Electronic component and film forming method

The alumina film with specific carbon and hydrogen atomic percentages addresses adhesion issues with organic-containing external electrodes, ensuring reliable adhesion and barrier performance through a misting and heating film forming method.

WO2024236846A1PCT designated stage expired Publication Date: 2024-11-21MURATA MFG CO LTD
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2023/044630
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-05-17
Filing Date
2023-12-13
Publication Date
2024-11-21

AI Technical Summary

Technical Problem

The adhesion between the alumina film and the external electrode, which contains organic components, is difficult to improve due to the inorganic nature of the alumina film and the organic components in the external electrode.

Method used

An alumina film containing specific atoms such as carbon and hydrogen is formed on the element body, with a specific atomic percentage distribution to ensure adhesion to the external electrode, and a film forming method using a misting process with ultrasonic waves and heating to maintain constant composition ratios.

Benefits of technology

The alumina film with specific atomic percentages of carbon and hydrogen ensures reliable adhesion to the external electrode, preventing cracks and maintaining barrier performance while supporting the electronic component's functionality.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JP2023044630_21112024_PF_FP_ABST
    Figure JP2023044630_21112024_PF_FP_ABST
Patent Text Reader

Abstract

This electronic component (10) comprises an element body (20) and an alumina film (50) containing aluminum atoms and oxygen atoms. The electronic component (10) comprises an internal electrode and an external electrode. The alumina film (50) contains one or more types of specific atoms selected from carbon atoms and hydrogen atoms. The area of the alumina film (50) excluding, in the alumina film (50), the range of 10% of the thickness of the alumina film (50) from the interface with the element body (20) toward the outer surface of the alumina film (50) and, in the alumina film (50), the range of 10% of the thickness of the alumina film (50) from the outer surface of the alumina film (50) toward the element body (20) is defined as a specific area (SA). When the specific area (SA) is divided into 10 equal parts in the thickness direction of the alumina film (50) and each resulting area is defined as a divided area, the atomic percentage of the specific atom in each divided area is 0.5 times to 1.5 times the atomic percentage of the same type of specific atom in the entire specific area (SA).
Need to check novelty before this filing date? Find Prior Art

Description

Electronic component and film formation method

[0001] The present disclosure relates to an electronic component and a film forming method.

[0002] The invention described in Patent Document 1 comprises an element body, internal electrodes, external electrodes, and a protective film. The internal electrodes are located inside the element body. The protective film covers the outer surface of the element body. The protective film is an alumina film containing aluminum atoms and oxygen atoms. The protective film is formed by high-frequency sputtering. The external electrodes are laminated on the outer surface of the protective film. The external electrodes are electrically connected to the internal electrodes. The external electrodes contain silver powder, an organic binder, and glass frit.

[0003] Japanese Patent Application Laid-Open No. 2003-272906

[0004] In the invention described in Patent Document 1, the protective film is made of a so-called inorganic component. On the other hand, the external electrodes laminated on the protective film contain not only inorganic components but also organic components. When the external electrodes contain organic components, it is difficult to improve the adhesion of the external electrodes to the protective film.

[0005] In order to solve the above-described problems, one aspect of the present disclosure is an electronic component comprising: an element body; an alumina film covering an outer surface of the element body and containing aluminum atoms and oxygen atoms; an internal electrode located inside the element body; and an external electrode electrically connected to the internal electrode and located on the outer surface of the alumina film, wherein the alumina film contains one or more specific atoms selected from carbon atoms and hydrogen atoms; a region of the alumina film excluding a range of 10% of the thickness of the alumina film from the interface with the element body toward the outer surface of the alumina film and a range of 10% of the thickness of the alumina film from the outer surface of the alumina film toward the element body is defined as a specific region; the specific region is divided into 10 equal parts in the thickness direction of the alumina film, and each region is defined as a divided region; and the atomic percentage of the specific atoms in each divided region is 0.5 to 1.5 times the atomic percentage of the specific atoms of the same type in the entire specific region.

[0006] In order to solve the above-described problems, one aspect of the present disclosure is a film formation method for forming an alumina film on an outer surface of an element body, the film formation method comprising: a loading step of loading the element body into a first chamber capable of heating an internal atmosphere; a mist-forming step of using ultrasonic waves to turn a liquid raw material containing aluminum atoms and oxygen atoms into a mist in a second chamber; a supply step of supplying the mist-like raw material from the second chamber into the first chamber together with a carrier gas; and a heating step of heating the atmosphere in the first chamber while performing the supply step, wherein the raw material further contains one or more atoms selected from carbon atoms and hydrogen atoms.

[0007] Even if the external electrodes contain an organic component, the adhesion between the alumina film and the external electrodes on the alumina film can be ensured.

[0008] FIG. 1 is a perspective view of an electronic component. FIG. 2 is a side view of the electronic component. FIG. 3 is a cross-sectional view taken along line 3-3 in FIG. 2. FIG. 4 is an explanatory diagram illustrating a method for manufacturing an electronic component. FIG. 5 is an explanatory diagram illustrating a method for manufacturing an electronic component. FIG. 6 is an explanatory diagram illustrating a method for manufacturing an electronic component. FIG. 7 is an explanatory diagram illustrating a method for manufacturing an electronic component. FIG. 8 is a table showing the composition analysis results for each sample piece. FIG. 9 is a graph showing the composition analysis results for the first sample piece. FIG. 10 is a graph showing the composition analysis results for the second sample piece. FIG. 11 is a graph showing the composition analysis results for the third sample piece.

[0009] An embodiment of an electronic component will now be described with reference to the drawings. The drawings may show components enlarged for ease of understanding. The dimensional proportions of the components may differ from those in the actual components or from those in other drawings.

[0010] <Regarding the Electronic Component> As shown in FIG. 1 , the electronic component 10 is, for example, a surface-mount type negative temperature coefficient thermistor component mounted on a circuit board or the like. Note that a negative temperature coefficient thermistor component has the characteristic that its resistance value decreases as the temperature increases. The electronic component 10 includes an element body 20. The element body 20 is generally rectangular prism-shaped and has a central axis CA. Note that, hereinafter, an axis extending along the central axis CA is referred to as a first axis X. Furthermore, one of the axes perpendicular to the first axis X is referred to as a second axis Y. Furthermore, an axis perpendicular to the first axis X and the second axis Y is referred to as a third axis Z. Additionally, one of the directions along the first axis X is referred to as a first positive direction X1, and the direction along the first axis X opposite to the first positive direction X1 is referred to as a first negative direction X2. One of the directions along the second axis Y is defined as a second positive direction Y1, and the direction along the second axis Y opposite to the second positive direction Y1 is defined as a second negative direction Y2. Furthermore, one of the directions along the third axis Z is defined as a third positive direction Z1, and the direction along the third axis Z opposite to the third positive direction Z1 is defined as a third negative direction Z2.

[0011] The outer surface 21 of the element body 20 has six flat surfaces 22. The term "surface" of the element body 20 as used herein refers to a surface that can be observed when the entire element body 20 is observed. In other words, even if there are minute irregularities or steps that are not visible unless a portion of the element body 20 is magnified and observed using a microscope or the like, the surface is still referred to as a flat or curved surface. The six flat surfaces 22 face in different directions. The six flat surfaces 22 are broadly divided into a first end surface 22A facing the first positive direction X1, a second end surface 22B facing the first negative direction X2, and four side surfaces 22C. The four side surfaces 22C are, respectively, a surface facing the third positive direction Z1, a surface facing the third negative direction Z2, a surface facing the second positive direction Y1, and a surface facing the second negative direction Y2.

[0012] Furthermore, on the outer surface 21 of the element body 20, the boundary portions between two adjacent flat surfaces 22 and the boundary portions between three adjacent flat surfaces 22 are curved. In other words, the corners of the element body 20 are so-called R-chamfered.

[0013] As shown in Fig. 2, the element body 20 has a larger dimension along the first axis X than along the third axis Z. Also, as shown in Fig. 1, the element body 20 has a larger dimension along the first axis X than along the second axis Y. The material of the element body 20 is a semiconductor. Specifically, the material of the element body 20 is a ceramic obtained by firing a metal oxide containing at least one of Mn, Fe, Ni, Co, Ti, Ba, Al, and Zn.

[0014] 3 , the electronic component 10 includes two first internal electrodes 41 and two second internal electrodes 42. The first internal electrodes 41 and the second internal electrodes 42 are located inside the element body 20.

[0015] The first internal electrode 41 is made of a conductive material. For example, the first internal electrode 41 is made of palladium. The second internal electrode 42 is made of the same material as the first internal electrode 41.

[0016] The first internal electrode 41 has a rectangular plate shape. The main surface of the first internal electrode 41 is perpendicular to the second axis Y. The second internal electrode 42 has the same rectangular plate shape as the first internal electrode 41. The main surface of the second internal electrode 42 is perpendicular to the second axis Y, similar to the first internal electrode 41.

[0017] The dimension of the first internal electrode 41 in the direction along the first axis X is smaller than the dimension of the element body 20 in the direction along the first axis X. Also, as shown in Fig. 1 , the dimension of the first internal electrode 41 in the direction along the third axis Z is approximately two-thirds of the dimension of the element body 20 in the direction along the third axis Z. The dimensions of the second internal electrode 42 in each direction are the same as those of the first internal electrode 41.

[0018] 3, the first internal electrodes 41 and the second internal electrodes 42 are positioned alternately in the direction along the second axis Y. That is, a total of four internal electrodes are arranged alternately in the order of the first internal electrode 41, the second internal electrode 42, the first internal electrode 41, and the second internal electrode 42 from the side surface 22C facing the second positive direction Y1 toward the second negative direction Y2. In this embodiment, the distances between the internal electrodes in the direction along the second axis Y are equal.

[0019] 1, the two first internal electrodes 41 and the two second internal electrodes 42 are both located at the center of the element body 20 in the direction along the third axis Z. On the other hand, as shown in Fig. 3, the first internal electrodes 41 are located closer to the first positive direction X1, and the second internal electrodes 42 are located closer to the first negative direction X2.

[0020] Specifically, the end of the first internal electrode 41 on the first positive direction X1 side coincides with the end of the element body 20 on the first positive direction X1 side. The end of the first internal electrode 41 on the first negative direction X2 side is located inside the element body 20 and does not reach the end of the element body 20 on the first negative direction X2 side. On the other hand, the end of the second internal electrode 42 on the first negative direction X2 side coincides with the end of the element body 20 on the first negative direction X2 side. The end of the second internal electrode 42 on the first positive direction X1 side is located inside the element body 20 and does not reach the end of the element body 20 on the first positive direction X1 side.

[0021] As shown in Fig. 3, the electronic component 10 includes an alumina film 50. The alumina film 50 covers the outer surface 21 of the element body 20. In this embodiment, the alumina film 50 covers the entire area of ​​the outer surface 21 of the element body 20. In this embodiment, the alumina film 50 indicates that the main component of the film is alumina. Specifically, the alumina film 50 is a film in which the total atomic percentage of aluminum atoms and oxygen atoms contained in the film is 80% or more.

[0022] The electronic component 10 includes a first external electrode 61 and a second external electrode 62. The first external electrode 61 is located on the outer surface of the alumina film 50. The first external electrode 61 includes a first base electrode 61A and a first metal layer 61B. The first base electrode 61A is laminated on the alumina film 50 over a portion of the outer surface 21 of the element body 20, including the first end face 22A. The first base electrode 61A is a five-sided electrode that covers the first end face 22A of the element body 20 and portions of the four side faces 22C facing the first positive direction X1. In this embodiment, the first base electrode 61A is made of a mixture of copper, glass, and organic resin. Therefore, the first base electrode 61A is a sintered body containing an organic component.

[0023] 3, the first metal layer 61B covers the first base electrode 61A from the outside. Therefore, the first metal layer 61B is laminated on the first base electrode 61A. Furthermore, a portion of the first metal layer 61B protrudes from the first base electrode 61A. In other words, a portion of the outer edge of the first metal layer 61B directly covers the alumina film 50 without the first base electrode 61A in between. Although not shown in the figure, the first metal layer 61B has a two-layer structure consisting of a nickel layer and a tin layer, in this order from the first base electrode 61A side.

[0024] The second external electrode 62 includes a second base electrode 62A and a second metal layer 62B. The second base electrode 62A is laminated on the alumina film 50 over a portion of the outer surface 21 of the element body 20, including the second end face 22B. The second base electrode 62A is a five-sided electrode that covers the second end face 22B of the element body 20 and portions of the four side faces 22C facing the first negative direction X2. In this embodiment, the material of the second base electrode 62A is the same as the material of the first external electrode 61, which is a mixture of copper, glass, and organic resin. Therefore, the second base electrode 62A, like the first base electrode 61A, is a sintered body containing an organic component.

[0025] The second metal layer 62B covers the second base electrode 62A from the outside. Therefore, the second metal layer 62B is stacked on the second base electrode 62A. Furthermore, a portion of the second metal layer 62B protrudes from the second base electrode 62A. In other words, a portion of the outer edge of the second metal layer 62B directly covers the alumina film 50 without the second base electrode 62A in between. Although not shown, the second metal layer 62B, like the first metal layer 61B, has a two-layer structure consisting of a nickel layer and a tin layer, in this order from the second base electrode 62A side.

[0026] The second external electrode 62 does not reach the first external electrode 61 on the side surface 22C, and is spaced apart from the first external electrode 61 in the direction along the first axis X. In addition, the first external electrode 61 and the second external electrode 62 are not stacked in the central portion of the side surface 22C of the element body 20 in the direction along the first axis X, and the alumina film 50 is exposed. Note that in Figures 1 to 3, the first external electrode 61 and the second external electrode 62 are shown by two-dot chain lines.

[0027] The first external electrode 61 and the end of the first internal electrode 41 on the first positive direction X1 side are connected via a first through portion 71 that penetrates the alumina film 50. Therefore, the first external electrode 61 is electrically connected to the first internal electrode 41. Note that, as will be described in detail later, the first through portion 71 is formed during the manufacturing process of the electronic component 10 when palladium that constitutes the first internal electrode 41 extends toward the first external electrode 61 side.

[0028] The second external electrode 62 and the end of the second internal electrode 42 on the first negative direction X2 side are connected via a second through portion 72 that penetrates the alumina film 50. Therefore, the second external electrode 62 is electrically connected to the second internal electrode 42. Like the first through portion 71, the second through portion 72 is formed by the palladium constituting the second internal electrode 42 extending toward the second external electrode 62 during the manufacturing process of the electronic component 10. Note that while FIG. 3 illustrates the first internal electrode 41 and the first through portion 71 as separate components with a boundary, in reality, there is no clear boundary between them. The same applies to the second through portion 72. The first through portion 71 is not shown in FIG. 1.

[0029] <Regarding the Alumina Film> As described above, the alumina film 50 contains aluminum atoms and oxygen atoms. Furthermore, in addition to aluminum atoms and oxygen atoms, the alumina film 50 also contains both carbon atoms and hydrogen atoms as specific atoms. Note that the alumina film 50 only needs to contain one or more atoms selected from carbon atoms and hydrogen atoms as the specific atoms.

[0030] The average thickness of the alumina film 50 is, for example, 0.05 μm or more and 2.0 μm or less. The thickness of the alumina film 50 is the shortest distance from the boundary surface of the alumina film 50 with the element body 20 to the outer surface of the alumina film 50. The average thickness of the alumina film 50 is calculated as follows. First, an arbitrary cross section of the element body 20 is photographed using an electron microscope. Next, a range in the photographed image in the direction along the outer surface of the alumina film 50 is identified. Within this range, the cross-sectional area of ​​the alumina film 50 is calculated by image processing for a measurement range of at least 5 μm or more. The thickness of the alumina film 50 is then calculated by dividing the cross-sectional area of ​​the alumina film 50 in the calculated measurement range by the length of the measurement range. This is the average thickness of the alumina film 50.

[0031] Here, the region of the alumina film 50 excluding the boundary with other substances is defined as the specific region SA. Specifically, the specific region SA is the region of the alumina film 50 excluding a range of 10% of the thickness of the alumina film 50 from the interface with the element body 20 toward the outer surface of the alumina film 50 and a range of 10% of the thickness of the alumina film 50 from the outer surface of the alumina film 50 toward the element body 20. That is, if the thickness of the alumina film 50 is 200 nm, the specific region SA is the central 160 nm region of the alumina film 50 excluding a range of 20 nm from the interface with the element body 20 toward the outer surface of the alumina film 50 and a range of 20 nm from the outer surface of the alumina film 50 toward the element body 20. In this embodiment, the boundary between the alumina film 50 and the element body 20 is defined as a location where atoms not contained in the alumina film 50 but contained in the element body 20 are detected.

[0032] The atomic percentage of aluminum atoms in the entire specific region SA is 30 at% or more and 40 at% or less. The atomic percentage of oxygen atoms in the entire specific region SA is 50 at% or more and 60 at% or less. The atomic percentage of hydrogen atoms in the entire specific region SA is 3.0 at% or more and 15.0 at% or less. The atomic percentage of carbon atoms in the entire specific region SA is 0.3 at% or more and 3.0 at% or less. The atomic percentages of each atom in the entire specific region SA are values ​​measured by composition analysis using RBS (Rutherford Backscattering Spectrometry).

[0033] Here, the specific area SA is divided into 10 equal parts in the thickness direction of the alumina film 50, and each of the divided areas is defined as a divided area. If the thickness of the alumina film 50 is 200 nm, each divided area is a region divided every 16 nm in the thickness direction of the alumina film 50. The atomic percentage of the specific atoms in each divided area is 0.5 to 1.5 times the atomic percentage of the same type of specific atoms in the entire specific area SA.

[0034] Specifically, the atomic percentage of carbon atoms in each divided region is 0.5 to 1.5 times the atomic percentage of carbon atoms in the entire specific region SA. If the atomic percentage of carbon atoms in the entire specific region SA is 1.6 at%, in this embodiment, the atomic percentage of carbon atoms in each divided region is 0.8 to 2.4 at%. If the variation in the atomic percentage of carbon atoms in each divided region is within the above range, it can be said that the atomic percentage of carbon atoms is approximately constant in the thickness direction within the specific region SA.

[0035] Furthermore, the atomic percentage of hydrogen atoms in each divided region is 0.5 to 1.5 times the atomic percentage of hydrogen atoms in the entire specific region SA. If the atomic percentage of hydrogen atoms in the entire specific region SA is 8 at%, the atomic percentage of carbon atoms in each divided region is 4 to 12 at%. If the variation in the atomic percentage of hydrogen atoms in each divided region is within the above range, it can be said that the atomic percentage of hydrogen atoms is generally constant in the thickness direction within the specific region SA.

[0036] Furthermore, the atomic percentages of aluminum atoms and oxygen atoms in each divided region are both minus 5 at% and plus 5 at% of the atomic percentages of the same type of atoms in the entire specific region SA. Specifically, if the atomic percentage of aluminum atoms in the entire specific region SA is 35 at%, the atomic percentage of aluminum atoms in each divided region is within the range of 30 at% and 40 at%. Furthermore, if the atomic percentage of oxygen atoms in the entire specific region SA is 55 at%, the atomic percentage of oxygen atoms in each divided region is within the range of 50 at% and 60 at%. Thus, if the variation in the atomic percentages of aluminum atoms and oxygen atoms in each divided region is within the above range, it can be said that the atomic percentages of aluminum atoms and oxygen atoms are generally constant in the thickness direction within the specific region SA.

[0037] <Method for Manufacturing Electronic Component> Next, a method for manufacturing electronic component 10 will be described. As shown in Fig. 4, the method for manufacturing electronic component 10 includes a laminate preparation step S11, a rounded chamfering step S12, a loading step S13, a mist-forming step S14, a supplying step S15, and a heating step S16. The method for manufacturing electronic component 10 also includes a conductor application step S17, a curing step S18, and a plating step S19.

[0038] First, in forming the element body 20, a laminate is prepared in the laminate preparation step S11. The laminate at this stage is in a state before R-chamfering and has a rectangular parallelepiped shape with six flat surfaces 22. For example, first, a plurality of ceramic sheets that will become the element body 20 are prepared. The sheets are thin plates. A conductive paste that will become the first internal electrode 41 is laminated on the sheets. A ceramic sheet that will become the element body 20 is laminated on the laminating paste. A conductive paste that will become the second internal electrode 42 is laminated on the sheets. In this manner, the ceramic sheets and the conductive paste are laminated. The laminated sheets are then pressed in the stacking direction using a mold press or other means. The pressed sheet is then cut to a predetermined size to form an unfired laminate. The unfired laminate is then fired at a high temperature to prepare the laminate.

[0039] Next, an R-chamfering process step S12 is performed. In the R-chamfering process step S12, the laminate prepared in the laminate preparation process S11 is R-chamfered. This process provides an element body 20 with R-chamfered corners.

[0040] Next, the introduction step S13 to the heating step S16 are performed in sequence. The introduction step S13 to the heating step S16 are performed using the film formation apparatus 100. As shown in FIG. 5 , the film formation apparatus 100 includes a first chamber 91. The first chamber 91 is capable of heating the atmosphere therein. Specifically, the first chamber 91 includes a heater 91A, a container body 91B, and an exhaust passage 91C. The heater 91A is located at the bottom of the container body 91B. By driving the heater 91A, the atmosphere within the container body 91B is heated. The exhaust passage 91C is connected to the container body 91B. The interior of the container body 91B is connected to the outside via the exhaust passage 91C.

[0041] The film forming apparatus 100 includes a second chamber 92, a liquid supply nozzle 93, and a gas supply nozzle 94. The second chamber 92 includes an ultrasonic generator 92A, a container body 92B, and a communication passage 92C. The ultrasonic generator 92A is located at the bottom of the container body 92B. By driving the ultrasonic generator 92A, the liquid supplied to the container body 92B can be converted into a mist. The communication passage 92C connects the container body 91B of the first chamber 91 to the container body 92B of the second chamber 92. In other words, the inside of the container body 92B of the second chamber 92 is connected to the inside of the container body 91B of the first chamber 91 via the communication passage 92C. The liquid supply nozzle 93 can supply liquid precursor material into the container body 92B. The gas supply nozzle 94 can supply carrier gas into the container body 92B.

[0042] 4, a loading step S13 is performed. As shown in FIG. 5, in the loading step S13, the element body 20 is loaded into the first chamber 91 of the film forming apparatus 100. Then, the heater 91A of the first chamber 91 is driven to heat the atmosphere in the first chamber 91.

[0043] Next, a mist-forming step S14 is performed. As shown in FIG. 6, in the mist-forming step S14, the liquid raw material is introduced into the second chamber 92 via the liquid supply nozzle 93. The ultrasonic generator 92A is then driven to turn the raw material into a mist using ultrasonic waves. Note that the mist-like state refers to a state in which the raw material is in the form of droplets with a particle size of 10 μm or less. The raw material contains aluminum acetylacetonate, methanol, and water. That is, the raw material contains aluminum atoms and oxygen atoms. Furthermore, the raw material contains carbon atoms and hydrogen atoms.

[0044] Next, as shown in FIG. 4 , a supply step S15 is performed. As shown in FIG. 7 , in the supply step S15, a carrier gas is supplied into the second chamber 92 via the gas supply nozzle 94. As a result, the mist-like raw material is supplied from the second chamber 92 to the first chamber 91 together with the carrier gas. The carrier gas is, for example, an inert gas such as oxygen, ozone, nitrogen, or argon. The carrier gas may also be a reducing gas such as hydrogen gas or forming gas. Note that excess carrier gas and excess raw material supplied into the first chamber 91 are exhausted to the outside of the film forming apparatus 100 via an exhaust passage 91C.

[0045] Next, as shown in FIG. 4 , a heating step S16 is performed. In the heating step S16, the atmosphere in the first chamber 91 is heated while the supplying step S15 is being performed. Specifically, in the heating step S16, the heater 91A is driven to heat the atmosphere in the first chamber 91. The heating reduces the particle size of the mist that flows from the second chamber 92 into the first chamber 91. The temperature in the first chamber 91 at this time is, for example, several hundred degrees. During the heating step S16, fine mist of the raw material adheres to the element body 20, thereby forming an alumina film 50 on the outer surface 21 of the element body 20. Furthermore, the atomic composition ratio of the raw material is kept constant during the mist-forming step S14, the supplying step S15, and the heating step S16. That is, the atomic composition ratio of the mist formed from the raw material is approximately the same at any time during the above steps. As this mist accumulates, the atomic percentage in the alumina film 50 becomes approximately constant throughout the entire alumina film 50. In particular, the atomic percentage of each atom is approximately constant in a specific area SA excluding the boundary with other objects in the alumina film 50. The steps from the introducing step S13 to the heating step S16 constitute a film formation method for forming the alumina film 50 on the outer surface 21 of the element body 20.

[0046] Next, a conductor application step S17 is performed. In this step S17, the element body 20 on which the alumina film 50 has been formed is removed from the film-forming apparatus 100. Then, a conductor paste is applied to two locations on the outer surface of the alumina film 50: a portion including a portion covering the first end face 22A of the element body 20, and a portion including a portion covering the second end face 22B of the element body 20. Specifically, the conductor paste is applied to cover the alumina film 50 over the entire first end face 22A and portions of the four side faces 22C. The conductor paste is also applied to cover the alumina film 50 over the entire second end face 22B and portions of the four side faces 22C.

[0047] Next, a curing step S18 is performed. Specifically, the curing step S18 involves heating the element body 20. In the curing step S18, the conductive paste applied in the conductive material application step S17 is fired to form the first base electrode 61A and the second base electrode 62A.

[0048] In this embodiment, during heating in the curing step S18, the Kirkendall effect, which arises from the difference in diffusion rate between the first internal electrode 41 and the first base electrode 61A, attracts palladium contained in the first internal electrode 41 toward the first base electrode 61A containing copper. As a result, the first through-hole 71 extends from the first internal electrode 41 toward the first base electrode 61A, penetrating the alumina film 50. This connects the first internal electrode 41 and the first base electrode 61A. The same applies to the second through-hole 72 connecting the second internal electrode 42 and the second base electrode 62A.

[0049] Next, a plating step S19 is performed. Electroplating is performed on the first base electrode 61A and the second base electrode 62A. As a result, a first metal layer 61B is formed on the surface of the first base electrode 61A. Furthermore, a second metal layer 62B is formed on the surface of the second base electrode 62A. Although not shown, the first metal layer 61B and the second metal layer 62B are electroplated with two types of metal, nickel and tin, to form a two-layer structure. In this manner, the electronic component 10 is formed.

[0050] <Atomic Percentage> Here, the alumina films 50 were formed under different film formation conditions, and the atomic percentage of each atom in each alumina film 50 was measured.

[0051] First, an alumina film 50 was formed on a silicon substrate by performing the mist-forming step S14, the supplying step S15, and the heating step S16 described above. Furthermore, three sample pieces were prepared by varying the temperature conditions in the heating step S16. The first sample piece was prepared by setting the heating time to 30 minutes and the heating temperature to 400°C in the heating step S16. The second sample piece was prepared by setting the heating time to 30 minutes and the heating temperature to 500°C in the heating step S16. The third sample piece was prepared by forming the alumina film 50 in the heating step S16 by setting the heating time to 30 minutes and the heating temperature to 400°C, followed by annealing in an atmosphere at 800°C.

[0052] As shown in FIG. 9 , a composition analysis was performed on the first sample piece using RBS. The composition analysis was performed on a portion of the sample piece located within an arbitrary range of 2 mm in diameter when viewed in a plan view perpendicular to the main surface of the silicon substrate. In the measurement results, the 0 nm point indicates the outer surface position of the alumina film 50. In the first sample piece, silicon atoms increased approximately 205 nm from the outer surface of the alumina film 50 toward the silicon substrate. That is, in the first sample piece, the boundary between the alumina film 50 and the silicon substrate was approximately 205 nm from the outer surface of the alumina film 50. In other words, the thickness of the alumina film 50 was approximately 205 nm. The region of the alumina film 50 of the first sample piece excluding the 20.5 nm range from the interface with the silicon substrate toward the outer surface of the alumina film 50 and the 20.5 nm range from the outer surface of the alumina film 50 toward the silicon substrate was designated the specific region SA. At this time, the atomic percentage of each atom contained in the alumina film 50 is approximately constant in the specific region SA. Specifically, as shown in FIG. 8, in the specific region SA, the atomic percentage of aluminum atoms is approximately constant at 33.2 at%. In the specific region SA, the atomic percentage of oxygen atoms is approximately constant at 52.5 at%. In the specific region SA, the atomic percentage of carbon atoms is approximately constant at 1.7 at%. In the specific region SA, the atomic percentage of hydrogen atoms is approximately constant at 12.6 at%.

[0053] As shown in FIG. 10 , the second sample piece was subjected to compositional analysis by RBS. The measurement range was the same as that of the first sample piece. In the second sample piece, silicon atoms increased approximately 390 nm from the outer surface of the alumina film 50. That is, the thickness of the alumina film 50 in the second sample piece was approximately 390 nm. The region of the alumina film 50 in the second sample piece excluding the 39 nm range from the interface with the silicon substrate toward the outer surface of the alumina film 50 and the 39 nm range from the outer surface of the alumina film 50 toward the silicon substrate was designated as the specific region SA. In this case, the atomic percentage of each atom contained in the alumina film 50 was approximately constant in the specific region SA. Specifically, as shown in FIG. 8 , the atomic percentage of aluminum atoms in the specific region SA was approximately constant at 37.4 at%. The atomic percentage of oxygen atoms in the specific region SA was approximately constant at 56.4 at%. In the specific area SA, the atomic percentage of carbon atoms was approximately constant at 0.6 at %, and the atomic percentage of hydrogen atoms was approximately constant at 5.6 at %.

[0054] As shown in FIG. 11 , a composition analysis was performed using RBS on the third sample piece. The measurement range was the same as that of the first sample piece. In the third sample piece, silicon atoms increased approximately 180 nm from the outer surface of the alumina film 50. That is, the thickness of the alumina film 50 in the third sample piece was approximately 180 nm. The region of the alumina film 50 in the third sample piece, excluding the 18 nm range from the interface with the silicon substrate toward the outer surface of the alumina film 50 and the 18 nm range from the outer surface of the alumina film 50 toward the silicon substrate, was designated as the specific region SA. In this case, the atomic percentage of each atom contained in the alumina film 50 was generally constant within the specific region SA, but slight variations in the atomic percentage of each atom were observed in a certain region of the alumina film 50 closer to the silicon substrate. However, even in this case, the variations in the atomic percentage of each atom were so slight that they could be considered constant. As shown in Figure 8, in the specific area SA, the atomic percentage of aluminum atoms was 38.8 at%, the atomic percentage of oxygen atoms was 56.2 at%, the atomic percentage of carbon atoms was 1.7 at%, and the atomic percentage of hydrogen atoms was 3.3 at%.

[0055] It is assumed that the specific region SA is divided into 10 equal parts in the thickness direction of the alumina film 50, and each of these regions is defined as a divided region. In this case, "the atomic percentage of carbon atoms is approximately constant in the specific region SA" means that the atomic percentage of specific atoms in each divided region is 0.5 to 1.5 times the atomic percentage of carbon atoms in the entire specific region SA. This also applies to "the atomic percentage of hydrogen atoms is approximately constant in the specific region SA." Furthermore, "the atomic percentage of aluminum atoms is approximately constant in the specific region SA" means that the atomic percentage of aluminum atoms in each divided region is within a range of minus 5 at.% to plus 5 at.% of the atomic percentage of aluminum atoms in the entire specific region SA. This also applies to "the atomic percentage of oxygen atoms is approximately constant in the specific region SA."

[0056] <Effects of the Present Embodiment> (1) According to the above embodiment, the alumina film 50 contains at least one of hydrogen atoms and carbon atoms. That is, the alumina film 50 of the above embodiment contains an organic component. The alumina film 50 containing these organic components can ensure adhesion between the alumina film 50 and the first base electrode 61A and the second base electrode 62A, which are sintered bodies containing the organic component.

[0057] Furthermore, in the above embodiment, the atomic percentage of carbon atoms in each divided region is 0.5 to 1.5 times the atomic percentage of carbon atoms in the entire specific region SA. That is, the carbon atoms are located generally uniformly without bias in the specific region SA. If the carbon atoms are concentrated in a portion of the alumina film 50, cracks are likely to occur at the carbon atom concentration during manufacturing due to differences in thermal shrinkage rates between the portion and other portions with different composition ratios. The configuration of the above embodiment can reduce the possibility of such cracks. Furthermore, the atomic percentage of hydrogen atoms in each divided region is 0.5 to 1.5 times the atomic percentage of hydrogen atoms in the entire specific region SA. Therefore, similar to the case of carbon atoms described above, the possibility of cracks occurring due to bias in hydrogen atoms can be reduced.

[0058] (2) In the above embodiment, at least 0.3 at % of carbon atoms are present in the specific region SA. Therefore, the effect of improving adhesion to the first base electrode 61A and the second base electrode 62A containing organic matter can be reliably obtained. Furthermore, in the above embodiment, the carbon atoms in the specific region SA are at most 3.0 at %. In other words, the amount of carbon atoms is not that large in terms of the proportion of the entire specific region SA. Therefore, it is possible to prevent the alumina film 50 from having an excess of carbon atoms, which would otherwise reduce its barrier performance.

[0059] (3) In the above embodiment, at least 3.0 at % of hydrogen atoms are present in the specific region SA. Therefore, the effect of improving adhesion to the first base electrode 61A and the second base electrode 62A, which contain organic matter, can be reliably obtained. Furthermore, in the above embodiment, the hydrogen atoms in the specific region SA are at most 15.0 at %. In other words, the amount of hydrogen atoms is not that large in terms of the proportion of the entire specific region SA. Therefore, it is possible to prevent a decrease in the barrier performance of the alumina film 50 due to an excess of hydrogen atoms in the alumina film 50.

[0060] (4) In the above embodiment, the atomic percentage of aluminum atoms and the atomic percentage of oxygen atoms in each divided region are both within a range of minus 5 at % and plus 5 at % of the atomic percentage of the same type of atoms in the entire specific region SA. In this way, the alumina component is distributed approximately evenly in the specific region SA, ensuring barrier performance throughout the entire alumina film 50.

[0061] (5) In the above embodiment, the atomic composition ratio of the raw material is constant throughout the mist-forming step S14, the supplying step S15, and the heating step S16. In the alumina film 50 formed using the mist formed from such raw material, specific atoms are unlikely to be unevenly positioned. Therefore, with the above configuration, the crack suppression effect described in (1) can be more significantly achieved.

[0062] <Modifications> The above embodiment and the following modifications can be implemented in combination with each other within the scope of technical compatibility.

[0063] In the above embodiment, the electronic component 10 is not limited to a negative temperature coefficient thermistor component. For example, the electronic component 10 may be a piezoelectric component, a multilayer ceramic capacitor, an inductor, or the like.

[0064] In the above embodiment, the number of first internal electrodes 41 and second internal electrodes 42 is not limited to the example in the above embodiment. The number of first internal electrodes 41 may be less than two or more than two. The same applies to the second internal electrodes 42.

[0065] In the above embodiment, the materials of the first base electrode 61A and the second base electrode 62A are not limited to the examples in the above embodiment. For example, the materials of the first base electrode 61A and the second base electrode 62A may be a mixture of silver and glass. Furthermore, the materials of the first base electrode 61A and the second base electrode 62A do not necessarily have to contain an organic component.

[0066] In the above embodiment, the alumina film 50 does not have to cover the entire element body 20. It is sufficient that the alumina film 50 covers at least a portion of the outer surface 21 of the element body 20.

[0067] In the above embodiment, the average thickness of the alumina film 50 is not limited to the example of the above embodiment. The average thickness of the alumina film 50 may be set to any thickness in consideration of the stresses and the like associated with the alumina film 50.

[0068] In the above embodiment, the atomic percentage of each atom in the alumina film 50 is merely an example. The alumina film 50 mainly comprises an alumina component, and the atomic percentage of a specific atom in a divided region may be 0.5 to 1.5 times the atomic percentage of the same type of specific atom in the entire specific region SA.

[0069] In the above embodiment, the atomic percentage of the divided region may be determined by measuring the atomic percentage at any number of points within the divided region and averaging the measured values.

[0070] In the above embodiment, the alumina film 50 may contain at least one specific atom selected from carbon atoms and hydrogen atoms. That is, the alumina film 50 may have only carbon atoms as specific atoms, or may have only hydrogen atoms as specific atoms.

[0071] In the above embodiment, the chemical raw materials used in the mist-forming step S14, the supplying step S15, and the heating step S16 are not limited to those in the above embodiment. For example, the raw materials may be organic salts containing aluminum, organic solvents, etc. Furthermore, the raw materials may or may not contain water.

[0072] In the above embodiment, the atomic composition ratio of the raw material may be changed during the execution of the mist-forming step S14, the supplying step S15, and the heating step S16. However, even when the raw material composition ratio is changed, the atomic percentage of the specific atoms in each divided region of the formed alumina film 50 must be 0.5 times or more and 1.5 times or less than the atomic percentage of the same type of specific atoms in the entire specific region SA.

[0073] In the above embodiment, the atomic percentage of carbon atoms in the entire specific region SA of the alumina film 50 may be less than 0.3 at %. Alternatively, the atomic percentage of carbon atoms in the entire specific region SA of the alumina film 50 may be greater than 3.0 at %.

[0074] In the above embodiment, the atomic percentage of hydrogen atoms in the entire specific region SA of the alumina film 50 may be less than 3.0 at %. Also, the atomic percentage of hydrogen atoms in the entire specific region SA of the alumina film 50 may be greater than 15.0 at %.

[0075] In the above embodiment, the atomic percentage of aluminum atoms and the atomic percentage of oxygen atoms in each divided region may be less than minus 5 at% of the atomic percentage of the same type of atoms in the entire specific region SA, or may be greater than plus 5 at%.

[0076] <Supplementary Notes> The technical concepts that can be derived from the above embodiments and modifications are described below. [1] An electronic component comprising: an element body, an alumina film covering an outer surface of the element body and containing aluminum atoms and oxygen atoms, an internal electrode located inside the element body, and an external electrode electrically connected to the internal electrode and located on the outer surface of the alumina film, wherein the alumina film contains one or more specific atoms selected from carbon atoms and hydrogen atoms, and wherein a region of the alumina film excluding a range of 10% of the thickness of the alumina film from a boundary surface with the element body toward the outer surface of the alumina film and a range of 10% of the thickness of the alumina film from the outer surface of the alumina film toward the element body is defined as a specific region, and the specific region is divided into 10 equal parts in the thickness direction of the alumina film, and each region is defined as a divided region, the atomic percentage of the specific atom in each divided region is 0.5 to 1.5 times the atomic percentage of the specific atom of the same type in the entire specific region.

[0077] [2] The electronic component according to [1], wherein the alumina film contains the carbon atoms as the specific atoms, and the atomic percentage of the carbon atoms in the entire specific region is 0.3 at % or more and 3.0 at % or less.

[0078] [3] The electronic component according to [1] or [2], wherein the alumina film contains hydrogen atoms as the specific atoms, and the atomic percentage of the hydrogen atoms in the entire specific region is 3.0 at% or more and 15.0 at% or less.

[0079] [4] The atomic percentage of the aluminum atoms and the atomic percentage of the oxygen atoms in each of the divided regions are both within a range of minus 5 at% or more and plus 5 at% or less of the atomic percentage of the same type of atoms in the entire specific region [1] to [3]. An electronic component according to any one of [1] to [3].

[0080] [5] A method for forming an alumina film on the outer surface of an element body, the method comprising: a loading step of loading the element body into a first chamber capable of heating the internal atmosphere; a mist-forming step of using ultrasonic waves to convert a liquid raw material containing aluminum atoms and oxygen atoms into a mist in a second chamber; a supply step of supplying the mist-like raw material from the second chamber into the first chamber together with a carrier gas; and a heating step of heating the atmosphere in the first chamber while performing the supply step, wherein the raw material further contains one or more atoms selected from carbon atoms and hydrogen atoms.

[0081] [6] The film forming method according to [5], wherein the atomic composition ratio of the raw material is kept constant during the mist-forming step, the supplying step, and the heating step.

[0082] SA...specific area 10...electronic component 20...element body 21...outer surface 41...first internal electrode 42...second internal electrode 50...alumina film 61...first external electrode 62...second external electrode

Claims

1. An electronic component comprising: an element body; an alumina film covering an outer surface of the element body and containing aluminum atoms and oxygen atoms; an internal electrode located inside the element body; and an external electrode electrically connected to the internal electrode and located on the outer surface of the alumina film, wherein the alumina film contains one or more specific atoms selected from carbon and hydrogen atoms, and a region of the alumina film excluding a range of 10% of the thickness of the alumina film from the interface with the element body toward the outer surface of the alumina film and a range of 10% of the thickness of the alumina film from the outer surface of the alumina film toward the element body is defined as a specific region, and the specific region is divided into 10 equal regions in the thickness direction of the alumina film, and each region is defined as a divided region, the atomic percentage of the specific atom in each of the divided regions is 0.5 to 1.5 times the atomic percentage of the specific atom of the same type in the entire specific region.

2. The electronic component according to claim 1, wherein the alumina film contains the carbon atoms as the specific atoms, and the atomic percentage of the carbon atoms in the entire specific region is 0.3 at % or more and 3.0 at % or less.

3. The electronic component according to claim 1 or 2, wherein the alumina film contains hydrogen atoms as the specific atoms, and the atomic percentage of the hydrogen atoms in the entire specific region is 3.0 at % or more and 15.0 at % or less.

4. An electronic component as claimed in any one of claims 1 to 3, wherein the atomic percentage of the aluminum atoms and the atomic percentage of the oxygen atoms in each of the divided regions are both within a range of minus 5 at % and plus 5 at % of the atomic percentage of the same type of atoms in the entire specific region.

5. A method for forming an alumina film on the outer surface of an element, comprising: a loading step of loading the element into a first chamber capable of heating the atmosphere inside; a mist-forming step of using ultrasonic waves to convert a liquid raw material containing aluminum atoms and oxygen atoms into a mist in a second chamber; a supply step of supplying the mist-like raw material from the second chamber into the first chamber together with a carrier gas; and a heating step of heating the atmosphere in the first chamber while performing the supply step, wherein the raw material further contains one or more atoms selected from carbon atoms and hydrogen atoms.

6. The film forming method according to claim 5, wherein a composition ratio of atoms contained in the raw material is kept constant during the mist-forming step, the supplying step, and the heating step.

Citation Information

Patent Citations

  • Metallic oxide film resistor and its manufacture

    JP1997289101A

  • Ceramic element and manufacturing method of the same

    JP2003272906A