Steel pipe and method for manufacturing same

The steel pipe's bainite structure with controlled crystal plane orientation and composition addresses SSCC resistance issues in sour environments, achieving stable SSCC resistance and high tensile strength through precise manufacturing processes.

WO2024237292A1PCT designated stage expired Publication Date: 2024-11-21JFE STEEL CORP
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2024/018028
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-05-17
Filing Date
2024-05-15
Publication Date
2024-11-21

AI Technical Summary

Technical Problem

Steel pipes used for transporting crude oil and natural gas in sour environments face challenges with sulfide stress corrosion cracking (SSCC) resistance due to localized corrosion, which is influenced by crystal plane orientation, and existing methods struggle to stably achieve high SSCC resistance while maintaining sufficient tensile strength.

Method used

A steel pipe with a bainite structure 0.25 mm below the surface, having a crystal plane orientation of {110} within 15° and an area ratio of 30% or less, is manufactured using a specific composition and controlled rolling and cooling processes to suppress local corrosion and enhance SSCC resistance.

Benefits of technology

The method stably achieves excellent SSCC resistance and high tensile strength of 520 MPa or more, suitable for line pipes in sour environments, by controlling the microstructure and composition of the steel pipe, thereby improving its durability and performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JP2024018028_21112024_PF_FP_ABST
    Figure JP2024018028_21112024_PF_FP_ABST
Patent Text Reader

Abstract

Provided are: a steel pipe stably having excellent SSCC resistance; and a method for manufacturing the same. This steel pipe has a component composition containing, in mass%, 0.020-0.080% of C, 0.50-1.80% of Mn, 0.01-0.50% of Mo, 0.0010-0.0080% of N, 0.01-0.50% of Si, 0.015% or less of P, 0.0015% or less of S, 0.010-0.080% of Al, and 0.0005-0.0050% of Ca, the remaining portion being Fe and unavoidable impurities. The structure at a position 0.25 mm outward in the pipe radial direction from the inner circumferential surface of the steel pipe is a bainite structure. The area proportion of bainite having a plane direction in which the crystal plane direction / {110 / } is oriented within 15° in the bainite structure is 30.0% or less.
Need to check novelty before this filing date? Find Prior Art

Description

Steel pipe and its manufacturing method

[0001] The present invention relates to a steel pipe suitable for use as a line pipe for transporting crude oil or natural gas, particularly to a steel pipe having excellent resistance to sulfide stress corrosion cracking (SSCC resistance) and suitable for use in sour environments containing hydrogen sulfide. The present invention also relates to a method for manufacturing the steel pipe.

[0002] In general, steel pipes are produced by forming steel plates produced by a plate mill or a hot rolling mill into steel pipes by UOE forming, press bending, roll forming, or the like.

[0003] Steel pipes for pipelines (line pipes) used to transport oil and natural gas are required to have various strengths, toughness, and weldability depending on the environment in which they are used. 2 Line pipes used in sour environments of petroleum or natural gas containing sulfur (S) are required to have properties capable of suppressing hydrogen induced cracking (HIC) and sulfide stress corrosion cracking (SSCC), i.e., sour resistance.

[0004] HIC occurs when hydrogen ions produced by corrosion reactions are adsorbed onto the steel surface, penetrate into the steel as atomic hydrogen, and then diffuse and accumulate around non-metallic inclusions such as MnS and hard second-phase structures in the steel, becoming molecular hydrogen, which then causes cracks due to the internal pressure. HIC is a problem in linepipes, which have a relatively low level of strength compared to oil country tubular goods, and many countermeasures have been disclosed.

[0005] On the other hand, SSCC is known to occur in the high hardness region of welds in oil country tubular goods and line pipes, and has generally not been considered a major problem in line pipes with relatively low hardness. However, it has been found that in line pipes with relatively high hardness, SSCC may occur due to localized corrosion in the base metal. Therefore, it is considered important to suppress localized corrosion in the base metal and improve SSCC resistance in line pipes used in sour environments.

[0006] Typically, the so-called TMCP (Thermo-Mechanical Control Process) technology, which combines controlled rolling and controlled cooling, is applied to the production of high-strength steel plates for line pipes. Increasing the cooling rate during controlled cooling is effective for increasing the strength of steel plates using this TMCP technology. However, when controlled cooling is performed at a high cooling rate, the surface layer of the steel plate is rapidly cooled, resulting in a higher hardness in the surface layer compared to the interior of the steel plate. Furthermore, in the case of steel pipes, work hardening occurs when the steel plate is formed into a tubular shape, which increases the hardness of the surface layer of the steel pipe, resulting in a decrease in SSCC resistance.

[0007] In order to solve the above problem, for example, Patent Document 1 discloses a method for forming a steel structure at a depth of 0.25 mm below the surface of a steel sheet, in which the dislocation density is 1.0 × 10 14 ~7.0 x 10 14 (m -2 This publication discloses a high-strength steel plate for sour-resistant line pipes having a tensile strength of 520 MPa or more and improved SSCC resistance by using a bainite structure of 1000 MPa or more and controlling the variation in Vickers hardness.

[0008] Furthermore, Patent Document 2 discloses a high-strength steel plate for sour-resistant line pipes having a tensile strength of 520 MPa or more, in which the steel structure at a depth of 0.25 mm below the surface of the steel plate is a bainite structure, and the area ratio of crystal grains in the bainite having a KAM (Kernel Average Misorientation) value of 0.4 or more is set to 50% or less, thereby improving SSCC resistance.

[0009] International Publication No. 2020 / 067209 International Publication No. 2021 / 020220

[0010] The steel pipe manufactured using the steel plate in which the variations in dislocation density and hardness are controlled as described in Patent Document 1 has excellent SSCC resistance. Although the steel pipe thus obtained has sufficient SSCC resistance, there is room for improvement in that the property cannot be stably obtained.

[0011] Furthermore, a steel pipe manufactured using a steel plate in which the KAM value is controlled in the bainite structure 0.25 mm below the surface of the steel plate, as described in Patent Document 2, has excellent SSCC resistance. Although the steel pipe thus obtained has sufficient SSCC resistance, there is room for improvement in that the property cannot be stably obtained.

[0012] The present invention has been made in view of the above circumstances, and aims to provide a high-strength steel pipe having stable excellent SSCC resistance and a method for manufacturing the same. Here, "high strength" means a tensile strength of 520 MPa or more.

[0013] In order to solve the above problems, the present inventors conducted extensive research on the microstructure of the inner surface of a steel pipe before and after evaluating SSCC resistance, as well as on the manufacturing method of the steel pipe, and have obtained the following findings. [1] SSCC initiates from localized corrosion. Furthermore, crystal plane orientation significantly affects localized corrosion. Therefore, it is important to control the crystal plane orientation of the structure of the extreme surface layer of the inner surface of the steel pipe, which is exposed to a sour environment, and to suppress localized corrosion, which is the initiation point of SSCC. [2] In order to consistently obtain excellent SSCC resistance, it is important to control the area fraction of bainite having a crystal plane orientation of {110} within 15° of the structure of the extreme surface layer of the inner surface of the steel pipe, specifically, the bainite structure 0.25 mm below the steel plate surface, to 30% or less. [3] In order to achieve the above-mentioned microstructure, it is important to appropriately control the total reduction during rolling and the cooling rate after rolling when manufacturing a steel plate for a steel pipe.

[0014] The present invention was made based on the above findings and further investigations, and the gist of the present invention is as follows: 1. A steel pipe having a chemical composition containing, by mass%, C: 0.020 to 0.080%, Mn: 0.50 to 1.80%, Mo: 0.01 to 0.50%, N: 0.0010 to 0.0080%, Si: 0.01 to 0.50%, P: 0.015% or less, S: 0.0015% or less, Al: 0.010 to 0.080%, and Ca: 0.0005 to 0.0050%, with the balance being Fe and unavoidable impurities, wherein the steel pipe has a bainite structure at a position 0.25 mm radially outward from the inner peripheral surface of the steel pipe, and the area ratio of bainite in the bainite structure having a crystal plane orientation of {110} within 15° is 30.0% or less.

[0015] 2. The steel pipe according to 1 above, wherein the chemical composition further contains, in mass%, one or more elements selected from the group consisting of Cu: 0.30% or less, Ni: 0.10% or less, Cr: 0.50% or less, Nb: 0.1% or less, V: 0.1% or less, Ti: 0.1% or less, Zr: 0.02% or less, Mg: 0.02% or less, and REM: 0.02% or less.

[0016] 3. A steel material having the chemical composition described in 1 or 2 above is heated to a temperature of 1000°C or higher and 1300°C or lower, and then hot-rolled under the condition that the total reduction rate A in the austenite region is 95% or lower to obtain a hot-rolled steel sheet, and the hot-rolled steel sheet is subjected to a cooling start temperature: a steel sheet surface temperature (Ar 3 a cooling stop temperature: an average cooling rate B in a temperature range of 750°C to 550°C at a steel plate 0.25 mm below the surface of the steel plate within a temperature range of 550°C or less at a steel plate temperature 0.25 mm below the surface of the steel plate is 20 to 50°C / s, and F, defined by the following formula (1) regarding the total rolling reduction A and the average cooling rate B, satisfies 0 to 30.00, and the steel plate after cooling is made into a steel pipe. F = 3.35A + 0.03B - 286.27 ... (1)

[0017] According to the present invention, excellent SSCC resistance can be stably achieved in a steel pipe. Furthermore, according to the method for manufacturing a steel pipe of the present invention, a steel pipe having excellent SSCC resistance can be stably manufactured.

[0018] 1 is a diagram illustrating the crystal plane orientation in a bainite structure. FIG. 2 is a diagram illustrating a method for collecting SSCC test specimens in a steel pipe.

[0019] Hereinafter, embodiments of the present invention will be described in detail. Note that the following description shows examples of preferred embodiments of the present invention, and the present invention is not limited thereto.

[0020] [Steel Pipe] A steel pipe according to one embodiment of the present invention is manufactured using a steel plate having a specific chemical composition and mechanical properties. The steel pipe is characterized in that, after the steel plate is formed into a steel pipe, the innermost surface layer of the steel pipe has a specific microstructure. The reasons for limiting the chemical composition, mechanical properties, and microstructure are explained below. Since the steel pipe is manufactured using a steel plate, the chemical composition of the steel pipe is the same as that of the steel plate used.

[0021] [Composition] First, the appropriate range of the composition of the steel pipe, i.e., the steel plate, and the reasons for limiting it will be described. In the following description, "%" as a unit of content represents "mass %" unless otherwise specified.

[0022] In the chemical composition of the steel pipe according to the present invention, it is important to specify the C content, Mn content, Mo content and N content in order to obtain the strength and SSCC resistance required for the steel pipe.

[0023] C: 0.020 to 0.080% C is an element that contributes to improving the strength of steel plate. If the C content is less than 0.020%, sufficient strength cannot be ensured, so the C content is set to 0.020% or more. Preferably, the C content is set to 0.025% or more. On the other hand, if the C content exceeds 0.080%, the hardness of the surface layer and central segregation increases during accelerated cooling, resulting in deterioration of SSCC resistance and HIC resistance. In addition, the toughness of the steel plate also deteriorates. For this reason, the C content is set to 0.080% or less. Preferably, the C content is set to 0.070% or less.

[0024] Mn: 0.50 to 1.80% Mn is an element that contributes to improving the strength and toughness of steel plate. If the Mn content is less than 0.50%, the above-mentioned effects are not fully realized. Therefore, the Mn content is set to 0.50% or more. Preferably, the Mn content is set to 0.80% or more. On the other hand, if the Mn content exceeds 1.80%, the hardness of the surface layer and central segregation increases during accelerated cooling, resulting in deterioration of SSCC resistance and HIC resistance. Weldability also deteriorates. Therefore, the Mn content is set to 1.80% or less. Preferably, the Mn content is set to 1.70% or less.

[0025] Mo: 0.01 to 0.50% Mo is an element that contributes to improving the strength and toughness of steel plate and improving SSCC resistance. If the Mo content is less than 0.01%, the above-mentioned effects are not fully exhibited. Therefore, the Mo content is set to 0.01% or more. Preferably, the Mo content is set to 0.10% or more. On the other hand, if the Mo content is too high, the hardenability becomes excessive, which increases hardness and deteriorates SSCC resistance. In addition, weldability also deteriorates. Therefore, the Mo content is set to 0.50% or less. Preferably, the Mo content is set to 0.40% or less.

[0026] N: 0.0010 to 0.0080% N is an element that contributes to improving the strength of the steel plate, and for this purpose, the N content is 0.0010% or more. Preferably, the N content is 0.0015% or more. On the other hand, if the N content exceeds 0.0080%, the hardness of the surface layer and central segregation increases during accelerated cooling, resulting in deterioration of SSCC resistance and HIC resistance. In addition, the toughness of the steel plate also deteriorates. For this reason, the N content is set to 0.0080% or less. Preferably, the N content is set to 0.0070% or less.

[0027] In the steel pipe according to the present invention, it is important to control the contents of C, Mn, Mo, and N. Furthermore, since it is desirable for steel pipes used in sour environments to ensure HIC resistance and toughness, the composition is such that the following components are added to the above components.

[0028] Si: 0.01 to 0.50% Si is added for deoxidation, but if the Si content is less than 0.01%, the deoxidation effect is insufficient. Therefore, the Si content is set to 0.01% or more. Preferably, the Si content is set to 0.05% or more. On the other hand, if the Si content exceeds 0.50%, the toughness and weldability of the steel plate deteriorate. Therefore, the Si content is set to 0.50% or less. Preferably, the Si content is set to 0.45% or less.

[0029] P: 0.015% or less P is an inevitable impurity element that deteriorates weldability and increases the hardness of the center segregation, thereby deteriorating HIC resistance. This tendency becomes more pronounced when the P content exceeds 0.015%, so the P content is set to 0.015% or less. Preferably, the P content is set to 0.008% or less. Meanwhile, since it is desirable to reduce P as much as possible to obtain the above-mentioned effects, the lower limit of the P content is not particularly limited and may be 0%. However, excessive reduction leads to increased refining costs, so from the viewpoint of industrial production, the P content is preferably set to 0.001% or more.

[0030] S: 0.0015% or less S is an inevitable impurity element, and since it forms MnS inclusions in the steel sheet and deteriorates HIC resistance, a small amount is preferable, but an S content of up to 0.0015% is acceptable. Preferably, the S content is 0.0010% or less. On the other hand, since it is desirable to reduce S as much as possible to obtain the above-mentioned effects, the lower limit of the S content is not particularly limited and may be 0%. However, excessive reduction leads to an increase in refining costs, so from the viewpoint of industrial production, the S content is preferably 0.0002% or more.

[0031] Al: 0.010 to 0.080% Al is added as a deoxidizer, but if the Al content is less than 0.010%, the added effect is ineffective. Therefore, the Al content is set to 0.010% or more, and preferably, the Al content is set to 0.015% or more. On the other hand, if the Al content exceeds 0.080%, the cleanliness of the steel decreases and the toughness of the steel plate deteriorates, so the Al content is set to 0.080% or less. Preferably, the Al content is set to 0.070% or less.

[0032] Ca: 0.0005 to 0.0050% Ca is an element effective in improving HIC resistance by controlling the morphology of sulfide-based inclusions, but if the Ca content is less than 0.0005%, the effect of adding it is insufficient. For this reason, the Ca content is set to 0.0005% or more, preferably 0.0008% or more. On the other hand, if the Ca content exceeds 0.0050%, not only does the above-mentioned effect saturate, but the cleanliness of the steel sheet also decreases, resulting in a deterioration in HIC resistance, so the Ca content is set to 0.0050% or less, preferably 0.0045% or less.

[0033] A steel pipe according to one embodiment of the present invention has a composition containing the above elements, with the balance being Fe and unavoidable impurities.

[0034] In addition, the chemical composition of the steel pipe in another embodiment of the present invention may further contain one or more elements selected from the group consisting of Cu, Ni, Cr, Nb, V, Ti, Zr, Mg and REM, for the purpose of further improving the properties of the steel pipe.

[0035] Cu: 0.30% or less Cu is an element effective in improving the toughness and increasing the strength of steel plate. When Cu is added, the Cu content is preferably 0.05% or more to obtain the above effects. However, if the Cu content exceeds 0.30%, microcracks called Fischer cracks are likely to occur in an environment with a hydrogen sulfide partial pressure of less than 1 bar. Therefore, when Cu is added, the upper limit is set to 0.30%. Preferably, it is set to 0.20% or less.

[0036] Ni: 0.10% or less Ni is an element effective in improving the toughness and increasing the strength of steel plate. When Ni is added, the Ni content is preferably 0.01% or more to obtain the above effects. However, if the Ni content exceeds 0.10%, microcracks called Fischer cracks are likely to occur in an environment with a hydrogen sulfide partial pressure of less than 1 bar. Therefore, when Ni is added, the upper limit is set to 0.10%. Preferably, it is set to 0.02% or less.

[0037] Cr: 0.50% or less Like Mn, Cr is an effective element for obtaining sufficient strength in steel sheets even with low C content. When Cr is added, the Cr content is preferably 0.05% or more to obtain the above effect. However, if the Cr content exceeds 0.50%, the hardenability becomes excessive, which increases hardness and deteriorates SSCC resistance. Weldability also deteriorates. Therefore, when Cr is added, the upper limit is set to 0.50%.

[0038] Nb: 0.1% or less Nb is an element that can be added optionally to increase the strength and toughness of steel sheets. When Nb is added, the Nb content is preferably 0.005% or more to obtain the above-mentioned effect. However, if the Nb content exceeds 0.1%, the toughness of the welded portion deteriorates. Therefore, when Nb is added, the upper limit is set to 0.1%.

[0039] V: 0.1% or less Like Nb, V is an element that can be added optionally to increase the strength and toughness of steel sheets. When V is added, the V content is preferably 0.005% or more to obtain the above-mentioned effect. However, if the V content exceeds 0.1%, the toughness of the welded portion deteriorates. Therefore, when V is added, the upper limit is set to 0.1%.

[0040] Ti: 0.1% or less Like Nb and V, Ti is an element that can be added optionally to increase the strength and toughness of steel sheets. When Ti is added, the Ti content is preferably 0.005% or more to obtain the above-mentioned effect. However, if the Ti content exceeds 0.1%, the toughness of the welded portion deteriorates. Therefore, when Ti is added, the upper limit is set to 0.1%.

[0041] Zr: 0.02% or less Zr is an element that can be added as needed to improve the toughness of steel sheets by refining crystal grains and to improve crack resistance by controlling the properties of inclusions. When Zr is added, the Zr content is preferably 0.0005% or more to obtain the above effects. However, when the Zr content exceeds 0.02%, the above effects saturate. Therefore, when Zr is added, the upper limit is set to 0.02%.

[0042] Mg: 0.02% or less Like Zr, Mg is an element that can be added as needed to improve the toughness of steel sheets by refining crystal grains and to improve crack resistance by controlling the properties of inclusions. When Mg is added, the Mg content is preferably 0.0005% or more to obtain the above effects. However, when the Mg content exceeds 0.02%, the above effects become saturated. Therefore, when Mg is added, the upper limit is set to 0.02%.

[0043] REM: 0.02% or less Like Zr and Mg, REM is an element that can be added optionally to improve the toughness of steel plate by refining crystal grains and to improve crack resistance by controlling the properties of inclusions. When REM is added, the REM content is preferably 0.0005% or more to obtain the above effects. However, when the REM content exceeds 0.02%, the above effects saturate. Therefore, when REM is added, the upper limit is set to 0.02%.

[0044] While the present disclosure discloses a technique for improving the SSCC resistance of steel pipes, it is preferable that sour gas resistance performance also satisfies HIC resistance along with SSCC resistance. To improve HIC resistance, it is preferable that the CP value calculated by the following formula (2) in the chemical composition of the steel pipe be 1.00 or less: CP = 4.46 [%C] + 2.37 [%Mn] / 6 + (1.74 [%Cu] + 1.7 [%Ni]) / 15 + (1.18 [%Cr] + 1.95 [%Mo] + 1.74 [%V]) / 5 + 22.36 [%P] (2) where [%X] in the formula (2) represents the content (mass%) of element X, and is set to 0 if the element is not present.

[0045] Here, the CP value is a formula devised to estimate the material quality of the center segregation region from the content of each alloy element. The higher the CP value defined by the above formula (2), the higher the concentration of elements in the center segregation region, and the higher the hardness of the center segregation region. Therefore, by setting the CP value calculated by the above formula (2) to 1.00 or less, it is possible to suppress the occurrence of cracks in the HIC test. Furthermore, since the lower the CP value, the lower the hardness of the center segregation region, so if even higher HIC resistance is required, the upper limit can be set to 0.95.

[0046] The balance other than the above elements consists of Fe and unavoidable impurities. However, other trace elements may be contained as long as they do not impair the effects of the present invention. For example, O is an element that is inevitably contained in steel sheet, but its content is permissible in the present invention as long as it is 0.0050% or less, preferably 0.0040% or less.

[0047] [Microstructure] Next, the microstructure of the steel pipe of the present invention will be described. In one embodiment of the present invention, the microstructure at a position 0.25 mm radially outward from the inner peripheral surface of the steel pipe (hereinafter also referred to as 0.25 mm below the inner surface of the steel pipe) is a bainite structure mainly composed of bainite. Here, "mainly composed of bainite" means that the area ratio of bainite is 95% or more.

[0048] Bainite structure: In order to maintain a constant maximum hardness at 0.25 mm below the surface of the inner surface of the steel pipe and improve SSCC resistance, the microstructure at 0.25 mm below the surface of the inner surface of the steel pipe needs to be a bainite structure. In particular, if hard phases such as martensite or island martensite (MA) are formed in the surface layer from the surface of the inner surface of the steel pipe to a depth of 0.25 mm, the hardness of the surface layer on the inner surface of the steel pipe increases, increasing the hardness variation in the surface layer on the inner surface of the steel pipe and hindering material uniformity. Therefore, the microstructure of the surface layer on the inner surface of the steel pipe needs to be a bainite structure.

[0049] Here, the bainite structure includes structures called lath bainite or granular bainite, which contribute to transformation strengthening and transform during or after accelerated cooling. The presence of heterogeneous structures such as ferrite, martensite, pearlite, island martensite, and retained austenite in the bainite structure can result in reduced strength and toughness of the steel pipe, as well as increased surface hardness. Therefore, the smaller the area fraction of structures other than bainite, the better. However, if the area fraction of structures other than bainite is sufficiently low, their effects can be ignored, and a certain amount is acceptable. Specifically, the total area fraction of structures other than bainite (ferrite, martensite, pearlite, island martensite, retained austenite, etc.) is preferably less than 5%.

[0050] Furthermore, it is essential that the area ratio of bainite having a crystal plane orientation of {110} within 15° in the bainite structure be 30% or less. The reason for controlling the microstructure in the surface layer region on the inner side of the steel pipe is that the inside of the steel pipe is in a sour environment and comes into contact with hydrogen sulfide. Also, the reason for controlling the microstructure 0.25 mm below the surface of the inner side of the steel pipe is that the crack depth at which the occurrence of SSCC is judged is at this 0.25 mm position.

[0051] Area fraction of bainite having a crystal plane orientation in which the {110} crystal plane orientation is within 15°: 30.0% or less The present inventors discovered that in a sour environment, the {110} crystal plane orientation of the bainite structure serves as the preferential dissolution plane and corrodes (localized corrosion). Furthermore, detailed studies were conducted, focusing on the crystal plane orientation of the bainite structure 0.25 mm below the surface of the inner surface of a steel pipe. Specifically, the inventors discovered that when the bainite structure is an aggregate of bainite with different crystal plane orientations on either side of a high-angle grain boundary with a misorientation of 15° or more, excellent SSCC resistance can be consistently achieved by setting the area fraction of bainite having a crystal plane orientation in which the {110} crystal plane orientation is within 15° of the {110} crystal plane orientation.

[0052] Here, for ease of understanding, "bainite having a plane orientation in which the crystal plane orientation {110} is oriented within 15°" will be explained with reference to Fig. 1, assuming that the inner peripheral surface (curved surface) of a steel pipe is a flat plate. That is, the above-mentioned bainite means bainite having a plane orientation in which an axis l perpendicular to the {110} plane is oriented within 15° with respect to an axis L perpendicular to the plate surface, as shown in Fig. 1. Note that, since the inner peripheral surface of a steel pipe is actually a curved surface, the above-mentioned axis L can be considered to be the normal to the above-mentioned inner peripheral surface.

[0053] It is believed that keeping the area fraction of bainite having the above-mentioned specific plane orientation to 30% or less will lead to the suppression of the initiation stage of localized corrosion, which is considered to be the starting point of SSCC. In other words, "bainite having a plane orientation in which the crystal plane orientation {110} is oriented within 15°" affects SSCC resistance, and by controlling the area fraction of this bainite to 30% or less, excellent SSCC resistance can be stably obtained, as shown in the examples described below. On the other hand, it has been found that conventional techniques that control the bainite area fraction by the proportion of crystal grains with a KAM value of 0.4 or more, or by controlling the dislocation density and hardness, sometimes fail to control the bainite area fraction to 30% or less, and in such cases, the desired SSCC resistance is not obtained.

[0054] [Tensile Strength of Steel Pipe] The tensile strength (TS) of the steel pipe according to the present invention is not particularly limited as long as the steel pipe can be manufactured. However, since SSCC resistance is less likely to be a problem in steel pipes with low tensile strength, the steel pipe according to the present invention preferably has a tensile strength of 520 MPa or more. In particular, steel pipes having a high tensile strength of 520 MPa or more can be suitably used for applications such as line pipes.

[0055] [Method of manufacturing steel pipe] Next, a method of manufacturing a steel pipe according to one embodiment of the present invention will be described. The steel pipe of the present invention can be manufactured by heating a steel material having the above-described chemical composition, hot-rolling the material to form a hot-rolled steel sheet, subjecting the hot-rolled steel sheet to controlled cooling under predetermined conditions to form a steel sheet, and then forming the steel sheet into a steel pipe.

[0056] Steel Material Any form of material can be used as the steel material. The steel material may be, for example, a steel slab. The method for producing the steel material is not particularly limited, but the steel material can be produced, for example, by melting molten steel having the above-mentioned composition by a conventional method and casting it. The melting can be carried out by any method, such as a converter, an electric furnace, or an induction furnace. Furthermore, from the viewpoint of productivity, the casting is preferably carried out by a continuous casting method, but may also be carried out by an ingot casting method.

[0057] Heating temperature: 1000° C. or higher and 1300° C. or lower The steel material is heated prior to hot rolling. The heating may be performed after the steel material obtained by a method such as casting has been cooled once, or the obtained steel material may be directly subjected to the heating without being cooled.

[0058] If the heating temperature of the steel material is less than 1000°C, the solid solution of carbides is insufficient and the strength required for a steel plate cannot be obtained. Therefore, the heating temperature is set to 1000°C or higher. On the other hand, if the heating temperature exceeds 1300°C, excessive energy is required, resulting in a decrease in productivity. Furthermore, the toughness of the steel plate also deteriorates. Therefore, the heating temperature is set to 1300°C or lower. Note that the heating temperature is the temperature inside the heating furnace, and the steel material is heated to the heating temperature all the way to the center.

[0059] - Total reduction in the austenite region: 95% or less Next, the heated steel material is hot-rolled to obtain a hot-rolled steel sheet. At that time, in order to produce a steel pipe that satisfies the conditions of the present invention, the total reduction in the austenite region (Ar) in the hot rolling is 3The total reduction in the austenite region (above the transformation point) is set to 95% or less. If the total reduction exceeds 95%, austenite with a crystal plane orientation of {111} develops on the sheet surface due to shear deformation, and a bainite texture with a crystal plane orientation of {110} develops after hot rolling and cooling. As a result, it becomes impossible to suppress the area fraction of bainite in which the crystal plane orientation of {110} is oriented within 15° in the bainite structure to 30% or less, which deteriorates the SSCC resistance of the steel pipe. For this reason, the total reduction is set to 95% or less. On the other hand, in order to ensure toughness, it is desirable to set the total reduction in the austenite region to 60% or more. Furthermore, from the viewpoint of improving strength and HIC resistance, hot rolling is preferably performed in the austenite region.

[0060] - Rolling end temperature In order to obtain high toughness as a steel pipe, the lower the hot rolling end temperature, the better, but on the other hand, the rolling efficiency decreases. Therefore, the rolling end temperature needs to be set taking into consideration the toughness and rolling efficiency required for the steel pipe. From the viewpoint of improving the strength and HIC resistance of the steel pipe, the rolling end temperature is set to a value lower than that of Ar 3 The rolling end temperature is the surface temperature of the steel material, and the surface temperature can be measured with a radiation thermometer or the like.

[0061] Here, Ar 3 The transformation point means the temperature at which ferrite transformation begins during cooling, and is calculated according to the following formula (3): 3 (°C) = 910 - 273 [% C] - 74 [% Mn] - 56 [% Ni] - 16 [% Cr] - 9 [% Mo] - 5 [% Cu] (3) where [% X] in the above formula (3) represents the content (mass%) of element X, and is set to 0 if the element is not contained.

[0062] Cooling: Next, the hot-rolled steel sheet after hot rolling is cooled in a temperature range from a cooling start temperature to a cooling stop temperature, which will be described later. Cooling start temperature: The surface temperature of the steel sheet (Ar 3 If the cooling start temperature is low, the amount of ferrite generated before cooling increases. 3If the temperature drop from the transformation point exceeds 10°C, ferrite will be generated in a volume fraction exceeding 5%, which will result in a significant decrease in the strength of the steel pipe and a deterioration in HIC resistance. 3 The cooling start temperature is set to a temperature equal to or lower than the rolling end temperature. The cooling start temperature is the surface temperature of the hot-rolled steel sheet, and can be measured using a radiation thermometer or the like.

[0063] Cooling rate: average cooling rate of 50°C / s or less from 750°C to 550°C at a steel plate temperature 0.25 mm below the surface. In order to increase the strength of the steel plate, i.e., the steel pipe, while reducing hardness variation within the steel plate and improving material uniformity, it is important to control the cooling rate of the surface layer of the steel plate. In particular, to obtain the desired microstructure 0.25 mm below the surface of the steel plate, it is necessary to control the average cooling rate of 50°C / s or less from 750°C to 550°C at a steel plate temperature 0.25 mm below the surface of the steel plate.

[0064] By making the average cooling rate as slow as possible, it is possible to create bainite having a crystal plane orientation where the {110} crystal plane orientation is not within 15°. Furthermore, as the average cooling rate is slowed, the maximum hardness can be reduced, thereby improving SSCC resistance. If the average cooling rate exceeds 50°C / s, the area fraction of bainite having a crystal plane orientation where the {110} crystal plane orientation is within 15° increases, and the maximum HV0.5 hardness at 0.25 mm below the steel sheet surface exceeds 230. Furthermore, the transformation texture develops, and the area fraction of bainite having a crystal plane orientation where the {110} crystal plane orientation is within 15° increases, resulting in a deterioration of SSCC resistance after the steel sheet is made into a pipe. Therefore, the average cooling rate is set to 50°C / s or less, preferably 30°C / s or less. Although there is no particular limitation on the lower limit of the average cooling rate, if the average cooling rate is too low, ferrite and pearlite are generated, resulting in a steel sheet, i.e., a steel pipe, having insufficient strength. From the viewpoint of preventing the insufficiency of strength, the average cooling rate is preferably 20°C / s or more.

[0065] F (= 3.35A + 0.03B - 286.27): 30.00 or less As described above, in order to achieve an area fraction of 30.0% or less for bainite having a crystal plane orientation in which the {110} crystal plane orientation is within 15° at 0.25 mm below the surface of the steel sheet, the total rolling reduction in the austenite region and the average cooling rate from 750°C to 550°C at the steel sheet temperature 0.25 mm below the surface of the steel sheet are important. The inventors conducted further studies and found that it is not sufficient to simply control the total rolling reduction and the average cooling rate within predetermined ranges, and that when the total rolling reduction is A (%), the average cooling rate is B (°C / s), and the area fraction of bainite having a crystal plane orientation in which the {110} crystal plane orientation is within 15° F (%), F can be expressed by the following formula (1): If F exceeds 30.00, the area ratio of bainite having a plane orientation in which the sheet surface {110} is oriented within 15° exceeds 30.0%, and SSCC resistance deteriorates. On the other hand, the lower limit of F may be 0 or more. F = 3.35A + 0.03B - 286.27 (1)

[0066] Cooling stop temperature: 550°C or less at the steel sheet temperature 0.25 mm below the steel sheet surface. The hot-rolled steel sheet after hot rolling is cooled from the cooling start temperature to the cooling stop temperature by controlled cooling. Here, by setting the cooling stop temperature to 550°C or less, which is the temperature range of bainite transformation, it is possible to generate a bainite phase. If the cooling stop temperature exceeds 550°C, the bainite transformation becomes incomplete, and sufficient strength cannot be obtained. Therefore, the cooling stop temperature is set to 550°C or less. Furthermore, if the cooling stop temperature is less than 250°C, the dislocation density increases, which significantly increases the hardness of the surface layer when the steel sheet is made into a pipe, and there is a risk of deterioration in SSCC resistance. Therefore, it is preferable that the cooling stop temperature be 250°C or more.

[0067] Furthermore, when cooling to a steel sheet temperature of 550°C or less at a point 0.25 mm below the steel sheet surface, if the cooling rate is slow, the cooling will not occur in a stable nucleate boiling state, which may result in variations in hardness at the very surface layer of the steel sheet, a higher maximum Vickers hardness value, and a deterioration in SSCC resistance. Therefore, the average cooling rate from 550°C at a steel sheet temperature 0.25 mm below the steel sheet surface to the cooling stop temperature is preferably 150°C / s or more. A more preferred average cooling rate is 170°C / s or more. There is no particular upper limit to the average cooling rate, but due to equipment constraints, it is preferably 250°C / s or less.

[0068] Although the steel sheet temperature at 0.25 mm below the surface of the steel sheet cannot be physically measured directly, it can be determined in real time from the results of calculating the temperature distribution within the sheet thickness cross section by differential calculation using, for example, a process computer based on the surface temperature of the hot-rolled steel sheet at the start of cooling measured with a radiation thermometer and the surface temperature of the hot-rolled steel sheet at the target time of cooling stop. The temperature at 0.25 mm below the steel sheet surface in the temperature distribution is referred to as "the steel sheet temperature at 0.25 mm below the steel sheet surface" in this specification.

[0069] Steel Pipe Next, the cooled steel plate is made into a steel pipe. Methods for making steel pipe from steel plate include, for example, forming the steel plate into a tubular shape by press bending, roll forming, UOE forming, etc., and then welding the butt joints. By using the above-mentioned manufacturing method, it is possible to manufacture steel pipes with excellent material uniformity within the steel plate that are suitable for transporting crude oil and natural gas, such as UOE steel pipes, electric resistance welded steel pipes, and spiral steel pipes.

[0070] For example, UOE steel pipes are manufactured by groove-forming the ends of steel plates, forming them into a steel pipe shape using a C press, a U press, or an O press, then seam-welding the butt joints by internal welding and external welding, and, if necessary, undergoing a pipe expansion process. Any welding method may be used as long as it can provide sufficient joint strength and joint toughness, but submerged arc welding is preferred from the viewpoints of excellent weld quality and manufacturing efficiency.

[0071] The functions and effects of the present invention will be described below using examples. It should be noted that the present invention is not limited to the following examples. A steel slab having the chemical composition shown in Table 1 was produced as a steel material by continuous casting. The obtained steel slab was heated to the heating temperature shown in Table 2 and then hot-rolled at the total reduction in the austenite region shown in Table 2 to produce a hot-rolled steel sheet having the thickness shown in Table 2. The obtained hot-rolled steel sheet was then subjected to controlled cooling using a water-cooled controlled cooling device under the conditions shown in Table 2 to produce a steel sheet. The end of the obtained steel sheet was then beveled and formed into a steel pipe shape using a C press, a U press, and an O press. The inner and outer butt joints were seam-welded by submerged arc welding, and the steel pipe was then produced through a pipe expansion process. Since actual pipe products were to be coated on the outside, an aging heat treatment was performed at 250°C for 1 hour to simulate the external coating process.

[0072]

[0073] (Measurement of Crystal Plane Orientation) In order to evaluate the microstructure of the steel pipe manufactured by the above-mentioned manufacturing method, measurements were performed by EBSD (Electron Backscatter Diffraction). That is, a test piece was taken from the inside of the steel pipe, and after removing the scale from the inside surface, mirror polishing and electrolytic polishing were performed so that the measurement surface was located at a depth of 0.25 mm from the surface after descaling. Next, using a scanning electron microscope, EBSD measurements were performed on the measurement surface at an acceleration voltage of 20 kV, a measurement area of ​​300 × 200 μm, and a step size of 0.2 μm. From the obtained measurement results, using EBSD analysis software, the area fraction of low-index planes {100} oriented within 15°, the area fraction of low-index planes {110} oriented within 15°, the area fraction of low-index planes {111} oriented within 15°, and the area fraction of high-index planes other than the above were calculated. From these calculation results, the area ratio where the crystal plane orientation {110} is oriented within 15° was calculated. The results are shown in Table 2.

[0074] As shown in Table 2, the steel pipes of the invention examples and comparative examples, except for Nos. 41 and 42, had a microstructure mainly composed of bainite. Here, "mainly composed of bainite" means that 95% or more of bainite was present. On the other hand, Nos. 41 and 42 had a microstructure mainly composed of bainite.

[0075] (Evaluation of SSCC Resistance) The SSCC resistance of steel pipes manufactured using the above-described manufacturing method was evaluated. As shown in Figure 2, SSCC test specimens measuring 5 x 25 x 125 mm were taken from the inner surface of the steel pipe. The inner surface of the steel pipe, which was the test surface, was left with black scale to preserve the state of the outermost layer. A four-point bending SSCC test was performed on the taken SSCC test specimens, applying a stress of 90% of the actual yield strength of each steel pipe, using NACE Standard TM0177 Solution B at a hydrogen sulfide partial pressure of 0.15 bar and a carbon dioxide partial pressure of 0.75 bar. If no cracks were observed after 720 hours of immersion, the SSCC resistance was judged to be "good," and if cracks were observed, the SSCC resistance was judged to be "poor." Here, "cracks" refers to cracks of 0.25 mm or more at the center of the test specimen in the longitudinal direction after the four-point bending test. The evaluation results of the SSCC resistance are also shown in Table 2.

[0076] (Measurement of Tensile Strength) The full-thickness test pieces in the circumferential direction of the steel pipes described above were used as tensile test pieces, and a tensile test was carried out in accordance with ASTM A370 to measure the tensile strength. The tensile strengths of the obtained steel pipes are also shown in Table 2.

[0077]

[0078] As shown in Table 2, all of the invention examples whose component compositions and manufacturing conditions satisfied the appropriate ranges of the present invention had high strength and good SSCC resistance.

[0079] In contrast, all of the comparative examples, whose composition and / or manufacturing conditions were outside the range of the present invention, exhibited poor tensile strength or SSCC resistance. Specifically, Nos. 3, 4, 11, 12, 21, 22, 25, and 28 had composition outside the range of the present invention, and thus exhibited poor tensile strength or SSCC resistance. Furthermore, No. 36, although its composition was within the range, had a total reduction in the austenite region exceeding 95% and an F value exceeding 30.00, resulting in an area fraction of bainite with a crystal plane orientation of {110} within 15° exceeding 30.0%, and thus exhibited poor SSCC resistance. No. 43, although its composition was within the range, had an average cooling rate of 50°C / s or higher and an F value exceeding 30.00, resulting in an area fraction of bainite with a crystal plane orientation of {110} within 15° exceeding 30.0%, and thus exhibited poor SSCC resistance. In addition, in No. 41, the cooling start temperature is the steel plate surface temperature (Ar 3 In No. 42, the cooling stop temperature was above 550°C at the steel plate temperature 0.25 mm below the surface of the steel plate, and the structure was less than 95% bainite, which was not a structure mainly composed of bainite, resulting in low tensile strength.

[0080] As can be seen from the results shown in Table 2, the steel pipes of the present invention were excellent in both the tensile strength of the steel plate and the SSCC resistance of the steel pipes. On the other hand, the steel pipes of the comparative examples outside the range of the present invention were low in tensile strength or had poor SSCC resistance.

Claims

1. A steel pipe having a composition containing, by mass%, the following: C: 0.020-0.080%, Mn: 0.50-1.80%, Mo: 0.01-0.50%, N: 0.0010-0.0080%, Si: 0.01-0.50%, P: 0.015% or less, S: 0.0015% or less, Al: 0.010-0.080%, Ca: 0.0005-0.0050%, with the balance being Fe and unavoidable impurities, wherein the structure at a position 0.25 mm radially outward from the inner surface of the steel pipe is a bainite structure, and the area ratio of bainite in the bainite structure having a crystal plane orientation of {110} within 15° is 30.0% or less.

2. The steel pipe according to claim 1, wherein the chemical composition further contains, by mass%, one or more selected from the group consisting of Cu: 0.30% or less, Ni: 0.10% or less, Cr: 0.50% or less, Nb: 0.1% or less, V: 0.1% or less, Ti: 0.1% or less, Zr: 0.02% or less, Mg: 0.02% or less and REM: 0.02% or less.

3. A steel material having the composition according to claim 1 or 2 is heated to a temperature of 1000°C or higher and 1300°C or lower, and then hot-rolled under conditions of a total rolling reduction A in the austenite region of 95% or less to obtain a hot-rolled steel sheet, and the hot-rolled steel sheet is cooled at a cooling start temperature: steel sheet surface temperature (Ar 3 -10°C) or more, and cooling stop temperature: within a temperature range of 550°C or less at a steel plate temperature 0.25 mm below the steel plate surface, an average cooling rate B in a temperature range of 750°C to 550°C at a steel plate temperature 0.25 mm below the steel plate surface is 50°C / s or less, and F, defined by the following formula (1) regarding the total rolling reduction A and the average cooling rate B, satisfies 0 to 30.00, is cooled to obtain a steel plate, and the cooled steel plate is used as a steel pipe. F=3.35A+0.03B-286.27 ... (1)

Citation Information

Patent Citations

  • High-strength steel sheet for sour resistant line pipe, manufacturing method thereof, and high-strength steel pipe made using high-strength steel sheet for sour resistant line pipe

    WO2021020220A1

  • Low yield ratio, high toughness steel sheet and method for manufacturing the same

    JP2014520208A

  • Steel material excellent in fatigue crack propagation property, manufacturing method therefor, and determination method of steel material excellent in fatigue crack propagation property

    JP2015127444A

  • High-strength steel plate for sour-resistant line pipe, its manufacturing method, and high-strength steel pipe using high-strength steel plate for sour-resistant line pipe

    JP7272442B2

  • High-strength steel plate for sour resistant line pipe, method for manufacturing same, and high-strength steel pipe using high-strength steel plate for sour resistant line pipe

    WO2018179512A1