Silicon carbide epitaxial substrate and method for manufacturing silicon carbide semiconductor device
The development of a silicon carbide epitaxial substrate with controlled defect formation and optimized growth conditions addresses yield improvement in silicon carbide semiconductor devices, enhancing their performance and quality.
Patent Information
- Application Number
- PCT/JP2024/015727
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-05-11
- Filing Date
- 2024-04-22
- Publication Date
- 2024-11-14
AI Technical Summary
The existing methods for manufacturing silicon carbide semiconductor devices face challenges in improving yield due to defects on the silicon carbide epitaxial substrates, which affect the quality and performance of the devices.
A silicon carbide epitaxial substrate with a specific defect structure, including defects with a contrast value of 90 or more and an areal density of 2 defects/cm², is developed, and a method involving controlled hydrogen flow rates and growth temperatures during epitaxial growth to minimize defect formation, thereby enhancing the yield of silicon carbide semiconductor devices.
The approach reduces the areal density of defects on the substrate, leading to improved yield and performance of silicon carbide semiconductor devices by optimizing the epitaxial growth conditions.
Smart Images

Figure JP2024015727_14112024_PF_FP_ABST
Abstract
Description
Silicon carbide epitaxial substrate and method for manufacturing silicon carbide semiconductor device
[0001] The present disclosure relates to a silicon carbide epitaxial substrate and a method for manufacturing a silicon carbide semiconductor device. This application claims priority to Japanese Patent Application No. 2023-078635, filed May 11, 2023. The entire contents of this Japanese patent application are incorporated herein by reference.
[0002] Japanese Patent Laid-Open Publication No. 2020-072156 (Patent Document 1) describes a method for manufacturing a silicon carbide semiconductor device in which a confocal scanning device is used to derive a contrast value on the surface of an epitaxial layer.
[0003] Japanese Patent Application Laid-Open No. 2020-072156
[0004] A silicon carbide epitaxial substrate according to the present disclosure includes a silicon carbide substrate, a silicon carbide epitaxial layer, and a plurality of defects. The silicon carbide epitaxial layer is provided on the silicon carbide substrate. The plurality of defects are formed in the silicon carbide epitaxial layer. The silicon carbide epitaxial layer constitutes a main surface. Each of the plurality of defects is exposed on the main surface. Each of the plurality of defects has a contrast value of 90 or more when photographed using a confocal scanning device. The surface density of the plurality of defects on the main surface is 2 defects / cm. 2 The area of each of the plurality of defects is 50 μm or less when viewed along a line perpendicular to the main surface. 2 That's all.
[0005] FIG. 1 is a schematic plan view showing the configuration of a silicon carbide epitaxial substrate according to this embodiment. FIG. 2 is a schematic cross-sectional view taken along line II-II in FIG. 1. FIG. 3 is an enlarged schematic plan view showing region III in FIG. 1. FIG. 4 is an enlarged schematic plan view showing region IV in FIG. 1. FIG. 5 is a schematic cross-sectional view taken along line V-V in FIG. 4. FIG. 6 is an enlarged schematic plan view showing region VI in FIG. 1. FIG. 7 is a schematic cross-sectional view taken along line VII-VII in FIG. 6. FIG. 8 is an enlarged schematic plan view showing region VIII in FIG. 1. FIG. 9 is a schematic cross-sectional view taken along line IX-IX in FIG. 8. FIG. 10 is a schematic cross-sectional view showing a state in which light is irradiated onto the first main surface and the triangular defect. FIG. 11 is a schematic view showing a step of identifying defects. FIG. 12 is a partial schematic cross-sectional view showing the configuration of an apparatus for manufacturing a silicon carbide epitaxial substrate. FIG. 13 is a flow diagram generally showing a method for manufacturing a silicon carbide epitaxial substrate according to this embodiment. FIG. 14 is a cross-sectional view schematically showing a step of preparing a silicon carbide substrate. FIG. 15 is a flow diagram generally showing a method for manufacturing a silicon carbide semiconductor device according to this embodiment. FIG. 16 is a cross-sectional view schematically showing a step of forming a body region. FIG. 17 is a cross-sectional view schematically showing a step of forming a source region. FIG. 18 is a cross-sectional view schematically showing a step of forming a trench in a first main surface of a silicon carbide epitaxial layer. FIG. 19 is a cross-sectional view schematically showing a step of forming a gate insulating film. FIG. 20 is a cross-sectional view schematically showing a step of forming a gate electrode and an interlayer insulating film. FIG. 21 is a cross-sectional view schematically showing a configuration of a silicon carbide semiconductor device according to this embodiment. FIG. 22 is a graph showing the areal density of defects having a contrast value of 90 or more and the hydrogen flow rate ratio in Samples 1 to 14. FIG. 23 is a graph showing the areal density of defects having a contrast value of 120 or more and the hydrogen flow rate ratio in Samples 1 to 14. Fig. 24 is a graph showing the areal density of defects having a contrast value of 150 or more versus the hydrogen flow rate ratio for Samples 1 to 14. Fig. 25 is a graph showing the areal density of defects having a contrast value of 90 or more versus the growth temperature / hydrogen flow rate for Samples 1 to 14. Fig. 26 is a graph showing the areal density of defects having a contrast value of 120 or more versus the growth temperature / hydrogen flow rate for Samples 1 to 14.FIG. 27 is a graph showing the areal density of defects with a contrast value of 150 or more in Samples 1 to 14 versus the growth temperature / hydrogen flow rate.
[0006] [Problem to be Solved by the Present Disclosure] An object of the present disclosure is to provide a silicon carbide epitaxial substrate and a method for manufacturing a silicon carbide semiconductor device that can improve the yield of silicon carbide semiconductor devices.
[0007] Effect of the Present Disclosure The present disclosure can provide a silicon carbide epitaxial substrate and a method for manufacturing a silicon carbide semiconductor device that can improve the yield of silicon carbide semiconductor devices.
[0008] [Description of Embodiments of the Present Disclosure] First, embodiments of the present disclosure will be listed and described.
[0009] (1) A silicon carbide epitaxial substrate according to the present disclosure includes a silicon carbide substrate, a silicon carbide epitaxial layer, and a plurality of defects. The silicon carbide epitaxial layer is provided on the silicon carbide substrate. The plurality of defects are formed in the silicon carbide epitaxial layer. The silicon carbide epitaxial layer constitutes a main surface. Each of the plurality of defects is exposed on the main surface. Each of the plurality of defects has a contrast value of 90 or more when photographed using a confocal scanning device. The surface density of the plurality of defects on the main surface is 2 defects / cm. 2 The area of each of the plurality of defects is 50 μm or less when viewed along a line perpendicular to the main surface. 2 That's all.
[0010] (2) In the silicon carbide epitaxial substrate according to (1), the plurality of defects may include a portion whose polytype is 3C. The plurality of defects and the silicon carbide epitaxial layer may form a recess.
[0011] (3) In the silicon carbide epitaxial substrate according to (1) above, the plurality of defects may include at least one of bumps, pits, carrots, triangular defects, and downfalls.
[0012] (4) In the silicon carbide epitaxial substrate according to any one of (1) to (3) above, when viewed along a straight line perpendicular to the main surface, for each of the plurality of defects, the longer of the length in a first direction and the length in a second direction perpendicular to the first direction may be 10 μm or more.
[0013] (5) In the silicon carbide epitaxial substrate according to any one of (1) to (4) above, the main surface may be in an as-grown state.
[0014] (6) A method for manufacturing a silicon carbide semiconductor device according to the present disclosure includes the following steps: preparing a silicon carbide epitaxial substrate according to any one of (1) to (5) above; and forming an electrode on the silicon carbide epitaxial layer.
[0015] [Details of the Embodiments of the Present Disclosure] Next, an embodiment of the present disclosure (hereinafter also referred to as the present embodiment) will be described with reference to the drawings. Note that the same or corresponding parts in the following drawings will be given the same reference numerals, and their description will not be repeated. In the crystallographic descriptions in this specification, individual orientations are indicated by [ ], collective orientations by < >, individual planes by ( ), and collective planes by {}. Furthermore, for negative indices, a "-" (bar) is placed before the number in crystallography, but in this specification, a negative sign is placed before the number.
[0016] <Silicon Carbide Epitaxial Substrate> FIG. 1 is a plan view schematically illustrating the configuration of a silicon carbide epitaxial substrate 100 according to this embodiment. FIG. 2 is a cross-sectional view schematically illustrating the configuration along line II-II in FIG. 1. As shown in FIGS. 1 and 2, the silicon carbide epitaxial substrate 100 according to this embodiment has a silicon carbide substrate 30 and a silicon carbide epitaxial layer 40. The silicon carbide epitaxial layer 40 is provided on the silicon carbide substrate 30. The silicon carbide epitaxial layer 40 is in contact with the silicon carbide substrate 30. The silicon carbide epitaxial substrate 100 has a first main surface 1 and a second main surface 2. The first main surface 1 is the surface of the silicon carbide epitaxial substrate 100. The second main surface 2 is opposite to the first main surface 1. Second main surface 2 is the back surface of silicon carbide epitaxial substrate 100 .
[0017] As shown in Fig. 1 , silicon carbide epitaxial substrate 100 has an outer peripheral edge 9. Outer peripheral edge 9 has, for example, an orientation flat 7 and an arc-shaped portion 8. Orientation flat 7 extends along a first direction 101. As shown in Fig. 1 , orientation flat 7 is linear when viewed along a line perpendicular to first main surface 1. Arc-shaped portion 8 is continuous with orientation flat 7. Arc-shaped portion 8 is arc-shaped when viewed along a line perpendicular to first main surface 1.
[0018] 1 , when viewed along a line perpendicular to the first main surface 1, the first main surface 1 extends along each of a first direction 101 and a second direction 102. When viewed along a line perpendicular to the first main surface 1, the second direction 102 is a direction perpendicular to the first direction 101.
[0019] The first direction 101 is, for example, the <11-20> direction. The first direction 101 may be, for example, the [11-20] direction. The first direction 101 may be a direction obtained by projecting the <11-20> direction onto the first main surface 1. From another perspective, the first direction 101 may be, for example, a direction including a <11-20> direction component.
[0020] The second direction 102 is, for example, the <1-100> direction. The second direction 102 may be, for example, the [1-100] direction. The second direction 102 may be, for example, a direction obtained by projecting the <1-100> direction onto the first main surface 1. From another perspective, the second direction 102 may be, for example, a direction including a <1-100> direction component.
[0021] First main surface 1 is a surface inclined with respect to the {0001} plane. The inclination angle (off angle) with respect to the {0001} plane is, for example, greater than 0° and equal to or less than 8°. The off angle is not particularly limited, but may be, for example, equal to or greater than 1°, or equal to or greater than 2°. The off angle is not particularly limited, but may be, for example, equal to or less than 7°, or equal to or less than 6°. First main surface 1 may be a surface inclined by the off angle with respect to the (000-1) plane, or may be a surface inclined by the off angle with respect to the (0001) plane. The inclination direction (off direction) of first main surface 1 is, for example, the <11-20> direction.
[0022] As shown in FIG. 1 , the maximum diameter W of the first main surface 1 is not particularly limited, but is, for example, 100 mm (4 inches) or more. The maximum diameter W may be 125 mm (5 inches) or more, or 150 mm (6 inches) or more. The maximum diameter W may be, for example, 200 mm (8 inches) or less. The maximum diameter W is the maximum distance between any two points on the outer circumferential edge 9.
[0023] In this specification, 4 inches refers to 100 mm or 101.6 mm (4 inches x 25.4 mm / inch). 5 inches refers to 125 mm or 127.0 mm (5 inches x 25.4 mm / inch). 6 inches refers to 150 mm or 152.4 mm (6 inches x 25.4 mm / inch). 8 inches refers to 200 mm or 203.2 mm (8 inches x 25.4 mm / inch).
[0024] 2 , silicon carbide substrate 30 defines second main surface 2. Second main surface 2 is provided on the side opposite interface 3 between silicon carbide substrate 30 and silicon carbide epitaxial layer 40. The polytype of silicon carbide defining silicon carbide substrate 30 is, for example, 4H.
[0025] As shown in FIG. 2 , silicon carbide epitaxial layer 40 forms first main surface 1. First main surface 1 is provided on the opposite side of interface 3. Silicon carbide epitaxial layer 40 has a buffer layer 41 and a drift layer 42. Drift layer 42 may be a single layer or may be two or more layers. The polytype of silicon carbide forming silicon carbide epitaxial layer 40 is, for example, 4H. First main surface 1 is in an as-grown state. The as-grown state refers to a state after epitaxial growth and in which silicon carbide epitaxial layer 40 has not been polished. First main surface 1 is in an epitaxially grown state. From another perspective, first main surface 1 is an unpolished surface. Even if a treatment that does not modify the surface state of SiC (silicon carbide) is performed on silicon carbide epitaxial substrate 100, first main surface 1 can be said to be in an as-grown state. The treatment that does not modify the surface state of SiC is, for example, cleaning.
[0026] Buffer layer 41 is provided on silicon carbide substrate 30. Buffer layer 41 is in contact with silicon carbide substrate 30. Drift layer 42 is provided on buffer layer 41. Drift layer 42 is in contact with buffer layer 41. Drift layer 42 constitutes first main surface 1.
[0027] As shown in Fig. 2 , the third direction 103 is a direction from the second main surface 2 toward the first main surface 1. The third direction 103 is perpendicular to both the first direction 101 and the second direction 102. The cross section shown in Fig. 2 is perpendicular to the first main surface 1 and parallel to the first direction 101.
[0028] Silicon carbide substrate 30 contains an n-type impurity such as nitrogen (N). The conductivity type of silicon carbide substrate 30 is, for example, n-type. The thickness of silicon carbide substrate 30 in third direction 103 is, for example, 200 μm or more and 600 μm or less. Silicon carbide epitaxial layer 40 contains an n-type impurity such as nitrogen. The conductivity type of silicon carbide epitaxial layer 40 is, for example, n-type.
[0029] The concentration of the n-type impurity contained in buffer layer 41 may be lower than the concentration of the n-type impurity contained in silicon carbide substrate 30. The concentration of the n-type impurity contained in buffer layer 41 is, for example, 1×10 18 atoms / cm 3 1x10 or more 19 atoms / cm 3 The thickness of buffer layer 41 in third direction 103 is, for example, not less than 0.1 μm and not more than 10 μm.
[0030] The concentration of the n-type impurity contained in the drift layer 42 may be lower than the concentration of the n-type impurity contained in the buffer layer 41. The concentration of the n-type impurity contained in the drift layer 42 may be, for example, 1×10 15 atoms / cm 3 1x10 or more 17 atoms / cm 3 The thickness of drift layer 42 in third direction 103 is, for example, not less than 5 μm and not more than 30 μm.
[0031] FIG. 3 is an enlarged schematic plan view showing region III in FIG. 1 . As shown in FIG. 3 , silicon carbide epitaxial substrate 100 has defect 90. Defect 90 is exposed on first main surface 1. Defect 90 includes at least one of bump 60, pit 50, carrot 72, triangular defect 20, and downfall 71. Details of each of bump 60, pit 50, carrot 72, triangular defect 20, and downfall 71 will be described later. Defect 90 is formed in silicon carbide epitaxial layer 40 (see FIG. 2 ). On first main surface 1, defect 90 forms a recess or protrusion. First main surface 1 has flat portion 10. Flat portion 10 is a portion of first main surface 1 where defect 90 is not exposed.
[0032] <Triangular Defect> Figure 4 is an enlarged schematic plan view showing region IV in Figure 1. The enlarged schematic plan view shown in Figure 4 shows a state observed by a confocal scanning device. As shown in Figure 4, silicon carbide epitaxial substrate 100 according to this embodiment has triangular defect 20. As shown in Figure 4, when viewed along a line perpendicular to first main surface 1, triangular defect 20 has, for example, a triangular shape.
[0033] Fig. 5 is a schematic cross-sectional view taken along line V-V in Fig. 4. The cross section shown in Fig. 5 is a cross section perpendicular to first main surface 1. As shown in Figs. 4 and 5, first recess 29 is formed in first main surface 1 of silicon carbide epitaxial substrate 100 according to this embodiment. First recess 29 is composed of silicon carbide epitaxial layer 40 and triangular defect 20. When viewed along a line perpendicular to first main surface 1, first recess 29 has a triangular outer shape. Defect 90 may include triangular defect 20 and first recess 29.
[0034] As shown in FIG. 4 , the triangular defect 20 has a first side portion 23, a second side portion 24, a first base portion 22, and a top surface portion 25. The second side portion 24 is continuous with the first side portion 23. The boundary between the second side portion 24 and the first side portion 23 is the vertex 21. From another perspective, the first side portion 23 and the second side portion 24 branch into two at the vertex 21. The first base portion 22 is continuous with each of the first side portion 23 and the second side portion 24. The first side portion 23 is continuous with one end (first end) of the first base portion 22, and the second side portion 24 is continuous with the other end (second end) of the first base portion 22. The top surface portion 25 is surrounded by the first side portion 23, the second side portion 24, and the first base portion 22. When viewed along a line perpendicular to the first main surface 1, the shape of the top surface portion 25 is triangular.
[0035] When viewed along a line perpendicular to the first main surface 1, the first side portion 23 is inclined with respect to each of the first direction 101 and the second direction 102. The first side portion 23 may be inclined from a line parallel to the first direction 101 toward the second direction 102. The second side portion 24 may be inclined from a line parallel to the first direction 101 in a direction opposite to the second direction 102. When viewed along a line perpendicular to the first main surface 1, the first base portion 22 extends along the second direction 102. When viewed along the line perpendicular to the first main surface 1, the width of the triangular defect 20 in the second direction 102 may increase from the vertex 21 toward the first base portion 22.
[0036] 4 , silicon carbide epitaxial layer 40 has a third side portion 63, a fourth side portion 64, and a second base portion 62. When viewed along a line perpendicular to first main surface 1, a portion of third side portion 63 may overlap first side portion 23 of triangular defect 20. When viewed along a line perpendicular to first main surface 1, a portion of fourth side portion 64 may overlap second side portion 24 of triangular defect 20.
[0037] 4 , when viewed along a line perpendicular to the first main surface 1, the fourth side portion 64 is connected to the third side portion 63 at the vertex 21. From another perspective, when viewed along a line perpendicular to the first main surface 1, the third side portion 63 and the fourth side portion 64 branch into two from the vertex 21. The second base portion 62 is connected to each of the third side portion 63 and the fourth side portion 64. The third side portion 63 is connected to one end (third end portion) of the second bottom portion 62, and the fourth side portion 64 is connected to the other end (fourth end portion) of the second bottom portion 62.
[0038] When viewed along a line perpendicular to the first main surface 1, the third side portion 63 is inclined with respect to each of the first direction 101 and the second direction 102. The third side portion 63 may be inclined from a line parallel to the first direction 101 toward the second direction 102. The third side portion 63 may be substantially parallel to the first side portion 23 of the triangular defect 20. The fourth side portion 64 may be inclined from a line parallel to the first direction 101 in a direction opposite to the second direction 102. The fourth side portion 64 may be substantially parallel to the second side portion 24 of the triangular defect 20. When viewed along a line perpendicular to the first main surface 1, the second base portion 62 extends along the second direction 102. When viewed along a line perpendicular to the first main surface 1, the second base portion 62 may be substantially parallel to the first base portion 22 of the triangular defect 20. When viewed along a line perpendicular to the first main surface 1 , the second base portion 62 is in the first direction 101 relative to the first base portion 22 .
[0039] As shown in FIG. 4 , the length of the first recess 29 in the first direction 101, as viewed along a line perpendicular to the first main surface 1, is defined as a first length A1. The first length A1 is the maximum distance between the vertex 21 and the second base 62, as viewed in a direction perpendicular to the first main surface 1. When the defect 90 is a triangular defect 20, the first length A1 is defined as the length of the defect 90 in the first direction 101. When viewed along a line perpendicular to the first main surface 1, the length of the first recess 29 in the second direction 102 is defined as a first width B1. The first width B1 may be equal to the length of the second base 62. When the defect 90 is a triangular defect 20, the first width B1 is defined as the length of the defect 90 in the second direction 102. The longer of the first length A1 and the first width B1 (first measurement length) is, for example, 10 μm or more and 80 μm or less.
[0040] The ratio of the first width B1 to the first length A1 is, for example, 0.5 or more and 5 or less. The ratio of the first width B1 to the first length A1 is not particularly limited, and may be, for example, 0.8 or more, or 1.2 or more. The ratio of the first width B1 to the first length A1 is not particularly limited, and may be, for example, 4 or less, or 3 or less. When viewed along a straight line perpendicular to the first main surface 1, the width of the first recess 29 in the second direction 102 may increase from the vertex 21 toward the second base portion 62.
[0041] 5 , the triangular defect 20 may have a first side surface portion 27 and a bottom surface portion 26. The first side surface portion 27 extends along a third direction 103. The bottom surface portion 26 extends along a fourth direction 104. The surface extending along the fourth direction 104 is a base surface. The bottom surface portion 26 is continuous with the first side surface portion 27. The boundary between the bottom surface portion 26 and the first side surface portion 27 is defined as a starting point 28.
[0042] The fourth direction 104 is inclined with respect to each of the first direction 101 and the third direction 103. The fourth direction 104 is inclined toward the third direction 103 with respect to the first direction 101. The angle formed between the fourth direction 104 and the first direction 101 is an off angle θ.
[0043] The top surface portion 25 is continuous with each of the bottom surface portion 26 and the first side surface portion 27. The top surface portion 25 extends along the first direction 101. The top surface portion 25 may be substantially parallel to the first main surface 1. The top surface portion 25 forms the bottom surface of the first recess 29. The plane orientation of the top surface portion 25 may be the same as the plane orientation of the first main surface 1.
[0044] The origin 28 is, for example, located within the drift layer 42. From another perspective, in the third direction 103, the origin 28 is, for example, located between the first main surface 1 and the buffer layer 41. The origin 28 may be located within the buffer layer 41. The length of the triangular defect 20 in the first direction 101 may increase from the origin 28 toward the top surface portion 25.
[0045] 5 , silicon carbide epitaxial layer 40 has second side surface portion 67 and third side surface portion 66. Second side surface portion 67 may extend along third direction 103. Second side surface portion 67 may extend along first side surface portion 27 of triangular defect 20.
[0046] The third side surface portion 66 is continuous with the second side surface portion 67. The third side surface portion 66 extends along the fourth direction 104. The third side surface portion 66 may extend along the bottom surface portion 26 of the triangular defect 20. The second side surface portion 67 and the third side surface portion 66 form the side surfaces of the first recess 29.
[0047] 4 and 5 , first recess 29 is defined by top surface portion 25 of triangular defect 20 and second side surface portion 67 and third side surface portion 66 of silicon carbide epitaxial layer 40. From another perspective, the bottom surface of first recess 29 is defined by triangular defect 20. The side surface of first recess 29 is defined by silicon carbide epitaxial layer 40.
[0048] The polytype of silicon carbide constituting triangular defect 20 is different from the polytype of silicon carbide constituting silicon carbide epitaxial layer 40. From another perspective, the polytype of silicon carbide constituting the bottom surface of first recess 29 is different from the polytype of silicon carbide constituting silicon carbide epitaxial layer 40. The polytype of silicon carbide constituting triangular defect 20 is, for example, 3C.
[0049] 5 , the depth of first recess 29 in third direction 103 is defined as a first depth C1. First depth C1 is the distance between flat portion 10 and top surface portion 25 in third direction 103. First depth C1 is not particularly limited, but is, for example, not less than 0.01 μm and not more than 10 μm.
[0050] The first depth C1 can be measured using, for example, a white light interference microscope manufactured by Nikon Corporation (product name "BW-D507"). A mercury lamp is used as the light source. The measurement field of view is 256 μm × 256 μm. Light emitted from the light source is split into two by a beam splitter. One light is irradiated onto a reference surface. The other light is irradiated onto the first principal surface 1 and the top surface portion 25. The light reflected from both surfaces forms an image on a camera. The first depth C1 is measured based on information about interference fringes obtained from the optical path difference caused by the unevenness formed on the first principal surface 1 and the top surface portion 25.
[0051] When the defect 90 is a triangular defect 20, the area of the defect 90, as viewed along a line perpendicular to the first main surface 1, is the sum of the area of the top surface portion 25 and the area of the third side surface portion 66 (first area). The first area is 50 μm 2 The first area is, for example, 6200 μm 2 It may be the following:
[0052] <Pits> Figure 6 is an enlarged schematic plan view showing region VI in Figure 1. The enlarged schematic plan view shown in Figure 6 shows a state observed by a confocal scanning device. As shown in Figure 6, for example, pits 50 may be present in first main surface 1 of silicon carbide epitaxial substrate 100. As shown in Figure 6, the shape of pit 50 when viewed along a line perpendicular to first main surface 1 is not particularly limited, and may be, for example, substantially circular.
[0053] The length of the pit 50 in the first direction 101 is defined as a second length A2. The length of the pit 50 in the second direction 102 is defined as a second width B2. The longer of the second length A2 and the second width B2 (second measurement length) is, for example, not less than 10 μm and not more than 50 μm.
[0054] The value obtained by dividing the second length A2 by the second width B2 is not particularly limited, but may be, for example, 0.1 to 10, or 0.2 to 5. When viewed along a line perpendicular to the first main surface 1, the shape of the pit 50 may be, for example, rod-like. When viewed along a line perpendicular to the first main surface 1, the area of the pit 50 is 50 μm 2 The area of the pit 50 is, for example, 100 μm2 It may be the following:
[0055] Fig. 7 is a cross-sectional schematic diagram taken along line VII-VII in Fig. 6. The cross section shown in Fig. 7 is a cross section perpendicular to the first main surface 1. As shown in Fig. 7, the pit 50 is a depression formed in the first main surface 1. In the cross-sectional view, the side surfaces constituting the pit 50 may be curved. The depth of the pit 50 in the third direction 103 is defined as a second depth C2. The second depth C2 is not particularly limited, but is, for example, not less than 0.01 µm and not more than 0.1 µm.
[0056] <Bump> Figure 8 is an enlarged schematic plan view showing region VIII in Figure 1. The enlarged schematic plan view shown in Figure 8 shows a state observed with a confocal scanning device. As shown in Figure 8, first main surface 1 of silicon carbide epitaxial substrate 100 may have, for example, bump 60. As shown in Figure 8, the shape of bump 60 when viewed along a line perpendicular to first main surface 1 is not particularly limited, and may be, for example, substantially circular.
[0057] The length of the bump 60 in the first direction 101 is a third length A3. The length of the bump 60 in the second direction 102 is a third width B3. The longer of the third length A3 and the third width B3 (third measured length) is, for example, not less than 10 μm and not more than 50 μm.
[0058] The value obtained by dividing the third length A3 by the third width B3 is not particularly limited, but may be, for example, 0.1 to 10, or 0.2 to 5. When viewed along a line perpendicular to the first main surface 1, the shape of the bump 60 may be, for example, rod-like. When viewed along a line perpendicular to the first main surface 1, the area of the bump 60 is 50 μm 2 The area of the bump 60 is, for example, 100 μm 2 It may be the following:
[0059] 9 is a schematic cross-sectional view taken along line IX-IX in FIG. 8. The cross section shown in FIG. 9 is a cross section perpendicular to the first main surface 1. As shown in FIG. 9, the bump 60 is a protrusion formed on the first main surface 1. In other words, the bump 60 forms a convex portion on the first main surface 1. In the cross-sectional view, the side surfaces constituting the bump 60 may be curved. The height C3 of the bump 60 in the third direction 103 is not particularly limited, but is, for example, not less than 0.01 μm and not more than 0.1 μm.
[0060] <Carrot> Silicon carbide epitaxial substrate 100 may have carrot 72. When viewed along a straight line perpendicular to first main surface 1, carrot 72 extends linearly in a direction inclined with respect to first direction 101 and second direction 102. When viewed along a straight line perpendicular to first main surface 1, carrot 72 extends, for example, in a direction inclined with respect to first direction 101.
[0061] The carrot 72 is a recess caused by a screw dislocation. In a cross section perpendicular to the direction in which the carrot 72 extends, there may be a pair of protrusions on both sides of the carrot 72. The carrot 72 is defined by a pair of side surfaces and a bottom surface. The bottom surface is continuous with each of the pair of side surfaces. A portion of the side surface is formed by the protrusion.
[0062] When viewed along a straight line perpendicular to the first main surface 1, the longer of the length of the carrot 72 in the first direction 101 and the length of the carrot 72 in the second direction 102 is, for example, 10 μm or more and 150 μm or less. When viewed along a straight line perpendicular to the first main surface 1, the area of the carrot 72 is 50 μm or less. 2 The area of the carrot 72 is, for example, 900 μm 2 It may be the following:
[0063] <Downfall> Silicon carbide epitaxial substrate 100 may have downfall 71. Downfall 71 is, for example, deposits adhering to the inner wall of a film formation apparatus that fall onto silicon carbide substrate 30. Downfall 71 is, for example, polycrystalline silicon carbide particles. Downfall 71 may be, for example, carbon particles or tantalum carbide particles.
[0064] The downfall 71 may be on the silicon carbide substrate 30. In the third direction 103, the downfall 71 may be located between the first main surface 1 and the interface 3. A second recess is formed around the downfall 71, for example, in the silicon carbide epitaxial layer 40. From another perspective, the downfall 71 is located in the second recess formed in the silicon carbide epitaxial layer 40.
[0065] When viewed along a straight line perpendicular to the first main surface 1, the longer of the length of the downfall 71 in the first direction 101 and the length of the downfall 71 in the second direction 102 is, for example, 10 μm or more and 50 μm or less. When viewed along a straight line perpendicular to the first main surface 1, the area of the downfall 71 is 50 μm. 2 The area of the downfall 71 is, for example, 100 μm 2 It may be the following:
[0066] <Defect> Next, the defect 90 will be described. A confocal scanning device is used to identify the defect 90. The confocal scanning device has a differential interference optical system. As the confocal scanning device, for example, the WASAVI series "SICA 6X" manufactured by Lasertec Corporation can be used. The magnification of the objective lens is, for example, 10x.
[0067] The contrast value of the defect 90 when the first principal surface 1 is imaged using a confocal scanning device is 90 or more. The contrast value of the defect 90 when the first principal surface 1 is imaged using a confocal scanning device may be, for example, 120 or more, or 150 or more. The contrast value of the defect 90 when the first principal surface 1 is imaged using a confocal scanning device may be, for example, 256 or less, or 230 or less.
[0068] The area of the defect 90 is 50 μm 2 The area of the defect 90 is, for example, 500 μm 2 It may be 1000 μm or more. 2 The area of the defect 90 may be, for example, 5000 μm 2 It may be less than 2000 μm 2 It may be the following:
[0069] First, to identify the defect 90, light is irradiated onto the first main surface 1 using a light source. The light source is, for example, a mercury-xenon lamp. The wavelength of the light is, for example, 546 nm. While the light is being irradiated, a grayscale image of the first main surface 1 viewed in a direction from the first main surface 1 toward the second main surface 2 is captured. Specifically, the grayscale image is captured of a region of the first main surface 1 excluding a region within 5 mm of the outer circumferential edge 9 when viewed along a straight line perpendicular to the first main surface 1 (edge exclusion).
[0070] The number of pixels in the captured grayscale image is, for example, 1024 pixels x 1024 pixels. The size of a pixel is, for example, 1 nm x 1 nm. In a grayscale image, pixels represent shades of black and white (brightness). Brightness is classified into 257 levels, from 0 (minimum) to 256 (maximum). In a grayscale image, areas with high brightness (bright areas) are displayed in white, and conversely, areas with low brightness (dark areas) are displayed in black.
[0071] Defect 90 forms a recess or protrusion on first main surface 1. Therefore, when light is irradiated onto first main surface 1, defect 90 has a brighter portion and a darker portion compared to flat portion 10 of first main surface 1.
[0072] 10 is a cross-sectional view showing a state in which light is irradiated onto the first main surface 1 and the triangular defect 20. The cross-sectional view shown in FIG. 10 corresponds to the cross-sectional view shown in FIG. 5. As shown in FIG. 10, light is irradiated in a direction along, for example, arrow R. The arrow R is inclined in a first direction 101 with respect to a line perpendicular to the first main surface 1, and is inclined in a second direction 102 with respect to the line perpendicular to the first main surface 1. The arrow R is inclined in the first direction 101 by, for example, 45° with respect to the line perpendicular to the first main surface 1. The arrow R is inclined in the second direction 102 by, for example, 45° with respect to the line perpendicular to the first main surface 1.
[0073] In this case, the light irradiated onto the third side surface portion 66 is reflected in a direction along the third direction 103, so the third side surface portion 66 becomes brighter than the flat portion 10. Conversely, the second side surface portion 67 blocks part of the light, so the portion of the bottom surface portion 26 close to the second side surface portion 67 (for example, point 99) becomes darker than the flat portion 10. It is considered that as the first depth C1 increases, the portion of the bottom surface portion 26 close to the second side surface portion 67 becomes darker.
[0074] Next, the defect 90 is identified using the captured grayscale image. Fig. 11 is a schematic diagram showing the process of identifying the defect 90. The schematic diagram shown in Fig. 11 shows an image created by performing the process of identifying the defect 90 on the triangular defect 20 shown in Fig. 4. In Fig. 11, a first region 81 and a second pixel 92 indicate pixels that display the defect 90. A third pixel 93 indicates a pixel that displays the flat portion 10.
[0075] First, the average luminance value of all pixels in the grayscale image is calculated. Specifically, the luminance of each pixel in the grayscale image is added together to calculate the total luminance value. This total value is divided by the total number of pixels in the grayscale image to obtain the average luminance value of all pixels. Next, the absolute value (luminance difference) of the difference between the luminance value of each pixel in the grayscale image and the average luminance value of all pixels is calculated. Pixels whose luminance difference is equal to or greater than a predetermined value (first value) are designated as first pixels 91. From another perspective, pixels that display bright or dark areas on the first main surface 1 are designated as first pixels 91. The first value is, for example, 30.
[0076] The first pixels 91 are the pixels marked with diagonal lines in Fig. 11. For example, in the grayscale image of the triangular defect 20 shown in Fig. 4, the pixels representing the first side portion 23, the second side portion 24, and the third side surface portion 66 are defined as the first pixels 91.
[0077] Next, a first region 81 is identified by connecting a plurality of first pixels 91 that are adjacent to one another. In this specification, "adjacent pixels" includes a state in which the respective sides of two pixels overlap, and a state in which the respective corners of two pixels overlap. The area of the first region 81 is calculated by multiplying the number of first pixels included in the first region 81 by the area of the pixel. If the area of the first region 81 is equal to or greater than a predetermined value (second value), the first region 81 is considered to be the outer edge of the defect 90. The second value is, for example, 1 μm 2 is.
[0078] The pixels surrounded by the first region 81 are determined to be second pixels 92. The second pixels 92 are pixels representing a portion of the defect 90 where the absolute value of the difference (brightness difference) between the second pixels 92 and the average brightness of all pixels is less than a first value. From another perspective, the pixels representing a portion of the defect 90 that is substantially parallel to the flat portion 10 are determined to be second pixels 92. The region formed by the first region 81 and the second pixels 92 is determined to be a defect region. The defect 90 is identified by measuring the contrast value and area of the defect region using the following measurement method.
[0079] <Contrast Value of Defect Area> A method for determining the contrast value of a defect area will be described. First, the pixel with the highest brightness (maximum brightness pixel) is identified among the first region 81 and the second pixel 92. Next, the pixel with the lowest brightness (minimum brightness pixel) is identified among the first region 81 and the second pixel 92. The contrast value is determined by subtracting the brightness of the minimum brightness pixel from the brightness of the maximum brightness pixel. From another perspective, the contrast value is the difference between the maximum brightness and the minimum brightness of the multiple pixels (first region 81 and second pixel 92) displaying the defect 90. The contrast value is classified into 257 levels, from 0 (minimum) to 256 (maximum).
[0080] <Area of Defective Area> A method for calculating the area of a defective area will be described. The number of first pixels 91 and the number of second pixels 92 that make up the first area 81 are measured. The total number of first pixels 91 and the number of second pixels 92 that make up the first area 81 is multiplied by the area of the pixel to obtain the area of the defective area.
[0081] <Area Density of Defects> The area density of defects 90 having a contrast value of 90 or more on the first principal surface 1 is 2 defects / cm 2 The surface density of defects 90 with a contrast value of 90 or more is, for example, 1.5 defects / cm 2 or less, or 1 piece / cm 2 It may be 0.7 particles / cm or less. 2The surface density of defects 90 having a contrast value of 90 or more may be, for example, 0.01 defects / cm 2 It may be 0.1 pieces / cm or more. 2 It may be more than that.
[0082] On the first main surface 1, the surface density of defects 90 having a contrast value of 120 or more is, for example, 2 defects / cm 2 On the first main surface 1, the surface density of defects 90 having a contrast value of 120 or more is, for example, 1.5 defects / cm 2 or less, or 1 piece / cm 2 It may be 0.7 particles / cm or less. 2 On the first main surface 1, the surface density of the defects 90 having a contrast value of 120 or more may be, for example, 0.01 defects / cm 2 It may be 0.1 pieces / cm or more. 2 It may be more than that.
[0083] On the first main surface 1, the surface density of defects 90 having a contrast value of 150 or more is, for example, 1.9 defects / cm 2 On the first main surface 1, the surface density of defects 90 having a contrast value of 150 or more is, for example, 1.5 defects / cm 2 or less, or 1 piece / cm 2 It may be 0.55 pieces / cm or less. 2 On the first main surface 1, the surface density of defects 90 having a contrast value of 150 or more may be, for example, 0.01 defects / cm 2 It may be 0.1 pieces / cm or more. 2 It may be more than that.
[0084] The area density of the defects 90 is calculated by dividing the number of defects 90 on the first main surface 1 by the area of the first main surface 1 .
[0085] <Defect Length> Next, a method for determining the length of the defect 90 in the first direction 101 and the length of the defect 90 in the second direction 102 when viewed along a straight line perpendicular to the first principal surface 1 will be described. First, two pixels among the first region 81 and the second pixel 92 that are furthest apart in the first direction 101 are identified. As shown in FIG. 11 , the distance between the two pixels in the first direction 101 is determined to be the length of the defect 90 (fourth length A4). Specifically, the fourth length A4 is the maximum distance in the first direction 101 between two points located on the outer edges of the two pixels.
[0086] Next, two pixels among the first region 81 and the second pixel 92 that are farthest apart in the second direction 102 are identified. As shown in Fig. 11 , the distance between the two pixels is determined as the width (fourth width B4) of the defect 90. Specifically, the fourth width B4 is the maximum distance in the second direction 102 between two points located on the outer edges of the two pixels.
[0087] When viewed along a line perpendicular to first main surface 1, the longer of fourth length A4 and fourth width B4 (fourth measurement length) is, for example, 10 μm or more. The fourth measurement length may be, for example, 80 μm or more, or 140 μm or more. The fourth measurement length may be, for example, 170 μm or less, or 150 μm or less.
[0088] <Silicon carbide epitaxial substrate manufacturing apparatus> Next, the configuration of an apparatus for manufacturing silicon carbide epitaxial substrate 100 will be described. FIG. 12 is a partial cross-sectional schematic diagram showing the configuration of an apparatus for manufacturing silicon carbide epitaxial substrate 100. An apparatus 300 for manufacturing silicon carbide epitaxial substrate 100 is, for example, a hot-wall horizontal CVD (Chemical Vapor Deposition) apparatus. As shown in FIG. 12 , apparatus 300 for manufacturing silicon carbide epitaxial substrate 100 mainly includes reaction chamber 201, gas supply unit 235, control unit 245, heating element 203, quartz tube 204, a heat insulating material (not shown), and an induction heating coil (not shown).
[0089] The heating element 203 has, for example, a cylindrical shape, and defines a reaction chamber 201 therein. The heating element 203 is made of, for example, graphite. The heating element 203 is provided inside a quartz tube 204. A heat insulating material surrounds the outer periphery of the heating element 203. The induction heating coil is wound, for example, along the outer periphery of the quartz tube 204. The induction heating coil is configured so that an alternating current can be supplied to it from an external power source (not shown). This causes the heating element 203 to be induction heated. As a result, the reaction chamber 201 is heated by the heating element 203.
[0090] The reaction chamber 201 is a space surrounded by an inner wall surface 205 of a heating element 203. A susceptor 210 that holds a silicon carbide substrate 30 is provided in the reaction chamber 201. The susceptor 210 is made of silicon carbide. The silicon carbide substrate 30 is placed on the susceptor 210. The susceptor 210 is placed on a stage 202. The stage 202 is rotatably supported by a rotation shaft 209. The rotation of the stage 202 causes the susceptor 210 to rotate.
[0091] Manufacturing apparatus 300 for silicon carbide epitaxial substrate 100 further includes gas inlet 207 and gas exhaust outlet 208. Gas exhaust outlet 208 is connected to an exhaust pump (not shown). Arrows in FIG. 12 indicate the flow of gas. Gas is introduced into reaction chamber 201 from gas inlet 207 and exhausted from gas exhaust outlet 208. The pressure inside reaction chamber 201 is adjusted by balancing the amount of gas supplied and the amount of gas exhausted.
[0092] The gas supply unit 235 is configured to be able to supply a mixed gas containing a source gas, a dopant gas, and a carrier gas to the reaction chamber 201. Specifically, the gas supply unit 235 includes, for example, a first gas supply unit 231, a second gas supply unit 232, a third gas supply unit 233, and a fourth gas supply unit 234.
[0093] The first gas supply unit 231 is configured to be able to supply a first gas containing, for example, carbon atoms. The first gas supply unit 231 is, for example, a gas cylinder filled with the first gas. The first gas is, for example, propane (C3H8) gas. The first gas may also be, for example, methane (CH4) gas, ethane (C2H6) gas, acetylene (C2H2) gas, etc.
[0094] The second gas supply unit 232 is configured to be able to supply a second gas containing, for example, silane gas. The second gas supply unit 232 is, for example, a gas cylinder filled with the second gas. The second gas is, for example, silane (SiH4) gas. The second gas may be a mixed gas of silane gas and a gas other than silane.
[0095] The third gas supply unit 233 is configured to be able to supply a third gas containing, for example, nitrogen atoms. The third gas supply unit 233 is, for example, a gas cylinder filled with the third gas. The third gas is a doping gas. The third gas is, for example, ammonia gas. Ammonia gas is more susceptible to thermal decomposition than nitrogen gas, which has a triple bond.
[0096] The fourth gas supply unit 234 is configured to be able to supply a fourth gas (carrier gas) containing, for example, hydrogen, and is, for example, a gas cylinder filled with hydrogen.
[0097] The control unit 245 is configured to be able to control the flow rate of the mixed gas supplied from the gas supply unit 235 to the reaction chamber 201. Specifically, the control unit 245 may include a first gas flow rate control unit 241, a second gas flow rate control unit 242, a third gas flow rate control unit 243, and a fourth gas flow rate control unit 244. Each control unit may be, for example, an MFC (Mass Flow Controller). The control unit 245 is disposed between the gas supply unit 235 and the gas inlet 207.
[0098] <Method for manufacturing silicon carbide epitaxial substrate> Next, a method for manufacturing silicon carbide epitaxial substrate 100 according to this embodiment will be described. Fig. 13 is a flow chart schematically showing a method for manufacturing silicon carbide epitaxial substrate 100 according to this embodiment. As shown in Fig. 13, the method for manufacturing silicon carbide epitaxial substrate 100 according to this embodiment mainly includes a step (S10) of preparing a silicon carbide substrate and a step (S20) of forming a silicon carbide epitaxial layer on the silicon carbide substrate.
[0099] First, a step (S10) of preparing a silicon carbide substrate is performed. A silicon carbide single crystal of polytype 4H is produced, for example, by sublimation deposition. Next, a silicon carbide substrate 30 is prepared by slicing the silicon carbide single crystal, for example, by a wire saw. The silicon carbide substrate 30 contains an n-type impurity, for example, nitrogen. The conductivity type of the silicon carbide substrate 30 is, for example, n-type. Next, mechanical polishing is performed on the silicon carbide substrate 30. Next, chemical mechanical polishing is performed on the silicon carbide substrate 30. FIG. 14 is a cross-sectional schematic diagram showing the step (S10) of preparing a silicon carbide substrate. As shown in FIG. 14, the silicon carbide substrate 30 has a second main surface 2. In this manner, the silicon carbide substrate 30 is prepared.
[0100] Next, a step (S20) of forming a silicon carbide epitaxial layer on the silicon carbide substrate is performed. Specifically, using a hot-wall horizontal CVD apparatus shown in FIG. 12 , silicon carbide epitaxial layer 40 is formed by epitaxial growth on silicon carbide substrate 30. In the epitaxial growth, for example, silane (SiH 4 ) and propane (C 3 H 8 ) are used as source gases, and hydrogen (H 2 ) is used as a carrier gas. In the epitaxial growth, an n-type impurity such as nitrogen is introduced into silicon carbide epitaxial layer 40.
[0101] In the step (S20) of forming a silicon carbide epitaxial layer on a silicon carbide substrate, first, buffer layer 41 is formed on silicon carbide substrate 30. The pressure inside reaction chamber 201 during the formation of buffer layer 41 is set to, for example, 6 kPa. The flow rate of first gas (propane gas) during the formation of buffer layer 41 is set to, for example, 20 sccm. The flow rate of second gas (silane gas) during the formation of buffer layer 41 is set to, for example, 60 sccm. The flow rate of fourth gas (hydrogen gas) during the formation of buffer layer 41 is set to, for example, 135 slm. The growth temperature during the formation of buffer layer 41 is set to, for example, 1600°C.
[0102] Next, drift layer 42 is formed on buffer layer 41. The pressure inside reaction chamber 201 during the formation of drift layer 42 is set to, for example, 4 kPa. The flow rate of first gas (propane gas) during the formation of drift layer 42 is set to, for example, 87 sccm. The flow rate of second gas (silane gas) during the formation of drift layer 42 is set to, for example, 200 sccm. The flow rate of fourth gas (hydrogen gas) during the formation of drift layer 42 is set to, for example, 129 slm. The growth temperature during the formation of drift layer 42 is set to, for example, 1660°C.
[0103] The value (hydrogen flow rate ratio) obtained by dividing the flow rate of the fourth gas (hydrogen gas) in forming the drift layer 42 by the flow rate of the fourth gas (hydrogen gas) in forming the buffer layer 41 is, for example, 0.96. When forming the drift layer 42, the value obtained by dividing the growth temperature by the flow rate of the fourth gas (hydrogen gas) is, for example, 12.9° C. / slm.
[0104] In this manner, silicon carbide epitaxial substrate 100 (see FIGS. 1 and 2 ) is fabricated. In the method for manufacturing silicon carbide epitaxial substrate 100 according to the present disclosure, first main surface 1 of silicon carbide epitaxial substrate 100 is not subjected to chemical mechanical polishing. This makes it possible to suppress the formation of scratches on first main surface 1 due to chemical mechanical polishing. Specifically, it is possible to suppress the formation of scratches having a longitudinal length of 1 mm or more. Furthermore, according to the method for manufacturing silicon carbide epitaxial substrate 100 according to the present disclosure, the areal density of defects 90 on first main surface 1 can be reduced without performing chemical mechanical polishing. This makes it possible to reduce the time required to manufacture silicon carbide epitaxial substrate 100.
[0105] <Method of Manufacturing Silicon Carbide Semiconductor Device> Next, a method of manufacturing silicon carbide semiconductor device 400 according to this embodiment will be described. Fig. 15 is a flow diagram that schematically shows a method of manufacturing silicon carbide semiconductor device 400 according to this embodiment. As shown in Fig. 15, the method of manufacturing silicon carbide semiconductor device 400 according to this embodiment mainly includes a step (S1) of preparing a silicon carbide epitaxial substrate, a step (S2) of processing silicon carbide epitaxial substrate 100, and a step (S3) of forming an electrode on the silicon carbide epitaxial layer.
[0106] First, the step of preparing a silicon carbide epitaxial substrate (S1) is performed. In the step of preparing a silicon carbide epitaxial substrate (S1), a silicon carbide epitaxial substrate 100 according to the present embodiment is prepared (see FIGS. 1 and 2).
[0107] Next, a step (S2) is performed of processing silicon carbide epitaxial substrate 100. Specifically, silicon carbide epitaxial substrate 100 is processed as follows: First, ions are implanted into silicon carbide epitaxial substrate 100.
[0108] 16 is a schematic cross-sectional view showing a step of forming a body region. In the step of forming the body region, p-type impurities such as aluminum are ion-implanted into first main surface 1 of silicon carbide epitaxial layer 40. This forms body region 113 having p-type conductivity. Portions where body region 113 is not formed become drift layer 42 and buffer layer 41. The thickness of body region 113 is, for example, 0.9 μm. Silicon carbide epitaxial layer 40 includes buffer layer 41, drift layer 42, and body region 113.
[0109] Next, a step of forming a source region is performed. FIG. 17 is a schematic cross-sectional view showing the step of forming the source region. Specifically, n-type impurities such as phosphorus are ion-implanted into the body region 113. This forms a source region 114 having n-type conductivity. The thickness of the source region 114 is, for example, 0.4 μm. The concentration of the n-type impurities in the source region 114 is higher than the concentration of the p-type impurities in the body region 113.
[0110] Next, a p-type impurity such as aluminum is ion-implanted into the source region 114 to form a contact region 118. The contact region 118 is formed to penetrate the source region 114 and the body region 113 and to be in contact with the drift layer 42. The concentration of the p-type impurity in the contact region 118 is higher than the concentration of the n-type impurity in the source region 114.
[0111] Next, activation annealing is performed to activate the implanted impurities. The temperature of the activation annealing is, for example, 1500° C. or higher and 1900° C. or lower. The activation annealing time is, for example, about 30 minutes. The atmosphere of the activation annealing is, for example, an argon atmosphere.
[0112] Next, a step of forming trenches in first main surface 1 of silicon carbide epitaxial layer 40 is performed. FIG. 18 is a cross-sectional schematic diagram showing the step of forming trenches in first main surface 1 of silicon carbide epitaxial layer 40. A mask 117 having openings is formed on first main surface 1 including source region 114 and contact region 118. Using mask 117, source region 114, body region 113, and a portion of drift layer 42 are removed by etching. As an etching method, for example, inductively coupled plasma reactive ion etching can be used. Specifically, for example, inductively coupled plasma reactive ion etching using SF or a mixed gas of SF and O as a reactive gas is used. A recess is formed in first main surface 1 by etching.
[0113] Next, thermal etching is performed on the recesses. Thermal etching can be performed, for example, by heating the first main surface 1 with the mask 117 formed thereon in an atmosphere containing a reactive gas having at least one type of halogen atom. The at least one type of halogen atom includes at least one of chlorine (Cl) atoms and fluorine (F) atoms. The atmosphere can include, for example, Cl2, BCl3, SF6, or CF4. For example, thermal etching is performed using a mixed gas of chlorine gas and oxygen gas as the reactive gas, with the heat treatment temperature set to, for example, 700°C or higher and 1000°C or lower. The reactive gas may contain a carrier gas in addition to the above-mentioned chlorine gas and oxygen gas. Examples of the carrier gas that can be used include nitrogen gas, argon gas, and helium gas.
[0114] 18 , a trench 56 is formed in the first main surface 1 by thermal etching. The trench 56 is defined by a sidewall surface 53 and a bottom wall surface 54. The sidewall surface 53 is formed by the source region 114, the body region 113, and the drift layer 42. The bottom wall surface 54 is formed by the drift layer 42. Next, the mask 117 is removed from the first main surface 1.
[0115] Next, a step of forming a gate insulating film is performed. FIG. 19 is a schematic cross-sectional view showing the step of forming a gate insulating film. Specifically, silicon carbide epitaxial substrate 100 having trench 56 formed in first main surface 1 is heated in an oxygen-containing atmosphere at a temperature of, for example, 1300° C. or higher and 1400° C. or lower. This forms gate insulating film 115 that is in contact with drift layer 42 at bottom wall surface 54, in contact with drift layer 42, body region 113, and source region 114 at sidewall surface 53, and in contact with source region 114 and contact region 118 at first main surface 1.
[0116] Next, a step of forming a gate electrode is performed. FIG. 20 is a cross-sectional view showing a step of forming a gate electrode and an interlayer insulating film. The gate electrode 127 is formed inside the trench 56 so as to contact the gate insulating film 115. The gate electrode 127 is disposed inside the trench 56 and is formed on the gate insulating film 115 so as to face each of the sidewall surface 53 and the bottom wall surface 54 of the trench 56. The gate electrode 127 is formed by, for example, a low pressure chemical vapor deposition (LPCVD) method.
[0117] Next, an interlayer insulating film 126 is formed. The interlayer insulating film 126 is formed so as to cover the gate electrode 127 and to be in contact with the gate insulating film 115. The interlayer insulating film 126 is formed by, for example, chemical vapor deposition. The interlayer insulating film 126 is made of, for example, a material containing silicon dioxide. Next, the interlayer insulating film 126 and part of the gate insulating film 115 are etched so as to form openings over the source region 114 and the contact region 118. As a result, the contact region 118 and the source region 114 are exposed from the gate insulating film 115.
[0118] Next, a step of forming a source electrode is performed. The source electrode 116 is formed so as to be in contact with each of the source region 114 and the contact region 118. The source electrode 116 is formed by, for example, a sputtering method. The source electrode 116 is made of a material containing, for example, Ti (titanium), Al (aluminum), and Si (silicon).
[0119] Next, alloying annealing is performed. Specifically, the source electrode 116 in contact with each of the source region 114 and the contact region 118 is maintained at a temperature of, for example, 900° C. or higher and 1100° C. or lower for about 5 minutes. As a result, at least a portion of the source electrode 116 is silicided. This forms the source electrode 116 in ohmic contact with the source region 114. The source electrode 116 may also form an ohmic contact with the contact region 118.
[0120] Next, the source wiring 119 is formed. The source wiring 119 is electrically connected to the source electrode 116. The source wiring 119 is formed so as to cover the source electrode 116 and the interlayer insulating film 126.
[0121] Next, a step of forming a drain electrode is carried out. First, silicon carbide substrate 30 is polished at second main surface 2. This reduces the thickness of silicon carbide substrate 30. Next, drain electrode 123 is formed. Drain electrode 123 is formed so as to be in contact with second main surface 2. In this manner, silicon carbide semiconductor device 400 according to this embodiment is manufactured.
[0122] 21 is a cross-sectional schematic diagram showing the configuration of a silicon carbide semiconductor device 400 according to this embodiment. The silicon carbide semiconductor device 400 is, for example, a MOSFET (Metal Oxide Semiconductor Field Effect Transistor). The silicon carbide semiconductor device 400 mainly includes a silicon carbide epitaxial substrate 100, a gate electrode 127, a gate insulating film 115, a source electrode 116, a drain electrode 123, a source wiring 119, and an interlayer insulating film 126. The silicon carbide epitaxial substrate 100 includes a buffer layer 41, a drift layer 42, a body region 113, a source region 114, and a contact region 118. Silicon carbide semiconductor device 400 may be, for example, an IGBT (Insulated Gate Bipolar Transistor).
[0123] Next, the effects of the method for manufacturing silicon carbide epitaxial substrate 100 and the method for manufacturing silicon carbide semiconductor device 400 according to this embodiment will be described.
[0124] The inventors have made the following findings while conducting a detailed investigation into the causes of the decrease in yield of silicon carbide semiconductor devices 400. Specifically, the inventors have found that when silicon carbide semiconductor devices 400 are fabricated using silicon carbide epitaxial substrates 100 on which defects having a certain shape are formed, silicon carbide semiconductor devices 400 are likely to suffer from poor characteristics. Specifically, when a contrast value is 90 or more when photographed using a confocal scanning device and an area of 50 μm when viewed along a line perpendicular to first main surface 1 is 90 or more, 2 It has been found that the above-described defects 90 affect the occurrence of defective characteristics of silicon carbide semiconductor device 400 .
[0125] As a result of extensive investigation, the inventors have found that in a method for manufacturing silicon carbide epitaxial substrate 100, the areal density of defects 90 described above can be reduced by focusing on the value obtained by dividing the flow rate of hydrogen gas in forming drift layer 42 by the flow rate of hydrogen gas in forming buffer layer 41 (hydrogen flow rate ratio) and the value obtained by dividing the growth temperature in forming drift layer 42 by the flow rate of hydrogen gas.
[0126] If the hydrogen flow rate ratio is small, the flow rate of hydrogen gas decreases when forming the drift layer 42, and the concentration of hydrogen gas inside the reaction chamber 201 decreases. As a result, the decomposition of silane gas and propane gas (growth gas) is accelerated. Therefore, if the hydrogen flow rate ratio is excessively small, the decomposition of the growth gas is excessively accelerated. As a result, it is thought that the amounts of silicon and carbon generated by the decomposition of the growth gas become excessively large compared to the amounts of silicon and carbon reacted during epitaxial growth.
[0127] Conversely, if the hydrogen flow rate ratio is too high, the hydrogen flow rate becomes excessively high compared to the growth gas flow rate when forming the drift layer 42. In this case, decomposition of the growth gas is excessively suppressed. As a result, the concentrations of silane and propane inside the reaction chamber 201 are thought to increase.
[0128] When forming the silicon carbide epitaxial layer 40, etching of the silicon carbide epitaxial layer 40 by hydrogen gas occurs simultaneously with the growth of the silicon carbide epitaxial layer 40. When forming the drift layer 42, if the value obtained by dividing the growth temperature by the flow rate of the fourth gas (hydrogen gas) is excessively large, the etching rate is considered to be excessively fast. Conversely, if the value obtained by dividing the growth temperature by the flow rate of the fourth gas (hydrogen gas) is excessively small, the etching rate is considered to be excessively slow.
[0129] In the silicon carbide epitaxial substrate 100 according to the present disclosure, the defect 90 has a contrast value of 90 or more when photographed using a confocal scanning device. 2 The surface density of the defects 90 on the first main surface 1 is 2 / cm 2 This reduces the area density of defects 90, which are a factor in reducing the yield of silicon carbide semiconductor devices 400. This enables the yield of silicon carbide semiconductor devices 400 to be improved.
[0130] In silicon carbide epitaxial substrate 100 according to the present disclosure, the longer of the lengths of defects 90 in first direction 101 and second direction 102, as viewed along a straight line perpendicular to first main surface 1 (fourth measurement length), may be 10 μm or more. In this manner, the areal density of defects 90 having a long fourth measurement length is reduced. As a result, the yield of silicon carbide semiconductor devices 400 can be improved.
[0131] <Sample Preparation> First, silicon carbide epitaxial substrates 100 according to Samples 1 to 14 were prepared. Silicon carbide epitaxial substrates 100 according to Samples 1 to 7 are comparative examples. Silicon carbide epitaxial substrates 100 according to Samples 8 to 14 are examples.
[0132]
[0133]
[0134] Table 1 shows the conditions for forming buffer layer 41 in the fabrication of silicon carbide epitaxial substrate 100 according to Sample 1 to Sample 14. Table 2 shows the conditions for forming drift layer 42 in the fabrication of silicon carbide epitaxial substrate 100 according to Sample 1 to Sample 14.
[0135] As shown in Tables 1 and 2, in the fabrication of silicon carbide epitaxial substrates 100 according to Samples 1 to 14, the value obtained by dividing the flow rate of the fourth gas (hydrogen flow rate) in the formation of drift layer 42 by the hydrogen flow rate in the formation of buffer layer 41 (hydrogen flow rate ratio) was changed. Specifically, the hydrogen flow rate ratio was set to 0.87 or more and 1.00 or less. In addition, in the fabrication of silicon carbide epitaxial substrates 100 according to Samples 1 to 14, the value obtained by dividing the growth temperature in the formation of drift layer 42 by the hydrogen flow rate (growth temperature / hydrogen flow rate) was changed. The growth temperature / hydrogen flow rate ratio was set to 12.3° C. / slm or more and 14.1° C. / slm or less. The hydrogen flow rate in the formation of drift layer 42 was set to 118 slm or more and 135 slm or less.
[0136] In fabricating silicon carbide epitaxial substrates 100 according to Samples 1 to 14, the growth temperature in forming buffer layer 41 was set to 1600°C. The pressure inside reaction chamber 201 in forming buffer layer 41 was set to 6 kPa. The flow rate of the second gas (silane flow rate) in forming buffer layer 41 was set to 60 sccm. The flow rate of the first gas (propane flow rate) in forming buffer layer 41 was set to 20 sccm. The flow rate of hydrogen in forming buffer layer 41 was set to 135 sccm.
[0137] In fabricating silicon carbide epitaxial substrates 100 according to Samples 1 to 14, the growth temperature in forming drift layer 42 was set to 1660°C. The pressure inside reaction chamber 201 in forming drift layer 42 was set to 4 kPa. The silane flow rate in forming drift layer 42 was set to 200 sccm. The propane flow rate in forming drift layer 42 was set to 87 sccm. In silicon carbide epitaxial substrates 100 according to Samples 1 to 14, first main surface 1 was in an as-grown state.
[0138] <Evaluation Method> The areal density of defects 90 on first main surface 1 was measured using the above-described measurement method for silicon carbide epitaxial substrates 100 according to Samples 1 to 14. Specifically, the areal density of defects 90 having a contrast value of 90 or more, the areal density of defects 90 having a contrast value of 120 or more, and the areal density of defects 90 having a contrast value of 150 or more were measured.
[0139] <Evaluation results>
[0140]
[0141] Table 3 shows the areal density of defects 90 in silicon carbide epitaxial substrates 100 for Samples 1 to 14. FIG. 22 is a graph showing the areal density of defects 90 having a contrast value of 90 or more and the hydrogen flow rate ratio for Samples 1 to 14. FIG. 23 is a graph showing the areal density of defects 90 having a contrast value of 120 or more and the hydrogen flow rate ratio for Samples 1 to 14. FIG. 24 is a graph showing the areal density of defects 90 having a contrast value of 150 or more and the hydrogen flow rate ratio for Samples 1 to 14. In each of FIGS. 22 , 23 , and 24 , the horizontal axis represents the hydrogen flow rate ratio. The vertical axis represents the areal density of defects 90. The point indicated by P1 represents the areal density of defects 90 in Sample 1. Similarly, the points indicated by P2 to P14 represent the areal densities of defects 90 in Samples 2 to 14.
[0142] As shown in Table 3, FIG. 22, FIG. 23, and FIG. 24, when the hydrogen flow rate ratio is less than 0.96 or greater than 0.96 (Samples 1 to 7), the surface density of defects 90 with a contrast value of 90 or greater is 2.29 defects / cm 2 The surface density of defects 90 with a contrast value of 120 or more was 2.20 defects / cm 2 The surface density of defects 90 with a contrast value of 150 or more was 1.98 defects / cm 2 That was all.
[0143] As shown in Table 3, FIG. 22, FIG. 23, and FIG. 24, when the hydrogen flow rate ratio was 0.96 (samples 8 to 14), the surface density of defects 90 with a contrast value of 90 or more was 1.43 defects / cm 2 The surface density of defects 90 with a contrast value of 120 or more was 1.36 defects / cm 2 The surface density of defects 90 with a contrast value of 150 or more was 1.30 defects / cm 2 It was as follows.
[0144] FIG. 25 is a graph showing the areal density of defects 90 having a contrast value of 90 or more versus the growth temperature / hydrogen flow rate in samples 1 to 14. FIG. 26 is a graph showing the areal density of defects 90 having a contrast value of 120 or more versus the growth temperature / hydrogen flow rate in samples 1 to 14. FIG. 27 is a graph showing the areal density of defects 90 having a contrast value of 150 or more versus the growth temperature / hydrogen flow rate in samples 1 to 14. In each of FIGS. 25, 26, and 27, the horizontal axis represents the growth temperature / hydrogen flow rate. The vertical axis represents the areal density of defects 90. The point indicated by P1 represents the areal density of defects 90 in sample 1. Similarly, the points indicated by P2 to P14 represent the areal densities of defects 90 in samples 2 to 14.
[0145] As shown in Table 3, FIGS. 25, 26, and 27, when the growth temperature / hydrogen flow rate is less than 12.9 or greater than 12.9 (samples 1 to 7), the areal density of defects 90 with a contrast value of 90 or greater is 2.29 defects / cm. 2 The surface density of defects 90 with a contrast value of 120 or more was 2.20 defects / cm 2 The surface density of defects 90 with a contrast value of 150 or more was 1.98 defects / cm 2 That was all.
[0146] As shown in Table 3, FIGS. 25, 26, and 27, when the growth temperature / hydrogen flow rate ratio was 12.9 (samples 8 to 14), the area density of defects 90 with a contrast value of 90 or more was 1.43 defects / cm 2The surface density of defects 90 with a contrast value of 120 or more was 1.36 defects / cm 2 The surface density of defects 90 with a contrast value of 150 or more was 1.30 defects / cm 2 It was as follows.
[0147] From the above results, it was confirmed that silicon carbide epitaxial substrate 100 according to the example had a reduced areal density of defects 90 compared to silicon carbide epitaxial substrate 100 according to the comparative example.
[0148] The embodiments and examples disclosed herein are illustrative in all respects and should not be considered limiting. The scope of the present invention is defined by the claims, not by the above-described embodiments, and is intended to include meanings equivalent to the claims and all modifications within the scope thereof.
[0149] 1 First main surface (main surface), 2 Second main surface, 3 Interface, 7 Orientation flat, 8 Arc-shaped portion, 9 Outer periphery, 10 Flat portion, 20 Triangular defect, 21 Vertex, 22 First base portion, 23 First edge portion, 24 Second edge portion, 25 Top surface portion, 26 Bottom surface portion, 27 First side portion, 28 Starting point, 29 First recess, 30 Silicon carbide substrate, 40 Silicon carbide epitaxial layer, 41 Buffer layer, 42 Drift layer, 50 Pit, 53 Side wall surface, 54 Bottom wall surface, 56 Trench, 60 Bump, 62 Second bottom portion, 63 Third edge portion, 64 Fourth edge portion, 66 Third side portion, 67 Second side portion, 71 Downfall, 72 Carrot, 81 First region, 90 Defect, 91 First pixel, 92 Second pixel, 93 Third pixel, 99 Point, 100 Silicon carbide epitaxial substrate, 101 First direction, 102 Second direction, 103 Third direction, 104 Fourth direction, 113 Body region, 114 Source region, 115 Gate insulating film, 116 Source electrode, 117 Mask, 118 Contact region, 119 Source wiring, 123 Drain electrode, 126 Interlayer insulating film, 127 Gate electrode (electrode), 201 Reaction chamber, 202 Stage, 203 Heating element, 204 Quartz tube, 205 Inner wall surface, 207 Gas inlet, 208 Gas exhaust port, 209 Rotation shaft, 210 Susceptor, 231 First gas supply unit, 232 Second gas supply unit, 233 Third gas supply unit, 234 Fourth gas supply unit, 235 Gas supply unit, 241 First gas flow rate control unit, 242 Second gas flow rate control unit, 243 Third gas flow rate control unit, 244 Fourth gas flow rate control unit, 245 Control unit, 300 Manufacturing apparatus, 400 Silicon carbide semiconductor device, A1 First length, A2 Second length, A3 Third length, A4 Fourth length, B1 First width, B2 Second width, B3 Third width, B4 Fourth width, C1 First depth, C2 Second depth, C3 Height, R Arrow, W Maximum diameter, θ Off-angle.
Claims
1. A semiconductor device comprising: a silicon carbide substrate; a silicon carbide epitaxial layer provided on the silicon carbide substrate; and a plurality of defects formed in the silicon carbide epitaxial layer, the silicon carbide epitaxial layer constituting a main surface, each of the plurality of defects being exposed at the main surface, each of the plurality of defects having a contrast value of 90 or more when photographed using a confocal scanning device, and an areal density of the plurality of defects on the main surface being 2 defects / cm. 2 The area of each of the plurality of defects is 50 μm or less when viewed along a straight line perpendicular to the main surface. 2 The above is a silicon carbide epitaxial substrate.
2. The silicon carbide epitaxial substrate according to claim 1, wherein the plurality of defects include a portion whose polytype is 3C, and the plurality of defects and the silicon carbide epitaxial layer form a recess.
3. The silicon carbide epitaxial substrate according to claim 1, wherein the plurality of defects include at least one of a bump, a pit, a carrot, a triangular defect, and a downfall.
4. A silicon carbide epitaxial substrate according to any one of claims 1 to 3, wherein, when viewed along a straight line perpendicular to the main surface, for each of the plurality of defects, the longer of a length in a first direction and a length in a second direction perpendicular to the first direction is 10 μm or more.
5. The silicon carbide epitaxial substrate according to any one of claims 1 to 4, wherein the main surface is in an as-grown state.
6. A method for manufacturing a silicon carbide semiconductor device, comprising the steps of: preparing a silicon carbide epitaxial substrate according to any one of claims 1 to 5; and forming an electrode on the silicon carbide epitaxial layer.
Citation Information
Patent Citations
Silicon carbide epitaxial wafer, apparatus for manufacturing silicon carbide epitaxial wafer, method for manufacturing silicon carbide epitaxial wafer, and semiconductor device
JP2017059670A
Method of manufacturing silicon carbide epitaxial wafer, method of manufacturing silicon carbide semiconductor device, and device of manufacturing silicon carbide epitaxial wafer