Resin composition and use thereof
The resin composition, featuring a combination of epoxy resin, surface-treated aluminum nitride, and alumina fillers, addresses the challenges of thermal conductivity and fluidity in multilayer printed wiring boards and component-embedded substrates, achieving high thermal conductivity and low linear expansion for improved performance.
Patent Information
- Application Number
- PCT/JP2024/013944
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-09-22
- Filing Date
- 2024-04-04
- Publication Date
- 2024-11-21
AI Technical Summary
Current resin compositions for multilayer printed wiring boards and component-embedded substrates face challenges in achieving high thermal conductivity, fluidity, and low linear expansion, with limitations in filler composition affecting their performance.
A resin composition comprising a combination of epoxy resin, surface-treated aluminum nitride filler, and alumina filler, with specific particle size and surface area ratios, and silane coupling agents, to enhance thermal conductivity and fluidity while reducing linear expansion.
The resin composition achieves high thermal conductivity, low linear expansion, and improved fluidity, enabling efficient production of multilayer printed wiring boards and component-embedded boards with enhanced heat dissipation and reliability.
Smart Images

Figure JPOXMLDOC01-APPB-T000001 
Figure JPOXMLDOC01-APPB-T000002 
Figure JPOXMLDOC01-APPB-T000003
Abstract
Description
Resin composition and its uses
[0001] The present invention relates to a resin composition and its use.
[0002] As electronic devices become more powerful and smaller, the wiring in multilayer printed wiring boards is becoming finer and denser. A known manufacturing technique for multilayer printed wiring boards is a build-up method in which insulating layers and conductor layers are alternately stacked. The insulating layer can be efficiently formed by using a film-like resin composition (resin composition film) for the insulating layer. A resin composition containing a thermosetting epoxy resin and silica is typically used as the resin composition film (Patent Document 1). The insulating layer is generally formed by overlaying the resin composition film on the conductor layer and thermally curing the resin composition while adhering the conductor layer and the resin composition using a vacuum laminator or a heat press.
[0003] Therefore, resin composition films are required to have high fluidity under lamination conditions in order to conform to the shape of the conductor layer, and it is common to use a combination of solid and liquid epoxy resins as epoxy resins. Furthermore, since the thermal linear expansion coefficients of the insulating layer and the conductor layer (copper wiring) are significantly different, there are reliability issues in multilayer printed wiring boards, such as cracks occurring during thermal cycling, and the insulating layer is also required to have low linear expansion. Therefore, resin composition films are generally highly filled with silica to reduce the linear expansion coefficient of the insulating layer.
[0004] As a high-density mounting method, electronic component-embedded substrate technology, in which electronic components, previously mounted on the surface of a substrate, are embedded inside the substrate using an encapsulating resin, is also attracting attention. Cavities are formed in the core of a resin substrate or copper substrate, and electronic components such as ICs and capacitors are placed in the cavities. The cavities are then filled with a thermosetting resin, thereby encapsulating and embedding the electronic components. The encapsulating resin can also be a resin composition film, such as that used in multilayer printed wiring boards. The resin composition film is layered on the core containing the electronic components, and the resin composition is embedded in the cavities using a heat press and thermally cured to achieve encapsulation (semi-additive method). Even when a resin composition is used in a component-embedded substrate, the resin composition must have high fluidity to fill the cavities, and the cured resin composition must have low linear expansion.
[0005] As a higher density mounting form, a module is also used in which a multilayer wiring layer is formed by the semi-additive method on the surface of a component-embedded substrate in which electronic components are embedded, and further electronic components are mounted on that surface.
[0006] Furthermore, in recent years, as electronic devices have become smaller and more powerful, the density and packaging of semiconductor elements in multilayer printed wiring boards and component-embedded boards has increased. As a result, the amount of heat generated by semiconductor elements has also increased, making it important to efficiently dissipate that heat from the board.
[0007] Therefore, in order to address these issues in the manufacture of multilayer printed wiring boards using the build-up method, it has been proposed to use a high-thermal conductivity resin composition that uses aluminum nitride, which has a higher thermal conductivity than silica, as the resin composition film (Patent Document 2). Specifically, Patent Document 2 proposes a resin composition that contains aluminum nitride or silicon nitride treated with a silane compound, an epoxy resin, and a curing agent, and in its examples, discloses a resin composition that exhibits a maximum thermal conductivity of 2.8 W / m·K.
[0008] JP 2011-132507 A International Publication No. 2014 / 208352
[0009] In view of the recent trend toward higher density and higher packaging of electronic devices, cured products made from resin compositions are required to have higher thermal conductivity. Furthermore, resin composition films used in multilayer printed wiring boards and component-embedded substrates are required to have not only high thermal conductivity but also high fluidity and low linear expansion.
[0010] However, increasing the filler filling rate in a resin composition to improve the thermal conductivity of the cured product may result in a decrease in the fluidity of the resin composition, and there are limitations to the composition of resin and filler. Therefore, conventional technologies have had limitations in achieving high thermal conductivity in resin compositions that can be used as resin composition films for producing multilayer printed wiring boards and component-embedded boards.
[0011] Therefore, an object of the present invention is to provide a resin composition that has high fluidity and, when cured, has low linear expansion and high thermal conductivity.
[0012] The resin composition of the present invention relates to, for example, the following [1] to
[13] : [1] A resin composition comprising: (A) an epoxy resin, (B) an aluminum nitride filler, and (C) an alumina filler, wherein the aluminum nitride filler (B) and the alumina filler (C) are contained in a total amount of 800 to 1,800 parts by mass per 100 parts by mass of the epoxy resin (A), the epoxy resin (A) comprises a solid epoxy resin (A-1) and a liquid epoxy resin (A-2), the aluminum nitride filler (B) has an average particle size D50 of 0.2 to 3 μm and a maximum particle size Dmax of 5 μm or less, and the alumina filler (C) has an average particle size D50 of 0.05 to 1.5 μm.
[0013] [2] The resin composition according to [1], wherein the aluminum nitride filler (B) is a surface-treated aluminum nitride filler that has been surface-treated with a silane coupling agent (SC1) having an organic reactive group containing an oxygen atom, a nitrogen atom, or a sulfur atom; the alumina filler (C) is a surface-treated alumina filler that has been surface-treated with a silane coupling agent (SC2) having an organic reactive group containing an oxygen atom, a nitrogen atom, or a sulfur atom, the organic reactive group being different from the organic reactive group possessed by the silane coupling agent (SC1); and the average particle size D50 of the aluminum nitride filler (B) is larger than the average particle size D50 of the alumina filler (C).
[0014] [3] The aluminum nitride filler (B) is a surface-treated aluminum nitride filler that has been surface-treated with a silane coupling agent (SC1) having an organic reactive group including a (meth)acrylic group, and the alumina filler (C) has an average particle size D50 (μm) and a specific surface area SA (m 2 The resin composition according to [2], wherein the alumina filler (C0) having a product of (A / g) and (B / g) of 2.6 or more is a surface-treated alumina filler that has been surface-treated with a silane coupling agent (SC2) having an organic reactive group containing an amino group with a secondary amine structure, which is different from the organic reactive group possessed by the silane coupling agent (SC1).
[0015] [4] In the alumina filler (C0), the average particle size D50 (μm) and the crystallite size L calculated from the half-width of the diffraction peak due to the (104) plane obtained by X-ray diffraction measurement 104 (μm) (D50 / L 104 ) is 6.0 or more. The resin composition according to [3].
[0016] [5] The alumina filler (C0) has a ratio (D90 / D10) of 90% particle diameter D90 to 10% particle diameter D10 calculated from a volume-based cumulative particle size distribution of 2.3 or less. The resin composition according to [3] or [4].
[0017] [6] The aluminum nitride filler (B) is a surface-treated aluminum nitride filler that has been surface-treated with a silane coupling agent (SC1) having an organic reactive group including an epoxy group, and the alumina filler (C) has an average particle size D50 (μm) and a specific surface area SA (m 2 The resin composition according to [2], wherein the alumina filler (C0) having a product of (A / g) and (B / g) of less than 2.6 is a surface-treated alumina filler that has been surface-treated with a silane coupling agent (SC2) having an organic reactive group containing an amino group with a secondary amine structure, which is different from the organic reactive group possessed by the silane coupling agent (SC1).
[0018] [7] In the alumina filler (C0), the average particle size D50 (μm) and the crystallite size L calculated from the half-width of the diffraction peak due to the (104) plane obtained by X-ray diffraction measurement 104 (μm) (D50 / L 104 ) is 6.0 or less. The resin composition according to [6].
[0019] [8] The resin composition according to any one of [2] to [7], wherein the silane coupling agent (SC2) has an organic reactive group containing a phenylamino group.
[0020] [9] The specific surface area SA of the aluminum nitride filler (B) is 0.5 to 10 m 2 / g, and the specific surface area SA of the alumina filler (C) is 1 to 50 m 2 / g. The resin composition according to any one of [1] to [8].
[0021]
[10] The resin composition according to any one of [1] to [9], wherein the ratio (S2 / S1) of the total surface area S1 of the aluminum nitride filler (B) to the total surface area S2 of the alumina filler (C) is 0.5 to 2.2.
[0022]
[11] A resin composition film comprising the resin composition according to any one of [1] to
[10] .
[0023]
[12] A multilayer printed wiring board comprising the resin composition according to any one of [1] to
[10] or a cured product thereof.
[0024]
[13] A component-embedded substrate comprising the resin composition according to any one of [1] to
[10] or a cured product thereof.
[0025] The resin composition of the present invention has high fluidity, and the cured product thereof has low linear expansion and high thermal conductivity. When the resin composition is formed into a film, it becomes possible to efficiently produce multilayer printed wiring boards and component-embedded boards with excellent heat dissipation performance.
[0026] Hereinafter, an example of an embodiment of the present invention will be described in detail. However, the present invention is not limited to the embodiment described below, and can be practiced with any modifications within the scope of the gist of the present invention. In this specification, "(meth)acrylic" represents both "acrylic" and "methacrylic", or either one of them.
[0027] A first resin composition of the present invention comprises (A) an epoxy resin, (B) an aluminum nitride filler, and (C) an alumina filler, wherein the aluminum nitride filler (B) and the alumina filler (C) are contained in a total amount of 800 to 1,800 parts by mass per 100 parts by mass of the epoxy resin (A), the epoxy resin (A) comprises a solid epoxy resin (A-1) and a liquid epoxy resin (A-2), the aluminum nitride filler (B) has an average particle size D50 of 0.2 to 3 μm and a maximum particle size Dmax of 5 μm or less, and the alumina filler (C) has an average particle size D50 of 0.05 to 1.5 μm.
[0028] A second resin composition of the present invention comprises (A) an epoxy resin, (B) an aluminum nitride filler, and (C) an alumina filler, wherein the aluminum nitride filler (B) and the alumina filler (C) are contained in a total amount of 800 to 1,800 parts by mass per 100 parts by mass of the epoxy resin (A), the epoxy resin (A) comprises a solid epoxy resin (A-1) and a liquid epoxy resin (A-2), and the aluminum nitride filler (B) is a surface-treated aluminum nitride filler that has been surface-treated with a silane coupling agent (SC1) having an organic reactive group containing an oxygen atom, a nitrogen atom, or a sulfur atom, and has an average particle size D50 of 0.2 to 3 μm and a maximum particle size Dmax of 5 μm or less, The resin composition is characterized in that the alumina filler (C) is a surface-treated alumina filler having an average particle size D50 of 0.05 to 1.5 μm, which has been surface-treated with a silane coupling agent (SC2) having an organic reactive group containing an oxygen atom, a nitrogen atom, or a sulfur atom, which is different from the organic reactive group possessed by the silane coupling agent (SC1); and the average particle size D50 of the aluminum nitride filler (B) is larger than the average particle size D50 of the alumina filler (C).
[0029] A third resin composition of the present invention comprises (A) an epoxy resin, (B) an aluminum nitride filler, and (C) an alumina filler, and the aluminum nitride filler (B) and the alumina filler (C) are contained in a total amount of 800 to 1,800 parts by mass per 100 parts by mass of the epoxy resin (A), the epoxy resin (A) comprises a solid epoxy resin (A-1) and a liquid epoxy resin (A-2), the aluminum nitride filler (B) is a surface-treated aluminum nitride filler that has been surface-treated with a silane coupling agent (SC1) having an organic reactive group including a (meth)acrylic group, and the alumina filler (C) has an average particle size D50 (μm) and a specific surface area SA (m 2alumina filler (C0) having a product of (A / g) and (B / g) of 2.6 or more is a surface-treated alumina filler that has been surface-treated with a silane coupling agent (SC2) having an organic reactive group containing an amino group with a secondary amine structure, the organic reactive group being different from the organic reactive group possessed by the silane coupling agent (SC1); and the average particle size D50 of the aluminum nitride filler (B) is larger than the average particle size D50 of the alumina filler (C).
[0030] A fourth resin composition of the present invention comprises (A) an epoxy resin, (B) an aluminum nitride filler, and (C) an alumina filler, and the aluminum nitride filler (B) and the alumina filler (C) are contained in a total amount of 800 to 1,800 parts by mass per 100 parts by mass of the epoxy resin (A), the epoxy resin (A) comprises a solid epoxy resin (A-1) and a liquid epoxy resin (A-2), the aluminum nitride filler (B) is a surface-treated aluminum nitride filler that has been surface-treated with a silane coupling agent (SC1) having an organic reactive group containing an epoxy group, and the alumina filler (C) has an average particle size D50 (μm) and a specific surface area SA (m 2 alumina filler (C0) having a product of (A / g) and (B / g) of less than 2.6 is a surface-treated alumina filler that has been surface-treated with a silane coupling agent (SC2) having an organic reactive group containing an amino group with a secondary amine structure, the organic reactive group being different from the organic reactive group possessed by the silane coupling agent (SC1); and the average particle size D50 of the aluminum nitride filler (B) is larger than the average particle size D50 of the alumina filler (C).
[0031] [Epoxy Resin (A)] The resin composition of the present invention contains an epoxy resin (A). The epoxy resin (A) preferably contains a compound containing one or more epoxy groups in the molecule (hereinafter, also referred to as a "reactive epoxy resin"). The reactive epoxy resin may be a low molecular weight compound having an epoxy group. The reactive epoxy resin more preferably contains two or more epoxy groups in the molecule.
[0032] The epoxy resin (A) preferably contains a reactive epoxy resin in an amount of 50% by mass or more based on the total amount of the epoxy resin (A). The inclusion of a reactive epoxy resin in the epoxy resin (A) tends to soften the resin composition and improve its fluidity. Therefore, when the resin composition is used as a resin composition film for producing a multilayer printed wiring board or a component-embedded substrate, the resin composition easily conforms to the shape of the conductor layer of the multilayer printed wiring board, the cavity of the component-embedded substrate, and the electronic component. Furthermore, the cured product obtained by heat-curing the resin composition after converting it into a desired shape exhibits high strength and heat resistance, thereby improving the reliability of the substrate, etc. The upper limit of the content of the reactive epoxy resin in the total amount of the epoxy resin (A) is not particularly limited, and the entire epoxy resin (A) may be a reactive epoxy resin.
[0033] The epoxy resin (A) includes a solid epoxy resin (A-1) and a liquid epoxy resin (A-2). In this specification, an epoxy resin that is solid at a temperature of 25°C is referred to as a solid epoxy resin (A-1), and an epoxy resin that is liquid at 25°C is referred to as a liquid epoxy resin (A-2).
[0034] When the epoxy resin (A) contains the solid epoxy resin (A-1), the strength and heat resistance of the cured product obtained by heat-curing the resin composition tend to be improved. On the other hand, since the melt viscosity of the solid epoxy resin (A-1) tends to be high, when the highly heat-resistant solid epoxy resin (A-1) is used in combination with the highly fluid liquid epoxy resin (A-2), the fluidity of the resin composition is improved, and the resin composition can conform to the desired substrate shape.
[0035] The solid epoxy resin (A-1) is preferably a reactive epoxy resin. Examples of the solid epoxy resin (A-1) include tetrafunctional naphthalene epoxy resins, trifunctional naphthalene epoxy resins, trisphenolmethane epoxy resins, phenol novolac epoxy resins, cresol novolac epoxy resins, bisphenol A novolac epoxy resins, naphthol novolac epoxy resins, naphthol cresol novolac epoxy resins, dicyclopentadiene epoxy resins, biphenyl aralkyl epoxy resins, bixylenol epoxy resins, naphthylene ether epoxy resins, biphenyl epoxy resins, and fluorene epoxy resins, and more preferred are tetrafunctional naphthalene epoxy resins, biphenyl aralkyl epoxy resins, trisphenolmethane epoxy resins, bixylenol epoxy resins, naphthylene ether epoxy resins, and fluorene epoxy resins.
[0036] Commercially available tetrafunctional naphthalene epoxy resins include, for example, "HP-4700" and "HP-4710" manufactured by DIC Corporation. Commercially available cresol novolac epoxy resins include, for example, "N-690" and "N-695" manufactured by DIC Corporation. Commercially available dicyclopentadiene epoxy resins include, for example, "HP-7200," "HP-7200L," and "HP-7200H" manufactured by DIC Corporation. Commercially available naphthylene ether epoxy resins include, for example, "HP-6000" and "HP-6000H" manufactured by DIC Corporation.
[0037] Commercially available trisphenolmethane epoxy resins include "EPPN-501H," "EPPN-501HY," and "EPPN-502H" manufactured by Nippon Kayaku Co., Ltd. Commercially available naphthol cresol novolac epoxy resins include "NC-7000L," "NC-7000H," and "NC-7300L" manufactured by Nippon Kayaku Co., Ltd. Commercially available biphenylaralkyl epoxy resins include "NC-3000H," "NC-3000," "NC-3000L," "NC-3100," and "NC-3500" manufactured by Nippon Kayaku Co., Ltd.
[0038] Commercially available naphthol novolac epoxy resins include, for example, "ESN475" and "ESN485" manufactured by Nippon Steel Chemical Co., Ltd. Commercially available biphenyl epoxy resins include, for example, "YX4000H" and "YL6121" manufactured by Mitsubishi Chemical Corporation Commercially available bixylenol epoxy resins include, for example, "YX4000HK" manufactured by Mitsubishi Chemical Corporation Commercially available fluorene epoxy resins include, for example, "YL7800" manufactured by Mitsubishi Chemical Corporation
[0039] From the viewpoint of moldability of the resin composition, the softening point of the solid epoxy resin (A-1) is preferably 40 to 130° C. The softening point is more preferably 45° C. or higher, even more preferably 50° C. or higher, and more preferably 110° C. or lower, even more preferably 100° C. or lower. The solid epoxy resin (A-1) may be used alone or in combination of two or more.
[0040] When producing the resin composition, the solid epoxy resin (A-1) may be used as a composition containing the solid epoxy resin (A-1) and an organic solvent. The organic solvent in the composition may be any solvent capable of dissolving the solid epoxy resin (A-1). Examples include acetone, methanol, ethanol, butanol, 2-propanol, 2-methoxyethanol, 2-ethoxyethanol, 1-methoxy-2-propanol, 2-acetoxy-1-methoxypropane, toluene, xylene, methyl ethyl ketone, N,N-dimethylformamide, methyl isobutyl ketone, N-methylpyrrolidone, n-hexane, cyclohexane, cyclohexanone, and solvent naphtha, which is a mixture thereof. Methyl ethyl ketone is preferred. From the viewpoint of ease of removal of the organic solvent, the boiling point of the organic solvent is preferably 200°C or lower, more preferably 180°C or lower. One organic solvent may be used alone, or two or more organic solvents may be used.
[0041] The content of nonvolatile matter in the composition is preferably 20 to 90 mass%, more preferably 30 to 80 mass%, and even more preferably 40 to 70 mass%, from the viewpoint of solubility of the solid epoxy resin (A-1) in the organic solvent. In this specification, the term "nonvolatile matter" refers to all components excluding the solvent. The content of the organic solvent in the composition is preferably 10 to 80 mass%, more preferably 20 to 70 mass%, and even more preferably 30 to 60 mass%. The composition may contain components other than the epoxy resin (A), aluminum nitride filler (B), and alumina filler (C) that may be contained in the resin composition.
[0042] When the epoxy resin (A) contains the liquid epoxy resin (A-2), the melt viscosity of the resin composition can be kept low, and the resin composition tends to have excellent flowability. Therefore, when a film made of the resin composition is molded under heat and pressure for use in a multilayer printed wiring board or a component-embedded board, the film made of the resin composition has excellent conformability to the shapes of the conductor layer and the cavity.
[0043] The liquid epoxy resin (A-2) is preferably a reactive epoxy resin, and examples of the liquid epoxy resin (A-2) include bisphenol A epoxy resin, bisphenol F epoxy resin, phenol novolac epoxy resin, and naphthalene epoxy resin, and more preferably bisphenol A epoxy resin and bisphenol F epoxy resin.
[0044] Commercially available bisphenol A epoxy resins include, for example, "jER828," "jER828EL," and "jER828US" manufactured by Mitsubishi Chemical Corporation. Commercially available bisphenol F epoxy resins include, for example, "jER806," "jER806H," and "jER807" manufactured by Mitsubishi Chemical Corporation, and "YDF-8170C" manufactured by Nippon Steel Chemical & Material Co., Ltd. Commercially available phenol novolac epoxy resins include, for example, "jER152" manufactured by Mitsubishi Chemical Corporation.
[0045] An example of a commercially available mixture of bisphenol A epoxy resin and bisphenol F epoxy resin is "ZX1059" manufactured by Nippon Steel Chemical & Material Co., Ltd. An example of a commercially available naphthalene epoxy resin is "HP4032," "HP4032D," and "HP4032SS" manufactured by DIC Corporation. The liquid epoxy resin (A-2) may be used alone or in combination of two or more types.
[0046] The viscosity of the liquid epoxy resin (A-2) at 25° C. is preferably 500 poise or less, more preferably 300 poise or less, and even more preferably 200 poise or less, and is preferably 5 poise or more, and more preferably 10 poise or more. When the viscosity of the liquid epoxy resin (A-2) at 25° C. is within the above range, the melt viscosity of the resin composition can be kept low, and the resin composition tends to have excellent flowability.
[0047] The ratio of the content of the solid epoxy resin (A-1) to the content of the liquid epoxy resin (A-2) (solid epoxy resin:liquid epoxy resin) is preferably in the range of 9:1 to 1:9, more preferably 4:1 to 1:4, even more preferably 3:1 to 1:3, and particularly preferably 2:1 to 1:2. By setting the content ratio of the solid epoxy resin (A-1) to the liquid epoxy resin (A-2) within the above range, it is possible to achieve both high fluidity of the resin composition and high heat resistance of the cured product.
[0048] The epoxy equivalent of the epoxy resin (A) is preferably 50 to 4500, more preferably 50 to 3000. The epoxy equivalent is further preferably 80 or more, particularly preferably 100 or more, and further preferably 2000 or less, particularly preferably 1000 or less. When the epoxy equivalent of the epoxy resin (A) is within the above range, the cured product obtained by curing the resin composition tends to have excellent crosslink density, and when the resin composition is used as a film, it tends to have sufficient heat resistance and mechanical strength. The epoxy equivalent can be measured according to JIS K7236. The epoxy equivalent is the mass of resin per equivalent of epoxy groups.
[0049] [Aluminum Nitride Filler (B)] The resin composition contains aluminum nitride filler (B). When the resin composition contains aluminum nitride filler (B), the cured product of the resin composition can have high thermal conductivity. The average particle size D50 of the aluminum nitride filler (B) is 0.2 to 3 μm. The average particle size D50 is preferably 0.3 μm or more, more preferably 0.5 μm or more, and preferably 2 μm or less, more preferably 1.5 μm or less. When the average particle size D50 of the aluminum nitride filler (B) is within the above range, the resin composition can be easily molded into a film having a thickness of several μm to several hundred μm, and cured products made of films having a thickness within the above range tend to have high thermal conductivity. The average particle size D50 in the present invention is the particle size at the cumulative 50% value on a volume basis in the particle size distribution measured by laser diffraction scattering. The particle size distribution can be measured by the method described in the Examples section below.
[0050] The maximum particle size Dmax of the aluminum nitride filler (B) is 5 μm or less, preferably 4.5 μm or less, and more preferably 4 μm or less. When the maximum particle size Dmax of the aluminum nitride filler (B) is within this range, the melt viscosity of the resin composition tends to decrease. Therefore, when a film made of the resin composition is heated and pressurized to be used in a multilayer printed wiring board or a component-embedded board, the film made of the resin composition has excellent conformability to the shapes of the conductor layer and the cavity.
[0051] The maximum particle size Dmax in the present invention is the maximum particle size (particle size at 100% cumulative volume) measured in the particle size distribution measured by a laser diffraction scattering method. The particle size distribution can be measured by the method described in the Examples section below.
[0052] The specific surface area SA of the aluminum nitride filler (B) is preferably 0.5 to 10 m 2 The specific surface area SA is more preferably 0.8 m 2 / g or more, more preferably 1.0m 2 / g or more, more preferably 7m 2 / g or less, more preferably 5m 2 / g or less. When the specific surface area SA of the aluminum nitride filler (B) is within the above range, the aluminum nitride filler (B) has excellent dispersibility in the epoxy resin (A), and the melt viscosity of the resin composition tends to be reduced. The specific surface area SA in the present invention can be measured by the BET method using a flow-type automatic specific surface area measuring device. The specific surface area SA can be measured by the method described in the Examples section below.
[0053] The aluminum nitride filler (B) may be an aluminum nitride filler that has not been surface-treated with a surface treatment agent, or may be an aluminum nitride filler that has been surface-treated with a surface treatment agent.
[0054] An example of a commercially available aluminum nitride filler that has not been surface-treated with a surface treatment agent is aluminum nitride filler HF-01D (manufactured by Tokuyama Corporation). As the aluminum nitride filler, commercially available aluminum nitride powder may be used after adjusting the particle size distribution using a sieve, a classifier, or the like. There are no particular restrictions on the method for producing the aluminum nitride filler that has not been surface-treated with a surface treatment agent, and aluminum nitride fillers produced by known methods can be used. Examples of methods for producing the aluminum nitride filler include direct nitridation, reduction nitridation, and vapor phase synthesis.
[0055] The aluminum nitride filler (B) may be an aluminum nitride filler that has been surface-treated with a surface treatment agent. Surface treatment with a surface treatment agent improves the water resistance of the aluminum nitride filler and enhances its affinity with the epoxy resin (A). This improves the filling ability of the aluminum nitride filler, and facilitates the improvement of the flowability of the resin composition. Examples of the surface treatment agent include silane compounds such as silane coupling agents, aluminate coupling agents, and titanate coupling agents. The surface treatment agent is preferably a silane compound, as it can increase the reactivity between the surface treatment agent and the aluminum nitride filler.
[0056] Examples of the silane compound used as the surface treatment agent include silane compounds having a reactive functional group and silane compounds having a non-reactive functional group. Examples of the silane compound having a reactive functional group include 3-glycidoxypropyltrimethoxysilane, 3-glycidoxypropyltriethoxysilane, 3-glycidoxypropylmethyldimethoxysilane, 3-glycidoxypropylmethyldiethoxysilane, 2-(3,4-epoxycyclohexyl)ethyltrimethoxysilane, 3-methacryloxypropyltrimethoxysilane, 3-methacryloxypropyltriethoxysilane, 3-methacryloxypropylmethyldimethoxysilane, 3-methacryloxypropylmethyldiethoxysilane, 3-acryloxypropyltrimethoxysilane, 3-mercaptopropyltrimethoxysilane, and the like. Silanes include alkoxysilanes such as 3-aminopropyltrimethoxysilane, 3-aminopropyltriethoxysilane, 2-aminoethyl-3-aminopropyltrimethoxysilane, 2-aminoethyl-3-aminopropylmethyldimethoxysilane, 3-dimethylaminopropyltrimethoxysilane, 3-diethylaminopropyltrimethoxysilane, 3-triethoxysilyl-N-(1,3-dimethyl-butylidene)propylamine, N-phenyl-3-aminopropyltrimethoxysilane, vinyltrimethoxysilane, vinyltriethoxysilane, p-styryltrimethoxysilane, and allyltrimethoxysilane.
[0057] Examples of silane compounds having a non-reactive functional group include methyltrimethoxysilane, dimethyldimethoxysilane, dimethyldiethoxysilane, trimethylmethoxysilane, ethyltrimethoxysilane, n-propyltrimethoxysilane, isobutyltrimethoxysilane, isobutyltriethoxysilane, n-hexyltrimethoxysilane, n-hexyltriethoxysilane, cyclohexyltrimethoxysilane, cyclohexylmethyldimethoxysilane, n-octyltriethoxysilane, phenyltrimethoxysilane, phenyltriethoxysilane, diphenyldimethoxysilane, diphenyldiethoxysilane, trifluoropropyltrimethoxysilane, and trifluoropropylmethyldimethoxysilane.
[0058] In addition to the above compounds, examples of silane compounds that can be used as the surface treatment agent include chlorosilanes such as vinyltrichlorosilane, methyltrichlorosilane, dimethyldichlorosilane, trichloromethylsilane, ethyldimethylchlorosilane, propyldimethylchlorosilane, phenyltrichlorosilane, trifluoropropyltrichlorosilane, and isopropyldiethylchlorosilane.
[0059] Among the silane compounds, those having high affinity with the epoxy resin (A) are preferred, and examples of silane compounds having high affinity include silane compounds having functional groups capable of reacting with epoxy groups, such as glycidoxy groups and amino groups.Furthermore, although their reactivity with epoxy groups is low, functional groups such as methacryloxy groups, acryloxy groups, phenyl groups, vinyl groups, and styryl groups also have high affinity with epoxy resins, and silane compounds having these functional groups are also suitable.
[0060] The surface treatment agent is preferably a silane coupling agent having an organic reactive group containing an oxygen atom, a nitrogen atom, or a sulfur atom, among the silane compounds. That is, the aluminum nitride filler (B) is preferably an aluminum nitride filler surface-treated with a silane coupling agent (SC1) having an organic reactive group containing an oxygen atom, a nitrogen atom, or a sulfur atom.
[0061] An aluminum nitride filler that has not been surface-treated with a silane coupling agent is also called an “untreated aluminum nitride filler,” and an aluminum nitride filler that has been surface-treated with a silane coupling agent (SC1) is also called a “surface-treated aluminum nitride filler.” Aluminum nitride fillers before being surface-treated with a silane coupling agent (SC1) are usually not surface-treated with a silane coupling agent.
[0062] The untreated aluminum nitride filler need not have been subjected to a surface treatment with a silane coupling agent, and may have been subjected to a water-resistant treatment that oxidizes the filler surface.
[0063] The silane coupling agent (SC1) is a silane compound having a hydrolyzable group and an organic reactive group containing an oxygen atom, a nitrogen atom, or a sulfur atom, and is preferably an alkoxysilane compound having an organic reactive group containing an oxygen atom, a nitrogen atom, or a sulfur atom.
[0064] The hydrolyzable group is directly bonded to the silicon atom. Examples of the hydrolyzable group include alkoxy groups such as methoxy and ethoxy groups. An organic reactive group containing an oxygen atom, nitrogen atom, or sulfur atom refers to a substituent other than a hydrolyzable group that contains a reactive functional group containing an oxygen atom, nitrogen atom, or sulfur atom and is bonded to a silicon atom. The reactive functional group containing an oxygen atom, nitrogen atom, or sulfur atom is preferably bonded to the silicon atom via a linear, branched, or cyclic alkylene group having 1 to 10 carbon atoms.
[0065] Examples of reactive functional groups containing an oxygen atom include a hydroxyl group, a carbonyl group, and an ether group bonded to two carbon atoms (-C-O-C- bond). The ether group bonded to two carbon atoms may be a cyclic ether group. Preferred reactive functional groups containing an oxygen atom include an epoxy group and a (meth)acrylic group.
[0066] Examples of reactive functional groups containing a nitrogen atom include -NR 1 R 2Examples of the R include an amino group, a cyano group, a pyrrolidinyl group, and an isocyanate group. 1 and R 2 R each independently represents a hydrogen atom, an alkyl group, or an aryl group. 1 and R 2 The number of carbon atoms in the alkyl group represented by R is preferably 1 to 30, more preferably 1 to 20, and even more preferably 1 to 10. The alkyl group may be linear, branched, or cyclic. 1 and R 2 The number of carbon atoms in the aryl group represented by is preferably 6 to 30, more preferably 6 to 20, and even more preferably 6 to 10. As the reactive functional group containing a nitrogen atom, an amino group having a secondary amine structure is preferred, and a methylamino group and a phenylamino group are more preferred.
[0067] Examples of the reactive functional group containing a sulfur atom include a mercapto group, a sulfide group, a sulfo group, and a sulfonyl group. Of the reactive functional groups containing a sulfur atom, a mercapto group is preferred.
[0068] The silane coupling agent (SC1) may have only one organic reactive group or two or more organic reactive groups. The organic reactive group may include, for example, a reactive functional group containing an oxygen atom and a reactive functional group containing a nitrogen atom.
[0069] Examples of the silane coupling agent (SC1) include 2-((3-(triethoxysilyl)propyl)carbamoyl)benzoic acid, triethoxysilylpropylmaleamic acid, 2-((3-(trimethoxysilyl)propyl)carbamoyl)benzoic acid, trimethoxysilylpropylmaleamic acid, 3-glycidoxypropyltrimethoxysilane, 3-glycidoxypropyltriethoxysilane, 3-glycidoxypropylmethyldimethoxysilane, 3-glycidoxypropylmethyldiethoxysilane, 2-(3,4-epoxycyclohexyl)ethyltrimethoxysilane, 3-methacryloxypropyltrimethoxysilane, 3-methacryloxypropyltriethoxysilane, 3-methacryloxypropylmethyldimethoxysilane, 3-methacryloxypropylmethyldiethoxysilane, 3-acryloxypropyltrimethoxysilane amine, 3-mercaptopropyltrimethoxysilane, 3-aminopropyltrimethoxysilane, 3-aminopropyltriethoxysilane, 2-aminoethyl-3-aminopropyltrimethoxysilane, 2-aminoethyl-3-aminopropylmethyldimethoxysilane, 3-dimethylaminopropyltrimethoxysilane, 3-diethylaminopropyltrimethoxysilane, 3-triethoxysilyl-N-(1,3-dimethyl-butylidene)propylamine, N-phenyl-3-aminopropyltrimethoxysilane, N-(vinylbenzyl)-2-aminoethyl-3-aminopropyltrimethoxysilane hydrochloride, tris-(trimethoxysilylpropyl)isocyanurate, 3-ureidopropyltriethoxysilane, 3-mercaptopropylmethyldimethoxysilane, and 3-(methylamino)propyltrimethoxysilane.
[0070] When the silane coupling agent (SC2) described later has an organic reactive group containing an amino group of a secondary amine structure, the silane coupling agent (SC1) preferably does not have an organic reactive group containing an amino group of a secondary amine structure.
[0071] The amount of the surface treatment agent used when surface treating an aluminum nitride filler with the surface treatment agent is preferably 0.1 to 5 parts by mass, more preferably 0.5 to 4 parts by mass, per 100 parts by mass of the aluminum nitride filler before surface treatment.
[0072] The surface treatment method using the surface treatment agent can be a known method, and may be either a dry surface treatment or a wet surface treatment. Dry surface treatment is a method in which the aluminum nitride filler before surface treatment is mixed with the surface treatment agent without using a large amount of solvent. Examples of dry surface treatment include a method in which the surface treatment agent is gasified and mixed with the aluminum nitride filler before surface treatment, a method in which the liquid surface treatment agent is sprayed or dropped and mixed with the aluminum nitride filler before surface treatment, and a method in which the surface treatment agent is diluted with a small amount of organic solvent to increase the amount of liquid, and then sprayed or dropped.
[0073] Wet surface treatment is a method in which a solvent is used when mixing an aluminum nitride filler before surface treatment with the surface treatment agent. For example, an example of the wet surface treatment is a method in which an aluminum nitride filler before surface treatment, the surface treatment agent, and a solvent are mixed together, and then the solvent is removed by drying or the like.
[0074] The aluminum nitride filler (B) may contain impurities such as alkaline earth elements and rare earth elements derived from raw materials or intentionally added during the synthesis process, with the upper limit being approximately 5 parts by mass per 100 parts by mass of the aluminum nitride filler (B). An amount of impurities that significantly reduces the crystallinity of aluminum nitride is undesirable because it causes a decrease in the thermal conductivity of the cured product made from the resin composition. The aluminum nitride content in the aluminum nitride filler (B) is preferably 95% by mass or more, more preferably 99% by mass or more. The aluminum nitride filler (B) may be one type or two or more types.
[0075] [Alumina Filler (C)] The resin composition contains alumina filler (C). The average particle size D50 of the alumina filler (C) is 0.05 to 1.5 μm. The average particle size D50 is preferably 0.1 μm or more, more preferably 0.15 μm or more, and preferably 1.0 μm or less, more preferably 0.8 μm or less. The average particle size D50 of the aluminum nitride filler (B) is preferably larger than the average particle size D50 of the alumina filler (C). When the average particle size D50 of the aluminum nitride filler (B) is larger than the average particle size D50 of the alumina filler (C), the alumina filler (C) penetrates into the gaps between the aluminum nitride fillers (B) in the resin composition. Therefore, even if the filling rates of the aluminum nitride filler (B) and the alumina filler (C) are increased, the fluidity of the resin composition tends not to decrease excessively. Furthermore, the contact area of the thermally conductive particles increases, which tends to improve the thermal conductivity of the cured product made of the resin composition. Furthermore, when the average particle size D50 of the alumina filler (C) is within the above range, the resin composition can be easily formed into a film having a thickness of about several μm to several hundred μm, and a cured product made of a film having a thickness within the above range tends to have high thermal conductivity.
[0076] The ratio of the average particle size D50 of the alumina filler (C) to the average particle size D50 of the aluminum nitride filler (B) (average particle size D50 of alumina filler (C) / average particle size D50 of aluminum nitride filler (B)) is preferably 0.02 to 0.9. The ratio is more preferably 0.05 or more, even more preferably 0.10 or more, and more preferably 0.8 or less, even more preferably 0.7 or less. When the ratio of average particle sizes D50 is within the above range, the aluminum nitride filler (B) and the alumina filler (C) have excellent fillability into the resin composition, and the melt viscosity of the resin composition tends to decrease.
[0077] The maximum particle size Dmax of the alumina filler (C) is preferably 5 μm or less, more preferably 4 μm or less, and even more preferably 3 μm or less. The specific surface area SA of the alumina filler (C) is preferably 1 to 50 m 2 The specific surface area SA is more preferably 1.5 m2 / g or more, more preferably 2m 2 / g or more, more preferably 30m 2 / g or less, more preferably 20m 2 The alumina filler (C) having a specific surface area SA within the above range has excellent dispersibility in the resin composition, and the melt viscosity of the resin composition tends to be reduced.
[0078] The higher the crystallinity of the alumina filler (C), the more preferable, and the higher the proportion of alpha crystals in the crystal system, the more preferable. The higher the crystallinity of the alumina filler (C), the more the thermal conductivity of the cured product made of the resin composition tends to improve. The crystallinity of the alumina filler (C) can be confirmed by X-ray diffraction.
[0079] The alumina filler (C) may be an alumina filler that has not been surface-treated with a surface treatment agent, or may be an alumina filler that has been surface-treated with a surface treatment agent. Surface treatment with a surface treatment agent can be performed by a known method, and may be performed by either a dry surface treatment or a wet surface treatment method. Examples of the surface treatment agent include silane compounds such as silane coupling agents, aluminate coupling agents, and titanate coupling agents. Examples of the silane compound include compounds similar to the silane compounds that can be used for the surface treatment of the aluminum nitride filler (B). The surface treatment agent is preferably a silane compound, more preferably a silane coupling agent. The amount of the surface treatment agent used when performing the surface treatment with the surface treatment agent is preferably 0.1 to 5 parts by mass, more preferably 0.5 to 4 parts by mass, per 100 parts by mass of the alumina filler before surface treatment.
[0080] An alumina filler that has not been surface-treated with a silane coupling agent is also referred to as an “untreated alumina filler.” Commercially available untreated alumina fillers include, for example, Advanced Alumina AA-03F (manufactured by Sumitomo Chemical Co., Ltd.), Advanced Alumina AA-04 (manufactured by Sumitomo Chemical Co., Ltd.), NXA-150 (manufactured by Sumitomo Chemical Co., Ltd.), spherical alumina ASFP-20 (manufactured by Denka Co., Ltd.), and AHPA-0.5AF (manufactured by Sasol).
[0081] An alumina filler that has not been surface-treated with a silane coupling agent is also referred to as "alumina filler (C0)." The 10% particle size D10 of the alumina filler (C0) is preferably 0.02 to 1.0 μm. The D10 is more preferably 0.05 μm or more, even more preferably 0.1 μm or more, and more preferably 0.9 μm or less, and even more preferably 0.7 μm or less. The average particle size D50 of the alumina filler (C0) is preferably 0.05 to 1.5 μm. The D50 is more preferably 0.1 μm or more, even more preferably 0.15 μm or more, and more preferably 1.0 μm or less, and even more preferably 0.8 μm or less. The 90% particle size D90 of the alumina filler (C0) is preferably 0.1 to 2.0 μm. The D90 is more preferably 0.2 μm or more, even more preferably 0.3 μm or more, and more preferably 1.5 μm or less, even more preferably 1.0 μm or less.
[0082] The 10% particle diameter D10 in the present invention is the particle diameter at the 10% cumulative volume value in the particle size distribution measured by the laser diffraction scattering method. The 90% particle diameter D90 in the present invention is the particle diameter at the 90% cumulative volume value in the particle size distribution measured by the laser diffraction scattering method. The particle size distribution can be measured by the method described in the Examples section below.
[0083] The specific surface area SA of the alumina filler (C0) is preferably 1 to 50 m 2 The specific surface area SA is more preferably 1.5 m 2 / g or more, more preferably 2m 2 / g or more, more preferably 30m 2 / g or less, more preferably 20m 2 / g or less.
[0084] <Second Resin Composition> In the second resin composition, the aluminum nitride filler (B) is an aluminum nitride filler surface-treated with a silane coupling agent (SC1) having an organic reactive group containing an oxygen atom, a nitrogen atom, or a sulfur atom, and the alumina filler (C) is an alumina filler surface-treated with a silane coupling agent (SC2) having an organic reactive group containing an oxygen atom, a nitrogen atom, or a sulfur atom. The organic reactive group of the silane coupling agent (SC2) is different from the organic reactive group of the silane coupling agent (SC1). That is, the silane coupling agent (SC2) is a silane coupling agent having an organic reactive group containing an oxygen atom, a nitrogen atom, or a sulfur atom, which is different from the organic reactive group of the silane coupling agent (SC1).
[0085] The second resin composition tends to have better dispersibility of the aluminum nitride filler (B) and the alumina filler (C) and higher fluidity than the first resin composition, and the cured product of the second resin composition tends to have higher thermal conductivity than the cured product of the first resin composition.
[0086] The alumina filler that has been surface-treated with the silane coupling agent (SC2) is also called a “surface-treated alumina filler.” The alumina filler before being surface-treated with the silane coupling agent (SC2) is usually not surface-treated with a silane coupling agent.
[0087] Silane coupling agent (SC2) can be the same silane coupling agent as silane coupling agent (SC1).Silane coupling agent (SC2) is preferably the silane coupling agent that has the organic reactive group that contains oxygen atom or nitrogen atom, more preferably the silane coupling agent that has the organic reactive group that contains epoxy group, (meth)acrylic group or the amino group of secondary amine structure, and further preferably the silane coupling agent that has the organic reactive group that contains (meth)acrylic group, methylamino group or phenylamino group.
[0088] In the past, adjusting the particle size distribution of the filler has been considered to improve the thermal conductivity of a cured resin composition and the fluidity of the resin composition. However, adjusting the particle size distribution of the filler can reduce the dispersibility of the filler, which can result in poor appearance of the resin composition film. To improve the poor appearance, additional kneading using a three-roll mill or the like is required when producing the resin composition. Since low filler dispersibility can increase the number of production steps, it is desirable that the filler used in the resin composition film has high dispersibility from the perspectives of equipment, labor hours, and production costs. The second resin composition has excellent dispersibility of the aluminum nitride filler (B) and the alumina filler (C). The following reasons are thought to be the reasons for this excellent dispersibility. In the second resin composition, the alumina filler (C) has a small particle size and a large specific surface area, which significantly affects the interaction between the filler and the epoxy resin (A). Furthermore, in the second resin composition, the alumina filler (C) is surface-treated with a silane coupling agent (SC2) having an organic reactive group containing an oxygen atom, a nitrogen atom, or a sulfur atom, and it is presumed that the affinity between the alumina filler (C) and the epoxy resin (A) is improved, thereby improving the dispersibility of the filler in the resin composition.
[0089] The dispersibility of the filler is related not only to the interaction between the epoxy resin (A) and the filler, but also to the interaction between the fillers themselves. When untreated aluminum nitride filler and untreated alumina filler are surface-treated with a silane coupling agent having the same organic reactive group, the dispersibility of the filler may be reduced due to the interaction between the silane coupling agents. On the other hand, when untreated aluminum nitride filler and untreated alumina filler are surface-treated with silane coupling agents having different organic reactive groups, the interaction between the silane coupling agents in the aluminum nitride filler (B) and the alumina filler (C) can be alleviated. As a result, it is presumed that the filling ability of the filler can be improved, thereby reducing the melt viscosity of the resin composition, and that the adhesion between the epoxy resin (A) and the filler can be increased, thereby improving the thermal conductivity of the cured product made of the resin composition.
[0090] The combination of the silane coupling agent (SC1) and the silane coupling agent (SC2) in the second resin composition is preferably a combination in which the silane coupling agent (SC1) has an organic reactive group containing at least one reactive functional group selected from the group consisting of a (meth)acrylic group, a phenylamino group, and an epoxy group, and the silane coupling agent (SC2) has an organic reactive group containing at least one reactive functional group selected from the group consisting of a (meth)acrylic group, a phenylamino group, and a methylamino group (however, excluding combinations in which the organic reactive groups in the silane coupling agent (SC1) and the silane coupling agent (SC2) both contain a (meth)acrylic group, a phenylamino group, a methylamino group, or an epoxy group), and more preferably a combination in which the silane coupling agent (SC1) has a methacryl group, and the silane coupling agent (SC2) has a phenylamino group, a combination in which the silane coupling agent (SC1) has a phenylamino group, and the silane coupling agent (SC2) has a methacryl group, a combination in which the silane coupling agent (SC1) has an acrylic group and the silane coupling agent (SC2) has a phenylamino group; a combination in which the silane coupling agent (SC1) has an epoxy group and the silane coupling agent (SC2) has a phenylamino group; a combination in which the silane coupling agent (SC1) has an epoxy group and the silane coupling agent (SC2) has a methacryl group; or a combination in which the silane coupling agent (SC1) has a methacryl group and the silane coupling agent (SC2) has a methylamino group.
[0091] <Third Resin Composition> In the third resin composition, the aluminum nitride filler (B) is an aluminum nitride filler that has been surface-treated with a silane coupling agent (SC1) having an organic reactive group including a (meth)acrylic group, and the alumina filler (C) has an average particle size D50 (μm) and a specific surface area SA (m 2The alumina filler (C0) having a product of (A / g) and (B / g) of 2.6 or more is surface-treated with a silane coupling agent (SC2) having an organic reactive group containing an amino group with a secondary amine structure, which is different from the organic reactive group possessed by the silane coupling agent (SC1). The third resin composition tends to have particularly high fluidity compared to the first resin composition.
[0092] The crystallite size L of the alumina filler (C0) used in the third resin composition 104 is preferably 20 to 120 nm. 104 is more preferably 30 nm or more, even more preferably 40 nm or more, particularly preferably 50 nm or more, and more preferably 100 nm or less, even more preferably 80 nm or less, particularly preferably 68 nm or less. 104 is calculated based on the half-width of the diffraction peak due to the (104) plane obtained from X-ray diffraction measurement by the method described in the Examples section below.
[0093] The average particle diameter D50 (μm) and specific surface area SA (m 2 / g) is preferably 2.6 or more, more preferably 2.7 or more, even more preferably 2.8 or more, and is preferably 10 or less.
[0094] The average particle size D50 (μm) and the crystallite size L of the alumina filler (C0) used in the third resin composition 104 (μm) (D50 / L 104 ) is preferably 6.0 or more, more preferably 6.2 or more, and even more preferably 6.4 or more. 104 There is no particular upper limit to the value, but it is generally 20 or less.
[0095] The ratio (D90 / D10) of the 90% particle diameter D90 to the 10% particle diameter D10 of the alumina filler (C0) used in the third resin composition is preferably 2.3 or less, more preferably 2.1 or less, and even more preferably 2.0 or less. The lower limit of D90 / D10 is not particularly limited as long as it is 1 or more, which is the theoretical minimum value.
[0096] An example of a commercially available alumina filler (C0) having physical property values within the above range is AHPA-0.5AF (manufactured by Sasol).
[0097] The reason why the third resin composition has high fluidity is thought to be as follows. It is presumed that the alumina filler (C0) having a product of the average particle diameter D50 and the specific surface area SA within the above range has a larger specific surface area relative to the particle diameter and more irregularities on the filler surface compared to other alumina fillers. Therefore, it is presumed that the alumina filler (C) also has a more irregular surface, which reduces the interaction between the alumina fillers (C), making the alumina filler (C) less likely to aggregate. Furthermore, if the alumina filler (C) is a surface-treated alumina filler that has been surface-treated with a silane coupling agent (SC2) having an amino group with a secondary amine structure, the alumina filler (C) becomes even less likely to aggregate due to the interaction between the silane coupling agents (SC2), while the affinity between the alumina filler (C) and the epoxy resin (A) is improved.
[0098] For these reasons, it is presumed that the dispersibility and filling property of the filler are improved, and the fluidity of the third resin composition is improved. By improving the filling property of the filler, the filling rate of the filler can be increased, and the thermal conductivity of the cured product made of the third resin composition is improved and the linear expansion property is reduced.
[0099] The fact that the specific surface area of the alumina filler (C0) is large relative to the particle size means that the size of the crystallites constituting the filler particles is small, and D50 / L 104 It is presumed that this is due to the fact that the specific surface area relative to the particle size of the alumina filler (C0) is in the above range. When the specific surface area relative to the particle size of the alumina filler (C0) is large, the particle size distribution of the alumina filler (C0) tends to be narrow, and D90 / D10 tends to be in the above range. In addition to the specific surface area relative to the particle size of the alumina filler (C0) being large, when the particle size distribution of the alumina filler (C0) is narrow and D90 / D10 is in the above range, the dispersibility and packing property of the filler are further improved, which is preferable.
[0100] In the third resin composition, if the alumina filler (C0) is surface-treated with a silane coupling agent having an amino group with a primary amine structure, the reactivity between the epoxy resin (A) and the alumina filler may become excessively high, which may lead to the agglomeration of the alumina filler. Also, in the third resin composition, if the alumina filler (C0) is surface-treated with a silane coupling agent having an amino group with a tertiary amine structure, the reactivity between the epoxy resin (A) and the alumina filler may become low, which may prevent the filler from being easily filled in the resin composition.
[0101] In the third resin composition, it is presumed that if the untreated aluminum nitride filler and the alumina filler (C0) are surface-treated with a silane coupling agent having a different organic reactive group, the interaction between the silane coupling agents of the aluminum nitride filler (B) and the alumina filler (C) can be alleviated, thereby improving the filling ability of the filler and improving the fluidity of the third resin composition.
[0102] <Fourth Resin Composition> In the fourth resin composition, the aluminum nitride filler (B) is an aluminum nitride filler that has been surface-treated with a silane coupling agent (SC1) having an organic reactive group including an epoxy group, and the alumina filler (C) has an average particle size D50 (μm) and a specific surface area SA (m 2 The alumina filler (C0) having a product of (A / g) and (B / g) of less than 2.6 is surface-treated with a silane coupling agent (SC2) having an organic reactive group containing an amino group with a secondary amine structure, which is different from the organic reactive group possessed by the silane coupling agent (SC1). The cured product of the fourth resin composition tends to have particularly high thermal conductivity compared to the cured product of the first resin composition.
[0103] The crystallite size L of the alumina filler (C0) used in the fourth resin composition 104 is preferably 30 to 150 nm. 104is more preferably 40 nm or more, even more preferably 60 nm or more, particularly preferably 70 nm or more, and more preferably 120 nm or less, even more preferably 100 nm or less, particularly preferably 90 nm or less.
[0104] The average particle diameter D50 (μm) and specific surface area SA (m 2 / g) is preferably less than 2.6, more preferably 2.3 or less, even more preferably 2.0 or less, and is preferably 1.0 or more.
[0105] The average particle size D50 (μm) and the crystallite size L of the alumina filler (C0) used in the fourth resin composition 104 (μm) (D50 / L 104 ) is preferably 6.0 or less, more preferably 5.5 or less, even more preferably 5.0 or less, and is preferably 1.0 or more.
[0106] The ratio (D90 / D10) of the 90% particle diameter D90 to the 10% particle diameter D10 of the alumina filler (C0) used in the fourth resin composition is preferably 8.0 or less, more preferably 6.0 or less, and even more preferably 4.0 or less. The lower limit of D90 / D10 is not particularly limited as long as it is 1 or more, which is the theoretical minimum value.
[0107] Examples of commercially available alumina fillers (C0) having physical property values within the above ranges include Advanced Alumina AA-03F (manufactured by Sumitomo Chemical Co., Ltd.), Advanced Alumina AA-04 (manufactured by Sumitomo Chemical Co., Ltd.), and NXA-150 (manufactured by Sumitomo Chemical Co., Ltd.).
[0108] The reason why the cured product of the fourth resin composition has high thermal conductivity is thought to be as follows. It is presumed that the alumina filler (C0) having the product of the average particle diameter D50 and the specific surface area SA in the above range has a smoother surface compared to other alumina fillers. Therefore, the surface of the alumina filler (C) is smooth, and the contact area between the alumina fillers (C) is large, facilitating heat conduction. The smooth surface of the alumina filler (C0) means that the crystallite size relative to the particle diameter is large, and the ratio D50 / L 104It is presumed that this is due to the fact that the adhesion between the alumina filler (C) and the epoxy resin (A) and between the alumina filler (C) and the aluminum nitride filler (B) is improved due to the interaction between the alumina filler (C) and the epoxy resin (A) and the interaction between the amino group derived from the silane coupling agent (SC2) in the alumina filler (C) and the epoxy group derived from the silane coupling agent (SC1) in the aluminum nitride filler (B), thereby reducing the interfacial thermal resistance between the filler and the resin and efficiently forming a heat conduction path, thereby improving thermal conductivity.
[0109] In addition, in the fourth resin composition, the improvement in adhesion between the aluminum nitride filler (B) and the resin due to the interaction between the epoxy groups derived from the silane coupling agent (SC1) in the aluminum nitride filler (B) and the curing agent described later is also presumed to reduce the interfacial thermal resistance between the filler and the resin and contribute to improving thermal conductivity.
[0110] <Silane Coupling Agent (SC2) in the Third Resin Composition and the Fourth Resin Composition> The amino group of the secondary amine structure is preferably a methylamino group or a phenylamino group, more preferably a phenylamino group. That is, the silane coupling agent (SC2) having an organic reactive group containing an amino group of a secondary amine structure preferably has an organic reactive group containing a methylamino group or a phenylamino group, more preferably has an organic reactive group containing a phenylamino group.
[0111] Examples of the silane coupling agent (SC2) having an organic reactive group containing an amino group of a secondary amine structure include N-phenyl-3-aminopropyltrimethoxysilane and 3-(methylamino)propyltrimethoxysilane. When the silane coupling agent (SC1) has an organic reactive group containing a (meth)acrylic group, the silane coupling agent (SC2) preferably does not have an organic reactive group containing a (meth)acrylic group. When the silane coupling agent (SC1) has an organic reactive group containing an epoxy group, the silane coupling agent (SC2) preferably does not have an organic reactive group containing an epoxy group.
[0112] [Content of Each Component] The resin composition contains 800 to 1800 parts by mass of aluminum nitride filler (B) and alumina filler (C) in total relative to 100 parts by mass of epoxy resin (A). The total content of aluminum nitride filler (B) and alumina filler (C) relative to 100 parts by mass of epoxy resin (A) is preferably 900 parts by mass or more, more preferably 1000 parts by mass or more, even more preferably 1100 parts by mass or more, and preferably 1600 parts by mass or less, more preferably 1500 parts by mass or less, even more preferably 1400 parts by mass or less, and particularly preferably 1300 parts by mass or less. When the total content of aluminum nitride filler (B) and alumina filler (C) in the resin composition is within the above range, it is possible to achieve a well-balanced improvement in the flowability of the resin composition, the low linear expansion of a cured product made of the resin composition, and the high thermal conductivity of the cured product. Furthermore, when the total content of the aluminum nitride filler (B) and the alumina filler (C) in the resin composition is within the above range, the dispersibility and filling property of the filler in the resin composition are also excellent.
[0113] The mass ratio of the content of the aluminum nitride filler (B) to the content of the alumina filler (C) (content of aluminum nitride filler (B) / content of alumina filler (C)) is preferably 95 / 5 to 20 / 80, more preferably 93 / 7 to 30 / 70, and even more preferably 90 / 10 to 40 / 60, from the viewpoint of dispersibility of the fillers.
[0114] In the first, second, and fourth resin compositions, the content ratio of the aluminum nitride filler (B) to the alumina filler (C) is preferably such that the ratio (S2 / S1) of the total surface area S1 of the aluminum nitride filler (B) to the total surface area S2 of the alumina filler (C) is 0.5 to 2.2. The ratio (S2 / S1) is preferably 0.8 or more, more preferably 1.0 or more, even more preferably 1.1 or more, and preferably 2.1 or less, more preferably 1.8 or less, and even more preferably 1.5 or less. By keeping the value of S2 / S1 within the above range, the thermal conductivity of the cured product made from the resin composition can be further increased. Although the reason for this is unclear, it is presumed that the balance of the interactions between the epoxy resin (A) and each filler improves the adhesion at the interface between the epoxy resin (A) and the filler, thereby improving the filler's packing ability.
[0115] The total surface area S1 of the aluminum nitride filler (B) can be calculated by multiplying the specific surface area SA of the aluminum nitride filler (B) by the content of the aluminum nitride filler (B). The total surface area S2 of the alumina filler (C) can be calculated by multiplying the specific surface area SA of the alumina filler (C) by the content of the alumina filler (C). The alumina filler (C) may be one type or two or more types.
[0116] [Other Components] The resin composition may contain components other than the epoxy resin (A), the aluminum nitride filler (B), and the alumina filler (C) (hereinafter also referred to as "other components"), provided that the effects of the present invention are not impaired. Examples of other components include curing agents, curing accelerators, resins other than the epoxy resin (A), fillers other than the aluminum nitride filler (B) and the alumina filler (C), flame retardants, rubber particles, thickeners, defoamers, leveling agents, adhesion promoters, antioxidants, UV inhibitors, and colorants.
[0117] Examples of the curing agent include an epoxy resin curing agent. When the epoxy resin (A) contains a reactive epoxy resin, the epoxy resin curing agent has the function of reacting with the reactive epoxy resin to cure. When the resin composition contains an epoxy resin curing agent, the cured product obtained by thermally curing the resin composition tends to have high strength and heat resistance.
[0118] Known curing agents can be used as the epoxy resin curing agent. Examples of epoxy resin curing agents include phenol-based curing agents, naphthol-based curing agents, active ester-based curing agents, cyanate ester-based curing agents, benzoxazine-based curing agents, and acid anhydride-based curing agents. From the viewpoints of the moldability of the resin composition into a film and the heat resistance of the cured product made of the resin composition, phenol-based curing agents, naphthol-based curing agents, and active ester-based curing agents are preferred. The curing agents may be used alone or in combination of two or more.
[0119] As the phenol-based curing agent and naphthol-based curing agent, those having a novolac structure are preferred from the viewpoint of the heat resistance and water resistance of the cured product made from the resin composition. As the phenol-based curing agent having a novolac structure, phenol novolac, cresol novolac, bisphenol A-type novolac, phenol aralkyl novolac, biphenyl aralkyl novolac, aminotriazine novolac (triazine structure-containing phenol novolac), triphenylmethane novolac, and cyclopentadiene phenol novolac are preferred. As the naphthol-based curing agent having a novolac structure, naphthol aralkyl-type phenol novolac, aralkyl-type naphthol-phenol novolac, and naphthol-cresol-type novolac are preferred.
[0120] Commercially available phenolic curing agents and naphthol curing agents include, for example, "GPH-103," "GPH-65," and "TKG-105" manufactured by Nippon Kayaku Co., Ltd.; "TD-2093," "TD-2090," "LF-6161," "LF-4871," "LA-7052," "LA-7054," "LA-1536," and "LA-1356" manufactured by DIC Corporation; "ZX-798" and "SN485" manufactured by Nippon Steel Chemical & Material Co., Ltd.; "TPM-100" and "GPNX" manufactured by Gun-ei Chemical Co., Ltd.; and "S-TPM" and "J-DDP" manufactured by JFE Chemical Corporation.
[0121] From the viewpoints of the formability of the resin composition into a film and the heat resistance of a cured product made from the resin composition, the reactive group equivalent (hydroxyl group equivalent) of the phenol-based curing agent and the naphthol-based curing agent is preferably 20 to 4000, more preferably 50 to 2000, and even more preferably 50 to 1000. The hydroxyl group equivalent is the mass of the resin per equivalent of hydroxyl groups.
[0122] Examples of active ester curing agents include active ester curing agents having a dicyclopentadiene structure, active ester curing agents having a naphthalene structure, active ester curing agents containing an acetylated product of phenol novolac, and active ester curing agents containing a benzoylated product of phenol novolac. From the viewpoint of the heat resistance and water resistance of the cured product of the resin composition, active ester curing agents having a dicyclopentadiene structure and active ester curing agents having a naphthalene structure are preferred. An example of a commercially available active ester curing agent having a dicyclopentadiene structure is "HPC-8000-65T" manufactured by DIC Corporation. An example of a commercially available active ester curing agent having a naphthalene structure is "HPC-8150-62T" manufactured by DIC Corporation.
[0123] From the viewpoints of the moldability of the resin composition into a film and the heat resistance of a cured product made from the resin composition, the reactive group equivalent (active ester group equivalent) of the active ester curing agent is preferably 50 to 2000, more preferably 50 to 1000, and even more preferably 100 to 500. The active ester group equivalent is the mass of resin per equivalent of active ester group.
[0124] The content of the curing agent in the resin composition is preferably 50 to 200 parts by mass, more preferably 65 to 150 parts by mass, and even more preferably 75 to 125 parts by mass per 100 parts by mass of the epoxy resin (A), from the viewpoint of the heat resistance and mechanical strength of the cured product of the resin composition. The total number of reactive groups, such as hydroxyl groups and active ester groups, of the curing agent is preferably 0.5 to 2, more preferably 0.6 to 1.5, and even more preferably 0.65 to 1.25, relative to the total number of epoxy groups in the epoxy resin (A). The total number of epoxy groups in the epoxy resin (A) is the sum of the values obtained by dividing the mass of each epoxy resin by the epoxy equivalent, for all epoxy resins. Similarly, the total number of reactive groups in the curing agent is the sum of the values obtained by dividing the mass of each curing agent by the reactive group equivalent.
[0125] Examples of the curing accelerator include an epoxy resin curing accelerator. An epoxy resin curing accelerator functions to promote the reaction between the epoxy groups of the epoxy resin (A) and the reactive groups of the curing agent, and to promote the polymerization of the epoxy groups. When the epoxy resin (A) contains a reactive epoxy resin, the resin composition containing an epoxy resin curing accelerator can easily be thermally cured, and the cured product tends to have high strength. The content of the epoxy resin curing accelerator in the resin composition is preferably 0.01 to 5 parts by mass, more preferably 0.05 to 3 parts by mass, and even more preferably 0.1 to 2 parts by mass, per 100 parts by mass of the epoxy resin (A).
[0126] The epoxy resin curing accelerator may be any known one without particular limitation, and examples thereof include amine-based curing accelerators, imidazole-based curing accelerators, phosphorus-based curing accelerators, and guanidine-based curing accelerators, with amine-based curing accelerators and imidazole-based curing accelerators being preferred. The curing accelerators may be used alone or in combination of two or more.
[0127] Examples of the amine curing accelerator include trialkylamines such as triethylamine and tributylamine, 4-dimethylaminopyridine, benzyldimethylamine, 2,4,6-tris(dimethylaminomethyl)phenol, and 1,8-diazabicyclo(5,4,0)-undecene.
[0128] Examples of the imidazole curing accelerator include 2-methylimidazole, 2-undecylimidazole, 2-heptadecylimidazole, 1,2-dimethylimidazole, 2-ethyl-4-methylimidazole, 1,2-dimethylimidazole, 2-ethyl-4-methylimidazole, 2-phenylimidazole, 2-phenyl-4-methylimidazole, 1-benzyl-2-methylimidazole, and 1-benzyl-2-phenylimidazole. nirimidazole, 1-cyanoethyl-2-methylimidazole, 1-cyanoethyl-2-undecylimidazole, 1-cyanoethyl-2-ethyl-4-methylimidazole, 1-cyanoethyl-2-phenylimidazole, 1-cyanoethyl-2-undecylimidazole, 1-cyanoethyl-2-phenylimidazolium trimellitate, 1-cyanoethyl-2-phenylimidazolium trimellitate, 2,4-diamino-6-[2'-methylimidazolyl-(1 ')]-ethyl-s-triazine, 2,4-diamino-6-[2'-undecylimidazolyl-(1')]-ethyl-s-triazine, 2,4-diamino-6-[2'-ethyl-4'-methylimidazolyl-(1')]-ethyl-s-triazine, 2,4-diamino-6-[2'-methylimidazolyl-(1')]-ethyl-s-triazine isocyanuric acid adduct, 2-phenylimidazole isocyanuric acid adduct, 2-fu Examples of the epoxy resin include imidazole compounds such as 2-phenyl-4,5-dihydroxymethylimidazole, 2-phenyl-4-methyl-5-hydroxymethylimidazole, 2,3-dihydro-1H-pyrrolo[1,2-a]benzimidazole, 1-dodecyl-2-methyl-3-benzylimidazolium chloride, 2-methylimidazoline, and 2-phenylimidazoline, as well as adducts of imidazole compounds with epoxy resins.
[0129] Examples of phosphorus-based curing accelerators include triphenylphosphine, phosphonium borate compounds, tetraphenylphosphonium tetraphenylborate, n-butylphosphonium tetraphenylborate, tetrabutylphosphonium decanoate, (4-methylphenyl)triphenylphosphonium thiocyanate, tetraphenylphosphonium thiocyanate, and butyltriphenylphosphonium thiocyanate.
[0130] Examples of guanidine curing accelerators include dicyandiamide, 1-methylguanidine, 1-ethylguanidine, 1-cyclohexylguanidine, 1-phenylguanidine, 1-(o-tolyl)guanidine, dimethylguanidine, diphenylguanidine, trimethylguanidine, tetramethylguanidine, pentamethylguanidine, 1,5,7-triazabicyclo[4.4.0]dec-5-ene, 7-methyl-1,5,7-triazabicyclo[4.4.0]dec-5-ene, 1-methylbiguanide, 1-ethylbiguanide, 1-n-butylbiguanide, 1-n-octadecylbiguanide, 1,1-dimethylbiguanide, 1,1-diethylbiguanide, 1-cyclohexylbiguanide, 1-allylbiguanide, 1-phenylbiguanide, and 1-(o-tolyl)biguanide.
[0131] When the resin composition contains a resin other than the epoxy resin (A) (hereinafter also referred to as "other resin"), the resin composition tends to have excellent flexibility. Therefore, when forming a film from the resin composition, the coating property is improved to obtain a uniform film, and the film becomes flexible, improving winding properties. In addition, the impact resistance of a cured product made from the resin composition is improved, making the cured product less likely to crack.
[0132] Examples of the other resin include thermoplastic resins such as phenoxy resin, polyvinyl acetal resin, polyolefin resin, polybutadiene resin, polyimide resin, polyamideimide resin, polyethersulfone resin, polyphenylene ether resin, and polysulfone resin, and among these, phenoxy resin, which has a structure similar to that of the epoxy resin (A), is preferred because it has good compatibility with the epoxy resin (A). The other resin may be used alone or in combination of two or more.
[0133] Examples of phenoxy resins include phenoxy resins having one or more skeletons selected from the group consisting of bisphenol A skeleton, bisphenol F skeleton, bisphenol S skeleton, bisphenolacetophenone skeleton, novolac skeleton, biphenyl skeleton, fluorene skeleton, dicyclopentadiene skeleton, norbornene skeleton, naphthalene skeleton, anthracene skeleton, adamantane skeleton, terpene skeleton, and trimethylcyclohexane skeleton. The terminal of the phenoxy resin may be any terminal structure such as a phenolic hydroxyl group or an epoxy group. The phenoxy resin may be used alone or in combination of two or more types.
[0134] Commercially available phenoxy resins containing a bisphenol acetophenone skeleton include, for example, "YX6954BH30" manufactured by Mitsubishi Chemical Corporation. Commercially available phenoxy resins containing a bisphenol S skeleton include, for example, "YX8100BH30" manufactured by Mitsubishi Chemical Corporation. Commercially available phenoxy resins include, for example, "YX7553BH30" manufactured by Mitsubishi Chemical Corporation.
[0135] The weight-average molecular weight of the phenoxy resin is preferably 5,000 to 10,000. The weight-average molecular weight of the phenoxy resin is a weight-average molecular weight measured by gel permeation chromatography in terms of polystyrene. The content of the other resins such as the phenoxy resin in the resin composition is preferably 0.1 to 50 parts by mass, more preferably 0.5 to 30 parts by mass, and even more preferably 1 to 20 parts by mass, per 100 parts by mass of the epoxy resin (A).
[0136] Fillers other than the aluminum nitride filler (B) and the alumina filler (C) (hereinafter also referred to as "other fillers") are fillers made of materials other than aluminum nitride and alumina. The other fillers may include, for example, silica, zinc oxide, magnesium oxide, titanium oxide, silicon nitride, boron nitride, aluminum hydroxide, magnesium hydroxide, silicon carbide, calcium carbonate, barium sulfate, talc, and diamond.
[0137] The content of the other filler in the resin composition is preferably 10 parts by mass or less, more preferably 5 parts by mass or less, and even more preferably 1 part by mass or less, per 100 parts by mass of the total amount of the aluminum nitride filler (B) and the alumina filler (C). Particularly preferably, the resin composition does not contain any other filler. The average particle size D50 of the other filler is preferably smaller than the average particle size D50 of the aluminum nitride filler (B), more preferably less than 2 μm, and even more preferably less than 1.5 μm. The maximum particle size Dmax of the other filler is preferably smaller than the maximum particle size Dmax of the aluminum nitride filler (B), more preferably less than 4.5 μm, and even more preferably less than 4 μm.
[0138] The flame retardant imparts flame retardancy to the resin composition when it is used in a semiconductor product. Examples of the flame retardant include organic phosphorus flame retardants, organic nitrogen-containing phosphorus compounds, nitrogen compounds, silicone flame retardants, and metal hydroxides. The flame retardants may be used alone or in combination of two or more.
[0139] When the resin composition contains rubber particles, the internal stress generated when the resin composition is thermally cured is alleviated, and the cured product tends to have excellent impact resistance because of reduced warpage. Examples of the rubber particles include fine particles such as core-shell rubber particles, cross-linked acrylonitrile butadiene rubber particles, cross-linked styrene butadiene rubber particles, and acrylic rubber particles. The average particle size D50 of the rubber particles is preferably 1 μm or less, more preferably 0.8 μm or less.
[0140] The method for producing the resin composition is not particularly limited, and the resin composition can be produced by mixing the epoxy resin (A), the aluminum nitride filler (B), the alumina filler (C), and other components, as needed, using a known method such as a blender or mixer. During the mixing, the components may be simultaneously added to a mixer or the like and mixed, or the components may be added sequentially to a mixer or the like and mixed. The order of addition when the components are sequentially added to a mixer or the like is not particularly limited. Furthermore, the mixing may be performed under heating, or in a controlled atmosphere such as an inert gas atmosphere, as needed.
[0141] [Physical Properties of Resin Composition] The resin composition of the present invention has high fluidity, and a cured product thereof has low linear expansion and high thermal conductivity.
[0142] Because the resin composition has high fluidity, a film made of the resin composition can conform to the shape of a conductor layer of a multilayer printed wiring board, a cavity of a component-embedded substrate, and an electronic component, thereby improving adhesion between the film made of the resin composition and the conductor layer, etc.
[0143] The minimum melt viscosity of the resin composition in the temperature range of 90 to 140° C. is preferably 13,000 poise or less, more preferably 9,000 poise or less, and even more preferably 6,000 poise or less.
[0144] In the manufacture of multilayer printed wiring boards using a film made of the resin composition, heat pressing is typically performed at an appropriate temperature selected within the range of 90 to 140°C. When the minimum melt viscosity within the temperature range of 90 to 140°C is within this range, the temperature conditions for heat-pressing the resin composition for use in multilayer printed wiring boards and component-embedded substrates can be selected to be close to the temperature at which the melt viscosity is minimum. Therefore, the resin composition can be handled under conditions that ensure high fluidity. From the standpoint of handleability, the minimum melt viscosity of the resin composition within the range of 90 to 140°C is preferably 300 poise or more, more preferably 500 poise or more. The melt viscosity of the resin composition is determined as a complex viscosity by measuring the temperature dispersion of dynamic viscoelasticity using a viscoelasticity measuring device (rotational rheometer).
[0145] The linear expansion coefficient of the cured product of the resin composition is preferably 25 ppm / ° C. or less, more preferably 22 ppm / ° C. or less. The linear expansion coefficient of the cured product of the resin composition is preferably closer to the linear expansion coefficient of copper, which is the conductor layer, of 17 ppm / ° C. The linear expansion coefficient can be measured using a thermomechanical analyzer and is determined from the slope of the change in linear expansion coefficient up to the glass transition temperature.
[0146] The relative density of the resin composition is preferably 0.85 or more, more preferably 0.90 or more, even more preferably 0.95 or more, and particularly preferably 0.97 or more. The relative density of the resin composition is expressed as the ratio of the density measured for a cured sample of the resin composition to the density (theoretical density) calculated from the densities and blending ratios of the components used, and is 1 when the theoretical density and the sample density are the same.
[0147] A high relative density indicates that the filler in the resin composition is highly packed, there are fewer defects such as voids in the resin composition, and the adhesion at the interface between each component is excellent. Therefore, when the relative density of the resin composition is high, the resin composition has excellent fluidity, and a cured product made from the resin composition tends to have excellent thermal conductivity, strength, durability, etc. The upper limit of the relative density is not particularly limited, but is preferably 1.1 or less, more preferably 1.0 or less. The density of the cured product made from the resin composition can be measured by the Archimedes method.
[0148] The thermal conductivity of the cured product made of the resin composition is preferably 3.5 W / m·K or more, more preferably 4.0 W / m·K or more, even more preferably 4.5 W / m·K or more, even more preferably 5.0 W / m·K or more, particularly preferably 5.5 W / m·K or more, and most preferably 6.0 W / m·K or more. When the thermal conductivity of the cured product is high, a film made of the resin composition can improve the heat dissipation properties of multilayer printed wiring boards and component-embedded substrates. The higher the thermal conductivity, the better, but it is generally 30 W / m·K or less. The thermal conductivity can be measured by temperature wave thermal analysis (i-phase method).
[0149] [Applications of Resin Composition] The resin composition has high fluidity, and a cured product of the resin composition has high thermal conductivity and low linear expansion, making the resin composition suitable for use as an insulating layer in multilayer printed wiring boards and as an encapsulating resin for component-embedded substrates. In addition to these applications, the resin composition can also be used in a wide range of applications requiring heat dissipation, such as adhesive films, insulating layers in metal-clad laminates, insulating resin sheets such as prepregs, underfill materials, die bonding materials, semiconductor encapsulants, and hole-filling resins. When the resin composition is used in applications requiring heat dissipation, it is industrially preferable to use the resin composition in the form of a resin composition film, in which the resin composition is molded into a film-like form.
[0150] The resin composition film of the present invention is a film formed from the resin composition of the present invention. The thickness of the resin composition film is preferably 5 to 250 μm, more preferably 10 to 200 μm, and even more preferably 20 to 150 μm.
[0151] The method for producing the resin composition film is not particularly limited, and the resin composition film can be produced by a conventionally known method. A suitable method for producing the resin composition film includes, for example, dissolving and mixing the resin composition in an organic solvent to prepare a varnish, applying the varnish to a support using a die coater or the like, and then drying the varnish by heating, blowing hot air, or the like, to remove the organic solvent.
[0152] Examples of the organic solvent include acetone, methanol, ethanol, butanol, 2-propanol, 2-methoxyethanol, 2-ethoxyethanol, 1-methoxy-2-propanol, 2-acetoxy-1-methoxypropane, toluene, xylene, methyl ethyl ketone, N,N-dimethylformamide, methyl isobutyl ketone, N-methyl-pyrrolidone, n-hexane, cyclohexane, cyclohexanone, and solvent naphtha, which is a mixture thereof. The organic solvents may be used alone or in combination of two or more.
[0153] From the viewpoint of ease of removal of the organic solvent during drying, the boiling point of the organic solvent is preferably 200° C. or lower, more preferably 180° C. or lower. The content of the organic solvent in the varnish is not particularly limited and may be appropriately adjusted taking into consideration factors such as coatability onto a support.
[0154] The varnish is preferably dried so that the total content of organic solvents in the resin composition film is preferably 10% by mass or less, more preferably 5% by mass or less. Although the boiling point of the organic solvents contained in the resin composition film varies, for example, by heating and drying the varnish at 60°C to 150°C for 1 to 5 minutes, the resin composition film can be obtained without excessive heat curing.
[0155] The resin composition film is preferably in a partially cured state, a so-called B-stage film. When the resin composition film is in a partially cured state, the resin composition film is not completely cured, so that the resin composition film can conform to the shape of a conductor layer when producing a multilayer printed wiring board or a component-embedded substrate. Further curing of the resin composition film can then be advanced to improve the strength and durability of the resin composition film.
[0156] As the support, various plastic films can be suitably used, for example, polyester films such as polyethylene terephthalate film, polybutylene terephthalate film, and polyethylene naphthalate, olefin films such as polyethylene film and polypropylene film, and polyimide film, among which polyethylene terephthalate film is preferred because it has excellent smoothness and heat resistance and is inexpensive.
[0157] From the viewpoints of wettability during coating of the resin composition film and releasability during the production of various semiconductor substrates, the coated surface of the plastic film support may be subjected to a release treatment, matte treatment, corona discharge treatment, etc. Metal foils such as copper foil and aluminum foil may be used as the support. Suitable copper foils include rolled copper foil and electrolytic copper foil. Using a metal foil as the support can eliminate the step of laminating the metal foil during the production of various substrates, thereby improving the adhesive strength between the support and the resin composition film. The thickness of the support is not particularly limited, but is preferably in the range of 5 to 150 μm, more preferably 10 to 100 μm, and even more preferably 10 to 60 μm.
[0158] A protective film similar to the support may be further laminated on the surface of the resin composition film that is not in contact with the support. The thickness of the protective film is not particularly limited, but is, for example, 5 to 40 μm. By laminating a protective film on the surface of the resin composition film that is not in contact with the support, adhesion of dust and the like to the surface of the resin composition film and scratches can be prevented, and the resin composition film can also be wound into a roll. When producing multilayer printed wiring boards, component-embedded substrates, and other semiconductor materials, the protective film is peeled off before use.
[0159] The resin composition film has high fluidity and embeddability, and a cured product of the resin composition has high thermal conductivity and low linear expansion, so the resin composition film can be suitably used to form an insulating layer of a multilayer printed wiring board and as a sealing resin for a component-embedded substrate. The resin composition film can also be used in a wide range of applications requiring heat dissipation, such as adhesive films, insulating layers of metal-clad laminates, insulating resin sheets such as prepregs, underfill materials, die bonding materials, semiconductor sealing materials, and hole-filling resins.
[0160] The present invention will be explained in more detail below with reference to examples, but the present invention is not limited to these examples.
[0161] The following components were used as materials for the resin composition: <Epoxy Resin (A)> Solid Epoxy Resin (A-1) Each of the following solid epoxy resins was dissolved in methyl ethyl ketone and used as a 50% by mass solution. EPPN-501HY (manufactured by Nippon Kayaku Co., Ltd., trisphenolmethane type epoxy resin, epoxy equivalent 166, softening point 60°C) NC-3000 (manufactured by Nippon Kayaku Co., Ltd., biphenylaralkyl type epoxy resin, epoxy equivalent 276, softening point 58°C) HP-4700 (manufactured by DIC Corporation, tetrafunctional naphthalene type epoxy resin, epoxy equivalent 163, softening point 92°C) Liquid epoxy resin (A-2) jER828 (manufactured by Mitsubishi Chemical Corporation, bisphenol A type epoxy resin, epoxy equivalent 189, viscosity (25°C) 135 poise) YDF-8170C (manufactured by Nippon Steel Chemical & Material Co., Ltd., bisphenol F type epoxy resin, epoxy equivalent 155-165, viscosity 10-15 poise)
[0162] <Aluminum nitride filler (B)> <Untreated aluminum nitride filler> HF-01D (manufactured by Tokuyama Corporation) Aluminum nitride powder H grade (manufactured by Tokuyama Corporation)
[0163] For the aluminum nitride fillers (B-1) to (B-4) and (B-6) to (B-10), untreated aluminum nitride fillers were surface-treated with a silane coupling agent (SC1) by the following method and used. For the aluminum nitride filler (B-5), an untreated aluminum nitride filler was used. Table 2 shows the combinations of untreated aluminum nitride fillers and silane coupling agents (SC1).
[0164] <Method for producing aluminum nitride filler (B)> 600 g of untreated aluminum nitride filler, 5 g of silane coupling agent (SC1), and 1,200 g of isopropyl alcohol were placed in a glass eggplant flask and stirred for 30 minutes with a fluororesin stirring blade. Subsequently, the isopropyl alcohol was removed under reduced pressure at 50°C using a rotary evaporator, and the resulting mixture was dried under reduced pressure at 100°C to perform a surface treatment.
[0165] <Alumina Filler (C)> <Alumina Filler (C0)> The following untreated alumina fillers were used as the alumina filler (C0): AA-03F (manufactured by Sumitomo Chemical Co., Ltd.) NXA-150 (manufactured by Sumitomo Chemical Co., Ltd.) AHPA-0.5AF (manufactured by Sasol) AA-04 (manufactured by Sumitomo Chemical Co., Ltd.) ASFP-20 (manufactured by Denka Co., Ltd.) AA-1.5 (manufactured by Sumitomo Chemical Co., Ltd.)
[0166] Untreated alumina fillers were used as alumina fillers (C-1) to (C-3) and alumina filler (C-16). Untreated alumina fillers that had been surface-treated with a silane coupling agent (SC2) by the following method were used as alumina fillers (C-4) to (C-15) and alumina filler (C-17). Combinations of untreated alumina fillers and silane coupling agents (SC2) are shown in Table 3.
[0167] <Method for producing alumina filler (C)> 600 g of untreated alumina filler, 5 g of a silane coupling agent (SC2), and 1,200 g of isopropyl alcohol were placed in a glass eggplant flask and stirred for 30 minutes with a fluororesin stirring blade. Next, the isopropyl alcohol was removed under reduced pressure at 50°C using a rotary evaporator, and the mixture was then dried under reduced pressure at 100°C to perform a surface treatment.
[0168] <Silane Coupling Agent (SC1) and Silane Coupling Agent (SC2)>- N-Phenyl-3-aminopropyltrimethoxysilane (manufactured by Shin-Etsu Chemical Co., Ltd., KBM-573) - 3-Methacryloxypropyltriethoxysilane (manufactured by Shin-Etsu Chemical Co., Ltd., KBE-503) - 3-(Methylamino)propyltrimethoxysilane (manufactured by Tokyo Chemical Industry Co., Ltd., T2868) - Phenyltrimethoxysilane (manufactured by Shin-Etsu Chemical Co., Ltd., KBM-103) - 3-Aminopropyltrimethoxysilane (manufactured by Shin-Etsu Chemical Co., Ltd., KBM-903) - 3-Acryloxypropyltrimethoxysilane (manufactured by Shin-Etsu Chemical Co., Ltd., KBM-5103) - 3-Glycidoxypropyltriethoxysilane (manufactured by Shin-Etsu Chemical Co., Ltd., KBE-403) - Octyltriethoxysilane (manufactured by Shin-Etsu Chemical Co., Ltd., KBE-3083) - 8-Glycidoxyoctyltrimethoxysilane (manufactured by Shin-Etsu Chemical Co., Ltd., KBM-4803)<Hardener>- GPH-103 (manufactured by Nippon Kayaku Co., Ltd., biphenyl aralkyl phenol novolak, hydroxyl equivalent 230, softening point 103 °C) - PHENOLITE TD-2090-60M (manufactured by DIC Corporation, phenol novolak resin, hydroxyl equivalent 104, methyl ethyl ketone solution with solid content of 60% by mass) - HPC-8000-65T (manufactured by DIC Corporation, active ester-based hardener having a dicyclopentadiene structure, active ester group equivalent 223, toluene solution with non-volatile content of 65% by mass) When using GPH-103, GPH-103 was dissolved in methyl ethyl ketone and used as a 50% by mass solution.
[0169] <Phenoxy Resin>- YX6954BH30 (manufactured by Mitsubishi Chemical Corporation, phenoxy resin containing bisphenol acetophenone skeleton, weight average molecular weight 40670, cyclohexanone / methyl ethyl ketone (1 / 1) solution with non-volatile content of 30% by mass)
[0170] <Hardening Accelerator> - 4-Dimethylaminopyridine (DMAP, manufactured by Fujifilm Wako Pure Chemical Corporation)
[0171] [Evaluation of Filler Properties] The physical properties of the untreated alumina filler, aluminum nitride filler (B) and alumina filler (C) were measured under the following conditions. The measurement results are shown in Tables 1 to 3.
[0172] <Average particle size and maximum particle size of filler> Untreated alumina filler, aluminum nitride filler (B) or alumina filler (C) was added to a dispersion medium to a concentration of 0.2 mass%, and the sample was dispersed by irradiating with ultrasonic waves of about 200 W for 2 minutes, and the particle size distribution of the sample was measured using a laser diffraction scattering particle size distribution meter (MICROTRACK-MT3300EXII, manufactured by Microtrack-Bell Co., Ltd.). Note that water was used as the dispersion medium when dispersing untreated aluminum nitride filler and untreated alumina filler, and ethanol was used when dispersing surface-treated aluminum nitride filler and surface-treated alumina filler. In the obtained volume frequency distribution (particle size distribution) of particle diameters, the volume frequencies were accumulated from the smallest particle diameter, and the particle diameter at which the accumulated value reached 10% was defined as the 10% particle diameter D10, the particle diameter at which the accumulated value reached 50% was defined as the average particle diameter D50, the particle diameter at which the accumulated value reached 90% was defined as the 90% particle diameter D90, and the maximum value of the measured particle diameters (particle diameter at 100% accumulated volume) was defined as the maximum particle diameter Dmax.
[0173] <Specific Surface Area of Filler> The specific surface areas SA of the untreated alumina filler, aluminum nitride filler (B), and alumina filler (C) were determined by the BET method (nitrogen adsorption single-point method) using a flow-type automatic specific surface area measuring device (Shimadzu Corporation, Flowsorb II-2300). For the measurement, 2 g of powdered untreated alumina filler, aluminum nitride filler (B), or alumina filler (C) dried at 100°C for 1 hour under a nitrogen gas flow was used.
[0174] <Crystallite size of untreated alumina filler> Using an X-ray diffractometer (SmartLab manufactured by Rigaku Corporation), the powder X-ray diffraction profile of the untreated alumina filler was measured under the following conditions: X-ray source: CuKα ray (wavelength: 0.15418 nm), X-ray output: 40 kV-200 mA, 2θ range: 20 to 60°, step width: 0.02°. Based on the obtained half-width of the diffraction peak due to the (104) plane of α-phase alumina around 2θ = 35.1°, the crystallite size calculated using the Scherrer formula was determined as L 104 The Scherrer constant was set to 0.94.
[0175] <Galactose ratio of untreated alumina filler> From the powder X-ray diffraction profile obtained above, the alpha phase ratio of the alumina filler was determined by the method described in JP-A-2007-055888. Specifically, the peak height (I 25.6 ) and the peak height (I 46 ) and the gelatinization rate was calculated according to the following formula (1): 25.6 / (I 25.6 +I 46 ) × 100% ... (1)
[0176]
[0177]
[0178]
[0179] Example 1 50 parts by mass of liquid epoxy resin (A-2) jER828 was blended with 135 parts by mass of curing agent HPC-8000-65T (non-volatile content 87.8 parts by mass), 33 parts by mass of phenoxy resin YX6954BH30 (non-volatile content 9.9 parts by mass), 0.8 parts by mass of curing accelerator DMAP, and 430 parts by mass of alumina filler (C-1), and the mixture was stirred and mixed.
[0180] To the above mixture, 100 parts by mass of a methyl ethyl ketone solution of solid epoxy resin (A-1) NC3000 (50 parts by mass of nonvolatile content), 740 parts by mass of aluminum nitride filler (B-1), and 300 parts by mass of methyl ethyl ketone were added, and the mixture was stirred for 30 minutes using a homodisper, followed by kneading using a three-roll mill. Further, methyl ethyl ketone was appropriately added to adjust the viscosity, and then the mixture was filtered and degassed to prepare a varnish of the resin composition.
[0181] Next, the varnish of the resin composition was uniformly applied to the release-treated surface of a support (release-treated polyethylene terephthalate film (HY-NS80, manufactured by Higashiyama Film Co., Ltd., thickness 38 μm)) so that the thickness after drying would be 80 μm, and the film was dried at 80° C. for 3 minutes to produce a resin composition film (B-stage).
[0182] Examples 2 to 22, Comparative Examples 1 to 7 Resin composition films were produced in the same manner as in Example 1, except that the compositions of the resin composition films were changed as shown in Tables 4 to 7.
[0183] [Examples 23 to 77, Comparative Examples 8 to 13] Resin composition films were produced in the same manner as in Example 1, except that the composition of the resin composition film was changed as shown in Tables 8 to 15, and that the kneading using a three-roll mill was not performed after stirring using a homodisper. The mass of each component shown in Tables 4 to 15 represents the mass of the non-volatile content.
[0184] [Evaluation of Physical Properties of Resin Compositions] The results of measuring the physical properties of the resin compositions under the following conditions are shown in Tables 4 to 15.
[0185] <Minimum Melt Viscosity> The resin composition film was peeled off from the support, and the melt viscosity was measured using a viscoelasticity measuring device (rotational rheometer) (MCR302e, manufactured by Anton Paar). Dynamic viscoelasticity was measured under the following conditions: geometry: parallel plates with a diameter of 10 mm, gap: 1 mm, temperature range: 60°C to 180°C, frequency: 1 Hz, strain: 10%, and the minimum value of the complex viscosity in the range of 90 to 140°C was taken as the minimum melt viscosity.
[0186] <Linear expansion coefficient> The resin composition film was cut into 5 mm wide strips and heat-cured at 180°C for 90 minutes. The obtained cured product was subjected to two consecutive measurements in the range of 30°C to 220°C by the tensile load method using a thermomechanical analyzer (TMA4000SE, manufactured by NETZSCH) with a sample length (between chucks): 20 mm, a load: 1 g, and a heating rate: 5°C / min. The linear expansion coefficient was calculated from the slope of the change in linear expansion coefficient from 30°C to the glass transition temperature (the temperature at which the slope of the TMA curve changes) in the second measurement.
[0187] <Thermal Conductivity> The resin composition film was heat-treated at 180°C for 90 minutes to be thermally cured. The thermal conductivity (W / m·K) of the obtained cured product was calculated based on the thermal diffusivity (m 2 / sec) x density (kg / m 3 ) × specific heat (J / kg K). The thermal diffusivity was calculated by the average value of 12 measurements performed on the same test piece by temperature wave thermal analysis (ai-Phase Mobile 1u, ISO22007-3, manufactured by i-Phase Corporation). The density was measured by the Archimedes method (XS204V, manufactured by Mettler Toledo), and the specific heat was measured by a differential scanning calorimeter (DSC) method (Thermo Plus Evo DSC8230, manufactured by Rigaku Corporation).
[0188] <Relative Density> The relative density of the cured product prepared for measuring thermal conductivity was calculated as the ratio of the actual density measured above to the theoretical value obtained by calculation, i.e., actual value / theoretical value. The theoretical density was calculated by setting the density of the aluminum nitride filler (B), the alumina filler (C), and the remaining components excluding the filler components at 3.26 g / m. 3 , 3.98 g / m 3 , and 1.17 g / m 3 was calculated from the blending ratio of each component.
[0189]
[0190]
[0191]
[0192]
[0193]
[0194]
[0195]
[0196]
[0197]
[0198]
[0199]
[0200]
[0201] When untreated alumina filler was used as the alumina filler (C), resin composition films having high thermal conductivity were obtained, particularly in Examples 1 to 4, 6, 8, 10, and 12 to 19, in which the ratio S2 / S1 of the total surface area of the aluminum nitride filler to the total surface area of the alumina filler was set in the range of 0.5 to 2.2.
[0202] When the total amount of filler is too small (Comparative Example 1), the melt viscosity is low, but the thermal conductivity is insufficient and the linear expansion coefficient is also large. When only aluminum nitride filler is used without blending alumina filler (Comparative Examples 3 to 6), the filling property of the filler is poor, resulting in a high melt viscosity, and the relative density and thermal conductivity are also low. When no alumina filler is used, or when untreated alumina filler is used as alumina filler (C), the melt viscosity is high when an aluminum nitride filler with a large maximum particle size Dmax is used (Comparative Examples 3, 5, and 7). When untreated alumina filler is used as alumina filler (C), the melt viscosity is high and the thermal conductivity is low when the average particle size of the alumina filler is large (Comparative Example 8).
[0203] When the aluminum nitride filler (B) is a surface-treated aluminum nitride filler that has been surface-treated with a silane coupling agent (SC1) having an organic reactive group containing an oxygen atom, a nitrogen atom, or a sulfur atom, and the alumina filler (C) is a surface-treated alumina filler that has been surface-treated with a silane coupling agent (SC2) having an organic reactive group containing an oxygen atom, a nitrogen atom, or a sulfur atom, which is different from the organic reactive group of the silane coupling agent (SC1), the resin composition film did not show any poor appearance even without kneading using a three-roll mill. By using such a configuration, it can be said that a resin composition with particularly excellent filler dispersibility was obtained.
Claims
1. A resin composition comprising: (A) an epoxy resin; (B) an aluminum nitride filler; and (C) an alumina filler; wherein the aluminum nitride filler (B) and the alumina filler (C) are contained in a total of 800 to 1,800 parts by mass per 100 parts by mass of the epoxy resin (A); the epoxy resin (A) comprises a solid epoxy resin (A-1) and a liquid epoxy resin (A-2); the aluminum nitride filler (B) has an average particle size D50 of 0.2 to 3 μm and a maximum particle size Dmax of 5 μm or less; and the alumina filler (C) has an average particle size D50 of 0.05 to 1.5 μm.
2. The resin composition according to claim 1, wherein the aluminum nitride filler (B) is a surface-treated aluminum nitride filler that has been surface-treated with a silane coupling agent (SC1) having an organic reactive group containing an oxygen atom, a nitrogen atom, or a sulfur atom; the alumina filler (C) is a surface-treated alumina filler that has been surface-treated with a silane coupling agent (SC2) having an organic reactive group containing an oxygen atom, a nitrogen atom, or a sulfur atom different from the organic reactive group possessed by the silane coupling agent (SC1); and the average particle size D50 of the aluminum nitride filler (B) is larger than the average particle size D50 of the alumina filler (C).
3. The aluminum nitride filler (B) is a surface-treated aluminum nitride filler that has been surface-treated with a silane coupling agent (SC1) having an organic reactive group including a (meth)acrylic group, and the alumina filler (C) has an average particle diameter D50 (μm) and a specific surface area SA (m 2 3. The resin composition according to claim 2, wherein the alumina filler (C0) having a product of 2.6 or more with respect to carboxyl group and carboxyl group (g) is a surface-treated alumina filler that has been surface-treated with a silane coupling agent (SC2) having an organic reactive group containing an amino group of a secondary amine structure, the organic reactive group being different from the organic reactive group possessed by the silane coupling agent (SC1).
4. The average particle size D50 (μm) of the alumina filler (C0) and the crystallite size L calculated from the half-width of the diffraction peak due to the (104) plane obtained by X-ray diffraction measurement 104 (μm) (D50 / L 104 4. The resin composition according to claim 3, wherein the modulus of elasticity is 6.0 or more.
5. The resin composition according to claim 3, wherein the ratio (D90 / D10) of the 90% particle diameter D90 to the 10% particle diameter D10 calculated from the volume-based cumulative particle size distribution in the alumina filler (C0) is 2.3 or less.
6. The aluminum nitride filler (B) is a surface-treated aluminum nitride filler that has been surface-treated with a silane coupling agent (SC1) having an organic reactive group including an epoxy group, and the alumina filler (C) has an average particle diameter D50 (μm) and a specific surface area SA (m 2 3. The resin composition according to claim 2, wherein the alumina filler (C0) having a product of (A / g) of less than 2.6 is a surface-treated alumina filler that has been surface-treated with a silane coupling agent (SC2) having an organic reactive group containing an amino group of a secondary amine structure, the organic reactive group being different from the organic reactive group possessed by the silane coupling agent (SC1).
7. The average particle size D50 (μm) of the alumina filler (C0) and the crystallite size L calculated from the half-width of the diffraction peak due to the (104) plane obtained by X-ray diffraction measurement 104 (μm) (D50 / L 104 7. The resin composition according to claim 6, wherein the modulus of elasticity is 6.0 or less.
8. The resin composition according to claim 2, wherein the silane coupling agent (SC2) has an organic reactive group containing a phenylamino group.
9. The specific surface area SA of the aluminum nitride filler (B) is 0.5 to 10 m 2 / g, and the specific surface area SA of the alumina filler (C) is 1 to 50 m 2 The resin composition according to claim 1 , wherein the molecular weight of the resin composition is 100% or more.
10. The resin composition according to claim 1, wherein the ratio (S2 / S1) of the total surface area S1 of said aluminum nitride filler (B) to the total surface area S2 of said alumina filler (C) is 0.5 to 2.
2.
11. A resin composition film comprising the resin composition according to any one of claims 1 to 10.
12. A multilayer printed wiring board comprising the resin composition according to any one of claims 1 to 10 or a cured product thereof.
13. A component-embedded substrate comprising the resin composition according to any one of claims 1 to 10 or a cured product thereof.
Citation Information
Patent Citations
FINE alpha-ALUMINA PARTICLE
JP2007055888A
Epoxy resin composition
JP2011132507A
Resin composition
WO2014208352A1
Resin composition, resin sheet, resin sheet cured product, resin sheet laminate, resin sheet laminate cured product and method for producing the same, semiconductor device and LED device
JP2017066336A
Resin composition
JP2019077758A
Cited By
Resin composition film
WO2026004520A1
Epoxy resin composition, cured object, semiconductor device, and method for producing semiconductor device
WO2026034369A1
Epoxy resin composition, cured object, underfill material, adhesive, and semiconductor package and production method therefor
WO2026100491A1