Thermoplastic resin and optical lens including same

The development of a thermoplastic resin with specific structural units addresses the challenges of achieving high refractive index and heat resistance in optical lenses, offering improved optical properties and manufacturing efficiency.

WO2024237154A1PCT designated stage expired Publication Date: 2024-11-21MITSUBISHI GAS CHEM CO INC
View PDF 15 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2024/017197
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-05-12
Filing Date
2024-05-09
Publication Date
2024-11-21

AI Technical Summary

Technical Problem

Conventional optical lenses face challenges in achieving high refractive index and heat resistance while maintaining moldability and productivity, with existing materials like optical glass being costly and difficult to mold, and optical resins lacking in heat resistance and humidity tolerance.

Method used

A thermoplastic resin is developed using specific monomers with a defined structure, incorporating structural units derived from compounds represented by certain general formulas, which are then used to create polycarbonate, polyester carbonate, or polyester resins with enhanced optical properties such as refractive index, Abbe number, and photoelastic coefficient.

Benefits of technology

The resulting thermoplastic resin exhibits improved optical properties, including a high refractive index, low water absorption, and heat resistance, making it suitable for high-performance optical lenses with enhanced manufacturing efficiency and cost-effectiveness.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JP2024017197_21112024_PF_FP_ABST
    Figure JP2024017197_21112024_PF_FP_ABST
Patent Text Reader

Abstract

The present invention makes it possible to provide a thermoplastic resin including a structural unit (A) that is derived from a compound represented by general formula (1). (In the formula, each R1 independently represents a hydrogen atom or a linear or branched C1-4 alkyl group, each R2 independently represents a C1-4 alkylene group, and each R3 independently represents a linear, branched or cyclic C4-6 alkyl group.)
Need to check novelty before this filing date? Find Prior Art

Description

Thermoplastic resin and optical lens containing same

[0001] The present invention relates to a thermoplastic resin and an optical lens containing the same. More particularly, the present invention relates to a polycarbonate resin, a polyester carbonate resin, or a polyester resin, and an optical lens containing the same.

[0002] Optical glass or optical resin is used as a material for optical lenses used in the optical systems of various cameras, such as cameras with integrated film, video cameras, etc. Optical glass is excellent in heat resistance, transparency, dimensional stability, chemical resistance, etc., but has problems such as high material costs, poor moldability, and low productivity.

[0003] On the other hand, optical lenses made of optical resins have the advantage that they can be mass-produced by injection molding, and polycarbonate, polyester carbonate, polyester resin, etc. are used as high refractive index materials for camera lenses.

[0004] When an optical resin is used as an optical lens, in addition to optical properties such as refractive index and Abbe number, it is required to have heat resistance, transparency, low water absorption, chemical resistance, low birefringence, moist heat resistance, etc. In particular, in recent years, there has been a demand for optical lenses with high refractive index and high heat resistance, and various resins have been developed (Patent Documents 1 to 5).

[0005] JP 2018-2893 A JP 2018-2894 A JP 2018-2895 A JP 2018-59074 A WO2017 / 078073

[0006] An object of the present invention is to provide a thermoplastic resin having excellent optical properties such as refractive index, Abbe number, and photoelastic coefficient, and an optical lens using the same.

[0007] As a result of extensive research to solve the conventional problems, the inventors discovered that by using a monomer having a specific structure as a raw material, a thermoplastic resin having excellent optical properties such as refractive index, Abbe number, and photoelastic coefficient can be obtained, and thus completed the present invention.

[0008] That is, the present invention includes the following aspects: <1> A thermoplastic resin containing a structural unit (A) derived from a compound represented by the following general formula (1). (In the formula, R 1 each independently represents a hydrogen atom or a linear or branched alkyl group having 1 to 4 carbon atoms; R 2 each independently represents an alkylene group having 1 to 4 carbon atoms; R 3 and each independently represent a linear, branched, or cyclic alkyl group having 4 to 6 carbon atoms.) <2> The thermoplastic resin according to <1> above, wherein the compound represented by general formula (1) is a compound represented by the following general formula (1A) or (1B): (In the formula, R 1 , R 2 and R 3 is the same as defined in the general formula (1). <3> R in the compound represented by the general formula (1) 3 is a t-butyl group or a cyclohexyl group. <4> The thermoplastic resin according to <1> above, wherein the thermoplastic resin is a polycarbonate resin, a polyester carbonate resin, or a polyester resin. <5> The thermoplastic resin according to <1> above, wherein the thermoplastic resin contains a structural unit (B) derived from a monomer represented by the following general formula (6) and / or a structural unit (C) derived from a monomer represented by the following general formula (7): (In general formula (6), R a and R b each independently represents a hydrogen atom, a halogen atom, an alkyl group having 1 to 20 carbon atoms which may have a substituent, an alkoxyl group having 1 to 20 carbon atoms which may have a substituent, a cycloalkyl group having 5 to 20 carbon atoms which may have a substituent, a cycloalkoxyl group having 5 to 20 carbon atoms which may have a substituent, an aryl group having 6 to 20 carbon atoms which may have a substituent, a heteroaryl group having 6 to 20 carbon atoms which contains one or more hetero ring atoms selected from O, N and S and which may have a substituent, an aryloxy group having 6 to 20 carbon atoms which may have a substituent, and -C≡C-R h R is selected from the group consisting of hrepresents an aryl group having 6 to 20 carbon atoms which may have a substituent, or a heteroaryl group having 6 to 20 carbon atoms which contains one or more hetero ring atoms selected from O, N, and S and which may have a substituent; X represents a single bond or an optionally substituted fluorene group; A and B each independently represent an optionally substituted alkylene group having 1 to 5 carbon atoms; m and n each independently represent an integer of 0 to 6; and a and b each independently represent an integer of 0 to 10. (In general formula (7), R c and R d are each independently selected from the group consisting of a hydrogen atom, a halogen atom, an alkyl group having 1 to 20 carbon atoms which may have a substituent, an alkoxyl group having 1 to 20 carbon atoms which may have a substituent, a cycloalkyl group having 5 to 20 carbon atoms which may have a substituent, a cycloalkoxyl group having 5 to 20 carbon atoms which may have a substituent, and an aryl group having 6 to 20 carbon atoms which may have a substituent; 1 represents a single bond, a fluorene group which may have a substituent, or any of the structural formulae represented by the following formulae (8) to (15): (In formulas (8) to (15), R 61 , R 62 , R 71 , R 72 , R 81 and R 82 each independently represents a hydrogen atom, a halogen atom, an alkyl group having 1 to 20 carbon atoms which may have a substituent, or an aryl group having 6 to 30 carbon atoms which may have a substituent, or R 61 and R 62 , or R 71 and R 72represent a carbon ring or hetero ring having 1 to 20 carbon atoms, which may have a substituent, formed by bonding together, and r and s each independently represent an integer of 0 to 5,000.) A and B each independently represent an alkylene group having 1 to 5 carbon atoms, which may have a substituent, p and q each independently represent an integer of 0 to 4, and a and b each independently represent an integer of 0 to 10.) <6> The thermoplastic resin according to <5> above, wherein in general formula (6) and general formula (7), A and B each independently represent an alkylene group having 2 or 3 carbon atoms. <7> The thermoplastic resin according to <5> above, which contains at least a structural unit derived from any one of BPEF, BNE, BNEF, DPBHBNA, BPM, and BCFL. <8> The thermoplastic resin according to <1> above, further comprising a structural unit derived from at least one monomer selected from the following group of monomers: (In the above formula, R 1 and R 2 each independently represents a hydrogen atom, a methyl group, or an ethyl group; R 3 and R 4each independently represent an aryl group, a hydrogen atom, a methyl group, an ethyl group, or an alkylene glycol having 2 to 5 carbon atoms. i and ii each independently represent an integer of 1 to 3.) <9> The thermoplastic resin according to <1> above, wherein the thermoplastic resin has a polystyrene-equivalent weight average molecular weight (Mw) of 10,000 to 100,000. <10> The thermoplastic resin according to <1> above, wherein the thermoplastic resin has a refractive index (nD) of 1.500 to 1.700. <11> The thermoplastic resin according to <1> above, wherein the thermoplastic resin has an Abbe number (ν) of 22.0 to 35.0. <12> The thermoplastic resin according to <1> above, wherein the thermoplastic resin has a glass transition temperature of 125 to 150°C. <13> The thermoplastic resin according to <1> above, wherein the thermoplastic resin has a photoelastic coefficient of 25 to 45. <14> The thermoplastic resin according to <1>, wherein the thermoplastic resin has a water absorption rate of 0.40% or less. <15> The thermoplastic resin according to <1>, wherein the thermoplastic resin has a rate of dimensional change upon water absorption of 0.045% or less. <16> An optical lens comprising the thermoplastic resin according to <1>.

[0009] According to the present invention, it is possible to provide a thermoplastic resin having excellent optical properties such as refractive index, Abbe number, and photoelastic coefficient, and an optical lens containing the same.

[0010] FIG. 1 is a chart showing differential scanning calorimetry (DSC) data for the crystals of bis[1-methyl-1-(4-hydroxyethoxy-3-cyclohexyl-6-methylphenyl)ethyl]benzene obtained in Synthesis Example 1. FIG. 2 is a chart showing powder X-ray diffraction (PXRD) measurement for the crystals of bis[1-methyl-1-(4-hydroxyethoxy-3-cyclohexyl-6-methylphenyl)ethyl]benzene obtained in Synthesis Example 1.

[0011] Hereinafter, the present invention will be described in detail by way of examples and synthesis examples. However, the present invention is not limited to the synthesis examples and examples exemplified, and can be carried out by any method as long as it does not significantly deviate from the content of the present invention.

[0012] <Thermoplastic Resin> One embodiment of the present invention is a thermoplastic resin containing a structural unit (A) derived from a compound represented by the following general formula (1). (In the formula, R 1 each independently represents a hydrogen atom or a linear or branched alkyl group having 1 to 4 carbon atoms; R 2 each independently represents an alkylene group having 1 to 4 carbon atoms; R 3 each independently represents a linear, branched, or cyclic alkyl group having 4 to 6 carbon atoms.

[0013] R in general formula (1) 1 Specific examples of the linear or branched alkyl group having 1 to 4 carbon atoms include a methyl group, an ethyl group, an isopropyl group, and a t-butyl group. 1 are each independently preferably a hydrogen atom, a methyl group, an ethyl group, an isopropyl group, or a t-butyl group, more preferably a hydrogen atom or a methyl group, and particularly preferably both are a methyl group. 1 As for the two R 1 It is preferable that both of R in the general formula (1) are the same substituent. 1 is a linear or branched alkyl group having 1 to 4 carbon atoms, the position at which it is bonded to the benzene ring is 3 is bonded to the 3-position, and when the oxygen atom is bonded to the 4-position, it is preferably bonded to the 5-position or the 6-position. 2 are each independently preferably a methylene group, a 1,2-ethylene group, a 1-methyl-1,2-ethylene group, or a 2-methyl-1,2-ethylene group, and are particularly preferably a 1,2-ethylene group. 2 As for the two R 2 It is preferable that both of R in the general formula (1) are the same substituent. 3are each independently preferably a branched or cyclic alkyl group having 4 to 6 carbon atoms, each independently preferably a branched tertiary alkyl group having 4 to 6 carbon atoms or a cyclic alkyl group having 5 or 6 carbon atoms, each independently preferably a t-butyl group or a cyclohexyl group, and both are particularly preferably a cyclohexyl group. 3 As for the two R 3 are preferably the same substituents.

[0014] The compound (1) of the present invention is preferably a compound represented by general formula (1A) (hereinafter may be referred to as compound (1A)) or a compound represented by general formula (1B) (hereinafter may be referred to as compound (1B)), and the compound represented by general formula (1A) is particularly preferred. R in general formula (1A) and general formula (1B) 1 , R 2 , and R 3 is the same as that in formula (1), and the preferred embodiments are also the same.

[0015] Specific examples of the compound (1) of the present invention include compounds represented by formulas (1-1) to (1-10). The compounds represented by formulas (1-1) to (1-5) are specific examples of compound (1A). Among them, compounds (1-1), (1-2), (1-4), and (1-5) are preferred, compounds (1-2), (1-4), and (1-5) are more preferred, compounds (1-2) and (1-4) are even more preferred, and compound (1-2) is particularly preferred. The compounds represented by formulas (1-6) to (1-10) are specific examples of compound (1B). Among them, compounds (1-6), (1-7), (1-9), and (1-10) are preferred, compounds (1-7), (1-9), and (1-10) are more preferred, compounds (1-7) and (1-9) are even more preferred, and compound (1-7) is particularly preferred.

[0016] <Method for producing the compound represented by general formula (1)> There are no particular limitations on the starting materials and production method used in the production of the bis[1-methyl-1-(4-hydroxyalkoxy-3-alkylphenyl)ethyl]benzene] compound represented by general formula (1) used in the present invention. For example, there may be mentioned a production method in which a bisphenol compound represented by the following general formula (2) is reacted with a hydroxyalkylene oxidizing agent: (In the formula, R 1 and R 3 is the same as defined in general formula (1).

[0017] R in the bisphenol compound represented by general formula (2) (hereinafter, sometimes referred to as compound (2)) 1 and R 3 is the same as that of general formula (1), and preferred embodiments are also the same. Compound (2) is preferably a compound represented by general formula (2A) (hereinafter may be referred to as compound (2A)) or a compound represented by general formula (2B) (hereinafter may be referred to as compound (2B)), and a compound represented by general formula (2A) is particularly preferred. (In the formula, R 1 and R 3 is the same as defined in general formula (1). R in general formula (2A) and general formula (2B) 1 and R 3 is the same as that in the general formula (1), and the preferred embodiments are also the same. Specific examples of the compound (2) include compounds represented by formulas (2-1) to (2-10). The compounds represented by formulas (2-1) to (2-5) are specific examples of compound (2A). Among them, compounds (2-1), (2-2), (2-4), and (2-5) are preferred, compounds (2-2), (2-4), and (2-5) are more preferred, compounds (2-2) and (2-4) are even more preferred, and compound (2-2) is particularly preferred. The compounds represented by formulas (2-6) to (2-10) are specific examples of compound (2B). Among them, compounds (2-6), (2-7), (2-9), and (2-10) are preferred, compounds (2-7), (2-9), and (2-10) are more preferred, compounds (2-7) and (2-9) are even more preferred, and compound (2-7) is particularly preferred.

[0018] The hydroxyalkylene oxidizing agent may be, for example, a carbonate (3) represented by the following general formula (3), such as ethylene carbonate or propylene carbonate, a halogenated alcohol such as 2-chloroethanol or 3-chloro-1-propanol, or an alkylene oxide such as ethylene oxide, depending on the target compound. The hydroxyalkylene oxidizing agent used is preferably a carbonate (3) represented by the general formula (3). (In the formula, R 2 is the same as defined in general formula (1). 2 is the same as that in general formula (1), and the preferred embodiments are also the same. The reaction formula for obtaining the compound used in the present invention when a carbonate (3) represented by general formula (3) is used as the hydroxyalkylene oxidizing agent is exemplified below. In addition, the following reaction scheme is exemplified when a hydroxyalkylene oxidizing reaction is carried out using compound (2-2) as compound (2) and ethylene carbonate as a hydroxyalkylene oxidizing agent to obtain compound (1-2) as compound (1). The method for producing the compound (1) when the carbonate (3) is used as the alkylene oxidizing agent as shown in the above reaction scheme will be described below.

[0019] (Amount of Raw Materials Used) The raw material molar ratio of compound (2) to carbonates (3), compound (2) / carbonates (3), is usually in the range of 1 / 2 to 1 / 5, preferably in the range of 1 / 2 to 1 / 4, more preferably in the range of 1 / 2 to 1 / 3, and particularly preferably in the range of 1 / 2 to 1 / 2.5.

[0020] (Basic Catalyst) In the above production method, it is preferable to use a basic catalyst during the reaction, and commonly known basic catalysts can be used. Specific examples include triorganophosphine compounds such as triphenylphosphine and tributylphosphine, amine catalysts such as 1-methylimidazole, and alkali catalysts such as potassium carbonate, calcium carbonate, magnesium carbonate, magnesium hydroxide, calcium hydroxide, sodium hydroxide, sodium bicarbonate, methoxysodium, and phenoxysodium. These basic catalysts may be used alone or in combination of two or more. The amount of the basic catalyst used is 0.001 to 10 wt %, preferably 0.01 to 5 wt %, and more preferably 0.1 to 5 wt %, of compound (2).

[0021] (Reaction Solvent) While the reaction can be carried out without a solvent by using an excess amount of carbonate (3), it is generally preferable to carry out the reaction using an organic solvent from the viewpoints of economy and operability. When a reaction solvent is used, various known solvents that are inert to the reaction can be used. Examples of such reaction solvents include aromatic hydrocarbon solvents such as toluene and xylene, ether solvents such as tetrahydrofuran, dioxane, and 1,2-dimethoxyethane, aliphatic ketone solvents such as acetone and methyl isobutyl ketone, halogenated hydrocarbon solvents such as chloroform and 1,2-dichloroethane, aliphatic alcohol solvents such as butanol and ethylene glycol, and polar solvents such as dimethylformamide and dimethyl sulfoxide. Among these, aromatic hydrocarbon solvents having 6 to 9 carbon atoms or aliphatic ketone solvents having 3 to 9 carbon atoms are preferred. There are no particular restrictions on the amount of reaction solvent used, but it is preferably in the range of 0.5 to 10 times by weight, and more preferably 0.5 to 5 times by weight, relative to compound (2).

[0022] (Phase Transfer Catalyst) In the above production method, it is preferable to use a phase transfer catalyst during the reaction, and commonly known phase transfer catalysts can be used. Specific examples of phase transfer catalysts that can be preferably used include quaternary ammonium salts or quaternary phosphonium salts, with quaternary ammonium salts being more preferred. Specific examples of quaternary ammonium salts include tetrabutylammonium chloride, tetrabutylammonium bromide, tetraethylammonium chloride, tetraethylammonium bromide, tetramethylammonium chloride, and tetramethylammonium bromide. Specific examples of quaternary phosphonium salts include tetrabutylphosphonium chloride, tetrabutylphosphonium bromide, and tetraphenylphosphonium bromide. These phase transfer catalysts may be used alone or in combination of two or more. The amount of this phase transfer catalyst used is in the range of 0.001 to 10% by weight, preferably 0.01 to 1% by weight, of compound (2).

[0023] (Reaction Conditions) The reaction temperature is not particularly limited as long as it is a temperature at which the reaction proceeds, but is usually carried out under heating. For example, although it depends on the type of solvent used, it is usually carried out in the range of 50 to 250°C, preferably in the range of 70 to 200°C, and more preferably in the range of 100 to 180°C. It is more preferable to carry out the reaction under solvent reflux. The reaction time depends on the reaction temperature, the amount and type of compound (2), carbonate (3), basic catalyst, reaction solvent, and phase transfer catalyst used, etc., but is usually about 3 to 48 hours. In this reaction, the time when the generation of carbon dioxide gas has subsided can be used as a guide for the completion of the reaction.

[0024] (Neutralization Step) When a basic catalyst is used in the above production method, it is preferable to carry out a neutralization step in which the basic catalyst is neutralized by adding an acid-containing water (e.g., hydrochloric acid, sulfuric acid), acetic acid, propionic acid, etc. to the obtained reaction solution. This neutralization step may be carried out after the hydrolysis step described below.

[0025] (Hydrolysis Step) In the reaction of the above production method, an excess amount of carbonates (3) is added, so carbonates (3) remain in the reaction solution even after completion of the reaction. If treatment such as heating is performed in this state, side reactions may proceed, and the purity and yield of the target compound, compound (1), may decrease. Therefore, it is preferable to add water to carry out the hydrolysis step of carbonates (3). The amount of water used is in the range of 1 to 10 moles relative to the amount of carbonates (3) used in the above reaction. The temperature may be below the boiling point of the reaction solution, but is usually in the range from room temperature to below the boiling point of the reaction solution. Specifically, the lower limit is 10°C or higher, more preferably 20°C or higher. The upper limit depends on the boiling point of the solvent used, but is preferably 150°C or lower.

[0026] (Post-treatment step) Thereafter, if necessary, in order to remove water-soluble impurities such as the basic catalyst, salts produced in the neutralization step, and glycols produced in the hydrolysis step, a water-washing step may be performed, preferably a water-washing step, in which a solvent that dissolves compound (1) and separates it from water (e.g., an aliphatic ketone solvent having 5 to 9 carbon atoms) is added to form a solution, and the solution is washed with water. The solution that has undergone the above steps can be subjected to steps such as crystallization, filtration, distillation, separation by column chromatography, etc., and a drying step, to obtain the target compound, compound (1). To further increase the purity, further purification by distillation, recrystallization, or column chromatography may be performed in accordance with conventional methods.

[0027] Another method for producing the bis[1-methyl-1-(4-hydroxyalkoxy-3-alkylphenyl)-1-methylethyl]benzene compound represented by the general formula (1) of the present invention includes a production method in which a 4-hydroxyalkoxy-3-alkylbenzene (benzene (4)) represented by the general formula (4) is reacted with a diol (5) represented by the general formula (5). (In the formula, R 1 , R 2 and R 3 is the same as defined in general formula (1).

[0028] <4-hydroxyalkoxy-3-alkylbenzenes represented by general formula (4)> R in the benzenes (4) 1 , R 2 and R 3 is the same as that in the general formula (1), and the preferred embodiments are also the same. Specific examples of the benzenes (4) include compounds represented by the formulae (4-1) to (4-5). Among these, compounds (4-1), (4-2), (4-4) and (4-5) are preferred, compounds (4-1), (4-2) and (4-5) are more preferred, compounds (4-1) and (4-2) are further preferred, and compound (4-2) is particularly preferred.

[0029] <Diol (5) Represented by General Formula (5)> Specific examples of diol (5) include 1,4-di(2-hydroxyisopropyl)benzene, 1,3-di(2-hydroxyisopropyl)benzene, and 1,2-di(2-hydroxyisopropyl)benzene. Among these, 1,4-di(2-hydroxyisopropyl)benzene or 1,3-di(2-hydroxyisopropyl)benzene is preferred, and 1,3-di(2-hydroxyisopropyl)benzene is particularly preferred.

[0030] In this production method, the amount of the benzene (4) used is preferably in the range of 5 to 12 mol, more preferably in the range of 7 to 10 mol, and even more preferably 8 mol, per mol of the diol (5).

[0031] The above production method is preferably carried out in the presence of an acid catalyst. Preferred acid catalysts include concentrated hydrochloric acid, sulfuric acid, and hydrochloric acid gas. It is particularly preferred to use hydrochloric acid gas until the reaction solution is saturated. The reaction is usually carried out in the presence of a solvent. There are no particular limitations on the solvent, as long as it does not inhibit the reaction. The above production method may be carried out in either air or an inert gas atmosphere; however, to suppress coloration of the reaction product, an inert gas atmosphere such as nitrogen or argon is preferred. The reaction temperature is usually in the range of 20 to 60°C, preferably in the range of 20 to 40°C. The reaction pressure may be normal pressure, or may be increased or reduced pressure, but normal pressure is preferred. The resulting reaction mixture can be separated and purified according to conventional methods to obtain compound (1).

[0032] <Crystals of Compound Represented by Formula (1-2)> Of the compounds (1) used in the present invention, crystals of the compound represented by formula (1-2) (compound (1-2): 1,3-bis[1-methyl-1-{4-(2-hydroxyethoxy)-3-cyclohexyl-6-methylphenyl}ethyl]benzene) are very useful because compound (1-2) can be handled as a crystalline solid and is therefore easy to handle and transport in industrial production. The crystals of compound (1-2) used in the present invention have an endothermic peak top temperature measured by differential scanning calorimetry in the range of 205 to 215°C, more preferably 206 to 214°C, even more preferably 207 to 213°C, and particularly preferably 207 to 211°C. Furthermore, the crystals of compound (1-2) used in the present invention have diffraction peaks at diffraction angles 2θ of 7.1±0.2°, 14.6±0.2°, and 16.1±0.2° in a powder X-ray diffraction peak pattern using Cu-Kα radiation. In addition, it is more preferable that the crystals have peaks at diffraction angles 2θ of 20.4±0.2°, 21.4±0.2°, 22.0±0.2°, and 23.3±0.2°. Furthermore, it is even more preferable that the crystals have peaks at diffraction angles 2θ of 11.8±0.2°, 12.4±0.2°, and 18.5±0.2°. The purity of the crystals of compound (1-2) used in the present invention is preferably 90% or more, more preferably 93% or more, even more preferably 95% or more, and particularly preferably 98% or more, in terms of area percentage by liquid chromatography analysis.

[0033] <Method for Producing Crystals of Compound Represented by Formula (1-2)> Crystals of compound (1-2) used in the present invention can be obtained by precipitating crystals from a solution containing compound (1-2) and an aliphatic ketone solvent having 5 to 9 carbon atoms. Crystals of compound (1-2) can be obtained by cooling a solution in which compound (1-2) is dissolved in an aliphatic ketone solvent having 5 to 9 carbon atoms, or by distilling off the aliphatic ketone solvent having 5 to 9 carbon atoms from the solution, thereby precipitating crystals. Alternatively, crystals can be obtained by mixing a hydrocarbon solvent with the solution. Among these, it is preferable to prepare a solution in which an aromatic hydrocarbon solvent having 6 to 9 carbon atoms is further added to a solution containing compound (1-2) and an aliphatic ketone solvent having 5 to 9 carbon atoms, and if necessary, to further reduce the solubility of compound (1-2), thereby precipitating the crystals. Examples of aliphatic ketone solvents having 5 to 9 carbon atoms include chain aliphatic ketone solvents having 5 to 9 carbon atoms, such as diethyl ketone (5 carbon atoms), methyl isobutyl ketone (6 carbon atoms), methyl amyl ketone (7 carbon atoms), and methyl hexyl ketone (8 carbon atoms), as well as cyclic aliphatic ketone solvents having 5 to 9 carbon atoms, such as cyclopentanone and cyclohexanone. Among these, cyclic aliphatic ketone solvents having 5 to 9 carbon atoms are preferred, with cyclopentanone or cyclohexanone being more preferred, and cyclohexanone being particularly preferred. By using such cyclic aliphatic ketone solvents having 5 to 9 carbon atoms, it is possible to wash the solution with water before precipitating crystals and remove water-soluble impurities, such as the basic catalyst, salts produced in the neutralization step, and glycols produced in the hydrolysis step. The amount of the aliphatic ketone solvent used is preferably in the range of 1 to 20 times by weight, more preferably 2 to 15 times by weight, even more preferably 2 to 10 times by weight, and particularly preferably 2 to 8 times by weight, relative to the weight of compound (1-2). Examples of aromatic hydrocarbon solvents having 6 to 9 carbon atoms include benzene, toluene, and xylene. Of these, aromatic hydrocarbon solvents having 7 or 8 carbon atoms are preferred, and toluene is particularly preferred. Examples of hydrocarbon solvents other than aromatic hydrocarbon solvents having 6 to 9 carbon atoms include linear or cyclic aliphatic hydrocarbon solvents having 5 to 10 carbon atoms.Specific examples of such a solvent include pentane, hexane, heptane, octane, isooctane, cyclopentane, and cyclohexane. Among these, a chain aliphatic hydrocarbon solvent having 6 to 8 carbon atoms or a cyclic aliphatic hydrocarbon solvent having 5 or 6 carbon atoms is preferred, with heptane, octane, isooctane, cyclopentane, or cyclohexane being more preferred. The amount of the hydrocarbon solvent used is preferably 1 to 10 times by weight, more preferably 1 to 7 times by weight, and even more preferably 1 to 5 times by weight, relative to the amount of compound (1-2). Furthermore, the amount of the hydrocarbon solvent used is preferably 0.1 to 4.0 times by weight, more preferably 0.2 to 2.0 times by weight, even more preferably 0.2 to 1.5 times by weight, and particularly preferably 0.2 to 1.0 times by weight, relative to the amount of the aliphatic ketone solvent having 5 to 9 carbon atoms. The temperature at which the hydrocarbon solvent is mixed with the solution of compound (1-2) in an aliphatic ketone having 5 to 9 carbon atoms varies depending on the aliphatic ketone used, but is preferably in the range of 50 to 120° C., more preferably in the range of 50 to 100° C., and even more preferably in the range of 50 to 90° C. The temperature at which crystals of compound (1-2) begin to precipitate is preferably in the range of 10 to 80° C., and more preferably in the range of 30 to 70° C.

[0034] The crystals obtained by the above method can be isolated by a conventional method, for example, by centrifugal filtration. It is also preferable to further wash the crystals with a solvent. The solvent used can be removed by drying the obtained crystals.

[0035] All steps in the above-mentioned production method for compound (1) used in the present invention, such as the hydroxyalkylene oxylation reaction step, neutralization step, hydrolysis step, crystallization step, filtration step, raw material mixing step, distillation step, and drying step, are preferably carried out in an atmosphere with little oxygen, which can cause oxidative deterioration, coloration, and electrostatic ignition due to volatile solvents, or in an inert gas atmosphere such as nitrogen or argon.

[0036] The thermoplastic resin according to one embodiment of the present invention is not particularly limited and may be a polyester resin, a polycarbonate resin, a polyester carbonate resin, an epoxy resin, a polyurethane resin, a polyacrylic acid ester resin, a polymethacrylic acid ester resin, or the like. However, it is preferably a polycarbonate resin, a polyester carbonate resin, or a polyester resin, and more preferably contains a structural unit (A) represented by the following formula: (In the formula, R 1 , R 2 and R 3 is the same as defined in general formula (1).

[0037] In a thermoplastic resin according to one embodiment of the present invention, the proportion of the structural unit (A) represented by the above formula relative to all structural units is not particularly limited, but is preferably 1 to 80 mol %, more preferably 1 to 60 mol %, and particularly preferably 5 to 50 mol % of all structural units. In other words, in addition to the structural unit (A) represented by the above formula, the thermoplastic resin according to one embodiment of the present invention can contain structural units derived from aliphatic dihydroxy compounds and structural units derived from aromatic dihydroxy compounds, which are generally used as structural units in polycarbonate resins and polyester carbonate resins. Specific examples of aliphatic dihydroxy compounds include, but are not limited to, 1,4-cyclohexanedimethanol, tricyclodecane dimethanol, 1,3-adamantanedimethanol, 2,2-bis(4-hydroxycyclohexyl)-propane, 3,9-bis(2-hydroxy-1,1-dimethylethyl)-2,4,8,10-tetraoxaspiro[5.5]undecane, 2-(5-ethyl-5-hydroxymethyl-1,3-dioxan-2-yl)-2-methylpropan-1-ol, isosorbide, 1,3-propanediol, 1,4-butanediol, and 1,6-hexanediol. Examples of aromatic dihydroxy compounds include various compounds, particularly 2,2-bis(4-hydroxyphenyl)propane (bisphenol A), bis(4-hydroxyphenyl)methane, 1,1-bis(4-hydroxyphenyl)ethane, 2,2-bis(4-hydroxy-3,5-dimethylphenyl)propane, 4,4'-dihydroxydiphenyl, bis(4-hydroxyphenyl)cycloalkane, bis(4-hydroxyphenyl)oxide, bis(4-hydroxyphenyl)sulfide, bis(4-hydroxyphenyl)sulfone, bis(4-hydroxyphenyl)sulfoxide, bis(4-hydroxyphenyl)ketone, bisphenoxyethanolfluorene, and the like.

[0038] Furthermore, the thermoplastic resin according to one embodiment of the present invention preferably contains a structural unit (B) derived from a monomer represented by the following general formula (6). In general formula (6), R a and Rb each independently represents a halogen atom, an alkyl group having 1 to 20 carbon atoms which may have a substituent, an alkoxyl group having 1 to 20 carbon atoms which may have a substituent, a cycloalkyl group having 5 to 20 carbon atoms which may have a substituent, a cycloalkoxyl group having 5 to 20 carbon atoms which may have a substituent, an aryl group having 6 to 20 carbon atoms which may have a substituent, a heteroaryl group having 6 to 20 carbon atoms which contains one or more hetero ring atoms selected from O, N and S and which may have a substituent, an aryloxy group having 6 to 20 carbon atoms which may have a substituent, and -C≡C-R h R h represents an aryl group having 6 to 20 carbon atoms which may have a substituent, or a heteroaryl group having 6 to 20 carbon atoms which contains one or more hetero ring atoms selected from O, N and S and which may have a substituent. a and R b is preferably a hydrogen atom, an aryl group having 6 to 20 carbon atoms which may have a substituent, or a heteroaryl group having 6 to 20 carbon atoms which contains one or more hetero ring atoms selected from O, N and S and which may have a substituent, more preferably a hydrogen atom, or an aryl group having 6 to 20 carbon atoms which may have a substituent, and even more preferably a hydrogen atom, or an aryl group having 6 to 12 carbon atoms which may have a substituent.

[0039] In general formula (6), X represents a single bond or a fluorene group which may have a substituent. X is preferably a single bond or a fluorene group which may have a substituent and has a total of 12 to 20 carbon atoms. In general formula (6), A and B each independently represent an alkylene group having 1 to 5 carbon atoms which may have a substituent, preferably an alkylene group having 2 or 3 carbon atoms. In general formula (6), m and n each independently represent an integer of 0 to 6, preferably an integer of 0 to 3, and more preferably 0 or 1. In general formula (6), a and b each independently represent an integer of 0 to 10, preferably an integer of 1 to 3, and more preferably 1 or 2.

[0040] Specific examples of the structural unit (B) include those derived from 2,2'-bis(2-hydroxyethoxy)-1,1'-binaphthalene (BNE), DPBHBNA, and the like.

[0041] Furthermore, the thermoplastic resin according to one embodiment of the present invention preferably contains a structural unit (C) derived from a monomer represented by the following general formula (7). In general formula (7), R c and R d are each independently selected from the group consisting of a halogen atom, an alkyl group having 1 to 20 carbon atoms which may have a substituent, an alkoxyl group having 1 to 20 carbon atoms which may have a substituent, a cycloalkyl group having 5 to 20 carbon atoms which may have a substituent, a cycloalkoxyl group having 5 to 20 carbon atoms which may have a substituent, and an aryl group having 6 to 20 carbon atoms which may have a substituent. c and R d is preferably a hydrogen atom, an aryl group having 6 to 20 carbon atoms which may have a substituent, or a heteroaryl group having 6 to 20 carbon atoms which contains one or more hetero ring atoms selected from O, N and S and which may have a substituent, more preferably a hydrogen atom, or an aryl group having 6 to 20 carbon atoms which may have a substituent, and even more preferably a hydrogen atom, or an aryl group having 6 to 12 carbon atoms which may have a substituent.

[0042] In the general formula (7), Y 1 represents a single bond, a fluorene group which may have a substituent, or any of the structural formulae represented by the following formulas (8) to (15), and is preferably a single bond or the structural formula represented by the following formula (8): In formulas (8) to (15), R 61 , R 62 , R 71 , R 72 , R 81 and R 82 each independently represents a hydrogen atom, a halogen atom, an alkyl group having 1 to 20 carbon atoms which may have a substituent, or an aryl group having 6 to 30 carbon atoms which may have a substituent, or R 61 and R 62 , or R 71 and R72 are bonded to each other to form a carbon ring or hetero ring having 1 to 20 carbon atoms, which may have a substituent. In formulas (8) to (15), r and s each independently represent an integer of 0 to 5,000.

[0043] In the general formula (7), A and B each independently represent an alkylene group having 1 to 5 carbon atoms, which may have a substituent, and preferably an alkylene group having 2 or 3 carbon atoms. In the general formula (7), p and q each independently represent an integer of 0 to 4, and preferably 0 or 1. In the general formula (7), a and b each independently represent an integer of 0 to 10, preferably an integer of 0 to 5, and more preferably an integer of 0 to 2, for example, 0 or 1.

[0044] Specific examples of the structural unit (C) include BCFL (9,9-bis(4-hydroxy-3-methylphenyl)fluorene), BPEF (9,9-bis(4-(2-hydroxyethoxy)phenyl)fluorene), BPPEF (9,9-bis(4-(2-hydroxyethoxy)-3-phenylphenyl)fluorene), BNEF (9,9-bis[6-(2-hydroxyethoxy)naphthalen-2-yl]fluorene), bisphenol A, bisphenol AP, bisphenol AF, bisphenol B, bisphenol BP, bisphenol C, bis(4-hydroxyphenyl)-2,2-dichloroethylene, bisphenol E, bisphenol F, bisphenol G, bisphenol M (BPM), bisphenol S, bisphenol P, bisphenol PH, bisphenol TMC, bisphenol P-AP (4,4'-(1-phenylethylidene)bisphenol), bisphenol P-CDE (4,4'-cyclohexyl methyl ether ... rhododecylidene bisphenol), bisphenol P-HTG (4,4'-(3,3,5-trimethylcyclohexylidene)bisphenol), bisphenol P-MIBK (4,4'-(1,3-dimethylbutylidene)bisphenol), bisphenol PEO-FL (bisphenoxyethanolfluorene), bisphenol P-3MZ (4-[1-(4-hydroxyphenyl)-3-methylcyclohexyl]phenol), bisphenol OC-F Examples of the structural unit (C) include those derived from L(4,4'-[1-[4-[1-(4-hydroxyphenyl)-1-methylethyl]phenyl]ethylidene]bisphenol), bisphenol Z, BP-2EO (2,2'-[[1,1'-biphenyl]-4,4'-diylbis(oxy)bisethanol), S-BOC (4,4'-(1-methylethylidene)bis(2-methylphenol),) TrisP-HAP (4,4',4''-ethylidene trisphenol), etc. Among these, preferred examples of the structural unit (C) are those derived from BPEF, BNEF, BPM, or BCFL.

[0045] The thermoplastic resin according to one embodiment of the present invention may contain a structural unit derived from a monomer represented by the following general formula (8). In the general formula (8), L1 each independently represents a divalent linking group; R 3 and R 4 each independently represents a halogen atom or a substituent having 1 to 20 carbon atoms which may contain an aromatic group; j3 and j4 each independently represents an integer of 0 to 4; and t represents an integer of 0 or 1.

[0046] The thermoplastic resin according to one embodiment of the present invention essentially contains the structural unit (A), but may also be a polymer containing the structural unit (B) but not the structural unit (C), a polymer containing the structural unit (C) but not the structural unit (B), a copolymer containing the structural unit (B) and the structural unit (C), a mixture of a polymer containing the structural unit (B) and a polymer containing the structural unit (C), or a combination thereof. Examples of polymers containing the structural unit (C) but not the structural unit (B) include those having structural units represented by the following formulas (I-1) to (I-3), and examples of copolymers having the structural unit (B) and the structural unit (C) include those having structural units represented by the following formulas (II-1) to (II-4). (In formula (I-1), m and n each represent an integer of 1 to 10, preferably an integer of 1 to 5, and more preferably 1; the number of repeating units in formula (I-3) is an integer of 1 to 10, preferably an integer of 1 to 5, and more preferably 1.) Furthermore, as the polymer having multiple types of structural units, either a block copolymer in which the values ​​of m and n are large, for example, 100 or more, or a random copolymer can be used, but a random copolymer is preferred, and more preferably a random copolymer in which the values ​​of m and n are 1 is used. (In formulas (II-1) to (II-4), m and n each independently represent an integer of 1 to 10, preferably an integer of 1 to 5, and more preferably 1.) Furthermore, as the polymer having multiple types of structural units, either a block copolymer in which the values ​​of m and n are large, for example, 100 or greater, or a random copolymer can be used, although a random copolymer is preferred, and more preferably a random copolymer in which the values ​​of m and n are 1. In the copolymer, the molar ratio of structural unit (B) to structural unit (C) is preferably 1:99 to 99:1, more preferably 10:90 to 90:10, even more preferably 15:85 to 85:15, and particularly preferably 30:70 to 70:30. Furthermore, in the mixture, the mass ratio of the polymer having the structural unit (B) to the polymer having the structural unit (C) is preferably 1:99 to 99:1, more preferably 10:90 to 90:10, even more preferably 15:85 to 85:15, and particularly preferably 30:70 to 70:30.

[0047] The thermoplastic resin according to one embodiment of the present invention preferably further contains a structural unit derived from at least one monomer selected from the following group of monomers: (In the above formula, R 1 and R 2 each independently represents a hydrogen atom, a methyl group, or an ethyl group; R 3 and R 4 each independently represents an aryl group, a hydrogen atom, a methyl group, an ethyl group, or an alkylene glycol having 2 to 5 carbon atoms; and i and ii each independently represent an integer of 1 to 3.

[0048] In a preferred embodiment of the polycarbonate resin of the present invention, impurities such as alcohol compounds such as phenolic compounds that may be generated as by-products during production, and diol components or carbonate diesters that remain unreacted may be present. The impurities, such as alcohol compounds such as phenolic compounds and carbonate diesters, may cause a decrease in strength or the generation of odor when molded into a product, so it is preferable that the content of these impurities is as small as possible.

[0049] The content of residual phenolic compounds is preferably 3,000 ppm by mass or less, more preferably 1,000 ppm by mass or less, and particularly preferably 300 ppm by mass or less, based on 100% by mass of the polycarbonate resin. The content of residual diol components is preferably 1,000 ppm by mass or less, more preferably 100 ppm by mass or less, and particularly preferably 10 ppm by mass or less, based on 100% by mass of the polycarbonate resin. The content of residual carbonate diesters is preferably 1,000 ppm by mass or less, more preferably 100 ppm by mass or less, and particularly preferably 10 ppm by mass or less, based on 100% by mass of the polycarbonate resin. In particular, it is preferable that the contents of compounds such as phenol and t-butylphenol are low, and it is preferable that the contents of these compounds are within the above ranges.

[0050] The content of phenolic compounds remaining in the polycarbonate resin can be measured by a method of analyzing phenolic compounds extracted from the polycarbonate resin using gas chromatography. The content of alcoholic compounds remaining in the polycarbonate resin can also be measured by a method of analyzing alcoholic compounds extracted from the polycarbonate resin using gas chromatography. The content of diol components and carbonate diesters remaining in the polycarbonate resin can also be measured by a method of extracting these compounds from the polycarbonate resin and analyzing them using gas chromatography.

[0051] The contents of by-produced alcohol compounds such as phenolic compounds, diol components, and carbonate diesters may be reduced to an undetectable level, but from the viewpoint of productivity, they may be contained in small amounts within a range that does not impair the effects. Furthermore, small amounts can improve the plasticity of the resin when it is melted.

[0052] The content of each of the remaining phenolic compounds, diol components, and carbonate diesters may be, for example, 0.01 ppm by mass or more, 0.1 ppm by mass or more, or 1 ppm by mass or more, relative to 100% by mass of the polycarbonate resin. The content of the remaining alcoholic compounds may be, for example, 0.01 ppm by mass or more, 0.1 ppm by mass or more, or 1 ppm by mass or more, relative to 100% by mass of the polycarbonate resin.

[0053] The contents of by-produced alcohol compounds such as phenolic compounds, diol components, and carbonate diesters in the polycarbonate resin can be adjusted to fall within the above ranges by appropriately adjusting the polycondensation conditions and apparatus settings, and can also be adjusted by the conditions of the extrusion step after polycondensation.

[0054] For example, the amount of residual by-produced alcohol compounds such as phenolic compounds is related to the type of carbonate diester used in the polymerization of the polycarbonate resin, the polymerization reaction temperature, the polymerization pressure, etc. By adjusting these factors, the amount of residual by-produced alcohol compounds such as phenolic compounds can be reduced.

[0055] For example, when a polycarbonate resin is produced using a dialkyl carbonate such as diethyl carbonate, the molecular weight is difficult to increase, resulting in a low-molecular-weight polycarbonate, and the content of by-product alkyl alcohol compounds tends to be high. Such alkyl alcohols are highly volatile, and if they remain in the polycarbonate resin, the moldability of the resin tends to deteriorate. Furthermore, if a large amount of by-product alcohol compounds such as phenolic compounds remain, odor problems may occur during resin molding, or the cleavage reaction of the resin skeleton may progress during compounding, resulting in a decrease in molecular weight. Therefore, it is preferable that the content of by-product alcohol compounds remaining in the obtained polycarbonate resin be 3,000 ppm by mass or less relative to 100% by mass of the polycarbonate resin. The content of the remaining alcohol compounds is preferably 3,000 ppm by mass or less, more preferably 1,000 ppm by mass or less, and particularly preferably 300 ppm by mass or less, relative to 100% by mass of the polycarbonate resin.

[0056] <Physical Properties of Thermoplastic Resin> (1) Refractive Index (nD) In ​​one embodiment of the present invention, one of the characteristics of the thermoplastic resin is that it has a high refractive index, and the refractive index is preferably 1.500 to 1.700, more preferably 1.550 to 1.700, and particularly preferably 1.580 to 1.650. In the present invention, the refractive index can be measured by the method described in the examples below.

[0057] (2) Abbe number (ν) In one embodiment of the present invention, the Abbe number of the thermoplastic resin is preferably 22.0 to 35.0, more preferably 22.0 to 33.0, even more preferably 23.0 to 32.0, and particularly preferably 23.0 to 30.0. In the present invention, the Abbe number can be measured by the method described in the examples below.

[0058] (3) Glass Transition Temperature (Tg) In one embodiment of the present invention, one of the characteristics of the thermoplastic resin is high heat resistance, and the glass transition temperature (Tg) is preferably 125 to 150° C., more preferably 125 to 145° C., even more preferably 125 to 140° C., and particularly preferably 127 to 135° C. In the present invention, the glass transition temperature can be measured by the method described in the examples below.

[0059] (4) Weight Average Molecular Weight (Mw) in Polystyrene Equivalents In one embodiment of the present invention, the weight average molecular weight of the thermoplastic resin in polystyrene equivalents is preferably 10,000 to 100,000, more preferably 10,000 to 80,000, and particularly preferably 10,000 to 60,000.

[0060] (5) Photoelastic Coefficient In one embodiment of the present invention, one of the characteristics of the thermoplastic resin is that it has a low photoelastic coefficient, and the photoelastic coefficient is preferably 25 to 45, more preferably 25 to 38, and particularly preferably 28 to 38. In the present invention, the photoelastic coefficient can be measured by the method described in the examples below.

[0061] (6) Water Absorption In one embodiment of the present invention, one of the features of the thermoplastic resin is that it has low water absorption, and the water absorption is preferably 0.40% or less, and more preferably 0.36% or less. The lower limit is usually about 0.1%. In the present invention, the water absorption can be measured by the method described in the examples below.

[0062] (7) Dimensional change rate upon water absorption In one embodiment of the present invention, one of the features of the thermoplastic resin is that it has a low dimensional change rate upon water absorption, and the dimensional change rate upon water absorption is preferably 0.045% or less, and more preferably 0.040% or less. The lower limit is usually about 0.01%. In the present invention, the dimensional change rate upon water absorption can be measured by the method described in the examples below.

[0063] <Thermoplastic Resin Composition> Another embodiment of the present invention is a thermoplastic resin composition containing the above-described thermoplastic resin and an additive. The thermoplastic resin composition of this embodiment can be used in combination with a resin other than the thermoplastic resin of the present invention containing the above-described structural unit (A), as long as the desired effects of this embodiment are not impaired. Examples of such resins include, but are not limited to, at least one resin selected from the group consisting of polycarbonate resins, polyester resins, polyestercarbonate resins, (meth)acrylic resins, polyamide resins, polystyrene resins, cycloolefin resins, acrylonitrile-butadiene-styrene copolymer resins, vinyl chloride resins, polyphenylene ether resins, polysulfone resins, polyacetal resins, and methyl methacrylate-styrene copolymer resins. Various known resins can be used, and one type can be added alone or two or more types can be added in combination to the thermoplastic resin composition.

[0064] [Antioxidant] The thermoplastic resin composition preferably contains an antioxidant as the additive. The antioxidant preferably contains at least one of a phenolic antioxidant and a phosphite-based antioxidant. Examples of phenolic antioxidants include 1,3,5-tris(3,5-di-tert-butyl-4-hydroxyphenylmethyl)-2,4,6-trimethylbenzene, 1,3,5-tris(3,5-di-tert-butyl-4-hydroxybenzyl)-1,3,5-triazine e-2,4,6(1H,3H,5H)-trione, 4,4',4''-(1-methylpropanyl-3-ylidene)tris(6-tert-butyl-m-cresol), 6,6'-di-tert-butyl-4,4'-butylidene-m-cresol, ocladecyl 3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate, pentane, methyl ... Examples of the hydroxybenzoate include pentaerythritol-tetrakis[3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate], 3,9-bis{2-[3-(3-tert-butyl-4-hydroxy-5-methylphenyl)propionyloxy]-1,1-dimethylethyl}-2,4,8,10-tetraoxospiro[5.5]undecane, and pentaerythritol-tetrakis[3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate], and preferably pentaerythritol-tetrakis[3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate].Phosphite antioxidants include 2-ethylhexyl diphenyl phosphite, isodecyl diphenyl phosphite, triisodecyl phosphite, triphenyl phosphite, 3,9-bis(octadecyloxy)-2,4,8,10-tetraoxy-3,9-diphosphaspiro[5.5]undecane, 3,9-bis(2,6-di-tert-butyl-4-methylphenoxy)-2,4,8,10-tetraoxa-3,9-diphosphaspiro[5.5]undecane, 2,2'-methylenebis(4,6-di-tert-butylphenyl)2-ethylhexyl phosphite, Examples of the antioxidant include tris(2,4-di-tert-butylphenyl)phosphite, tris(nonylphenyl)phosphite, tetra-C12-15-alkyl(propane-2,2-diylbis(4,1-phenylene))bis(phosphite), and 3,9-bis(2,6-di-tert-butyl-4-methylphenoxy)-2,4,8,10-tetraoxa-3,9-diphosphaspiro[5.5]undecane, and preferably 3,9-bis(2,6-di-tert-butyl-4-methylphenoxy)-2,4,8,10-tetraoxa-3,9-diphosphaspiro[5.5]undecane. As the antioxidant, any one of the above may be used alone, or a mixture of two or more may be used.

[0065] The antioxidant content in the thermoplastic resin composition is preferably 1 ppm by weight to 3,000 ppm by weight based on the total weight of the resin composition, more preferably 50 ppm by weight to 2,500 ppm by weight, even more preferably 100 ppm by weight to 2,000 ppm by weight, particularly preferably 150 ppm by weight to 1,500 ppm by weight, and even more preferably 200 ppm by weight to 1,200 ppm by weight.

[0066] [Release Agent] The thermoplastic resin composition preferably contains a release agent as the additive. Examples of the release agent include ester compounds, such as glycerin fatty acid esters such as mono- and diglycerides of glycerin fatty acid, glycol fatty acid esters such as propylene glycol fatty acid esters and sorbitan fatty acid esters, higher alcohol fatty acid esters, and full esters or mono-fatty acid esters of aliphatic polyhydric alcohols and aliphatic carboxylic acids. When an ester of aliphatic polyhydric alcohols and aliphatic carboxylic acids is used as the release agent, either a monoester or a full ester can be used, but other than a full ester, such as a monoester, may also be used. Specific examples of the release agent include the following.That is, sorbitan fatty acid esters such as sorbitan stearate, sorbitan laurate, sorbitan oleate, sorbitan trioleate, sorbitan tribehenate, sorbitan stearate, sorbitan tristearate, and sorbitan caprylate; propylene glycol fatty acid esters such as propylene glycol monostearate, propylene glycol monooleate, propylene glycol monobehenate, propylene glycol monolaurate, and propylene glycol monopalmitate; higher alcohol fatty acid esters such as stearyl stearate; glycerin monohydroxystearates such as glycerin monostearate and glycerin mono-12-hydroxystearate, glycerin monooleate, glycerin monobehenate, glycerin monocaprylate, glycerin monocaprate, and glycerin Examples of the monoglycerides include monoglycerides such as monolaurate, and mono-diglycerides such as glycerin monodistearate, glycerin monodistearate, glycerin monodibehenate, and glycerin monodiolate; acetylated monoglycerides of glycerin fatty acid esters such as glycerin diacetomonolaurate; organic acid monoglycerides of glycerin fatty acid esters such as citric acid fatty acid monoglyceride, succinic acid fatty acid monoglyceride, and diacetyltartaric acid fatty acid monoglyceride; and polyglycerin fatty acid esters such as diglycerin stearate, diglycerin laurate, diglycerin oleate, diglycerin monostearate, diglycerin monolaurate, diglycerin monomyristate, diglycerin monooleate, tetraglycerin stearate, decaglycerin laurate, decaglycerin oleate, and polyglycerin polyricinoleate.

[0067] The thermoplastic resin composition preferably contains 1 ppm by weight to 5,000 ppm by weight of the release agent based on the total weight of the resin composition, more preferably 50 ppm by weight to 4,000 ppm by weight, even more preferably 100 ppm by weight to 3,500 ppm by weight, particularly preferably 500 ppm by weight to 13,000 ppm by weight, and even more preferably 1,000 ppm by weight to 2,500 ppm by weight.

[0068] [Other Additives] In addition to the antioxidant and mold release agent described above, other additives may be added to the thermoplastic resin composition. For example, additives that may be contained in the thermoplastic resin composition include compounding agents, catalyst deactivators, heat stabilizers, plasticizers, fillers, UV absorbers, rust inhibitors, dispersants, antifoaming agents, leveling agents, flame retardants, lubricants, dyes, pigments, bluing agents, nucleating agents, and clarifying agents. The content of other additives other than the antioxidant and mold release agent in the thermoplastic resin composition is preferably 10 ppm by weight to 5.0% by weight, more preferably 100 ppm by weight to 2.0% by weight, and even more preferably 1000 ppm by weight to 1.0% by weight, but is not limited thereto. The above-mentioned additives may adversely affect transmittance, so it is preferable not to add them in excess; for example, the total amount added is within the above-mentioned range.

[0069] <Optical Members> The thermoplastic resin or thermoplastic resin composition of the present invention (hereinafter simply referred to as "resin composition") can be suitably used for optical members. In one embodiment of the present invention, an optical member comprising the resin composition of the present invention is provided. In one embodiment of the present invention, optical members include, but are not limited to, optical disks, transparent conductive substrates, optical cards, sheets, films, optical fibers, lenses, prisms, optical films, substrates, optical filters, hard coat films, and the like. The resin composition of the present invention can be molded by a casting method with high flowability, and is therefore particularly suitable for producing thin optical members. In a preferred embodiment of the present invention, the optical member produced using the resin composition of the present invention may be an optical lens. In another preferred embodiment of the present invention, the optical member produced using the resin composition of the present invention may be an optical film.

[0070] When an optical element containing the resin composition of the present invention is produced by injection molding, molding is preferably performed under conditions of a cylinder temperature of 260 to 350°C and a mold temperature of 90 to 170°C. More preferably, molding is performed under conditions of a cylinder temperature of 270 to 320°C and a mold temperature of 100 to 160°C. If the cylinder temperature is higher than 350°C, the resin composition will decompose and discolor, and if it is lower than 260°C, the melt viscosity will be high, making molding difficult. Furthermore, if the mold temperature is higher than 170°C, it will be difficult to remove a molded piece made of the resin composition from the mold. On the other hand, if the mold temperature is lower than 90°C, the resin will harden too quickly in the mold during molding, making it difficult to control the shape of the molded piece and making it difficult to sufficiently transfer the shape of the molded piece.

[0071] <Optical Lens> In one embodiment of the present invention, the resin composition can be suitably used for optical lenses. Optical lenses produced using the resin composition of the present invention have a high refractive index and excellent heat resistance, and are therefore extremely useful in fields where expensive high refractive index glass lenses have traditionally been used, such as telescopes, binoculars, and television projectors. For example, in smartphone lenses, a lens molded from a thermoplastic resin containing the structural unit (A) and a resin containing any one of the structural units of formulas (II-1) to (II-4), or (In the above formula, R 1 and R 2 each independently represents a hydrogen atom, a methyl group, or an ethyl group; R 3 and R 4 each independently represents a hydrogen atom, a methyl group, an ethyl group, or an alkylene glycol having 2 to 5 carbon atoms.) A lens molded from a resin containing a structural unit derived from any one of the monomers of the above formulas can be superimposed on the resin to be used as a lens unit.

[0072] The optical lens of the present invention is preferably implemented as an aspherical lens, if necessary. Since an aspherical lens can substantially eliminate spherical aberration with a single lens, it is not necessary to eliminate spherical aberration by combining multiple spherical lenses, which allows for weight reduction and reduced molding costs. Therefore, aspherical lenses are particularly useful as camera lenses, among other optical lenses.

[0073] Furthermore, because the optical lens of the present invention has high molding fluidity, it is particularly useful as a material for optical lenses that are thin, small, and have complex shapes. Specifically, the lens size preferably has a central thickness of 0.05 to 3.0 mm, more preferably 0.05 to 2.0 mm, and even more preferably 0.1 to 2.0 mm. The diameter is preferably 1.0 to 20.0 mm, more preferably 1.0 to 10.0 mm, and even more preferably 3.0 to 10.0 mm. Furthermore, the lens preferably has a meniscus shape, with one side convex and the other concave. The optical lens of the present invention can be molded by any method, such as mold molding, cutting, polishing, laser machining, electrical discharge machining, or etching. Among these, mold molding is more preferred in terms of production costs.

[0074] <Optical Film> In one embodiment of the present invention, the resin composition can be suitably used for optical films. In particular, optical films produced using the polycarbonate resin of the present invention have excellent transparency and heat resistance, and are therefore suitable for use as films for liquid crystal substrates, optical memory cards, etc. In order to minimize the inclusion of foreign matter in the optical film, the molding environment must naturally be a low-dust environment, preferably class 6 or less, and more preferably class 5 or less.

[0075] The present invention will be described in detail below by showing examples of the present invention together with comparative examples, but the present invention is not limited to these examples. The physical properties of the obtained resin were measured according to the following methods and apparatus.

[0076] 1) Weight-average molecular weight (Mw) The weight-average molecular weight of the obtained resin was measured by gel permeation chromatography (GPC) and calculated in terms of standard polystyrene. The apparatus, column, and measurement conditions used were as follows: GPC apparatus: HLC-8420GPC, manufactured by Tosoh Corporation Columns: TSKgel SuperHM-M x 3, manufactured by Tosoh Corporation TSKgel guard column SuperH-H x 1, manufactured by Tosoh Corporation TSKgel SuperH-RC x 1, manufactured by Tosoh Corporation Detector: RI detector Standard polystyrene: Standard polystyrene kit PStQuick C, manufactured by Tosoh Corporation Sample solution: 0.2% by mass tetrahydrofuran solution Eluent: tetrahydrofuran Eluent flow rate: 0.6 mL / min Column temperature: 40°C

[0077] 2) Glass transition temperature (Tg): Measured according to JIS K7121-1987 using a differential scanning calorimeter with a temperature increase program of 10°C / min. Differential scanning calorimeter: TA Instruments DSC2500

[0078] 3) Refractive index (nD) Test specimens were prepared by molding polycarbonate resin into V-shaped blocks according to JIS B 7071-2:2018. The refractive index was measured at 23°C using a refractometer (Shimadzu KPR-3000).

[0079] 4) Abbe number (ν) Using the same test piece (V-block) as used in the refractive index measurement, the refractive index was measured at wavelengths of 486 nm, 589 nm, and 656 nm at 23°C using a refractometer, and the Abbe number was calculated using the following formula: Refractometer: KPR-3000 manufactured by Shimadzu Corporation ν=(nD-1) / (nF-nC) nD: refractive index at wavelength 589 nm nC: refractive index at wavelength 656 nm nF: refractive index at wavelength 486 nm

[0080] 5) Photoelastic coefficient The obtained resin was dissolved in dichloromethane to obtain a resin solution. This resin solution was spread on a tray, and the solvent was evaporated to obtain a 0.1 mm thick film, which was used as a sample piece. The photoelastic coefficient was measured using an ellipsometer. Measurement method: The photoelastic coefficient was calculated by measuring the change in birefringence with respect to the change in load at a wavelength of 633 nm. Ellipsometer: Ellipsometer M-220 manufactured by JASCO Corporation

[0081] 6) Water absorption (%) Test pieces obtained by injection molding were dried in a hot air dryer for 6 hours. Thereafter, the mass of the test piece was measured and designated as M0. Next, this test piece was placed in an environmental tester controlled under high temperature and high humidity conditions. The test piece was removed after 72 hours, and the mass was measured and designated as Mt. The water absorption (%) was calculated using the following formula: Water absorption (%) = (Mt - M0) / M0 x 100 The mass was measured in an environment controlled at 23°C ± 2°C (21°C to 25°C).

[0082] 7) Dimensional change rate upon water absorption (%) A test piece obtained by injection molding was dried in a hot air dryer for 6 hours. Thereafter, the dimensions of the test piece were measured and designated as D0. Next, this test piece was placed in an environmental test machine controlled under high temperature and high humidity conditions. The test piece was removed after 72 hours, and the dimensions were measured and designated as Dt. The dimensional change rate upon water absorption (%) was calculated using the following formula: Dimensional change rate (%) = (Dt - D0) / D0 x 100 The dimensions were measured in an environment controlled at 23°C ± 2°C (21°C to 25°C). Measuring equipment: Image dimension measuring instrument LM-1100 (manufactured by KEYENCE Corporation)

[0083] Synthesis Example 1 (Production of Compound (1-2)) 25.0 g of compound (2-2), 5.9 g of ethylene carbonate, 45.0 g of toluene, 0.62 g of potassium hydroxide, and 0.45 g of tetrabutylammonium bromide were charged into a four-neck flask, and the atmosphere in the flask was replaced with nitrogen. The liquid temperature in the flask was then raised to 105-110°C, and stirring was continued for 10 hours. The liquid temperature was then lowered to 90°C, 8.8 g of water was added, and the mixture was maintained at that temperature for 1 hour. The liquid temperature was then raised to 85°C, and 3.4 g of 12% aqueous hydrochloric acid was added to neutralize the reaction liquid. The temperature was then lowered to 25°C, and cooling and stirring were continued overnight. The crystals were then separated by filtration. 17.8 g of the separated crystals and 178.0 g of cyclohexanone were charged into a four-neck flask and dissolved. 35.6 g of water was added to the flask, and the mixture was heated to 90°C. The solution was stirred at that temperature for 30 minutes, allowed to stand, and the separated aqueous layer was removed. This water-washing procedure was repeated three times. The solution after the water wash was cooled to 60°C, and 53.4 g of toluene was added, causing crystals to begin to precipitate. The solution was then cooled to 25°C and stirred overnight. The precipitated crystals were filtered off and dried to obtain 8.7 g of compound (1-2). The analytical methods for the compounds are shown below Table 1.

[0084] 1 H-NMR (400 MHz, solvent: CDCl 3 ) δ<ppm>: 1.30-1.86 (m, 19H), 2.49 (s, 1H), 2.88-2.90 (s, 1H), 3.99-4.00 (2H), 4.05-4.06 (2H), 6.47-7.28 (m, 4H). 13 C-NMR (400 MHz, solvent: CDCl 3 ​) δ <ppm>: 21.57, 26.46, 27.23, 30.96, 33.45, 37.33, 43.09, 61.91, 69.75, 115.96, 122.33, 124.42, 127.66, 132.47, 134.79, 140.02, 151.15, 153.55. The obtained crystals were analyzed by HPLC, and the purity was found to be 98.6%. Differential scanning calorimetry (DSC) analysis of the obtained crystals of compound (1-2) revealed that the top temperature of the endothermic peak was 209.4 ° C. The differential scanning calorimetry (DSC) data is shown in Figure 1. The diffraction angles 2θ (°) of the diffraction peaks that appeared in powder X-ray diffraction (PXRD) measurement of the obtained crystals of compound (1-2) and peaks with relative integrated intensities of 30 or more based on the peak with the largest integrated intensity are shown in Table 1. The PXRD measurement chart is shown in Figure 2.

[0085]

[0086] <Analysis Method> 1. Reaction Composition and Purity Analysis (Analysis Values ​​are Area Percentages) Measuring Instrument: High Performance Liquid Chromatography Analyzer (Shimadzu Corporation) Pump: LC-20AD Column Oven: CTO-20A Detector: SPD-20A Detection Wavelength: 280 nm Column: HALO-C18 Oven Temperature: 50°C Flow Rate: 0.7 mL / min Mobile Phase: (A) 0.2 vol% acetic acid aqueous solution, (B) methanol Gradient Conditions: (A) vol% (time from start of analysis) 50% (0 min) → 80% (4 min) → 100% (14 min) → 100% (19 min) 2. NMR Analysis Measuring Instrument: Fourier Transform Nuclear Magnetic Resonance AVANCE III HD 400 (Bruker) Measurement samples were dissolved in deuterated chloroform (CDCl 3 ) and 13 C-NMR and 1The H-NMR spectrum was measured. 3. Thermal Analysis 3 mg of the crystals obtained in Synthesis Example 1 were weighed into an aluminum pan, and thermal analysis of the crystals was performed using a differential scanning calorimeter (DSC7020, manufactured by Hitachi High-Tech Science Corporation) under the following operating conditions, using aluminum oxide as a control. The top temperature of the endothermic peak that appeared in the analysis was taken as the melting point. (Operating Conditions) Heating rate: 10°C / min Measurement temperature range: 30 to 350°C Measurement atmosphere: open, nitrogen 50 mL / min. 4. X-ray Diffraction Method (XRD) 0.1 g of the compound obtained in the example was filled into the sample filling section of a glass test plate, and measurement was performed using the following apparatus and conditions. [Measurement device] MiniFlex600-C / Rigaku Corporation [Measurement conditions] X-ray source: CuKα Tube voltage: 40 kV Tube current: 15 mA Scan axis: 2θ / θ Mode: Continuous Measurement range: 2θ = 5° to 90° Step: 0.02° Speed ​​measurement time: 10° / min. Entrance slit: 0.25° Receiving slit: 13.00 mm

[0087] (Example 1) As raw materials, 27.8234 g (0.0634 mol) of 9,9-bis[4-(2-hydroxyethoxy)phenyl]fluorene (BPEF) represented by the following structural formula, 17.2898 g (0.0272 mol) of 2,2'-[(1,3-phenylenebis(propane-2,2-diyl))bis(2-cyclohexyl-5-methyl-4,1-phenylene))bis(oxy))bis(ethan-1-ol) (Bis3M6CM-2EO, crystals of compound (1-2) represented by the following structural formula), 20.0000 g (0.0934 mol) of diphenyl carbonate (DPC), and 2.5 × 10 -2 20 μl (5.0 × 10 -7 (mol) was placed in a 300 mL reactor equipped with a stirrer and a distillation device, and the system was purged with nitrogen. The reactor was immersed in an oil bath heated to 200°C to initiate the transesterification reaction. The temperature was raised to 240°C over 140 minutes, and the pressure was reduced to 0.1 kPa or less. After maintaining this for 30 minutes, nitrogen gas was introduced into the reaction system to return the pressure to 101.3 kPa, and a polycarbonate resin was obtained. The physical properties of the obtained resin are shown in Table 2.

[0088] (Examples 2 and 3, Comparative Example 1) Polycarbonate resins were obtained in the same manner as in Example 1, except that the dihydroxy compounds (diols) in the raw materials were those shown in Table 2. The physical properties of the obtained resins are shown in Table 2.

[0089]

Claims

1. A thermoplastic resin containing a structural unit (A) derived from a compound represented by the following general formula (1): (In the formula, R 1 each independently represents a hydrogen atom or a linear or branched alkyl group having 1 to 4 carbon atoms; R 2 each independently represents an alkylene group having 1 to 4 carbon atoms; R 3 each independently represents a linear, branched or cyclic alkyl group having 4 to 6 carbon atoms.

2. The thermoplastic resin according to claim 1, wherein the compound represented by the general formula (1) is a compound represented by the following general formula (1A) or (1B): (In the formula, R 1 , R 2 and R 3 is the same as defined in general formula (1).

3. R ​​in the compound represented by the general formula (1) 3 The thermoplastic resin according to claim 1, wherein is a t-butyl group or a cyclohexyl group.

4. The thermoplastic resin according to claim 1, wherein the thermoplastic resin is a polycarbonate resin, a polyester carbonate resin, or a polyester resin.

5. The thermoplastic resin according to claim 1, comprising a structural unit (B) derived from a monomer represented by the following general formula (6) and / or a structural unit (C) derived from a monomer represented by the following general formula (7): (In general formula (6), R a and R b each independently represents a hydrogen atom, a halogen atom, an alkyl group having 1 to 20 carbon atoms which may have a substituent, an alkoxyl group having 1 to 20 carbon atoms which may have a substituent, a cycloalkyl group having 5 to 20 carbon atoms which may have a substituent, a cycloalkoxyl group having 5 to 20 carbon atoms which may have a substituent, an aryl group having 6 to 20 carbon atoms which may have a substituent, a heteroaryl group having 6 to 20 carbon atoms which contains one or more hetero ring atoms selected from O, N and S and which may have a substituent, an aryloxy group having 6 to 20 carbon atoms which may have a substituent, and -C≡C-R h R is selected from the group consisting of h represents an aryl group having 6 to 20 carbon atoms which may have a substituent, or a heteroaryl group having 6 to 20 carbon atoms which contains one or more hetero ring atoms selected from O, N, and S and which may have a substituent; X represents a single bond or a fluorene group which may have a substituent; A and B each independently represent an alkylene group having 1 to 5 carbon atoms which may have a substituent; m and n each independently represent an integer of 0 to 6; and a and b each independently represent an integer of 0 to 10. (In general formula (7), R c and R d are each independently selected from the group consisting of a hydrogen atom, a halogen atom, an alkyl group having 1 to 20 carbon atoms which may have a substituent, an alkoxyl group having 1 to 20 carbon atoms which may have a substituent, a cycloalkyl group having 5 to 20 carbon atoms which may have a substituent, a cycloalkoxyl group having 5 to 20 carbon atoms which may have a substituent, and an aryl group having 6 to 20 carbon atoms which may have a substituent; 1 represents a single bond, a fluorene group which may have a substituent, or any one of the structural formulae represented by the following formulae (8) to (15), (In formulas (8) to (15), R 61 , R 62 , R 71 , R 72 , R 81 and R 82 each independently represents a hydrogen atom, a halogen atom, an alkyl group having 1 to 20 carbon atoms which may have a substituent, or an aryl group having 6 to 30 carbon atoms which may have a substituent, or R 61 and R 62 , or R 71 and R 72 are bonded to each other to form a carbon ring or hetero ring having 1 to 20 carbon atoms which may have a substituent; r and s each independently represent an integer of 0 to 5,000; A and B each independently represent an alkylene group having 1 to 5 carbon atoms which may have a substituent; p and q each independently represent an integer of 0 to 4; a and b each independently represent an integer of 0 to 10.

6. The thermoplastic resin according to claim 5, wherein in said general formula (6) and said general formula (7), A and B each independently represent an alkylene group having 2 or 3 carbon atoms.

7. The thermoplastic resin according to claim 5, wherein the thermoplastic resin contains at least a structural unit derived from any one of BPEF, BNE, BNEF, DPBHBNA, BPM, and BCFL.

8. The thermoplastic resin according to claim 1, further comprising a structural unit derived from at least one monomer selected from the following group of monomers: (In the above formula, R 1 and R 2 each independently represents a hydrogen atom, a methyl group, or an ethyl group; R 3 and R 4 each independently represents an aryl group, a hydrogen atom, a methyl group, an ethyl group, or an alkylene glycol having 2 to 5 carbon atoms; and each of i and ii independently represents an integer of 1 to 3.

9. The thermoplastic resin according to claim 1, wherein the weight average molecular weight (Mw) of the thermoplastic resin in terms of polystyrene is 10,000 to 100,000.

10. The thermoplastic resin according to claim 1, wherein the refractive index (nD) of the thermoplastic resin is 1.500 to 1.

700.

11. The thermoplastic resin according to claim 1, wherein the Abbe number (ν) of the thermoplastic resin is 22.0 to 35.

0.

12. The thermoplastic resin according to claim 1, wherein the thermoplastic resin has a glass transition temperature of 125 to 150°C.

13. The thermoplastic resin according to claim 1, wherein the thermoplastic resin has a photoelastic coefficient of 25 to 45.

14. The thermoplastic resin according to claim 1, wherein the thermoplastic resin has a water absorption rate of 0.40% or less.

15. The thermoplastic resin according to claim 1, wherein the rate of dimensional change due to water absorption of said thermoplastic resin is 0.045% or less.

16. An optical lens comprising the thermoplastic resin of claim 1.

Citation Information

Patent Citations

  • Thermoplastic resin

    JP2018002893A

  • Thermoplastic resin

    JP2018002894A

  • Thermoplastic resin

    JP2018002895A

  • Polyester resin having fluorene skeleton

    JP2018059074A

  • Polycarbonate resin

    WO2017078073A1