Hydrophilic powder, water-dispersible cosmetic composition, and cosmetic

The hydrophilic powder, with a hydrophobizing agent and polyglycerin fatty acid esters, addresses the low water dispersibility and resistance issues of hydrophobized inorganic powders in cosmetics by creating a balanced coating that enhances both properties, improving the cosmetic's performance and productivity.

WO2024232430A1PCT designated stage expired Publication Date: 2024-11-14TAYCA CORP

Patent Information

Application Number
PCT/JP2024/017417
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-05-10
Filing Date
2024-05-10
Publication Date
2024-11-14

AI Technical Summary

Technical Problem

Inorganic powders used in cosmetics, such as sunscreens, face challenges with low water dispersibility after hydrophobization, leading to reduced water resistance and increased risk of detachment due to moisture, necessitating a balance between dispersibility and water resistance.

Method used

A hydrophilic powder is developed with a hydrophobizing agent and polyglycerin fatty acid esters, applied to inorganic oxides like zinc, titanium, or silicon, creating a coating layer that enhances water dispersibility and resistance, using a combination of hydrophobizing agents like silicone oil and fatty acids, and polyglycerin fatty acid esters with specific polymerization degrees and carbon numbers.

Benefits of technology

The hydrophilic powder improves the cosmetic's water dispersibility and resistance, allowing for better skin adhesion and reduced dust generation during preparation, while maintaining UV shielding ability, thus enhancing the productivity and performance of water-dispersible cosmetic compositions.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JPOXMLDOC01-APPB-T000001
    Figure JPOXMLDOC01-APPB-T000001
  • Figure JPOXMLDOC01-APPB-T000002
    Figure JPOXMLDOC01-APPB-T000002
  • Figure JPOXMLDOC01-APPB-T000003
    Figure JPOXMLDOC01-APPB-T000003
Patent Text Reader

Abstract

The present invention provides: a hydrophilic powder containing a hydrophobizing agent and having good dispersibility in water; a water-dispersible cosmetic composition including said hydrophilic powder and having excellent producibility; and a cosmetic composed of said water-dispersible cosmetic composition. A hydrophilic powder according to the present invention is characterized by comprising a coating layer on the surface of at least one inorganic oxide selected from the group consisting of zinc, titanium, silicon, aluminum, and cerium, said coating layer including: a hydrophobizing agent; and a polyglycerin fatty acid ester having a polyglycerin-derived moiety having a degree of polymerization of 5-10 and a fatty acid-derived moiety having a total carbon number of 8-42. A water-dispersible cosmetic composition according to the present invention is characterized in that said hydrophilic powder and water are added. A cosmetic according to the present invention is characterized in that said water-dispersible cosmetic composition is added.
Need to check novelty before this filing date? Find Prior Art

Description

Hydrophilic powder, water-dispersible cosmetic composition, and cosmetic

[0001] The present invention relates to a hydrophilic powder that contains a hydrophobic treatment agent and has good dispersibility in water, a water-dispersible cosmetic composition that contains the hydrophilic powder and has excellent productivity, and a cosmetic that is composed of the water-dispersible cosmetic composition.

[0002] In cosmetics such as sunscreens, which are prepared by dispersing inorganic powder in water as a medium and are applied to the skin, the inorganic powder is subjected to a hydrophobic treatment (water-repellent treatment) to prevent the inorganic powder, which is an active ingredient, from being detached from the skin by moisture such as sweat (Patent Documents 1 and 2, etc.).

[0003] However, inorganic powders that have been subjected to hydrophobic treatment have extremely low wettability in water, making them difficult to disperse in water, which is a medium for cosmetics. Therefore, a surfactant is usually added to water to improve the dispersibility of the inorganic powder in water.

[0004] On the other hand, there has also been a proposal to coat the surface of a hydrophobized inorganic powder with a hydrophobic treatment agent and a polyether-modified silicone having an HLB (Hydrophile-Lipophile Balance) of 8 or more in order to increase the dispersibility of the hydrophobized inorganic powder in water, suppress the elution of the inorganic powder in water, and improve the washability when used in cosmetics (Patent Document 3).

[0005] JP 2011-136965 A JP 2017-137252 A JP 2016-222589 A

[0006] According to the technology described in Patent Document 3, the dispersibility of a hydrophobized inorganic powder in water can be improved. However, in order to further improve the productivity of cosmetics containing a hydrophobized inorganic powder and water, it is preferable to further improve the dispersibility of the inorganic powder in water. On the other hand, inorganic powders with improved dispersibility in water have excellent affinity with water, so there is a concern that the water resistance of the cosmetics after application to the skin, etc. will decrease. For these reasons, inorganic powders for water-borne cosmetics are required to achieve both water resistance provided by a hydrophobizing agent and dispersibility in water at an even higher level.

[0007] The present invention has been made in view of the above circumstances, and an object of the present invention is to provide a hydrophilic powder that contains a hydrophobic treatment agent and has good dispersibility in water, a water-dispersible cosmetic composition that contains the hydrophilic powder and has excellent productivity, and a cosmetic that is composed of the water-dispersible cosmetic composition.

[0008] The hydrophilic powder of the present invention is characterized by having a coating layer on the surface of at least one inorganic oxide selected from the group consisting of zinc, titanium, silicon, aluminum, and cerium, the coating layer containing a hydrophobizing agent and a polyglycerol fatty acid ester having a moiety derived from polyglycerol having a degree of polymerization of 5 to 10 and a moiety derived from a fatty acid having a total carbon number of 8 to 42.

[0009] The water-dispersible cosmetic composition of the present invention is characterized by comprising the hydrophilic powder of the present invention and water.

[0010] Furthermore, the cosmetic of the present invention is characterized in that it contains the water-dispersible cosmetic composition of the present invention.

[0011] According to the present invention, it is possible to provide a hydrophilic powder that contains a hydrophobic treatment agent and has good dispersibility in water, a water-dispersible cosmetic composition that contains the hydrophilic powder and has excellent productivity, and a cosmetic that is composed of the water-dispersible cosmetic composition.

[0012] <Hydrophilic Powder> The hydrophilic powder of the present invention has a coating layer on the surface of at least one inorganic oxide selected from the group consisting of zinc, titanium, silicon, aluminum, and cerium, which coating layer contains a hydrophobizing agent and a polyglycerol fatty acid ester having a moiety derived from polyglycerol having a degree of polymerization of 5 to 10 and a moiety derived from a fatty acid having a total carbon number of 8 to 42.

[0013] The inorganic oxide constituting the hydrophilic powder is chemically stable and has ultraviolet shielding properties, and functions as an active ingredient in cosmetics to which the hydrophilic powder is applied, for example.

[0014] The hydrophilic powder may contain only one of zinc, titanium, silicon, aluminum, and cerium, or may contain two or more of them. For example, when the cosmetic to which the hydrophilic powder is applied is a sunscreen, it preferably contains titanium or zinc as the inorganic oxide.

[0015] Inorganic oxides with various physical properties can be appropriately selected and used depending on the requirements of the cosmetic in which the hydrophilic powder is used. For example, the average particle size (average primary particle size) is preferably 5 to 1,000 nm from the viewpoint of effectively forming a coating layer on the surface. Furthermore, from the viewpoint of imparting good UV-shielding ability to the cosmetic to which the hydrophilic powder is applied, the average particle size of the inorganic oxide is preferably 5 to 200 nm, and more preferably 10 to 150 nm. The average particle size of the inorganic oxide referred to here is the number-average particle size of the Heywood diameter (diameter equivalent to a circle with a projected area) of 500 or more inorganic oxide particles, obtained by analyzing an image of the inorganic oxide taken with a transmission electron microscope using the image analysis particle size distribution measurement software "Mac-View."

[0016] The inorganic oxide may be surface-treated with hydrated silica, aluminum hydroxide, or the like.

[0017] As the hydrophobic treatment agent constituting the coating layer of the hydrophilic powder, one or more materials selected from the group consisting of silicone oil, fatty acid, and alkylsilane are preferably used.

[0018] Examples of silicone oils include so-called straight silicone oils such as dimethicone (dimethylpolysiloxane), phenyldimethicone (methylphenylpolysiloxane), and hydrogendimethicone (methylhydrogenpolysiloxane); and so-called branched silicone oils such as trimethylsiloxysilicate and triethoxysilylethylpolydimethylsiloxyethylhexyldimethicone.

[0019] Examples of fatty acids include lauric acid, myristic acid, palmitic acid, stearic acid, isostearic acid, oleic acid, and behenic acid.

[0020] Examples of alkylsilanes include alkoxysilanes such as methyltrimethoxysilane, dimethyldimethoxysilane, phenyltrimethoxysilane, methyltriethoxysilane, dimethyldiethoxysilane, phenyltriethoxysilane, n-propyltrimethoxysilane, n-propyltriethoxysilane, hexyltrimethoxysilane, hexyltriethoxysilane, octyltriethoxysilane, and decyltrimethoxysilane; and silazanes such as hexamethyldisilazane.

[0021] Examples of polyglycerol fatty acid esters that constitute the coating layer of the hydrophilic powder and have a polyglycerol-derived moiety with a polymerization degree of 5 to 10 and a fatty acid-derived moiety with a total carbon number of 8 to 42 include polyglyceryl-6 caprylate (HLB: 15), polyglyceryl-10 caprate (HLB: 17), polyglyceryl-10 laurate (HLB: 17), polyglyceryl-10 myristate (HLB: 17), polyglyceryl-5 stearate (HLB: 15), polyglyceryl-10 stearate (HLB: 17), polyglyceryl-5 stearate (HLB: 15), polyglyceryl-10 stearate (HLB: 17), polyglyceryl-6 caprylate (HLB: 15), polyglyceryl-10 caprate (HLB: 17), polyglyceryl-10 laurate (HLB: 17), polyglyceryl-5 myristate (HLB: 15), polyglyceryl-10 stearate (HLB: 17), polyglyceryl-5 stearate (HLB: 15), polyglyceryl-10 stearate (HLB: 17), polyglyceryl-6 caprylate (HLB: 15), polyglyceryl-10 stearate (HLB: 17), polyglyceryl-6 caprate ... monoesters of saturated fatty acids and polyglycerol such as polyglyceryl-5 oleate (HLB: 15) and polyglyceryl-10 oleate (HLB: 15); diesters of saturated fatty acids and polyglycerol such as polyglyceryl-10 distearate (HLB: 11); triesters of saturated fatty acids and polyglycerol such as polyglyceryl-6 trilaurate (HLB: 8); and the like having an HLB of 8 to 17.

[0022] By using a polyglycerol fatty acid ester having a moiety derived from polyglycerol with a degree of polymerization of 5 to 10 and a moiety derived from a fatty acid with a total carbon number of 8 to 42 in the coating layer of a hydrophilic powder, it is possible to further increase the dispersibility of the hydrophilic powder in water (affinity with water) compared to, for example, the use of polyether-modified silicone, and also to further improve the water resistance of a cosmetic containing the hydrophilic powder after application to the skin.

[0023] In recent years, cosmetics that use naturally derived ingredients have become popular, and plant-derived materials are also available as polyglycerol fatty acid esters having a moiety derived from polyglycerol with a degree of polymerization of 5 to 10 and a moiety derived from a fatty acid with a total carbon number of 8 to 42, so this need can be met.

[0024] The coating layer of the hydrophilic powder may contain a hydrophobic treatment agent and a polyglycerol fatty acid ester having a moiety derived from polyglycerol with a degree of polymerization of 5 to 10 and a moiety derived from a fatty acid with a total carbon number of 8 to 42. Preferably, the coating layer has a multilayer structure having a layer (A) containing a hydrophobic treatment agent, formed on the inorganic oxide side, and a layer (B) formed on the outside of the layer (A), containing a polyglycerol fatty acid ester having a moiety derived from polyglycerol with a degree of polymerization of 5 to 10 and a moiety derived from a fatty acid with a total carbon number of 8 to 42.

[0025] A polyglycerol fatty acid ester having a moiety derived from a polyglycerol having a degree of polymerization of 5 to 10 and a moiety derived from a fatty acid having a total carbon number of 8 to 42 has the function of dispersing a powder containing a hydrophobic treatment agent well in water, which is a medium, in cosmetics and cosmetic compositions that serve as a base for cosmetics, while desirably not impairing the water resistance of the powder (the property that makes it difficult for the powder to detach from the skin due to sweat, etc.) after it has been applied to the skin as a cosmetic. The polyglycerol fatty acid ester contained in the coating layer of the hydrophilic powder contributes to improving the water dispersibility of the hydrophilic powder when the hydrophilic powder is dispersed in water in a cosmetic or cosmetic composition. On the other hand, when a cosmetic containing the hydrophilic powder is applied to the skin and the water medium is removed by drying, even if moisture such as sweat adheres thereto, the water resistance provided by the hydrophobic treatment agent contained in the hydrophilic powder is not significantly impaired. However, when the coating layer of the hydrophilic powder has a multilayer structure having the above layer (A) and the above layer (B), the effect of improving water dispersibility provided by the polyglycerol fatty acid ester having a moiety derived from a polyglycerol having a degree of polymerization of 5 to 10 and a moiety derived from a fatty acid having a total carbon number of 8 to 42, and the effect of improving the water resistance of the powder provided by the hydrophobic treatment agent, are more effectively exhibited.

[0026] From the viewpoint of ensuring a satisfactory water resistance improvement effect due to its use, the content of the hydrophobic treatment agent in the hydrophilic powder is preferably 0.5 parts by mass or more, and more preferably 1 part by mass or more, when the amount of inorganic oxide is taken as 100 parts by mass. However, if the amount of the hydrophobic treatment agent in the hydrophilic powder is too large, for example, the amount of inorganic oxide may become too small, and the effect of its use may be reduced. Therefore, the content of the hydrophobic treatment agent in the hydrophilic powder is preferably 30 parts by mass or less, and more preferably 25 parts by mass or less, when the amount of inorganic oxide is taken as 100 parts by mass.

[0027] Furthermore, from the viewpoint of ensuring a favorable water dispersibility-improving effect due to its use, the content of the polyglycerol fatty acid ester having a polyglycerol-derived moiety with a degree of polymerization of 5 to 10 and a fatty acid-derived moiety with a total carbon number of 8 to 42 in the hydrophilic powder is preferably 2 parts by mass or more, more preferably 5 parts by mass or more, per 100 parts by mass of the inorganic oxide. However, if the content of the polyglycerol fatty acid ester having a polyglycerol-derived moiety with a degree of polymerization of 5 to 10 and a fatty acid-derived moiety with a total carbon number of 8 to 42 in the hydrophilic powder is too high, for example, the amount of inorganic oxide or the amount of hydrophobic treatment agent may become too small, potentially reducing the effect of their use. Therefore, the content of the polyglycerol fatty acid ester having a polyglycerol-derived moiety with a degree of polymerization of 5 to 10 and a fatty acid-derived moiety with a total carbon number of 8 to 42 in the hydrophilic powder is preferably 30 parts by mass or less, more preferably 25 parts by mass or less, per 100 parts by mass of the inorganic oxide.

[0028] The hydrophilic powder can be produced by forming a coating layer containing a hydrophobic treatment agent and a polyglycerol fatty acid ester having a moiety derived from a polyglycerol with a degree of polymerization of 5 to 10 and a moiety derived from a fatty acid with a total carbon number of 8 to 42 on the surface of an inorganic oxide. However, it is preferable to produce the hydrophilic powder by a method in which a surface treatment is first performed using a hydrophobic treatment agent to form a layer (A) containing the hydrophobic treatment agent, and then a layer (B) containing a polyglycerol fatty acid ester having a moiety derived from a polyglycerol with a degree of polymerization of 5 to 10 and a moiety derived from a fatty acid with a total carbon number of 8 to 42 is formed.

[0029] Various inorganic oxides that have been surface-treated with a hydrophobic treatment agent (inorganic oxides having a layer (A) containing a hydrophobic treatment agent) are commercially available, and these can be used.

[0030] When forming layer (B) containing a polyglycerol fatty acid ester having a polyglycerol-derived moiety with a degree of polymerization of 5 to 10 and a fatty acid-derived moiety with a total carbon number of 8 to 42 on an inorganic oxide having layer (A), the polyglycerol fatty acid ester is in a liquid, paste, or powder form, and therefore, for example, a method can be employed in which the inorganic oxide having layer (A) and the polyglycerol fatty acid ester are mixed and stirred, dried as necessary, and then crushed as necessary.

[0031] <Water-Dispersible Cosmetic Composition> The water-dispersible cosmetic composition of the present invention is a composition used in cosmetics, and contains the hydrophilic powder of the present invention and water. The hydrophilic powder of the present invention has excellent water dispersibility, and therefore can be dispersed in water quickly during the preparation of the water-dispersible cosmetic composition, thereby suppressing the generation of dust caused by the powder and shortening the time required to prepare the water-dispersible cosmetic composition. In this way, the water-dispersible cosmetic composition of the present invention has good productivity.

[0032] The amount of hydrophilic powder contained in the water-dispersible cosmetic composition can be appropriately set as needed, but is usually 1 to 50% by mass.

[0033] The water-dispersible cosmetic composition can be blended with various components required for the cosmetic to be applied.

[0034] The components to be blended into the water-dispersible cosmetic composition may be any of the various components that are commonly used in cosmetics that use water as a medium. For example, when the water-dispersible cosmetic composition is used as a sunscreen, aqueous thickeners, moisturizers, etc. may be used.

[0035] Examples of aqueous thickeners include those containing at least one group selected from the group consisting of a carboxyl group, a carboxylate group (a salt of a carboxyl group), a sulfonic acid group, and a sulfonate group (a salt of a sulfonic acid group) in the molecule. More specific examples include copolymers (synthetic polymers) such as (sodium acrylate / sodium acryloyldimethyltaurate) copolymer, (hydroxyethyl acrylate / sodium acryloyldimethyltaurate) copolymer, (ammonium acryloyldimethyltaurate / vinylpyrrolidone) copolymer, (dimethylacrylamide / sodium acryloyldimethyltaurate) crosspolymer, (acrylates / C10-30 alkyl acrylate) crosspolymer, and carboxyvinyl polymer; and copolymers (natural polysaccharides) such as xanthan gum and carrageenan. The water-dispersible cosmetic composition may contain only one of the above-exemplified aqueous thickeners, or two or more of them.

[0036] The amount of the aqueous thickener in the water-dispersible cosmetic composition is, for example, preferably 0.1% by mass or more, more preferably 0.5% by mass or more, and preferably 5% by mass or less, more preferably 3% by mass or less.

[0037] Examples of the moisturizing agent include polyhydric alcohols such as ethylene glycol, trimethylene glycol, propylene glycol, butylene glycol, pentylene glycol, diethylene glycol, triethylene glycol, dipropylene glycol, glycerin, and diglycerin.

[0038] The blending amount of the moisturizing agent in the water-dispersible cosmetic composition is, for example, preferably 1% by mass or more, more preferably 5% by mass or more, and preferably 40% by mass or less, more preferably 30% by mass or less.

[0039] The amount of water in the water-dispersible cosmetic composition is usually 20 to 70% by mass.

[0040] The water-dispersible cosmetic composition can be prepared by mixing and dispersing the hydrophilic powder, water, and other necessary ingredients such as a thickener and a moisturizer in a conventional manner.

[0041] <Cosmetics> The cosmetics of the present invention are prepared by blending the water-dispersible cosmetic composition of the present invention. The cosmetics can take the form of an oil-in-water or water-in-oil emulsion cosmetic containing an oily component, or a non-emulsified aqueous cosmetic containing no oily component.

[0042] Cosmetics can contain a required amount of hydrophilic powder depending on the intended use, but the amount of hydrophilic powder is usually 0.1 to 40% by mass.

[0043] Furthermore, the amount of water to be blended as a medium in cosmetics may be determined as required depending on the intended use, but is usually 10 to 80% by mass.

[0044] Furthermore, when a water-based thickener is blended into a cosmetic, such as when the cosmetic is prepared using a water-dispersible cosmetic composition containing a water-based thickener, the amount of the water-based thickener blended is usually 0.1 to 3 mass %.

[0045] Furthermore, when a moisturizing agent is blended into a cosmetic, such as when the cosmetic is prepared using a water-dispersible cosmetic composition containing a moisturizing agent, the amount of moisturizing agent blended is usually 4 to 30% by mass.

[0046] Cosmetics can contain ingredients required depending on the intended use, etc., selected from the various ingredients contained in ordinary cosmetics. Examples of such ingredients include fats and oils, hydrocarbons, higher alcohols, ester oils, waxes, silicones, lower alcohols, surfactants, preservatives, pH adjusters, etc.

[0047] The cosmetic of the present invention can be prepared by mixing and dispersing the water-dispersible cosmetic composition of the present invention and various components (water and the above-exemplified components) used as needed using a conventional method.

[0048] The present invention will be described in detail below based on examples, but the present invention is not limited to these examples.

[0049] (Preparation of Hydrophilic Powder) Example 1 100 g of zinc oxide surface-treated with myristic acid (average primary particle size of zinc oxide: 25 nm, amount of myristic acid: 5.0 parts by mass relative to 100 parts by mass of zinc oxide) and 11 g of polyglyceryl-10 oleate ("Sunsoft Q-17S-C (trade name)" manufactured by Taiyo Kagaku Co., Ltd.) were mixed and stirred for 20 minutes using a bench blender, and then dried at 105°C for 2 hours using a dryer. The dried mixture was pulverized using a pin mill to obtain a hydrophilic powder. The amount of polyglyceryl-10 oleate in the obtained hydrophilic powder was 11.6 parts by mass relative to 100 parts by mass of zinc oxide.

[0050] Example 2 A hydrophilic powder was prepared in the same manner as in Example 1, except that zinc oxide surface-treated with palmitic acid (zinc oxide average primary particle size: 25 nm, amount of palmitic acid: 5.0 parts by mass per 100 parts by mass of zinc oxide) was used instead of zinc oxide surface-treated with myristic acid.

[0051] Example 3 A hydrophilic powder was prepared in the same manner as in Example 1, except that zinc oxide surface-treated with stearic acid (zinc oxide average primary particle size: 25 nm, amount of stearic acid: 5.0 parts by mass per 100 parts by mass of zinc oxide) was used instead of zinc oxide surface-treated with myristic acid.

[0052] Example 4 A hydrophilic powder was prepared in the same manner as in Example 1, except that zinc oxide surface-treated with isostearic acid (zinc oxide average primary particle size: 25 nm, amount of isostearic acid: 5.0 parts by mass per 100 parts by mass of zinc oxide) was used instead of zinc oxide surface-treated with myristic acid.

[0053] Example 5 A hydrophilic powder was prepared in the same manner as in Example 1, except that zinc oxide surface-treated with oleic acid (zinc oxide average primary particle size: 25 nm, amount of oleic acid: 5.0 parts by mass per 100 parts by mass of zinc oxide) was used instead of zinc oxide surface-treated with myristic acid.

[0054] Example 6 A hydrophilic powder was prepared in the same manner as in Example 1, except that zinc oxide surface-treated with behenic acid (zinc oxide average primary particle size: 25 nm, amount of behenic acid: 5.0 parts by mass per 100 parts by mass of zinc oxide) was used instead of zinc oxide surface-treated with myristic acid.

[0055] Example 7 A hydrophilic powder was prepared in the same manner as in Example 1, except that zinc oxide surface-treated with dimethicone (average primary particle size of zinc oxide: 25 nm, amount of dimethicone: 5.0 parts by mass per 100 parts by mass of zinc oxide) was used instead of zinc oxide surface-treated with myristic acid.

[0056] Example 8 A hydrophilic powder was prepared in the same manner as in Example 1, except that zinc oxide surface-treated with hydrogen dimethicone (average primary particle size of zinc oxide: 25 nm, amount of hydrogen dimethicone: 5.0 parts by mass per 100 parts by mass of zinc oxide) was used instead of zinc oxide surface-treated with myristic acid.

[0057] Example 9 A hydrophilic powder was prepared in the same manner as in Example 1, except that zinc oxide surface-treated with triethoxysilylethyl polydimethylsiloxyethylhexyl dimethicone (zinc oxide average primary particle size: 25 nm, amount of triethoxysilylethyl polydimethylsiloxyethylhexyl dimethicone: 6.0 parts by mass per 100 parts by mass of zinc oxide) was used instead of zinc oxide surface-treated with myristic acid. The amount of polyglyceryl-10 oleate in the obtained hydrophilic powder was 11.7 parts by mass per 100 parts by mass of zinc oxide.

[0058] Example 10 A hydrophilic powder was prepared in the same manner as in Example 1, except that zinc oxide surface-treated with octyltriethoxysilane (zinc oxide average primary particle size: 25 nm, amount of octyltriethoxysilane: 8.0 parts by mass per 100 parts by mass of zinc oxide) was used instead of zinc oxide surface-treated with myristic acid. The amount of polyglyceryl-10 oleate in the obtained hydrophilic powder was 11.9 parts by mass per 100 parts by mass of zinc oxide.

[0059] Example 11 A hydrophilic powder was prepared in the same manner as in Example 1, except that 100 g of zinc oxide surface-treated with hydrous silica and then surface-treated with triethoxysilylethyl polydimethylsiloxyethylhexyl dimethicone and hydrogen dimethicone (average primary particle size of zinc oxide: 25 nm, amount of hydrous silica: 20.1 parts by mass per 100 parts by mass of zinc oxide, amount of triethoxysilylethyl polydimethylsiloxyethylhexyl dimethicone: 4.9 parts by mass per 100 parts by mass of zinc oxide, amount of hydrogen dimethicone: 4.9 parts by mass per 100 parts by mass of zinc oxide (total of hydrophobic treatment agents: 9.8 parts by mass per 100 parts by mass of zinc oxide)) was used instead of the zinc oxide surface-treated with myristic acid, and 12 g of polyglyceryl-10 oleate ("Sunsoft Q-17S-C (trade name)" manufactured by Taiyo Kagaku Co., Ltd.) was used. The amount of polyglyceryl-10 oleate in the obtained hydrophilic powder was 15.6 parts by mass per 100 parts by mass of zinc oxide.

[0060] Example 12 A hydrophilic powder was prepared in the same manner as in Example 1, except that 100 g of zinc oxide surface-treated with isostearic acid (average primary particle size of zinc oxide: 15 nm, amount of isostearic acid: 6.1 parts by mass per 100 parts by mass of zinc oxide) and 13.5 g of polyglyceryl-10 oleate ["Sunsoft Q-17S-C (trade name)" manufactured by Taiyo Kagaku Co., Ltd.] were used instead of zinc oxide surface-treated with myristic acid. The amount of polyglyceryl-10 oleate in the obtained hydrophilic powder was 14.3 parts by mass per 100 parts by mass of zinc oxide.

[0061] Example 13 A hydrophilic powder was prepared in the same manner as in Example 1, except that 100 g of zinc oxide surface-treated with isostearic acid (average primary particle size of zinc oxide: 35 nm, amount of isostearic acid: 3.3 parts by mass per 100 parts by mass of zinc oxide) and 7.2 g of polyglyceryl-10 oleate ["Sunsoft Q-17S-C (trade name)" manufactured by Taiyo Kagaku Co., Ltd.] were used instead of zinc oxide surface-treated with myristic acid. The amount of polyglyceryl-10 oleate in the obtained hydrophilic powder was 7.4 parts by mass per 100 parts by mass of zinc oxide.

[0062] Example 14 A hydrophilic powder was prepared in the same manner as in Example 1, except that 100 g of zinc oxide surface-treated with isostearic acid (average primary particle size of zinc oxide: 50 nm, amount of isostearic acid: 1.9 parts by mass per 100 parts by mass of zinc oxide) and 4.3 g of polyglyceryl-10 oleate ["Sunsoft Q-17S-C (trade name)" manufactured by Taiyo Kagaku Co., Ltd.] were used instead of zinc oxide surface-treated with myristic acid. The amount of polyglyceryl-10 oleate in the obtained hydrophilic powder was 4.4 parts by mass per 100 parts by mass of zinc oxide.

[0063] Example 15 A hydrophilic powder was prepared in the same manner as in Example 1, except that 100 g of zinc oxide surface-treated with isostearic acid (average primary particle size of zinc oxide: 90 nm, amount of isostearic acid: 1.0 part by mass per 100 parts by mass of zinc oxide) and 2.2 g of polyglyceryl-10 oleate ["Sunsoft Q-17S-C (trade name)" manufactured by Taiyo Kagaku Co., Ltd.] were used instead of zinc oxide surface-treated with myristic acid. The amount of polyglyceryl-10 oleate in the obtained hydrophilic powder was 2.2 parts by mass per 100 parts by mass of zinc oxide.

[0064] Example 16 A hydrophilic powder was prepared in the same manner as in Example 4, except that polyglyceryl-10 laurate was used instead of polyglyceryl-10 oleate.

[0065] Example 17 A hydrophilic powder was prepared in the same manner as in Example 4, except that polyglyceryl-6 trilaurate was used instead of polyglyceryl-10 oleate.

[0066] Example 18 A hydrophilic powder was prepared in the same manner as in Example 4, except that polyglyceryl-10 myristate was used instead of polyglyceryl-10 oleate.

[0067] Example 19 A hydrophilic powder was prepared in the same manner as in Example 4, except that polyglyceryl-10 stearate was used instead of polyglyceryl-10 oleate.

[0068] Example 20 A hydrophilic powder was prepared in the same manner as in Example 4, except that polyglyceryl-10 distearate was used instead of polyglyceryl-10 oleate.

[0069] Example 21 A hydrophilic powder was prepared in the same manner as in Example 4, except that polyglyceryl-10 caprate was used instead of polyglyceryl-10 oleate.

[0070] Example 22 A hydrophilic powder was prepared in the same manner as in Example 4, except that polyglyceryl-6 caprylate was used instead of polyglyceryl-10 oleate.

[0071] Example 23 A hydrophilic powder was prepared in the same manner as in Example 4, except that polyglyceryl-5 oleate was used instead of polyglyceryl-10 oleate.

[0072] Example 24 A hydrophilic powder was prepared in the same manner as in Example 4, except that polyglyceryl-5 stearate was used instead of polyglyceryl-10 oleate.

[0073] Example 25 100 g of titanium oxide surface-treated with aluminum hydroxide and then surface-treated with stearic acid (titanium oxide average primary particle size: 8 nm, aluminum hydroxide content: 19.9 parts by mass per 100 parts by mass of titanium oxide, stearic acid content: 30 parts by mass per 100 parts by mass of titanium oxide) was mixed with 25 g of the same polyglyceryl-10 oleate used in Example 1, stirred for 20 minutes using a bench blender, and then dried at 105°C for 2 hours using a dryer. The dried product was pulverized using a pin mill to obtain a hydrophilic powder. The amount of polyglyceryl-10 oleate in the obtained hydrophilic powder was 37.5 parts by mass per 100 parts by mass of titanium oxide.

[0074] Example 26 100 g of titanium oxide surface-treated with aluminum hydroxide and then surface-treated with isostearic acid (titanium oxide average primary particle size 10 nm, amount of aluminum hydroxide 24.4 parts by mass per 100 parts by mass of titanium oxide, amount of isostearic acid 14.4 parts by mass per 100 parts by mass of titanium oxide) was mixed with 23 g of the same polyglyceryl-10 oleate used in Example 1, stirred for 20 minutes using a benchtop blender, and then dried for 2 hours at 105°C using a dryer. The dried product was pulverized using a pin mill to obtain a hydrophilic powder. The amount of polyglyceryl-10 oleate in the obtained hydrophilic powder was 31.9 parts by mass per 100 parts by mass of titanium oxide.

[0075] Example 27 100 g of titanium oxide surface-treated with stearic acid (titanium oxide average primary particle size: 20 nm, stearic acid content: 17.6 parts by mass per 100 parts by mass of titanium oxide) was mixed with 17.6 g of the same polyglyceryl-10 oleate used in Example 1, and the mixture was stirred for 20 minutes using a bench blender, followed by drying at 105°C for 2 hours using a dryer. The dried mixture was pulverized using a pin mill to obtain a hydrophilic powder. The amount of polyglyceryl-10 oleate in the obtained hydrophilic powder was 20.7 parts by mass per 100 parts by mass of titanium oxide.

[0076] Example 28 100 g of titanium oxide surface-treated with aluminum hydroxide and then surface-treated with isostearic acid (titanium oxide average primary particle size: 250 nm, amount of aluminum hydroxide: 2.8 parts by mass per 100 parts by mass of titanium oxide, amount of isostearic acid: 4.1 parts by mass per 100 parts by mass of titanium oxide) was mixed with 5 g of the same polyglyceryl-10 oleate used in Example 1, stirred for 20 minutes using a bench blender, and then dried for 2 hours at 105°C using a dryer. The dried product was pulverized using a pin mill to obtain a hydrophilic powder. The amount of polyglyceryl-10 oleate in the obtained hydrophilic powder was 5.3 parts by mass per 100 parts by mass of titanium oxide.

[0077] Comparative Example 1 A powder was prepared in which zinc oxide, which had been surface-treated with isostearic acid, was coated with polyglyceryl-5 trioleate in the same manner as in Example 4, except that polyglyceryl-10 oleate was replaced with polyglyceryl-5 trioleate.

[0078] Comparative Example 2 The same zinc oxide surface-treated with isostearic acid as that used in Example 4 was used as the powder in Comparative Example 2 without further treatment.

[0079] The hydrophilic powders of Examples 1 to 28 and the powders of Comparative Examples 1 and 2 were evaluated for water dispersibility (1) to (5) by the following methods.

[0080] <Water Dispersibility (1)> 12 g of the hydrophilic powder of the Example or the powder of the Comparative Example was placed in a 100 mL polyethylene cup, and 18 g of ion-exchanged water was then added. The appearance of the cup was visually observed and the water dispersibility was evaluated according to the following criteria. Note that the cup containing the powder of Comparative Example 2 was filled with a solution of 16.7 g of ion-exchanged water and 1.3 g of a surfactant (polyglyceryl-10 oleate) dissolved in 16.7 g of ion-exchanged water instead of the ion-exchanged water.

[0081] Evaluation criteria for water dispersibility (1): ◯ (good): ion-exchanged water becomes cloudy. × (poor): ion-exchanged water remains clear.

[0082] <Water Dispersibility (2)> 12 g of the hydrophilic powder of the Example or the powder of the Comparative Example was placed in a 100 mL polyethylene cup, and 18 g of ion-exchanged water was then added. The mixture was stirred using a stirrer, and the state of the mixture was visually observed, and the water dispersibility was evaluated according to the following criteria. Note that the cup containing the powder of Comparative Example 2 was filled with the same solution as used in the evaluation of water dispersibility (1) instead of ion-exchanged water.

[0083] Evaluation criteria for water dispersibility (2): ◯ (good): ion-exchanged water becomes cloudy. × (poor): ion-exchanged water remains clear.

[0084] <Water Dispersibility (3)> 12 g of the hydrophilic powder of the Example or the powder of the Comparative Example was placed in a 100 mL polyethylene cup, and 18 g of ion-exchanged water was then added. The mixture was dispersed using a disper at 3,000 rpm for 5 minutes, and the state of the mixture was visually observed, and the water dispersibility was evaluated according to the following criteria. Note that the cup containing the powder of Comparative Example 2 was filled with the same solution as used in the evaluation of water dispersibility (1) instead of ion-exchanged water.

[0085] Evaluation criteria for water dispersibility (3) ◯ (good): The hydrophilic powder or powder does not float near the water surface. × (poor): The hydrophilic powder or powder floats near the water surface.

[0086] <Water Dispersibility (4)> 12 g of the hydrophilic powder of the Example or the powder of the Comparative Example was placed in a 100 mL polyethylene cup, and 18 g of ion-exchanged water was then added, followed by dispersion using a disperser at 3,000 rpm for 5 minutes. The contents of the cup were then transferred to another cup, and the water dispersibility was evaluated according to the following criteria. Note that the cup containing the powder of Comparative Example 2 was filled with the same solution as used in the evaluation of water dispersibility (1) instead of ion-exchanged water.

[0087] Evaluation criteria for water dispersibility (4): ◯ (good): No hydrophilic powder or powder remains at the bottom of the original polyethylene cup. × (poor): Hydrophilic powder or powder remains at the bottom of the original polyethylene cup.

[0088] <Water Dispersibility (5)> 12 g of the hydrophilic powder of the Example or the powder of the Comparative Example was placed in a 100 mL polyethylene cup, and 18 g of ion-exchanged water was then added. The powder was dispersed using a disper at a rotation speed of 1,400 rpm. The state of the dispersion was visually observed, and the water dispersibility was evaluated according to the following criteria. Note that the cup containing the powder of Comparative Example 2 was filled with the same solution as used in the evaluation of water dispersibility (1) instead of ion-exchanged water.

[0089] Evaluation criteria for water dispersibility (5): ◯ (good): No dust is generated when dispersed with a disperser. × (poor): Dust is generated when dispersed with a disperser.

[0090] The compositions of the hydrophilic powders of the examples and the powders of the comparative examples are shown in Tables 1 to 4, and the evaluation results of the water dispersibility are shown in Tables 5 and 6. In Table 3, a "-" in the "Surface Treatment" column of "Inorganic Oxide" indicates that the inorganic oxide has not been subjected to a surface treatment, and "Al Hydroxide" indicates aluminum hydroxide. In Table 4, a "-" in the "Polyglycerin Fatty Acid Ester" column indicates that a coating layer containing a polyglycerin fatty acid ester is not formed. In Tables 1 to 4, the "content (parts by mass)" is the amount when the inorganic oxide, zinc oxide or titanium oxide, is taken as 100 parts by mass.

[0091]

[0092]

[0093]

[0094]

[0095]

[0096]

[0097] As shown in Tables 1 to 6, the hydrophilic powders of Examples 1 to 28, in which the surface of a specific inorganic oxide was coated with a coating layer containing a hydrophobizing agent and a polyglycerol fatty acid ester having a polyglycerol-derived moiety with a degree of polymerization of 5 to 10 and a fatty acid-derived moiety with a total carbon number of 8 to 42, had better water-dispersibility than the powder of Comparative Example 1, which used a polyglycerol fatty acid ester in which the polyglycerol-derived moiety had a degree of polymerization of 5 and the fatty acid-derived moiety had a total carbon number of 54. Furthermore, the hydrophilic powders of the Examples exhibited better water-dispersibility than the powder of Comparative Example 2, which was constructed without the polyglycerol fatty acid ester having a polyglycerol-derived moiety with a degree of polymerization of 5 to 10 and a fatty acid-derived moiety with a total carbon number of 8 to 42 in the coating layer, when the powder was evaluated by adding a surfactant to water. Therefore, the water-dispersible cosmetic composition prepared using the hydrophilic powders of the Examples can suppress dust generation and can be prepared in a short time, ensuring excellent productivity.

[0098] Comparative Example 3 A hydrophilic powder was prepared in the same manner as in Example 4, except that polyether-modified silicone (PEG-11 methyl ether dimethicone, "KF-6018" manufactured by Shin-Etsu Chemical Co., Ltd.) was used instead of polyglyceryl-10 oleate, and the surface of zinc oxide that had been surface-treated with isostearic acid was coated with polyether-modified silicone. The composition of the hydrophilic powder of Comparative Example 3 is also shown in Table 4.

[0099] The hydrophilic powders of Example 4 and Comparative Example 3 were evaluated for their dispersion speed in water by the following method. 12 g of the hydrophilic powder of Example 4 or 12 g of the hydrophilic powder of Comparative Example 3 was added to 18 g of ion-exchanged water placed in a 100 mL polyethylene cup, and the time until the hydrophilic powder dispersed in the ion-exchanged water and the entire ion-exchanged water became completely cloudy was measured. The results are shown in Table 7.

[0100]

[0101] As shown in Table 7, the hydrophilic powder of Example 4 had a higher dispersion rate in water than the hydrophilic powder of Comparative Example 3, and was superior in dispersibility in water (affinity with water).

[0102] (Preparation of Water-Dispersible Cosmetic Compositions) Examples 29 to 36 and Comparative Examples 4 to 7 The hydrophilic powders of the Examples or the powders of the Comparative Examples, a moisturizer, and water were mixed in the compositions shown in Tables 8 and 9, and dispersed using a disper at a rotation speed of 3000 rpm for 5 minutes to prepare the water-dispersible cosmetic compositions of Examples 29 to 36 and Comparative Examples 4 to 7.

[0103] The water-dispersible cosmetic compositions thus obtained were visually inspected for the presence or absence of aggregates and evaluated according to the following criteria. The results are shown in Tables 8 and 9.

[0104] Evaluation criteria for the presence or absence of aggregates in the water-dispersible cosmetic composition: ◯ (good): no aggregates observed × (poor): aggregates observed

[0105] The numerical values ​​shown in Tables 8 and 9 indicate the blending amount of each component when the entire water-dispersible cosmetic composition is taken as 100% by mass, and the unit "% by mass" has been omitted (the same applies to Table 10 described below).

[0106]

[0107]

[0108] As shown in Table 8, no aggregates were observed in the water-dispersible cosmetic compositions of Examples 29 to 36, which were prepared using the hydrophilic powder of Example 4 or Example 28. As such, the hydrophilic powders of the Examples had good water-dispersibility even when blended with a humectant to prepare water-dispersible cosmetic compositions, and the water-dispersible cosmetic compositions of the Examples had high productivity.

[0109] In contrast, as shown in Table 9, in the compositions of Comparative Examples 4 to 7 prepared using the powder of Comparative Example 1, aggregates were observed.

[0110] Examples 37 to 46 The hydrophilic powders of the Examples, the aqueous thickeners, and water were mixed in the compositions shown in Table 10, and dispersed in the same manner as in Example 29, etc., to prepare water-dispersible cosmetic compositions.

[0111] The aqueous thickeners (1) to (5) in Table 10 are as follows: Aqueous thickener (1): A 1% by mass aqueous solution of carboxyvinyl polymer, pH adjusted to 5 with KOH Aqueous thickener (2): Xanthan gum Aqueous thickener (3): (Acrylates / C10-30 alkyl acrylate) crosspolymer Aqueous thickener (4): (Hydroxyethyl acrylate / Sodium acryloyldimethyltaurate) copolymer Aqueous thickener (5): Carrageenan

[0112] The resulting water-dispersible cosmetic compositions were visually inspected for the presence or absence of aggregates and evaluated according to the same criteria as in Example 28. The results are also shown in Table 10.

[0113]

[0114] As shown in Table 10, no aggregates were observed in the water-dispersible cosmetic compositions of Examples 37 to 46, which were prepared using the hydrophilic powder of Example 4 or Example 28. As such, the hydrophilic powders of the Examples had good water-dispersibility even when blended with an aqueous thickener to prepare water-dispersible cosmetic compositions, and the water-dispersible cosmetic compositions of the Examples had high productivity.

[0115] Comparative Example 8 A water-dispersible cosmetic composition of Comparative Example 8 was prepared in the same manner as in Comparative Example 4, except that the hydrophilic powder of Comparative Example 3 was used. The composition of the water-dispersible cosmetic composition of Comparative Example 8 is also shown in Table 9.

[0116] The water-dispersible cosmetic compositions of Example 29 and Comparative Example 8 were evaluated for water resistance by the following method. Each of the water-dispersible cosmetic compositions was applied to an evaluation plate ("HELIOPLATE (registered trademark) SB6" manufactured by Helioscreen) at a concentration of 1.3 mg / cm 2 The coating was applied in an amount of 100g and dried at room temperature for 10 minutes to prepare a measurement sample, and then the SPF was measured before the water resistance test using an SPF analyzer (UV-2000S manufactured by Labsphere).

[0117] 500 g of ion-exchanged water was weighed into a 500 mL beaker, and each measurement sample after the SPF measurement was immersed in the water while stirring with a stirrer to create a vortex in the center and left to stand for 10 minutes. After 10 minutes, the measurement sample was removed and dried at 25°C for 2 hours. Thereafter, the SPF after the water resistance test was measured using the same SPF analyzer as above.

[0118] Then, for each measurement sample, the rate of change in SPF before and after the water resistance test was calculated based on the following formula: Rate of change in SPF (%) = 100 × (SPF after water resistance test - SPF before water resistance test) ÷ (SPF before water resistance test)

[0119] The smaller the rate of change in SPF determined by the water resistance evaluation, the smaller the decrease in UV blocking ability before and after the water resistance test. This means that the amount of the component of the water-dispersible cosmetic composition (i.e., the hydrophilic powder) applied to the evaluation plate that is released during the water resistance test is small, and the water resistance of the hydrophilic powder is excellent.

[0120] The results are shown in Table 11.

[0121]

[0122] As shown in Table 11, the water-dispersible cosmetic composition of Example 29, which incorporated the hydrophilic powder of Example 4 having a coating layer containing a polyglycerol fatty acid ester having a polyglycerol-derived moiety with a degree of polymerization of 5 to 10 and a fatty acid-derived moiety with a total carbon number of 8 to 42, showed a smaller rate of change in SPF after the water resistance test than the water-dispersible cosmetic composition of Comparative Example 8, which incorporated the hydrophilic powder of Comparative Example 3 having a coating layer containing a polyether-modified silicone. These results demonstrate that the hydrophilic powder of Example 4, which used a polyglycerol fatty acid ester having a polyglycerol-derived moiety with a degree of polymerization of 5 to 10 and a fatty acid-derived moiety with a total carbon number of 8 to 42, exhibited superior water resistance when applied to cosmetics than the hydrophilic powder of Comparative Example 3, which used polyether-modified silicone.

[0123] (Preparation of Cosmetic Preparation) Example 47 The aqueous cosmetic preparation of Example 47 was prepared by mixing the hydrophilic powders of Examples 4 and 27 with the components in the amounts shown in Table 12. The values ​​shown in Table 12 indicate the amount of each component when the entire cosmetic preparation is taken as 100% by mass, and the unit "% by mass" has been omitted (the same applies to Tables 13 and 14 described below).

[0124]

[0125] Example 48 Using the hydrophilic powders of Examples 4 and 27, an aqueous phase and an oil phase were prepared in the amounts shown in Table 13, and then the aqueous phase and the oil phase were mixed together to produce the oil-in-water emulsion cosmetic of Example 48.

[0126]

[0127] Example 49 Using the hydrophilic powders of Examples 4 and 25, an aqueous phase and an oil phase were prepared in the proportions shown in Table 14, and then the aqueous phase and the oil phase were mixed to prepare the water-in-oil emulsion cosmetic of Example 49.

[0128]

[0129] No aggregates were observed in any of the cosmetics of Examples 47 to 49. Thus, even when cosmetics were produced by blending an aqueous phase (water-dispersible cosmetic composition) prepared using the hydrophilic powder of the Examples, they had good water dispersibility and high productivity.

[0130] The present invention can be implemented in other forms without departing from the spirit of the present invention. The embodiments disclosed in this application are merely examples, and the present invention is not limited to these embodiments. The scope of the present invention shall be interpreted in accordance with the appended claims rather than the description in the above specification, and all modifications within the scope of the claims are included in the scope of the claims.

[0131] The cosmetic of the present invention can be applied to various cosmetic preparations that contain inorganic oxide powder, such as sunscreens, foundations, emulsions, skin creams, etc. The hydrophilic powder of the present invention can constitute the water-dispersible cosmetic composition of the present invention, and the water-dispersible cosmetic composition of the present invention can constitute the cosmetic of the present invention.

Claims

1. A hydrophilic powder characterized in that the surface of at least one inorganic oxide selected from the group consisting of zinc, titanium, silicon, aluminum and cerium has a coating layer containing a hydrophobizing agent and a polyglycerol fatty acid ester having a portion derived from polyglycerol having a degree of polymerization of 5 to 10 and a portion derived from a fatty acid having a total carbon number of 8 to 42.

2. The hydrophilic powder according to claim 1, wherein the hydrophobic treatment agent comprises at least one material selected from the group consisting of silicone oil, fatty acid and alkylsilane.

3. The hydrophilic powder according to claim 1 or 2, wherein the coating layer has a multilayer structure having a layer (A) containing a hydrophobizing agent formed on the inorganic oxide side, and a layer (B) containing a polyglycerol fatty acid ester having a portion derived from polyglycerol having a degree of polymerization of 5 to 10 and a portion derived from a fatty acid having a total carbon number of 8 to 42 formed on the outside of the layer (A).

4. A water-dispersible cosmetic composition comprising the hydrophilic powder according to any one of claims 1 to 3 and water.

5. The water-dispersible cosmetic composition according to claim 4, further comprising a water-based thickener.

6. The water-dispersible cosmetic composition according to claim 5, wherein the aqueous thickener contains in its molecule at least one group selected from the group consisting of a carboxyl group, a carboxylate group, a sulfonic acid group and a sulfonate group.

7. The water-dispersible cosmetic composition according to claim 6, wherein the aqueous thickener is at least one copolymer selected from the group consisting of sodium acrylate / sodium acryloyldimethyltaurate copolymer, hydroxyethyl acrylate / sodium acryloyldimethyltaurate copolymer, ammonium acryloyldimethyltaurate / vinylpyrrolidone copolymer, dimethylacrylamide / sodium acryloyldimethyltaurate crosspolymer, acrylates / C10-30 alkyl acrylate crosspolymer, carboxyvinyl polymer, xanthan gum, and carrageenan.

8. The water-dispersible cosmetic composition according to any one of claims 4 to 7, further comprising a moisturizing agent.

9. A cosmetic preparation comprising the water-dispersible cosmetic composition according to any one of claims 4 to 8.

Citation Information

Patent Citations

  • Powder composition for three-dimensional forming, and cake powder cosmetic

    JP2005306844A

  • Surface-treated powder

    JP2018168141A

  • Dispersible powder and cosmetic

    JP2021031396A

Cited By

  • Cosmetic composition

    JP7850337B1