Polyethylene resin composition

A polyethylene resin composition with enhanced properties is achieved through a multi-step polymerization process, addressing the limitations of conventional polyethylene in heat resistance, stiffness, and transparency, resulting in films with improved mechanical strength and recyclability.

WO2024237471A1PCT designated stage expired Publication Date: 2024-11-21LG CHEM LTD
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
PCT/KR2024/004219
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2024-04-01
Filing Date
2024-04-02
Publication Date
2024-11-21

AI Technical Summary

Technical Problem

Conventional polyethylene-based packaging materials lack heat resistance, stiffness, and transparency compared to other resins, making them inferior for applications requiring these properties, and there is a need for a composition that enhances stretchability, mechanical properties, and transparency while being recyclable.

Method used

A polyethylene resin composition is developed with specific conditions including a bimodal molecular weight distribution, controlled density, and optimized crystallinity, achieved through a three-step polymerization process using Ziegler-Natta and metallocene catalysts, which involves primary and secondary polymerization reactions to create a blend of high-density and low-density polyethylenes with improved physical properties.

Benefits of technology

The resulting polyethylene resin composition exhibits excellent stretchability, mechanical properties, and transparency, enabling the production of films with high strength and resistance to defects during stretching, while also being recyclable.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure KR2024004219_21112024_PF_FP_ABST
    Figure KR2024004219_21112024_PF_FP_ABST
Patent Text Reader

Abstract

Provided in the present invention is a polyethylene resin composition with excellent stretchability, mechanical properties, and transparency.
Need to check novelty before this filing date? Find Prior Art

Description

polyethylene resin composition

[0001] Cross-citation with related application(s)

[0002] This application claims the benefit of priority to Korean Patent Application No. 10-2023-0063112, filed May 16, 2023, and Korean Patent Application No. 10-2024-0044221, filed April 1, 2024, the entire contents of which are incorporated herein by reference.

[0003] The present invention relates to a polyethylene resin composition having excellent stretchability, mechanical properties, and transparency.

[0004]

[0005] Conventional multilayer film packaging materials typically use composite materials blended with polyamide (PA), polyethylene terephthalate (PET), and polypropylene (PP). However, with increasing consumer concern for the environment, single-material packaging materials that are easily recyclable are gaining attention. Consequently, the food packaging and distribution industry is increasingly shifting towards "all-PE" films made solely from the versatile polyethylene (PE).

[0006] However, polyethylene has the disadvantage of lower heat resistance, stiffness, and transparency compared to resins such as polypropylene and polyterephthalate.

[0007] To address this, active development is underway to improve the mechanical properties of blown or cast films by uniaxial or biaxial stretching. To apply this technology, polyethylene must possess excellent stretchability and mechanical properties, while also possessing an appropriate level of transparency.

[0008] Accordingly, research and development are required for the production of polyethylene resin compositions with excellent stretchability, mechanical properties, and transparency.

[0009]

[0010] In order to solve the problems of the above-mentioned prior art, the present invention aims to provide a polyethylene resin composition having excellent stretchability, mechanical properties, and transparency.

[0011] In addition, the present invention aims to provide a film manufactured using the polyethylene resin composition and exhibiting excellent stretchability, mechanical properties, and transparency.

[0012]

[0013] In order to solve the above-mentioned problem, according to the present invention, a polyethylene resin composition satisfying the following conditions (a1) to (a5) is provided:

[0014] (a1) MI 2.16 (ASTM D 1238, 190℃, 2.16 kg): 0.5 to 3.0 g / 10 min

[0015] (a2) Density (ASTM D792): 0.940 to 0.955 g / cm3

[0016] (a3) MFRR(MI 21.6 / MI 2.16 ): 60 or more and less than 80

[0017] (a4) Molecular weight distribution (Mw / Mn): 10 to 14

[0018] (a5) When analyzing the temperature rise elution fraction (TREF), for the total weight of the entire elution fraction,

[0019] Content of polymer fraction eluting in the range of 25 to 90°C: 20 to 50 wt%; and

[0020] Content of polymer fraction eluting in the range of 90 to 120°C: 50 to 80 wt%.

[0021] In addition, according to the present invention, a method for producing a polyethylene resin composition is provided, including a first step of first polymerizing an ethylene monomer in the presence of a Ziegler-Natta catalyst in a first reactor, then moving the produced polymerization product to a second reactor, and introducing at least one of an ethylene monomer and a C4-C8 alpha-olefin monomer to perform a second polymerization reaction to produce a first polyethylene; a second step of introducing hydrogen and polymerizing an ethylene monomer and a C4-C8 alpha-olefin monomer in the presence of a catalyst containing a metallocene compound represented by the following chemical formula 1 in a separate single reactor to produce a second polyethylene; and a third step of mixing the first polyethylene and the second polyethylene in a weight ratio of 90:10 to 70:30.

[0022] [Chemical Formula 1]

[0023]

[0024] In the above chemical formula 1,

[0025] B is boron,

[0026] M is a group 4 transition metal,

[0027] R1 to R4 are each independently hydrogen, C 1-20 Alkyl, C 3-20 Cycloalkyl, or C 6-20 Aryl, or C in which R1 and R2 or R3 and R4 are combined with each other and are substituted or unsubstituted 6-60 Forming an aromatic ring,

[0028] R5 and R6 are each independently C 1-20 Alkyl, C 3-20 Cycloalkyl, or C 6-20 Aryl, or R5 and R6 are combined to form C 3-60 Aliphatic ring or C 6-60 Forming an aromatic ring,

[0029] X1 and X2 are each independently C 1-20 Alkyl or -O(CO)R', where R' is C 1-20It is alkyl,

[0030] Q is C comprising at least one selected from the group consisting of substituted or unsubstituted N, O and S. 2-60 It is a heterocycle,

[0031] Y and Y' are elements that constitute Q,

[0032] Y is N, O, or S,

[0033] Y' is an element of Q adjacent to Y, and is either N or C.

[0034] In addition, according to the present invention, a film comprising the polyethylene resin composition is provided, specifically, a stretched film.

[0035]

[0036] According to the present invention, a polyethylene resin composition exhibiting excellent stretchability, mechanical properties and transparency, and a film manufactured using the same can be provided.

[0037]

[0038] Figure 1 is a graph showing the results of temperature rise elution fraction (TREF) analysis for the polyethylene resin compositions of Examples 5 and 6 and Comparative Examples 10 and 14.

[0039]

[0040] In the present invention, terms such as first, second, etc. are used to describe various components, and the terms are used only for the purpose of distinguishing one component from another.

[0041] Furthermore, the terminology used herein is merely for the purpose of describing exemplary embodiments and is not intended to limit the present invention. The singular expression includes the plural expression unless the context clearly indicates otherwise. In this specification, it should be understood that the terms "comprise," "include," or "have" indicate the presence of a feature, number, step, component, or combination thereof, but do not preclude the possibility of the presence or addition of one or more other features, numbers, steps, components, or combinations thereof.

[0042] Also, throughout this specification, the term “polyethylene” or “ethylene (co)polymer” is a concept that includes both ethylene homopolymer and / or copolymer of ethylene and alpha-olefin.

[0043] The present invention is susceptible to various modifications and takes various forms. Specific embodiments are illustrated and described in detail below. However, this is not intended to limit the present invention to specific disclosed forms, but rather to encompass all modifications, equivalents, and alternatives falling within the spirit and technical scope of the present invention.

[0044] Hereinafter, the polyethylene resin composition of the present invention will be described in detail.

[0045]

[0046] The polyethylene resin composition according to the present invention can exhibit excellent stretchability, mechanical properties, and transparency through content control according to melt index, density, weight average molecular weight (Mw), and crystallinity.

[0047] Specifically, the polyethylene resin composition according to the present invention,

[0048] Satisfies the following conditions (a1) to (a5):

[0049] (a1) MI 2.16(ASTM D 1238, 190℃, 2.16 kg): 0.5 to 3.0 g / 10 min

[0050] (a2) Density (ASTM D792): 0.940 to 0.955 g / cm3

[0051] (a3) MFRR(MI 21.6 / MI 2.16 ): 60 or more and less than 80

[0052] (a4) Molecular weight distribution (Mw / Mn): 10 to 14

[0053] (a5) When analyzing the temperature rise elution fraction (TREF), for the total weight of the entire elution fraction,

[0054] Content of polymer fraction eluting in the range of 25 to 90°C: 20 to 50 wt%; and

[0055] Content of polymer fraction eluting in the range of 90 to 120°C: 50 to 80 wt%.

[0056]

[0057] Specifically, the polyethylene resin composition exhibits a bimodal molecular weight distribution curve in a graph of a molecular weight distribution curve in which the logarithmic value (log Mw) of the weight average molecular weight (Mw) (g / mol) is plotted on the x-axis and the molecular weight distribution (dwt / dlog Mw) for the logarithmic value is plotted on the y-axis during GPC analysis.

[0058] In the present invention, a bimodal molecular weight distribution means that the molecular weight distribution curve on the GPC graph has two peaks. In this case, if the two peaks have independent peak shapes and do not exist separately, but partially overlap and exist as a shoulder peak with no minimum value between the maximum values ​​of the two peaks, this is also included as a peak. In other words, if it is not interpreted as a single peak forming a normal distribution, but can be deconvoluted into two distributions, it is defined as a bimodal structure.

[0059] This bimodal molecular weight distribution signifies an increase in the distribution of low and high molecular weights within the polyethylene resin composition. This molecular weight distribution structure can exhibit improved physical properties, and in particular, compared to polyethylene resin compositions exhibiting a unimodal molecular weight distribution, it can strengthen the molecular structure morphology that favors biaxial stretching, thereby exhibiting superior extensibility.

[0060] Typically, biaxially oriented polyethylene (BOPE) films are manufactured by stretching cast sheets in both the machine direction (MD) and the transverse direction (TD). Because biaxial stretching must be completed from MD to TD, excellent stretchability is required for polyethylene used in BOPE films.

[0061] In order to secure stretchability in polyethylene, secondary crystallization must occur as late as possible during stretching in the MD direction, and a structure must exist that enables interlamellar lateral linking between lamellar layers within the polyethylene to enable subsequent stretching in the TD direction.

[0062] The polyethylene resin composition according to the present invention has a high density and a controlled molecular structure through optimal mixing of a first polyethylene (HDPE) with controlled physical properties such as MI and a low-density second polyethylene (LDPE).

[0063] Specifically, in the polyethylene resin composition according to the present invention, the first polyethylene can enhance rigidity through optimization of the ultra-high molecular weight region, and the second polyethylene can enhance the stretchability of the resin composition by enhancing the low molecular weight, low crystallinity portion for inter-lamellar chain movement.

[0064] In addition, the polyethylene resin composition according to the present invention exhibits normal comonomer distribution and can exhibit excellent biaxial stretchability by β-relaxation.

[0065] β-relaxation is due to the movement of polymer chains between lamellar crystals, and this increased fluidity can result in excellent stretchability during film production.

[0066] This type of β-relaxation can be confirmed by the presence of a peak (β-relaxation peak) expressed between -40°C and 10°C in a temperature-dependent loss modulus graph during dynamic mechanical analysis (DMA) of a polyethylene resin composition.

[0067] Additionally, the polyethylene resin composition according to the present invention has an optimized content distribution based on crystallinity. This optimized crystal distribution can be confirmed through TREF analysis.

[0068] Specifically, the polyethylene resin composition according to the present invention satisfies the following conditions during TREF analysis:

[0069] For the total weight of the entire elution fraction,

[0070] Content of polymer fraction eluting in the range of 25 to 90°C: 20 to 50 wt%; and

[0071] Content of polymer fraction eluting in the range of 90 to 120°C: 50 to 80 wt%.

[0072] More specifically, the polyethylene resin composition according to the present invention, when analyzed by TREF, has a content of a polymer fraction eluted in a range of 25 to 90°C of 20 wt% or more, or 25 wt% or more, or 30 wt% or more, and 50 wt% or less, or 45 wt% or less, or 43 wt% or less, or 40% or less, based on the total weight of the entire eluted fraction.

[0073] In addition, the polyethylene resin composition according to the present invention, when subjected to TREF analysis, has a content of a polymer fraction eluted in a range of 90 to 120°C of specifically 50 wt% or more, or 55 wt% or more, or 57 wt% or more, or 60 wt% or more, and 80 wt% or less, or 75 wt% or less, or 70 wt% or less, based on the total weight of the entire eluted fraction.

[0074] In addition, the polyethylene resin composition can further satisfy the following conditions during TREF analysis:

[0075] For the total weight of the entire elution fraction,

[0076] Content of polymer fraction eluting in the range of 40 to 70°C: 1 to 30 wt%; and

[0077] Content of polymer fraction eluting in the range of 100 to 105°C: 30 to 45 wt%.

[0078] More specifically, the polyethylene resin composition according to the present invention, when subjected to TREF analysis, has a content of a polymer fraction eluted in a range of 40 to 70°C of specifically 1 wt% or more, or 2 wt% or more, or 2.5 wt% or more, or 7 wt% or more, and 30 wt% or less, or 25 wt% or less, or 22 wt% or less, or 15 wt% or less, based on the total weight of the entire eluted fraction.

[0079] In addition, the polyethylene resin composition according to the present invention, when subjected to TREF analysis, has a content of a polymer fraction eluted in a range of 100 to 105°C of 30 wt% or more, or 33 wt% or more, or 35 wt% or more, and 45 wt% or less, or 44.5 wt% or less, or 40 wt% or less, based on the total weight of the entire eluted fraction.

[0080] In TREF analysis, a lower elution temperature indicates lower crystallinity. Both the polymer fraction eluting at an elution temperature of 25 to 90°C and the polymer fraction eluting at a temperature of 40 to 70°C are low-crystallization fractions, and satisfying the above-mentioned content conditions can enhance the extensibility, toughness, and transparency of the polyethylene resin composition.

[0081] In addition, both the polymer fraction eluted in the range of 90 to 120°C and the polymer fraction eluted in the range of 100 to 105°C are high-crystalline portions, and can increase the rigidity of the polyethylene resin composition by satisfying the above-mentioned content conditions.

[0082] In particular, since the polyethylene resin composition has a high content of a high crystallinity fraction eluted at a dissolution temperature of 100 to 105°C of 30 wt% or more, it can exhibit excellent stiffness and heat resistance when producing a stretched film.

[0083] Meanwhile, the content ratio of the fraction eluted by the elution temperature range of the polyethylene resin composition is calculated as a percentage (weight %) of the content ratio of the polymer fractions eluted in the corresponding temperature range based on the total weight of the entire eluted fraction obtained through TREF analysis.

[0084] In addition, the specific measurement method and measurement conditions for TREF analysis of the polyethylene resin composition are as described in the experimental example below.

[0085] In addition to the above-mentioned molecular structure, the polyethylene resin composition according to the present invention has a melt index (MI) measured at a temperature of 190° C. and a load of 2.16 kg according to ASTM D1238 standard. 2.16 ) may be 0.5 g / 10 min or more and 3.0 g / 10 min or less.

[0086] In general, the lower the MI, the better the melt strength, and as a result, the yield and processability are improved because the loss due to thickness deviation or neck-in phenomenon is minimized in the production of MDO films where blown stability (or bubble stability) is important. However, if the MI is too low, it causes excessive processing load in the production of MDO films, making film extrusion difficult, and there is a problem that the temperature must be increased to lower the processing viscosity during uniaxial stretching. On the other hand, the higher the MI, the better the flowability, which is advantageous in the production of BOPE films using the cast process. In addition, since a low molecular weight is required when performing the biaxial stretching process after producing the cast sheet, the MI must be high. However, if the MI is too high, the processing viscosity is too low, which reduces the process stability during extrusion and stretching. Therefore, in the present invention, by controlling the melt index of the polyethylene resin composition within the above-mentioned range, excellent processability is exhibited and it is advantageous in the extrusion and stretching processes.

[0087] More specifically, the melting index (MI) 2.16 ) may be 0.5 g / 10 min or more, or 0.8 g / 10 min or more, or 0.85 g / 10 min or more, or 0.87 g / 10 min or more, or 0.94 g / 10 min or more, or 1 g / 10 min or more, or 1.2 g / 10 min or more, or 1.21 g / 10 min or more, or 1.3 g / 10 min or more, and 3.0 g / 10 min or less, or 2.5 g / 10 min or less, or 2.0 g / 10 min or less, or 1.5 g / 10 min or less, or 1.49 g / 10 min or less, or 1.45 g / 10 min or less.

[0088] In addition, the polyethylene resin composition according to the present invention has a high density of 0.940 to 0.955 g / cm3. Accordingly, it can exhibit excellent strength characteristics. More specifically, the density of the polyethylene resin composition is 0.940 g / cm3. 3 or 0.942 g / cm 3 or 0.944 g / cm 3 and 0.955 g / cm 3 or less, or 0.954 g / cm 3 or less, or 0.951 g / cm 3 or less, or 0.950 g / cm 3 or less, or 0.949 g / cm 3 It could be as follows:

[0089] Meanwhile, the density of the polyethylene resin composition is a value measured according to ASTM D792 standard.

[0090] In addition, the polyethylene resin composition has a melt index (MI) measured at a temperature of 190°C and a load of 21.6 kg according to ASTM D1238. 21.6 ) was measured at a temperature of 190℃ and a load of 2.16 kg, and the melting index (MI) 2.16 ) is the MFRR (MI) ratio 21.6 / MI 2.16 ) is 60 or more and less than 80. More specifically, MFRR(MI 21.6 / MI 2.16 ) may be 60 or more, or 60.5 or more, or 61 or more, or 63 or more, and less than 80, or 77 or less, or 75 or less, or 70 or less.

[0091] In addition, the polyethylene resin composition has a molecular weight distribution (Mw / Mn) of 10 or more and 14 or less. More specifically, it may be 10 or more, or 10.5 or more, or 10.8 or more, or 11 or more, and 14 or less, 13.8 or less, or 13 or less, or 12 or less.

[0092] In the present invention, the molecular weight distribution of the polyethylene resin composition can be calculated by measuring the weight average molecular weight (Mw) and the number average molecular weight (Mn) through gel permeation chromatography (GPC) analysis, and then dividing the measured weight average molecular weight (Mw) by the number average molecular weight (Mn). In this case, the weight average molecular weight and the number average molecular weight are conversion values ​​for standard polystyrene. The specific measuring method and conditions for the molecular weight distribution of the polyethylene resin composition are as described in the experimental examples below.

[0093] In addition, the polyethylene resin composition according to the present invention can further satisfy one or more, two or more, or all three of the following conditions (b1) to (b3), in addition to the above-described physical property requirements:

[0094] (b1) Weight average molecular weight (Mw): 100,000 to 160,000 g / mol

[0095] (b2) Relaxation Time: 0.1 to 0.9 seconds

[0096] (b3) Shear Thinning Index: 0.2 to 0.5

[0097] Specifically, the polyethylene resin composition according to the present invention may have a weight average molecular weight (Mw) of 100,000 g / mol or more and 160,000 g / mol or less.

[0098] If Mw is too high, it is disadvantageous for the Cast and BOPE manufacturing processes, and if Mw is too low, it is disadvantageous for the Blown and MDO manufacturing processes due to low melting strength. Therefore, in the present invention, by controlling Mw within the above-mentioned range, both the Cast and BOPE manufacturing processes and the Blown and MDO manufacturing processes are possible.

[0099] More specifically, the weight average molecular weight (Mw) of the polyethylene resin composition may be 100,000 g / mol or more, or 110,000 g / mol or more, or 120,000 g / mol or more, and 160,000 g / mol or less, or 155,000 g / mol or less, or 150,000 g / mol or less, or 148,000 g / mol or less, or 147,000 g / mol or less, or 146,800 g / mol or less.

[0100] Meanwhile, in the present invention, the weight-average molecular weight (Mw) and number-average molecular weight (Mn) of the polyethylene resin composition can be measured through gel permeation chromatography (GPC) analysis, and each is a conversion value for standard polystyrene. The specific measurement method and conditions are as described in the experimental examples below.

[0101] In addition, the polyethylene resin composition exhibits a long stress relaxation time of 0.1 to 0.9 seconds.

[0102] Conventionally, bimodal high-density polyethylene used in the production of stretched films has a short stress relaxation time and a high degree of crystallinity, resulting in poor stretchability. Specifically, a short stress relaxation time leads to rapid stress relaxation, which increases disorientation and shrinkage, resulting in non-uniform lamella and film thickness distribution and film breakage. However, the polyethylene resin composition according to the present invention exhibits a longer stress relaxation time even under equivalent melt index conditions by blending a second polyethylene with a long stress relaxation time and a low degree of crystallinity during its production, thereby exhibiting excellent stretchability.

[0103] Meanwhile, the stress relaxation time of the polyethylene resin composition can be calculated by performing an oscillatory shear experiment using a rotational rheometer while continuously applying a strain (strain, 0.5%) within a linear viscosity range under conditions of a temperature of 190°C and an angular frequency of 0.01 Hz to 100 Hz (0.0628 rad / s to 628 rad / s), and then measuring the viscosity of the polyethylene resin composition using the Carreau-Yasuda Model of the following mathematical equation 1.

[0104] [Mathematical Formula 1]

[0105]

[0106] In the above mathematical formula 1,

[0107] The above η is the viscosity (Pa·s) of the polyethylene resin composition measured above,

[0108] The above η0 is the zero-point shear viscosity (Pa·s), and is the viscosity in the section where the viscosity value does not change when the angular frequency approaches 0. In the present invention, the log-log graph with each frequency (unit: Hz) as the x-axis and the viscosity measurement value η (unit: Pa·s) of the polyethylene resin composition measured above as the y-axis can be calculated by fitting the curve to the Carreau-Yasuda Model of the above mathematical equation 1.

[0109] Also, the above is the shear rate applied to the polyethylene resin composition, which is the same value as each frequency converted to rad / s by the Cox Merz Rule,

[0110] The above λ is the stress relaxation time (seconds) of the polyethylene resin composition, and in the present invention, it can be calculated by fitting a log-log graph with each frequency (Hz) as the x-axis and the viscosity measurement value η (Pa·s) of the polyethylene resin composition measured above as the y-axis to the Carreau-Yasuda Model of the above mathematical expression 1.

[0111] In addition, the above n is a shear thinning index, and in the present invention, a log-log graph with each frequency (Hz) as the x-axis and the viscosity measurement value η (Pa·s) of the polyethylene resin composition measured above as the y-axis can be calculated by fitting it to the Carreau-Yasuda Model of the above mathematical expression 1.

[0112] The above a is a shape parameter that transitions between the Newtonian plateau and the power law region, and in the present invention, it can be calculated by fitting a log-log graph with each frequency (Hz) as the x-axis and the viscosity measurement value η(Pa·s) of the polyethylene resin composition measured above as the y-axis to the Carreau-Yasuda Model of the above mathematical expression 1.

[0113] More specifically, the polyethylene resin composition exhibits a long stress relaxation time of 0.1 seconds or more, or 0.15 seconds or more, or 0.17 seconds or more, or 0.2 seconds or more, and 0.9 seconds or less, 0.89 seconds or less, or 0.7 seconds or less, or 0.68 seconds or less, or 0.65 seconds or less.

[0114] The method for measuring the stress relaxation time of the above polyethylene resin composition is described in detail in the following experimental examples.

[0115] Additionally, the polyethylene resin composition exhibits a shear thinning index of 0.2 to 0.5.

[0116] The shear thinning index indicates the crystallization rate and the uniformity of the crystallization rate. The higher the shear thinning index, the slower the crystallization rate, and the higher the uniformity of the crystallization rate, which can exhibit excellent stretchability. Polyethylene, which is conventionally used in the production of stretched films, has a high degree of crystallinity and therefore a low shear thinning index. Accordingly, the crystallization rate is fast, but the uniformity of the crystallization rate is low, which exhibits unstable crystallization behavior, and as a result, exhibits deteriorated stretchability. On the other hand, the polyethylene resin composition according to the present invention exhibits a high shear thinning index by mixing a second polyethylene having a long stress relaxation time and low crystallization rate during the production. Accordingly, the crystallization rate is slow, the uniformity of the crystallization rate is high, which exhibits stable crystallization behavior, and can exhibit excellent stretchability. Furthermore, by exhibiting a shear thinning index within the above-mentioned range, it can exhibit even better stretchability.

[0117] More specifically, the polyethylene resin composition may exhibit a shear thinning index of 0.2 or more, or 0.22 or more, or 0.25 or more, and 0.5 or less, or 0.4 or less, or 0.36 or less.

[0118] In the present invention, the shear thinning index of the polyethylene resin composition is measured by performing an oscillatory shear experiment using a rotational rheometer while applying a strain (strain, 0.5%) within a linear viscosity range under conditions of a temperature of 190°C and an angular frequency of 0.01 Hz to 100 Hz (0.0628 rad / s to 628 rad / s), and measuring the viscosity of the polyethylene resin composition. Then, a log-log graph is obtained with the angular frequency (Hz) as the x-axis and the viscosity measurement value η (Pa·s) of the polyethylene resin composition measured above as the y-axis, and then fitting the graph to the Carreau-Yasuda Model of the above mathematical equation 1.

[0119] The polyethylene resin composition according to the present invention satisfies all of the above-described molecular structure and physical property conditions, thereby exhibiting excellent stretchability, high mechanical properties, and transparency. Consequently, there is no concern about defects such as breakage or shrinkage occurring during TD stretching when producing a biaxially oriented film, and the resulting biaxially oriented film exhibits excellent stretchability, high mechanical strength, and transparency.

[0120] Meanwhile, the polyethylene resin composition according to the present invention specifically has a density (ASTM D792) of 0.950 g / cm3 or more and an MI 2.16 (ASTM D 1238, 190℃, 2.16 kg) High-density first polyethylene satisfying 0.5 to 2 g / 10min, and density of 0.925 g / ㎤ or less and MI 2.16 (ASTM D 1238, 190℃, 2.16 kg) Contains low density secondary polyethylene of 1 to 5 g / 10 min.

[0121] The above first polyethylene is manufactured by using a Ziegler-Natta catalyst advantageous for a broad molecular weight distribution and a multimodal slurry polymerization process utilizing multiple reactors, thereby satisfying all of the above-mentioned physical property conditions and further satisfying the following conditions (c1) to (c5). Accordingly, the first polyethylene can enhance stiffness by increasing the content of the ultra-high molecular region in the polyethylene resin composition:

[0122] (c1) Density (ASTM D792): 0.950 g / cm 3 or 0.952 g / cm 3 and 0.965 g / cm 3 or less, or 0.960 g / cm 3 or less, or 0.958 g / cm 3 below

[0123] (c2) MI 2.16(ASTM D 1238, 190℃, 2.16 kg): 0.5 g / 10min or more, or 0.8 g / 10min or more, or 1 g / 10min or more, and 2 g / 10min or less, or 1.5 g / 10min or less

[0124] (c3) MFRR(MI 21.6 / MI 2.16 ): 50 or more, or 80 or more, and 100 or less, or 90 or less, or 85 or less

[0125] (c4) Weight average molecular weight (Mw): 130,000 g / mol or more, or 140,000 g / mol or more, or 142,000 g / mol or more, and 160,000 g / mol or less, or 155,000 g / mol or less, or 150,000 g / mol or less

[0126] (c5) Molecular weight distribution (Mw / Mn): 10 or more, or 13 or more, or 14 or more, or 14.1 or more, and 16 or less, or 15.5 or less, or 15.2 or less.

[0127] The first polyethylene may be specifically at least one of an ethylene homopolymer and an ethylene / C4-C8 alpha olefin copolymer. In addition, the ethylene / C4-C8 alpha olefin copolymer may be an ethylene / 1-butene copolymer.

[0128] Meanwhile, the second polyethylene can be manufactured using a metallocene catalyst and a unimodal slurry polymerization process using a single reactor, thereby satisfying the conditions (d1) to (d5) below. Accordingly, the second polyethylene can enhance low-molecular-weight, low-crystallinity for interlamellar chain movement within the polyethylene resin composition, thereby improving stretchability.

[0129] (d1) Density (ASTM D792): 0.910 g / cm 3 and 0.925 g / cm 3 or less, or 0.920 g / cm3 or less, or 0.918 g / cm 3 below

[0130] (d2) MI 2.16 (ASTM D 1238, 190℃, 2.16 kg): 1 g / 10min or more, 5 g / 10min or less, or 3 g / 10min or less

[0131] (d3) MFRR(MI 21.6 / MI 2.16 ): 10 or more, or 15 or more, and 50 or less, or 20 or less

[0132] (d4) Weight average molecular weight (Mw): 50,000 g / mol or more, or 70,000 g / mol or more, and 130,000 g / mol or less, or 120,000 g / mol or less

[0133] (d5) Molecular weight distribution (Mw / Mn): 1 or more, or 2 or more, or 2.4 or more, and 10 or less, or 3 or less, or 2.5 or less.

[0134] Meanwhile, the polyethylene resin composition exhibits a long stress relaxation time and exhibits excellent ductility as the crystallization rate is slow. In the case of the first polyethylene, there is a short stress relaxation time due to high density and a high crystallinity, resulting in poor ductility. In contrast, the second polyethylene exhibits a long stress relaxation time and a high shear thinning index, and also exhibits T in the Loss modulus (E") curve. β Since the peak is expressed, the shortcomings of the first polyethylene described above can be compensated for.

[0135] The second polyethylene may be specifically at least one of an ethylene / C4-C8 alpha olefin copolymer, and more specifically an ethylene / 1-hexene copolymer or an ethylene / 1-octene copolymer.

[0136] The above-mentioned first polyethylene and second polyethylene are included in a weight ratio of 90:10 to 70:30. When the above-mentioned weight ratio condition is satisfied, the physical properties of the above-mentioned polyethylene resin composition are easily improved and are also superior in terms of improvement effect. More specifically, the above-mentioned first polyethylene and second polyethylene may be mixed in a weight ratio of 90:10 to 77:23, or 90:10 to 80:20, or 90:10 to 83:17, or 83:17 to 70:30, or 80:20 to 70:30, or 77:23 to 70:30.

[0137] Meanwhile, the polyethylene resin composition according to the present invention as described above comprises a first step of producing first polyethylene by first polymerizing an ethylene monomer in the presence of a Ziegler-Natta catalyst in a first reactor, then moving the produced polymerization product to a second reactor, and introducing at least one of an ethylene monomer and a C4-C8 alpha-olefin monomer to perform a second polymerization reaction;

[0138] A second step of producing a second polyethylene by polymerizing an ethylene monomer and a C4-C8 alpha-olefin monomer while adding hydrogen in the presence of a catalyst containing a metallocene compound represented by the following chemical formula 1 in a separate single reactor; and

[0139] It can be manufactured by a manufacturing method including a third step of mixing the first polyethylene and the second polyethylene in a weight ratio of 90:10 to 70:30:

[0140] [Chemical Formula 1]

[0141]

[0142] In the above chemical formula 1,

[0143] B is boron,

[0144] M is a group 4 transition metal,

[0145] R1 to R4 are each independently hydrogen, C 1-20 Alkyl, C 3-20 Cycloalkyl, or C6-20 Aryl, or C in which R1 and R2 or R3 and R4 are combined with each other and are substituted or unsubstituted 6-60 Forming an aromatic ring,

[0146] R5 and R6 are each independently C 1-20 Alkyl, C 3-20 Cycloalkyl, or C 6-20 Aryl, or R5 and R6 are combined to form C 3-60 Aliphatic ring or C 6-60 Forming an aromatic ring,

[0147] X1 and X2 are each independently C 1-20 Alkyl or -O(CO)R', where R' is C 1-20 It is alkyl,

[0148] Q is C comprising at least one selected from the group consisting of substituted or unsubstituted N, O and S. 2-60 It is a heterocycle,

[0149] Y and Y' are elements that constitute Q,

[0150] Y is N, O, or S,

[0151] Y' is an element of Q adjacent to Y, and is either N or C.

[0152]

[0153] Meanwhile, in this specification, unless otherwise specifically limited, the following terms may be defined as follows:

[0154] The above halogen may be fluoro (F), chloro (Cl), bromo (Br) or iodo (I).

[0155] The above alkyl may be straight-chain or branched-chain alkyl. Specifically, the above C 1-20 Alkyl is C 1-20 Straight chain alkyl; C 1-10 Straight chain alkyl; C 1-5 Straight chain alkyl; C 3-20 Branched chain alkyl; C 3-15 Branched chain alkyl; or C 3-10It may be a branched chain alkyl. More specifically, C 1-20 Alkyl includes, but is not limited to, a methyl group, an ethyl group, an n-propyl group, an iso-propyl group, an n-butyl group, an iso-butyl group, a tert-butyl group, an n-pentyl group, or an iso-pentyl group. Meanwhile, in the present specification, "iPr" means an iso-propyl group.

[0156] The above cycloalkyl may be a cyclic alkyl. Specifically, the above C 3-20 Cycloalkyl is C 3-20 Cyclic alkyl; C 3-15 Cyclic alkyl; or C 3-10 It may be a cyclic alkyl. More specifically, it includes, but is not limited to, cyclopropyl, cyclobutyl, cyclopentyl, 3-methylcyclopentyl, 2,3-dimethylcyclopentyl, cyclohexyl, 3-methylcyclohexyl, 4-methylcyclohexyl, 2,3-dimethylcyclohexyl, 3,4,5-trimethylcyclohexyl, 4-tert-butylcyclohexyl, cycloheptyl, cyclooctyl, etc. Meanwhile, "Cy" in the present specification means cycloalkyl having 3 to 6 carbon atoms.

[0157] The above alkenyl may be a straight-chain, branched-chain or cyclic alkenyl. Specifically, the above C 2-20 Alkenyl is C 2-20 Straight-chain alkenyl, C 2-10 Straight-chain alkenyl, C 2-5 Straight-chain alkenyl, C 3-20 Branched-chain alkenyl, C 3-15 Branched-chain alkenyl, C 3-10 Branched-chain alkenyl, C 5-20 Cyclic alkenyl or C 5-10 It may be a cyclic alkenyl. More specifically, C 2-20 Alkenyl can be ethenyl, propenyl, butenyl, pentenyl or cyclohexenyl.

[0158] The above alkoxy may be a straight-chain, branched-chain or cyclic alkoxy group. Specifically, the above C 1-20 Alkoxy is C 1-20Straight-chain alkoxy group; C 1-10 Straight chain alkoxy; C 1-5 Straight-chain alkoxy group; C 3-20 Branched or cyclic alkoxy; C 3-15 Branched or cyclic alkoxy; or C 3-10 It may be a branched or cyclic alkoxy. More specifically, C 1-20 Alkoxy includes, but is not limited to, a methoxy group, an ethoxy group, an n-propoxy group, an iso-propoxy group, an n-butoxy group, an iso-butoxy group, a tert-butoxy group, an n-pentoxy group, an iso-pentoxy group, a neo-pentoxy group, or a cyclohexene group.

[0159] The above alkoxyalkyl is -R a -OR b Alkyl (-R) with a structure containing a ) is one or more hydrogens of alkoxy (-OR b ) may be a substituent substituted with C. Specifically, the above C 2-20 Alkoxyalkyl includes, but is not limited to, a methoxymethyl group, a methoxyethyl group, an ethoxymethyl group, an iso-propoxymethyl group, an iso-propoxyethyl group, an iso-propoxyhectyl group, a tert-butoxymethyl group, a tert-butoxyethyl group, or a tert-butoxyhexyl group.

[0160] The above aryl includes monocyclic, bicyclic, or tricyclic aromatic hydrocarbons. According to one embodiment of the present invention, the aryl group may have 6 to 60 carbon atoms or 6 to 20 carbon atoms, and specifically includes, but is not limited to, phenyl, naphthyl, anthracenyl, dimethylanilinyl, anisolyl, and the like.

[0161] The above heteroaryl is a heteroaryl containing at least one of O, N, and S as a heteroatom, and the number of carbon atoms is not particularly limited, but may be 2 to 60 carbon atoms or 2 to 20 carbon atoms. Examples of heteroaryl include xanthene, thioxanthen, thiophene, furan, pyrrole, imidazole, thiazole, oxazole, oxadiazole, triazole, pyridyl, bipyridyl, pyridinyl, pyrimidyl, triazine, acridyl, pyridazine, pyrazinyl, quinolinyl, quinazoline, quinoxalinyl, phthalazinyl, pyridopyrimidinyl, pyridopyrazinyl, pyrazinopyrazinyl, isoquinoline, indole, carbazole, benzoxazole, benzimidazole, benzothiazole, benzocarbazole, benzothiophene, dibenzothiophene, benzofuranyl, Examples include, but are not limited to, phenanthroline, isoxazolyl, thiadiazolyl, phenothiazinyl, and dibenzofuranyl groups.

[0162] The above heterocycle includes both an aliphatic ring comprising at least one selected from the group consisting of N, O, and S, and an aromatic ring comprising at least one selected from the group consisting of N, O, and S.

[0163] And, the group 4 transition metal may be titanium (Ti), zirconium (Zr), hafnium (Hf), or rutherfordium (Rf), specifically titanium (Ti), zirconium (Zr), or hafnium (Hf), more specifically zirconium (Zr) or hafnium (Hf), but is not limited thereto.

[0164] The above-described substituents may be optionally substituted with one or more substituents selected from the group consisting of a hydroxy group; a halogen; an alkyl or alkenyl, an aryl, an alkoxy; an alkyl or alkenyl, an aryl, an alkoxy containing one or more heteroatoms of groups 14 to 16; an amino; a silyl; an alkylsilyl or alkoxysilyl; a phosphine group; a phosphide group; a sulfonate group; and a sulfone group, within a range that exhibits the same or similar effect as the desired effect.

[0165]

[0166] Each step is explained in detail below.

[0167] First, the first step for producing a polyethylene resin composition according to the present invention is a step for producing first polyethylene.

[0168] Specifically, in the presence of a Ziegler-Natta catalyst in a first reactor, an ethylene monomer is subjected to a first polymerization reaction, and then the resulting polymerization product is transferred to a second reactor, and at least one of an ethylene monomer and a C4-C8 alpha-olefin monomer is introduced to perform a second polymerization reaction, thereby producing a first polyethylene.

[0169] Since the above first polyethylene is produced by slurry polymerization using multiple reactors, two or more reactors, for example, two or more continuous stirred tank reactors (CSTR), may be used. Specifically, in the above production method, a first reactor in which a first slurry polymerization reaction for producing the first polyethylene occurs, and a second reactor connected to the first reactor in which a second slurry polymerization reaction occurs may be used.

[0170] In addition, the polymerization process in the first and second reactors is performed by a slurry polymerization process.

[0171] In solution polymerization, the catalyst is activated by high-temperature and high-pressure reactions, so the resulting resin composition exhibits poor extensibility due to a narrow molecular weight distribution (MWD) and low high-molecular-weight tail content. However, in the slurry polymerization process of the present invention, polymerization is performed at a relatively low temperature, thereby ensuring a molecular structure containing a wide MWD and a large amount of high-molecular-weight tail, as required for a polyethylene resin composition for transparent film production. As a result, excellent biaxial extensibility can be achieved.

[0172] In addition, the Ziegler-Natta catalyst used in the production of the first polyethylene may be specifically a magnesium-supported titanium catalyst. In addition, the magnesium-supported titanium catalyst may further comprise a halogenated hydrocarbon.

[0173] Specifically, the magnesium-supported titanium catalyst comprises a solid magnesium support. Examples of the magnesium support include magnesium, magnesium oxide, magnesium chloride, silica-magnesia, or magnesia, and any one or a mixture of two or more thereof may be used. Among these, considering the catalytic activity and the ease of achieving optimal physical property conditions of the polyethylene resin composition, the magnesium support may be magnesium.

[0174] Meanwhile, the magnesium-supported titanium catalyst includes a titanium-containing compound represented by the following chemical formula 2 as a main catalyst:

[0175] [Chemical Formula 2]

[0176] Ti(OR 1 ) m X 1 4-m

[0177] In the above chemical formula 2,

[0178] R 1 are the same or different, and are alkyl groups having 1 to 10 carbon atoms,

[0179] X 1is a halogen element, more specifically Cl, Br or I,

[0180] m is an integer from 0 to 4.

[0181] In the above chemical formula 2, R 1 Specifically, it can be an alkyl group having 1 or more carbon atoms, or 2 or more carbon atoms, or 3 or more carbon atoms, and 10 or less carbon atoms, or 8 or less carbon atoms, or 5 or less carbon atoms.

[0182] Also, X 1 can be specifically Br, or Cl, and more specifically Cl.

[0183] Specific examples of the titanium-containing compound include titanium tetrachloride (TiCl4) or chlorinated titanium oxide, and either one or a mixture of the two may be used.

[0184] In addition, the catalyst including the titanium-containing compound may include Mg:Ti in a molar ratio of 1:1 to 10:1, or a molar ratio of 2:1 to 7:1, or a molar ratio of 4:1 to 5:1, based on the content of Mg in the magnesium support and the content of Ti in the titanium-containing compound. When included in the molar ratio range described above, it may exhibit better catalytic activity.

[0185] In addition, the shape of the catalyst is not particularly limited, but may be in the form of spherical fine particles, for example.

[0186] In addition, the average particle size of the catalyst may be 5 to 100 μm, and more specifically, 5 μm or more, or 8 μm or more, or 10 μm or more, and 100 μm or less, or 50 μm or less, or 20 μm or less, or 13 μm or less.

[0187] Meanwhile, in the present invention, the average particle size of the catalyst can be measured through scanning electron microscopy (SEM) observation. Specifically, after obtaining an SEM image in which 100 or more catalyst particles are observed, a random straight line is drawn, and the average size of the catalyst particles can be calculated through the length of the straight line, the number of particles included in the straight line, and the magnification.

[0188] Additionally, the magnesium-supported titanium catalyst may further include a halogenated hydrocarbon.

[0189] Halogenated hydrocarbons change the electrical properties of titanium by coordinating around titanium, which acts as an active site, and the large volume of halogenated hydrocarbons forms sufficient three-dimensional space between titanium atoms, so that the catalytic activity during polyethylene polymerization can be greatly improved.

[0190] The above halogenated hydrocarbon may be specifically an alkane having 1 to 12 carbon atoms, a cycloalkane having 3 to 12 carbon atoms, an alkene having 2 to 12 carbon atoms, an alkyne having 2 to 12 carbon atoms, or an aromatic hydrocarbon having 6 to 30 carbon atoms, substituted with at least one halogen group, and the halogen group may be fluoro, chloro, or bromo.

[0191] Specific examples include bromoform, tetrachloroethane, hexachloroethane, pentachloroethane, 1,1,2,2-tetrachloroethane, 1-bromo-1-chloroethane, 1,2-dibromoethane, 1,2-dichloroethane, bromoethane, hexachloropropane, 1,2,3-trichloropropane, 1,2-dichloropropane, 1-chloropropane, 2-chloropropane, chlorobutane, dichlorobutane, 1-chloro-2-methylpropane, n-butyl chloride, tert-butyl chloride, 1-chloro-3-methylbutane, 1-chloropentane, 1,5-dichloropentane, bromopentane, neopentyl chloride, 1-chloroheptane, cyclopropyl bromide, Examples thereof include cyclobutyl chloride, cyclohexyl chloride, cyclohexyl bromide, vinylidene chloride, 1,2,3,3-tetrachloropropene, 1,2-dibromo-1-propene, 1,3-dichloropropene, hexachloro-1,3-butadiene, 2-bromo-2-butene, propargyl chloride, chlorobenzene, tetrachlorobenzene, trichlorobenzene, dichlorobenzene, 4-chlorobenzyl chloride, benzyl chloride, or 1,1-dichloro-2-phenylcyclopropane, and any one of these or a mixture of two or more thereof may be used.

[0192] The above halogenated hydrocarbon may be included in an amount of 0.1 mol or more, or 0.12 mol or more, or 0.13 mol or more, and 500 mol or less, or 100 mol or less, or 50 mol or less, or 10 mol or less, or 1 mol or less, or 0.5 mol or less, based on 1 mol of the titanium-containing compound as the main catalyst.

[0193] The above-described Ziegler-Natta catalyst may be manufactured by a manufacturing method comprising a support treatment step of mixing raw materials of a magnesium support with alcohol and reacting them; and a titanium-containing compound loading step of reacting the product obtained as a result of the above step with a titanium-containing compound represented by the above chemical formula 1, and further comprising a step of contacting the product with a halogenated hydrocarbon for reaction during the support treatment step and the titanium-containing compound loading step, or after the titanium-containing compound loading step. Accordingly, the manufacturing method of the polyethylene resin composition according to the present invention may further comprise, before the first step, a step for manufacturing the Ziegler-Natta catalyst, specifically, the support treatment step and the titanium-containing compound loading step, and a step of contacting the product with a halogenated hydrocarbon for reaction during the support treatment step and the titanium-containing compound loading step, or after the titanium-containing compound loading step:

[0194] Specifically, the support treatment step for producing the Ziegler-Natta catalyst can be performed by mixing and reacting the raw material for the magnesium support with alcohol in a non-polar solvent.

[0195] Specific examples of the above alcohols include methanol, ethanol, 1-propanol, isopropanol, n-butanol, isobutanol, 1-pentanol, isopentanol, n-hexanol, 1-octanol, 2-ethyl-1-hexanol, etc., and any one of these or a mixture of two or more thereof may be used. Among these, ethanol or 2-ethyl-1-hexanol may be used.

[0196] The above alcohol may be used in an amount of 1 mol or more, 1.5 mol or more, or 2 mol or more, and 10 mol or less, or 8 mol or less, or 6 mol or less, per mol of the raw material of the magnesium carrier.

[0197] Meanwhile, the raw material for the magnesium support may include the magnesium support itself, such as magnesium, magnesium oxide, magnesium chloride, or silica-magnesia; or a magnesium alcoholate, such as magnesium ethylate; and one or a mixture of two or more thereof may be used. For example, when magnesium alcoholate is used as the raw material for the magnesium support, it is converted into magnesium chloride by titanium tetrachloride (TiCl4) introduced as the main catalyst and is included as a support in the final catalyst.

[0198] The method of mixing the raw material of the magnesium carrier and the alcohol may be performed by, specifically, adding the alcohol to a slurry prepared by mixing the raw material of the magnesium carrier with a non-polar solvent such as hexane, or adding a solution of the alcohol dissolved in a non-polar solvent to the slurry, and then stirring the slurry at a temperature of 20 to 150°C until a transparent solution is obtained. As a result of the mixing, a uniform solution of the magnesium carrier is obtained, and at this time, an adduct is formed in the solution in which crystals of the magnesium carrier are surrounded by alcohol molecules.

[0199] Next, the step of supporting the titanium-containing compound for producing the Ziegler-Natta catalyst is performed by reacting the reaction product of the magnesium support and alcohol produced in the support treatment step with the titanium-containing compound.

[0200] Specifically, the reaction product of the magnesium carrier and alcohol generated in the carrier treatment step may be performed by directly adding the titanium-containing compound, or by adding a solution of the titanium compound dissolved in a non-polar solvent, and reacting at -50 to 120°C or -20 to 80°C.

[0201] The type and content of the above titanium-containing compound are as described above.

[0202] In addition, when the titanium-containing compound is added, the reaction product of the magnesium carrier and alcohol generated in the carrier treatment step may be stirred at 10 to 500 rpm, or 50 to 400 rpm.

[0203] Meanwhile, in the production of the Ziegler-Natta catalyst, a step of introducing a halogenated hydrocarbon when introducing alcohol to the magnesium support in the support treatment step; introducing a halogenated hydrocarbon when introducing the titanium-containing compound in the support step of the titanium-containing compound; or introducing a halogenated hydrocarbon after the completion of the support step of the titanium-containing compound to cause a reaction may be further performed.

[0204] The types and contents of the above halogenated hydrocarbons are as described above.

[0205] The Ziegler-Natta catalyst manufactured through the above-described manufacturing method can be used as is during polyethylene polymerization, or can be used after being slurried in a non-polar solvent.

[0206] In addition, the Ziegler-Natta catalyst can be used together with an organometallic compound represented by the following chemical formula 3 as a cocatalyst.

[0207] [Chemical Formula 3]

[0208] R 2 n MX 2 (3-n)

[0209] In the above chemical formula 3,

[0210] M is selected from the group consisting of elements of groups IB, IIA, IIIB and IVB of the periodic table,

[0211] R 2 are each the same or different and are alkyl groups having 1 to 10 carbon atoms,

[0212] X 2 is a halogen,

[0213] n is an integer from 1 to 3.

[0214] In the above chemical formula 3, M is specifically aluminum, and R 2 is an alkyl group having 1 to 5 carbon atoms, or 2 to 4 carbon atoms, and X 2 is Cl or Br.

[0215] Specific examples of the organometallic compound represented by the above chemical formula 3 include triethylaluminum, methylaluminum dichloride, methylaluminum dibromide, dimethylaluminum chloride, dimethylaluminum bromide, propylaluminum dichloride, propylaluminum dibromide, butylaluminum dichloride, butylaluminum dibromide, dibutylaluminum chloride, dibutylaluminum bromide, isobutylaluminum dichloride, isobutylaluminum dibromide, diisobutylaluminum chloride, diisobutylaluminum bromide, hexylaluminum dichloride, hexylaluminum dibromide, dihexylaluminum chloride, dihexylaluminum bromide, octylaluminum dichloride, octylaluminum dibromide, dioctylaluminum chloride, Examples include dioctyl aluminum bromide, and one or a mixture of two or more of these may be used.

[0216] Meanwhile, since the cocatalyst affects the polymerization activity of the magnesium-supported catalyst, the polymerization activity of the catalyst can be further increased by controlling the cocatalyst content. For example, in the case of the organometallic compound represented by the above chemical formula 3, aluminum may be used in an amount of 3 moles or more, or 10 moles or more, or 25 moles or more, and 200 moles or less, or 100 moles or less, per 1 mole of titanium in the catalyst.

[0217] The above-mentioned cocatalyst may be added to the polyethylene polymerization reaction after mixing with the Ziegler-Natta catalyst, or may be added separately before or after the addition of the Ziegler-Natta catalyst. Accordingly, the method for producing a polyethylene resin composition according to the present invention may further include a step of introducing the cocatalyst during the production of the first polyethylene in the first step.

[0218] In addition, the above primary polymerization reaction is performed under the condition of introducing hydrogen gas.

[0219] Since the amount of hydrogen gas introduced affects the properties of the copolymer being manufactured, the amount introduced is appropriately determined depending on the properties to be implemented. For example, in the present invention, the amount of hydrogen gas introduced during the first polymerization reaction may be 0.001 to 0.5 wt% based on the total weight of ethylene monomer introduced into the first reactor. When hydrogen gas is introduced in the above range, the combined properties of the polyethylene resin composition described above can be easily implemented. More specifically, it may be introduced in an amount of 0.001 wt% or more, or 0.01 wt% or more, or 0.05 wt% or more, or 0.07 wt% or more, and 0.5 wt% or less, or 0.3 wt% or less, or 0.15 wt% or less.

[0220] The reaction product generated by the polymerization reaction under the above polymerization conditions is continuously transferred to the second reactor connected to the first reactor.

[0221] In the second reactor, an additional polymerization reaction occurs between the first polyethylene transferred from the first reactor and the ethylene or C4 to C10 alpha olefin second comonomer introduced into the second reactor.

[0222] The above secondary polymerization reaction may also be carried out in the presence of a catalyst.

[0223] In this case, the catalyst that can be used is a Ziegler-Natta catalyst, as described in the first step. Accordingly, the Ziegler-Natta catalysts used in the first and second polymerization reactions may be the same or different. When the same Ziegler-Natta catalyst is used in the first and second polymerization reactions, it is easier to control the physical properties of the polyethylene resin composition produced and thereby implement the above physical property conditions.

[0224] In addition, the secondary polymerization reaction may be performed under conditions of hydrogen addition or non-addition. For example, when hydrogen gas is added, the hydrogen gas may be added in an amount of 0.001 to 0.05 wt% based on the total combined weight of monomers including the second comonomer of ethylene and alpha olefin introduced into the second reactor.

[0225] In addition, during the secondary polymerization reaction, only ethylene may be introduced without introducing a comonomer, or C4-C8 alpha olefin may be introduced as a comonomer.

[0226] When C4-C8 alpha olefin is introduced as a comonomer in the secondary polymerization reaction, the total amount of ethylene and the total amount of comonomer introduced into the first and second reactors can satisfy a weight ratio of 1:0.001 to 1:0.1. When the total amount of ethylene and the total amount of comonomer introduced into the first and second reactors satisfy the above-mentioned weight ratio range, the physical properties of the polyethylene resin composition described above can be more easily implemented.

[0227] In addition, the polymerization temperature (T1) and pressure (P1) during the first polymerization reaction are higher than the polymerization temperature (T2) and pressure (P2) during the second polymerization reaction. In addition to controlling the amount of comonomer input as described above, by increasing the temperature and pressure conditions during the first polymerization reaction, it is possible to more easily implement a bimodal molecular weight distribution and NCD structure in the polyethylene resin composition.

[0228] Specifically, the difference (T1-T2) between the polymerization temperature (T1) during the first polymerization reaction and the polymerization temperature (T2) during the second polymerization reaction may be 3°C or more, or 4°C or more, or 5°C or more, and 10°C or less, or 8°C or less, or 6°C or less.

[0229] In addition, the difference (P1-P2) between the pressure (P1) during the first polymerization reaction and the pressure (P2) during the second polymerization reaction may be 2 bar or more, or 3 bar or more, or 3.2 bar or more, and 6 bar or less, or 5.5 bar or less, or 5.3 bar or less.

[0230] In addition, while satisfying the above-mentioned temperature difference and pressure difference, in the manufacturing method according to the present invention, the polymerization temperature (T1) during the first polymerization reaction may be 70 to 90°C, and the polymerization temperature (T2) during the second polymerization reaction may be 70 to 90°C.

[0231] In addition, the pressure (P1) during the first polymerization reaction may be 5 to 10 bar, and the pressure (P2) during the second polymerization reaction may be 1 to 5 bar.

[0232] Through the two-step polymerization process described above, first polyethylene satisfying the above-mentioned physical property conditions is manufactured.

[0233] Next, the second stage is the second polyethylene manufacturing stage.

[0234] The above second polyethylene can be produced by polymerizing an ethylene monomer and a C4-C8 alpha-olefin monomer in a separate single reactor while adding hydrogen in the presence of a catalyst containing a metallocene compound represented by the above chemical formula 1.

[0235] The metallocene compound represented by the above chemical formula 1, unlike the conventionally used CGC (constrained geometry catalyst) type precursor, employs a bridge structure containing a boron anion. Conventional CGC type precursors include a neutral bridge structure containing silicon, resulting in a negatively charged ligand unit. This causes structural limitations, making it difficult to express various physical properties when producing olefin polymers.

[0236] On the other hand, the metallocene compound represented by the chemical formula 1 according to the present invention can have a neutral ligand unit because the bridge structure is negatively charged. The ligand unit of the present invention is a heterocycle Q of the chemical formula 1, wherein Y, an element of Q, forms a coordination bond with a metal, and Y', an element of Q adjacent to Y, is connected to the bridge. Accordingly, in the present invention, by employing various neutral ligand units satisfying the above structure, a catalyst having higher activity and high polymerizability than existing CGC precursors can be manufactured.

[0237] In addition, the metallocene compound represented by the above chemical formula 1 includes an alkyl or carboxylate as a metal substituent, which acts as a good leaving group and promotes the reaction with a cocatalyst such as MAO, thereby increasing the activity.

[0238] Therefore, by using the metallocene compound, it is possible to maintain a high melting index of polyethylene, reduce the low molecular weight region component, narrow the molecular weight distribution, and increase the SCB content to increase the molecular entanglement contribution (Effective Number of Physical Cross-link), thereby producing polyethylene with reduced total volatile organic compound (TVOC) emissions.

[0239] Specifically, in the above chemical formula 1, M may be zirconium (Zr).

[0240] Also, in the above chemical formula 1, R1 to R4 are each independently hydrogen, C 1-10 Alkyl or C 6-20 Aryl, or C in which R1 and R2 or R3 and R4 are combined with each other and are substituted or unsubstituted 6-20An aromatic ring can be formed. Preferably, R1 to R4 are each independently hydrogen or methyl, or R1 and R2 or R3 and R4 can be combined with each other to form a benzene ring or a 1,2,3,4-tetrahydronaphthalene ring, wherein the benzene ring or the 1,2,3,4-tetrahydronaphthalene ring is unsubstituted or substituted with 1 to 4 substituents selected from the group consisting of methyl, tertbutyl, and 4-tertbutylphenyl.

[0241] Also, in the above chemical formula 1, R5 and R6 are each independently C 1-10 Alkyl, or C 6-20 Aryl, or R5 and R6 are combined to form C 3-20 Aliphatic ring, or C 6-20 An aromatic ring can be formed. Preferably, R5 and R6 are each independently methyl or phenyl, or R5 and R6 can be combined with each other to form a cyclooctane ring.

[0242] More preferably, R5 and R6 can each be phenyl.

[0243] In addition, in the above chemical formula 1, X1 and X2 can each independently be methyl or acetate.

[0244] Also, in the above chemical formula 1, when X1 or X2 is -O(CO)R', R' can specifically be methyl.

[0245] Also, in the above chemical formula 1, X1 and X2 may be the same as each other.

[0246] In addition, in the above chemical formula 1, Q is C including at least one heteroatom selected from the group consisting of substituted or unsubstituted N, O and S. 2-20 It may be a heterocycle.

[0247] Specifically, Q may be a pyridine ring, a quinoline ring, a 4,5-dihydrooxazole ring, a pyrazole ring, or a benzoxazole ring, and Q may be unsubstituted or substituted with one to four substituents selected from the group consisting of methyl, isopropyl, and diphenylamino.

[0248] More specifically, Q may be a pyridine ring, a 4,5-dihydrooxazole ring, a pyrazole ring, or a benzoxazole ring, wherein Q may be unsubstituted or substituted with one to four substituents selected from the group consisting of methyl, isopropyl, and diphenylamino.

[0249] In addition, in the above chemical formula 1, Y is a heteroatom that forms a coordination bond with the metal M, and preferably, Y may be N.

[0250] Meanwhile, specific examples of the metallocene compound represented by the above chemical formula 1 include compounds represented by the following chemical formulas, but the present invention is not limited thereto:

[0251]

[0252]

[0253] .

[0254]

[0255] The metallocene compound represented by the above chemical formula 1 can be manufactured by, for example, a manufacturing method such as the following reaction scheme 1 when X1 and X2 are the same, but is not limited thereto, and can be manufactured according to a known manufacturing method for an organic compound and a metallocene compound. The above manufacturing method can be further specified in the manufacturing example described below.

[0256] [Reaction Formula 1]

[0257]

[0258] In the above reaction formula 1, B, M, R1 to R6, X1, X2, Q, Y and Y' are as defined in the above chemical formula 1.

[0259] Meanwhile, the catalyst composition for producing the second polyethylene may include the metallocene compound of the above chemical formula 1 as a single catalyst, or may include a carrier and optionally a cocatalyst together with the metallocene compound.

[0260] As the carrier, a carrier having a highly reactive hydroxyl group, silanol group, or siloxane group on the surface can be used. For this purpose, a carrier whose surface has been modified by calcination or whose surface has had moisture removed by drying can be used. For example, silica manufactured by calcining silica gel, silica dried at high temperature, silica-alumina, and silica-magnesia can be used, and these can typically contain oxides, carbonates, sulfates, and nitrates such as Na2O, K2CO3, BaSO4, and Mg(NO3)2.

[0261] Furthermore, any cocatalyst used in the polymerization of olefins under a typical metallocene catalyst can be used. Such cocatalysts facilitate the formation of bonds between hydroxyl groups on the carrier and Group 13 transition metals. Furthermore, since the cocatalyst exists solely on the surface of the carrier, it can contribute to securing the unique properties of the specific hybrid catalyst composition of the present invention without fouling, such as polymer particles sticking to the reactor walls or each other.

[0262] In addition, when producing the second polyethylene, a C4 to C8 alpha-olefin comonomer is introduced. Specifically, the C4 to C8 alpha-olefin may be one or more or a mixture of two or more selected from the group consisting of 1-butene, 1-pentene, 1-hexene, 4-methyl-1-pentene, and 1-octene, and preferably 1-butene or 1-hexene.

[0263] The C4 to C8 alpha-olefin comonomer introduced during the production of the second polyethylene may be introduced in an amount of 0.1 to 10 parts by weight, more specifically, 0.1 parts by weight or more, or 1 part by weight or more, or 5 parts by weight or more, or 6 parts by weight or more, and 10 parts by weight or less, or 8 parts by weight or less, based on 100 parts by weight of ethylene monomer. When the above-mentioned weight ratio range conditions are satisfied, the physical properties of the above-mentioned second polyethylene can be more easily implemented.

[0264] In addition, the polymerization reaction for producing the second polyethylene is performed under the condition of hydrogen input.

[0265] At this time, the amount of hydrogen input can be appropriately adjusted to implement the properties of the second polyethylene described above. For example, in the present invention, the amount of hydrogen gas input can be 0.0001 to 0.05 parts by weight based on the total weight of monomers including ethylene and C4 to C8 alpha olefin comonomers. When hydrogen gas is input in the above range, the combined properties of the polyethylene resin composition described above can be easily implemented. More specifically, it can be input in an amount of 0.0001 parts by weight or more, or 0.0005 parts by weight or more, or 0.0007 parts by weight or more, and 0.05 parts by weight or less, or 0.005 parts by weight or less, or 0.002 parts by weight or less.

[0266] In addition, the polymerization reaction for producing the second polyethylene can be performed under conditions of a temperature of 70 to 90°C and a pressure of 5 to 10 bar.

[0267] In addition, the manufacturing method according to the present invention may further include a step of performing an additional polymerization reaction on unreacted monomers included in the polymerization reaction product in a post reactor after the polymerization reaction for manufacturing the second polyethylene.

[0268] At this time, the additional polymerization reaction can be performed under the same reaction conditions as the above polymerization reaction, specifically, under conditions of a temperature of 70 to 90°C and a pressure of 5 to 10 bar.

[0269] Through the two-step polymerization process described above, a second polyethylene that satisfies the above-mentioned physical property conditions is manufactured.

[0270] Step 3 is a step of manufacturing a polyethylene resin composition by mixing the first polyethylene manufactured in the first step and the second polyethylene manufactured in the second step.

[0271] The first polyethylene and the second polyethylene may be mixed at an appropriate mixing ratio to realize the properties of the polyethylene resin composition described above. Specifically, the first polyethylene and the second polyethylene may be mixed at a weight ratio of 90:10 to 70:30.

[0272] In addition, the above mixing process is not particularly limited and can be performed according to a conventional mixing process.

[0273] Meanwhile, the manufacturing method according to the present invention may further include a step of melting and extruding the obtained mixture after the mixing process in the third step is completed.

[0274] A polyethylene resin composition in pellet form can be manufactured through the above-described melting and extrusion process.

[0275] Since the polymerization product obtained after the polymerization reaction in the first and second steps is in powder form, the types of antioxidants that can be used are limited, and the antioxidant content varies significantly from powder to powder, resulting in significant variations in the physical properties of products manufactured using the polymer. However, by performing the melting and extrusion processes, the components, including the antioxidant, are uniformly mixed, and the resulting product can possess uniform physical properties.

[0276] Meanwhile, in the present invention, the term "pellet" or "pellet-type" refers to small particles or pieces formed by extrusion of a raw material, and includes all shapes classified as pellets in the relevant technical field, such as circular, flat, sliver, polygonal, and rod-shaped. In addition, the size of the pellet is appropriately determined according to the use and shape and is not particularly limited. However, in order to be able to distinguish it from powder having a small average diameter of about 1 mm, the pellet in the present invention is defined as having an average diameter of 2 mm or more. Here, the "diameter" is the longest distance among any straight line distances on the outer surface of the pellet, and can be measured using an imaging microscope or the like.

[0277] The above melt extrusion process can be performed using a conventional extruder, and the specific method and conditions are not particularly limited as long as the morphological conditions of the pellet are satisfied.

[0278] In addition, during the melt extrusion, one or more additives such as an antioxidant, a stabilizer, a neutralizer, a slip agent, an anti-blocking agent, a UV stabilizer, an antistatic agent, etc. may be further added within a range that does not deteriorate the physical properties of the polyethylene resin composition. The polyethylene resin composition thus manufactured may further include one or more additives such as an antioxidant, a neutralizer, a slip agent, an anti-blocking agent, a UV stabilizer, an antistatic agent, etc. Meanwhile, in the present invention, the additives do not affect the physical properties of the polyethylene resin composition, and can improve the processability and the quality of the manufactured product when manufacturing a product using the resin composition.

[0279] For example, the antioxidant may include a phenol-based antioxidant; a phosphorus-based antioxidant; an amine-based antioxidant, etc., and any one of these or a mixture of two or more thereof may be used. Specific examples of the antioxidant include a phenol-based antioxidant such as tetrakis[methylene-3-(3,5-di-tert-butyl-4-hydroxyphenyl-propionate)]methane (CAS 6683-19-8) or 1,3,5-trimethyl-2,4,6-tris(3,5-di-tert-butyl-4-hydroxybenzyl)benzene; Phosphorus antioxidants such as tris(2,4-di-tert.-butylphenyl)phosphite, bis(2,4-di-tert.-butylphenyl)pentaerythritol diphosphite, and bis(2,4-dicumylphenyl)pentaerythritol diphosphite; or amine antioxidants such as phenylnaphthylamine, 4,4'-(α,α-dimethylbenzyl)diphenylamine, and N,N'-di-2-naphthyl-p-phenylenediamine; and any one of these or a mixture of two or more thereof may be used. Alternatively, commercially available Irganox™ 1010 (BASF), Irganox™ 3114 (BASF), Irganox™ 1076 (BASF), Irgafos™ 168 (BASF), Irgafos™ 626 (BASF), or Cyanox™ 1790 (CYTEC) may be used.

[0280] Among these, the polyethylene resin composition may include a mixture of a phenolic primary antioxidant and a phosphorus secondary antioxidant. At this time, the phenolic primary antioxidant may be added in an amount of 50 ppm or more, or 200 ppm or more, or 250 ppm or more, and 500 ppm or less, or 300 ppm or less, based on the total weight of the mixture of the first polyethylene and the second polyethylene, and the phosphorus secondary antioxidant may be added in an amount of 50 ppm or more, or 200 ppm or more, or 250 ppm or more, and 500 ppm or less, or 300 ppm or less, based on the total weight of the mixture of the first polyethylene and the second polyethylene. Accordingly, the polyethylene resin composition may include the phenolic primary antioxidant in an amount of 50 ppm or more, or 200 ppm or more, or 250 ppm or more, and 500 ppm or less, or 300 ppm or less, based on the total weight of the resin composition, and the phosphorus secondary antioxidant in an amount of 50 ppm or more, or 200 ppm or more, or 250 ppm or more, and 500 ppm or less, or 300 ppm or less.

[0281] In addition, the stabilizer may include magnesium aluminum hydroxy carbonate (hydrotalcite), aluminum magnesium zinc carbonate hydroxide, or aluminum magnesium calcium carbonate hydroxide, and any one of these or a mixture of two or more thereof may be used. In addition, commercially available DHT-4A (manufactured by Kyowa Chemical Industry) may also be used. The stabilizer may be added in an amount of 100 ppm or more, or 200 ppm or more, or 300 ppm or more, and 1000 ppm or less, or 700 ppm or less, or 500 ppm or less, based on the total weight of the mixture of the first polyethylene and the second polyethylene. Accordingly, the polyethylene resin composition may contain the stabilizer in an amount of 100 ppm or more, or 200 ppm or more, or 300 ppm or more, and 1000 ppm or less, or 700 ppm or less, or 500 ppm or less, based on the total weight of the resin composition.

[0282] In addition, examples of the neutralizing agent include calcium stearate (Ca-St), calcium palmitate, zinc stearate, or zinc palmitate, and one or a mixture of two or more thereof may be used. The neutralizing agent may be added in an amount of 100 ppm or more, or 300 ppm or more, or 500 ppm or more, and 1000 ppm or less, or 700 ppm or less, based on the total weight of the mixture of the first polyethylene and the second polyethylene. Accordingly, the polyethylene resin composition may contain the neutralizing agent in an amount of 100 ppm or more, or 300 ppm or more, or 500 ppm or more, and 1000 ppm or less, or 700 ppm or less, based on the total weight of the resin composition.

[0283] Additionally, the above melting and extrusion process can be performed according to a conventional method. For example, it can be performed at an extrusion temperature of 180 to 220°C, or 180 to 210°C, using an extruder such as a twin screw extruder.

[0284] A polyethylene resin composition satisfying the above-described physical property conditions is manufactured using the above-described manufacturing method.

[0285] The manufactured polyethylene resin composition exhibits excellent stretchability, high mechanical strength, and transparency. Accordingly, there is no concern about defects such as breakage or shrinkage during TD stretching when manufacturing biaxially oriented films. Furthermore, the manufactured biaxially oriented films are transparent and exhibit excellent stretch ratio and strength characteristics.

[0286] Accordingly, according to the present invention, a composition for manufacturing a film comprising the above-described polyethylene resin composition, and a film manufactured using the above-described polyethylene resin composition, specifically, a stretched film, are provided.

[0287] The composition for producing the above film can be produced in the same manner as a conventional composition for producing a film, except that it includes the above-described polyethylene resin composition.

[0288] In addition, the film-making composition may further include, in addition to the polyethylene resin composition described above, another polyethylene resin composition having a different composition or properties from the polyethylene resin composition. In this case, the other polyethylene resin composition may be included in a mixed state with the polyethylene resin composition, and the content thereof may be appropriately determined depending on the intended use and the desired properties. For example, the other polyethylene resin composition may be included in an amount greater than 0% by weight and less than or equal to 40% by weight based on the total weight of the film-making composition.

[0289] Additionally, the film may be specifically a stretched film or a biaxially stretched film.

[0290] The above film can be manufactured according to a method for manufacturing a conventional film or a stretched film, except that it contains the above-mentioned polyethylene resin composition.

[0291] The above film exhibits excellent stretchability and strength properties by including the above polyethylene resin composition. Specifically, the film according to the present invention may be a stretched film having a machine direction (MD) stretch ratio of 4 to 7 times, or 5 to 6 times, and a transverse direction (TD) stretch ratio of 4 to 9 times, or 8 to 9 times.

[0292] In addition, the film may satisfy the following conditions (e1) to (e3):

[0293] (e1) When the thickness is 2 mm, the MD direction tensile strength is 100 MPa or more and the TD direction tensile strength is 170 MPa or more as measured according to the standard of ASTM D638.

[0294] (e2) When the thickness is 2 mm, the 1% secant elastic modulus in the MD direction is 800 to 1400 MPa and the 1% secant elastic modulus in the TD direction is 1100 to 2300 MPa, measured according to ASTM D882.

[0295] (e3) When stretched at a stretch ratio of 5X8(MDXTD) times or more and the thickness is 20μm, the haze measured according to ISO 13468 standard: 30% or less.

[0296] More specifically, when the film has a thickness of 2 mm, the MD tensile strength measured according to the standard of ASTM D638 may be 100 MPa or more, or 105 MPa or more, or 109 MPa or more, or 112 MPa or more, or 114 MPa or more. Since the higher the tensile strength, the better, the upper limit thereof is not particularly limited, but as an example, the upper limit of the MD tensile strength may be 200 MPa or less, or 150 MPa or less, or 130 MPa or less, or 125 MPa or less, or 122 Mpa or less.

[0297] In addition, when the film has a thickness of 2 mm, the TD tensile strength measured according to the standard of ASTM D638 may be 170 MPa or more, or 175 MPa or more, or 178 MPa or more, or 179 MPa or more, or 180 MPa or more. Since the higher the tensile strength, the better, the upper limit thereof is not particularly limited, but as an example, the upper limit of the TD tensile strength may be 300 MPa or less, or 200 MPa or less, or 190 MPa or less, or 185 MPa or less, or 182 Mpa or less.

[0298] In addition, the film may have a 1% secant elastic modulus in the MD direction of 800 MPa or more, or 805 MPa or more, or 175 MPa or more, or 178 MPa or more, or 179 MPa or more, or 180 MPa or more, measured according to ASTM D882 when the thickness is specifically 2 mm. Since the tensile strength is better the upper limit thereof is not particularly limited, but as an example, the upper limit of the tensile strength in the TD direction may be 300 MPa or less, or 200 MPa or less, or 190 MPa or less, or 185 MPa or less, or 182 Mpa or less.

[0299] In addition, when the film is stretched at a stretch ratio of 5X8 (MDXTD) times or more and has a thickness of 20 μm, the haze value measured according to ISO 13468 may be specifically 30% or less, or 15% or less, or 10% or less, or 8% or less, or 5% or less, or 4% or less, or 3% or less, or 2% or less, or 1% or less. Since the lower the haze, the better, the lower limit thereof is not particularly limited, but may be, for example, 0% or more, or 0.1% or more.

[0300]

[0301] Hereinafter, preferred examples are presented to aid in understanding the present invention. However, the following examples are provided solely to facilitate a better understanding of the present invention and are not intended to limit the scope of the present invention.

[0302] Catalyst Manufacturing

[0303] Synthesis Example 1 (Ziegler-Natta catalyst for producing Polymer A)

[0304] 34 g of anhydrous magnesium chloride (99 wt% or more, moisture content less than 1%) was added to a 2-liter Buchi reactor dried with nitrogen, and 600 ml of purified hexane having a moisture content of less than 0.5 ppm was added to the reactor. While stirring the resulting reaction mass, 175 ml of anhydrous 2-ethyl-1-hexanol was added, and the mixture was stirred at a temperature of 130°C for about 2 hours to prepare a homogeneous solution of a magnesium support.

[0305] While stirring the above homogeneous solution at a temperature of 35°C and a speed of 200 rpm, 200 ml of TiCl4 was slowly added over 1 hour and stirred for another hour. During this process, a solid substance was generated. After the solid substance was precipitated, the liquid portion was removed, and the separated solid substance was washed several times with hexane until the titanium concentration of the washing solution became 0.5 mmol or less. To the washed solid substance, purified hexane was added so that the total volume became 1 liter. The titanium concentration in the resulting hexane slurry was 30 mM. To the hexane slurry, 7 ml of cyclohexyl chloride was added at a temperature of 40°C and stirred for 1 hour to obtain a Ziegler-Natta catalyst supported on magnesium.

[0306] The manufactured catalyst contained TiCl4 as a main catalyst and cyclohexyl chloride at a molar ratio of 0.13 per 1 mol of the main catalyst. In addition, the molar ratio of Mg:Ti in the catalyst was 4:1, and the average size of the catalyst particles was 8 μm.

[0307]

[0308] Synthesis Example 2 (Metallocene catalyst for producing Polymer B)

[0309] Step 1: Preparation of catalyst precursor

[0310] (1a)

[0311] 2-Bromopyridine (1 eq.) was dissolved in tetrahydrofuran (0.1 M), and n-butyllithium (1 eq.) was slowly added dropwise at -90 ℃, and stirred at the same temperature for 1 hour. Then, chlorodiphenylborane (1 eq.) was dissolved in toluene (0.3 M), and slowly added dropwise to the first reactant at -78 ℃, and stirred for 1 hour. After stirring at room temperature for 12 hours, the solvent was vacuum-dried, toluene was added, and the solid was removed through a filter, etc., and the residue was vacuum-dried to obtain diphenyl(pyridin-2-yl)borane.

[0312] After dissolving the diphenyl(pyridin-2-yl)borane (1 eq.) prepared above in tetrahydrofuran (0.1 M), a solution of lithium tetramethylcyclopentadienide (Li(CpMe4), 1 eq.) in tetrahydrofuran (0.1 M) was slowly added dropwise at 0 ℃ and stirred at room temperature overnight. After vacuum-drying the solvent, toluene / diethyl ether (volume ratio 3 / 1, 0.3 M) was added and dissolved, and MCl4 (1 eq.) was mixed with toluene (0.2 M) and added at -78 ℃ and stirred at room temperature overnight. After completion of the reaction, the solvent was vacuum-dried, dichloromethane was added, and salts were removed through a filter, etc., and the filtrate was vacuum-dried, and dichloromethane / hexane was added to recrystallize. The resulting solid was filtered and vacuum-dried to obtain Dichloro{diphenyl(pyridin-2-yl-κN)(η 5 -2,3,4,5-tetramethylcyclopenta-2,4-dien-1-ylidene)borate}zirconium(IV) was obtained.

[0313] Dichloro{diphenyl(pyridin-2-yl-κN)(η) prepared above5 -2,3,4,5-tetramethylcyclopenta-2,4-dien-1-ylidene)borate}zirconium(IV)(1 eq.) was dissolved in toluene / diethyl ether (volume ratio 3 / 1, 0.3 M), and then a solution of methyl lithium (2 eq.) in hexane or diethyl ether was slowly added dropwise at -78 ℃, and the mixture was stirred at room temperature for 12 hours. After completion of the reaction, the solvent was vacuum-dried, dichloromethane was added, and salts were removed through a filter, etc., and the filtrate was vacuum-dried, and then dichloromethane / hexane was added to recrystallize. The resulting solid was filtered and vacuum-dried to obtain a catalyst precursor (1a).

[0314] 1 H NMR (500 MHz, CDCl3, ppm): δ 8.32(d, 1H), 8.05(d, 4H), 7.70(t, 1H), 7.42(t, 1H), 7.40(t, 4H), 7.23(d, 1H), 7.17(t, 2H), 2.08(s, 6H), 1.93(s, 6H) 0.95(s, 6H)

[0315]

[0316] Step 2: Catalyst Preparation

[0317] After adding 50 mL of toluene to a pico reactor, 7 g of silica gel (SYLOPOL 952X, calcinated under 250 ℃) was added under Ar, and 8.5 mmol / g of methylaluminoxane (MAO) was slowly injected at room temperature and stirred at 95 ℃ for 24 hours to react. After completion of the reaction, cool to room temperature, leave for 15 minutes, and decant the solvent using a cannula. Add toluene (400 mL), stir for 1 minute, leave for 15 minutes, and decant the solvent using a cannula.

[0318] 60 μmol of the catalyst precursor (1a) prepared in the above step 1 was dissolved in 30 mL of toluene and transferred to a reactor using a cannula. The reaction was carried out with stirring at 80°C for 2 hours. After the reaction was completed and precipitation was complete, the mixture was cooled to room temperature and left for 15 minutes, and the solvent was decanted using a cannula. The upper layer solution was removed, and the remaining reaction product was washed with toluene. After washing again with hexane, 2 wt% of N,N-bis(2-hydroxyethyl)pentadeylamine (Atmer 163) as an antistatic agent based on the weight (g) of silica was dissolved in 3 mL of hexane and stirred at room temperature for 10 minutes. After the reaction was completed and precipitation was complete, the upper layer was removed and transferred to a glass filter to remove the solvent.

[0319] A silica-supported metallocene catalyst in the form of solid particles was obtained by primary drying under vacuum at room temperature for 5 hours and secondary drying under vacuum at 45°C for 4 hours.

[0320]

[0321] <First Polyethylene Manufacturing>

[0322] Manufacturing Example 1-1 (Manufacturing of polymer A1)

[0323] Polyethylene was produced by a method of producing polyethylene by polymerization in the presence of a Ziegler-Natta catalyst system using a bimodal slurry process using two 100 L continuous stirred tank reactors (CSTRs) and a post reactor.

[0324] Specifically, a catalyst slurry in which the Ziegler-Natta catalyst prepared in Synthesis Example 1 was dispersed at 12.7 g per 1 L of hexane, 18 kg / hr of hexane, 5.5 kg / hr of ethylene, 5 g / hr of hydrogen, and 160 ml / hr of triethylaluminum (TEAL) (concentration 300 mM) were injected into the first reactor, and a first polymerization reaction was performed to prepare the first polyethylene. At this time, the temperature in the first reactor was maintained at 80°C, the pressure was maintained at 6 bar, and the residence time of the reactants was maintained at 5.0 hour, and the polymer-containing slurry mixture formed as a result of the polymerization reaction was continuously transferred to a second reactor connected in series with the first reactor while maintaining a constant liquid level in the reactor.

[0325] When the polymer-containing slurry mixture manufactured in the first reactor was transferred to the second reactor, hexane 19 kg / hr, ethylene 4.5 kg / hr, and triethylaluminum (TEAL) 55 ml / hr (concentration 300 mM) were injected into the second reactor, and a secondary polymerization reaction was performed to manufacture second polyethylene. At this time, the temperature in the second reactor was maintained at 75°C, the pressure at 2 bar, and the residence time of the reactants at 2.4 hours, and the polymer mixture formed as a result of the polymerization reaction was continuously transferred to a post reactor connected in series with the second reactor while maintaining a constant liquid level in the reactor.

[0326] The temperature within the above-described post-reactor was maintained at 78°C. In the post-reactor, unreacted monomers within the polymer mixture transferred from the second reactor were polymerized. The resulting polymerization product was subjected to solvent removal and drying, yielding an ethylene homopolymer (A1) as the first polyethylene.

[0327]

[0328] Manufacturing Example 1-2 (Manufacturing of polymer A2)

[0329] An ethylene / 1-butene copolymer (A2) was produced as the first polyethylene by the same method as in Manufacturing Example 1-1, except that 1-butene was additionally injected into the second reactor at a rate of 4 ml / min.

[0330]

[0331] Manufacturing Example 1-3 (Manufacturing of polymer A3)

[0332] An ethylene / 1-butene copolymer (A3) was manufactured as the first polyethylene by the same method as in Manufacturing Example 1-1, except that hydrogen was injected into the first reactor at 7 g / hr, 1-butene was additionally injected at 4 ml / min, and 1-butene was additionally injected into the second reactor at 4 ml / min.

[0333]

[0334] <Manufacturing of Second Polyethylene>

[0335] Manufacturing Example 2-1 (Manufacturing of polymer B1)

[0336] Secondary polyethylene was produced by polymerization in the presence of a metallocene catalyst system using a single polymerization reactor and a post reactor.

[0337] Specifically, a catalyst slurry prepared by dispersing the metallocene catalyst of Synthesis Example 2 in an amount of 6.5 g per 1 L of hexane in a polymerization reactor was injected at 145 ml / hr, hexane at 18 kg / hr, ethylene at 10 kg / hr, hydrogen at 0.1 g / hr, 1-hexene at 0.6 kg / hr, and triethylaluminum (TEAL) at 20 ml / hr (concentration 300 mM), and a polymerization reaction was performed. At this time, the temperature in the polymerization reactor was maintained at 70°C, the pressure at 7 bar, and the residence time of the reactants at 3.0 hours. When the polymerization reaction was completed, the prepared polymer-containing slurry was transferred to a post reactor.

[0338] The above post-reactor was maintained at 70°C, and polymerization of unreacted monomers in the polymer-containing slurry produced in the polymerization reactor was performed. The resulting polymerization product was subjected to solvent removal and drying to obtain an ethylene / 1-hexene copolymer (B1) as a second polyethylene.

[0339]

[0340] Manufacturing Example 2-2 (Manufacturing of polymer B2)

[0341] An ethylene / 1-octene copolymer (B2) was produced as a second polyethylene in the same manner as in Manufacturing Example 2-2, except that 0.6 kg / hr of 1-octene instead of 1-hexene and 0.15 g / hr of hydrogen were injected into the polymerization reactor.

[0342]

[0343] Experimental Example 1

[0344] The physical properties of the first and second polyethylenes manufactured in the above manufacturing examples were measured using the following methods. The results are shown in Table 1.

[0345] (1) Melting index (MI) 2.16 )[g / 10min]

[0346] MI under 190℃ and 2.16kg load conditions according to ASTM D1238 2.16 was measured.

[0347]

[0348] (2) MFRR(MI 21.6 / MI 2.16 )

[0349] MI under 190℃ and 21.6kg load conditions according to ASTM D1238 21.6 Measure MI 21.6 MI measured above (190 ℃, 21.6 kg load) 2.16 (190 ℃, 2.16 kg load) divided by MFRR(MI) 21.6 / MI 2.16 ) was produced.

[0350]

[0351] (3) Density [g / cm 3 ]

[0352] Density was measured according to ASTM D792.

[0353]

[0354] (4) Weight average molecular weight (Mw) and molecular weight distribution (Mw / Mn)

[0355] For the polyethylene manufactured in the above manufacturing example, the weight average molecular weight (Mw) and number average molecular weight (Mn) were measured through gel permeation chromatography (GPC) analysis, and the measured weight average molecular weight was divided by the number average molecular weight to obtain the molecular weight distribution (MWD).

[0356] Specifically, the measurement sample was measured using a Waters PL-GPC220 instrument using a Polymer Laboratories PLgel MIX-B 300 mm length column. The measurement temperature was 160℃, 1,2,4-trichlorobenzene was used as a solvent, and the flow rate was measured at a rate of 1 mL / min. The polyethylene sample was pretreated by dissolving it in 1,2,4-trichlorobenzene containing 0.025% BHT at 160℃ for 4 hours using a GPC analysis instrument PL-GP220, and then prepared at a concentration of 20 mg / 10 mL, and then supplied in an amount of 200 μL. The values ​​of Mw and Mn were measured using a calibration curve formed using a polystyrene standard foam. The weight average molecular weights (g / mol) of polystyrene standards were 9 types: 2,000 / 10,000 / 30,000 / 70,000 / 200,000 / 700,000 / 2,000,000 / 4,000,000 / 10,000,000.

[0357]

[0358] In the above table 1, k is 'x10 3 ' means.

[0359]

[0360] <Manufacture of polyethylene resin composition>

[0361] Examples 1 to 18 and Comparative Examples 1 to 17

[0362] The first and second polyethylenes manufactured in the above manufacturing examples were mixed at various weight ratios to manufacture a polyethylene resin composition.

[0363] Specifically, the first and second polyethylenes were mixed under the weight ratio conditions described in Table 2 or Table 3 below, and 300 ppm of DHT-4A (Magnesium aluminum hydroxycarbonate) manufactured by Kyowa Chemical Industry Co., Ltd. as a stabilizer, 300 ppm of Irganox 1010 manufactured by BASF Co., Ltd. as a primary antioxidant, and 300 ppm of Irgafos 168 manufactured by BASF Co., Ltd. as a secondary antioxidant were added based on the total weight of the resulting mixture, and then mixed, and extruded at an extrusion temperature of 190°C using a twin screw extruder (TEK 30 MHS, manufactured by SMPLATECH CO., Ltd., diameter 32 pi, L / D=40) to manufacture a polyethylene resin composition in the form of pellets.

[0364]

[0365] Comparative examples 18 to 22

[0366] A polyethylene resin composition was prepared by mixing the first and second polyethylenes according to the same method as in Example 1, except that the first and second polyethylenes were mixed according to the weight ratio conditions described in Table 3.

[0367] <The first polyethylene>

[0368] A4: MI 2.16 =50 g / 10min and density=0.965 g / cm 3 Polyethylene of

[0369] A5: MI 2.16=5.1 g / 10min and density=0.961 g / cm 3 Polyethylene of

[0370] <2nd Polyethylene>

[0371] B3: MI 2.16 =0.4 g / 10min and density=0.940 g / cm 3 Polyethylene of

[0372] B4: MI 2.16 =3.5 g / 10min and density=0.904 g / cm 3 Polyethylene of

[0373] B5: MI 2.16 =1.0 g / 10min and density=0.905 g / cm 3 Polyethylene of

[0374] B6: MI 21.6 =3.5 g / 10min and density=0.940 g / cm 3 Polyethylene (TL2000, manufactured by LG Chemical)

[0375]

[0376] Comparative Example 23

[0377] As a polyethylene resin composition, LUTENE-H PE0235 manufactured by LG Chemical was used.

[0378]

[0379] Comparative Example 24

[0380] As a polyethylene resin composition, LUTENE-H ME5500 manufactured by LG Chemical was used.

[0381]

[0382]

[0383]

[0384]

[0385]

[0386] Experimental Example 2

[0387] Temperature Rising Elution Fractionation (TREF) analysis was performed on the polyethylene resin compositions of the above examples and comparative examples using the following method, and the content ratio of polymer fractions eluted by temperature range was obtained.

[0388] Specifically, a 30 mg polyethylene resin composition sample was introduced into a TREF device (manufactured by PolymerChar), dissolved in 20 mL of trichlorobenzene solvent at 150°C for 60 minutes, and then stabilized at 140°C for 20 minutes. This was cooled to 35°C at a cooling rate of 0.5°C / min and maintained for 10 minutes. Thereafter, the column was heated at a heating rate of 1°C / min from 35°C to 140°C, while the solvent trichlorobenzene was passed through the column at a flow rate of 0.5 mL / min, and the concentration of the eluted polymer was measured. Other measurement conditions were as follows. From the concentration measurement results, a TREF analysis graph was derived in which the elution temperature (Te) (°C) was plotted on the x-axis and the elution amount (dw / dt) was plotted on the y-axis.

[0389] <TREF 측정 조건>

[0390] Dissolution Rate: 40 ℃ / min

[0391] Stabilization Rate: 40℃ / min

[0392] Crystallization Rate: 0.5℃ / min

[0393] Elution Rate: 1 ℃ / min

[0394] Cleaning rate: 30 ℃ / min

[0395] Dissolution temperature: 150℃

[0396] Stabilization temperature: 140℃

[0397] Crystallization temperature: 35℃

[0398] Elution init temp: 35 ℃

[0399] Elution temperature: 140 ℃

[0400] Post-elution temperature: 150℃

[0401] Cleaning temperature: 150 ℃

[0402] Dissolution time: 60 min

[0403] Stabilization time: 20 min

[0404] Crystallization time: 10 min

[0405] Pre-injection time: 10 min

[0406] Soluble Fraction time: 10 min

[0407] Post-elution time: 10 min

[0408] Cleaning time: 10 min

[0409] Cleaning cycles: 1

[0410]

[0411] Based on the total weight of the entire elution fraction obtained through the above TREF analysis, the content ratio of the polymer fraction eluted by temperature range was calculated as a percentage (weight %). The results are shown in Tables 4 and 5 below.

[0412] In addition, the results of temperature rise elution fraction (TREF) analysis for the polyethylene resin compositions of Examples 5 and 6 and Comparative Examples 10 and 14 are shown in Fig. 1.

[0413]

[0414] Example No. 25-90℃40-70℃90-120℃100-105℃125.32.774.744.2230.88.769.240.9336.214.763.837.5426.43.973.643.5531.08.969.040.7634.913.265.138.3729.06.871.041.9834.112.365.938.9939.117. 860.935.81030.07.970.041.31134.412.765.638.71242.421.457.633.81332.710.867.339.71437.315.962.736.91542.321.057.734.01632.010.168.040.11739.518.360.535.51845.224.654.832.0

[0415] Comparative Example No. 25-90℃40-70℃90-120℃100-105℃119.80.380.247.5223.91.276.145.0328.05.772.042.5474.456.625.614.2585.468.514.67.5622.60.377.445.9739.017.761.035.9823.00.377.045.5942.821.957.233.51026.54.073.543.51141.620.658.434.21227.0 4.673.043.21345.424.854.631.91430.48.269.641.11544.323.555.732.61630.98.869.140.81748.127.751.930.31817.10.182.949.21927.35.072.742.92023.50.876.545.32123.40.676.645.42218.90.181.148.02329.47.270.641.72428.05.772.042.5

[0416] In Tables 4 and 5 above, the temperature range indicator "-" includes both the lower and upper limits of the numerical range. For example, 25-90℃ means the range is 25℃ or higher and 90℃ or lower.

[0417]

[0418] Experimental Example 3

[0419] The physical properties of the polyethylene resin compositions manufactured in the above examples and comparative examples were measured as follows, and the results are shown in Tables 6 and 7 below.

[0420] (1) Density: Measured at 23℃ according to ASTM D792.

[0421]

[0422] (2) Melting index (MI) 2.16 ): MI at 190℃ and 2.16kg load condition according to ASTM D1238 2.16 was measured.

[0423]

[0424] (3) MFRR(MI 21.6 / MI 2.16 )

[0425] MI under 190℃ and 21.6kg load conditions according to ASTM D1238 21.6 Measure MI 21.6 MI measured above (190 ℃, 21.6 kg load) 2.16 (190 ℃, 2.16 kg load) divided by MFRR(MI) 21.6 / MI 2.16 ) was produced.

[0426]

[0427] (4) Weight average molecular weight (Mw) and molecular weight distribution

[0428] The polyethylene resin compositions according to the above examples and comparative examples were analyzed by gel permeation chromatography (GPC) to measure the weight average molecular weight (Mw) and number average molecular weight (Mn), and the molecular weight distribution (MWD) was obtained by dividing the weight average molecular weight measured above by the number average molecular weight.

[0429] Specifically, the measurement sample was measured using a Waters PL-GPC220 instrument using a Polymer Laboratories PLgel MIX-B 300 mm length column. The measurement temperature was 160°C, 1,2,4-trichlorobenzene was used as a solvent, and the flow rate was measured at a rate of 1 mL / min. The polyethylene resin composition sample was pretreated by dissolving it in 1,2,4-trichlorobenzene containing 0.025% BHT at 160°C for 4 hours using a GPC analysis instrument PL-GP220, and then preparing it at a concentration of 20 mg / 10 mL, and then supplying it in an amount of 200 μL. The values ​​of Mw and Mn were measured using a calibration curve formed using polystyrene standards. The weight average molecular weights (g / mol) of polystyrene standards were 9 types: 2,000 / 10,000 / 30,000 / 70,000 / 200,000 / 700,000 / 2,000,000 / 4,000,000 / 10,000,000.

[0430] In addition, through the above GPC analysis, a molecular weight distribution graph was drawn with the logarithmic value (log Mw) of the weight average molecular weight (Mw) (g / mol) as the x-axis and the molecular weight distribution (dwt / dlog Mw) for the logarithmic value as the y-axis, and the shape of the molecular weight distribution curve was confirmed.

[0431]

[0432] (5) Stress relaxation time (λ) (sec) and shear thinning index

[0433] The viscosity of a polyethylene resin composition was measured using a rotational rheometer at a temperature of 190°C, a strain of 0.5%, and an angular frequency of 0.01 Hz to 100 Hz. Then, the stress relaxation time (λ) (seconds) and shear thinning index of polyethylene were obtained using the Carreau-Yasuda Model of the following mathematical equation 1.

[0434] Specifically, for the polyethylene resin compositions of the above examples and comparative examples, compression molded samples were prepared using 25 mm diameter plates (plate-to-plate gap = 1.2 mm) in a nitrogen atmosphere at 190°C, and then oscillatory shear tests were performed using DHR-2 from TA-Instrument at a temperature of 190°C and at each frequency condition of 0.01 Hz to 100 Hz (corresponding to 0.0628 rad / s to 628 rad / s) while continuously applying strain (0.5%) within the linear viscosity range. Five measurement points were created per 10 units.

[0435] Through the above oscillatory shear experiment, the viscosity value was measured, and a log-log graph was obtained with each frequency (Hz) as the x-axis and the viscosity measurement value η (Pa·s) of the polyethylene resin composition measured above as the y-axis, and then the curve was fitted with the Carreau-Yasuda Model of the following mathematical equation 1, and the zero-point shear viscosity (η0) (Pa·s) and parameter a value, as well as the stress relaxation time (λ) (sec) and shear thinning index were calculated, respectively. In this experimental example, the zero-point shear viscosity (η0), parameter a value, stress relaxation time (λ), and shear thinning index were obtained, respectively, using the TRIOS program of TA Instruments.

[0436] [Mathematical Formula 1]

[0437]

[0438] In the above mathematical formula 1,

[0439] The above η is the viscosity (Pa·s) of the polyethylene resin composition measured above,

[0440] The above η0 is the zero-point shear viscosity (Pa·s), and is the viscosity in the section where the viscosity value does not change when the angular frequency approaches 0. In the present invention, a log-log graph with each frequency (Hz) as the x-axis and the viscosity measurement value η (Pa·s) of the polyethylene resin composition measured above as the y-axis was calculated by fitting the curve to the Carreau-Yasuda Model of the above mathematical equation 1.

[0441] Also, the above is the shear rate applied to the polyethylene resin composition, which is the same value as each frequency converted to rad / s by the Cox Merz Rule,

[0442] The above λ is the stress relaxation time (seconds) of the polyethylene resin composition, and in the present invention, it was calculated by fitting a log-log graph with each frequency (Hz) as the x-axis and the viscosity measurement value η (Pa·s) of the polyethylene resin composition measured above as the y-axis using the Carreau-Yasuda Model of the above mathematical formula 1.

[0443] In addition, the above n is a shear thinning index, and in the present invention, a log-log graph with each frequency (Hz) as the x-axis and the viscosity measurement value η (Pa·s) of the polyethylene resin composition measured above as the y-axis was calculated by fitting the curve to the Carreau-Yasuda Model of the above mathematical formula 1.

[0444] The above a is a shape parameter that transitions between the Newtonian plateau and the power law region, and in the present invention, a log-log graph with each frequency (Hz) as the x-axis and the viscosity measurement value η (Pa·s) of the polyethylene resin composition measured above as the y-axis was calculated by fitting the curve to the Carreau-Yasuda Model of the above mathematical formula 1.

[0445]

[0446]

[0447]

[0448]

[0449] In the above table, N / A means not measured.

[0450]

[0451] Experimental Example 4

[0452] The stretchability and film properties of the stretched film produced using the polyethylene resin compositions of the above examples and comparative examples were evaluated by the following methods.

[0453] (1) Manufacture of cast film and biaxially oriented film

[0454] The polyethylene resin compositions of the above examples and comparative examples were manufactured into cast sheets having a thickness of 0.72 mm using a Bruckner lab extruder line (L / D ratio: 42, Screw diameter: 25 mm, Melt / T-Die temperature: 250°C).

[0455] For the manufactured cast sheet, biaxial stretching was performed into a polyethylene film measuring 90 mm x 90 mm (width x length) using a Bruckner Lab Stretcher KARO 5.0 film biaxial stretching machine. At this time, after preheating for 60 seconds at a temperature condition of 110 to 130°C, sequential stretching was performed in the MD → TD direction, and the stretching speed was 300 % / s.

[0456] The final film thickness was 20㎛ based on a stretching ratio of 5X8.

[0457] However, the polyethylene resin compositions of Comparative Examples 1, 6, 8 and 19 were not stretchable and thus could not be used to produce a biaxially stretched film.

[0458] <Conditions for manufacturing stretch film>

[0459] Sample size: 90 mm x 90 mm

[0460] Stretch profile: sequential

[0461] Stretch rate: 5 x 8

[0462] Stretch speed: 100-400 % / s

[0463] Stretch temp: 110-130 ℃

[0464] Preheat: 60 s

[0465]

[0466] (2) Maximum extension ratio

[0467] For the cast film manufactured in the above (1), the maximum stretching ratio in the MD x TD direction that can be stretched without causing breakage or defects in the film was measured during biaxial stretching using a Lab Stretcher KARO 5.0 film biaxial stretching machine from Bruckner.

[0468] <Measurement conditions>

[0469] Sample size: 90 mm x 90 mm

[0470] Stretch profile: sequential

[0471] Stretch rate: 5 to 6 times in MD direction, 4 to 9 times in TD

[0472] Stretch speed: 100 to 400 % / s

[0473] Stretch temp.: 110 to 130 ℃

[0474] Preheat temp.: 100 s.

[0475]

[0476] (3) Toughness

[0477] Toughness was measured according to ASTM D638.

[0478] Specifically, the polyethylene resin compositions of the above examples and comparative examples were hot pressed (190°C) to produce 2 mm thick sheets, and then cut to produce PE specimens according to ASTM D638 standards. The PE specimens produced above were horizontally fixed on a Zwick tensile tester (UTM), and a tensile test was performed by pulling the upper PE sheet portion in the MD or TD direction at room temperature (23±5°C). The tensile strength when pulled at a speed of 50 mm / min was expressed as Toughness [MPa]. When the tensile strength value in the MD direction is 100 MPa or more, and when the tensile strength value in the TD direction is 170 MPa or more, it is judged to be excellent.

[0479]

[0480] (4) Stiffness

[0481] Stiffness was measured according to ASTM D 882.

[0482] Specifically, the polyethylene resin compositions of the above examples and comparative examples were hot pressed (190°C) to produce 2 mm thick sheets, and then cut to produce PE specimens according to ASTM D 882 standards. The PE specimens produced above were horizontally fixed on a Zwick tensile tester (UTM), and a tensile test was performed by pulling the upper PE sheet portion at room temperature (23±5°C). The 1% secant modulus of elasticity (or Modulus of Elasticity) when pulled at a speed of 5 mm / min was expressed as Stiffness [MPa]. If the 1% secant modulus of elasticity or Stiffness in the MD and TD directions is 800 MPa or more, it is judged to be excellent.

[0483]

[0484] (5) Transparency

[0485] For the biaxially oriented film manufactured in the above (1), the haze [%] of the film was measured according to the ISO 13468 standard. A smaller haze value indicates better transparency, and a haze value of 30% or less is generally considered to be excellent.

[0486]

[0487]

[0488]

[0489]

[0490] In the above table, N / A means not measured.

[0491] When a stretched film was manufactured using the polyethylene resin composition of the example, it was confirmed that the mechanical properties and transparency were improved along with excellent stretch ratio characteristics.

[0492] Meanwhile, in the case of Comparative Examples 1, 6, 8 and 18, stretching was impossible due to the high density of the polyethylene resin composition, and thus a stretched film could not be manufactured.

[0493] In addition, in the case of Comparative Examples 4 and 5 containing only low-density polyethylene, transparency was excellent due to the low-density characteristics of the resin composition, but the content of the elution fraction in the low-temperature region was high and the content of the elution fraction in the high-temperature region was low in the TREF analysis, so that the stiffness in the MD and TD directions was greatly reduced.

[0494] Meanwhile, in Comparative Examples 14 and 16, which included a mixture of low-density and high-density polyethylene, but had a high content of high-density first polyethylene and a low content of low-density second polyethylene, the Toughness and transparency properties were significantly deteriorated due to an excessively broad molecular weight distribution. In addition, in Comparative Examples 7, 9, 11, 13, 15, and 17, which had a low content of high-density first polyethylene and a high content of low-density polyethylene, the transparency was excellent, but the Stiffness was significantly deteriorated along with the Tensile Strength in the TD direction during film production due to the low MFRR properties or low density.

[0495] In addition, Comparative Examples 2, 3, 10, and 12, which had a wide molecular weight distribution along with a high MFRR, showed deterioration in elongation characteristics, toughness in the MD and TD directions, and transparency characteristics, and among these, the deterioration in transparency characteristics was the greatest.

[0496] In addition, in the case of Comparative Examples 19 to 21, it was difficult to manufacture the cast sheet due to the high MI and MFRR, and the stretchability was poor during film manufacture. In addition, due to the wide molecular weight distribution, the manufactured film showed reduced tensile strength and transparency characteristics in the TD direction.

[0497] Comparative Example 22 had excessively high MI and MFRR, which resulted in a processing viscosity that was too low, making it difficult to manufacture a cast sheet with a normal thickness deviation. In addition, due to the low elution content in the low-temperature region during TREF analysis, the stretchability was poor during film manufacture.

[0498] In addition, Comparative Example 23 had poor stretchability during film production due to its low MI and high viscosity characteristics, and Comparative Example 24 had poor stretchability during film production due to its high MI and low viscosity characteristics.

Claims

1. A polyethylene resin composition satisfying the following conditions (a1) to (a5): (a1) MI 2.16 (ASTM D1238, 190℃, 2.16 kg): 0.5 to 3.0 g / 10 min (a2) Density (ASTM D792): 0.940 to 0.955 g / cm3 (a3) MFRR(MI 21.6 / MI 2.16 ): 60 or more and less than 80 (a4) Molecular weight distribution (Mw / Mn): 10 to 14 (a5) When analyzing the temperature rise elution fraction (TREF), for the total weight of the entire elution fraction, Content of polymer fraction eluting in the range of 25 to 90°C: 20 to 50 wt%, and Content of polymer fraction eluting in the range of 90 to 120°C: 50 to 80 wt%.

2. In paragraph 1, The above polyethylene resin composition satisfies the following conditions when analyzing the temperature rise elution fraction: For the total weight of the entire elution fraction, Content of polymer fraction eluting in the range of 40 to 70°C: 1 to 30 wt%; and Content of polymer fraction eluting in the range of 100 to 105°C: 30 to 45 wt%.

3. In paragraph 1, The polyethylene resin composition further satisfies one or more of the conditions (b1) to (b3) below: (b1) Weight average molecular weight (Mw): 100,000 to 160,000 g / mol (b2) Stress relaxation time: 0.1 to 0.9 seconds (b3) Shear discourse index: 0.2 to 0.

5.

4. In paragraph 1, The above polyethylene resin composition, Density (ASTM D792) 0.950 g / cm3 or higher and MI 2.16 (ASTM D1238, 190℃, 2.16 kg) First polyethylene satisfying the condition of 0.5 to 2 g / 10 min; and Density (ASTM D792) 0.925 g / cm3 or less and MI 2.16 (ASTM D1238, 190℃, 2.16 kg) A polyethylene resin composition comprising 1 to 5 g / 10 min of second polyethylene; in a weight ratio of 90:10 to 70:

30.

5. In paragraph 4, The above first polyethylene is a polyethylene resin composition that further satisfies the conditions (c1) to (c5) below: (c1) Density (ASTM D792): 0.950 to 0.965 g / cm 3 (c2) MI 2.16 (ASTM D1238, 190℃, 2.16 kg): 0.5 to 2 g / 10min (c3) MFRR(MI 21.6 / MI 2.16 ): 50 to 100 (c4) Weight average molecular weight (Mw): 130,000 to 160,000 g / mol (c5) Molecular weight distribution (Mw / Mn): 10 to 16.

6. In paragraph 4, A polyethylene resin composition wherein the first polyethylene is at least one of an ethylene homopolymer and an ethylene / C4-C8 alpha-olefin copolymer.

7. In paragraph 4, The above second polyethylene is a polyethylene resin composition that satisfies the conditions (d1) to (d5) below: (d1) Density (ASTM D792): 0.910 to 0.925 g / cm 3 (d2) MI 2.16 (ASTM D1238, 190℃, 2.16 kg): 1 to 5 g / 10min (d3) MFRR(MI 21.6 / MI 2.16 ): 10 to 50 (d4) Weight average molecular weight (Mw): 50,000 to 130,000 g / mol (d5) Molecular weight distribution (Mw / Mn): 1 to 10.

8. In paragraph 4, A polyethylene resin composition wherein the second polyethylene is an ethylene / C4-C8 alpha olefin copolymer.

9. A first step of manufacturing first polyethylene by first polymerizing ethylene in the presence of a Ziegler-Natta catalyst in a first reactor, then moving the produced polymerization product to a second reactor, and adding at least one of ethylene and C4-C8 alpha-olefin to perform a second polymerization reaction; A second step of producing second polyethylene by polymerizing ethylene and C4-C8 alpha-olefin while adding hydrogen in the presence of a catalyst containing a metallocene compound represented by the following chemical formula 1 in a separate single reactor; and A third step of mixing the first polyethylene and the second polyethylene in a weight ratio of 90:10 to 70:30; Method for producing a polyethylene resin composition according to Article 1: [Chemical Formula 1] In the above chemical formula 1, B is boron, M is a group 4 transition metal, R1 to R4 are each independently hydrogen, C 1-20 Alkyl, C 3-20 Cycloalkyl, or C 6-20 Aryl, or C in which R1 and R2 or R3 and R4 are combined with each other and are substituted or unsubstituted 6-60 Forming an aromatic ring, R5 and R6 are each independently C 1-20 Alkyl, C 3-20 Cycloalkyl, or C 6-20 Aryl, or R5 and R6 are combined to form C 3-60 Aliphatic ring or C 6-60 Forming an aromatic ring, X1 and X2 are each independently C 1-20 Alkyl or -O(CO)R', where R' is C 1-20 It is alkyl, Q is C comprising at least one selected from the group consisting of substituted or unsubstituted N, O and S. 2-60 It is a heterocycle, Y and Y' are elements that constitute Q, Y is N, O, or S, Y' is an element of Q adjacent to Y, and is either N or C.

10. In paragraph 9, A method for producing a polyethylene resin composition, wherein the Ziegler-Natta catalyst is a magnesium-supported titanium catalyst.

11. In paragraph 9, A method for producing a polyethylene resin composition, wherein the Ziegler-Natta catalyst further comprises a halogenated hydrocarbon.

12. In paragraph 9, A method for producing a polyethylene resin composition, wherein the first polymerization reaction in the first step is performed under conditions in which hydrogen gas is introduced in an amount of 0.001 to 0.5 wt% based on the total weight of ethylene introduced into the first reactor.

13. In paragraph 9, A method for producing a polyethylene resin composition, wherein the metallocene compound represented by the above chemical formula 1 is any one of the compounds represented by the following chemical formula: .

14. In paragraph 9, A method for producing a polyethylene resin composition, wherein in the second step, the C4-C8 alpha-olefin monomer is added in an amount of 0.1 to 10 parts by weight based on 100 parts by weight of ethylene monomer.

15. In paragraph 9, A method for producing a polyethylene resin composition, wherein the polymerization reaction in the second step is performed under conditions in which hydrogen gas is introduced in an amount of 0.0001 to 0.05 wt% based on the total weight of monomers including ethylene monomer and C4-C8 alpha-olefin monomer.

16. A film comprising a polyethylene resin composition according to paragraph 1.

17. In paragraph 16, The above film satisfies the conditions (e1) to (e3) below: (e1) When the thickness is 2 mm, the MD direction tensile strength is 100 MPa or more and the TD direction tensile strength is 170 MPa or more as measured according to the standard of ASTM D638. (e2) When the thickness is 2 mm, the 1% secant elastic modulus in the MD direction is 800 to 1400 MPa and the 1% secant elastic modulus in the TD direction is 1100 to 2300 MPa, measured according to ASTM D882. (e3) When stretched at a stretch ratio of 5X8(MDXTD) times or more and the thickness is 20μm, HAZE measured according to ISO 13468 standard: 30% or less.

Citation Information

Patent Citations

  • Polyethylene resin composition and laminated film composed of the composition

    JP2004256613A

  • Physical blends of polyethylenes

    KR1020040047921A

  • Polyethylene blends with good contact transparency

    KR1020070041677A

  • Polyethylene resin compositions for stretch wrap film and film manufactured thereby

    KR1020140002351A

  • Method, program, and apparatus for processing medical data for training of deep learning model

    KR102526487B1