Multilayer body and cured product obtained by curing same

The laminate, featuring a bisphenol A polycarbonate base layer and a curable resin layer with specific properties, addresses the trade-off between hardness and moldability, achieving excellent three-dimensional formability and post-molding hardness for thermoformable films, particularly suitable for uneven surfaces.

WO2024237127A1PCT designated stage expired Publication Date: 2024-11-21MITSUBISHI GAS CHEM CO INC
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2024/016928
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-10-06
Filing Date
2024-05-07
Publication Date
2024-11-21

AI Technical Summary

Technical Problem

Thermoformable films face a trade-off between hardness and moldability, with higher hardness leading to reduced formability, and existing laminates struggle with achieving both high hardness and three-dimensional formability for molded products with uneven surfaces.

Method used

A laminate comprising a base layer of bisphenol A polycarbonate with a curable resin layer containing a (meth)acryloyl polymer, which has an acrylic equivalent of 200 to 600 g/mol, and an intermediate glass transition temperature of 100 to 140°C, allowing for excellent hardness and three-dimensional formability by maintaining the curable resin layer in an uncured state during molding and curing it post-molding.

Benefits of technology

The laminate achieves high hardness and three-dimensional formability, preventing cracks during vacuum forming and enabling conformable lamination on uneven surfaces, resulting in a cured product with enhanced scratch resistance and chemical resistance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JPOXMLDOC01-APPB-C000001
    Figure JPOXMLDOC01-APPB-C000001
  • Figure JPOXMLDOC01-APPB-C000002
    Figure JPOXMLDOC01-APPB-C000002
  • Figure JPOXMLDOC01-APPB-C000003
    Figure JPOXMLDOC01-APPB-C000003
Patent Text Reader

Abstract

Provided is a multilayer body which is excellent in terms of hardness and three-dimensional moldability. This multilayer body comprises a base material layer (a) and a curable resin layer (b) that contains a (meth)acryloyl polymer having an acrylic equivalent of 200-600 g / mol. The base material layer (a) contains 96% by mass or more of a bisphenol A type polycarbonate with respect to the total mass of the base material layer (a), and the midpoint glass transition temperature (Tmg) of the base material layer (a) is 100-140°C.
Need to check novelty before this filing date? Find Prior Art

Description

Laminate and cured product obtained by curing the same

[0001] The present invention relates to a laminate and a cured product obtained by curing the laminate.

[0002] Thermoforming films (also called functional films or decorative films) are suitably used to impart desired properties (for example, scratch resistance, chemical resistance, designability, etc.) to the surface of a molded product.

[0003] When applying a thermoforming film to a molded product, various molding methods are used, such as vacuum forming, pressure forming, film insert molding, in-mold molding, and three-dimensional decoration (TOM) molding.

[0004] When a molded article needs to have properties such as scratch resistance, the thermoforming film must have high hardness. Therefore, the thermoforming film is often formed into a laminate with a hard coating layer formed by curing a resin. However, the higher the hardness of the thermoforming film, the lower the moldability and the less conformability it has to the molded article. In other words, there is a trade-off between hardness and moldability in thermoforming films.

[0005] Conventionally, methods for achieving both hardness and formability in thermoforming films have been investigated. For example, Patent Document 1 describes an invention relating to a thermoforming sheet comprising at least three layers laminated in this order: Layer A containing a polycarbonate-based resin, Layer B containing an acrylic-based resin, and Layer C formed from an uncured product of an acrylate-based active energy ray-curable resin composition. The invention is characterized in that Layer A has a glass transition temperature (Tg) of 100°C or higher and 145°C or lower.

[0006] Patent Document 1 describes that, according to the invention, high moldability can be achieved by leaving the C layer, which corresponds to the hard coat layer, in an uncured state when applied to a molded article, and that a hard coat layer with high hardness can be obtained by curing the C layer by post-exposure to active energy rays after applying the thermoforming sheet to the molded article (after molding).

[0007] Japanese Patent Application Laid-Open No. 2021-146687

[0008] The thermoforming film described in Patent Document 1 achieves both hardness and formability, but there is room for improvement in three-dimensional formability. Therefore, the present invention provides a laminate that is excellent in hardness and three-dimensional formability.

[0009] The present invention is, for example, as follows.

[0010] [1] A laminate comprising a substrate layer (a) and a curable resin layer (b) containing a (meth)acryloyl polymer having an acrylic equivalent of 200 to 600 g / mol, wherein the substrate layer (a) contains 96 mass % or more of bisphenol A polycarbonate relative to the total mass of the substrate layer (a), and the intermediate glass transition temperature (Tmg) of the substrate layer (a) is 100 to 140° C. [2] The bisphenol A polycarbonate is a laminate comprising bisphenol A, a carbonate binder, and a compound represented by the following formula (1): [In the above formula (1), R 1 is an alkyl group having 8 to 36 carbon atoms or an alkenyl group having 8 to 36 carbon atoms, R 2 and a monohydric phenol end-terminator represented by formula (1) which includes at least one member selected from the group consisting of 2-hexyldecyl parahydroxybenzoate, hexadecyl parahydroxybenzoate, dodecyl parahydroxybenzoate, and 2-ethylhexyl parahydroxybenzoate. [4] The laminate according to the above item [1], wherein the (meth)acryloyl polymer is a polycarbonate obtained by reacting a monohydric phenol end-terminator represented by formula (2): [5] The laminate according to any one of the above [1] to [3], comprising a repeating unit represented by the following formula (2): [in the above formula (2), m is a single bond or an alkylene group having 1 to 4 carbon atoms, n is hydrogen or an alkyl group having 1 to 4 carbon atoms, p is a single bond or an alkylene group having 1 to 2 carbon atoms, and q is hydrogen or an alkyl group having 1 to 12 carbon atoms which may be substituted with at least one substituent selected from the group consisting of an epoxy group, a hydroxyl group, and a (meth)acryloyl group]. The laminate according to [4] above, comprising at least one repeating unit represented by the formula: [6] The laminate according to any one of [1] to [5] above, wherein the (meth)acryloyl polymer has an acrylic equivalent of 200 to 500 g / mol. [7] The laminate according to any one of [1] to [6] above, wherein the curable resin layer (b) further comprises a leveling agent. [8] The laminate according to [7] above, wherein the leveling agent comprises a fluorine-based leveling agent. [9] The laminate according to any one of [1] to [8] above, wherein the curable resin layer (b) further comprises inorganic particles.

[10] The laminate according to [9] above, wherein the inorganic particles have an average particle size of 20 to 60 nm.

[11] The laminate according to any one of [1] to

[10] above, wherein the curable resin layer (b) further comprises a light stabilizer.

[12] The laminate according to any one of [1] to

[11] above, wherein the curable resin layer (b) further comprises a polymerization inhibitor.

[13] The laminate according to any one of [1] to

[12] above, wherein the thickness of the curable resin layer (b) is 5 μm or more.

[14] The laminate according to any one of [1] to

[13] above, further comprising an acrylic layer (c), wherein the base layer (a), the acrylic layer (c), and the curable resin layer (b) are laminated in this order.

[15] The laminate according to

[14] above, wherein the thickness of the acrylic layer (c) is 20 μm or more.

[16] The laminate according to any one of [1] to

[15] above, which is used for vacuum forming.

[17] The laminate according to any one of [1] to

[16] above, which is used for turn-on-metal forming.

[18] A cured product obtained by curing the laminate according to any one of [1] to

[17] above.

[0011] According to the present invention, a laminate having excellent hardness and three-dimensional formability is provided, which allows it to be suitably molded, for example, by three-dimensional decoration (TOM) molding.

[0012] Hereinafter, embodiments of the present invention will be described in detail.

[0013] 1. Laminate The laminate according to the present invention comprises a substrate layer (a) and a curable resin layer (b) containing a (meth)acryloyl polymer having an acrylic equivalent of 200 to 600 g / mol. The substrate layer (a) contains 96 mass % or more of bisphenol A polycarbonate based on the total mass of the substrate layer (a). The intermediate glass transition temperature (Tmg) of the substrate layer (a) is 100 to 140°C.

[0014] The laminate has excellent hardness and three-dimensional formability. Specifically, the laminate includes a curable resin layer (b), i.e., an uncured resin layer (b), and has a predetermined structure, so that it has excellent formability, particularly three-dimensional formability. Furthermore, after molding the laminate, the curable resin layer (b) is cured to form a cured film, and the cured product obtained from the laminate has high hardness.

[0015] In this specification, the term "intermediate glass transition temperature (Tmg)" refers to a value obtained by analyzing a DSC curve obtained by differential scanning calorimetry (DSC). Specifically, of the line A obtained by extending the low-temperature side baseline of the DSC curve to the high-temperature side, the tangent line B to the inflection point, and the line C obtained by extending the high-temperature side baseline to the low-temperature side, the intersection of line A and tangent line B is defined as the starting glass transition temperature (Tig), and the tangent line B and tangent line C is defined as the ending glass transition temperature (Teg). The intermediate glass transition temperature (Tmg) is the midpoint between the starting glass transition temperature (Tig) and the ending glass transition temperature (Teg). Generally, the term "glass transition temperature" refers to the starting glass transition temperature (Tig), which is lower than the intermediate glass transition temperature (Tmg). The intermediate glass transition temperature (Tmg) is measured by the method described in the Examples.

[0016] In one embodiment, the laminate according to the present invention is used for vacuum forming. Vacuum forming is a forming method in which forming is performed under vacuum conditions, and examples thereof include in-mold forming and three-dimensional decoration (TOM) forming. When a laminate including a curable resin layer (b) is applied to a molded product (when molding), it is preferable not to harden the curable resin layer (b) during molding, but to harden the curable resin layer (b) after molding. However, when molding is performed under vacuum conditions, radicals are generated from oxygen atoms contained in the curable resin layer (b), which can cause unintended hardening of the curable resin layer (b) during vacuum molding. As a result, cracks can occur in the curable resin layer (b) after molding. According to the laminate according to the present invention, even when molding is performed under vacuum conditions, a laminate can be formed without generating cracks, and cracks can be prevented from occurring in the curable resin layer (b) of the laminate.

[0017] In one embodiment, the laminate of the present invention is used in three-dimensional decoration (TOM) molding. The three-dimensional decoration (TOM) molding includes (1) a vacuum process in which a lower chamber with an opening at the top and in which a molded product having a textured surface is placed, an upper chamber with an opening at the bottom and in which a heater is placed, and the laminate of the present invention sandwiched between the lower chamber and the upper chamber are airtightly sealed, and then placed under vacuum conditions, (2) a heating process in which the laminate is heated using the heater, (3) a contact process in which the molded product having textured surfaces is brought into contact with the heated laminate, (4) an upper chamber de-vacuum process in which the upper chamber is placed under atmospheric pressure, and (5) a lower chamber de-vacuum process in which the lower chamber is placed under atmospheric pressure. That is, three-dimensional decorative (TOM) molding involves heating a laminate to soften it under vacuum conditions, pushing a molded product up from below the laminate to bring them into contact (the laminate is tightly laminated by the molded product due to its own weight), and then creating a pressure difference in the upper chamber under atmospheric pressure to apply pressure from the upper chamber to the lower chamber to complete the lamination. This allows for the production of a three-dimensionally decorated molded product including a molded product with a textured surface and a laminate placed on the textured surface. Note that three-dimensional decorative (TOM) molding may further include an upper chamber pressurization step of introducing compressed air into the upper chamber after the upper chamber de-vacuuming step. Furthermore, three-dimensional decorative (TOM) molding may further include a trimming step of removing a portion of the laminate placed on the textured surface and a curing step of curing the laminate after the lower chamber de-vacuuming step. When using conventional laminates, attempting to perform three-dimensional decorative (TOM) molding often results in the laminate being unable to be laminated to a molded product with a textured surface with high conformability, and even if lamination is possible, cracks may occur in the laminate. However, the laminate of the present invention can be laminated with high conformability to molded articles having uneven surfaces, and the resulting laminate is less likely to crack. That is, the laminate of the present invention has excellent three-dimensional moldability. Furthermore, the laminate having the configuration of the present invention can produce a cured product with high hardness.

[0018] <Substrate Layer (a)> The substrate layer (a) contains bisphenol A polycarbonate. The substrate layer (a) may further contain other resins, plasticizers, additives, and the like.

[0019] [Bisphenol A Polycarbonate] Bisphenol A polycarbonate is a resin containing structural units derived from bisphenol A (BPA) in an amount of 80% by mass or more, preferably 90% by mass or more, more preferably 95% by mass or more, even more preferably 97% by mass or more, and particularly preferably 98 to 100% by mass, based on the mass of all structural units of bisphenol A polycarbonate excluding terminal structures.

[0020] In one embodiment, the bisphenol A polycarbonate is preferably a polycarbonate obtained by reacting bisphenol A, a carbonate binder, and a monohydric phenol end-terminator represented by the following formula (1):

[0021] (Bisphenol A) Bisphenol A (BPA) is represented by the following formula.

[0022] (Compound for Derivation of Other Structural Units) Bisphenol A polycarbonate may be formed by further reacting with a compound for derivation of other structural units. By using the compound for derivation of other structural units, the physical properties of the bisphenol A polycarbonate (e.g., mid-glass transition temperature (Tmg), viscosity-average molecular weight, etc.) can be adjusted.

[0023] The compound from which the other structural units are derived is a polymerizable compound other than bisphenol A, and examples thereof include bisphenol compounds other than bisphenol A and organosiloxanes.

[0024] Examples of bisphenol compounds other than bisphenol A include bis(4-hydroxyphenyl)methane (bisphenol F: BPF), bis(2-hydroxyphenyl)methane, 2,4'-dihydroxydiphenylmethane, bis(4-hydroxy-3-methylphenyl)methane, 1,1-bis(4-hydroxyphenyl)ethane (bisphenol E: BPE), 1,1-bis(4-hydroxy-3-methylphenyl)ethane, 2,2-bis(4-hydroxy-3-methylphenyl)propane (bisphenol C: BPC), 2,2-bis(4-hydroxy-3-isopropylphenyl)propane (bisphenol G: BPG), 2,2-bis(4-hydroxyphenyl)butane (bisphenol B: BPB), 2,2-bis(4-hydroxy-3-t-butylphenyl)propane, 5,5'-(1-methylethylidene)-bis[1,1'-(bisphenyl)-2-ol]propane (bisphenol PH: BPPH), 1,1-bis(4-hydroxyphenyl)-2-methylpropane (bisphenol IBTD), 2,2-bis(4-hydroxyphenyl)-4-methylpentane (bisphenol MIBK), 1,1-bis(4-hydroxyphenyl)-2-ethylhexane (bisphenol IOTD), 1,1-bis(4-hydroxyphenyl)decane, 1,1-bis(4-hydroxyphenyl)cyclohexane (bisphenol Z: BPZ), 1,1-bis(4-hydroxyphenyl)-3,3,5-trimethylcyclohexane (bisphenol TMC), 1,1-bis(4-hydroxy-3-methylphenyl)cyclohexane, 1,1-bis(4-hydroxyphenyl)cycloundecane, 1,1-bis(4-hydroxyphenyl)cyclododecane, 1,1-bis(4-hydroxyphenyl)-1-phenylethane (bisphenol AP: BPAP), bis(4-hydroxyphenyl)diphenylmethane (bisphenol BP;BPBP), bis(4-hydroxyphenyl) sulfide, bis(4-hydroxyphenyl) ether, bis(4-hydroxyphenyl) sulfoxide, bis(4-hydroxyphenyl) sulfone, 2,4'-dihydroxydiphenyl sulfone, bis(2-hydroxyphenyl) sulfone, bis(4-hydroxy-3-methylphenyl) sulfone bis(4-hydroxyphenyl) ketone, 9,9-bis(4-hydroxyphenyl) fluorene, 9,9-bis(4-hydroxy-3-methylphenyl) fluorene, 9,9-bis(4-hydroxy-3-ethylphenyl) fluorene, 4,4'-[1,4-phenylenebis(1-methylethylidene)]bisphenol, 4,4'-[1,3-phenylenebis(1-methylethylidene)]bisphenol, 1,3-bis(4-hydroxyphenyl)-5,7-dimethyladamantane, and the like.

[0025] Examples of organosiloxanes include α,ω-bis[3-(o-hydroxyphenyl)propyl]polydimethylsiloxane and α,ω-bis[3-(o-hydroxyphenyl)propyl]polydimethyldiphenyl random copolymerized siloxane.

[0026] The compounds from which the other structural units are derived may be used alone or in combination of two or more.

[0027] The amount of the compound that derives other structural units added is preferably 50 moles or less, and more preferably 0.1 to 40 moles, per mole of bisphenol A.

[0028] (Carbonate Binder) The carbonate binder is not particularly limited, and examples thereof include carbonyl compounds such as phosgene, triphosgene, carbon monoxide, carbon dioxide, and carbonate diesters.

[0029] Examples of the carbonic acid diester include dialkyl carbonate compounds such as dimethyl carbonate, diethyl carbonate, and di-tert-butyl carbonate, and substituted diphenyl carbonates such as diphenyl carbonate, di-p-tolyl carbonate, phenyl-p-tolyl carbonate, and di-p-chlorophenyl carbonate.

[0030] Among these, the carbonate binder preferably contains at least one of phosgene, triphosgene, diphenyl carbonate, and substituted diphenyl carbonate, and more preferably contains at least one of phosgene and diphenyl carbonate. The carbonate binders may be used alone or in combination of two or more.

[0031] (Monohydric Phenol End Capper Represented by Formula (1)) The monohydric phenol end capper represented by formula (1) has the function of adjusting the midpoint glass transition temperature (Tmg) of bisphenol A polycarbonate.

[0032] In the above formula (1), R 1 is an alkyl group having 8 to 36 carbon atoms or an alkenyl group having 8 to 36 carbon atoms, and R 2 are each independently a hydrogen atom, a halogen atom, an alkyl group having 1 to 20 carbon atoms which may be substituted with a halogen atom or an aryl group having 6 to 12 carbon atoms, or an aryl group having 6 to 12 carbon atoms which may be substituted with a halogen atom, an alkyl group having 1 to 20 carbon atoms, or an aryl group having 6 to 12 carbon atoms. In this specification, the "alkyl group" and the "alkenyl group" may be linear or branched, but are preferably linear.

[0033] More preferably, the monohydric phenol end-terminator represented by formula (1) is represented by the following general formula (1-a):

[0034] In the above formula (1-a), R 1 is an alkyl group having 8 to 36 carbon atoms or an alkenyl group having 8 to 36 carbon atoms.

[0035] R in formula (1) or formula (1-a) 1 It is more preferable that the number of carbon atoms in R is within a specific numerical range. 1 The upper limit of the number of carbon atoms in R is preferably 36, more preferably 22, and particularly preferably 18. 1 The lower limit of the number of carbon atoms is preferably 8, and more preferably 12.

[0036] R1 When the upper limit of the carbon number of R is appropriate, the solubility of the monohydric phenol end-terminator represented by formula (1) in organic solvents tends to be high, which is preferable from the viewpoints of increasing the productivity in the production of bisphenol A polycarbonate resin and increasing the transparency of the bisphenol A polycarbonate resin. 1 When the number of carbon atoms in R is 36 or less, a bisphenol A polycarbonate resin having high transparency can be obtained, and the productivity in producing the bisphenol A polycarbonate resin is high and economical. 1 When the number of carbon atoms is 22 or less, the monohydric phenol end-terminator represented by formula (1) has particularly excellent solubility in organic solvents, and can significantly increase the productivity in producing bisphenol A polycarbonate resin, thereby improving the economic efficiency.

[0037] R 1 When the lower limit of the carbon number of R is appropriate, the glass transition temperature of the bisphenol A polycarbonate resin is not too high, and the resin has favorable thermoformability, which is preferable. 1 When a monohydric phenol end-terminator represented by formula (1), in which R is an alkyl group having 16 carbon atoms, is used, the intermediate glass transition temperature, melt fluidity, moldability, drawdown resistance, and solvent solubility of the monohydric phenol end-terminator represented by formula (1) during production of the bisphenol A polycarbonate resin are excellent, and it is particularly preferred as the end-terminator to be used for the bisphenol A polycarbonate resin of the present invention.

[0038] In one embodiment, R in formula (1) or formula (1-a) 1 is preferably dodecyl, tridecyl, tetradecyl, pentadecyl, hexadecyl, heptadecyl, octadecyl, 2-ethylhexyl, or 2-hexyldecyl, more preferably tetradecyl, pentadecyl, hexadecyl, heptadecyl, or 2-hexyldecyl, even more preferably hexadecyl or 2-hexyldecyl, and particularly preferably 2-hexyldecyl.

[0039] In one embodiment, R in formula (1) 2are each independently preferably hydrogen, a halogen atom, methyl, ethyl, propyl, isopropyl, butyl, t-butyl, or phenyl, more preferably hydrogen, a fluorine atom, a chlorine atom, methyl, ethyl, or phenyl, and even more preferably hydrogen, a fluorine atom, a chlorine atom, methyl, or ethyl. 2 is preferably hydrogen.

[0040] In one embodiment, the monohydric phenol end-terminator represented by formula (1) preferably includes at least one selected from the group consisting of parahydroxybenzoic acid 2-hexyldecyl ester, parahydroxybenzoic acid hexadecyl ester, parahydroxybenzoic acid dodecyl ester, and parahydroxybenzoic acid 2-ethylhexyl ester, more preferably includes at least one of parahydroxybenzoic acid 2-hexyldecyl ester and parahydroxybenzoic acid hexadecyl ester, and even more preferably includes parahydroxybenzoic acid 2-hexyldecyl ester.

[0041] The monohydric phenol end-terminator represented by the above formula (1) may be used alone or in combination of two or more kinds.

[0042] The amount of the monohydric phenol end-terminator represented by formula (1) used is preferably 0.02 to 0.07 mol, more preferably 0.025 to 0.06 mol, per 1 mol of bisphenol A.

[0043] The amount of the monohydric phenol end-terminator represented by formula (1) used is preferably 0.02 to 0.07 mol, more preferably 0.025 to 0.06 mol, per 1 mol of the carbonate binder.

[0044] (Other end-capping agents) Bisphenol A polycarbonate may be formed by further reacting with other end-capping agents. The other end-capping agents are end-capping agents other than the monohydric phenol end-capping agent represented by formula (1), and are preferably end-capping agents that do not have unsaturated groups. The use of the other end-capping agents makes it possible to adjust the physical properties of the bisphenol A polycarbonate (e.g., the midpoint glass transition temperature (Tmg), the viscosity average molecular weight, etc.).

[0045] Other end-stoppers include those derived from monohydric phenol compounds.

[0046] Examples of the monohydric phenol compound include phenol, p-cresol, o-cresol, 2,4-xylenol, p-tert-butylphenol, p-hexylphenol, p-heptylphenol, p-octylphenol, p-cumylphenol, etc. These monohydric phenol compounds may be used alone or in combination of two or more.

[0047] The amount of the other terminal terminator used is preferably 0.5 mol or less, more preferably 0.2 mol or less, and even more preferably 0.1 mol or less, per mol of the terminal terminator represented by formula (1).

[0048] The amount of the other end terminator used is preferably 0.02 to 0.07 mol, more preferably 0.025 to 0.06 mol, per 1 mol of bisphenol A.

[0049] The intermediate glass transition temperature (Tmg) of the bisphenol A polycarbonate is preferably 100 to 140° C., more preferably 125 to 140° C., even more preferably 128 to 140° C., and still more preferably 128 to 135° C. If the intermediate glass transition temperature (Tmg) of the bisphenol A polycarbonate is in the above range, it is preferable because it is easy to control the intermediate glass transition temperature (Tmg) of the base layer (a).

[0050] The viscosity average molecular weight of the bisphenol A polycarbonate is preferably 14,000 or more, more preferably 16,000 or more, even more preferably 20,000 or more, particularly preferably 24,000 or more, and very preferably 26,000 or more. The viscosity average molecular weight of the bisphenol A polycarbonate is preferably 40,000 or less, more preferably 38,000 or less, even more preferably 36,000 or less, particularly preferably 34,000 or less, and very preferably 32,000 or less. In one embodiment, the viscosity average molecular weight of the bisphenol A polycarbonate is preferably 14,000 to 40,000, more preferably 16,000 to 38,000, even more preferably 18,000 to 36,000, particularly preferably 20,000 to 34,000, and very preferably 24,000 to 32,000. In this specification, the "viscosity average molecular weight" is measured by the method described in the Examples. When the bisphenol A polycarbonate is a mixture of two or more bisphenol A polycarbonates having different molecular weights, the viscosity average molecular weight after mixing is used.

[0051] The content of bisphenol A polycarbonate is 96% by mass or more, more preferably 98% by mass or more, and even more preferably 100% by mass, based on the total mass of the base layer (a).

[0052] [Plasticizer] The base layer (a) may further contain a plasticizer, which has the function of adjusting the intermediate glass transition temperature (Tmg) of the base layer.

[0053] The plasticizer is not particularly limited, but examples thereof include polyesters, polyethers, aromatic phosphonate compounds, and aromatic ester compounds.

[0054] Examples of the polyester include aliphatic polyesters such as polycaprolactone (PCL); and aromatic polyesters such as polyethylene terephthalate modified resins and polycaprolactone polyethylene terephthalate modified resins.

[0055] Examples of polycaprolactone polyethylene terephthalate-modified resins include glycol-modified polyethylene terephthalate (PETG) and glycol-modified polycyclohexylene dimethylene terephthalate (PCTG). PETG is a PET (a PET consisting of terephthalic acid units, which are dicarboxylic acid units, and ethylene glycol units, which are glycol units) in which some of the ethylene glycol units have been replaced with 1,4-cyclohexanedimethanol units. The content of 1,4-cyclohexanedimethanol units is preferably less than 50 mol%, more preferably 30 to 40 mol%, based on the total glycol units. PCTG is a PCT (a PET consisting of terephthalic acid units, which are dicarboxylic acid units, and 1,4-cyclohexanedimethanol units, which are glycol units) in which some of the glycol units have been replaced with glycol units. The content of glycol units is preferably less than 50 mol%, more preferably 30 to 40 mol%, based on the total glycol units.

[0056] The number average molecular weight of the polyester is preferably 10,000 to 100,000, and more preferably 20,000 to 60,000. In this specification, the value of "number average molecular weight" is measured by gel permeation chromatography.

[0057] Examples of the polyether include polyethers having at least one selected from the group consisting of ethylene glycol units, propylene glycol units, butylene glycol units, trimethylene glycol units, and tetramethylene glycol units. Specifically, the polyether may be a homopolymer or a copolymer, and if it is a copolymer, it may be a random copolymer, an alternating copolymer, a block copolymer, a graft copolymer, or a combination thereof. Specific examples of the polyether include polyethylene glycol, polypropylene glycol, polybutylene butylene glycol, and block copolymers of polyethylene glycol and polypropylene glycol. The number-average molecular weight of the polyether is preferably 500 to 4,000, more preferably 600 to 3,000, and even more preferably 800 to 2,000.

[0058] Examples of aromatic phosphonate compounds include triphenyl phosphate, tricresyl phosphate, trixylenyl phosphate, cresyl diphenyl phosphate, 2-ethylhexyl diphenyl phosphate, tert-butylphenyl diphenyl phosphate, bis-(tert-butylphenyl)phenyl phosphate, tris-(tert-butylphenyl)phosphate, isopropylphenyl diphenyl phosphate, bis-(isopropylphenyl)diphenyl phosphate, tris-(isopropylphenyl)phosphate, resorcinol bis-diphenyl phosphate, resorcinol poly(di-2,6-xylyl)phosphate, resorcinol bis-dixylenyl phosphate, bisphenol A bis-diphenyl phosphate, and biphenyl bis-diphenyl phosphate. The molecular weight of the aromatic phosphonate compound is preferably 200 to 1,000, and more preferably 400 to 800.

[0059] Examples of aromatic ester compounds include diethylene glycol dibenzoate, glyceryl tribenzoate, trimethylolpropane tribenzoate, pentaerythritol tetrabenzoate, etc. The molecular weight of the aromatic ester compound is preferably 200 to 1,000, and more preferably 400 to 800.

[0060] Of the above, the plasticizer preferably contains a polyester or an aromatic phosphonate compound, more preferably contains a polyester, further preferably contains at least one of polycaprolactone (PCL), glycol-modified polyethylene terephthalate (PETG), and glycol-modified polycyclohexylene dimethylene terephthalate (PCTG), and particularly preferably contains polycaprolactone (PCL). The above plasticizers may be used alone or in combination of two or more.

[0061] The content of the plasticizer is preferably 4% by mass or less, more preferably 3% by mass or less, and even more preferably 0.1 to 2% by mass, based on the total mass of the base layer (a). When the content of the plasticizer is 4% by mass or less, the base layer (a) can contain bisphenol A polycarbonate in a content of 96% by mass or more.

[0062] [Additives] The base layer (a) may further contain additives. The additives are not particularly limited, but include polycarbonates other than bisphenol A polycarbonates, antioxidants, transesterification inhibitors, release agents, heat stabilizers, flame retardants, flame retardant assistants, ultraviolet absorbers, colorants, antistatic agents, fluorescent brighteners, antifogging agents, flow improvers, plasticizers, dispersants, antibacterial agents, antiblocking agents, impact improvers, sliding improvers, hue improvers, and acid trapping agents. These additives may be used alone or in combination of two or more.

[0063] The content of the additive is preferably 4% by mass or less, more preferably 3% by mass or less, and even more preferably 0.1 to 2% by mass, relative to the total mass of the base layer (a). When the content of the additive is 4% by mass or less, the base layer (a) can contain bisphenol A polycarbonate in a content of 96% by mass or more.

[0064] [Configuration of Base Layer (a)] The intermediate glass transition temperature (Tmg) of the base layer (a) is 100 to 140° C., preferably 110 to 140° C., more preferably 120 to 140° C., even more preferably 120 to 135° C., and particularly preferably 125 to 135° C. The intermediate glass transition temperature (Tmg) of the base layer (a) can be controlled by appropriately adjusting the structure of the bisphenol A polycarbonate (for example, the content of structural units derived from bisphenol A (BPA), the types and contents of other structural units, the type of end-capping agent used, the viscosity average molecular weight, etc.), the type and content of the plasticizer added to the base layer (a), etc.

[0065] The thickness of the substrate layer (a) is preferably 10 to 800 μm, more preferably 20 to 500 μm, and even more preferably 30 to 400 μm. In one embodiment, the thickness of the substrate layer (a) is preferably 20 to 140 μm, more preferably 30 to 120 μm, and even more preferably 60 to 120 μm. In another embodiment, the thickness of the substrate layer (a) is preferably 140 to 500 μm, more preferably 150 to 400 μm, even more preferably 180 to 300 μm, and particularly preferably 180 to 260 μm.

[0066] The Charpy impact strength of the substrate layer (a) is 30 kJ / m 2 It is preferable that the concentration is 45 kJ / m or more. 2 In this specification, the "Charpy impact strength" is measured by the method described in the examples.

[0067] <Curable Resin Layer (b)> The curable resin layer (b) contains a (meth)acryloyl polymer having an acrylic equivalent of 200 to 600 g / mol. Because the curable resin layer (b) is in an uncured state, it has excellent three-dimensional moldability when attempting to mold the laminate of the present invention. Therefore, when three-dimensional molding is performed, the curable resin layer (b) easily conforms, and cracks are less likely to occur in the curable resin layer (b) after molding. Furthermore, the cured product obtained by curing the laminate has high hardness and may have improved scratch resistance, chemical resistance, etc. In this specification, "(meth)acryloyl" means methacryloyl and / or acryloyl. Similarly, "(meth)acrylic" and "(meth)acrylate" mean methacrylic and / or acrylic, methacrylate and / or acrylate.

[0068] [(Meth)acryloyl Polymer] The (meth)acryloyl polymer preferably contains a repeating unit represented by the following formula (2).

[0069]

[0070] In the above formula (2), m is a single bond or an alkylene group having 1 to 4 carbon atoms, preferably methylene or ethylene, and more preferably methylene.

[0071] n is hydrogen or an alkyl group having 1 to 4 carbon atoms, preferably hydrogen, methyl, or ethyl, more preferably hydrogen or methyl, and even more preferably hydrogen.

[0072] p is a single bond or an alkylene group having 1 to 2 carbon atoms, preferably a single bond or methylene, and more preferably a single bond.

[0073] q is hydrogen or an alkyl group having 1 to 12 carbon atoms which may be substituted with at least one substituent selected from the group consisting of an epoxy group, a hydroxyl group, and a (meth)acryloyl group, preferably an alkyl group having 1 to 4 carbon atoms which may be substituted with at least one substituent selected from the group consisting of an epoxy group and a (meth)acryloyl group, and more preferably an alkyl group having 1 to 2 carbon atoms which may be substituted with at least one substituent selected from the group consisting of an epoxy group and a (meth)acryloyl group.

[0074] In one embodiment, the (meth)acryloyl polymer preferably contains at least one repeating unit represented by the following formulas (2-a) to (2-c):

[0075]

[0076] The content of the repeating unit represented by formula (2-a) is preferably 30 to 85 mol %, more preferably 40 to 80 mol %, based on the total number of moles of the (meth)acryloyl polymer.

[0077] The content of the repeating unit represented by formula (2-b) is preferably 5 to 30 mol %, more preferably 10 to 25 mol %, based on the total number of moles of the (meth)acryloyl polymer.

[0078] The content of the repeating unit represented by formula (2-c) is preferably 10 to 40 mol %, more preferably 10 to 35 mol %, based on the total number of moles of the (meth)acryloyl polymer.

[0079] The above-mentioned (meth)acryloyl polymers may be used alone or in combination of two or more kinds.

[0080] The molar ratio of the repeating unit represented by formula (2-a) to the repeating unit represented by formula (2-b) is preferably 4.5 to 5.5:1.5 to 2.5. The molar ratio of the repeating unit represented by formula (2-a) to the repeating unit represented by formula (2-c) is preferably 4.5 to 5.5:2.5 to 3.5. The molar ratio of the repeating unit represented by formula (2-b) to the repeating unit represented by formula (2-c) is preferably 1.5 to 2.5:2.5 to 3.5.

[0081] The acrylic equivalent of the (meth)acryloyl polymer is 200 to 600 g / mol, and from the viewpoint of increasing the hardness of the cured product, it is preferably 200 to 500 g / mol, more preferably 200 to 400, and even more preferably 200 to 300. In this specification, the (meth)acrylic equivalent (g / mol) means the molecular weight per (meth)acryloyl group, and can be calculated by the method described in the examples.

[0082] The weight average molecular weight of the (meth)acryloyl polymer is preferably 5,000 to 200,000, more preferably 10,000 to 150,000, even more preferably 15,000 to 100,000, and particularly preferably 20,000 to 50,000. In this specification, the "weight average molecular weight" is calculated by the method described in the examples.

[0083] The content of the (meth)acryloyl polymer is preferably 50% by mass or more, more preferably 60% by mass or more, still more preferably 60 to 100% by mass, and particularly preferably 60 to 90% by mass, relative to the total mass of the curable resin layer (b).

[0084] [Polyfunctional Acrylate Compound] The curable resin layer (b) may further contain a polyfunctional acrylate compound. The polyfunctional acrylate compound can improve the hardness of the cured product by reacting with, for example, a (meth)acryloyl group, an epoxy group, a hydroxyl group, or the like, contained in the (meth)acryloyl polymer. In this specification, "polyfunctional" means difunctional or more, preferably trifunctional or more, more preferably trifunctional to octafunctional, and even more preferably trifunctional to hexafunctional.

[0085] The polyfunctional acrylate compound is not particularly limited, but examples thereof include pentaerythritol triacrylate, pentaerythritol tetraacrylate, and dipentaerythritol hexaacrylate.

[0086] The content of the polyfunctional acrylate compound is preferably 70% by mass or less, more preferably 50% by mass or less, and even more preferably 30% by mass or less, based on the total content of the (meth)acryloyl polymer and the polyfunctional acrylate compound.

[0087] [Inorganic Particles] The curable resin layer (b) may further contain inorganic particles, which can improve the hardness and scratch resistance of the cured product.

[0088] The inorganic particles are not particularly limited, but examples thereof include silica, alumina, titania, zirconia, diamond, and the like.

[0089] The inorganic particles may be surface-treated. By surface-treating the inorganic particles, they can be stably dispersed in the curable resin layer (b). The surface treatment agent used here is not particularly limited, but includes silane compounds, alcohols, amines, carboxylic acids, sulfonic acids, phosphonic acids, and the like. These surface treatment agents may be used alone or in combination of two or more. By the surface treatment, polymerizable groups (preferably vinyl groups and (meth)acrylic groups) can be introduced onto the inorganic particle surfaces.

[0090] The inorganic particles described above may be used alone or in combination of two or more kinds.

[0091] The average particle size of the inorganic particles is preferably 5 to 95 nm, more preferably 8 to 70 nm, and from the viewpoint of improving the scratch resistance of the resulting cured product, is further preferably 20 to 60 nm, and particularly preferably 30 to 60 nm. In this specification, "particle size" refers to the maximum distance between two points on the outer surface of a particle. The "average particle size" is measured by the method described in the Examples.

[0092] The content of the inorganic particles is preferably 5 to 60% by mass, more preferably 10 to 50% by mass, and even more preferably 20 to 40% by mass, based on the total mass of the curable resin layer (b).

[0093] [Leveling Agent] The curable resin layer (b) may further contain a leveling agent. The leveling agent has functions such as leveling properties (making the coating film flat and smooth) and improving the fingerprint wiping properties, stain resistance, and abrasion resistance of the cured product.

[0094] The leveling agent is not particularly limited, but examples thereof include fluorine-based leveling agents and silicone-based leveling agents.

[0095] Examples of the fluorine-based leveling agent include compounds having a perfluoropolyether bond. Commercially available fluorine-based leveling agents can be used, such as Megafac RS-56, RS-75, RS-76-E, RS-76-NS, RS-78, and RS-90 (manufactured by DIC Corporation), KY-1203, X-71-1203E, KY-1207, and KY-1211 (manufactured by Shin-Etsu Chemical Co., Ltd.), Optool UD120 (manufactured by Daikin Industries, Ltd.), and Ftergent 710FL, 220P, 208G, 601AD, 602A, 650A, 228P, and 240GFTX-218 (manufactured by Neos Corporation).

[0096] Examples of silicone leveling agents include acrylic group-containing polyether-modified polydimethylsiloxane, etc. Commercially available silicone leveling agents can be used, such as BYK-UV3500 and BYK-UV3505 (manufactured by BYK Japan KK).

[0097] Among these, the leveling agent preferably contains a fluorine-based leveling agent from the viewpoint of improving the ease of wiping off fingerprints from the cured product, etc. The above-mentioned leveling agents may be used alone or in combination of two or more kinds.

[0098] The content of the leveling agent is preferably 0.001 to 10 mass %, more preferably 0.001 to 5 mass %, even more preferably 0.01 to 4 mass %, and particularly preferably 0.1 to 3 mass %, relative to the total mass of the curable resin layer (b).

[0099] [Photopolymerization initiator] The curable resin layer (b) may further contain a photopolymerization initiator. The photopolymerization initiator has a function of accelerating the curing reaction when curing the curable resin layer (b).

[0100] The photopolymerization initiator is not particularly limited, but examples thereof include 1-hydroxycyclohexylphenylketone (Irgacure 184), 2-hydroxy-2-methyl-1-phenylpropan-1-one (Irgacure 1173), 2,4,6-trimethylbenzoyldiphenylphosphine oxide (Irgacure TPO), bis(2,4,6-trimethylbenzoyl)phenylphosphine oxide (Irgacure 819), 2,2'-dimethoxy-2-phenylacetophenone (Irgacure 651), oligo(2-hydroxy-2-methyl-1-[4-(1-methylvinyl)phenyl]propanone (Esacure ONE), 1-hydroxycyclohexylphenylketone (Omnirad Among these, from the viewpoint of increasing heat resistance, the photopolymerization initiator preferably contains at least one of oligo(2-hydroxy-2-methyl-1-[4-(1-methylvinyl)phenyl]propanone (EsacureONE) and 1-hydroxycyclohexyl-phenyl ketone (Omnirad 184), and more preferably contains 1-hydroxycyclohexyl-phenyl ketone (Omnirad 184). The above-mentioned photopolymerization initiators may be used alone or in combination of two or more.

[0101] The content of the photopolymerization initiator is preferably 1 to 10 mass %, more preferably 1 to 6 mass %, even more preferably 2 to 5 mass %, and particularly preferably 2 to 4 mass %, relative to the total mass of the curable resin layer (b).

[0102] [Light Stabilizer] The curable resin layer (b) may further contain a light stabilizer, which has the function of improving the weather resistance of the cured product.

[0103] The light stabilizer is not particularly limited, but examples thereof include hindered amine light stabilizers.

[0104] Examples of hindered amine light stabilizers include bis(1-undecaneoxy-2,2,6,6-tetramethylpiperidin-4-yl)carbonate (ADK STAB LA-81), tetrakis(1,2,2,6,6-pentamethyl-4-piperidyl)butane-1,2,3,4-tetracarboxylate (ADK STAB LA-52), tetrakis(2,2,6,6-tetramethyl-4-piperidyl)butane-1,2,3,4-tetracarboxylate (ADK STAB LA-57), and 1,2,2,6,6-pentamethyl-4-piperidyl methacrylate (ADK STAB LA-82). Examples thereof include bis(2,2,6,6-tetramethyl-1-octyloxy-4-piperidyl)sebacate (Tinuvin 123), bis(2,2,6,6-tetramethyl-4-piperidyl)sebacate (Tinuvin 770DF), and bis(1,2,2,6,6-pentamethyl-4-piperidyl)-((3,5-bis(1,1-dimethylethyl)-4-hydroxyphenyl)methyl)butyl malonate (Tinuvin 144).

[0105] Among these, the light stabilizer preferably includes a hindered amine light stabilizer. The above light stabilizers may be used alone or in combination of two or more.

[0106] The content of the light stabilizer is preferably 0.1 to 15 mass %, more preferably 0.1 to 7 mass %, even more preferably 0.3 to 5 mass %, and particularly preferably 0.3 to 3 mass %, relative to the total mass of the curable resin layer (b).

[0107] [Polymerization inhibitor] The curable resin layer (b) may further contain a polymerization inhibitor. The polymerization inhibitor has functions such as suppressing a polymerization reaction of the curable resin layer (b) due to light, heat, etc., and improving the storage stability of the laminate.

[0108] The polymerization inhibitor is not particularly limited, but examples thereof include phenothiazine, mequinol (4-methoxyphenol), hydroquinone, 2-hydroxynaphthoquinone, N-isopropyl-N'-phenyl-p-phenylenediamine, 6-ethoxy-2,2,4-trimethyl-1,2-dihydroquinoline, 2,2,6,6-tetramethyl-4-oxopiperidine-1-oxyl, and 2-mercaptobenzimidazole.

[0109] Among these, the polymerization inhibitor preferably contains at least one of phenothiazine, mequinol, and hydroquinone, and more preferably contains phenothiazine. The above-mentioned polymerization inhibitors may be used alone or in combination of two or more.

[0110] The content of the polymerization inhibitor is preferably 0.001 to 5 mass %, more preferably 0.01 to 4 mass %, and even more preferably 0.01 to 3 mass %, relative to the total mass of the curable resin layer (b).

[0111] [Additives] The curable resin layer (b) may further contain additives.

[0112] The additives are not particularly limited, but examples thereof include heat stabilizers, antioxidants, flame retardants, flame retardant assistants, ultraviolet absorbers, release agents, colorants, antistatic agents, fluorescent brighteners, antifogging agents, flow improvers, plasticizers, dispersants, antibacterial agents, etc. These additives may be used alone or in combination of two or more.

[0113] [Configuration of Curable Resin Layer (b)] The curable resin layer (b) is in an uncured state, and for example, the (meth)acryloyl polymer has a polymerizable functional group (such as a (meth)acryloyl group, an epoxy group, or a hydroxyl group). The curable resin layer (b) is easy to conform and is less likely to crack after molding, resulting in excellent three-dimensional moldability. However, for example, within the scope of the present invention, the (meth)acryloyl polymer in the curable resin layer (b) may have a crosslinked structure due to a curing reaction of some of the (meth)acryloyl groups during the molding process.

[0114] The thickness of the curable resin layer (b) is preferably 1 μm or more, more preferably 3 μm or more, and from the viewpoint of increasing hardness, is further preferably 5 μm or more, particularly preferably 5 to 30 μm, and most preferably 5 to 10 μm.

[0115] <Acrylic Layer (c)> The laminate may further include an acrylic layer (c). The acrylic layer (c) has functions such as improving the impact resistance of the laminate and improving the hardness of the cured product.

[0116] In one embodiment, the laminate preferably includes a substrate layer (a), an acrylic layer (c), and a curable resin layer (b) laminated in this order. By disposing the acrylic layer (c) between the substrate layer (a) and the curable resin layer (b), the adhesion between the substrate layer (a) and the curable resin layer (b) can be improved.

[0117] The acrylic layer (c) preferably contains a (meth)acrylic resin.

[0118] [(Meth)acrylic Resin] The (meth)acrylic resin is not particularly limited as long as it is a polymer of a (meth)acrylic acid ester. Examples of the (meth)acrylic acid ester include methyl (meth)acrylate, ethyl (meth)acrylate, and butyl (meth)acrylate.

[0119] The (meth)acrylic resin may be a homopolymer or a copolymer.

[0120] Among these, the (meth)acrylic resin preferably contains polymethyl methacrylate (PMMA) resin from the viewpoints of high transparency, excellent moldability, etc. The above-mentioned (meth)acrylic resins may be used alone or in combination of two or more.

[0121] The content of the (meth)acrylic resin is preferably 60% by mass or more, more preferably 80% by mass or more, even more preferably 90% by mass or more, and particularly preferably 90 to 100% by mass, based on the total mass of the acrylic layer (c).

[0122] [Additives] The acrylic layer (c) may further contain additives.

[0123] The additives are not particularly limited, and examples thereof include ultraviolet absorbers, antioxidants, coloring inhibitors, inorganic particles, etc. These additives may be used alone or in combination of two or more. [Configuration of Acrylic Layer (c)] The thickness of the acrylic layer (c) is preferably 5 μm or more, more preferably 10 μm or more, and from the viewpoint of increasing the hardness of the cured product, further preferably 20 μm or more, particularly preferably 30 μm or more, very preferably 30 to 80 μm, and most preferably 40 to 60 μm.

[0124] 2. Method for Producing Laminated Body According to one aspect of the present invention, there is provided a method for producing a laminated body.

[0125] In one embodiment, the method for producing a laminate includes a step (1-1) of forming a base layer (a) from a first resin composition, and a step (2-1) of forming a curable resin layer (b) from a second resin composition on the base layer (a).

[0126] In this case, instead of step (1-1), step (1-2) of co-extruding the first resin composition and the third resin composition to form a precursor including the base layer (a) and the acrylic layer (c) may be included. When step (1-2) is included, step (2-2) of forming a curable resin layer (b) from the second resin composition on the acrylic layer (c) on the precursor is included instead of step (2-1).

[0127] In this case, the first resin composition contains bisphenol A polycarbonate, the second resin composition contains a (meth)acryloyl polymer having an acrylic equivalent of 200 to 600 g / mol, and the third resin composition contains a (meth)acrylic resin.

[0128] Each step will be described below.

[0129] <Step (1-1)> Step (1-1) is a step of forming a substrate layer (a) from a first resin composition.

[0130] [First Resin Composition] The first resin composition contains bisphenol A polycarbonate. In addition, the first resin composition may further contain a plasticizer, an additive, and the like.

[0131] The bisphenol A polycarbonate, plasticizer, and additives used are the same as those described above.

[0132] The composition of the first resin composition is appropriately adjusted so that the substrate layer (a) has a desired structure.

[0133] [Method for Forming Base Layer (a)] The method for forming the base layer (a) is not particularly limited, but it is preferable to extrude the first resin composition.

[0134] The melting temperature of the first resin composition is not particularly limited, but is preferably 230 to 320°C, and more preferably 260 to 300°C.

[0135] The cooling temperature of the first resin composition is not particularly limited, but is preferably 50 to 200°C, and more preferably 70 to 150°C.

[0136] <Step (1-2)> Step (1-2) is a step of co-extruding the first resin composition and the third resin composition to form a precursor including the substrate layer (a) and the acrylic layer (c).

[0137] [First Resin Composition] The first resin composition used is the same as that used in step (1-1).

[0138] [Third Resin Composition] The third resin composition contains a (meth)acrylic resin. In addition, the third resin composition may further contain additives and the like.

[0139] The composition of the third resin composition is appropriately adjusted so that the acrylic layer (c) has a desired structure.

[0140] [Method for forming precursor] The precursor is formed by co-extruding the first resin composition and the third resin composition, thereby forming a precursor including the base layer (a) and the acrylic layer (c).

[0141] The melting temperature and cooling temperature of the first resin composition are the same as those in the step (1-1).

[0142] The melting temperature of the third resin composition is not particularly limited, but is preferably 200 to 280°C, and more preferably 210 to 260°C.

[0143] The cooling temperature of the third resin composition is not particularly limited, but is preferably 50 to 200°C, and more preferably 70 to 150°C.

[0144] <Step (2-1)> Step (2-1) is a step of forming a curable resin layer (b) from a second resin composition on the substrate layer (a) formed in step (1-1).

[0145] [Second Resin Composition] The second resin composition contains a (meth)acryloyl polymer having an acrylic equivalent of 200 to 600 g / mol. In addition, the second resin composition may further contain a polyfunctional acrylate compound, inorganic particles, a leveling agent, a photopolymerization initiator, a light stabilizer, a polymerization inhibitor, an additive, a dilution solvent, etc.

[0146] The dilution solvent is not particularly limited, but examples thereof include acetone, methyl ethyl ketone, cyclohexanone, etc. These dilution solvents may be used alone or in combination of two or more.

[0147] The composition of the second resin composition is appropriately adjusted so that the curable resin layer (b) has a desired structure.

[0148] [Method of Forming Curable Resin Layer (b)] The method of forming the curable resin layer (b) is not particularly limited, but is preferably a method of applying the second resin composition onto the substrate layer (a).

[0149] Examples of the method for applying the second resin composition include spray coating, spin coating, bar coating, gravure coating, and die coating.

[0150] The coating film formed by application is preferably dried. For example, by drying, the dilution solvent that may be contained in the second resin composition is evaporated, and the curable resin layer (b) can be obtained.

[0151] The temperature for drying the coating is preferably 50 to 200°C, more preferably 70 to 150°C.

[0152] <Step (2-2)> Step (2-2) is a step of forming a curable resin layer (b) from a second resin composition on the acrylic layer (c) in the precursor formed in step (1-2), and can be performed in the same manner as step (2-1).

[0153] 3. Cured Product According to one embodiment of the present invention, a cured product is provided. The cured product is obtained by curing the above-described laminate. In this specification, "curing of a laminate" means curing the curable resin layer (b) of the laminate to obtain a cured film. Furthermore, "cured film" means a cured film (single-layer film) obtained by curing the curable resin layer (b). Furthermore, "cured product" means a laminate of two or more layers including the cured film and each layer derived from the laminate (such as the substrate layer (a)).

[0154] In one embodiment, the cured product includes a substrate layer (a) and a cured film of the curable resin layer (b). In another embodiment, the cured product includes a substrate layer (a), a cured film of the curable resin layer (b), and an acrylic layer (c). The cured product is preferably formed by laminating the substrate layer (a), the acrylic layer (c), and the cured film of the curable resin layer (b) in this order. In this case, the configurations of the substrate layer (a) and the acrylic layer (c) are usually the same as those in the laminate.

[0155] The cured film of the curable resin layer (b) has high hardness. As a result, the cured product may have high scratch resistance, chemical resistance, etc. In one embodiment, the cured product may have high fingerprint wiping properties, weather-resistant adhesion, etc.

[0156] Since the cured product can be used as a thermoforming film (functional film, decorative film), it is preferably formed so as to cover the surface of a molded article. That is, in one embodiment, there is provided a thermoforming film-containing molded article comprising a molded article and the cured product according to the present invention arranged on the surface of the molded article.

[0157] The molded article is not particularly limited, but is preferably a molded article having an uneven surface, and examples of the molded article include goggles, sinks, organs, beds, and vehicle housings.

[0158] In a preferred embodiment, the molded article is a molded article having a textured surface, and the laminate is three-dimensionally decorated and molded (TOM molding) onto the molded article, thereby providing a three-dimensionally decorated molded article comprising a molded article having a textured surface and a laminate arranged on the textured surface.

[0159] 4. Method for Producing a Cured Product According to one aspect of the present invention, there is provided a method for producing a cured product. The method for producing a cured product includes a curing step of curing the above-described laminate. The method for producing a cured product may further include a molding step of three-dimensionally molding the laminate onto a surface of a molded article.

[0160] [Molding process] The molding process is a process of three-dimensionally molding a laminate on the surface of a molded article. Since the curable resin layer (b) of the laminate is in an uncured state, the three-dimensional moldability of the laminate is high. As a result, even when three-dimensional molding is performed, the conformability of the laminate is high, and cracks are less likely to occur in the laminate after molding.

[0161] (Molded Article) The molded article is not particularly limited, but for example, the above-mentioned molded articles can be used.

[0162] (Laminate) As the laminate, the above-mentioned materials are used.

[0163] (Three-dimensional molding) Three-dimensional molding includes three-dimensional decoration (TOM) molding. As described above, the three-dimensional decoration (TOM) molding includes: (1) a vacuum process in which a lower chamber with an opening at the top in which a molded product having a textured surface is placed, an upper chamber with an opening at the bottom in which a heater is placed, and the laminate of the present invention sandwiched between the lower chamber and the upper chamber are airtight, and then placed under vacuum conditions; (2) a heating process in which the laminate is heated using the heater; (3) a contact process in which the molded product having textured surfaces is brought into contact with the heated laminate; (4) an upper chamber de-vacuum process in which the upper chamber is placed under atmospheric pressure; and (5) a lower chamber de-vacuum process in which the lower chamber is placed under atmospheric pressure. Furthermore, after the upper chamber de-vacuum process, an upper chamber pressurization process in which compressed air is introduced into the upper chamber may be further included. Furthermore, after the lower chamber de-vacuum process, a trimming process in which a portion of the laminate placed on the textured surface is removed may be further included.

[0164] [Curing Step] The curing step is a step of curing the laminate. More specifically, it is a step of curing the curable resin layer (b) in the laminate by a curing reaction to obtain a cured film of the curable resin layer (b).

[0165] The curing reaction is not particularly limited, but is preferably carried out by irradiation with active energy rays.

[0166] Examples of the active energy rays include ultraviolet rays, electron beams, and radioactive rays, and ultraviolet rays are preferred.

[0167] The irradiation dose of the active energy ray is not particularly limited, but is preferably 100 to 5000 mJ / cm as the cumulative exposure dose at an ultraviolet wavelength of 365 nm. 2 is preferably 300 to 3000 mJ / cm 2 It is more preferable that:

[0168] The present invention will be specifically described below with reference to examples, but the present invention is not limited to these examples.

[0169] 1. Raw Materials (1) Polycarbonate Resins T-1380: Bisphenol A (BPA) polycarbonate resin using parahydroxybenzoic acid hexadecyl ester (p-HBAHE) as an end-capping agent (manufactured by Mitsubishi Gas Chemical Company, Inc., viscosity average molecular weight: 25,500, Tig: 126°C, Tmg: 131°C) T-1300: Bisphenol A (BPA) polycarbonate resin using parahydroxybenzoic acid hexadecyl ester (p-HBAHE) as an end-capping agent (manufactured by Mitsubishi Gas Chemical Company, Inc., viscosity average molecular weight: 30,500, Tig: 132°C, Tmg: 136°C) S-1000: Bisphenol A (BPA) polycarbonate resin using para-tertiary butylphenol (pt-BPh) as an end-capping agent (manufactured by Mitsubishi Engineering-Plastics Corporation, viscosity average molecular weight: 25,000, Tig: 147°C, Tmg: 151°C) FPC-0330: Bisphenol C (BPC) polycarbonate resin using para-tertiary butylphenol (pt-BPh) as an end-capping agent (manufactured by Mitsubishi Gas Chemical Company, Inc., viscosity average molecular weight: 32,000, Tig: 123°C, Tmg: 126°C)

[0170] The structures of parahydroxybenzoic acid hexadecyl ester (p-HBAHE) and para-tert-butylphenol (pt-BPh) are as follows:

[0171] (2) Plasticizers PLACCEL H1P: polycaprolactone (PCL) (manufactured by Daicel Corporation) SKYGREEN (registered trademark) J2003: PCTG (glycol-modified polycyclohexylene dimethylene terephthalate) (manufactured by SK Chemical Co., Ltd., a polyester in which 80 mol% of ethylene glycol, a raw material for PET, is replaced with cyclohexanedimethanol) PX200: resorcinol poly(di-2,6-xylyl)phosphate (manufactured by Daihachi Chemical Industry Co., Ltd.)

[0172] (3) PMMA (polymethyl methacrylate) resin Delpet 80HD: PMMA resin (manufactured by Asahi Kasei Corporation, methyl methacrylate (MMA):methyl acrylate = 99% by mass: 1% by mass, weight average molecular weight: 124,600)

[0173] (4) Curable resin raw materials SMP-360A: acryloyl group-containing polymer (manufactured by Kyoeisha Chemical Co., Ltd., acrylic equivalent 360 g / mol) SMP-220A: acryloyl group-containing polymer (manufactured by Kyoeisha Chemical Co., Ltd., acrylic equivalent 220 g / mol) SMP-550A: acryloyl group-containing polymer (manufactured by Kyoeisha Chemical Co., Ltd., acrylic equivalent 550 g / mol) PGM-AC4130Y: nanosilica (manufactured by Nissan Chemical Co., Ltd., average particle size 45 nm, surface acrylic treatment, PGM dispersion) MEK-AC2140Z: nanosilica (manufactured by Nissan Chemical Co., Ltd., average particle size 12 nm, surface acrylic treatment, MEK dispersion) MEK-AC5140Z: nanosilica (manufactured by Nissan Chemical Co., Ltd., average particle size 80 nm, surface acrylic treatment, MEK dispersion) Omnirad 184: Photopolymerization initiator (manufactured by IGM RESINS B.V.) Adekastab LA-81: Hindered amine light stabilizer (manufactured by ADEKA Corporation) Phenothiazine (PTZ): Polymerization inhibitor (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.) RS-90: Fluorine-based leveling agent (manufactured by DIC Corporation) BYK-UV3500: Silicone-based leveling agent (manufactured by BYK)

[0174] 2. Measurement Method (1) Glass Transition Temperature The glass transition temperature (Tg) of various resins and resin compositions was measured by performing two cycles of temperature increase and decrease under the following differential scanning calorimetry (DSC) conditions, and measuring the glass transition temperature during the second temperature increase cycle. The intersection of a line (line A) extending the low-temperature baseline toward the high-temperature side and a tangent to the inflection point (tangent B) was defined as the starting glass transition temperature (Tig). The intersection of a line (line C) extending the high-temperature baseline toward the low-temperature side and a tangent to the inflection point (tangent B) was defined as the ending glass transition temperature (Teg). The midpoint between the starting glass transition temperature (Tig) and the ending glass transition temperature (Teg) was defined as the intermediate glass transition temperature (Tmg).

[0175] Measurement starting temperature: 30°C, heating rate: 10°C / min, final temperature: 250°C, cooling rate: 20°C / min. Measurement device: differential scanning calorimeter "DSC7020" (manufactured by Hitachi High-Tech Science Corporation).

[0176] (2) Viscosity-average molecular weight The viscosity-average molecular weight was calculated using Schnell's viscosity formula. Specifically, first, the intrinsic viscosity [η] (unit: dL / g) of the resin was measured using methylene chloride as a solvent. The temperature was set at 25°C. The specific viscosity [η] at each solution concentration [C] (g / dL) was measured using an Ubbelohde viscometer. sp The intrinsic viscosity was calculated from the obtained specific viscosity value and concentration using the following formula:

[0177] Next, the viscosity average molecular weight [Mv] was calculated using Schnell's viscosity formula, i.e., η = 1.23 × 10 -4 Mv 0.83 was calculated from

[0178] (3) Weight-average molecular weight The weight-average molecular weight (Mw) was measured by gel permeation chromatography. Specifically, an LC-20AD system (manufactured by Shimadzu Corporation) was used as the gel permeation chromatography apparatus, and an LF-804 (manufactured by Shodex) was connected to the column. The column temperature was set to 40°C. An RID-10A (manufactured by Shimadzu Corporation) was used as the RI detector. Chloroform was used as the eluent, and a calibration curve was created using standard polystyrene (manufactured by Tosoh Corporation).

[0179] (4) Acrylic Equivalent The acrylic equivalent was calculated using the formula "molecular weight / number of (meth)acryloyl groups".

[0180] (5) Average Particle Diameter The average particle diameter was determined by randomly selecting 30 inorganic particles observed with a transmission electron microscope (TEM), determining the maximum distance between two points on the outer surface of each particle as the particle diameter, and calculating the average value of these distances.

[0181] (6) Charpy Impact Strength The Charpy impact strength of the substrate layer (a) was measured in accordance with JIS K 7111-1:2012. Specifically, the polycarbonate and plasticizer used in Examples 1 to 22 and Comparative Examples 1 to 8 were melt-kneaded at a cylinder temperature of 260°C using a vented twin-screw injection molding machine ("PE-100" manufactured by Sodick Corporation, intermeshing co-rotating twin screws with a diameter of 29 mm, plunger diameter of 28 mm) and a molded body (test piece) measuring 80 mm in length, 10 mm in width, and 3 mm in thickness was produced at a mold temperature of 70°C. Thereafter, a notched Charpy impact test was performed in accordance with JIS K7111-1:2012 to measure the Charpy impact strength. The unit is kJ / m 2 As shown.

[0182] 3. Production of Laminate [Example 1] A laminate was produced in which a substrate layer (a), an acrylic layer (c), and a curable resin layer (b) were laminated in this order. (1) Production of Laminate (Precursor) of Substrate Layer (a) and Acrylic Layer (c) T-1380, a polycarbonate resin, was melt-kneaded at a cylinder temperature of 280°C using a vented twin-screw extruder TEX30α (manufactured by The Japan Steel Works, Ltd.) with a screw diameter of 32 mm and a screw L / D = 31.5, and pellets were obtained by strand cutting.

[0183] A laminate (precursor) of a base layer (a) and an acrylic layer (c) was produced using the pellets and PMMA (polymethyl methacrylate) resin Delpet 80HD. Specifically, a multilayer extrusion device was used, including a single-screw extruder with a shaft diameter of 32 mm, a single-screw extruder with a shaft diameter of 65 mm, a feed block connected to all extruders, and a 650 mm wide T-die connected to the feed block. PMMA resin (Delpet 80HD) was continuously introduced into the single-screw extruder with a shaft diameter of 32 mm at a cylinder temperature of 240 ° C., and the pellets were continuously introduced into the single-screw extruder with a shaft diameter of 65 mm at a cylinder temperature of 280 ° C. and extruded. In this case, the extrusion rates of the PMMA resin and the pellets were controlled so that the thickness of the acrylic layer (c) was 35 μm, and the thickness of the base layer (a) was 90 μm. The feed block connected to all extruders was equipped with two-type, two-layer distribution pins, and the laminar flow was laminated and extruded into a sheet using a T-die. The sheet was then cooled while transferring a mirror finish using three mirror-finished rolls set at temperatures of 100°C, 90°C, and 120°C from the upstream side, to produce a laminate (precursor) consisting of a substrate layer (a) containing T-1380, a polycarbonate resin, and an acrylic layer (c) containing Delpet 80HD, a PMMA resin.

[0184] (2) Production of Laminate A laminate was produced by forming the curable resin layer (b) on the acrylic layer (c) of a laminate (precursor) of the base material layer (a) and the acrylic layer (c).

[0185] A curable resin composition was obtained by mixing 70 parts by mass of SMP-360A, an acryloyl group-containing polymer, 30 parts by mass of PGM-AC4130Y, a nanosilica, 3 parts by mass of Omnirad 184, a photopolymerization initiator, 1 part by mass of RS-90, a fluorine-based leveling agent, and cyclohexanone, a dilution solvent, with stirring. Cyclohexanone was added in an amount such that the solids concentration of the curable resin composition would be 25% by weight.

[0186] Of the laminate of the base material layer (a) and the acrylic layer (c), the curable resin composition was applied onto the acrylic layer (c) using a bar coater so that the film thickness after drying would be 4 μm, and the resulting coating film was dried for 3 minutes at 130° C. to form the curable resin layer (b). In this way, a laminate in which the base material layer (a), the acrylic layer (c), and the curable resin layer (b) were laminated in this order was produced.

[0187] [Examples 2 to 20] Laminates in which a base material layer (a), an acrylic layer (c), and a curable resin layer (b) were laminated in this order were produced in the same manner as in Example 1, except that the types and amounts of raw materials used and the thickness of each layer were changed as shown in Tables 1-1 and 1-2.

[0188] Example 21 A laminate of a substrate layer (a) and a curable resin layer (b) was produced.

[0189] (1) Preparation of a monolayer film comprising a substrate layer (a) Using pellets of T-1380, a polycarbonate resin obtained in the same manner as in Example 1, a monolayer film comprising a substrate layer (a) was produced. Specifically, using a T-die melt extruder consisting of a vented twin-screw extruder TEX30α (manufactured by The Japan Steel Works, Ltd.) with a barrel diameter of 32 mm and a screw L / D = 31.5, the pellets were continuously introduced and extruded under conditions of discharge 10 kg / h, screw rotation speed 63 rpm, and cylinder temperature 280 ° C. The pellets were extruded into a sheet form using a T-die connected to the extruder, and cooled while transferring a mirror surface with three mirror-finished rolls set at temperatures of 120 ° C., 120 ° C., and 120 ° C. from the upstream side to obtain a monolayer film comprising a substrate layer (a) comprising T-1380, a polycarbonate resin.

[0190] (2) Production of Laminate A curable resin layer (b) was formed on the base material layer (a) in the same manner as in Example 1 so as to have the composition shown in Table 1, and a laminate in which the base material layer (a) and the curable resin layer (b) were laminated was produced.

[0191] Example 22, Comparative Examples 1 to 8 A laminate in which a base material layer (a), an acrylic layer (c), and a curable resin layer (b) were laminated in this order, or a laminate in which a base material layer (a) and a curable resin layer (b) were laminated, was produced in the same manner as in Example 1 or Example 21, except that the types and amounts of raw materials used and the thickness of each layer were changed as shown in Tables 1 to 3. 4. Evaluation Various evaluations were carried out on the laminates produced in Examples 1 to 22 and Comparative Examples 1 to 8.

[0192] <TOM Formability> Tom forming was carried out using the laminate, and conformability and cracks were evaluated.

[0193] The laminate was cut into a size of 330 mm x 330 mm, and an adhesive layer was attached to the base layer (a) side. A spare lens for safety goggles (manufactured by TRUSCO Corporation: part number TSG-005SP) was used as the adherend. The laminate with the adhesive layer and the adherend were placed in upper and lower boxes within a TOM molding machine NGF-0709-S (manufactured by Fuse Vacuum Co., Ltd.). The pressure inside the upper and lower boxes was reduced to 0.1 kPa, and the laminate with the adhesive layer was heated to 140°C or 150°C. Compressed air at 0.3 MPa was then introduced only into the upper box to obtain a TOM molded product.

[0194] The conformability of the TOM molded body was evaluated as follows. The evaluation was carried out by five experts and judged by majority vote. The results are shown in Table 2 below. ◯: The laminate conforms to the shape of the adherend. Δ: The laminate does not conform to the shape of the adherend to a certain extent. ×: The laminate does not conform to the shape of the adherend.

[0195] The cracks in the TOM molded body were evaluated as follows. The evaluation was carried out by five experts and judged by majority vote. The results are shown in Table 2 below. ◯: No cracks in the laminate Δ: Fine cracks are observed on the surface of the laminate ×: Large cracks are observed in the laminate

[0196] <Pencil Hardness> The pencil strength of the cured product obtained by curing the laminate was evaluated.

[0197] The cured product was produced as follows: The curable resin layer (b) of the laminate was irradiated with ultraviolet light using a conveyor-type UV irradiator ECS-401GX (manufactured by Eye Graphics Co., Ltd.). At this time, the ultraviolet light irradiation was at 700 mJ / cm. 2 (UV illuminometer manufactured by Oak Corporation, measurement wavelength 360 nm) As a result, a cured product was produced in which the curable resin layer (b) of the laminate was cured.

[0198] The pencil hardness of the cured product of the curable resin layer (b) was measured according to the conditions of JIS K 5600-5-4: 1999, and was evaluated based on the hardest pencil grit that did not cause scratches. The results are shown in Table 2 below.

[0199] The pencil hardness increases in the following order: 6B, 5B, 4B, 3B, 2B, B, HB, F, H, 2H, 3H, 4H, 5H, 6H, 7H, 8H, and 9H.

[0200] <Chemical Resistance> The chemical resistance of the cured product obtained by curing the laminate was evaluated. The cured product used was the same as that produced for the pencil hardness evaluation.

[0201] Neutrogena SPF 70 (a sunscreen containing homosalate, octocrylene, octisalate, and avobenzone) was applied to the surface of the cured product of the curable resin layer (b) and allowed to stand at 80°C for 1 hour. The surface was then washed with a neutral detergent, and the appearance was evaluated according to the following criteria. The results are shown in Table 2 below. ◯: No abnormalities on the surface ×: Whitening was observed on the surface.

[0202] <Abrasion Resistance> The abrasion resistance of the cured product obtained by curing the laminate was evaluated. The cured product used was the same as that produced for the pencil hardness evaluation.

[0203] The surface of the cured product of the curable resin layer (b) was coated with #0000 steel wool at 100 gf / cm 2 The surface was scratched by moving the tool back and forth 15 times under a pressure of 1000 psi. The appearance after scratching was evaluated according to the following criteria. The results are shown in Table 2 below. ◎: No scratches observed ○: Very slight scratches observed △: Scratches observed in some areas ×: Scratches observed over the entire surface

[0204] Weather-resistant adhesion The weather-resistant adhesion of the cured product obtained by curing the laminate was evaluated. The cured product used was the same as that produced for the pencil hardness evaluation.

[0205] The surface of the cured product of the curable resin layer (b) was irradiated with light under the following conditions: Apparatus: SUV-W161 (manufactured by Iwasaki Electric Co., Ltd.) Light source: Metal halide lamp Test environment: 63°C (black panel temperature), 50% RH Illuminance: 50 mW / cm 2 (Wavelength 365 nm) Irradiation cycle: 24 hours (continuous irradiation)

[0206] After irradiation, the surface of the cured product of the curable resin layer (b) was evaluated for weather-resistant adhesion according to JIS K5600-5-6:1999 using the following criteria. The results are shown in Table 2 below. ⊚: The edges of the cuts are completely smooth and no peeling occurs in any of the grids. ◯: Peeling occurs in less than 40% of the grids. ×: Peeling occurs in 40% or more of the grids.

[0207] <Fingerprint Wiping Efficiency> The fingerprint wiping ability of the cured product obtained by curing the laminate was evaluated. The cured product used was the same as that produced for the pencil hardness evaluation.

[0208] A fingerprint was left on the surface of the cured product of the curable resin layer (b). The fingerprint was then wiped off with a cloth, and the ease of wiping off the fingerprint was evaluated according to the following criteria. The results are shown in Table 2 below. ◯: The fingerprint disappeared after 2 to 4 wipes. Δ: The fingerprint disappeared after 5 wipes. ×: The fingerprint disappeared after 6 or more wipes.

[0209]

[0210] The results in Table 2 show that the laminates of Examples 1 to 22 have excellent three-dimensional formability. In addition, it was found that the cured products obtained by curing the laminates of Examples 1 to 22 have high hardness.

Claims

1. A laminate comprising: a substrate layer (a); and a curable resin layer (b) containing a (meth)acryloyl polymer having an acrylic equivalent of 200 to 600 g / mol; wherein the substrate layer (a) contains 96% by mass or more of bisphenol A polycarbonate relative to the total mass of the substrate layer (a); and the intermediate glass transition temperature (Tmg) of the substrate layer (a) is 100 to 140°C.

2. The bisphenol A polycarbonate is a polycarbonate obtained by mixing bisphenol A, a carbonate binder, and a compound represented by the following formula (1): [In the above formula (1), R 1 is an alkyl group having 8 to 36 carbon atoms or an alkenyl group having 8 to 36 carbon atoms; R 2 each independently represents a hydrogen atom, a halogen atom, an alkyl group having 1 to 20 carbon atoms which may be substituted with a halogen atom or an aryl group having 6 to 12 carbon atoms, or an aryl group having 6 to 12 carbon atoms which may be substituted with a halogen atom, an alkyl group having 1 to 20 carbon atoms, or an aryl group having 6 to 12 carbon atoms which may be substituted with an aryl group having 6 to 12 carbon atoms.

3. The laminate according to claim 2, wherein the monohydric phenol end terminator represented by formula (1) comprises at least one selected from the group consisting of 2-hexyldecyl parahydroxybenzoate, hexadecyl parahydroxybenzoate, dodecyl parahydroxybenzoate, and 2-ethylhexyl parahydroxybenzoate.

4. The (meth)acryloyl polymer is represented by the following formula (2):

2. The laminate according to claim 1, comprising a repeating unit represented by the following formula (2): [in the above formula (2), m is a single bond or an alkylene group having 1 to 4 carbon atoms, n is hydrogen or an alkyl group having 1 to 4 carbon atoms, p is a single bond or an alkylene group having 1 to 2 carbon atoms, and q is hydrogen or an alkyl group having 1 to 12 carbon atoms which may be substituted with at least one substituent selected from the group consisting of an epoxy group, a hydroxyl group, and a (meth)acryloyl group].

5. The (meth)acryloyl polymer is represented by the following formulas (2-a) to (2-c): The laminate according to claim 4 , comprising at least one repeating unit represented by:

6. The laminate according to claim 1, wherein the (meth)acryloyl polymer has an acrylic equivalent of 200 to 500 g / mol.

7. The laminate according to claim 1, wherein the curable resin layer (b) further comprises a leveling agent.

8. The laminate according to claim 7, wherein the leveling agent comprises a fluorine-based leveling agent.

9. The laminate according to claim 1, wherein the curable resin layer (b) further comprises inorganic particles.

10. The laminate according to claim 9, wherein the inorganic particles have an average particle size of 20 to 60 nm.

11. The laminate according to claim 1, wherein the curable resin layer (b) further comprises a light stabilizer.

12. The laminate according to claim 1, wherein the curable resin layer (b) further contains a polymerization inhibitor.

13. The laminate according to claim 1, wherein the thickness of the curable resin layer (b) is 5 μm or more.

14. The laminate according to claim 1, further comprising an acrylic layer (c), wherein the substrate layer (a), the acrylic layer (c), and the curable resin layer (b) are laminated in this order.

15. The laminate according to claim 14, wherein the thickness of the acrylic layer (c) is 20 μm or more.

16. The laminate of claim 1, which is used for vacuum forming.

17. The laminate according to claim 1, which is used in TOM molding.

18. A cured product obtained by curing the laminate according to any one of claims 1 to 17.

Citation Information

Patent Citations

  • Thermoforming sheet, decorative sheet, and molding using them

    JP2021146687A

  • Resin plate, scratch-resistant resin plate using the same, protective plate for display, display window protective plate of portable information terminal, protective plate for touch panel, and method for manufacturing the resin plate

    JP2013086272A

  • Layered resin product, and transparent substrate material and transparent protective material using same

    WO2022034837A1

  • Multilayer body and method for producing same

    WO2022168811A1