product
The packaging structure with a specific multilayer design, including EVOH and inorganic vapor-deposited layers, addresses the challenge of maintaining gas barrier and appearance integrity with sodium chloride contents, while ensuring recyclability by optimizing layer thickness and composition.
Patent Information
- Application Number
- PCT/JP2024/017032
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-05-09
- Filing Date
- 2024-05-08
- Publication Date
- 2024-11-14
AI Technical Summary
Packaging materials with polyolefin multilayer structures, containing an inorganic vapor-deposited layer on an EVOH layer, face challenges in maintaining gas barrier properties and appearance when storing contents with sodium chloride, while also being recyclable.
A packaging structure with a multilayer design that includes an EVOH layer as the main barrier component, an inorganic vapor-deposited layer, a heat seal layer, and additional layers like an adhesive and polyolefin layers, where the total thickness of polyolefin layers on the inner side is 45 μm or more, and the inorganic vapor-deposited layer is 7 nm to 100 nm thick, ensuring recyclability and preventing deterioration.
The solution effectively maintains gas barrier properties and appearance when storing contents with high sodium chloride content, while allowing for efficient recycling by suppressing gelation and maintaining excellent appearance and barrier properties.
Smart Images

Figure JPOXMLDOC01-APPB-T000001 
Figure JPOXMLDOC01-APPB-T000002
Abstract
Description
product
[0001] The present invention relates to a product having a package and contents.
[0002] Packaging materials for long-term storage of foods and other foods often require gas barrier properties, including oxygen barrier properties. The use of packaging materials with high gas barrier properties can prevent oxidative deterioration of foods and other foods due to oxygen intrusion and the proliferation of microorganisms. Metal foils or metal-deposited layers made of aluminum or other metals, and inorganic oxide-deposited layers made of silicon oxide or aluminum oxide or other inorganic oxides, are widely used to improve gas barrier properties. Meanwhile, resin layers with gas barrier properties, such as vinyl alcohol polymers and polyvinylidene chloride, are also widely used. Vinyl alcohol polymers exhibit gas barrier properties by crystallizing and densifying due to hydrogen bonding between hydroxyl groups in the molecules. Among these, ethylene-vinyl alcohol copolymers (hereinafter sometimes abbreviated as "EVOH") are suitable for melt molding due to their excellent thermal stability. Therefore, with the development of coextrusion technology, multilayer films with an EVOH layer as an intermediate layer have become widely used as gas barrier packaging materials (Patent Document 1).
[0003] Furthermore, in recent years, driven by environmental and waste issues, there has been a growing global demand for post-consumer recycling (hereinafter sometimes simply referred to as "recycling"), which involves recovering and recycling packaging materials consumed in the market. Recycling typically involves shredding recovered packaging materials, separating and cleaning them as necessary, and then melt-mixing them using an extruder. The pellets obtained in this manner are then used to manufacture various molded products. In this regard, packaging materials are required to be composed of as single a material as possible (mono-materialization), which allows for the production of high-purity, high-quality recycled resins. To this end, there has been an increasing demand for barrier films primarily made of polyolefins, which are widely used as packaging materials. A vapor-deposited multilayer film has been proposed, which combines gas barrier properties and recyclability by laminating an inorganic vapor-deposited layer on the EVOH layer of a polypropylene-based multilayer film (Patent Document 2).
[0004] International Publication No. 2020 / 071513 International Publication No. 2020 / 184523
[0005] In a package using a polyolefin-based multilayer structure in which an inorganic vapor deposition layer is laminated on an EVOH layer, the appearance and gas barrier properties of the package may deteriorate during storage of contents containing sodium chloride. On the other hand, if a package in which aluminum foil is laminated instead of the inorganic vapor deposition layer is used for the purpose of suppressing deterioration of the appearance, it is difficult to uniformly mix with other components in the melt-mixing step during recovery and recycling, making it difficult to maintain a good balance of appearance characteristics, gas barrier properties, and recyclability.
[0006] In view of the above circumstances, an object of the present invention is to provide a packaging product that uses a polyolefin-based multilayer structure in which an inorganic vapor deposition layer is laminated on an EVOH layer, and that maintains recyclability while suppressing deterioration in appearance and gas barrier properties when contents containing sodium chloride are stored.
[0007] According to the present invention, the above-mentioned object can be achieved by the following: [1] a product comprising a package having a multilayer structure and a content accommodated in the package and having a sodium chloride content of 1% by mass or more, the multilayer structure comprising a barrier layer (A) containing an ethylene-vinyl alcohol copolymer (a) (hereinafter may be abbreviated as "EVOH (a)") as a main component, an inorganic vapor-deposited layer (B) laminated on the barrier layer (A) and having an average thickness of 7 nm or more and 100 nm or less, and a heat-seal layer (E) containing a polyolefin (e) as a main component, which is the outermost layer of the barrier layer (A) on the side opposite to the side on which the inorganic vapor-deposited layer (B) is laminated, the total average thickness of the layers containing a polyolefin-based resin as a main component laminated on the side of the barrier layer (A) opposite to the side on which the inorganic vapor-deposited layer (B) is laminated is 45 μm or more, and the heat-seal layer (E) is located on the inner surface side of the package; [2] the product of [1], in which the barrier layer (A) is stretched at least uniaxially; [3] The product of [1] or [2], wherein the average thickness of the barrier layer (A) is 0.1 μm or more and 20 μm or less; [4] Any of the products of [1] to [3], wherein the ratio of the average thickness of the barrier layer (A) to the average thickness of the multilayer structure is 5% or less; [5] Any of the products of [1] to [4], wherein the inorganic vapor deposition layer (B) is composed of aluminum, aluminum oxide, or silicon oxide; [6] Any of the products of [1] to [5], wherein the average thickness of the heat seal layer (E) is 20 μm or more and 200 μm or less; [7] Any of the products of [1] to [6], wherein the multilayer structure has an adhesive layer (C) containing an adhesive resin (c) as a main component and a polyolefin layer (D) containing a polyolefin (d) as a main component, and has a layer configuration in which the inorganic vapor deposition layer (B), barrier layer (A), adhesive layer (C), polyolefin layer (D), and heat seal layer (E) are laminated in this order; [8] The product of [7], in which the barrier layer (A), the adhesive layer (C), and the polyolefin layer (D) are stretched in at least one direction; [9] The product of [7] or [8], in which the barrier layer (A), the adhesive layer (C), and the polyolefin layer (D) are co-extruded films;
[10] Any of the products of [7] to [9], in which the polyolefin layer (D) and the heat seal layer (E) are made of the same resin type as the main component resin;
[11] Any of the products of [1] to
[10] , in which the sodium chloride content of the contents is 5% by mass or less;
[12] The product of any one of [1] to
[11] , wherein the contents contain lipids;
[13] The product of
[12] , wherein the lipid content of the contents is 95% by mass or less;
[14] The product of
[12] or
[13] , wherein the lipids contain triglycerides as a main component.
[0008] According to the present invention, a packaging body can be provided that uses a polyolefin-based multilayer structure in which an inorganic vapor-deposited layer is laminated on the surface of an EVOH layer, and that maintains recyclability while suppressing deterioration in appearance and gas barrier properties when contents containing sodium chloride are stored. Here, "recyclability" in this specification means that when recycled materials from the packaging included in the product of the present invention are melt-kneaded to produce a recycled composition, gelation of the resin is suppressed and a recycled composition with excellent appearance can be efficiently produced, and this can be evaluated by a recyclability test described in the examples.
[0009] Hereinafter, embodiments of the present invention will be described. Note that in the following description, specific materials (compounds, etc.) that exhibit specific functions may be exemplified, but the present invention is not limited to embodiments using such materials. Furthermore, the exemplified materials may be used alone or in combination, unless otherwise specified.
[0010] The product of the present invention comprises a package having a multilayer structure and a content contained in the package, the content having a sodium chloride content of 1% by mass or more. The multilayer structure comprises a barrier layer (A) containing EVOH (a) as a primary component, an inorganic vapor deposition layer (B) laminated on the barrier layer (A) and having an average thickness of 7 nm or more and 100 nm or less, and a heat-seal layer (E) containing polyolefin (e) as a primary component and serving as the outermost layer on the side of the barrier layer (A) opposite to the side on which the inorganic vapor deposition layer (B) is laminated. The sum of the average thicknesses of the layers containing polyolefin-based resins as primary components laminated on the side of the barrier layer (A) opposite to the side on which the inorganic vapor deposition layer (B) is laminated is 45 μm or more, and the heat-seal layer (E) is located on the inner surface of the package. Here, the barrier layer (A) and the inorganic vapor deposition layer (B) may be laminated directly or via another layer such as an adhesive layer. The heat-seal layer (E) as the outermost layer of the multilayer structure means that the heat-seal layer (E) is exposed. Furthermore, the phrase "the total average thickness of layers containing a polyolefin resin as a main component which are laminated on the side of the barrier layer (A) opposite to the side on which the inorganic vapor deposition layer (B) is laminated is 45 μm or more" means that the total average thickness of layers containing a polyolefin resin as a main component which are laminated on the side of the barrier layer (A) opposite to the side on which the inorganic vapor deposition layer (B) is laminated is 45 μm or more, and does not exclude the inclusion of another layer on the side of the barrier layer (A) opposite to the side on which the inorganic vapor deposition layer (B) is laminated.
[0011] The multilayer structure in the product of the present invention tends to have excellent gas barrier properties while maintaining recyclability by having a barrier layer (A) containing EVOH (a) as a main component. Furthermore, by having an inorganic vapor deposition layer (B) having an average thickness of 7 nm to 100 nm laminated on the barrier layer (A), the multilayer structure also tends to have excellent gas barrier properties. Furthermore, by having the total average thickness of layers containing polyolefin resins as a main component laminated on the side of the barrier layer (A) opposite to the side on which the inorganic vapor deposition layer (B) is laminated being 45 μm or more, deterioration of the appearance and gas barrier properties tends to be suppressed even when the package contains contents containing 1 mass % or more of sodium chloride.
[0012] In this specification, "major component" refers to a component that is present at more than 50% by mass. Unless otherwise specified, the "average thickness" of each layer refers to the average thickness measured at any five locations. "ppm" refers to the mass content (ppm by mass). "Polyethylene" refers to ethylene homopolymers, copolymers of 80 mol% or more ethylene and 20 mol% or less α-olefin monomers, and copolymers of 90 mol% or more ethylene and less than 10 mol% non-olefin monomers whose functional groups contain no atoms other than carbon, oxygen, and hydrogen atoms. "Polypropylene" refers to propylene homopolymers, copolymers of 80 mol% or more propylene and 20 mol% or less α-olefin monomers, and copolymers of 90 mol% or more propylene and less than 10 mol% non-olefin monomers whose functional groups contain no atoms other than carbon, oxygen, and hydrogen atoms. "Acid-modified polyethylene" refers to a polymer obtained by modifying polyethylene with an acid. Acid-modified polyethylene may be a polymer in which at least one of acid groups and acid anhydride groups has been introduced into polyethylene. "Acid-modified polypropylene" refers to a polymer obtained by modifying polypropylene with an acid. Acid-modified polypropylene may be a polymer in which at least one of an acidic group and an acid anhydride group has been introduced into polypropylene. "Polyolefin" refers to a homopolymer or copolymer of one or more α-olefin monomers, and a copolymer of 90 mol% or more of one or more α-olefin monomers and less than 10 mol% of a non-olefin monomer whose functional group contains no atoms other than carbon, oxygen, and hydrogen atoms. "Acid-modified polyolefin" refers to a polymer obtained by modifying a polyolefin with an acid. Acid-modified polyolefin may be a polymer in which at least one of an acidic group and an acid anhydride group has been introduced into the polyolefin. "Polyolefin-based resin" refers to polyolefins and modified polyolefins (such as acid-modified polyolefins). Modified polyolefins refer to polymers obtained by modifying polyolefins. Furthermore, the "surface (or surface layer)" of a multilayer film or multilayer structure does not refer to the front or back, but rather to the exposed surface.That is, a multilayer film or a multilayer structure has two surfaces. Similarly, a multilayer film or a multilayer structure has two outermost layers. In this specification, "consisting essentially of" means that optional components may be included to the extent that the effects of the present invention are not affected, and "consisting only of" means that optional components other than impurities that are inevitably included are excluded. In addition, in this specification, a numerical range described using "to" means that the numerical values before and after "to" are included as the lower and upper limits.
[0013] [Barrier layer (A)] The multilayer structure of the product of the present invention has good gas barrier properties due to the provision of a barrier layer (A) containing EVOH (a) as a main component. Furthermore, since the barrier layer (A) has good affinity with the inorganic vapor deposition layer (B) described below, when the inorganic vapor deposition layer (B) is laminated directly on the barrier layer (A), the gas barrier properties are even better, and the gas barrier properties tend to be maintained even when subjected to physical stress, particularly bending. A plurality of barrier layers (A) may be provided.
[0014] EVOH (a) is usually obtained by saponifying an ethylene-vinyl ester copolymer obtained by polymerizing ethylene and a vinyl ester. The ethylene unit content of EVOH (a) is preferably 10 mol% or more and 65 mol% or less, more preferably 20 mol% or more and 60 mol% or less, and even more preferably 25 mol% or more and 55 mol% or less. When the ethylene unit content of EVOH (a) is 10 mol% or more, the melt moldability of EVOH (a) is improved. Furthermore, when the ethylene unit content of EVOH (a) is 65 mol% or less, the gas barrier properties of the multilayer structure in the product of the present invention are improved. The ethylene unit content is the content (mol%) of ethylene units relative to all monomer units constituting EVOH.
[0015] The saponification degree of EVOH (a) is preferably 90 mol% or more. The saponification degree means the ratio of the number of vinyl alcohol units to the total number of vinyl alcohol units and vinyl ester units in EVOH (a). The saponification degree of EVOH (a) is more preferably 95 mol% or more, and even more preferably 99 mol% or more. When the saponification degree is 90 mol% or more, the gas barrier property of the multilayer structure in the product of the present invention tends to be improved. The upper limit of the saponification degree of EVOH (a) may be 100 mol%. The ethylene unit content and saponification degree of EVOH (a) are 1 It is determined by H-NMR measurement.
[0016] EVOH (a) may be a mixture of two or more types of EVOH having different ethylene unit contents. In this case, the difference in ethylene unit content between the EVOHs having the most different ethylene unit contents is preferably 30 mol% or less, more preferably 20 mol% or less, even more preferably 15 mol% or less, and may be 3 mol% or more. Similarly, EVOH (a) may be a mixture of two or more types of EVOH having different degrees of saponification. In this case, the difference in saponification degree between the EVOHs having the most different degrees of saponification is preferably 7 mol% or less, more preferably 5 mol% or less, and may be 0.5 mol% or more.
[0017] EVOH (a) may contain other monomer units other than ethylene units, vinyl ester units, and vinyl alcohol units, as long as the effects of the present invention are not impaired. In particular, by introducing a modifying group containing a primary hydroxyl group having a specific structure, it may be possible to achieve high levels of both gas barrier properties and moldability of EVOH (a). The content of other monomer units is preferably 5% by mass or less, more preferably 3% by mass or less, even more preferably 1% by mass or less, and particularly preferably substantially none. Examples of such other monomers include alkenes such as propylene, butylene, pentene, and hexene; 3-acyloxy-1-propene, 3-acyloxy-1-butene, 4-acyloxy-1-butene, 3,4-diacyloxy-1-butene, 3-acyloxy-4-methyl-1-butene, 4-acyloxy-2-methyl-1-butene, 4-acyloxy-3-methyl-1-butene, 4-acyloxy-4-methyl ... 1-butene, 3,4-diacyloxy-2-methyl-1-butene, 4-acyloxy-1-pentene, 5-acyloxy-1-pentene, 4,5-diacyloxy-1-pentene, 4-acyloxy-1-hexene, 5-acyloxy-1-hexene, 6-acyloxy-1-hexene, 5,6-diacyloxy-1-hexene, 1,3-diacetoxy-2-methyl- Examples of suitable vinyl silane compounds include alkenes having an ester group such as ethylenepropane or saponified products thereof; unsaturated acids such as acrylic acid, methacrylic acid, crotonic acid, itaconic acid, or the like, or their anhydrides, salts, or mono- or dialkyl esters; nitriles such as acrylonitrile and methacrylonitrile; amides such as acrylamide and methacrylamide; olefin sulfonic acids such as vinyl sulfonic acid, allyl sulfonic acid, and methallylsulfonic acid, or their salts; vinyl silane compounds such as vinyltrimethoxysilane, vinyltriethoxysilane, vinyltri(β-methoxyethoxy)silane, and γ-methacryloxypropylmethoxysilane; alkyl vinyl ethers, vinyl ketone, N-vinylpyrrolidone, vinyl chloride, and vinylidene chloride.
[0018] The EVOH (a) may be post-modified by a technique such as urethanization, acetalization, cyanoethylation, or oxyalkylenation.
[0019] The melt flow rate (MFR) of EVOH (a) measured in accordance with JIS K7210 (2014) (210°C, under a load of 2.16 kg) is preferably 0.2 to 30 g / 10 min. The MFR of EVOH (a) is more preferably 1.0 g / 10 min or more, even more preferably 5.0 g / 10 min or more, and particularly preferably 10 g / 10 min or more. On the other hand, the MFR of EVOH (a) is more preferably 25 g / 10 min or less, even more preferably 20 g / 10 min or less.
[0020] (Other Compounds) The barrier layer (A) may contain compounds other than the EVOH (a) to the extent that the effects of the present invention are not impaired. Examples of the other compounds include carboxylic acid compounds, phosphoric acid compounds, boron compounds, metal salts (alkali metal salts, alkaline earth metal salts, etc.), antioxidants, UV absorbers, plasticizers, lubricants, fillers, antistatic agents, etc. The content of the other compounds in the barrier layer (A) is usually 5% by mass or less, preferably 2% by mass or less, more preferably 1% by mass or less, and even more preferably 0.5% by mass or less. From the viewpoint of suppressing the formation of particles and coloration during melt molding of a pulverized product of a multilayer structure including the barrier layer (A), it is preferable to contain an alkali metal ion, a carboxylic acid, and / or a phosphoric acid compound. Furthermore, by containing a boron compound, the melt viscosity of the barrier layer (A) and the pulverized product of the multilayer structure including the barrier layer (A) can be controlled.
[0021] The carboxylic acid compound may be a monocarboxylic acid, a polycarboxylic acid, or a combination thereof. The carboxylic acid compound may be an ion, and the carboxylic acid ion may form a salt with a metal ion. The content of carboxylic acid and carboxylic acid ion in the barrier layer (A) is preferably 50 to 400 ppm. As the carboxylic acid compound, for example, an aliphatic carboxylic acid such as acetic acid or stearic acid is preferably used. When the barrier layer (A) contains a carboxylic acid compound, discoloration during melt molding tends to be prevented.
[0022] The phosphate compound is not particularly limited, and various acids such as phosphoric acid and phosphorous acid, and salts thereof, can be used. The phosphate may be contained in the form of primary phosphate, secondary phosphate, or tertiary phosphate, with primary phosphate being preferred. The cation species is also not particularly limited, but alkali metal salts are preferred. Among these, sodium dihydrogen phosphate and potassium dihydrogen phosphate are preferred. When the barrier layer (A) contains a phosphate compound, the content of the phosphate compound in the barrier layer (A) is preferably 5 to 100 ppm, calculated as phosphate radicals. A phosphate compound content of 5 ppm or more tends to improve discoloration resistance during melt molding. On the other hand, a phosphate compound content of 100 ppm or less tends to improve melt moldability.
[0023] The boron compound is not particularly limited, and examples thereof include boric acids, borate esters, borate salts, and boron hydrides. Specifically, examples of boric acids include orthoboric acid, metaboric acid, and tetraboric acid. Examples of borate esters include triethyl borate and trimethyl borate. Examples of borates include alkali metal salts, alkaline earth metal salts, and borax of the various boric acids listed above. Among these compounds, orthoboric acid (hereinafter sometimes simply referred to as boric acid) is preferred. When the barrier layer (A) contains a boron compound, the content of the boron compound in the barrier layer (A) is preferably 50 to 400 ppm, calculated as elemental boron. A boron compound content of 50 ppm or more tends to suppress torque fluctuations during heat melting. On the other hand, a boron compound content of 400 ppm or less tends to maintain good moldability.
[0024] The cation species of the alkali metal salt is not particularly limited, but sodium salt or potassium salt is preferred. The anion species of the alkali metal salt is also not particularly limited. It can be added as a carboxylate, carbonate, hydrogencarbonate, phosphate, hydrogenphosphate, borate, hydroxide, etc. When the barrier layer (A) contains an alkali metal salt, the content of the alkali metal salt in the barrier layer (A) is preferably 40 to 500 ppm in terms of metal element. When the content of the alkali metal salt is 40 ppm or more, interlayer adhesion tends to be good. On the other hand, when the content of the alkali metal salt is 500 ppm or less, melt stability tends to be excellent.
[0025] The cation species of the alkaline earth metal salt is not particularly limited, but magnesium salt or calcium salt is preferred. The anion species of the alkaline earth metal salt is also not particularly limited. It can be added as a carboxylate, carbonate, hydrogencarbonate, phosphate, hydrogenphosphate, borate, hydroxide, etc. The content of the alkaline earth metal salt in the barrier layer (A) is preferably 10 to 300 ppm. When the barrier layer (A) contains an alkaline earth metal salt, deterioration during repeated melt-molding of the molded body and the generation of deteriorated products such as gel tend to be suppressed. It is also preferable to use a polyvalent metal salt such as a zinc salt instead of the alkaline earth metal salt.
[0026] As the antioxidant, ultraviolet absorber, plasticizer, lubricant, filler and antistatic agent, those exemplified below can be used.
[0027] Antioxidants: 2,5-di-t-butylhydroquinone, 2,6-di-t-butyl-p-cresol, 4,4'-thiobis(6-t-butylphenol), 2,2'-methylenebis(4-methyl-6-t-butylphenol), octadecyl-3-(3',5'-di-t-butyl-4'-hydroxyphenyl)propionate, 4,4'-thiobis(6-t-butylphenol), etc.
[0028] Ultraviolet absorbers: ethylene-2-cyano-3,3'-diphenylacrylate, 2-(2'-hydroxy-5'-methylphenyl)benzotriazole, 2-(2'-hydroxy-3'-t-butyl-5'-methylphenyl)5-chlorobenzotriazole, 2-hydroxy-4-methoxybenzophenone, 2,2'-dihydroxy-4-methoxybenzophenone, 2-hydroxy-4-octoxybenzophenone, etc.
[0029] Plasticizers: dimethyl phthalate, diethyl phthalate, dioctyl phthalate, wax, liquid paraffin, phosphate ester, etc.
[0030] Lubricants: stearic acid amide, oleic acid amide, erucic acid amide, behenic acid amide, ethylene bisstearic acid amide, methylol stearic acid amide, N-oleyl palmitamide, N-stearyl erucamide, liquid paraffin, natural paraffin, synthetic paraffin, polyolefin wax, stearyl alcohol, lauryl alcohol, stearic acid, lauric acid, myristic acid, behenic acid, montanic acid, stearyl stearate, stearyl laurate, calcium stearate, magnesium stearate, zinc stearate, lead stearate, etc.
[0031] Fillers: fiberglass, asbestos, ballastonite, calcium silicate, etc.
[0032] Antistatic agents: glycerin mono fatty acid esters, fatty acid diethanolamides, alkyldiethanolamines, alkyl sulfonates, alkylbenzene sulfonates, alkyltrimethylammonium salts, alkylbenzyldimethylammonium salts, alkylbetaines, alkylimidazolium betaines, etc.
[0033] The barrier layer (A) may further contain a thermoplastic resin other than EVOH (a). Examples of thermoplastic resins other than EVOH (a) include various polyolefins (polyethylene, polypropylene, poly-1-butene, poly-4-methyl-1-pentene, ethylene-propylene copolymers, copolymers of ethylene and an α-olefin having 4 or more carbon atoms, copolymers of polyolefins and maleic anhydride, ethylene-vinyl ester copolymers, ethylene-acrylic acid ester copolymers, and modified polyolefins obtained by graft-modifying these with unsaturated carboxylic acids or derivatives thereof), various polyamides (nylon 6, nylon 6.6, nylon 6 / 66 copolymer, nylon 11, nylon 12, polymetaxylylene adipamide, etc.), various polyesters (polyethylene terephthalate, polybutylene terephthalate, polyethylene naphthalate, etc.), polyvinyl chloride, polyvinylidene chloride, polystyrene, polyacrylonitrile, polyurethane, polycarbonate, polyacetal, polyacrylate, and modified polyvinyl alcohol resins. The content of the thermoplastic resin in the barrier layer (A) is usually less than 40% by mass, preferably less than 30% by mass, more preferably less than 20% by mass, even more preferably less than 10% by mass, and may be less than 5% by mass or even less than 1% by mass, and it is particularly preferable that the barrier layer (A) is substantially free of the thermoplastic resin.
[0034] From the viewpoint of more significantly achieving the effects of the present invention, the proportion of EVOH (a) in the resin constituting the barrier layer (A) is preferably 60% by mass or more, more preferably 70% by mass or more, even more preferably 80% by mass, even more preferably 90% by mass or more, particularly preferably 95% by mass or more, and may be 98% by mass or more or 99% by mass or more. The resin constituting the barrier layer (A) may be substantially EVOH (a) alone. From the viewpoint of more significantly achieving the effects of the present invention, the proportion of EVOH (a) in the barrier layer (A) is preferably 60% by mass or more, more preferably 70% by mass or more, even more preferably 80% by mass, even more preferably 90% by mass or more, particularly preferably 95% by mass or more, and may be 98% by mass or more or 99% by mass or more. The barrier layer (A) may consist essentially of EVOH (a) alone. The upper limit of the proportion of EVOH (a) in the barrier layer (A) may be 100% by mass.
[0035] The barrier layer (A) is preferably stretched at least uniaxially. That is, the barrier layer (A) is preferably uniaxially or biaxially stretched. When the barrier layer (A) is a stretched layer, particularly when it is a biaxially stretched layer, even a relatively thin barrier layer (A) can have good gas barrier properties.
[0036] When the barrier layer (A) is a stretched layer, it is preferably stretched at least uniaxially by 2 times or more but less than 12 times, and more preferably stretched at least uniaxially by 3 times or more but less than 6 times. It is also preferably stretched biaxially by 2 times or more but less than 12 times, and more preferably stretched biaxially by 3 times or more but less than 6 times.
[0037] The lower limit of the average thickness of the barrier layer (A) is preferably 0.1 μm, more preferably 0.3 μm. When the average thickness of the barrier layer (A) is equal to or greater than the above lower limit, it is possible to improve the gas barrier property, etc. The upper limit of the average thickness of the barrier layer (A) is preferably 20 μm, more preferably 15 μm, and may be 10 μm, 5 μm, 3 μm, 2 μm, or 1 μm. When the average thickness of the barrier layer (A) is equal to or less than the above upper limit, it is possible to reduce the thickness and weight of the multilayer structure, etc.
[0038] The oxygen permeability of the barrier layer (A) is 50 mL 20 μm / (m 2 ·day·atm) or less, and 10mL·20μm / (m 2 ·day·atm) or less is more preferable, and 5 mL ·20 μm / (m 2 ·day·atm) or less is more preferable, and 1 mL·20 μm / (m 2 Here, the oxygen permeability is a value measured in accordance with the method described in ISO 14663-2 Annex C (1999) under conditions of 20°C and 65% RH.
[0039] The barrier layer (A) may consist of a single layer or multiple layers.
[0040] The barrier layer (A) can be a resin film. The method for producing a resin film having a barrier layer (A) is not particularly limited, and examples thereof include a melting method, a solution method, and a calendaring method. Among these, the melting method is preferred. Examples of the melting method include a casting method and an inflation method. Among these, the casting method is preferred. Alternatively, a stretched film stretched by a known method can also be used.
[0041] The resin composition used to form the barrier layer (A) can be produced by melt-kneading EVOH (a) and, if necessary, other components. Each component may be blended in a solid state, such as a powder, or as a melt. Alternatively, the components may be blended as a solute in a solution or a dispersoid in a dispersion. An aqueous solution and an aqueous dispersion are preferred as the solution and dispersion, respectively. For melt-kneading, known mixing or kneading devices, such as a kneader-ruder, extruder, mixing roll, or Banbury mixer, can be used. The temperature range during melt-kneading can be adjusted appropriately depending on the melting point of the EVOH (a) and each component used, and is typically 150 to 250°C. Alternatively, the barrier layer (A) may be produced by pre-adding some components to EVOH (a) and then melt-kneading the additional components as described above. Pre-adding some components to EVOH (a) involves immersing EVOH (a) in the form of pellets or powder in a solution containing the dissolved components.
[0042] [Inorganic Vapor Deposition Layer (B)] The multilayer structure in the product of the present invention includes an inorganic vapor deposition layer (B) having an average thickness of 7 nm to 100 nm laminated on the barrier layer (A). Here, another layer such as an adhesive layer may be provided between the barrier layer (A) and the inorganic vapor deposition layer (B), or the barrier layer (A) and the inorganic vapor deposition layer (B) may be laminated directly. However, it is preferable that the barrier layer (A) and the inorganic vapor deposition layer (B) are laminated directly. By providing the inorganic vapor deposition layer (B) on the barrier layer (A), good barrier properties tend to be exhibited. The inorganic vapor deposition layer (B) can be formed by vapor deposition of an inorganic substance. Examples of inorganic substances include metals (e.g., aluminum), metal oxides (e.g., silicon oxide, aluminum oxide), metal nitrides (e.g., silicon nitride), metal nitride oxides (e.g., silicon oxynitride), and metal carbonitrides (e.g., silicon carbonitride). Among these, inorganic vapor deposition layers (B) formed of aluminum, aluminum oxide, silicon oxide, magnesium oxide, or silicon nitride are preferred from the viewpoint of industrial productivity, and inorganic vapor deposition layers (B) composed of aluminum, aluminum oxide, or silicon oxide are more preferred. When light-blocking properties are to be imparted to the packaging material, it is preferably composed of aluminum. From the viewpoints of visibility of the contents as a packaging material and suitability for microwave ovens, it is preferably composed of aluminum oxide or silicon oxide. Note that even if the metal vapor deposition layer is made of aluminum, irreversible oxidation may occur, and some aluminum oxide may be contained. When some aluminum oxide is contained in the metal vapor deposition layer, the ratio (Omol / Almol) of the amount of oxygen atoms (Omol) to the amount of aluminum atoms (Almol) constituting the metal vapor deposition layer is preferably 0.5 or less, more preferably 0.3 or less, even more preferably 0.1 or less, and particularly preferably 0.05 or less.
[0043] The method for forming the inorganic vapor deposition layer (B) is not particularly limited, and examples thereof include physical vapor deposition methods such as vacuum deposition (e.g., resistance heating deposition, electron beam deposition, molecular beam epitaxy, etc.), sputtering, and ion plating; and chemical vapor deposition methods such as thermal chemical vapor deposition (e.g., catalytic chemical vapor deposition), photochemical vapor deposition, plasma chemical vapor deposition (e.g., capacitively coupled plasma, inductively coupled plasma, surface wave plasma, electron cyclotron resonance, dual magnetron, atomic layer deposition, etc.), and metalorganic chemical vapor deposition.
[0044] The average thickness of the inorganic vapor deposition layer (B) is 7 nm or more and 100 nm or less. The average thickness of the inorganic vapor deposition layer (B) is preferably 15 nm or more, more preferably 30 nm or more. The average thickness of the inorganic vapor deposition layer (B) is preferably 80 nm or less, more preferably 70 nm or less. The average thickness of the inorganic vapor deposition layer (B) is the average value of thicknesses at any 10 points on a cross section of the inorganic vapor deposition layer (B) measured using an electron microscope.
[0045] When the inorganic vapor deposition layer (B) is made of aluminum, the molar ratio of aluminum to aluminum hydroxide (Al / Al(OH)) at the center of the inorganic vapor deposition layer (B) in the depth direction (thickness direction) measured by a TEM-EDS device is 3 ) is preferably 1.1 or more, more preferably 1.5 or more, even more preferably 2.0 or more, particularly preferably 2.5 or more, and may be 2.6 or more. The molar ratio is preferably within the above range even after the storage test described in the Examples (storage for 200 days at 43°C and 50% RH). When the molar ratio is within the above range, the appearance and oxygen barrier properties tend to be well maintained. Aluminum hydroxide is thought to be produced when aluminum or aluminum oxide is corroded by the influence of sodium chloride, moisture, etc., and the molar ratio can be used as an index of the degree of corrosion.
[0046] [Heat-seal layer (E)] The multilayer structure in the product of the present invention has a heat-seal layer (E) that is the outermost layer of the barrier layer (A) on the side opposite to the side on which the inorganic vapor deposition layer (B) is laminated. Furthermore, in the multilayer structure, the total average thickness of the layers containing a polyolefin resin as a main component and laminated on the side of the barrier layer (A) opposite to the side on which the inorganic vapor deposition layer (B) is laminated is 45 μm or more. Examples of the total average thickness of the layers containing a polyolefin resin as a main component and laminated on the side of the barrier layer (A) opposite to the side on which the inorganic vapor deposition layer (B) is laminated being 45 μm or more include a case where the average thickness of the heat-seal layer (E) is 45 μm or more, a case where a polyolefin layer (D) described below is present between the heat-seal layer (E) and the barrier layer (A), and the total average thickness of the polyolefin layer (D) and the heat-seal layer (E) is 45 μm or more, etc.
[0004] Thus, by providing a layer containing a polyolefin resin as a main component with a certain thickness or more on the inner side (the heat seal layer (E) side) of the barrier layer (A) (EVOH layer) (i.e., on the side of the heat seal layer (E)), deterioration of the appearance and gas barrier property tends to be suppressed even when a product containing contents with a sodium chloride content of 1% by mass or more is stored. The reason for this is unclear, but if the average thickness of the polyolefin resin layer on the inner side (the heat seal layer (E) side) of the barrier layer (A) is less than 45 μm, the inorganic vapor deposition layer (B) is affected by the contents, tending to deteriorate the gas barrier property and appearance. This is thought to be due to the fact that the barrier layer (A) is a hydrophilic resin. While it is desirable to employ a configuration in which the inorganic vapor deposition layer (B) is laminated on the barrier layer (A) to achieve high barrier property, it is difficult to suppress deterioration of the inorganic vapor deposition layer (B) due to the contents, which poses a problem in achieving both gas barrier property and maintaining the gas barrier property when storing specific contents. The present inventors have conducted research and have found a solution to this problem, and this invention is the present invention.
[0047] Examples of the polyolefin (e) contained as a main component in the heat seal layer (E) include homopolymers or copolymers of olefins such as polyethylene (linear low-density polyethylene, low-density polyethylene, medium-density polyethylene, high-density polyethylene, etc.), ethylene-propylene copolymer, polypropylene, propylene-α-olefin (α-olefin having 4 to 20 carbon atoms) copolymer, polybutene, and polypentene. Among these, polyethylene or polypropylene is preferred, and polypropylene is more preferred. One or more types of polyolefins can be used.
[0048] The proportion of the polyolefin (e) in the heat-seal layer (E) is preferably 60% by mass or more, more preferably 70% by mass or more, even more preferably 80% by mass or more, even more preferably 90% by mass or more, particularly preferably 95% by mass or more, and may be 98% by mass or more or 99% by mass or more. The upper limit of the proportion of the polyolefin (e) in the heat-seal layer (E) may be 100% by mass.
[0049] The heat seal layer (E) may be a non-stretched layer or a stretched layer, but from the viewpoint of good heat sealability, it is preferable that the heat seal layer (E) is a non-stretched layer.
[0050] The lower limit of the average thickness of the heat-sealable layer (E) is preferably 20 μm, more preferably 30 μm, and even more preferably 40 μm. When the average thickness of the heat-sealable layer (E) is equal to or greater than the above lower limit, deterioration of the appearance and gas barrier properties of the product of the present invention tends to be suppressed even after storage. The upper limit of the average thickness of the heat-sealable layer (E) is preferably 200 μm, more preferably 150 μm, and even more preferably 100 μm. When the average thickness of the heat-sealable layer (E) is equal to or less than the above upper limit, it is possible to reduce the thickness of the multilayer structure.
[0051] The heat seal layer (E) may consist of a single layer or multiple layers.
[0052] The multilayer structure in the product of the present invention may have an adhesive layer (C) containing an adhesive resin (c) as a main component and a polyolefin layer (D) containing a polyolefin (d) as a main component. Alternatively, the multilayer structure may have a layer configuration in which an inorganic vapor deposition layer (B), a barrier layer (A), an adhesive layer (C), a polyolefin layer (D), and a heat seal layer (E) are laminated in this order. While other layers (e.g., adhesive layers described below) may be present between the layers, it is preferable that the layers are directly laminated. By providing the multilayer structure with such a layer configuration, deterioration of the appearance and gas barrier properties of the product of the present invention can be further suppressed even after storage, and the recyclability of the package tends to be improved.
[0053] [Adhesive Layer (C)] The multilayer structure in the product of the present invention may have an adhesive layer (C) containing an adhesive resin (c) as a main component, from the viewpoint of obtaining a multilayer structure with excellent appearance. The adhesive resin (c) is preferably an acid-modified polyolefin, and more preferably a carboxylic acid-modified polyolefin obtained by graft polymerizing an unsaturated carboxylic acid such as maleic anhydride or a derivative thereof onto a polyolefin. The melting point of the adhesive resin (c) mainly depends on the polyolefin before carboxylic acid modification. The above description of the polyolefin (e) can be applied to the polyolefin as is. The adhesive resin (c) is preferably an acid-modified polyethylene or acid-modified polypropylene, and more preferably acid-modified polypropylene. When the adhesive resin (c), which is the main component of the adhesive layer (C), is an acid-modified polyolefin, the adhesive layer (C) is a layer containing a polyolefin resin as a main component.
[0054] The proportion of the acid-modified polyolefin in the adhesive resin (c) is preferably 70% by mass or more, more preferably 80% by mass or more, and even more preferably 95% by mass or more, and may be substantially composed of only the acid-modified polyolefin. The proportion of the adhesive resin (c) in the adhesive layer (C) is preferably 70% by mass or more, more preferably 80% by mass or more, and even more preferably 95% by mass or more, and may be 97% by mass or more or 99% by mass or more, and may be substantially composed of only the adhesive resin (c). The upper limit of the proportion of the adhesive resin (c) in the adhesive layer (C) may be 100% by mass.
[0055] [Polyolefin Layer (D)] The multilayer structure in the product of the present invention may have a polyolefin layer (D) from the viewpoint of improving the water vapor barrier property and flex resistance and suppressing deterioration in the appearance and gas barrier property of the product of the present invention after storage.
[0056] The polyolefin layer (D) contains a polyolefin (d) as a main component. As the polyolefin (d), the same polyolefins as those described above as the polyolefin (e) can be used, and preferred embodiments thereof are also the same as the preferred embodiments of the polyolefin (e) described above.
[0057] The content of the polyolefin (d) in the polyolefin layer (D) is preferably 80% by mass or more, more preferably 90% by mass or more, even more preferably 97% by mass or more, and may be 99% by mass or more. The upper limit of the content of the polyolefin (d) in the polyolefin layer (D) may be 100% by mass.
[0058] The polyolefin layer (D) may be a non-stretched layer or a stretched layer, but from the viewpoint of further suppressing deterioration of the appearance and gas barrier properties when contents containing sodium chloride are stored, it is preferably stretched at least uniaxially, and more preferably stretched biaxially.
[0059] The lower limit of the average thickness per polyolefin layer (D) is preferably 1 μm, more preferably 5 μm. When the average thickness of the polyolefin layer (D) is equal to or greater than the above lower limit, sufficient moisture resistance and the like can be obtained. The upper limit of the average thickness per polyolefin layer (D) is preferably 100 μm, more preferably 50 μm, even more preferably 40 μm, and may even be 30 μm. When the average thickness of the polyolefin layer (D) is equal to or less than the above upper limit, the multilayer structure can be made thinner.
[0060] The polyolefin layer (D) may consist of a single layer or a plurality of layers.
[0061] In the multilayer structure of the product of the present invention, the polyolefin layer (D') may be provided as the outermost layer on the side opposite the heat-sealable layer (E). When the multilayer structure includes the polyolefin layer (D') as the outermost layer, it is preferable that the polyolefin layer (D') be a stretched layer from the viewpoint of increasing the melting point difference with the heat-sealable layer (E) and improving the heat-sealability. The polyolefin layer (D') is a layer containing polyolefin as a main component. Specific and preferred embodiments of the polyolefin contained in the polyolefin layer (D') and the average thickness of the polyolefin layer (D') are the same as those of the polyolefin (d) contained in the polyolefin layer (D) and the average thickness of the polyolefin layer (D) described above. However, the polyolefin (d) contained in the polyolefin layer (D) and the polyolefin contained in the polyolefin layer (D') may be the same or different. Furthermore, the average thickness of the polyolefin layer and the average thickness of the polyolefin layer (D') may be the same or different.
[0062] The adhesive layer (C), the polyolefin layer (D), the polyolefin layer (D'), and the heat seal layer (E) may contain other components such as antioxidants, plasticizers, heat stabilizers (melt stabilizers), photoinitiators, deodorizers, UV absorbers, antistatic agents, lubricants, colorants, fillers, desiccants, bulking agents, pigments, dyes, processing aids, flame retardants, and antifogging agents, provided that the total amount of these components relative to each layer is less than 50% by mass, preferably less than 40% by mass, more preferably less than 30% by mass, even more preferably less than 20% by mass, and particularly preferably less than 10% by mass, and may be less than 5% by mass, less than 3% by mass, or less than 1% by mass, as long as the effects of the present invention are not impaired.
[0063] The barrier layer (A), adhesive layer (C), and polyolefin layer (D) are preferably stretched at least uniaxially, and more preferably biaxially. In such cases, deterioration of appearance after a storage test can be reduced, and deterioration of oxygen barrier properties after a storage test can be reduced. When the barrier layer (A), adhesive layer (C), and polyolefin layer (D) are uniaxially stretched, they are preferably stretched at least 2 times but less than 12 times in the uniaxial direction, and more preferably stretched 3 times or more but less than 6 times in the uniaxial direction. When the barrier layer (A), adhesive layer (C), and polyolefin layer (D) are biaxially stretched, they are preferably stretched 2 times or more but less than 10 times in the longitudinal direction and 2 times or more but less than 15 times in the transverse direction, and more preferably stretched 3 times or more but less than 6 times in the longitudinal direction and 6 times or more but less than 12 times in the transverse direction.
[0064] The barrier layer (A), adhesive layer (C), and polyolefin layer (D) are preferably stretched together. For example, the barrier layer (A), adhesive layer (C), and polyolefin layer (D) may be formed into a multilayer film in which they are laminated in this order, and then stretched.
[0065] The method for producing a multilayer film comprising a barrier layer (A), an adhesive layer (C), and a polyolefin layer (D) is not particularly limited, but a coextrusion method is preferred. That is, the multilayer film comprising a barrier layer (A), an adhesive layer (C), and a polyolefin layer (D) is preferably a coextruded film. The method for producing a coextruded film is not particularly limited, but it is generally produced by a melt molding method in which the films are melt-extruded using an extruder.
[0066] [Multilayer structure] The multilayer structure in the product of the present invention has an inorganic vapor deposition layer (B) on a barrier layer (A), a heat seal layer (E) on the outermost surface of the barrier layer (A) opposite to the surface having the inorganic vapor deposition layer (B), and the total average thickness of layers containing a polyolefin resin as a main component laminated on the surface of the barrier layer (A) opposite to the surface having the inorganic vapor deposition layer (B) is 45 μm or more. Therefore, in the multilayer structure in the product of the present invention, the inorganic vapor deposition layer (B) is located on the surface of the barrier layer (A) opposite to the content. The multilayer structure having such a configuration can suppress deterioration in the appearance and gas barrier properties of the product of the present invention after storage.
[0067] The total average thickness of the layers containing a polyolefin resin as a main component laminated on the side of the barrier layer (A) opposite to the side on which the inorganic vapor deposition layer (B) is laminated is preferably 60 μm or more, more preferably 80 μm or more, from the viewpoint of maintaining the appearance and gas barrier properties of the product of the present invention at a higher level after storage. The total average thickness may be 150 μm or less, or 120 μm or less.
[0068] The average thickness of the multilayer structure is preferably 250 μm or less, more preferably 200 μm or less, and even more preferably 150 μm or less, from the viewpoint of improving heat sealability. The average thickness of the multilayer structure may be 50 μm or more, or may be 60 μm or more.
[0069] The ratio of the average thickness of the barrier layer (A) to the average thickness of the multilayer structure is preferably 5% or less. When this ratio is 5% or less, recyclability tends to be improved. From the viewpoint of further improving recyclability, this ratio is more preferably 3% or less, and even more preferably 2% or less. This ratio may be 0.1% or more.
[0070] In the multilayer structure, the heat seal layer (E) can be laminated by a known method, such as a coextrusion method, an extrusion coating method, a lamination method, etc. When a lamination method is used, an adhesive layer described below may be provided.
[0071] The multilayer structure is not particularly limited, and examples thereof include the following layer structures. In the layer structures below, the barrier layer (A) is represented as A, the inorganic vapor deposition layer (B) as B, the heat seal layer (E) as E, the adhesive layer (C) as C, the polyolefin layer (D) as D, and the polyolefin layer (D') as D', and " / " means that the layers are directly laminated, and " / / " means that the layers are laminated via an adhesive layer or that the layers are directly laminated. Regarding " / / ", a preferred embodiment is that the layers are laminated via an adhesive layer. (1) B / A / / E (2) B / A / C / E (3) B / A / C / D / / E (4) D' / / B / A / / E (5) D' / / B / A / C / E (6) D' / / B / A / C / D / / E Among these, D' / / B / A / C / D / / E is preferred from the viewpoint of further suppressing deterioration of appearance and gas barrier properties when contents containing sodium chloride are stored while maintaining industrial productivity and recyclability.
[0072] From the viewpoint of improving recyclability, it is preferable that the multilayer structure does not have a metal layer having an average thickness of 1 μm or more.
[0073] In the multilayer structure, it is preferable that the resins that are the main components of the polyolefin layer (D) and the heat-seal layer (E) are the same resin type from the viewpoint of improving recyclability. Here, the same resin type means that, for example, when the resin that the heat-seal layer (E) mainly contains is polypropylene, the resin that the polyolefin layer (D) mainly contains is also polypropylene. In addition, in the multilayer structure, it is also preferable that the resins that are the main components of the adhesive layer (C), the polyolefin layer (D), and the heat-seal layer (E) are the same resin type from the viewpoint of improving recyclability. Regarding the same resin type, for example, if it is a polypropylene-based resin (polypropylene or modified polypropylene), it is the same resin type regardless of whether it is modified or not, the difference in average molecular weight, etc. For example, it is preferable that the resins that are the main components of the adhesive layer (C), the polyolefin layer (D), and the heat-seal layer (E) are all polypropylene-based resins (polypropylene or modified polypropylene).
[0074] Furthermore, in the multilayer structure, the resins that are the main components of the polyolefin layer (D), the polyolefin layer (D'), and the heat-seal layer (E) are preferably the same resin type, and more preferably these resins are polypropylene-based resins.Furthermore, the resins that are the main components of the adhesive layer (C), the polyolefin layer (D), the polyolefin layer (D'), and the heat-seal layer (E) are preferably the same resin type, and more preferably these resins are polypropylene-based resins.
[0075] Each layer constituting the multilayer structure may be laminated via an adhesive layer, if necessary. The adhesive layer can be formed by applying a known adhesive and drying it. The adhesive is preferably a two-component reactive polyurethane adhesive in which a polyisocyanate component and a polyol component are mixed and reacted. The thickness of the adhesive layer is not particularly limited, but is preferably 1 to 5 μm, and more preferably 2 to 4 μm.
[0076] The multilayer structure may include layers other than those described above, provided that the effects of the present invention are not impaired. Examples of such layers include a printed layer. The printed layer may be included anywhere in the multilayer structure of the present invention, but is preferably located on at least one surface of the barrier layer (A). Examples of the printed layer include a film obtained by applying a solution containing a pigment or dye and, if necessary, a binder resin, followed by drying. Examples of methods for applying the printed layer include gravure printing and various other application methods using a wire bar, spin coater, die coater, or the like. The thickness of the printed layer is not particularly limited, but is preferably 0.5 to 10 μm, more preferably 1 to 4 μm.
[0077] The multilayer structure may have an inorganic vapor deposition layer other than the inorganic vapor deposition layer (B), but preferably does not include an inorganic vapor deposition layer on the content side of the barrier layer (A). When the multilayer structure does not include an inorganic vapor deposition layer on the content side of the barrier layer (A), deterioration of the appearance and gas barrier property after storage tends to be further suppressed.
[0078] [Packaging] The packaging in the product of the present invention comprises the multilayer structure and has a heat seal layer (E) on the inner surface. In the packaging, the heat seal layer (E) may be located on the inner surface, and the heat seal layer (E) may be the innermost layer of the packaging. The packaging is preferably a packaging obtained by heat sealing the heat seal layers (E) of the multilayer structure together. The packaging may be formed from the multilayer structure. The packaging is used for packaging purposes, and its shape is not limited. The packaging may be in the form of a sheet, or may be formed into a predetermined shape such as a bag.
[0079] The packaging material is formed into various forms depending on the application, such as vertical form-fill-seal bags, spouted pouches, laminated tube containers, container lids, etc.
[0080] [Contents] The product of the present invention has a content contained in a package, the content having a sodium chloride content of 1% by mass or more. When the content contains 1% by mass or more of sodium chloride, deterioration of the inorganic vapor deposition layer (B) tends to be accelerated, which may lead to deterioration of the appearance and gas barrier property. However, by using the multilayer structure, deterioration of the inorganic vapor deposition layer (B) tends to be suppressed.
[0081] The sodium chloride content in the contents is preferably 5% by mass or less, more preferably 3% by mass or less, and even more preferably 2.5% by mass or less. When the sodium chloride content is 5% by mass or less, deterioration of the appearance and gas barrier properties of the product after storage tends to be reduced. The sodium chloride content in the contents may be 1.5% by mass or more. When the sodium chloride content in the contents is 1.5% by mass or more, the problem of the present invention becomes more pronounced, and the effect of suppressing deterioration of the appearance and gas barrier properties by the multilayer structure in the product of the present invention becomes more pronounced.
[0082] Furthermore, it is preferable that the contents contain lipids, since this makes the object of the present invention more pronounced. When the contents contain lipids, the lipid content is preferably 95% by mass or less, more preferably 90% by mass or less, and even more preferably 80% by mass or less. When the contents contain lipids, the lipid content may be 50% by mass or more, or 60% by mass or more.
[0083] Examples of the lipid include monoglycerides, diglycerides, triglycerides, free fatty acids (oleic acid), sterols, etc. Among these, triglycerides are more preferred. Triglycerides are preferably the main component of lipids. The lipid may contain one or more types.
[0084] The contents may contain moisture. The amount of moisture is not particularly limited, but is preferably 5% by mass or more, more preferably 10% by mass or more. When the contents contain moisture, the amount may be 80% by mass or less, or 70% by mass or less.
[0085] Examples of contents containing moisture include fats and oils such as butter and margarine, and condiments such as sauces, ketchup, and mayonnaise. These may be liquid, paste, or solid. The contents may be food or beverage products.
[0086] The product of the present invention can maintain its appearance and gas barrier properties for a long period of time even when the contents contain 1% by mass or more of sodium chloride. Furthermore, the same effects can be achieved even when the contents contain lipids.
[0087] The present invention will be explained in more detail below using examples, but the present invention is not limited to these examples in any way.
[0088] [Evaluation method] (1) Appearance after storage test The pouches (15 cm square) obtained in the examples and comparative examples were stored for 200 days under conditions of 43°C and 50% RH using a thermo-hygrostat (a thermo-hygrostat PR-3J manufactured by Espec Corporation). The appearance characteristics of the pouches after 200 days of storage were evaluated according to the following criteria. D was determined to be no inhibition of whitening. Evaluation criteria A: Almost no change in appearance was observed compared to before storage. B: Whitening and discoloration were observed in an area of less than 1 / 4 of the pouch. C: Whitening and discoloration were observed in an area of 1 / 4 or more but less than 1 / 2 of the pouch. D: Whitening and discoloration were observed in 1 / 2 or more of the pouch.
[0089] (2) OTR (Oxygen Transmission Rate) After Storage Test The pouches (15 cm square) obtained in the Examples and Comparative Examples were stored for 200 days under conditions of 43°C and 50% RH using a thermo-hygrostat (a thermo-hygrostat PR-3J manufactured by Espec Corporation). After 200 days of storage, the contents were removed from the inside of the pouch, the pouch was washed with water, and the moisture and the like were wiped off. Then, a 50 cm diameter hole was placed in the center of the pouch. 2The sample was cut into a circular shape with an area of 100 mm and humidity conditioned for one week under conditions of 20°C and 65% RH. Thereafter, the oxygen transmission rate was measured with the outer layer (opposite to the heat seal layer (E)) as the oxygen supply side and the heat seal layer (E) as the carrier gas side. Specifically, the oxygen transmission rate (unit: cc / (m)) was measured using an oxygen transmission amount measuring device ("MOCON OX-TRAN2 / 21" manufactured by Modern Controls) under conditions of a temperature of 20°C, a humidity of 65% RH on the oxygen supply side, a humidity of 65% RH on the carrier gas side, an oxygen pressure of 1 atmosphere, and a carrier gas pressure of 1 atmosphere. 2 The gas barrier properties were evaluated based on the following criteria: A: 0.1 cc / (m³ / day·atm) was measured, and nitrogen gas containing 2% by volume of hydrogen gas was used as the carrier gas. D: It was determined that the deterioration of the gas barrier properties could not be suppressed. Evaluation criteria: A: 0.1 cc / (m³ / day·atm) was measured, and the gas barrier properties were evaluated based on the following ... 2 ・day・atm) or more, 0.5cc / (m 2 ・day・atm) B: 0.5cc / (m 2 ・day・atm) or more, 1cc / (m 2 ・day・atm) C: 1cc / (m 2 ・day・atm) or more, 10cc / (m 2 · day · atm) less than D: 10cc / (m 2 ・day・atm) or more
[0090] (3) Recyclability The multilayer structures obtained in the examples and comparative examples were crushed into pieces of 4 mm square or less. The crushed material was dry-blended with polypropylene resin (PP1) in a mass ratio (crushed material / PP1) of 20 / 80, and a monolayer film with an average thickness of 20 μm was produced by extrusion under the following conditions. A control monolayer film with an average thickness of 20 μm was also produced using only polypropylene resin. Extruder: Toyo Seiki Seisakusho Co., Ltd. Single-screw extruder Screw diameter: 20 mmφ (L / D = 20, compression ratio = 3.5, full-flight type) Extrusion temperature: C1 / C2 / C3 / D = 190 / 230 / 230 / 230°C Take-up roll temperature: 80°C The resulting monolayer film was visually compared with the control monolayer film and evaluated according to the following criteria. D was determined to be poor recyclability. Evaluation criteria: A: The amount of particles was almost the same as that of the control. B: The amount of particles 0.5 mm or less was slightly higher than that of the control. C: The amount of particles 0.5 mm or less was 30% or more higher than that of the control. D: The amount of particles over 0.5 mm was 30% or more higher than that of the control.
[0091] (4) Al(OH) in the inorganic vapor deposition layer (B) 3 The pouches (15 cm square) obtained in the examples and comparative examples were stored for 200 days under conditions of 43 ° C. and 50% RH using a thermo-hygrostat (a thermo-hygrostat "PR-3J" manufactured by Espec Corporation). After 200 days of storage, the contents were removed, washed with water, and then a cross-sectional piece of the pouch was cut out using a Leica ultramicrotome "EM UC7". The mass ratio of aluminum element to oxygen element was measured for the center of the depth direction of the inorganic vapor deposition layer (B) of the cut-out cross-sectional piece using a TEM (Transmission Electron Microscope)-EDS (Energy Dispersive X-ray Spectroscopy) device "EX-24063JGT" manufactured by JEOL Ltd. The molar ratio of aluminum to oxygen (Al / O) was calculated from this mass ratio, and the Al / Al(OH) ratio in the inorganic vapor deposition layer was calculated based on this molar ratio. 3 The molar ratio was calculated.
[0092] [Materials used] EVOH1: EVOH (ethylene content 48 mol%, saponification degree 99.9 mol%, MFR (210°C, 2.16 kg load) 14.8 g / 10 min) PET: PET film ("FE2001" manufactured by Futamura Chemical Co., Ltd., average thickness 12 μm) MAhPE: maleic anhydride modified PE ("Admer (trademark) NF518" manufactured by Mitsui Chemicals, Inc., MFR (190°C, under 2.16 kg load) 2.4 g / 10 min) MAhPP: maleic anhydride modified PP ("Admer (trademark) QF500" manufactured by Mitsui Chemicals, Inc., MFR (230°C, under 2.16 kg load) 3.0 g / 10 min) PP1: PP ("Novatec (trademark) PP" manufactured by Japan Polypropylene Corporation EA7AD", density 0.90 g / cc, MFR (230°C, under a load of 2.16 kg) 1.4 g / 10 min). In the examples, when biaxially stretched, it was designated as BOPP1, and when unstretched, it was designated as CPP1. MDOPE: LDPE (Novatec (trademark) LD LJ400, manufactured by Japan Polypropylene Corporation, density 0.921 g / cc, MFR (190°C, under a load of 2.16 kg) 1.5 g / 10 min). In the examples, when uniaxially stretched in the MD direction, it was designated as MDOPE. BOPP2: Biaxially oriented PP film (Toyobo Co., Ltd., "Pylen™ Film OT P2161", average thickness 20 μm) CPP2: Non-oriented PP film (Tocello Co., Ltd., "RXC-22", average thickness 70 μm) CPP3: Non-oriented PP film (Tocello Co., Ltd., "RXC-22", average thickness 50 μm) CPP4: Non-oriented PP film (average thickness 30 μm) obtained by extruding PP (Japan Polypropylene Corporation, "Novatec™ PP FX4GF", density 0.90 g / cc, MFR (230°C, under a load of 2.16 kg) 5.0 g / 10 min)) using a single-screw extruder (Plastics Technology Research Institute Co., Ltd. GT-32-A) CPP5: PP (Japan Polypropylene Corporation, "Novatec™ PP FX4GF, density 0.90 g / cc, MFR (230°C, under a load of 2.16 kg) 5.0 g / 10 min) was extruded in a single-screw extruder (Plastics Technology Research Institute Co., Ltd. GT-32-A) to produce an unstretched PP film (average thickness 10 μm).
[0093] Example 1 A three-kind, three-layer co-extruded film (EVOH1 / MAhPP / PP1=4.5 μm / 4.5 μm / 180 μm) was produced using EVOH1, PP1, and MAhPP under the following conditions. EVOH extruder: single-screw extruder (Toyo Seiki Co., Ltd., Lab Machine ME-type CO-EXT) EVOH screw: diameter 20 mmφ, L / D 20, full-flight screw EVOH extrusion temperatures: feed section / compression section / metering section / die = 175 / 210 / 220 / 230°C MAhPP extruder: single-screw extruder (Technovel Co., Ltd., SZW20GT-20MG-STD) MAhPP screw: diameter 20 mmφ, L / D 20, full-flight screw MAhPP extrusion temperatures: feed section / compression section / metering section / die = 150 / 200 / 220 / 230°C PP extruder: single-screw extruder (Plastics Technology Research Institute Co., Ltd., GT-32-A) PP screw: diameter 32 mmφ, L / D 28, full-flight screw PP extrusion temperatures: feeding section / compression section / metering section / die = 170 / 220 / 230 / 230°C Die: 300mm wide, 3-type, 3-layer coat hanger die (manufactured by Plastics Engineering Research Institute)
[0094] The obtained coextruded film was stretched 3 times in the longitudinal direction and 3 times in the transverse direction at 160°C using a tenter-type simultaneous biaxial stretching device to obtain a biaxially stretched coextruded film (EVOH1 / MAhPP / BOPP1=0.5 μm / 0.5 μm / 20 μm).
[0095] On the surface of EVOH1 of the obtained biaxially stretched co-extruded film, aluminum was vacuum-deposited using an "EWA-105" manufactured by Japan Vacuum Engineering Co., Ltd., to an average thickness of 50 nm, to produce a vapor-deposited film having an aluminum vapor-deposited layer (Al / EVOH1 / MAhPP / BOPP1=50 nm / 0.5 μm / 0.5 μm / 20 μm). The obtained vapor-deposited film was evaluated according to the method described in the above evaluation method (4). The results are shown in Table 2. Next, a two-component adhesive (Takelac™ A-520 and Takenate™ A-50 manufactured by Mitsui Chemicals, Inc.) was applied to one side of each of the biaxially oriented polypropylene film (BOPP2) and the unoriented polypropylene film (CPP2) so that the average thickness after drying was 2 μm, and then dried to form an adhesive layer (tie). This was then laminated with the resulting vapor-deposited film to produce a multilayer structure (BOPP2 / tie / Al / EVOH1 / MAhPP / BOPP1 / tie / CPP2=20 μm / 2 μm / 50 nm / 0.5 μm / 0.5 μm / 20 μm / 2 μm / 70 μm). The recyclability of the resulting multilayer structure was evaluated according to the method described in Evaluation Method (3) above. The results are shown in Table 2. In the obtained multilayer structure, the total average thickness of the layers containing a polyolefin resin as a main component, which were laminated on the side of the barrier layer (A) opposite to the side on which the inorganic vapor deposition layer (B) was laminated, was 90.5 μm.
[0096] The resulting multilayer structure was cut into two pieces measuring A4 size (210 mm x 297 mm), and the CPP2 sheets were stacked together and heat-sealed along three sides to produce a three-sided bag (package). Next, edible oil, vinegar, eggs, and salt were mixed together to produce mayonnaise. The resulting mayonnaise contained 1.9% by weight of sodium chloride, 75% by weight of lipids, and 15% by weight of water. 50 g of the resulting mayonnaise was poured into the opening of the three-sided bag, and the opening was heat-sealed to produce a pouch (product) filled with the contents. The resulting pouches were evaluated for appearance and OTR (oxygen barrier resistance) after storage testing according to the methods described in Evaluation Methods (1) and (2) above. The results are shown in Table 2.
[0097] [Examples 2 to 4, 12, 14, Comparative Examples 1, 2, 4] Multilayer structures and pouches were produced and evaluated in the same manner as in Example 1, except that the type and average thickness of the inorganic vapor deposition layer (B), the average thickness of the polyolefin (PO) layer (D), the type and average thickness of the heat seal (E), and the layer structure were changed as shown in Table 1. The results are shown in Table 2. Note that in Examples 3 and 14, the evaluation described in the above evaluation method (4) was not performed.
[0098] Example 5 A multilayer structure and a pouch were produced and evaluated in the same manner as in Example 1, except that a uniaxially stretched co-extruded film produced under the following conditions was used instead of the biaxially stretched co-extruded film. The results are shown in Table 2. A three-kind, three-layer co-extruded film (EVOH1 / MAhPE / PE = 10 μm / 10 μm / 100 μm) was produced using EVOH1, PE, and MAhPE under the following conditions. EVOH extruder: single-screw extruder (Toyo Seiki Co., Ltd., Lab Machine ME-type CO-EXT) EVOH screw: diameter 20 mmφ, L / D 20, full-flight screw EVOH extrusion temperatures: feed section / compression section / metering section / die = 175 / 210 / 220 / 230°C MAhPE extruder: single-screw extruder (Technovel Co., Ltd., SZW20GT-20MG-STD) MAhPE screw: diameter 20 mmφ, L / D 20, full-flight screw MAhPP extrusion temperatures: feed section / compression section / metering section / die = 170 / 190 / 210 / 230°C PE extruder: single-screw extruder (Plastics Technology Research Institute Co., Ltd., GT-32-A) PE screw: diameter 32 mmφ, L / D 28, full-flight screw PE extrusion temperatures: feeding section / compression section / metering section / die = 170 / 190 / 210 / 230°C Die: 300mm wide, 3-type, 3-layer coat hanger die (manufactured by Plastics Engineering Research Institute)
[0099] The obtained coextruded film was uniaxially stretched 5 times in the machine direction (MD direction) at 115°C using a uniaxial stretching device to obtain a uniaxially stretched coextruded film (EVOH1 / MAhPE / MDOPE = 2.0 µm / 2.0 µm / 20 µm).
[0100] [Examples 6 and 7] Multilayer structures and pouches were prepared and evaluated in the same manner as in Example 1, except that the ratios of the ingredients were adjusted so that the composition of the mayonnaise used as the contents of the pouches was as shown in Table 2. The results are shown in Table 2.
[0101] Example 8 A multilayer structure and a pouch were prepared and evaluated in the same manner as in Example 1, except that 50 g of 1.9% by mass saline solution was filled in the pouch. The results are shown in Table 1.
[0102] Example 9 A multilayer structure and a pouch were produced and evaluated in the same manner as in Example 1, except that a biaxially stretched EVOH-1 film produced under the following conditions was used instead of the biaxially stretched coextruded film. The results are shown in Table 2. EVOH-1 was melted at 240°C using a single-screw extruder and extruded through a die onto a casting roll. At the same time, air was blown onto the film using an air knife at a speed of 30 m / s, yielding an unstretched film with an average thickness of 120 μm. The unstretched film was contacted with 80°C warm water for 10 seconds, stretched 3.2 times in the longitudinal direction and 3.0 times in the transverse direction at 90°C using a tenter-type simultaneous biaxial stretching apparatus, and further heat-treated for 5 seconds in a tenter set at 170°C to yield a biaxially stretched EVOH-1 film with an average thickness of 12 μm.
[0103] Example 10 A multilayer structure and a pouch were produced and evaluated in the same manner as in Example 1, except that the conditions were changed so that the average thickness of the coextruded film was EVOH1 / MAhPP / PP = 2.0 μm / 2.0 μm / 40 μm, and a vapor-deposited film was produced without stretching, and the unstretched polypropylene sealant film was changed from CPP2 to CPP4. The results are shown in Table 2.
[0104] Example 11 A laminate (BOPP2 / tie / Al / EVOH / MAhPP / BOPP1=20 μm / 2 μm / 50 nm / 0.5 μm / 0.5 μm / 20 μm) was prepared without laminating an unstretched polypropylene film (CPP2) to a vapor-deposited film, and an unstretched polypropylene film (CPP3) was heat-sealed to the surface of BOPP1 of the laminate at 200° C. for 30 seconds to prepare a multilayer structure. A multilayer structure and a pouch were prepared and evaluated in the same manner as in Example 1. The results are shown in Table 2.
[0105] [Example 13] A multilayer structure and a pouch were produced and evaluated in the same manner as in Example 2, except that the conditions were changed so that the average thickness of the co-extruded film was EVOH1 / MAhPP / PP = 0.5 μm / 0.5 μm / 20 μm, and the deposited film was produced without stretching. The results are shown in Table 2.
[0106] [Comparative Example 3] A multilayer structure and a pouch were produced and evaluated in the same manner as in Example 1, except that a biaxially stretched PET film (PET) having an average thickness of 12 μm was used instead of the biaxially stretched coextruded film. The results are shown in Table 2.
[0107] [Reference Example 1] A multilayer structure and a pouch were produced and evaluated in the same manner as in Example 2, except that mayonnaise containing 0.5% by mass of sodium chloride, 75% by mass of lipids, and 15% by mass of water was prepared and used as the mayonnaise content. The results are shown in Table 2.
[0108] [Reference Example 2] A multilayer structure and a pouch were produced and evaluated in the same manner as in Comparative Example 2, except that mayonnaise containing 0.5% by mass of sodium chloride, 75% by mass of lipids, and 15% by mass of water was prepared and used as the mayonnaise content. The results are shown in Table 2.
[0109] [Reference Example 3] A multilayer structure and a pouch were produced and evaluated in the same manner as in Comparative Example 1, except that mayonnaise containing 0.5% by mass of sodium chloride, 75% by mass of lipids, and 15% by mass of water was prepared and used as the mayonnaise content. The results are shown in Table 2.
[0110]
[0111]
[0112] Comparison of Reference Examples 1 and 2 reveals that when the sodium chloride content of the mayonnaise is less than 1% by mass, deterioration in appearance and gas barrier properties does not occur, even when a heat seal layer is included on the side of the barrier layer (A) where the inorganic vapor deposition layer (B) is laminated. Comparison of Reference Examples 1 and 3 reveals that when the sodium chloride content of the mayonnaise is less than 1% by mass, deterioration in appearance and gas barrier properties does not occur, even when the total average thickness of the layers containing a polyolefin resin as a main component laminated on the side of the barrier layer (A) opposite to the side where the inorganic vapor deposition layer (B) is laminated is less than 45 μm. Therefore, it can be seen that the deterioration in appearance and gas barrier properties is a previously unknown problem observed when the sodium chloride content is 1% by mass or more and has a specific layer structure, and that this problem can be solved when the total average thickness of the layers containing a polyolefin resin as a main component laminated on the side of the barrier layer (A) opposite to the side where the inorganic vapor deposition layer (B) is laminated is 45 μm or more, as in Examples 1 to 14.
Claims
1. A product comprising: a packaging body having a multilayer structure; and a content contained in the packaging body, the content having a sodium chloride content of 1 mass % or more, wherein the multilayer structure comprises: a barrier layer (A) containing an ethylene-vinyl alcohol copolymer (a) as a main component; an inorganic vapor deposition layer (B) laminated on the barrier layer (A) and having an average thickness of 7 nm or more and 100 nm or less; and a heat seal layer (E) containing a polyolefin (e) as a main component and being the outermost layer on the side of the barrier layer (A) opposite to the side on which the inorganic vapor deposition layer (B) is laminated, wherein the total average thickness of the layers containing a polyolefin-based resin as a main component laminated on the side of the barrier layer (A) opposite to the side on which the inorganic vapor deposition layer (B) is laminated is 45 μm or more, and the heat seal layer (E) is located on the inner surface side of the packaging body.
2. The article of claim 1, wherein the barrier layer (A) is at least uniaxially oriented.
3. The product according to claim 1 or 2, wherein the average thickness of the barrier layer (A) is from 0.1 μm to 20 μm.
4. The product according to any one of claims 1 to 3, wherein the ratio of the average thickness of the barrier layer (A) to the average thickness of the multilayer structure is 5% or less.
5. The product according to any one of claims 1 to 4, wherein the inorganic vapor deposition layer (B) is composed of aluminum, aluminum oxide or silicon oxide.
6. The product according to any one of claims 1 to 5, wherein the average thickness of the heat seal layer (E) is 20 µm or more and 200 µm or less.
7. The product according to any one of claims 1 to 6, wherein the multilayer structure has an adhesive layer (C) containing an adhesive resin (c) as a main component and a polyolefin layer (D) containing a polyolefin (d) as a main component, and has a layer configuration in which an inorganic vapor deposition layer (B), a barrier layer (A), the adhesive layer (C), the polyolefin layer (D) and a heat seal layer (E) are laminated in this order.
8. The article of claim 7, wherein the barrier layer (A), the adhesive layer (C) and the polyolefin layer (D) are at least uniaxially oriented.
9. The product according to claim 7 or 8, wherein the barrier layer (A), the adhesive layer (C) and the polyolefin layer (D) are coextruded films.
10. The product according to any one of claims 7 to 9, wherein the resins constituting the main components of the polyolefin layer (D) and the heat seal layer (E) are the same type of resin.
11. The product according to any one of claims 1 to 10, wherein the content of sodium chloride is 5% by mass or less.
12. The product of any one of claims 1 to 11, wherein the contents include lipids.
13. The product according to claim 12, wherein the lipid content of the filling is 95% by weight or less.
14. The product according to claim 12 or 13, wherein the lipid comprises primarily triglycerides.
Citation Information
Patent Citations
Multilayer structure and packaging material comprising same
WO2020071513A1
Laminate, packaging material, and packaging container
JP2023048870A
Heat-sealable laminate, layered substrate, laminate for gas barrier intermediate layer, laminate for packaging material, and packaging material
WO2020045629A1
Multilayer structure, and packaging material for retort using same
WO2020184523A1