Polymer composite thin film, gas separation body provided with polymer composite thin film, gas separation device provided with polymer composite thin film, and method for manufacturing polymer composite thin film

The combination of two polymer thin films with reinforcing materials in the polymer composite thin film addresses the energy and cost inefficiencies of existing gas separation technologies, achieving efficient gas separation with improved mechanical strength and stability.

WO2024237095A1PCT designated stage expired Publication Date: 2024-11-21NANOMEMBRANE TECHNOLOGIES INC
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2024/016718
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-05-15
Filing Date
2024-04-30
Publication Date
2024-11-21

AI Technical Summary

Technical Problem

Existing gas separation technologies, such as cryogenic distillation and pressure swing adsorption, face challenges with high energy consumption and processing costs, while polymer thin films with carbon nanotubes improve mechanical strength but risk membrane rupture due to thinning, compromising structural stability.

Method used

A polymer composite thin film is created by combining two polymer thin films with different properties and incorporating reinforcing materials like carbon nanotubes or cellulose nanofibers, achieving a balance of gas permeability and selectivity while maintaining structural integrity through a crosslinked oxyethylene chain-containing polymer layer.

Benefits of technology

The polymer composite thin film exhibits enhanced gas selectivity and permeability, enabling efficient separation of CO2 and O2 from air, reducing energy consumption and processing costs, while maintaining mechanical strength and structural stability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JP2024016718_21112024_PF_FP_ABST
    Figure JP2024016718_21112024_PF_FP_ABST
Patent Text Reader

Abstract

[Problem] To provide a polymer composite thin film that has high permeability and selectivity with respect to a prescribed gas, and that has practical structural stability, by combining two polymer thin films having different properties or furthermore combining a reinforcing material (reinforcing layer). [Solution] A polymer composite thin film 1 is configured from a first polymer thin film 2 that has selective permeability with respect to a prescribed gas, and a second polymer thin film 3 that is provided overlapping with the first polymer thin film 2 and contains at least an oxyethylene chain.
Need to check novelty before this filing date? Find Prior Art

Description

Polymer composite membrane, gas separator equipped with polymer composite membrane, gas separation device equipped with polymer composite membrane, and method for manufacturing polymer composite membrane

[0001] The present invention relates to a polymer composite thin film that mainly contains a polymer material, and in particular to a polymer composite thin film that has high functionality and significantly improved membrane strength, a gas separator and gas separation device that include this polymer composite thin film, and a method for manufacturing a polymer composite thin film.

[0002] Recently, atmospheric CO2 has been considered a factor in climate change and global warming. 2 In light of this situation, the CO concentration in the air is increasing. 2 atmospheric CO 2 so that a net reduction in concentration is achieved 2 There is a strong demand for advances in direct air capture (DAC) technology, which directly captures and safely and permanently stores airborne pollutants.

[0003] In relation to DAC, O contained in the atmosphere 2 , N 2 YaCO 2 There is known an air separation technique for separating gas components such as toluene, toluene, toluene- ...

[0004] Specifically, air separation technologies include cryogenic distillation, which cools a gas mixture at room temperature to a liquid or solid state and separates each component by distillation, pressure swing adsorption (PSA), which adsorbs a specific gas onto an adsorbent under pressurized or normal pressure, removes the non-adsorbed components, and then desorbs the adsorbed gas by reducing the pressure, and CO2 is adsorbed onto a solid adsorbent such as activated carbon or zeolite. 2 After adsorption, CO 2 A solid adsorption method for desorbing the

[0005] These methods all have the drawback of high energy consumption and high processing costs for gas separation. Gas separation using polymer membranes has been widely studied as a means of creating economically advantageous DAC or air separation technologies that, in principle, require low energy consumption.

[0006] In the field of gas separation membrane technology, a membrane for gas separation is known that includes a support layer and a selective polymer layer disposed on the support layer, where the support layer includes a gas-permeable polymer and a hydrophilic additive dispersed in the gas-permeable polymer, and the selective polymer layer includes a selective polymer matrix and carbon nanotubes dispersed in the selective polymer matrix (Patent Document 1).

[0007] Special Publication No. 2020-531260

[0008] According to the technology described in Patent Document 1, the CO 2 The transmittance is 617-807 GPU under reduced pressure, CO 2 / N 2 The selectivity is reported to be 161 to 187. Example 2A (CO 2 under reduced pressure) does not contain carbon nanotubes in the selective polymer layer. 2 The transmittance is 473 GPU, CO 2 / N 2 The difference from the previous example (selectivity ratio = 194) is believed to be due to the fact that the addition of carbon nanotubes improved the mechanical strength of the selective polymer layer, preventing it from being drawn into the pores of the support layer, which is a nanoporous substrate (see Patent Document 1 [Table 13], etc.).

[0009] However, although Patent Document 1 suggests that carbon nanotubes improve the mechanical strength of the selective polymer layer, it does not suggest that the addition of carbon nanotubes can make the selective polymer layer thinner and improve gas permeability. However, Patent Document 1 emphasizes the importance of "preventing the selective polymer layer from being drawn into the pores of the support layer," and since thinning the layer makes the selective polymer layer facing the pores more likely to be drawn into the pores, increasing the risk of membrane rupture, there is no motivation to actively try to make the layer thinner.

[0010] The present invention has been devised to solve these problems of the conventional technology, and aims to provide a polymer composite thin film that has high permeability and selectivity to a specified gas and practical structural stability (self-supporting ability) by combining two polymer thin films with different properties or by further combining (composite) a reinforcing material, a gas separator comprising the polymer composite thin film, a gas separation device comprising the polymer composite thin film, and a method for producing a polymer composite thin film.

[0011] The present invention, which has been made to solve the above-mentioned problems, provides a polymer composite thin film comprising a first polymer thin film having selective permeability to a predetermined gas, and a second polymer thin film superimposed on the first polymer thin film and containing at least an oxyethylene chain.

[0012] This makes it possible to combine two polymer thin films with different properties to obtain a polymer composite thin film that has a good balance between gas permeability and gas selectivity.

[0013] In addition, in the present invention, carbon nanotubes or cellulose nanofibers are dispersed in the second polymer thin film, which increases the mechanical strength of the second polymer thin film and makes it possible to reduce the thickness of the polymer composite thin film.

[0014] In addition, in the present invention, carbon nanotubes or cellulose nanofibers are dispersed in the first polymer thin film, which increases the mechanical strength of the first polymer thin film and makes it possible to reduce the thickness of the polymer composite thin film.

[0015] Furthermore, the present invention provides a reinforcing layer made of carbon nanotubes or cellulose nanofibers between the first polymer thin film and the second polymer thin film, which increases the mechanical strength of the polymer composite thin film including the reinforcing layer and enables the polymer composite thin film to be made thinner.

[0016] In addition, in the present invention, the second polymer thin film is composed of a crosslinked polymer containing an oxyethylene chain, which stabilizes the physical properties of the second polymer thin film and makes it possible to prevent breakage of the polymer composite thin film containing the second polymer thin film.

[0017] In addition, in the present invention, the crosslinked polymer containing oxyethylene chains is in a partially crosslinked state, which makes it possible to ensure gas permeability of the second polymer thin film.

[0018] In addition, in the present invention, the total thickness of the first polymer thin film and the second polymer thin film is set to 20 nm to 1000 nm, which makes it possible to obtain a polymer composite thin film 1 that is self-supporting and has high gas permeability and gas selectivity.

[0019] The present invention also provides a polymer composite membrane that selectively allows carbon dioxide and oxygen to permeate from air, exhaust gas, and other mixed gases, thereby enabling carbon dioxide concentration, oxygen enrichment, and nitrogen enrichment.

[0020] In addition, in the present invention, the first polymer thin film is mainly composed of polysiloxane, which makes it possible to manufacture the polymer composite thin film at lower cost using commonly available materials.

[0021] The present invention also provides a gas separator comprising a polymer composite thin film and a support for supporting the polymer composite thin film, whereby the gas separator can be constructed by superposing (transferring) the polymer composite thin film onto the support.

[0022] The present invention also provides a gas separation device comprising a gas separator and a gas supply unit that supplies gas to the gas separator, thereby making it possible to provide a gas separation device that can obtain oxygen-enriched air, carbon dioxide-enriched air, and nitrogen-enriched air.

[0023] In addition, in the present invention, the gas supply unit supplies gas so that the gas permeates through the second polymer membrane and then the first polymer membrane in this order, thereby making it possible to obtain oxygen-enriched air, carbon dioxide-enriched air, and nitrogen-enriched air using a polymer composite membrane with excellent gas selectivity.

[0024] In addition, in the present invention, the gas supply unit supplies gas so that the gas permeates through the first polymer thin film and then the second polymer thin film, thereby making it possible to produce oxygen-enriched air, carbon dioxide-enriched air, and nitrogen-enriched air with high efficiency using a polymer composite thin film with excellent gas permeability.

[0025] The present invention also provides a method for producing a polymer composite thin film, comprising: a first step of preparing an oxyethylene chain-containing polymer solution and a polymer material-containing solution containing a polymer material that has selective permeability to a predetermined gas when formed into a thin film; a second step of applying the oxyethylene chain-containing polymer solution to a substrate on which a sacrificial layer has been formed so as to cover the sacrificial layer, thereby forming a second polymer thin film; a third step of crosslinking the second polymer thin film; a fourth step of applying and curing the polymer material-containing solution so as to cover the crosslinked second polymer thin film, thereby forming a first polymer thin film; and a fifth step of dissolving the sacrificial layer and peeling off a polymer composite thin film composed of the first polymer thin film and the second polymer thin film from the substrate.

[0026] This makes it possible to manufacture a polymer composite thin film that has a good balance between gas permeability and gas selectivity by combining two polymer thin films with different properties.

[0027] Thus, according to the present invention, by combining two polymer thin films with different properties, or by further combining (composite) a reinforcing material, it is possible to obtain a polymer composite thin film that has high permeability and selectivity to a specified gas and practical structural stability (self-supporting ability), a gas separator comprising a polymer composite thin film, a gas separation device comprising a polymer composite thin film, and a method for producing a polymer composite thin film.

[0028] 1A and 1B are explanatory diagrams showing the configuration of a polymer composite thin film 1 according to a first embodiment of the present invention and a gas separator 6 including the polymer composite thin film 1; FIG. 1A is an explanatory diagram showing the configuration of a polymer composite thin film 1 according to a second embodiment of the present invention and a gas separator 6 including the polymer composite thin film 1; FIG. 1B is an explanatory diagram showing the configuration of a polymer composite thin film 1 according to a third embodiment of the present invention and a gas separator 6 including the polymer composite thin film 1; and FIG. 1C is an explanatory diagram showing the configuration of a polymer composite thin film 1 according to a fourth embodiment of the present invention and a gas separator 6 including the polymer composite thin film 1; and FIG. 1D is an explanatory diagram showing the configuration of a gas separation device 110 including a gas separator 6 according to the present invention.

[0029] 1(a) and 1(b) are explanatory diagrams showing the configuration of a polymer composite thin film 1 and a gas separator 6 including the polymer composite thin film 1 according to a first embodiment of the present invention. The gas separator 6 is composed of a polymer composite thin film 1 and a support 5. The polymer composite thin film 1 is composed of a first polymer thin film 2 having selective permeability to a predetermined gas and a second polymer thin film 3 containing at least an oxyethylene chain. The second polymer thin film 3 and the first polymer thin film 2 are both non-porous and are superimposed so as to be in contact with each other. The gas separator 6 may be configured so that the first polymer thin film 2 is in contact with the support 5 as shown in FIG. 1(a) or so that the second polymer thin film 3 is in contact with the support 5 as shown in FIG. 1(b).

[0030] Examples of materials that can be used to form the first polymer thin film 2 include vinyl polymers, polysiloxanes, and cross-linked polymers, with polydimethylsiloxane (hereinafter referred to as "PDMS") being particularly suitable. Vinyl polymers and polysiloxanes are known to have low mechanical strength and are unable to maintain their independence when used alone, especially at thicknesses of 10 nm or less. In this case, adding a reinforcing material 10 to the first polymer thin film 2, primarily composed of vinyl polymers or polysiloxanes, or overlaying a reinforcing layer 4 on the first polymer thin film 2, as described below, can achieve both functionality and independence.

[0031] On the other hand, crosslinkable polymers are considered to be self-sustaining materials even at film thicknesses (e.g., 100 nm or less) at which they can effectively exhibit their functionality. Here, a crosslinkable polymer (crosslinked polymer) refers to a polymer having a three-dimensional network structure (crosslinked structure) formed by bonding multiple linear polymer chains through a chemical reaction, and includes, for example, radical crosslinking of linear polymers and epoxy resins in which epoxy groups and amino groups as functional groups are crosslinked through a chemical reaction.

[0032] Regarding epoxy resin, an example of a self-supporting polymer thin film with a film thickness of 20 nm is published in “A Large, Freestanding, 20 nm Thick Nanomembrane Based on an Epoxy Resin,” H. Watanabe T. Kunitake, ADVANCED MATERIALS Volume 19, Issue 7, Pages 909-912, 2007 (https: / / onlinelibrary.wiley.com / doi / abs / 10.1002 / adma.200601630).

[0033] A compound containing an oxyethylene chain can be suitably used as a material for forming the second polymer thin film 3. The oxyethylene chain has gas separation properties whether it is contained in the main chain or in the side chain of the polymer. Examples of polymer materials containing an oxyethylene chain in the main chain include polyethylene glycol diacrylate (hereinafter sometimes referred to as "PEGDA"), polyethylene glycol dimethacrylate, polyethylene glycol, and poly(ethylene oxide).

[0034] Examples of polymeric materials that may be contained in side chains include poly(ethylene glycol) methyl ether acrylate (hereinafter sometimes referred to as "PEGMA") and poly(ethylene glycol) methyl ether methacrylate. The acrylates listed above are particularly preferred because they can be easily polymerized and various acrylates can be arbitrarily combined. These polymeric materials may be polymerized after mixing the materials, or each material may be polymerized and then mixed. When mixing PEGMA and PEGDA, the volume ratio of PEGMA:PEGDA is preferably in the range of 10:0 to 5:5. Compounds containing oxyethylene chains may be in any of the so-called main chain, side chain, and star-shaped configurations, and also include ethylene oxide polymers that are easily crosslinked by radical reactions.

[0035] Acrylate, a polymer raw material, can be easily polymerized by using a polymerization initiator. There are no particular limitations on the method for polymerizing, but for example, the reaction can be promoted by heating using benzoyl peroxide. Alternatively, the reaction can be promoted by irradiating light using 1-hydroxycyclohexyl phenyl ketone.

[0036] Polyallylamine, polyethyleneimine, etc. may also be added as a material constituting the second polymer thin film 3. In this case, the amount of polyallylamine, etc. added may be about 10 wt % relative to PEGMA.

[0037] The first polymer thin film 2, which is mainly made of vinyl polymer or polysiloxane, has excellent gas permeability, and the thinner the film, the higher the gas permeability. The first polymer thin film 2 also has a high permeability to a predetermined gas (CO 2 , O 2 ), but CO 2 / N 2 On the other hand, the second polymer thin film 3 containing oxyethylene chains has excellent gas separation performance (selectivity), especially for CO 2 / N 2 However, to maintain sufficient gas permeability, it is necessary to make the film as thin as possible and / or to lower the degree of cross-linking. Therefore, by combining a first polymer thin film 2 and a second polymer thin film 3, which have different properties (selectivities), (composite of two polymer layers), a polymer composite thin film 1 having both excellent gas permeability and gas selectivity can be obtained.

[0038] Here, the total thickness of the first polymer thin film 2 and the second polymer thin film 3 is about 1000 GPU. 2 From the viewpoint of ensuring transmittance, the thickness is preferably 10 nm to 2 μm, and more preferably 20 nm to 1000 nm (the same applies to the second to fourth embodiments). Note that, in the first embodiment, it is more preferable that the thickness of the first polymer thin film 2 is 30 nm or more (e.g., 120 to 1300 nm) and the thickness of the second polymer thin film 3 is 10 nm or more (e.g., 18 to 113 nm), from the viewpoint of providing the polymer composite thin film 1 with self-supporting properties as a whole.

[0039] The support 5 may be, for example, a porous polyacrylonitrile (hereinafter sometimes referred to as "PAN") layer having numerous fine pores and high gas permeability, or a composite membrane having such a layer on its outermost surface. Alternatively, an alumina sheet (product example: Anodisc) made porous by anodization may be used as the support 5. Other examples include membrane filters made of polyethersulfone, polycarbonate, polyimide, etc.

[0040] When a predetermined gas (here, air) is supplied to the gas separator 6 including the first polymer thin film 2 and the second polymer thin film 3, carbon dioxide (CO 2 ) and oxygen (O 2 ) are selectively and more permeable (the same applies to the second to fourth embodiments). 2 Effectively recover or 2 The concentration of can be increased.

[0041] The manufacturing process of the polymer composite membrane 1 and the gas separator 6 including the polymer composite membrane 1 in the first embodiment will be described below.

[0042] <Preparation> As a preparation for obtaining an oxyethylene chain-containing polymer solution, the monomer PEGMA is first polymerized. The oxyethylene chain-containing polymer is prepared by radical polymerization of PEGMA. Toluene is used as the reaction solvent, and after the polymerization reaction, a powder of polymerized PEGMA (hereinafter sometimes referred to as "P(PEGMA)") is obtained by reprecipitation using hexane and drying the precipitate.

[0043] <Step 1> Step 1 involves preparing an oxyethylene chain-containing polymer solution containing an oxyethylene chain, and preparing a polymeric material-containing solution containing a polymeric material that exhibits selective permeability to a predetermined gas when thin-filmed. Note that "preparation" in Step 1 includes preparation or procuring a commercially available product. Here, an oxyethylene chain-containing polymer solution is prepared by dissolving P(PEGMA) powder and a photopolymerization initiator in a predetermined solvent, and a PDMS preparation solution (polymeric material-containing solution) is prepared by mixing PDMS, a PDMS curing agent, and a solvent in a predetermined ratio. The photopolymerization initiator may be present in a range of 0.01 to 20 wt % relative to P(PEGMA). Examples of solvents that can be used to prepare the oxyethylene chain-containing polymer solution include ethanol, toluene, xylene, and a mixture of ethanol and water. Examples of solvents that can be used to prepare the polymeric material-containing solution include hexane, toluene, and cyclohexane.

[0044] <Second Step> The second step is a step of applying an oxyethylene chain-containing polymer solution onto the substrate on which the sacrificial layer has been formed so as to cover the sacrificial layer, thereby forming a second polymer thin film 3. First, a water-soluble polymer is applied by spin coating onto a cleaned glass substrate (hereinafter sometimes referred to as the "substrate") to form a sacrificial layer. Next, the oxyethylene chain-containing polymer solution prepared in the first step is applied by spin coating so as to cover the sacrificial layer, thereby forming the second polymer thin film 3.

[0045] <Third Step> The third step is a step of crosslinking the second polymer thin film 3. As described above, the oxyethylene chain-containing polymer solution contains a photopolymerization initiator, and crosslinking is initiated and progressed by UV (ultraviolet) irradiation. That is, the second polymer thin film 3 is composed of a crosslinked polymer containing oxyethylene chains (a polymer layer in which linear polymer chains of P(PEGMA) are crosslinked to each other).

[0046] The crosslinking was carried out in a nitrogen atmosphere (O 2 It is preferable to carry out the process in an atmosphere free from O. 2 In this case, polymerization inhibition due to the crosslinking reaction can be prevented. It is also preferable to control the UV irradiation time (or energy) to stop the crosslinking reaction when the second polymer thin film 3 is in a rubbery state (i.e., when the entropy elasticity is maintained or when functional groups contributing to the crosslinking reaction remain in the second polymer thin film 3). In this case, the crosslinked polymer containing oxyethylene chains constitutes the second polymer thin film 3 in a partially crosslinked state.

[0047] By making the second polymer thin film 3 rubbery, dissolution of the second polymer thin film 3 in water is suppressed when the polymer composite thin film 1 is separated from the substrate in the fifth step described below. That is, by crosslinking P(PEGMA) molecules together, the physical properties of the second polymer thin film 3 are stabilized, and it becomes possible to produce a polymer composite thin film 1 including the second polymer thin film 3 without breakage or the like. Furthermore, by stopping the progress of crosslinking in the rubbery state (making it partially crosslinked), it becomes possible to ensure the gas permeability of the second polymer thin film 3.

[0048] <Fourth Step> The fourth step is a step of applying and curing a PDMS preparation solution, i.e., a polymer material-containing solution, so as to cover the cross-linked second polymer thin film 3, thereby forming the first polymer thin film 2. The polymer material-containing solution (PDMS preparation solution) prepared in the first step is applied by spin coating so as to cover the cross-linked second polymer thin film 3, and then cured.

[0049] <Fifth Step> The fifth step is a step of dissolving the sacrificial layer and peeling off the polymer composite thin film 1 composed of the first polymer thin film 2 and the second polymer thin film 3 from the substrate. Through the steps described above, the sacrificial layer, the second polymer thin film 3, and the first polymer thin film 2 are formed on the substrate in that order from the side closest to the substrate. The substrate on which the polymer composite thin film 1 is formed is immersed in water, and the sacrificial layer is dissolved in water, thereby peeling off the polymer composite thin film 1 from the substrate.

[0050] The polymer composite thin film 1 peeled from the substrate is then transferred to a support 5 to obtain a gas separator 6. When transferring, the configuration shown in Fig. 1(a) or the configuration shown in Fig. 1(b) can be selected. As will be described later, the gas separation characteristics of the gas separator 6 differ depending on whether the gas is permeated from the first polymer thin film 2 to the second polymer thin film 3 or the second polymer thin film 3 to the first polymer thin film 2. Users can select the configuration of the gas separator 6 depending on the required characteristics.

[0051] According to the above process, first, an oxyethylene chain-containing polymer solution was prepared by dissolving P(PEGMA) in ethanol so that the content thereof was 0.05 g / mL and the content thereof was 0.0005 g / mL.

[0052] A PDMS preparation solution (polymer material-containing solution) was prepared by dissolving polydimethylsiloxane, hydroxyl-terminated (PDMS) in hexane so that the content was 0.038 g / mL, the content of trimethoxy(methyl)silane was 0.0016 g / mL, and the content of diisopropoxybis(ethylacetoacetate)titanium was 0.0008 g / mL.

[0053] The oxyethylene chain-containing polymer solution prepared by the above-mentioned procedure was applied by spin coating (3000 rpm / 1 minute) onto a substrate on which a layer (sacrificial layer) of sodium polystyrene sulfonate (hereinafter sometimes referred to as "PSS") had been formed. 2 The substrate was left to stand in the atmosphere for 30 minutes, and then irradiated with UV light in the same atmosphere to form a second polymer thin film 3.

[0054] Next, the PDMS preparation solution prepared by the above-described procedure was applied by spin coating (3000 rpm / 1 minute) so as to cover the second polymer thin film 3. Thereafter, the substrate was left standing in the air for one day to harden the PDMS and form the first polymer thin film 2.

[0055] Next, the substrate was immersed in water to dissolve the sacrificial layer and peel off the polymer composite thin film 1 from the substrate. Then, the polymer composite thin film 1 was transferred to the support 5 in such a manner that the first polymer thin film 2 of the polymer composite thin film 1 was in contact with the support 5, thereby obtaining a gas separator 6.

[0056] A polymer composite thin film 1 and a gas separator 6 were prepared under the same conditions as in Example 1, except that an oxyethylene chain-containing polymer solution was used in which the P(PEGMA) content was 0.04 g / mL and the photopolymerization initiator content was 0.0004 g / mL.

[0057] A polymer composite thin film 1 and a gas separator 6 were prepared under the same conditions as in Example 1, except that an oxyethylene chain-containing polymer solution was used in which the P(PEGMA) content was 0.03 g / mL and the photopolymerization initiator content was 0.0003 g / mL.

[0058] A polymer composite thin film 1 and a gas separator 6 were prepared under the same conditions as in Example 1, except that an oxyethylene chain-containing polymer solution with a P(PEGMA) content of 0.005 g / mL and a photopolymerization initiator content of 0.00005 g / mL and a PDMS preparation solution with a PDMS content of 0.076 g / mL were used.

[0059] A polymer composite thin film 1 and a gas separator 6 were prepared under the same conditions as in Example 1, except that an oxyethylene chain-containing polymer solution with a P(PEGMA) content of 0.005 g / mL and a photopolymerization initiator content of 0.00005 g / mL and a PDMS preparation solution with a PDMS content of 0.114 g / mL were used.

[0060] A polymer composite thin film 1 and a gas separator 6 were produced under the same conditions as in Example 1, except that an oxyethylene chain-containing polymer solution with a P(PEGMA) content of 0.01 g / mL and a photopolymerization initiator content of 0.0001 g / mL and a PDMS preparation solution with a PDMS content of 0.2 g / mL were used (Comparative Example).

[0061] A comparative example will be described below. A PDMS preparation solution was obtained in the same manner as in Example 1. 2 After plasma cleaning, a sacrificial layer was formed by spin-coating (3000 rpm / 1 minute) an aqueous solution of PSS (15 wt %) onto the substrate, and then the substrate was dried by heating.

[0062] Next, the PDMS preparation solution was applied by spin coating (3000 rpm / 1 minute) so as to cover the sacrificial layer. The substrate was then left to stand in the air for one day to harden the PDMS. Next, the substrate was immersed in water to dissolve the sacrificial layer and peel the polymer thin film from the substrate. The PDMS thin film was then transferred to a support 5 to obtain a gas separator 6. The polymer thin film of the comparative example may be referred to as a "PDMS thin film" hereinafter. The PDMS thin film corresponds to the first polymer thin film 2 described above.

[0063] Table 1 below shows the presence or absence of self-supporting ability, the thickness of the first polymer thin film 2, the thickness of the second polymer thin film 3, and the CO 2 Transparency, N 2 Transparency, O 2 Permeability, selectivity CO 2 / N 2 , O 2 / N 2 , CO 2 / O 2The film thicknesses of the first polymer thin film 2 and the second polymer thin film 3 are the results of observing the cross section of the polymer composite thin film 1 with a scanning electron microscope (SEM) after preparing multiple gas separators 6 under the same conditions, and the gas permeability is the result of a gas permeability test in which gas is passed through the gas separator 6 in the order of the second polymer thin film 3 and then the first polymer thin film 2 (the same applies to [Table 3], [Table 4], and [Table 5]). Here, 1 GPU = 3.35 x 10 -10 mol・m -2 ・s -1 ・Pa -1 is.

[0064] The gas permeability test is specifically conducted using CO 2 Gas, N 2 gas, and O 2 The gases were individually supplied to the gas separator 6, and the membrane area was 0.785 cm 2 The volume of the liquid that permeated the second polymer thin film 3 and the first polymer thin film 2 was measured by a soap film flowmeter.

[0065]

[0066] As shown in Table 1, the polymer composite thin film 1 of Examples 1 to 6 and the comparative example all possess self-supporting properties. The presence or absence of self-supporting properties was determined based on whether or not the thin film (film) can maintain its flat membrane shape without rupture or the like when it is peeled from the substrate in a stripping solution and then lifted up into the air while floating in the solution. That is, a film that maintains its membrane structure without rupture even in the air is judged to be "self-supporting," whereas a film that maintains its membrane structure while floating in the stripping solution after peeling but easily ruptures when taken out into the air is judged to be "not self-supporting."

[0067] In Examples 1 to 3, the thickness of the first polymer thin film 2 containing PDMS is almost the same as that of the PDMS thin film of the comparative example, and it can be considered that the second polymer thin film 3 is superimposed on the PDMS thin film of the comparative example. The thinner the second polymer thin film 3, the higher the gas permeability. However, by superimposing the second polymer thin film 3 on the first polymer thin film 2, the thickness of the polymer composite thin film 1 also increases, which results in a decrease in CO 2 , N2 , O 2 The permeability is lower than that of the comparative example. 2 / N 2 is significantly improved compared to the comparative example, and O 2 / N 2 is also found to be improved.

[0068] Furthermore, P(PEGMA), i.e., the second polymer thin film 3 containing oxyethylene chains, is very soft and fragile when used alone. However, as shown in Examples 4 to 6, by overlapping it with the first polymer thin film 2, the second polymer thin film 3 can be made very thin (20 nm or less). This ensures the self-supporting properties of the entire membrane, enabling it to exhibit high gas selectivity.

[0069] A polymer composite thin film 1 and a gas separator 6 were prepared under the same conditions as in Example 1, except that an oxyethylene chain-containing polymer solution with a P(PEGMA) content of 0.03 g / mL and a photopolymerization initiator content of 0.0003 g / mL and a PDMS preparation solution with a PDMS content of 0.076 g / mL were used.

[0070] A polymer composite thin film 1 and a gas separator 6 were prepared under the same conditions as in Example 1, except that an oxyethylene chain-containing polymer solution with a P(PEGMA) content of 0.03 g / mL and a photopolymerization initiator content of 0.0003 g / mL and a PDMS preparation solution with a PDMS content of 0.114 g / mL were used.

[0071] A gas separator 6 was prepared under the same conditions as in Example 7, except that the polymer composite thin film 1 was transferred to the support 5 in such a manner that the second polymer thin film 3 of the polymer composite thin film 1 was in contact with the support 5.

[0072] A gas separator 6 was prepared under the same conditions as in Example 8, except that the polymer composite thin film 1 was transferred to the support 5 in such a manner that the second polymer thin film 3 of the polymer composite thin film 1 was in contact with the support 5.

[0073] Table 2 below shows the results of Examples 7 to 10 regarding the presence or absence of self-supporting ability, the thickness of the first polymer thin film 2, the thickness of the second polymer thin film 3, and the CO 2 Transparency, N 2 Transparency, O2 Permeability, selectivity CO 2 / N 2 , O 2 / N 2 , CO 2 / O 2 Shows.

[0074]

[0075] Here, the gas permeability test results are shown for Examples 7 and 8, in which the second polymer thin film 3 is in contact with the support 5, in which the gas is allowed to permeate from the second polymer thin film 3 to the first polymer thin film 2 (see FIG. 1(a)), and for Examples 9 and 10, in which the first polymer thin film 2 is in contact with the support 5, in which the gas is allowed to permeate from the first polymer thin film 2 to the second polymer thin film 3 (see FIG. 1(b)). Table 2 shows that when the gas is allowed to permeate from the second polymer thin film 3 to the first polymer thin film 2, the gas selectivity is superior, while when the gas is allowed to permeate from the first polymer thin film 2 to the second polymer thin film 3, the gas permeability is superior.

[0076] Second Embodiment Fig. 2(a) is an explanatory diagram showing the configuration of a polymer composite thin film 1 and a gas separator 6 including the polymer composite thin film 1 according to a second embodiment of the present invention. In the second embodiment, the components of the gas separator 6 are the same as those in the first embodiment, but the second embodiment differs from the first embodiment in that a reinforcing material 10 is dispersed in the second polymer thin film 3. Here, carbon nanotubes 11 and cellulose nanofibers 12 can be suitably used as the reinforcing material 10. Carbon nanotubes 11 and cellulose nanofibers 12 are high in mechanical strength as materials, and the second polymer thin film 3 in which they are dispersed exhibits high mechanical strength.

[0077] The carbon nanotubes 11 may be either single-walled carbon nanotubes (SWNT) or multi-walled carbon nanotubes (MWNT) (hereinafter, these may be collectively referred to as "CNT"). CNTs can form a tube network due to their high aspect ratio (SWNT: diameter 0.5 to 3 nm, length up to 10 μm, MWNT: diameter 5 to 100 nm, length up to 20 μm), and their mechanical properties are obtained by a combination of stiffness, strength, and tensile strength.

[0078] The cellulose nanofibers 12 include oxidized cellulose nanofibers, and a mixture of cellulose nanofibers 12 and oxidized cellulose nanofibers (hereinafter, these may be collectively referred to as "CNF") may also be used as the organic polymer. CNF forms fibrils, which are small fibers (fibrous structures). Fibrils have high mechanical strength as a material, and dispersing the reinforcing material 10 made of CNF in the second polymer thin film 3 results in extremely high overall mechanical strength. Furthermore, CNF can be produced at low cost by mechanical defibration from abundant resources such as wood, and as a plant fiber, it is an environmentally friendly material.

[0079] The CNTs and CNFs preferably have a diameter smaller than the thickness of the polymer composite thin film 1 (e.g., up to 200 nm), more preferably smaller than the thickness of the second polymer thin film 3 in the first embodiment described above (e.g., up to 70 nm), and even more preferably smaller than the thickness of the second polymer thin film 3 in the second embodiment (e.g., up to 35 nm). By selecting CNTs and CNFs with a diameter smaller than the thickness of the polymer composite thin film 1, the mechanical strength can be improved and the functionality (here, gas permeability and gas selectivity) of the polymer composite thin film 1 as a whole can be exhibited. Furthermore, by using CNTs and CNFs with a diameter smaller than the thickness of the second polymer thin film 3 (or first polymer thin film 2), the functionality of the second polymer thin film 3 (first polymer thin film 2) can be fully exhibited (the same applies to the third and fourth embodiments).

[0080] In Figure 2(a) (and also in Figures 2(b) and 2(c)), the reinforcing material 10 having the same fiber length is depicted as being aligned in a specific direction, but this is merely a schematic depiction. The CNTs and CNFs vary in length, and are oriented in all directions, forming an entangled network (tube network or fiber network) that is contained in the second polymer thin film 3 (the first polymer thin film 2 in Figure 2(b) and the reinforcing layer 4 in Figure 2(c) (hereinafter, these may be collectively referred to as "thin film / layer"). However, by adjusting the amount of CNTs and CNFs added, the distribution of CNTs and CNFs is limited (controlled) so that the network density in the thin film / layer is extremely sparse. This prevents a decrease in the functionality (particularly permeability) of the polymer composite thin film 1.

[0081] In a sparse network, a first region A1 where multiple reinforcing materials 10 are present, a second region A2 where a single reinforcing material 10 is present, and a third region A3 where no reinforcing material 10 is present are mixed in the thickness direction of the thin film / layer within the plane A. This can also be said to have a region in the thickness direction of the thin film / layer where multiple reinforcing materials 10 do not overlap each other. Furthermore, when the area of ​​the first region A1 is S1, the area of ​​the second region A2 is S2, and the area of ​​the third region A3 is S3, the thin film / layer is configured so that S1 < S2 < S3. Here, if the proportion of S3 in the plane A is defined as the void ratio, the void ratio is preferably greater than 90%.

[0082] The following describes the steps for producing the polymer composite thin film 1 and the gas separator 6 including the polymer composite thin film 1 in the second embodiment. <First Step> This is a step of preparing an oxyethylene chain-containing polymer-reinforcing material-containing solution containing an oxyethylene chain-containing polymer and a reinforcing material 10, and preparing a polymer material-containing solution containing a polymer material that has selective permeability to a predetermined gas when formed into a thin film.

[0083] As in the first step of the first embodiment, a photopolymerization initiator is added to P(PEGMA) powder in an amount of 1 wt % relative to the P(PEGMA), and this is dissolved in a predetermined amount of ethanol to prepare an oxyethylene chain-containing polymer solution. When carbon nanotubes 11 are used as the reinforcing material 10, the carbon nanotubes 11 are dispersed in ethanol to prepare a CNT dispersion liquid.

[0084] On the other hand, when cellulose nanofibers 12 are used as the reinforcing material 10, the cellulose nanofibers 12 are dispersed in ethanol to prepare a CNF dispersion. At this time, it is preferable to prepare the CNF dispersion so as not to contain aggregates that may cause damage to the thin film during production.

[0085] The above-described oxyethylene chain-containing polymer solution is mixed with a CNT dispersion or a CNF dispersion to prepare an oxyethylene chain-containing polymer-reinforcement-containing solution containing an oxyethylene chain-containing polymer and a reinforcing material 10. Note that the "step of preparing a polymer material-containing solution containing a polymer material that has selective permeability to a predetermined gas when formed into a thin film" is the same as the first step described in the first embodiment, and therefore a description thereof will be omitted.

[0086] <Second Step> The second step is a step of forming a second polymer thin film 3 by applying a solution containing an oxyethylene chain-containing polymer and a reinforcing material onto the substrate on which the sacrificial layer has been formed so as to cover the sacrificial layer. As in the second step of the first embodiment, a sacrificial layer made of PSS is formed on the substrate. Next, the solution containing an oxyethylene chain-containing polymer and a reinforcing material prepared in the first step is applied so as to cover the sacrificial layer, thereby forming the second polymer thin film 3. Thereafter, the second polymer thin film 3 is heated under N 2 Leave it in the atmosphere.

[0087] By using spin coating when applying the oxyethylene chain-containing polymer-reinforcing material-containing solution, a strong external force acts on the reinforcing material 10 contained in the solution, and the carbon nanotubes 11 or cellulose nanofibers 12 contained in the reinforcing material 10 are unable to form a three-dimensional tube (fiber) network, i.e., in the thickness direction of the film. As a result, the reinforcing material 10 is swept away by the solvent (ethanol in this case) and arranged on a plane, forming a substantially two-dimensional tube (fiber) network (the sparse network described above).

[0088] <Steps 3 to 5> Step 3 is a step of crosslinking the second polymer thin film 3. Step 4 is a step of applying and curing a polymer material-containing solution so as to cover the crosslinked second polymer thin film 3, thereby forming the first polymer thin film 2. Step 5 is a step of dissolving the sacrificial layer and peeling the polymer composite thin film 1, which is composed of the first polymer thin film 2 and the second polymer thin film 3, from the substrate. These steps are similar to steps 3 to 5 described in the first embodiment, and therefore will not be described again. The polymer composite thin film 1 peeled from the substrate is then transferred to a support 5, thereby obtaining a gas separator 6. As described in the first embodiment, the first polymer thin film 2 may be configured to contact the support 5 during transfer, or the second polymer thin film 3 may be configured to contact the support 5.

[0089] 1 g of P(PEGMA) powder and 0.01 g of photopolymerization initiator were dissolved in ethanol to prepare an oxyethylene chain-containing polymer solution with a P(PEGMA) content of 0.01 g / mL and a photopolymerization initiator content of 0.0001 g / mL. Furthermore, a CNT dispersion was added to the oxyethylene chain-containing polymer solution to prepare an oxyethylene chain-containing polymer-reinforcement material-containing solution containing 0.00003 g / mL of carbon nanotubes 11. Separately, a PDMS preparation solution was prepared in the same manner as in Example 1.

[0090] Next, a sacrificial layer was formed on the substrate using PSS in the same manner as in Example 1. Furthermore, the oxyethylene chain-containing polymer-reinforcing material-containing solution prepared by the above-mentioned procedure was applied by spin coating onto the substrate on which the sacrificial layer had been formed. The substrate on which the oxyethylene chain-containing polymer-reinforcing material-containing solution had been applied was then heated at 2000 K for 1 hour. 2 The mixture was left standing in the atmosphere for 30 minutes.

[0091] Thereafter, UV irradiation was carried out in the same atmosphere to crosslink the oxyethylene chain-containing polymer-reinforcing material-containing layer, thereby forming a second polymer thin film 3. In Example 4, the UV irradiation time was also controlled to stop the progress of crosslinking when the second polymer thin film 3 was in a rubbery state.

[0092] Next, the PDMS preparation solution prepared by the above-described procedure was applied by spin coating (3000 rpm / 1 minute) so as to cover the second polymer thin film 3. Thereafter, the substrate was left standing in the air for one day to harden the PDMS and form the first polymer thin film 2.

[0093] Next, the substrate was immersed in water to dissolve the sacrificial layer and peel off the polymer composite thin film 1. Then, similar to Example 1, the polymer composite thin film 1 was transferred to the support 5 in such a manner that the first polymer thin film 2 of the polymer composite thin film 1 was in contact with the support 5, thereby obtaining a gas separator 6.

[0094] A polymer composite membrane 1 and a gas separator 6 were produced under the same conditions as in Example 11, except that a solution containing an oxyethylene chain-containing polymer and a reinforcing material containing 0.000015 g / mL of carbon nanotubes 11 was used.

[0095] A polymer composite thin film 1 and a gas separator 6 were produced under the same conditions as in Example 11, except that a solution containing an oxyethylene chain-containing polymer and a reinforcing material, containing 0.0000039 g / mL of carbon nanotubes 11, was used.

[0096] An oxyethylene chain-containing polymer solution was prepared by dissolving 0.5 g of P(PEGMA) powder and 0.005 g of photopolymerization initiator in ethanol, resulting in a P(PEGMA) concentration of 0.03 g / mL and a photopolymerization initiator content of 0.0003 g / mL. Furthermore, a CNF dispersion was added to the oxyethylene chain-containing polymer solution to prepare an oxyethylene chain-containing polymer-reinforcement material-containing solution containing 0.00024 g / mL of cellulose nanofibers 12. Separately, a PDMS preparation solution was prepared in the same manner as in Example 1.

[0097] Next, a sacrificial layer was formed on the substrate using PSS in the same manner as in Example 1, and a second polymer thin film 3 was formed on the sacrificial layer using an oxyethylene chain-containing polymer-reinforcement-containing solution in the same manner as in Example 11, and the progress of crosslinking was stopped in the rubber state. Furthermore, a first polymer thin film 2 was formed using a PDMS preparation solution so as to cover the second polymer thin film 3. Next, a polymer composite thin film 1 composed of the second polymer thin film 3 and the first polymer thin film 2 was peeled off from the sacrificial layer. The polymer composite thin film 1 was then transferred to a support 5 in the same manner as in Example 1, and a gas separator 6 was obtained.

[0098] Table 3 below shows the results of Examples 11 to 14 regarding the presence or absence of self-supporting ability, the thickness of the first polymer thin film 2, the thickness of the second polymer thin film 3, the amount of reinforcing material 10 added to the second polymer thin film 3, the amount of reinforcing material 10 added, and the CO 2 Transparency, N 2 Transparency, O 2 Permeability, selectivity CO 2 / N 2 , O 2 / N 2 , CO 2 / O 2 Table 3 also shows data for comparative examples.

[0099] As shown in Table 3, the polymer composite thin films 1 of Examples 11 to 14 are all self-supporting. In all cases, the thickness of the first polymer thin film 2 containing PDMS is approximately the same as that of the PDMS thin film of the comparative example, and the polymer composite thin films 1 of Examples 11 to 14 can be considered to be constructed by superimposing the second polymer thin film 3 containing the reinforcing material 10 on the PDMS thin film of the comparative example.

[0100] By superposing the second polymer thin film 3 on the first polymer thin film 2, the total film thickness also increases. 2 , N 2 , O 2 On the other hand, in Examples 12 and 13, the CO 2 The permeability exceeds 10,000 GPU, a value comparable to that of the comparative example. 2 / N 2 is significantly improved compared to the comparative example, and O 2 / N 2 is also found to be improved.

[0101] Here, in Examples 11 to 13, carbon nanotubes 11 were added to the second polymer thin film 3. Comparing this with Examples 1 to 3 (in which the second polymer thin film 3 did not include a reinforcing material 10), the film thickness of the second polymer thin film 3 in Examples 11 to 13 was 38 nm, while the film thickness of the second polymer thin film 3 in Examples 1 to 3 was 113 nm to 74 nm. That is, in Examples 11 to 13, the addition of carbon nanotubes 11 as the reinforcing material 10 to the second polymer thin film 3 improved the mechanical strength, and it became possible to configure the second polymer thin film 3 (and consequently the polymer composite thin film 1) thinner.

[0102] In Example 14, cellulose nanofibers 12 were added to the second polymer thin film 3. The thickness of the second polymer thin film 3 in Example 14 was 74 nm, which was the same as the thickness of the second polymer thin film 3 in Example 3. The cellulose nanofibers 12 added to the second polymer thin film 3 functioned as a barrier, preventing CO 2 Although it is thought that the permeability will decrease (5459 GPU in Example 3 and 3586 GPU in Example 14), it is clear that the cellulose nanofibers 12 improve the mechanical strength of the second polymer thin film 3, and the configuration of Example 14 can be suitably used, for example, in cases where there is a large difference in air pressure between the upstream and downstream sides of the gas separator 6.

[0103] Third Embodiment FIG. 2( b ) is an explanatory diagram showing the configuration of a polymer composite thin film 1 and a gas separator 6 including the polymer composite thin film 1 according to a third embodiment of the present invention. In the third embodiment, the components of the gas separator 6 are the same as those in the first embodiment. However, the third embodiment differs from the first and second embodiments in that a reinforcing material 10 is dispersed in the first polymer thin film 2. As in the second embodiment, CNTs and CNFs can be suitably used as the reinforcing material 10. The first polymer thin film 2 having dispersed CNTs or CNFs exhibits extremely high mechanical strength. In particular, by selecting CNTs or CNFs with a diameter smaller than the thickness of the first polymer thin film 2, the functionality of the first polymer thin film 2 can be fully exhibited. In the first polymer thin film 2, the reinforcing material 10 also forms the aforementioned sparse network.

[0104] Hereinafter, a description will be given of the manufacturing process of the polymer composite thin film 1 and the gas separator 6 including the polymer composite thin film 1 in the third embodiment. <First Step> This is a step of preparing an oxyethylene chain-containing polymer solution containing oxyethylene chains, and preparing a polymer material-reinforcement material-containing solution containing a polymer material that has selective permeability to a predetermined gas when formed into a thin film and a reinforcing material 10.

[0105] As in the first step of the first embodiment, a photopolymerization initiator is added to P(PEGMA) powder in an amount of 1 wt % relative to P(PEGMA), and this is dissolved in a predetermined amount of ethanol to prepare an oxyethylene chain-containing polymer solution.

[0106] A CNT dispersion (or CNF dispersion) and a polymer material-containing solution (PDMS preparation solution) are prepared in the same manner as in the second embodiment. The polymer material-containing solution is mixed with the CNT dispersion or CNF dispersion to prepare a polymer material-reinforcement material-containing solution containing a polymer material (here, PDMS) and the reinforcing material 10.

[0107] <Second Step and Third Step> The second step is a step of applying an oxyethylene chain-containing polymer solution onto the substrate on which the sacrificial layer has been formed so as to cover the sacrificial layer, thereby forming a second polymer thin film 3. The third step is a step of crosslinking the second polymer thin film 3. The second and third steps are the same as those in the first embodiment, and therefore a description thereof will be omitted.

[0108] <Fourth Step> This is a step of applying and curing a solution containing a polymer material and a reinforcing material so as to cover the crosslinked second polymer thin film 3, thereby forming the first polymer thin film 2. The solution containing a polymer material and a reinforcing material prepared in the first step is applied so as to cover the crosslinked second polymer thin film 3. Thereafter, the first polymer thin film 2 is allowed to stand in the atmosphere for one day to cure.

[0109] <Fifth Step> This is a step of dissolving the sacrificial layer and peeling off the polymer composite thin film 1 composed of the first polymer thin film 2 and the second polymer thin film 3 from the substrate. Since the fifth step is the same as in the first embodiment, a description thereof will be omitted. The polymer composite thin film 1 peeled off from the substrate is transferred to a support 5, thereby obtaining a gas separator 6.

[0110] An oxyethylene chain-containing polymer solution was prepared with a P(PEGMA) content of 0.01 g / mL and a photopolymerization initiator content of 0.0001 g / mL in the same manner as in Example 11. Separately, a PDMS preparation solution was prepared in the same manner as in Example 1. Furthermore, a CNT dispersion was added to the PDMS preparation solution to prepare a polymer material-reinforcement material-containing solution containing 0.000015 g / mL of carbon nanotubes 11.

[0111] Next, a sacrificial layer was formed on the substrate using PSS in the same manner as in Example 1. Furthermore, the oxyethylene chain-containing polymer solution prepared by the above-mentioned operation was applied by spin coating onto the substrate on which the sacrificial layer was formed. The substrate on which the oxyethylene chain-containing polymer solution was applied was then heated at 2000 K for 1 hour. 2 The substrate was left to stand in the atmosphere for 30 minutes, and then irradiated with UV light in the same atmosphere to crosslink the oxyethylene chain-containing polymer, thereby forming a second polymer thin film 3.

[0112] Next, the polymer material-reinforcement material-containing solution prepared by the above-described procedure was applied by spin coating (3000 rpm / 1 minute) so as to cover the second polymer thin film 3. Thereafter, the substrate was left standing in the air for one day, and the polymer material-reinforcement material-containing solution was cured to form the first polymer thin film 2. Next, the substrate was immersed in water to dissolve the sacrificial layer and peel the polymer composite thin film 1 from the substrate. The polymer composite thin film 1 was then placed on a support 5 in the same manner as in Example 1, to obtain a gas separator 6.

[0113] An oxyethylene chain-containing polymer solution was prepared in the same manner as in Example 3, with a P(PEGMA) content of 0.03 g / mL and a photopolymerization initiator content of 0.0003 g / mL. Separately, a PDMS preparation solution was prepared in the same manner as in Example 1. Furthermore, a CNF dispersion was added to the PDMS preparation solution to prepare a polymer material-reinforcement material-containing solution containing 0.0000004 g / mL of cellulose nanofibers 12. Other conditions were the same as in Example 15, and a polymer composite thin film 1 and a gas separator 6 were obtained.

[0114] A polymer composite membrane 1 and a gas separator 6 were obtained in the same manner as in Example 16, except that an oxyethylene chain-containing polymer solution having a P(PEGMA) content of 0.01 g / mL and a photopolymerization initiator content of 0.0001 g / mL was used as the oxyethylene chain-containing polymer solution.

[0115] Table 4 below shows the results of Examples 15 to 17, including the presence or absence of self-supporting ability, the thickness of the first polymer thin film 2, the thickness of the second polymer thin film 3, the amount of reinforcing material 10 added to the first polymer thin film 2, the amount of reinforcing material 10 added, and the CO 2 Transparency, N 2 Transparency, O 2 Permeability, selectivity CO 2 / N 2 , O 2 / N 2 , CO 2 / O 2 Table 4 also shows data for comparative examples.

[0116] As shown in Table 4, the polymer composite thin films 1 of Examples 15 to 17 all have self-supporting properties. In all cases, the thickness of the first polymer thin film 2 containing PDMS is approximately the same as that of the PDMS thin film of the comparative example, and the polymer composite thin films 1 of Examples 15 to 17 can be considered to be structurally the PDMS thin film of the comparative example to which the reinforcing material 10 has been added, with the second polymer thin film 3 superimposed thereon.

[0117] By superposing the second polymer thin film 3 on the first polymer thin film 2 containing PDMS and the reinforcing material 10, the overall film thickness also increases.2 , N 2 , O 2 The permeability is lower than that of the comparative example. 2 / N 2 is significantly improved compared to the comparative example, and O 2 / N 2 is also found to be improved.

[0118] Here, in Example 15, carbon nanotubes 11 were added to the first polymer thin film 2, and in Example 17, cellulose nanofibers 12 were added to the first polymer thin film 2. Compared with Examples 1 to 3 (in which the first polymer thin film 2 did not include a reinforcing material 10), the film thickness of the second polymer thin film 3 in Examples 15 and 17 was 38 nm, and the film thickness of the second polymer thin film 3 in Examples 1 to 3 was 113 nm to 74 nm. That is, in Examples 15 and 17, the second polymer thin film 3 was supported by the first polymer thin film 2 including the reinforcing material 10, thereby improving the overall mechanical strength and enabling the second polymer thin film 3 (and consequently the polymer composite thin film 1) to be configured thinner.

[0119] Fourth Embodiment FIG. 2( c ) is an explanatory diagram showing the configuration of a polymer composite thin film 1 and a gas separator 6 including the polymer composite thin film 1 according to a fourth embodiment of the present invention. In the fourth embodiment, the gas separator 6 is composed of a polymer composite thin film 1 and a support 5. The polymer composite thin film 1 is composed of a first polymer thin film 2, a reinforcing layer 4, and a second polymer thin film 3, with the reinforcing layer 4 being disposed between the first polymer thin film 2 and the second polymer thin film 3. The reinforcing layer 4 is composed of a reinforcing material 10 such as carbon nanotubes 11 and cellulose nanofibers 12. That is, the fourth embodiment differs from the previous embodiments in that the reinforcing layer 4 composed of the reinforcing material 10 is provided independently. Carbon nanotubes 11 and cellulose nanofibers 12 have high mechanical strength, and the reinforcing layer 4 composed of these materials exhibits extremely high mechanical strength, thereby improving the overall strength of the polymer composite thin film 1. In the reinforcing layer 4, the reinforcing material 10 also forms the aforementioned sparse network.

[0120] In the fourth embodiment, the configurations of the first polymer thin film 2, the second polymer thin film 3, and the support 5 are the same as in the first embodiment, so a description thereof will be omitted. Hereinafter, a manufacturing process for the polymer composite thin film 1 and the gas separator 6 including the polymer composite thin film 1 in the fourth embodiment will be described. <First Step> This is a step of preparing a reinforcing material dispersion liquid containing a reinforcing material 10, an oxyethylene chain-containing polymer solution containing an oxyethylene chain, and a polymer material-containing solution containing a polymer material that has selective permeability to a predetermined gas when formed into a thin film.

[0121] As in the first step of the first embodiment, a photopolymerization initiator (1 wt % relative to the P(PEGMA)) is added to P(PEGMA) powder, and this is dissolved in a predetermined amount of ethanol to prepare an oxyethylene chain-containing polymer solution. As in the second embodiment, a CNT dispersion or a CNF dispersion (hereinafter, these may be collectively referred to as "reinforcement material dispersion") and a polymer material-containing solution (PDMS preparation solution) are prepared.

[0122] <Second Step and Third Step> The second step is a step of applying an oxyethylene chain-containing polymer solution onto the substrate on which the sacrificial layer has been formed so as to cover the sacrificial layer, thereby forming a second polymer thin film 3. The third step is a step of crosslinking the second polymer thin film 3. The second and third steps are the same as those in the first embodiment, and therefore a description thereof will be omitted.

[0123] <Fourth Step> This is a step of applying a reinforcing material dispersion to cover the cross-linked second polymer thin film 3 to form a reinforcing layer 4. When forming the reinforcing layer 4, the reinforcing material dispersion prepared in the first step is applied to cover the cross-linked second polymer thin film 3.

[0124] <Step 5> This is a step of applying and curing a polymer material-containing solution so as to cover the reinforcing layer 4, thereby forming the first polymer thin film 2. The polymer material-containing solution (PDMS preparation solution) prepared in Step 1 is applied so as to cover the reinforcing layer 4, thereby forming the first polymer thin film 2. Thereafter, the first polymer thin film 2 is left to stand in the atmosphere for one day, and the first polymer thin film 2 is cured.

[0125] <Sixth Step> This is a step of dissolving the sacrificial layer to peel the polymer composite thin film 1 from the substrate. The substrate is formed with the sacrificial layer, second polymer thin film 3, reinforcing layer 4, and first polymer thin film 2 in order from the substrate's closest, which together constitute the polymer composite thin film 1. The substrate is immersed in water to dissolve the sacrificial layer in the water, thereby peeling the polymer composite thin film 1 from the substrate. The polymer composite thin film 1 peeled from the substrate is then transferred to a support 5, thereby obtaining a gas separator 6.

[0126] In the fourth embodiment, the reinforcing layer 4 may be formed after forming a sacrificial layer (fourth step), and then the second polymer thin film 3 may be formed and crosslinked by applying an oxyethylene chain-containing polymer solution so as to cover the reinforcing layer 4 (second and third steps), and then the first polymer thin film 2 may be formed by applying a PDMS preparation solution so as to cover the second polymer thin film 3 (fifth step), thereby producing the polymer composite thin film 1. The gas separator 6 may then be configured so that the reinforcing layer 4 and the support 5 constituting the polymer composite thin film 1 are in contact with each other, or the gas separator 6 may be configured so that the first polymer thin film 2 and the support 5 are in contact with each other.

[0127] An oxyethylene chain-containing polymer solution with a P(PEGMA) content of 0.01 g / mL and a photopolymerization initiator content of 0.0001 g / mL was prepared in the same manner as in Example 11. Separately, a PDMS preparation solution was prepared in the same manner as in Example 1. Furthermore, a reinforcing material dispersion containing 0.00003 g / mL of carbon nanotubes 11 was prepared.

[0128] Next, a sacrificial layer was formed on the substrate using PSS in the same manner as in Example 1. Furthermore, the oxyethylene chain-containing polymer solution prepared by the above-mentioned procedure was applied to the substrate on which the sacrificial layer was formed by spin coating (3000 rpm, 1 min). Then, the substrate on which the oxyethylene chain-containing polymer solution was applied was heated at 2000 K for 1 minute. 2 The substrate was left to stand in the atmosphere for 30 minutes, and then irradiated with UV light in the same atmosphere to crosslink the P(PEGMA) and form a second polymer thin film 3.

[0129] Next, the reinforcing material dispersion liquid prepared by the above-described procedure was applied by spin coating (3000 rpm / 1 minute) so as to cover the second polymer thin film 3, thereby forming a reinforcing layer 4. Next, the PDMS preparation liquid prepared by the above-described procedure was applied by spin coating (3000 rpm / 1 minute) so as to cover the reinforcing layer 4. Thereafter, the substrate was left standing in the air for one day, and the PDMS was cured to form a first polymer thin film 2. In this way, a sacrificial layer and a polymer composite thin film 1 were formed on the substrate.

[0130] Next, the substrate was immersed in water to dissolve the sacrificial layer and peel off the polymer composite thin film 1 from the substrate. The polymer composite thin film 1 was then transferred to the support 5 in such a manner that the first polymer thin film 2 of the polymer composite thin film 1 was in contact with the support 5, thereby obtaining a gas separator 6. When the cross section of the polymer composite thin film 1 was observed with an SEM, the reinforcing layer 4 could not be clearly identified.

[0131] A polymer composite thin film 1 and a gas separator 6 were produced under the same conditions as in Example 18, except that a reinforcing material dispersion containing 0.000015 g / mL of carbon nanotubes 11 was used. In Example 19, too, the reinforcing layer 4 could not be clearly identified in SEM observation of the cross section of the polymer composite thin film 1.

[0132] A polymer composite thin film 1 and a gas separator 6 were produced under the same conditions as in Example 18, except that a reinforcing material dispersion containing 0.0006 g / mL of cellulose nanofibers 12 was used. In Example 20, when the cross section of the polymer composite thin film 1 was observed by SEM, the reinforcing layer 4 could not be clearly identified.

[0133] Table 5 below shows the results of Examples 18 to 20, including the presence or absence of self-supporting ability, the thickness of the first polymer thin film 2, the thickness of the second polymer thin film 3, the material constituting the reinforcing layer 4, the amount of reinforcing material 10 added, and the CO 2 Transparency, N 2 Transparency, O 2 Permeability, selectivity CO 2 / N 2 , O 2 / N 2 , CO 2 / O 2 Table 5 also shows data for comparative examples.

[0134] As shown in Table 5, the polymer composite thin films 1 of Examples 18 to 20 all have self-supporting properties. In all cases, the thickness of the first polymer thin film 2 containing PDMS is approximately the same as that of the PDMS thin film of the comparative example, and the polymer composite thin films 1 of Examples 18 to 20 can be considered to be structurally the same as the PDMS thin film of the comparative example, with the reinforcing material 10 unevenly distributed on one surface and the second polymer thin film 3 superimposed thereon.

[0135] By superposing the second polymer thin film 3 on the first polymer thin film 2 containing PDMS and the reinforcing material 10, the overall film thickness also increases. 2 , N 2 , O 2 The permeability is lower than that of the comparative example. 2 / N 2 is significantly improved compared to the comparative examples, and all the results except for Example 20 are 2 / N 2 is also found to be improved.

[0136] Here, in Examples 18 and 19, the reinforcing layer 4 was formed of carbon nanotubes 11, and in Example 20, the reinforcing layer 4 was formed of cellulose nanofibers 12. Compared with Examples 1 to 3 (in which the first polymer thin film 2 and the second polymer thin film 3 did not include the reinforcing material 10), the thickness of the second polymer thin film 3 in Examples 18 and 19 was 38 nm, and the thickness of the second polymer thin film 3 in Examples 1 to 3 was 113 nm to 74 nm. That is, in Examples 18 and 19, the second polymer thin film 3 was supported by the first polymer thin film 2 including the reinforcing layer 4, thereby improving the overall mechanical strength and enabling the second polymer thin film 3 (and consequently the polymer composite thin film 1) to be formed thinner.

[0137] In the gas separators 6 of the second to fourth embodiments, as described in the first embodiment (Examples 7 to 10), the gas selectivity was superior when the gas was allowed to permeate through the second polymer thin film 3 first and then the first polymer thin film 2, while the gas permeability was superior when the gas was allowed to permeate through the first polymer thin film 2 first and then the second polymer thin film 3.

[0138] As described above, according to the first to fourth embodiments, a polymer composite membrane 1 having a good balance of gas permeability and gas selectivity can be realized by combining two polymer membranes with different properties, or by further combining (composite) a reinforcing material 10, or by combining a reinforcing layer 4.

[0139] Fifth Embodiment Fig. 3 is an explanatory diagram showing the configuration of a gas separation device 110 including a gas separator 6 according to the present invention. As shown in Fig. 3, the gas separation device 110 is composed of a blower 114, a pre-filter 111, a dust collecting filter 112, and a gas separator 6, and an air flow path 119 is formed from an intake port 115 to a first outlet 116a (and a second outlet 116b).

[0140] The blower 114 is configured by, for example, an air compressor. When the blower 114 is driven, air is sucked in from an intake port 115, and passes through a flow path 119 as an air flow AF, passing through the pre-filter 111, the dust collecting filter 112, and the gas separator 6 in this order.

[0141] The air that has permeated the gas separator 6 is discharged as an air flow AFO from a first outlet 116a provided downstream of the gas separator 6. On the other hand, the air that has not permeated the gas separator 6 is discharged as an air flow AFN from a second outlet 116b provided upstream of the gas separator 6.

[0142] To perform gas separation, a pressure difference is required between the upstream space (first space S1) and the downstream space (here, external space S0) across the gas separator 6. In the gas separation device 110 of the fifth embodiment, to ensure this pressure difference, an air cock 117 is connected to the second outlet 116b to limit the outflow rate of the air flow AFN, and compressed air is delivered by a blower 114 to adjust the first space S1 to a positive pressure relative to the external space S0 (1 atmosphere). For polymer composite membranes 1 mounted on the gas separator 6 that have high permeability, the air pressure in the first space S1 can be set to a gentle value, such as about 2 atmospheres (pressure difference between the first space S1 and the external space S0 = 1 atmosphere). Furthermore, the polymer composite membrane 1 according to the present invention has extremely high gas selectivity, allowing efficient gas separation even when the pressure difference between the front and rear of the gas separator 6 is small.

[0143] Furthermore, the polymer composite thin film 1 according to the present invention (particularly the second to fourth embodiments) has extremely high mechanical strength because it is configured to include the reinforcing material 10 in the polymer composite thin film 1. Therefore, it is possible to set the pressure difference between the first space S1 and the external space S0 as high as about 10 atmospheres.

[0144] The pre-filter 111 is the first filter through which the air drawn in by the blower 114 passes, and it captures relatively large dust particles contained in the airflow AF. The dust collection filter 112 is the next filter through which the air that has passed through the pre-filter 111 passes, and a HEPA (High Efficiency Particulate Air) filter, for example, is preferably used.

[0145] The gas separator 6 is provided therein with the polymer composite membrane 1 described in the first to fourth embodiments. The gas supply unit (here, the blower 114) supplies gas so that the gas permeates through the second polymer membrane 3 and then the first polymer membrane 2 (or through the first polymer membrane 2 and then the second polymer membrane 3). This allows the user of the gas separation device 110 to select a configuration of the gas separator 6 with better gas selectivity or gas permeability, and obtain oxygen-enriched air, carbon dioxide-enriched air, or nitrogen-enriched air.

[0146] As shown in Tables 1 to 5, the polymer composite thin film 1 according to the present invention has a 2 Compared to CO 2 and O 2 Since the permeability of the air is high, the air flow AFO that passes through the gas separator 6 and is discharged from the first outlet 116a has a higher O2 content than normal air. 2 and CO 2 On the other hand, the air flow AFN discharged from the second outlet 116b without passing through the gas separator 6 has a higher concentration of nitrogen than normal air (i.e., nitrogen-enriched air).

[0147] The airflow AFO is the CO 2 Since the carbon dioxide enriched air is enriched in CO, the gas separation device 110 captures the CO 2 Here, the gas separator 6 may have a multi-stage configuration in which a plurality of polymer composite membranes 1 are arranged in series. 2 / N 2 When the selectivity is set to 2.2 and the number of stages of the polymer composite thin film 1 is set to P, the O 2 / N 2 The selectivity ratio is 2.2^P, and increasing the number of stages makes it possible to further increase the oxygen concentration. Of course, when P is increased, the total gas permeability in the gas separator 6 decreases. In this case, this can be addressed by increasing the capacity of the air compressor that constitutes the blower 114.

[0148] In addition, the present inventors have reported in "Polymer Journal (2021) 53:111-119 A new strategy for membrane-based direct air capture" that by configuring the polymer thin film in the gas separator 6 in multiple stages, CO 2 It has been reported that the gas separation device 110 with multi-stage polymer membranes can be installed in various sizes and scales, and new CO 2The polymer composite membrane 1 according to the present invention has high permeability, extremely high gas selectivity, and extremely high mechanical strength, and therefore can be used to recover CO from the air. 2 Ya O 2 It is extremely useful for concentrating and recovering

[0149] Furthermore, the airflow AFO is utilized in fish farms that utilize oxygen-enriched air, oxygen combustion power plants, oxygen combustion boilers, etc. 2 The concentration is also increasing, but by passing it through activated carbon or water, for example, the CO 2 is relatively easy to remove, 2 It is possible to obtain large amounts of oxygen-enriched air with reduced increase in concentration.

[0150] On the other hand, AFN airflow can be used for firefighting, for example. Combustion requires three elements: combustible material, an oxygen supplier, and an ignition source. However, combustion of combustible material in air will not continue unless the oxygen concentration exceeds a critical level. By ensuring that the nitrogen concentration exceeds 85% (oxygen concentration falls below 14%), combustion of most combustible materials can be suppressed. Furthermore, AFN airflow (nitrogen-enriched air) can be used in corrosion and decay prevention systems (preservation systems) to prevent the deterioration of food, artwork, etc. due to oxidation.

[0151] In addition, in thermal power plants where fossil fuels such as coal, oil, and LNG gas are burned in boilers and the heat from the combustion creates steam that turns turbines to generate electricity, AFO (air enriched with oxygen) airflow is normally used to improve combustion efficiency, but if the boiler becomes abnormally hot due to a malfunction or other reason, AFN (air enriched with nitrogen) airflow can be supplied to prevent fires.

[0152] The air flow AFO may be not only air as described above, but also exhaust gas from an internal combustion engine or other mixed gases. In this case, too, the exhaust gas or other mixed gases can be enriched with carbon dioxide, oxygen, or nitrogen.

[0153] Among polysiloxanes, PDMS is known to have a particularly large free volume. In fact, the cavity radius inside the polymer estimated by positron annihilation spectroscopy is thought to be less than 1 nm (see Yampolskii, Pinnau, and Freeman, 2006, John Wiley & Sons, Ltd., "Materials Science of Membranes for Gas and Vapor Separation," p. 125). Therefore, nanoparticles exceeding this size have difficulty permeating the PDMS membrane, and the airflow AFO becomes clean air that does not contain nanoparticles.

[0154] In this way, the gas separation device 110 equipped with the polymer composite thin film 1 of the present invention not only has high permeability, selectivity, and mechanical strength, but also has the function of removing nano-sized particles that cannot be removed even by the above-mentioned dust collection filter 112.By applying the polymer composite thin film 1, it is possible to realize a clean room system (air purifier) ​​with extremely high levels of cleanliness.

[0155] The polymer composite membrane 1 and gas separation device 110 according to the present invention have been described above based on specific embodiments or examples, but these are merely examples, and the present invention is not limited to these embodiments and examples.

[0156] The polymer composite membrane 1 according to the present invention has high gas permeability, gas selectivity, and mechanical strength, and the gas separation device 110 equipped with the polymer composite membrane 1 has high gas separation properties. Therefore, for example, it is possible to separate CO, which is a greenhouse gas generated by the combustion of fossil fuels, from the gas separation device 110. 2 Carbon dioxide capture and storage (CCS) is used to separate and capture carbon dioxide from sources such as power plants and factories, and carbon dioxide is extracted from the air. 2 This can be suitably applied to a DAC that directly recovers

[0157] REFERENCE SIGNS LIST 1 Polymer composite thin film 2 First polymer thin film 3 Second polymer thin film 4 Reinforcement layer 5 Support 6 Gas separator 10 Reinforcement material 11 Carbon nanotube 12 Cellulose nanofiber 110 Gas separation device 114 Blower

Claims

1. A polymer composite thin film comprising: a first polymer thin film having selective permeability to a predetermined gas; and a second polymer thin film overlapping the first polymer thin film and containing at least an oxyethylene chain.

2. The polymer composite thin film according to claim 1, characterized in that carbon nanotubes or cellulose nanofibers are dispersed in the second polymer thin film.

3. The polymer composite thin film according to claim 1, characterized in that carbon nanotubes or cellulose nanofibers are dispersed in the first polymer thin film.

4. The polymer composite thin film according to claim 1, further comprising a reinforcing layer formed of carbon nanotubes or cellulose nanofibers between the first polymer thin film and the second polymer thin film.

5. A polymer composite thin film described in any one of claims 1 to 4, characterized in that the second polymer thin film is composed of a crosslinked polymer containing the oxyethylene chain.

6. The polymer composite thin film according to claim 5, wherein the crosslinked polymer containing oxyethylene chains is in a partially crosslinked state.

7. A polymer composite thin film according to any one of claims 1 to 4, characterized in that the total thickness of the first polymer thin film and the second polymer thin film is 20 nm to 1000 nm.

8. The polymer composite thin film according to any one of claims 1 to 4, which is selectively permeable to carbon dioxide and oxygen from air, exhaust gas, and other mixed gases.

9. The polymer composite thin film according to any one of claims 1 to 4, characterized in that the first polymer thin film is mainly composed of polysiloxane.

10. A gas separator comprising: a polymer composite thin film according to any one of claims 1 to 4; and a support for supporting said polymer composite thin film.

11. A gas separation device comprising: a gas separator as described in claim 10; and a gas supply unit that supplies gas to the gas separator, wherein the gas supply unit supplies gas so that the gas permeates through the second polymer thin film and then the first polymer thin film.

12. A gas separation device comprising: a gas separator as described in claim 9; and a gas supply unit that supplies gas to the gas separator, wherein the gas supply unit supplies gas so that the gas permeates through the first polymer thin film and then the second polymer thin film.

13. A method for producing a polymer composite thin film comprising: a first step of preparing an oxyethylene chain-containing polymer solution and preparing a polymer material-containing solution containing a polymer material that has selective permeability to a predetermined gas when formed into a thin film; a second step of applying the oxyethylene chain-containing polymer solution onto a substrate on which a sacrificial layer has been formed so as to cover the sacrificial layer to form a second polymer thin film; a third step of crosslinking the second polymer thin film; a fourth step of applying and curing the polymer material-containing solution so as to cover the second polymer thin film after crosslinking to form a first polymer thin film; and a fifth step of dissolving the sacrificial layer and peeling off a polymer composite thin film composed of the first polymer thin film and the second polymer thin film from the substrate.

14. A method for producing a polymer composite thin film comprising: a first step of preparing an oxyethylene chain-containing polymer-reinforcing material-containing solution containing an oxyethylene chain-containing polymer and a reinforcing material, and preparing a polymer material-containing solution containing a polymer material having selective permeability to a predetermined gas when formed into a thin film; a second step of applying the oxyethylene chain-containing polymer-reinforcing material-containing solution onto a substrate on which a sacrificial layer has been formed, so as to cover the sacrificial layer, to form a second polymer thin film; a third step of crosslinking the second polymer thin film; a fourth step of applying and curing the polymer material-containing solution so as to cover the second polymer thin film after crosslinking, to form a first polymer thin film; and a fifth step of dissolving the sacrificial layer, and peeling off a polymer composite thin film composed of the first polymer thin film and the second polymer thin film from the substrate.

15. A method for producing a polymer composite thin film comprising: a first step of preparing an oxyethylene chain-containing polymer solution and preparing a polymer material-reinforcement-containing solution containing a polymer material that has selective permeability to a predetermined gas when formed into a thin film and a reinforcing material; a second step of applying the oxyethylene chain-containing polymer solution onto a substrate on which a sacrificial layer has been formed so as to cover the sacrificial layer to form a second polymer thin film; a third step of crosslinking the second polymer thin film; a fourth step of applying and curing the polymer material-reinforcement-containing solution so as to cover the second polymer thin film after crosslinking to form a first polymer thin film; and a fifth step of dissolving the sacrificial layer and peeling off a polymer composite thin film composed of the first polymer thin film and the second polymer thin film from the substrate.

16. A method for producing a polymer composite thin film, comprising: a first step of preparing a reinforcing material dispersion containing a reinforcing material, an oxyethylene chain-containing polymer solution, and a polymer material-containing solution containing a polymer material that has selective permeability to a predetermined gas when formed into a thin film; a second step of forming a second polymer thin film by applying the oxyethylene chain-containing polymer solution onto a substrate on which a sacrificial layer has been formed so as to cover the sacrificial layer; a third step of crosslinking the second polymer thin film; a fourth step of forming a reinforcing layer by applying the reinforcing material dispersion so as to cover the second polymer thin film after crosslinking; a fifth step of forming a first polymer thin film by applying and curing the polymer material-containing solution so as to cover the reinforcing layer; and a sixth step of dissolving the sacrificial layer and peeling off a polymer composite thin film composed of the first polymer thin film and the second polymer thin film from the substrate.

17. The method for producing a polymer composite thin film according to any one of claims 14 to 16, characterized in that the reinforcing material is a carbon nanotube or a cellulose nanofiber.

18. A method for producing a polymer composite thin film according to any one of claims 13 to 16, characterized in that in the third step, the second polymer thin film is crosslinked in a nitrogen atmosphere.

19. A method for producing a polymer composite thin film described in any one of claims 13 to 16, characterized in that in the third step, the progress of crosslinking is stopped while functional groups that contribute to the crosslinking reaction remain in the second polymer thin film.

Citation Information

Patent Citations

  • Freshness keeping gas permselective membrane

    JP2003024756A

  • Gas separation membranes

    JP2020531260A

  • Air separation film and method for producing air separation film, and air separation device and oxygen mask

    JP2022180867A