Metal oxide particle having core-shell structure and method for producing same
Core-shell metal oxide particles with a titanium oxide core and another metal oxide shell, partially exposed and forming a P-O-Ti bond, address the limitations of conventional plastic lenses by enhancing scratch resistance and weatherability while maintaining a high refractive index, thus improving the performance of plastic eyeglass lenses.
Patent Information
- Application Number
- PCT/JP2024/015238
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-05-16
- Filing Date
- 2024-04-17
- Publication Date
- 2024-11-21
AI Technical Summary
Conventional plastic eyeglass lenses suffer from insufficient hardness, scratch resistance, electrostatic charging, dustiness, water absorption, and poor heat resistance, limiting their application due to their low refractive index and photoactivity issues when mixed with titanium oxide-based coatings.
Development of core-shell metal oxide particles with a titanium oxide core and a shell of another metal oxide, where the core is partially exposed, forming a P-O-Ti bond upon contact with a P-OH compound, and having a refractive index of 1.85 or more, to enhance scratch resistance and weatherability while maintaining high refractive index.
The core-shell structure improves the scratch resistance and weather resistance of the lenses while maintaining a high refractive index, preventing excessive shell particle accumulation and ensuring the refractive index remains within the desired range of 1.85 to 2.30.
Smart Images

Figure JP2024015238_21112024_PF_FP_ABST
Abstract
Description
Metal oxide particles having a core-shell structure and a method for producing the same
[0001] The present invention relates to modified metal oxide particles in which metal oxide particles containing titanium oxide are used as cores and are coated with metal oxide particles other than titanium oxide, and to a method for producing such particles.
[0002] Plastic molded products are used in large quantities due to their advantages such as light weight, easy processability, and impact resistance, but on the other hand, they have practical drawbacks for use as eyeglass lenses, window materials, etc., such as insufficient hardness, susceptibility to scratches, susceptibility to solvent attack, electrostatic charge and dust attraction, and insufficient heat resistance. Therefore, it has been proposed to apply a protective coating to plastic molded products. A large number of types of coating solutions for forming the protective coating have been proposed.
[0003] A coating solution for forming a film, whose main component (resin component or film-forming component) is an organosilicon compound or its hydrolyzate, is used for forming a hard film similar to that of an inorganic system for eyeglass lenses (see Patent Document 1).
[0004] Since the abrasion resistance of the above-mentioned coating solution for forming a film is still unsatisfactory, a solution containing colloidally dispersed silica sol has been proposed and has been put to practical use for eyeglass lenses (see Patent Document 2).
[0005] Incidentally, most conventional plastic eyeglass lenses have been manufactured by cast polymerization of diethylene glycol bisallyl carbonate monomer. This lens has a refractive index of approximately 1.50, which is lower than the refractive index of glass lenses, approximately 1.52, and therefore has the disadvantage that the rim thickness of lenses for myopia is thick. For this reason, in recent years, development has been underway to develop monomers with refractive indices higher than diethylene glycol bisallyl carbonate, and high-refractive-index resin materials with refractive indices ranging from 1.54 to 1.76 have been proposed (see Patent Documents 3 and 4).
[0006] For such high refractive index resin lenses, a method has been proposed in which a colloidal dispersion of metal oxide fine particles of Sb or Ti is used as a coating material (see Patent Documents 5 and 6).
[0007] Also disclosed is a coating composition comprising a silane coupling agent and a stable modified metal oxide sol having a primary particle size of 2 to 100 nm, the coating comprising metal oxide colloid particles (a) having a primary particle size of 2 to 60 nm as a core, and particles (c) obtained by coating the surface of the core with a coating (b) consisting of colloidal particles of an acidic oxide, the coating containing (c) being 2 to 50 mass % in terms of metal oxide. Specific examples of colloidal particles that can be used include a modified titanium oxide-zirconium oxide-stannic oxide composite colloid coated with alkylamine-containing antimony pentoxide (see Patent Document 7). Also disclosed is a titanium oxide-stannic oxide-zirconium oxide composite colloid stabilized with alkylamine and oxycarboxylic acid (see Patent Document 8).
[0008] JP-A-52-16586 JP-A-53-111336 JP-A-55-13747 JP-A-64-54021 1986-151801 JP 63-275682 JP 2001-123115 JP 10-306258
[0009] The present invention provides modified core-shell metal oxide particles, which are used in compositions for obtaining coated articles with high refractive index and high moldability, such as for nanoimprinting, and which have a core made of titanium oxide-containing metal oxide particles and a shell made of metal oxide particles other than titanium oxide, with the core coated and part of the core exposed, as well as a method for producing the same.
[0010] In a first aspect, the present invention provides core-shell type metal oxide particles comprising a core comprising metal oxide particles having an average primary particle diameter of 3 to 100 nm, and a shell comprising metal oxide particles having an average primary particle diameter of 1 to 7 nm coating the surface of the core, wherein the average primary particle diameters satisfy the relationship (metal oxide particles of the core) > (metal oxide particles of the shell), and when component (a) is titanium oxide and component (b) is a metal oxide other than titanium oxide, the core is a particle comprising component (a) or a combination of components (a) and (b), and the shell is a particle comprising component (b), and the core satisfies the following requirements A and B: Requirement A: In a test in which the core-shell type metal oxide particles are brought into contact with a compound having a P—OH bond, the formation of a P—O—Ti bond in the core-shell type metal oxide particles is observed by NMR, and Requirement B: The refractive index of the core-shell type metal oxide particles is 1.85 or more. As a second aspect, the core-shell type metal oxide particle according to the first aspect, in which the component (b) is at least one metal oxide particle selected from the group consisting of zirconium oxide, silicon dioxide, aluminum oxide, tin oxide, zinc oxide, iron oxide, niobium oxide, tantalum oxide, antimony oxide, and tungsten oxide; as a third aspect, the core-shell type metal oxide particle according to the first or second aspect, in which the mass ratio of (metal oxide other than titanium oxide) / (titanium oxide) is in the range of 0.05 to 1.0; as a fourth aspect, the core-shell type metal oxide particle according to any one of the first to third aspects, in which an intermediate layer is present between the core particle and the shell particle, and the intermediate layer is metal oxide particle composed of a combination of at least one metal oxide particle selected from the group consisting of zirconium oxide, silicon dioxide, aluminum oxide, tin oxide, zinc oxide, iron oxide, niobium oxide, tantalum oxide, antimony oxide, and tungsten oxide as the component (D), in which the mass ratio of (metal oxide other than titanium oxide) / (titanium oxide) is in the range of 0.05 to 1.0; According to a fifth aspect, the core-shell type metal oxide particles according to any one of the first to fourth aspects, in which the surfaces of the core-shell type metal oxide particles are coated with a compound having a P—OH bond or a Si—OH bond. According to a sixth aspect, the compound having a Si—OH bond is represented by any one of formulas (1) to (3):
[0011]
[0012] (In formula (1), R 1 are each an alkyl group, a halogenated alkyl group, an alkenyl group, an aryl group, or an organic group having a polyether group, an epoxy group, a (meth)acryloyl group, a mercapto group, an amino group, a ureido group, or a cyano group, and are bonded to a silicon atom by a Si—C bond, and R 2 represents an alkoxy group, an acyloxy group, or a halogen group, and a represents an integer of 1 to 3. In formulas (2) and (3), R 3 and R 5 are each an alkyl group having 1 to 3 carbon atoms or an aryl group having 6 to 30 carbon atoms and bonded to a silicon atom by a Si—C bond, and R 4 and R 6 each represents an alkoxy group, an acyloxy group, or a halogen group; Y represents an alkylene group, an NH group, or an oxygen atom; b is an integer of 1 to 3; c is an integer of 0 or 1; and d is an integer of 1 to 3.) The core-shell type metal oxide particles according to any one of the first to fifth aspects, wherein the compound having a P—OH bond is at least one silane compound selected from the group consisting of formulas (4) to (6):
[0013]
[0014] (In formulas (4) to (6), X 1 , X 2 , and X 3 each represents an alkylene group having 2 to 20 carbon atoms; f, h, and j each represent an integer of 1 to 100; e, g, and i each represent an integer of 1 to 3; Y 1 , Y 2 , and Y 3represents a hydrogen atom, an alkyl group having 1 to 20 carbon atoms, an alkenyl group having 2 to 20 carbon atoms, an aryl group having 6 to 30 carbon atoms, or a (meth)acrylic group. the core-shell type metal oxide particles according to any one of the first to fifth aspects, wherein the phosphate ester is at least one kind of phosphate ester selected from the group consisting of: an eighth aspect, the core-shell type metal oxide particles according to the seventh aspect, wherein the phosphate ester is a polyoxyethylene alkyl (C6-20) ether phosphate ester having an alkyl group having 6 to 20 carbon atoms; a ninth aspect, a core-shell type metal oxide sol obtained by dispersing the core-shell type metal oxide particles according to any one of the first to eighth aspects as a dispersoid in a dispersion medium comprising an alcohol, ester, ketone, amide, hydrocarbon, silicone, a compound containing an unsaturated bond between linear carbon atoms, an oxirane compound, water, or a combination thereof, the core-shell type metal oxide sol having an average particle size of 5 to 500 nm as measured by a dynamic light scattering method; and a tenth aspect, the core-shell type metal oxide sol according to the ninth aspect, further comprising a surfactant, wherein the surfactant is an anionic surfactant, a cationic surfactant, a nonionic surfactant, or an amphoteric surfactant. As an eleventh aspect, the core-shell metal oxide sol according to the ninth or tenth aspect further contains a secondary amine or a tertiary amine having a total of 5 to 35 carbon atoms; as a twelfth aspect, a varnish containing the core-shell metal oxide particles according to any one of the first to eighth aspects and a thermosetting or photocurable resin; as a thirteenth aspect, the varnish according to the twelfth aspect, which is a hard coating agent or a composition for nanoimprints; as a fourteenth aspect, the present invention provides a method for producing a core-shell metal oxide sol comprising the steps of: (i) preparing a sol (A) containing metal oxide particles having an average primary particle diameter of 3 to 60 nm as a dispersion medium, and (B) containing metal oxide particles having an average primary particle diameter of 1 to 7 nm as a dispersion medium, in water; (ii) step: mixing the sol (A) and the sol (B) at a rate of 22 to 1000 parts by mass per minute of the solid content of one of the sols charged in the container relative to 100 parts by mass of the solid content of the other sol;As a fifteenth aspect, there is provided a method for producing a core-shell type metal oxide sol according to the fourteenth aspect, in which step (i) or step (ii) further includes step (S-1): adding a secondary amine or a tertiary amine having a total of 5 to 35 carbon atoms to the aqueous sol. As a sixteenth aspect, there is provided a method for producing a core-shell type metal oxide sol according to the fourteenth or fifteenth aspect, in which step (ii) is followed by at least one step selected from step (T-1), step (T-2), and step (T-3). Step (T-1): adding at least one silane compound selected from the group consisting of formulae (1) to (3) or at least one phosphoric acid ester selected from the group consisting of formulae (4) to (6) to the core-shell type metal oxide sol obtained in step (ii). Step (T-2): replacing the dispersion medium of the core-shell type metal oxide sol obtained in step (ii) with a dispersion medium consisting of an alcohol, an ester, a ketone, an amide, or a hydrocarbon. Step (T-3): adding a surfactant to the core-shell metal oxide sol obtained in step (ii); and According to a seventeenth aspect, there is provided the method for producing a core-shell metal oxide sol according to any one of the fourteenth to sixteenth aspects, in which the steps are step (i), step (S-1), step (ii), step (S-1), step (T-2), step (T-1), and step (T-2), in that order.
[0015] The present invention provides modified metal oxide particles in which a core is made of titanium oxide-containing metal oxide particles and a shell is made of metal oxide particles other than titanium oxide. Titanium oxide has a high refractive index and is therefore used as a high refractive index material. However, because titanium oxide particles are highly photoactive, when mixed with various binders or resin components as a matrix component, discoloration or deterioration of the matrix component may occur.
[0016] Core-shell type modified metal oxide particles have been proposed in which titanium oxide particles are coated with metal oxide particles other than titanium oxide to suppress photoactivity. When titanium oxide particles or metal oxide particles containing titanium oxide particles, which form the core of the core-shell type metal oxide particles, are coated with metal oxide particles other than titanium oxide, which form the shell, complete coating may reduce the proportion of titanium oxide components, and the refractive index of the core-shell type metal oxide particles may not be improved.
[0017] In the present invention, in order to maintain a high refractive index in the core-shell type metal oxide particles, the core particles are not completely covered with shell particles, but rather core-shell type modified metal oxide particles are provided in which a part of the core particle surface is exposed. The part of the core is exposed because, in a test in which the core-shell type metal oxide particles are brought into contact with a compound having a P-OH bond, formation of a P-O-Ti bond is observed in the core-shell type metal oxide particles. 31 By observing the P-NMR spectrum, it can be determined that a P—O—Ti bond is present, and it can be confirmed that the particles are core-shell type metal oxide particles in which part of the core is exposed.
[0018] In the core-shell metal oxide particles of the present invention, the core-shell metal oxide particles have a part of the core particle surface exposed. When particle A having a part of the core particle surface exposed and a similar particle B are coated on a substrate or on the irregularities of the substrate surface, the exposed part of the core particle interacts with the part of the shell particle, and the coated material and filler function as an integrated mass, and for example, when coated on a substrate, the weather resistance is improved.
[0019] Furthermore, when a high refractive index material is prepared by combining core particles having a higher refractive index than shell particles and shell particles having a lower refractive index than core particles, a sol containing core-shell metal oxide particles with a portion of the core particle surface exposed does not contain excess shell particles, and therefore when such a sol is used to prepare a coating or filler, it is possible to suppress a decrease in the refractive index of the coating or filler after curing. In the present invention, the refractive index of the core-shell metal oxide particles is 1.85 or more, and can be, for example, in the range of 1.85 to 2.30.
[0020] The core-shell metal oxide particles in the methanol solvent dispersion sol used in Example 1 were 31 The presence or absence of P-O-Ti bonds was confirmed by P-NMR. 31 P-NMR spectrum. The metal oxide particles having only the core in the methanol solvent dispersion sol used in Comparative Example 1 were 31 The presence or absence of P-O-Ti bonds was confirmed by P-NMR. 31 P-NMR spectrum of the core-shell metal oxide particles in the methanol solvent dispersion sol used in Comparative Example 3. 31 The presence or absence of P-O-Ti bonds was confirmed by P-NMR. 31 P-NMR spectrum.
[0021] The present invention provides core-shell type metal oxide particles comprising a core comprising metal oxide particles with an average primary particle diameter of 3 to 60 nm, and a shell covering the surface of the core and comprising metal oxide particles with an average primary particle diameter of 1 to 7 nm, wherein the average primary particle diameters satisfy the relationship (core metal oxide particles) > (shell metal oxide particles), and when component (a) is titanium oxide and component (b) is a metal oxide other than titanium oxide, the core is a particle comprising component (a) or a combination of components (a) and (b), and the shell is a particle comprising component (b), and the core-shell type metal oxide particles satisfy the following requirements A and B: Requirement A: In a test in which the core-shell type metal oxide particles are brought into contact with a compound having a P—OH bond, the formation of a P—O—Ti bond in the core-shell type metal oxide particles is observed by NMR, and Requirement B: The refractive index of the core-shell type metal oxide particles is 1.85 or more. In the present invention, the refractive index of the core-shell type metal oxide particles is 1.85 or more, and for example, core-shell type metal oxide particles having a refractive index in the range of 1.85 to 2.30 can be obtained.
[0022] The component (a) can be titanium oxide, and the component (b) can be at least one metal oxide particle selected from the group consisting of zirconium oxide, silicon dioxide, aluminum oxide, tin oxide, zinc oxide, iron oxide, niobium oxide, tantalum oxide, antimony oxide, and tungsten oxide.
[0023] The core particle is preferably a particle composed of component (a) or a combination of component (a) and component (b), and examples thereof include titanium oxide particles, composite particles of titanium oxide particles and tin oxide particles, composite particles of titanium oxide particles and zirconium oxide particles, and composite particles of titanium oxide particles, tin oxide particles, and zirconium oxide particles.
[0024] The shell particles are preferably particles made of component (b), and can be, for example, particles of at least one metal oxide selected from the group consisting of zirconium oxide, silicon dioxide, aluminum oxide, tin oxide, zinc oxide, iron oxide, niobium oxide, tantalum oxide, antimony oxide, and tungsten oxide.
[0025] For example, core-shell metal oxide particles comprising a combination of a core particle and a shell particle include combinations of core particle / shell particle such as titanium oxide particle / composite particle of tin oxide and silicon dioxide, composite particle of titanium oxide and tin oxide / composite particle of tin oxide and silicon dioxide, composite particle of titanium oxide particle and zirconium oxide particle / composite particle of tin oxide and silicon dioxide, composite particle of titanium oxide particle, tin oxide particle and zirconium oxide particle / composite particle of tin oxide and silicon dioxide, titanium oxide particle / antimony oxide particle, and composite particle of titanium oxide and tin oxide / antimony oxide particle.
[0026] The core-shell type metal oxide particles are obtained with a mass ratio of (metal oxide other than titanium oxide) / (titanium oxide) in the range of 0.05 to 1.0, or 0.1 to 1.0, or 0.15 to 1.0.
[0027] In the present invention, an intermediate layer exists between the core particle and the shell particle, and the intermediate layer is a metal oxide particle comprising a combination of at least one selected from the group consisting of zirconium oxide, silicon dioxide, aluminum oxide, tin oxide, zinc oxide, iron oxide, niobium oxide, tantalum oxide, antimony oxide, and tungsten oxide as component (D), and the mass ratio of (metal oxide other than titanium oxide) / (titanium oxide) can be set within the range of 0.05 to 1.0, or 0.1 to 1.0, or 0.15 to 1.0. Core-shell metal oxide particles and metal oxide particles having an intermediate layer between the core particle and the shell particle are tested for the formation of P-O-Ti bonds in a test in which the oxide particles are brought into contact with a compound having a P-OH bond. 31 This is observed by P-NMR spectrum. This indicates that a P-O-Ti bond exists between the core particle and the compound having a P-OH bond, and confirms that the particles are core-shell type metal oxide particles in which a part of the core is exposed. This indicates that the core particle is partially exposed in core-shell type metal oxide particles and metal oxide particles in which an intermediate layer exists between the core particle and the shell particle.
[0028] Examples of metal oxide particles used for the core include titanium oxide, titanium oxide-tin oxide composite oxide, titanium oxide-zirconium oxide composite oxide, and titanium oxide-zirconium oxide-tin oxide composite oxide. These particles have an average primary particle diameter of 5 to 500 nm, 5 to 300 nm, 5 to 250 nm, or 5 to 60 nm, as determined by transmission electron microscope observation, and preferably have an average primary particle diameter of 3 to 100 nm, 3 to 80 nm, 3 to 60 nm, 3 to 40 nm, 3 to 20 nm, or 5 to 40 nm. For example, examples of metal oxide particles used for the coating include particles of at least one metal oxide selected from the group consisting of zirconium oxide, silicon dioxide, aluminum oxide, tin oxide, zinc oxide, iron oxide, niobium oxide, tantalum oxide, antimony oxide, and tungsten oxide. These particles have an average primary particle diameter of 1 to 10 nm, 1 to 7 nm, or 1 to 5 nm, as determined by transmission electron microscope observation.
[0029] Examples of the metal oxide particles include metal oxide particles in which the above-mentioned silicon dioxide, tin oxide, antimony oxide, tungsten oxide, aluminum oxide, and zirconium oxide are present alone, or composite metal oxide particles in which a plurality of the above-mentioned metal oxides are bonded together. Examples of the composite metal oxide particles include tin oxide-silicon dioxide composite metal oxide particles, tin oxide-zirconium oxide-silicon dioxide composite metal oxide particles, tin oxide-tungsten oxide-silicon dioxide composite metal oxide particles, and antimony oxide-silicon dioxide composite metal oxide particles. When the metal oxide particles used for coating contain silicon dioxide, the ratio of silicon dioxide to other metal oxides can be set to a (silicon dioxide) / (other metal oxide) mass ratio of 0.1 to 5.0.
[0030] When a core-shell structure is used, coating with metal oxide particles having a different metal oxide component or a different metal oxide content from the metal oxide of the core (core) can include cases where the metal oxide components of the core and the coating are different, or cases where the metal oxide components of the core and the coating partially overlap but the blending ratios of the metal oxides are different. In the case of a core-shell structure, the mass ratio of the core metal oxide particles to the coating metal oxide particles can be set in the range of (coated metal oxide particles) / (core metal oxide particles) = 0.05 to 0.40. For example, in the case of a tin oxide-silicon dioxide composite oxide used for coating, sodium stannate or potassium stannate can be used as the alkali stannate, with sodium stannate being preferred.
[0031] As the alkali silicate, sodium silicate or potassium silicate can be used. The alkali stannate and alkali silicate are prepared as an aqueous solution containing silicon dioxide / stannic oxide in a mass ratio of 0.1 to 5, and then the cations present in the aqueous solution can be removed using a cation exchange resin. The alkali stannate and alkali silicate are measured and dissolved in water so that the mass ratio of silicon dioxide / stannic oxide is 0.1 to 5.0. The preferred solids concentration of the aqueous solution is (SnO 2 +SiO 2) is 1 to 12 mass %. The prepared aqueous solution is subjected to cation exchange resin removal of cations. A hydrogen-type strongly acidic cation exchange resin is preferred as the cation exchange resin, and for example, Amberlite (trade name) 120B or the like can be used by packing it in a column. By carrying out this cation exchange, the silicic acid component and the stannic acid component are polymerized, and silicon dioxide-stannic oxide composite colloidal particles having an average primary particle size of 1 to 4 nm can be produced.
[0032] The silicon dioxide-stannic oxide composite colloidal particles are poorly stable and gel within a few hours of standing. Therefore, after the cation exchange, an amine compound is quickly added to stabilize the particles, resulting in a silicon dioxide / stannic oxide composite colloidal particle having a mass ratio of 0.1 to 5.0 and an M / (SnO 2 +SiO 2 It is necessary to obtain an aqueous sol of silicon dioxide-stannic oxide composite oxide colloidal particles having an average primary particle size of 1 to 4 nm stabilized by an amine compound present in a molar ratio of (SnO 2 +SiO 2 ) is 0.1 to 10 mass %. For stabilization of the silicon dioxide-stannic oxide composite colloidal particles produced by the cation exchange, M / (SnO 2 +SiO 2 It is appropriate to add the amine compound in an amount such that the molar ratio of M / (SnO) (where M represents an amine compound) is 0.1 to 1.0. 2 +SiO 2 Addition of an amine compound in which the molar ratio of 1 to 2 is less than 0.1 to 1.0 is not preferred because the composition loses stability and gels after standing for several hours.
[0033] Next, an aqueous sol of metal oxide colloid particles (a) for use in the core, having an average primary particle size of 5 to 60 nm, and a silicon dioxide / stannic oxide mass ratio of 0.1 to 5.0 and an M / (SnO 2 +SiO 2The aqueous sol of modified metal oxide colloid particles (a) is obtained by mixing an aqueous sol of silicon dioxide-stannic oxide composite oxide colloid particles (b) used for the shell having an average primary particle size of 1 to 4 nm, stabilized with an amine compound in a molar ratio of (a) / (b) (where M represents an amine compound), at a mass ratio of (b) / (a) of 0.05 to 0.40, thereby obtaining an aqueous sol of modified metal oxide colloid particles in which the metal oxide colloid particles (a) are coated with the silicon dioxide-stannic oxide composite oxide colloid particles (b). The solids concentration of the aqueous sol of the metal oxide colloid particles (a) is 0.5 to 50 mass%, and preferably 5 to 30 mass%.
[0034] The aqueous sol of the metal oxide colloidal particles (a) can have a pH of 5 to 11.5, preferably 7 to 11.5. The pH of the aqueous sol can be adjusted as needed with an alkaline component. Examples of the alkaline component include hydroxides of alkali metals such as lithium, sodium, and potassium; hydroxides of alkaline earth metals such as calcium, magnesium, and strontium; ammonia; alkylamines such as ethylamine, triethylamine, isopropylamine, and n-propylamine; aralkylamines such as benzylamine; alicyclic amines such as piperidine; alkanolamines such as monoethanolamine and triethanolamine; and quaternary ammonium hydroxides. The aqueous sol of the metal oxide colloidal particles (a) and the aqueous sol of the coated particles (b) are preferably mixed under stirring.
[0035] The mixing ratio of the silicon dioxide-stannic oxide composite oxide colloid particles (b) to the metal oxide colloid particles (a) is preferably 0.05 to 0.40 in terms of mass ratio (b) / (a). If the mass ratio is less than 0.05, the metal oxide colloid particles (a), which serve as cores, cannot be sufficiently coated with the silicon dioxide-stannic oxide composite oxide colloid particles (b), and a stable hydrophilic organic solvent dispersion sol or a hydrophobic organic solvent dispersion sol having a water solubility of 0.05 to 12% by mass cannot be obtained. Furthermore, a mass ratio of 0.40 or more is sufficient, and complete coating may be achieved. Next, the resulting aqueous sol of modified metal oxide colloid particles is subjected to cation exchange. For the cation exchange, a hydrogen-type strongly acidic cation exchange resin is preferably used.
[0036] Next, the resulting aqueous sol was treated with a molar ratio of M / (SnO 2 +SiO 2 The amount of the amine compound added is such that the ratio M / (SnO 2 +SiO 2 If the molar ratio of M / (SnO) is less than 0.001, the dispersion stability of the hydrophilic organic solvent dispersion sol of the present invention becomes insufficient, which is not preferable. 2 +SiO 2 If the molar ratio of the silane compound to the surface of the modified metal oxide colloidal particles exceeds 0.08, this may hinder bonding. The metal oxide particles of the present invention are obtained via a metal oxide sol. The metal oxide sol can be obtained by the following method.
[0037] The method for producing a core-shell metal oxide sol includes the following steps (i) and (ii): step (i): preparing a sol (A) containing metal oxide particles having an average primary particle size of 3 to 60 nm as a dispersion medium, and a sol (B) containing metal oxide particles having an average primary particle size of 1 to 7 nm as a dispersion medium, and step (ii): mixing the sol (A) and the sol (B) at a rate of 22 to 1,000 parts by mass, 22 to 500 parts by mass, or 22 to 100 parts by mass per minute of 100 parts by mass of the solids content of one sol charged in a container, or 22 to 500 parts by mass, or 22 to 100 parts by mass per minute of 100 parts by mass of the solids content of the other sol. Sol (A) is an aqueous sol containing the core particles, and sol (B) is an aqueous sol containing the shell particles. In the present invention, the above step (i) or step (ii) may further include step (S-1): a step of adding a secondary amine or a tertiary amine having a total of 5 to 35 carbon atoms to the aqueous sol.
[0038] Furthermore, in the present invention, at least one step selected from steps (T-1), (T-2), and (T-3) can be added after step (ii) above. Step (T-1) is a step of adding at least one silane compound selected from the group consisting of formulas (1) to (3) or at least one phosphate ester selected from the group consisting of formulas (4) to (6) to the core-shell metal oxide sol obtained in step (ii). Step (T-2) is a step of solvent-substituting the dispersion medium of the core-shell metal oxide sol obtained in step (ii) with a dispersion medium consisting of an alcohol, ester, ketone, amide, or hydrocarbon. Step (T-3) is a step of adding a surfactant to the core-shell metal oxide sol obtained in step (ii).
[0039] In the present invention, the steps can be arranged in the order of step (i), step (S-1), step (ii), step (S-1), step (T-2), step (T-1), and step (T-2).
[0040] Furthermore, the step (T-3) can be added to any step.
[0041] The present invention can further contain a secondary amine or a tertiary amine having a total carbon atom number of 5 to 35. The content of the amine is determined by the SiO 2 The amount of the secondary amine can be set to 0.01 to 10.0 mmol, or 0.01 to 5.0 mmol per 100 g of the solvent. Examples of the secondary amine include ethyl-n-propylamine, ethylisopropylamine, dipropylamine, diisopropylamine, ethylbutylamine, n-propylbutylamine, dibutylamine, ethylpentylamine, n-propylpentylamine, isopropylpentylamine, dipentylamine, ethyloctylamine, i-propyloctylamine, butyloctylamine, and dioctylamine.
[0042] Examples of the tertiary amine include triethylamine, ethyl di-n-propylamine, diethyl n-propylamine, tri-n-propylamine, triisopropylamine, ethyl dibutylamine, diethyl butylamine, isopropyl dibutylamine, diisopropyl ethylamine, diisopropyl butylamine, tributylamine, ethyl dipentylamine, diethyl pentylamine, tripentylamine, methyl dioctylamine, dimethyl octylamine, ethyl dioctylamine, diethyl octylamine, trioctylamine, benzyl dibutylamine, diazabicycloundecene, etc. Among the above amines, secondary amines and tertiary amines having an alkyl group having a total of 6 to 35 carbon atoms are preferred, such as diisopropylamine, tripentylamine, triisopropylamine, dimethyl octylamine, trioctylamine, etc.
[0043] In the present invention, the silane compound is a silane coupling agent, and the photoactive metal oxide particles (A) can be coated with a hydrolyzate of at least one silane compound selected from the group consisting of formulas (1) to (3). The obtained hydrophilic organic solvent dispersion sol can be coated with a hydrolyzate of at least one silane compound selected from the group consisting of formulas (1) to (3). In formula (1), R 1are each an alkyl group, a halogenated alkyl group, an alkenyl group, an aryl group, or an organic group having a polyether group, an epoxy group, a (meth)acryloyl group, a mercapto group, an amino group, a ureido group, or a cyano group, and are bonded to a silicon atom by a Si—C bond, and R 2 represents an alkoxy group, an acyloxy group, or a halogen group, and a represents an integer of 1 to 3. In formulas (2) and (3), R 3 and R 5 are each an alkyl group having 1 to 3 carbon atoms or an aryl group having 6 to 30 carbon atoms and bonded to a silicon atom by a Si—C bond, and R 4 and R 6 each represents an alkoxy group, an acyloxy group, or a halogen group; Y represents an alkylene group, an NH group, or an oxygen atom; b is an integer of 1 to 3; c is an integer of 0 or 1; and d is an integer of 1 to 3.
[0044] The alkyl group is an alkyl group having 1 to 18 carbon atoms, and examples thereof include a methyl group, an ethyl group, an n-propyl group, an i-propyl group, a cyclopropyl group, an n-butyl group, an i-butyl group, an s-butyl group, a t-butyl group, a cyclobutyl group, a 1-methyl-cyclopropyl group, a 2-methyl-cyclopropyl group, an n-pentyl group, a 1-methyl-n-butyl group, a 2-methyl-n-butyl group, a 3-methyl-n-butyl group, a 1,1-dimethyl-n-propyl group, a 1,2-dimethyl-n-propyl group, a 2,2-dimethyl-n-propyl group, a 1-ethyl- n-propyl group, cyclopentyl group, 1-methyl-cyclobutyl group, 2-methyl-cyclobutyl group, 3-methyl-cyclobutyl group, 1,2-dimethyl-cyclopropyl group, 2,3-dimethyl-cyclopropyl group, 1-ethyl-cyclopropyl group, 2-ethyl-cyclopropyl group, n-hexyl group, 1-methyl-n-pentyl group, 2-methyl-n-pentyl group, 3-methyl-n-pentyl group, 4-methyl-n-pentyl group, 1,1-dimethyl-n-butyl group, 1,2-dimethyl-n-butyl group, 1,3-dimethyl-n-butyl group , 2,2-dimethyl-n-butyl group, 2,3-dimethyl-n-butyl group, 3,3-dimethyl-n-butyl group, 1-ethyl-n-butyl group, 2-ethyl-n-butyl group, 1,1,2-trimethyl-n-propyl group, 1,2,2-trimethyl-n-propyl group, 1-ethyl-1-methyl-n-propyl group, 1-ethyl-2-methyl-n-propyl group, cyclohexyl group, 1-methyl-cyclopentyl group, 2-methyl-cyclopentyl group, 3-methyl-cyclopentyl group, 1-ethyl-cyclobutyl group, 2-ethyl-cyclobutyl group group, 3-ethyl-cyclobutyl group, 1,2-dimethyl-cyclobutyl group, 1,3-dimethyl-cyclobutyl group, 2,2-dimethyl-cyclobutyl group, 2,3-dimethyl-cyclobutyl group, 2,4-dimethyl-cyclobutyl group, 3,3-dimethyl-cyclobutyl group, 1-n-propyl-cyclopropyl group, 2-n-propyl-cyclopropyl group, 1-i-propyl-cyclopropyl group, 2-i-propyl-cyclopropyl group, 1,2,2-trimethyl-cyclopropyl group, 1,2,3-trimethyl-cyclopropyl group, 2,2,Examples of the alkylene group include, but are not limited to, 3-trimethylcyclopropyl, 1-ethyl-2-methylcyclopropyl, 2-ethyl-1-methylcyclopropyl, 2-ethyl-2-methylcyclopropyl, and 2-ethyl-3-methylcyclopropyl groups, as well as hexyl, heptyl, octyl, nonyl, decyl, undecyl, dodecyl, tridecyl, tetradecyl, pentadecyl, hexadecyl, heptadecyl, and octadecyl groups. Examples of the alkylene group include alkylene groups derived from the alkyl groups described above.
[0045] The aryl group is an aryl group having 6 to 30 carbon atoms, and examples thereof include a phenyl group, a naphthyl group, an anthracene group, and a pyrene group. The alkenyl group is an alkenyl group having 2 to 10 carbon atoms, and examples thereof include ethenyl, 1-propenyl, 2-propenyl, 1-methyl-1-ethenyl, 1-butenyl, 2-butenyl, 3-butenyl, 2-methyl-1-propenyl, 2-methyl-2-propenyl, 1-ethylethenyl, 1-methyl-1-propenyl, 1-methyl-2-propenyl, 1-pentenyl, 2-pentenyl, 3-pentenyl, 4-pentenyl, 1-n-propylethenyl, 1-methyl-1-butenyl, 1-methyl-2-butenyl, 1-methyl-3-butenyl, 2-ethyl-2-propenyl, 2-methyl-1-butenyl, 2-methyl-2-butenyl, 2-methyl-3-butenyl, 3 ...2-butenyl, 1-methyl-3-butenyl, 2-methyl-2-propenyl, 2-methyl-3-butenyl, 3-n-propylethenyl, 1-methyl-1-butenyl, 1-methyl-2-butenyl, 1-methyl-3-butenyl, 2-methyl-2-propenyl, 2-methyl-3-butenyl, 3-n-propylethenyl, 1-methyl-2-butenyl, 1-methyl-3-butenyl, 2-methyl-2-butenyl, 2-methyl-3-butenyl, 3-n-propylethenyl Examples of alkyl groups include, but are not limited to, 1-methyl-1-butenyl group, 3-methyl-2-butenyl group, 3-methyl-3-butenyl group, 1,1-dimethyl-2-propenyl group, 1-i-propylethenyl group, 1,2-dimethyl-1-propenyl group, 1,2-dimethyl-2-propenyl group, 1-cyclopentenyl group, 2-cyclopentenyl group, 3-cyclopentenyl group, 1-hexenyl group, 2-hexenyl group, 3-hexenyl group, 4-hexenyl group, 5-hexenyl group, 1-methyl-1-pentenyl group, 1-methyl-2-pentenyl group, 1-methyl-3-pentenyl group, 1-methyl-4-pentenyl group, 1-n-butylethenyl group, 2-methyl-1-pentenyl group, and 2-methyl-2-pentenyl group.
[0046] The alkoxy group includes alkoxy groups having 1 to 10 carbon atoms, such as methoxy, ethoxy, n-propoxy, i-propoxy, n-butoxy, i-butoxy, s-butoxy, t-butoxy, n-pentyloxy, 1-methyl-n-butoxy, 2-methyl-n-butoxy, 3-methyl-n-butoxy, 1,1-dimethyl-n-propoxy, 1,2-dimethyl-n-propoxy, 2,2-dimethyl-n-propoxy, 1-ethyl-n-propoxy, and n-hexyloxy, but is not limited to these.
[0047] Examples of the acyloxy group having 2 to 10 carbon atoms include, but are not limited to, a methylcarbonyloxy group, an ethylcarbonyloxy group, an n-propylcarbonyloxy group, an i-propylcarbonyloxy group, an n-butylcarbonyloxy group, an i-butylcarbonyloxy group, an s-butylcarbonyloxy group, a t-butylcarbonyloxy group, an n-pentylcarbonyloxy group, a 1-methyl-n-butylcarbonyloxy group, a 2-methyl-n-butylcarbonyloxy group, a 3-methyl-n-butylcarbonyloxy group, a 1,1-dimethyl-n-propylcarbonyloxy group, a 1,2-dimethyl-n-propylcarbonyloxy group, a 2,2-dimethyl-n-propylcarbonyloxy group, a 1-ethyl-n-propylcarbonyloxy group, an n-hexylcarbonyloxy group, a 1-methyl-n-pentylcarbonyloxy group, and a 2-methyl-n-pentylcarbonyloxy group. The halogen group includes fluorine, chlorine, bromine, iodine, and the like.
[0048] The organic group having a polyether group includes a polyetherpropyl group having an alkoxy group. For example, (CH 3 O) 3 SiC 3 H 6 (OC 2 H 4 ) nOCH 3n can be in the range of 1 to 100, or 1 to 10. Examples of organic groups having an epoxy group include a 2-(3,4-epoxycyclohexyl)ethyl group and a 3-glycidoxypropyl group. The (meth)acryloyl group refers to both an acryloyl group and a methacryloyl group. Examples of organic groups having a (meth)acryloyl group include a 3-methacryloxypropyl group and a 3-acryloxypropyl group.
[0049] An example of an organic group having a mercapto group is a 3-mercaptopropyl group. Examples of organic groups having an amino group include a 2-aminoethyl group, a 3-aminopropyl group, an N-2-(aminoethyl)-3-aminopropyl group, an N-(1,3-dimethyl-butylidene)aminopropyl group, an N-phenyl-3-aminopropyl group, and an N-(vinylbenzyl)-2-aminoethyl-3-aminopropyl group. An example of an organic group having a ureido group is a 3-ureidopropyl group. An example of an organic group having a cyano group is a 3-cyanopropyl group. Compounds represented by the above formulas (2) and (3) are preferably compounds capable of forming trimethylsilyl groups on the surface of silica particles. Examples of such compounds include the following:
[0050]
[0051] In the above formula, R 12 is an alkoxy group, for example, a methoxy group or an ethoxy group. As the silane compound, a silane compound manufactured by Shin-Etsu Chemical Co., Ltd. can be used. This is a process in which the silane compound reacts with a hydroxyl group on the surface of silica particles, for example, a silanol group in the case of silica particles, to coat the surface of the silica particles with the silane compound through a siloxane bond. The reaction temperature can be from 20°C to the boiling point of the dispersion medium, for example, in the range of 20°C to 100°C. The reaction time can be about 0.1 to 6 hours.
[0052] The silane compound is applied to the surface of the silica particles in such an amount that the number of silicon atoms in the silane compound is 0.1 / nm 2 ~6.0 pieces / nm 2The silica particle surfaces can be coated by adding a silane compound equivalent to the coating amount to the silica sol. Water is required for the hydrolysis of the silane compound, and if the sol is an aqueous solvent, the aqueous solvent can be used. When the aqueous medium is replaced with an organic solvent (C), the remaining water in the solvent can be used. For example, water present in an amount of 0.01 to 1% by mass can be used. Furthermore, hydrolysis can be carried out with or without a catalyst. When carried out without a catalyst, the silica particle surfaces are acidic. When a catalyst is used, examples of hydrolysis catalysts include metal chelate compounds, organic acids, inorganic acids, organic bases, and inorganic bases. Examples of metal chelate compounds used as hydrolysis catalysts include triethoxy mono(acetylacetonato)titanium and triethoxy mono(acetylacetonato)zirconium. Examples of organic acids used as hydrolysis catalysts include acetic acid and oxalic acid. Examples of inorganic acids used as hydrolysis catalysts include hydrochloric acid, nitric acid, sulfuric acid, hydrofluoric acid, and phosphoric acid. Examples of organic bases used as hydrolysis catalysts include pyridine, pyrrole, piperazine, and quaternary ammonium salts. Examples of inorganic bases used as hydrolysis catalysts include ammonia, sodium hydroxide, and potassium hydroxide.
[0053] The organic acid is at least one organic acid selected from the group consisting of divalent aliphatic carboxylic acids, aliphatic oxycarboxylic acids, amino acids, and chelating agents, where the divalent aliphatic carboxylic acids are oxalic acid, malonic acid, and succinic acid, the aliphatic oxycarboxylic acids are glycolic acid, lactic acid, malic acid, tartaric acid, and citric acid, the amino acids are glycine, alanine, valine, leucine, serine, and threonine, and the chelating agents include ethylenediaminetetraacetic acid, L-aspartic acid-N,N-diacetic acid, and diethylenetriaminepentaacetic acid. Examples of organic acid salts include alkali metal salts, ammonium salts, and amine salts of the above organic acids. Examples of alkali metal salts include sodium and potassium.
[0054] The phosphate ester that can be used in the present invention includes at least one phosphate ester compound selected from the group consisting of formulas (4) to (6). 1 , X 2 , and X 3 each represents an alkylene group having 2 to 20 carbon atoms; f, h, and j each represent an integer of 1 to 100; e, g, and i each represent an integer of 1 to 3; Y 1 , Y 2 , and Y 3 Each represents a hydrogen atom, an alkyl group having 1 to 20 carbon atoms, an alkenyl group having 2 to 20 carbon atoms, or a (meth)acrylic group. A polyoxyethylene alkyl (C6-20) ether phosphate ester having an alkyl group having 6 to 20 carbon atoms can be used.
[0055] The phosphate ester is preferably a polyoxyethylene alkyl ether phosphate ester, and the phosphate ester may be one in which the terminal alkyl group (Y1) of the formula (4) has 6 to 10 or 12 to 15 carbon atoms. Examples of such products include products manufactured by Toho Chemical Industry Co., Ltd., under the trade names Phosphanol RA-600 and RS-610. In the present invention, a sol is obtained in which core-shell metal oxide particles are dispersed as a dispersoid in a dispersing medium comprising an alcohol, ester, ketone, amide, hydrocarbon, silicone, a compound containing an unsaturated bond between linear carbon atoms, an oxirane compound, water, or a combination thereof, and the sol has an average particle size measured by a dynamic light scattering method of 5 to 500 nm, 10 to 200 nm, 10 to 100 nm, 10 to 60 nm, 10 to 40 nm, or 10 to 30 nm.
[0056] The dispersion medium used in the present invention is water and an organic solvent, and the organic solvent is an alcohol having 1 to 10 carbon atoms, such as methanol, ethanol, n-propanol, i-propanol, n-butanol, isobutanol, n-pentanol, ethylene glycol, ethylene glycol monomethyl ether, propylene glycol monomethyl ether, propylene glycol monoethyl ether, propylene glycol monopropyl ether, etc. The ketone is a linear or cyclic aliphatic ketone having 3 to 30 carbon atoms, such as methyl ethyl ketone, diethyl ketone, methyl propyl ketone, methyl isobutyl ketone, diisopropyl ketone, diisobutyl ketone, methyl amyl ketone, cyclohexanone, etc.
[0057] The ethers are linear or cyclic aliphatic ethers having 3 to 30 carbon atoms, such as diethyl ether and tetrahydrofuran. The esters are linear or cyclic esters having 2 to 30 carbon atoms, such as ethyl acetate, n-butyl acetate, sec-butyl acetate, methoxybutyl acetate, amyl acetate, n-propyl acetate, isopropyl acetate, ethyl lactate, butyl lactate, ethylene glycol monomethyl ether acetate, propylene glycol monomethyl ether acetate, propylene glycol monoethyl ether acetate, propylene glycol monopropyl ether acetate, phenyl acetate, phenyl lactate, and phenyl propionate. The amides are aliphatic amides having 3 to 30 carbon atoms, such as dimethylacetamide, dimethylformamide, N-methylpyrrolidone, and N-ethylpyrrolidone. The hydrocarbons are linear or cyclic aliphatic or aromatic hydrocarbons having 6 to 30 carbon atoms, such as hexane, heptane, octane, nonane, decane, benzene, toluene, and xylene.
[0058] The surfactants that can be used in the present invention include anionic surfactants, cationic surfactants, amphoteric surfactants, and nonionic surfactants.
[0059] Examples of anionic surfactants that can be used in the present invention include sodium and potassium salts of fatty acids, alkylbenzenesulfonates, higher alcohol sulfates, polyoxyethylene alkyl ether sulfates, α-sulfofatty acid esters, α-olefinsulfonates, monoalkylphosphates, and alkanesulfonates. For example, alkylbenzenesulfonates include sodium, potassium, and lithium salts, such as sodium C10-C16 alkylbenzenesulfonate, C10-C16 alkylbenzenesulfonic acid, and sodium alkylnaphthalenesulfonate.
[0060] Examples of higher alcohol sulfates include sodium dodecyl sulfate (sodium lauryl sulfate) having 12 carbon atoms, triethanolamine lauryl sulfate, and triethanolammonium lauryl sulfate.
[0061] Examples of polyoxyethylene alkyl ether sulfates include sodium polyoxyethylene styrenated phenyl ether sulfate, ammonium polyoxyethylene styrenated phenyl ether sulfate, sodium polyoxyethylene decyl ether sulfate, ammonium polyoxyethylene decyl ether sulfate, sodium polyoxyethylene lauryl ether sulfate, ammonium polyoxyethylene lauryl ether sulfate, sodium polyoxyethylene tridecyl ether sulfate, sodium polyoxyethylene oleyl cetyl ether sulfate, etc. Examples of α-olefin sulfonates include sodium α-olefin sulfonate, etc.
[0062] Examples of alkanesulfonates include sodium 2-ethylhexyl sulfate. Examples of cationic surfactants used in the present invention include alkyltrimethylammonium salts, dialkyldimethylammonium salts, alkyldimethylbenzylammonium salts, and amine salt-based agents. Alkyltrimethylammonium salts are quaternary ammonium salts and have chloride ions or bromide ions as counterions. Examples include dodecyltrimethylammonium chloride, cetyltrimethylammonium chloride, coconut alkyltrimethylammonium chloride, and alkyl(C16-18)trimethylammonium chloride.
[0063] Dialkyldimethylammonium salts have two lipophilic main chains and two methyl groups. Examples include bis(hydrogenated tallow)dimethylammonium chloride. Examples include didecyldimethylammonium chloride, dicoconuclear alkyldimethylammonium chloride, dihydrogenated tallow alkyldimethylammonium chloride, and dialkyl(C14-18)dimethylammonium chloride. Alkyldimethylbenzylammonium salts are quaternary ammonium salts having one lipophilic main chain, two methyl groups, and a benzyl group, and examples include benzauconium chloride. Examples include alkyl(C8-18)dimethylbenzylammonium chloride. Amine salt agents include those in which the hydrogen atoms of ammonia are substituted with one or more hydrocarbon groups, such as N-methylbishydroxyethylamine fatty acid ester hydrochloride.
[0064] Examples of amphoteric surfactants that can be used in the present invention include N-alkyl-β-alanine-type alkylamino fatty acid salts, alkylcarboxybetaine-type alkylbetaines, and N,N-dimethyldodecylamine oxide-type alkylamine oxides, such as lauryl betaine, stearyl betaine, 2-alkyl-N-carboxymethyl-N-hydroxyethylimidazolinium betaine, and lauryldimethylamine oxide.
[0065] The nonionic surfactant used in the present invention is selected from polyoxyethylene alkyl ethers, polyoxyethylene alkylphenol ethers, alkyl glucosides, polyoxyethylene fatty acid esters, sucrose fatty acid esters, sorbitan fatty acid esters, polyoxyethylene sorbitan fatty acid esters, and fatty acid alkanolamides. Examples of polyoxyethylene alkyl ethers include polyoxyethylene dodecyl ether (polyoxyethylene lauryl ether), polyoxyalkylene lauryl ether, polyoxyethylene tridecyl ether, polyoxyalkylene tridecyl ether, polyoxyethylene myristyl ether, polyoxyethylene cetyl ether, polyoxyethylene oleyl ether, polyoxyethylene stearyl ether, polyoxyethylene behenyl ether, polyoxyethylene-2-ethylhexyl ether, and polyoxyethylene isodecyl ether.
[0066] Examples of polyoxyethylene alkylphenol ethers include polyoxyethylene styrenated phenyl ether, polyoxyethylene nonylphenyl ether, polyoxyethylene distyrenated phenyl ether, and polyoxyethylene tribenzyl phenyl ether.
[0067] Alkyl glucosides include decyl glucoside and lauryl glucoside.
[0068] Examples of polyoxyethylene fatty acid esters include polyoxyethylene monolaurate, polyoxyethylene monostearate, polyoxyethylene monooleate, polyethylene glycol distearate, polyethylene glycol dioleate, polypropylene glycol dioleate, etc. Examples of sorbitan fatty acid esters include sorbitan monocaprylate, sorbitan monolaurate, sorbitan monomyristate, sorbitan monopalmitate, sorbitan monostearate, sorbitan distearate, sorbitan tristearate, sorbitan monooleate, sorbitan trioleate, sorbitan monosesquioleate, and ethylene oxide adducts thereof.
[0069] Examples of polyoxyethylene sorbitan fatty acid esters include polyoxyethylene sorbitan monolaurate, polyoxyethylene sorbitan monopalmitate, polyoxyethylene sorbitan monostearate, polyoxyethylene sorbitan tristearate, polyoxyethylene sorbitan monooleate, polyoxyethylene sorbitan trioleate, and polyoxyethylene sorbitan triisostearate.
[0070] Examples of fatty acid alkanolamides include coconut oil fatty acid diethanolamide, beef tallow fatty acid diethanolamide, lauric acid diethanolamide, and oleic acid diethanolamide.
[0071] Further examples include polyoxyalkyl ethers or polyoxyalkyl glycols such as polyoxyethylene polyoxypropylene glycol and polyoxyethylene fatty acid esters, polyoxyethylene hydrogenated castor oil ether, sorbitan fatty acid ester alkyl ether, alkyl polyglucoside, sorbitan monooleate, and sucrose fatty acid ester.
[0072] The present invention provides a composition (varnish) containing core-shell metal oxide particles and a thermosetting or photocurable resin. The composition of the present invention can be further mixed with a thermosetting or photocurable resin to produce a varnish.
[0073] The present invention provides a film-forming composition containing the organic solvent sol and an organic resin. The film-forming composition can be obtained by removing the organic solvent from the organic solvent sol to obtain a film-forming composition containing core-shell metal oxide particles and an organic resin. In the case of a thermosetting film-forming composition, the heat curing agent can be added in a range of 0.01 to 50 phr, or 0.01 to 10 phr, relative to the resin containing functional groups such as epoxy groups or (meth)acryloyl groups. For example, the heat curing agent can be added in a ratio of 0.5 to 1.5 equivalents, preferably 0.8 to 1.2 equivalents, relative to the functional groups such as epoxy groups or (meth)acryloyl groups. The equivalent weight of the heat curing agent relative to the curable resin is expressed as the equivalent ratio of the heat curing agent to the functional group. Examples of heat curing agents include phenolic resins, amine-based curing agents, polyamide resins, imidazoles, polymercaptans, acid anhydrides, thermal radical generators, and thermal acid generators. Radical generator-based curing agents, acid anhydride-based curing agents, and amine-based curing agents are particularly preferred. Although these thermosetting agents can be used by dissolving them in a solvent even if they are solid, evaporation of the solvent reduces the density of the cured product and creates pores, resulting in reduced strength and reduced water resistance. Therefore, it is preferable that the curing agent itself is liquid at room temperature and normal pressure. Examples of phenolic resins include phenol novolac resins and cresol novolac resins.
[0074] Examples of amine curing agents include piperidine, N,N-dimethylpiperazine, triethylenediamine, 2,4,6-tris(dimethylaminomethyl)phenol, benzyldimethylamine, 2-(dimethylaminomethyl)phenol, diethylenetriamine, triethylenetetramine, tetraethylenepentamine, diethylaminopropylamine, N-aminoethylpiperazine, di(1-methyl-2-aminocyclohexyl)methane, menthenediamine, isophoronediamine, diaminodicyclohexylmethane, 1,3-diaminomethylcyclohexane, xylenediamine, metaphenylenediamine, diaminodiphenylmethane, diaminodiphenylsulfone, 3,3'-diethyl-4,4'-diaminodiphenylmethane, and diethyltoluenediamine. Of these, liquids such as diethylenetriamine, triethylenetetramine, tetraethylenepentamine, diethylaminopropylamine, N-aminoethylpiperazine, di(1-methyl-2-aminocyclohexyl)methane, menthenediamine, isophoronediamine, diaminodicyclohexylmethane, 3,3'-diethyl-4,4'-diaminodiphenylmethane, and diethyltoluenediamine can be preferably used.
[0075] The polyamide resin is a polyamide amine produced by condensation of dimer acid and polyamine, and has primary and secondary amines in the molecule.
[0076] Examples of imidazoles include 2-methylimidazole, 2-ethyl-4-methylimidazole, 1-cyanoethyl-2-undecylimidazolium trimellitate, and epoxyimidazole adduct.
[0077] The polymercaptan is, for example, one in which a mercaptan group is present at the end of a polypropylene glycol chain or one in which a mercaptan group is present at the end of a polyethylene glycol chain, and is preferably liquid. The acid anhydride curing agent is preferably an anhydride of a compound having multiple carboxyl groups in one molecule. Examples of these acid anhydride curing agents include phthalic anhydride, trimellitic anhydride, pyromellitic anhydride, benzophenone tetracarboxylic acid anhydride, ethylene glycol bistrimellitate, glycerol tristrimellitate, maleic anhydride, tetrahydrophthalic anhydride, methyl tetrahydrophthalic anhydride, endomethylene tetrahydrophthalic anhydride, methyl endomethylene tetrahydrophthalic anhydride, methylbutenyl tetrahydrophthalic anhydride, dodecenyl succinic anhydride, hexahydrophthalic anhydride, methylhexahydrophthalic anhydride, succinic anhydride, methylcyclohexene dicarboxylic anhydride, and chlorendic anhydride. Examples of thermal acid generators include sulfonium salts and phosphonium salts, with sulfonium salts being preferred. For example, the following compounds can be mentioned.
[0078]
[0079] R may be an alkyl group having 1 to 12 carbon atoms or an aryl group having 6 to 20 carbon atoms, with an alkyl group having 1 to 12 carbon atoms being particularly preferred. Among these, the following are preferred, which are liquid at room temperature and normal pressure: methyltetrahydrophthalic anhydride, methyl-5-norbornene-2,3-dicarboxylic anhydride (methylnadic anhydride, methylhimic anhydride), hydrogenated methylnadic anhydride, methylbutenyltetrahydrophthalic anhydride, dodecenylsuccinic anhydride, methylhexahydrophthalic anhydride, and a mixture of methylhexahydrophthalic anhydride and hexahydrophthalic anhydride. These liquid acid anhydrides have a viscosity of about 10 mPa·s to 1,000 mPa·s when measured at 25°C. Examples of thermal radical generators include 2,2'-azobis(isobutyronitrile), 2,2'-azobis(2-methylbutyronitrile), 2,2'-azobis(2,4-dimethylvaleronitrile), 4,4'-azobis(4-cyanovaleric acid), 2,2'-azobis(2-methylpropionate)dimethyl, 2,2'-azobis(2-methylpropionamidine) dihydrochloride, 2,2'-azobis[2-(2-imidazolin-2-yl)propane]dihydrochloride, tert-butyl hydroperoxide, cumene hydroperoxide, di-tert-butyl peroxide, dicumyl peroxide, and benzoyl peroxide. These are available from Tokyo Chemical Industry Co., Ltd.
[0080] Furthermore, when obtaining the cured product, a curing aid may be used in combination as appropriate. Examples of curing aids include organic phosphorus compounds such as triphenylphosphine and tributylphosphine; quaternary phosphonium salts such as ethyltriphenylphosphonium bromide and methyltriphenylphosphonium diethyl phosphate; and quaternary ammonium salts such as 1,8-diazabicyclo(5,4,0)undecane-7-ene, salts of 1,8-diazabicyclo(5,4,0)undecane-7-ene and octylic acid, zinc octylate, and tetrabutylammonium bromide. These curing aids can be contained in a ratio of 0.001 to 0.1 parts by mass per part by mass of curing agent. A thermosetting varnish is obtained by mixing the resin, curing agent, and, if desired, curing aid in the composition. Mixing can be carried out in a reaction vessel using a stirring blade or kneader.
[0081] Mixing is performed by a heated mixing method at a temperature of 60°C to 100°C for 0.5 to 1 hour. The resulting curable film-forming composition is a thermosetting coating composition and has an appropriate viscosity for use, for example, as a liquid encapsulant. The liquid thermosetting film-forming composition can be prepared to any viscosity and can be used as a transparent encapsulant for LEDs and the like by casting, potting, dispensing, printing, or other methods, thereby enabling partial encapsulation at any desired location. The liquid thermosetting composition is directly mounted on an LED or the like using the method described above, and then dried and cured to obtain a cured epoxy resin product. The thermosetting film-forming composition (thermosetting coating composition) is applied to a substrate and heated at a temperature of 80 to 200°C to obtain a cured product. In the case of a photocurable resin composition among the above-mentioned film-forming compositions, a photocuring agent (photoradical generator, photoacid generator) can be added in a range of 0.01 to 50 phr, or 0.01 to 10 phr, to a resin containing a functional group such as an epoxy group or a (meth)acryloyl group. For example, the photocuring agent (photoradical generator, photoacid generator) can be contained in a ratio of 0.5 to 1.5 equivalents, preferably 0.8 to 1.2 equivalents, to the functional group such as an epoxy group or a (meth)acryloyl group. The equivalent of the photocuring agent to the curable resin is expressed as the equivalent ratio of the photocuring agent to the functional group.
[0082] The photoradical generator is not particularly limited as long as it generates radicals directly or indirectly upon irradiation with light. Examples of the photoradical generator include photoradical polymerization initiators such as imidazole compounds, diazo compounds, bisimidazole compounds, N-arylglycine compounds, organic azide compounds, titanocene compounds, aluminate compounds, organic peroxides, N-alkoxypyridinium salt compounds, and thioxanthone compounds. Examples of the azide compound include p-azidobenzaldehyde, p-azidoacetophenone, p-azidobenzoic acid, p-azidobenzalacetophenone, 4,4'-diazidochalcone, 4,4'-diazidodiphenyl sulfide, and 2,6-bis(4'-azidobenzal)-4-methylcyclohexanone. Examples of the diazo compound include 1-diazo-2,5-diethoxy-4-p-tolylmercaptobenzeneborofluoride, 1-diazo-4-N,N-dimethylaminobenzene chloride, and 1-diazo-4-N,N-diethylaminobenzeneborofluoride.
[0083] Examples of the bisimidazole compound include 2,2'-bis(o-chlorophenyl)-4,5,4',5'-tetrakis(3,4,5-trimethoxyphenyl)1,2'-bisimidazole and 2,2'-bis(o-chlorophenyl)4,5,4',5'-tetraphenyl-1,2'-bisimidazole. Examples of the titanocene compound include dicyclopentadienyl-titanium-dichloride, dicyclopentadienyl-titanium-bisphenyl, dicyclopentadienyl-titanium-bis(2,3,4,5,6-pentafluorophenyl), dicyclopentadienyl-titanium-bis(2,3,5,6-tetrafluorophenyl), dicyclopentadienyl-titanium-bis(2,4,6-trifluorophenyl), dicyclopentadienyl-titanium-bis(2,6-difluorophenyl), dicyclopentadienyl bis(methylcyclopentadienyl)-titanium-bis(2,3,4,5,6-pentafluorophenyl), bis(methylcyclopentadienyl)-titanium-bis(2,3,5,6-tetrafluorophenyl), bis(methylcyclopentadienyl)-titanium-bis(2,6-difluorophenyl), and dicyclopentadienyl-titanium-bis(2,6-difluoro-3-(1H-pyrrol-1-yl)-phenyl).
[0084] Further examples of the photoradical generator include 1,3-di(tert-butyldioxycarbonyl)benzophenone, 3,3',4,4'-tetrakis(tert-butyldioxycarbonyl)benzophenone, 3-phenyl-5-isoxazolone, 2-mercaptobenzimidazole, 2,2-dimethoxy-1,2-diphenylethan-1-one, 1-hydroxy-cyclohexyl-phenyl-ketone, and 2-benzyl-2-dimethylamino-1-(4-morpholinophenyl)-butanone.
[0085] These photoradical polymerization agents are available, for example, as Irgacure TPO (component: 2,4,6-trimethylbenzoyldiphenylphosphine oxide) (c1-1-1), manufactured by BASF, Omnirad 819 (component: bis(2,4,6-trimethylbenzoyl)phenylphosphine oxide) (c1-1-2), manufactured by IGM RESINS, and Irgacure 184 (component: 1-hydroxycyclohexylphenyl ketone) (c1-1-3).
[0086]
[0087] The photoacid generator is not particularly limited as long as it generates an acid directly or indirectly upon irradiation with light. Specific examples of the photoacid generator include triazine compounds, acetophenone derivative compounds, disulfone compounds, diazomethane compounds, sulfonic acid derivative compounds, onium salts such as iodonium salts, sulfonium salts, phosphonium salts, and selenium salts, metallocene complexes, and iron arene complexes. The onium salt used as the photoacid generator includes iodonium salts such as diphenyliodonium chloride, diphenyliodonium trifluoromethanesulfonate, diphenyliodonium mesylate, diphenyliodonium tosylate, diphenyliodonium bromide, diphenyliodonium tetrafluoroborate, diphenyliodonium hexafluoroantimonate, diphenyliodonium hexafluoroarsenate, bis(p-tert-butylphenyl)iodonium hexafluorophosphate, bis(p-tert-butylphenyl)iodonium mesylate, bis(p-tert-butylphenyl)iodonium tosylate, bis(p-tert-butylphenyl)iodonium trifluoromethanesulfonate, bis(p-tert-butylphenyl)iodonium Examples of the iodonium salt include bis(alkylphenyl)iodonium salts such as iodonium tetrafluoroborate, bis(p-tert-butylphenyl)iodonium chloride, bis(p-chlorophenyl)iodonium chloride, bis(p-chlorophenyl)iodonium tetrafluoroborate, and further bis(4-t-butylphenyl)iodonium hexafluorophosphate; alkoxycarbonylalkoxy-trialkylaryl iodonium salts (for example, 4-[(1-ethoxycarbonyl-ethoxy)phenyl]-(2,4,6-trimethylphenyl)-iodonium hexafluorophosphate); and bis(alkoxyaryl)iodonium salts (for example, bis(alkoxyphenyl)iodonium salts such as (4-methoxyphenyl)phenyliodonium hexafluoroantimonate).
[0088] Examples of sulfonium salts include triphenylsulfonium salts such as triphenylsulfonium chloride, triphenylsulfonium bromide, tri(p-methoxyphenyl)sulfonium tetrafluoroborate, tri(p-methoxyphenyl)sulfonium hexafluorophosphonate, tri(p-ethoxyphenyl)sulfonium tetrafluoroborate, triphenylsulfonium triflate, triphenylsulfonium hexafluoroantimonate, and triphenylsulfonium hexafluorophosphate; and sulfonium salts such as (4-phenylthiophenyl)diphenylsulfonium hexafluoroantimonate, (4-phenylthiophenyl)diphenylsulfonium hexafluorophosphate, bis[4-(diphenylsulfonio)phenyl]sulfide-bis-hexafluoroantimonate, bis[4-(diphenylsulfonio)phenyl]sulfide-bis-hexafluorophosphate, and (4-methoxyphenyl)diphenylsulfonium hexafluoroantimonate.
[0089] Examples of phosphonium salts include triphenylphosphonium chloride, triphenylphosphonium bromide, tri(p-methoxyphenyl)phosphonium tetrafluoroborate, tri(p-methoxyphenyl)phosphonium hexafluorophosphonate, tri(p-ethoxyphenyl)phosphonium tetrafluoroborate, 4-chlorobenzenediazonium hexafluorophosphate, benzyltriphenylphosphonium hexafluoroantimonate, etc. Examples of phosphonium salts include selenium salts such as triphenylselenium hexafluorophosphate, and metallocene complexes such as (η5 or η6-isopropylbenzene)(η5-cyclopentadienyl)iron(II) hexafluorophosphate.
[0090] The following compounds can also be used as photoacid generators.
[0091]
[0092]
[0093]
[0094]
[0095]
[0096]
[0097]
[0098]
[0099]
[0100] As the photoacid generator, sulfonium salt compounds and iodonium salt compounds are preferred. The anion species thereof is CF 3 SO 3 - , C 4 F 9 SO 3 - , C 8 F 17 SO 3 - , camphorsulfonate anion, tosylate anion, BF 4 - , P.F. 6 - , AsF 6 - and SbF 6 - and the like. Anion species such as phosphorus hexafluoride and antimony hexafluoride, which exhibit strong acidity, are particularly preferred. The film-forming composition of the present invention may contain conventional additives as needed. Examples of such additives include pigments, colorants, thickeners, sensitizers, antifoaming agents, coatability improvers, lubricants, stabilizers (antioxidants, heat stabilizers, light resistance stabilizers, etc.), plasticizers, dissolution promoters, fillers, antistatic agents, and the like. These additives may be used alone or in combination of two or more.
[0101] Examples of methods for applying the film-forming composition of the present invention include flow coating, spin coating, spray coating, screen printing, casting, bar coating, curtain coating, roll coating, gravure coating, dipping, and slit coating. In the present invention, the photo-coating composition (film-forming composition) can be applied to a substrate and cured by light irradiation. Heating can also be performed before or after light irradiation. The thickness of the coating can be selected from a range of approximately 0.01 μm to 10 mm depending on the application of the cured product. For example, when used as a photoresist, the thickness can be approximately 0.05 to 10 μm (particularly 0.1 to 5 μm), when used as a printed wiring board, the thickness can be approximately 5 μm to 5 mm (particularly 100 μm to 1 mm), and when used as an optical thin film, the thickness can be approximately 0.1 to 100 μm (particularly 0.3 to 50 μm). When a transparent coating is obtained, the visible light transmittance of the coating can be 80% or more, or 90% or more, typically 90 to 96%.
[0102] When a photoacid generator is used, the light to be irradiated or exposed may be, for example, gamma rays, X-rays, ultraviolet light, or visible light, and is usually visible light or ultraviolet light, particularly ultraviolet light. The wavelength of the light is, for example, about 150 to 800 nm, preferably about 150 to 600 nm, and more preferably about 150 to 400 nm. The amount of irradiation light varies depending on the thickness of the coating film, but is, for example, about 2 to 20,000 mJ / cm. 2 , preferably 5 to 5000 mJ / cm 2The light source can be selected depending on the type of light to be exposed. For example, in the case of ultraviolet light, a low-pressure mercury lamp, a high-pressure mercury lamp, an ultra-high-pressure mercury lamp, a deuterium lamp, a halogen lamp, or laser light (e.g., a helium-cadmium laser or an excimer laser) can be used. Such light irradiation causes the curing reaction of the composition to proceed. When a thermal acid generator is used, or when a photoacid generator is used, heating of the coating film, which is optionally performed after light irradiation, is carried out at, for example, 60 to 350°C, preferably about 100 to 300°C. The heating time can be selected from the range of 3 seconds or more (e.g., about 3 seconds to 5 hours), for example, 5 seconds to 2 hours, preferably about 20 seconds to 30 minutes, and typically about 1 minute to 3 hours (e.g., about 5 minutes to 2.5 hours).
[0103] Furthermore, when forming a pattern or image (e.g., when producing a printed wiring board, etc.), the coating film formed on the substrate may be subjected to pattern exposure. This pattern exposure may be performed by scanning with laser light or by irradiating with light through a photomask. The non-irradiated areas (unexposed areas) generated by such pattern exposure are developed (or dissolved) with a developer to form a pattern or image. Examples of the developer include aqueous alkaline solutions and organic solvents. Examples of aqueous alkaline solutions include aqueous solutions of alkali metal hydroxides such as potassium hydroxide, sodium hydroxide, potassium carbonate, and sodium carbonate; aqueous solutions of quaternary ammonium hydroxides such as tetramethylammonium hydroxide, tetraethylammonium hydroxide, and choline; and aqueous amine solutions such as ethanolamine, propylamine, and ethylenediamine.
[0104] The alkaline developer is generally an aqueous solution of 10% by weight or less, preferably a 0.1 to 3.0% by weight aqueous solution. Furthermore, alcohols or surfactants can be added to the developer, each of which is preferably added in an amount of 0.05 to 10 parts by weight per 100 parts by weight of the developer. Among these, a 0.1 to 2.38% by weight aqueous solution of tetramethylammonium hydroxide can be used. Furthermore, the organic solvent used in the developer can be a common organic solvent, such as acetone, acetonitrile, toluene, dimethylformamide, methanol, ethanol, isopropanol, propylene glycol methyl ether, propylene glycol ethyl ether, propylene glycol propyl ether, propylene glycol butyl ether, propylene glycol methyl ether acetate, propylene glycol ethyl ether acetate, propylene glycol propyl ether acetate, propylene glycol butyl ether acetate, ethyl lactate, or cyclohexanone. These can be used alone or in combination. In particular, propylene glycol methyl ether, propylene glycol methyl ether acetate, ethyl lactate, etc. can be preferably used.
[0105] In the present invention, an adhesion promoter can be added for the purpose of improving adhesion to the substrate after development. These adhesion promoters include chlorosilanes such as trimethylchlorosilane, dimethylvinylchlorosilane, methyldiphenylchlorosilane, and chloromethyldimethylchlorosilane; alkoxysilanes such as trimethylmethoxysilane, dimethyldiethoxysilane, methyldimethoxysilane, dimethylvinylethoxysilane, diphenyldimethoxysilane, and phenyltriethoxysilane; silazanes such as hexamethyldisilazane, N,N'-bis(trimethylsilyl)urea, dimethyltrimethylsilylamine, and trimethylsilylimidazole; vinyltrichlorosilane, 3-chloropropyltrimethoxysilane, and 3-chloropropyltrimethoxysilane; Examples of adhesion promoters include silanes such as 3-aminopropyltriethoxysilane, 3-methacryloxypropyltrimethoxysilane, 3-glycidoxypropyltrimethoxysilane, and 3-(N-piperidinyl)propyltrimethoxysilane; heterocyclic compounds such as benzotriazole, benzimidazole, indazole, imidazole, 2-mercaptobenzimidazole, 2-mercaptobenzothiazole, 2-mercaptobenzoxazole, urazole, thiouracil, mercaptoimidazole, and mercaptopyrimidine; and urea or thiourea compounds such as 1,1-dimethylurea and 1,3-dimethylurea. These adhesion promoters can be used alone or in combination of two or more. The amount of these adhesion promoters added is typically 18% by mass or less, preferably 0.0008 to 9% by mass, and more preferably 0.04 to 9% by mass, based on the solid content.
[0106] The present invention may contain a sensitizer. Usable sensitizers include anthracene, phenothiazene, perylene, thioxanthone, and benzophenone thioxanthone. Further examples of sensitizing dyes include thiopyrylium salt dyes, merocyanine dyes, quinoline dyes, styrylquinoline dyes, ketocoumarin dyes, thioxanthene dyes, xanthene dyes, oxonol dyes, cyanine dyes, rhodamine dyes, and pyrylium salt dyes. Anthracene sensitizers are particularly preferred. When used in combination with a cationic curing catalyst (radiation-sensitive cationic polymerization initiator), they dramatically improve sensitivity and also possess radical polymerization initiation capabilities. In hybrid systems that combine the cationic curing system and radical curing system of the present invention, the catalyst species can be simplified. Specific anthracene compounds that are effective include dibutoxyanthracene and dipropoxyanthraquinone. The amount of the sensitizer added is 0.01 to 20% by weight, preferably 0.01 to 10% by weight, based on the solid content.
[0107] The composition of the present invention can be photocured or thermally cured using a photoradical generator, a thermal radical generator, a photoacid generator, or a thermal acid generator. When a photoacid generator or a thermal acid generator is used, for example, commonly used epoxy curing agents (e.g., amines or acid anhydrides) are not used, or even if they are used, the content of these agents is extremely small, thereby improving the storage stability of the composition.
[0108] The above composition has been found to be applicable to photocationic polymerization. It has a higher curing rate than conventional liquid epoxy compounds (e.g., alicyclic epoxy compounds with an epoxycyclohexyl ring). Because of its fast curing rate, it is possible to reduce the amount of acid generator added or use a weak acid generator. Reducing the amount of acid generator is important for preventing metal corrosion, as active acid species may remain even after UV irradiation. Because of its fast curing rate, thick film curing is possible. Curing by UV irradiation can be applied to materials (equipment) that are sensitive to heat.
[0109] Thermosetting and photocurable materials using the coating-forming composition of the present invention are characterized by rapid curing, transparency, and little shrinkage on cure, and can be used to coat or bond electronic components, optical components (anti-reflective coatings), and precision mechanical components.
[0110] The above composition (varnish) can be suitably used as a hard coating agent or a composition for nanoimprints.
[0111] Other applications include the use of this material in bonding mobile phone and camera lenses, optical elements such as light-emitting diodes (LEDs) and semiconductor lasers (LDs), liquid crystal panels, biochips, camera lenses and prisms, magnetic components in hard disks of computers and other devices, pickups in CD and DVD players (the part that captures the optical information reflected from the disc), speaker cones and coils, motor magnets, circuit boards, electronic components, and internal engine components of automobiles and the like.
[0112] As a hard coating material for surface protection of automobile bodies, lamps, electrical appliances, building materials, plastics, etc., it can be applied to, for example, automobile and motorcycle bodies, headlight lenses and mirrors, plastic lenses for eyeglasses, mobile phones, game consoles, optical films, ID cards, etc.
[0113] Examples of ink materials for printing on metals such as aluminum and plastics include inks for printing on cards such as credit cards and membership cards, switches on electrical appliances and office equipment, and keyboards, as well as inks for inkjet printers for CDs, DVDs, etc.
[0114] Examples of applications include a technology for curing resins in combination with 3D CAD to create complex three-dimensional objects, application in stereolithography such as for manufacturing models of industrial products, and application in optical fiber coating, adhesion, optical waveguides, thick-film resists, etc. The film-forming composition of the present invention can also be suitably used as an insulating resin for electronic materials such as antireflection films, semiconductor encapsulation materials, adhesives for electronic materials, printed wiring board materials, interlayer insulating film materials, and encapsulants for power modules, as well as an insulating resin for use in high-voltage equipment such as generator coils, transformer coils, and gas-insulated switchgear.
[0115] [Total Metal Oxide Concentration] The sol was weighed in a crucible and pre-dried by heating at 110° C. for 30 minutes to remove the solvent, and then calcined at 600° C. for 30 minutes. The crucible was weighed, and the total metal oxide concentration was calculated from the weight of the residue.
[0116] [X-ray diffraction measurement] The sol was dried on a hot plate at 110°C and pulverized for 15 minutes using a mortar and pestle to obtain a dry powder, which was measured using an XRD device (manufactured by Rigaku Corporation, product name MiniFlex600) to obtain an X-ray diffraction pattern.
[0117] [Viscosity] Measured using a BM type viscometer (25°C).
[0118] [Average Particle Diameter by Dynamic Light Scattering (Dynamic Light Scattering Particle Diameter, DLS Average Secondary Particle Diameter)] The sol was diluted with a dispersion solvent, and the particle diameter was measured using the parameters of the solvent with a dynamic light scattering measuring device (manufactured by Malvern Instruments Ltd., trade name Zetasizer).
[0119] [Average Primary Particle Diameter Measured by Transmission Electron Microscopy] The sol was dropped onto a copper mesh and dried, and observed using a transmission electron microscope (manufactured by JEOL Ltd., trade name: JEM-1020) at an acceleration voltage of 100 kV. The average value of measurements for 100 particles was determined as the average primary particle diameter.
[0120] [ 31 P-NMR test of colloidal particles in sol 31 P-NMR was measured using the following procedure. (Preparation of dry powder of phosphate-treated colloidal particles) 3.0 mass % of an 85% aqueous solution of phosphoric acid relative to the solid content of the colloidal particles was added to 10.0 g of the sol, and the colloidal particle surfaces were treated with phosphoric acid by stirring for 0.5 hours. The resulting sol was then thoroughly washed by ultrafiltration to remove phosphoric acid not bound to the particles. The washed sol was dried on a hot plate at 60°C for 3 hours, and the dried powder was ground in an agate mortar for 10 minutes to prepare a dry powder of phosphate-treated colloidal particles.
[0121] (by solid-state NMR 31 P-NMR analysis) The dry powder was sealed in a sample tube (diameter 2.5 mm) used for solid-state NMR measurement, and analyzed by DD / MAS.31 P solid-state NMR measurements were carried out. The instrument used was a nuclear magnetic resonance instrument, trade name AVANCE3 (manufactured by Bruker, 500 MHz), and measurements were taken under the following conditions: Probe diameter: 4.0 mm, Rotation speed: 30,000 Hz, Relaxation waiting time: 10 s, Number of accumulations: 8,000. From the obtained spectrum, peak division was carried out for each peak derived from the metal species to which phosphate was bound, and the presence or absence of a main peak (Ti-O-P) derived from Ti atoms, which are the core components of the colloidal particles, was examined. Ti-O-P: δ = 3 to 5 ppm. Particles in which a Ti-O-P peak could be confirmed were marked with "○", and those in which it could not be confirmed were marked with "×".
[0122] [Color retention rate of dye upon UV irradiation at 490 nm] To an aqueous dispersion or a methanol dispersion of inorganic oxide fine particles in an amount equivalent to 0.05 g in solids weight, an appropriate solvent was added so that the water / methanol ratio was 1 / 1 (weight ratio) and the solids concentration was 0.5 wt%. Next, the obtained dispersion was mixed with a glycerin solution of a sunset yellow dye with a solids concentration of 0.02 wt% in a weight ratio (dispersion weight / glycerin solution weight) of 1 / 3 to prepare a sample, which was then placed in a quartz cell with a depth of 1 mm, a width of 1 cm, and a height of 5 cm. Next, using an ultraviolet lamp (SLUV-6 manufactured by ASONE) with a wavelength range of I-line (wavelength 365 nm) selected, an intensity of 0.4 mW / cm was measured on the surface of the quartz cell with a width of 1 cm and a height of 5 cm. 2 The sample was irradiated with ultraviolet light at a wavelength of 490 nm (A0) before and after the ultraviolet light irradiation (A1) at a wavelength of 490 nm using a UV-visible-near-infrared spectrophotometer (Shimadzu Corporation, trade name UV-3600), and the color retention rate of the dye was calculated using the following formula:
[0123] Remaining color rate (%) = A1 / A0 x 100
[0124] [Refractive Index of Particles] The refractive index of the colloidal particles in the sol was measured by the following procedures i) to iii).
[0125] i) Preparation of a coating solution containing colloidal particle organic solvent dispersion sol 20.00 g of 3-glycidoxypropyltrimethoxysilane (manufactured by Momentive, trade name SILQUEST A-187T) was weighed into a plastic container, to which 18.57 g of methanol and 4.57 g of 0.01 N hydrochloric acid aqueous solution were added, followed by stirring at room temperature for 5 hours. 3 ) in methanol (10% by mass Al(acac) 3 6.00 g of 3-glycidoxypropyltrimethoxysilane was added as a curing agent and stirred for 10 minutes to prepare a partial hydrolyzate of 3-glycidoxypropyltrimethoxysilane (concentration: 43% by mass). The partial hydrolyzate of 3-glycidoxypropyltrimethoxysilane, colloid particle dispersion sol, water, methanol, and 0.25 g of a methanol solution of a leveling agent (DOWSIL trade name, L-7604) (10% by mass L-7604) were weighed into a brown bottle so that the final solvent composition was 1 / 4 by weight of water / solvents other than water, and the colloid particle amounts in the organic solvent dispersion sol were 50 phr, 100 phr, and 150 phr, respectively, and the resulting mixture was stirred at room temperature for 30 minutes to prepare a coating liquid containing colloid particle organic solvent dispersion sol (solids concentration: 10.0% by mass, colloid particle amounts: 50 phr, 100 phr, and 150 phr).
[0126] ii) Preparation of particle-containing film The colloidal particle organic solvent dispersion sol-containing coating liquid obtained in i) was irradiated with UV- 3 Approximately 0.5 mL of the solution was dropped onto the treated Si substrate and coated using a spin coater (Mikasa Co., Ltd., product name Opticoat MS-B100) so that the film thickness after coating would be 1.0 μm. The substrate was then baked on a hot plate at 80°C for 5 minutes and heat-treated in an oven at 120°C for 1 hour to prepare particle-blended films (particle blending amounts: 50 phr, 100 phr, and 150 phr).
[0127] iii) Measurement of refractive index of particle-blended films, calculation of refractive index of particles The refractive index of the particle-blended films obtained in ii) (particle blending amounts: 50 phr, 100 phr, 150 phr) was measured using an ellipsometer (multi-angle incident spectroscopic ellipsometer, product name VASE, manufactured by J.A. Woollam Japan Co., Ltd.). Separately, the refractive index of a particle-free film prepared in the same manner using only a partial hydrolyzate of 3-glycidoxypropyltrimethoxysilane was also measured. The measured refractive index of the blended film was plotted against the particle blending amount, and the particle refractive index was calculated by extrapolating so that the particle blending amount was 100 mass%.
[0128] [Dispersion Stability] After a storage test of the dispersion liquid at 50°C for 1 week, samples in which the particle size measured by dynamic light scattering was less than 1.2 times that before the storage test were evaluated as unchanged and were marked with "○", and samples in which the particle size measured by dynamic light scattering was changed by 1.2 times or more compared to that before the storage test were evaluated as "×".
[0129] The cured films were formed on urethane plastic lens substrates or glass substrates by the methods described below, for example, in (Example 9 Cured Film Evaluation - A1) or (Example 13 Cured Film Evaluation - A5), and evaluated at 25°C and 50% humidity.
[0130] (1) Film Refractive Index The reflectance of a cured film formed on a glass substrate was measured using a reflectance measuring device (manufactured by Olympus Corporation, trade name USPM-RU). From the measured reflectance, the refractive index of the cured film was calculated using optical simulation.
[0131] (2) Transparency The cured film formed on a urethane plastic lens substrate or a glass substrate was visually inspected for cloudiness under fluorescent light in a dark room. The evaluation criteria were as follows: ○: Almost no cloudiness occurred ×: Cloudiness occurred and whitening was evident
[0132] (3) Light resistance: Using an ultraviolet fluorescent lamp accelerated weathering tester (manufactured by Q-Lab, product name QUV) equipped with a UV-A lamp, a light resistance of 0.89 W / m 2A cured film formed on a urethane plastic lens or a glass substrate was irradiated with ultraviolet light for 24 hours under conditions of 340 nm (340 nm). The evaluation criteria are as follows: ∘: No cracks or film peeling were observed. ×: Cracks or film peeling were observed.
[0133] (4) Scratch Resistance The surface of a cured film formed on a urethane-based plastic lens substrate or a glass substrate was rubbed with steel wool #0000, and the cured film was visually inspected for scratches in a bright room under a fluorescent lamp. The scratch resistance test was conducted once per 10 seconds with a load of 1 kg. The evaluation criteria were as follows: ○: No scratches were visible to the naked eye. ×: Scratches were visible to the naked eye.
[0134] (5) Nanoimprinting A coating liquid containing a colloidal particle organic solvent dispersion sol was spin-coated onto a quartz substrate and heated on a hot plate at 100°C for 1 minute to produce a film from which the solvent had been removed. The resulting film was irradiated with ultraviolet light using a nanoimprinter (manufactured by Meisho Kiko Co., Ltd., product name NM-0801HB) while a release-treated quartz mold (manufactured by Kyodo International Co., Ltd., product name DTM-2-1) was pressed against the substrate at 1000 N, thereby transferring and curing a concave-convex pattern. The mold was peeled from the resulting cured film, and the formed pattern was observed with an SEM (manufactured by JEOL Ltd., product name JSM-6010LV). The evaluation criteria were as follows: ○: The pattern was transferred, and the imprinting properties were good. ×: The pattern was not transferred, and the imprinting properties were poor.
[0135] Reference Example 1: Preparation of titanium oxide-stannic oxide composite oxide colloidal particles (A1) to serve as cores 319.5 g of a 25% by mass aqueous solution of tetramethylammonium hydroxide was dissolved in 947.1 g of pure water, and then 7.4 g of metastannic acid (SnO 2 6.3 g in terms of titanium tetraisopropoxide), 236.6 g (TiO 2To the resulting solution, 82.0 g of oxalic acid dihydrate (containing 66.6 g in terms of oxalic acid equivalent) and 82.0 g of oxalic acid dihydrate (containing 58.5 g in terms of oxalic acid equivalent) were added under stirring. The mixed solution was maintained at 80°C for 2 hours, and then the pressure was reduced to 580 Torr and maintained for 2 hours to prepare a mixed solution. The mixed solution was placed in a glass-lined autoclave vessel, subjected to hydrothermal treatment at 140°C for 5 hours, cooled to room temperature, and then removed. The obtained sol was a water-dispersed sol of titanium oxide-stannic oxide composite oxide colloidal particles (A1), and had a total metal oxide concentration (TiO 2 , and SnO 2 The sol was dried at 110° C. and the powder was subjected to X-ray diffraction analysis, which confirmed that the powder was a rutile crystal.
[0136] Reference Example 2: Preparation of titanium oxide-stannic oxide composite oxide colloidal particles (A2) to serve as cores 319.5 g of a 25% by mass aqueous solution of tetramethylammonium hydroxide was dissolved in 947.1 g of pure water, and then 14.8 g of metastannic acid (SnO 2 12.5g in terms of titanium tetraisopropoxide), 236.6g (TiO 2 To the resulting solution, 82.0 g of oxalic acid dihydrate (containing 66.6 g in terms of oxalic acid equivalent) and 82.0 g of oxalic acid dihydrate (containing 58.5 g in terms of oxalic acid equivalent) were added under stirring. The mixed solution was maintained at 80°C for 2 hours, and then the pressure was reduced to 580 Torr and maintained for 2 hours to prepare a mixed solution. The mixed solution was placed in a glass-lined autoclave vessel, subjected to hydrothermal treatment at 140°C for 5 hours, cooled to room temperature, and then removed. The obtained sol was a water-dispersed sol of titanium oxide-stannic oxide composite oxide colloidal particles (A2), and had a total metal oxide concentration (TiO 2 , and SnO 2 The sol was dried at 110°C and the powder was subjected to X-ray diffraction analysis, which confirmed that the powder was a rutile crystal.
[0137] (Reference Example 3): Preparation of titanium oxide colloidal particles (A3) to serve as cores 319.5 g of a 25% by mass aqueous solution of tetramethylammonium hydroxide was dissolved in 947.1 g of pure water, and 236.6 g of titanium tetraisopropoxide (TiO2 To the mixture, 82.0 g of oxalic acid dihydrate (containing 66.6 g in terms of oxalic acid equivalent) and 82.0 g of oxalic acid dihydrate (58.5 g in terms of oxalic acid equivalent) were added under stirring. The mixed solution was maintained at 80°C for 2 hours, and then the pressure was reduced to 580 Torr and maintained for 2 hours to prepare a mixed solution. The mixed solution was placed in a glass-lined autoclave vessel, subjected to hydrothermal treatment at 140°C for 5 hours, cooled to room temperature, and then removed. The obtained sol was a water-dispersed sol of titanium oxide colloidal particles (A3), and had a total metal oxide concentration (TiO 2 The sol was dried at 110°C and the powder was subjected to X-ray diffraction analysis, which confirmed that the sol was anatase-type crystals.
[0138] (Reference Example 4): Preparation of silicon dioxide-stannic oxide composite oxide colloidal particles (B1) to be coated. 2 77.2 g of sodium stannate (containing 29.8% by mass of sodium stannate in terms of sodium stannate equivalent) was dissolved in 668.8 g of pure water, and then sodium stannate NaSnO 3 ・H 2 O(SnO 2 Into this aqueous solution, 20.9 g of silicon dioxide-stannic oxide composite oxide colloidal particles (B1) was dissolved, containing 55.1% by mass of silicon dioxide. The resulting aqueous solution was passed through a column packed with a hydrogen-type cation exchange resin (Amberlite (trade name) IR-120B). Next, 7.2 g of diisopropylamine was added to the resulting aqueous dispersion sol. The resulting sol was an aqueous dispersion sol of alkaline silicon dioxide-stannic oxide composite oxide colloidal particles (B1), with a pH of 8.0 and a total metal oxide concentration (SiO 2 , and SnO 2 ) 1.7% by mass, and the average primary particle diameter was 3 nm as determined by observation with a transmission electron microscope.
[0139] (Reference Example 5): Preparation of antimony pentoxide colloidal particles (B2) to be coated Antimony trioxide (Sb 2 O 3To the mixture were added 125 g of potassium hydroxide (containing 99.5% by mass as KOH), 660 g of pure water, and 125 g of potassium hydroxide (containing 95% by mass as KOH), and 84 g of 35% hydrogen peroxide was gradually added under stirring. The resulting aqueous solution of potassium antimonate was diluted to 2.2% by mass and passed through a column packed with hydrogen cation exchange resin. To the ion-exchanged antimonic acid solution, 2.5 g of diisopropylamine was added under stirring. The resulting sol was an aqueous dispersion sol of antimony pentoxide colloidal particles (B2), with a pH of 10.8 and Sb 2 O 5 The concentration was 1.5% by mass, and the average primary particle diameter was 6 nm as determined by observation with a transmission electron microscope.
[0140] (Production Example 1): Preparation of titanium oxide-stannic oxide composite oxide colloidal particles (C1) modified with silicon dioxide-stannic oxide composite oxide 1500.0 g of the aqueous dispersion sol of titanium oxide-stannic oxide composite oxide colloidal particles (A1) prepared in Reference Example 1 was added with stirring to 661.8 g of the aqueous dispersion sol of alkaline silicon dioxide-stannic oxide composite oxide colloidal particles (B1) prepared in Reference Example 4, and the mixture was heated at 95°C for 3 hours, after which the mixture was passed through a column packed with a cation exchange resin (Amberlite (trade name) IR-120B, manufactured by Organo Corporation). 667 parts by mass of the solids of the sol that would become the core were added to the container relative to 100 parts by mass of the solids of the coating sol filled in the container, and the addition was carried out over 10 minutes at a rate of 66.7 parts by mass per minute. To the obtained water-dispersed sol, 2.5 g of tri-n-pentylamine was added, and the mixture was concentrated by an ultrafiltration membrane method to obtain a water-dispersed sol of titanium oxide-stannic oxide composite oxide colloidal particles (C1) modified with silicon dioxide-stannic oxide composite oxide. This water-dispersed sol had a pH of 5.2, a total metal oxide (TiO 2 , SnO 2 , and SiO 2 ) concentration was 30.5% by mass, viscosity was 5.0 mPa·s, and DLS average secondary particle diameter was 15 nm.
[0141] (Production Example 2): Preparation of titanium oxide-stannic oxide composite oxide colloidal particles (C2) modified with silicon dioxide-stannic oxide composite oxide 1500.0 g of the aqueous dispersion sol of titanium oxide-stannic oxide composite oxide colloidal particles (A1) prepared in Reference Example 1 was added with stirring to 330.9 g of the aqueous dispersion sol of alkaline silicon dioxide-stannic oxide composite oxide colloidal particles (B1) prepared in Reference Example 4, and the mixture was heated at 95°C for 3 hours, after which the mixture was passed through a column packed with a cation exchange resin (Amberlite (trade name) IR-120B, manufactured by Organo Corporation). 1340 parts by mass of the solids of the sol serving as the core was added to the container relative to 100 parts by mass of the solids of the coating sol filled in the container, and the addition was carried out over 20 minutes at a rate of 67 parts by mass per minute. To the obtained water-dispersed sol, 2.0 g of tri-n-pentylamine was added, and the mixture was concentrated by an ultrafiltration membrane method to obtain a water-dispersed sol of titanium oxide-stannic oxide composite oxide colloidal particles (C2) modified with silicon dioxide-stannic oxide composite oxide. This water-dispersed sol had a pH of 5.2, a total metal oxide (TiO 2 , SnO 2 , and SiO 2 ) concentration was 30.5% by mass, viscosity was 6.0 mPa·s, and DLS average secondary particle diameter was 18 nm.
[0142] (Production Example 3): Preparation of titanium oxide-stannic oxide-zirconium oxide composite oxide colloidal particles (C3) modified with silicon dioxide-stannic oxide composite oxide Zirconium oxychloride (ZrO 2 82.7 g of a zirconium oxychloride solution (containing 21.2% by mass in terms of ZrO) was diluted with 501.1 g of pure water to obtain 583.8 g of an aqueous solution of zirconium oxychloride (ZrO 2A 100.0 g aqueous dispersion sol of titanium dioxide-stannic oxide composite oxide colloidal particles (A2) prepared in Reference Example 2 was prepared, and 1750.0 g of the aqueous dispersion sol of titanium oxide-stannic oxide composite oxide colloidal particles (A2) prepared in Reference Example 2 was added under stirring. Hydrolysis was then carried out by heating at 95°C for 5 hours, yielding an aqueous dispersion sol of titanium oxide-stannic oxide-zirconium oxide composite oxide colloidal particles having a thin film layer of zirconium oxide formed on the surface. 1852.9 g of the aqueous dispersion sol of alkaline silicon dioxide-stannic oxide composite oxide colloidal particles (B1) prepared in Reference Example 4 was added to 2330.0 g of the obtained aqueous dispersion sol under stirring, and the mixture was passed through a column packed with 500 mL of anion exchange resin (Amberlite (trade name) IRA-410, manufactured by Organo Corporation). The aqueous dispersion sol after passing through was then heated at 95°C for 5 hours, and then passed through a column packed with cation exchange resin (Amberlite (trade name) IR-120B, manufactured by Organo Corporation). The solid content of the coating sol added to the container was 30 parts by mass relative to 100 parts by mass of the sol solids that served as the core filled in the container, and the addition was carried out over one minute at a rate of 30 parts by mass per minute. 3.5 g of tri-n-pentylamine was added to the obtained water-dispersed sol, and the mixture was concentrated by an ultrafiltration membrane method to obtain a water-dispersed sol of titanium oxide-stannic oxide-zirconium oxide composite oxide colloidal particles (C3) modified with silicon dioxide-stannic oxide composite oxide. This water-dispersed sol had a pH of 5.2, a total metal oxide content (TiO 2 , ZrO 2 , SnO 2 , and SiO 2 ) concentration was 30.5% by mass, viscosity was 5.0 mPa·s, and DLS average secondary particle diameter was 20 nm.
[0143] (Production Example 4): Preparation of titanium oxide-stannic oxide-zirconium oxide composite oxide colloidal particles (C4) modified with silicon dioxide-stannic oxide composite oxide Zirconium oxychloride (ZrO 2 82.7 g of a zirconium oxychloride solution (containing 21.2% by mass in terms of ZrO) was diluted with 501.1 g of pure water to obtain 583.8 g of an aqueous solution of zirconium oxychloride (ZrO 2A 100.0 g aqueous dispersion sol of titanium dioxide-stannic oxide composite oxide colloidal particles (A1) prepared in Reference Example 1 was prepared, and 1750.0 g of the aqueous dispersion sol of titanium dioxide-stannic oxide composite oxide colloidal particles (A1) prepared in Reference Example 1 was added under stirring. Hydrolysis was then carried out by heating to 95°C, yielding an aqueous dispersion sol of titanium oxide-stannic oxide-zirconium oxide composite oxide colloidal particles having a thin film layer of zirconium oxide formed on the surface. 2470.6 g of the aqueous dispersion sol of alkaline silicon dioxide-stannic oxide composite oxide colloidal particles (B1) prepared in Reference Example 4 was added to 2330.0 g of the obtained aqueous dispersion sol under stirring, and the mixture was passed through a column packed with 500 mL of anion exchange resin (Amberlite (trade name) IRA-410, manufactured by Organo Corporation). The aqueous dispersion sol after passing through was then heated at 95°C for 5 hours and then passed through a column packed with cation exchange resin. The solid content of the coating sol added to the container was 40 parts by mass relative to 100 parts by mass of the sol solids that served as the core filled in the container, and the addition was carried out over one minute at a rate of 40 parts by mass per minute. 5.6 g of tri-n-pentylamine was added to the obtained water-dispersed sol, and the mixture was concentrated by an ultrafiltration membrane method to obtain a water-dispersed sol of titanium oxide-stannic oxide-zirconium oxide composite oxide colloidal particles (C4) modified with silicon dioxide-stannic oxide composite oxide. This water-dispersed sol had a pH of 5.1, a total metal oxide content (TiO 2 , ZrO 2 , SnO 2 , and SiO 2 ) concentration was 30.5% by mass, viscosity was 5.0 mPa·s, and DLS average secondary particle diameter was 25 nm.
[0144] (Production Example 5): Preparation of titanium oxide-stannic oxide-zirconium oxide composite oxide colloidal particles (C5) modified with silicon dioxide-stannic oxide composite oxide Zirconium oxychloride (ZrO 2 82.7 g of a zirconium oxychloride solution (containing 21.2% by mass in terms of ZrO) was diluted with 501.1 g of pure water to obtain 583.8 g of an aqueous solution of zirconium oxychloride (ZrO 2A 100.0 g aqueous dispersion sol of titanium dioxide-stannic oxide composite oxide colloidal particles (A1) prepared in Reference Example 1 was prepared, and 1750.0 g of the aqueous dispersion sol of titanium dioxide-stannic oxide composite oxide colloidal particles (A1) prepared in Reference Example 1 was added under stirring. Hydrolysis was then carried out by heating to 95°C, yielding an aqueous dispersion sol of titanium oxide-stannic oxide-zirconium oxide composite oxide colloidal particles having a thin film layer of zirconium oxide formed on the surface. 3088.2 g of the aqueous dispersion sol of alkaline silicon dioxide-stannic oxide composite oxide colloidal particles (B1) prepared in Reference Example 4 was added to 2330.0 g of the obtained aqueous dispersion sol under stirring, and the mixture was passed through a column packed with 500 mL of anion exchange resin (Amberlite (trade name) IRA-410, manufactured by Organo Corporation). The aqueous dispersion sol after passing through was then heated at 95°C for 5 hours and then passed through a column packed with cation exchange resin. The solid content of the coating sol added to the container was 50 parts by mass relative to 100 parts by mass of the sol solids that constituted the core filled in the container, and the addition was carried out over 2 minutes at a rate of 25 parts by mass per minute. 6.2 g of tri-n-pentylamine was added to the obtained water-dispersed sol, and the mixture was concentrated by an ultrafiltration membrane method to obtain a water-dispersed sol of titanium oxide-stannic oxide-zirconium oxide composite oxide colloidal particles (C4) modified with silicon dioxide-stannic oxide composite oxide. This water-dispersed sol had a pH of 5.0, a total metal oxide content of 100% (TiO 2 , ZrO 2 , SnO 2 , and SiO 2 ) concentration was 30.5% by mass, viscosity was 5.4 mPa·s, and DLS average secondary particle diameter was 24 nm.
[0145] (Production Example 6): Preparation of titanium oxide-stannic oxide composite oxide colloidal particles (C6) modified with antimony pentoxide colloidal particles. 1500.0 g of the aqueous dispersion sol of titanium oxide-stannic oxide composite oxide colloidal particles (A1) prepared in Reference Example 1 was added to 1500.0 g of the aqueous dispersion sol of alkaline antimony pentoxide colloidal particles (B2) prepared in Reference Example 5 under stirring, heated at 95°C for 3 hours, and then passed through a column packed with a cation exchange resin. The solid content of the core sol added to the container was 333 parts by mass relative to 100 parts by mass of the solid content of the coating sol filled in the container. The addition was carried out over 10 minutes at a rate of 33.3 parts by mass per minute. 1.8 g of diisobutylamine was added to the obtained aqueous dispersion sol, and the mixture was concentrated by ultrafiltration membrane to obtain an aqueous dispersion sol of titanium oxide-stannic oxide composite oxide colloidal particles (C6) modified with antimony pentoxide colloidal particles. This water-dispersed sol had a pH of 5.6 and contained a total of 100% of metal oxides (TiO 2 , SnO 2 , and Sb 2 O 5 ) concentration was 30.5% by mass, viscosity was 5.5 mPa·s, and DLS average secondary particle diameter was 18 nm.
[0146] (Production Example 7): Preparation of anatase-type titanium oxide colloidal particles (C7) modified with silicon dioxide-stannic oxide composite oxide. 1500.0 g of the aqueous dispersion sol of anatase-type titanium oxide colloidal particles (A3) prepared in Reference Example 3 was added to 1764.7 g of the aqueous dispersion sol of alkaline silicon dioxide-stannic oxide composite oxide colloidal particles (B1) prepared in Reference Example 4 under stirring, heated at 95°C for 3 hours, and then passed through a column packed with a cation exchange resin. The solid content of the core sol added to the container was 250 parts by mass per 100 parts by mass of the coating sol solids filled in the container, and the addition was carried out over 10 minutes at a rate of 25.0 parts by mass per minute. 4.5 g of diisobutylamine was added to the obtained aqueous dispersion sol, and the mixture was concentrated by ultrafiltration membrane to obtain an aqueous dispersion sol of anatase-type titanium oxide colloidal particles (C7) modified with silicon dioxide-stannic oxide composite oxide. This water-dispersed sol had a pH of 5.2 and a total metal oxide (TiO 2 , SnO 2 , and SiO2 ) concentration was 30.5% by mass, viscosity was 6.5 mPa·s, and DLS average secondary particle diameter was 28 nm.
[0147] (Production Example 8): Preparation of titanium oxide-stannic oxide composite oxide colloidal particles (C8) whose cores have been surface-modified with polyoxyethylene alkyl ether phosphate To 1500.0 g of the aqueous dispersion sol of the titanium oxide-stannic oxide composite oxide colloidal particles (A1) prepared in Reference Example 1, 15.0 g of polyoxyethylene alkyl ether phosphate (RS-710, manufactured by Toho Chemical Industry Co., Ltd.) was added as a surface modifier under stirring to surface-modify the particles. The resulting sol was concentrated by ultrafiltration membrane method to obtain an aqueous dispersion sol of titanium oxide-stannic oxide composite oxide colloidal particles (C8) whose cores have been surface-modified with polyoxyethylene alkyl ether phosphate. This aqueous dispersion sol had a pH of 2.8, a total metal oxide (TiO 2 , SnO 2 ) concentration was 30.0 mass %, viscosity was 6.5 mPa·s, and DLS average secondary particle diameter was 26 nm.
[0148] (Production Example 9): Preparation of titanium oxide-stannic oxide composite oxide colloidal particles (C9) modified with silicon dioxide-stannic oxide composite oxide 1500.0 g of the aqueous dispersion sol of titanium oxide-stannic oxide composite oxide colloidal particles (A1) prepared in Reference Example 1 was added with stirring to 4411.8 g of the aqueous dispersion sol of alkaline silicon dioxide-stannic oxide composite oxide colloidal particles (B1) prepared in Reference Example 4, and the mixture was heated at 95°C for 3 hours, after which the mixture was passed through a column packed with a cation exchange resin (Amberlite (trade name) IR-120B, manufactured by Organo Corporation). 100 parts by mass of the solids content of the sol serving as the core was added to the container relative to 100 parts by mass of the solids content of the coating sol filled in the container, and the addition was carried out over 10 minutes at a rate of 10 parts by mass per minute. To the obtained water-dispersed sol, 3.1 g of tri-n-pentylamine was added, and the mixture was concentrated by an ultrafiltration membrane method to obtain a water-dispersed sol of titanium oxide-stannic oxide composite oxide colloidal particles (C1) modified with silicon dioxide-stannic oxide composite oxide. This water-dispersed sol had a pH of 5.2, a total metal oxide (TiO 2 , SnO 2 , and SiO2 ) concentration was 30.5% by mass, viscosity was 5.0 mPa·s, and DLS average secondary particle diameter was 20 nm.
[0149] (Production Example 10): Preparation of titanium oxide-stannic oxide-zirconium oxide composite oxide colloidal particles (C10) modified with silicon dioxide-stannic oxide composite oxide 2 82.7 g of a zirconium oxychloride solution (containing 21.2% by mass in terms of ZrO) was diluted with 501.1 g of pure water to obtain 583.8 g of an aqueous solution of zirconium oxychloride (ZrO 2 A 100.0 g aqueous dispersion sol of titanium dioxide-stannic oxide composite oxide colloidal particles (A1) prepared in Reference Example 1 was prepared, and 1750.0 g of the aqueous dispersion sol of titanium dioxide-stannic oxide composite oxide colloidal particles (A1) prepared in Reference Example 1 was added under stirring. Hydrolysis was then carried out by heating to 95°C, yielding an aqueous dispersion sol of titanium oxide-stannic oxide-zirconium oxide composite oxide colloidal particles having a thin film layer of zirconium oxide formed on the surface. 6176.4 g of the aqueous dispersion sol of alkaline silicon dioxide-stannic oxide composite oxide colloidal particles (B1) prepared in Reference Example 4 was added to 2330.0 g of the obtained aqueous dispersion sol under stirring, and the mixture was passed through a column packed with 500 mL of anion exchange resin (Amberlite (trade name) IRA-410, manufactured by Organo Corporation). The aqueous dispersion sol after passing through the mixture was then heated at 95°C for 5 hours and then passed through a column packed with cation exchange resin. The solid content of the coating sol added to the container was 100 parts by mass relative to 100 parts by mass of the sol solids that served as the core filled in the container, and the addition was carried out over 5 minutes at a rate of 20 parts by mass per minute. 10.2 g of tri-n-pentylamine was added to the obtained water-dispersed sol, and the mixture was concentrated by an ultrafiltration membrane method to obtain a water-dispersed sol of titanium oxide-stannic oxide-zirconium oxide composite oxide colloidal particles (C10) modified with silicon dioxide-stannic oxide composite oxide. This water-dispersed sol had a pH of 5.4, a total metal oxide content of 10.2 g, and a total metal oxide content of 10.2 g. 2 , ZrO 2 , SnO 2 , and SiO 2 ) concentration was 30.5% by mass, viscosity was 5.8 mPa·s, and DLS average secondary particle diameter was 21 nm.
[0150] Example 1 The dispersion medium of 100 g of the aqueous dispersion sol of titanium oxide-stannic oxide composite oxide colloidal particles (C1) modified with silicon dioxide-stannic oxide composite oxide obtained in Production Example 1 was replaced with methanol using a rotary evaporator to obtain a methanol dispersion sol of titanium oxide-stannic oxide composite oxide colloidal particles (C1) modified with silicon dioxide-stannic oxide composite oxide. 1.52 g of polyoxyethylene alkyl ether phosphate (manufactured by Toho Chemical Industry Co., Ltd.: trade name RS-710) was added as a surface modifier to 100 g of the obtained sol under stirring, and the particles were surface-modified by heating under reflux at 65°C for 5 hours. This surface-modified methanol dispersion sol had a pH of 4.5, a total metal oxide (TiO 2 , SnO 2 , and SiO 2 The concentration was 20.5% by mass, the viscosity was 2.3 mPa·s, and the DLS average secondary particle size was 16 nm. 31 P-NMR showed that P-O-Ti was "bonded," the residual color rate was 54%, the mass ratio of (metal oxide other than titanium oxide) / (titanium oxide) was 0.26, the particle refractive index was 2.25, and the dispersion stability was "good."
[0151] FIG. 1 shows the titanium oxide-stannic oxide composite oxide colloidal particles (C1) modified with silicon dioxide-stannic oxide composite oxide used in Example 1. 31 In the P-NMR spectrum, there are areas where the shell layer covering the core is partially missing, exposing the core, and when these core-shell modified metal oxide particles are contacted with an aqueous phosphoric acid solution, a peak is confirmed near δ = 3 to 5 ppm, which is attributable to a (Ti-O-P) bond between a Ti atom in the core and a P atom present in the phosphoric acid in the shell layer via an oxygen atom, and this is deemed to indicate that a (Ti-O-P) bond is "present." In other words, there are areas in the core-shell metal oxide particles where part of the shell layer covering the core is missing, exposing the core.
[0152] (Example 2) A sol was prepared in the same manner as in Example 1, except that the colloidal particles in Example 1 were changed to (C2) obtained in Production Example 2. At this time, the methanol dispersion sol had a pH of 4.2, a total metal oxide (TiO 2 , SnO 2 , and SiO2 The concentration was 30.5% by mass, the viscosity was 4.5 mPa·s, and the DLS average secondary particle diameter was 45 nm. 31 P-NMR showed that P-O-Ti was "bonded," the residual color rate was 22%, the mass ratio of (metal oxide other than titanium oxide) / (titanium oxide) was 0.18, the particle refractive index was 2.30, and the dispersion stability was "good."
[0153] (Example 3) A sol was prepared in the same manner as in Example 1, except that the colloidal particles in Example 1 were changed to (C3) obtained in Production Example 3. At this time, the methanol dispersion sol had a pH of 4.5, a total metal oxide (TiO 2 , ZrO 2 , SnO 2 , and SiO 2 The concentration was 30.5% by mass, the viscosity was 4.5 mPa·s, and the DLS average secondary particle diameter was 28 nm. 31 P-NMR showed that P-O-Ti was "bonded," the residual color rate was 88%, (metal oxide other than titanium oxide) / (titanium oxide) was 0.85, the particle refractive index was 2.10, and the dispersion stability was "good."
[0154] (Example 4) A sol was prepared in the same manner as in Example 1, except that the colloidal particles in Example 1 were changed to (C4) obtained in Production Example 4. At this time, the methanol dispersion sol had a pH of 4.6, a total metal oxide (TiO 2 , ZrO 2 , SnO 2 , and SiO 2 The concentration was 30.5% by mass, the viscosity was 4.5 mPa·s, and the DLS average secondary particle size was 21 nm. 31 P-NMR showed that P-O-Ti was "bonded," the color retention rate was 98%, the mass ratio of (metal oxide other than titanium oxide) / (titanium oxide) was 0.83, the particle refractive index was 2.10, and the dispersion stability was "good."
[0155] (Example 5) A sol was prepared in the same manner as in Example 1, except that the colloidal particles in Example 1 were changed to (C5) obtained in Production Example 5. At this time, the methanol dispersion sol had a pH of 4.4, a total metal oxide (TiO 2 , ZrO 2 , SnO 2 , and SiO 2The concentration was 30.5% by mass, the viscosity was 4.5 mPa·s, and the DLS average secondary particle diameter was 29 nm. 31 P-NMR showed that P-O-Ti was "bonded," the color retention rate was 98%, the mass ratio of (metal oxide other than titanium oxide) / (titanium oxide) was 0.97, the particle refractive index was 2.00, and the dispersion stability was "○."
[0156] (Example 6) A sol was prepared in the same manner as in Example 1, except that the colloidal particles in Example 1 were changed to (C6) obtained in Production Example 6. At this time, the methanol dispersion sol had a pH of 4.0, a total metal oxide (TiO 2 , SnO 2 , and Sb 2 O 5 The concentration was 20.5% by mass, the viscosity was 2.5 mPa·s, and the DLS average secondary particle size was 20 nm. 31 P-NMR showed that P-O-Ti was "bonded," the residual color rate was 10%, the mass ratio of (metal oxide other than titanium oxide) / (titanium oxide) was 0.42, the particle refractive index was 2.25, and the dispersion stability was "good."
[0157] (Example 7) A sol was prepared in the same manner as in Example 1, except that the colloidal particles in Example 1 were changed to (C7) obtained in Production Example 7. At this time, the methanol-dispersed sol had a pH of 4.2, a total metal oxide (TiO 2 , SnO 2 , and SiO 2 The concentration was 20.5% by mass, the viscosity was 2.3 mPa·s, and the DLS average secondary particle diameter was 29 nm. 31 P-NMR showed that P-O-Ti was "bonded," the residual color rate was 40%, the mass ratio of (metal oxide other than titanium oxide) / (titanium oxide) was 0.40, the particle refractive index was 2.20, and the dispersion stability was "good."
[0158] Example 8 A sol was prepared in the same manner as in Example 1, except that the surface modifier was changed to 2.0 g of phenyltrimethoxysilane (manufactured by Shin-Etsu Chemical Co., Ltd., product name KBM-103). At this time, the methanol-dispersed sol had a pH of 5.9 and a total metal oxide (TiO 2 , SnO 2 , and SiO 2The concentration was 30.5% by mass, the viscosity was 2.0 mPa·s, and the DLS average secondary particle size was 16 nm. 31 P-NMR showed that P-O-Ti was "bonded," the residual color rate was 54%, (metal oxide other than titanium oxide) / (titanium oxide) was 0.26, the particle refractive index was 2.25, and the dispersion stability was "good."
[0159] Example 9: Evaluation of Cured Film - A1 A PGME-dispersed sol was prepared by again using a rotary evaporator to replace the dispersion medium of 100 g of a methanol-dispersed sol of titanium oxide-stannic oxide composite oxide colloidal particles (C1) that had been surface-modified with polyoxyethylene alkyl ether phosphate (manufactured by Toho Chemical Industry Co., Ltd.: trade name RS-710) obtained in Example 1 with propylene glycol monomethyl ether (PGME). The PGME-dispersed sol had a pH of 4.7, a total metal oxide (TiO 2 , SnO 2 , and SiO 2 The concentration was 20.5% by mass, the viscosity was 4.5 mPa·s, and the DLS average secondary particle size was 12 nm. 31 P-NMR showed that P-O-Ti was "bonded," the residual color rate was 54%, the mass ratio of (metal oxide other than titanium oxide) / (titanium oxide) was 0.26, the particle refractive index was 2.25, and the dispersion stability was "good."
[0160] Next, a cured film was prepared using this sol according to the following procedure. 2.0 g of a mixture of dipentaerythritol hexaacrylate and pentaacrylate (manufactured by Nippon Kayaku Co., Ltd., trade name KAYARAD DPHA) as a resin binder and 4.9 g of PGME were added to a brown bottle equipped with a magnetic stirrer, and 22.9 g of the sol of Example 9 was added while stirring. Next, 0.02 g of a photoradical polymerization initiator (manufactured by BASF Corporation, trade name Irgacure OXE01) and 0.3 g of a PGME solution (KP-412 concentration 10.0% by mass) of a methacrylic group-type surface modifier (manufactured by Shin-Etsu Chemical Co., Ltd., trade name KP-412) were added, followed by stirring for 0.5 hours to prepare a coating liquid. Glass substrates were prepared, and the coating liquid was applied to them by spin coating at room temperature of 25°C and humidity of 50% (film thickness of 1 μm). After volatilizing the solvent at 100°C for 1 minute, the coating liquid was applied to the glass substrates with an integrated light intensity of 1000 mJ / cm. 2 The coating solution was then cured with ultraviolet light using a high-pressure mercury lamp until the cured film reached a refractive index of 1.80, transparency of "○", and light resistance of "○". The coating solution was also used to evaluate imprintability, which was also evaluated as "○".
[0161] Example 10 Cured Film Evaluation-A2 To 100 g of the methanol dispersion sol of titanium oxide-stannic oxide composite oxide colloidal particles (C1) modified with silicon dioxide-stannic oxide composite oxide and surface-modified with polyoxyethylene alkyl ether phosphate (manufactured by Toho Chemical Industry Co., Ltd.: trade name RS-710) obtained in Example 1, 1.5 g of RS-710 was further added, and the dispersion medium was again replaced with propylene glycol monomethyl ether acetate (hereinafter, PGMEA) using a rotary evaporator to prepare a PGMEA dispersion sol. At this time, the PGMEA dispersion sol had a pH of 4.1, a total metal oxide (TiO 2 , SnO 2 , and SiO 2 The concentration was 20.5% by mass, the viscosity was 5.5 mPa·s, and the DLS average secondary particle size was 20 nm. 31 P-NMR showed that P-O-Ti was "bonded," the residual color rate was 54%, the mass ratio of (metal oxide other than titanium oxide) / (titanium oxide) was 0.26, the particle refractive index was 2.20, and the dispersion stability was "good."
[0162] Next, a cured film was prepared. The cured film was prepared in the same manner as in Example 9, Cured Film Evaluation-A1, except that the sol in Example 9, Cured Film Evaluation-A1, was changed to the sol of this Example 10. The obtained cured film had a refractive index of 1.80, transparency of "○", and light resistance of "○". Furthermore, when the same coating liquid was used to evaluate imprintability, it was evaluated as "○".
[0163] (Example 11 Cured Film Evaluation-A3) A cured film was prepared in the same manner as in Example 9 Cured Film Evaluation-A1, except that the resin binder was changed to a urethane acrylate with a trade name of UA4200 (manufactured by Shin-Nakamura Chemical Co., Ltd.). The obtained cured film had a refractive index of 1.80, transparency of "○", and light resistance of "○". Furthermore, when the same coating liquid was used to evaluate imprintability, it was rated as "○".
[0164] Example 12 Cured Film Evaluation-A4 A cured film was prepared in the same manner as in Example 9 Cured Film Evaluation-A1, except that the resin binder used in Example 9 Cured Film Evaluation-A1 was changed to Aronix MT-3010 (manufactured by Toagosei Co., Ltd.). The resulting cured film had a refractive index of 1.80, transparency of "○", and light resistance of "○". The imprintability was also evaluated using the same coating liquid, and was rated as "○".
[0165] Example 13: Evaluation of Cured Film -A5 A sol was prepared in the same manner as in Example 3, except that the surface modifier was changed to 2.5 g of 3-methacryloxypropyltrimethoxysilane (manufactured by Shin-Etsu Chemical Co., Ltd., product name KBM-503). The methanol-dispersed sol had a pH of 5.7 and a total metal oxide (TiO 2 , ZrO 2 , SnO 2 , and SiO 2 The concentration was 30.5% by mass, the viscosity was 1.8 mPa·s, and the DLS average secondary particle size was 16 nm. 31 P-NMR showed that P-O-Ti was "bonded," the color retention rate was 88%, the mass ratio of (metal oxide other than titanium oxide) / (titanium oxide) was 0.85, the particle refractive index was 2.00, and the dispersion stability was "good."
[0166] Next, a cured film was prepared using this sol according to the following procedure. 25.8 g of γ-glycidoxypropyltrimethoxysilane was added to a glass container equipped with a magnetic stirrer, and 6.2 g of 0.01 N hydrochloric acid was added dropwise while stirring. After the dropwise addition was completed, stirring was continued for 0.5 hours to obtain a partial hydrolyzate of γ-glycidoxypropyltrimethoxysilane. Next, 22.5 g of propylene glycol monomethyl ether, 7.0 g of methanol, 85.6 g of the methanol-dispersed sol of Example 13, and 2.2 g of aluminum acetylacetonate as a curing agent were added to 32.0 g of the partial hydrolyzate of γ-glycidoxypropyltrimethoxysilane described above, and the mixture was stirred for 2 hours to prepare a coating liquid for hard coating. A urethane-based plastic lens (refractive index n D A hard coat coating solution (film thickness 3 μm) was applied to these by dip coating, the solvent was evaporated at 80° C. for 10 minutes, and then the coating was cured by heat treatment at 120° C. for 2 hours. The obtained cured film was evaluated as having a refractive index of 1.67, transparency of “good”, light resistance of “good”, and scratch resistance of “good”.
[0167] Example 14: Evaluation of Cured Film -A6 A sol was prepared in the same manner as in Example 3, except that the surface modifier was changed to 3.7 g of an allyl isocyanurate-based silane coupling agent (manufactured by Shin-Etsu Chemical Co., Ltd., product name X-12-1290). The methanol-dispersed sol had a pH of 5.7 and a total metal oxide (TiO 2 , ZrO 2 , SnO 2 , and SiO 2 The concentration was 30.5% by mass, the viscosity was 1.9 mPa·s, and the DLS average secondary particle size was 18 nm. 31 P-NMR showed that P-O-Ti was "bonded," the color retention rate was 88%, the mass ratio of (metal oxide other than titanium oxide) / (titanium oxide) was 0.85, the particle refractive index was 2.00, and the dispersion stability was "good."
[0168] Next, a cured film was prepared. The cured film was prepared in the same manner as in Example 13, Cured Film Evaluation-A5, except that the sol in Example 13, Cured Film Evaluation-A5, was changed to the sol of this Example 14. The obtained cured film had a refractive index of 1.67, and was evaluated as having transparency of "○", light resistance of "○", and scratch resistance of "○".
[0169] Example 15 Cured Film Evaluation - A7 An MEK-dispersed sol was prepared by again using a rotary evaporator to replace the dispersion medium of 100 g of a methanol-dispersed sol of titanium oxide-stannic oxide composite oxide colloidal particles (C3) that had been surface-modified with 3-methacryloxypropyltrimethoxysilane (manufactured by Shin-Etsu Chemical Co., Ltd., product name KBM-503) used in Example 13 with methyl ethyl ketone (hereinafter, MEK). The obtained MEK-dispersed sol had a pH of 6.0, a total metal oxide (TiO 2 , ZrO 2 , SnO 2 , and SiO 2 The concentration was 30.5% by mass, the viscosity was 2.1 mPa·s, and the DLS average secondary particle size was 17 nm. 31 P-NMR showed that P-O-Ti was "bonded," the color retention rate was 88%, the mass ratio of (metal oxide other than titanium oxide) / (titanium oxide) was 0.85, the particle refractive index was 2.00, and the dispersion stability was "good."
[0170] Next, a cured film was prepared using this sol according to the following procedure. 17.6 g of a mixture of dipentaerythritol hexaacrylate and pentaacrylate (manufactured by Nippon Kayaku Co., Ltd., trade name KAYARAD DPHA) as a resin binder, 5.2 g of methanol, and 18.3 g of PGME were added to a brown bottle equipped with a magnetic stirrer, and 57.2 g of the sol of this Example 15 was added while stirring. Next, 0.9 g of a photoradical polymerization initiator (manufactured by BASF Corporation, trade name Irgacure OXE01) and 0.9 g of a PGME solution (L-7001 concentration 2.0% by mass) of polyether-modified silicone oil (manufactured by Dow Corning Toray Co., Ltd., trade name L-7001) were added, and the mixture was stirred for 0.5 hours to prepare a coating liquid. Glass substrates were prepared, and the coating liquid was applied to them by spin coating (film thickness 3 μm). After volatilizing the solvent at 80° C. for 2 minutes, the coating liquid was applied to the glass substrates with an integrated light intensity of 1000 mJ / cm 2 2 The resulting cured film was evaluated as having a refractive index of 1.67, transparency of "good", light resistance of "good", and scratch resistance of "good".
[0171] Example 16: Evaluation of Cured Film - A8 A MEK-dispersed sol was prepared by again using a rotary evaporator to replace the dispersion medium of 100 g of a methanol-dispersed sol of titanium oxide-stannic oxide composite oxide colloidal particles (C1) that had been surface-modified with an allyl isocyanurate-based silane coupling agent (X-12-1290 manufactured by Shin-Etsu Chemical Co., Ltd.) used in Example 14 with MEK. The obtained MEK-dispersed sol had a pH of 5.9, a total metal oxide (TiO 2 , ZrO 2 , SnO 2 , and SiO 2 The concentration was 30.5% by mass, the viscosity was 1.7 mPa·s, and the DLS average secondary particle size was 15 nm. 31 P-NMR showed that P-O-Ti was "bonded," the color retention rate was 88%, the mass ratio of (metal oxide other than titanium oxide) / (titanium oxide) was 0.85, the particle refractive index was 2.00, and the dispersion stability was "good."
[0172] Next, a cured film was prepared. The cured film was prepared in the same manner as in Example 15, Cured Film Evaluation-A7, except that the sol in Example 15, Cured Film Evaluation-A7, was changed to the sol of this Example 16. The obtained cured film had a refractive index of 1.67, and was evaluated as having transparency of "○", light resistance of "○", and scratch resistance of "○".
[0173] Comparative Example 1: Cured Film Evaluation - B1 The dispersion medium of 100 g of the titanium oxide-stannic oxide composite oxide colloidal particles (C8) whose cores have been surface-modified with polyoxyethylene alkyl ether phosphate obtained in Production Example 8 was replaced with methanol using a rotary evaporator to obtain a methanol-dispersed sol of titanium oxide-stannic oxide composite oxide colloidal particles (C8) whose cores have been surface-modified with polyoxyethylene alkyl ether phosphate. This methanol-dispersed sol had a pH of 3.5, a total metal oxide (TiO 2 , and SnO 2 The concentration was 20.5% by mass, the viscosity was 2.3 mPa·s, and the DLS average secondary particle diameter was 32 nm. 31 P-NMR analysis of P-O-Ti showed that it was "bonded," the residual color rate was 0%, the mass ratio of (metal oxide other than titanium oxide) / (titanium oxide) was 0.10, the particle refractive index was 2.10, and the dispersion stability was "x."
[0174] FIG. 2 shows the titanium oxide-stannic oxide composite oxide colloidal particles (A1) obtained in Production Example 8 used in Comparative Example 1. 31 This is a P-NMR spectrum, and although there is no shell layer covering the core and the phosphoric acid aqueous solution comes into direct contact with the core, a peak was confirmed near δ = 3 to 5 ppm, which is attributable to a (Ti-O-P) bond formed between a Ti atom in the core and a P atom present in the phosphoric acid via an oxygen atom, and the (Ti-O-P) bond was determined to be "present." In other words, the (Ti-O-P) bond was present in the metal oxide particle consisting of the core alone.
[0175] Next, a cured film was prepared. The cured film was prepared in the same manner as in Example 13, Cured Film Evaluation-A5, except that the weight of the metal oxide in this Comparative Example 1 was changed so that the weight of the metal oxide was the same as in Example 13, Cured Film Evaluation-A5. The obtained cured film had a refractive index of 1.70, transparency of "○", and light resistance of "×", which were insufficient, and was evaluated as scratch resistance of "○".
[0176] Comparative Example 2: Cured Film Evaluation - B2 The dispersion medium of 100 g of the titanium oxide-stannic oxide composite oxide colloidal particles (C9) modified with silicon dioxide-stannic oxide composite oxide obtained in Production Example 9 was replaced with methanol using a rotary evaporator. The solvent was then replaced with PGME to obtain a PGME dispersion sol. The PGME dispersion sol had a pH of 4.7, a total metal oxide (TiO 2 , SnO 2 , and SiO 2 The concentration was 20.5% by mass, the viscosity was 4.5 mPa·s, and the DLS average secondary particle diameter was 21 nm. 31 P-NMR analysis of P-O-Ti showed "no bonds," the color retention rate was 98%, the mass ratio of (metal oxide other than titanium oxide) / (titanium oxide) was 1.38, the particle refractive index was 1.78, and the dispersion stability was "good."
[0177] Next, a cured film was prepared using this sol according to the following procedure. 1.3 g of a mixture of dipentaerythritol hexaacrylate and pentaacrylate (manufactured by Nippon Kayaku Co., Ltd., trade name KAYARAD DPHA) as a resin binder and 3.0 g of PGME were added to a brown bottle equipped with a magnetic stirrer, and 25.3 g of the sol of this Comparative Example 2 was added while stirring. Next, 0.01 g of a photoradical polymerization initiator (manufactured by BASF Corporation, trade name Irgacure OXE01) and 0.3 g of a PGME solution (KP-412 concentration 10.0% by mass) of a methacrylic group-type surface modifier (manufactured by Shin-Etsu Chemical Co., Ltd., trade name KP-412) were added, and the mixture was stirred for 0.5 hours to prepare a coating liquid. Glass substrates were prepared, and the coating liquid was applied to them by spin coating (film thickness 1 μm). After volatilizing the solvent at 100° C. for 1 minute, the coating liquid was applied to the glass substrates with an integrated light intensity of 1000 mJ / cm 2The coating solution was then cured with ultraviolet light using a high-pressure mercury lamp until the cured film reached a refractive index of 1.65, transparency of "good", and light resistance of "good". The coating solution was also used to evaluate imprintability, resulting in an evaluation of "poor".
[0178] Comparative Example 3 Cured Film Evaluation-B3 A sol was prepared in the same manner as in Example 13 Cured Film Evaluation-A5, except that the sol in Example 13 Cured Film Evaluation-A5 was changed to the titanium oxide-stannic oxide-zirconium oxide composite oxide colloidal particles (C10) modified with silicon dioxide-stannic oxide composite oxide obtained in Production Example 10. The methanol-dispersed sol had a pH of 5.7, a total metal oxide content of 10.5% (TiO 2 , ZrO 2 , SnO 2 , and SiO 2 The concentration was 30.5% by mass, the viscosity was 1.6 mPa·s, and the DLS average secondary particle size was 22 nm. 31 P-NMR showed that P-O-Ti had "no bonds," the color retention rate was 98%, the mass ratio of (metal oxide other than titanium oxide) / (titanium oxide) was 1.85, and the particle refractive index was 1.70, which were all insufficient, and the dispersion stability was "good."
[0179] FIG. 3 shows the results of the titanium oxide-stannic oxide-zirconium oxide composite oxide colloidal particles (C10) modified with silicon dioxide-stannic oxide composite oxide obtained in Production Example 10 used in Comparative Example 3. 31 This is a P-NMR spectrum, and titanium oxide-stannic oxide-zirconium oxide composite oxide colloidal particles (C10) modified with silicon dioxide-stannic oxide composite oxide obtained in Production Example 10 were used. However, the cores were sufficiently coated with the shell layer, with no exposed core portions. Therefore, when these core-shell modified metal oxide particles were contacted with an aqueous phosphoric acid solution, no peak was observed near δ = 3 to 5 ppm, which is attributable to a (Ti-O-P) bond formed between the Ti atom in the core and the P atom present in the phosphoric acid via an oxygen atom, and the (Ti-O-P) bond was recorded as "no bond." In other words, in the core-shell metal oxide particles, there were no portions where the shell layer covering the core was missing and the core was exposed, and the core was completely covered with the shell layer.
[0180] Next, a cured film was prepared. The cured film was prepared in the same manner as in Example 13, Cured Film Evaluation-A5, except that the sol in Example 13, Cured Film Evaluation-A5, was changed to the sol of this Comparative Example 13. The obtained cured film had a refractive index of 1.56, and was evaluated as having transparency of "○", light resistance of "○", and scratch resistance of "○".
[0181] Comparative Example 4 Cured Film Evaluation - B4 In Comparative Example 3 Cured Film Evaluation B3, 100 g of a methanol dispersion sol of titanium oxide-stannic oxide composite oxide colloidal particles (C10) modified with silicon dioxide-stannic oxide composite oxide and surface-modified with 3-methacryloxypropyltrimethoxysilane (manufactured by Shin-Etsu Chemical Co., Ltd., product name KBM-503) was again subjected to rotary evaporator to replace the dispersion medium with MEK, thereby preparing an MEK dispersion sol. The obtained MEK dispersion sol had a pH of 6.2, a total metal oxide (TiO 2 , ZrO 2 , SnO 2 , and SiO 2 The concentration was 30.5% by mass, the viscosity was 2.0 mPa·s, and the DLS average secondary particle size was 25 nm. 31 P-NMR showed that P-O-Ti had "no bonds," the color retention rate was 98%, the mass ratio of (metal oxide other than titanium oxide) / (titanium oxide) was 1.85, and the particle refractive index was 1.70, which were all insufficient, and the dispersion stability was "good."
[0182] Next, a cured film was prepared in the same manner as in Example 15, Cured Film Evaluation-A7, except that the sol in Example 15, Cured Film Evaluation-A7 was changed to the sol of this Comparative Example 4. The obtained cured film had a refractive index of 1.56, and was evaluated as having transparency of "○", light resistance of "○", and scratch resistance of "○".
[0183] The present invention provides modified core-shell metal oxide particles, which are used in compositions for obtaining coated articles with high refractive index and high moldability, such as for nanoimprinting, and which have a core made of titanium oxide-containing metal oxide particles and a shell made of metal oxide particles other than titanium oxide, with the core coated and part of the core exposed, as well as a method for producing the same.
Claims
1. A core-shell type metal oxide particle comprising a core containing metal oxide particles with an average primary particle diameter of 3 to 100 nm, and a shell covering the surface of the core and containing metal oxide particles with an average primary particle diameter of 1 to 7 nm, wherein the average primary particle diameter satisfies the relationship of (core metal oxide particles) > (shell metal oxide particles), and when component (a) is titanium oxide and component (b) is a metal oxide other than titanium oxide, the core is a particle consisting of component (a) or a combination of components (a) and (b), and the shell is a particle consisting of component (b), and the above core-shell type metal oxide particle satisfies the following requirements A and B: Requirement A: In a test in which the core-shell type metal oxide particle is brought into contact with a compound having a P-OH bond, the formation of a P-O-Ti bond is observed in the core-shell type metal oxide particle by NMR, and Requirement B: The refractive index of the core-shell type metal oxide particle is 1.85 or more.
2. The core-shell type metal oxide particles according to claim 1, wherein component (b) is at least one metal oxide particle selected from the group consisting of zirconium oxide, silicon dioxide, aluminum oxide, tin oxide, zinc oxide, iron oxide, niobium oxide, tantalum oxide, antimony oxide, and tungsten oxide.
3. The core-shell type metal oxide particles according to claim 1 or 2, wherein the mass ratio of (metal oxide other than titanium oxide) / (titanium oxide) is in the range of 0.05 to 1.
0.
4. Core-shell type metal oxide particles according to any one of claims 1 to 3, wherein an intermediate layer is present between the core particle and the shell particle, the intermediate layer being metal oxide particles comprising a combination of at least one kind selected from the group consisting of zirconium oxide, silicon dioxide, aluminum oxide, tin oxide, zinc oxide, iron oxide, niobium oxide, tantalum oxide, antimony oxide, and tungsten oxide as component (D), and the mass ratio of (metal oxide other than titanium oxide) / (titanium oxide) is in the range of 0.05 to 1.
0.
5. The core-shell type metal oxide particles according to any one of claims 1 to 4, wherein the surfaces of the core-shell type metal oxide particles are coated with a compound having a P-OH bond or a Si-OH bond.
6. The compound having a Si—OH bond is represented by the formula (1) to (3): (In formula (1), R 1 each represents an alkyl group, a halogenated alkyl group, an alkenyl group, an aryl group, or an organic group having a polyether group, an epoxy group, a (meth)acryloyl group, a mercapto group, an amino group, a ureido group, or a cyano group, and is bonded to a silicon atom via a Si-C bond; R 2 Each represents an alkoxy group, an acyloxy group, or a halogen group, a represents an integer of 1 to 3, and in formula (2) and formula (3), R 3 and R 5 are each an alkyl group having 1 to 3 carbon atoms or an aryl group having 6 to 30 carbon atoms and bonded to a silicon atom by a Si—C bond; R 4 and R 6 each represents an alkoxy group, an acyloxy group, or a halogen group, Y represents an alkylene group, an NH group, or an oxygen atom, b is an integer of 1 to 3, c is an integer of 0 or 1, and d is an integer of 1 to 3. The core-shell type metal oxide particle according to any one of claims 1 to 5, 7. A compound having a P-OH bond represented by formula (4) to formula (6): (In formulas (4) to (6), X 1 , X 2 , and X 3 each represents an alkylene group having 2 to 20 carbon atoms; f, h, and j each represent an integer of 1 to 100; e, g, and i each represent an integer of 1 to 3; Y 1 , Y 2 , and Y 3 each represents a hydrogen atom, an alkyl group having 1 to 20 carbon atoms, an alkenyl group having 2 to 20 carbon atoms, an aryl group having 6 to 30 carbon atoms, or a (meth)acrylic group.
8. The core-shell type metal oxide particles according to claim 7, wherein the phosphate ester is a polyoxyethylene alkyl (C6-20) ether phosphate ester having an alkyl group having 6 to 20 carbon atoms.
9. A core-shell metal oxide sol comprising the core-shell metal oxide particles according to any one of claims 1 to 8 dispersed as a dispersoid in a dispersion medium consisting of an alcohol which may have an ether bond, an ester, a ketone, an amide, a hydrocarbon, a silicone, a compound containing an unsaturated bond between linear carbon atoms, an oxirane compound, water, or a combination thereof, the core-shell metal oxide sol having an average particle size of 5 to 500 nm as determined by a dynamic light scattering method.
10. The core / shell metal oxide sol according to claim 9, further comprising a surfactant, which is an anionic surfactant, a cationic surfactant, a nonionic surfactant, or an amphoteric surfactant.
11. The core / shell metal oxide sol according to claim 9 or 10, further comprising a secondary amine or a tertiary amine having a total of 5 to 35 carbon atoms.
12. A varnish comprising the core-shell type metal oxide particles according to any one of claims 1 to 8 and a thermosetting or photosetting resin.
13. The varnish according to claim 12, which is a hard coat agent or a composition for nanoimprinting.
14. A method for producing a core-shell metal oxide sol according to any one of claims 9 to 11, comprising the following steps (i) and (ii): step (i): preparing a sol (A) containing metal oxide particles having an average primary particle diameter of 3 to 60 nm as a dispersion medium in water, and a sol (B) containing metal oxide particles having an average primary particle diameter of 1 to 7 nm as a dispersion medium in water, as measured by nitrogen gas adsorption; and step (ii): mixing the sol (A) and the sol (B) at a rate of 22 to 1,000 parts by mass per minute of the solid content of one sol charged in a container relative to 100 parts by mass of the solid content of the other sol added to the container.
15. The method for producing a core / shell metal oxide sol according to claim 14, further comprising the step (S-1) of adding a secondary amine or a tertiary amine having a total of 5 to 35 carbon atoms to the aqueous sol in the step (i) or (ii).
16. The method for producing a core-shell metal oxide sol according to claim 14 or 15, further comprising, after the step (ii), at least one step selected from the following steps (T-1), (T-2) and (T-3): step (T-1): adding at least one silane compound selected from the group consisting of formulas (1) to (3) or at least one phosphoric acid ester selected from the group consisting of formulas (4) to (6) to the core-shell metal oxide sol obtained in the step (ii), step (T-2): replacing the dispersion medium of the core-shell metal oxide sol obtained in the step (ii) with a dispersion medium consisting of an alcohol, an ester, a ketone, an amide or a hydrocarbon, and step (T-3): adding a surfactant to the core-shell metal oxide sol obtained in the step (ii).
17. A method for producing a core-shell metal oxide sol according to any one of claims 14 to 16, wherein the steps are step (i), step (S-1), step (ii), step (S-1), step (T-2), step (T-1), and step (T-2), in that order.
Citation Information
Patent Citations
Surfaceetreated product of plastics and its preparation
JP1977016586A
Coating composition
JP1978111336A
Copolymer for lenses of high refractive index
JP1980013747A
Transparent coated composite body
JP1987151801A
Coating composition containing titanium oxide
JP1988275682A