Long-life accumulator bladder and preparation method therefor
Through the combination of nitrile glue with specific ratios and vulcanization treatment, accumulator capsules with excellent mechanical properties and high fatigue life are formed, which solves the problem of short life of the energy storage capsule in the prior art, and realizes the Long life, safe and reliable application in hydraulic systems.
Patent Information
- Application Number
- PCT/CN2023/142201
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-05-12
- Filing Date
- 2023-12-27
- Publication Date
- 2024-11-21
AI Technical Summary
The existing accumulator has a short life span, which is unable to take into account high fatigue life, high mechanical properties and flexural cracking properties, making it difficult to use long life and safely and reliably in hydraulic systems.
Using components such as nitrile glue, carbon black, spray carbon black, plasticizer, zinc oxide, silane coupling agent, anti-aging agent, accelerator and vulcanization accelerator, etc., through specific mixing and vulcanization treatment, it has excellent mechanical properties. and capsule materials with high fatigue life, and ensure processing technology through pressure-retaining vulcanization process.
It realizes the good oil resistance, strength, elasticity and high fatigue life characteristics of the accumulator capsule, has excellent flexural cracking and good processing technology, and extends the service life of the equipment.
Smart Images

Figure CN2023142201_21112024_PF_FP_ABST
Abstract
Description
Long-life accumulator capsule and preparation method thereof Technical Field
[0001] The invention belongs to the technical field of hydraulic energy storage rubber, relates to a long-life accumulator capsule, and also relates to a preparation method of the accumulator capsule. Background Art
[0002] The bladder accumulator primarily consists of an accumulator housing, a bladder, and inlet and outlet valves. It performs multiple functions, including energy storage, pressure stabilization, leak repair, and buffering. It is widely used in hydraulic systems in coal mining, metallurgy, petrochemicals, construction, and other industries, and is a traditional, irreplaceable hydraulic component.
[0003] However, existing accumulator bladder manufacturers have problems such as outdated original formulas, single processing technology, varying raw material quality, and cutting corners in the operation process. As a result, the quality of accumulator bladders is not good enough and cannot take into account the characteristics of high fatigue life, high mechanical properties, flex crack resistance, and processing technology. Therefore, it is difficult to use them in hydraulic systems for a long time, safely and reliably.
[0004] Summary of the Invention
[0005] The purpose of the present invention is to provide a long-life accumulator capsule, which solves the problem of short life of the accumulator bladder in the prior art.
[0006] The technical solution adopted by the present invention is that the long-life accumulator capsule comprises the following components in parts by weight:
[0007] 90-110 parts of nitrile rubber, 40-50 parts of carbon black N330, 10-20 parts of spray carbon black, 20-30 parts of plasticizer dioctyl sebacate (DOS), 2-4 parts of zinc oxide ZnO, 1-2 parts of stearic acid (SA), 1-2 parts of silane coupling agent Si669, 1.4-2.6 parts of antioxidant, 1.4-2.6 parts of accelerator, 0.4-0.6 part of vulcanization accelerator DM, and 0.4-0.6 part of sulfur S; the nitrile rubber is NBR DN401 nitrile rubber with an acrylonitrile content of 18%.
[0008] The antioxidant comprises 1-2 parts of antioxidant 2,2,4-trimethyl-1,2-dihydroquinoline (RD) and 0.4-0.6 parts of antioxidant 2-mercaptobenzimidazole (MB).
[0009] The accelerator comprises 1-2 parts of accelerator N-cyclohexyl-2-benzothiazole sulfenamide (CBS) and 0.4-0.6 parts of accelerator tetramethylthiuram disulfide (TMTD).
[0010] Another object of the present invention is to provide a method for preparing a long-life accumulator capsule.
[0011] Another technical solution adopted by the present invention is a method for preparing a long-life accumulator capsule, comprising the following steps:
[0012] Step 1, according to weight parts, weigh 90-110 parts of nitrile rubber, 40-50 parts of carbon black N330, 10-20 parts of spray carbon black, 20-30 parts of plasticizer dioctyl sebacate (DOS), 2-4 parts of zinc oxide ZnO, 1-2 parts of SA, 1-2 parts of silane coupling agent Si669, 1-2 parts of antioxidant RD, 0.4-0.6 parts of antioxidant MB, 1-2 parts of accelerator CBS, 0.4-0.6 parts of accelerator TMTD, 0.4-0.6 parts of vulcanization accelerator DM, and 0.4-0.6 parts of sulfur S;
[0013] Step 2, first plasticize the nitrile rubber with an open mill and then transfer it to an internal mixer, then add carbon black N330, spray carbon black, SA, zinc oxide ZnO, silane coupling agent Si669, antioxidant RD, antioxidant MB, accelerator CBS, accelerator TMTD, plasticizer dioctyl sebacate (DOS) in sequence, knead for 10 minutes, discharge, and cool to obtain a mixed rubber;
[0014] Step 3, re-refining the rubber mixture on an open mill, adding a vulcanization accelerator DM during the re-refining process to obtain a capsule film;
[0015] Step 4: The capsule film is re-refined in an open mill, processed into a rubber strip, and placed into the inlet of an injection molding machine. The strip is injected through a nozzle until the mold cavity is full. After pressure-maintaining vulcanization, air is blown in and the mold is demoulded to obtain a long-life accumulator capsule.
[0016] The beneficial effects of the present invention are as follows: the long-life accumulator capsule of the present invention uses NBR DN401 with an acrylonitrile content of 18% by mass and a vulcanizing agent S (sulfur), which makes the accumulator capsule have good oil resistance and mechanical properties; the unique chain structure of carbon black and spray carbon black can physically adsorb colloids, effectively reducing the apparent activation energy of the vulcanization reaction in the SA rubber vulcanization system and increasing the network structure parameters of the vulcanized rubber, thereby making the capsule material have good mechanical properties such as strength and elasticity, as well as excellent high fatigue life characteristics; the antioxidant RD, the antioxidant MB, the accelerator CBS, and the accelerator TMTD can give the vulcanized rubber good flex cracking resistance. The preparation method of the long-life accumulator capsule of the present invention is to add reinforcing agents, plasticizers, vulcanizing agents and other processing aids to the raw rubber in sequence, and obtain a rubber strip after plasticating and mixing operations. The rubber strip is melted and injected into the mold cavity by a three-dimensional injection molding machine, and vulcanized under pressure. The interaction of the additives and the vulcanization integral molding make the capsule bulge without tearing during the demolding process, and has good processability. BRIEF DESCRIPTION OF THE DRAWINGS
[0017] FIG1 is a diagram showing the results of test phase 1 in a fatigue life test report of a long-life accumulator capsule of the present invention;
[0018] FIG2 is a diagram showing the results of test phase 2 in the fatigue life test report of the long-life accumulator capsule of the present invention;
[0019] FIG3 is a diagram showing the results of test phase 3 in the fatigue life test report of the long-life accumulator capsule of the present invention. DETAILED DESCRIPTION
[0020] The present invention will be described in detail below with reference to the accompanying drawings and specific embodiments.
[0021] The long-life accumulator capsule comprises the following components in parts by weight:
[0022] 90-110 parts of nitrile rubber, 40-50 parts of carbon black N330, 10-20 parts of spray carbon black, 20-30 parts of plasticizer dioctyl sebacate (DOS), 2-4 parts of zinc oxide ZnO, 1-2 parts of stearic acid (SA), 1-2 parts of silane coupling agent Si669, 1-2 parts of antioxidant 2,2,4-trimethyl-1,2-dihydroquinoline (RD), 0.4-0.6 parts of antioxidant 2-mercaptobenzimidazole (MB), 1-2 parts of accelerator N-cyclohexyl-2-benzothiazole sulfenamide (CBS), 0.4-0.6 parts of accelerator tetramethylthiuram disulfide (TMTD), 0.4-0.6 parts of vulcanization accelerator DM, and 0.4-0.6 parts of sulfur S. The nitrile rubber is a low acrylonitrile content nitrile rubber produced by Japan's ZEON company, and the acrylonitrile content is 18% NBR DN401 nitrile rubber.
[0023] Vulcanization is the process of converting linear macromolecules into a three-dimensional network structure under certain temperature and pressure. The present invention changes the crosslinking density and structure of the rubber by regulating the ratio of the vulcanizer to the accelerator. Through orthogonal experiments, with flex cracking resistance as the goal and comprehensive economic cost, the optimal flex cracking resistance was finally obtained under the conditions of accelerator CBS (1-2 parts), accelerator TMTD (0.4-0.6 parts), and sulfur S (0.4-0.6 parts). The bladder accumulator utilizes the incompressibility of oil and the compressibility of gas to achieve hydraulic pressure accumulation. The bladder is in a long-term cycle of expansion and contraction, which inevitably requires the bladder material to have good high fatigue life characteristics. The present invention adopts carbon black and spray carbon black. The unique chain structure of carbon black and spray carbon black can physically adsorb colloids, effectively reducing the apparent activation energy of the vulcanization reaction in the SA rubber vulcanization system, increasing the network structure parameters of the vulcanized rubber, so that the capsule material has good mechanical properties such as strength and elasticity, as well as excellent high fatigue life characteristics; reinforcing agents, plasticizers, vulcanizing agents and other processing aids are added to the raw rubber in sequence, and after plasticizing and mixing operations, a rubber strip is obtained. The rubber strip is melted and injected into a mold cavity by a three-dimensional injection machine, and pressure-maintained vulcanization is carried out. The auxiliary agents cooperate with each other and the vulcanization is integrated into the molding, so that the capsule does not tear during the air-inflating demoulding process, and has good processing technology.
[0024] A method for preparing a long-life accumulator capsule comprises the following steps.
[0025] Step 1, according to weight parts, weigh 90-110 parts of nitrile rubber, 40-50 parts of carbon black N330, 10-20 parts of spray carbon black, 20-30 parts of plasticizer dioctyl sebacate (DOS), 2-4 parts of zinc oxide ZnO, 1-2 parts of SA, 1-2 parts of silane coupling agent Si669, 1-2 parts of antioxidant RD, 0.4-0.6 parts of antioxidant MB, 1-2 parts of accelerator CBS, 0.4-0.6 parts of accelerator TMTD, 0.4-0.6 parts of vulcanization accelerator DM, and 0.4-0.6 parts of sulfur S;
[0026] Step 2, first use an open mill to plasticize the nitrile rubber and then transfer it to an internal mixer, the temperature in the open mill is 40-60°C, the time is 2-5min, the temperature in the internal mixer is 100-120°C, the time is 1-3min, and then carbon black N330, spray carbon black, SA, zinc oxide ZnO, silane coupling agent Si669, antioxidant RD, antioxidant MB, accelerator CBS, accelerator TMTD, plasticizer dioctyl sebacate (DOS) are added in sequence, kneaded for 10min, discharged, and cooled to obtain a mixed rubber; plasticizer dioctyl sebacate (DOS) is a liquid additive, and other additives such as carbon black, accelerator, antioxidant are solid powder additives. In the process of adding small materials, the principle of "solid first, then liquid" is followed;
[0027] Step 3, refining the rubber mix on an open mill, during which the temperature is 30-50°C, thin-passing is performed 8-18 times, and "triangle packing" is performed 8-18 times. During the refining process, a vulcanization accelerator DM is added to obtain a capsule film;
[0028] Step 4: Re-refining the capsule film through the open mill and processing it into a rubber strip. After the injection molding machine is working stably, the rubber strip is placed into the injection molding machine feed port and injected through the nozzle until the mold cavity is filled. After pressure-maintaining and vulcanization, an appropriate amount of air is blown in to prevent the capsule from tearing. A protective device is placed for demoulding to obtain a long-life accumulator capsule.
[0029] Through the above methods, the long-life accumulator capsule of the present invention uses NBR DN401 with an acrylonitrile content of 18% by mass and a vulcanizing agent S (sulfur), resulting in the accumulator capsule having excellent oil resistance and mechanical properties. The unique chain structure of carbon black and spray carbon black can physically adsorb colloids, effectively reducing the apparent activation energy of the vulcanization reaction in the SA rubber vulcanization system and increasing the network structure parameters of the vulcanized rubber, thereby giving the capsule material good mechanical properties such as strength and elasticity, as well as excellent high fatigue life characteristics. The test report is shown in Figure 1. The antioxidant RD, antioxidant MB, accelerator CBS, and accelerator TMTD can impart good flex cracking resistance to the vulcanized rubber. The preparation method of the long-life accumulator capsule of the present invention sequentially adds processing aids such as a reinforcing agent, a plasticizer, and a vulcanizing agent to the raw rubber. After plasticating and mixing operations, a rubber strip is obtained. The rubber strip is melted and injected into the mold cavity using a three-dimensional injection molding machine and vulcanized under pressure. The interaction of the additives and the integrated vulcanization molding ensure that the capsule bulges and does not tear during the demolding process, thus having good processability.
[0030] Example 1
[0031] Step 1, according to weight parts, weighed 100 parts of NBR DN401 nitrile rubber with an acrylonitrile content of 18%, 40 parts of carbon black N330, 10 parts of spray carbon black, 20 parts of plasticizer dioctyl sebacate (DOS), 3 parts of zinc oxide ZnO, 1.5 parts of SA, 1.5 parts of silane coupling agent Si669, 1.5 parts of antioxidant RD, 0.5 parts of antioxidant MB, 1.5 parts of accelerator CBS, 0.5 parts of accelerator TMTD, 0.5 parts of vulcanization accelerator DM, and 0.5 parts of sulfur S;
[0032] Step 2, first use an open mill to plasticize the nitrile rubber and then transfer it to an internal mixer, the temperature in the open mill is 40°C, the time is 5 minutes, and the temperature in the internal mixer is 100°C, the time is 3 minutes; then add carbon black N330, spray carbon black, SA, zinc oxide ZnO, silane coupling agent Si669, antioxidant RD, antioxidant MB, accelerator CBS, accelerator TMTD, plasticizer dioctyl sebacate (DOS), knead for 10 minutes, discharge, and cool to obtain a mixed rubber; plasticizer dioctyl sebacate (DOS) is a liquid additive, and other additives such as carbon black, accelerator, antioxidant are solid powder additives. In the process of adding small materials, the principle of "solid first, liquid later" is followed;
[0033] Step 3, refining the mixed rubber on an open mill at a temperature of 30°C, thinning it 18 times, and making "triangle bags" 18 times. During the refining process, vulcanization accelerator DM is added to obtain capsule film;
[0034] Step 4: The capsule film is re-refined in an open mill, processed into a rubber strip, and placed into the inlet of an injection molding machine. The strip is injected through a nozzle until the mold cavity is full. After pressure-maintaining vulcanization, air is blown in and the mold is demoulded to obtain a long-life accumulator capsule.
[0035] Example 2
[0036] Step 1, according to weight parts, weighed 100 parts of NBR DN401 nitrile rubber with an acrylonitrile content of 18%, 45 parts of carbon black N330, 10 parts of spray carbon black, 25 parts of plasticizer dioctyl sebacate (DOS), 3 parts of zinc oxide ZnO, 1.5 parts of SA, 1.5 parts of silane coupling agent Si669, 1.5 parts of antioxidant RD, 0.5 parts of antioxidant MB, 1.5 parts of accelerator CBS, 0.5 parts of accelerator TMTD, 0.5 parts of vulcanization accelerator DM, and 0.5 parts of sulfur S;
[0037] Step 2, first use an open mill to plasticize the nitrile rubber and then transfer it to an internal mixer, the temperature in the open mill is 40°C, the time is 4 minutes, and the temperature in the internal mixer is 100°C, the time is 3 minutes; then add carbon black N330, spray carbon black, SA, zinc oxide ZnO, silane coupling agent Si669, antioxidant RD, antioxidant MB, accelerator CBS, accelerator TMTD, plasticizer dioctyl sebacate (DOS), knead for 10 minutes, discharge, and cool to obtain a mixed rubber; plasticizer dioctyl sebacate (DOS) is a liquid additive, and other additives such as carbon black, accelerator, antioxidant are solid powder additives. In the process of adding small materials, the principle of "solid first, liquid later" is followed;
[0038] Step 3, the mixed rubber is re-refined on an open mill at a temperature of 35°C, thinned 15 times, and triangularly packaged 15 times. During the re-refining process, a vulcanization accelerator DM is added to obtain a capsule film;
[0039] Step 4: The capsule film is re-refined in an open mill, processed into a rubber strip, and placed into the inlet of an injection molding machine. The strip is injected through a nozzle until the mold cavity is full. After pressure-maintaining vulcanization, air is blown in and the mold is demoulded to obtain a long-life accumulator capsule.
[0040] Example 3
[0041] Step 1, according to weight parts, weighed 100 parts of NBR DN401 nitrile rubber with an acrylonitrile content of 18%, 45 parts of carbon black N330, 10 parts of spray carbon black, 25 parts of plasticizer dioctyl sebacate (DOS), 3 parts of zinc oxide ZnO, 1.5 parts of SA, 1.5 parts of silane coupling agent Si669, 1.5 parts of antioxidant RD, 0.5 parts of antioxidant MB, 1.5 parts of accelerator CBS, 0.5 parts of accelerator TMTD, 0.5 parts of vulcanization accelerator DM, and 0.5 parts of sulfur S;
[0042] Step 2, first use an open mill to plasticize the nitrile rubber and then transfer it to an internal mixer, the temperature in the open mill is 50°C, the time is 2 minutes, and the temperature in the internal mixer is 110°C, the time is 3 minutes; then add carbon black N330, spray carbon black, SA, zinc oxide ZnO, silane coupling agent Si669, antioxidant RD, antioxidant MB, accelerator CBS, accelerator TMTD, plasticizer dioctyl sebacate (DOS), knead for 10 minutes, discharge, and cool to obtain a mixed rubber; plasticizer dioctyl sebacate (DOS) is a liquid additive, and other additives such as carbon black, accelerator, antioxidant are solid powder additives. In the process of adding small materials, the principle of "solid first, liquid later" is followed;
[0043] Step 3, refining the mixed rubber on an open mill at a temperature of 40°C, thinning it 12 times, and making "triangle bags" 12 times. During the refining process, vulcanization accelerator DM is added to obtain capsule film;
[0044] Step 4: The capsule film is re-refined in an open mill, processed into a rubber strip, and placed into the inlet of an injection molding machine. The strip is injected through a nozzle until the mold cavity is full. After pressure-maintaining vulcanization, air is blown in and the mold is demoulded to obtain a long-life accumulator capsule.
[0045] Example 4
[0046] Step 1, according to weight parts, weighed 100 parts of NBR DN401 nitrile rubber with an acrylonitrile content of 18%, 50 parts of carbon black N330, 15 parts of spray carbon black, 30 parts of plasticizer dioctyl sebacate (DOS), 3 parts of zinc oxide ZnO, 1.5 parts of SA, 1.5 parts of silane coupling agent Si669, 1.5 parts of antioxidant RD, 0.5 parts of antioxidant MB, 1.5 parts of accelerator CBS, 0.5 parts of accelerator TMTD, 0.5 parts of vulcanization accelerator DM, and 0.5 parts of sulfur S;
[0047] Step 2, first use an open mill to plasticize the nitrile rubber and then transfer it to an internal mixer, the temperature in the open mill is 50°C, the time is 3 minutes, and the temperature in the internal mixer is 110°C, the time is 2 minutes; then add carbon black N330, spray carbon black, SA, zinc oxide ZnO, silane coupling agent Si669, antioxidant RD, antioxidant MB, accelerator CBS, accelerator TMTD, plasticizer dioctyl sebacate (DOS), knead for 10 minutes, discharge, and cool to obtain a mixed rubber; plasticizer dioctyl sebacate (DOS) is a liquid additive, and other additives such as carbon black, accelerator, and antioxidant are solid powder additives. In the process of adding small materials, the principle of "solid first, then liquid" is followed;
[0048] Step 3, refining the mixed rubber on an open mill at a temperature of 45°C, thinning it 8 times, and making "triangle bags" 8 times. During the refining process, vulcanization accelerator DM is added to obtain capsule film;
[0049] Step 4: The capsule film is re-refined in an open mill, processed into a rubber strip, and placed into the inlet of an injection molding machine. The strip is injected through a nozzle until the mold cavity is full. After pressure-maintaining vulcanization, air is blown in and the mold is demoulded to obtain a long-life accumulator capsule.
[0050] Example 5
[0051] Step 1, according to weight parts, weighed 100 parts of NBR DN401 nitrile rubber with an acrylonitrile content of 18%, 50 parts of carbon black N330, 20 parts of spray carbon black, 30 parts of plasticizer dioctyl sebacate (DOS), 3 parts of zinc oxide ZnO, 1.5 parts of SA, 1.5 parts of silane coupling agent Si669, 1.5 parts of antioxidant RD, 0.5 parts of antioxidant MB, 1.5 parts of accelerator CBS, 0.5 parts of accelerator TMTD, 0.5 parts of vulcanization accelerator DM, and 0.5 parts of sulfur S;
[0052] Step 2, first use an open mill to plasticize the nitrile rubber and then transfer it to an internal mixer, the temperature in the open mill is 60°C, the time is 2 minutes, and the temperature in the internal mixer is 120°C, the time is 1 minute; then add carbon black N330, spray carbon black, SA, zinc oxide ZnO, silane coupling agent Si669, antioxidant RD, antioxidant MB, accelerator CBS, accelerator TMTD, plasticizer dioctyl sebacate (DOS) in sequence, knead for 10 minutes, discharge, and cool to obtain a mixed rubber; plasticizer dioctyl sebacate (DOS) is a liquid additive, and other additives such as carbon black, accelerator, and antioxidant are solid powder additives. In the process of adding small materials, the principle of "solid first, liquid later" is followed;
[0053] Step 3, refining the mixed rubber on an open mill at a temperature of 50°C, thinning it 8 times, and making "triangle bags" 8 times. During the refining process, vulcanization accelerator DM is added to obtain capsule film;
[0054] Step 4: The capsule film is re-refined in an open mill, processed into a rubber strip, and placed into the inlet of an injection molding machine. The strip is injected through a nozzle until the mold cavity is full. After pressure-maintaining vulcanization, air is blown in and the mold is demoulded to obtain a long-life accumulator capsule.
[0055] The various properties of the accumulator capsule obtained in the above embodiment were tested, and the results are shown in the following table:
[0056] As can be seen from the above table, the accumulator capsule obtained by the present invention has good flex crack resistance, high fatigue life characteristics, good oil resistance and mechanical properties such as strength and elasticity.
Claims
1. Long-life accumulator capsule, characterized in that, The following components are included in parts by weight: 90-110 parts of nitrile rubber, 40-50 parts of carbon black N330, 10-20 parts of spray carbon black, 20-30 parts of plasticizer dioctyl sebacate (DOS), 2-4 parts of zinc oxide ZnO, 1-2 parts of stearic acid (SA), 1-2 parts of silane coupling agent Si669, 1.4-2.6 parts of antioxidant, 1.4-2.6 parts of accelerator, 0.4-0.6 parts of vulcanization accelerator dibenzothiazole disulfide (DM), and 0.4-0.6 parts of sulfur S; the nitrile rubber is NBR DN401 nitrile rubber with an acrylonitrile content of 18%.
2. The long-life accumulator capsule according to claim 1, characterized in that The antioxidant comprises 1-2 parts of antioxidant 2,2,4-trimethyl-1,2-dihydroquinoline (RD) and 0.4-0.6 parts of antioxidant 2-mercaptobenzimidazole (MB).
3. The long-life accumulator capsule according to claim 1, characterized in that: The accelerator comprises 1-2 parts of accelerator N-cyclohexyl-2-benzothiazole sulfenamide (CBS) and 0.4-0.6 parts of accelerator tetramethylthiuram disulfide (TMTD).
4. The method for preparing a long-life accumulator capsule according to claim 1, characterized in that: The following steps are involved: Step 1, according to weight parts, weigh 90-110 parts of nitrile rubber, 40-50 parts of carbon black N330, 10-20 parts of spray carbon black, 20-30 parts of plasticizer DOS, 2-4 parts of zinc oxide ZnO, 1-2 parts of SA, 1-2 parts of silane coupling agent Si669, 1-2 parts of antioxidant RD, 0.4-0.6 parts of antioxidant MB, 1-2 parts of accelerator CBS, 0.4-0.6 parts of accelerator TMTD, 0.4-0.6 parts of vulcanization accelerator DM, and 0.4-0.6 parts of sulfur S; Step 2: First, plasticize the nitrile rubber with an open mill and transfer it to an internal mixer, then add carbon black N330, spray carbon black, SA, zinc oxide ZnO, silane coupling agent Si669, antioxidant RD, antioxidant MB, accelerator CBS, accelerator TMTD, plasticizer dioctyl sebacate (DOS) in sequence, After kneading for 10 minutes, the mixture was discharged and cooled to obtain a rubber mix; Step 3, re-refining the mixed rubber on an open mixing mill, adding a vulcanization accelerator DM during the re-refining process to obtain a capsule film; Step 4: Re-refining the capsule film through an open mill, processing it into a rubber strip, placing it into the inlet of an injection machine, injecting it through a nozzle until the mold cavity is full, and after pressure-maintaining vulcanization, blowing in air, and demolding to obtain a long-life accumulator capsule.
Citation Information
Patent Citations
Low-temperature accumulator capsule and preparation method thereof
CN103205036A
Oil-resistant air tank capsule and preparation method thereof
CN104177674A
Rubber material for rubber bag of hydraulic accumulator
CN107484417A
Hydrogenated butyronitrile capsule for energy accumulator
CN111333932A
Long-life energy accumulator capsule and preparation method thereof
CN116535751A