Heat resistant alloy having nitriding resistance
The heat-resistant alloy with tailored compositions effectively addresses nitriding resistance and creep rupture strength challenges in ammonia gas decomposition processes, ensuring structural integrity and efficiency in high-temperature environments by inhibiting nitrogen diffusion and forming stable austenite phases.
Patent Information
- Application Number
- PCT/JP2024/017217
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2024-05-08
- Filing Date
- 2024-05-09
- Publication Date
- 2024-11-14
AI Technical Summary
High-pressure ammonia gas decomposition processes require a heat-resistant alloy with excellent nitriding resistance and high-temperature creep rupture strength to prevent nitrogen diffusion and maintain structural integrity in cracking tubes, especially in high-temperature environments.
A heat-resistant alloy composition with specific ranges of C, Si, Mn, P, S, Ni, Cr, and optional elements like Nb, Ti, and Mo, which enhances nitriding resistance and high-temperature creep rupture strength, is developed, featuring a high Ni content to inhibit nitrogen diffusion and form stable austenite phases, along with elements that suppress nitride layer growth.
The alloy exhibits excellent nitriding resistance, high-temperature creep rupture strength, and castability, suitable for high-pressure ammonia gas pyrolysis equipment, reducing nitrogen diffusion and extending rupture time under stress, thus optimizing performance in high-temperature applications.
Smart Images

Figure JP2024017217_14112024_PF_FP_ABST
Abstract
Description
Heat-resistant alloy with excellent nitriding resistance
[0001] The present invention relates to a heat-resistant alloy having excellent resistance to nitriding.
[0002] Decarbonization is required to achieve carbon neutrality. Hydrogen gas is attracting attention as a next-generation energy source that does not emit carbon dioxide. However, there are challenges in safely and efficiently storing and transporting hydrogen gas.
[0003] For this reason, hopes are pinned on ammonia. Ammonia is a hydrogen carrier with a high hydrogen density, and is easy to liquefy, transport, and store, allowing for stable imports from overseas. This ammonia can be used as a fuel because it can be burned without being decomposed, but the hydrogen gas obtained by thermal decomposition of ammonia is often used in technologies such as hydrogen power generation turbines, fuel cells, and hydrogen reduction steelmaking. For this reason, producing hydrogen by thermal decomposition of ammonia is extremely useful.
[0004] Patent Document 1 discloses an ammonia gas thermal decomposition device that uses a catalyst. In this ammonia gas thermal decomposition device, ammonia gas that has been preheated to about 300°C to 700°C is introduced into a reactor that contains a catalyst, whereby the ammonia gas is thermally decomposed into hydrogen gas and nitrogen gas.
[0005] Japanese Patent Application Laid-Open No. 2022-109042
[0006] Ammonia gas generates nitrogen atoms during thermal decomposition, which diffuse into the alloy that makes up the cracking tube and nitride the alloy. For this reason, the heat-resistant alloy that makes up the cracking tube must be nitridation-resistant. In general, Al, Cr, Mo, and Ti are elements that easily combine with nitrogen to form nitrides, and the higher the Ni content, the more difficult it is to nitride.
[0007] For example, in nitriding equipment (gas nitriding furnaces) that perform gas nitriding of metals, stainless steels or Ni-based alloys with a high Ni content are used as furnace materials.
[0008] The hydrogen production process by ammonia decomposition is preferably a high-pressure process. This is because it is advantageous for reducing the volume of mass production facilities and for supplying the hydrogen to downstream processes such as power generation. High pressure here means a pressure higher than about 1.0 MPa, and the higher the pressure, the more desirable it is. However, high-pressure operation requires high-temperature creep rupture strength for the cracking tube.
[0009] An object of the present invention is to provide a heat-resistant alloy which is excellent in nitriding resistance and high-temperature creep rupture strength.
[0010] The heat-resistant alloy of the present invention consists of, in mass %, C: 0.2% to 0.6%, Si: more than 0% but not more than 2.5%, Mn: more than 0% but not more than 2.0%, P: 0.03% or less, S: 0.03% or less, Ni: 33.0% to 50.0%, Cr: 24.0% to 50.0%, the balance being Fe and impurities, and optionally Nb: more than 0% but not more than 1.8%, optionally rare earth elements: more than 0% but not more than 0.5%, optionally Ti: more than 0% but not more than 0.5% and / or Zr: more than 0% but not more than 0.5%, optionally W: more than 0% but not more than 2.0% and / or Mo: more than 0% but not more than 0.5%.
[0011] The heat-resistant alloy preferably contains: C: 0.45% to 0.55%, Si: more than 0% and not more than 1.5%, Ni: 33.0% to 50.0%, Cr: 24.0% to 27.0%, and Nb: more than 0% and 1.0%.
[0012] The heat-resistant alloy preferably contains: C: 0.4% to 0.6%, Si: more than 0% and not more than 2.0%, Ni: 40.0% to 50.0%, Cr: 24.0% to 38.0%, and Nb: 0.5% to 1.8%.
[0013] The heat-resistant alloy preferably contains C: 0.2% to 0.5%, Ni: 40.0% to 50.0%, Cr: 30.0% to 50.0%, and optionally Ti: more than 0% to 0.4% or less.
[0014] The creep rupture strength of the heat-resistant alloy is preferably 20 MPa or more at 900°C for 1000 hours.
[0015] The activation energy of nitrogen diffusion in the heat-resistant alloy is preferably 35 kJ / mol or more.
[0016] The heat-resistant alloy is preferably a centrifugally cast product.
[0017] The above heat-resistant alloy is suitable for use in a high-temperature atmosphere of 500°C or higher.
[0018] The cracking tube for the ammonia gas thermal decomposition apparatus of the present invention can be formed from the heat-resistant alloy described above.
[0019] The heat-resistant alloy according to the present invention has excellent nitriding resistance and high-temperature creep rupture strength. Therefore, it is suitable for use as a cracking tube in an ammonia gas thermal cracking apparatus used at high temperatures of 500°C or higher. The cracking tube is particularly suitable for use in an ammonia gas thermal cracking apparatus used in a high-pressure process, and is advantageous for reducing the volume of mass production facilities and supplying the material to downstream processes such as power generation.
[0020] Fig. 1 is a photograph of the cross section of the structure of the test specimen of Comparative Example 1. Fig. 2 is a graph plotting the creep rupture strength and nitride layer thickness of the test specimen of Example 1. Fig. 3 is a graph plotting the creep rupture strength and activation energy of the test specimen of Example 2. Fig. 4 is an EPMA image of the test specimens of Inventive Example 1 and Comparative Example 1.
[0021] Hereinafter, embodiments of the present invention will be described in detail. Unless otherwise specified, "%" means "% by mass."
[0022] The heat-resistant alloy of the present invention, which has excellent nitriding resistance, is used, for example, as a cracking tube for an ammonia gas thermal decomposition apparatus. The cracking tube is heated from the outside to 500 to 1000°C in a non-catalytic environment, with ammonia gas as the raw material flowing through it. 3 → N 2 + 3H 2 The pyrolysis shown in is carried out to produce nitrogen gas and hydrogen gas.
[0023] The heat-resistant alloy of the present invention having excellent nitriding resistance consists, in mass %, of C: 0.2% to 0.6%, Si: more than 0% but not more than 2.5%, Mn: more than 0% but not more than 2.0%, P: 0.03% or less, S: 0.03% or less, Ni: 33.0% to 50.0%, Cr: 24.0% to 50.0%, and the balance being Fe and impurities.
[0024] The reasons for limiting the ingredients are explained below.
[0025] C: 0.2% to 0.6% C improves castability and increases high-temperature creep rupture strength. It also combines with Cr or selected elements such as Ti and Nb to form carbides, which increases high-temperature strength. For this reason, at least 0.2% is included. However, if the content is too high, Cr 7 C 3 Primary carbides of carbon are likely to be widely formed, and secondary carbides are excessively precipitated during heat treatment, resulting in a decrease in ductility and toughness. Therefore, the upper limit is set to 0.6%. The lower limit of the C content is preferably 0.20% or 0.25%, and more preferably 0.30%. The upper limit of the C content is preferably 0.60% or 0.55%, and more preferably 0.50%.
[0026] Si: more than 0% to 2.5% Si is added as a deoxidizer for the molten alloy, to increase the fluidity of the molten alloy, and to improve oxidation resistance. However, excessive addition of Si leads to reduced ductility, reduced high-temperature creep rupture strength, poor surface quality after casting, and reduced weldability. For this reason, the upper limit of the Si content is set to 2.5%. A Si content of 2.0% is preferable, and 1.7% is more preferable.
[0027] Mn: more than 0% to 2.0% Mn acts as a deoxidizer for the molten alloy and fixes S in the molten alloy, improving weldability and ductility. However, excessive addition of Mn reduces high-temperature creep rupture strength and oxidation resistance, so the upper limit is set to 2.0%. It is more preferable that the Mn content be 1.5% or less.
[0028] P: 0.03% or less, S: 0.03% or less P and S are impurities that are inevitably mixed in during melting, and a mixing amount of 0.03% or less is acceptable. The amount of these impurities mixed in is preferably small, and may be zero.
[0029] Ni: 33.0% to 50.0%. Ni is an essential element for excellent nitriding resistance, ensuring cyclic oxidation resistance and metal structure stability, ensuring high-temperature creep strength, and stabilizing austenitization of heat-resistant alloys. Furthermore, when added in combination with Cr or selectively added W, Ti, or Zr, Ni contributes to improving high-temperature strength and oxidation resistance. Ni is also known to contribute to improving nitriding resistance. Ni hardly dissolves nitrogen in Ni, and is expected to inhibit the diffusion of nitrogen in the material. For this reason, Ni should be contained in an amount of at least 33.0%. However, excessive Ni addition saturates its effects and is economically disadvantageous, so its upper limit is set at 50.0%. The lower limit of Ni content is preferably 37.0%, and more preferably 40.0%.
[0030] Cr: 24.0% to 50.0% Cr contributes to improving high-temperature strength and cyclic oxidation resistance. Cr, together with Ni and Fe, also exhibits excellent heat resistance in high-temperature ranges exceeding 1000°C. Cr also bonds with C to form carbides, which has the effect of increasing high-temperature strength. Cr is also expected to pin nitrogen atoms by forming fine nitrides, thereby suppressing the growth of nitride layers due to nitrogen diffusion. Therefore, Cr is contained in an amount of at least 24.0%. However, Cr is an element that easily bonds with N, and Cr carbides (Cr 23 C 6 The C and N in the Cr content are substituted, nitriding the alloy. Since excessive production of Cr carbides and Cr nitrides reduces ductility, a lower Cr content is preferable, with the upper limit being 50.0%. The lower limit of the Cr content is 24.0%, and the upper limit is 50.0%, with 46.0% being preferred and 43.0% being more preferred.
[0031] The balance is Fe and impurities. The impurities include impurities that are inevitably mixed in during melting. Fe is an element that promotes the penetration and diffusion of nitrogen in the material, and the less Fe there is, the better for nitriding resistance. Although it is the balance, Fe is preferably 40.0% or less.
[0032] The heat-resistant alloy having the above-described structure may selectively contain the following elements.
[0033] Nb: more than 0% to 1.8% Nb is an element that easily forms carbides and contributes to improving creep rupture strength and high-temperature tensile strength. Nb also contributes to improving aging ductility. As with Cr, Nb is expected to have the effect of pinning nitrogen atoms by forming nitrides and suppressing the growth of nitride layers due to nitrogen diffusion, thereby improving nitriding resistance. Therefore, it is preferable to selectively include Nb. The lower limit of Nb is preferably 0.3%. However, excessive addition of Nb leads to ductility, so the upper limit is set to 1.8% or less, preferably 1.5% or less.
[0034] Rare Earth Elements (REM): More than 0% but Not More than 0.5% REM refers to 18 elements, consisting of the 15 lanthanide series elements from La to Lu in the periodic table, plus Y, Hf, and Sc. The REM contained in heat-resistant alloys can be primarily Ce, La, and Nd, and these three elements preferably account for approximately 80% or more of the total rare earth elements, more preferably approximately 90% or more. REM are desirably added selectively because they dissolve in the base metal and contribute to improving oxidation resistance. To achieve these effects, when REM are added, it is preferable to add an appropriate amount, with the upper limit set at 0.5%.
[0035] Ti: more than 0% but not more than 0.5% and / or Zr: more than 0% but not more than 0.5%. One or both of Ti and Zr are selectively added to improve oxidation resistance and high-temperature compressive creep strength. Ti is an element that easily forms carbides and also contributes to improving high-temperature tensile strength. Like Cr, Ti is expected to improve nitridation resistance by forming nitrides to pin nitrogen atoms and inhibit the growth of nitride layers due to nitrogen diffusion. Zr also has a denitrification effect. To achieve these effects, Ti and Zr can be selectively added. On the other hand, Ti is also an element that easily bonds with N, which can lead to poor castability due to a decrease in the alloy's fluidity and the risk of machining difficulties. Therefore, if Ti is added, its upper limit is set to 0.5%, preferably 0.3%. Zr reduces hot plastic workability (e.g., bending), so its upper limit is set to 0.5%, preferably 0.4%.
[0036] W: more than 0% but not more than 2.0% and / or Mo: more than 0% but not more than 0.5%. W and Mo are elements that dissolve in the base metal, strengthen the austenite phase of the base metal, and improve creep rupture strength. Either one or both can be selectively added. However, excessive W or Mo content reduces ductility and carburization resistance. Excessive W or Mo content also reduces the oxidation resistance of the base metal, and Mo exerts twice the effect of W equivalently. Therefore, the upper limit for W addition is set to 2.0% and the upper limit for Mo addition is set to 0.5%. A more preferable upper limit for W is 1.8%, and a more preferable upper limit for Mo is 0.4%.
[0037] Ta: 0% to 0.5% Ta forms carbides with C, an inevitable impurity contained in Ni-based alloys, and refines the crystal grains in the Ni-based alloy, thereby improving the high-temperature strength of the Ni-based alloy and can be selectively added to improve corrosion resistance. However, excessive inclusion of Ta can impair the workability of the Ni-based alloy and reduce its strength. Therefore, when Ta is added, the upper limit of its content is set to 0.5%, and 0.3% is more preferable.
[0038] In a specific embodiment, the heat-resistant alloy of the present invention consists of: C: 0.45% to 0.55%, Si: more than 0% but not more than 1.5%, Mn: more than 0% but not more than 2.0%, P: 0.03% or less, S: 0.03% or less, Ni: 33.0% to 50.0%, Cr: 24.0% to 27.0%, Nb: more than 0% but not more than 1.0%, the balance being Fe and impurities, and optionally rare earth elements: more than 0% but not more than 0.5%, optionally Ti: more than 0% but not more than 0.5%, optionally W: more than 0% but not more than 1.0%, and / or Mo: more than 0% but not more than 0.5%.
[0039] In a specific embodiment, the heat-resistant alloy of the present invention consists of: C: 0.4% to 0.6%, Si: more than 0% but not more than 2.0%, Mn: more than 0% but not more than 2.0%, P: 0.03% or less, S: 0.03% or less, Ni: 40.0% to 50.0%, Cr: 24.0% to 38.0%, Nb: 0.5% to 1.8%, the balance being Fe and impurities, and optionally rare earth elements: more than 0% but not more than 0.5%, optionally Ti: more than 0% but not more than 0.5%, optionally W: more than 0% but not more than 1.0%, and / or Mo: more than 0% but not more than 0.5%.
[0040] In a specific embodiment, the heat-resistant alloy of the present invention consists of: C: 0.2% to 0.5%, Si: more than 0% but not more than 2.5%, Mn: more than 0% but not more than 2.0%, P: 0.03% or less, S: 0.03% or less, Ni: 40.0% to 50.0%, Cr: 30.0% to 50.0%, the balance being Fe and impurities, and optionally Nb: more than 0% but not more than 1.8%, optionally rare earth elements: more than 0% but not more than 0.5%, optionally Ti: more than 0% but not more than 0.5%, optionally W: more than 0% but not more than 1.0%, and / or Mo: more than 0% but not more than 0.5%.
[0041] The heat-resistant alloy of the present invention has excellent nitriding resistance. This is because the alloy contains a large amount of Ni, which is difficult to nitride, and forms a stable austenite phase. Furthermore, the alloy does not contain a large amount of elements that easily combine with nitrogen atoms to form nitrogen artifacts. Nitriding resistance can be evaluated, for example, by the thickness of the nitride layer formed on the cast body in the nitriding environment shown in the Examples.
[0042] Furthermore, the heat-resistant alloy of the present invention, containing the above-described elements, has a high activation energy for nitrogen diffusion and excellent resistance to nitriding. This reduces the amount of nitrogen penetrating into the casting in a nitriding environment, preventing the nitrided layer from thickening. The activation energy for nitrogen diffusion is preferably 35 kJ / mol or more, more preferably 38 kJ / mol or more, and even more preferably 40 kJ / mol or more. While a higher activation energy for nitrogen diffusion is preferable, referring to the second example, the upper limit is 100 kJ / mol, preferably 80 kJ / mol.
[0043] The activation energy of nitrogen diffusion was derived as follows: a heat-resistant alloy was exposed to nitriding atmospheres of different temperatures, and the diffusion coefficient D at each temperature was derived according to the parabolic law of diffusion. Next, an Arrhenius plot was created using the reciprocal of the temperature and the natural logarithm of the diffusion coefficient D. The activation energy of the heat-resistant alloy was then derived from the slope of the Arrhenius plot. The diffusion coefficient D was derived by collecting data at multiple points in the temperature range of 600°C to 950°C.
[0044] The heat-resistant alloy of the present invention has excellent creep rupture strength, particularly high-temperature creep rupture strength. This is due to the inclusion of C, Ni, and optionally Nb and Ti. When used as a cracking tube for an ammonia gas thermal decomposition apparatus, the creep rupture strength is preferably such that the rupture time is 1000 hours or more at a test temperature of 900°C and a stress of 20 MPa, more preferably such that the rupture time is 1000 hours or more at a test temperature of 900°C and a stress of 25 MPa, and more preferably such that the rupture time is 1000 hours or more at a test temperature of 900°C and a stress of 30 MPa.
[0045] The heat-resistant alloy of the present invention also has excellent castability. This is due to the optimized content of alloying elements such as Ni and Cr, and the compositional design that takes into account the fluidity of the molten metal. Castings made from the heat-resistant alloy of the present invention can be produced by blending the component elements so that the composition falls within the above-mentioned composition ranges and by casting methods such as centrifugal casting or static casting.
[0046] As described above, the heat-resistant alloy of the present invention has excellent nitriding resistance and high-temperature creep rupture strength, and also has excellent castability, and is therefore suitable for application to cracking tubes in ammonia gas thermal cracking apparatuses used in nitriding environments where high-pressure ammonia gas is supplied in high-temperature atmospheres of, for example, 500°C or higher. In particular, cracking tubes made of the heat-resistant alloy of the present invention are suitable for application to ammonia gas thermal cracking apparatuses used in high-pressure processes, and are advantageous for reducing the volume in mass production facilities and for supplying the material to downstream processes such as power generation applications.
[0047] <<Example 1>> Cracking tubes were produced by centrifugal casting to confirm their castability, each having the alloy composition (unit: mass%, balance: Fe and impurities) of Examples 1 to 3 and Comparative Examples 1 to 3 shown in Table 1. Comparative Example 1 was made of SUS310S, Comparative Example 2 was made of Inconel 625 (registered trademark), and Comparative Example 3 was made of Hastelloy C276 (registered trademark).
[0048]
[0049] Test specimens were cut from each of the resulting cracking tubes and subjected to creep rupture tests and ammonia exposure tests. The details of the tests are given below, and the results are shown in Table 2.
[0050]
[0051] The heat-resistant alloy of the present invention contains slightly more carbon and silicon to optimize castability, and has superior castability compared to the materials listed as comparative examples. For production by centrifugal casting, excellent castability, i.e., good fluidity, is desirable, and the heat-resistant alloy of the present invention is a reasonable choice. Castability was evaluated in Example 2.
[0052] Furthermore, the heat-resistant alloy of the present invention has excellent high-temperature oxidation resistance. Elements that contribute to high-temperature oxidation resistance include Ni and Cr. Ni itself is an element with high high-temperature oxidation resistance. Cr forms a chromium oxide film on the surface, which protects the surface and inhibits oxidation of the material.
[0053] In the heat-resistant alloy of the present invention, Ni and Cr are contained in approximately equal amounts, and therefore, while having excellent high-temperature oxidation resistance, it is also possible to have other properties such as high creep rupture strength.
[0054] <Creep rupture strength test> The creep rupture strength of the test specimens was measured at a temperature of 900°C for 1000 hours in accordance with JIS Z 2271. The results are shown in Table 2. The value for Comparative Example 2 was at 927°C.
[0055] The creep rupture strength is preferably 20 MPa or more, more preferably 25 MPa or more, and even more preferably 30 MPa or more. Referring to Table 2, it can be seen that all of the inventive examples have a creep rupture strength of 30 MPa or more, which is sufficient creep rupture strength. On the other hand, Comparative Examples 1 and 2 had low creep rupture strength. Comparative Example 3 had a creep rupture strength of about 20 MPa.
[0056] Ammonia Exposure Test: The test specimen was placed in a furnace tube placed in an electric furnace, and the atmosphere inside the furnace tube was replaced with nitrogen gas. The furnace tube was then heated to 600°C, and the atmosphere inside the furnace tube was replaced with ammonia gas. The test specimen was exposed to ammonia gas for 100 hours and then removed.
[0057] Each of the removed test pieces was polished in the thickness direction, and the cross section was observed under an optical microscope to measure the thickness of the nitrided layer. The results are shown in Table 2. For reference, a photograph of the cross section of the structure of the test piece of Comparative Example 1 is shown in Figure 1. The part indicated by the reference numeral 10 is the nitrided layer.
[0058] Regarding nitriding, if the thickness of the nitrided layer formed in the ammonia exposure test is 100 μm or less, it can be determined that the nitriding resistance is good. Referring to Table 2, it can be seen that in Invention Examples 1 to 3 and Comparative Examples 2 and 3, the nitrided layer thickness is 100 μm or less, and therefore the nitriding resistance is excellent. On the other hand, in Comparative Example 1, as shown in FIG. 1, the nitrided layer 10 is thicker than 100 μm, and therefore the nitriding resistance is poor. Comparing the Invention Examples, no nitrided layer was observed in Invention Example 3, and the nitriding resistance was very good. While nitrided layers were formed in Invention Examples 1 and 2, Invention Example 2 was thin at 22.1 μm, and Invention Example 1 was also 100 μm or less, so the nitriding resistance was good.
[0059] <Creep rupture strength and nitriding resistance> The creep rupture strength of each test specimen and the thickness of the nitrided layer formed in the ammonia exposure test were plotted on a graph with the creep rupture strength on the vertical axis and the nitrided layer thickness on the horizontal axis, as shown in Figure 2.
[0060] In the graph of Figure 2, creep rupture strength and nitriding resistance improve as you move toward the upper left. Inventive Examples 1 to 3 are located in the upper left of the graph, and it is clear that they are excellent in creep rupture strength and nitriding resistance. In Figure 2, the dotted line indicates the range consisting of a nitride layer thickness of 100 μm or less, at which it can be determined that nitriding resistance is provided, and the more desirable lower limit of creep rupture strength of 30 MPa or more. All of the inventive examples are inside the dotted line, and all of the comparative examples are outside the dotted line.
[0061] <<Second Example>> For the test pieces of Invention Examples 1 to 3 and Comparative Examples 1 and 2 produced in the first example, the activation energy of nitrogen diffusion was derived, and castability and the like were verified.
[0062] <Activation Energy> The method for deriving the activation energy of nitrogen diffusion is as described above. The results are shown in Table 3. It was found that all of Inventive Examples 1 to 3 had high activation energies of nitrogen diffusion. In particular, Inventive Example 3 showed a higher value than Inventive Examples 1 and 2. Similarly, Comparative Example 2 also had a high activation energy of nitrogen diffusion. Table 3 lists the thickness of the nitride layer in Example 1 again, and it can be seen that the higher the activation energy, the thinner the nitride layer.
[0063]
[0064] <Creep Rupture Strength and Activation Energy> Figure 3 is a graph plotting creep rupture strength on the vertical axis and activation energy of nitrogen diffusion on the horizontal axis. The creep rupture strength was measured using the value measured in Example 1 (see Table 3). In the graph of Figure 3, creep rupture strength and nitridation resistance are superior toward the upper right, due to the higher activation energy of nitrogen diffusion. Examples 1 to 3 are located in the upper right of the graph, demonstrating excellent creep rupture strength and nitridation resistance. In Figure 3, dotted lines indicate the ranges where the desirable lower limit of the activation energy of nitrogen diffusion for nitridation resistance is 35 kJ / mol or more, and the more desirable lower limit of creep rupture strength is 30 MPa or more. All of the inventive examples are inside the dotted line, while all of the comparative examples are outside the dotted line.
[0065] <Castability> Castability was evaluated by observing the surface condition of the test piece to determine the flowability of the molten metal. Castability was evaluated in three stages: "○" (good), "△" (fair), and "×" (poor). Referring to Table 3, all of Invention Examples 1 to 3 had good castability. This was due to the addition of slightly larger amounts of carbon and silicon. Comparative Example 2 had a relatively high activation energy, but poor castability.
[0066] <EPMA Analysis> The ammonia exposure test of Example 1 and Comparative Example 1 was performed on the test specimens of Inventive Example 1 and Comparative Example 1, except that the temperature conditions were changed to 850°C. The other conditions were the same as those of Example 1. The nitrogen distribution of the obtained test specimens was measured using an EPMA (electron probe microanalyzer). Figure 4 shows an EPMA image of Inventive Example 1 (a) and an EPMA image of Comparative Example 1 (b). Referring to the figure, it can be seen that the nitride layer 10 is confirmed in both test specimens (the nitride layer 10 and the area below it are the test specimen), but that the nitride layer 10 formed in Inventive Example 1 is sufficiently thinner than that in Comparative Example 1 due to the high activation energy of nitrogen diffusion.
[0067] The above description is for the purpose of explaining the present invention, and should not be construed as limiting the invention described in the claims or narrowing its scope. Furthermore, the configuration of each part of the present invention is not limited to the above embodiment, and various modifications are possible within the technical scope described in the claims.
Claims
1. A heat-resistant alloy with excellent nitriding resistance consisting of, in mass%, C: 0.2% to 0.6%, Si: more than 0% but not exceeding 2.5%, Mn: more than 0% but not exceeding 2.0%, P: 0.03% or less, S: 0.03% or less, Ni: 33.0% to 50.0%, Cr: 24.0% to 50.0%, the balance being Fe and impurities, and optionally containing Nb: more than 0% but not exceeding 1.8%, optionally rare earth elements: more than 0% but not exceeding 0.5%, optionally Ti: more than 0% but not exceeding 0.5% and / or Zr: more than 0% but not exceeding 0.5%, optionally W: more than 0% but not exceeding 2.0%, and / or Mo: more than 0% but not exceeding 0.5%.
2. A heat-resistant alloy with excellent nitriding resistance as described in claim 1, having the following contents: C: 0.45% to 0.55%, Si: over 0% and up to 1.5%, Ni: 33.0% to 50.0%, Cr: 24.0% to 27.0%, and Nb: over 0% and 1.0%.
3. A heat-resistant alloy with excellent nitriding resistance as described in claim 1, having the following composition: C: 0.4% to 0.6%, Si: more than 0% and not more than 2.0%, Ni: 40.0% to 50.0%, Cr: 24.0% to 38.0%, Nb: 0.5% to 1.8%.
4. A heat-resistant alloy with excellent nitriding resistance as set forth in claim 1, comprising: C: 0.2% to 0.5%, Ni: 40.0% to 50.0%, Cr: 30.0% to 50.0%, and optionally Ti: more than 0% and not more than 0.4%.
5. A heat-resistant alloy with excellent nitriding resistance as set forth in any one of claims 1 to 4, having a creep rupture strength of 20 MPa or more at 900°C for 1,000 hours.
6. A heat-resistant alloy with excellent nitriding resistance according to any one of claims 1 to 4, wherein the activation energy of nitrogen diffusion is 35 kJ / mol or more.
7. A heat-resistant alloy having excellent nitriding resistance according to any one of claims 1 to 4, which is a centrifugally cast body.
8. A heat-resistant alloy having excellent nitriding resistance according to any one of claims 1 to 4, which is used in a high-temperature atmosphere of 500°C or higher.
9. A cracking tube for an ammonia gas thermal decomposition apparatus, which is formed from the heat-resistant alloy according to any one of claims 1 to 4.
Citation Information
Patent Citations
Ammonia decomposition apparatus
JP2022109042A
C - - - [mechitsukugatareitoukimo[mechitsukugatareitoukimo][tayousurotsutoraina[tayousurotsutoraina]
JP1975008004A
JP1975008005A
Cr-ni series heat resistant steel
JP1991236448A
Cr-ni heat resistant steel
JP1993239599A