Method for manufacturing separator, and separator manufactured thereby
The method of manufacturing a lithium secondary battery separator using polyolefin and a pore-forming agent, with specific stretching and heat treatment, addresses the balance of mechanical strength and heat resistance, improving battery performance and lifespan by reducing thermal contraction and maintaining air permeability.
Patent Information
- Application Number
- PCT/KR2024/002161
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-05-16
- Filing Date
- 2024-02-20
- Publication Date
- 2024-11-21
AI Technical Summary
Lithium secondary battery separators face challenges in balancing mechanical strength, processability, heat resistance, and breathability, particularly with ultra-high molecular weight polyethylene, which affects battery capacity and lifespan due to high heat shrinkage and reduced ion movement paths.
A method involving processing a composition of polyolefin and a pore-forming agent to create a porous membrane through sequential biaxial stretching and heat setting, followed by applying a functional layer to achieve specific stretching ratios and thermal contraction rates, enhancing puncture strength and heat resistance while maintaining breathability.
The method results in a separator with improved processability, heat resistance, and puncture strength, reducing thermal contraction and maintaining air permeability, thus enhancing the performance and lifespan of lithium secondary batteries.
Smart Images

Figure 000001 
Figure 000002 
Figure 000003
Abstract
Description
Method for manufacturing a separation membrane and a separation membrane manufactured using the same
[0001] The present invention relates to a method for manufacturing a separation membrane and a separation membrane manufactured using the same.
[0002] Lithium secondary batteries are widely used as power sources for various electrical products that require miniaturization and lightweighting, such as smartphones, laptops, and tablet PCs. As their application areas expand to include smart grids and medium- to large-sized batteries for electric vehicles, there is a growing demand for the development of lithium secondary batteries with large capacity, long lifespan, and high stability.
[0003] Recently, thinning separators has emerged as a technological challenge to increase the capacity of lithium secondary batteries. However, this thinning entails a decrease in mechanical strength, so a balanced approach is necessary. To this end, separators utilizing resins with higher weight-average molecular weights than general-purpose polyethylene, such as ultra-high molecular weight polyethylene, are continuously being developed.
[0004] Ultra-high molecular weight polyethylene (UHMWPE) typically refers to polyethylene with a weight-average molecular weight of 1,000,000 or more. According to Japanese Patent Laid-Open No. 60-242035 and other publications, UHMWPE is known to have superior mechanical strength, wear resistance, uniformity, self-lubrication, and chemical resistance compared to general-purpose polyethylene, such as high-density polyethylene and low-density polyethylene.
[0005] However, ultra-high molecular weight polyethylene has a problem in that it is difficult to process due to its low flowability even in a completely molten state due to its high molecular weight, and the heat resistance of the manufactured separator decreases, such as an increase in the heat shrinkage rate at high temperatures (150°C).
[0006] Meanwhile, to improve the heat resistance of the separator, a separator coated with ceramic particles on the surface of a porous support, so-called ceramic-coated separators, have been proposed. However, the ceramic-coated separator still has significant technical challenges with regard to breathability. That is, when a heat-resistant layer containing ceramic particles is coated on the surface of the porous support, the heat resistance of the separator is improved, but the heat-resistant layer closes the pores formed in the porous support, thereby reducing the breathability of the separator, and thus the ion transport path between the positive and negative electrodes is reduced, resulting in a significant deterioration in the charge and discharge performance of the battery.
[0007] An attempt was made to improve the adhesion to the electrode and extend the life of the battery by additionally forming an adhesive layer having adhesion to the electrode on the surface of the porous support and / or the surface of the heat-resistant layer.
[0008] A separator coated with a functional layer, such as a heat-resistant layer or an adhesive layer, is generally manufactured by applying a composition for forming the functional layer to one or both sides of the porous support while moving the porous support at a constant speed, and then drying the composition. However, when the porous support includes or is made of ultra-high molecular weight polyethylene, there is a problem in that the heat shrinkage rate of the porous support further increases due to the heat applied to the separator during drying to form the functional layer.
[0009] The present invention is intended to solve the problems of the prior art described above, and the purpose of the present invention is to provide a method for manufacturing a separation membrane capable of achieving and improving processability, heat resistance, and puncture strength in a balanced manner, and a separation membrane manufactured using the same.
[0010] One aspect of the present invention provides a method for manufacturing a separation membrane, comprising the steps of: (a) processing a composition comprising polyolefin and a pore-forming agent to obtain a base sheet; (b) stretching the base sheet in a machined direction (MD) and a transverse direction (TD) and removing the pore-forming agent to obtain a porous membrane; and (c) stretching the porous membrane in a transverse direction (TD) and heat-setting it; and satisfying the conditions (1) to (3) below.
[0011] (1) 7 ≤ Mb ≤ 8, (2) 0< Mb / Tb <1, (3) 0 < Mb / (Tb*Tc) <0.5,
[0012] In the above (1) to (3), Mb and Tb are the elongation ratios of the base sheet along the longitudinal direction (MD) and the transverse direction (TD), respectively, in the above step (b), and Tc is the elongation ratio of the porous membrane along the transverse direction (TD) in the above step (c).
[0013] In one embodiment, the weight average molecular weight (Mw) of the polyolefin may be 1,000,000 to 4,000,000.
[0014] In one embodiment, the polyolefin may include one selected from the group consisting of polyethylene, polypropylene, polybutylene, polymethylpentene, ethylene vinyl acetate, ethylene butylacrylate, ethylene ethyl acrylate, and combinations or copolymers of two or more thereof.
[0015] In one embodiment, the Tc may be 1.5 to 2.0.
[0016] In one embodiment, the ratio of Mb to Tc (Mb / Tc) may be 3.0 to 5.0.
[0017] In one embodiment, the pore forming agent may be a paraffin oil having a kinematic viscosity of 50 to 100 cSt at 40°C.
[0018] In one embodiment, the thickness of the base sheet obtained in step (a) may be 1,000 to 1,500 μm, the thickness of the porous film obtained in step (c) may be 10 μm or less, and the puncture strength may be 500 gf or more.
[0019] In one embodiment, after step (c), the method may further include a step (d) of forming a functional layer by applying a coating solution containing a binder and a solvent to at least one surface of the porous film and drying the coating solution.
[0020] In one embodiment, the binder is polyvinylidene fluoride, polyvinylidene fluoride-hexafluoropropylene, polyvinylidene fluoride-trichloroethylene, polymethyl methacrylate, polyacrylonitrile, polyvinylpyrrolidone, polyvinylacetate, ethylene vinyl acetate, polyimide, polyethylene oxide, cellulose acetate, cellulose acetate butyrate, cellulose acetate propionate, cyanoethyl pullulan, cyanoethyl polyvinyl alcohol, cyanoethyl cellulose, hydroxyethyl cellulose, cyanoethyl sucrose, pullulan, carboxymethyl cellulose, polyvinyl alcohol, polyvinyl butyral, acrylonitrile-acrylic acid copolymer, ethylene-acrylic acid copolymer, styrene-butadiene copolymer, It may be one selected from the group consisting of alkyl acrylate-acrylonitrile copolymers, polyethylene glycol, acrylic rubber, and combinations of two or more thereof.
[0021] In one embodiment, the solvent may be one selected from the group consisting of methanol, ethanol, propanol, butanol, methoxyethanol, ethoxyethanol, lactone, acetonitrile, n-methyl-2-pyrrolidone (NMP), formic acid, nitromethane, acetic acid, dimethyl sulfoxide, water, and combinations of two or more thereof.
[0022] In one embodiment, the coating solution may further include one inorganic particle selected from the group consisting of SiO2, AlO(OH), Mg(OH)2, Al(OH)3, TiO2, BaTiO3, Li2O, LiF, LiOH, Li3N, BaO, Na2O, Li2CO3, CaCO3, LiAlO2, Al2O3, SiO, SnO, SnO2, PbO2, ZnO, P2O5, CuO, MoO, V2O5, B2O3, Si3N4, CeO2, Mn3O4, Sn2P2O7, Sn2B2O5, Sn2BPO6, and combinations of two or more thereof.
[0023] Another aspect of the present invention provides a separation membrane manufactured using the above method for manufacturing the separation membrane and satisfying the following conditions (i) to (iii).
[0024] (i) A longitudinal (MD) heat shrinkage of 5% or less at 150°C, (ii) A transverse (TD) heat shrinkage of 5% or less at 150°C, (iii) A ratio of the transverse (TD) heat shrinkage to the longitudinal (MD) heat shrinkage of 1.1 or less at 150°C.
[0025] A method for manufacturing a separation membrane according to one aspect of the present invention comprises the steps of: (a) processing a composition comprising polyolefin and a pore-forming agent to obtain a base sheet; (b) stretching the base sheet in a longitudinal direction (MD) and a transverse direction (TD) and removing the pore-forming agent to obtain a porous membrane; and (c) stretching the porous membrane in a transverse direction (TD) and heat-setting it; and by satisfying the conditions of (1) to (3) below, processability, heat resistance, and puncture strength can be implemented and improved in a balanced manner.
[0026] (1) 7 ≤ Mb ≤ 8, (2) 0< Mb / Tb <1, (3) 0 < Mb / (Tb*Tc) <0.5,
[0027] In the above (1) to (3), Mb and Tb are the elongation ratios of the base sheet along the longitudinal direction (MD) and the transverse direction (TD), respectively, in the above step (b), and Tc is the elongation ratio of the porous membrane along the transverse direction (TD) in the above step (c).
[0028] The effects of the present invention are not limited to the effects described above, and should be understood to include all effects that can be inferred from the detailed description of the present invention or the composition of the invention described in the claims.
[0029]
[0030] The present invention will be described below. However, the present invention can be implemented in various different forms and is therefore not limited to the embodiments described herein.
[0031] Throughout the specification, when a part is said to be "connected" to another part, this includes not only "directly connected" but also "indirectly connected" with other elements intervening. Furthermore, when a part is said to "include" a component, this does not exclude other components, but rather implies that the other components may be included, unless otherwise specifically stated.
[0032] One aspect of the present invention provides a method for manufacturing a separation membrane, comprising the steps of: (a) processing a composition comprising polyolefin and a pore-forming agent to obtain a base sheet; (b) stretching the base sheet in a machined direction (MD) and a transverse direction (TD) and removing the pore-forming agent to obtain a porous membrane; and (c) stretching the porous membrane in a transverse direction (TD) and heat-setting it; and satisfying the conditions (1) to (3) below.
[0033] (1) 7 ≤ Mb ≤ 8, (2) 0< Mb / Tb <1, (3) 0 < Mb / (Tb*Tc) <0.5,
[0034] In the above (1) to (3), Mb and Tb are the elongation ratios of the base sheet along the longitudinal direction (MD) and the transverse direction (TD), respectively, in the above step (b), and Tc is the elongation ratio of the porous membrane along the transverse direction (TD) in the above step (c).
[0035] In the above step (a), a composition including a polyolefin and a pore-forming agent can be extruded and discharged through a T-die to obtain a base sheet. The weight average molecular weight (Mw) of the polyolefin may be 1,000,000 to 4,000,000, preferably 1,500,000 to 3,000,000, more preferably 1,500,000 to 2,500,000, and the molecular weight distribution (Mw / Mn) may be 3 to 7. If the weight average molecular weight of the polyolefin is less than 1,000,000, the mechanical strength of the separator may be reduced, and if it exceeds 4,000,000, the heat shrinkage rate may excessively increase, thereby reducing the heat resistance. In addition, if the molecular weight distribution of the polyolefin is less than 3, the dispersibility with the pore-forming agent may be reduced, which may result in a decrease in the uniformity of the manufactured membrane, and if it is more than 7, the mechanical properties of the membrane may be reduced. The terms "weight average molecular weight" and "molecular weight distribution" used herein may mean values measured by gel permeation chromatography (GPC) using polystyrene as a standard sample according to the method described in the literature (Macromolecules, Vol. 34, No. 19, pp. 6812-6820 (2001), etc.).
[0036] The above polyolefin may include, but is not limited to, one selected from the group consisting of polyethylene, polypropylene, polybutylene, polymethylpentene, ethylene vinyl acetate, ethylene butylacrylate, ethylene ethyl acrylate, and combinations or copolymers of two or more thereof, preferably polyethylene and / or polypropylene, and more preferably polyethylene.
[0037] The above pore-forming agent may be one selected from the group consisting of paraffin oil, paraffin wax, mineral oil, solid paraffin, soybean oil, rapeseed oil, palm oil, coconut oil, di-2-ethylhexyl phthalate, dibutyl phthalate, diisononyl phthalate, diisodecyl phthalate, bis(2-propylheptyl) phthalate, naphthene oil, and combinations of two or more thereof, preferably paraffin oil, and more preferably paraffin oil having a kinematic viscosity of 50 to 100 cSt at 40°C, but is not limited thereto. The composition may comprise 10 to 50 wt%, preferably 20 to 40 wt%, of the polyolefin, and 50 to 90 wt%, preferably 60 to 80 wt%, of the pore-forming agent.
[0038] The thickness of the base sheet obtained in the above step (a) may be 1,000 to 1,500 μm, preferably 1,200 to 1,500 μm. If the composition includes an ultra-high molecular weight polyolefin, for example, an ultra-high molecular weight polyethylene having a weight average molecular weight of 2,000,000 or more, it is difficult to control the thickness of the base sheet to less than 1,000 μm through extrusion or casting, and if the thickness of the base sheet exceeds 1,500 μm, there is a problem that it is difficult to thin the separator even through subsequent stretching.
[0039] In the step (b), the base sheet can be stretched in the longitudinal direction (MD) and the transverse direction (TD), and the pore-forming agent can be removed to obtain a porous membrane. The stretching can be performed by sequential biaxial stretching in which the base sheet is stretched in the longitudinal direction (MD) at a preset stretching ratio and then stretched in the transverse direction (TD), or by simultaneous biaxial stretching in which the base sheet is simultaneously stretched in the longitudinal direction (MD) and the transverse direction (TD). The term "stretch ratio" used herein means the ratio of the longitudinal direction (MD) or transverse direction (TD) length of the base sheet after stretching to the longitudinal direction (MD) or transverse direction (TD) length before stretching, and can be interpreted as having the same meaning as stretch ratio, stretch ratio, etc.
[0040] The longitudinal (MD) stretching of the above base sheet can be performed using a roll stretching machine. The roll stretching machine is a device that stretches the base sheet along the transport direction of the base sheet in a process line, and the direction of stretching the base sheet by the roll stretching machine can be defined as the longitudinal direction (MD, mechanical direction). The roll stretching machine includes a plurality of rolls installed along the transport direction of the base sheet, and can stretch the base sheet along the longitudinal direction at a preset magnification by rotating the rolls located at the rear end faster than the rolls located at the front end.
[0041] The transverse direction (TD) stretching of the above base sheet can be performed using a tenter stretching machine. The tenter stretching machine is a device that stretches the base sheet in a direction perpendicular to the transport direction of the base sheet in a process line, and can stretch the base sheet along the transverse direction at a preset magnification by fixing the transverse ends of the base sheet with predetermined members such as chucks and clips and then spacing the members apart in the transverse direction.
[0042] The pore-forming agent can be selectively extracted and removed from the base sheet by applying a predetermined extraction solvent to the base sheet. The pore-forming agent can be extracted and removed by immersing the base sheet in an impregnation tank containing a solution containing the extraction solvent for a predetermined period of time.
[0043] The content of the pore-forming agent remaining on the surface and / or inside the porous film after extraction may be 1 wt% or less. The extraction solvent may be, for example, methyl ethyl ketone, hexane, dichloromethane, etc., but is not limited thereto. The time required for extraction and removal of the pore-forming agent may be determined by the thickness, porosity, etc. of the base sheet and / or the porous film, but when the thickness and porosity of the porous film are 1 to 10 μm and 30 to 70 vol%, respectively, it may be 10 minutes or less, preferably, 5 minutes or less.
[0044] In addition, the porous membrane from which the pore-forming agent has been extracted and removed may be heated to remove the extraction solvent remaining in the porous membrane. Some of the extraction solvent applied in step (b) may remain on the surface and / or inside the porous membrane. The remaining extraction solvent may deteriorate the subsequent process and the properties of the separation membrane manufactured thereby, so the extraction solvent remaining in the porous membrane may be removed by appropriately heating the porous membrane to a temperature higher than the boiling point of the extraction solvent.
[0045] In the above step (c), the porous membrane can be obtained by stretching it in the transverse direction (TD) and heat-setting it.
[0046] The above heat setting refers to a process of forcibly fixing the porous membrane, which is about to shrink, by applying heat to the porous membrane after stretching it in the transverse direction (TD) and then relaxing and fixing it, thereby removing residual stress. A high heat setting temperature is advantageous in reducing the thermal shrinkage rate of the membrane, but if the temperature is excessively high, the porous membrane may partially melt, closing the formed pores, which may reduce the air permeability.
[0047] The heat-setting temperature is preferably selected within a range where 10 to 30 wt% of the crystalline portion of the porous film melts. When the heat-setting temperature is selected within the above range, the problem of insufficient rearrangement of polyolefin molecules within the porous film, resulting in ineffective residual stress relief, and the problem of reduced air permeability due to partial melting and pore closure can be prevented. For example, the heat-setting temperature may be 120 to 140°C, preferably 123 to 135°C, and the heat-setting time may be 5 seconds to 1 minute.
[0048] In relation to the stretching performed in steps (b) and (c), the method for manufacturing the separation membrane can satisfy the following conditions (1) to (3).
[0049] (1) 7 ≤ Mb ≤ 8, (2) 0< Mb / Tb <1, (3) 0 < Mb / (Tb*Tc) <0.5,
[0050] In the above (1) to (3), Mb and Tb are the elongation ratios of the base sheet along the longitudinal direction (MD) and the transverse direction (TD), respectively, in the above step (b), and Tc is the elongation ratio of the porous membrane along the transverse direction (TD) in the above step (c).
[0051] The above condition (1) relates to the stretching ratio (Mb) of the base sheet along the longitudinal direction (MD) in the step (b), and the Mb may be 7 to 8, preferably 7 to 7.5. If the Mb is less than 7, the structural properties required for the porous membrane, such as pore size, porosity, and air permeability, may be reduced, and if it exceeds 8, the thermal shrinkage rate in the longitudinal direction (MD) of the separator may increase, thereby reducing heat resistance. In particular, when the Mb is adjusted to a preset range, it can be understood that the base sheet is relatively and substantially shrunk in the transverse direction (TD) while being stretched in the longitudinal direction (MD), and therefore, such shrinkage can contribute to reducing the residual stress accumulated in the base sheet and / or the porous membrane by subsequent stretching in the transverse direction (TD), thereby reducing the thermal shrinkage rate of the separator and improving heat resistance. In addition, when the heat resistance of the porous membrane is improved, the resistance to heat applied to the porous membrane during the coating and drying process for forming a functional layer on the surface of the porous membrane can also be improved, thereby preventing the membrane from being arbitrarily deformed and / or transformed.
[0052] The above condition (2) relates to the ratio of the stretching ratio along the longitudinal direction (MD) of the base sheet to the stretching ratio along the transverse direction (TD) of the base sheet in the step (b), and the ratio may be greater than 0 and less than 1, preferably, 0.5 to 0.95, more preferably, 0.7 to 0.9. Here, the Tb may be 8.0 to 10.0, preferably, 8.5 to 9.5. The Tb is the stretching ratio along the transverse direction (TD) during the biaxial stretching performed in the step (b), and by controlling the Tb to be smaller than the Mb, the residual stress accumulated in the base sheet due to the stretching in the transverse direction (TD) during the biaxial stretching can be reduced, thereby contributing to lowering the thermal shrinkage rate of the separator and improving the heat resistance. In addition, if the Tb is less than 0.5, the structural properties required for the porous membrane, such as pore size, porosity, pore orientation, and air permeability, may be reduced.
[0053] The above condition (3) relates to the ratio of the stretching ratio along the longitudinal direction (MD) of the base sheet in the step (b) to the total stretching ratio along the transverse direction (TD) throughout the entire process of manufacturing the separator, and the ratio may be greater than 0 and less than 0.5, preferably, 0.3 or more, and more preferably, 0.4 or more. Here, the Tc may be 1.5 to 2.0, preferably, 1.7 to 1.9. When the Mb / (Tb*Tc) is 0.5 or more, both the longitudinal direction (MD) and transverse direction (TD) heat shrinkage rates of the separator increase, and in particular, the transverse direction (TD) heat shrinkage rate rapidly increases, which may result in a decrease in heat resistance.
[0054] In the above step (c), the ratio (Mb / Tc) of the elongation ratio (Tc) along the longitudinal direction (MD) of the base sheet in the above step (b) to the elongation ratio (Mb) along the transverse direction (TD) of the porous membrane may be 3.0 to 5.0, preferably 3.5 to 4.8, more preferably 3.5 to 4.5, but is not limited thereto.
[0055] The thickness of the porous film obtained in the above step (c) may be 10 μm or less, preferably 1 to 8 μm, and more preferably 2 to 7 μm. If the thickness of the porous film exceeds 10 μm, it is difficult to make the separator thin and to miniaturize and integrate the battery including the same, and if it is less than 1 μm, the mechanical strength of the separator, particularly, the puncture strength, may be reduced. The puncture strength of the porous film obtained in the above step (c) may be 500 gf or more, preferably 500 to 1,000 gf, and more preferably 510 to 800 gf.
[0056] The separator obtained in the above step (c) can be applied as is when assembling a battery, and if necessary, a functional layer, which will be described later, can be formed on its surface and applied.
[0057] After the step (c), the step (d) may further include a step of applying a coating solution containing a binder and a solvent to at least one surface of the porous film and drying the coating solution to form a functional layer. Specifically, in the step (d), a coating solution containing a binder and a solvent may be applied to at least one surface of the porous film and dried to collectively remove the solvent and other liquid residues contained in the coating solution, thereby forming a functional layer. The functional layer may be formed on one surface of the porous film, and, if necessary, on both surfaces. The functional layers formed on both surfaces of the porous film may have the same thickness, composition, and effect, and in some cases, at least one of these may be different.
[0058] The above binder is polyvinylidene fluoride, polyvinylidene fluoride-hexafluoropropylene, polyvinylidene fluoride-trichloroethylene, polymethyl methacrylate, polyacrylonitrile, polyvinylpyrrolidone, polyvinylacetate, ethylene vinyl acetate, polyimide, polyethylene oxide, cellulose acetate, cellulose acetate butyrate, cellulose acetate propionate, cyanoethyl pullulan, cyanoethyl polyvinyl alcohol, cyanoethyl cellulose, hydroxyethyl cellulose, cyanoethyl sucrose, pullulan, carboxymethyl cellulose, polyvinyl alcohol, polyvinyl butyral, acrylonitrile-acrylic acid copolymer, ethylene-acrylic acid copolymer, styrene-butadiene copolymer, It may be one selected from the group consisting of alkyl acrylate-acrylonitrile copolymer, polyethylene glycol, acrylic rubber, and a combination of two or more thereof, and preferably, carboxymethyl cellulose and alkyl acrylate-acrylonitrile copolymer, but is not limited thereto. For example, in the functional layer, the carboxymethyl cellulose and the alkyl acrylate-acrylonitrile copolymer may be present in a weight ratio of 1:0.5 to 1.5, respectively.
[0059] The above coating solution may further include one inorganic particle selected from the group consisting of SiO2, AlO(OH), Mg(OH)2, Al(OH)3, TiO2, BaTiO3, Li2O, LiF, LiOH, Li3N, BaO, Na2O, Li2CO3, CaCO3, LiAlO2, Al2O3, SiO, SnO, SnO2, PbO2, ZnO, P2O5, CuO, MoO, V2O5, B2O3, Si3N4, CeO2, Mn3O4, Sn2P2O7, Sn2B2O5, Sn2BPO6, and combinations of two or more thereof, and the inorganic particle may contribute to improving the heat resistance of the functional layer and the separator. The inorganic particle may preferably be Al2O3 and / or AlO(OH), but is not limited thereto.
[0060] The content of the inorganic particles in the functional layer may be 50 to 95 wt%. If the content of the inorganic particles in the functional layer is less than 50 wt%, the required level of heat resistance cannot be imparted, and if it exceeds 95 wt%, the dispersibility of the inorganic particles may be reduced or the coating workability and processability may be reduced.
[0061] The above-mentioned inorganic particles tend to aggregate by binding due to electrostatic attraction. Such aggregation of the inorganic particles may deteriorate the uniformity of physical properties on the surface of the separation membrane. In this regard, the coating solution may further include an additive for improving the dispersibility of the inorganic particles, such as a dispersant, a surfactant, etc. In particular, the coating solution may include sodium hexametaphosphate ((NaPO3)6) as a dispersant, and the content of the sodium hexametaphosphate in the functional layer may be 0.01 to 1 wt%, preferably, 0.01 to 0.5 wt%. The sodium hexametaphosphate is adsorbed to the edge of the inorganic particles, particularly, the plate-shaped inorganic particles, thereby weakening the (-) charge of the edge, effectively preventing the aggregation of the inorganic particles, thereby improving the storage stability of the coating solution for forming the functional layer and the dispersibility of the inorganic particles in the functional layer.
[0062] To obtain a water-soluble coating solution, the solvent may be one selected from the group consisting of methanol, ethanol, propanol, butanol, methoxyethanol, ethoxyethanol, lactone, acetonitrile, n-methyl-2-pyrrolidone (NMP), formic acid, nitromethane, acetic acid, dimethyl sulfoxide, water, and a combination of two or more thereof, preferably, ethanol and water, more preferably, ethanol and water may be mixed in a weight ratio of 1:10 to 50, but is not limited thereto.
[0063] The above coating solution may contain 30 to 100 parts by weight of inorganic particles and 1 to 20 parts by weight of binder per 100 parts by weight of solvent, and may preferably be water-soluble (aqueous or water-based). The solid content of the above coating solution may be adjusted to 20 to 50% by weight, preferably 30 to 40% by weight, taking into account the balance between processability, workability, and heat resistance.
[0064] The thickness of the functional layer may be 1 to 10 μm. If the thickness of the functional layer is less than 1 μm, the required level of adhesiveness and heat resistance cannot be provided, and if it exceeds 10 μm, the separator may become thick, which may hinder high capacity, miniaturization, and integration of the battery or device.
[0065] Meanwhile, before applying the coating solution to both sides of the porous film in the step (d), the porous film can be plasma treated in the presence of a mixed gas containing sulfur dioxide (SO2) and oxygen (O2).
[0066] By hydrophilizing the surface of the porous membrane and / or the surface of the internal pores through the plasma treatment, the bonding strength between both sides of the porous membrane and the coating solution can be improved, and thus the durability of the membrane, particularly long-term durability and heat resistance, can be significantly improved.
[0067] In the past, a wet process was mainly used to hydrophilize the surface of a porous membrane by immersing it in sulfuric acid or the like for a certain period of time to sulfonate it. However, in this case, the wet process is performed separately from the plasma treatment, either before or after the plasma treatment, making the process complex and generating a large amount of process waste liquid.
[0068] In this regard, since the process gas used in the plasma treatment includes not only conventional air, oxygen, and / or inert gas but also a certain amount of sulfur dioxide gas, it is possible to maximize the hydrophilicity and ionic conductivity of the porous membrane by generating a functional group such as -SO3 on the surface of the porous membrane and the surface of the internal pores, i.e., sulfonating, through a single dry process called the plasma treatment without a wet process such as immersing the porous membrane in sulfuric acid, etc., and simplifying the conventional complicated process, and is also advantageous from an environmental perspective.
[0069] The mixed gas, which is the process gas used in the plasma treatment, may contain 50 to 90 vol% of sulfur dioxide and 10 to 50 vol% of oxygen, preferably 60 to 80 vol% of sulfur dioxide and 20 to 40 vol% of oxygen, and more preferably 70 to 80 vol% of sulfur dioxide and 20 to 30 vol% of oxygen. If the content of sulfur dioxide in the mixed gas is less than 50 vol%, the required level of hydrophilicity for the porous film cannot be achieved, and if it exceeds 90 vol%, the process may become unstable.
[0070] The above plasma treatment can be performed for 0.5 to 90 minutes, preferably 0.5 to 20 minutes. If the plasma treatment is performed for less than 0.5 minutes, the porous membrane cannot be hydrophilized and sulfonated to the required level, and if it is performed for more than 90 minutes, the degree of hydrophilization and sulfonation may converge to a certain level, which may lower the process efficiency.
[0071] A separation membrane manufactured using the above separation membrane manufacturing method can satisfy the following (i) to (iii).
[0072] (i) a longitudinal (MD) heat shrinkage of 5% or less, preferably 1.0 to 4.5%, more preferably 1.9 to 4.0%, at 150°C, (ii) a transverse (TD) heat shrinkage of 5% or less, preferably 1.0 to 4.8%, more preferably 1.5 to 4.0%, at 150°C, (iii) a ratio of the transverse (TD) heat shrinkage to the longitudinal (MD) heat shrinkage of 1.1 or less, preferably 0.5 to 1.0, more preferably 0.6 to 0.9, at 150°C.
[0073] Hereinafter, embodiments of the present invention will be described in detail.
[0074] Example 1
[0075] 20 parts by weight of ultra-high molecular weight polyethylene (UHMWPE) having a weight average molecular weight of 2,000,000 and a molecular weight distribution (Mw / Mn) of 5 and 80 parts by weight of paraffin oil having a kinematic viscosity of 70 cSt at 40°C were mixed and fed into a twin-screw extruder (inner diameter 58 mm, L / D=56). Under the conditions of a screw rotation speed of 40 rpm and 200°C, the mixture was extruded from the twin-screw extruder through a T-Die having a width of 630 mm and then passed through a casting roll having a temperature of 17°C to produce a base sheet having a thickness of 1,450 μm.
[0076] The above base sheet was stretched 8.0 times in the longitudinal direction (MD) in a roll stretching machine at 105°C (MDO process) and 9.5 times in the transverse direction (TD) in a tenter stretching machine at 125°C (TDO1 process), then immersed in a dichloromethane leaching tank at 25°C to extract and remove paraffin oil for 1 minute, and dried at 50°C for 5 minutes to produce a porous membrane. The porous membrane was stretched 1.7 times in the transverse direction (TD) at 134°C (TDO2 process), and then heat-set in an 18% relaxed state to produce a first separator having a thickness of 7 μm.
[0077] Carboxymethylcellulose salt (CMC), acrylic-acrylonitrile copolymer latex, alumina (aluminum oxide, Al2O3), dispersant ((NaPO3)6), surfactant, water, and ethanol were mixed in the ratios shown in Table 1 below and then dispersed using a ball mill to prepare a water-dispersed ceramic slurry.
[0078] Classification Input amount (g) Solid content (g) Solid content (%) Dry content (%) Water 1,500,000 Ethanol 70,000 CMC 27 27 100 3.3 Acrylic-acrylonitrile copolymer latex 70 3 1.5 4 5 3.9 Alumina 75 0 75 0 100 9 2.4 (NaPO3) 61.5 1.5 1000.2 Surfactant 22 1000.2 Total 2,421,8 12-100
[0079]
[0080] The above-mentioned water-dispersed ceramic slurry was applied to one side of the above-mentioned first separator, and gravure coated using a 110-mesh coating roll, and then dried in a hot air oven at a temperature of 80°C for 1 hour to manufacture a second separator including a functional layer (heat-resistant layer) having a thickness of 3 μm.
[0081] Example 2
[0082] The first and second separators were manufactured in the same manner as in Example 1, except that the base sheet was stretched 7.5 times in the longitudinal direction (MD) in the MDO process.
[0083] Example 3
[0084] The first and second separators were manufactured in the same manner as in Example 1, except that the base sheet was stretched 7.0 times in the longitudinal direction (MD) in the MDO process.
[0085] Example 4
[0086] The first and second separators were manufactured in the same manner as in Example 1, except that in the TDO1 process, the base sheet was stretched 9.0 times in the transverse direction (TD), and in the TDO2 process, the porous membrane was stretched 1.9 times in the transverse direction (TD).
[0087] Example 5
[0088] The first and second separators were manufactured in the same manner as in Example 4, except that the base sheet was stretched 7.5 times in the longitudinal direction (MD) in the MDO process.
[0089] Example 6
[0090] The first and second separators were manufactured in the same manner as in Example 4, except that the base sheet was stretched 7.0 times in the longitudinal direction (MD) in the MDO process.
[0091] Example 7
[0092] The first and second separators were manufactured in the same manner as in Example 1, except that in the TDO1 process, the base sheet was stretched 8.5 times in the transverse direction (TD), and in the TDO2 process, the porous membrane was stretched 2.0 times in the transverse direction (TD).
[0093] Example 8
[0094] The first and second separators were manufactured in the same manner as in Example 7, except that the base sheet was stretched 7.5 times in the longitudinal direction (MD) in the MDO process.
[0095] Example 9
[0096] The first and second separators were manufactured in the same manner as in Example 7, except that the base sheet was stretched 7.0 times in the longitudinal direction (MD) in the MDO process.
[0097] Comparative Example 1
[0098] The first and second separators were manufactured in the same manner as in Example 4, except that the base sheet was stretched 9.0 times in the longitudinal direction (MD) in the MDO process.
[0099] Comparative Example 2
[0100] The first and second separators were manufactured in the same manner as in Comparative Example 1, except that the base sheet was stretched 8.5 times in the transverse direction (TD) in the TDO1 process.
[0101] Comparative Example 3
[0102] The first and second separators were manufactured in the same manner as in Comparative Example 1, except that the base sheet was stretched 8.0 times in the transverse direction (TD) in the TDO1 process.
[0103] Comparative Example 4
[0104] The first and second separation membranes were manufactured in the same manner as in Comparative Example 1, except that the porous membrane was stretched 2.0 times in the transverse direction (TD) in the TDO2 process.
[0105] Comparative Example 5
[0106] The first and second separation membranes were manufactured in the same manner as in Comparative Example 1, except that the porous membrane was stretched 1.7 times in the transverse direction (TD) in the TDO2 process.
[0107] Comparative Example 6
[0108] The first and second separation membranes were manufactured in the same manner as in Comparative Example 1, except that the porous membrane was stretched 1.5 times in the transverse direction (TD) in the TDO2 process.
[0109] Comparative Example 7
[0110] The first and second separation membranes were manufactured in the same manner as in Comparative Example 1, except that the porous membrane was stretched 1.8 times in the transverse direction (TD) in the TDO2 process.
[0111] Comparative Example 8
[0112] The first and second separators were manufactured in the same manner as in Comparative Example 7, except that the base sheet was stretched 8.5 times in the longitudinal direction (MD) in the MDO process.
[0113] Comparative Example 9
[0114] The first and second separators were manufactured in the same manner as in Comparative Example 7, except that the base sheet was stretched 8.3 times in the longitudinal direction (MD) in the MDO process.
[0115] Comparative Example 10
[0116] 20 parts by weight of ultra-high molecular weight polyethylene (UHMWPE) having a weight average molecular weight of 2,000,000 and a molecular weight distribution (Mw / Mn) of 5 and 80 parts by weight of paraffin oil having a kinematic viscosity of 70 cSt at 40°C were mixed and fed into a twin-screw extruder (inner diameter 58 mm, L / D=56). The first and second membranes were manufactured in the same manner as in Example 1, except that the mixture was extruded from the twin-screw extruder at a screw rotation speed of 40 rpm and 200°C through a T-Die having a width of 630 mm and then passed through a casting roll having a temperature of 17°C to manufacture a base sheet having a thickness of 1,500 μm.
[0117] Comparative Example 11
[0118] 20 parts by weight of ultra-high molecular weight polyethylene (UHMWPE) having a weight average molecular weight of 2,000,000 and a molecular weight distribution (Mw / Mn) of 5 and 80 parts by weight of paraffin oil having a kinematic viscosity of 70 cSt at 40°C were mixed and fed into a twin-screw extruder (inner diameter 58 mm, L / D=56). The first and second separation membranes were manufactured in the same manner as in Example 1, except that the mixture was extruded from the twin-screw extruder at a screw rotation speed of 40 rpm and 200°C through a T-Die having a width of 630 mm and then passed through a casting roll having a temperature of 17°C to manufacture a base sheet having a thickness of 1,700 μm.
[0119] The main control variables of the method for manufacturing a separation membrane according to the above examples and comparative examples are as shown in Table 2 below. In Table 2 below, Mb and Tb are the elongation ratios of the base sheet along the longitudinal direction (MD) and the transverse direction (TD), respectively, and Tc is the elongation ratio of the porous membrane along the transverse direction (TD).
[0120] Classification MbTbTcMb / TbMb / (Tb*Tc)Example 18.09.51.70.8420.495Example 27.59.51.70.7890.464Example 37.09.51.70.7370.433Example 48.09.01.90.8890.468Example 57.59.01.90.8330.439Example 67.09.01.90.7780.409Example 78.08.52.00.9410.471Example 87.58.52.00.8820.441Example 97.08.52.00.8240.412Comparative Example 19.09.01.91.0000.526Comparative Example 29.08.51.91.0590.557Comparative Example 39.08.01.91.1250.592Comparative Example 49.09.02.01.0000.500Comparative Example 59.09.01.71.0000.588Comparative Example 69.09.01.51.0000.667Comparative Example 79.09.01.81.0000.556Comparative Example 88.59.01.80.9440.525Comparative Example 98.39.01.80.9220.512
[0121]
[0122] Experimental example
[0123] The puncture strength of the first separator and the thermal shrinkage rate of the second separator according to the above examples and comparative examples were measured using the following methods. Unless otherwise specified regarding temperature, measurements were made at room temperature (25°C), and the results are shown in Table 3 below.
[0124] -Puncture strength (gf): Using a puncture strength measuring device, a force was applied with a stick to the first membrane specimen measuring 100 mm x 50 mm until the specimen was punctured, and the force applied was measured.
[0125] -Thermal shrinkage rate (%): A second membrane specimen measuring 200*200mm was left between A4 papers in an oven at 150℃ for 1 hour, then cooled to room temperature. The contracted lengths of the specimen in the longitudinal direction (MD) and transverse direction (TD) were measured, and the thermal shrinkage rate was calculated using the following formula.
[0126] Heat shrinkage rate (%) = {(l3-l4) / l3}*100
[0127] In the above formula, l3 is the longitudinal or transverse length of the second membrane specimen before shrinkage, and l4 is the longitudinal or transverse length of the second membrane specimen after shrinkage.
[0128] Classification 1 Separator puncture strength 2nd Separator MD heat shrinkage (A) 2nd Separator TD heat shrinkage (B) B / A Example 15 154.14.5 1.098 Example 25 123.5 3.20.914 Example 35 201.91.5 0.789 Example 45 054.44.8 1.091 Example 55 213.83.20.842 Example 65 032.41.70.708 Example 75 183.94.11.051 Example 85 323.23.10.969 Example 95 092.61.80.692 Comparative Example 15 0215.5 25.01.613 Comparative Example 250815.521.21.368Comparative Example 351116.519.31.170Comparative Example 453117.241.02.384Comparative Example 550816.228.21.741Comparative Example 651216.918.81.112Comparative Example 752217.220.21.174Comparative Example 851910.29.80.961Comparative Example 95138.58.10.953Comparative Example 105156.513.02.000Comparative Example 1153215.525.01.613
[0129]
[0130] The foregoing description of the present invention is for illustrative purposes only, and those skilled in the art will readily appreciate that the present invention can be readily modified into other specific forms without altering the technical spirit or essential characteristics of the present invention. Therefore, the embodiments described above should be understood as illustrative in all respects and not restrictive. For example, each component described as a single entity may be implemented in a distributed manner, and similarly, components described as distributed may be implemented in a combined manner.
[0131] The scope of the present invention is indicated by the claims set forth below, and all changes or modifications derived from the meaning and scope of the claims and their equivalent concepts should be interpreted as being included in the scope of the present invention.
Claims
1. (a) A step of obtaining a base sheet by processing a composition including polyolefin and a pore-forming agent; (b) a step of stretching the base sheet in the longitudinal direction (MD) and the transverse direction (TD) and removing the pore forming agent to obtain a porous membrane; and (c) a step of stretching the porous membrane in the transverse direction (TD) and heat-setting it; Satisfying the conditions (1) to (3) below, Method for manufacturing membrane: (1) 7 ≤ Mb ≤ 8, (2) 0< Mb / Tb <1, (3) 0 < Mb / (Tb*Tc) <0.5, In the above (1) to (3), Mb and Tb are the elongation ratios of the base sheet along the longitudinal direction (MD) and the transverse direction (TD), respectively, in the above step (b), and Tc is the elongation ratio of the porous membrane along the transverse direction (TD) in the above step (c).
2. In paragraph 1, The weight average molecular weight (Mw) of the above polyolefin is 1,000,000 to 4,000,000. Method for manufacturing a membrane.
3. In paragraph 2, The above polyolefin comprises one selected from the group consisting of polyethylene, polypropylene, polybutylene, polymethylpentene, ethylene vinyl acetate, ethylene butylacrylate, ethylene ethyl acrylate, and combinations or copolymers of two or more thereof. Method for manufacturing a membrane.
4. In paragraph 1, The above Tc is 1.5 to 2.0, Method for manufacturing a membrane.
5. In paragraph 1, The ratio of the above Mb to the above Tc (Mb / Tc) is 3.0 to 5.0, Method for manufacturing a membrane.
6. In paragraph 1, The above pore forming agent is a paraffin oil having a kinematic viscosity of 50 to 100 cSt at 40°C. Method for manufacturing a membrane.
7. In paragraph 1, The thickness of the base sheet obtained in the above step (a) is 1,000 to 1,500 μm, The thickness of the porous membrane obtained in the above step (c) is 10㎛ or less, and the puncture strength is 500gf or more. Method for manufacturing a membrane.
8. In paragraph 1, After step (c) above, (d) further comprising a step of applying a coating solution containing a binder and a solvent to at least one surface of the porous film and drying it to form a functional layer; Method for manufacturing a membrane.
9. In paragraph 8, The above binder is polyvinylidene fluoride, polyvinylidene fluoride-hexafluoropropylene, polyvinylidene fluoride-trichloroethylene, polymethyl methacrylate, polyacrylonitrile, polyvinylpyrrolidone, polyvinylacetate, ethylene vinyl acetate, polyimide, polyethylene oxide, cellulose acetate, cellulose acetate butyrate, cellulose acetate propionate, cyanoethyl pullulan, cyanoethyl polyvinyl alcohol, cyanoethyl cellulose, hydroxyethyl cellulose, cyanoethyl sucrose, pullulan, carboxymethyl cellulose, polyvinyl alcohol, polyvinyl butyral, acrylonitrile-acrylic acid copolymer, ethylene-acrylic acid copolymer, styrene-butadiene copolymer, One selected from the group consisting of alkyl acrylate-acrylonitrile copolymers, polyethylene glycol, acrylic rubbers, and combinations of two or more thereof. Method for manufacturing a membrane.
10. In paragraph 8, The solvent is one selected from the group consisting of methanol, ethanol, propanol, butanol, methoxyethanol, ethoxyethanol, lactone, acetonitrile, n-methyl-2-pyrrolidone (NMP), formic acid, nitromethane, acetic acid, dimethyl sulfoxide, water, and a combination of two or more thereof. Method for manufacturing a membrane.
11. In paragraph 8, The coating solution further comprises one inorganic particle selected from the group consisting of SiO2, AlO(OH), Mg(OH)2, Al(OH)3, TiO2, BaTiO3, Li2O, LiF, LiOH, Li3N, BaO, Na2O, Li2CO3, CaCO3, LiAlO2, Al2O3, SiO, SnO, SnO2, PbO2, ZnO, P2O5, CuO, MoO, V2O5, B2O3, Si3N4, CeO2, Mn3O4, Sn2P2O7, Sn2B2O5, Sn2BPO6 and combinations of two or more thereof. Method for manufacturing a membrane.
12. Manufactured using a method for manufacturing a membrane according to any one of Articles 8 to 11, Satisfying the conditions (i) to (iii) below, Membrane: (i) A longitudinal (MD) heat shrinkage rate of 5% or less at 150℃; (ii) Transverse direction (TD) heat shrinkage of 5% or less at 150℃; (iii) The ratio of the transverse direction (TD) heat shrinkage to the longitudinal direction (MD) heat shrinkage at 150℃ is 1.1 or less.
Citation Information
Patent Citations
Polyolefin microporous membrane
JP2023020701A
High permeable polyethylene separator, and preparation method thereof
KR1020140071095A
Continuous glucose monitoring system
KR102331553B1
KR20190059859A
KR20220083881A