistant fiber bundles are heated in an unentangled state.
16. The method for producing carbon fiber bundles according to claim 14 or 15, wherein the carbon fiber precursor acrylic fiber bundles and the flame-resistant fiber bundles are heated in a substantially untwisted state.
17. A method for producing a carbon fiber bundle according to any one of claims 14 to 16, comprising the following steps (1) and (2): (1) a coagulation step in which an acrylonitrile-based polymer solution is discharged into the air from a discharge hole by using a dry-wet spinning method, and then coagulated in a coagulation bath of an aqueous solution having an organic solvent concentration of 79.3% by mass or more and 82.0% by mass or less at a temperature of 10°C or less to obtain a coagulated yarn bundle containing the organic solvent; and (2) a second drawing step in which the coagulated yarn bundle obtained in the coagulation step is drawn at a draw ratio of 2.0 times to 3.2 times in a warm aqueous solution having an organic solvent concentration of 40% by mass or more and 65% by mass or less at a temperature of 75°C or more to obtain the carbon fiber precursor acrylic fiber bundle.
18. A method for producing a carbon fiber bundle according to any one of claims 14 to 17, comprising a first drawing step between the solidification step and the second drawing step, in which the solidified yarn bundle obtained in the solidification step is drawn in air at a draw ratio of 1.00 times or more and 1.20 times or less.
19. A method for producing a carbon fiber bundle according to any one of claims 14 to 18, wherein in the second drawing step, after the coagulated yarn bundle is drawn, the organic solvent is removed, and the bundle is shrunk or drawn in warm water at a temperature of 90°C or higher at a draw ratio of 0.96 to 1.30, and then drawn in a pressurized water vapor atmosphere at a draw ratio of 3.7 to 4.2 to obtain the carbon fiber precursor acrylic fiber bundle.
20. A method for producing a carbon fiber bundle according to any one of claims 14 to 19, wherein the concentration of the organic solvent in the aqueous solution used in the coagulation step is 79.8% by mass or more and 81.2% by mass or less.
21. The method for producing a carbon fiber bundle according to any one of claims 14 to 20, wherein the organic solvent is dimethylformamide.
22. A method for producing a carbon fiber bundle according to any one of claims 14 to 21, comprising the following steps (3) to (6): (3) a flame-resistant step of heating a carbon fiber precursor acrylic fiber bundle or a carbon fiber precursor acrylic fiber bundle obtained in the second drawing step in an oxidizing atmosphere to obtain a flame-resistant fiber bundle; (4) a first carbonization step of heating the flame-resistant fiber bundle obtained in the flame-resistant step in a non-oxidizing atmosphere having a temperature gradient in an atmosphere temperature range of 300°C to 900°C at an elongation rate of 4.0% to 5.0%; (5) a second carbonization step of heating the fiber bundle after the first carbonization step in a non-oxidizing atmosphere having a temperature gradient in an atmosphere temperature range of 1000°C to 1800°C while applying a tension of 0.15 cN / dtex to the fiber bundle in a non-oxidizing atmosphere. (6) A third carbonization step of heating the fiber bundle while applying a tension of 0.15 cN / dtex or more and 0.23 cN / dtex or less to the fiber bundle in a non-oxidizing atmosphere having a temperature gradient in an atmospheric temperature range of 1700°C or more and 2300°C or less after the second carbonization step.
23. The flame retardant process comprises heating the carbon fiber precursor acrylic fiber bundle or the carbon fiber precursor acrylic fiber bundle obtained in the second stretching process in an oxidizing atmosphere having a temperature gradient in a range of an atmospheric temperature of 220° C. or more and 280° C. or less at an elongation rate of 3.0% or more and 8.0% or less, and forming a carbon fiber precursor acrylic fiber bundle having a density of 1.33 g / cm 3 1.36g / cm or more 3 The method for producing a carbon fiber bundle according to claim 22, which comprises the steps of obtaining a flame-resistant fiber bundle as follows:
24. The method for producing a carbon fiber bundle according to claim 22 or 23, wherein the difference between the maximum atmospheric temperature in the second carbonization step and the inlet atmospheric temperature in the third carbonization step is 700° C. or less.
25. The method for producing a carbon fiber bundle according to claim 22 or 23, wherein the difference between the maximum atmospheric temperature in the second carbonization step and the inlet atmospheric temperature in the third carbonization step is 500° C. or less.
26. A method for producing a carbon fiber bundle according to any one of claims 14 to 25, wherein the maximum heating temperature in the heating in the non-oxidizing atmosphere is 2100 to 2300°C.
Citation Information
Patent Citations
Carbon fiber and method for producing the same
JP2002327339A
Carbon fiber bundle, manufacturing method therefor, prepeg, and carbon-fiber-reinforced composite material
WO2019203088A1
Preparation method of high-strength high-modulus wear-resisting polyacrylonitrile-based carbon fiber through dry spraying and wet spinning
CN110409018A
Prepreg, carbon fiber composite material and method for producing the same
JP2011219514A
Carbon fiber bundle and method for production of the same
JP2018145541A