Silica fine particle dispersion for polishing, composition for polishing, and method for producing silica fine particle dispersion for polishing
A silica fine particle dispersion with a specific size range and distribution, combined with additives, addresses the challenges of high polishing rate and surface smoothness, enhancing both efficiency and reproducibility in electronic material polishing.
Patent Information
- Application Number
- PCT/JP2024/016468
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-08-31
- Filing Date
- 2024-04-26
- Publication Date
- 2024-11-21
AI Technical Summary
Conventional silica fine particle dispersions for polishing electronic materials face challenges in achieving a high polishing rate without deteriorating surface flatness and increasing the occurrence of scratches, with existing methods either resulting in poor reproducibility or requiring complex and equipment-intensive production processes.
A silica fine particle dispersion with specific surface area equivalent particle diameters between 5 nm and 200 nm, containing a mixture of truly spherical and irregularly shaped particles with a broad particle size distribution, is dispersed in a solvent, along with additives like polishing accelerators and surfactants, to enhance polishing efficiency and reduce scratches.
The dispersion achieves a high polishing rate while maintaining surface smoothness and reducing scratches, with improved reproducibility and reduced equipment load in production.
Smart Images

Figure JPOXMLDOC01-APPB-T000001 
Figure JPOXMLDOC01-APPB-T000002 
Figure JPOXMLDOC01-APPB-T000003
Abstract
Description
Polishing silica fine particle dispersion, polishing composition, and method for producing polishing silica fine particle dispersion
[0001] The present invention relates to a dispersion of fine silica particles for polishing, which is suitable for polishing various electronic materials such as silicon wafers, silicon carbide wafers, sapphire wafers, compound semiconductor wafers, and magnetic disks.
[0002] Conventionally, silica sol, fumed silica, fumed alumina, etc. have been used as polishing particles. In the manufacture of semiconductor integrated circuit-equipped substrates, aluminum wiring is formed on a silicon wafer, and an oxide film such as silica is then formed on top of this as an insulating film. In this case, unevenness is generated by the wiring, so this oxide film is polished to flatten it. In polishing such substrates, the surface after polishing must be flat without steps or unevenness, smooth without microscopic scratches, and have a high polishing rate.
[0003] A common method for achieving a high polishing rate is to use large abrasive grains. However, if the particle size of the abrasive grains becomes too large, the flatness of the substrate surface after polishing tends to deteriorate. Therefore, it is known that making the abrasive grains non-spherical, that is, making the abrasive grains irregularly shaped particles (irregular particles), is effective in achieving a high polishing rate without deteriorating the surface flatness. As a method for obtaining large, irregularly shaped particles, as disclosed in Patent Document 1, a method is known in which porous silica gel is pulverized using a bead mill or the like to prepare an irregularly shaped porous gel, and the irregularly shaped gel is grown by adding silicic acid or the like to obtain large, irregularly shaped particles with a high degree of irregularity.
[0004] In addition, as another method for obtaining a high polishing rate, it is known that the use of particles having a wide particle size distribution is also useful.As a method for producing particles having a wide particle size distribution, as disclosed in Patent Document 2, a method is known in which a predetermined silica sol is continuously added to a stirred and heated reaction vessel, silicic acid is added to the reaction vessel to grow particles, and the reaction solution is continuously withdrawn from an overflow line, thereby obtaining a silica sol having a broad particle size distribution.
[0005] JP 2018-177576 A JP 2012-503586 A
[0006] The irregular-shaped particles (non-spherical particles) described in Patent Document 1 have a relatively high polishing rate when used in polishing applications compared to spherical particles. However, the irregular-shaped particles described in Patent Document 1 have problems in that they tend to worsen the surface roughness and surface waviness of the polished substrate after polishing processing, and are prone to scratching. Furthermore, multiple attempts to produce irregular-shaped particles using the manufacturing method described in Patent Document 1 have revealed problems such as poor reproducibility of particle size and tendency for polishing performance to vary.
[0007] The spherical silica microparticles with a broad particle size distribution described in Patent Document 2 have a superior polishing rate compared to spherical silica microparticles with a sharp particle size distribution. However, it has been known that even silica microparticles with a broad particle size distribution cannot achieve the polishing rate achieved by irregularly shaped silica microparticles. Furthermore, the method for producing spherical silica microparticles with a broad particle size distribution described in Patent Document 2 requires the simultaneous addition of three components—seed particles (or a seed particle dispersion), an acidic silicic acid solution, and an alkaline component—to a reaction vessel while strictly controlling conditions (temperature, pH, etc.), resulting in a large equipment load and complicated production management. Furthermore, when the inventors actually conducted a tracing experiment, they found that although the particle size distribution was broad, the particle size distribution exhibited a tailing effect toward larger particles. Therefore, even if the average particle size was desirable, the silica microparticles contained some extremely large particles ranging from several hundred nanometers to microns, resulting in frequent scratches.
[0008] An object of the present invention is to provide a dispersion of fine silica particles for polishing, which, when applied to polishing, exhibits an excellent polishing rate and can suppress the occurrence of scratches on a substrate to be polished.
[0009] According to one aspect of the present invention, there is provided a dispersion of silica fine particles for polishing, which is obtained by dispersing in a solvent a particle group containing silica fine particles (having a particle diameter converted into specific surface area in the range of 5 nm to 200 nm) and which satisfies the following requirements 1) to 4): 1) The average sphericity of the particle group is in the range of 0.85 to 1.00; 2) In the weight-converted particle diameter distribution of the particle group, the cumulative 10% particle diameter (D 10 ), cumulative 90% particle diameter (D 90 ) and cumulative 50% particle diameter (D 50 ) satisfies the following formula (F1): 0.5≦(D 90 -D 10 ) / D 50 ≦3.0 (F1) 3) The particle group has a weight-equivalent particle size distribution with a distribution peak on the large particle size side 4) The particle group contains irregular-shaped particles in a range of 0.01% by number to 10% by number.
[0010] According to one aspect of the present invention, there is provided a polishing composition comprising the silica fine particle dispersion for polishing according to the aspect of the present invention and at least one selected from a polishing accelerator, a surfactant, a heterocyclic compound, a pH adjuster, and a pH buffer.
[0011] According to one aspect of the present invention, there is provided a method for producing a silica fine particle dispersion for polishing, comprising the following steps 1a to 3a: (Step 1a) introducing a seed particle dispersion and an alkali into a reaction vessel maintained in an unheated state to obtain a prepared liquid (Step 2a); following Step 1a, stirring the prepared liquid uniformly, then heating it to 40°C or higher but not exceeding 98°C and maintaining it at the same temperature range, followed by simultaneously carrying out the following treatments A and B, and then aging the reaction liquid at 40°C or higher but not exceeding 98°C for 20 minutes or longer but not longer than 120 minutes; Treatment A: preparing a reaction liquid by continuously or intermittently adding an acidic silicic acid solution and an alkali to the reaction vessel filled with the prepared liquid; Treatment B: continuously or intermittently withdrawing a portion of the reaction liquid from the reaction vessel; and (Step 3a) mixing the reaction liquid remaining in the reaction vessel at the end of Step 2a with the reaction liquid withdrawn in Treatment B of Step 2a to obtain a silica fine particle dispersion for polishing.
[0012] According to one aspect of the present invention, there is provided a method for producing a silica fine particle dispersion for polishing, comprising the following steps 1b to 4b: (Step 1b) A step of introducing an acidic silicic acid liquid and an alkali into an unheated reaction vessel to obtain a first preparation; (Step 2b) Following step 1b, a step of uniformly stirring the first preparation, subsequently heating it to 40°C or higher and 98°C or lower, and maintaining the temperature within the same range; and subsequently, continuously or intermittently adding an acidic silicic acid liquid while maintaining the temperature within the same range to obtain a second preparation; (Step 3b) Following step 2b, a step of simultaneously carrying out the following processes A and B: Process A: Continuously or intermittently adding an acidic silicic acid liquid and an alkali to the reaction vessel filled with the second preparation to prepare a reaction liquid; Process B: Continuously or intermittently withdrawing a portion of the reaction liquid from the reaction vessel of process A. (Step 4b) A step of aging the reaction solution obtained in the treatments A and B of step 3b at a temperature in the range of 40°C to 98°C for 20 minutes to 120 minutes, and then adding and mixing the reaction solution extracted in the treatment B of step 3b to obtain a dispersion of silica fine particles for polishing.
[0013] According to the present invention, it is possible to provide a dispersion of fine silica particles for polishing, which, when applied to polishing purposes, exhibits an excellent polishing rate and can suppress the occurrence of scratches on a substrate to be polished, and a method for producing the same.
[0014] [Silica microparticle dispersion for polishing] First, the silica microparticle dispersion for polishing according to this embodiment will be described. The silica microparticle dispersion for polishing according to this embodiment is prepared by dispersing a particle group containing silica microparticles as abrasive grains in a solvent. The particle group must also satisfy the following requirements 1 to 4. In this specification, the "silica microparticle dispersion for polishing" may be simply referred to as the "dispersion". The "particle group containing silica microparticles" dispersed in the silica microparticle dispersion for polishing may also be simply referred to as the "particle group".
[0015] Although the reasons why the silica microparticle dispersion for polishing according to this embodiment exhibits an excellent polishing rate, improves the surface roughness of the substrate being polished, and suppresses scratching when used in polishing applications are not entirely clear, the inventors speculate as follows. Specifically, the particle group according to this embodiment has a broad particle size distribution. Therefore, compared with conventional polishing abrasive grains, the polishing rate can be improved. Furthermore, the particle size distribution has a peak on the larger particle size side, i.e., there is no tailing on the larger particle size side, and therefore no extremely large particles are included. Furthermore, the particle shape is spherical, which improves surface roughness and suppresses scratching. Furthermore, the particle group according to this embodiment is primarily composed of spherical silica microparticles, but also contains trace amounts of irregularly shaped silica microparticles. These irregularly shaped silica microparticles improve the polishing rate, and because the amount of these irregularly shaped silica microparticles is so small, they have little adverse effect on surface roughness or scratches. The inventors speculate that the above-mentioned effects of the present invention are achieved in this manner. Furthermore, according to the first method for producing a silica microparticle dispersion for polishing of this embodiment, seed particles are added to an unheated reaction vessel during preparation, but no seed particles are added thereafter. This prevents the seed particles from agglomerating, and since seed particles are not added during preparation, the load on the production equipment and the process management burden are reduced, making it possible to efficiently produce a silica microparticle dispersion for polishing. The inventors believe that the effects of the present invention are achieved in this manner. Furthermore, according to the second method for producing a silica microparticle dispersion for polishing of this embodiment, an acidic silicic acid liquid is added to an unheated reaction vessel during preparation. This prevents the acidic silicic acid liquid from drying out, and since seed particles are not added during preparation in step 3b, the load on the production equipment and the process management burden are reduced, making it possible to efficiently produce a silica microparticle dispersion for polishing. The inventors believe that the effects of the present invention are achieved in this manner.
[0016] The requirements and characteristics of the silica fine particle dispersion for polishing according to this embodiment, that is, the particle size converted into specific surface area, the average sphericity, the cumulative particle size distribution converted into weight, the peak of the particle size distribution, the irregular particle rate, and the coefficient of variation of the particle size distribution area, will be explained below.Unless otherwise specified, the explanation of the effect or performance due to each requirement or characteristic means the effect or performance when the silica fine particle dispersion for polishing according to this embodiment is applied to polishing purposes.
[0017] (Specific surface area-equivalent particle diameter) The specific surface area-equivalent particle diameter of the particle group according to this embodiment must be in the range of 5 nm to 200 nm. When the specific surface area-equivalent particle diameter is within this range, when the silica microparticle polishing dispersion according to this embodiment is used as silica microparticles for polishing silicon wafers, magnetic disks, or semiconductor substrates, a high polishing rate can be obtained, and further scratching on the object to be polished can be suppressed, resulting in a smoother surface of the object to be polished. If the particle diameter is less than 5 nm, it becomes more difficult to achieve a polishing rate that is practically sufficient. If the particle diameter exceeds 200 nm, scratches tend to occur more easily on the substrate to be polished. The specific surface area-equivalent particle diameter of the particle group is preferably in the range of 10 nm to 150 nm, and more preferably in the range of 20 nm to 100 nm.
[0018] (Average Sphericity) The average sphericity of the particle group according to this embodiment must be in the range of 0.85 to 1.00 (Requirement 1). The particle group includes spherical particles. In this embodiment, spherical particles refer to particles having an average sphericity in the range of 0.85 to 1.00. The average sphericity can be calculated by calculating the minor axis / major axis of each silica microparticle from the results of observation of an electron microscope photograph, as described below, and then calculating the simple average. When the average sphericity of the particle group is 0.85 or more, when the silica microparticle dispersion for polishing according to this embodiment, in which such particles are dispersed in a solvent, is used for polishing purposes, the surface roughness of the polished substrate can be smoothed and the occurrence of scratches can be suppressed. Note that even if the particle group contains irregularly shaped particles in the range of 0.01% by number to 10.0% by number, scratches can also be suppressed as long as the average sphericity of the particle group is within the above range. Note that the effects of irregularly shaped particles (irregularly shaped silica particles) contained in the particle group are described below. The average sphericity of the particle group is preferably in the range of 0.90 to 1.00, and more preferably in the range of 0.92 to 1.00. A specific method for measuring the average sphericity of the particle group according to this embodiment is described below.
[0019] (Weight-converted cumulative particle size distribution) In the weight-converted cumulative particle size distribution of the particle group according to this embodiment, the cumulative 10% particle size (D 10 ), cumulative 90% particle diameter (D 90 ) and cumulative 50% particle diameter (D 50 ) must satisfy the following formula (F1) (Requirement 2). 90 -D 10 ) / D 50 ≦3.0 (F1) (D 90 -D 10 ) / D 50 The value of indicates the width of the particle size distribution, and (D 90 -D 10 ) / D 50 The larger the value of (D 90 -D 10 ) / D 50A large value of indicates that the dispersion contains both small and large particles. Here, large particles exhibit a high polishing rate, while small particles exhibit a scratch repair effect. Therefore, it can be said that a silica microparticle dispersion having such a particle size distribution can achieve both a high polishing rate and the suppression of scratch occurrence. (D 90 -D 10 ) / D 50 If the value of is in the range of 0.5 or more and 3.0 or less, it can be said that the particle size distribution is sufficiently broad and that the polishing rate is high and that the polishing rate is appropriate for the amount of small particles and large particles. Generally, the larger the particle size, the higher the polishing rate. However, as the size increases, the problem of scratches on the substrate tends to occur. However, if the particle size distribution satisfies the above range, the content of large particles and small particles is well balanced, and scratches caused by large particles can be repaired by the small particles, which is preferable. ((D 90 -D 10 ) / D 50 The value of (a) is preferably in the range of 0.6 or more and 2.0 or less, and more preferably in the range of 0.8 or more and 1.8 or less.
[0020] (Peak of particle size distribution) In the weight-equivalent particle size distribution of the particle group according to this embodiment, it is necessary to have a distribution peak on the large particle size side (requirement 3). Here, having a distribution peak on the large particle size side means that the D 50This means that the particle size distribution has a peak on the larger particle size side than the cumulative 50% particle size (particle size accumulated from the smallest particle size). When the particle size distribution has a peak on the larger particle size side, the particle size distribution does not tail on the larger particle size side. On the other hand, a distribution that tails on the larger particle size side contains extremely large particles. Generally, the larger the particle size, the faster the polishing rate, but scratches tend to occur more easily and the surface roughness tends to deteriorate. However, extremely large particles tend to cause irreparable scratches. Therefore, particles that have a peak on the larger particle size side but do not tail on the larger particle size side tend to suppress fatal scratches. Furthermore, by combining the above requirement 2 and requirement 3, scratches caused by the peak on the larger particle size side are repaired by small particles that have a slow polishing rate but have the function of smoothing the surface, so that both the polishing rate and surface roughness can be improved. Note that the particle diameter (D) of the weight-equivalent particle size distribution, which is the criterion for having a distribution peak on the larger particle size side, is 50 ) is preferably D 60 is recommended.
[0021] (Ratio of irregularly shaped particles) The particle group according to this embodiment must contain 0.01% by number or more and 10.0% by number or less of irregularly shaped particles that are not spherical (Requirement 4). Non-spherical irregularly shaped particles are particles with a minor axis / major axis ratio of less than 0.85, which can be calculated from the results of observation of electron microscope photographs described below. Such irregularly shaped particles generally exhibit high polishing rates but are prone to causing scratches on the substrate surface. However, if the ratio of irregularly shaped particles (number of irregularly shaped particles / total number of particles x 100) is in the range of 0.01% by number or more and 10.0% by number or less, when the particle group according to this embodiment is used as abrasive grains for polishing, the irregularly shaped particles contained in this range of number percent contribute to a high polishing rate, while the remaining spherical particles suppress the generation of scratches on the substrate surface and can even repair any scratches that occur, thereby achieving both a high polishing rate and smoothness of the polished substrate surface after polishing. If the irregular-shaped particle ratio of the particle group is less than 0.01% by number, the irregular-shaped particles will not have the effect of improving the polishing rate. If the irregular-shaped particle ratio of the particle group exceeds 10.0% by number, the tendency for scratches to increase due to the irregular-shaped particles will become stronger. The irregular-shaped particle ratio is preferably in the range of 0.05% by number to 10.0% by number, more preferably in the range of 0.10% by number to 10.0% by number, and particularly preferably in the range of 1.0% by number to 10.0% by number. In this embodiment, the irregular-shaped particles refer to irregular-shaped silica particles. The irregular-shaped particle ratio may also be in the range of 0.01% by number to 8.0% by number, or in the range of 0.01% by number to 5.0% by number.
[0022] The irregular-shaped particle ratio can be measured as follows. That is, the silica microparticle dispersion is observed in a photograph or image taken with an electron microscope at a magnification of 200,000 times. Specifically, an image is taken so that 200 or more particles are included in the same field of view, and the minor axis / major axis ratio of each of the 200 or more silica microparticles in the obtained photograph or image is measured. The number (n) of particles (irregular-shaped particles) with a minor axis / major axis ratio of less than 0.85 is determined, and the irregular-shaped particle ratio is calculated using the following formula: Irregular-shaped particle ratio = (n / 200) x 100 [number %]. The irregular-shaped particle ratio in the particle group according to this embodiment is preferably in the range of 1.3 to 9.0% by number, more preferably 1.8 to 8.0% by number, and particularly preferably 2.0 to 7.0% by number.
[0023] (Coefficient of variation of particle size distribution area) In this embodiment, it is preferable that the particle group further satisfies the following requirement 5): 5) In the particle size distribution of the particle group, which is composed of particle size / number of particles, the cumulative 1% particle size (D 1 ) to obtain the cumulative 99% particle diameter (D 99) is divided into six equal particle size ranges, S1, S2, S3, S4, S5, and S6, and the coefficient of variation (CV value) of the particle size distribution area corresponding to each particle size range is 20.0% or more and 70.0% or less. Since the particle size distribution of ordinary silica sol exhibits a normal distribution, the CV value is high, exceeding 70.0%. In contrast, when the CV value is in the range of 20.0% or more and 70.0% or less, the areas S1 to S6 are relatively uniform, and the shape of the particle size distribution is roughly trapezoidal or rectangular, while having a peak on the larger particle size side. Such a particle size distribution contains a relatively uniform mixture of large particles with a high polishing rate, small particles that suppress scratches, and medium particles that provide a good balance between polishing rate and scratch suppression. Therefore, it is possible to achieve both a high polishing rate and scratch suppression. When the CV value is less than 20.0%, it is virtually difficult to obtain such a particle size distribution. On the other hand, if the CV value exceeds 70.0%, the polishing rate tends to decrease because the distribution approaches a normal distribution. The CV value is more preferably in the range of 22.0% to 65.0%, and particularly preferably in the range of 25.0% to 62.0%.
[0024] (Silica / Polyethyleneimine [Mass Ratio] at Equivalence Point) In this embodiment, it is preferable that the silica fine particle dispersion for polishing further satisfies the following requirement 6): 6) In streaming potential measurement (using cationic polymeric polyethyleneimine [weight average molecular weight 600] as a titration reagent), the mass ratio of polyethyleneimine to silica at the equivalence point is in the range of 1.0 to 1.9.
[0025] The silica fine particle dispersion according to this embodiment is prepared by adjusting the amount (V [g]) of the cationic solid content [cationic polymer polyethyleneimine (weight average molecular weight 600)] added in the cationic titration solution in the criterion and the amount (V [g]) of SiO 2 Ratio of solid content [g] (V / SiO 2 ) is preferably in the range of 1.0 or more and 1.9 or less. 2When the V / SiO ratio is in the range of 1.0 or more and 1.9 or less, a good polishing rate can be obtained when such a silica fine particle dispersion is used for polishing. 2 If the V / SiO ratio is less than 1.0, when a cationic additive is mixed into the polishing solution and the solution is subjected to polishing, the polishing rate may decrease due to a decrease in the dispersion stability of the silica fine particles, which is undesirable. 2 However, if the V / SiO ratio exceeds 1.9, when a cationic additive is mixed into the polishing solution and the solution is subjected to polishing, the cationic additive adsorbed in excess to the silica fine particles may inhibit polishing, resulting in a decrease in the polishing rate, which is undesirable. 2 More preferably, V / SiO is in the range of 1.3 or more and 1.8 or less. 2 is determined by cation titration.
[0026] (Silica microparticles) It can be confirmed that the silica microparticles according to this embodiment are made of silica, for example, by an ICP (inductively coupled plasma) optical emission spectrometer. 1 g of an aqueous dispersion containing silica microparticles according to this embodiment is collected in a 30 mL zirconia bowl with a lid, dried (200° C., 20 minutes), and then added with Na 2 O 2 2 g of the sample was added to 1 g of NaOH and dissolved for 15 minutes. 10 mL of 98% by mass sulfuric acid and 10 mL of pure water were added and dissolved, and then the solution was diluted to 500 mL with pure water to prepare a sample. The silicon content of the obtained sample was measured using an ICP device (Shimadzu Corporation, ICPS-8100, analysis software ICPS-8000).
[0027] The particle group according to this embodiment is made of silica, but may contain 10% by mass or less of components other than silica. Examples of components other than silica include Al, Ti, Fe, Ca, Mg, Cr, Ni, Cu, Zn, K, or Na, or oxides thereof. As described above, it can be confirmed, for example, by using an ICP device, that the particle group of the present invention is made of silica. In addition, the content of components other than silica that may be contained in the particle group of the present invention can be identified and quantified, for example, by using an inductively coupled plasma optical emission spectrometer. Note that Ni, Cu, K, and Na can be identified and quantified using an atomic absorption spectrophotometer.
[0028] (Solvent) As described above, the dispersion according to this embodiment is a dispersion of the particle group according to this embodiment in a solvent. Examples of the solvent include water, alcohols such as methyl alcohol, ethyl alcohol, and isopropyl alcohol, and water-soluble organic solvents such as ethers, esters, and ketones. Alternatively, the solvent may be a mixed solvent of water and an organic solvent.
[0029] The content of the particle group contained in the dispersion liquid according to the present embodiment is preferably in the range of 1% by mass to 50% by mass, more preferably in the range of 10% by mass to 50% by mass. Here, the content of the particle group is determined by subjecting the silica fine particle dispersion liquid to ignition loss at 1000°C, weighing the obtained solid content, and calculating the alkali content in terms of oxide (Na 2 The concentration obtained by subtracting the amount of the particles (e.g., O) was determined as the content of the particle group according to this embodiment.
[0030] [Polishing Composition] Next, the polishing composition according to this embodiment will be described. The polishing composition according to this embodiment contains the polishing silica microparticle dispersion according to this embodiment or the particle group according to this embodiment and a solvent, and further contains components that impart necessary performance, including polishing performance. Examples of the components that impart necessary performance include polishing accelerators, surfactants, hydrophilic compounds, heterocyclic compounds, pH adjusters, and pH buffers. The polishing composition may contain only one of these components as the components that impart necessary performance, or may contain two or more of them. The polishing composition according to this embodiment is also called a "polishing slurry."
[0031] The silica fine particle dispersion for polishing or the polishing composition according to this embodiment can be used as a CMP slurry, for example, for polishing semiconductor wafers such as silicon wafers, or for polishing substrates for hard disk drives, liquid crystal glass, sapphire substrates, compound semiconductors, GaN substrates, SiC substrates, etc.
[0032] Examples of polishing accelerators include acids such as sulfuric acid, nitric acid, phosphoric acid, oxalic acid, and hydrofluoric acid, as well as the sodium salts, potassium salts, and ammonium salts of these acids, and mixtures thereof.When the composition of the present invention contains these polishing accelerators, when polishing a polished material consisting of multiple components, the polishing rate of a specific component of the polished material can be accelerated, thereby ultimately obtaining a flat polished surface.When the polishing composition of this embodiment contains a polishing accelerator, its content is preferably in the range of 0.1% by mass to 10% by mass, more preferably in the range of 0.5% by mass to 5% by mass.
[0033] At least one of the surfactants and hydrophilic compounds may be added, such as cationic, anionic, nonionic, or amphoteric surfactants or hydrophilic compounds, to improve the dispersibility and stability of the polishing composition.
[0034] Both the surfactant and the hydrophilic compound have the effect of reducing the contact angle with the polished surface and promoting uniform polishing. At least one of the surfactant and the hydrophilic compound can be selected from the following group, for example:
[0035] Anionic surfactants include carboxylates, sulfonates, sulfates, and phosphates. Carboxylate salts include soaps, N-acylamino acid salts, polyoxyethylene or polyoxypropylene alkyl ether carboxylates, and acylated peptides. Sulfonates include alkyl sulfonates, alkylbenzene and alkylnaphthalene sulfonates, naphthalene sulfonates, sulfosuccinates, α-olefin sulfonates, and N-acylsulfonates. Sulfate salts include sulfated oils, alkyl sulfates, alkyl ether sulfates, polyoxyethylene or polyoxypropylene alkyl allyl ether sulfates, and alkylamide sulfates. Phosphate salts include alkyl phosphates, polyoxyethylene or polyoxypropylene alkyl allyl ether phosphates, and the like.
[0036] Examples of cationic surfactants include aliphatic amine salts, aliphatic quaternary ammonium salts, benzalkonium chloride salts, benzethonium chloride, pyridinium salts, and imidazolinium salts. Examples of amphoteric surfactants include carboxybetaine type, sulfobetaine type, aminocarboxylate salts, imidazolinium betaine, lecithin, and alkylamine oxide.
[0037] Examples of nonionic surfactants include ether type, ether ester type, ester type, and nitrogen-containing type. Ether type surfactants include polyoxyethylene alkyl and alkylphenyl ethers, alkylarylformaldehyde condensed polyoxyethylene ethers, polyoxyethylene polyoxypropylene block polymers, and polyoxyethylene polyoxypropylene alkyl ethers. Ether ester type surfactants include polyoxyethylene ethers of glycerin esters, polyoxyethylene ethers of sorbitan esters, and polyoxyethylene ethers of sorbitol esters. ester type surfactants include polyethylene glycol fatty acid esters, glycerin esters, polyglycerin esters, sorbitan esters, propylene glycol esters, and sucrose esters. Nitrogen-containing surfactants include fatty acid alkanolamides, polyoxyethylene fatty acid amides, and polyoxyethylene alkylamides. Other examples include fluorine-based surfactants.
[0038] The surfactant is preferably an anionic surfactant or a nonionic surfactant, and the salt includes ammonium salt, potassium salt, and sodium salt, with ammonium salt and potassium salt being particularly preferred.
[0039] Further, other surfactants, hydrophilic compounds, etc. include esters (glycerin esters, sorbitan esters, alanine ethyl esters, etc.), ethers (polyethylene glycol, polypropylene glycol, polytetramethylene glycol, polyethylene glycol alkyl ethers, polyethylene glycol alkenyl ethers, alkyl polyethylene glycols, alkyl polyethylene glycol alkyl ethers, alkyl polyethylene glycol alkenyl ethers, alkenyl polyethylene glycols, alkenyl polyethylene glycol alkyl ethers, alkenyl polyethylene glycol alkenyl ethers, polypropylene glycol alkyl ethers, polypropylene glycol alkenyl ethers, alkyl polypropylene glycols, alkyl polypropylene glycol alkyl ethers, alkyl polypropylene glycol alkenyl ethers, and alkenyl polypropylene glycols, etc.), polysaccharides (alginic acid, pectinic acid, carboxymethylcellulose, curdlan, pullulan, etc.), amino acid salts (glycine ammonium salt and glycerin ammonium salt), sodium salt, etc.), polycarboxylic acids and their salts (polyaspartic acid, polyglutamic acid, polylysine, polymalic acid, polymethacrylic acid, ammonium polymethacrylate salt, sodium polymethacrylate salt, polyamic acid, polymaleic acid, polyitaconic acid, polyfumaric acid, poly(p-styrenecarboxylic acid), polyacrylic acid, polyacrylamide, aminopolyacrylamide, ammonium polyacrylate salt, sodium polyacrylate salt, polyamic acid, ammonium polyamic acid salt, sodium polyamic acid salt, polyglyoxylic acid, etc.), vinyl polymers (polyvinyl alcohol, polyvinylpyrrolidone, polyacrolein, etc.), sulfonic acids and their salts (ammonium methyl taurate salt, sodium methyl taurate salt, sodium methyl sulfate salt, ethylammonium sulfate salt, butylammonium sulfate salt, sodium vinyl sulfonate salt, sodium 1-allylsulfonate salt, sodium 2-allylsulfonate salt, sodium methoxymethylsulfonate salt, ammonium ethoxymethylsulfonate salt, sodium 3-ethoxypropylsulfonate, etc.),and amides such as propionamide, acrylamide, methylurea, nicotinamide, succinamide, and sulfanilamide.
[0040] When the substrate to be polished is a glass substrate or the like, any surfactant can be suitably used. However, when the substrate is a silicon substrate for a semiconductor integrated circuit or the like, and the influence of contamination by alkali metals, alkaline earth metals, halides, or the like must be avoided, it is desirable to use an acid or ammonium salt surfactant.
[0041] When the polishing composition of this embodiment contains at least one of a surfactant and a hydrophilic compound, the total content thereof is preferably 0.001 g or more and 10 g or less, more preferably 0.01 g or more and 5 g or less, and particularly preferably 0.1 g or more and 3 g or less, per liter of the polishing composition of this embodiment.
[0042] The surfactant or hydrophilic compound may be used alone or in combination of two or more kinds.
[0043] When the polishing composition according to this embodiment contains a metal, a heterocyclic compound may be added to the substrate to be polished. This heterocyclic compound forms a passivation layer or a dissolution-inhibiting layer on the metal, thereby inhibiting erosion of the substrate. Here, a "heterocyclic compound" refers to a compound having a heterocycle containing one or more heteroatoms. A heteroatom refers to an atom other than a carbon atom or a hydrogen atom. A heterocycle refers to a cyclic compound containing at least one heteroatom. A heteroatom refers only to atoms that form part of the ring system of a heterocycle, and does not refer to atoms that are external to the ring system, separated from the ring system by at least one non-conjugated single bond, or that are part of a further substituent of the ring system. Preferred heteroatoms include, but are not limited to, nitrogen, sulfur, oxygen, selenium, tellurium, phosphorus, silicon, and boron. Examples of heterocyclic compounds that can be used include imidazole, benzotriazole, benzothiazole, and tetrazole. More specific examples include 1,2,3,4-tetrazole, 5-amino-1,2,3,4-tetrazole, 5-methyl-1,2,3,4-tetrazole, 1,2,3-triazole, 4-amino-1,2,3-triazole, 4,5-diamino-1,2,3-triazole, 1,2,4-triazole, 3-amino-1,2,4-triazole, and 3,5-diamino-1,2,4-triazole, but are not limited to these.
[0044] When the polishing composition of this embodiment contains a heterocyclic compound, the content thereof is preferably in the range of 0.001 mass % or more and 1.0 mass % or less, more preferably in the range of 0.001 mass % or more and 0.7 mass % or less, and even more preferably in the range of 0.002 mass % or more and 0.4 mass % or less.
[0045] In order to enhance the effects of the above-mentioned additives, the pH of the polishing composition can be adjusted by adding an acid or a base as needed.
[0046] When the polishing composition according to this embodiment is adjusted to a pH of 7 or higher, an alkaline pH adjuster is used. Preferably, sodium hydroxide, aqueous ammonia, ammonium carbonate, or an amine such as ethylamine, methylamine, triethylamine, or tetramethylamine is used.
[0047] When the polishing composition according to this embodiment is adjusted to a pH of less than 7, an acidic pH adjuster is used. For example, hydroxy acids such as lactic acid, citric acid, malic acid, tartaric acid, and glyceric acid are used.
[0048] To maintain a constant pH value of the polishing composition according to this embodiment, a pH buffer may be used, such as phosphates and borates, such as ammonium dihydrogen phosphate, diammonium hydrogen phosphate, and ammonium tetraborate tetrahydrate, or organic acids.
[0049] The concentration of abrasive particles in the polishing composition of this embodiment is preferably in the range of 0.5% by mass or more and 50% by mass or less, more preferably in the range of 5% by mass or more and 30% by mass or less.If the concentration is less than 0.5% by mass, depending on the type of substrate or insulating film, the concentration is too low, and the polishing speed is slow, which may cause productivity problems.If the concentration of abrasive particles exceeds 50% by mass, the stability of the abrasive becomes insufficient, and the polishing speed and polishing efficiency do not further improve.In addition, in the process of supplying the dispersion liquid for polishing treatment, dried matter may be produced and adhere, which may cause scratches.
[0050] [First method for producing silica fine particle dispersion for polishing] Next, a first method for producing a silica fine particle dispersion for polishing according to this embodiment will be described. The silica fine particle dispersion for polishing according to this embodiment described above can be suitably produced, for example, by the first method for producing a silica fine particle dispersion for polishing according to this embodiment. The first method for producing a dispersion according to this embodiment includes the following steps 1a to 3a.
[0051] (Step 1a) In step 1a, a seed particle dispersion and an alkali are introduced as raw materials into a reaction vessel maintained in an unheated state, and a solvent is added as necessary to prepare a blended liquid. When these raw materials are introduced into the reaction vessel, splashing occurs on the bottom or inner wall of the reaction vessel or on the liquid surface (the liquid surface of the introduced seed particle dispersion and alkali). If the raw materials are introduced into a heated reaction vessel, these splashed raw materials are likely to dry out, causing problems such as the formation of coarse aggregates. If the raw materials are introduced gradually to prevent splashing, the blending time becomes longer and economical efficiency is reduced. Furthermore, if the seed particle dispersion and alkali are added to a heated reaction vessel, the seed particle dispersion and alkali are heated from the beginning of the addition, which can lead to the problem of seed particle aggregation occurring at an early stage. The unheated state means that no operation to raise the temperature of the reaction vessel is performed. Note that if the temperature of the reaction vessel exceeds 40°C in an unheated state due to seasonal high temperatures, etc., it is recommended to cool the reaction vessel to a temperature below 40°C. The temperatures of the seed particle dispersion and the alkali at the stage of introducing them into the reaction vessel are preferably both less than 40°C. As the seed particle dispersion, a silica fine particle dispersion is used as described below. The amounts of the seed particle dispersion and the alkali are added so that the molar ratio of silica to alkali (in terms of oxide) in the prepared solution is in the range of 20 to 160, and further adjusted by adding a solvent as necessary so that the silica concentration in the prepared solution is in the range of 1 mass % to 15 mass %. Here, the molar ratio of silica to alkali (in terms of oxide) is calculated by the following formula: molar ratio = [SiO 2 moles of] / [A 2The molar ratio of silica to alkali (oxide equivalent) is expressed as [number of moles of O] (where A represents an alkali metal, ammonia, an organic alkali, or aqueous glass, etc.). If the molar ratio of silica to alkali (oxide equivalent) is less than 20, the amount of alkali is excessive, resulting in an excessively high ionic strength in the preparation, causing the silica fine particles to aggregate, making it difficult to obtain spherical particles or causing sedimentation. Even if sedimentation does not occur, the number of aggregates of silica fine particles increases, making it difficult to obtain a monodispersed silica sol. On the other hand, if the molar ratio of silica to alkali (oxide equivalent) exceeds 160, the alkali concentration in the preparation becomes low, and when an acidic silicic acid solution is added in the subsequent step 2a, the pH of the reaction solution becomes significantly low. As a result, the added acidic silicic acid solution does not deposit on the surface of the seed particles, and self-nucleation by silicic acid occurs, which ultimately tends to make it difficult to obtain a silica sol with the desired particle size. The molar ratio of silica to alkali (oxide equivalent) is preferably in the range of 40 to 140, more preferably in the range of 50 to 130, and particularly preferably in the range of 60 to 120. When the silica concentration in the preparation is less than 1 mass%, monodispersed silica microparticles are easily obtained, but the low silica concentration in the preparation makes production inefficient and uneconomical. Furthermore, when the silica concentration exceeds 15 mass%, the silica microparticles tend to aggregate during preparation, making it difficult to obtain monodispersed silica microparticles. The silica concentration in the preparation is more preferably in the range of 2 to 10 mass%, and particularly preferably in the range of 3 to 8 mass%. When the molar ratio of silica to alkali (oxide equivalent) and the silica concentration in the preparation are within the aforementioned ranges, most of the seed particles avoid aggregation, but some of them aggregate to form irregularly shaped particles. As a result, the silica fine particles contained in the silica fine particle dispersion according to this embodiment are mostly spherical particles, but contain 1.0% to 10% by number of irregularly shaped particles.
[0052] (Seed Particle Dispersion) A silica microparticle dispersion can be used as the seed particle dispersion used in step 1a. In this case, the seed particles are silica microparticles. The size of the seed particles (specific surface area-equivalent particle diameter) is not particularly limited, as it can be selected arbitrarily depending on the size of the silica microparticle dispersion to be finally prepared. Typically, a size smaller than the size of the silica microparticles to be finally prepared is selected. Note that, when the silica microparticle dispersion to be finally prepared is used for polishing purposes, the specific surface area-equivalent particle diameter of the seed particles is preferably selected in the range of 5 nm to 200 nm. Furthermore, the silica concentration of the seed particle dispersion is preferably in the range of 1 mass % to 50 mass %, more preferably in the range of 3 mass % to 50 mass %. A silica concentration of less than 1 mass % is undesirable because it reduces the production efficiency in steps 1a to 3a. A silica concentration of more than 50 mass % is undesirable because it reduces the stability of the silica microparticles, making it more likely to produce agglomerated particles, for example.
[0053] (Alkali) Examples of the alkali added in step 1a include alkali silicates such as sodium silicate (water glass) and potassium silicate, alkali metals such as sodium hydroxide, potassium hydroxide, and lithium hydroxide, ammonia, and organic alkalis such as organic amines. Here, the alkali is usually added as an aqueous alkali solution. The alkali concentration of the aqueous alkali solution is not particularly limited, but is usually used in the range of 1% by mass to 50% by mass.
[0054] (Solvent) Examples of the solvent added as needed in step 1a include water, ion-exchanged water, pure water, ultrapure water, a mixed solvent containing water and a water-soluble organic solvent, and a water-soluble organic solvent.
[0055] (Step 2a) In step 2a, the preparation liquid prepared in step 1a is stirred uniformly, heated, and maintained at a temperature (40°C to 98°C) for a certain period of time, followed by the simultaneous implementation of the following treatments A and B. Treatment A: A reaction liquid is prepared by continuously or intermittently adding an acidic silicic acid solution and an alkali to the reaction vessel filled with the preparation liquid. Treatment B: A portion of the reaction liquid is continuously or intermittently withdrawn from the reaction vessel.
[0056] (Retention Temperature and Retention Time) In step 2a, the preparation obtained in step 1a is heated to a temperature of 40°C to 98°C while stirring and maintained at this temperature range for a certain period of time. The retention time is preferably in the range of 20 minutes to 120 minutes, more preferably 30 minutes to 90 minutes. This temperature retention activates the surfaces of the seed particles, making them suitable for particle growth in subsequent treatments. This temperature retention also allows the preparation to be sufficiently homogenized. A retention time of less than 20 minutes results in insufficient surface activation, which can lead to uneven particle growth upon subsequent addition of an acidic silicic acid solution and may result in self-nucleation by silicic acid. Furthermore, a retention time of more than 120 minutes does not further promote surface activation of the seed particles, and the longer retention time reduces production efficiency and reduces economic viability. As mentioned above, the retention temperature is preferably in the range of 40°C to 98°C, and it is desirable to maintain it constant within this temperature range.
[0057] Subsequently, a process A is carried out in which the seed particles are grown to a desired size by adding an acidic silicic acid solution (here, the addition of alkali and the addition of the acidic silicic acid solution for particle growth are carried out simultaneously in order to maintain the pH of the reaction solution), and a process B is carried out in which a portion of the reaction solution is withdrawn from the reaction vessel. Note that the "prepared solution" is referred to as the "reaction solution" after the start of the addition of the acidic silicic acid solution, because the particle growth reaction of the seed particles progresses with the addition of the acidic silicic acid solution. The reaction solution withdrawn in the process B can be mixed with the reaction solution remaining in the reaction vessel in step 3a to obtain a silica microparticle dispersion having a broader particle size distribution (a wider particle size distribution range).
[0058] (Acidic silicic acid solution) The acidic silicic acid solution can be obtained by dealkalizing an aqueous solution of alkali silicate with a cation exchange resin. The concentration of the acidic silicic acid solution is 2 The pH of the acidic silicic acid solution is preferably in the range of 0.1% by mass to 10% by mass, more preferably in the range of 1% by mass to 7% by mass. The amount (total amount) of the acidic silicic acid solution added to the prepared liquid or reaction liquid in step 2a is determined based on the SiO content of the acidic silicic acid solution. 2 When the amount (number of moles) of SiO2 contained in the prepared solution is represented by Ma and the number of moles of SiO2 contained in the prepared solution is represented by Ms, the value of Ma / Ms is preferably in the range of 1 to 20. The value of Ma / Ms is more preferably in the range of 2 to 15. If the value of Ma / Ms is less than 1, the growth of silica microparticles in the silica microparticle dispersion obtained by the production method of this embodiment will be slow, and further, the distribution will not be very broad, resulting in an insufficient polishing rate when used as an abrasive. On the other hand, if the value of Ma / Ms exceeds 20, the particle size of the silica microparticles in the silica microparticle dispersion obtained by the production method of this embodiment will be too large, and when used as an abrasive, the occurrence of scratches on the substrate to be polished will be significant, which is undesirable. Furthermore, in such cases, the preparation time will be very long, resulting in poor economic efficiency.
[0059] (Reaction Temperature) The temperature of the preparation or reaction liquid when the acidic silicic acid liquid is added to the preparation or reaction liquid is preferably in the range of 40°C or higher and 98°C or lower. If the temperature of the preparation or reaction liquid is lower than 40°C, the added acidic silicic acid liquid is less likely to dissolve and therefore less likely to deposit on the surface of the seed particles. This results in self-nucleation by silicic acid, making it impossible to obtain the desired size. If the temperature of the preparation or reaction liquid exceeds 98°C, the added acidic silicic acid liquid dissolves sufficiently and the seed particles grow, but the excessively high temperature of the preparation or reaction liquid poses problems in terms of energy efficiency and safety. It is more preferable that the temperature of the preparation or reaction liquid when the acidic silicic acid liquid is added to the preparation or reaction liquid be in the range of 50°C or higher and 98°C or lower.
[0060] (Addition Rate of Acidic Silica Solution) In this embodiment, in treatment A of step 2a, the addition rate of the acidic silicic acid solution when it is added to the reaction vessel filled with the prepared liquid is expressed as dry g [g] of silica in the acidic silicic acid solution added per minute per mass [g] of silica particles contained in the solution in the reaction vessel. Here, [g / min·g] is used as the unit of the addition rate of the acidic silicic acid solution to the liquid. Note that the term "solution" is a convenient general term for the liquid filled in the reaction vessel. Before the start of treatment A, the reaction vessel is filled only with the prepared liquid, and as the addition of the acidic silicic acid solution begins, the particle growth reaction progresses and the reaction liquid is formed. The solution encompasses the prepared liquid and the reaction liquid, and refers to the liquid present in the reaction vessel. The addition rate of the acidic silicic acid solution to the liquid is preferably in the range of 0.0001 g / min·g to 0.05 g / min·g. Within the above range, the acidic silicic acid solution added for particle growth dissolves in the alkali in the preparation liquid and deposits on the seed particle surfaces, thereby promoting particle growth of the seed particles. If the addition rate of the acidic silicic acid solution to the liquid is less than 0.0001 g / min·g, the preparation time becomes too long for practical use, reducing practicality and economic efficiency. If the addition rate of the acidic silicic acid solution to the liquid exceeds 0.05 g / min·g, self-nucleation may proceed without the silicic acid being deposited on the particle surfaces, which is undesirable. The addition rate of the acidic silicic acid solution to the liquid is more preferably in the range of 0.0005 g / min·g to 0.02 g / min·g, and particularly preferably in the range of 0.002 g / min·g to 0.01 g / min·g. In this embodiment, the addition rate of the acidic silicic acid solution to the liquid can be calculated using the following formula, where S is the addition rate of the acidic silicic acid solution (in terms of dry silica) per unit mass of dry silica contained in the solution in the reaction vessel: (S) = (addition rate of acidic silicic acid solution per dry silica) [g / min] ÷ (mass of dry silica in the solution in the reaction vessel) [g] Here, for example, when the addition rate of the acidic silicic acid solution per dry silica mass changes in two stages, the dry silica mass of the particles in the reaction vessel is calculated using the dry silica mass in the reaction vessel at the end of the first and second stages of addition, respectively. When the addition rate does not change, it is calculated using the dry silica mass in the reaction vessel at the end of treatment A in step 2a.In addition, in this specification, the addition rate of the acidic silicic acid liquid is calculated as described above in terms of the amount of acidic silicic acid liquid added (in terms of dry silica) per unit mass (unit area of seed particles) per unit time, whether the addition of the acidic silicic acid liquid is continuous or intermittent.
[0061] The addition rate [g / min] of the acidic silicic acid solution is changed one or more times, and the addition rate at the nth time is set to L n When [g / min] is used, L n+1 <L n It is preferable to satisfy the relationship: where n is a positive integer. That is, it is desirable to change the addition rate of the acidic silicic acid liquid during preparation one or more times and gradually decrease the addition rate. In step 2a, in order to grow particles to the desired size, acidic silicic acid liquid is added to grow the particles, but in the present invention, the reaction liquid is continuously withdrawn, so the number of particles decreases. Therefore, the acidic silicic acid liquid may not deposit on the particle surface, and self-nucleation by silicic acid may occur. By decreasing the addition rate of the acidic silicic acid liquid from the second stage onwards, the occurrence of self-nucleation can be prevented and particles can be grown to the desired size.
[0062] (Alkali Addition Rate) In treatment A of step 2a, it is desirable to add an alkali continuously or intermittently to the prepared solution simultaneously with the addition of the acidic silicic acid solution in order to maintain the pH of the reaction solution. The alkali addition rate depends on the type and concentration of the alkali and cannot be uniformly limited, but it is desirable to add the alkali so that the pH of the reaction solution is in the range of 8.5 to 13.0.
[0063] (SiO of the solution in the reaction vessel 2 / A 2 In step 2a, an acidic silicic acid solution is added continuously or intermittently to the solution in the reaction vessel, but the reaction solution (hereinafter also referred to as "extracted solution") is continuously or intermittently extracted, so the pH of the reaction solution tends to decrease. When the pH decreases, the added acidic silicic acid solution becomes difficult to dissolve, and self-nucleation by silicic acid tends to occur easily. Therefore, in order to maintain the pH of the solution in the reaction vessel, it is desirable to add an alkali to adjust the pH. At this time, the SiO of the solution in the reaction vessel 2 / A 2 By adding an alkali so that the O molar ratio falls within the range of 20 to 160, the pH can be adjusted to a desired value.
[0064] (pH of the solution in the reaction vessel) As described above, the SiO 2 / A 2 The type of alkali to be added to adjust the O molar ratio to 20 or more and 160 or less is not particularly limited, but examples thereof include sodium hydroxide, potassium hydroxide, lithium hydroxide, ammonia, and organic amines. The pH of the reaction solution adjusted by adding an alkali is preferably in the range of 8.5 or more and 13.0 or less, more preferably in the range of 9.0 or more and 12.5 or less. If the pH exceeds 13.0, the ionic strength in the reaction solution becomes too high, causing the silica fine particles to aggregate and settle, or the particles to become irregular in shape, making it difficult to obtain the desired particles. If the pH is less than 8.5, the added acidic silicic acid solution becomes difficult to dissolve, so self-nucleation by silicic acid tends to occur.
[0065] (Process B) In process B of step 2a, an acidic silicic acid solution is continuously or intermittently added to the solution in the reaction vessel while continuously withdrawing the withdrawn liquid. In the early stage of withdrawal, the particle growth reaction has started but the seed particles have not yet grown sufficiently, so small silica microparticles are withdrawn. However, in the later stage of withdrawal, the seed particles have grown sufficiently, so large silica microparticles are withdrawn. By continuously withdrawing the withdrawn liquid in this manner, silica microparticles with a wide particle size distribution are obtained from the withdrawn liquid. It is also desirable to mix the reaction liquid remaining in the reaction vessel with the withdrawn liquid. In step 2a, withdrawal is carried out continuously, but it is desirable to carry out the withdrawal under conditions where the prepared liquid remains in the reaction vessel. The remaining prepared liquid is the largest particle with the most particle growth. By mixing this prepared liquid with the withdrawn liquid, particles with a wider distribution are obtained, and the components of the remaining reaction liquid become the components of the large particle peak of the silica microparticles according to this embodiment. Furthermore, by adjusting the withdrawal rate ratio, the shape of the distribution can be adjusted to one that also has a peak on the small particle side, and the peak ratio between the small particle side and the large particle side can also be adjusted. If the remaining preparation liquid and the withdrawn liquid are not mixed, the distribution shape will have no peak on the large particle side. The inventors conducted a tracing experiment and found that in a process in which a seed particle dispersion and an acidic silicic acid liquid are continuously added in a reaction vessel equipped with an overflow line, as in the manufacturing method of Patent Document 1, adjusting the withdrawal rate ratio does not result in a particle size distribution that has a peak on the large particle side as in the present invention.
[0066] (Withdrawal Speed Ratio) The production method according to this embodiment is characterized in that, while an acidic silicic acid solution is added to the reaction solution to grow particles, the reaction solution is withdrawn in order to broaden the particle size distribution. When the addition rate [g / min] (calculated as dry silica) of the acidic silicic acid solution during treatment A in step 2a is X, and the withdrawal rate [g / min] (calculated as dry silica) during withdrawal of the reaction solution (withdrawal solution) from the reaction vessel during treatment B in step 2a is Z, the withdrawal speed ratio (X / Z) defined by the following formula is preferably in the range of 0.2 to 3.0, more preferably in the range of 0.5 to 2.0, and particularly preferably in the range of 0.6 to 1.8. Withdrawal rate ratio (X / Z) = (dry silica [g] of acidic silicic acid solution per hour) / (dry silica [g] of withdrawn solution per hour) Generally, when the withdrawal rate ratio is 1.0, the rate of dry silica added to the reaction vessel and the rate of dry silica withdrawn are the same, so the dry silica in the reaction vessel is constant, and although it depends on the concentration of the raw material, the liquid level in the reaction vessel is usually roughly constant. When the withdrawal rate ratio is greater than 1.0, the amount of withdrawal is small, so the dry silica in the reaction vessel increases, and usually the liquid level in the reaction vessel gradually rises. On the other hand, when the withdrawal rate ratio is less than 1.0, the dry silica in the reaction vessel decreases, and usually the liquid level in the reaction vessel gradually drops. In this embodiment, when the withdrawal rate ratio is less than 0.2, the withdrawal rate is too fast, so the reaction vessel becomes empty or nearly empty in a short reaction time, and the reaction must be terminated, and the particle size distribution is not sufficiently broad. On the other hand, if the withdrawal rate ratio is more than 3.0, the addition rate of the acidic silicic acid solution is too fast, which tends to cause self-nucleation by the acidic silicic acid solution. In addition, the dry silica in the reaction vessel gradually increases, and the level of the prepared liquid usually rises. Therefore, the reaction vessel may overflow. Even if the reaction vessel does not overflow, the size of the reaction vessel must be increased, which is not economical.
[0067] (Heat Aging) In step 2a, after treatment A and treatment B have been carried out, it is preferable to heat-age the remaining reaction liquid. The aging temperature is preferably in the range of 40°C to 98°C, more preferably in the range of 60°C to 98°C. The aging time is preferably in the range of 20 minutes to 120 minutes, more preferably in the range of 30 minutes to 90 minutes. Such heat-aging can complete the reaction. If heat-aging is not carried out, the added acidic silicic acid liquid may remain without being deposited on the particle surface, which may impair the stability of the silica sol.
[0068] In step 2a, when the acidic silicic acid solution is added, a base may be added as a pH adjuster as needed to adjust the pH of the dispersion within the above range. Examples of the base include alkali metal hydroxides such as NaOH and KOH, metal carbonates such as potassium oxide, sodium carbonate, and ammonium carbonate, amines such as ammonia, monoethanolamine, and piperazine, and basic nitrogen compounds such as quaternary ammonium hydroxides such as tetramethylammonium.
[0069] (Step 3a) In step 3a, the reaction liquid remaining in the reaction vessel at the end of step 2a is mixed with the reaction liquid withdrawn in process B of step 2a to obtain a silica fine particle dispersion for polishing. In process B of step 2a, continuous withdrawal is performed, but it is desirable to perform the withdrawal under conditions where the reaction liquid remains in the reaction vessel. The reaction liquid remaining in the reaction vessel contains the particles with the largest particle size, which have grown the most. This is because mixing this reaction liquid with the withdrawn liquid results in particles with a wider distribution. Furthermore, when this reaction liquid and the withdrawn liquid are mixed, the particle size distribution becomes a distribution with a peak on the large particle side. Furthermore, by adjusting the withdrawal rate ratio, the distribution shape can be adjusted to a distribution shape with a peak on the small particle side as well, and the peak ratio between the small particle side and the large particle side can also be adjusted. Note that if the reaction liquid remaining in the reaction vessel and the withdrawn liquid are not mixed, the distribution shape does not have a peak on the large particle side.
[0070] (Concentration Step) The silica fine particle dispersion for polishing obtained by the first method for producing a silica fine particle dispersion for polishing according to this embodiment, which includes steps 1a to 3a, may be concentrated to a desired concentration after adjusting the temperature to a range of from room temperature to about 50°C. The concentration method is not particularly limited, but the concentration can be performed using an ultrafiltration membrane, a rotary evaporator, or the like. If desired, coarse particles may be removed by centrifugation or a filtration process using a filter, etc.
[0071] [Second Method for Producing Silica Fine Particle Dispersion for Polishing] Next, a second method for producing a silica fine particle dispersion for polishing according to this embodiment will be described. The silica fine particle dispersion for polishing according to this embodiment described above can be suitably produced, for example, by the second method for producing a silica fine particle dispersion for polishing according to this embodiment. The second method for producing a dispersion according to this embodiment must include the following steps 1b to 4b.
[0072] (Step 1b) In Step 1b, the raw materials, an acidic silicic acid solution and an alkali, are introduced into a reaction vessel maintained in an unheated state, and a solvent is added as necessary to prepare a first preparation. In this specification, the first preparation is also referred to as the "Step 1b solution." When these raw materials are introduced into the reaction vessel, splashing occurs on the bottom or inner wall of the reaction vessel or on the liquid surface (the liquid surface of the introduced acidic silicic acid solution and alkali). If the raw materials are introduced into a heated reaction vessel, these splashed raw materials tend to dry out, resulting in the formation of large, problematic aggregates. Introducing the raw materials gradually to avoid splashing increases the preparation time and reduces economic efficiency. When the seed particle dispersion and alkali are added to a heated reaction vessel, as in the process of Patent Document 2, the seed particle dispersion and alkali are heated from the beginning of the addition, which can lead to the problem of seed particle aggregation occurring early on. The "unheated state" refers to the absence of any operation to raise the temperature of the reaction vessel. If the temperature of the reaction vessel exceeds 40° C. in an unheated state due to seasonal high temperatures or the like, it is recommended to cool the reaction vessel so that the temperature is less than 40° C. It is preferable that the temperatures of the acidic silicic acid solution and alkali when introduced into the reaction vessel are both less than 40° C.
[0073] (Acidic silicic acid solution) The acidic silicic acid solution can be obtained by dealkalizing an aqueous solution of alkaline silicate with a cation exchange resin. The concentration of the acidic silicic acid solution is 2 The silica concentration in the first preparation is preferably in the range of 0.1% by mass to 10% by mass, more preferably in the range of 1% by mass to 7% by mass, and particularly preferably in the range of 2% by mass to 6% by mass, in terms of oxide. The pH of the acidic silicic acid solution is preferably in the range of 1 to 3. The amounts of the acidic silicic acid solution and alkali are added so that the molar ratio of silica to alkali (in terms of oxide) in the first preparation is in the range of 1 to 10, and further adjusted by adding a solvent as necessary so that the silica concentration in the preparation is in the range of 0.1% by mass to 15% by mass. Here, the molar ratio of silica to alkali (in terms of oxide) is defined as the molar ratio = [SiO 2 moles of] / [A 2The molar ratio of silica to alkali (oxide equivalent) is expressed as [number of moles of O] (where A represents alkali metal, ammonia, organic alkali, or alkali metal in aqueous glass, etc.). If the molar ratio of silica to alkali (oxide equivalent) is less than 1, the amount of alkali is excessive, so the ionic strength in the first preparation becomes excessively high, and the silica microparticles produced in the subsequent steps 2b and 3b aggregate, making it difficult to obtain spherical particles or causing sedimentation. Even if sedimentation does not occur, the number of aggregates of silica microparticles increases, making it difficult to obtain a monodispersed silica sol. On the other hand, if the molar ratio of silica to alkali (oxide equivalent) exceeds 10, the amount of silica is large, so only small particles are obtained, making it difficult to adjust to the desired size. In addition, because the amount of alkali is relatively small, the pH of the reaction solution becomes significantly lower when an acidic silicic acid solution is added in the subsequent step 2b. As a result, the added acidic silicic acid solution does not deposit on the surface of the produced silica microparticles, and self-nucleation by silicic acid occurs, which ultimately tends to make it difficult to obtain a silica sol with the desired particle size. The molar ratio of silica to alkali is preferably in the range of 2 to 8, more preferably in the range of 2.5 to 6. When the silica concentration in the first preparation is less than 0.1% by mass, monodispersed silica microparticles are easily obtained, but the low silica concentration in the first preparation makes production inefficient and uneconomical. Furthermore, when the silica concentration exceeds 15% by mass, the silica microparticles tend to aggregate during preparation, making it difficult to obtain monodispersed silica microparticles. The silica concentration in the first preparation is more preferably in the range of 0.2% to 10% by mass, and particularly preferably in the range of 0.3% to 8% by mass. When the molar ratio of silica to alkali (oxide equivalent) and the silica concentration in the first preparation are within the aforementioned ranges, most of the silica microparticles avoid aggregation, but some aggregate to form irregularly shaped particles. As a result, the silica microparticles contained in the silica microparticle dispersion according to this embodiment are mostly spherical particles, but contain irregularly shaped particles at a number of 1.0% to 10% by number.
[0074] (Alkali) Examples of the alkali added in step 1b include alkali silicates such as sodium silicate (water glass) and potassium silicate, alkali metals such as sodium hydroxide, potassium hydroxide, and lithium hydroxide, ammonia, and organic alkalis such as organic amines. Here, the alkali is usually added as an aqueous alkali solution. The alkali concentration of the aqueous alkali solution is not particularly limited, but is usually used in the range of 1% by mass to 50% by mass.
[0075] (Solvent) Examples of the solvent added as needed in step 1b include water, ion-exchanged water, pure water, ultrapure water, a mixed solvent containing water and a water-soluble organic solvent, and a water-soluble organic solvent.
[0076] (Step 2b) In step 2b, the preparation liquid prepared in step 1b is uniformly stirred, heated, and maintained at a constant temperature (40°C to 98°C) for a certain period of time, and then, while maintaining the same temperature range, an acidic silicic acid solution is added continuously or intermittently to produce silica fine particles, thereby obtaining a second preparation liquid. In this specification, the second preparation liquid obtained in step 2b is also referred to as "step 2b liquid."
[0077] (Retention Temperature and Retention Time) In step 2b, the first preparation prepared in step 1b is heated to a temperature of 40°C to 98°C while stirring and maintained at this temperature for a certain period of time. The retention time is preferably 10 minutes to 120 minutes, more preferably 20 minutes to 90 minutes. This temperature maintenance allows the preparation to be sufficiently homogenized. A retention time of less than 10 minutes results in insufficient homogenization, and the subsequent addition of the acidic silicic acid solution tends to result in non-uniform generation and particle growth of silica microparticles. Furthermore, a retention time of more than 120 minutes prevents further homogenization of the preparation, and the longer retention time reduces production efficiency and reduces economic viability. Subsequently, while maintaining the temperature of the preparation at a temperature of 40°C to 98°C, the acidic silicic acid solution is added to generate silica microparticles. More specifically, at the beginning of the addition of the acidic silicic acid solution, core particles (silicic acid polymers) are first generated, and these core particles continue to grow with the added acidic silicic acid solution, thereby generating silica microparticles. The addition time of the acidic silicic acid solution is preferably 3 hours or more and 48 hours or less. If it is less than 3 hours, the addition speed of the acidic silicic acid solution is too fast, and self-nucleation of the acidic silicic acid solution is likely to occur in addition to the desired silica fine particles. If the addition time is more than 48 hours, self-nucleation of the acidic silicic acid solution does not occur, but the preparation time becomes too long, resulting in poor economic efficiency. The particle size distribution of the silica fine particles produced in this step 2b shows a normal distribution, which is a relatively sharp particle size distribution. The amount (total amount) of the acidic silicic acid solution added in step 2b is determined based on the SiO contained in the second preparation liquid. 2 The molar ratio of the alkali A contained in the second preparation is defined as M2S, and the oxide equivalent of the alkali A (i.e., A 2When the molar ratio of M2S to M2A (calculated as O) is taken as M2A, the value of M2S / M2A is preferably in the range of 20 to 160. If the value of M2S / M2A is less than 20, the growth of silica microparticles in the silica microparticle dispersion obtained by the production method of this embodiment will be slow and their size will be small, resulting in an insufficient polishing rate when used as an abrasive. On the other hand, if the value of M2S / M2A exceeds 160, the particle size of the silica microparticles in the silica microparticle dispersion obtained by the production method of this embodiment will be too large, and when used as an abrasive, the occurrence of scratches on the substrate to be polished will be significant, which is undesirable. Furthermore, in such cases, the preparation time will be extremely long, resulting in poor economic efficiency. The value of M2S / M2A is more preferably in the range of 40 to 140, even more preferably in the range of 50 to 130, and particularly preferably in the range of 60 to 120.
[0078] (Step 3b) In step 3b, following step 2b, the following processes A and B are carried out simultaneously. Process A: An acidic silicic acid solution and an alkali are each added continuously or intermittently to the reaction vessel filled with the second preparation to prepare a reaction solution. Process B: A portion of the reaction solution in the reaction vessel is continuously or intermittently withdrawn.
[0079] In step 3b, the second preparation liquid filled in a reaction vessel is added with acidic silicic acid solution to prepare a reaction liquid that grows silica microparticles to a desired size (here, in order to maintain the pH of the reaction liquid, alkali is added and acidic silicic acid solution for particle growth is added simultaneously), and the process B of extracting a part of the reaction liquid from the reaction vessel is carried out simultaneously.In step 3b, the second preparation liquid (step 2b liquid) immediately undergoes particle growth reaction by adding acidic silicic acid solution, so after the start of adding acidic silicic acid solution in step 3b, it is also referred to as "reaction liquid" or "step 3b liquid" for convenience.In step 4b, as will be described in detail later, the reaction liquid remaining in the reaction vessel after step 3b is aged at high temperature, and then the reaction liquid extracted in step B is added and mixed, thereby obtaining the silica microparticle dispersion liquid for polishing according to this embodiment with a broader particle size distribution (wider particle size distribution range).
[0080] Regarding the amount of acidic silicic acid solution added to the step 3b solution in step 3b, where M3S is the number of moles of silica contained in the step 3b solution and M3A is the number of moles of alkali in terms of oxide contained in the step 3b solution, the value of M3S / M3A is preferably in the range of 20 to 160. If the value of M3S / M3A is less than 20, the growth of silica microparticles in the silica microparticle dispersion obtained by the production method of this embodiment will be slow, and the size will be small and it will be difficult to achieve a broad distribution, resulting in an insufficient polishing rate even when used as an abrasive. On the other hand, if the value of M3S / M3A exceeds 160, the particle size of the silica microparticles in the silica microparticle dispersion obtained by the production method of this embodiment will be too large, and when used as an abrasive, the occurrence of scratches on the polished substrate will be significant, which is undesirable. Furthermore, in such cases, the preparation time will be very long, which will reduce economic efficiency. The value of M3S / M3A is more preferably in the range of 40 or more and 140 or less, further preferably in the range of 50 or more and 130 or less, and particularly preferably in the range of 60 or more and 120 or less.
[0081] (Reaction temperature) The temperature of the step 3b liquid when adding the acidic silicic acid liquid to the step 3b liquid is preferably in the range of 40°C or higher and 98°C or lower. If the temperature of the step 3b liquid is lower than 40°C, the added acidic silicic acid liquid is less likely to dissolve, making it difficult to deposit on the surface of the silica microparticles. As a result, self-nucleation by silicic acid occurs, making it impossible to obtain the desired size. If the temperature of the step 3b liquid is higher than 98°C, the added acidic silicic acid liquid is sufficiently dissolved and the silica microparticles grow, but the temperature of the silica microparticle dispersion or reaction liquid is excessively high, which poses problems in terms of energy efficiency and safety. It is more preferable that the temperature of the step 3b liquid when adding the acidic silicic acid liquid to the step 3b liquid is in the range of 50°C or higher and 98°C or lower.
[0082] (Addition rate of acidic silicic acid solution) In this embodiment, in the treatment A of step 3b, the addition rate when the acidic silicic acid solution is added to the reaction vessel filled with the solution of step 3b is expressed as the dry silica [g] in the acidic silicic acid solution added per minute per mass [g] of silica particles contained in the solution in the reaction vessel. Here, [g / min g] is used as the unit of the addition rate of the acidic silicic acid solution to the liquid. Note that the "solution" is a convenient name for the liquid filled in the reaction vessel, and the silica microparticle dispersion filled in the reaction vessel becomes a reaction liquid as the particle growth reaction progresses with the start of the addition of the acidic silicic acid solution in treatment A. The solution encompasses the silica microparticle dispersion or the reaction liquid, and refers to the liquid present in the reaction vessel. Note that in this specification, the silica component contained in the liquid is also referred to as "dry silica". The addition rate of the acidic silicic acid solution to the liquid is preferably in the range of 0.0001 g / min g to 0.05 g / min g. Within the above range, the acidic silicic acid solution added for particle growth is dissolved by the alkali in the step 3 solution and precipitates on the surface of the silica microparticles, thereby promoting particle growth of the silica microparticles. If the addition rate of the acidic silicic acid solution to the liquid is less than 0.0001 g / min·g, the blending time becomes too long for practical use, reducing practicality and economic efficiency. If the addition rate of the acidic silicic acid solution to the liquid exceeds 0.05 g / min·g, self-nucleation may proceed without the silicic acid being precipitated on the particle surface, which is undesirable. The addition rate of the acidic silicic acid solution to the liquid is more preferably in the range of 0.0005 g / min·g to 0.02 g / min·g, and particularly preferably in the range of 0.001 g / min·g to 0.01 g / min·g. In treatment A of step 3b of this embodiment, the addition rate of the acidic silicic acid solution to the liquid can be calculated using the following formula, where S is the addition rate of the acidic silicic acid solution (in terms of dry silica) per unit mass of dry silica contained in the solution in the reaction vessel: (S) = (addition rate of acidic silicic acid solution per dry silica) [g / min] ÷ (mass of dry silica in solution in reaction vessel) [g] Here, for example, if the addition rate of acidic silicic acid solution per dry silica mass changes in two stages, the dry silica mass of the particles in the reaction vessel is calculated using the dry silica mass in the reaction vessel at the end of the first and second stages of addition, respectively.When the addition rate does not change, the calculation is made using the dry silica mass in the reaction vessel at the end of treatment A in step 3b. In this specification, the addition rate of the acidic silicic acid solution is calculated as described above using the amount of acidic silicic acid solution added (in terms of dry silica) per unit mass (unit area of silica fine particles) per unit time, whether the addition of the acidic silicic acid solution is continuous or intermittent.
[0083] The addition rate [g / min] of the acidic silicic acid solution is changed one or more times, and the addition rate at the nth time is set to L n When [g / min] is used, L n+1 ≦L n It is preferable to satisfy the relationship: where n is a positive integer. That is, it is desirable to change the addition rate of the acidic silicic acid liquid during preparation one or more times and gradually decrease the addition rate. In step 3b, in order to grow particles to the desired size, acidic silicic acid liquid is added to grow the particles, but in the present invention, the reaction liquid is continuously withdrawn, so the number of particles decreases. Therefore, the acidic silicic acid liquid may not deposit on the particle surface, and self-nucleation by silicic acid may occur. By decreasing the addition rate of the acidic silicic acid liquid from the second stage onwards, the occurrence of self-nucleation can be prevented and particles can be grown to the desired size.
[0084] (Alkali Addition Rate) In treatment A of step 3b, it is desirable to add alkali continuously or intermittently to the step 3b solution simultaneously with the addition of the acidic silicic acid solution in order to maintain the pH of the reaction solution. The alkali addition rate depends on the type and concentration of the alkali and cannot be uniformly limited, but it is desirable to add it so that the pH of the reaction solution is in the range of 8.5 to 13.0. If the pH of the reaction solution exceeds 13.0, the ionic strength in the reaction solution becomes too high, causing the silica microparticles to aggregate and settle, or the particles to become irregular in shape, making it difficult to obtain the desired particles. If the pH is less than 8.5, the added acidic silicic acid solution becomes difficult to dissolve, which tends to cause self-nucleation by silicic acid. It is more preferable that the pH of the reaction solution is in the range of 9.0 to 12.5.
[0085] (SiO of the solution in the reaction vessel 2 / A 2In step 3b, an acidic silicic acid solution is added continuously or intermittently to the solution in the reaction vessel, but the reaction solution is also extracted continuously or intermittently, so the pH of the reaction solution tends to decrease. When the pH decreases, the added acidic silicic acid solution becomes less soluble, and self-nucleation by silicic acid tends to occur easily. Therefore, in order to maintain the pH of the solution in the reaction vessel, it is desirable to add an alkali to adjust the pH. At this time, the SiO of the solution in the reaction vessel 2 / A 2 By adding an alkali so that the O molar ratio falls within the range of 20 to 160, the pH can be adjusted to a desired value.
[0086] (pH of the solution in the reaction vessel) As described above, the SiO 2 / A 2 The type of alkali to be added to adjust the O molar ratio to 20 or more and 160 or less is not particularly limited, but examples thereof include sodium hydroxide, potassium hydroxide, lithium hydroxide, ammonia, and organic amines. The pH of the reaction solution adjusted by adding an alkali is preferably in the range of 8.5 or more and 13.0 or less, more preferably in the range of 9.0 or more and 12.5 or less. If the pH exceeds 13.0, the ionic strength in the reaction solution becomes too high, causing the silica fine particles to aggregate and settle, or the particles to become irregular in shape, making it difficult to obtain the desired particles. If the pH is less than 8.5, the added acidic silicic acid solution becomes difficult to dissolve, so self-nucleation by silicic acid tends to occur.
[0087] (Process B) In Process B of step 3b, an acidic silicic acid solution is continuously or intermittently added to the solution in the reaction vessel to generate a reaction solution, and a portion of the reaction solution is continuously withdrawn. Here, the withdrawn reaction solution is also referred to as the "extracted solution." In the early stages of withdrawal, the particle growth reaction has started but the silica microparticles have not yet grown sufficiently, so small silica microparticles are extracted. However, in the later stages of withdrawal, the silica microparticles have grown sufficiently, so large silica microparticles are extracted. By continuously withdrawing the extracted solution in this way, silica microparticles with a wide particle size distribution can be obtained from the extracted solution. It is also desirable to mix the reaction solution remaining in the reaction vessel with the extracted solution. In step 3b, continuous withdrawal is performed, but it is desirable to perform the withdrawal under conditions where the prepared solution remains in the reaction vessel. The remaining prepared solution is the particles with the largest particle size, with the most particle growth. By mixing this prepared solution with the extracted solution, particles with a wider distribution can be obtained, and the components of the remaining reaction solution become the components of the large particle peak of the silica microparticles according to this embodiment. Furthermore, by adjusting the withdrawal rate ratio, the shape of the distribution can be adjusted to one that also has a peak on the small particle side, and the peak ratio between the small particle side and the large particle side can also be adjusted. If the remaining preparation liquid and the withdrawn liquid are not mixed, the distribution shape will have no peak on the large particle side. The inventors conducted a tracing experiment and found that in a process in which a seed particle dispersion and an acidic silicic acid liquid are continuously added in a reaction vessel equipped with an overflow line, as in the manufacturing method of Patent Document 1, adjusting the withdrawal rate ratio does not result in a particle size distribution that has a peak on the large particle side as in the present invention.
[0088] (Withdrawal Speed Ratio) The production method according to this embodiment is characterized in that, while an acidic silicic acid solution is added to the reaction solution to grow particles, the reaction solution is withdrawn in order to broaden the particle size distribution. When the addition rate [g / min] (calculated as dry silica) of the acidic silicic acid solution during addition in treatment A of step 3b is X, and the withdrawal rate [g / min] (calculated as dry silica) during withdrawal of the reaction solution (withdrawal solution) from the reaction vessel in treatment B of step 3b is Z, the withdrawal speed ratio (X / Z) defined by the following formula is preferably in the range of 0.2 to 3.0, more preferably in the range of 0.5 to 2.0, and particularly preferably in the range of 0.6 to 1.8. Withdrawal rate ratio (X / Z) = (dry silica [g] of acidic silicic acid solution per hour) / (dry silica [g] of withdrawn solution per hour) Generally, when the withdrawal rate ratio is 1.0, the rate of dry silica added to the reaction vessel and the rate of dry silica withdrawn are the same, so the dry silica in the reaction vessel is constant, and although it depends on the concentration of the raw material, the liquid level in the reaction vessel is usually roughly constant. When the withdrawal rate ratio is greater than 1.0, the amount of withdrawal is small, so the dry silica in the reaction vessel increases, and usually the liquid level in the reaction vessel gradually rises. On the other hand, when the withdrawal rate ratio is less than 1.0, the dry silica in the reaction vessel decreases, and usually the liquid level in the reaction vessel gradually drops. In this embodiment, when the withdrawal rate ratio is less than 0.2, the withdrawal rate is too fast, so the reaction vessel becomes empty or nearly empty in a short reaction time, and the reaction must be terminated, and the particle size distribution is not sufficiently broad. On the other hand, if the withdrawal rate ratio is more than 3.0, the addition rate of the acidic silicic acid solution is too fast, which tends to cause self-nucleation by the acidic silicic acid solution. In addition, the dry silica in the reaction vessel gradually increases, and the level of the prepared liquid usually rises. Therefore, the reaction vessel may overflow. Even if the reaction vessel does not overflow, the size of the reaction vessel must be increased, which is not economical.
[0089] In step 3b, when the acidic silicic acid solution is added, a base may be added as a pH adjuster as needed to adjust the pH of the dispersion within the above range. Examples of the base include alkali metal hydroxides such as NaOH and KOH, metal carbonates such as potassium oxide, sodium carbonate, and ammonium carbonate, amines such as ammonia, monoethanolamine, and piperazine, and basic nitrogen compounds such as quaternary ammonium hydroxides such as tetramethylammonium.
[0090] (Step 4b) In step 4b, the reaction liquid remaining in the reaction vessel at the end of step 3b is heated and aged, and then mixed with the reaction liquid extracted in treatment B of step 3b to obtain a dispersion of silica fine particles for polishing.
[0091] (Heat aging) The remaining reaction liquid needs to be heat-aged. The aging temperature needs to be in the range of 40°C or higher and 98°C or lower, and more preferably in the range of 60°C or higher and 98°C or lower. The aging time needs to be in the range of 20 minutes or higher and 120 minutes or lower, and more preferably in the range of 30 minutes or higher and 90 minutes or lower. Such heat aging can complete the reaction. If heat aging is not performed, the added acidic silicic acid liquid may remain without being deposited on the particle surface, and the stability of the silica sol may be impaired.
[0092] (Mixing Treatment) In the process B of step 3b, as described above, continuous withdrawal is performed, but it is necessary to perform the withdrawal under conditions in which the reaction liquid remains in the reaction vessel. The reaction liquid remaining in the reaction vessel contains particles with the largest particle size, which have grown the most. This is because mixing this reaction liquid with the withdrawn liquid results in particles with a wider distribution. Furthermore, when this reaction liquid and the withdrawn liquid are mixed, the particle size distribution becomes a distribution with a peak on the large particle side. Furthermore, by adjusting the withdrawal rate ratio, the shape of the distribution can be adjusted to a distribution shape with a peak on the small particle side as well, and the peak ratio between the small particle side and the large particle side can also be adjusted. Note that when the reaction liquid remaining in the reaction vessel and the withdrawn liquid are not mixed, the distribution shape does not have a peak on the large particle side.
[0093] (Concentration Step) The silica fine particle dispersion for polishing obtained by the second method for producing a silica fine particle dispersion for polishing according to this embodiment, which includes steps 1b to 4b, may be concentrated to a desired concentration after adjusting the temperature to a range of from room temperature to about 50°C. The concentration method is not particularly limited, but the concentration can be performed using an ultrafiltration membrane, a rotary evaporator, or the like. If desired, coarse particles may be removed by centrifugation or a filtration process using a filter, etc.
[0094] Next, the present invention will be described in more detail with reference to examples, but the present invention is not limited to these examples. Furthermore, the methods for measuring various properties of silica microparticles or silica microparticle dispersions in the examples and comparative examples were as follows, unless otherwise specified.
[0095] (1) Particle diameter converted into specific surface area The particle diameter converted into specific surface area can be calculated by measuring the specific surface area Sa of the silica fine particles and using the following formula: (De) (nm) = 6000 / (ρ × Sa) (where ρ is the density of the silica fine particles, 2.2 [g / cm 3 ].) The specific surface area of the silica fine particles is 100 m 2 When the specific surface area (SA) is 4000 / g or more, sintering proceeds during firing in the BET method. In this case, the specific surface area (SA) was determined by the titration method, and the specific surface area-equivalent particle diameter (De) was calculated from the formula (De) = 6000 / (SA × ρ). <BET method> 50 mL of a silica fine particle dispersion containing silica fine particles (silica concentration 40% by mass) was dissolved in HNO 3The pH was adjusted to 3.5 with 100 mL of 1-propanol, 40 mL of 1-propanol was added, and the sample was dried at 110°C for 16 hours. The sample was then crushed in a mortar and calcined in a muffle furnace at 500°C for 1 hour to prepare a measurement sample. Then, using a specific surface area measuring device (manufactured by Yuasa Ionics, model number Multisorb 12), the nitrogen adsorption method (BET method) was used to calculate the specific surface area from the amount of nitrogen adsorbed by the BET single-point method. Specifically, 0.5 g of the sample was placed in a measurement cell and degassed for 20 minutes at 300°C in a mixed gas flow of 30 v% nitrogen and 70 v% helium. The sample was then maintained at liquid nitrogen temperature in the mixed gas flow, and nitrogen was adsorbed onto the sample at equilibrium. Next, the sample temperature was gradually raised to room temperature while the mixed gas was flowing. The amount of nitrogen desorbed during this period was detected, and the specific surface area of the silica microparticles was calculated using a calibration curve prepared in advance. <Titration Method> First, SiO 2 A sample equivalent to 1.5 g of the sample was placed in a beaker and transferred to a thermostatic reactor (25°C), and pure water was added to bring the volume to 90 mL. The following operations were performed in a thermostatic reactor maintained at 25°C. Next, 0.1 mol / L hydrochloric acid aqueous solution was added to the beaker to adjust the pH to 3.6. 30 g of sodium chloride was then added, and the mixture was diluted to 150 mL with pure water and stirred for 10 minutes. A pH electrode was then attached, and 0.1 mol / L sodium hydroxide solution was added dropwise while stirring to adjust the pH to 4.0. The sample adjusted to pH 4.0 was then titrated with 0.1 mol / L sodium hydroxide solution. The titer and pH values were recorded at four or more points in the pH range of 8.7 to 9.3, and a calibration curve was created using the titer of 0.1 mol / L sodium hydroxide solution as X and the pH value at that time as Y. Then, the consumption amount V (mL) of 0.1 mol / L sodium hydroxide solution required to change the pH from 4.0 to 9.0 per 1.5 g of SiO2 was calculated from the formula V = (A × f × 100 × 1.5) / (W × C), and the specific surface area was calculated using this amount V according to the formula SA = 29.0V - 28. In the above formula, A is the amount of SiO2 consumed. 2 where f is the titer (mL) of 0.1 mol / L sodium hydroxide solution required per 1.5 g to change the pH from 4.0 to 9.0, C is the SiO2 concentration (%) of the sample, and W is the amount of sample taken (g).
[0096] (2) Weight-converted particle size distribution and weight-average particle size (D 50 The silica particle dispersion was diluted with a 0.05% by mass aqueous solution of sodium dodecyl sulfate to a solids concentration of 2% by mass. 0.1 mL of this was then injected with a syringe into a known disc centrifugal particle size distribution analyzer (manufactured by CPS INSTRUMENTS) and measured in a density gradient solution of 8% to 24% sucrose at 18,000 rpm to determine the weight-equivalent particle size distribution. From the measurement results of the weight-equivalent particle size distribution, the cumulative 10% particle size (D 10 ), cumulative 90% particle diameter (D 90 ) and cumulative 50% particle diameter (D 50 ) was calculated.
[0097] (3) Average sphericity and irregular particle ratio of particle groups measured by image analysis Using a scanning electron microscope (magnification 200,000 times), 200 silica microparticles contained in a silica microparticle dispersion were measured in an image or photograph containing 200 or more silica microparticles in the same field of view. 200 randomly selected silica microparticles were measured for their minor and major diameters, and the minor diameter / major diameter ratio was calculated for each randomly selected field of view to create a particle size distribution for the particle group. In this specification, an ultra-high resolution field emission scanning electron microscope S-5500 (manufactured by Hitachi High-Technologies Corporation) was used as the scanning electron microscope. The specific method for measuring silica microparticles was to define the maximum diameter of the projected silica microparticle image as the major axis, measure its length, and define this value as the major axis. Furthermore, a point was determined on the major axis that bisects the major axis, and two points where a straight line perpendicular to this intersects with the outer edge of the silica microparticle image were determined. The distance between these two points was measured and defined as the minor axis, and the irregularity (minor axis / major axis ratio) was calculated. From the particle size distribution of the particle group, the average sphericity of the particle group and the irregular particle ratio (number of irregular shaped particles / total number of particles×100) were calculated.
[0098] (4) Coefficient of variation of particle size distribution area A silica fine particle dispersion liquid having a silica concentration of 1% by mass was prepared, and the coefficient of variation was determined from the weight-equivalent particle size distribution of the particle group using a disc centrifugal particle size distribution measuring device (manufactured by CPS INSTRUMENTS). In the weight-equivalent particle size distribution of the particle group, the cumulative 1% particle size (D1 ) to obtain the cumulative 99% particle diameter (D 99 The particle size range from 1 to 6 was divided into six equal parts, and the particle size ranges were designated as S1, S2, S3, S4, S5, and S6. The coefficient of variation (CV value) of the particle size distribution area corresponding to each particle size range was calculated.
[0099] (5) Polishing test method <SiO 2 Polishing of a film> The polishing abrasive dispersion obtained in each of the examples and comparative examples was prepared. Here, the solid content concentration was 1.0 mass % and nitric acid was added to adjust the pH to 6.0. Next, a SiO2 film prepared by a deposition method was used as a substrate to be polished. 2 Insulating film or SiO produced by thermal oxidation 2 A substrate having a thermal oxide film (each 2 μm thick) was prepared. Next, this substrate to be polished was placed in a polishing apparatus (NF300, manufactured by Nanofactor Co., Ltd.), and polishing was performed using a polishing pad ("IC-1000 / SUBA400 concentric type" manufactured by Nitta Haas Corporation) with a substrate load of 0.08 MPa, a table rotation speed of 87 rpm, and a polishing head rotation speed of 93 rpm. The polishing abrasive dispersion was supplied at a rate of 20 mL / min for 15 minutes. The weight change of the substrate to be polished before and after polishing was then determined, and the polishing rate was calculated. <Polishing of Aluminum Hard Disks> The polishing abrasive dispersion obtained in each of the Examples and Comparative Examples was prepared. Here, the solids concentration was 9% by mass, and the pH was adjusted to 2.0 by adding nitric acid. An aluminum hard disk substrate was set in a polishing machine (NF300, manufactured by Nanofactor Co., Ltd.) and polished using a polishing pad (Polytex φ12, manufactured by Nitta Haas Co., Ltd.) with a substrate load of 0.05 MPa, a table rotation speed of 30 rpm, and a polishing head rotation speed of 60 rpm, while supplying a polishing abrasive dispersion at a rate of 20 mL / min for 10 minutes. The entire surface was observed using Zoom 15 with an ultrafine defect visualization macro device (product name: Micro-Max, manufactured by VISION PSYTEC Co., Ltd.), and a 65.97 cm 2 The number of scratches (linear marks) present on the polished substrate surface corresponding to the number of scratches was counted and totaled.
[0100] (6) Measurement of the mass ratio of polyethyleneimine to silica mass at the equivalent point In the flow potential measurement (using cationic polymer polyethyleneimine [weight average molecular weight 600] as titration reagent), the mass ratio of polyethyleneimine to silica mass at the equivalent point was measured. Specifically, for the obtained dispersion of silica particles for polishing, the cationic solid content [cationic polymer polyethyleneimine (weight average molecular weight 600)] added amount (V [g]) of the cationic titration solution in the knick and the SiO 2 Ratio of solid content [g] (V / SiO 2 The cation titration was carried out as follows, and V / SiO 2 was determined. The cation titration was carried out by dropping 0.08% by mass of polyethyleneimine (molecular weight 600) as the cation titrant into 80 g of silica particle dispersion liquid adjusted to a solid content concentration of 0.5% by mass. The amount of the cation titrant dropped (mL) was plotted on the x-axis and the streaming potential (mV) of the dispersion liquid on the y-axis, to obtain a potential flow curve that plotted the relationship between the amount dropped and the streaming potential. In this potential flow curve, the point (inflection point) where the amount of change in streaming potential relative to the amount dropped significantly changes is designated as the knick. The amount of cationic solid content added (V, g) was determined from the amount of the cation colloid titrant dropped at the knick. From these results, V / SiO 2 V: Amount of cationic solids added to the cationic titrant in the test piece (g) SiO 2 : solid content of silica fine particles subjected to titration (g)
[0101] [Preparation of Acidic Silicic Acid Solution] Aqueous sodium silicate solution (silica concentration 24.06 mass%, Na 2 Pure water was added to the resulting sodium silicate solution (silica concentration: 5% by mass). 18 kg of the resulting sodium silicate solution was added to 6 L of a strongly acidic cation exchange resin (SK1BH, manufactured by Mitsubishi Chemical Corporation) at a space velocity of 3.0 h -1 The acidic silicic acid solution was passed through the reactor at a rate of 1000 rpm, and 18 kg of the solution (silica concentration: 4.5% by mass, pH: 2.7) was obtained. In the following Examples and Comparative Examples, this acidic silicic acid solution or an acidic silicic acid solution equivalent to this acidic silicic acid solution was appropriately concentrated or diluted and used as the raw material.
[0102] [Example 1-1] 4527 g of pure water at a temperature of 25°C was placed in an unheated blending tank (a reaction vessel with an internal volume of 10 L), and a silica fine particle dispersion (Cataloid SI-50, manufactured by JGC Catalysts and Chemicals, SiO 2 Concentration 48.35% by mass, Na 2 A potassium hydroxide solution (KOH concentration 48.7% by mass, specific surface area converted particle diameter 26.2 nm, liquid temperature 25°C) was added to obtain a diluted silica microparticle dispersion. A potassium hydroxide solution (KOH concentration 48.7% by mass, Super Kali R manufactured by Toagosei Co., Ltd.) was diluted with pure water to a KOH concentration of 4.8% by mass, and 20.83 g of the potassium hydroxide solution was added to the diluted silica microparticle dispersion and stirred until homogeneous. After stirring, the mixture was heated to 95°C and maintained for 30 minutes. Subsequently, an acidic silicic acid solution (SiO 2 14.198 kg of an aqueous solution of potassium hydroxide (KOH concentration: 4.45% by mass) and 1.475 kg of an aqueous solution of potassium hydroxide (KOH concentration: 1.0% by mass) were added over 18 hours. 2The addition rate of the aqueous solution of potassium hydroxide (KOH concentration 4.45% by mass, pH 2.7) was 14.40 g / min from the start of addition until 9 hours had elapsed, and 11.90 g / min from 9 hours to 18 hours had elapsed. The addition rate of the aqueous potassium hydroxide solution (KOH concentration 1.0% by mass) was 1.54 g / min from the start of addition until 9 hours had elapsed, and 1.19 g / min from 9 hours to 18 hours had elapsed. Simultaneously with the addition of the acidic silicic acid solution and the aqueous potassium hydroxide solution, 15.04 kg of a portion of the reaction solution (hereinafter also referred to as the "extracted liquid") was extracted from the blending tank. The extraction rate of the extracted liquid was 15.93 g / min from the start of extraction until 9 hours had elapsed, and 11.92 g / min from 9 hours to 18 hours had elapsed. After the addition of the acidic silicic acid solution and the aqueous potassium hydroxide solution and the withdrawal of the withdrawn solution were completed, 5.59 kg of reaction solution remained in the blending tank. This solution was maintained at 95°C for 1 hour and then cooled to room temperature. The ratio of dry silica in the acidic silicic acid solution during the reaction to dry silica in the withdrawn solution (dry silica in acidic silicic acid solution / dry silica in the withdrawn solution) is shown in Table 1. In the present specification, the silica solid content (mass) is also referred to as "dry silica". The reaction solution remaining in the blending tank and the withdrawn solution were mixed until uniform. The resulting mixed solution had a pH of 10.2, a specific surface area-based particle size of 45.5 nm, and SiO 2 The concentration was 4.03% by mass. This mixture was filtered using an ultrafiltration membrane SIP-1013 manufactured by Asahi Kasei Corporation. 2 The resulting dispersion was concentrated to a concentration of 12.0% by mass to obtain a dispersion of fine silica particles for polishing. The obtained dispersion of fine silica particles for polishing was evaluated using the methods described above, and the evaluation results were as shown in Table 2. The conditions for preparing the dispersion of fine silica particles for polishing in Example 1 are shown in Table 1.
[0103] [Examples 1-2 and 1-3] A dispersion of fine silica particles for polishing was obtained in the same manner as in Example 1-1, except that the conditions for preparation were changed as shown in Table 1. The obtained dispersion of fine silica particles for polishing was then evaluated in the same manner as in Example 1-1. The obtained results are shown in Table 2.
[0104] Comparative Example 1-1: 4522 g of pure water at 95°C was added to a 10 L blending tank, and a silica fine particle dispersion (Cataloid SI-50, manufactured by JGC Catalysts and Chemicals, SiO 2 Concentration 48.35% by mass, Na 2 461.2 g of a solution (O concentration 0.49 mass%, specific surface area converted particle diameter 26.2 nm, liquid temperature 25°C) was added. 16.56 g of a solution prepared by diluting 48.6 mass% NaOH (sodium hydroxide manufactured by JGC Catalysts and Chemicals) with pure water to 4.8 mass% was added, and the mixture was stirred until homogenous and held for 30 minutes. Thereafter, SiO 2 21.520 kg of acidic silicic acid solution with a concentration of 4.55% by mass, 7.121 kg of a 0.25% by mass NaOH aqueous solution, and a silica fine particle dispersion (Cataloid SI-50 manufactured by JGC Catalysts and Chemicals Co., Ltd.) were mixed with pure water to obtain a SiO 2 3.519 kg of a solution diluted to a concentration of 12% was added over 48 hours. At this time, the addition rate of the acidic silicic acid solution was 7.47 g / min, the addition rate of the 0.25 mass% NaOH aqueous solution was 2.47 g / min, and the addition rate of the silica microparticle dispersion was 1.22 g / min. Furthermore, simultaneously with the addition, 32.47 kg of the preparation was withdrawn from the preparation tank. At this time, the withdrawal rate was 11.27 g / min. After the addition and withdrawal were completed, 4.49 kg of the preparation remained in the preparation tank, and this solution was cooled to room temperature. Note that the silica dry ratio of the acidic silicic acid solution silica dry to the withdrawn solution during preparation (acidic silicic acid solution silica dry / extracted solution silica dry) was 0.69. The reaction solution remaining in the preparation tank and the withdrawn reaction solution were mixed until uniform. The resulting mixture had a pH of 10.3, a specific surface area-equivalent particle diameter of 33.3 nm, and SiO 2 The concentration was 4.36% by mass. This mixture was filtered using an ultrafiltration membrane SIP-1013 manufactured by Asahi Kasei Corporation. 2 The silica fine particle dispersion was concentrated to a concentration of 12.0% by mass to obtain a silica fine particle dispersion. The obtained silica fine particle dispersion was evaluated in the same manner as in Example 1. The results are shown in Table 2. The conditions for preparing the silica fine particle dispersion in Comparative Example 1-1 are shown in Table 1.
[0105] Comparative Example 1-2 Cataloid SI-45P (silica fine particle dispersion) manufactured by JGC Catalysts and Chemicals, Ltd. was evaluated in the same manner as in Example 1. The results obtained are shown in Table 2.
[0106]
[0107]
[0108] Example 2-1 In a blending tank having an internal volume of 10 L, 304.66 g of pure water was added, and further, 6.72 g of an aqueous potassium hydroxide solution (KOH having a KOH concentration of 48.7% by mass (Super Potassium R manufactured by Toagosei Co., Ltd.)) was added. 2 160.88 g of an acidic silicic acid solution (concentration: 4.55% by mass) was added and stirred until the mixture was homogenized. After stirring, the mixture was heated to 98°C and maintained at this temperature for 30 minutes. 2 2.918 kg of the acidic silicic acid solution (concentration: 4.55% by mass) was added over 11 hours. At this time, the addition rate of the acidic silicic acid solution was 4.42 g / min. After the addition was completed, 351.27 g of pure water was added to maintain the temperature at 98°C. Next, the acidic silicic acid solution (SiO 2 14.338 kg of 0.5% by mass aqueous solution of potassium hydroxide (KOH concentration 4.55% by mass) and 3.046 kg of aqueous potassium hydroxide solution (KOH concentration 0.5% by mass) were added over 24 hours. Furthermore, simultaneously with the addition of the acidic silicic acid solution and the addition of the aqueous potassium hydroxide solution, a total of 17.24 kg of the reaction solution was withdrawn from the blending tank. The acidic silicic acid solution addition rate, 0.5% by mass aqueous potassium hydroxide solution addition rate, and withdrawal rate for each elapsed time period are shown in Table 3. The rate of addition of dry silica of the acidic silicic acid solution relative to dry silica for each elapsed time period is also shown in Table 3. After completion of addition and withdrawal, 3.50 kg of reaction solution remained in the blending tank, and this solution was held at 98°C for 1 hour and cooled to room temperature. The ratio of dry silica of the acidic silicic acid solution to dry silica of the withdrawn solution for each elapsed time period during blending (dry silica of acidic silicic acid solution / dry silica of withdrawn solution) is shown in Table 3. The reaction solution remaining in the mixing tank was mixed with the extracted reaction solution until homogeneous. The resulting mixture had a pH of 10.1, a specific surface area-based particle diameter of 36.9 nm, and SiO 2 The concentration was 3.75% by mass. This mixture was filtered using an ultrafiltration membrane SIP-1013 manufactured by Asahi Kasei Corporation.2 The resulting dispersion of silica particles for polishing was concentrated to a concentration of 12.0% to obtain a dispersion of silica particles for polishing. The obtained dispersion of silica particles for polishing was subjected to various evaluations using the methods described above, and the evaluation results were as shown in Table 4.
[0109] [Examples 2-2 and 2-3] A silica fine particle dispersion for polishing was obtained in the same manner as in Example 2-1, except that the preparation conditions were changed as shown in Table 3. The obtained silica fine particle dispersion for polishing was then evaluated in the same manner as in Example 2-1. The obtained results are shown in Table 4.
[0110] Comparative Example 2-1 A dispersion of fine silica particles for polishing was obtained in the same manner as in Comparative Example 1-1. The obtained dispersion of fine silica particles for polishing was then evaluated in the same manner as in Example 2-1. The obtained results are shown in Table 4.
[0111] Comparative Example 2-2 Cataloid SI-45P (silica fine particle dispersion) manufactured by JGC Catalysts and Chemicals Co., Ltd. was evaluated in the same manner as in Example 2-1. The obtained results are shown in Table 4.
[0112]
[0113] In Table 3, "addition rate of dry silica of acidic silicic acid solution relative to dry silica (at the end of the first stage)" refers to the mass [g] of dry silica in the acidic silicic acid solution added per minute per mass [g] of silica particles (dry silica) contained in the solution in the reaction vessel filled with the solution of step 3b in treatment A of step 3b. Here, "at the end of the first stage" refers to the end of the first addition when the addition rate of the acidic silicic acid solution is changed multiple times; in Example 2-1, the first time is the 4th hour, the second time is the 8th hour, the third time is the 12th hour, and so on.
[0114]
[0115] Examples 3-1 to 3-6 Examples 3-1 to 3-6 are shown below. The conditions for preparing each example are shown in Table 5. The obtained dispersion of silica fine particles for polishing was evaluated in the same manner as in Example 1-1. The obtained results are shown in Table 6.
[0116] Example 3-1: 4,408 g of pure water was added to a 10 L blending tank, and a silica fine particle dispersion (Cataloid SI-50, manufactured by JGC Catalysts and Chemicals, SiO 2 Concentration 48.43% by mass, Na 2 309.7 g of an aqueous solution of potassium hydroxide (concentration 48.7% by mass, Super Kali R manufactured by Toagosei Co., Ltd.) diluted with pure water to a concentration of 4.8% by mass was added, and the mixture was stirred until homogeneous. After stirring, the mixture was heated to 98°C and maintained for 30 minutes. Then, an acidic silicic acid solution (SiO 2 10.462 kg of an aqueous solution of potassium hydroxide (concentration: 4.50% by mass) and 4.385 kg of an aqueous solution of potassium hydroxide (concentration: 0.25% by mass) were added over 22 hours. Furthermore, simultaneously with the addition, 14.66 kg of the prepared liquid was withdrawn from the blending tank. The addition rate of the acidic silicic acid liquid and the addition and withdrawal rates of the aqueous solution of potassium hydroxide (concentration: 0.25% by mass) at this time are shown in Table 5. After the addition and withdrawal were completed, 4.55 kg of the prepared liquid remained in the blending tank, and this solution was held at 98°C for 1 hour and cooled to room temperature. The silica dry ratio of the acidic silicic acid liquid during blending to the silica dry ratio of the withdrawn liquid (acidic silicic acid liquid silica dry / extracted liquid silica dry) is shown in Table 5. The prepared liquid remaining in the blending tank and the withdrawn prepared liquid were mixed until uniform. The resulting mixed liquid had a pH of 10.2, a specific surface area-equivalent particle size of 44.0 nm, and SiO 2 The concentration was 3.17% by mass. This mixture was filtered using an ultrafiltration membrane SIP-1013 manufactured by Asahi Kasei Corporation. 2 The mixture was concentrated to a concentration of 12.0% by mass.
[0117] (Example 3-2) 4,381 g of pure water was added to a blending tank having an internal volume of 10 L, and a silica fine particle dispersion (Cataloid SI-50 manufactured by JGC Catalysts and Chemicals, SiO concentration 48.43 mass%, Na 2 309.7 g of an aqueous solution of potassium hydroxide (concentration 48.7% by mass, Super Kali R manufactured by Toagosei Co., Ltd.) diluted with pure water to a concentration of 4.8% by mass was added, and the mixture was stirred until homogeneous. After stirring, the mixture was heated to 98°C and maintained for 30 minutes. Then, 309.7 g of an acidic silicic acid solution (SiO 210.462 kg of an aqueous solution of potassium hydroxide (concentration: 4.50% by mass) and 4.315 kg of an aqueous solution of potassium hydroxide (concentration: 0.33% by mass) were added over 22 hours. Furthermore, simultaneously with the addition, 14.48 kg of the prepared liquid was withdrawn from the blending tank. The addition rate of the acidic silicic acid liquid and the addition and withdrawal rates of the aqueous solution of potassium hydroxide (concentration: 0.33% by mass) at this time are shown in Table 5. After the addition and withdrawal were completed, 4.68 kg of the prepared liquid remained in the blending tank, and this solution was held at 98°C for 1 hour and then cooled to room temperature. The silica dry ratio of the acidic silicic acid liquid during blending to the silica dry ratio of the withdrawn liquid (acidic silicic acid liquid silica dry / extracted liquid silica dry) is shown in Table 5. The prepared liquid remaining in the blending tank and the withdrawn prepared liquid were mixed until uniform. The resulting mixed liquid had a pH of 10.3, a specific surface area-equivalent particle size of 47.8 nm, and SiO 2 The concentration was 3.17% by mass. This mixture was filtered using an ultrafiltration membrane SIP-1013 manufactured by Asahi Kasei Corporation. 2 The mixture was concentrated to a concentration of 12.0% by mass.
[0118] (Example 3-3) 4371 g of pure water was added to a blending tank having an internal volume of 10 L, and a silica fine particle dispersion (Cataloid SI-50 manufactured by JGC Catalysts and Chemicals, SiO2 concentration 48.43 mass%, Na 2 309.7 g of an aqueous solution of potassium hydroxide (concentration 48.7% by mass, Super Kali R manufactured by Toagosei Co., Ltd.) diluted to 4.8% by mass with pure water was added, and the mixture was stirred until homogeneous. After stirring, the mixture was heated to 98°C and maintained for 30 minutes. Then, an acidic silicic acid solution (SiO 210.347 kg of an aqueous solution of potassium hydroxide (concentration: 4.50% by mass) and 4.391 kg of an aqueous solution of potassium hydroxide (concentration: 0.25% by mass) were added over 29 hours. Furthermore, simultaneously with the addition, 14.52 kg of the prepared liquid was withdrawn from the blending tank. The addition rate of the acidic silicic acid liquid and the addition and withdrawal rates of the aqueous solution of potassium hydroxide (concentration: 0.25% by mass) at this time are shown in Table 5. After the addition and withdrawal were completed, 4.54 kg of the prepared liquid remained in the blending tank, and this solution was held at 98°C for 1 hour and then cooled to room temperature. The ratio of dry silica of the acidic silicic acid liquid during blending to dry silica of the withdrawn liquid (dry silica of acidic silicic acid liquid / dry silica of withdrawn liquid) is shown in Table 5. The prepared liquid remaining in the blending tank and the withdrawn prepared liquid were mixed until uniform. The resulting mixed liquid had a pH of 10.1, a specific surface area-equivalent particle size of 45.5 nm, and SiO 2 The concentration was 3.19% by mass. This mixture was filtered using an ultrafiltration membrane SIP-1013 manufactured by Asahi Kasei Corporation. 2 The mixture was concentrated to a concentration of 12.0% by mass.
[0119] (Example 3-4) 4381 g of pure water was added to a blending tank having an internal volume of 10 L, and a silica fine particle dispersion (Cataloid SI-50 manufactured by JGC Catalysts and Chemicals, SiO concentration 48.43 mass%, Na 2 309.7 g of an aqueous solution of potassium hydroxide (concentration 48.7% by mass, Super Kali R manufactured by Toagosei Co., Ltd.) diluted with pure water to a concentration of 4.8% by mass was added, and the mixture was stirred until homogeneous. After stirring, the mixture was heated to 98°C and maintained for 30 minutes. Then, 309.7 g of an acidic silicic acid solution (SiO 210.462 kg of an aqueous solution of potassium hydroxide (concentration: 4.50% by mass) and 4.390 kg of an aqueous solution of potassium hydroxide (concentration: 0.33% by mass) were added over 29 hours. Furthermore, simultaneously with the addition, 14.81 kg of the prepared liquid was withdrawn from the blending tank. The addition rate of the acidic silicic acid liquid and the addition and withdrawal rates of the aqueous solution of potassium hydroxide (concentration: 0.33% by mass) at this time are shown in Table 5. After the addition and withdrawal were completed, 4.49 kg of the prepared liquid remained in the blending tank, and this solution was held at 98°C for 1 hour and cooled to room temperature. The ratio of dry silica of the acidic silicic acid liquid during blending to dry silica of the withdrawn liquid (dry silica of acidic silicic acid liquid / dry silica of withdrawn liquid) is shown in Table 5. The prepared liquid remaining in the blending tank and the withdrawn prepared liquid were mixed until uniform. The resulting mixed liquid had a pH of 10.3, a specific surface area-equivalent particle size of 47.0 nm, and SiO 2 The concentration was 3.17% by mass. This mixture was filtered using an ultrafiltration membrane SIP-1013 manufactured by Asahi Kasei Corporation. 2 The mixture was concentrated to a concentration of 12.0% by mass.
[0120] (Example 3-5) 47.12 kg of pure water was added to a blending tank having an internal volume of 200 L, and a silica fine particle dispersion (Cataloid SI-50 manufactured by JGC Catalysts and Chemicals, SiO concentration 48.39 mass%, Na 2 4350 g of an aqueous solution of potassium hydroxide (concentration 48.7% by mass, Super Kali R manufactured by Toagosei Co., Ltd.) diluted to 4.8% by mass with pure water was added, and the mixture was stirred until homogeneous. After stirring, the mixture was heated to 95°C and maintained for 30 minutes. Then, an acidic silicic acid solution (SiO 2147.75 kg of an aqueous solution of potassium hydroxide (concentration: 4.50% by mass) and 15.5 kg of an aqueous solution of potassium hydroxide (concentration: 1.0% by mass) were added over 18 hours. Furthermore, simultaneously with the addition, 165.05 kg of the prepared liquid was withdrawn from the blending tank. The addition rate of the acidic silicic acid liquid and the addition rate and withdrawal rate of the aqueous solution of potassium hydroxide (concentration: 1.0% by mass) at this time are shown in Table 5. After the addition and withdrawal were completed, 48.95 kg of the prepared liquid remained in the blending tank, and this solution was held at 95°C for 1 hour and cooled to room temperature. The ratio of dry silica of the acidic silicic acid liquid during blending to dry silica of the withdrawn liquid (dry silica of acidic silicic acid liquid / dry silica of withdrawn liquid) is shown in Table 5. The prepared liquid remaining in the blending tank and the withdrawn prepared liquid were mixed until uniform. The resulting mixed liquid had a pH of 10.3, a specific surface area-equivalent particle size of 44.7 nm, and SiO 2 The concentration was 4.07% by mass. This mixture was filtered using an ultrafiltration membrane SIP-2013 manufactured by Asahi Kasei Corporation. 2 The mixture was concentrated to a concentration of 12.0% by mass.
[0121] (Example 3-6) Into a blending tank having an internal volume of 10 L, 3,494 g of pure water was added, and further, a silica fine particle dispersion liquid (Cataloid SI-50 manufactured by JGC Catalysts and Chemicals, SiO concentration 48.39 mass%, Na 2 289.3 g of an aqueous solution of potassium hydroxide (concentration 48.7% by mass, Super Kali R manufactured by Toagosei Co., Ltd.) diluted to 4.8% by mass with pure water was added, and the mixture was stirred until homogenous. After stirring, the mixture was heated to 98°C and maintained for 30 minutes. Then, 289.3 g of an acidic silicic acid solution (SiO 215.193 kg of an aqueous solution of potassium hydroxide (concentration: 4.50% by mass) and 3.157 kg of an aqueous solution of potassium hydroxide (concentration: 0.5% by mass) were added over 22 hours. Furthermore, simultaneously with the addition, 18.21 kg of the prepared liquid was withdrawn from the blending tank. The addition rate of the acidic silicic acid liquid and the addition and withdrawal rates of the aqueous solution of potassium hydroxide (concentration: 0.5% by mass) at this time are shown in Table 5. After the addition and withdrawal were completed, 3.66 kg of the prepared liquid remained in the blending tank, and this solution was held at 98°C for 1 hour and then cooled to room temperature. The ratio of dry silica of the acidic silicic acid liquid during blending to dry silica of the withdrawn liquid (dry silica of acidic silicic acid liquid / dry silica of withdrawn liquid) is shown in Table 5. The prepared liquid remaining in the blending tank and the withdrawn prepared liquid were mixed until uniform. The resulting mixed liquid had a pH of 10.1, a specific surface area-equivalent particle size of 49.6 nm, and SiO 2 The concentration was 3.68% by mass. This mixture was filtered using an ultrafiltration membrane SIP-1013 manufactured by Asahi Kasei Corporation. 2 The mixture was concentrated to a concentration of 12.0% by mass.
[0122]
[0123]
Claims
1. A dispersion of silica fine particles for polishing, comprising a particle group containing silica fine particles (having a particle diameter converted into a specific surface area in the range of 5 nm to 200 nm) and satisfying the following requirements 1) to 4) dispersed in a solvent. 1) The particle group has an average sphericity in the range of 0.85 to 1.
00. 2) In the weight-converted particle size distribution of the particle group, the cumulative 10% particle size (D 10 ), cumulative 90% particle diameter (D 90 ) and cumulative 50% particle size (D 50 ) satisfies the following formula (F1). 90 -D 10 ) / D 50 ≦3.0 (F1) 3) The particle group has a weight-converted particle size distribution having a distribution peak on the large particle size side 4) The particle group contains irregularly shaped particles in a range of 0.01% by number to 10% by number.
2. The dispersion of fine silica particles for polishing according to claim 1, further satisfying the following requirement 5): 5) In the particle size distribution of the particle group consisting of the particle size / number of particles, the cumulative 1% particle size (D 1 ) to obtain the cumulative 99% particle diameter (D 99 ) is divided into six equal particle size ranges S1, S2, S3, S4, S5, and S6, and the CV value of the particle size distribution area corresponding to each particle size range is in the range of 20.0% or more and 70.0% or less.
3. A silica microparticle dispersion for polishing as described in claim 1 or claim 2, wherein in a flow potential measurement of the silica microparticle dispersion for polishing (using cationic polymeric polyethyleneimine [weight average molecular weight 600] as a titration reagent), the mass ratio of polyethyleneimine to the mass of silica at the equivalence point is in the range of 1.0 or more and 1.9 or less.
4. A method for producing a dispersion of silica fine particles for polishing, comprising the following steps 1a to 3a. (Step 1a) A step of introducing a seed particle dispersion and an alkali into a reaction vessel that is kept unheated to obtain a mixed liquid. (Step 2a) Following step 1a, the mixed liquid is stirred uniformly, then heated to 40°C to 98°C and held at the same temperature range, and then the next steps A and B are carried out simultaneously, and the reaction liquid is aged at 40°C to 98°C for 20 minutes to 120 minutes. Treatment A: A reaction liquid is prepared by continuously or intermittently adding an acidic silicic acid liquid and an alkali to the reaction vessel filled with the mixed liquid. Treatment B: A part of the reaction liquid is continuously or intermittently withdrawn from the reaction vessel. (Step 3a) A step of mixing the reaction liquid remaining in the reaction vessel at the end of step 2a with the reaction liquid withdrawn in treatment B of step 2a to obtain a dispersion of silica fine particles for polishing.
5. A method for producing a dispersion of silica fine particles for polishing according to claim 4, wherein the ratio (X / Z) of the addition rate of the acidic silicic acid liquid to the withdrawal rate of the reaction liquid is in the range of 0.2 to 3.0, where X is the addition rate [g / min] (calculated as dry silica) of the acidic silicic acid liquid and Z is the withdrawal rate [g / min] (calculated as dry silica) of the reaction liquid.
6. The addition rate [g / min] of the acidic silicic acid liquid in the step 2a is changed at least once, and the n-th addition rate is set to L n [g / min], L n+1 <L n 6. The method for producing a dispersion liquid of fine silica particles for polishing according to claim 4 or 5, which satisfies the following relationship:
7. A method for producing a dispersion of silica fine particles for polishing, comprising the following steps 1b to 4b. (Step 1b) A step of introducing an acidic silicic acid liquid and an alkali into a reaction vessel that is kept unheated to obtain a first preparation. (Step 2b) Following step 1b, a step of uniformly stirring the first preparation, then heating it to 40°C or higher and 98°C or lower, maintaining the temperature within the same range, and then continuously or intermittently adding an acidic silicic acid liquid while maintaining the temperature within the same range to obtain a second preparation. (Step 3b) Following step 2b, a step of simultaneously carrying out the following processes A and B. Process A: An acidic silicic acid liquid and an alkali are each continuously or intermittently added to the reaction vessel filled with the second preparation to prepare a reaction liquid. Process B: A part of the reaction liquid in the reaction vessel of process A is continuously or intermittently withdrawn. (Step 4b) A step of aging the reaction liquid obtained in the treatments A and B of the step 3b at a temperature in the range of 40°C to 98°C for 20 minutes to 120 minutes, and then adding and mixing the reaction liquid extracted in the treatment B of the step 3b to obtain a dispersion of silica fine particles for polishing.
8. A method for producing a dispersion of silica fine particles for polishing according to claim 7, wherein, when the addition rate [g / min] (calculated as dry silica) of the acidic silicic acid liquid in step 3b is X, and the withdrawal rate [g / min] (calculated as dry silica) of the reaction liquid is Z, the ratio (X / Z) of the addition rate of the acidic silicic acid liquid to the withdrawal rate of the reaction liquid is in the range of 0.2 to 3.
0.
9. The addition rate [g / min] of the acidic silicic acid liquid in the step 3b is changed at least once, and the addition rate for the nth time is set to L n [g / min], L n+1 <L n 9. The method for producing a dispersion liquid of fine silica particles for polishing according to claim 7 or 8, which satisfies the following relationship:
Citation Information
Patent Citations
Warty-surfaced sphere-form inorganic oxide sol, method for producing same, and abrasive containing the sol
JP2009091197A
Method for producing confetti-like silica sol
JP2010024119A
Method for producing silica sol having a controllable wide particle size distribution and minimum particle size
JP2012503586A
Silica-based particle dispersion and method for producing the same
JP2021059490A