Method for producing composite particles
The method of emulsifying and curing silicone rubber on core particles with a cationic surfactant addresses the challenges of shape and size maintenance, achieving uniform coating and preventing agglomeration, enhancing the properties of composite particles for cosmetic applications.
Patent Information
- Application Number
- PCT/JP2024/017930
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-05-17
- Filing Date
- 2024-05-15
- Publication Date
- 2024-11-21
AI Technical Summary
Existing methods for producing composite particles with silicone rubber-coated core particles face challenges in maintaining the shape and size of core particles, as well as achieving uniform coating, due to issues like agglomeration and incomplete adhesion of silicone rubber.
A method involving the emulsification of a curable liquid silicone composition to form an oil-in-water emulsion, followed by curing and adsorption of silicone rubber spherical particles onto core particles using a cationic surfactant, with subsequent removal of moisture to fix the silicone rubber on the surface, ensuring uniform coating and preventing agglomeration.
The method effectively maintains the shape and size of core particles, achieves uniform silicone rubber adhesion, and prevents agglomeration, resulting in composite particles with improved light diffusivity, skin adhesion, and drop stability when used in cosmetics.
Smart Images

Figure JP2024017930_21112024_PF_FP_ABST
Abstract
Description
Method for producing composite particles
[0001] The present invention relates to a method for producing composite particles.
[0002] Various powder treatments have been used to achieve the desired functionality of makeup cosmetics such as foundations and primers. Silicone rubber-coated powders have been proposed, which are said to have light diffusing properties that improve the natural finish, excellent adhesion to the skin, and a soft, moist feel. Furthermore, in powder cosmetics, they are said to have excellent drop stability.
[0003] Several methods have been proposed for producing particles in which silicone rubber is attached to and coated on the surface of core particles.
[0004] Patent Document 1 proposes a method of pulverizing and mixing silica and silicone rubber, but because the silica particles that serve as core particles are pulverized, it is not possible to obtain particles that maintain their original shape and particle size. In other words, it is not possible to obtain particles with a specific shape such as a sphere, plate, or rod, and it is also difficult to control the particle size.
[0005] Patent Documents 2 and 3 propose a method of mixing core particles with a curable silicone that becomes silicone rubber and then curing the silicone, but all or some of the particles have a structure in which multiple core particles exist within the particle, which increases the particle size, making it difficult to maintain the shape of the core particles and control the particle size. Also, if the proportion of silicone is low, it is difficult to coat all of the core particles.
[0006] Patent Document 4 proposes a method in which an aqueous dispersion of silica particles and a curable silicone that will become silicone rubber are emulsified and dispersed in water, and then the silicone is cured. However, the particles obtained in powder form have a structure containing multiple silica particles that will become core particles, and the high content of silicone rubber makes it difficult for the properties of the core particles to be expressed.
[0007] Patent Document 5 proposes a method in which a mixture of inorganic particles and an emulsion of curable silicone that becomes silicone rubber is spray-dried while simultaneously curing the silicone, but this method can result in particles containing multiple inorganic particles that become core particles, or particles consisting only of uncoated silicone rubber.
[0008] Patent Document 6 proposes a method in which core particles and silicone rubber particles dispersed in a dispersion medium are mixed together, and then the dispersion medium is evaporated. However, since the particles aggregate when the dispersion medium is evaporated, it becomes difficult to maintain the shape of the core particles and control the particle size.
[0009] Patent Document 7 proposes a method in which a crosslinking agent is added to a mixture of core particles and an emulsion of slightly crosslinked silicone, followed by centrifugation to form a cake-like substance, which is then dried and cured into rubber at the same time; however, the core particles solidify together during curing and it is difficult to completely loosen them, making it difficult to maintain the shape of the core particles and control the particle size.
[0010] JP 8-3451, JP 3-294357, JP 2017-214565, JP 3-281536, JP 5-32914, JP 2010-163375, International Publication WO 2018 / 084176
[0011] In view of the above circumstances, the present invention aims to provide a method for producing composite particles in which silicone rubber is adhered to the surface of a core particle, in which the composite particles do not contain multiple core particles, the particles do not strongly aggregate or adhere to each other, the shape and particle size of the core particles are largely maintained, and almost all of the compounded silicone rubber is adhered to the surface of almost all of the core particles.
[0012] In order to solve the above problems, the present invention provides a method for producing composite particles comprising core particles having a volume average particle size of 1 to 50 μm and having silicone rubber adhered to the surface thereof, the method comprising the steps of: (i) emulsifying a curable liquid silicone composition using a surfactant to produce an oil-in-water emulsion, and then curing the curable liquid silicone composition to produce an aqueous dispersion of silicone rubber spherical particles having a volume average particle size of 50 to 1,000 nm; (ii) mixing the core particles, the aqueous dispersion of silicone rubber spherical particles produced in step (i), a cationic surfactant, and water to adsorb the silicone rubber particles to the surfaces of the core particles, thereby producing a mixture containing the core particles having the silicone rubber particles adsorbed thereon; and (iii) volatilizing and removing water contained in the mixture containing the core particles having the silicone rubber particles adsorbed thereon produced in step (ii), thereby fixing the silicone rubber particles adsorbed to the surfaces of the core particles. the amount of the core particles is in the range of 1 to 100 parts by mass relative to 100 parts by mass of water contained in the mixed liquid prepared in step (ii), the amount of the silicone rubber spherical particles is in the range of 0.1 to 25 parts by mass relative to 100 parts by mass of the core particles, and the amount of the cationic surfactant is in the range of 0.02 to 0.9 parts by mass relative to 100 parts by mass of water.
[0013] With this method for producing composite particles, the composite particles do not contain multiple core particles, the particles do not strongly aggregate or adhere to each other, the shape and particle size of the core particles are largely maintained, and composite particles can be produced in which almost all of the compounded silicone rubber adheres to the surface of almost all of the core particles.
[0014] The core particles may be made of at least one of inorganic particles and organic particles.
[0015] As described above, in the method for producing composite particles of the present invention, either inorganic particles or organic particles can be used as core particles, or inorganic-organic composite particles can also be used, and one type can be used alone or two or more types can be used in appropriate combination.
[0016] The silicone rubber spherical particles preferably have a rubber hardness in the range of 5 to 95 as measured by a Type A durometer as specified in JIS K6253.
[0017] If the rubber hardness is 5 or more, the adhesive will have low and good cohesion, and when used in cosmetics, the cosmetic will not suffer from reduced slipperiness or spreadability or from creasing. Also, if the rubber hardness is 95 or less, the adhesive will be able to impart good adhesion to the skin, a soft and moist feel, and drop stability to the cosmetic when used in cosmetics.
[0018] According to the present invention, composite particles can be produced in which the core particles do not contain multiple core particles, the particles do not strongly aggregate or adhere to each other, the shape and particle size of the core particles are largely maintained, and substantially all of the incorporated silicone rubber adheres to the surface of substantially all of the core particles. Furthermore, when incorporated into cosmetics, the composite particles produced by the production method of the present invention can improve the natural finish feeling due to their light diffusibility, provide excellent adhesion to the skin, and provide a soft and moist feel, and in the case of powder cosmetics, can provide excellent drop stability.
[0019] 1 is an electron microscope photograph of composite particles obtained in Example 6. 2 is an electron microscope photograph of composite particles obtained in Example 7. 3 is an electron microscope photograph of composite particles obtained in Example 8. 4 is an electron microscope photograph of composite particles obtained in Example 9. 5 is an electron microscope photograph of composite particles obtained in Example 10. 6 is an electron microscope photograph of composite particles obtained in Example 11. 7 is an electron microscope photograph of composite particles obtained in Example 12. 8 is an electron microscope photograph of cellulose particles used in the Examples and Comparative Examples. 9 is an electron microscope photograph of composite particles obtained in Example 13. 10 is an electron microscope photograph of composite particles obtained in Example 18. 11 is an electron microscope photograph of silica particles used in the Examples and Comparative Examples.
[0020] As a result of extensive research into the above-mentioned problems, the inventors discovered that the above-mentioned object could be achieved by adsorbing silicone rubber particles onto the surface of core particles in an aqueous solution of a cationic surfactant, and then removing the water, and thus completed the present invention.
[0021] The present invention will be described in detail below. [Composite Particles] The composite particles produced by the composite particle production method of the present invention are composite particles in which silicone rubber is attached to the surface of a core particle.
[0022] Most composite particles have a structure in which the number of core particles in the composite particle is one. The existence of this structure can be confirmed by comparative observation of the raw material core particle and the manufactured composite particle under an electron microscope. If the shape and size of the composite particle are roughly the same as those of the core particle, it is determined to have the above structure.
[0023] When particles are observed overlapping under an electron microscope, it is difficult to determine whether they are separate particles or have bonded together to form a single particle. In other words, it is difficult to determine whether the number of core particles in a composite particle is a single structure, or whether multiple structural particles are bonded together to form multiple core particles within the particle. In this case, this can be confirmed by measuring the particle size. If the shape of a particle size distribution diagram with particle size on the horizontal axis and frequency on the vertical axis is approximately the same as that of the core particle, it is determined that the number of core particles in the composite particle is a single structure.
[0024] The core particles may be inorganic particles, organic particles, or inorganic-organic composite particles, and may be used alone or in appropriate combination of two or more types. Particles that are substantially usable in cosmetics and particles of any particle size range are applicable. Furthermore, as long as their geometric form is one that is commonly used in cosmetics, they may be any shape, such as spherical, polyhedral, spindle-shaped, needle-shaped, or plate-shaped, and may be either non-porous or porous.
[0025] The volume average particle diameter of the core particles is in the range of 1 to 50 μm, preferably 2 to 30 μm. If the particle diameter is 1 μm or more, effects such as a dry feel and smoothness in use and the effect of imparting extensibility can be obtained, while if it is 50 μm or less, a rough feel does not occur. The volume average particle diameter is measured by the Coulter counter method (electrical resistance method).
[0026] Examples of inorganic particles include titanium oxide, titanium mica, zirconium oxide, zinc oxide, cerium oxide, magnesium oxide, barium sulfate, calcium sulfate, magnesium sulfate, calcium carbonate, magnesium carbonate, talc, cleaved talc, mica, kaolin, sericite, muscovite, synthetic mica, phlogopite, lepidolite, biotite, lepidolite, lithia mica, silicic acid, silica (silicon dioxide), hydrous silicon dioxide, aluminum silicate, magnesium silicate, aluminum magnesium silicate, calcium silicate, barium silicate, strontium silicate, metal tungstate, hydroxyapatite, vermiculite, higilite, bentonite, montmorillonite, hectorite, zeolite, ceramics, secondary calcium phosphate, alumina, aluminum hydroxide, boron nitride, boron nitride, and glass particles.
[0027] inorganic black pigments such as black iron oxide and carbon black; inorganic purple pigments such as manganese violet and cobalt violet; inorganic green pigments such as chromium hydroxide, chromium oxide, cobalt oxide and cobalt titanate; inorganic blue pigments such as iron blue and ultramarine; colored pigments such as lakes of tar-based pigments and lakes of natural pigments; pearl pigments such as titanium oxide-coated mica, titanium oxide-coated mica, bismuth oxychloride, titanium oxide-coated bismuth oxychloride, titanium oxide-coated talc, fish scale foil, and titanium oxide-coated colored mica; and metal powder pigments such as aluminum powder, copper powder, and stainless steel powder.
[0028] Examples of organic resin particles include particles of polyethylene; polypropylene; polystyrene; divinylbenzene resin; polyvinyl chloride; methacrylic resin; polytetrafluoroethylene; methacrylic-styrene copolymer; polyamide; polycarbonate; polyesters such as polyethylene terephthalate, polybutylene succinate, polyhydroxybutyric acid, and polycaprolactone; cellulose; cellulose derivatives; phenolic resin; melamine resin; benzoguanamine resin; epoxy resin; and polyurethane.
[0029] Further examples include organic dyes, and specific examples thereof include tar dyes such as Red No. 3, Red No. 104, Red No. 106, Red No. 201, Red No. 202, Red No. 204, Red No. 205, Red No. 220, Red No. 226, Red No. 227, Red No. 228, Red No. 230, Red No. 401, Red No. 505, Yellow No. 4, Yellow No. 5, Yellow No. 202, Yellow No. 203, Yellow No. 204, Yellow No. 401, Blue No. 1, Blue No. 2, Blue No. 201, Blue No. 404, Green No. 3, Green No. 201, Green No. 204, Green No. 205, Orange No. 201, Orange No. 203, Orange No. 204, Orange No. 206, and Orange No. 207; and natural dyes such as carminic acid, laccaic acid, carthamine, brazilian, and crocin.
[0030] The inorganic-organic composite particles may be composite particles in which the surfaces of inorganic particles commonly used in cosmetics are coated with organic particles by a known method.
[0031] The particles may be surface-treated with metal soap, silane, silicone, silicone resin, fluorine compound, amino acid, iron oxide, titanium oxide, iron oxide, titanium oxide, or aluminum hydroxide.
[0032] There are no particular restrictions on the shape of the silicone rubber attached to the surface of the core particles, but as will be described later, in the manufacturing method of the present invention, the silicone rubber will be spherical, have a shape like fused spherical particles, have a nodular shape, or be in the form of a film.
[0033] The density of the rubber attached to the surface of the core particle is not particularly limited. That is, the rubber may be sparsely attached to the surface of the core particle, or may be attached to cover the surface of the core particle without any gaps. The shape and density of the attached rubber can be confirmed using an electron microscope.
[0034] The amount of silicone rubber attached to the core particles is in the range of 0.1 to 25 parts by mass, preferably 0.2 to 20 parts by mass, and more preferably 0.5 to 15 parts by mass or more, per 100 parts by mass of the core particles. An attachment amount of 0.1 part by mass or more can impart a natural finish due to light diffusion, good adhesion to the skin, a soft and moist feel, and drop stability to the cosmetic. An attachment amount of 25 parts by mass or less results in low cohesion, and prevents the cosmetic from losing its slipperiness and spreadability or from becoming sloppy.
[0035] The rubber constituting the silicone rubber is preferably non-sticky, and its rubber hardness, measured using a Type A durometer as specified in JIS K6253, is preferably in the range of 5 to 95, more preferably 10 to 80. A rubber hardness of 5 or higher results in low cohesion, preventing the cosmetic from losing its slipperiness and spreadability or from becoming distorted. A rubber hardness of 95 or lower can impart good adhesion to the skin, a soft and moist feel, and drop stability to the cosmetic. The rubber hardness refers to the value measured using a test piece prepared using the rubber composition and having the shape and dimensions specified in JIS K6253.
[0036] Silicone rubber is a compound represented by the formula -(R 2 SiO 2/2 ) a Preferably, the cured product has linear organosiloxane blocks represented by the formula: R is a substituted or unsubstituted monovalent hydrocarbon group having 1 to 30 carbon atoms, and a is a positive integer of 5 to 5,000.
[0037] The above R has 1 to 30 carbon atoms, preferably 1 to 22, and more preferably 1 to 18. Examples of R include alkyl groups such as methyl, ethyl, propyl, butyl, pentyl, hexyl, heptyl, octyl, decyl, undecyl, dodecyl, tetradecyl, pentadecyl, hexadecyl, heptadecyl, octadecyl, nonadecyl, icosyl, henicosyl, docosyl, tricosyl, tetracosyl, and triacontyl; aryl groups such as phenyl, tolyl, and naphthyl; benzyl, phenyl ... Examples of such groups include aralkyl groups such as phenethyl groups; alkenyl groups such as vinyl groups and allyl groups; cycloalkyl groups such as cyclopentyl groups, cyclohexyl groups and cycloheptyl groups; and hydrocarbon groups in which some or all of the hydrogen atoms bonded to carbon atoms of these groups have been substituted with atoms such as halogen atoms (fluorine atoms, chlorine atoms, bromine atoms and iodine atoms) and / or substituents such as acryloyloxy groups, methacryloyloxy groups, epoxy groups, glycidoxy groups and carboxyl groups. Preferred are alkyl groups having 1 to 18 carbon atoms or phenyl groups, and it is preferred that 50 mol % or more of all R groups are methyl groups.
[0038] Silicone rubber is obtained from a curable liquid silicone composition, and its curing can be exemplified by addition reactions, condensation reactions, radical reactions, etc. The curable liquid silicone composition contains a component having a reactive group for the above curing reaction (a component having both reactive groups, or a component having one reactive group and a component having the other reactive group), a curing catalyst, and a radical generator.
[0039] When silicone rubber is produced by curing through an addition reaction, the curable liquid silicone composition may contain (A) an organopolysiloxane having alkenyl groups, (B) an organohydrogenpolysiloxane having silicon-bonded hydrogen atoms, and an addition reaction catalyst.
[0040] The component (A) is represented by the following average composition formula (1): 1 b R 2 c SiO (4-b-c)/2(1) is an organopolysiloxane having at least two alkenyl groups in one molecule. 1 are each independently an unsubstituted or substituted monovalent hydrocarbon group having 1 to 30 carbon atoms and not containing an alkenyl group. 2 are each independently an alkenyl group having 2 to 6 carbon atoms, and b and c are positive numbers satisfying the conditions 0<b<3, 0<c≦3, and 0.1≦b+c≦3.
[0041] The organopolysiloxanes represented by the average composition formula (1) may be used alone or in combination of two or more.
[0042] R 1 R has 1 to 30 carbon atoms, preferably 1 to 22, and more preferably 1 to 18. 1 is a monovalent hydrocarbon group excluding an alkenyl group among those exemplified above for R, and R 1 Preferably, 50 mol % or more of R are methyl groups. 2 b and c are positive numbers that preferably satisfy the following conditions: 0<b≦2.295, 0.005≦c≦2.3, and 0.5≦b+c≦2.3.
[0043] The kinematic viscosity of component (A) at 25°C is 100,000 mm 2 / s or less, and more preferably 10,000 mm 2 The kinematic viscosity is preferably 100,000 mm / s or less. 2 When the kinematic viscosity is 0.7 mm / s or less, it is particularly easy to obtain silicone microparticles with a narrow particle size distribution in the preparation of an aqueous dispersion of silicone rubber particles, which will be described later. 2 / s or more, especially 2 mm 2 In the present invention, the kinematic viscosity may be a value measured at 25°C using a capillary viscometer.
[0044] The structure of component (A) may be linear, cyclic, or branched, with linear or branched structures with few branching units being particularly preferred. There are no particular restrictions on the bonding position of the alkenyl group, and the alkenyl group may be bonded to either a side chain or terminal silicon atom of the molecule, with bonding to both terminal silicon atoms of the linear organopolysiloxane being particularly preferred.
[0045] An example of a linear structure is one represented by the following general formula (2).
[0046] (In the formula, R 1 , R 2 is the same as above, d is a positive number, e is 0 or a positive number, and f is 0, 1, 2, or 3, provided that e and f are numbers that satisfy e+2×f≧2.
[0047] Examples of branched structures include R 1 SiO 3/2 The following general formula (3) is exemplified:
[0048] (In the formula, R 1 , R 2 is the same as above, g is a positive number, h is 0 or a positive number, i is a positive number, and j is 0, 1, 2, or 3, provided that h and j are numbers that satisfy h+j≧1.
[0049] SiO 4/2 Examples of the structure branched by the unit include those represented by the following general formula (4).
[0050] (In the formula, R 1 , R 2 is the same as above, k is a positive number, l is 0 or a positive number, m is a positive number, and n is 0, 1, 2, or 3, provided that l and n are numbers that satisfy l+n≧1.
[0051] Further, examples include those represented by the following unit formula (5) and having two or more alkenyl groups per molecule.
[0052] [R 1 3 SiO 1/2 ] o [R 2(R 1 ) 2 SiO 1/2 ] p [SiO 4/2 ] q [(OR 3 ) SiO 3/2 ] r (5) (wherein, R 1 , R 2 is the same as above, and R 3 is a hydrogen atom or an unsubstituted monovalent hydrocarbon group having 1 to 6 carbon atoms, o is 0 or a positive number, p is a positive number, q is a positive number, and r is 0 or a positive number.
[0053] The component (B) is represented by the following average composition formula (6): 4 s H t SiO (4-s-t)/2 (6) is an organohydrogenpolysiloxane having at least two hydrogen atoms bonded to silicon atoms (referred to as SiH groups) in one molecule. 4 are each independently an unsubstituted or substituted monovalent hydrocarbon group having 1 to 30 carbon atoms that does not contain an alkenyl group, and s and t are numbers that satisfy the conditions 0<s<3, 0<t≦3, and 0.1≦s+t≦3.
[0054] The organopolysiloxanes represented by the average composition formula (6) may be used alone or in combination of two or more.
[0055] R 4 R has 1 to 30 carbon atoms, preferably 1 to 22, and more preferably 1 to 18. 4 is R 1 Preferably, 80 mol % or more of the monovalent hydrocarbon groups are methyl groups, and more preferably 95 mol % or more of the monovalent hydrocarbon groups are methyl groups. Preferably, s and t are positive numbers satisfying the conditions 0<s≦2.295, 0.005≦t≦2.3, and 0.5≦s+t≦2.3.
[0056] The kinematic viscosity of component (B) at 25°C is 100,000 mm 2 / s or less, and more preferably 10,000 mm 2 / s or less. 2 When the kinematic viscosity is 0.4 mm / s or less, it is particularly easy to obtain silicone microparticles with a narrow particle size distribution in the preparation of an aqueous dispersion of silicone rubber particles, which will be described later. 2 / s or more, especially 2 mm 2 / s or more is sufficient.
[0057] The structure of component (B) may be linear, cyclic, or branched, with linear or branched being particularly preferred. There are no particular restrictions on the bonding position of the hydrogen atoms bonded to silicon atoms, and they may be bonded to silicon atoms in either the side chains or terminals of the molecule.
[0058] An example of a linear structure is one represented by the following general formula (7).
[0059] (In the formula, R 4 is the same as above, u is a positive number, v is 0 or a positive number, and w is 0, 1, 2, or 3, provided that v and w are numbers that satisfy v+2×w≧2.
[0060] Examples of branched structures include R 4 SiO 3/2 The following general formula (8) branched by the unit:
[0061] (In the formula, R 4 is the same as above, x is a positive number, y is 0 or a positive number, z is a positive number, and a1 is 0, 1, 2, or 3, provided that y and a1 are numbers that satisfy y+a1≧1.
[0062] SiO 4/2 An example of a structure branched by units of the formula (9) is one represented by the following general formula (9).
[0063] (In the formula, R 4 are the same as above, b1 is a positive number, c1 is 0 or a positive number, d1 is a positive number, and e1 is 0, 1, 2, or 3, provided that c1 and e1 are numbers that satisfy c1 + e1 ≧ 1.
[0064] Further, examples include those represented by the following unit formula (10) having two or more hydrogen atoms bonded to silicon atoms per molecule: [R 4 3 SiO 1/2 ] f1 [H(R 4 ) 2 SiO 1/3 ] g1 [SiO 4/2 ] h1 [(OR 5 ) SiO 3/2 ] i1 (10) In the formula, R 4 is the same as above, and R 5 is a hydrogen atom or an unsubstituted monovalent hydrocarbon group having 1 to 6 carbon atoms, f1 is 0 or a positive number, g1 is a positive number, h1 is a positive number, and i1 is 0 or a positive number.
[0065] As described above, component (A) is an organopolysiloxane having two or more alkenyl groups per molecule, and component (B) is an organohydrogenpolysiloxane having two or more silicon-bonded hydrogen atoms per molecule. However, the combination of an organopolysiloxane (A) having only two alkenyl groups with an organohydrogenpolysiloxane (B) having only two SiH groups is excluded. This is because the combination of an organopolysiloxane having two alkenyl groups as component (A) with an organohydrogensiloxane having two SiH groups as component (B) results in a sticky cured product, making it impossible to obtain a silicone rubber. That is, when component (A) has two alkenyl groups, at least one component (B) is an organohydrogensiloxane having three or more SiH groups; and when component (B) has two SiH groups, at least one component (A) is an organosiloxane having three or more alkenyl groups.
[0066] The amount of component (B) relative to component (A) is preferably an amount such that the ratio of the number of SiH groups in component (B) to the number of monovalent alkenyl groups in component (A) is 0.5 to 2, and more preferably 0.7 to 1.5. When component (B) is blended in an amount such that the ratio of the number of SiH groups falls within the above range, the resulting cured silicone rubber is not sticky and has appropriate reactivity.
[0067] Examples of the catalyst for the addition reaction include platinum group metal catalysts used in hydrosilylation reactions. Examples include platinum group metals such as platinum (including platinum black), rhodium, and palladium; 2 PtCl 4 ・XH 2 O, H 2 PtCl 6 ・XH 2 O, NaHPtCl 6 ・XH 2 O, KHPtCl 6 ・XH 2 O, Na 2 PtCl 6 ・XH 2 O.K. 2 PtCl 4 ・XH 2 O, PtCl 4 ・XH 2 O, PtCl 2 , Na 2 HPtCl 4 ・XH 2 O (wherein X is an integer of 0 to 6, preferably 0 or 6), chloroplatinic acid, and chloroplatinate salts; alcohol-modified chloroplatinic acid; platinum chloride, complexes of chloroplatinic acid and olefins, complexes of chloroplatinic acid and vinyl group-containing siloxanes, complexes of platinum and vinyl group-containing siloxanes; platinum black, platinum group metals such as palladium supported on carriers such as alumina, silica, and carbon; rhodium-olefin complexes; chlorotris(triphenylphosphine)rhodium (Wilkinson's catalyst), etc. These may be used alone or in combination of two or more.
[0068] The platinum group metal catalyst may be added in an amount effective as a hydrosilylation reaction catalyst, and the amount of platinum group metal in the platinum group metal catalyst relative to the total amount of components (A) and (B), calculated by mass, is usually about 0.1 to 500 ppm, preferably about 0.5 to 200 ppm, and more preferably about 1 to 100 ppm.
[0069] The silicone rubber may contain silicone oil, organosilane, inorganic powder, organic powder, antioxidant, and the like.
[0070] [Method for producing composite particles] In the present invention, the composite particles are produced by a method comprising the following steps: (i) emulsifying a curable liquid silicone composition using a surfactant to produce an oil-in-water emulsion, and then curing the curable liquid silicone composition to produce an aqueous dispersion of silicone rubber spherical particles having a volume average particle size of 50 to 1,000 nm; (ii) mixing the core particles, the aqueous dispersion of silicone rubber spherical particles produced in step (i), a cationic surfactant, and water to adsorb the silicone rubber particles to the surfaces of the core particles, thereby producing a mixed liquid containing the core particles having the silicone rubber particles adsorbed thereon; and (iii) volatilizing and removing water contained in the mixed liquid containing the core particles having the silicone rubber particles adsorbed thereon, produced in step (ii), to fix the silicone rubber particles adsorbed to the surfaces of the core particles.
[0071] In addition, in the method for producing composite particles of the present invention, the amount of the core particles relative to 100 parts by mass of water contained in the mixed liquid prepared in step (ii) is in the range of 1 to 100 parts by mass, and the amount of the silicone rubber spherical particles relative to 100 parts by mass of the core particles is in the range of 0.1 to 25 parts by mass.
[0072] The aqueous dispersion of silicone rubber spherical particles in step (i) can be prepared by a known method. The above-mentioned curable liquid silicone composition is emulsified using a surfactant to prepare an oil-in-water emulsion, and then the curable liquid silicone is cured by an addition reaction, a condensation reaction, a radical reaction, or the like. To incorporate silicone oil, organosilane, inorganic powder, organic powder, antioxidant, etc. into the silicone rubber particles, these can be incorporated into the curable liquid silicone composition. If this method involves emulsifying the curable liquid silicone composition and then carrying out a curing reaction, the resulting silicone rubber particles will be spherical in shape.
[0073] When making the water dispersion of silicone rubber spherical particles by curing by addition reaction, the method can be mentioned that surfactant and water are added to the curable liquid silicone composition that comprises the organopolysiloxane with the above-mentioned (A) alkenyl group and (B) organohydrogenpolysiloxane with silicon atom-bonded hydrogen atom, emulsify, make oil-in-water emulsion, and then add platinum group metal catalyst to carry out addition reaction.It is also possible to use the method that platinum group metal catalyst is mixed in advance with the curable liquid silicone composition, but in this case, it is necessary to adjust temperature, adjust catalyst amount or mix regulator etc. so that reaction does not proceed before emulsification is completed.
[0074] The surfactant used for emulsification is not particularly limited and may be a nonionic surfactant, an anionic surfactant, a cationic surfactant, or an amphoteric surfactant. Preferably, it is a nonionic surfactant. These may be used alone or in appropriate combination of two or more.
[0075] Examples of nonionic surfactants include polyoxyethylene alkyl ethers, polyoxyethylene polyoxypropylene alkyl ethers, polyoxyethylene alkylphenyl ethers, polyethylene glycol fatty acid esters, sorbitan fatty acid esters, polyoxyethylene sorbitan fatty acid esters, polyoxyethylene sorbitan fatty acid esters, polyoxyethylene sorbit fatty acid esters, glycerin fatty acid esters, polyoxyethylene glycerin fatty acid esters, polyglycerin fatty acid esters, propylene glycol fatty acid esters, polyoxyethylene castor oil, polyoxyethylene hydrogenated castor oil, polyoxyethylene hydrogenated castor oil fatty acid esters, polyoxyethylene alkylamines, polyoxyethylene fatty acid amides, polyoxyethylene-modified organopolysiloxanes, and polyoxyethylene polyoxypropylene-modified organopolysiloxanes.
[0076] Examples of anionic surfactants include alkyl sulfate salts such as sodium lauryl sulfate, polyoxyethylene alkyl ether sulfate salts, polyoxyethylene alkylphenyl ether sulfate salts, sulfate salts of fatty acid alkylolamides, alkylbenzenesulfonates, polyoxyethylene alkylphenyl ether sulfonates, α-olefinsulfonates, α-sulfofatty acid ester salts, alkylnaphthalenesulfonates, alkyldiphenylether disulfonates, alkanesulfonates, N-acyltaurates, dialkylsulfosuccinates, monoalkylsulfosuccinates, polyoxyethylene alkyl ether sulfosuccinates, fatty acid salts, polyoxyethylene alkyl ether carboxylates, N-acylamino acid salts, monoalkyl phosphate salts, dialkyl phosphate ester salts, and polyoxyethylene alkyl ether phosphate salts.
[0077] Examples of the cationic surfactant include alkyltrimethylammonium salts, dialkyldimethylammonium salts, trialkylmethylammonium salts, polyoxyethylenealkyldimethylammonium salts, dipolyoxyethylenealkylmethylammonium salts, tripolyoxyethylenealkylammonium salts, alkylbenzyldimethylammonium salts, alkylpyridinium salts, monoalkylamine salts, and monoalkylamidoamine salts.
[0078] Examples of amphoteric surfactants include alkyldimethylamine oxide, alkyldimethylcarboxybetaine, alkylamidopropyldimethylcarboxybetaine, alkylhydroxysulfobetaine, and alkylcarboxymethylhydroxyethylimidazolinium betaine.
[0079] For emulsification, a general emulsifying disperser may be used, and examples thereof include a high-speed rotation centrifugal radiation type agitator such as a Homodisper, a high-speed rotation shear type agitator such as a Homomixer, a high-pressure jet type emulsifying disperser such as a homogenizer, a colloid mill, an ultrasonic emulsifier, etc. The stirring speed, time, etc. are not particularly limited as long as emulsification is possible and the desired particle size can be obtained.
[0080] The volume average particle size of the rubber particles in the aqueous dispersion of silicone rubber spherical particles is preferably smaller than that of the core particles. If the volume average particle size is smaller than that of the core particles, the cosmetic can be imparted with a natural finish due to light diffusion, good adhesion to the skin, a soft and moist feel, and drop stability. The volume average particle size is in the range of 50 to 1,000 nm, preferably 100 to 500 nm. If the volume average particle size is 1,000 nm or less, it can adhere to the core particles. The volume average particle size is measured by a laser diffraction / scattering method.
[0081] The core particles used in step (ii) may be the inorganic particles, organic particles, or inorganic-organic composite particles described above, and may be used alone or in appropriate combination of two or more types. A pre-prepared aqueous dispersion or an aqueous dispersion synthesized in water may also be used as is.
[0082] In step (ii), the amount of core particles is in the range of 1 to 100 parts by mass, preferably 5 to 50 parts by mass, and more preferably 10 to 30 parts by mass, per 100 parts by mass of water contained in the mixed liquid. When the amount of core particles is 1 part by mass or more, production efficiency increases. Furthermore, when the amount of core particles is 100 parts by mass or less, the dynamic viscosity of the mixed liquid does not become too high, making it easier for the silicone rubber particles to adhere.
[0083] In step (ii), the amount of the aqueous dispersion of silicone rubber spherical particles should be such that the amount of silicone rubber adheres to the surface of the core particles. The amount of silicone rubber spherical particles in the aqueous dispersion of silicone rubber spherical particles is in the same range as the amount of silicone rubber relative to the core particles in the composite particles described above, and is in the range of 0.1 to 25 parts by mass, preferably 0.2 to 20 parts by mass, and more preferably 0.5 to 15 parts by mass or more, per 100 parts by mass of the core particles.
[0084] The cationic surfactant used in step (ii) has the effect of causing the silicone rubber particles to adsorb to the core particles. The cationic surfactant adsorbs to the surface of the silicone rubber particles, increasing the zeta potential (a value that represents the charged state of a solid surface) of the rubber particle surface, which in turn increases the difference in zeta potential with the core particles, presumably resulting in electrostatic interaction between the silicone rubber particles and the core particles.
[0085] The cationic surfactant used in step (ii) may be any of those mentioned above, and may be in the form of an aqueous solution, a solution in a water-soluble organic solvent such as an alcohol, or an aqueous solution containing a water-soluble organic solvent.
[0086] The amount of cationic surfactant used in step (ii) is in the range of 0.02 to 0.9 parts by mass, more preferably 0.03 to 0.7 parts by mass, per 100 parts by mass of water contained in the mixed liquid. If the amount is 0.02 to 0.9 parts by mass, the silicone rubber particles can be adsorbed onto the surface of the core particles.
[0087] If the aqueous dispersion of silicone rubber spherical particles prepared in step (i) contains a cationic surfactant, and the desired amount of cationic surfactant is added in step (ii), there is no need to add additional cationic surfactant because the cationic surfactant is already mixed in. This type of case is also included in the mixing of the aqueous dispersion of silicone rubber spherical particles prepared in step (i), the cationic surfactant, and water in step (ii) of the present invention.
[0088] In step (ii), a surfactant other than a cationic surfactant or a water-soluble polymer may be contained. This surfactant is the same as the surfactant used for emulsifying the silicone rubber spherical particles in the aqueous dispersion prepared in step (i). When the core particles are blended in the form of an aqueous dispersion, a surfactant other than a cationic surfactant or a water-soluble polymer may be contained as a dispersant. Furthermore, in step (ii), a surfactant other than a cationic surfactant or a water-soluble polymer may be blended.
[0089] The surfactants other than the cationic surfactants are not particularly limited and include nonionic surfactants, anionic surfactants, and amphoteric surfactants, as described above, with nonionic surfactants or amphoteric surfactants being preferred.
[0090] Examples of water-soluble polymers include nonionic and anionic water-soluble polymers, with nonionic water-soluble polymers being preferred. It is desirable not to use cationic water-soluble polymers, as they may inhibit the adsorption of silicone rubber particles to the core particle surface.
[0091] Examples of nonionic water-soluble polymers include polyvinyl alcohol, polyacrylamide, polyvinylpyrrolidone, polyethylene oxide, polymethyl vinyl ether, polyisopropylacrylamide, methyl cellulose, hydroxypropyl methyl cellulose, starch, guar gum, and xanthan gum.
[0092] Examples of anionic water-soluble polymers include sodium polyacrylate, carboxyvinyl polymer, polysodium styrene sulfonate, sodium naphthalene sulfonate condensates, sodium cellulose sulfate, sodium carboxymethyl cellulose, carboxymethyl starch, sodium alginate, gum arabic, carrageenan, and derivatives thereof obtained by copolymerizing these with a monomer having a nonionic group or an anionic group.
[0093] In step (ii), the core particles, the aqueous dispersion of silicone rubber spherical particles, the cationic surfactant, and water may be mixed using a stirring blade such as a paddle blade, a propeller blade, a swept blade, or an anchor blade.
[0094] The core particles, the aqueous dispersion of silicone rubber spherical particles, the cationic surfactant, and water are preferably mixed by stirring the core particles, cationic surfactant, and water, and then the aqueous dispersion of silicone rubber spherical particles is added while stirring. The core particles, cationic surfactant, and water may be added in any order. Alternatively, the core particles and water are preferably mixed by stirring, and then the aqueous dispersion of silicone rubber spherical particles is added, and then the cationic surfactant is added while stirring.
[0095] When the core particles are used in the form of an aqueous dispersion, the order may be to first stir and mix the aqueous dispersion of silicone rubber spherical particles, the cationic surfactant, and water, and then add the aqueous dispersion of core particles while stirring. The order in which the aqueous dispersion of silicone rubber spherical particles, the cationic surfactant, and water are added may be any order. Alternatively, the order in which the aqueous dispersion of core particles, the aqueous dispersion of silicone rubber spherical particles, and water are mixed and then add the cationic surfactant while stirring may be any order. The order in which the aqueous dispersion of core particles, the aqueous dispersion of silicone rubber spherical particles, and water are added may be any order.
[0096] In step (ii), an acid or alkali may be added to lower or raise the pH of the water. If the change in pH increases the zeta potential difference between the core particles and the silicone rubber spherical particles, this may facilitate adsorption of the silicone rubber spherical particles to the core particles.
[0097] In step (ii), a water-soluble organic solvent such as alcohol may be added to the mixture to facilitate the adsorption of the silicone rubber spherical particles to the core particles.
[0098] The temperature in step (ii) is not particularly limited, and may be in the range of 0 to 100°C.
[0099] After mixing the core particles, the aqueous dispersion of silicone rubber spherical particles, the cationic surfactant, and water, it is preferable to continue stirring for a while until the silicone rubber spherical particles are adsorbed onto the core particles.
[0100] In step (iii), the removal by volatilization of water (the moisture content of the mixed liquid) from the mixed liquid containing the core particles having adsorbed silicone rubber particles produced in step (ii) can be carried out, for example, by heating under normal pressure or reduced pressure, and specific examples include a method in which the mixed liquid is left to stand under heating to remove the moisture, a method in which the mixed liquid is stirred and fluidized under heating to remove the moisture, a method in which the mixed liquid is sprayed and dispersed in a hot air current as in a spray dryer, a method in which a fluidized heat medium is used, etc. Note that, as a pretreatment for this operation, the mixed liquid may be concentrated by methods such as thermal dehydration, filtration separation such as pressure filtration, centrifugation, decantation, etc.
[0101] When an acid or alkali is added in step (ii), the mixture may be neutralized by adding an acid or alkali before removing the water by evaporation, and if necessary, washed with water, alcohol, or the like.
[0102] The adhesion of the silicone rubber particles to the core particle surface in step (iii) is presumably achieved through the following process: When the amount of moisture decreases due to the evaporation of water, capillary forces are generated between the core particle and the silicone rubber spherical particles adsorbed on its surface. The capillary forces attract the silicone rubber particles to the core particle surface, causing them to deform and spread across the core particle surface, increasing the adhesive area with the core particle. This increases the adhesive force, and the particles remain adhered even after the water is removed and the capillary forces disappear.
[0103] The shape of the silicone rubber that adheres to the surface of the core particles after the water has evaporated away varies depending on the hardness of the rubber: if the rubber hardness is high, it is spherical; if the rubber hardness is low, it takes on a shape resembling fused spherical particles; and if the rubber hardness is even lower, it takes on a nodular or film-like shape.
[0104] The deformation of the silicone rubber spherical particles due to adhesion to the surface of the core particles is presumably due to the capillary force that occurs between the core particles and the silicone rubber spherical particles in step (iii) as described above.It is also presumed that the capillary force that occurs between the silicone rubber spherical particles themselves also has an effect.
[0105] In the method for producing composite particles of the present invention, the produced composite particles may have low agglomeration properties as described above, but may be weakly agglomerated. In such cases, when the particles obtained by removing water from the mixed solution are agglomerated, the particles may be crushed using a crusher such as a jet mill, a ball mill, or a hammer mill.
[0106] The composite particles of the present invention may have their surfaces treated with a silylating agent, silicone oil, waxes, paraffins, organic fluorine compounds, surfactants, or the like in order to impart or improve water repellency or improve dispersibility in oil agents.
[0107] The present invention will be described in more detail below with reference to examples and comparative examples, but the present invention is not limited to the following examples. In the examples, the kinematic viscosity is a value measured using a capillary viscometer at 25°C, and "%" representing concentration and content means "% by mass".
[0108] Example 1 (Step (i): Preparation of an aqueous dispersion of silicone rubber spherical particles) 2 313 g of a vinyl group-containing dimethylpolysiloxane (A1) having a kinematic viscosity of 117 mm3 / s, 287 g of methylhydrogenpolysiloxane (B1) (amount equivalent to 1.15 hydrosilyl groups per vinyl group) and 0.1 g of dl-α-tocopherol (antioxidant) were placed in a 1-liter glass beaker and mixed and dissolved using a homomixer. 45 g of polyoxyethylene lauryl ether (trade name: Emulgen 109P, manufactured by Kao Corporation) and 150 g of water were added and stirred using a homomixer. When the mixture was thickened, stirring was continued for an additional 15 minutes. Next, 402 g of water was added to dilute the mixture, and the mixture was passed through a homogenizer at a pressure of 100 MPa to obtain a uniform white emulsion. 498.5 g of this emulsion was transferred to a 1-liter glass flask equipped with an anchor-type stirring blade stirrer, and the temperature was adjusted to 20-25°C. After that, a mixed solution of 0.5 g of an isododecane solution of a platinum-vinyl group-containing disiloxane complex (platinum content 0.5%) and 1 g of polyoxyethylene lauryl ether (trade name: Emulgen 109P, manufactured by Kao Corporation) was added with stirring, and the mixture was stirred at the same temperature for 24 hours to obtain an aqueous dispersion of silicone rubber spherical particles.
[0109] The volume average particle size of the silicone rubber spherical particles was measured using a laser diffraction / scattering particle size distribution analyzer LA-960 (manufactured by Horiba, Ltd.) and was found to be 320 nm.
[0110] Separately from the preparation of the aqueous dispersion of silicone rubber spherical particles, a vinyl group-containing dimethylpolysiloxane (A1) represented by the following formula (11), a methylhydrogenpolysiloxane (B1) represented by the following formula (12), and an isododecane solution of a platinum-vinyl group-containing disiloxane complex (platinum content 0.5%) were mixed in the above-mentioned proportions, poured into an aluminum petri dish to a thickness of 10 mm, left at 25°C for 6 hours, and then heated in a thermostatic chamber at 50°C for 1 hour. The resulting cured product was a non-sticky rubber elastic body, and its hardness, measured with a Durometer A hardness tester, was 73.
[0111] (A1): Vinyl group-containing dimethylpolysiloxane
[0112] (B1): Methylhydrogenpolysiloxane
[0113] Example 2 (Step (i): Preparation of aqueous dispersion of silicone rubber spherical particles) 2 343 g of a vinyl group-containing dimethylpolysiloxane (A2) having a kinematic viscosity of 30 mm 2 57 g of methylhydrogenpolysiloxane (B2) with a methylhydrogen group ratio of 1 / s (amount resulting in 1.15 hydrosilyl groups per vinyl group) and 0.1 g of dl-α-tocopherol (antioxidant) were placed in a 1-liter glass beaker and mixed and dissolved using a homomixer. 30 g of polyoxyethylene lauryl ether (trade name: Emulgen 109P, manufactured by Kao Corporation) and 40 g of water were added and stirred using a homomixer, resulting in a viscosity increase to the point where stirring was no longer possible. The thickened mixture was kneaded for 15 minutes using a homodisper. 527 g of water was then added and mixed using a homomixer, resulting in a uniform white emulsion. This emulsion was transferred to a 1-liter glass flask equipped with an anchor-type stirring blade stirrer, and the temperature was adjusted to 20-25°C. After that, a mixed solution of 1 g of an isododecane solution of a platinum-vinyl group-containing disiloxane complex (platinum content 0.5%) and 2 g of polyoxyethylene lauryl ether (trade name: Emulgen 109P, manufactured by Kao Corporation) was added with stirring, and the mixture was stirred at the same temperature for 24 hours to obtain an aqueous dispersion of silicone rubber spherical particles.
[0114] The volume average particle size of the silicone rubber spherical particles was measured using a laser diffraction / scattering particle size distribution analyzer LA-960 (manufactured by Horiba, Ltd.) and was found to be 330 nm.
[0115] Separately from the preparation of the aqueous dispersion of silicone rubber spherical particles, a vinyl group-containing dimethylpolysiloxane (A2) represented by the following formula (13), a methylhydrogenpolysiloxane (B2) represented by the following formula (14), and an isododecane solution of a platinum-vinyl group-containing disiloxane complex (platinum content 0.5%) were mixed in the above-mentioned proportions, poured into an aluminum petri dish to a thickness of 10 mm, left at 25°C for 6 hours, and then heated in a thermostatic chamber at 50°C for 1 hour. The resulting cured product was a non-sticky rubber elastic body, and its hardness, measured with a Durometer A hardness tester, was 50.
[0116] (A2): Vinyl group-containing dimethylpolysiloxane
[0117] (B2): Methylhydrogenpolysiloxane
[0118] Example 3 (Step (i): Preparation of an aqueous dispersion of silicone rubber spherical particles) 2 365 g of a vinyl group-containing dimethylpolysiloxane (A3) having a kinematic viscosity of 30 mm / s, 235 g of methylhydrogenpolysiloxane (B2) with a methylhydrogen group ratio of 1.17 per vinyl group (B2) and 0.1 g of dl-α-tocopherol (antioxidant) were placed in a 1-liter glass beaker and mixed and dissolved using a homomixer. 30 g of polyoxyethylene lauryl ether (product name: Emulgen 109P, manufactured by Kao Corporation) and 35 g of water were added and stirred using a homomixer, resulting in a viscosity increase that made the mixture unstirrable. The thickened mixture was kneaded for 15 minutes using a homodisper. 532 g of water was then added and mixed using a homomixer, resulting in a uniform white emulsion. This emulsion was transferred to a 1-liter glass flask equipped with an anchor-type stirring blade stirrer, and the temperature was adjusted to 20-25°C. After that, a mixed solution of 1 g of an isododecane solution of a platinum-vinyl group-containing disiloxane complex (platinum content 0.5%) and 2 g of polyoxyethylene lauryl ether (trade name: Emulgen 109P, manufactured by Kao Corporation) was added with stirring, and the mixture was stirred at the same temperature for 24 hours to obtain an aqueous dispersion of silicone rubber spherical particles.
[0119] The volume average particle size of the silicone rubber spherical particles was measured using a laser diffraction / scattering particle size distribution analyzer LA-960 (manufactured by Horiba, Ltd.) and was found to be 310 nm.
[0120] Separately from the preparation of the aqueous dispersion of silicone rubber spherical particles, a vinyl group-containing dimethylpolysiloxane (A3) represented by the following formula (15), a methylhydrogenpolysiloxane (B2) represented by the above formula (14), and an isododecane solution of a platinum-vinyl group-containing disiloxane complex (platinum content 0.5%) were mixed in the above-mentioned proportions, poured into an aluminum petri dish to a thickness of 10 mm, left at 25°C for 6 hours, and then heated in a thermostatic chamber at 50°C for 1 hour. The resulting cured product was a non-sticky rubber elastic body, and its hardness, measured with a Durometer A hardness tester, was 43.
[0121] (A3): Vinyl group-containing dimethylpolysiloxane
[0122] [Example 4] (Step (i): Preparation of aqueous dispersion of silicone rubber spherical particles) 2 384 g of a vinyl group-containing dimethylpolysiloxane (A4) having a kinematic viscosity of 30 mm 2 16 g of methylhydrogenpolysiloxane (B2) with a methylhydrogen group ratio of 1 / s (amount resulting in 1.18 hydrosilyl groups per vinyl group) and 0.1 g of dl-α-tocopherol (antioxidant) were placed in a 1-liter glass beaker and mixed and dissolved using a homomixer. 32 g of polyoxyethylene lauryl ether (trade name: Emulgen 109P, manufactured by Kao Corporation) and 36 g of water were added and stirred using a homomixer, resulting in a viscosity increase to the point where stirring was no longer possible. The thickened mixture was kneaded for 15 minutes using a homodisper. 530 g of water was then added and mixed using a homomixer, resulting in a uniform white emulsion. This emulsion was transferred to a 1-liter glass flask equipped with an anchor-type stirring blade stirrer, and the temperature was adjusted to 20-25°C. After that, a mixed solution of 0.6 g of an isododecane solution of a platinum-vinyl group-containing disiloxane complex (platinum content 0.5%) and 1 g of polyoxyethylene lauryl ether (trade name: Emulgen 109P, manufactured by Kao Corporation) was added with stirring, and the mixture was stirred at the same temperature for 24 hours to obtain an aqueous dispersion of silicone rubber spherical particles.
[0123] The volume average particle size of the silicone rubber spherical particles was measured using a laser diffraction / scattering particle size distribution analyzer LA-960 (manufactured by Horiba, Ltd.) and was found to be 320 nm.
[0124] Separately from the preparation of the aqueous dispersion of silicone rubber spherical particles, a vinyl group-containing dimethylpolysiloxane (A4) represented by the following formula (16), a methylhydrogenpolysiloxane (B2) represented by the above formula (14), and an isododecane solution of a platinum-vinyl group-containing disiloxane complex (platinum content 0.5%) were mixed in the above-mentioned proportions, poured into an aluminum petri dish to a thickness of 10 mm, left at 25°C for 6 hours, and then heated in a thermostatic chamber at 50°C for 1 hour. The resulting cured product was a non-sticky rubber elastic body, and its hardness, measured with a Durometer A hardness tester, was 27.
[0125] (A4): Vinyl group-containing dimethylpolysiloxane
[0126] Example 5 (Step (i): Preparation of aqueous dispersion of silicone rubber spherical particles) 2 393 g of vinyl group-containing dimethylpolysiloxane (A5) having a kinematic viscosity of 30 mm 2 7 g of methylhydrogenpolysiloxane (B2) with a methylhydrogen group ratio of 1.19 per vinyl group and 0.1 g of dl-α-tocopherol (antioxidant) were placed in a 1-liter glass beaker and mixed and dissolved using a homomixer. 42 g of polyoxyethylene lauryl ether (product name: Emulgen 109P, manufactured by Kao Corporation) and 35 g of water were added and stirred using a homomixer, resulting in a viscosity that was too high to stir. The thickened mixture was kneaded for 15 minutes using a homodisper. 521 g of water was then added and mixed using a homomixer, resulting in a uniform white emulsion. This emulsion was transferred to a 1-liter glass flask equipped with an anchor-type stirring blade stirrer, and the temperature was adjusted to 20-25°C. After that, a mixed solution of 0.6 g of an isododecane solution of a platinum-vinyl group-containing disiloxane complex (platinum content 0.5%) and 1 g of polyoxyethylene lauryl ether (trade name: Emulgen 109P, manufactured by Kao Corporation) was added with stirring, and the mixture was stirred at the same temperature for 24 hours to obtain an aqueous dispersion of silicone rubber spherical particles.
[0127] The volume average particle size of the silicone rubber spherical particles was measured using a laser diffraction / scattering particle size distribution analyzer LA-960 (manufactured by Horiba Ltd.) and was found to be 300 nm.
[0128] Separately from the preparation of the aqueous dispersion of silicone rubber spherical particles, a vinyl group-containing dimethylpolysiloxane (A5) represented by formula (17) below, a methylhydrogenpolysiloxane (B2) represented by formula (14) above, and an isododecane solution of a platinum-vinyl group-containing disiloxane complex (platinum content 0.5%) were mixed in the above-mentioned proportions, poured into an aluminum petri dish to a thickness of 10 mm, left at 25°C for 6 hours, and then heated in a thermostatic chamber at 50°C for 1 hour. The resulting cured product was a non-sticky rubber elastic body, and its hardness, measured with a Durometer A hardness tester, was 20.
[0129] (A5): Vinyl group-containing dimethylpolysiloxane
[0130] Example 6 (Steps (ii) and (iii): Adsorption and adhesion of silicone rubber particles to the surface of cellulose particles (core particles)) A 1-liter glass flask equipped with an anchor-type stirring blade stirrer was charged with 75 g of cellulose particles (trade name: CELLULOBEADS D5, manufactured by Daito Chemical Industry Co., Ltd., shape = spherical, volume average particle size = 12 μm, electron microscope photograph: Figure 8) (an amount equivalent to 17.9 parts by mass of cellulose particles per 100 parts by mass of water), 2.8 g of a 30% aqueous solution of lauryltrimethylammonium chloride (trade name: CATION BB, manufactured by NOF Corporation) (an amount equivalent to 0.2 parts by mass of lauryltrimethylammonium chloride per 100 parts by mass of water), and 412.2 g of water. The pH of the solution at this time was 6.6. While stirring with a blade, 10 g of the aqueous dispersion of silicone rubber spherical particles obtained in Example 1 (an amount such that the silicone rubber particles were 5.3 parts by mass per 100 parts by mass of cellulose particles) was added, and the mixture was stirred for 2 hours, at a liquid temperature of 25°C.
[0131] The resulting mixture was filtered using a pressure filter with a filter paper (product name: Quantitative Filter Paper No. 5B, manufactured by Toyo Roshi Kaisha, Ltd.) with a particle retention diameter of 4 μm to separate the particles. The filtrate was colorless and transparent, and it was determined that the silicone rubber particles had not passed through the filter paper, suggesting that the silicone rubber particles were possibly adsorbed onto the surface of the cellulose particles. The resulting hydrous particles were placed in a stainless steel tray, and the water was removed by evaporation at 105°C in a hot air flow dryer. The dried product was crushed using a jet mill to obtain particles.
[0132] When the obtained particles were observed under an electron microscope, it was confirmed that spherical particles of approximately 300 nm in size were attached to the entire surface of particles with the same shape and diameter as the cellulose particles, and that they were composite particles in which silicone rubber was attached to the surface of the cellulose particles. The electron microscope photograph is shown in Figure 1. Furthermore, no adhesion between the composite particles was observed, and it was determined that the shape and diameter of the cellulose particles had been maintained.
[0133] The volume average particle size of the obtained composite particles was measured using an electrical resistance particle size distribution analyzer (Multisizer 3, manufactured by Beckman Coulter, Inc.) and found to be 12 μm. The particle size distribution was approximately the same as that of the cellulose particles, and it was determined that the shape and particle size of the cellulose particles were maintained.
[0134] Examples 7 to 12 (Steps (ii) and (iii): Adsorption and Fixation of Silicone Rubber Particles to the Surface of Cellulose Particles (Core Particles)) Particles were obtained in the same manner as in Example 6, except that the type of cationic surfactant, the type and amount of silicone rubber particle aqueous dispersion, and the amount of water were as shown in Table 1.
[0135] The mixed solution was filtered through a filter paper, and the filtrate was observed for its appearance, and the silicone rubber adhesion to the surface of the cellulose particles (core particles) was observed under an electron microscope. The results of the volume average particle size measurement are shown in Table 1.
[0136] Observation under an electron microscope of the particles obtained in Example 7 showed that spherical particles of approximately 300 nm in size and particles resembling fused spherical particles were attached to the entire surface of particles having the same shape and diameter as the cellulose particles, confirming that the particles were composite particles in which silicone rubber was attached to the surface of the cellulose particles. An electron microscope photograph is shown in Figure 2. Furthermore, no adhesion between the composite particles was observed, and it was determined that the shape and diameter of the cellulose particles were maintained.
[0137] When the particles obtained in Example 8 were observed under an electron microscope, it was confirmed that spherical particles of approximately 300 nm in size and particles shaped like fused spherical particles were attached to the entire surface of particles having the same shape and diameter as the cellulose particles, forming composite particles with silicone rubber attached to the surface of the cellulose particles. An electron microscope photograph is shown in Figure 3. Furthermore, no adhesion between the composite particles was observed, and it was determined that the shape and diameter of the cellulose particles were maintained.
[0138] Observation under an electron microscope of the particles obtained in Example 9 showed that a nodular coating was attached to the entire surface of particles with the same shape and particle size as the cellulose particles, confirming that the particles were composite particles in which silicone rubber was attached to the surface of the cellulose particles. An electron microscope photograph is shown in Figure 4. Furthermore, no adhesion between the composite particles was observed, and it was determined that the shape and particle size of the cellulose particles were maintained.
[0139] Observation under an electron microscope of the particles obtained in Example 10 showed that a nodular coating was attached to the entire surface of particles with the same shape and particle size as the cellulose particles, confirming that the particles were composite particles in which silicone rubber was attached to the surface of the cellulose particles. An electron microscope photograph is shown in Figure 5. Furthermore, no adhesion between the composite particles was observed, and it was determined that the shape and particle size of the cellulose particles were maintained.
[0140] Observation of the particles obtained in Example 11 under an electron microscope revealed that spherical particles of approximately 300 nm in size were sparsely attached to the surface of particles of the same shape and diameter as the cellulose particles, confirming that the particles were composite particles in which silicone rubber was attached to the surface of the cellulose particles. An electron microscope photograph is shown in Figure 6. Furthermore, no adhesion between the composite particles was observed, and it was determined that the shape and diameter of the cellulose particles were maintained.
[0141] When the particles obtained in Example 12 were observed under an electron microscope, sparse nodules were observed on the surface of particles of the same shape and diameter as the cellulose particles, confirming that they were composite particles in which silicone rubber was adhered to the surface of the cellulose particles. An electron microscope photograph is shown in Figure 7. Furthermore, no adhesion between the composite particles was observed, and it was determined that the shape and diameter of the cellulose particles were maintained.
[0142] Comparative Example 1 (Steps (ii) and (iii): Adsorption and adhesion of silicone rubber particles to the surface of cellulose particles (core particles)) 75 g of the above-mentioned cellulose particles as core particles (an amount equivalent to 17.8 parts by mass of cellulose particles per 100 parts by mass of water) and 415.0 g of water were placed in a 1 liter glass flask equipped with a stirrer using an anchor-shaped stirring blade. The pH of the liquid at this time was 6.4. No cationic surfactant was added. With impeller stirring, 10 g of the aqueous dispersion of silicone rubber spherical particles obtained in Example 1 (an amount equivalent to 5.3 parts by mass of silicone rubber particles per 100 parts by mass of cellulose particles) was added, and the mixture was stirred for 2 hours. The liquid temperature at this time was 25°C.
[0143] The resulting mixture was filtered using a pressure filter with filter paper having a particle retention diameter of 4 μm (product name: Quantitative Filter Paper No. 5B, manufactured by Toyo Roshi Kaisha, Ltd.) to separate the particles. The filtrate was cloudy, indicating that the silicone rubber particles had passed through the filter paper, meaning that at least the silicone rubber particles that had passed through the filter paper were not adsorbed onto the surfaces of the cellulose particles.
[0144] The obtained water-containing particles were placed in a stainless steel tray, and the water was removed by evaporation in a hot air fluidized dryer at a temperature of 105° C. The dried product was crushed in a jet mill to obtain particles.
[0145] When the resulting particles were observed under an electron microscope, no silicone rubber was found to be attached to the surface of the cellulose particles.
[0146] (Note 1) Cationic surfactants D-1: 30% aqueous solution of lauryltrimethylammonium chloride (trade name: Cation BB, manufactured by NOF Corporation) D-2: 30% aqueous solution of cetyltrimethylammonium chloride (trade name: Courtamine 60W, manufactured by Kao Corporation) D-3: 25% aqueous solution of stearyltrimethylammonium chloride (trade name: Cation AB-250AQ, manufactured by NOF Corporation) (Note 2) Nonionic surfactant: Polyoxyethylene lauryl ether contained in an aqueous dispersion of silicone rubber spherical particles
[0147] Example 13 (Steps (ii) and (iii): Adsorption and Fixation of Silicone Rubber Particles to the Surface of Silica (Core Particles)) A 1-liter glass flask equipped with an anchor-type stirring blade stirrer was charged with 75 g of silica (trade name: SILICA MICRO BEAD P-1500, manufactured by JGC Catalysts and Chemicals Co., Ltd., shape = spherical, volume average particle size = 16 μm, electron microscope photograph: FIG. 11) (an amount such that the silica was 17.8 parts by mass per 100 parts by mass of water), 2.8 g of a 30% aqueous solution of lauryltrimethylammonium chloride (trade name: CATION BB, manufactured by NOF Corporation) (an amount such that the lauryltrimethylammonium chloride was 0.2 parts by mass per 100 parts by mass of water), and 412.2 g of water. The pH of the solution at this time was 6.8. While stirring with a blade, 10 g of the aqueous dispersion of silicone rubber particles obtained in Example 2 (an amount equivalent to 5.3 parts by mass of silicone rubber particles per 100 parts by mass of silica) was added and stirred for 2 hours, at a liquid temperature of 25°C.
[0148] The resulting suspension was filtered using a pressure filter with a filter paper with a particle retention size of 4 μm (product name: Quantitative Filter Paper No. 5B, manufactured by Toyo Roshi Kaisha, Ltd.) to separate the particles. The filtrate was colorless and transparent, and it was determined that the silicone rubber particles had not passed through the filter paper, suggesting that the silicone rubber particles were possibly adsorbed to the silica surface.
[0149] The obtained water-containing particles were placed in a stainless steel tray, and the water was removed by evaporation in a hot air fluidized dryer at a temperature of 105° C. The dried product was crushed in a jet mill to obtain particles.
[0150] When the obtained particles were observed under an electron microscope, it was confirmed that spherical particles of approximately 300 nm in size were attached to the entire surface of particles with the same shape and diameter as silica, and that they were composite particles with silicone rubber attached to the silica surface. The electron microscope photograph is shown in Figure 9. Furthermore, no adhesion between the composite particles was observed, and it was determined that the shape and diameter of the silica were maintained.
[0151] The volume average particle size of the obtained composite particles was measured using an electrical resistance particle size distribution analyzer (Multisizer 3, manufactured by Beckman Coulter, Inc.) and found to be 16 μm. The particle size distribution was approximately the same as that of silica, and it was determined that the shape and particle size of silica were maintained.
[0152] [Examples 14 to 20, Comparative Examples 2 to 4] (Steps (ii) and (iii): Adsorption and Fixation of Silicone Rubber Particles to the Surface of Silica (Core Particles)) Particles were obtained in the same manner as in Example 13, except that the type of cationic surfactant, the type and amount of aqueous silicone rubber particle dispersion, and the amount of water were as shown in Tables 2 and 3.
[0153] The mixed solution was filtered through a filter paper, and the filtrate was observed for its appearance, and the silicone rubber adhesion to the surface of the silica particles (core particles) was observed under an electron microscope. The results of the volume average particle size measurement are shown in Tables 2 and 3.
[0154] When the particles obtained in Example 18 were observed under an electron microscope, nodules were observed all over the surface of particles with the same shape and particle size as silica, confirming that they were composite particles with silicone rubber adhered to the silica surface. An electron microscope photograph is shown in Figure 10. Furthermore, no adhesion between the composite particles was observed, and it was determined that the shape and particle size of the silica were maintained.
[0155] The particles obtained in Examples 14 to 17, 19, and 20 also had the properties shown in Tables 2 and 3, and were determined to maintain the shape and particle size of silica similar to the particles obtained in Example 18.
[0156] When the particles obtained in Comparative Examples 2 to 4 were observed under an electron microscope, no silicone rubber was found to be attached to the surface of the silica particles.
[0157] (Note 3) Cationic surfactants D-1: 30% aqueous solution of lauryltrimethylammonium chloride (trade name: Cation BB, manufactured by NOF Corporation) D-4: 75% isopropyl alcohol solution of dialkyl (C12-C18) dimethylammonium chloride (trade name: Courtamine D-2345P, manufactured by Kao Corporation) D-5: 80% aqueous solution of trioctylmethylammonium chloride (trade name: TOMAC 80% aqueous solution, manufactured by Nippon Specialty Chemical Industry Co., Ltd.) D-6: 20% aqueous solution of tri(polyoxyethylene)stearylammonium chloride (Catinal SPC-20V-S, manufactured by Toho Chemical Industry Co., Ltd.) D-7: 50% aqueous solution of benzalkonium chloride (Nikkol CA-101, manufactured by Nikko Chemicals Co., Ltd.)
[0158]
[0159] In Examples 6 to 22, composite particles were produced in which the core particles did not contain multiple core particles, the particles did not strongly aggregate or adhere to each other, the shape and particle size of the core particles were largely maintained, and substantially all of the incorporated silicone rubber adhered to the surface of substantially all of the core particles. On the other hand, in Comparative Examples 1 and 2, no cationic surfactant was incorporated in step (ii), so no silicone rubber adhered to the core particle surface, and the desired composite particles could not be produced. Furthermore, in Comparative Example 3, the amount of cationic surfactant in step (ii) was insufficient, and in Comparative Example 4, the amount of cationic surfactant in step (ii) was excessive, so no silicone rubber adhered to the core particle surface, and the desired composite particles could not be produced.
[0160] The present invention is not limited to the above-described embodiments. The above-described embodiments are merely examples, and anything that has substantially the same configuration as the technical idea described in the claims of the present invention and that exhibits similar effects is included within the technical scope of the present invention.
Claims
1. A method for producing composite particles comprising attaching silicone rubber to the surfaces of core particles having a volume average particle size of 1 to 50 μm, comprising the steps of: (i) emulsifying a curable liquid silicone composition using a surfactant to prepare an oil-in-water emulsion, and then curing the curable liquid silicone composition to prepare an aqueous dispersion of silicone rubber spherical particles having a volume average particle size of 50 to 1,000 nm; (ii) mixing the core particles, the aqueous dispersion of silicone rubber spherical particles prepared in step (i), a cationic surfactant, and water to adsorb the silicone rubber particles to the surfaces of the core particles, thereby preparing a mixed liquid containing the core particles having the silicone rubber particles adsorbed thereto; and (iii) volatilizing and removing water contained in the mixed liquid containing the core particles having the silicone rubber particles adsorbed thereto prepared in step (ii), thereby fixing the silicone rubber particles adsorbed to the surfaces of the core particles. wherein the amount of the core particles is in the range of 1 to 100 parts by mass relative to 100 parts by mass of water contained in the mixed liquid prepared in step (ii), the amount of the silicone rubber spherical particles is in the range of 0.1 to 25 parts by mass relative to 100 parts by mass of the core particles, and the amount of the cationic surfactant is in the range of 0.02 to 0.9 parts by mass relative to 100 parts by mass of water.
2. The method for producing composite particles according to claim 1, characterized in that the core particles are made of at least one of inorganic particles and organic particles.
3. A method for producing composite particles as described in claim 1 or 2, characterized in that the rubber hardness of the silicone rubber spherical particles is in the range of 5 to 95 when measured using a Type A durometer specified in JIS K6253.
Citation Information
Patent Citations
Composite particle containing polyorganosiloxane and its production
JP1997208644A
Composite particle, method for producing the same and cosmetic product
JP2011001332A
Method for producing composite particle
JP2013035758A