Semiconductor power module and production method for same
The semiconductor power module employs a silicone resin and cage-type silsesquioxane with a hydrolyzable group-containing organosilicon compound to enhance adhesion and maintain high withstand voltage, addressing the issue of low adhesion and reliability in existing modules.
Patent Information
- Application Number
- PCT/JP2023/018313
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-05-16
- Publication Date
- 2024-11-21
AI Technical Summary
Existing semiconductor power modules face challenges in maintaining high withstand voltage over a long period due to low adhesion of organosilicon polymer-based sealing materials, which can lead to peeling and reduced reliability.
A semiconductor power module using a silicone resin and cage-type silsesquioxane with a hydrolyzable group-containing organosilicon compound, forming covalent bonds to enhance adhesion and reduce the dielectric constant through nano-sized pores, ensuring high withstand voltage and long-term reliability.
The solution effectively improves the adhesion between the semiconductor element and the sealing material, maintaining high withstand voltage and ensuring long-term reliability by reducing the dielectric constant and preventing peeling.
Smart Images

Figure JP2023018313_21112024_PF_FP_ABST
Abstract
Description
Semiconductor power module and manufacturing method thereof
[0001] The present disclosure relates to a high-voltage semiconductor power module in which a semiconductor element is sealed with a sealing material.
[0002] Semiconductor power modules are essential for efficiently controlling electronic devices such as motors, and demand for them has been increasing in recent years. For example, a semiconductor power module contains a semiconductor element and an insulating resin that encapsulates it. It is required to be designed with a high withstand voltage structure to prevent leakage current from occurring between the collector electrode (positive electrode) and the emitter electrode (negative electrode), to which an extremely high voltage is applied, without passing through the normal current path. In recent years, semiconductor power modules have become increasingly high-voltage capable, with products with a withstand voltage of 6.5 kV being used in electric trains and other applications.
[0003] International Publication No. 2005-013361 (Patent Document 1) discloses that a semiconductor element and at least a portion of an electrical connection means for electrically connecting the semiconductor element to an external device can be sealed with an organosilicon polymer containing a first organosilicon polymer having at least one selected from the group consisting of polyphenylsilsesquioxane, polymethylsilsesquioxane, polyethylsilsesquioxane, and polypropylsilsesquioxane, which have a crosslinked structure with siloxane (Si—O—Si bond), and a second organosilicon polymer having at least one selected from the group consisting of polydimethylsiloxane, polydiethylsiloxane, polydiphenylsiloxane, and polymethylphenylsiloxane, which have a linear siloxane linkage structure, thereby enabling high voltage resistance and high heat resistance.
[0004] International Publication No. 2005-013361
[0005] However, the organosilicon polymer contained in the encapsulant described in Patent Document 1 is an organosilicon polymer whose main skeleton has a cross-linked structure with siloxane, and therefore the adhesion of the encapsulant to semiconductor elements, etc. is low, and there is a concern that the encapsulant may peel off, and it may not be possible to maintain a high withstand voltage for a long period of time.
[0006] An object of the present disclosure is to provide a semiconductor power module that can achieve high voltage resistance over a long period of time.
[0007] The present disclosure relates to the following semiconductor power module and a manufacturing method thereof.
[0008] 1. A semiconductor power module comprising: a semiconductor element and an encapsulant; the semiconductor element has a surface in contact with the encapsulant; the semiconductor element has an electrode on at least one of the surfaces in contact with the encapsulant; the encapsulant comprises a first silicone gel containing a silicone resin, a cage-type silsesquioxane, and a first hydrolyzable-group-containing organosilicon compound; the cage-type silsesquioxane has two or more Si—H groups or vinyl groups in one molecule; the cage-type silsesquioxane forms covalent bonds with the silicone resin or the first hydrolyzable-group-containing organosilicon compound at two or more positions in one molecule; the ratio of the cage-type silsesquioxane to the silicone resin is less than 2 wt %; the first hydrolyzable-group-containing organosilicon compound has two or more vinyl groups in one molecule; the first hydrolyzable-group-containing organosilicon compound forms covalent bonds with the silicone resin or the cage-type silsesquioxane at two or more positions in one molecule; and the first hydrolyzable-group-containing organosilicon compound is bonded to an electrode.
[0009] a first hydrolyzable group-containing organosilicon compound having two or more Si-H groups or vinyl groups in one molecule; a second hydrolyzable group-containing organosilicon compound having two or more covalent bonds in one molecule with the silicone resin or the first hydrolyzable group-containing organosilicon compound; a ratio of the cage silsesquioxane to the silicone resin being less than 2% by weight; a second hydrolyzable group-containing organosilicon compound having two or more vinyl groups in one molecule; and a second hydrolyzable group-containing organosilicon compound bonded to an electrode.
[0010] A method for manufacturing a semiconductor power module, comprising: a first mixing step of preparing a first mixed liquid by mixing a silicone resin, a cage silsesquioxane, and a first hydrolyzable group-containing organosilicon compound; an injection step of injecting the first mixed liquid into a semiconductor element portion; and a curing step of curing the first mixed liquid, wherein the cage silsesquioxane has two or more Si-H groups or vinyl groups per molecule, the first hydrolyzable group-containing organosilicon compound has two or more vinyl groups per molecule, and the ratio of the cage silsesquioxane to the silicone resin is less than 2 wt %.
[0011] A method for manufacturing a semiconductor power module, the method comprising: a second mixing step of mixing a silicone resin with a cage silsesquioxane to prepare a second mixed liquid; an application step of applying a second hydrolyzable group-containing organosilicon compound diluted with a solvent onto an electrode surface of a semiconductor element; an injection step of injecting the second mixed liquid into a semiconductor element portion; and a curing step of curing the second mixed liquid, wherein the cage silsesquioxane has two or more Si-H groups or vinyl groups per molecule, the second hydrolyzable group-containing organosilicon compound has two or more vinyl groups per molecule, and the ratio of the cage silsesquioxane to the silicone resin is less than 2% by weight.
[0012] According to the present disclosure, by using less than 2 wt % of a cage silsesquioxane having two or more Si-H groups or vinyl groups per molecule in the silicone gel contained in the encapsulant, and by using a hydrolyzable group-containing organosilicon compound having two or more vinyl groups per molecule, it is possible to achieve both a high withstand voltage due to the low dielectric constant of the encapsulant caused by the nano- (millimeter) sized pores contained in the cage silsesquioxane, and improved adhesion at the interface between the electrodes of the semiconductor element and the encapsulant caused by the hydrolyzable group-containing organosilicon compound having two or more vinyl groups per molecule, and it is possible to achieve a high withstand voltage over a long period of time.
[0013] FIG. 1 is a cross-sectional schematic diagram of a semiconductor power module in embodiment 1. FIG. 2 is a top view of a semiconductor element. FIG. 3 is a cross-sectional schematic diagram of a semiconductor power module in embodiment 2. FIG. 4 is a top view of an interdigital electrode substrate used in the examples. FIG. 5 is a schematic diagram illustrating a method for measuring a discharge start voltage performed in the examples. FIG. 6 is a top view of an evaluation module used in the examples. FIG. 7 is a schematic cross-sectional diagram of the evaluation module used in the examples.
[0014] Embodiment 1. A first embodiment of the present disclosure will be described. The semiconductor power module according to the first embodiment includes a semiconductor element and a sealing material, and the semiconductor element has at least one surface that contacts the sealing material. FIG. 1 is a cross-sectional view of the semiconductor power module according to the first embodiment of the present disclosure. In FIG. 1, the semiconductor power module 100 includes a metal base plate 4, an insulating substrate 3 bonded and disposed on the metal base plate 4, a semiconductor element 5 bonded and disposed on the insulating substrate 3, a plurality of external terminals 2 for electrical connection to the outside, a case 6 attached to the metal base plate 4 so as to surround components such as the external terminals 2, the insulating substrate 3, and the semiconductor element 5, a sealing material 1 filled in the space defined by the metal base plate 4 and the case 6 to seal the components such as the insulating substrate 3 and the semiconductor element 5, and a lid 7 that closes the upper opening of the case 6.
[0015] The insulating substrate 3 is made of ceramic such as silicon nitride, alumina, or aluminum nitride, and has a circuit network (metal pattern) 3a bonded to both sides of the insulating substrate 3.
[0016] The semiconductor element 5 is not particularly limited, and examples thereof include elements such as a MOSFET (Metal Oxide Semiconductor Field Effect Transistor), an IGBT (Insulated Gate Bipolar Transistor), an SBD (Schottky Barrier Diode), and an FWD (Free Wheeling Diode) formed on a Si substrate, a SiC substrate, a GaN substrate, or the like.
[0017] The metal base plate 4 and the insulating substrate 3, and the insulating substrate 3 and the semiconductor element 5 are joined by soldering, metal nanoparticles, metal diffusion, ultrasonic bonding, etc. The semiconductor elements 5 and the semiconductor elements 5 and the circuit network (metal pattern) 3a (made of copper or aluminum) of the insulating substrate 3 are electrically connected by wire bonding, i.e., by wires 8.
[0018] The semiconductor element 5 has an electrode on the surface that contacts the encapsulant 1. The electrode may be disposed so as to contact the encapsulant 1. An electric field relaxation pattern called a guard ring may be formed on the semiconductor element 5. As shown in FIG. 2, the guard ring 10 is composed of a plurality of spaced-apart conductive rings that are formed around the outer periphery of the surface of the semiconductor element 5. The electrode 9 is formed in a region surrounded by the guard ring 10 on the surface of the semiconductor element 5. The number of guard rings 10 is appropriately determined depending on the type of semiconductor element 5. Furthermore, a semiconductive SinSiN film (semi-insulating silicon nitride film) for electric field relaxation is formed between the conductive rings of the guard ring 10 on the surface of the semiconductor element 5 by CVD.
[0019] The encapsulating material 1 includes a first silicone gel (c-1) containing a silicone resin (a), a cage-type silsesquioxane (b1), and a first hydrolyzable group-containing organosilicon compound (b2-1). The first silicone gel (c-1) may be used in part or all of the encapsulating material 1. The first silicone gel (c-1) is preferably used in the entire encapsulating material 1. In the silicone gel (c), the cage-type silsesquioxane (b) forms covalent bonds with the silicone resin (a) or the first hydrolyzable group-containing organosilicon compound (b2-1) at two or more positions within one molecule, and the first hydrolyzable group-containing organosilicon compound (b2-1) forms covalent bonds with the silicone resin (a) or the cage-type silsesquioxane (b1) at two or more positions within one molecule. This prevents poor curing and allows for the provision of a sound encapsulating material. Furthermore, since the first silicone gel (c-1) is highly flexible, the stress acting on the wires 8 is small, and the long-term reliability of wire bonding can be ensured.
[0020] The silicone resin (a) of the sealing material 1 is preferably an addition type silicone. Examples of the silicone resin (a) that can be used include polydimethylsiloxane, polydiethylsiloxane, polydiphenylsiloxane, and polymethylphenylsiloxane.
[0021] The cage oligosilsesquioxane (b1) can be a substance having a three-dimensional ring-closed structure formed by siloxane bonds and having functional groups at each vertex of a cubic silica structure at the center. By including the cage silsesquioxane (b1), the dielectric constant of the encapsulant 1 can be reduced due to the nano-sized pores possessed by the cage silsesquioxane (b1), thereby improving the withstand voltage. The cage silsesquioxane (b1) has two or more Si—H groups or vinyl groups per molecule. The cage silsesquioxane (b1) may have a functional group other than a Si—H group or a vinyl group per molecule. By having two or more Si—H groups or vinyl groups per molecule, the cage silsesquioxane (b1) has polymerizability, thereby reducing the effect of adding the cage silsesquioxane (b1) on structural changes in the silicone gel (c).
[0022] The cage silsesquioxane (b1) may have previously formed a covalent bond with the silicone resin (a) or the first hydrolyzable group-containing organosilicon compound (b2-1), or may be mixed with the silicone resin (a) before the curing reaction of the silicone gel (c) and introduced by forming a covalent bond during the curing reaction of the silicone gel (c).
[0023] Examples of the cage-type silsesquioxane (b1) include 1-(trivinylsiloxy)-3,4,7,9,11,13,15-heptacyclopentylcyclo[9.5.1.1 3,9 .1 5,15 .1 7,13 ]octasiloxane (also called trivinylsiloxy-POSS) and octakis(dimethylsiloxy)octasilsesquioxane.
[0024] From the viewpoint of reactivity, it is desirable that the cage silsesquioxane (b1) is compatible with the silicone resin (a), but it is not necessarily required that they be compatible. Even if they are not compatible, they will form a uniform gel as long as they are uniformly dispersed during the curing reaction of the silicone resin (c).
[0025] The mixing ratio of the cage silsesquioxane (b1) is less than 2% by weight relative to the silicone resin (a). If it is 2% by weight or more, the hardness of the first silicone gel (c-1) increases, and the stress acting on the wire increases, making it impossible to ensure long-term reliability of wire bonding. The mixing ratio of the cage silsesquioxane (b1) is desirably in the range of 0.001 to 1% by weight relative to the silicone resin (a). If it is 0.001% by weight or more, the effects of low dielectric constant and high voltage resistance tend to be easily obtained.
[0026] The first hydrolyzable group-containing organosilicon compound (b2-1) has two or more vinyl groups per molecule. The hydrolyzable group may be, for example, an alkoxy group. Examples of the alkoxy group include a methoxy group, an ethoxy group, a propoxy group, and a butoxy group. The first hydrolyzable group-containing organosilicon compound (b2-1) has two or more vinyl groups per molecule, which makes it polymerizable and reduces the effect of the addition of the first hydrolyzable group-containing organosilicon compound (b2-1) on structural changes in the first silicone gel (c-1). Furthermore, the first hydrolyzable group-containing organosilicon compound (b2-1) can bond to the electrode-bearing surface of the semiconductor element [hereinafter also referred to as the electrode surface (e)] via the hydrolyzable group, thereby improving adhesion between the encapsulant and the semiconductor element, reducing concerns about peeling, and enabling a high withstand voltage to be maintained over the long term.
[0027] Examples of the first hydrolyzable group-containing organosilicon compound (b2-1) include 1,3-divinyl-1,3-dimethyl-1,3-dimethoxydisiloxane.
[0028] The first hydrolyzable group-containing organosilicon compound (b2-1) may have previously formed a covalent bond with the silicone resin (a) or the cage silsesquioxane (b1), or may be mixed with the silicone resin (a) before the curing reaction of the first silicone gel (c-1) and introduced by forming a covalent bond during the curing reaction of the first silicone gel (c-1).
[0029] From the viewpoint of reactivity, the hydrolyzable group-containing organosilicon compound (b2-1) is preferably compatible with the silicone resin, but does not necessarily have to be compatible. Even if it is not compatible, it will form a uniform gel if it is uniformly dispersed during the curing reaction of the silicone resin (b).
[0030] The mixing ratio of the first hydrolyzable group-containing organosilicon compound (b2-1) to the silicone resin (a) is preferably in the range of 0.001 to 1 wt %. If the mixing ratio is less than 0.001 wt %, the effect of improving adhesion to semiconductor elements and the like is poor, and the effect of increasing the withstand voltage tends to be difficult to achieve. If the mixing ratio exceeds 1 wt %, the proportion of the hydrolyzable group-containing organosilicon compound with a low withstand voltage relative to the silicone resin (a) increases, which tends to easily lead to a decrease in withstand voltage.
[0031] The penetration of the first silicone gel (c-1) measured with a quarter cone is preferably in the range of 55 to 75. If it is below 55, the protection effect of the semiconductor element and wire against vibrations and the like is reduced, which leads to reliability. If it is above 75, the stress acting on the wire increases, making it impossible to ensure long-term reliability of wire bonding.
[0032] The method for manufacturing the semiconductor power module 100 can include the following steps: a first mixing step of preparing a first mixed liquid by mixing an addition type silicone resin (a), a cage silsesquioxane (b2), and a first hydrolyzable group-containing organosilicon compound (b2-1); an injection step of injecting the first mixed liquid into a semiconductor element portion; and a curing step of curing the first mixed liquid.
[0033] In the first mixing step, the mixing ratio of the cage silsesquioxane (b1) is less than 2% by weight relative to the silicone resin (a). If it is 2% by weight or more, long-term reliability cannot be ensured. The mixing ratio of the cage silsesquioxane (b1) is preferably in the range of 0.001 to 1% by weight relative to the silicone resin (a). If it is 0.001% by weight or more, the effects of lowering the dielectric constant and increasing the withstand voltage tend to be more easily obtained. Mixing can be performed by a known method.
[0034] In the first mixing step, the mixing ratio of the first hydrolyzable group-containing organosilicon compound (b2-1) to the silicone resin (a) is preferably in the range of 0.001 to 1 wt %. If the mixing ratio is less than 0.001 wt %, the effect of improving adhesion to semiconductor elements and the like is poor, and the effect of increasing the withstand voltage tends to be difficult to achieve. If the mixing ratio exceeds 1 wt %, the proportion of the hydrolyzable group-containing organosilicon compound with a low withstand voltage relative to the silicone resin (a) increases, which tends to easily lead to a decrease in withstand voltage.
[0035] The semiconductor element portion may be a portion where components such as the semiconductor element 5 are surrounded by the metal base plate and the case 6. The first mixed liquid may be cured by heating.
[0036] Second Embodiment A second embodiment of the present disclosure will be described. Explanation of the same configurations and operations as those described in the first embodiment will be omitted, and only differences from the first embodiment will be described below.
[0037] A semiconductor power module according to a second embodiment includes a semiconductor element, a sealing material, and a primer layer. The semiconductor element has at least one surface that contacts the primer layer, and the semiconductor element has an electrode on at least one of the surfaces that contacts the primer layer. Figure 3 is a cross-sectional view of the semiconductor power module according to the second embodiment of the present invention. The semiconductor power module 100 of the second embodiment includes a metal base plate 4, an insulating substrate 3 bonded to and disposed on the metal base plate 4, a semiconductor element 5 bonded to and disposed on the insulating substrate 3, a plurality of external terminals 2 for electrical connection to the outside, a case 6 attached to the metal base plate 4 so as to surround components such as the external terminals 2, the insulating substrate 3, and the semiconductor element 5, a sealing material 1 that fills the space defined by the metal base plate 4 and the case 6 and seals the components such as the insulating substrate 3 and the semiconductor element 5, a lid 7 that closes the upper opening of the case 6, and a primer layer 11 disposed on the electrode surface (e) of the semiconductor element 5. The primer layer 11 may contact the electrodes of the semiconductor element 5.
[0038] The primer layer 11 contains a second hydrolyzable group-containing organosilicon compound (b2-2). The primer layer 11 can be formed by applying a primer liquid prepared by dissolving the second hydrolyzable group-containing organosilicon compound (b2-2) in a volatile solvent using any method, such as spraying or brushing.
[0039] The second hydrolyzable group-containing organosilicon compound (b2-2) has two or more vinyl groups in one molecule. The same description as for the first hydrolyzable group-containing organosilicon compound (b2-1) applies to the second hydrolyzable group-containing organosilicon compound (b2-2).
[0040] The solvent may be any volatile solvent, and examples thereof include acetone, methyl ethyl ketone, toluene, cyclohexane, ethanol, methanol, propanol, and 2-butanone.
[0041] The sealing material 1 is disposed after the solvent in the primer layer 11 has evaporated. The primer layer may be subjected to a heat treatment before disposing the sealing material 1. The heat treatment allows the primer layer to adhere more firmly to the electrode surface (e) of the semiconductor element 5 via the hydrolyzable groups.
[0042] The encapsulant 1 includes a second silicone gel (c-2) containing a silicone resin (a) and a cage silsesquioxane (b1). The second silicone gel (c-2) may be used in part or all of the encapsulant 1. The second silicone gel (c-2) is preferably used in the entire encapsulant 1. The cage silsesquioxane (b1) forms covalent bonds with the silicone resin (a) at two or more positions within one molecule. In the second embodiment, the second silicone gel (c-2) may or may not contain the first hydrolyzable group-containing organosilicon compound (b2-1) described above. When the second silicone gel (c-2) contains the first hydrolyzable group-containing organosilicon compound (b2-1), the first hydrolyzable group-containing organosilicon compound (b2-1) may be the same type as or different from the second hydrolyzable group-containing organosilicon compound (b2-2). The second silicone gel (c-2) is highly flexible, so that the stress acting on the wires 8 is small, and the long-term reliability of the wire bonding can be ensured.
[0043] The primer layer 11 forms covalent bonds with the electrode surface (e) on the semiconductor element surface via the hydrolyzable groups and with the silicone gel (c) via the vinyl groups, thereby significantly improving the adhesion between the second silicone gel (c-2) and the electrode (e) on the semiconductor element surface, reducing the risk of peeling and enabling a high withstand voltage to be maintained over the long term.
[0044] The method for manufacturing the semiconductor power module 100 can include the following steps: a second mixing step of preparing a second mixed liquid by mixing the addition type silicone resin (a) and the cage silsesquioxane (b2); a coating step of coating the electrode surface of the semiconductor element with a second hydrolyzable group-containing organosilicon compound diluted with a solvent; an injection step of injecting the second mixed liquid into the semiconductor element portion; and a curing step of curing the second mixed liquid.
[0045] In the second mixing step, the mixing ratio of the cage silsesquioxane (b2) is desirably in the range of 0.001 to 1 wt % relative to the silicone resin (a). The second mixed liquid may or may not contain the first hydrolyzable group-containing organosilicon compound (b2-1) described above. When the second mixed liquid contains the first hydrolyzable group-containing organosilicon compound (b2-1), the first hydrolyzable group-containing organosilicon compound (b2-1) may be the same type as or different from the second hydrolyzable group-containing organosilicon compound.
[0046] In the coating step, a primer layer 11 can be formed. The second hydrolyzable group-containing organosilicon compound can be diluted so that its concentration in the solvent is approximately 0.001 to 2% by weight. The second hydrolyzable group-containing organosilicon compound diluted with the solvent can be applied to the electrode surface (e) of the semiconductor element 5 by any method, such as spraying or brushing. After the coating step and before the injection step, the solvent may be volatilized and the coating film may then be heat-treated. Heat treatment can make the compound adhere more firmly to the electrode surface (e) of the semiconductor element 5 via the hydrolyzable groups.
[0047] It should be noted that the present invention is not limited to the above-described embodiment, and can be freely modified without departing from the spirit of the present invention.
[0048] As examples of the implementation, the measurement of the penetration depth, the measurement of the discharge inception voltage using a comb electrode, and the performance evaluation of the power module were carried out.
[0049] Examples 1 to 90 and Comparative Examples 127 to 144 (Preparation of Sealant) SE-1885 (product name of Dow Corning Toray Co., Ltd.) was used as the silicone resin. Octakis(dimethylsiloxy)octasilsesquioxane, which has two or more Si—H groups in one molecule, was used as the cage silsesquioxane. 1,3-divinyl-1,3-dimethyl-1,3-dimethoxydisiloxane, which has two or more vinyl groups in one molecule, was used as the hydrolyzable group-containing organosilicon compound.
[0050] 200 g each of SE-1885 solution A and solution B were weighed out so that the mass ratio was 1:1, and mixed by stirring. Next, a cage silsesquioxane and a hydrolyzable group-containing organosilicon compound were added in the combinations shown in Tables 1 to 12, mixed, and degassed under reduced pressure for 2 minutes. The cage silsesquioxane and the hydrolyzable group-containing organosilicon compound were added in proportions of 0.0001 wt %, 0.001 wt %, 0.01 wt %, 0.1 wt %, 1 wt %, and 2 wt %, respectively, relative to SE-1885, to prepare encapsulants.
[0051] (Preparation of Primer Liquid) When performing the primer treatment, a solution of 1% by weight of 1,3-divinyl-1,3-dimethyl-1,3-dimethoxydisiloxane dissolved in acetone was used as the primer liquid.
[0052] (Method for Measuring Penetration and Discharge Inception Voltage) A method for measuring discharge inception voltage using a comb-shaped electrode will now be described. FIG. 4 is a diagram of a comb-shaped electrode substrate 12, which is an evaluation substrate. As shown in FIG. 4, a DBC (Direct Bond Copper) substrate, which is formed by bonding copper to one surface of an insulating substrate 13, is nickel-plated on one surface and then patterned by etching to form a comb-shaped counter electrode pattern 14. The comb-shaped counter electrode pattern 14 has a two-layer structure of nickel and copper. The insulating substrate 13 is a silicon nitride substrate measuring 45.2 mm × 34 mm × 0.635 mm. The comb-shaped counter electrode pattern 14 is a pattern in which pairs of electrode combs are alternately arranged with a 1 mm gap between them.
[0053] When the primer treatment was performed, a primer liquid was impregnated into Bemcot and applied to the interdigitated electrode substrate 12. When the primer treatment was performed, two types of samples were prepared: one that was heat-treated at 100°C for 30 minutes after the primer treatment, and one that was left to volatilize the solvent at 23°C ± 2°C.
[0054] The discharge starting voltage was measured in a state where the interdigital electrode substrate 12 was housed in a case 15 and sealed with a sealing material 1, as shown in FIG.
[0055] A sealing material was poured into the case 15 containing the interdigitated electrode substrate 12, and the case was placed in an oven at 100° C. and heated for 1 hour to harden.
[0056] After curing, the penetration was measured using a quarter cone. The evaluation criteria were as follows: a penetration of 55 to 75 was marked as O, and a penetration of any other range was marked as X. The results are shown in Tables 1 to 5 and 12.
[0057] Next, an AC voltage was applied at a voltage increase rate of 0.5 kV / 30 seconds to the electrode wires 16, 17 drawn out from each electrode lead portion 14a of the comb-shaped counter electrode pattern 14 of the comb-shaped electrode substrate 12, and the discharge inception voltage was measured. As a criterion, the voltage value at which a charge of 10 pc was observed was defined as the partial discharge inception voltage, with 6.5 kV or more being marked as ◯ and less than 6.5 kV being marked as ×. The results are shown in Tables 1 to 5 and 12.
[0058] (Performance Evaluation Method for Power Semiconductor Module) Next, a performance evaluation method for a power semiconductor module will be described. Fig. 6 is a top view showing a state in which semiconductor elements are mounted on a metal base plate of an evaluation module, and Fig. 7 is a cross-sectional view showing a module assembly of the evaluation module.
[0059] A copper plate measuring 190 mm x 140 mm x 3 mm was used as the metal base plate 4. The DBC substrate 18 was made by directly bonding a copper circuit network (metal pattern) 3a to both sides of an insulating substrate 3 made of silicon nitride measuring 51 mm x 30 mm x 1 mm. The semiconductor elements 5 mounted on the DBC substrate 18 were an IGBT 5a and an FWD (Free Wheeling Diode) 5b.
[0060] Then, as shown in Fig. 6, six DBC substrates 18 were mounted on a metal base plate 4, and three IGBTs 5a and three FWDs 5b were mounted on each DBC substrate 18. The DBC substrates 18 were electrically connected to each other by wire bonding. As shown in Fig. 7, a frame-shaped case 6 was attached to the metal base plate 4 so as to surround the DBC substrates 18, thereby producing a module assembly 110. A sealing material was poured into the module assembly 110, which was then placed in an oven at 100°C and heated for one hour to harden.
[0061] After thermal aging at 175°C for 100 hours, the module underwent a vibration test (10-500 Hz / 15 minutes, 10 G, 6 hours). The evaluation module was then evaluated for two criteria: device leakage current at room temperature and partial discharge due to AC. Device leakage current was evaluated by applying a DC voltage of 5200 V to the evaluation module at room temperature and measuring the device leakage current. A measured device leakage current of less than 20 mA was marked with a ◎, a value of 20 mA to 30 mA with a ○, a value of 30 mA or greater with an ×, and a value that rendered the test impossible due to wire breakage or other reasons. Partial discharge was evaluated by increasing the voltage applied to the evaluation module in 0.5 kV steps at 30-second intervals and measuring the discharge charge. A value of ◎ was used when the voltage at which the discharge charge measured 10 pC or greater was 11.5 kV or greater, a value of ○ when the voltage was less than 11.5 kV but 10 kV or greater, a value of × when the voltage was less than 10 kV, and a value that rendered the test impossible due to wire breakage or other reasons. Tables 1 to 5 and 12 show the results of measuring the interfacial insulation resistance using the interdigital electrodes and the performance evaluation of the power module.
[0062] <Comparative Examples 1 to 126> Measurements of penetration and discharge inception voltage and performance evaluations of power semiconductor modules were carried out in the same manner as in Example 1, except that the sealing material in Example 1 was changed to a sealing material prepared as follows, and that when primer treatment was performed, a primer solution prepared as follows was used. The results are shown in Tables 6 to 11.
[0063] (Preparation of Encapsulant) The silicone resin used was SE-1885 (a product name of Toray Dow Corning Co., Ltd.). The cage silsesquioxane used was octaphenyloctasilsesquioxane, which does not have two or more Si—H groups and vinyl groups in one molecule. The hydrolyzable group-containing organosilicon compound used was triethoxyvinylsilane, which does not have two or more vinyl groups in one molecule.
[0064] 200 g each of SE-1885 solution A and solution B were weighed out so that the mass ratio was 1:1, and the mixture was stirred and mixed. Next, a cage silsesquioxane and a hydrolyzable group-containing organosilicon compound were added in the combinations shown in Tables 1 to 12, mixed, and degassed under reduced pressure for 2 minutes. The cage silsesquioxane and the hydrolyzable group-containing organosilicon compound were added in proportions of 0.0001 wt %, 0.001 wt %, 0.01 wt %, 0.1 wt %, 1 wt %, and 2 wt %, respectively, relative to SE-1885, to prepare encapsulants.
[0065] (Preparation of Primer Liquid) When performing the primer treatment, a solution in which 1 wt % of triethoxyvinylsilane was dissolved in acetone was used as the primer liquid.
[0066]
[0067]
[0068]
[0069]
[0070]
[0071]
[0072]
[0073]
[0074]
[0075]
[0076]
[0077]
[0078] First, the results of measuring the penetration and the partial discharge inception voltage using a comb electrode will be described. In a comparison between Examples 1 to 90 and Comparative Examples 127 to 144, when octakis(dimethylsiloxy)octasilsesquioxane, which has two or more Si—H groups per molecule, and 1,3-divinyl 1,3-dimethyl 1,3-dimethoxydisiloxane, which has two or more vinyl groups per molecule, were used, the penetration was in the range of 55 to 75 when the octakis(dimethylsiloxy)octasilsesquioxane was added at a ratio of less than 2 wt %, whereas it exceeded 75 when the octakis(dimethylsiloxy)octasilsesquioxane was added at a ratio of 2 wt %. This is thought to be due to the increased hardness caused by the large addition amount. On the other hand, in Comparative Examples 1 to 126, which used octaphenyloctasilsesquioxane without two or more Si—H groups per molecule and triethoxyvinylsilane without two or more vinyl groups per molecule, the penetration was outside the range. In all cases, this is thought to be due to poor curing.
[0079] Next, the results of measuring the partial discharge inception voltage using a comb-shaped electrode are described. In Examples 1 to 90 and Comparative Examples 127 to 144, which used octakis(dimethylsiloxy)octasilsesquioxane, which has two or more Si—H groups per molecule, and 1,3-divinyl-1,3-dimethyl-1,3-dimethoxydisiloxane, which has two or more vinyl groups per molecule, when the addition ratio of octakis(dimethylsiloxy)octasilsesquioxane and 1,3-divinyl-1,3-dimethyl-1,3-dimethoxydisiloxane was both 0.001 to 1 wt %, the partial discharge inception voltage was 6.5 kV or higher. When either of the addition ratios was less than 0.001 wt %, the effect of lowering the dielectric constant and improving adhesion was somewhat weak, resulting in a decrease in the discharge inception voltage. When the addition ratio of octasilsesquioxane was 2 wt %, the change in the chemical structure of the sealing material was significant, resulting in a decrease in the discharge inception voltage.
[0080] On the other hand, in Comparative Examples 1 to 126, which used octaphenyloctasilsesquioxane having no more than two Si—H groups in one molecule and triethoxyvinylsilane having no more than two vinyl groups in one molecule, the discharge inception voltage was less than 6.5 kV. In both cases, this is thought to be due to poor curing.
[0081] Next, the results of evaluating the performance of power semiconductor modules are described. In Examples 1 to 90 and Comparative Examples 127 to 144, which used octakis(dimethylsiloxy)octasilsesquioxane, which has two or more Si—H groups per molecule, and 1,3-divinyl 1,3-dimethyl 1,3-dimethoxydisiloxane, which has two or more vinyl groups per molecule, when the addition ratio of octasilsesquioxane and 1,3-divinyl 1,3-dimethyl 1,3-dimethoxydisiloxane was 0.001 to 1 wt%, both leakage current and partial discharge were evaluated as ◯ or ⊚. This is believed to be because an addition ratio in the range of 0.001 to 1 wt% significantly reduced the dielectric constant and improved adhesion. When primer treatment was performed, both leakage current and partial discharge tended to improve. This is believed to be because primer treatment improved adhesion at the electrode / encapsulant interface of the semiconductor element. When any of the above addition ratios is below 0.001 wt%, the effect of lowering the dielectric constant and the effect of improving adhesion are somewhat poor, and it is believed that this is rated as ×. When the addition ratio of 1,3-divinyl 1,3-dimethyl 1,3-dimethoxydisiloxane is 2 wt%, the change in the chemical structure of the encapsulant is significant, resulting in a rating of ×. When the addition ratio of octakis(dimethylsiloxy)octasilsesquioxane is 2 wt%, the change in the chemical structure of the encapsulant is significant, resulting in a rating of XX. On the other hand, in Comparative Examples 1 to 126, which used octaphenyloctasilsesquioxane having no more than two Si—H groups per molecule and triethoxyvinylsilane having no more than two vinyl groups per molecule, both leakage current and partial discharge were rated as × or XX. Both are believed to be due to poor curing.
[0082] REFERENCE SIGNS LIST 1 Sealing material, 2 External terminal, 3 Insulating substrate, 3a Circuit network (metal pattern), 4 Metal base plate, 5 Semiconductor element, 5a IGBT, 5b FWD, 6 Case, 7 Lid, 8 Wire, 9 Electrode, 10 Guard ring, 11 Primer layer, 12 Interdigital electrode substrate, 13 Insulating substrate, 14 Interdigital counter electrode pattern, 14a Electrode lead-out portion, 15 Case, 16, 17 Electrode wire, 18 DBC substrate, 100 Semiconductor power module, 110 Module assembly.
Claims
1. A semiconductor device comprising a semiconductor element and an encapsulant, wherein the semiconductor element has a surface in contact with the encapsulant, and the semiconductor element has an electrode on at least one of the surfaces in contact with the encapsulant, the encapsulant comprises a first silicone gel comprising a silicone resin, a cage-type silsesquioxane, and a first hydrolyzable group-containing organosilicon compound, wherein the cage-type silsesquioxane has two or more Si-H groups or vinyl groups in one molecule, the cage-type silsesquioxane forms covalent bonds with the silicone resin or the first hydrolyzable group-containing organosilicon compound at two or more positions in one molecule, a ratio of the cage-type silsesquioxane to the silicone resin is less than 2% by weight, the first hydrolyzable group-containing organosilicon compound has two or more vinyl groups in one molecule, and the first hydrolyzable group-containing organosilicon compound forms covalent bonds with the silicone resin or the cage-type silsesquioxane at two or more positions in one molecule, The first hydrolyzable group-containing organosilicon compound is bonded to the electrode.
2. A semiconductor power module comprising: a semiconductor element, a primer layer, and a sealing material, wherein the semiconductor element has at least one surface in contact with the primer layer, the semiconductor element has an electrode on at least one of the surfaces in contact with the primer layer, the sealing material comprises a second silicone gel comprising a silicone resin and a cage-type silsesquioxane, the cage-type silsesquioxane having two or more Si-H groups or vinyl groups in one molecule, the cage-type silsesquioxane forming covalent bonds with the silicone resin or the first hydrolyzable group-containing organosilicon compound at two or more positions in one molecule, a ratio of the cage-type silsesquioxane to the silicone resin being less than 2% by weight, the primer layer comprising a second hydrolyzable group-containing organosilicon compound, the second hydrolyzable group-containing organosilicon compound having two or more vinyl groups in one molecule, and the second hydrolyzable group-containing organosilicon compound being bonded to the electrode.
3. The cage silsesquioxane is 1-(trivinylsiloxy)-3,4,7,9,11,13,15-heptacyclopentylcyclo[9.5.1.13,9 .1 5,15 .1 7,13 3. The semiconductor power module according to claim 1, wherein the organic solvent is at least one selected from the group consisting of octasiloxane and octakis(dimethylsilyloxy)octasilsesquioxane.
4. A semiconductor power module as described in claim 1 or 2, wherein at least one of the first hydrolyzable group-containing organosilicon compound and the second hydrolyzable group-containing organosilicon compound contains 1,3 divinyl-1,3 dimethyl-1,3 dimethoxydisiloxane.
5. A semiconductor power module according to claim 1 or 2, wherein the ratio of said cage-type silsesquioxane to said silicone resin is in the range of 0.001 to 1% by weight.
6. The semiconductor power module according to claim 1, wherein the ratio of said first hydrolyzable group-containing organosilicon compound to said silicone resin is in the range of 0.001 to 1% by weight.
7. A semiconductor power module according to claim 1 or 2, wherein the penetration of said first silicone gel or said second silicone gel when measured with a quarter cone is 55 to 75.
8. The semiconductor power module according to claim 1 or 2, wherein the electrodes contain copper or aluminum.
9. The semiconductor power module according to claim 1 or 2, wherein the first silicone gel or the second silicone gel has a voltage value of 6.5 kV or more when measured under the following conditions: Conditions: A semiconductor power module comprising an insulating substrate, and a first comb-shaped counter electrode pattern and a second comb-shaped counter electrode pattern, each having a plurality of comb-tooth electrodes, arranged on a main surface of the insulating substrate, the first comb-shaped counter electrode pattern and the second comb-shaped counter electrode pattern are arranged opposite each other so that their comb-tooth electrodes enter into the gaps between the comb-tooth electrodes, and the comb-tooth electrodes have a gap of 1 mm between the comb-tooth electrodes in the portions that enter into the gaps between the comb-tooth electrodes, and the comb-tooth electrodes are sealed with the silicone gel, and a voltage value at which a charge of 10 pC is observed is measured when a voltage is applied between the first comb-shaped counter electrode pattern and the second comb-shaped counter electrode pattern.
10. A method for manufacturing a semiconductor power module as described in claim 1, comprising: a first mixing step of preparing a first mixed liquid by mixing a silicone resin, a cage-type silsesquioxane, and a first hydrolyzable group-containing organosilicon compound; an injection step of injecting the first mixed liquid into a semiconductor element portion; and a curing step of curing the first mixed liquid, wherein the cage-type silsesquioxane has two or more Si-H groups or vinyl groups in one molecule, the first hydrolyzable group-containing organosilicon compound has two or more vinyl groups in one molecule, and the ratio of the cage-type silsesquioxane to the silicone resin is less than 2% by weight.
11. A method for producing a semiconductor power module as described in claim 2, comprising: a second mixing step of preparing a second mixed liquid by mixing a silicone resin and a cage-type silsesquioxane; a coating step of coating a second hydrolyzable group-containing organosilicon compound diluted with a solvent onto an electrode surface of a semiconductor element; an injection step of injecting the second mixed liquid into a semiconductor element portion; and a curing step of curing the second mixed liquid, wherein the cage-type silsesquioxane has two or more Si-H groups or vinyl groups in one molecule, the second hydrolyzable group-containing organosilicon compound has two or more vinyl groups in one molecule, and the ratio of the cage-type silsesquioxane to the silicone resin is less than 2% by weight.
Citation Information
Patent Citations
Silicone resin, sealing material, and optical semiconductor device
JP2012102167A
Polycarbonate resin composition, molded article, and structural member for photovoltaic power generation
JP2016186046A