Void-containing biaxially oriented polypropylene film
The optimization of polypropylene film composition and processing for biaxial orientation addresses the challenge of balancing heat resistance and rigidity, resulting in a thinner, more efficient film with reduced wrinkles and improved processing speed.
Patent Information
- Application Number
- PCT/JP2024/001657
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-05-25
- Filing Date
- 2024-01-22
- Publication Date
- 2024-11-14
AI Technical Summary
Cavity-containing biaxially oriented polypropylene films struggle to balance heat resistance with film rigidity and thickness, leading to issues like wrinkles and misalignment during heat sealing, while also being heavier than desired.
A polypropylene film composition with a polypropylene resin as the main component, incorporating a cavity developing agent and a surface layer, optimized for biaxial orientation to achieve a balance of heat resistance, rigidity, and reduced thickness, using specific resin properties and processing methods to enhance crystallinity and molecular alignment.
The film exhibits improved heat resistance, reduced heat shrinkage, and increased rigidity, allowing for thinner designs suitable for various applications like labeling and packaging, with reduced wrinkles and enhanced line speed in bag-making processes.
Smart Images

Figure JPOXMLDOC01-APPB-T000001 
Figure JPOXMLDOC01-APPB-T000002 
Figure JPOXMLDOC01-APPB-T000003
Abstract
Description
Void-containing biaxially oriented polypropylene film
[0001] The present invention relates to a void-containing biaxially oriented polypropylene film, and more particularly to a void-containing biaxially oriented polypropylene film that can be widely used for labels, adhesives, release agents, and packaging.
[0002] The void-containing biaxially oriented polypropylene film has minute voids inside the film, which gives it opacity and cushioning properties, and it is used as synthetic paper for packaging materials, labels, and image receiving paper for printing.
[0003] Methods for forming fine voids in biaxially oriented polypropylene films include: (1) adding an inorganic filler and forming voids by peeling it off from the resin during the stretching process; (2) adding microcapsules and forming voids by generating gas through heat; and (3) adding a solvent-soluble substance and, after film formation, immersing the film in a solvent to melt and remove the soluble substance to form voids. However, the most widely used method in practice is to add inorganic particles such as calcium carbonate to the resin as a void-forming agent and utilize the interfacial peeling that occurs at the interface between the void-forming agent and the resin during stretching (see, for example, Patent Documents 1 to 5, etc.).
[0004] When a void-containing biaxially oriented polypropylene film is used as a packaging material, heat resistance during processing is important. For example, a void-containing biaxially oriented polypropylene film that is improved in terms of wrinkles and displacement due to heat shrinkage during heat sealing has been proposed (see, for example, Patent Document 6).
[0005] However, recently, there has been a demand for thinner films while maintaining not only heat resistance but also film strength for void-containing biaxially oriented polypropylene films, but there has been no film that satisfies these requirements.
[0006] JP 55-126056, JP 2005-22300, JP 1-4338, JP 11-5852, JP 2003-231225, WO 15 / 012308
[0007] The present invention has been made in view of the problems of the prior art. That is, an object of the present invention is to provide a void-containing biaxially oriented polypropylene film that not only has heat resistance even at high temperatures but also has higher film rigidity. Another object of the present invention is to provide a void-containing biaxially oriented polypropylene film that not only has heat resistance even at high temperatures but also has higher film rigidity and is lighter in weight.
[0008] The present inventors have conducted extensive research to achieve the above object and have discovered the present invention. Specifically, the void-containing biaxially oriented polypropylene film of the present invention is: [1] A void-containing biaxially oriented polypropylene film comprising a polypropylene resin as a main component and a polypropylene resin composition containing at least a void-producing agent, and satisfying the following (1) to (3): (1) an apparent density of 0.65 g / cm 3 Above, 0.85g / cm 3 (2) The stress at 5% elongation in the longitudinal direction of the film (F5MD) at 23°C is 25 MPa or more, and the stress at 5% elongation in the width direction of the film (F5TD) at 23°C is 110 MPa or more. (3) The heat shrinkage in the longitudinal direction at 150°C is 6% or less, and the heat shrinkage in the width direction at 150°C is 10% or less. [2] A void-containing biaxially oriented polypropylene film having a base layer A made of a polypropylene resin composition containing a polypropylene resin as a main component and at least a void-producing agent, and a surface layer B made of a polypropylene resin composition on at least one side thereof, which satisfies the following (1) to (3). (1) The apparent density is 0.65 g / cm 3 Above, 0.85g / cm 3(2) The stress at 5% elongation in the longitudinal direction of the film (F5MD) at 23°C is 25 MPa or more, and the stress at 5% elongation in the width direction of the film (F5TD) at 23°C is 110 MPa or more. (3) The heat shrinkage rate in the longitudinal direction at 150°C is 6% or less, and the heat shrinkage rate in the width direction at 150°C is 10% or less. [3] A void-containing biaxially oriented propylene film made of a polypropylene resin composition containing a polypropylene resin as the main component and at least a void-developing agent, which satisfies the following (1) to (3): (1) The apparent density is 0.65 g / cm 3 Above, 0.85g / cm 3 (2) The stress at 5% elongation in the longitudinal direction of the film (F5MD) at 23°C is 25 MPa or more, and the stress at 5% elongation in the width direction of the film (F5TD) at 23°C is 110 MPa or more. (3) The heat shrinkage rate in the longitudinal direction at 150°C is 6% or less, and the heat shrinkage rate in the width direction at 150°C is 10% or less. [4] A void-containing biaxially oriented polypropylene film having a base layer A made of a polypropylene resin composition containing a polypropylene resin as a main component and at least a void-producing agent, and having a surface layer B made of a polypropylene resin composition on at least one side thereof, and satisfying the following (1) to (3): (1) The apparent density is 0.65 g / cm 3 Above, 0.85g / cm 3 (2) The stress at 5% elongation in the longitudinal direction of the film (F5MD) at 23°C is 25 MPa or more, and the stress at 5% elongation in the width direction of the film (F5TD) at 23°C is 110 MPa or more. (3) The heat shrinkage rate in the longitudinal direction at 150°C is 6% or less, and the heat shrinkage rate in the width direction at 150°C is 10% or less. [5] The void-containing biaxially oriented polypropylene film according to any one of [1] to [4], wherein the total light transmittance of the void-containing biaxially oriented polypropylene film is 40% or less. [6] The void-containing biaxially oriented polypropylene film according to any one of [1] to [5], wherein the total thickness of the void-containing biaxially oriented polypropylene film is 5 μm or more and 100 μm or less.
[0009] The void-containing biaxially oriented polypropylene film of the present invention not only has heat resistance but also has high film rigidity, allowing it to be made thinner and used in a wide range of applications, including labeling, adhesives, release agents, and packaging. Furthermore, because of its excellent heat resistance, when used as a packaging material, for example, it reduces wrinkling and slippage due to heat shrinkage during heat sealing, allowing the heat sealing temperature to be set higher. This also makes it possible to increase the line speed in bag-making processes.
[0010] The void-containing biaxially oriented polypropylene film of the present invention will be described in more detail below. The void-containing biaxially oriented polypropylene film of the present invention is composed of a polypropylene resin composition containing a polypropylene resin as the main component and at least a void-producing agent. The term "main component" refers to a polypropylene resin content of 60% by mass or more in the polypropylene resin composition, more preferably 70% by mass or more, even more preferably 75% by mass or more, and particularly preferably 80% by mass or more. A second embodiment of the biaxially oriented polypropylene film may include a substrate layer A composed of a polypropylene resin composition containing a polypropylene resin as the main component and at least a void-producing agent, and a surface layer B composed of a polypropylene resin composition on at least one side. The surface layer B may be present on one or both sides, and the surface layer B is composed of a polypropylene resin composite containing a polypropylene resin as the main component. The term "main component" refers to a polypropylene resin content of 60% by mass or more in the polypropylene resin composition, more preferably 70% by mass or more, even more preferably 75% by mass or more, and particularly preferably 80% by mass or more.
[0011] The polypropylene resin composition constituting the void-containing biaxially oriented polypropylene film of the first embodiment of the present invention and the polypropylene resin composition constituting the base layer A of the void-containing biaxially oriented polypropylene film of the second embodiment of the present invention are described below. (Polypropylene Resin) The polypropylene resin used as the main component of the polypropylene resin composition can be a polypropylene homopolymer or a copolymer with ethylene and / or an α-olefin having 4 or more carbon atoms. A propylene homopolymer that is substantially free of ethylene and / or an α-olefin having 4 or more carbon atoms is preferred. Even if ethylene and / or an α-olefin having 4 or more carbon atoms is contained, the amount of ethylene and / or an α-olefin having 4 or more carbon atoms is preferably 1 mol% or less, more preferably 0.5 mol% or less, even more preferably 0.3 mol% or less, and particularly preferably 0.1 mol% or less. Within this range, crystallinity is likely to be improved. Examples of the α-olefin component having 4 or more carbon atoms that constitutes such a copolymer include 1-butene, 1-pentene, 3-methylpentene-1, 3-methylbutene-1, 1-hexene, 4-methylpentene-1, 5-ethylhexene-1, 1-octene, 1-decene, 1-dodecene, 1-tetradecene, 1-hexadecene, 1-heptadecene, 1-octadecene, 1-eicosene, etc. The polypropylene resin used as the main component of the polypropylene resin composition may be a mixture of two or more different polypropylene homopolymers, a copolymer with ethylene and / or an α-olefin having 4 or more carbon atoms, or a mixture thereof.
[0012] (Stereoregularity of Polypropylene Resin) The mesopentad fraction (hereinafter sometimes abbreviated as mmmm%), which is an index of the stereoregularity of the polypropylene resin used as the main component of the polypropylene resin composition, is preferably in the range of 97.5 to 99.9%, more preferably in the range of 98.5 to 99.7%, even more preferably in the range of 98.5 to 99.5%, and particularly preferably in the range of 98.5 to 99.3%. When it is 97.5% or more, the crystallinity of the polypropylene resin is increased, and the melting point, crystallinity, and crystal orientation of the crystals in the film are improved, making it easier to obtain rigidity and heat resistance at high temperatures. When it is 99.9% or less, it is easier to reduce costs in terms of polypropylene production and makes it less likely to break during film formation. The mesopentad fraction is measured by nuclear magnetic resonance spectroscopy (the so-called NMR method). In order to set the mesopentad fraction of the polypropylene resin used as the main component of the polypropylene resin composition within the above-mentioned range, a method of washing the obtained polypropylene resin powder with a solvent such as n-heptane, a method of appropriately selecting a catalyst and / or co-catalyst, and a method of appropriately selecting the components of the polypropylene resin composition, and the like are preferably employed.
[0013] (Melting temperature of polypropylene resin) The lower limit of the melting temperature (hereinafter sometimes abbreviated as Tm) of the polypropylene resin used as the main component of the polypropylene resin composition, measured by DSC, is preferably 160°C or higher, more preferably 161°C or higher, even more preferably 162°C or higher, still more preferably 163°C or higher, and particularly preferably 164°C or higher. When Tm is 160°C or higher, rigidity and heat resistance at high temperatures are easily obtained. The upper limit of Tm is preferably 170°C or lower, more preferably 169°C or lower, even more preferably 168°C or lower, still more preferably 167°C or lower, and particularly preferably 166°C or lower. When Tm is 170°C or lower, it is easy to suppress cost increases in terms of polypropylene production, and breakage during film formation is less likely. The melting temperature can also be further increased by blending a crystal nucleating agent with the polypropylene resin. Tm is the main peak temperature of the endothermic peak accompanying melting, which is observed when 5 mg of polypropylene resin is packed into an aluminum pan, set in a differential scanning calorimeter (DSC), heated from 30°C to 230°C at a heating rate of 10°C / min under a nitrogen atmosphere, and held at 230°C for 5 minutes to melt the resin composition, then cooled to 30°C at a heating rate of -10°C / min, held at 30°C for 5 minutes, and then heated again at a heating rate of 10°C / min.
[0014] (Crystallization Temperature of Polypropylene Resin) The lower limit of the crystallization temperature (hereinafter sometimes abbreviated as Tc) of the polypropylene resin used as the main component of the polypropylene resin composition, measured by DSC, is preferably 105°C or higher, more preferably 108°C or higher, and even more preferably 110°C or higher. If Tc is 105°C or higher, crystallization is likely to proceed during cooling after width direction stretching and the subsequent heat treatment step, making it easier to obtain rigidity and heat resistance at high temperatures. The upper limit of Tc is preferably 135°C or lower, more preferably 133°C or lower, even more preferably 132°C or lower, still more preferably 130°C or lower, particularly preferably 128°C or lower, and most preferably 127°C or lower. If Tc is 135°C or lower, it is less likely to increase the cost of polypropylene production and less likely to break during film formation. The crystallization temperature can also be further increased by blending a crystal nucleating agent into the polypropylene resin. Tc is the main peak temperature of the exothermic peak observed when 5 mg of polypropylene resin is packed into an aluminum pan, set in a differential scanning calorimeter (DSC), heated from 30°C to 230°C at a heating rate of 10°C / min in a nitrogen atmosphere, and held at 230°C for 5 minutes to melt the resin composition, and then cooled to 30°C at a cooling rate of -10°C / min.
[0015] (Melt Flow Rate of Polypropylene Resin) The lower limit of the melt flow rate (MFR) (230°C, 2.16 kgf) of the polypropylene resin used as the main component of the polypropylene resin composition is preferably 5.0 g / 10 min or more, more preferably 5.5 g / 10 min or more, even more preferably 6.0 g / 10 min or more, particularly preferably 6.3 g / 10 min or more, and most preferably 6.5 g / 10 min or more. When the melt flow rate (MFR) of the polypropylene resin is 5.0 g / 10 min or more, the amount of low molecular weight components in the polypropylene resin constituting the film increases, which makes it easier to increase the crystallinity of the film and also reduces entanglement of polypropylene molecular chains in the amorphous portion, making it easier to reduce the heat shrinkage rate. In order to make the melt flow rate (MFR) of the polypropylene resin within the above range, a method of controlling the average molecular weight or molecular weight distribution of the polypropylene resin is preferably adopted.
[0016] That is, the lower limit of the amount of components having a molecular weight of 100,000 or less in the GPC cumulative curve of the polypropylene resin used as the main component of the polypropylene resin composition is preferably 35% by mass or more, more preferably 38% by mass or more, even more preferably 40% by mass or more, particularly preferably 41% by mass or more, and most preferably 42% by mass or more. The upper limit of the amount of components having a molecular weight of 100,000 or less in the GPC cumulative curve is preferably 65% by mass or less, more preferably 60% by mass or less, and even more preferably 58% by mass or less. When the amount of components having a molecular weight of 100,000 or less in the GPC cumulative curve is 65% by mass or less, film strength is less likely to decrease. In this case, if the polypropylene resin contains high-molecular-weight components or long-chain branched components having a long relaxation time, the amount of components having a molecular weight of 100,000 or less contained in the polypropylene resin can be easily adjusted without significantly changing the overall viscosity, which makes it easy to improve film formability without significantly affecting rigidity or thermal shrinkage.
[0017] (Molecular Weight Distribution of Polypropylene Resin) The lower limit of the weight average molecular weight (Mw) / number average molecular weight (Mn), which is an index of the breadth of the molecular weight distribution of the polypropylene resin composition, is preferably 3.0 or more, more preferably 3.3 or more, and even more preferably 3.5 or more. The upper limit of Mw / Mn is preferably 20 or less, more preferably 15 or less, and even more preferably 12 or less. When the Mw / Mn of the polypropylene resin composition is 3.0 or more, the proportion of high molecular weight components with long relaxation times increases, making it easier to maintain film formability. Furthermore, when the Mw / Mn of the polypropylene resin composition is 20 or less, it is easier to obtain a biaxially oriented polypropylene film with a low heat shrinkage rate. Mw / Mn can be obtained using gel permeation chromatography (GPC).
[0018] The molecular weight distribution of polypropylene resins can be adjusted by polymerizing components of different molecular weights in a series of plants in multiple stages, blending components of different molecular weights offline in a kneader, polymerizing by blending catalysts with different performances, or using a catalyst that can achieve the desired molecular weight distribution. The shape of the molecular weight distribution obtained by GPC may be a smooth molecular weight distribution with a single peak in a GPC chart with the logarithm (log M) of molecular weight (M) on the horizontal axis and the differential distribution value (weight fraction per log M) on the vertical axis, or a molecular weight distribution with multiple peaks or shoulders. In the polypropylene resin composition, the above polypropylene resins may be used alone, or multiple different polypropylene resins may be mixed and used. Mainly using polypropylene resins characterized by the above-mentioned stereoregularity and molecular weight not only facilitates peeling at the interface with the void-producing agent, but also increases the volume of the voids, making it easier to reduce the apparent density.
[0019] (Void-Generating Agent) The polypropylene resin composition is primarily composed of polypropylene resin, and it is preferable to add a void-generating agent to form voids. Preferred void-generating agents include inorganic fine particles such as calcium carbonate and kaolin, and organic fine particles such as crosslinked polymethyl acrylate, with calcium carbonate being particularly preferred. The surfaces of these particles can be subjected to various surface treatments, and these can be used alone or in combination of two or more. Alternatively, a resin that is incompatible with polypropylene resin, such as a polycarbonate resin or a polystyrene resin, can be blended to form a sea-island structure during melt extrusion, dispersing the incompatible resin in the form of fine particles to form a void-generating agent. The amount of void-generating agent in the polypropylene resin composition is preferably 0.1% by mass or more and 25% by mass or less, more preferably 1.0% by mass or more and 15% by mass or less, and even more preferably 2.0% by mass to 10% by mass. When the void-generating agent is 0.1% by mass or more, a sufficient amount of voids is formed, resulting in improved hiding power and cushioning properties. When the void generating agent is 25% by mass or less, breakage during film formation is less likely to occur, improving productivity. Furthermore, fisheyes and foreign matter are reduced, resulting in improved surface appearance. Furthermore, since there are not too many cavities, surface strength is maintained, rigidity is not reduced, and firmness is maintained. The average particle size of the void generating agent is preferably 0.2 μm or more and 10 μm or less, and particularly preferably 0.5 μm or more and 5 μm or less. At 0.2 μm or more, cavities are easily formed, while at 10 μm or less, fisheyes and foreign matter are reduced, and surface appearance is maintained. The average particle size of the void generating agent described above was measured using a Microtrac HRA X-100, and the average particle size of the void generating agent can be measured using a Microtrac HRA X-100.
[0020] (Making Agent) The polypropylene resin composition can contain inorganic or organic fine particles to enhance hiding power. Examples of inorganic fine particles include titanium dioxide, tungsten oxide, silica, and zeolite, with titanium dioxide being particularly preferred. The shape of the masking agent is not particularly limited, and may be spherical, cubic, ellipsoidal, conical, or irregular. Various surface treatments can be applied to the surface of these masking agent particles to improve their dispersibility in the polypropylene resin. The masking agent particles can be used alone or in combination of two or more. The amount of masking agent in the polypropylene resin composition is preferably 0.1% by mass or more and 20% by mass or less, more preferably 0.5% by mass or more and 15% by mass or less, and even more preferably 1.0% by mass or more and 10% by mass or less. When the amount of masking agent is 0.1% by mass or more, sufficient hiding power is easily obtained. When the amount of masking agent is 20% by mass or less, breakage is less likely to occur during film formation, and productivity is maintained. Furthermore, fisheyes and foreign matter are reduced, and the surface appearance is maintained. The average particle size of the opacifying agent fine particles is preferably 0.10 μm or more and 1.0 μm or less, and particularly preferably 0.20 μm or more and 0.50 μm or less. When the average particle size of the opacifying agent fine particles is 0.10 μm or more, a hiding effect can be obtained. Even when the average particle size is 1.0 μm or less, a hiding effect can be obtained. The average particle size of the opacifying agent fine particles was measured using a Microtrac HRA X-100.
[0021] (Other Additives) Additives and other resins may be added to the polypropylene resin composition as needed. Examples of additives include antioxidants, UV absorbers, antistatic agents, lubricants, nucleating agents, adhesives, antifogging agents, flame retardants, and antiblocking agents. Examples of other resins include polypropylene resins other than the specific polypropylene resin used in the present invention, random copolymers of propylene and ethylene and / or α-olefins having 4 or more carbon atoms, and various elastomers. The amount of other additives in the polypropylene resin composition is preferably 5% by mass or less, and the amount of other resins added is preferably 5% by mass or less of the resin composition constituting the void-containing biaxially oriented polypropylene film. The other additives and other resins can be blended with the polypropylene resin using a Henschel mixer or the like, or master pellets prepared in advance using a melt kneader can be diluted with polypropylene to the desired concentration, or the entire amount can be melt-kneaded in advance.
[0022] By using a resin composition primarily composed of the aforementioned polypropylene resin, the crystallinity of the void-containing biaxially oriented polypropylene film can be increased, thereby reducing the heat shrinkage rate at high temperatures. This allows for higher stretching ratios than conventional techniques, which had concerns about increased heat shrinkage rates, and has succeeded in increasing the rigidity of the void-containing biaxially oriented polypropylene film. Furthermore, using a resin composition primarily composed of the aforementioned polypropylene resin not only facilitates peeling at the interface with the void-producing agent, but also increases the volume of the voids, making it easier to reduce the apparent density. Therefore, it is possible to reduce the apparent density using the same amount of void-producing agent as before.
[0023] (Surface Layer B) Next, the polypropylene resin composition constituting the surface layer B of the void-containing biaxially oriented polypropylene film of the second embodiment will be described. The surface layer B is mainly composed of polypropylene resin, and is provided for the purpose of improving the gloss of the film, providing heat sealability, and adhesion to the functional layer to the film surface. The properties of the polypropylene resin can be adjusted depending on the purpose, and various additives other than the polypropylene resin can also be contained.
[0024] When the surface layer B is used to impart gloss to the film, the polypropylene resin and additives that are suitable for use in the base layer A described above can basically be used, but it is preferable not to contain a cavity-forming agent in order to efficiently impart gloss.
[0025] When the surface layer B is used to impart heat sealability to the film, the surface layer B preferably comprises a polypropylene-based resin composition containing as a main component a polypropylene-α-olefin copolymer having 4 mol% or more of ethylene and / or α-olefins having 4 or more carbon atoms. The term "main component" means that the proportion of the polypropylene resin in the polypropylene-based resin composition is 70% by mass or more, more preferably 80% by mass or more, even more preferably 90% by mass or more, and even more preferably 95% by mass or more.
[0026] The polypropylene-α-olefin copolymer containing 4 mol% or more of ethylene and / or α-olefins having 4 or more carbon atoms is preferably at least one polypropylene copolymer selected from the group consisting of propylene-butene copolymer, propylene-ethylene-butene copolymer, and propylene-ethylene copolymer. The polypropylene-α-olefin copolymer containing 4 mol% or more of ethylene and / or α-olefins having 4 or more carbon atoms preferably has a melting point of 135°C or less. A melting point of 135°C or less makes it easy to lower the heat seal rise temperature and also to improve the maximum heat seal strength.
[0027] The lower limit of the melt flow rate (MFR) (230°C, 2.16 kgf) of the polypropylene-α-olefin copolymer containing 4 mol% or more of ethylene and / or α-olefins having 4 or more carbon atoms is preferably 5.0 g / 10 min or more, more preferably 5.5 g / 10 min or more, even more preferably 6.0 g / 10 min or more, and particularly preferably 6.3 g / 10 min or more. The upper limit is preferably 8.0 g / 10 min or less, more preferably 7.5 g / 10 min or less, even more preferably 7.0 g / 10 min or less, and particularly preferably 6.8 g / 10 min or less. When the polypropylene resin composition constituting the surface layer B contains 70 mass% or more of the polypropylene-α-olefin copolymer containing 4 mol% or more of ethylene and / or α-olefins having 4 or more carbon atoms, the maximum heat seal strength attained can be increased, and the hermeticity of the bag after bag formation can be easily improved.
[0028] Preferred embodiments of polypropylene-α-olefin copolymers containing 4 mol% or more of ethylene and / or α-olefins having 4 or more carbon atoms are shown below. (Propylene-Butene Copolymer) The butene content in the propylene-butene copolymer is preferably 20 mol% or more. By making it 20 mol% or more, it is easy to increase the heat seal strength and improve the sealability. There is no particular upper limit for the butene content, but if the butene content is too high, the film surface may become sticky and the slipperiness and blocking resistance may decrease, so it may be determined appropriately within a range that does not cause such defects. Examples of propylene-butene copolymers with a high butene content include "SPX78J1" manufactured by Sumitomo Chemical Co., Ltd. and "XR110H" manufactured by Mitsui Chemicals, Inc.
[0029] (Propylene-ethylene-butene copolymer) The butene content in the propylene-ethylene-butene copolymer is preferably 5 mol% or more. The upper limit of the butene content is not particularly limited, but if the butene content is too high, the film surface may become sticky, and the slipperiness and blocking resistance may decrease. Therefore, the upper limit may be appropriately determined within a range that does not cause such defects. An example of the propylene-ethylene-butene copolymer with a high butene content is "FSX66E8" manufactured by Sumitomo Chemical Co., Ltd.
[0030] (Propylene-ethylene copolymer) The ethylene content in the propylene-ethylene copolymer is preferably 4 mol% or more. The upper limit of the ethylene content is not particularly limited, but if the ethylene content is too high, the film surface may become sticky, and the slipperiness and blocking resistance may decrease. Therefore, the upper limit may be appropriately determined within a range that does not cause such defects. Examples of the propylene-ethylene copolymer with a high ethylene content include "PC540R" manufactured by SunAllomer Co., Ltd. and "VM3588FL" manufactured by Mitsui Chemicals, Inc.
[0031] The amount of ethylene and / or α-olefins having 4 or more carbon atoms in the polypropylene-α-olefin copolymer is preferably 4.5 mol% or more, more preferably 5.0 mol% or more, and even more preferably 5.5 mol% or more. The amount of ethylene and / or α-olefins having 4 or more carbon atoms in the polypropylene-α-olefin copolymer is preferably 10 mol% or less, more preferably 8.0 mol% or less.
[0032] (Additives) As long as the effects of the present invention are not impaired, the polypropylene resin composition constituting the surface layer B may contain various additives for improving qualities such as slipperiness and antistatic properties, such as lubricants such as wax and metal soap, plasticizers, processing aids, and known heat stabilizers, antioxidants, antistatic agents, and ultraviolet absorbers that are commonly added to polypropylene films.
[0033] The functional layer is a layer having at least one function such as coating properties, design properties, water vapor barrier properties, oxygen barrier properties, thermal conductivity, low dielectric properties, high dielectric properties, and heat resistance, and examples thereof include a vapor deposition layer, a coating layer, and a printed layer. When the surface layer B is used to impart adhesion to the functional layer to the film, it preferably contains 25% by mass to 85% by mass of a mid-melting point polypropylene resin, which can improve adhesion to the vapor deposition layer, the coating layer, and the like. When the melting point of the mid-melting point polypropylene resin is 158°C or less, adhesion to the functional layer can be improved. When the melting point is 130°C or higher, productivity during film formation can be ensured and roughness of the film surface can be suppressed. The melting point of the mid-melting point polypropylene resin is preferably 134°C or higher and 150°C or lower, more preferably 138°C or higher and 143°C or lower. When the content of the mid-melting point polypropylene resin is 25% by mass or higher, adhesion to the vapor deposition layer, the coating layer, and the like can be improved. By setting the content of the mid-melting point polypropylene resin to 85% by mass or less, productivity can be ensured during film production, and roughening of the film surface can be suppressed. The surface layer B preferably contains 30% by mass or more and 80% by mass or less of the mid-melting point polypropylene resin, and more preferably 35% by mass or more and 75% by mass or less.
[0034] On the other hand, the surface layer B preferably contains a high-melting-point polypropylene resin having a melting point higher than that of the mid-melting-point polypropylene resin in order to maintain the thermal dimensional stability and mechanical strength of the biaxially oriented polypropylene film. The high-melting-point polypropylene resin preferably has a melting point of 160°C or higher and 170°C or lower, and more preferably 161°C or higher and 165°C or lower. The surface layer B preferably contains 15% by mass or higher and 75% by mass or lower, more preferably 20% by mass or higher and 70% by mass or lower, and even more preferably 25% by mass or higher and 65% by mass or lower, of the high-melting-point polypropylene resin.
[0035] When the surface layer B also contains a high-melting point polypropylene resin, the total amount of the high-melting point polypropylene resin and the mid-melting point polypropylene resin relative to the total resin contained in the surface layer B is preferably 60 to 100 mass%, more preferably 70 to 100 mass%, even more preferably 80 to 100 mass%, even more preferably 90 to 100 mass%, particularly preferably 95 to 100 mass%, and most preferably 98 to 100 mass%.
[0036] Various suitable physical properties of the mid-melting point polypropylene resin and the high-melting point polypropylene resin are described below. When two or more different polypropylene resins are used as the mid-melting point polypropylene resin, it is preferable that the mass-averaged physical properties of each polypropylene resin fall within the numerical ranges described below. When two or more different polypropylene resins are used as the high-melting point polypropylene resin, it is preferable that the mass-averaged physical properties of each polypropylene resin fall within the numerical ranges described below.
[0037] The melt flow rate (MFR; 230°C, 2.16 kgf) of the mid-melting point polypropylene resin is preferably 2.0 g / 10 min or more and 10 g / 10 min or less, more preferably 3.0 g / 10 min or more and 8.0 g / 10 min or less, and even more preferably 4.0 g / 10 min or more and 7.0 g / 10 min or less. The melt flow rate (MFR; 230°C, 2.16 kgf) of the high-melting point polypropylene resin is preferably 2.0 g / 10 min or more and 10 g / 10 min or less, more preferably 3.0 g / 10 min or more and 6.0 g / 10 min or less. Furthermore, the difference between the MFR of the mid-melting point polypropylene resin and the MFR of the high-melting point polypropylene resin is preferably 2.0 g / 10 min or less, more preferably 1.5 g / 10 min or less.
[0038] The weight-average molecular weight (Mw) of the mid-melting point polypropylene resin is preferably 180,000 to 500,000. It is more preferably 190,000 to 320,000, even more preferably 200,000 to 300,000, and particularly preferably 230,000 to 260,000. If the Mw is less than 180,000, the melt viscosity is low, which may result in instability during casting and poor film formability. If the Mw exceeds 500,000, the amount of components with a molecular weight of 100,000 or less becomes too small, which may result in a reduced heat shrinkage rate at high temperatures.
[0039] The Mw of the high-melting-point polypropylene resin is preferably 180,000 to 500,000. It is more preferably 210,000 to 400,000, even more preferably 240,000 to 350,000, and particularly preferably 270,000 to 320,000. If the Mw is less than 180,000, the melt viscosity is low, which may result in instability during casting and poor film formability. If the Mw exceeds 500,000, the amount of components with a molecular weight of 100,000 or less becomes too small, which may result in a reduced heat shrinkage rate at high temperatures. It is also preferable that the Mw of the high-melting-point polypropylene resin be higher than that of the mid-melting-point polypropylene resin.
[0040] The number average molecular weight (Mn) of the mid-melting point polypropylene resin is preferably 20,000 to 200,000. It is more preferably 30,000 to 80,000, even more preferably 40,000 to 70,000, and particularly preferably 45,000 to 55,000. If Mn is less than 20,000, the melt viscosity is low, which may result in instability during casting and poor film formability. If Mn exceeds 200,000, the heat shrinkage rate at high temperatures may be reduced.
[0041] The Mn of the high-melting point polypropylene resin is preferably 20,000 to 200,000. It is more preferably 30,000 to 80,000, even more preferably 40,000 to 70,000, and particularly preferably 50,000 to 60,000. If the Mn is less than 20,000, the melt viscosity is low, which may result in instability during casting and poor film formability. If the Mn exceeds 200,000, the heat shrinkage rate at high temperatures may decrease. It is also preferable that the Mn of the high-melting point polypropylene resin is higher than the Mn of the mid-melting point polypropylene resin.
[0042] The molecular weight distribution (Mw / Mn) of the mid-melting point polypropylene resin is preferably 2.8 to 10, more preferably 3.2 to 9.0, even more preferably 3.5 to 9.0, particularly preferably 4.0 to 8.0, and most preferably 4.5 to 6.0. The molecular weight distribution (Mw / Mn) of the high-melting point polypropylene resin is preferably 2.8 to 10, more preferably 3.2 to 9.0, even more preferably 3.5 to 9.0, particularly preferably 3.7 to 8.0, and most preferably 4.0 to 6.0. It is also preferable that the Mw / Mn of the high-melting point polypropylene resin is larger than the Mw / Mn of the mid-melting point polypropylene resin.
[0043] High-melting-point polypropylene resins, mid-melting-point polypropylene resins, and low-melting-point polypropylene resins are obtained by polymerizing the raw material propylene using known catalysts such as Ziegler-Natta catalysts and metallocene catalysts. To obtain a mid-melting-point polypropylene resin having a melting point of 130°C or higher and 158°C or lower, ethylene and / or an α-olefin having 4 or more carbon atoms may be copolymerized, or a polypropylene resin with reduced stereoregularity may be used depending on the catalyst used. The content of α-olefin components other than propylene in the mid-melting-point polypropylene resin (the total amount of ethylene and α-olefins having 4 or more carbon atoms) is preferably 0 to 15 mol%, more preferably 2 to 10 mol%.
[0044] The surface layer B may contain additives or other resins other than polypropylene resin. Examples of additives include antiblocking agents, antioxidants, UV absorbers, nucleating agents, adhesives, antifogging agents, flame retardants, inorganic or organic fillers, etc. From the viewpoint of imparting slip properties and antiblocking properties to the surface layer B, the surface layer B preferably contains an antiblocking agent. Examples of other resins include polyolefin resins other than the polypropylene resin used in the surface layer B and various elastomers. These may be sequentially polymerized using a multi-stage reactor, blended with polypropylene resin using a Henschel mixer, master pellets prepared in advance using a melt kneader may be diluted with polypropylene to a predetermined concentration, or the entire amount may be melt kneaded in advance and used. With respect to the total resin contained in the surface layer B, the total amount of the high-melting point polypropylene resin and the mid-melting point polypropylene resin is preferably 70 to 100 mass%, more preferably 80 to 100 mass%, even more preferably 90 to 100 mass%, particularly preferably 95 to 100 mass%, and most preferably 98 to 100 mass%.
[0045] The antiblocking agent can be appropriately selected from inorganic and organic particles. Among these, silicon compounds are particularly preferred. Examples of silicon compounds include silica, silicates, and compounds having a main skeleton formed by siloxane bonds. Porous silica microparticles are particularly preferred. When using porous silica, those with a pore volume of 0.8 mL / g or more and 2 mL / g or less are preferred, and those with a pore volume of 1.1 mL / g or more and 1.8 mL / g or less are more preferred. The particle shape may be spherical or irregular, with irregular shapes being preferred. The average particle size of the particles is preferably 1 μm or more and 5 μm or less, more preferably 2 μm or more and 4 μm or less. The average particle size is determined by taking a photograph using a scanning electron microscope and measuring the Feret's diameter in the horizontal direction using an image analyzer. The content of the antiblocking agent is preferably 100 ppm to 10,000 ppm, more preferably 300 ppm to 6,000 ppm, even more preferably 800 ppm to 4,000 ppm, and particularly preferably 1,200 ppm to 2,700 ppm, based on the total mass of the surface layer B. By setting the content within the above ranges, the three-dimensional average roughness and Martens hardness of the surface layer B can be controlled. At 100 ppm or more, the film has excellent slip properties and anti-blocking properties, while at 10,000 ppm or less, the excessive addition of the antiblocking agent is unlikely to result in a decrease in light transmittance, or the antiblocking agent penetrating the functional layer when laminating the functional layer, or the antiblocking agent protruding from the surface layer B is unlikely to cause the functional layer formed near the surface layer B to become sparse, resulting in poor functional expression of the functional layer, such as a decrease in barrier properties or poor adhesion.
[0046] When the surface layer B contains an antiblocking agent, the dropout rate of the antiblocking agent in the surface layer B is preferably 10% or less, more preferably 8% or less, even more preferably 6% or less, and particularly preferably 4% or less. A dropout rate of 10% or less can prevent guide roll contamination during post-processing such as coating or vapor deposition. Furthermore, the generation of voids due to dropout of the antiblocking agent can be prevented, and a laminate with excellent gas barrier properties can be obtained when metal and / or metal oxide is vapor-deposited. The lower limit of the dropout rate is not particularly limited, but is, for example, 0.3% or more.
[0047] (Thickness Configuration of Base Material Layer A and Surface Layer B) The lower limit of the thickness of the surface layer B varies depending on the application and method of use, but is preferably 0.5 μm or more, more preferably 0.8 μm or more, and even more preferably 1.0 μm or more in terms of the functional expression of the surface layer B. The upper limit of the thickness of the surface layer B varies depending on the application and method of use, but is preferably 4 μm or less, more preferably 3 μm or less in terms of rigidity, heat resistance at high temperatures, light weight, and hiding power.
[0048] The lower limit of the ratio of the thickness of the base layer A to the thickness of the entire film is preferably 70% or more, more preferably 75% or more, even more preferably 80% or more, and particularly preferably 85% or more, from the viewpoints of rigidity, heat resistance at high temperatures, light weight, and hiding power. The upper limit of the ratio of the thickness of the base layer A to the thickness of the entire film is preferably 98% or less, more preferably 95% or less, and even more preferably 92% or less, in order to maintain the function of the surface layer B.
[0049] The lower limit of the ratio of the thickness of the surface layer B to the thickness of the entire film is preferably 2% or more, more preferably 3% or more, even more preferably 5% or more, and particularly preferably 8% or more, in terms of the functional expression of the surface layer B. The upper limit of the ratio of the thickness of the base layer B to the thickness of the entire film is preferably 30% or less, more preferably 23% or less, even more preferably 20% or less, and particularly preferably 15% or less, in terms of rigidity, heat resistance at high temperatures, light weight, and hiding power.
[0050] (Layer Structure) The layer structure of the biaxially oriented laminated polyolefin film of the present invention may be surface layer B / substrate layer A or surface layer B / substrate layer A / surface layer B. The substrate layer A and the surface layer B are preferably in direct contact with each other, but an intermediate layer may be provided between the substrate layer A and the surface layer B. The raw material composition of the intermediate layer is preferably intermediate between the substrate layer A and the surface layer B. By doing so, for example, peeling between the substrate layer A and the surface layer B can be made less likely to occur, and the lamination strength and heat seal strength can be improved.
[0051] By using a resin composition primarily composed of the aforementioned polypropylene resin, the crystallinity of the void-containing biaxially oriented polypropylene film can be increased, thereby reducing the heat shrinkage rate at high temperatures. This allows for higher stretching ratios than conventional techniques, which had concerns about increased heat shrinkage rates, and has succeeded in increasing the rigidity of the void-containing biaxially oriented polypropylene film. Furthermore, using a resin composition primarily composed of the aforementioned polypropylene resin not only facilitates peeling at the interface with the void-producing agent, but also increases the volume of the voids, making it easier to reduce the apparent density. Therefore, it is possible to reduce the apparent density using the same amount of void-producing agent as before.
[0052] (Method for producing void-containing biaxially oriented polypropylene film) The void-containing biaxially oriented polypropylene film of the present invention and the biaxially oriented polypropylene film having a base layer A containing a polypropylene resin and a void-producing agent and a surface layer B made of a polypropylene resin composition on at least one side are preferably obtained by producing an unstretched sheet made of a polypropylene resin composition containing the above-mentioned polypropylene resin as a main component and biaxially stretching it. As the biaxial stretching method, any of inflation simultaneous biaxial stretching, tenter simultaneous biaxial stretching, and tenter sequential biaxial stretching can be used, but from the viewpoint of film production stability and thickness uniformity, tenter sequential biaxial stretching is preferably used. In particular, stretching in the longitudinal direction and then in the width direction is preferred, but a method in which stretching in the width direction and then in the longitudinal direction is also acceptable.
[0053] Next, a method for producing the void-containing biaxially oriented polypropylene film of the present invention and a biaxially oriented polypropylene film having a base layer A containing a polypropylene resin and a void-forming agent and a surface layer B consisting of a polypropylene resin composition on at least one side will be described below, but the method is not necessarily limited to this.
[0054] The following describes an example of the first embodiment of a void-containing polypropylene film, employing the tenter sequential biaxial stretching method. First, a resin composition containing a polypropylene resin is heated and melted in a single-screw or twin-screw extruder, extruded through a T-die into a sheet, and then placed on a cooling roll for cooling and solidification. To accelerate solidification, the sheet cooled by the cooling roll may be further cooled, for example, by immersing it in a water bath. Next, the sheet is stretched in the longitudinal direction between two pairs of heated stretching rolls by increasing the rotation speed of the rear stretching roll, thereby obtaining a uniaxially stretched film. Subsequently, the uniaxially stretched film is preheated and then stretched in the width direction at a specific temperature while holding the film edges in a tenter-type stretching machine, thereby obtaining a biaxially stretched film. After the width direction stretching step is completed, the biaxially stretched film is heat-treated at a specific temperature. During the heat treatment step, the film may be relaxed in the width direction. The biaxially oriented polypropylene film thus obtained may be optionally subjected to a corona discharge treatment on at least one side, and then wound up on a winder to obtain a film roll.
[0055] Each step will be described in detail below. (Extrusion Step) First, a polypropylene resin composition containing a polypropylene resin as a main component is heated and melted in a single-screw or twin-screw extruder at a temperature in the range of 200°C to 300°C, and the sheet-shaped molten polypropylene resin composition is extruded from a T-die and brought into contact with a metal cooling roll to be cooled and solidified. The resulting unstretched sheet may be further cooled by being placed in a water bath. The temperature of the cooling roll, or the cooling roll and water bath, is preferably in the range of 10°C or higher and Tc (°C) or lower. To reduce the apparent density and increase the rigidity, the cooling temperature is preferably 40°C or higher, more preferably 60°C or higher, even more preferably 70°C or higher, even more preferably 75°C or higher, and particularly preferably 80°C or higher. On the other hand, a cooling temperature of 100°C or lower is preferred to facilitate the subsequent stretching step and reduce thickness unevenness, and a temperature of 90°C or lower is more preferred. The thickness of the unstretched sheet is preferably 6000 μm or less in terms of cooling efficiency, more preferably 5500 μm or less, and can be appropriately adjusted depending on the thickness of the film after sequential biaxial stretching. The thickness of the unstretched sheet can be controlled by the extrusion speed of the polypropylene resin composition, the lip width of the T-die, etc.
[0056] (Longitudinal Stretching Step) The lower limit of the longitudinal stretching ratio is preferably 3.5 times or more, more preferably 4.0 times or more, and particularly preferably 4.3 times or more. Within this range, strength is easily increased and thickness unevenness is reduced. The upper limit of the longitudinal stretching ratio is preferably 7 times or less, more preferably 6 times or less, and particularly preferably 5 times or less. Within this range, width direction stretching in the width direction stretching step is easy and productivity is improved. The lower limit of the longitudinal stretching temperature is preferably 125°C or more, more preferably 130°C or more, and even more preferably 135°C or more. Within this range, subsequent width direction stretching is easy and thickness unevenness is reduced. The upper limit of the longitudinal stretching temperature is preferably 155°C or less, more preferably 150°C or less, and even more preferably 145°C or less. Within the above range, the heat shrinkage rate is easily reduced and there is little risk of the film melting onto the stretching rolls, making stretching difficult, or of the film becoming rough on the surface, resulting in a decrease in quality. The longitudinal stretching may be carried out in two or more stages using three or more pairs of stretching rolls.
[0057] (Preheating step) Before the width direction stretching step, the uniaxially stretched film after longitudinal stretching must be heated in the range of 165°C or higher and 175°C or lower to soften the polypropylene resin composition. By setting the temperature to 165°C or higher, softening of the uniaxially stretched film progresses, making it easier to stretch in the width direction. Furthermore, by setting the temperature to 175°C or lower, orientation during width direction stretching progresses, rigidity is easily developed, and cavities are less likely to collapse. Here, the maximum temperature in the preheating step is defined as the preheating temperature.
[0058] (Width Direction Stretching Step) The lower limit of the temperature in the width direction stretching step is preferably 155°C or higher, more preferably 158°C or higher, and even more preferably 160°C or higher. When the width direction stretching temperature is 155°C or higher, the heat shrinkage rate of the resulting biaxially oriented film is likely to be reduced. Furthermore, the upper limit of the temperature in the width direction stretching step is preferably 174°C or lower, more preferably 172°C or lower, and even more preferably 171°C or lower. When the width direction stretching temperature is 174°C or lower, stretching unevenness is unlikely to occur, rigidity is likely to be developed, and cavities are unlikely to be crushed. In this case, the start of width direction stretching may be when the preheating temperature is reached, or when the temperature is lowered after reaching the preheating temperature to a temperature lower than the preheating temperature.
[0059] The lower limit of the final width direction stretching ratio in the width direction stretching step is preferably 11 times or more, more preferably 12 times or more. If it is 11 times or more, rigidity is likely to be increased and thickness unevenness is likely to be reduced. The upper limit of the width direction stretching ratio is preferably 20 times or less, more preferably 17 times or less, and even more preferably 15 times or less. If it is 20 times or less, the heat shrinkage rate is likely to be reduced and the film is unlikely to break during stretching.
[0060] By using a highly crystalline polypropylene resin with high stereoregularity and a high melting point and employing the width-direction stretching process described above, the polypropylene resin molecules are highly aligned in the main orientation direction (the width direction in the width-direction stretching process described above), resulting in a very strong crystalline orientation in the resulting biaxially oriented film, which tends to produce crystals with a high melting point. Furthermore, the orientation of the amorphous portions between the crystals is also enhanced in the main orientation direction (the width direction in the width-direction stretching process described above). Because many high-melting-point crystals exist around the amorphous portions, the elongated polypropylene molecules in the amorphous portions are less likely to relax at temperatures below the melting point of the crystals, and tend to maintain their tensed state. Therefore, the entire biaxially oriented film can maintain high rigidity even at high temperatures. Furthermore, because many high-melting-point crystals exist around the amorphous portions, the elongated polypropylene resin molecules in the amorphous portions are less likely to relax at temperatures below the melting point of the crystals, and the molecules are less likely to entangle with each other, resulting in a weakened heat shrinkage stress. Therefore, the heat shrinkage rate at high temperatures of 150°C is also likely to decrease.
[0061] It is also worth noting that by increasing the low molecular weight components of the polypropylene resin, the crystallinity of the film is more likely to be increased, and the entanglement of polypropylene resin molecular chains in the amorphous portion is reduced, thereby further reducing the heat shrinkage rate.
[0062] (Heat Treatment Step) It is preferable to heat-treat the film upon completion of width direction stretching, i.e., immediately after reaching the final width direction stretch ratio. The lower limit of the heating temperature at this time is preferably 160°C or higher, more preferably 163°C or higher, and even more preferably 164°C or higher. The upper limit of the heating temperature is preferably 175°C or lower, more preferably 173°C or lower, and even more preferably 170°C or lower. Heat treatment at 160°C or higher relaxes the molecular chain orientation formed during stretching and promotes crystallization, making it easy to reduce the heat shrinkage rate at high temperatures. On the other hand, heat treatment at 175°C or lower prevents excessive orientation relaxation, making it difficult for rigidity to decrease and cavities to collapse. The temperature can be gradually increased from the temperature at the end of width direction stretching to the temperature during heating, but it can also be increased in steps or in a single step. Raising the temperature in steps or in a single step is preferable because it is easier to control the orientation of the molecular chains in the film.
[0063] At this time, it is preferable to simultaneously perform a relaxation treatment at a relaxation rate of 5% or less to eliminate the constraint of the molecular chains due to excessive entanglement while maintaining the molecular chain orientation. This heat treatment step reduces the number of molecular chains constrained by entanglement, thereby increasing the crystallinity and making it easier to increase the thickness of the crystalline lamellae. This allows the film to exhibit sufficient heat resistance even at high temperatures, making it easier to achieve both rigidity and heat resistance. The relaxation rate can also be referred to as the relaxation rate, and the relaxation treatment can also be referred to as the relaxation treatment. Specific examples of heat treatment methods include providing a zone with a higher temperature than the stretching zone after the completion of widthwise stretching, or increasing the zone temperature in the latter half of stretching and passing the film through a zone with the same temperature after the completion of stretching to increase the film temperature. Examples of heating methods include blowing hot air or heating with an infrared heater, but are not particularly limited as long as they are methods that increase the film temperature beyond the completion of widthwise stretching. The upper limit of the relaxation rate is preferably 5% or less, more preferably 4% or less, and even more preferably 3.5% or less. Within the above range, the rigidity is less likely to decrease and the film thickness fluctuation is likely to be small. If the relaxation rate is higher than 5%, many of the oriented molecular chains are relaxed, so the rigidity is likely to decrease. If it is desired to further increase the rigidity, the relaxation treatment does not need to be performed. Furthermore, in order to suppress sagging of the film, the relaxation rate may be slightly expanded within the range in which the characteristics of the present invention can be obtained.
[0064] (Surface Treatment) It is preferable to subject at least one side of the surface of the obtained biaxially oriented laminated polypropylene film to a corona treatment. The wet tension of the treated film is preferably 35 mN / m or more, more preferably 36 mN / m or more, and even more preferably 37 mN / m or more.
[0065] The void-containing biaxially oriented polypropylene film thus obtained is typically formed into a roll having a width of 2000 mm to 12000 mm and a length of 1000 m to 50000 m, and wound into a roll. It is then slit according to the intended use and provided as a slit roll having a width of 300 mm to 2000 mm and a length of 500 m to 5000 m. The overall thickness of the void-containing biaxially oriented polypropylene film is preferably 5 μm to 100 μm, more preferably 10 μm to 80 μm, and even more preferably 15 μm to 60 μm.
[0066] Next, an example of a surface layer B / substrate layer A / surface layer B configuration will be described, taking the case of employing a tenter sequential biaxial stretching method. First, a molten polypropylene resin composition multilayer sheet having a surface layer B / substrate layer A / surface layer B configuration is extruded through a T-die. For example, a method can be used in which polypropylene resins discharged from different flow paths of two or more extruders are co-extruded while being laminated in multiple layers using a multi-layer feed block, static mixer, multi-layer multi-manifold die, or the like. First, a resin composition containing polypropylene resin is heated and melted in a single-screw or twin-screw extruder, extruded into a sheet form through a T-die, and then cooled and solidified by being brought to rest on a cooling roll. To promote solidification, the sheet cooled by the cooling roll may be further cooled, for example, by immersing it in a water bath. Next, the sheet is stretched in the longitudinal direction between two pairs of heated stretching rolls by increasing the rotation speed of the rear stretching roll to obtain a uniaxially stretched film. Subsequently, the uniaxially stretched film is preheated, and then stretched in the width direction at a specific temperature while holding the film edges in a tenter-type stretching machine, to obtain a biaxially stretched film. After the width direction stretching step is completed, the biaxially stretched film is heat-treated at a specific temperature. In the heat treatment step, the film may be relaxed in the width direction. If necessary, the biaxially oriented polypropylene film thus obtained may be subjected to a corona discharge treatment on at least one side, and then wound up on a winder to obtain a film roll.
[0067] Each step will be described in detail below. (Extrusion Step) First, a polypropylene resin composition containing a polypropylene resin as a main component is heated and melted in a single-screw or twin-screw extruder at a temperature in the range of 200°C to 300°C, and the sheet-shaped molten polypropylene resin composition is extruded from a T-die and brought into contact with a metal cooling roll to be cooled and solidified. The resulting unstretched sheet may be further cooled by being placed in a water bath. The temperature of the cooling roll, or the cooling roll and water bath, is preferably in the range of 10°C or higher and Tc (°C) or lower. To reduce the apparent density and increase the rigidity, the cooling temperature is preferably 40°C or higher, more preferably 60°C or higher, even more preferably 70°C or higher, and particularly preferably 80°C or higher. On the other hand, a cooling temperature of 100°C or lower is preferred to facilitate the subsequent stretching step and reduce thickness unevenness, and a temperature of 90°C or lower is more preferred. The thickness of the unstretched sheet is preferably 6000 μm or less in terms of cooling efficiency, more preferably 5500 μm or less, and can be appropriately adjusted depending on the thickness of the film after sequential biaxial stretching. The thickness of the unstretched sheet can be controlled by the extrusion speed of the polypropylene resin composition, the lip width of the T-die, etc.
[0068] (Longitudinal Stretching Step) The lower limit of the longitudinal stretching ratio is preferably 3.5 times or more, more preferably 4.0 times or more, and particularly preferably 4.3 times or more. Within this range, strength is easily increased and thickness unevenness is reduced. The upper limit of the longitudinal stretching ratio is preferably 7 times or less, more preferably 6 times or less, and particularly preferably 5 times or less. Within this range, width direction stretching in the width direction stretching step is easy and productivity is improved. The lower limit of the longitudinal stretching temperature is preferably 125°C or more, more preferably 130°C or more, and even more preferably 135°C or more. Within this range, subsequent width direction stretching is easy and thickness unevenness is reduced. The upper limit of the longitudinal stretching temperature is preferably 155°C or less, more preferably 150°C or less, and even more preferably 145°C or less. Within the above range, the heat shrinkage rate is easily reduced and there is little risk of the film melting onto the stretching rolls, making stretching difficult, or of the film becoming rough on the surface, resulting in a decrease in quality. The longitudinal stretching may be carried out in two or more stages using three or more pairs of stretching rolls.
[0069] (Preheating step) Before the width direction stretching step, the uniaxially stretched film after longitudinal stretching must be heated in the range of 165°C or higher and 175°C or lower to soften the polypropylene resin composition. By setting the temperature to 165°C or higher, softening of the uniaxially stretched film progresses, making it easier to stretch in the width direction. Furthermore, by setting the temperature to 175°C or lower, orientation during width direction stretching progresses, rigidity is easily developed, and cavities are less likely to collapse. Here, the maximum temperature in the preheating step is defined as the preheating temperature.
[0070] (Width Direction Stretching Step) The lower limit of the temperature in the width direction stretching step is preferably 155°C or higher, more preferably 158°C or higher, and even more preferably 160°C or higher. When the width direction stretching temperature is 155°C or higher, the heat shrinkage rate of the resulting biaxially oriented film is likely to be reduced. Furthermore, the upper limit of the temperature in the width direction stretching step is preferably 174°C or lower, more preferably 172°C or lower, and even more preferably 171°C or lower. When the width direction stretching temperature is 174°C or lower, stretching unevenness is unlikely to occur, rigidity is likely to be developed, and cavities are unlikely to be crushed. In this case, the start of width direction stretching may be when the preheating temperature is reached, or when the temperature is lowered after reaching the preheating temperature to a temperature lower than the preheating temperature.
[0071] The lower limit of the final width direction stretching ratio in the width direction stretching step is preferably 11 times or more, more preferably 12 times or more. If it is 11 times or more, rigidity is likely to be increased and thickness unevenness is likely to be reduced. The upper limit of the width direction stretching ratio is preferably 20 times or less, more preferably 17 times or less, and even more preferably 15 times or less. If it is 20 times or less, the heat shrinkage rate is likely to be reduced and the film is unlikely to break during stretching.
[0072] By using a highly crystalline polypropylene resin with high stereoregularity and a high melting point for Layer A and employing the width-direction stretching process described above, the polypropylene resin molecules are highly aligned in the main orientation direction (the width direction in the width-direction stretching process described above), which results in a very strong crystalline orientation in the resulting biaxially oriented film, and the formation of crystals with high melting points is likely to occur. Furthermore, the orientation of the amorphous portions between the crystals is also enhanced in the main orientation direction (the width direction in the width-direction stretching process described above). Because many high-melting-point crystals exist around the amorphous portions, the elongated polypropylene molecules in the amorphous portions are less likely to relax at temperatures below the melting point of the crystals, and are therefore more likely to maintain their tensed state. Therefore, the entire void-containing biaxially oriented laminated polypropylene film can maintain high rigidity even at high temperatures. Furthermore, because many high-melting-point crystals exist around the amorphous portions, the elongated polypropylene resin molecules in the amorphous portions are less likely to relax at temperatures below the melting point of the crystals, and the molecules are less likely to entangle with each other, resulting in a weaker heat shrinkage stress. Therefore, the heat shrinkage rate at high temperatures of 150°C is also likely to decrease.
[0073] It is also worth noting that by increasing the low molecular weight component of the polypropylene resin, the crystallinity of the film is more likely to be increased, and the entanglement of polypropylene resin molecular chains in the amorphous portion is reduced, thereby further reducing the heat shrinkage rate.
[0074] (Heat Treatment Step) It is preferable to heat-treat the film upon completion of width direction stretching, i.e., immediately after reaching the final width direction stretch ratio. The lower limit of the heating temperature at this time is preferably 160°C or higher, more preferably 163°C or higher, and even more preferably 164°C or higher. The upper limit of the heating temperature is preferably 175°C or lower, more preferably 173°C or lower, and even more preferably 170°C or lower. Heat treatment at 160°C or higher relaxes the molecular chain orientation formed during stretching and promotes crystallization, making it easy to reduce the heat shrinkage rate at high temperatures. On the other hand, heat treatment at 175°C or lower prevents excessive orientation relaxation, making it difficult for rigidity to decrease and cavities to collapse. The temperature can be gradually increased from the temperature at the end of width direction stretching to the temperature during heating, but it can also be increased in steps or in a single step. Raising the temperature in steps or in a single step is preferable because it is easier to control the orientation of the molecular chains in the film.
[0075] At this time, it is preferable to simultaneously perform a relaxation treatment at a relaxation rate of 5% or less to eliminate the constraint of the molecular chains due to excessive entanglement while maintaining the molecular chain orientation. This heat treatment step reduces the number of constrained molecular chains due to entanglement, thereby increasing the crystallinity and making it easier to increase the lamellar thickness in the crystalline portion. This allows for sufficient heat resistance even at high temperatures, thereby achieving a better balance between rigidity and heat resistance. Specific heat treatment methods include providing a zone with a higher temperature than the stretching zone after the completion of widthwise stretching, or increasing the zone temperature in the latter half of stretching and passing the film through a zone at the same temperature after the completion of stretching, thereby increasing the film temperature. Heating methods include blowing hot air and heating with an infrared heater, but are not particularly limited as long as they increase the film temperature after the completion of widthwise stretching. The upper limit of the relaxation rate is preferably 5% or less, more preferably 4% or less, and even more preferably 3.5% or less. Within the above range, rigidity is less likely to decrease and film thickness fluctuations are likely to be reduced. If the relaxation rate is higher than 5%, many of the oriented molecular chains will relax, which will tend to reduce rigidity. If you want to further increase rigidity, relaxation treatment may not be necessary. Furthermore, to prevent sagging of the film, the film may be slightly expanded within a range in which the properties of the present invention can be obtained.
[0076] (Surface Treatment) It is preferable to subject at least one side of the surface of the obtained biaxially oriented laminated polypropylene film to a corona treatment. The wet tension of the treated film is preferably 35 mN / m or more, more preferably 36 mN / m or more, and even more preferably 37 mN / m or more.
[0077] The void-containing biaxially oriented polypropylene film thus obtained is typically formed into a roll having a width of 2000 mm to 12000 mm and a length of 1000 m to 50000 m, and wound into a roll. It is then slit according to the intended use and provided as a slit roll having a width of 300 mm to 2000 mm and a length of 500 m to 5000 m. The overall thickness of the void-containing biaxially oriented polypropylene film is preferably 5 μm to 100 μm, more preferably 10 μm to 80 μm, and even more preferably 15 μm to 60 μm.
[0078] (Characteristics of void-containing biaxially oriented polypropylene film) The void-containing biaxially oriented polypropylene film of the present invention and the void-containing biaxially oriented polypropylene film having a base layer A containing a polypropylene resin and a void-producing agent and a surface layer B made of a polypropylene resin composition on at least one side are characterized by the following properties. Here, the "MD direction" in the biaxially oriented polypropylene film of the present invention is the direction corresponding to the flow direction in the film production process, and the "TD direction" is the direction perpendicular to the flow direction in the film production process. For polypropylene films whose flow direction in the film production process is unknown, wide-angle X-rays are incident perpendicular to the film surface, and the scattering peak derived from the (110) plane of the α-crystals is scanned in the circumferential direction, and the direction with the greatest diffraction intensity in the obtained diffraction intensity distribution is defined as the "MD direction," and the direction perpendicular to that is defined as the "TD direction." In addition, in a void-containing biaxially oriented polypropylene film and a void-containing biaxially oriented polypropylene film having a base layer A containing polypropylene resin and a void-producing agent, and a surface layer B consisting of a polypropylene resin composition on at least one side, the "F side" refers to the side on which the sheet-like molten resin extruded from a T-die comes into contact with the cooling roll during the film production process, and the "B side" refers to the side on which the sheet-like molten resin does not come into contact with the cooling roll during the same process.
[0079] (Apparent Density) The upper limit of the apparent density of the void-containing polypropylene film of the present invention and the void-containing biaxially oriented polypropylene film having a base layer A containing a polypropylene resin and a void-producing agent and a surface layer B made of a polypropylene resin composition on at least one side is preferably 0.85 g / cm 3 or less, more preferably 0.80 g / cm 3 More preferably, it is 0.75 g / cm or less. 3 The lower limit of the apparent density is preferably 0.65 g / cm 3 More preferably, 0.67 g / cm 3 When the thickness is within the above range, the film can have a sufficient stiffness and the handling properties are improved.
[0080] (Stress at 5% Elongation at 23°C) The lower limit of the stress at 5% elongation in the machine direction (MD) at 23°C of the void-containing biaxially oriented polypropylene film of the present invention and the void-containing biaxially oriented polypropylene film having a base layer A containing a polypropylene resin and a void-developing agent and a surface layer B made of a polypropylene resin composition on at least one side thereof (F5MD) is preferably 25 MPa or more, more preferably 30 MPa or more, and even more preferably 35 MPa or more. The upper limit of F5MD is preferably 50 MPa or less, more preferably 45 MPa or less, and even more preferably 40 MPa or less. Within the above range, the high rigidity makes it easy to maintain the shape of labels and packaging bags, and the film is less likely to deform during processing such as printing, making it less likely to cause printing pitch deviation when transferring printing ink.
[0081] The lower limit of the stress at 5% elongation in the TD direction (F5TD) at 23°C of the void-containing biaxially oriented polypropylene film of the present invention and the void-containing biaxially oriented polypropylene film having a base layer A containing a polypropylene resin and a void-developing agent and a surface layer B made of a polypropylene resin composition on at least one side is preferably 110 MPa or more, more preferably 115 MPa or more, and even more preferably 120 MPa or more. The upper limit of F5TD is preferably 200 MPa or less, more preferably 180 MPa or less, and even more preferably 160 MPa or less. Within the above range, the high rigidity makes it easy to maintain the shape of labels and packaging bags, and the film is less likely to deform during processing such as printing, making it less likely to cause printing pitch deviation when transferring printing ink.
[0082] (Heat shrinkage rate at 150°C) The upper limit of the heat shrinkage rate at 150°C in the MD direction of the void-containing biaxially oriented polypropylene film of the present invention and the void-containing biaxially oriented polypropylene film having a base layer A containing a polypropylene resin and a void-producing agent and a surface layer B made of a polypropylene resin composition on at least one side is preferably 6% or less, more preferably 5% or less, even more preferably 4% or less, and particularly preferably 3% or less. The lower limit of the heat shrinkage rate at 150°C in the MD direction is preferably 0% or more, more preferably 0.5% or more. Within the above range, it becomes easier to use in applications where there is a possibility of exposure to high temperatures of around 150°C. In addition, shrinkage wrinkles due to heating during printing or adhesive processing are less likely to occur, and shrinkage wrinkles at the sealed portion are less likely to occur during heat sealing, resulting in a better finish.
[0083] The upper limit of the heat shrinkage rate at 150°C in the TD direction of the void-containing biaxially oriented polypropylene film of the present invention and the void-containing biaxially oriented polypropylene film having a base layer A containing a polypropylene resin and a void-producing agent and a surface layer B made of a polypropylene resin composition on at least one side is preferably 10% or less, more preferably 9% or less, even more preferably 8% or less, particularly preferably 7% or less, and most preferably 6% or less. The lower limit of the heat shrinkage rate at 150°C in the TD direction is preferably -5% or more, more preferably 0% or more. Within the above range, it is easier to use in applications where exposure to high temperatures of around 150°C is possible. Furthermore, shrinkage wrinkles due to heating during printing or adhesive processing and shrinkage wrinkles at the sealed portion during heat sealing are less likely to occur, resulting in a better finish. The heat shrinkage rate at 150°C can be reduced by increasing the low-molecular-weight polypropylene component in the raw polypropylene resin composition or by adjusting the stretching conditions, heat treatment conditions, and fixation conditions.
[0084] (Thickness unevenness) The upper limit of thickness unevenness of a square sample 1 m long taken from a roll consisting of the wound void-containing biaxially oriented polypropylene film of the present invention and a void-containing biaxially oriented polypropylene film having a base layer A containing polypropylene resin and a void-forming agent and a surface layer B consisting of a polypropylene resin composition on at least one side is preferably 20% or less, more preferably 17% or less, and even more preferably 12% or less.
[0085] (Total Light Transmittance) The upper limit of the total light transmittance of the void-containing biaxially oriented polypropylene film of the present invention and the void-containing biaxially oriented polypropylene film having a base layer A containing a polypropylene resin and a void-producing agent and a surface layer B made of a polypropylene resin composition on at least one side is preferably 40% or less, more preferably 30% or less, and even more preferably 25% or less. The lower limit of the total light transmittance is preferably 0% or more. Within the above range, the film is easy to use in applications requiring opacity. The total light transmittance can be controlled by adjusting the amount of the opacifying agent or void-producing agent. It can also be controlled by adjusting film-forming conditions such as the stretching temperature, stretching ratio, and heat treatment temperature.
[0086] (Gloss) The void-containing biaxially oriented polypropylene film of the present invention and the void-containing biaxially oriented polypropylene film having a base layer A containing a polypropylene resin and a void-producing agent and a surface layer B made of a polypropylene resin composition on at least one side thereof preferably have a gloss of 50% or more, more preferably 80% or more, and even more preferably 100% or more. The upper limit of gloss is 300% or less as a practical value from the viewpoint of production.
[0087] (Wet Tension) The wet tension of the film surface of the void-containing biaxially oriented polypropylene film of the present invention and the void-containing biaxially oriented polypropylene film having a base layer A containing a polypropylene resin and a void-producing agent and a surface layer B made of a polypropylene resin composition on at least one side is preferably 35 mN / m or more, more preferably 36 mN / m or more, and even more preferably 37 mN / m or more. A wet tension of 35 mN / m or more improves adhesion to printing inks, coating agents, and pressure-sensitive adhesives. To achieve a wet tension of 35 mN / m or more, it is preferable to perform a physicochemical surface treatment such as corona treatment or flame treatment. For example, in corona treatment, it is preferable to heat the film using a preheating roll and a treatment roll and discharge it in the air.
[0088] (Heat shrinkage at 120°C) The upper limit of the heat shrinkage in the MD direction at 120°C of the biaxially oriented laminated polypropylene film of the present invention and the void-containing biaxially oriented polypropylene film having a base layer A containing a polypropylene resin and a void-developing agent and a surface layer B made of a polypropylene resin composition on at least one side is 3.0% or less, preferably 2.5% or less, more preferably 2.0% or less, and particularly preferably 1.5% or less. The upper limit of the heat shrinkage in the TD direction at 120°C is 2.0% or less, preferably 1.5% or less, more preferably 1.0% or less, and particularly preferably 0.6% or less. Within the above range, shrinkage wrinkles due to heating during printing or adhesive processing are less likely to occur, and shrinkage wrinkles at the sealed portion are less likely to occur during heat sealing, resulting in a better finish.
[0089] (Breaking Strength) The lower limit of the tensile breaking strength in the MD direction of the void-containing biaxially oriented polypropylene film of the present invention, and the void-containing biaxially oriented polypropylene film having a base layer A containing a polypropylene resin and a void-developing agent, and a surface layer B made of a polypropylene resin composition on at least one side, is preferably 40 MPa or more, more preferably 50 MPa or more, even more preferably 60 MPa or more, and even more preferably 70 MPa or more. A tensile breaking strength of 40 MPa or more tends to result in excellent durability of the packaging bag. A higher tensile breaking strength in the MD direction is preferable in terms of durability, etc., but as a practical value for production, the upper limit is 200 MPa or less. The lower limit of the tensile breaking strength in the TD direction of the biaxially oriented laminated polypropylene film of the present invention, and the void-containing biaxially oriented polypropylene film having a base layer A containing a polypropylene resin and a void-developing agent, and a surface layer B made of a polypropylene resin composition on at least one side, is preferably 260 MPa or more, more preferably 270 MPa or more, even more preferably 280 MPa or more, even more preferably 290 MPa or more, and particularly preferably 295 MPa or more. If the tensile strength is 260 MPa or more, the durability of the film tends to be excellent. The higher the tensile breaking strength in the TD direction, the better in terms of durability, but the upper limit is 400 MPa or less as a realistic value in production. The tensile breaking strength can be adjusted within the above range by adjusting the stretch ratio, relaxation rate, and temperature conditions during film formation.
[0090] (Elongation at break) The lower limit of the tensile elongation at break in the MD direction of the void-containing biaxially oriented polypropylene film of the present invention and the void-containing biaxially oriented polypropylene film having a base layer A containing a polypropylene resin and a void-developing agent and a surface layer B made of a polypropylene resin composition on at least one side is preferably 120% or more, more preferably 140% or more, even more preferably 160% or more, even more preferably 180% or more, and particularly preferably 190% or more. If it is 120% or more, film breakage tends to be reduced. The upper limit of the tensile elongation at break in the MD direction is a practical value of 300% or less. The lower limit of the tensile elongation at break in the TD direction of the biaxially oriented laminated polypropylene film of the present invention is preferably 15% or more, more preferably 18% or more, even more preferably 21% or more, even more preferably 24% or more, and particularly preferably 27% or more. If it is 15% or more, film breakage tends to be reduced. The upper limit of the tensile elongation at break in the TD direction is a practical value of 70% or less. The tensile elongation at break can be adjusted within the above range by adjusting the draw ratio, relaxation rate, and temperature conditions during film formation.
[0091] (Dynamic friction coefficient) The void-containing biaxially oriented polypropylene film of the present invention and the void-containing biaxially oriented polypropylene film having a base layer A containing a polypropylene resin and a void-developing agent and a surface layer B made of a polypropylene resin composition on at least one side thereof preferably have a dynamic friction coefficient of 0.50 or less, more preferably 0.45 or less, and even more preferably 0.40 or less. The lower limit of the dynamic friction coefficient is 0.10 or more as a practical value from the viewpoint of production.
[0092] This application claims the benefit of priority based on Japanese Patent Application No. 2023-078073 filed on May 10, 2023, and Japanese Patent Application No. 2023-086472 filed on May 25, 2023. The entire contents of the specifications of Japanese Patent Application No. 2023-078073 filed on May 10, 2023, and Japanese Patent Application No. 2023-086472 filed on May 25, 2023 are incorporated herein by reference.
[0093] The present invention will be explained in more detail below with reference to examples and comparative examples, but the present invention is not limited to the following examples, and can of course be practiced with appropriate modifications within the scope of the above and below aims, all of which are included within the technical scope of the present invention. The methods for measuring physical properties in the following examples and comparative examples are as follows.
[0094] 1) Melt flow rate (MFR, g / 10 min) Measured in accordance with JIS K 7210 at a temperature of 230°C.
[0095] 2) Molecular weight and molecular weight distribution The molecular weight and molecular weight distribution were determined using gel permeation chromatography (GPC) with monodisperse polystyrene standards. The columns and solvents used in the GPC measurements are as follows: Solvent: 1,2,4-trichlorobenzene Column: TSKgel GMH HR -H(20)HT x 3 Flow rate: 1.0 ml / min Detector: RI Measurement temperature: 140°C The number average molecular weight (Mn), mass average molecular weight (Mw), and Z+1 average molecular weight (Mz+1) are each defined by the number of molecules (Ni) of the molecular weight (Mi) at each elution position of the GPC curve obtained via the molecular weight calibration curve, using the following formulas: Number average molecular weight: Mn = Σ(Ni·Mi) / ΣNi Mass average molecular weight: Mw = Σ(Ni·Mi 2 ) / Σ(Ni・Mi) Z+1 average molecular weight: Mz+1=Σ(Ni・Mi 4 ) / Σ(Ni·Mi 3 ) Molecular weight distribution: Mw / Mn, Mz+1 / Mn The molecular weight at the peak position of the GPC curve was taken as Mp. When the baseline was unclear, the baseline was set in the range from the lowest point of the high molecular weight side skirt of the elution peak on the high molecular weight side closest to the elution peak of the standard substance. From the obtained GPC curve, peak separation was performed into two or more components with different molecular weights. The molecular weight distribution of each component was assumed to be a Gaussian function, and Mw / Mn = 4 was set so that it would be similar to the molecular weight distribution of ordinary polypropylene. From the obtained curves of each component, the average molecular weight of each component was calculated.
[0096] 3) Stereoregularity The mesopentad fraction ([mmmm]%) and the average meso-sequence length were measured by13 The mesopentad fraction was calculated according to the method described in Zambelli et al., Macromolecules, Vol. 6, p. 925 (1973), and the average meso-sequence length was calculated according to the method described in J. C. Randall, "Polymer Sequence Distribution," Chapter 2 (1977) (Academic Press, New York). 13 C-NMR measurement was performed using an AVANCE 500 manufactured by BRUKER at 110°C by dissolving 200 mg of a sample in a mixed solution of o-dichlorobenzene and deuterated benzene in a ratio of 8:2 (volume ratio) at 135°C.
[0097] 4) Crystallization temperature (Tc), melting temperature (Tm) Thermal measurements were performed under a nitrogen atmosphere using a PerkinElmer DSC8500 differential scanning calorimeter. Approximately 5 mg was cut out from a polypropylene resin pellet and sealed in an aluminum pan for measurement. The temperature was raised to 230°C and held for 5 minutes, then cooled to 30°C at a rate of -10°C / min, and the exothermic peak temperature was taken as the crystallization temperature (Tc). The temperature was then held at 30°C for 5 minutes, and then raised to 230°C at 10°C / min, and the main endothermic peak temperature was taken as the melting temperature (Tm).
[0098] 5) Film Formability After TD stretching, the film was evaluated as ◯ if it did not break for 30 minutes, △ if it broke once, and × if it broke two or more times.
[0099] 6) Thickness Unevenness A 1-m-long square sample was cut from a roll of void-containing biaxially oriented polypropylene film and divided into 10 equal sections in each of the MD and TD directions to prepare 100 measurement samples. The thickness was measured at approximately the center of each measurement sample using a contact-type film thickness meter. The average value of the obtained 100 data points was calculated, and the difference (absolute value) between the minimum and maximum values was also calculated. The absolute value of the difference between the minimum and maximum values was divided by the average value to determine the thickness unevenness of the void-containing biaxially oriented polypropylene film. The relationship between the film thickness uniformity and thickness unevenness was evaluated as follows: ∘: Thickness unevenness was 15% or less, indicating excellent thickness uniformity. ×: Thickness unevenness was greater than 15%, indicating poor thickness uniformity.
[0100] 7) Total light transmittance (unit: %) Measured according to JIS K 7375 using an NDH5000 manufactured by Nippon Denshoku Industries Co., Ltd. The smaller the total light transmittance, the better the hiding power. The relationship between total light transmittance and hiding power was evaluated as follows: ◯: Total light transmittance was 30% or less, and hiding power was excellent. ×: Total light transmittance was more than 30%, and hiding power was poor.
[0101] 8) 120°C Heat Shrinkage (%) Measured in accordance with JIS Z 1712. A void-containing biaxially oriented polypropylene film was cut into a width of 20 mm and a length of 200 mm in both the MD and TD directions, and was hung in a hot air oven set to 120°C and heated for 5 minutes. The length after heating was measured, and the heat shrinkage was calculated as the ratio of the shrunk length to the original length.
[0102] 9) 150°C Heat Shrinkage (%) Measured in accordance with JIS Z 1712. A void-containing biaxially oriented polypropylene film was cut into 20 mm widths and 200 mm lengths in both the MD and TD directions, and then hung in a hot air oven set to 150°C for 5 minutes. The length after heating was measured, and the heat shrinkage was calculated as the ratio of the shrunken length to the original length. The smaller the 150°C heat shrinkage, the better the dimensional stability. The relationship between the 150°C heat shrinkage and the dimensional stability at heat was evaluated as follows: Good: The 150°C heat shrinkage in the film width direction was 10% or less, indicating excellent dimensional stability at heat. Bad: The 150°C heat shrinkage in the film width direction was more than 10%, indicating poor dimensional stability.
[0103] 10) Tensile Test The tensile strength of the film in the longitudinal and transverse directions was measured at 23°C in accordance with JIS K 7127. Samples were cut to a size of 15 mm x 200 mm and set in a tensile tester (Instron 5965, a dual-column tabletop tester manufactured by Instron Japan Co., Ltd.) with a chuck width of 100 mm. The tensile test was performed at a tensile speed of 200 mm / min. From the obtained strain-stress curve, the stress at 5% elongation was designated as F5. The tensile strength at break and the tensile elongation at break were defined as the strength and elongation, respectively, at the time the sample broke. The film's stiffness was evaluated using the stress at 5% elongation in the transverse direction (F5TD) of the film at 23°C. When comparing films of the same thickness, the higher the F5TD, the better the stiffness. The relationship between F5TD and stiffness was evaluated as follows. ◯: F5TD in the film width direction is 110 MPa or more, and the film has excellent stiffness. ×: F5TD in the film width direction is less than 110 MPa, and the film has poor stiffness.
[0104] 11) Apparent density (g / cm 3 The sample was cut to a size of 280 mm x 400 mm and its weight was measured using an analytical balance. The thickness was then measured using a dial gauge, and the results were applied to the following equation (1) to calculate the apparent density. 3 ) = weight (g) / (area (cm 2 ) × thickness (μm)) (1) The lightness of the film was evaluated using apparent density. When comparing films of the same thickness, the lower the apparent density, the better the lightness. The relationship between apparent density and lightness was evaluated as follows: Good: The apparent density of the film is 0.85 g / cm 3 x: The apparent density of the film is 0.85 g / cm or less, and the film is excellent in lightness. 3 and is less lightweight.
[0105] 12) Gloss: Measured at 23° C. in accordance with JIS Z 8741 using a VG7000 manufactured by Nippon Denshoku Industries Co., Ltd.
[0106] 13) Wetting tension According to JIS K 6768-1999, the film was aged at 23°C and 50% relative humidity for 24 hours, and then the corona-treated surface of the film was measured using the following procedure. 1) Measurements are made in a standard laboratory atmosphere (see JIS K 7100) at a temperature of 23°C and a relative humidity of 50%. 2) A test piece is placed on the substrate of a hand coater, and several drops of the test mixture are placed on the test piece. The wire bar is immediately pulled to spread the test mixture evenly. When using a cotton swab or brush to spread the test mixture, the liquid must be spread to at least 6 cm. 2 The test piece is quickly spread over an area of 100 mm or more. The amount of liquid should be such that it forms a thin layer without forming a puddle. The wetting tension is determined by observing the liquid film of the test mixture in a bright place and observing the state of the liquid film after 3 seconds. If the liquid film remains the same as when applied for 3 seconds or more without breaking, it is considered to be wet. If the wetting is maintained for 3 seconds or more, proceed to the mixture with the next highest surface tension. Conversely, if the liquid film breaks in 3 seconds or less, proceed to the mixture with the next lowest surface tension. Repeat this procedure to select a mixture that can accurately wet the surface of the test piece for 3 seconds. 3) Wash the wire bar with methanol and dry it after each use. 4) Repeat this procedure of selecting a mixture that can wet the surface of the test piece for 3 seconds at least three times. The surface tension of the mixture selected in this way is considered to be the wetting tension of the film.
[0107] 14) Dynamic friction coefficient A sample film was prepared by cutting out a piece measuring 400 mm in the longitudinal direction and 100 mm in the width direction from the obtained film. This was aged for 12 hours in an atmosphere of 23°C and 65% RH, and then divided into a test piece measuring 300 mm in the longitudinal direction and 100 mm in the width direction for the test table and a test piece measuring 100 mm in the longitudinal direction and 100 mm in the width direction for the sliding piece. The test piece for the test table was set on the test table, and the test piece for the sliding piece was subjected to a metal load (1.5 kg, area 39.7 mm 2 The test pieces were set on the bottom of a square plate (approx. 150 mm). The test pieces were set so that the measurement surfaces were in contact with each other. In accordance with JIS K 7125, a tensile tester (Tensilon RTG-1210 manufactured by A&D Co., Ltd.) was used to measure the dynamic friction coefficient of the sliding piece test piece under conditions of a sliding speed of 200 mm / min, 23°C, and 65% RH, and the average of three measurements was used.
[0108] (Example 1) [Base layer A] As the polypropylene resin constituting the void-containing biaxially oriented polypropylene film, a propylene homopolymer "FLX80H5" (manufactured by Sumitomo Chemical Co., Ltd.) (PP-1) having Mw / Mn = 3.6, MFR = 7.5, [mmmm] = 98.9% and a propylene homopolymer "EL80F5" (manufactured by Sumitomo Chemical Co., Ltd.) (PP-2) having Mw / Mn = 9.6, MFR = 11, [mmmm] = 98.8% were used. The polypropylene resin composition for the base layer A was prepared by dry blending 13% by mass of a calcium carbonate-containing masterbatch (MB-1) consisting of 50% by mass of a polypropylene random copolymer "FS2011DG3" (manufactured by Sumitomo Chemical Co., Ltd.) (PP-3) having 62% by mass of PP-1, 18% by mass of PP-2, Mw / Mn = 4.0, MFR = 2.5, [mmmm] = 97.0% and 50% by mass of calcium carbonate ("PO220B-10" manufactured by Bihoku Funka Kogyo Co., Ltd.), and 7% by mass of a titanium dioxide masterbatch (MB-T) consisting of 40% by mass of PP-3 and 60% by mass of titanium dioxide ("R-11 P" manufactured by Sakai Chemical Industry Co., Ltd.). [Surface layer B] A polypropylene resin composition for the surface layer B was prepared by dry blending 64% by mass of PP-1, 30% by mass of PP-3, and 6% by mass of the lubricant-containing masterbatch "MBB05L" (manufactured by Japan Polypropylene Corporation) (MB-2). First, the polypropylene resin compositions constituting the base layer A and the surface layer B were heated and melted at 250 ° C. in an extruder using a multi-layer feed block, and the molten polypropylene resin composition was co-extruded from a T-die at 250 ° C. into a sheet while being laminated in a configuration of surface layer B / base layer A / surface layer B. The sheet was cooled and solidified with a cooling roll at 80 ° C., then stretched 4.5 times in the longitudinal direction at 140 ° C., then clamped at both ends with clips, introduced into a hot air oven, preheated at 167 ° C., stretched 12.5 times in the width direction at 164 ° C., and then heat-treated at 165 ° C. with a relaxation rate of 3.0% during heat treatment. The film was then subjected to a corona treatment on one side (side F) and wound up on a winder. The thickness of the film thus obtained was 25 μm, and the thickness configuration was surface layer B / base layer A / surface layer B = 2 / 21 / 2 μm. Table 1 shows the molecular structure of the polypropylene resin, Table 2 shows the blending amounts and film-forming conditions, and Table 3 shows the physical properties.As shown in Table 3, the porous biaxially oriented polypropylene film had a high F5 value in the width direction and a low heat shrinkage rate at 150°C.
[0109] (Example 2) A film was obtained in the same manner as in Example 1, except that a dry blend of 80 mass% of PP-1, 13 mass% of MB-1, and 7 mass% of MB-T was used as the polypropylene resin composition for the base layer A. As shown in Table 3, the void-containing biaxially oriented polypropylene film had a high F5 value in the width direction and a low heat shrinkage at 150°C.
[0110] (Example 3) A film was obtained in the same manner as in Example 1, except that the film thickness was 35 μm, the thickness configuration was surface layer B / base layer A / surface layer B=2 / 31 / 2 μm, the preheating temperature before width direction stretching was 168° C., and the width direction stretching temperature was 165° C. As shown in Table 3, the resulting void-containing biaxially oriented polypropylene film had a high width direction F5 value and a low heat shrinkage at 150° C.
[0111] (Example 4) A film was obtained in the same manner as in Example 1, except that the film thickness was 45 μm, the thickness configuration was surface layer B / base layer A / surface layer B=2 / 41 / 2 μm, the preheating temperature before width direction stretching was 170° C., and the width direction stretching temperature was 167° C. As shown in Table 3, the void-containing biaxially oriented polypropylene film had a high width direction F5 value and a low heat shrinkage at 150° C.
[0112] (Example 5) A film was obtained in the same manner as in Example 1, except that the surface layer B was not laminated and the film thickness was 45 μm, the preheating temperature before width direction stretching was 170° C., and the width direction stretching temperature was 167° C. As shown in Table 3, the obtained film was a void-containing biaxially oriented polypropylene film with a high F5 value in the width direction and a low heat shrinkage rate at 150° C.
[0113] Example 6 A film was obtained in the same manner as in Example 1, except that a polypropylene resin composition for base layer A was a dry blend of 62 mass% PP-1, 18 mass% PP-2, 6 mass% MB-1, and 14 mass% MB-T, the film thickness was 45 μm, the thickness configuration was surface layer B / base layer A / surface layer B=2 / 41 / 2 μm, the preheating temperature before width direction stretching was 172° C., and the width direction stretching temperature was 169° C. As shown in Table 3, the resulting void-containing biaxially oriented polypropylene film had a high F5 value in the width direction and a low heat shrinkage at 150° C.
[0114] Comparative Example 1 A film was obtained in the same manner as in Example 1, except that the film thickness was 45 μm, the thickness configuration was surface layer B / base layer A / surface layer B=2 / 41 / 2 μm, and the polypropylene resin composition for base layer A was a dry blend of 91% by mass of propylene homopolymer "HU300" (manufactured by Samsung Total Chemical Co., Ltd.) (PP-4) having Mw / Mn=8.9, MFR=3.0, and [mmmm]=97.1%, 5% by mass of MB-1, and 4% by mass of MB-T. The width direction stretching ratio was 8.2 times, the relaxation rate during heat treatment was 7.4%, the preheating temperature before width direction stretching was 173°C, and the width direction stretching temperature was 160°C. Table 1 shows the molecular structure of the polypropylene resin, Table 4 shows the blending amounts and film-forming conditions, and Table 5 shows the physical properties. As shown in Table 5, the void-containing biaxially oriented polypropylene film had a low heat shrinkage at 150°C, but a low F5 value in the width direction.
[0115] (Comparative Example 2) A film was obtained in the same manner as in Comparative Example 1, except that the widthwise stretching ratio was 12.5 times, the relaxation rate during heat treatment was 3%, the preheating temperature before widthwise stretching was 175°C, and the widthwise stretching temperature was 162°C. As shown in Table 5, the obtained void-containing biaxially oriented polypropylene film had a high F5 value in the widthwise direction but a high heat shrinkage rate at 150°C.
[0116] (Comparative Example 3) A dry blend of 80% by mass of PP-4, 13% by mass of MB-1, and 7% by mass of MB-T was used as the polypropylene resin composition for the base layer A, and a film was obtained in the same manner as in Comparative Example 1, except that the preheating temperature before width direction stretching was 167°C and the width direction stretching temperature was 160°C. As shown in Table 5, the obtained void-containing biaxially oriented polypropylene film had a low heat shrinkage at 150°C but a low width direction F5 value.
[0117] (Comparative Example 4) A film was obtained in the same manner as in Comparative Example 3, except that the draw ratio in the width direction was 12.5 times, the relaxation rate during heat treatment was 3%, and the width direction stretching temperature was 164°C. As shown in Table 5, the void-containing biaxially oriented polypropylene film had a high F5 value in the width direction but a high heat shrinkage rate at 150°C.
[0118] (Comparative Example 5) A film was obtained in the same manner as in Example 1, except that the widthwise stretching ratio was 10.0 times, the preheating temperature before widthwise stretching was 165°C, and the widthwise stretching temperature was 162°C. As shown in Table 5, the obtained void-containing biaxially oriented polypropylene film had a low heat shrinkage at 150°C but a low widthwise F5 value.
[0119] (Comparative Example 6) A dry blend of 80% by mass of PP-3, 13% by mass of MB-1, and 7% by mass of MB-T was used as the polypropylene resin composition for the base layer A, and a dry blend of 94% by mass of PP-3 and 6% by mass of MB-2 was used as the polypropylene resin composition for the surface layer B. A film was obtained in the same manner as in Example 1, except that the longitudinal stretching temperature was 130°C, the preheating temperature before width direction stretching was 167°C, and the width direction stretching temperature was 162°C. As shown in Table 5, the resulting void-containing biaxially oriented polypropylene film had a low F5 value and a high heat shrinkage at 150°C.
[0120]
[0121]
[0122]
[0123]
[0124]
[0125] The void-containing biaxially oriented polypropylene film of the present invention can be used in a wide range of applications, including label applications, adhesive applications, release applications, and packaging applications. The void-containing biaxially oriented polypropylene film of the present invention not only has heat resistance, but also has higher film rigidity, allowing for thinner films. Furthermore, because of its excellent heat resistance, when used as a packaging material, for example, there is less wrinkling or slippage due to heat shrinkage during heat sealing, allowing for higher heat-sealing temperatures. This also makes it possible to increase the line speed during bag-making processing.
Claims
1. A void-containing biaxially oriented polypropylene film made of a polypropylene resin composition containing a polypropylene resin as a main component and at least a void generating agent, which satisfies the following (1) to (3): (1) An apparent density of 0.65 g / cm 3 Above, 0.85g / cm 3 (2) The stress at 5% elongation in the longitudinal direction of the film (F5MD) at 23° C. is 25 MPa or more, and the stress at 5% elongation in the width direction of the film (F5TD) at 23° C. is 110 MPa or more. (3) The heat shrinkage rate in the longitudinal direction at 150° C. is 6% or less, and the heat shrinkage rate in the width direction at 150° C. is 10% or less.
2. A void-containing biaxially oriented polypropylene film having a base layer A made of a polypropylene resin composition containing a polypropylene resin as a main component and at least a void generating agent, and a surface layer B made of a polypropylene resin composition on at least one side of the base layer A, which satisfies the following (1) to (3): (1) An apparent density of 0.65 g / cm 3 Above, 0.85g / cm 3 (2) The stress at 5% elongation in the longitudinal direction of the film (F5MD) at 23° C. is 25 MPa or more, and the stress at 5% elongation in the width direction of the film (F5TD) at 23° C. is 110 MPa or more. (3) The heat shrinkage rate in the longitudinal direction at 150° C. is 6% or less, and the heat shrinkage rate in the width direction at 150° C. is 10% or less.
3. A void-containing biaxially oriented polypropylene film made of a polypropylene resin composition containing a polypropylene resin as a main component and at least a void generating agent, and satisfying the following (1) to (3): (1) An apparent density of 0.65 g / cm 3 Above, 0.85g / cm 3 (2) The stress at 5% elongation in the longitudinal direction of the film (F5MD) at 23° C. is 25 MPa or more, and the stress at 5% elongation in the width direction of the film (F5TD) at 23° C. is 110 MPa or more. (3) The heat shrinkage rate in the longitudinal direction at 150° C. is 6% or less, and the heat shrinkage rate in the width direction at 150° C. is 10% or less.
4. A void-containing biaxially oriented polypropylene film having a base layer A made of a polypropylene resin composition containing a polypropylene resin as a main component and at least a void generating agent, and a surface layer B made of a polypropylene resin composition on at least one side of the base layer A, which satisfies the following (1) to (3): (1) An apparent density of 0.65 g / cm 3 Above, 0.85g / cm 3 (2) The stress at 5% elongation in the longitudinal direction of the film (F5MD) at 23° C. is 25 MPa or more, and the stress at 5% elongation in the width direction of the film (F5TD) at 23° C. is 110 MPa or more. (3) The heat shrinkage rate in the longitudinal direction at 150° C. is 6% or less, and the heat shrinkage rate in the width direction at 150° C. is 10% or less.
5. A hollow biaxially oriented polypropylene film according to any one of claims 1 to 4, wherein the hollow biaxially oriented polypropylene film has a total light transmittance of 40% or less.
6. A hollow biaxially oriented polypropylene film according to any one of claims 1 to 4, wherein the thickness of the hollow biaxially oriented polypropylene film is 5 μm or more and 100 μm or less.
Citation Information
Patent Citations
Polypropylene resin composition for drawn film
JP2000302925A
Cavity-containing polypropylene film
WO2015012308A1
Cavity-containing polypropylene film