Thermoplastic resin composition production method and thermoplastic resin composition

The method of mixing specific thermoplastic resin units addresses the refractive index challenges and environmental concerns in thermoplastic resin production, enabling efficient reuse and reducing waste in the thermoplastic resin molding process.

WO2024237238A1PCT designated stage expired Publication Date: 2024-11-21MITSUBISHI GAS CHEM CO INC
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2024/017657
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-05-18
Filing Date
2024-05-13
Publication Date
2024-11-21

AI Technical Summary

Technical Problem

Conventional thermoplastic resins used for optical applications often fail to meet desired refractive index requirements, leading to inefficiencies in product commercialization and high environmental impact due to waste generation in the molding process, particularly in injection molding, where scraps are difficult to reuse.

Method used

A method for producing a thermoplastic resin composition by mixing multiple types of thermoplastic resins with specific structural units, such as fluorene and bisphenol-based units, to achieve a refractive index of 1.550 to 1.700, allowing for easy reuse of recycled materials and reducing environmental impact.

Benefits of technology

The method enables the production of thermoplastic resin compositions with desired optical properties, enhances recycling efficiency, and minimizes environmental impact by utilizing recycled materials effectively.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JP2024017657_21112024_PF_FP_ABST
    Figure JP2024017657_21112024_PF_FP_ABST
Patent Text Reader

Abstract

The present invention provides a thermoplastic resin composition production method with which it is possible to reliably produce a thermoplastic resin composition having desired properties, as well as facilitate thermoplastic resin recycling and reduce the environmental load. The problem is solved by the following thermoplastic resin composition production method. Specifically provided is a thermoplastic resin composition production method at least including a mixing step for mixing a first thermoplastic resin that includes a structural unit (A) derived from a monomer represented by any one of general formulas (1a)-(1c), and a second thermoplastic resin that includes a structural unit (B) derived from a monomer represented by general formula (2), wherein the refractive index of the first thermoplastic resin is 1.650 or less, the refractive index of the second thermoplastic resin is 1.570 or more, and the refractive index of the thermoplastic resin composition is 1.550-1.700.
Need to check novelty before this filing date? Find Prior Art

Description

Method for producing thermoplastic resin composition and thermoplastic resin composition

[0001] The present invention relates to a method for producing a thermoplastic resin composition containing a thermoplastic resin such as polycarbonate, and in particular to a method for producing a thermoplastic resin composition containing a mixture of multiple types of thermoplastic resins.

[0002] Thermoplastic resins used as optical materials have been known (for example, Patent Documents 1 and 2). Optical thermoplastic resins are generally required to have good properties such as refractive index and Abbe number.

[0003] Furthermore, thermoplastic resins are usually molded into products such as lenses and optical films through a molding process such as injection molding.

[0004] International Publication No. WO 2014 / 073496 International Publication No. WO 2015 / 166951

[0005] Conventional thermoplastic resins, such as those primarily used for optical applications, do not necessarily have properties suited to their intended use. For example, while a thermoplastic resin with a high refractive index is generally desirable for optical applications, it is often difficult to commercialize a product using only a high refractive index material. As a specific example, in a lens unit that does not use a high refractive index material or that combines lenses with different refractive indices, a medium- to low-refractive index material may also be required.

[0006] Furthermore, it is not easy to produce only molded products through molding processes such as injection molding of thermoplastic resins. Usually, waste materials other than molded products are generated due to the thermoplastic resin injected into gaps in the mold, such as sprues, runners, and gates. These waste materials are often discarded as waste because they are difficult to recycle. Therefore, conventional thermoplastic resin molded products can have problems with yields not reaching sufficient levels. Furthermore, there is a need to reduce the environmental impact of the thermoplastic resin molding process and expand recycling.

[0007] As a result of intensive research to solve the above problems, the present inventors have found that a method for producing a thermoplastic resin composition in which multiple predetermined types of thermoplastic resins are mixed can reliably achieve desired properties, primarily for optical applications, and also facilitate the recycling of the thermoplastic resins, thereby reducing the environmental burden.

[0008] The present invention includes the following: [1] A method for producing a thermoplastic resin composition, comprising at least a mixing step of mixing a first thermoplastic resin containing a structural unit (A) derived from a monomer represented by any one of the following general formulas (1a) to (1c), and a second thermoplastic resin containing a structural unit (B) derived from a monomer represented by the following general formula (2), wherein the refractive index of the first thermoplastic resin is 1.650 or less, the refractive index of the second thermoplastic resin is 1.570 or more, and the refractive index of the thermoplastic resin composition is 1.550 to 1.700. (In general formulas (1a) to (1c), R c and R d are each independently selected from the group consisting of a hydrogen atom, a halogen atom, an alkyl group having 1 to 20 carbon atoms which may have a substituent, an alkoxyl group having 1 to 20 carbon atoms which may have a substituent, a cycloalkyl group having 5 to 20 carbon atoms which may have a substituent, a cycloalkoxyl group having 5 to 20 carbon atoms which may have a substituent, and an aryl group having 6 to 20 carbon atoms which may have a substituent, and each Y is independently a single bond, a fluorene group which may have a substituent, or any of the structural formulas represented by the following formulas (i) to (vii): (In formulas (i) to (vii), R 61 , R 62 , R 71 and R 72 each independently represents a hydrogen atom, a halogen atom, an alkyl group having 1 to 20 carbon atoms which may have a substituent, or an aryl group having 6 to 30 carbon atoms which may have a substituent, or 61 and R 62 , or R 71 and R 72are bonded to each other to form a carbocyclic or heterocyclic ring having 4 to 20 carbon atoms, which may have a substituent; r and s each independently represent an integer of 0 to 5,000. A and B each independently represent an alkylene group having 1 to 5 carbon atoms, which may have a substituent; p and q each independently represent an integer of 0 to 4; a and b each independently represent an integer of 0 to 10. (In formula (2), R 1 ~R 4 are each independently a hydrogen atom, an alkyl group which may have a substituent, or an aryl group which may have a substituent, Z is a single bond or a group represented by the following general formula (3): (In formula (3), R 5 and R 6 are each a hydrogen atom, an optionally substituted alkyl group, or an optionally substituted aryl group, or 5 and R 6 represents a carbon ring or hetero ring having 4 to 20 carbon atoms, which may have a substituent, formed by bonding together, and c represents an integer of 1 to 3. [2] A method for producing a thermoplastic resin composition according to the above [1], wherein at least one of the first thermoplastic resin and the second thermoplastic resin comprises a recycled thermoplastic resin. [3] A method for producing a thermoplastic resin composition according to the above [1], wherein the refractive index of the thermoplastic resin composition is 1.570 to 1.650. [4] A method for producing a thermoplastic resin composition according to the above [1], wherein, based on the total number of structural units of the first thermoplastic resin and the second thermoplastic resin, the content of the structural unit (A) is 20 to 90 mol % and the content of the structural unit (B) is 10 to 80 mol %. [5] A method for producing a thermoplastic resin composition according to the above [1], wherein at least one of the first thermoplastic resin and the second thermoplastic resin is a copolymer having both the structural unit (A) and the structural unit (B). [6] The method for producing a thermoplastic resin composition according to the above [1], wherein the first thermoplastic resin has only the structural unit (A). [7] The method for producing a thermoplastic resin composition according to the above [1], wherein an additive is mixed with the first thermoplastic resin and the second thermoplastic resin in the mixing step.

[0009] [8] A thermoplastic resin composition comprising a mixture of a first thermoplastic resin containing a structural unit (A) derived from a monomer represented by any one of the following general formulas (1a) to (1c), and a second thermoplastic resin containing a structural unit (B) derived from a monomer represented by the following general formula (2), wherein the refractive index of the first thermoplastic resin is 1.650 or less, the refractive index of the second thermoplastic resin is 1.570 or more, and the refractive index of the thermoplastic resin composition is 1.550 to 1.700. (In general formulas (1a) to (1c), R c and R d are each independently selected from the group consisting of a hydrogen atom, a halogen atom, an alkyl group having 1 to 20 carbon atoms which may have a substituent, an alkoxyl group having 1 to 20 carbon atoms which may have a substituent, a cycloalkyl group having 5 to 20 carbon atoms which may have a substituent, a cycloalkoxyl group having 5 to 20 carbon atoms which may have a substituent, and an aryl group having 6 to 20 carbon atoms which may have a substituent, and each Y is independently a single bond, a fluorene group which may have a substituent, or any of the structural formulas represented by the following formulas (i) to (vii): (In formulas (i) to (vii), R 61 , R 62 , R 71 and R 72 each independently represents a hydrogen atom, a halogen atom, an alkyl group having 1 to 20 carbon atoms which may have a substituent, or an aryl group having 6 to 30 carbon atoms which may have a substituent, or 61 and R 62 , or R 71 and R 72 are bonded to each other to form a carbocyclic or heterocyclic ring having 4 to 20 carbon atoms, which may have a substituent; r and s each independently represent an integer of 0 to 5,000. A and B each independently represent an alkylene group having 1 to 5 carbon atoms, which may have a substituent; p and q each independently represent an integer of 0 to 4; a and b each independently represent an integer of 0 to 10. (In formula (2), R 1 ~R4 are each independently a hydrogen atom, an alkyl group, or an aryl group, Z is a single bond or a group represented by the following general formula (3): (In formula (3), R 5 and R 6 are each a hydrogen atom, an optionally substituted alkyl group, or an optionally substituted aryl group, or 5 and R 6 represents a carbon ring or hetero ring having 4 to 20 carbon atoms, which may have a substituent, formed by bonding together, and c, which is not a carbon atom, represents an integer of 1 to 3. [9] The thermoplastic resin composition according to the above item [8], which contains a mold release agent and / or an antioxidant in the thermoplastic resin.

[10] An optical lens comprising the thermoplastic resin composition according to the above item [8] or [9].

[0010] According to the present invention, a thermoplastic resin composition having desired properties, particularly for optical applications, can be reliably produced by mixing a plurality of predetermined types of thermoplastic resins. Furthermore, the method for producing a thermoplastic resin composition of the present invention facilitates the reuse of the thermoplastic resin, thereby expanding recycling and reducing the environmental load.

[0011] 1. Components of the Thermoplastic Resin Composition to be Produced 1-1. Thermoplastic Resin Composition The method for producing a thermoplastic resin composition of the present invention includes a mixing step of mixing at least a first thermoplastic resin containing a structural unit (A) derived from a monomer represented by any one of the general formulas (1a) to (1c) above, and a second thermoplastic resin containing a structural unit (B) derived from a monomer represented by the general formula (2) above. Details of the first and second thermoplastic resins will be described later, but the structural unit (A) contained in the first thermoplastic resin can be, for example, a fluorene-based structural unit having a fluorene ring. Furthermore, the structural unit (B) contained in the second thermoplastic resin can be, for example, a bisphenol-based structural unit derived from a bisphenol-based compound.

[0012] In the method for producing a thermoplastic resin composition of the present invention, the first thermoplastic resin and the second thermoplastic resin are used as a mixture, so recycled materials such as small pieces of each resin that are difficult to reuse can be easily utilized in the production of the thermoplastic resin composition. Therefore, at least one of the first thermoplastic resin and the second thermoplastic resin may contain recycled materials, or at least one of the first thermoplastic resin and the second thermoplastic resin may be exclusively recycled materials. Furthermore, both the first thermoplastic resin and the second thermoplastic resin may be exclusively recycled materials. A recycled material refers to a thermoplastic resin that has been molded at least once to have a predetermined shape and then re-used as a raw material without the predetermined shape. Furthermore, recycled materials also include scraps other than molded products that are generated during the processing of a thermoplastic resin to produce a molded product having a predetermined shape.

[0013] In the thermoplastic resin composition, it is preferable that at least one of the first thermoplastic resin and the second thermoplastic resin is a copolymer containing both the structural unit (A) and the structural unit (B). Furthermore, in the thermoplastic resin composition, both the first thermoplastic resin and the second thermoplastic resin may be a copolymer containing both the structural unit (A) and the structural unit (B).

[0014] In the thermoplastic resin composition, it is preferable that the content of the structural unit (A) is 20 to 95 mol % and the content of the structural unit (B) is 5 to 80 mol % based on the total number of structural units, i.e., the total number of moles, of the first thermoplastic resin and the second thermoplastic resin.

[0015] The content of the structural unit (A) based on the total number of moles of the first thermoplastic resin and the second thermoplastic resin is preferably 25 to 95 mol% or 25 to 90 mol%, more preferably 30 to 95 mol% or 30 to 90 mol%, even more preferably 40 to 90 mol%, 45 to 90 mol%, 40 to 85 mol%, or 45 to 85 mol%, and particularly preferably 55 to 85 mol%, 60 to 85 mol%, 60 to 80 mol%, or 65 to 80 mol%. Furthermore, the content of the structural unit (A) based on the total number of moles of the structural units of the thermoplastic resin composition, i.e., the total number of moles of all structural units of the resin contained in the thermoplastic resin composition, is preferably 25 to 95 mol% or 25 to 90 mol%, more preferably 30 to 95 mol% or 30 to 90 mol%, even more preferably 40 to 90 mol%, 45 to 90 mol%, 40 to 85 mol%, or 45 to 85 mol%, and particularly preferably 55 to 85 mol%, 60 to 85 mol%, 60 to 80 mol%, or 65 to 80 mol%.

[0016] The content of the structural unit (B) based on the total number of moles of the first thermoplastic resin and the second thermoplastic resin is preferably 5 to 75 mol% or 5 to 70 mol%, more preferably 5 to 60 mol% or 10 to 60 mol%, even more preferably 10 to 55 mol%, 10 to 50 mol%, 15 to 50 mol%, or 15 to 45 mol%, and particularly preferably 15 to 35 mol%, 15 to 30 mol%, 20 to 35 mol%, or 20 to 30 mol%. Furthermore, the content of the structural unit (B) based on the total number of moles of the structural units of the thermoplastic resin composition, i.e., the total number of moles of all structural units of the resin contained in the thermoplastic resin composition, is preferably 5 to 75 mol% or 5 to 70 mol%, more preferably 5 to 60 mol% or 10 to 60 mol%, even more preferably 10 to 55 mol%, 10 to 50 mol%, 15 to 50 mol%, or 15 to 45 mol%, and particularly preferably 15 to 35 mol%, 15 to 30 mol%, 20 to 35 mol%, or 20 to 30 mol%.

[0017] In the thermoplastic resin composition, the content of the first thermoplastic resin containing the structural unit (A) is preferably 5 to 95 wt%, 5 to 85 wt%, or 10 to 80 wt%, more preferably 15 to 70 wt%, or 20 to 65 wt%, and even more preferably 30 to 70 wt%, 30 to 65 wt%, 35 to 70 wt%, or 35 to 65 wt% based on the total weight of all thermoplastic resins. Also, in the thermoplastic resin composition, the content of the second thermoplastic resin containing the structural unit (B) is preferably 5 to 95 wt%, 10 to 90 wt%, or 15 to 85 wt%, more preferably 20 to 75 wt%, or 20 to 70 wt%, and even more preferably 35 to 75 wt%, 35 to 70 wt%, 40 to 75 wt%, or 40 to 70 wt% based on the total weight of all thermoplastic resins. In addition, with respect to a thermoplastic resin having both the structural unit (A) and the structural unit (B), one in which the number of moles of the structural unit (A) is greater than that of the structural unit (B) is referred to as a first thermoplastic resin, and one in which the number of moles of the structural unit (B) is greater than that of the structural unit (A) is referred to as a second thermoplastic resin.

[0018] In the thermoplastic resin composition, the total content of the first thermoplastic resin containing the structural unit (A) and the second thermoplastic resin containing the structural unit (B) is preferably 40% by weight or more, more preferably 50% by weight or more or 60% by weight or more, even more preferably 70% by weight or more or 80% by weight or more, and particularly preferably 90% by weight or more or 95% by weight or more, based on the total weight of all thermoplastic resins. It is particularly preferred that all of the thermoplastic resins contained in the thermoplastic resin composition are substantially the first thermoplastic resin or the second thermoplastic resin.

[0019] In the thermoplastic resin composition, the total content of the first thermoplastic resin containing the structural unit (A) and the second thermoplastic resin containing the structural unit (B) is preferably 40% by weight or more, more preferably 50% by weight or more, even more preferably 70% by weight or more, and particularly preferably 90% by weight or more, based on the total weight of the thermoplastic resin composition. Thus, the thermoplastic resin composition may contain components other than the first and second thermoplastic resins. For example, the thermoplastic resin composition may contain thermoplastic resins, additives, etc., the details of which will be described later, other than the first and second thermoplastic resins.

[0020] The type of thermoplastic resin contained in the thermoplastic resin composition is not particularly limited, but is preferably a polycarbonate resin, a polyester resin, or a polyestercarbonate resin, and more preferably a polycarbonate resin. The thermoplastic resin contained in the thermoplastic resin composition may have a random copolymer, a block copolymer, or an alternating copolymer structure, or may be a homopolymer.

[0021] 1-2. First Thermoplastic Resin The first thermoplastic resin contains at least a structural unit (A) derived from a monomer represented by any one of general formulas (1a) to (1c). In general formulas (1a) to (1c), R c and R d are each independently selected from the group consisting of a hydrogen atom, a halogen atom, an alkyl group having 1 to 20 carbon atoms which may have a substituent, an alkoxyl group having 1 to 20 carbon atoms which may have a substituent, a cycloalkyl group having 5 to 20 carbon atoms which may have a substituent, a cycloalkoxyl group having 5 to 20 carbon atoms which may have a substituent, and an aryl group having 6 to 20 carbon atoms which may have a substituent. c and R dare preferably each independently selected from a hydrogen atom, an alkyl group having 1 to 20 carbon atoms which may have a substituent, an alkoxyl group having 1 to 20 carbon atoms which may have a substituent, a cycloalkyl group having 5 to 20 carbon atoms which may have a substituent, and an aryl group having 6 to 20 carbon atoms which may have a substituent, and more preferably are each independently selected from a hydrogen atom, an alkyl group having 1 to 20 carbon atoms which may have a substituent, and an aryl group having 6 to 20 carbon atoms which may have a substituent. c and R d is more preferably selected from a hydrogen atom and an aryl group having 6 to 20 carbon atoms which may have a substituent.

[0022] In general formulas (1a) to (1c), A and B each independently represent an alkylene group having 1 to 5 carbon atoms which may have a substituent, preferably an alkylene group having 1 to 3 carbon atoms which may have a substituent, and more preferably an alkylene group having 1 or 2 carbon atoms which may have a substituent. In general formulas (1a) to (1c), p and q each independently represent an integer of 0 to 4, preferably an integer of 0 to 3, and more preferably 0 or 1. Furthermore, in general formulas (1a) to (1c), a and b each independently represent an integer of 0 to 10, preferably an integer of 0 to 5, more preferably an integer of 0 to 3, and particularly preferably 0 or 1.

[0023] R in general formulas (1a) to (1c) c and R d Among the options, the number of carbon atoms in the alkyl group having 1 to 20 carbon atoms, which may have a substituent, and the alkoxy group having 1 to 20 carbon atoms, which may have a substituent, is preferably 1 to 10, more preferably 1 to 6, and even more preferably 1 to 3, or 1. c and R d Among the options, the carbon number of the cycloalkyl group having 5 to 20 carbon atoms, which may have a substituent, and the carbon number of the cycloalkoxyl group having 5 to 20 carbon atoms, which may have a substituent, is preferably 5 to 10, more preferably 6 to 8, and even more preferably 6 or 7.c and R d Among the options above, the number of carbon atoms in the aryl group having 6 to 20 carbon atoms, which may have a substituent, is preferably 6 to 12, more preferably 6 to 10, and even more preferably 6 to 8, or 6.

[0024] In the general formulas (1a) to (1c), each Y is independently a single bond, a fluorene group which may have a substituent, or any of the structural formulae represented by the following formulas (i) to (vii): In formulas (i) to (vii), R 61 , R 62 , R 71 and R 72 each independently represents a hydrogen atom, a halogen atom, an alkyl group having 1 to 20 carbon atoms which may have a substituent, or an aryl group having 6 to 30 carbon atoms which may have a substituent, or 61 and R 62 , or R 71 and R 72 are bonded to each other to form a carbocyclic or heterocyclic ring having 4 to 20 carbon atoms, which may have a substituent; r and s each independently represent an integer of 0 to 5,000. A and B each independently represent an alkylene group having 1 to 5 carbon atoms, which may have a substituent; p and q each independently represent an integer of 0 to 4; a and b each independently represent an integer of 0 to 10.

[0025] R 61 , R 62 , R 71 and R 72 Among the options, the number of carbon atoms in the alkyl group having 1 to 20 carbon atoms, which may have a substituent, is preferably 1 to 10, more preferably 1 to 6, and even more preferably 1 to 3, or 1. 61 , R 62 , R 71 and R 72 Among the options, the number of carbon atoms of the aryl group having 6 to 30 carbon atoms, which may have a substituent, is preferably 6 to 20, more preferably 6 to 10, and even more preferably 6 to 8. 61 and R 62are bonded to each other to form, or R 71 and R 72 The number of carbon atoms in the carbocyclic or heterocyclic ring having 4 to 20 carbon atoms, which may have a substituent, formed by bonding together, is preferably 5 to 10, and more preferably 6 to 8. The number of carbon atoms in the carbocyclic or heterocyclic ring having 4 to 20 carbon atoms, which may have a substituent, includes the C atom represented by formula (i) as one. Furthermore, r and s are preferably 0 to 1000, for example, 0 to 500, 0 to 100, etc.

[0026] In general formulas (1a) to (1c), A and B are preferably alkylene groups having 1 to 3 carbon atoms, which may have a substituent, and more preferably alkylene groups having 1 or 2 carbon atoms. p and q are preferably integers of 0 to 2, and more preferably 0 or 1. a and b are preferably integers of 0 to 5, and more preferably integers of 0 to 3, and even more preferably 0 or 1.

[0027] In the general formulae (1a) to (1c), each Y is preferably a single bond or an optionally substituted fluorene group, more preferably an optionally substituted fluorene group.

[0028] Examples of the substituents that can be contained in the structural unit (A) of the above formulas (1a) to (1c) include halogen atoms, hydroxy groups, carboxy groups, cyano groups, C1 to C10 amide groups, C1 to C10 alkyl groups, C5 to C10 cycloalkyl groups, C1 to C10 alkoxy groups, C5 to C10 cycloalkyloxy groups, C2 to C10 alkyloxycarbonyl groups, C5 to C10 cycloalkyloxycarbonyl groups, C7 to C15 aryloxycarbonyl groups, C2 to C10 alkylcarbonyloxy groups, C5 to C10 cycloalkylcarbonyloxy groups, C7 to C15 arylcarbonyloxy groups, C2 to C10 alkylcarbonyloxy groups, C5 to C10 cycloalkylcarbonyloxy groups, C7 to C15 arylcarbonyloxy groups, C2 to C10 hydroxyalkylcarbonyl groups, and glycidyloxycarbonyl groups. The carbon numbers in the general formulas (1a) to (1c) include the number of carbon atoms in the substituents.

[0029] Preferred specific examples of the monomer of the above formula (1a) include BPEF (9,9-bis(4-(2-hydroxyethoxy)phenyl)fluorene), BPPEF (9,9-bis(4-(2-hydroxyethoxy)-3-phenylphenyl)fluorene), and the like.

[0030] A preferred specific example of the monomer of the above formula (1c) is a fluorene compound represented by the following formula (1c-1). A' and B' in general formula (1c-1) are the same as the above-mentioned A and B in formula (1c), respectively. Specifically, A' and B' in formula (1c-1) each independently represent an alkylene group having 1 to 5 carbon atoms which may have a substituent, preferably an alkylene group having 1 to 3 carbon atoms which may have a substituent, and more preferably an alkylene group having 1 or 2 carbon atoms which may have a substituent. Furthermore, a' and b' in general formula (1c-1) are also the same as the above-mentioned a and b in formula (1c), respectively. Specifically, a' and b' in formula (1c-1) each independently represent an integer of 0 to 10, preferably an integer of 0 to 5, more preferably an integer of 0 to 3, and particularly preferably 0 or 1.

[0031] A specific preferred example of the monomers of the above formula (1c) and formula (1c-1) is BNEF (9,9-bis(6-(2-hydroxyethoxy)naphthalen-2-yl)fluorene). The monomer compounds of the above formulas (1a) to (1c) may be used alone or in combination of two or more to form the structural unit (A).

[0032] The first thermoplastic resin is preferably a copolymer having the structural unit (B) together with the structural unit (A). In such a copolymer, the content of the structural unit (A) is preferably 5 to 90 mol%, 10 to 90 mol%, or 15 to 85 mol%, more preferably 20 to 75 mol% or 20 to 70 mol%, even more preferably 35 to 75 mol%, 35 to 70 mol%, 40 to 75 mol%, or 40 to 70 mol%, and particularly preferably 45 to 65 mol%, 45 to 60 mol%, 50 to 60 mol%, or 50 to 55 mol%, based on the total number of moles of the fluorene-based structural unit (A) and the fluorene-based structural unit (B).

[0033] In the first thermoplastic resin, the content of the structural unit (A) in all structural units is preferably 40 mol% or more, more preferably 50 mol% or 60 mol% or more, even more preferably 70 mol% or 80 mol% or more, and particularly preferably 90 mol% or 95 mol% or more.

[0034] The first thermoplastic resin may be a copolymer containing both the structural unit (A) and the structural unit (B), or may be a polymer having only the structural unit (A), such as a homopolymer. Note that the thermoplastic resin composition may contain a mixture of multiple different types of first thermoplastic resins containing the above-mentioned structural unit (A).

[0035] 1-3. Second Thermoplastic Resin The second thermoplastic resin contains at least a structural unit (B) derived from a monomer represented by the following general formula (2): In formula (2), R 1 ~R 4 are each independently a hydrogen atom, an alkyl group which may have a substituent, or an aryl group which may have a substituent, and Z is a single bond or a group represented by the following general formula (3): In formula (3), R 5 and R 6 are each a hydrogen atom, an alkyl group, or an aryl group, or 5 and R6 represents a carbon ring or hetero ring having 4 to 20 carbon atoms, which may have a substituent, formed by bonding together. 5 and R 6 The lower case c, which is not C meaning a carbon atom and is bonded to the group, represents an integer of 1 to 3.

[0036] R in the above formula (2) 1 ~R 4 is preferably selected from a hydrogen atom, an alkyl group having 1 to 10 carbon atoms which may have a substituent, and an aryl group having 6 to 20 carbon atoms which may have a substituent, more preferably selected from a hydrogen atom, an alkyl group having 1 to 6 carbon atoms which may have a substituent, and an aryl group having 6 to 12 carbon atoms which may have a substituent, and even more preferably selected from a hydrogen atom, an alkyl group having 1 to 3 carbon atoms, and an aryl group having 6 to 8 carbon atoms.

[0037] In addition, Z in formula (2) is preferably a group represented by the above general formula (3). 5 and R 6 may each be a hydrogen atom, an alkyl group which may have a substituent, or an aryl group which may have a substituent. 5 and R 6 are each preferably selected from a hydrogen atom, an alkyl group having 1 to 10 carbon atoms, and an aryl group having 6 to 20 carbon atoms, more preferably selected from a hydrogen atom, an alkyl group having 1 to 6 carbon atoms, and an aryl group having 6 to 12 carbon atoms, and even more preferably selected from a hydrogen atom, an alkyl group having 1 to 3 carbon atoms, and an aryl group having 6 to 8 carbon atoms. 5 and R 6 may be bonded to each other to form a carbon ring or hetero ring having 4 to 20 carbon atoms which may have a substituent. In this case, R 5 and R 6 preferably forms a carbon ring having 6 to 16 carbon atoms, which may have a substituent, and more preferably forms a carbon ring having 8 to 12 carbon atoms, which may have a substituent. In formula (3), c represents an integer of 1 to 3, preferably an integer of 1 or 2, and more preferably 1.

[0038] The second thermoplastic resin may be a copolymer containing both the structural unit (B) and the structural unit (A), or may be a polymer containing only the structural unit (B), such as a homopolymer. Note that the thermoplastic resin composition may contain a mixture of multiple different types of second thermoplastic resins containing the above-mentioned structural unit (B).

[0039] Examples of the substituent that can be contained in the structural unit (B) of formula (2) above include a halogen atom, a hydroxy group, a carboxy group, a cyano group, an amide group having 1 to 10 carbon atoms, an alkyl group having 1 to 10 carbon atoms, a cycloalkyl group having 5 to 10 carbon atoms, an alkoxy group having 1 to 10 carbon atoms, a cycloalkyloxy group having 5 to 10 carbon atoms, an alkyloxycarbonyl group having 2 to 10 carbon atoms, a cycloalkyloxycarbonyl group having 5 to 10 carbon atoms, an aryloxycarbonyl group having 7 to 15 carbon atoms, an alkylcarbonyloxy group having 2 to 10 carbon atoms, a cycloalkylcarbonyloxy group having 5 to 10 carbon atoms, an arylcarbonyloxy group having 7 to 15 carbon atoms, a hydroxyalkylcarbonyl group having 2 to 10 carbon atoms, and a glycidyloxycarbonyl group. The number of carbon atoms in formula (2) includes the number of carbon atoms of the substituent.

[0040] Specific preferred examples of the monomer that forms the structural unit (B) of formula (2) include bisphenol A, bisphenol AP, bisphenol AF, bisphenol B, bisphenol BP, bisphenol C, bis(4-hydroxyphenyl)-2,2-dichloroethylene, bisphenol E, bisphenol F, bisphenol G, bisphenol M, bisphenol S, bisphenol P, bisphenol PH, bisphenol TMC, bisphenol P-AP (4,4'-(1-phenylethylidene)bisphenol), bisphenol P-CDE (4,4'-cyclododecylidenebisphenol), bisphenol P-HTG (4,4'-(3,3,5-trimethylcyclohexylidene)bisphenol), bisphenol P-MIBK (4,4'-(1,3-dimethylbutylidene)bisphenol), bisphenol P-AP (4,4'-(1-phenylethylidene)bisphenol), bisphenol P-CDE (4,4'-cyclododecylidenebisphenol), bisphenol P-MIBK (4,4'-(1,3-dimethylbutylidene)bisphenol), bisphenol P-MIBK (4,4'-(1,3-dimethylbutylidene)bisphenol), bisphenol P-AP (4,4'-(1-phenylethylidene)bisphenol), bisphenol P-CDE (4,4'-cyclododecylidenebisphenol), bisphenol P-HTG (4,4'-(3,3,5-trimethylcyclohexylidene)bisphenol), bisphenol P-MIBK (4,4'-(1,3-dimethylbutylidene)bisphenol), bisphenol P-MIBK (4,4'-(1,3-dimethylbutylidene)bisphenol), bisphenol P-AP (4,4'-(1-phenylethylidene)bisphenol), bisphenol P-CDE (4,4'-cyclododecylidenebisphenol), bisphenol P-MIBK (4,4'-(1,3-dimethylbutylide Examples thereof include those derived from phenol PEO-FL (bisphenoxyethanol fluorene), bisphenol P-3MZ (4-[1-(4-hydroxyphenyl)-3-methylcyclohexyl]phenol), bisphenol OC-FL (4,4'-[1-[4-[1-(4-hydroxyphenyl)-1-methylethyl]phenyl]ethylidene]bisphenol), bisphenol Z, BP-2EO (2,2'-[[1,1'-biphenyl]-4,4'-diylbis(oxy)bisethanol), S-BOC (4,4'-(1-methylethylidene)bis(2-methylphenol), bisphenol OC-FL (4,4'-[1-[4-[1-(4-hydroxyphenyl)-1-methylethyl]phenyl]ethylidene]bisphenol), TrisP-HAP (4,4',4''-ethylidene trisphenol), and the like. Among these, more preferred specific examples of the structural unit (B) include those derived from bisphenol A, bisphenol C, bisphenol TMC, etc. The monomer compounds of the above formula (2) may be used alone or in combination of two or more to form the structural unit (B).

[0041] 1-4. Other Thermoplastic Resins The thermoplastic resin composition may contain a thermoplastic resin (other thermoplastic resin) other than the first thermoplastic resin and the second thermoplastic resin described above. For example, the thermoplastic resin composition may contain a thermoplastic resin having a structural unit (C) derived from a monomer represented by the following general formula (5): In general formula (5), R a and R b each independently represents a hydrogen atom, a halogen atom, an alkyl group having 1 to 20 carbon atoms which may have a substituent, an alkoxyl group having 1 to 20 carbon atoms which may have a substituent, a cycloalkyl group having 5 to 20 carbon atoms which may have a substituent, a cycloalkoxyl group having 5 to 20 carbon atoms which may have a substituent, an aryl group having 6 to 20 carbon atoms which may have a substituent, a heteroaryl group having 6 to 20 carbon atoms which contains one or more hetero ring atoms selected from O, N and S and which may have a substituent, an aryloxy group having 6 to 20 carbon atoms which may have a substituent, and -C≡C-R h and R h is an aryl group having 6 to 20 carbon atoms which may have a substituent, or a heteroaryl group having 6 to 20 carbon atoms which contains one or more hetero ring atoms selected from O, N, and S and which may have a substituent.

[0042] R in general formula (5) a and R b is preferably selected from a hydrogen atom, an alkyl group having 1 to 20 carbon atoms which may have a substituent, an alkoxyl group having 1 to 20 carbon atoms which may have a substituent, a cycloalkyl group having 5 to 20 carbon atoms which may have a substituent, and an aryl group having 6 to 20 carbon atoms which may have a substituent, and more preferably selected from a hydrogen atom, an alkyl group having 1 to 20 carbon atoms which may have a substituent, and an aryl group having 6 to 20 carbon atoms which may have a substituent. a and R b is more preferably selected from a hydrogen atom and an aryl group having 6 to 20 carbon atoms which may have a substituent.

[0043] In general formula (5), X is a single bond or an alkylene group having 3 or less carbon atoms which may have a substituent, preferably a single bond or an alkylene group having 2 or less carbon atoms which may have a substituent, more preferably a single bond or an alkylene group having 1 carbon atom which may have a substituent, and particularly preferably a single bond. In general formula (5), A and B each independently represent an alkylene group having 1 to 5 carbon atoms which may have a substituent, preferably an alkylene group having 1 to 3 carbon atoms which may have a substituent, and more preferably an alkylene group having 1 or 2 carbon atoms which may have a substituent. In general formula (5), m and n each independently represent an integer of 0 to 6, preferably an integer of 0 to 3, and more preferably 0 or 1. In general formula (5), a and b each independently represent an integer of 0 to 10, preferably an integer of 0 to 5, more preferably an integer of 0 to 3, and particularly preferably 0 or 1.

[0044] R in general formula (5) a and R b Among the options, the number of carbon atoms in the alkyl group having 1 to 20 carbon atoms, which may have a substituent, and the alkoxy group having 1 to 20 carbon atoms, which may have a substituent, is preferably 1 to 10, more preferably 1 to 6, and even more preferably 1 to 3, or 1. a and R b Among the options, the carbon number of the cycloalkyl group having 5 to 20 carbon atoms, which may have a substituent, and the carbon number of the cycloalkoxy group having 5 to 20 carbon atoms, which may have a substituent, are each preferably 5 to 10, more preferably 6 to 8, and even more preferably 6 or 7. a and R b Among the options above, the number of carbon atoms in the aryl group having 6 to 20 carbon atoms which may have a substituent, the heteroaryl group having 6 to 20 carbon atoms which contains one or more hetero ring atoms selected from O, N and S and which may have a substituent, and the aryloxy group having 6 to 20 carbon atoms which may have a substituent are each preferably 6 to 12, more preferably 6 to 10, and even more preferably 6 to 8, or 6.

[0045] Examples of the substituent that can be contained in the structural unit (C) of formula (5) include a halogen atom, a hydroxy group, a carboxy group, a cyano group, an amide group having 1 to 10 carbon atoms, an alkyl group having 1 to 10 carbon atoms, a cycloalkyl group having 5 to 10 carbon atoms, an alkoxy group having 1 to 10 carbon atoms, a cycloalkyloxy group having 5 to 10 carbon atoms, an alkyloxycarbonyl group having 2 to 10 carbon atoms, a cycloalkyloxycarbonyl group having 5 to 10 carbon atoms, an aryloxycarbonyl group having 7 to 15 carbon atoms, an alkylcarbonyloxy group having 2 to 10 carbon atoms, a cycloalkylcarbonyloxy group having 5 to 10 carbon atoms, an arylcarbonyloxy group having 7 to 15 carbon atoms, a hydroxyalkylcarbonyl group having 2 to 10 carbon atoms, and a glycidyloxycarbonyl group. The number of carbon atoms in formula (5) includes the number of carbon atoms of the substituent.

[0046] Specific preferred examples of the monomer that forms the structural unit (C) of formula (5) include 2,2'-bis(hydroxy(poly)alkoxy)-diaryl-1,1'-binaphthalenes, 2,2'-bis(hydroxy(poly)alkoxy)-dinaphthyl-1,1'-binaphthalenes, and the like. Of these monomer compounds, 2,2'-bis(2-hydroxyethoxy)-6,6'-diphenyl-1,1'-binaphthalene, 2,2'-bis(2-hydroxyethoxy)-6,6'-di(naphthalen-1-yl)-1,1'-binaphthalene, 2,2'-bis(2-hydroxymethoxy)-6,6'-diphenyl-1,1'-binaphthalene, 2,2'-bis(2-hydroxymethoxy)-6,6'-di(naphthalen-1-yl)-1,1'-binaphthalene, 2,2'-bis(2-hydroxypropoxy)-6,6'-diphenyl-1,1'-binaphthalene, and 2,2'-bis(2-hydroxypropoxy)-6,6'-di(naphthalen-1-yl)-1,1'-binaphthalene are preferred. The monomer compound of formula (5) may be used alone or in combination to form the structural unit (C). Specific preferred examples of the monomer compound of formula (5) include the following:

[0047] The thermoplastic resin composition may also contain a thermoplastic resin having a structural unit derived from an aliphatic diol which may have a substituent. Specific examples of the aliphatic diol which may have a substituent include ethylene glycol, 1,2-propylene glycol, 1,3-propanediol, 1,3-butanediol, 2-methyl-1,3-propanediol, 1,3-pentanediol, 2,4-pentanediol, 2-methyl-1,3-butanediol, neopentyl glycol, 1,3-hexanediol, 3-methyl-1,3-butanediol, 1,5-pentanediol, 2-methyl-1,5-pentanediol, 3-methyl-1,5-pentanediol, 1,5-hexanediol, 2-ethyl-1,5-pentanediol, and 2-propyl-1,5-pentanediol. aliphatic diols such as 2,2-diethyl-1,3-propanediol, 2-methyl-2-propyl-1,3-propanediol, 2-butyl-2-ethyl-1,3-propanediol, 2-methyl-1,2-propanediol, 1,4-butanediol, 1,6-hexanediol, 2,5-hexanediol, 1,9-nonanediol, 2-methyl-1,8-octanediol, diethylene glycol, triethylene glycol, metaxylylene glycol, paraxylylene glycol, polyethylene glycol, polypropylene glycol, and polybutylene glycol;1,3-Cyclohexanediol, 1,4-cyclohexanediol, 1,3-bis(hydroxymethyl)cyclohexane, 1,4-bis(hydroxymethyl)cyclohexane, 1,3-cyclohexanedimethanol, 1,4-cyclohexanedimethanol, 1,2-decahydronaphthalenedimethanol, 1,3-decahydronaphthalenedimethanol, 1,4-decahydronaphthalenedimethanol, 1,5-decahydronaphthalenedimethanol, 1,6-decahydronaphthalenedimethanol, 2,7-decahydronaphthalenedimethanol, tetralin dimethanol alicyclic diols such as norbornane dimethanol, tricyclodecane dimethanol, 5-methylol-5-ethyl-2-(1,1-dimethyl-2-hydroxyethyl)-1,3-dioxane, pentacyclododecane dimethanol, 3,9-bis(1,1-dimethyl-2-hydroxyethyl)-2,4,8,10-tetraoxaspiro[5.5]undecane (or (β,β,β',β'-tetramethyl-2,4,8,10-tetraoxaspiro[5,5]undecane-3,9-diethanol (SPG (spiroglycol)));

[0048] Examples of the substituents that can be contained in the structural units derived from aliphatic diols include halogen atoms, hydroxy groups, carboxy groups, cyano groups, C1-10 amide groups, C1-10 alkyl groups, C5-10 cycloalkyl groups, C1-10 alkoxy groups, C5-10 cycloalkyloxy groups, C2-10 alkyloxycarbonyl groups, C5-10 cycloalkyloxycarbonyl groups, C7-15 aryloxycarbonyl groups, C2-10 alkylcarbonyloxy groups, C5-10 cycloalkylcarbonyloxy groups, C7-15 arylcarbonyloxy groups, C2-10 hydroxyalkylcarbonyl groups, and glycidyloxycarbonyl groups. The number of carbon atoms in the structural units derived from aliphatic groups includes the number of carbon atoms in the substituents.

[0049] 1-5. Secondary Components The thermoplastic resin composition may contain components other than the thermoplastic resin. For example, at least one additive selected from a mold release agent, an antioxidant, and the like. The thermoplastic resin composition preferably contains either a mold release agent or an antioxidant, or both. In the thermoplastic resin composition, the content of secondary components such as additives other than the thermoplastic resin is preferably 20% by weight or less, more preferably 15% by weight or less or 10% by weight or less, even more preferably 7% by weight or less or 5% by weight or less, and particularly preferably 3% by weight or less or 2% by weight or less, based on the total weight.

[0050] Specific examples of additives contained in the thermoplastic resin composition include the following. Mold Release Agents Examples of mold release agents include carboxylic acid esters, polysiloxane compounds, and paraffin wax (polyolefin-based). Specific examples include at least one compound selected from the group consisting of aliphatic carboxylic acids, esters of aliphatic carboxylic acids and alcohols, aliphatic hydrocarbon compounds with a number-average molecular weight of 200 to 15,000, and polysiloxane-based silicone oils. Examples of aliphatic carboxylic acids include saturated or unsaturated aliphatic mono-, di-, or tri-carboxylic acids. Here, aliphatic carboxylic acids also include alicyclic carboxylic acids. Among these, preferred aliphatic carboxylic acids are mono- or di-carboxylic acids having 6 to 36 carbon atoms, and more preferred are saturated aliphatic mono-carboxylic acids having 6 to 36 carbon atoms. Specific examples of aliphatic carboxylic acids include palmitic acid, stearic acid, valeric acid, caproic acid, capric acid, lauric acid, arachic acid, behenic acid, lignoceric acid, cerotic acid, melissic acid, tetraacontanoic acid, montanic acid, glutaric acid, adipic acid, and azelaic acid. The same aliphatic carboxylic acids as those described above can be used as the aliphatic carboxylic acids in the esters of aliphatic carboxylic acids and alcohols. On the other hand, examples of alcohols include saturated or unsaturated monohydric or polyhydric alcohols. These alcohols may have a substituent such as a fluorine atom or an aryl group. Among these, monohydric or polyhydric saturated alcohols having 30 or less carbon atoms are preferred, and aliphatic saturated monohydric or polyhydric alcohols having 30 or less carbon atoms are more preferred. Here, aliphatic compounds also include alicyclic compounds. Specific examples of alcohols include octanol, decanol, dodecanol, stearyl alcohol, behenyl alcohol, ethylene glycol, diethylene glycol, glycerin, pentaerythritol, 2,2-dihydroxyperfluoropropanol, neopentylene glycol, ditrimethylolpropane, dipentaerythritol, etc. The above-mentioned ester compounds may contain aliphatic carboxylic acids and / or alcohols as impurities, or may be a mixture of multiple compounds.Specific examples of esters of aliphatic carboxylic acids and alcohols include beeswax (a mixture primarily composed of myricyl palmitate), stearyl stearate, behenyl behenate, stearyl behenate, glycerin monopalmitate, glycerin monostearate, glycerin distearate, glycerin tristearate, pentaerythritol monopalmitate, pentaerythritol monostearate, pentaerythritol distearate, pentaerythritol tristearate, and pentaerythritol tetrastearate. Aliphatic hydrocarbons having a number-average molecular weight of 200 to 15,000 include liquid paraffin, paraffin wax, microcrystalline wax, polyethylene wax, Fischer-Tropsch wax, and α-olefin oligomers having 3 to 12 carbon atoms. Aliphatic hydrocarbons also include alicyclic hydrocarbons. These hydrocarbon compounds may also be partially oxidized. Among these, paraffin wax, polyethylene wax, or partially oxidized polyethylene wax are preferred, with paraffin wax and polyethylene wax being more preferred. The number average molecular weight is preferably 200 to 5000. These aliphatic hydrocarbons may be a single substance or a mixture of substances with various constituent components and molecular weights, as long as the main component is within the above range. Examples of polysiloxane-based silicone oils include dimethyl silicone oil, phenylmethyl silicone oil, diphenyl silicone oil, and fluorinated alkyl silicone. Two or more of these may be used in combination.

[0051] The addition ratio of the release agent is preferably 0.001 parts by mass or more, more preferably 0.01 parts by mass or more, and preferably 2 parts by mass or less, more preferably 1 part by mass or less, relative to 100 parts by mass of the thermoplastic resin. Only one type of release agent may be used, or two or more types may be used. When two or more types are used, it is preferable that the total amount is within the above range.

[0052] Antioxidant Examples of the antioxidant include phenol-based antioxidants, hindered phenol-based antioxidants, bisphenol-based antioxidants, and polyphenol-based antioxidants.

[0053] Specifically, 2,6-di-tert-butyl-4-methylphenol, tris(3,5-di-tert-butyl-4-hydroxybenzyl)isocyanurate, n-octadecyl-3-(3',5'-di-tert-butyl-4'-hydroxyphenyl)propionate, tetrakis[methylene-3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate]methane, 4,4'-butylidenebis-(3-methyl-6-tert-butylphenol), triethylene glycol-bis[3-(3-tert t-butyl-4-hydroxy-5-methylphenyl)propionate], 3,9-bis{2-[3-(3-tert-butyl-4-hydroxy-5-methylphenyl)propionyloxy]-1,1-dimethylethyl}-2,4,8,10-tetraoxaspiro[5,5]undecane, pentaerythritol tetrakis[3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate], thiodiethylene bis[3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate], N,N' -hexane-1,6-diylbis[3-(3,5-di-tert-butyl-4-hydroxyphenylpropionamide)], 2,4-dimethyl-6-(1-methylpentadecyl)phenol, diethyl [[3,5-bis(1,1-dimethylethyl)-4-hydroxyphenyl]methyl]phosphate, 3,3',3",5,5',5"-hexa-tert-butyl-a,a',a"-(mesitylene-2,4,6-triyl)tri-p-cresol, 4,6-bis(octylthiomethyl)-o-cresol, ethylenebis(oxa hexamethylenebis[3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate], hexamethylenebis[3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate], 1,3,5-tris(3,5-di-tert-butyl-4-hydroxybenzyl)-1,3,5-triazine-2,4,6(1H,3H,5H)-trione, 2,6-di-tert-butyl-4-(4,6-bis(octylthio)-1,3,5-triazin-2-ylamino)phenol, and the like.Examples of phenol-based antioxidants include "Irganox 1010" (registered trademark, the same applies hereinafter) and "Irganox 1076" manufactured by BASF, and "Adekastab AO-50" and "Adekastab AO-60" manufactured by Adeka Corporation.

[0054] The antioxidant is preferably added in an amount of 0.001 parts by mass or more, more preferably 0.01 parts by mass or more, and preferably 1 part by mass or less, more preferably 0.5 parts by mass or less, relative to 100 parts by mass of the thermoplastic resin. Only one type of antioxidant may be contained, or two or more types may be contained. When two or more types are contained, it is preferable that the total amount is within the above range.

[0055] 2. Method for Producing Thermoplastic Resin Composition The method for producing a thermoplastic resin composition is described below. Thermoplastic resins such as the first and second thermoplastic resins can be produced by known methods. For example, a thermoplastic resin can be produced by carrying out a polymerization reaction in a reaction system containing a monomer compound and a catalyst at a polymerization temperature of 200 to 250°C and a pressure of 760 to 200 mmHg. For example, a thermoplastic resin such as a polycarbonate resin can be produced by melt polycondensation using monomer compounds represented by the above general formulas (1) to (3) and carbonate precursors such as carbonate diesters as raw materials in the presence of a basic compound catalyst, a transesterification catalyst, or a mixed catalyst containing both, or in the absence of a catalyst.

[0056] The method for producing a thermoplastic resin composition includes at least a mixing step of mixing multiple types of thermoplastic resins. In the mixing step, different types of thermoplastic resins and the secondary components described above are preferably melt-kneaded or dissolved in a solvent and blended, and then the solvent is volatilized. Suitable solvents include, for example, halogenated organic solvents and THF. A thermoplastic resin composition can be produced by a method including such a mixing step. In the mixing step, additives may be mixed with the thermoplastic resin by a known method.

[0057] 3. Method for Adjusting the Properties of Thermoplastic Resin Composition The above-described mixing step can also be used as part of a method for adjusting the properties of a thermoplastic resin composition. For example, by mixing first and second thermoplastic resins having different parameter values ​​such as refractive index in a predetermined ratio, the property values ​​of the resulting thermoplastic resin composition can be adjusted to a predetermined level.

[0058] 4. Properties of Thermoplastic Resin Composition and Thermoplastic Resin Preferred properties of the thermoplastic resin composition and thermoplastic resin are as follows.

[0059] 4-1. Refractive Index The refractive index (nD) of the thermoplastic resin composition according to JIS B 7071-2:2018 is 1.550 to 1.700, and can be adjusted appropriately depending on the application of the composition. For example, to form a lens unit using multiple lenses, a thermoplastic resin composition having a refractive index within a wide range is desired. Preferred refractive index (nD) ranges of the thermoplastic resin composition include, for example, 1.570 to 1.650, 1.570 to 1.680, 1.580 to 1.670, 1.590 to 1.660, 1.600 to 1.650, 1.610 to 1.645, 1.620 to 1.640, 1.623 to 1.637, 1.625 to 1.635, 1.628 to 1.630, or 1.628 to 1.629. Furthermore, the refractive index (nD) of the thermoplastic resin composition can be preferably in the range of 1.570 or more, 1.580 or more, 1.590 or more, 1.600 or more, 1.610 or more, 1.620 or more, 1.630 or more, 1.640 or more, 1.650 or more, 1.660 or more, 1.670 or more, 1.680 or more, or 1.690 or more.

[0060] The refractive index (nD) of the first thermoplastic resin according to JIS B 7071-2:2018 is 1.650 or less. The refractive index of the first thermoplastic resin is preferably greater than that of the second thermoplastic resin and can be adjusted appropriately depending on the application of the thermoplastic resin composition containing the first thermoplastic resin. For example, preferred refractive index (nD) ranges of the first thermoplastic resin include 1.700 or less, 1.655 or less, 1.645 or less, 1.640 or less, 1.635 or less, 1.630 or less, 1.625 or less, 1.620 or less, 1.615 or less, 1.610 or less, 1.605 or less, and 1.600 or less. The preferred range of the refractive index (nD) of the first thermoplastic resin composition may be 1.600 to 1.670, 1.610 to 1.665, 1.620 to 1.660, 1.625 to 1.655, 1.630 to 1.650, or 1.635 to 1.645.

[0061] The refractive index (nD) of the first thermoplastic resin according to JIS B 7071-2:2018 is 1.570 or higher. The refractive index of the second thermoplastic resin is preferably smaller than that of the first thermoplastic resin and can be adjusted appropriately depending on the application of the thermoplastic resin composition containing the second thermoplastic resin. For example, preferred refractive index (nD) ranges of the first thermoplastic resin include 1.560 or higher, 1.565 or higher, 1.575 or higher, 1.580 or higher, 1.585 or higher, 1.590 or higher, 1.595 or higher, 1.600 or higher, 1.605 or higher, 1.610 or higher, 1.615 or higher, and 1.620 or higher. The preferred range of the refractive index (nD) of the second thermoplastic resin composition may be 1.560 to 1.630, 1.565 to 1.625, 1.570 to 1.620, 1.575 to 1.615, 1.580 to 1.610, or 1.585 to 1.605.

[0062] 4-2. Total Light Transmittance (TT (%)) The total light transmittance (%) of the thermoplastic resin composition, measured by the method described below, is preferably 60% or more, more preferably 70% or more, more preferably 80% or more, and particularly preferably 85% or more. 4-3. YI Value The YI value of the thermoplastic resin composition, measured by the method described below, is preferably 20 or less, more preferably 16 or less or 14 or less, more preferably 12 or less, 10 or less, 9.0 or less or 8.0 or less, and particularly preferably 7.0 or less, 6.0 or less or 5.0 or less. 4-4. Haze The haze value of the thermoplastic resin composition, measured by the method described below, is preferably 2.0 or less or 1.6 or less, more preferably 1.2 or less or 1.0 or less, more preferably 0.8 or less or 0.6 or less, and particularly preferably 0.4 or less or 0.3 or less.

[0063] 4-5. Abbe Number (νd) The Abbe number (νd) of the thermoplastic resin composition, measured by the method described below, is preferably 32 or less or 31 or less, more preferably 30 or less or 29 or less, even more preferably 28 or less or 26 or less, and particularly preferably 25 or less or 24.5 or less. However, the Abbe number (νd) of the thermoplastic resin composition can be adjusted appropriately depending on the application of the composition. For example, a preferred Abbe number (νd) range for a thermoplastic resin composition for a certain application may be, for example, 20 to 32, 21 to 30, 22 to 28, or 23 to 26. The Abbe number (νd) of the first thermoplastic resin, measured by the method described below, may be, for example, 20 to 28, 21 to 27, 22 to 26, or 23 to 25. The Abbe number (νd) of the second thermoplastic resin, measured by the method described below, may be, for example, 22 to 32, 23 to 31, 24 to 30, or 25 to 29.

[0064] 4-6. Glass transition temperature (Tg) The glass transition temperature (Tg) value of the thermoplastic resin composition according to JIS K7121-1987 is preferably 100 to 200°C, more preferably 110 to 180°C, even more preferably 120 to 160°C, and particularly preferably 130 to 155°C. 4-7. Melt volume rate (MVR) The MVR value (unit: cm) of the thermoplastic resin composition according to JIS K7210 3 / 10 min) is preferably 15 or more, further preferably 20 or more, further preferably 25 or more, and particularly preferably 30 or more. A resin or resin composition with a large MVR value can be said to have high fluidity.

[0065] The weight average molecular weight of the thermoplastic resin contained in the thermoplastic resin composition is preferably 10,000 to 300,000, more preferably 10,000 to 200,000, and even more preferably 10,000 to 100,000, for example, more preferably 20,000 to 80,000, still more preferably 30,000 to 70,000, and particularly preferably 40,000 to 65,000. The weight average molecular weight of the thermoplastic resin is measured, for example, as a polystyrene-equivalent weight average molecular weight (Mw) as follows.

[0066] Using GPC (gel permeation chromatography), a calibration curve is prepared using chloroform as a developing solvent and standard polystyrene (Shodex STANDARD, SM-105) of known molecular weight (molecular weight distribution = 1). The elution time and molecular weight value of each peak from the measured standard polystyrene are plotted, and a calibration curve is prepared by approximating using a cubic equation. Then, based on the obtained calibration curve, the weight average molecular weight (Mw) can be calculated as a polystyrene equivalent value using the following formula. [Calculation formula] Mw = Σ(W i ×M i ) / Σ(W i ) (In the above formula, i is the i-th division point when dividing the molecular weight M, W i is the i-th weight, M irepresents the i-th molecular weight. The molecular weight M represents the molecular weight in polystyrene equivalent at the same elution time on the calibration curve.)

[0067] 5. Molded Articles Comprising Thermoplastic Resin Composition The thermoplastic resin composition of the present invention can be used for extrusion molding, blow molding, injection molding, etc. Molded articles (molded articles) obtained from the thermoplastic resin composition include extrusion molded articles, hollow molded articles, precision parts, thin injection molded articles, etc. Specific examples of molded articles using the thermoplastic resin of the present invention as optical materials include optical components such as optical lenses, optical films, liquid crystal displays, light guide plates, various films such as optical disk substrates, and housings for electronic devices such as smartphones.

[0068] The present invention will be specifically described below with reference to examples, but the present invention is not limited to these examples.

[0069] The methods for measuring the properties of the thermoplastic resins or thermoplastic resin compositions obtained in the examples and comparative examples are as follows. (1) Total light transmittance (TT), YI, and haze The obtained resins were molded into 3 mm thick pieces, and the total light transmittance (TT), YI, and haze were measured using a spectroscopic haze meter. The total light transmittance (TT) was measured in accordance with JIS K 7361-1:1997, the YI value was measured in accordance with JIS K 7373:2006, and the haze was measured in accordance with JIS K-7136:2000. Measuring instrument: "SH 7000" manufactured by Nippon Denshoku Industries Co., Ltd.

[0070] (2) Refractive index (nD) Based on JIS B 7071-2:2018, the obtained resin or resin composition was molded to obtain a V-block of a predetermined shape and used as a test piece. The refractive index was measured at 23 ° C using a refractometer (KPR-3000 manufactured by Shimadzu Corporation). (3) Abbe number (νd) Using the same test piece (V-block) as used in the refractive index measurement, the refractive index was measured at wavelengths of 486 nm, 589 nm, and 656 nm at 23 ° C using a refractometer, and the Abbe number was calculated using the following formula. Refractometer: KPR-3000 manufactured by Shimadzu Corporation ν = (nD-1) / (nF-nC) nD: refractive index at a wavelength of 589 nm nC: refractive index at a wavelength of 656 nm nF: refractive index at a wavelength of 486 nm Refractometer: KPR-3000 manufactured by Shimadzu Corporation

[0071] (4) Glass transition temperature (Tg) Measured using a differential scanning calorimeter with a temperature increase program of 10°C / min based on JIS K7121-1987. Differential scanning calorimeter: X-DSC7000 manufactured by Hitachi High-Tech Science Corporation. (5) Melt volume rate (MVR) The obtained resin or resin composition was dried in vacuum at 120°C for 4 hours and measured in accordance with JIS K7210. Measuring device: Melt Indexer T-111 manufactured by Toyo Seiki Seisaku-sho, Ltd. Measurement conditions: Measured at a temperature of 260°C and a load of 2160 g. Procedure: MVR (unit: cm) was calculated from the amount of resin extruded per 10 minutes from a standard die installed at the bottom of the cylinder. 3 The MVR is an index showing the fluidity of a resin, and a larger value indicates higher fluidity in the resin or resin composition.

[0072] Polymerization Example 1 As raw materials, 6.06 kg (26.56 mol) of 2,2-bis(4′-hydroxyphenyl)propane (bisphenol A: BPA), 8.81 kg (20.08 mol) of 9,9-bis[4-(2-hydroxyethoxy)phenyl]fluorene (BPEF), 10.28 kg (48.00 mol) of DPC, and 2.41×10 sodium bicarbonate were used. -2 g (2.86 x 10 -4(mol) was placed in a 50-liter reactor equipped with a stirrer and a distillation device. After nitrogen replacement in the reaction system, the reaction system was heated to 205°C over 20 minutes under a nitrogen atmosphere of 760 Torr. The raw materials were then melted while the pressure was reduced to 700 Torr over 10 minutes. The mixture was held in this state for 10 minutes, stirred, and then held for another 100 minutes, after which the pressure was reduced to 205 Torr over 20 minutes. The pressure in the reaction system was then adjusted to 180 Torr over 10 minutes and held under conditions of 215°C and 180 Torr for 20 minutes. The pressure in the reaction system was then adjusted to 150 Torr over another 10 minutes and held under conditions of 230°C and 150 Torr for 30 minutes, after which the pressure was reduced to 120 Torr and 235°C and the temperature was increased. The pressure in the reaction system was then reduced to 100 Torr over 10 minutes and held for 10 minutes. The pressure in the reaction system was reduced to 1 Torr or less over an additional 50 minutes, and the reaction mixture was maintained at 235°C and 1 Torr or less for 40 minutes. After the reaction was completed, nitrogen was blown into the reactor to increase pressure, and the resulting polycarbonate resin was pelletized and withdrawn. To 100 parts by weight of the withdrawn polycarbonate resin pellets, 0.1 parts by weight of glycerin monostearate (Rikemal S-100A, manufactured by Riken Vitamin Co., Ltd.) and 0.1 parts by weight of pentaerythritol tetrakis[3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate] (ADEKA Corporation; Adekastab AO-60) were compounded using a vented twin-screw extruder (TEM-26SX, manufactured by Shibaura Machine Co., Ltd.; co-rotating) to obtain a polycarbonate resin containing the additives.

[0073] Polymerization Example 2 Raw materials were 1.38 kg (6.10 mol) of 2,2-bis(4′-hydroxyphenyl)propane (bisphenol A: BPA), 17.77 kg (40.53 mol) of 9,9-bis[4-(2-hydroxyethoxy)phenyl]fluorene (BPEF), 10.28 kg (48.00 mol) of DPC, and 2.41×10 sodium bicarbonate. -2 g (2.86 x 10 -4Except for using 100 parts by weight of a glyceryl laurate copolymer (Poem M-300, manufactured by Riken Vitamin Co., Ltd.) and 0.1 parts by weight of pentaerythritol tetrakis[3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate] (ADEKA Corporation; Adekastab AO-60) as additives, 0.1 part by weight was compounded with 100 parts by weight of the polycarbonate resin pellets using a vented twin-screw extruder (TEM-26SX, manufactured by Shibaura Machine Co., Ltd.; co-rotating) to obtain a polycarbonate resin mixed with the additives.

[0074] Polymerization Example 3 As raw materials, 20.43 kg (46.59 mol) of 9,9-bis[4-(2-hydroxyethoxy)phenyl]fluorene (BPEF), 10.28 kg (48.00 mol) of DPC, and 2.41×10 sodium bicarbonate were used. -2 g (2.86 x 10 -4 A polycarbonate resin containing additives was obtained in the same manner as in Polymerization Example 1, except that the copolymer (100%) (mol) was used.

[0075] (Comparative Examples 1 to 3 (Recovery of Waste Resins 1 to 3)) Optical lenses were molded using the polycarbonate resins obtained in Polymerization Examples 1 to 3, respectively, and the sprues and runners of the resulting molded bodies (recycled products 1 to 3) were recovered. The thermoplastic resins of the respective recovered products were designated as Comparative Examples 1 to 3.

[0076] Example 1 31.19% by mass of the above-mentioned recycled product 1, 68.81% by mass of the above-mentioned recycled product 2, 0.1 parts by weight of glycerin monostearate (manufactured by Riken Vitamin Co., Ltd.; Rikemal S-100A) and 0.1 parts by weight of pentaerythritol tetrakis [3- (3,5-di-tert-butyl-4-hydroxyphenyl) propionate] (manufactured by ADEKA Corporation; Adekastab AO-60) were melt-mixed in an extruder to obtain a resin composition. The extruder used for melt mixing was a vented twin-screw extruder (TEM-26SX manufactured by Shibaura Machine Co., Ltd.; rotation in the same direction), and the extrusion conditions were a discharge rate of 15 kg / h, a screw rotation speed of 300 rpm, a vent vacuum of 3 kPa, and extrusion temperatures from the first feed port to the die portion were 200, 220, 240, 260, 260, 260, 260, 255, and 255° C. The physical properties of the obtained composition are shown in Table 1 below.

[0077] Examples 2 to 5 Resin compositions were obtained in the same manner as in Example 1, except that the components were melt-mixed in the proportions shown in Table 1. The physical properties of the resulting compositions are shown in Table 1 below.

[0078] The molecular structures and abbreviations of the monomer compounds used in the above polymerization examples are as follows:

[0079] Polymerization Example 4 9,9-bis[4-(2-hydroxyethoxy)phenyl]fluorene (BPEF) 9.30 kg (21.20 mol), SPG 3.05 kg (10.00), 1,1-bis(4-hydroxyphenyl)-3,3,5-trimethylcyclohexane (Bis-TMC) 4.77 kg (15.37 mol), DPC 10.28 kg (48.00 mol), and sodium bicarbonate 2.41 × 10 -2 g (2.86 x 10 -4(mol) was placed in a 50-liter reactor equipped with a stirrer and a distillation device. After nitrogen replacement in the reaction system, the reaction system was heated to 205°C over 20 minutes under a nitrogen atmosphere of 760 Torr. The raw materials were then melted while the pressure was reduced to 700 Torr over 10 minutes. The mixture was held in this state for 10 minutes, stirred, and then held for another 100 minutes, after which the pressure was reduced to 205 Torr over 20 minutes. The pressure in the reaction system was then adjusted to 180 Torr over 10 minutes and held under conditions of 215°C and 180 Torr for 20 minutes. The pressure in the reaction system was then adjusted to 150 Torr over another 10 minutes and held under conditions of 230°C and 150 Torr for 30 minutes, after which the pressure was reduced to 120 Torr and 235°C and the temperature was increased. The pressure in the reaction system was then reduced to 100 Torr over 10 minutes and held for 10 minutes. The pressure in the reaction system was further reduced to 1 Torr or less over 50 minutes, and the reaction system was maintained at 235° C. and 1 Torr or less for 40 minutes. After the reaction was completed, nitrogen was blown into the reactor to pressurize it, and the produced polycarbonate resin was removed while being pelletized. 100 parts by weight of the extracted polycarbonate resin pellets were compounded with 0.2 parts by weight of glycerin monostearate (Rikemal S-100A, manufactured by Riken Vitamin Co., Ltd.), 0.1 part by weight of pentaerythritol tetrakis[3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate] (ADK STAB AO-60, manufactured by ADEKA Corporation), and 0.03 part by weight of 3,9-bis(2,6-di-tert-butyl-4-methylphenoxy)-2,4,8,10-tetraoxa-3,9-diphosphaspiro[5.5]undecane (ADK STAB PEP-36, manufactured by ADEKA Corporation) as additives using a vented twin-screw extruder (TEM-26SX, manufactured by Shibaura Machine Co., Ltd., rotating in the same direction) to obtain a polycarbonate resin mixed with the additives.

[0080] Comparative Example 4 (Recovery of Waste Resin 4) An optical lens was molded using the polycarbonate resin obtained in Polymerization Example 4, and the sprue and runner of the obtained molded body (recycled product 4) were recovered. The recovered thermoplastic resin was used as Comparative Example 4.

[0081] Example 6 50.0% by mass of the polycarbonate resin of Polymerization Example 4 described above, 50.0% by mass of the recycled product 4 described above, 0.1 parts by weight of glycerin monostearate (manufactured by Riken Vitamin Co., Ltd.; Rikemal S-100A) and 0.1 parts by weight of pentaerythritol tetrakis [3- (3,5-di-tert-butyl-4-hydroxyphenyl) propionate] (manufactured by ADEKA Corporation; Adekastab AO-60) were melt-mixed in an extruder to obtain a resin composition. The extruder used for melt mixing was a vented twin-screw extruder (TEM-26SX manufactured by Shibaura Machine Co., Ltd.; rotation in the same direction), and the extrusion conditions were a discharge rate of 15 kg / h, a screw rotation speed of 300 rpm, a vent vacuum of 3 kPa, and extrusion temperatures from the first feed port to the die portion were 200, 220, 240, 260, 260, 260, 260, 260, 255, and 255° C. The physical properties of the obtained composition are shown in Table 2 below.

[0082]

[0083] The molecular structures and abbreviations of the monomer compounds used in the above polymerization examples are as follows:

[0084] As is clear from the results of the above examples and comparative examples, it was confirmed that a thermoplastic resin composition with desired properties could be produced by mixing two or more of the thermoplastic resins of Comparative Examples 1 and 2, which are copolymers, and Comparative Example 3, which is a homopolymer. For example, it was found that the thermoplastic resin compositions of Examples 1 to 5, in which the refractive index was adjusted to a narrow range of 1.628 to 1.629, which is different from the refractive index values ​​of either the copolymer or the homopolymer, could be realized by varying the blending ratio between the copolymer and the homopolymer. Furthermore, although the difference was not as great as that of the refractive index, other properties, such as YI, haze, and MVR, could also be adjusted depending on the blending ratio of the copolymer and the homopolymer of the comparative examples. In particular, it was confirmed that the thermoplastic resin composition of Example 6, which is a mixture of new and recycled resins of the same type, could also utilize recycled materials by adjusting the blending ratio of the YI, haze, and MVR values.

[0085] As illustrated in the above examples, the method for producing a thermoplastic resin composition of the present invention involves mixing multiple different types of thermoplastic resins, and therefore allows for easy and effective recycling of, for example, leftover thermoplastic resin generated when injected into gaps in a mold's sprue, runner, gate, etc. Therefore, the thermoplastic resin composition of the present invention can be produced by a simple method that includes recycling, and can reliably achieve the desired properties, particularly for optical applications.

Claims

1. A method for producing a thermoplastic resin composition, comprising at least a mixing step of mixing a first thermoplastic resin containing a structural unit (A) derived from a monomer represented by any one of the following general formulas (1a) to (1c), and a second thermoplastic resin containing a structural unit (B) derived from a monomer represented by the following general formula (2), wherein the first thermoplastic resin has a refractive index of 1.650 or less, the second thermoplastic resin has a refractive index of 1.570 or more, and the thermoplastic resin composition has a refractive index of 1.550 to 1.

700. (In general formulas (1a) to (1c), R c and R d are each independently selected from the group consisting of a hydrogen atom, a halogen atom, an alkyl group having 1 to 20 carbon atoms which may have a substituent, an alkoxyl group having 1 to 20 carbon atoms which may have a substituent, a cycloalkyl group having 5 to 20 carbon atoms which may have a substituent, a cycloalkoxyl group having 5 to 20 carbon atoms which may have a substituent, and an aryl group having 6 to 20 carbon atoms which may have a substituent, each Y is independently a single bond, a fluorene group which may have a substituent, or any of the structural formulas represented by the following formulas (i) to (vii): (In formulas (i) to (vii), R 61 , R 62 , R 71 and R 72 each independently represents a hydrogen atom, a halogen atom, an alkyl group having 1 to 20 carbon atoms which may have a substituent, or an aryl group having 6 to 30 carbon atoms which may have a substituent, or 61 and R 62 , or R 71 and R 72 are bonded to each other to form a carbon ring or hetero ring having 4 to 20 carbon atoms, which may have a substituent; r and s each independently represent an integer from 0 to 5,000; A and B each independently represent an alkylene group having 1 to 5 carbon atoms, which may have a substituent; p and q each independently represent an integer from 0 to 4; a and b each independently represent an integer from 0 to 10. (In formula (2), R 1 ~R4 each independently represents a hydrogen atom, an alkyl group which may have a substituent, or an aryl group which may have a substituent; Z represents a single bond or a group represented by the following general formula (3): (In formula (3), R 5 and R 6 are each a hydrogen atom, an optionally substituted alkyl group, or an optionally substituted aryl group, or 5 and R 6 are bonded to each other to form a carbon ring or hetero ring having 4 to 20 carbon atoms which may have a substituent, and c represents an integer of 1 to 3.

2. The method for producing a thermoplastic resin composition according to claim 1, wherein at least one of the first thermoplastic resin and the second thermoplastic resin comprises a recycled thermoplastic resin.

3. The method for producing a thermoplastic resin composition according to claim 1, wherein the refractive index of the thermoplastic resin composition is 1.570 to 1.

650.

4. A method for producing a thermoplastic resin composition according to claim 1, wherein the content of the structural unit (A) is 20 to 95 mol % and the content of the structural unit (B) is 5 to 80 mol % based on the total number of structural units of the first thermoplastic resin and the second thermoplastic resin.

5. A method for producing a thermoplastic resin composition according to claim 1, wherein at least one of the first thermoplastic resin and the second thermoplastic resin is a copolymer having both the structural unit (A) and the structural unit (B).

6. The method for producing a thermoplastic resin composition according to claim 1, wherein the first thermoplastic resin has only the structural unit (A).

7. The method for producing a thermoplastic resin composition according to claim 1, wherein an additive is mixed with the first thermoplastic resin and the second thermoplastic resin in the mixing step.

8. A thermoplastic resin composition comprising a mixture of a first thermoplastic resin containing a structural unit (A) derived from a monomer represented by any one of the following general formulas (1a) to (1c), and a second thermoplastic resin containing a structural unit (B) derived from a monomer represented by the following general formula (2), wherein the first thermoplastic resin has a refractive index of 1.650 or less, the second thermoplastic resin has a refractive index of 1.570 or more, and the thermoplastic resin composition has a refractive index of 1.550 to 1.

700. (In general formulas (1a) to (1c), R c and R d are each independently selected from the group consisting of a hydrogen atom, a halogen atom, an alkyl group having 1 to 20 carbon atoms which may have a substituent, an alkoxyl group having 1 to 20 carbon atoms which may have a substituent, a cycloalkyl group having 5 to 20 carbon atoms which may have a substituent, a cycloalkoxyl group having 5 to 20 carbon atoms which may have a substituent, and an aryl group having 6 to 20 carbon atoms which may have a substituent, each Y is independently a single bond, a fluorene group which may have a substituent, or any of the structural formulas represented by the following formulas (i) to (vii): (In formulas (i) to (vii), R 61 , R 62 , R 71 and R 72 each independently represents a hydrogen atom, a halogen atom, an alkyl group having 1 to 20 carbon atoms which may have a substituent, or an aryl group having 6 to 30 carbon atoms which may have a substituent, or 61 and R 62 , or R 71 and R 72 are bonded to each other to form a carbon ring or hetero ring having 4 to 20 carbon atoms, which may have a substituent; r and s each independently represent an integer from 0 to 5,000; A and B each independently represent an alkylene group having 1 to 5 carbon atoms, which may have a substituent; p and q each independently represent an integer from 0 to 4; a and b each independently represent an integer from 0 to 10. (In formula (2), R 1 ~R 4each independently represents a hydrogen atom, an alkyl group which may have a substituent, or an aryl group which may have a substituent; Z represents a single bond or a group represented by the following general formula (3): (In formula (3), R 5 and R 6 are each a hydrogen atom, an optionally substituted alkyl group, or an optionally substituted aryl group, or 5 and R 6 are bonded to each other to form a carbon ring or hetero ring having 4 to 20 carbon atoms which may have a substituent, and c represents an integer of 1 to 3.

9. The thermoplastic resin composition according to claim 8, further comprising a mold release agent and / or an antioxidant in the thermoplastic resin.

10. An optical lens comprising the thermoplastic resin composition according to claim 8 or 9.

Citation Information

Patent Citations

  • Polycarbonate resin, production method therefor, and optical molded body

    WO2014073496A1

  • Polycarbonate resin composition, and optical material and optical lens each manufactured using same

    WO2015166951A1

  • Polycarbonate resin and optical member

    JP2001342247A

  • Polycarbonate resin composition containing recycled material and molded article

    JP2016079333A

  • Thermoplastic resin composition

    JP2021001310A