Polyarylate resin
By adding a controlled amount of formate to the polyarylate resin, the thermal degradation and coloration issues during melt molding are effectively addressed, resulting in improved color tone and stability, suitable for applications like automotive and electronic components.
Patent Information
- Application Number
- PCT/JP2024/017456
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-06-27
- Filing Date
- 2024-05-10
- Publication Date
- 2024-11-21
AI Technical Summary
Polyarylate resins experience thermal deterioration and coloration issues during melt molding, limiting their applications due to insufficient suppression of discoloration and undesirable color tone changes, especially at high temperatures.
Incorporating a specific amount of formate, preferably sodium formate, into the polyarylate resin during the polymerization process, with a content of 0.1 to 2.0 ppm, to enhance color tone and thermochromic properties, thereby suppressing thermal degradation and yellowing.
The controlled formate content in the polyarylate resin significantly improves the color tone and discoloration resistance, ensuring the resin maintains its transparency and mechanical strength even under high-temperature conditions, suitable for applications requiring stable color and transparency.
Smart Images

Figure JPOXMLDOC01-APPB-M000001 
Figure JPOXMLDOC01-APPB-M000002 
Figure JPOXMLDOC01-APPB-T000003
Abstract
Description
Polyarylate Resin
[0001] The present invention relates to a polyarylate resin and a method for producing the same.
[0002] Polyarylate resins composed of aromatic dicarboxylic acid components and dihydric phenol components are amorphous, transparent, and have excellent heat resistance, and are being used in a variety of applications. Among these, amorphous polyarylate resins composed of residues of terephthalic acid and isophthalic acid and residues of 2,2-bis(4-hydroxyphenyl)propane (bisphenol A) are one of the few super engineering plastics, and because they are transparent, highly heat-resistant, and have excellent mechanical strength and dimensional stability, their molded articles are widely used in fields such as electrical and electronics, automobiles, and machinery.
[0003] However, due to its excellent heat resistance, polyarylate resins are often processed at higher melt-molding temperatures than general-purpose polymers, which makes them prone to thermal degradation and discoloration during melting. Furthermore, molded articles tend to yellow when used at high temperatures for long periods. Therefore, their use has been limited in applications where color tone and transparency are required and color change over time is undesirable, such as automobile lamp lenses and camera lenses for in-car or mobile phone cameras.
[0004] In order to solve the above problems, various methods have been studied for adding modifiers such as dyes, pigments, and antioxidants during melt molding or melt kneading. For example, Patent Document 1 proposes a method of melt kneading a dye, pigment, and sulfur-containing carboxylic acid ester with a polycarbonate resin. Furthermore, Patent Document 2 proposes a method of melt kneading a phenolic compound, a phosphorus-based compound, and a lactone-based compound with a polyarylate resin. However, these methods are based solely on the modification by additives added during melt kneading, and therefore there is a need to improve the color tone and thermal discoloration of the polyarylate resin itself, from the perspective of reducing the number and amount of additives used.
[0005] In order to improve the color tone and thermal discoloration of the polyarylate resin itself, it is necessary to devise a method for producing the polyarylate resin from raw materials. As polymerization methods for polyarylate resin, melt polymerization, solution polymerization, and interfacial polymerization are known. In particular, the interfacial polymerization method is suitable for polymers with high heat resistance, because the reaction proceeds to a high degree of polymerization at temperatures close to room temperature, resulting in a resin with excellent color tone, and making full use of the transparency and heat resistance that are inherent characteristics of the polyarylate resin.
[0006] Furthermore, as described in Patent Document 3, although not limited to the interfacial polymerization method, adding a reducing agent such as sodium hydrosulfite during the polymerization step is effective in preventing discoloration of the dihydric phenol compound, which is the monomer, and further, coloration of the resulting polyarylate resin.
[0007] On the other hand, Patent Document 4 discloses a technique for producing an aromatic polycarbonate having excellent color tone and heat resistance by using sodium hydrosulfite as a reducing agent added during the polymerization step.
[0008] Furthermore, Patent Document 5 discloses a technology for producing polycarbonate with excellent hue by limiting the sodium formate content in sodium hydrosulfite used in the production of polycarbonate to 0.3 wt % or less. In particular, Patent Document 5 proposes that if the sodium formate content in the sodium hydrosulfite used in the production of polycarbonate is more than 0.3 wt %, the hue of the resin will deteriorate when heated.
[0009] JP-A-4-120164 JP-A-2002-265766 JP-A-1-18939 JP-A-7-233253 Patent No. 5544681
[0010] However, the conventional techniques have had the following problems: - It is not possible to obtain a polyarylate resin with a sufficiently excellent color tone. - When molding using a polyarylate resin, coloration due to thermal degradation during melt molding cannot be sufficiently suppressed.
[0011] An object of the present invention is to provide a polyarylate resin that can be more sufficiently inhibited from discoloring due to thermal degradation during melt molding and that has a sufficiently excellent color tone.
[0012] As a result of extensive research to solve this problem, the present inventors have found that when a polyarylate resin contains an appropriate amount of formate, the color tone of the polyarylate resin is sufficiently excellent and coloration due to thermal degradation during melt molding can be more sufficiently suppressed.
[0013] The gist of the present invention is as follows. <1> A polyarylate resin containing an aromatic dicarboxylic acid component and a dihydric phenol component as monomer components, and having a formate content of 0.1 to 2.0 ppm. <2> The polyarylate resin according to <1>, wherein the polyarylate resin has a color difference a value of -1.0 to 0.5. <3> The polyarylate resin according to <1> or <2>, wherein the polyarylate resin has a granular shape. <4> The polyarylate resin according to any one of <1> to <3>, wherein the formate is sodium formate. <5> The polyarylate resin according to any one of <1> to <4>, wherein a molded plate having a thickness of 3 mm obtained by injection molding the polyarylate resin has a YI value of 22 or less. <6> A method for producing a polyarylate resin by polymerizing an aromatic dicarboxylic acid component and a dihydric phenol component, wherein a dithionite having a formate content of 0.4 to 1.5 mass% is added in an amount of 0.05 to 4.0 mass% relative to the dihydric phenol component. <7> A method for producing a polyarylate resin according to <6>, wherein the dithionite is sodium dithionite (also known as sodium hydrosulfite) produced by a sodium formate method. <8> A method for producing a polyarylate resin according to <6> or <7>, which comprises producing the polyarylate resin according to any one of <1> to <5>.
[0014] The polyarylate resin of the present invention has a sufficiently good color tone of the polyarylate resin itself, and can be more sufficiently inhibited from coloring due to thermal degradation during melt molding.
[0015] The present invention will be described in detail below. The polyarylate resin of the present invention is an aromatic polyester resin obtained from an aromatic dicarboxylic acid component (including its functional derivative) and a dihydric phenol component, and contains these components as monomer components. Therefore, the polyarylate resin of the present invention can also be expressed as containing residues of an aromatic dicarboxylic acid component and a dihydric phenol component. The structure of the polyarylate resin of the present invention is not particularly limited, and the present invention is applicable to polyarylate resins of any structure. The functional derivative refers to an organic compound in which the carboxyl group of an aromatic dicarboxylic acid is replaced with a more reactive substituent, and includes, for example, an acid halide compound having an acid halide group, as described below.
[0016] The aromatic dicarboxylic acid component for introducing the aromatic dicarboxylic acid residue into the polyarylate resin is an organic compound containing an aromatic ring and two carboxyl groups per molecule. The carboxyl groups may be acid halide groups. The acid halide groups are groups in which the hydroxyl groups of the carboxyl groups are substituted with halogen atoms. Specific examples of such aromatic dicarboxylic acid components include terephthalic acid, isophthalic acid, phthalic acid, chlorophthalic acid, nitrophthalic acid, 2,5-naphthalenedicarboxylic acid, 2,6-naphthalenedicarboxylic acid, 2,7-naphthalenedicarboxylic acid, 1,5-naphthalenedicarboxylic acid, methyl terephthalic acid, 4,4'-biphenyldicarboxylic acid, 2,2'-biphenyldicarboxylic acid, 4,4'-diphenyletherdicarboxylic acid, 4,4'-diphenylmethanedicarboxylic acid, 4,4'-diphenylsulfonedicarboxylic acid, 4,4'-diphenylisopropylidenedicarboxylic acid, 1,2-bis(4-carboxyphenoxy)ethane, 5-sodium sulfoisophthalic acid, diphenic acid, and derivatives thereof (e.g., acid halides). These aromatic dicarboxylic acids can be used alone or in combination of two or more. Among these, it is preferred that the polyarylate resin contains at least one of terephthalic acid and isophthalic acid, and preferably both, from the viewpoint of further improving color tone and discoloration resistance.
[0017] In this specification, the term "color tone" refers to the color tone of the polyarylate resin itself, and refers to a property in which the color difference a value measured by a colorimeter is smaller. The term "discoloration resistance" refers to a property in which coloration due to thermal degradation during melt molding of the polyarylate resin is more sufficiently suppressed, and refers to a property in which the yellow index (YI) value measured by a color tone measuring device of the obtained molded product is smaller.
[0018] The total content of terephthalic acid and isophthalic acid in the polyarylate resin is not particularly limited, and from the viewpoint of further improving color tone and discoloration resistance, it is preferably 50% by mass or more, more preferably 70% by mass or more, even more preferably 90% by mass or more, particularly preferably 95% by mass or more, and sufficiently preferably 100% by mass, based on the total amount of aromatic dicarboxylic acid components. The total content of terephthalic acid and isophthalic acid may be the total content of residues of terephthalic acid and isophthalic acid.
[0019] When the polyarylate resin contains at least one of terephthalic acid (e.g., terephthalic acid chloride) and isophthalic acid (e.g., isophthalic acid chloride) as an aromatic dicarboxylic acid component, the content ratio thereof is not particularly limited, and from the viewpoint of further improving color tone and discoloration resistance, the mass ratio of terephthalic acid / isophthalic acid is preferably 0 / 100 to 100 / 0, more preferably 10 / 90 to 90 / 10, even more preferably 20 / 80 to 80 / 20, sufficiently preferably 30 / 70 to 70 / 30, even more sufficiently preferably 40 / 60 to 60 / 40, particularly preferably 45 / 55 to 55 / 45, and most preferably 50 / 50. The content ratio of terephthalic acid and isophthalic acid may be the content ratio of residues of terephthalic acid and isophthalic acid.
[0020] The dihydric phenol component for introducing dihydric phenol residues constituting the polyarylate resin is an organic compound containing two phenolic hydroxyl groups per molecule. The phenolic hydroxyl group is a hydroxyl group directly bonded to an aromatic ring. Specific examples of such dihydric phenol components include 2,2-bis(4-hydroxyphenyl)propane (bisphenol A), 2,2-bis(3-methyl-4-hydroxyphenyl)propane (bisphenol C), 1,1-bis(4-hydroxyphenyl)cyclohexane (bisphenol Z), 1,1-bis(4-hydroxyphenyl)-1-phenylethane (bisphenol AP), 2,2-bis(4-hydroxy-3-methylphenyl)propane, 2,2-bis(3,5-dimethyl-4-hydroxyphenyl)propane, 2,2-bis(4-hydroxy-3,5-dibromophenyl)propane, Examples of suitable hydroxyl groups include 2,2-bis(4-hydroxy-3,5-dichlorophenyl)propane, 4,4'-dihydroxydiphenyl sulfone (bisphenol S), 4,4'-dihydroxydiphenyl ether, 4,4'-dihydroxydiphenyl sulfide, 4,4'-dihydroxydiphenyl ketone, 4,4'-dihydroxydiphenylmethane, 4,4'-dihydroxybiphenyl [4,4'-biphenol], 1,1-bis(4-hydroxyphenyl)-3,3,5-trimethylcyclohexane (bisphenol TMC), 4,4'-(1,3-dimethylbutylidene)diphenol, and resorcinol. These compounds may be used alone or in combination of two or more. From the viewpoint of further improving color tone and discoloration resistance, the polyarylate resin preferably contains one or more dihydric phenol components selected from the group consisting of bisphenol A, bisphenol C, bisphenol Z, 2,2-bis(3,5-dimethyl-4-hydroxyphenyl)propane, and bisphenol TMC, and more preferably contains bisphenol A.In a more preferred embodiment, from the viewpoint of further improving color tone and discoloration resistance, the polyarylate resin preferably contains, as the dihydric phenol component, one or more dihydric phenol components selected from the group consisting of bisphenol A, bisphenol TMC, and bisphenol S (particularly, at least one of bisphenol A and bisphenol TMC).
[0021] The content of bisphenol A in the polyarylate resin is not particularly limited, and from the viewpoint of further improving color tone and discoloration resistance, it is preferably 0 to 100 mass%, more preferably 40 to 100 mass%, even more preferably 60 to 100 mass%, particularly preferably 80 to 100 mass%, and sufficiently preferably 100 mass%, based on the total amount of dihydric phenol components. The content of bisphenol A may be the content of bisphenol A residues.
[0022] The total content of bisphenol A and bisphenol TMC in the polyarylate resin is not particularly limited, and from the viewpoint of further improving color tone and discoloration resistance, it is preferably 50 mol% or more, more preferably 70 mol% or more, even more preferably 90 mol% or more, particularly preferably 95 mol% or more, and sufficiently preferably 100 mol% based on the total amount of dihydric phenol components. The total content of bisphenol A and bisphenol TMC may be the total content of residues of bisphenol A and bisphenol TMC.
[0023] When the polyarylate resin contains at least one of bisphenol A and bisphenol TMC as a dihydric phenol component, the content ratio thereof is not particularly limited, and from the viewpoint of further improving color tone and discoloration resistance, the molar ratio of bisphenol A / bisphenol TMC is preferably 0 / 100 to 100 / 0, more preferably 20 / 80 to 100 / 0, even more preferably 50 / 50 to 100 / 0, sufficiently preferably 70 / 30 to 100 / 0, even more sufficiently preferably 80 / 20 to 100 / 0, particularly preferably 95 / 5 to 100 / 0, and most preferably 100 / 0. The content ratio of bisphenol A and bisphenol TMC may be the content ratio of residues of bisphenol A and bisphenol TMC.
[0024] The polyarylate resin may contain at least one dihydric alcohol component selected from the group consisting of ethylene glycol, propylene glycol, butanediol, pentanediol, hexanediol, heptanediol, octanediol, dodecanediol, neopentyl glycol, cyclohexanediol, 1,4-dihydroxymethylcyclohexane, and the like, in place of a portion of the dihydric phenol component, as long as the properties and effects of the present invention are not impaired.
[0025] The content of the dihydric alcohol component in the polyarylate resin is not particularly limited, and may be, for example, 50% by mass or less relative to the total amount of the dihydric phenol components, and from the viewpoint of further improving color tone and discoloration resistance, it is preferably 20% by mass or less, more preferably 10% by mass or less, even more preferably 5% by mass or less, particularly preferably 1% by mass or less, and sufficiently preferably 0% by mass. The content of the dihydric alcohol component may be the content of residues of the dihydric alcohol component.
[0026] The polyarylate resin may further contain a tri- or higher functional polyvalent monomer component, provided that the properties and effects of the present invention are not impaired. When the polyarylate resin contains a tri- or higher functional polyvalent monomer component, a branched structure is introduced into the polyarylate resin. Examples of tri- or higher functional polyvalent monomer components include tricarboxylic acid components such as 1,3,5-benzenecarboxylic acid; and triol components such as 4,4',4''-trihydroxytriphenylmethane.
[0027] The content of the polyvalent monomer component in the polyarylate resin is not particularly limited, and may be, for example, 20% by mass or less relative to the total amount of the dihydric phenol component and the aromatic dicarboxylic acid component, and from the viewpoint of further improving color tone and discoloration resistance, it is preferably 10% by mass or less, more preferably 5% by mass or less, even more preferably 2% by mass or less, particularly preferably 1% by mass or less, and sufficiently preferably 0% by mass. The content of the polyvalent monomer component may be the content of residues of the polyvalent monomer component.
[0028] The polyarylate resin may contain a terminal blocking agent to adjust the molecular weight. Examples of the terminal blocking agent include one or more compounds selected from the group consisting of monohydric phenols such as phenol, cresol, p-tert-butylphenol, 2,3,5-trimethylphenol, 2,3,6-trimethylphenol, and cumylphenol; monohydric acid chlorides such as benzoic acid chloride, methanesulfonyl chloride, and phenyl chloroformate; monohydric alcohols such as methanol, ethanol, n-propanol, isopropanol, n-butanol, 2-butanol, pentanol, hexanol, dodecyl alcohol, stearyl alcohol, benzyl alcohol, and phenethyl alcohol; and monohydric carboxylic acids such as acetic acid, propionic acid, octanoic acid, cyclohexanecarboxylic acid, benzoic acid, toluic acid, phenylacetic acid, p-tert-butylbenzoic acid, and p-methoxyphenylacetic acid. From the viewpoint of further improving color tone and discoloration resistance, the end-capping agent is preferably a monohydric phenol (particularly p-tert-butylphenol).
[0029] The content of the terminal blocking agent in the polyarylate resin is not particularly limited, and from the viewpoint of further improving color tone and discoloration resistance, it is preferably 0.2 to 20 parts by mass, more preferably 0.6 to 10 parts by mass, even more preferably 1.2 to 6 parts by mass, and particularly preferably 2 to 5 parts by mass, per 100 parts by mass of the dihydric phenol component. The content of the terminal blocking agent may be the content of residues of the terminal blocking agent.
[0030] The polyarylate resin of the present invention contains formate at 0.1 to 2.0 ppm. From the viewpoint of further improving color tone and discoloration resistance, the formate content is preferably 0.1 to 1.5 ppm, more preferably 0.1 to 0.8 ppm, even more preferably 0.1 to 0.5 ppm, and particularly preferably 0.2 to 0.4 ppm. In the present invention, by containing formate in the polyarylate resin in the appropriate amount as described above, not only is the color tone of the polyarylate resin itself sufficiently excellent, but the discoloration resistance of molded articles containing the polyarylate resin is also sufficiently excellent. If the formate content exceeds 2 ppm, thermal degradation during melt molding is accelerated, resulting in significant yellowing of the resin molded article. On the other hand, if the formate content of the polyarylate resin is less than 0.1 ppm, the color difference a value of the powder or granule will be very low, but the effect of suppressing thermal discoloration during melt molding will be insufficient, resulting in significant yellowing of the resin molded article.
[0031] The formate may be an alkali metal salt of formic acid, such as sodium formate, potassium formate, etc. From the viewpoint of further improving color tone and discoloration resistance, the formate is preferably sodium formate, and the above content is preferably the content of sodium formate.
[0032] The content of formate is determined by extracting formate from 0.5 g of polyarylate resin with 50 mL of ultrapure water and quantitatively analyzing the extracted formate by ion chromatography (IC).
[0033] The formate contained in the polyarylate resin of the present invention may be a residue of the formate contained in a reducing agent (e.g., dithionite (particularly sodium hydrosulfite)) used in the production of the polyarylate resin, or may be an additive newly added after the production of the polyarylate resin.
[0034] The content of formate can be controlled by the following method: dissolving and washing the polyarylate resin with an organic solvent capable of dissolving the polyarylate resin, thereby reducing the content of formate. Various organic solvents can dissolve polyarylate resins depending on the monomer components that make up the resin, but examples include aliphatic chlorinated solvents such as dichloromethane, 1,2-dichloroethane, chloroform, 1,1,1-trichloroethane, 1,1,2,2-tetrachloroethane, dibromomethane, tribromomethane, bromoethane, 1,1-dibromoethane, and 1-bromopropane, aromatic chlorinated solvents such as chlorobenzene, o-dichlorobenzene, m-dichlorobenzene, and p-dichlorobenzene, amide solvents such as N,N-dimethylformamide, N,N-dimethylacetamide, and N-methyl-2-pyrrolidone, ether solvents such as 1,4-dioxane, 1,3-dioxolane, and tetrahydrofuran, aromatic hydrocarbon solvents such as benzene, toluene, and xylene, and mixtures thereof. When producing polyarylate resins, the content of formate contained in the dithionite (especially sodium hydrosulfite) used as a reducing agent is adjusted. For example, reducing the formate content of dithionite (particularly sodium hydrosulfite) can reduce the formate content of the polyarylate resin. Furthermore, increasing the formate content of dithionite (particularly sodium hydrosulfite) can increase the formate content of the polyarylate resin. The amount of dithionite (particularly sodium hydrosulfite) used as a reducing agent during the production of the polyarylate resin is adjusted. For example, reducing the amount of dithionite (particularly sodium hydrosulfite) used can reduce the formate content of the polyarylate resin. Furthermore, increasing the amount of dithionite (particularly sodium hydrosulfite) used can increase the formate content of the polyarylate resin. During the production of the polyarylate resin, strengthening the washing step with pure water (e.g., extending the washing time) can reduce the formate content of the polyarylate resin.By employing one or more of the above-mentioned methods, or by employing two or more of them in combination, the content of formate in the polyarylate resin can be controlled.
[0035] The color difference a value of the polyarylate resin of the present invention is usually −1.0 to 0.5, and from the viewpoint of further improving color tone and discoloration resistance, it is preferably −1.0 to 0.2, more preferably −1.0 to −0.1, even more preferably −1.0 to −0.4, and particularly preferably −0.8 to −0.45.
[0036] The color difference a value is obtained by filling a measurement container with polyarylate resin so that there are no gaps, and measuring in reflection mode with a colorimetric color difference meter (for example, a colorimetric color difference meter (ZE6000) manufactured by Nippon Denshoku Industries Co., Ltd.) The polyarylate resin used for measurement has a particulate shape, and the particle diameter of the particles is 0.7 to 5.0 mm (some of the particles may contain fine powder).
[0037] The YI value of a 3 mm thick plate obtained by injection molding the polyarylate resin of the present invention is usually 22 or less, and from the viewpoint of further improving color tone and discoloration resistance, it is preferably 19.5 or less, more preferably 14 or less, even more preferably 10 or less, and particularly preferably 9 or less. There is no particular limitation on the lower limit of the YI value, and the YI value is usually 1 or more, particularly 4 or more.
[0038] The YI value is measured by subjecting a 3 mm thick plate obtained by injection molding a polyarylate resin at a resin temperature of 360°C using a general injection molding machine (for example, a J110AD injection molding machine manufactured by JSW Corporation) to a color measurement device (for example, an SZ-Σ90 colorimeter manufactured by Nippon Denshoku Industries Co., Ltd.). The polyarylate resin used for molding has a particulate shape, and the particle diameter of the particles is 0.7 to 5.0 mm (some fine powder may be included).
[0039] In general, from the viewpoints of mechanical properties and workability during melt molding and melt kneading, the polyarylate resin of the present invention preferably has an inherent viscosity of 0.40 to 1.30 dl / g, more preferably 0.45 to 1.10 dl / g, even more preferably 0.45 to 0.90 dl / g, particularly preferably 0.50 to 0.80 dl / g, and sufficiently preferably 0.50 to 0.60 dl / g.
[0040] The inherent viscosity (ηinh) is an index of molecular weight, and a value measured by the following method is used. A resin solution of polyarylate resin is prepared using 1,1,2,2-tetrachloroethane as a solvent so that the concentration is 1 g / dl, and the relative viscosity (ηrel) is measured at a temperature of 25°C. The inherent viscosity is calculated from the obtained relative viscosity using the following formula: ηinh(dl / g) = Ln(ηrel) / c (c: concentration)
[0041] The polymerization method for the polyarylate resin is not particularly limited as long as the resulting polyarylate resin has the above-mentioned properties, and may be a known method, for example, the following methods: a solution polymerization method in which a dicarboxylic acid halide containing an aromatic dicarboxylic acid component is reacted with a diol containing a dihydric phenol component in an organic solvent; a melt polymerization method in which the dicarboxylic acid and diol are heated in the presence of acetic anhydride or diallyl carbonate; and an interfacial polymerization method in which a dicarboxylic acid halide dissolved in an organic solvent that is not miscible with water is mixed with a diol dissolved in an alkaline aqueous solution.
[0042] From the viewpoint of further improving color tone and resistance to discoloration, the polymerization method for the polyarylate resin used in the present invention is preferably an interfacial polymerization method, since the reaction proceeds to a high degree of polymerization at a relatively low temperature.
[0043] When applying the interfacial polymerization method, the organic solvent used is not particularly limited as long as it is immiscible with water and dissolves the divalent carboxylic acid halide used and the resulting polyarylate resin. Suitable organic solvents include aliphatic chlorinated solvents such as dichloromethane, 1,2-dichloroethane, chloroform, 1,1,1-trichloroethane, and tetrachloroethane; aromatic chlorinated solvents such as chlorobenzene and o-dichlorobenzene; and mixtures thereof. In the isolation and drying process of the resulting polyarylate resin, it is best to avoid organic solvents with excessively high boiling points. Among these, aliphatic chlorinated solvents (particularly dichloromethane) are preferred as organic solvents.
[0044] In the interfacial polymerization method, it is preferable to use a dithionite produced by the sodium formate method as the reducing agent, because the formate content in the polyarylate resin can be easily achieved, and as a result, the polyarylate resin of the present invention having excellent color tone and discoloration resistance can be easily produced.
[0045] The dithionite may be an alkali metal salt of dithionous acid, such as sodium dithionite (also known as sodium hydrosulfite), potassium dithionite, etc. From the viewpoint of further improving color tone and discoloration resistance, the dithionite is preferably sodium hydrosulfite.
[0046] From the viewpoint of further improving color tone and discoloration resistance, sodium hydrosulfite produced by the sodium formate method is preferred as the dithionite. Dithionite produced by a method other than the sodium formate method (e.g., an electrolytic method) does not contain formate itself.
[0047] The sodium formate method is a method for producing sodium hydrosulfite using sodium formate. Specifically, sodium formate is dissolved in aqueous alcohol (e.g., aqueous methanol), and sodium hydroxide and sulfurous anhydride are added to the solution to cause a reaction.
[0048] The content of formate contained in the dithionite (particularly the content of sodium formate contained in sodium hydrosulfite produced by the sodium formate method) is preferably 0.4 to 1.5 mass%, more preferably 0.4 to 1.0 mass%, even more preferably 0.5 to 1.0 mass%, and particularly preferably 0.5 to 0.8 mass%, from the viewpoint of further improving color tone and discoloration resistance. If the content of formate (particularly sodium formate) is too low or too high, it becomes difficult for the resulting polyarylate resin to achieve the formate content of the polyarylate resin of the present invention, and discoloration due to thermal degradation during melt molding cannot be sufficiently suppressed. The content of formate (particularly sodium formate) is the ratio to the total amount of dithionite (particularly the total amount of sodium hydrosulfite). The total amount of dithionite refers to the total amount of dithionite and formate contained in said dithionite, and in particular, when by-products and decomposition products are contained in the dithionite, this refers to the total amount including said by-products and decomposition products. The total amount of sodium hydrosulfite refers to the total amount of sodium hydrosulfite and sodium formate contained in said sodium hydrosulfite, and in particular, when by-products and decomposition products are contained in the sodium hydrosulfite, this refers to the total amount including said by-products and decomposition products.
[0049] Methods for quantifying formate contained in dithionite (particularly methods for quantifying formate contained in sodium hydrosulfite produced by the sodium formate method) include the method specified in "Specifications and Criteria for Food Additives, etc. (Ministry of Health and Welfare Notification No. 370 of 1959) Section 2: Food Additives (as of November 30, 2017)" and methods for detecting organic acids by ion chromatography. In the present invention, the method for detecting organic acids by ion chromatography is adopted.
[0050] The content of formate contained in dithionite (particularly sodium hydrosulfite) can be controlled, for example, by washing and purifying the dithionite (particularly the obtained sodium hydrosulfite) with an aqueous methanol solution. Specifically, the content of formate (particularly sodium formate) can be controlled by adjusting the number of washes with the aqueous methanol solution and the methanol concentration of the aqueous methanol solution. For example, the more the number of washes, the lower the content of formate (particularly sodium formate). On the other hand, the fewer the number of washes, the higher the content of formate (particularly sodium formate). Furthermore, for example, the higher the methanol concentration of the aqueous methanol solution, the lower the content of formate (particularly sodium formate). On the other hand, the lower the methanol concentration of the aqueous methanol solution, the higher the content of formate (particularly sodium formate).
[0051] From the viewpoint of further improving color tone and discoloration resistance, the amount of reducing agent (e.g., dithionite (particularly sodium hydrosulfite produced by the sodium formate method)) added is preferably 0.05 to 4.0 mass%, more preferably 0.1 to 2.0 mass%, even more preferably 0.2 to 1.5 mass%, sufficiently preferably 0.2 to 1.1 mass%, and even sufficiently preferably 0.3 to 0.8 mass%, relative to the mass of the dihydric phenol component used. If the amount of reducing agent added is too small or too large, it becomes difficult to achieve the formate content of the polyarylate resin of the present invention. For example, if the amount added is less than 0.05 mass%, the effect of preventing discoloration of the dihydric phenol component is insufficient, and discoloration due to thermal degradation during melt molding cannot be sufficiently suppressed. On the other hand, if the amount added is increased to more than 4.0 mass%, the formate content of the polyarylate resin of the present invention will be too high, and discoloration due to thermal degradation during melt molding cannot be sufficiently suppressed.
[0052] A polymerization catalyst may be used in the interfacial polymerization method. Examples of the polymerization catalyst for the interfacial polymerization method include tertiary amines such as trimethylamine, triethylamine, tri-n-butylamine, tri-n-propylamine, tri-isopropylamine, trihexylamine, tridecylamine, N,N-dimethylcyclohexylamine, pyridine, quinoline, and dimethylaniline; quaternary ammonium salts such as trimethylbenzylammonium halide, triethylbenzylammonium halide, tri-n-propylbenzylammonium halide, and tri-n-butylbenzylammonium halide; quaternary phosphonium salts such as trimethylbenzylphosphonium halide, tetramethylbenzylphosphonium halide, triethylbenzylphosphonium halide, tri-n-butylbenzylphosphonium halide, tetra-n-butylphosphonium halide, triphenylbenzylphosphonium halide, and tetraphenylphosphonium halide; and crown ethers such as 18-crown-6, 18-benzocrown-6, 18-dibenzocrown-6, and 15-crown-5. In particular, quaternary ammonium salts (particularly trimethylbenzylammonium halide and tri-n-butylbenzylammonium halide) are preferred in terms of polymerization rate and cost.
[0053] The amount of the polymerization catalyst used is not particularly limited, and from the viewpoint of further improving color tone and discoloration resistance, it is preferably 0.1 to 5 mass %, more preferably 0.1 to 3 mass %, and even more preferably 0.1 to 1.5 mass %, based on the dihydric phenol component.
[0054] When producing the polyarylate resin of the present invention by interfacial polymerization, the following method is preferably employed. A dihydric phenol component, end-capping agent, reducing agent, and polymerization catalyst are dissolved in an alkaline aqueous solution to obtain an aqueous layer. Separately, an aromatic dicarboxylic acid component is dissolved in an organic solvent to obtain an organic layer. The two incompatible liquids (the aqueous and organic layers described above) are mixed under strong stirring, and a polymerization reaction is carried out until a high degree of polymerization is achieved due to interlayer migration of the dihydric phenol component and end-capping agent component in the aqueous layer. After completion of the reaction, stirring is stopped, and the resulting mixture is separated into an organic layer in which the resulting polyarylate resin is dissolved and an aqueous layer in which by-products such as salts and unreacted monomers are dissolved. The organic layer is then neutralized with an inorganic acid such as acetic acid or phosphoric acid.
[0055] The organic layer after neutralization contains unreacted monomers, low-molecular-weight polyarylate resins, by-product salts, and other impurities. To remove these impurities, the organic layer is thoroughly washed with pure water using a method such as static separation or centrifugation. Both static separation and centrifugation involve extracting various impurities contained in the organic layer into pure water, and either method may be used as appropriate. Washing with pure water can reduce the formate content in the polyarylate resin. Furthermore, increasing the number of times and duration of washing with pure water can further reduce the formate content.
[0056] The process of granulating polyarylate resin from the organic layer in which the thoroughly washed polyarylate resin is dissolved includes the hot water granulation method in which the organic solvent is distilled off in hot water, the kneader method in which the organic solvent is evaporated by heating in a kneader or the like and the residual polymer is pulverized, the spray dry method in which the organic solvent is sprayed with a spray to instantly evaporate the organic solvent, and the reprecipitation method in which the organic solvent solution is introduced into a poor solvent for the polyarylate resin to precipitate and precipitate the polymer component, etc. Any method may be used as appropriate, but in the present invention, the hot water granulation method is preferred in view of the properties of the particles obtained and the simplicity of the equipment.
[0057] When dichloromethane is used as the organic solvent, in hot water granulation, hot water at 50°C is placed in a hot water jacket tank equipped with an agitator, stirred, and then the hot water is withdrawn from the bottom of the tank, introduced into a wet pulverizer, and returned to the same tank in a circulating manner while supplying an organic solvent solution in which polyarylate resin has been dissolved.While maintaining the liquid temperature in the tank at 50°C, the organic solvent is distilled off to granulate the polyarylate resin, and a polyarylate / hot water slurry is obtained in the wet pulverizer on the circulation line, taking care not to generate large particles.This slurry is then withdrawn through a filter to obtain only the polyarylate resin powder.
[0058] The granulated polyarylate resin powder is dried by an appropriate method using an appropriate dryer depending on the production volume, etc. At this time, if the drying temperature exceeds 140°C, the vaporized dichloromethane will undergo thermal decomposition, generating hydrogen chloride, which will severely corrode the inner walls of the dryer. Therefore, operation at 140°C or less (particularly 120 to 135°C) is desirable. By setting the drying temperature to 120 to 135°C, it is possible to sufficiently remove water and dichloromethane while keeping the formate content of the polyarylate resin within the above-mentioned range.
[0059] When the polyarylate resin of the present invention has a powdery or granular shape (or a powdery or granular form), the particle diameter of the particles is 0.7 to 5.0 mm (some particles may contain fine powder). Furthermore, the polyarylate resin of the present invention may contain some particles in which two or more particles are pressed together.
[0060] The particle size of the polyarylate resin is a value obtained by measuring 50 randomly selected particles of the polyarylate resin using a microscope (VHX-6000) manufactured by Keyence Corporation.
[0061] The polyarylate resin of the present invention can be melt-kneaded with various thermoplastic resins and various additives to produce a polyarylate resin composition with characteristic properties. Kneading methods include those using common extruders, such as single-screw extruders, twin-screw extruders, roll mixers, and Brabender mixers. Among these, the twin-screw extruder method is preferred because it ensures a good kneading state of multiple raw materials. It is also preferable to use a static mixer or dynamic mixer in combination. The raw materials may be added from a hopper or a side feeder. The resin composition obtained by melt-kneading is preferably in the form of pellets. The polyarylate resin composition contains the polyarylate resin of the present invention and may further contain at least one selected from thermoplastic resins and additives. For example, the polyarylate resin composition may contain only a polyarylate resin, a thermoplastic resin, and an additive. In this case, the polyarylate resin composition may or may not contain the thermoplastic resin and the additive independently.
[0062] Examples of thermoplastic resins include nylon resin, polycarbonate resin, polyester resin, polyphenylene ether resin, polystyrene resin, etc. The polyester resin refers to polyester other than the polyarylate resin of the present invention.
[0063] The content of the thermoplastic resin in the polyarylate resin composition is not particularly limited, and may be, for example, 100% by mass or less, particularly 50% by mass or less, relative to the polyarylate resin, and from the viewpoint of further improving color tone and discoloration resistance, it is preferably 10% by mass or less, more preferably 5% by mass or less, and even more preferably 1% by mass or less. The lower limit of the content of the thermoplastic resin is not particularly limited, and the content of the thermoplastic resin may be 0% by mass.
[0064] As additives, additives that may be conventionally added to polyarylate resins can be used, such as antioxidants, lubricants, dyes and pigments, flow improvers, flame retardants, and fillers. Examples of antioxidants include various antioxidants such as hindered phenols, hindered amines, thioethers, and phosphorus-based antioxidants. Examples of lubricants include fatty acid salts, such as stearates. Examples of dyes and pigments include metal complex dyes, anthraquinone dyes, perinone dyes, carbon black and inorganic metal-based inorganic pigments, and organic pigments containing organic compounds, such as azo pigments and polycyclic pigments. Examples of flow improvers include inorganic compounds such as fatty acid salts, and organic compounds containing fluorine-based and amide-based compounds. Examples of flame retardants include various halogen-based, phosphorus-based, nitrogen-based, and hydrated metal-based flame retardants. Examples of fillers include inorganic fillers such as glass, mica, talc, and silica.
[0065] The content of additives in the polyarylate resin composition is not particularly limited, and may be, for example, 50% by mass or less, particularly 30% by mass or less, relative to the polyarylate resin. From the viewpoint of further improving color tone and discoloration resistance, it is preferably 10% by mass or less, more preferably 5% by mass or less, even more preferably 1% by mass or less, particularly preferably 0.8% by mass or less, sufficiently preferably 0.4% by mass or less, and even sufficiently preferably 0% by mass. When two or more additives are contained, the total content thereof may be within the above range. The lower limit of the content of additives is not particularly limited, and the content of additives may be 0% by mass.
[0066] In particular, the content of the antioxidant in the polyarylate resin composition is not particularly limited, but the polyarylate resin composition of the present invention is sufficiently excellent in color tone and discoloration resistance even without containing an antioxidant. Therefore, the content of the antioxidant in the polyarylate resin composition may be 20% by mass or less, particularly 10% by mass or less, relative to the polyarylate resin. From the viewpoint of further improving color tone and discoloration resistance, it is preferably 5% by mass or less, more preferably 1% by mass or less, even more preferably 0.4% by mass or less, particularly preferably 0.2% by mass or less, and sufficiently preferably 0% by mass. When two or more antioxidants are contained, the total content thereof may be within the above range.
[0067] The present invention will be described in detail with reference to examples, but the present invention is not limited to these examples and various modifications and applications are possible within the scope of the present invention.
[0068] <Method for Quantifying Formate in Sodium Hydrosulfite> (1) Method for Quantifying Sodium Formate in Sodium Hydrosulfite Approximately 0.1 g of sodium hydrosulfite was weighed into a PP container, and 20 mL of ultrapure water was added. The solution was then left to stand overnight at room temperature to dissolve. The solution was then diluted 100 times with ultrapure water, and the diluted solution was filtered through a 0.2 μm membrane filter and quantitatively analyzed by ion chromatography (IC). A calibration curve method (multi-point calibration curve) was used for quantification.
[0069] <Method for Evaluating Polyarylate Resin Powder> (1) Method for Quantifying Residual Sodium Formate in Polyarylate Resin Powder Approximately 0.5 g of freeze-pulverized polyarylate resin powder was placed in a PP (polypropylene) container and weighed. The freeze-pulverized polyarylate resin consisted of particles with a particle diameter of 0.3 to 1.5 mm, including fine powder of 0.3 mm or less. The particle diameter was obtained by measuring 50 random particles using a Keyence microscope (VHX-6000). Next, 50 mL of ultrapure water was added, and extraction was performed by heating in a dryer set at 120°C for 1 hour. The mixture was then filtered through a 0.2 μm membrane filter and quantitatively analyzed by ion chromatography (IC). For quantification, a calibration curve method (single-point calibration curve) was used to calculate the amount of formate ions using the following formula 1, which was then converted to the amount of sodium formate using formula 2.
[0070]
[0071] A = Concentration of calibration standard sample (formic acid) B = IC peak area of sample to be analyzed C = IC peak area of blank D = Dilution ratio E = IC peak area of calibration standard sample F = Weight of sample to be analyzed
[0072]
[0073] G = amount of formate ions H = sodium formate formula weight (68.01) I = formate ion formula weight (45.02)
[0074] (2) Color difference a value of polyarylate resin powder A color difference meter (ZE6000) manufactured by Nippon Denshoku Industries Co., Ltd. was used. The polyarylate resin powder was packed into a measurement container without gaps, set on a sample holder, and measured in reflection mode. The particle diameter of the particles was 0.7 to 5.0 mm (some fine powder may be included).
[0075] (3) Yellow Index YI Value of Injection-Molded Article of Polyarylate Resin Powder The obtained polyarylate resin powder was molded into a 3 mm thick sample plate at a resin temperature of 360°C using a general injection molding machine (for example, a J110AD injection molding machine manufactured by JSW Corporation), and the yellow index YI value was measured using a color measurement device (SZ-Σ90 type colorimeter manufactured by Nippon Denshoku Industries Co., Ltd.). The evaluation was based on the following criteria: ⊚: 10 or less (excellent); ⊚: more than 10 and 14 or less (good); ○: more than 14 and 19.5 or less (good); △: more than 19.5 and 22 or less (pass: no practical problems); ×: more than 22 (fail: practical problems).
[0076] <Sodium Hydrosulfite> Sodium hydrosulfite was produced by the following method.
[0077] Sodium hydrosulfite A (manufacturing method: sodium formate method) (sodium formate content: 0.7% by mass) and sodium hydrosulfite B (manufacturing method: sodium formate method) (sodium formate content: 0.9% by mass). Sodium hydrosulfite was manufactured by the sodium formate method. The amount of sodium formate contained in the manufactured sodium hydrosulfite was quantitatively analyzed by ion chromatography (IC). The sodium formate content varied slightly depending on the manufacturing lot; one with a sodium formate content of 0.7% by mass was designated sodium hydrosulfite A, and one with a sodium formate content of 0.9% by mass was designated sodium hydrosulfite B.
[0078] Sodium hydrosulfite C (manufacturing method: sodium formate method): sodium formate content 3.0% by mass (used in Comparative Examples 1, 2, 6, and 7). Sodium hydrosulfite C was produced by blending commercially available sodium formate with sodium hydrosulfite A (sodium formate content 0.7% by mass) so that the sodium formate content was 3.0% by mass.
[0079] Sodium hydrosulfite D (production method: electrolysis): sodium formate content 0 mass % (used in Comparative Examples 5, 10, and 11) Sodium hydrosulfite D was produced by electrolysis.
[0080] <Inherent Viscosity of Polyarylate Resin> A resin solution was prepared using 1,1,2,2-tetrachloroethane as a solvent to a concentration of 1 g / dl, and the relative viscosity (ηrel) was measured at a temperature of 25°C. The inherent viscosity was calculated from the obtained relative viscosity using the following formula: ηinh(dl / g) = Ln(ηrel) / c (c: concentration).
[0081] Example 1 (Method of Synthesizing Polyarylate Resin Powder) 100 parts by mass of 2,2-bis(4-hydroxyphenyl)propane (bisphenol A), 3.8 parts by mass of p-tert-butylphenol, 37 parts by mass of sodium hydroxide, 0.6 parts by mass of trimethylbenzylammonium chloride, and sodium hydrosulfite A were charged into a reaction vessel equipped with a stirrer, in an amount of 0.5% by mass relative to the mass of the dihydric phenol component, and dissolved in 1,103 parts by mass of water to form an aqueous layer. Separately, 92 parts by mass of a 1 / 1 mixture of terephthaloyl chloride and isophthaloyl chloride was dissolved in 895 parts by mass of dichloromethane to form an organic layer. This organic layer was added to the previously prepared aqueous layer with vigorous stirring, and a polymerization reaction was carried out at 15°C for 2 hours. Thereafter, the aqueous layer and the organic layer were separated, and 10 parts by mass of acetic acid was added to the organic layer to terminate the reaction. The solution was then repeatedly washed with water until neutral, yielding a 17% by mass dichloromethane solution of polyarylate. The dichloromethane solution of polyarylate was granulated by a hot water granulation method, and the water and dichloromethane were thoroughly dried using a paddle-type hot air dryer at 120 to 135°C to obtain the polyarylate resin powder granules of Example 1. The particle diameter of the particles was 0.7 to 5.0 mm (some fine powder may be included). Other characteristic values of the obtained polyarylate resin powder granules were as shown in Table 1.
[0082] Example 2 Polyarylate resin powder particles were synthesized in the same manner as in the "Method for synthesizing polyarylate resin powder particles" carried out in Example 1, except that sodium hydrosulfite A was added in an amount of 1.0 mass % relative to the mass of the dihydric phenol component, and p-tert-butylphenol was 1.6 mass parts. The particle diameter of the particles was 0.7 to 5.0 mm (some fine powder may be included). Other characteristic values of the obtained polyarylate resin powder particles were as shown in Table 1.
[0083] Example 3 Polyarylate resin powder particles were synthesized in the same manner as in the "method for synthesizing polyarylate resin powder particles" carried out in Example 1, except that sodium hydrosulfite B was added in an amount of 1.2 mass % relative to the mass of the dihydric phenol component, and p-tert-butylphenol was 1.2 parts by mass. The particle diameter of the particles was 0.7 to 5.0 mm (some fine powder may be included). Other characteristic values of the obtained polyarylate resin powder particles were as shown in Table 1.
[0084] Example 4 Polyarylate resin powder particles were synthesized in the same manner as in the "method for synthesizing polyarylate resin powder particles" carried out in Example 1, except that sodium hydrosulfite B was added in an amount of 3.0 mass % relative to the mass of the dihydric phenol component, and p-tert-butylphenol was 0.9 parts by mass. The particle diameter of the particles was 0.7 to 5.0 mm (some fine powder may be included). Other characteristic values of the obtained polyarylate resin powder particles were as shown in Table 1.
[0085] Example 5 Polyarylate resin powder granules were synthesized in the same manner as in the "method for synthesizing polyarylate resin powder granules" carried out in Example 1, except that a 4 / 1 mixture of terephthalic acid chloride and isophthalic acid chloride was used, sodium hydrosulfite A was added in an amount of 0.5 mass% relative to the mass of the dihydric phenol component, and p-tert-butylphenol was used in an amount of 1.2 mass parts. The particle diameter of the particles was 0.7 to 5.0 mm (some fine powder may be included). Other characteristic values of the obtained polyarylate resin powder granules were as shown in Table 1.
[0086] Example 6 Polyarylate resin powder granules were synthesized in the same manner as in Example 1, except that a 1 / 4 mixture of terephthalic acid chloride and isophthalic acid chloride was used, sodium hydrosulfite A was added in an amount of 0.5 mass% relative to the mass of the dihydric phenol component, and p-tert-butylphenol was used in an amount of 1.2 mass parts. The particle diameter of the particles was 0.7 to 5.0 mm (some fine powder may be included). Other characteristic values of the obtained polyarylate resin powder granules were as shown in Table 1.
[0087] Example 7 Polyarylate resin powder particles were synthesized in the same manner as in the "method for synthesizing polyarylate resin powder particles" performed in Example 1, except that the bisphenol A / bisphenol TMC ratio was 9 / 1 (mol %), sodium hydrosulfite A was added in an amount of 0.5 mass % relative to the mass of the dihydric phenol component, and p-tert-butylphenol was 1.2 mass parts. The particle diameter of the particles was 0.7 to 5.0 mm (some fine powder may be included). Other characteristic values of the obtained polyarylate resin powder particles were as shown in Table 1.
[0088] Example 8 Polyarylate resin powder particles were synthesized in the same manner as in the "method for synthesizing polyarylate resin powder particles" performed in Example 1, except that the bisphenol A / bisphenol TMC ratio was 6 / 4 (mol %), sodium hydrosulfite A was added in an amount of 0.5 mass % relative to the mass of the dihydric phenol component, and p-tert-butylphenol was 1.2 mass parts. The particle diameter of the particles was 0.7 to 5.0 mm (some fine powder may be included). Other characteristic values of the obtained polyarylate resin powder particles were as shown in Table 1.
[0089] Example 9 Polyarylate resin powder particles were synthesized in the same manner as in the "method for synthesizing polyarylate resin powder particles" performed in Example 1, except that the bisphenol A / bisphenol TMC ratio was 3 / 7 (mol %), sodium hydrosulfite A was added in an amount of 0.5 mass % relative to the mass of the dihydric phenol component, and p-tert-butylphenol was 1.2 mass parts. The particle diameter of the particles was 0.7 to 5.0 mm (some fine powder may be included). Other characteristic values of the obtained polyarylate resin powder particles were as shown in Table 1.
[0090] Example 10 Polyarylate resin powder particles were synthesized in the same manner as in the "method for synthesizing polyarylate resin powder particles" carried out in Example 1, except that bisphenol TMC was 100 mol %, sodium hydrosulfite A was added in an amount of 0.5 mass % relative to the mass of the dihydric phenol component, and p-tert-butylphenol was 1.2 mass parts. The particle diameter of the particles was 0.7 to 5.0 mm (some fine powder may be included). Other characteristic values of the obtained polyarylate resin powder particles were as shown in Table 1.
[0091] Example 11 Polyarylate resin powder particles were synthesized in the same manner as in the "method for synthesizing polyarylate resin powder particles" performed in Example 1, except that bisphenol TMC was 100 mol %, sodium hydrosulfite B was added in an amount of 1.2 mass % relative to the mass of the dihydric phenol component, and p-tert-butylphenol was 0.5 mass parts. The particle diameter of the particles was 0.7 to 5.0 mm (some fine powder may be included). Other characteristic values of the obtained polyarylate resin powder particles were as shown in Table 1.
[0092] Example 12 Polyarylate resin powder particles were synthesized in the same manner as in the "method for synthesizing polyarylate resin powder particles" performed in Example 1, except that bisphenol TMC was 100 mol %, sodium hydrosulfite B was added in an amount of 3.0 mass % relative to the mass of the dihydric phenol component, and p-tert-butylphenol was 0.8 mass parts. The particle diameter of the particles was 0.7 to 5.0 mm (some fine powder may be included). Other characteristic values of the obtained polyarylate resin powder particles were as shown in Table 1.
[0093] (Comparative Example 1) Polyarylate resin powder particles were synthesized in the same manner as in the "method for synthesizing polyarylate resin powder particles" carried out in Example 1, except that sodium hydrosulfite C was added in an amount of 3.0 mass % relative to the mass of the dihydric phenol component. The particle diameter of the particles was 0.7 to 5.0 mm (some fine powder may be included). Other characteristic values of the obtained polyarylate resin powder particles were as shown in Table 2.
[0094] (Comparative Example 2) Polyarylate resin powder particles were synthesized in the same manner as in the "method for synthesizing polyarylate resin powder particles" carried out in Example 1, except that sodium hydrosulfite C was added in an amount of 0.5% by mass relative to the mass of the dihydric phenol component. The particle diameter of the particles was 0.7 to 5.0 mm (some fine powder may be included). Other characteristic values of the obtained polyarylate resin powder particles were as shown in Table 2.
[0095] (Comparative Example 3) Polyarylate resin powder particles were synthesized in the same manner as in the "method for synthesizing polyarylate resin powder particles" carried out in Example 1, except that sodium hydrosulfite B was added in an amount of 7.0 mass % relative to the mass of the dihydric phenol component. The particle diameter of the particles was 0.7 to 5.0 mm (some fine powder may be included). Other characteristic values of the obtained polyarylate resin powder particles were as shown in Table 2.
[0096] Comparative Example 4 Polyarylate resin powder particles were synthesized in the same manner as in the "method for synthesizing polyarylate resin powder particles" carried out in Example 1, except that sodium hydrosulfite A was added in an amount of 0.1% by mass relative to the mass of the dihydric phenol component. The particle diameter of the particles was 0.7 to 5.0 mm (some fine powder may be included). Other characteristic values of the obtained polyarylate resin powder particles were as shown in Table 2.
[0097] (Comparative Example 5) Polyarylate resin powder particles were synthesized in the same manner as in the "method for synthesizing polyarylate resin powder particles" carried out in Example 1, except that sodium hydrosulfite D was added in an amount of 0.5% by mass relative to the mass of the dihydric phenol component. The particle diameter of the particles was 0.7 to 5.0 mm (some fine powder may be included). Other characteristic values of the obtained polyarylate resin powder particles were as shown in Table 2.
[0098] Comparative Example 6 Polyarylate resin powder granules were synthesized in the same manner as in the "method for synthesizing polyarylate resin powder granules" carried out in Example 1, except that bisphenol TMC was 100 mol %, sodium hydrosulfite C was added in an amount of 4.0 mass % relative to the mass of the dihydric phenol component, and p-tert-butylphenol was 1.2 mass parts. The particle diameter of the particles was 0.7 to 5.0 mm (some fine powder may be included). Other characteristic values of the obtained polyarylate resin powder granules were as shown in Table 2.
[0099] Comparative Example 7 Polyarylate resin powder granules were synthesized in the same manner as in the "method for synthesizing polyarylate resin powder granules" carried out in Example 1, except that bisphenol TMC was 100 mol %, sodium hydrosulfite C was added in an amount of 0.5 mass % relative to the mass of the dihydric phenol component, and p-tert-butylphenol was 1.2 mass parts. The particle diameter of the particles was 0.7 to 5.0 mm (some fine powder may be included). Other characteristic values of the obtained polyarylate resin powder granules were as shown in Table 2.
[0100] (Comparative Example 8) Polyarylate resin powder granules were synthesized in the same manner as in the "method for synthesizing polyarylate resin powder granules" carried out in Example 1, except that bisphenol TMC was 100 mol %, sodium hydrosulfite B was added in an amount of 8.0 mass % relative to the mass of the dihydric phenol component, and p-tert-butylphenol was 1.2 mass parts. The particle diameter of the particles was 0.7 to 5.0 mm (some fine powder may be included). Other characteristic values of the obtained polyarylate resin powder granules were as shown in Table 2.
[0101] (Comparative Example 9) Polyarylate resin powder granules were synthesized in the same manner as in the "method for synthesizing polyarylate resin powder granules" carried out in Example 1, except that bisphenol TMC was 100 mol %, sodium hydrosulfite A was added in an amount of 0.1 mass % relative to the mass of the dihydric phenol component, and p-tert-butylphenol was 1.2 mass parts. The particle diameter of the particles was 0.7 to 5.0 mm (some fine powder may be included). Other characteristic values of the obtained polyarylate resin powder granules were as shown in Table 2.
[0102] (Comparative Example 10) Polyarylate resin powder granules were synthesized in the same manner as in the "Method for synthesizing polyarylate resin powder granules" carried out in Example 1, except that bisphenol TMC was 100 mol %, sodium hydrosulfite D was added in an amount of 0.5 mass % relative to the mass of the dihydric phenol component, and p-tert-butylphenol was 1.2 mass parts. The particle diameter of the particles was 0.7 to 5.0 mm (some fine powder may be included). Other characteristic values of the obtained polyarylate resin powder granules were as shown in Table 2.
[0103] (Comparative Example 11) Polyarylate resin powder granules were synthesized in the same manner as in the "method for synthesizing polyarylate resin powder granules" performed in Example 1, except that the bisphenol TMC / bisphenol S ratio was 7 / 3 (mol %), sodium hydrosulfite D was added in an amount of 0.5 mass % relative to the mass of the dihydric phenol component, and p-tert-butylphenol was 2.8 mass parts. The particle diameter of the particles was 0.7 to 5.0 mm (some fine powder may be included). Other characteristic values of the obtained polyarylate resin powder granules were as shown in Table 2.
[0104]
[0105]
[0106] Each of the polyarylate resins obtained in the Examples and Comparative Examples had the same monomer composition ratio as the charged ratio of the monomers.
[0107] The above examples and comparative examples have revealed the following: By adjusting the amount of sodium formate contained in the polyarylate resin to an appropriate amount, the color tone of the polyarylate resin itself becomes good, and yellowing of molded products caused by thermal degradation due to heat melting can be more sufficiently reduced; and The polyarylate resin of the present invention can be produced by using a specific amount of sodium hydrosulfite having a specific sodium formate content.
[0108] The polyarylate resin of the present invention is useful in various applications requiring prevention of yellowing of molded articles, such as lamp covers and camera lenses mounted on automobiles, camera lenses mounted on mobile phones and smartphones, modules constituting electronic substrates, and as a replacement for plastic materials in parts that are primarily made of glass.
Claims
1. A polyarylate resin containing an aromatic dicarboxylic acid component and a dihydric phenol component as monomer components, and having a formate content of 0.1 to 2.0 ppm.
2. The polyarylate resin according to claim 1, wherein the polyarylate resin has a color difference a value of -1.0 to 0.
5.
3. The polyarylate resin according to claim 1, wherein the polyarylate resin is in the form of powder or granules.
4. The polyarylate resin of claim 1, wherein the formate salt is sodium formate.
5. The polyarylate resin according to claim 1, wherein a molded plate having a thickness of 3 mm obtained by injection molding said polyarylate resin has a YI value of 22 or less.
6. A method for producing a polyarylate resin by polymerizing an aromatic dicarboxylic acid component and a dihydric phenol component, wherein a dithionite having a formate content of 0.4 to 1.5% by mass is added in an amount of 0.05 to 4.0% by mass relative to the dihydric phenol component.
7. The method for producing a polyarylate resin according to claim 6, wherein the dithionite is sodium dithionite produced by the sodium formate method.
8. A method for producing the polyarylate resin according to claim 6, which produces the polyarylate resin according to any one of claims 1 to 5.
Citation Information
Patent Citations
Thermoplastic polymer improved treatment
JP1984206404A
Method of manufacturing polycarbonate
JP2009096937A
Polyarylate and method for producing the same
JP2010083986A
Polyarylate resin, polyarylate resin composition and molded body comprising the polyarylate resin composition