Laminate and functional film comprising same
The laminate structure with a metal deposition layer and conductive polymer coating layer addresses the visibility and energy efficiency issues of existing window coatings by controlling solar energy transmittance and reflectance, achieving efficient energy shielding and improved visibility.
Patent Information
- Application Number
- PCT/KR2024/006240
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-05-15
- Filing Date
- 2024-05-09
- Publication Date
- 2024-11-21
AI Technical Summary
Existing external light blocking coatings for windows, often using metal or metal alloys, suffer from excessive low visible light transmittance and absorption, leading to visibility issues due to reflection phenomena, necessitating a solution that balances energy efficiency with visibility.
A laminate structure comprising a metal deposition layer on the outer surface and a polymer coating layer on the inner surface, with the polymer coating layer made of conductive polymers like polyaniline, polythiophene, and PEDOT:PSS, and a thickness between 0.3 μm and 3.0 μm, to control total solar energy transmittance and visible light reflectance.
The laminate effectively reduces total solar energy transmittance to 20% or less, maintains high visible light transmittance of 25 to 30%, and achieves low internal visible light reflectance of 25% or less, enhancing energy efficiency while improving visibility by minimizing reflection.
Smart Images

Figure KR2024006240_21112024_PF_FP_ABST
Abstract
Description
Laminate and functional film comprising same
[0001] The present invention relates to a laminate having a heat-blocking function and low-reflection properties and a functional film including the laminate.
[0002]
[0003] External light blocking coatings are often applied to vehicles and / or building windows. In particular, some countries, including South Korea, support projects to improve the energy performance of private buildings through laws such as the Green Building Promotion Act. Furthermore, these laws mandate the installation of high-performance windows and doors, which require them to meet window energy efficiency ratings. Therefore, demand for thermal energy blocking films to ensure energy efficiency in heating and cooling is expected to grow further.
[0004] It is common to apply metal or metal alloy to the functional layer for applying external light blocking coating film to windows, but in this case, a reflection phenomenon may occur.
[0005] For example, Korean Patent Publication No. 10-1470901 provides a heat reflective film including a substrate layer mainly made of PET or PC; a coating layer on which a coating agent that reflects infrared rays while absorbing heat is deposited on the upper portion of the substrate layer; an adhesive layer on which an adhesive that selectively blocks ultraviolet and infrared rays is adhered on the lower portion of the substrate layer; and a thin film layer on which a thin film having visibility and shielding properties is selectively further deposited between the substrate layer and the coating layer or the substrate layer and the adhesive layer. However, the visible light transmittance and / or absorbance may be excessively low, and the total solar energy transmittance may be too low, which may make it difficult to secure a field of vision.
[0006] Therefore, there is a need to develop a functional film that can secure internal energy efficiency while ensuring visibility by appropriately lowering the transmittance.
[0007]
[0008] The present invention aims to solve the above-described problems by providing a laminate having a lowered total solar energy transmittance and a functional film including the laminate.
[0009] In addition, the present invention aims to provide a laminate and a functional film including the laminate, which improve the problem of reflection that may occur in films having a conventional metal deposition configuration by having a low reflection function for visible light.
[0010] However, the problems to be solved by the present invention are not limited to the problems mentioned above, and other problems not mentioned will be clearly understood by those skilled in the art from the description below.
[0011]
[0012] The present invention relates to a laminate comprising a metal deposition layer formed on an outer surface facing a light source; and a polymer coating layer formed on a lower surface of the metal deposition layer, wherein the thickness of the polymer coating layer exceeds 0.3 μm and is less than 3.0 μm.
[0013] The present invention relates to a polymer coating layer comprising: polyaniline, polythiophene, polyethylenedioxythiophene (PEDOT), polyimide, polystyrenesulfonate (PSS), polypyrrole, polyacetylene, poly(p-phenylene), poly(p-phenylene sulfide), poly(p-phenylenevinylene), polythiophene poly(thienylenevinylene), poly(3,4-ethylenedioxythiophene) poly(styrenesulfonate), (PEDOT:PSS)], and combinations thereof.
[0014] In the present invention, the laminate may further include a substrate, and the polymer coating layer may be included on one side or both sides of the substrate.
[0015] In the present invention, the metal of the metal layer may include at least one selected from Ag, Cu, Au, Al, Ce, Pr, Nd, Pm, Sm, Eu, Gd, Tb, Dy, Ho, Er, Tm, Yb, Lu, Sc, Ti, V, Cr, Mn, Fe, Co, Ni, Zn, Y, Zr, Nb, Mo, Tc, Ru, Rh, Pd, Cd, In, Sn, Hf, Ta, W, Re, Os, Ir, Pt, Tl, Pb, Bi, Ga, Ge, Sb, Ac, Th, and alloys thereof.
[0016] In the present invention, the laminate may further include at least one selected from a protective film and an adhesive layer.
[0017] Additionally, the present invention may relate to a functional film including the laminate.
[0018] In addition, the present invention provides a total solar energy transmittance (T) of the functional film. TS ) may be less than 20%.
[0019] In addition, the present invention provides a total solar energy transmittance (T) of the functional film. TS ) can be 15 to 20%.
[0020] In addition, the present invention may have a visible light transmittance of the functional film of 25 to 30%.
[0021] In addition, the present invention may be characterized in that the visible light reflectance measured from the inside of the functional film is 25% or less.
[0022] In addition, the present invention may be characterized in that the visible light reflectance measured from the inside of the functional film is 15 to 25%.
[0023]
[0024] According to the laminate according to the present invention and the functional film including the laminate, energy economy can be improved by effectively shielding total solar energy.
[0025] In addition, according to the laminate according to the present invention and the functional film including the laminate, the visible light transmittance is suitably high while the inner visible light reflectance is low, so that the problem of visibility obstruction due to the indoor / outdoor reflection phenomenon can be improved.
[0026]
[0027] Figure 1 illustrates a laminated structure of a laminate according to one embodiment of the present invention.
[0028] Figure 2 illustrates a laminated structure of a laminate according to another embodiment of the present invention.
[0029] In the above drawings 1 and 2, arrows indicate light sources. In addition, each symbol in the drawings represents the following.
[0030] 110: Metal deposition layer
[0031] 120: Polymer coating layer
[0032] 130: Substrate layer
[0033] 140: Protective film
[0034] 150: Adhesive film
[0035]
[0036] The present invention relates to a laminate and a functional film including the laminate, which improves energy efficiency and improves visibility problems by lowering the transmittance of total solar energy and having a low-reflection function.
[0037] More specifically, the laminate comprises a metal deposition layer formed on an outer surface facing a light source; and a polymer coating layer formed on a lower surface of the metal deposition layer, wherein the polymer coating layer has a thickness of more than 0.3 μm and less than 3.0 μm. The total solar energy transmittance (T) of the functional film including the laminate is TS ) is 20% or less, preferably 15 to 20%, has a visible light transmittance of 25 to 30%, and has a visible light reflectance measured from the inside of 25% or less, preferably 15 to 25%.
[0038]
[0039] Hereinafter, embodiments of the present invention will be described in more detail with reference to the drawings. However, the following drawings attached to this specification illustrate preferred embodiments of the present invention and, together with the contents of the invention described above, serve to further understand the technical concept of the present invention. Therefore, the present invention should not be interpreted as being limited to the matters described in such drawings.
[0040] The terms used herein are for the purpose of describing embodiments and are not intended to limit the present invention. In this specification, singular forms also include plural forms, unless specifically stated otherwise.
[0041] As used herein, the words "comprises" and / or "comprising" are used to mean that they do not exclude the presence or addition of one or more other components, steps, operations, and / or elements other than the components, steps, operations, and / or elements mentioned. Like reference numerals refer to like elements throughout the specification.
[0042] Spatially relative terms such as “below,” “bottom,” “lower,” “above,” “top,” and “upper” can be used to easily describe the relationship between one element or component and other elements or components, as depicted in the drawings. Spatially relative terms should be understood to include different orientations of the elements during use or operation in addition to the orientation depicted in the drawings. For example, if an element depicted in a drawing is flipped over, an element described as “below” or “lower” of another element may end up “above” the other element. Thus, the exemplary term “below” can include both the above and below directions. Elements can also be oriented in other directions, and thus spatially relative terms can be interpreted based on their orientation.
[0043]
[0044] <Laminate>
[0045] FIG. 1 is a diagram showing a laminated structure of a laminate according to an embodiment of the present invention. Referring to FIG. 1, the laminate according to an embodiment of the present invention may include a metal deposition layer (110) formed on an outer surface facing a light source; and a polymer coating layer (120) formed on a lower surface of the metal deposition layer, and the thickness of the polymer coating layer (120) may be characterized in that it exceeds 0.3 μm and is less than 3.0 μm.
[0046] A laminate according to one embodiment of the present invention may further include a substrate, and may include a polymer coating layer included on one side or both sides of the substrate on the lower surface of the metal deposition layer, thereby lowering the transmittance of solar energy while having an excellent heat blocking rate, so that when a functional film including the laminate of the present invention is deposited, the energy efficiency of heating and cooling can be improved, and an effect of improving visibility due to overhead light occurring indoors and outdoors can be provided.
[0047] More specifically, in the laminate of the present invention, the side facing the light source and the side not facing the light source are distinguished, and the side facing the light source is defined as the outer side, and the side not facing the light source is defined as the inner side. For example, in FIG. 1, the arrow indicates a light source, and in FIG. 1, the metal deposition layer (110) is the side facing the light source in the laminate of the present invention. The laminate of the present invention is characterized in that the metal deposition layer (110) and the polymer coating layer (120) are laminated in this order from the outer side, and this lamination order is advantageous in that the total solar energy transmittance, which determines the heat blocking function from external solar energy, can be effectively controlled.
[0048]
[0049] Metal deposition layer (110)
[0050] The above metal deposition layer (110) is provided to reflect solar energy, and is preferably formed on the outer surface facing the light source from the viewpoint of effectively reflecting and / or blocking thermal energy from solar energy. The above metal deposition layer may include at least one selected from among Ag, Cu, Au, Al, Ce, Pr, Nd, Pm, Sm, Eu, Gd, Tb, Dy, Ho, Er, Tm, Yb, Lu, Sc, Ti, V, Cr, Mn, Fe, Co, Ni, Zn, Y, Zr, Nb, Mo, Tc, Ru, Rh, Pd, Cd, In, Sn, Hf, Ta, W, Re, Os, Ir, Pt, Tl, Pb, Bi, Ga, Ge, Sb, Ac, Th, and alloys thereof, but a material included in a metal deposition layer of a functional film commonly used in the relevant field may be used without special limitation.
[0051] The method for manufacturing the metal deposition layer is not particularly limited, and it is common to use a coating method that is performed by a sputter deposition method, electron beam deposition method, thermal deposition method, chemical vapor deposition method, or solution process that is commonly used in the field.
[0052] The above metal deposition layer (110) is generally 3 to 150 nm, preferably 30 to 100 nm, and more preferably 80 to 100 nm. If it is less than the above range, there is a disadvantage in that the uniformity of the metal deposition layer is reduced when forming the metal deposition layer or the property of reflecting external solar energy is reduced, so that the required solar energy transmittance cannot be reached. If it exceeds the above range, there may also be a problem in that the desired heat blocking characteristic value cannot be satisfied.
[0053]
[0054] Polymer coating layer (120)
[0055] The polymer coating layer (120) may be used for purposes such as solar energy absorption by lowering the reflectance of incident light and controlling the transmittance, but is not limited thereto, and may be provided according to various needs. According to the present invention, the polymer coating layer (120) may be formed by directly contacting the lower surface of the metal deposition layer (110), and may be included on one or both sides of the substrate, and when included in multiple layers on both sides of the substrate, the total solar energy transmittance, visible light transmittance, and / or inner visible light reflectance may be better.
[0056] The polymer coating layer (120) may be formed using any polymer resin known in the art without limitation, and may be, for example, an epoxy-based, cellulose-based, acrylic-based, vinyl chloride-based, vinyl acetate-based, polyvinyl alcohol-based, polyurethane-based, polyester-based, polyethylene-based, or other polymer resins. These may be used singly or in combination of two or more. In particular, the present invention provides that the polymer coating layer may include a conductive polymer, and the conductive polymer may be, for example, polyaniline, polythiophene, polyethylenedioxythiophene (PEDOT), polyimide, polystyrenesulfonate (PSS), polypyrrole, polyacetylene, poly(p-phenylene), poly(p-phenylene sulfide), poly(p-phenylenevinylene), polythiophene poly(thienylenevinylene), poly(3,4-ethylenedioxythiophene) poly(styrenesulfonate). [Poly(3,4-ethylenedioxythiophene) poly(styrenesulfonate), (PEDOT:PSS)] and combinations thereof may be included, and among them, (poly(3,4-ethylenedioxythiophene) poly(styrenesulfonate) [Poly(3,4-ethylenedioxythiophene) poly(styrenesulfonate)](PEDOT:PSS) is preferable in that it has high electrical conductivity, excellent stability, good processability, and excellent coating properties and crack resistance, which are important factors in film formation.
[0057] The polymer coating layer (120) is formed from a composition for forming a polymer coating layer including the polymer, and may further include a solvent, etc. The solvent may include a common solvent used in the field of compositions, and for example, solvents such as deionized water; alcohol compounds such as methanol, ethanol, isopropanol, butanol, and propylene glycol methoxy alcohol; ketone compounds such as methyl ethyl ketone, methyl butyl ketone, methyl isobutyl ketone, diethyl ketone, and dipropyl ketone; acetate compounds such as methyl acetate, ethyl acetate, butyl acetate, and propylene glycol methoxy acetate; cellosolve compounds such as methyl cellosolve, ethyl cellosolve, and propyl cellosolve; and hydrocarbon compounds such as hexane, heptane, benzene, toluene, and xylene may be used. These may be used alone or in combination of two or more, but are not limited thereto.
[0058] The polymer coating layer (120) may be formed by directly contacting a surface of an adhesive layer that has undergone pretreatment, such as corona treatment or plasma treatment, to improve adhesion. The pretreatment is not limited to corona treatment or plasma treatment, and any conventional or later developed pretreatment process may be used within a scope that does not impede the purpose of the present invention.
[0059] According to one embodiment of the present invention, when the thickness of the polymer coating layer exceeds 0.3㎛ and is less than 3.0㎛, there is an advantage in that it absorbs light in the infrared region of solar energy coming from the outside while maintaining an appropriate visible light transmittance, thereby blocking solar energy. In addition, below the above range, the polymer coating layer is too thin, so the solar energy blocking and absorption characteristics are reduced, which may have a disadvantage in that heat blocking and low reflection effects cannot be exhibited, and above the above range, the polymer coating layer is excessively thick, so that the amount of light energy absorbed is large, making it difficult to secure a field of vision.
[0060]
[0061] Description (130)
[0062] The above laminate may further include a substrate (130). The substrate (130) serves to structurally support the components included in the laminate and the functional film including the laminate.
[0063] In one or more embodiments, the substrate (130) may be implemented in the form of a substrate film having a rigid material such as glass or having flexible properties. When the substrate (130) is implemented to be flexible, specific examples of materials that can be applied to the substrate film include polyester-based resins such as polyethylene terephthalate, polyethylene isophthalate, polyethylene naphthalate, and polybutylene terephthalate; cellulose-based resins such as diacetyl cellulose and triacetyl cellulose; polycarbonate-based resins; acrylic-based resins such as polymethyl (meth) acrylate and polyethyl (meth) acrylate; styrene-based resins such as polystyrene and acrylonitrile-styrene copolymers; polyolefin-based resins such as polyethylene, polypropylene, polyolefins having a cyclo-based or norbornene structure, and ethylene-propylene copolymers; vinyl chloride-based resins; amide-based resins such as nylon and aromatic polyamides; imide-based resins; Examples of the transparent optical film include films containing thermoplastic resins such as polyethersulfone resins; sulfone resins; polyetheretherketone resins; sulfated polyphenylene resins; vinyl alcohol resins; vinylidene chloride resins; vinyl butyral resins; allylate resins; polyoxymethylene resins; and epoxy resins. Films made of blends of the above thermoplastic resins can also be used. In addition, films made of thermosetting resins such as (meth)acrylic, urethane, acrylic urethane, epoxy, and silicone resins or ultraviolet-curable resins can also be used. The thickness of such a transparent optical film can be appropriately determined, but is generally determined to be 1 µm to 500 µm. In particular, considering workability such as strength and handleability, and thin layer property, the thickness is preferably 1 µm to 300 µm, and more preferably 5 µm to 200 µm.
[0064] Such a base film may contain one or more suitable additives. Examples of the additives include ultraviolet absorbers, antioxidants, lubricants, plasticizers, release agents, anti-coloring agents, flame retardants, nucleating agents, antistatic agents, pigments, and colorants. The base film may have a structure including various functional layers, such as a hard coating layer, an antireflection layer, and a gas barrier layer, on one or both sides of the film. The functional layers are not limited to those described above, and may include various functional layers known to be usable in the art depending on the intended use.
[0065] Additionally, the substrate film may be surface-treated, if necessary. Such surface treatments include dry treatments such as plasma treatment, corona treatment, and primer treatment, and chemical treatments such as alkaline treatment including saponification treatment.
[0066]
[0067] etc
[0068] Referring to FIG. 2, according to another embodiment of the present invention, the laminate may further include a protective film (140) and / or an adhesive layer (150).
[0069]
[0070] Protective film (140)
[0071] The above protective film (140) is intended to protect the laminate from post-processing and external environments, and may be used as a multi-layer structure in which one or more protective films are laminated, or may be used in combination with other functional layers. The protective film may be positioned on the outermost surface to perform a protective function, but is not limited thereto.
[0072] In one or more embodiments, the protective film (140) is selected from the group consisting of polyethylene terephthalate (PET), polyethylene isophthalate (PEI), polyethylene naphthalate (PEN), polybutylene terephthalate (PBT), diacetyl cellulose, triacetyl cellulose (TAC), polycarbonate (PC), polyethylene (PE), polypropylene (PP), polymethyl acrylate (PMA), polymethyl methacrylate (PMMA), polyethyl acrylate (PEA), polyethyl methacrylate (PEMA), and cyclic olefin polymer (COP). It may include one or more types. In particular, it is more preferable to manufacture a resin film having excellent properties such as transparency, mechanical strength, thermal stability, moisture barrier properties, and isotropy, for example, polyesters such as polyethylene terephthalate (PET), polyethylene naphthalate (PEN), and polybutylene terephthalate; celluloses such as diacetyl cellulose and triacetyl cellulose; polycarbonates; and polymethyl methacrylate.
[0073]
[0074] Adhesive film (150)
[0075] The adhesive film (150) may further include an adhesive developed in the past or later, and in one or more embodiments, an acrylic adhesive, a rubber adhesive, a silicone adhesive, a urethane adhesive, a polyvinyl alcohol adhesive, a polyvinyl pyrrolidone adhesive, a polyacrylamide adhesive, a cellulose adhesive, a vinyl alkyl ether adhesive, etc. may be used. The adhesive film (150) is not particularly limited as long as it has adhesiveness and viscoelasticity, but in terms of ease of acquisition, etc., it may preferably be an acrylic adhesive, and may include, for example, a (meth)acrylate copolymer, a crosslinking agent, and a solvent. The adhesive film may be positioned at the innermost lower part of the laminate so as to be in contact with the adherend, but is not limited thereto.
[0076] The crosslinking agent may be a crosslinking agent developed in the past or later, and may include, for example, a polyisocyanate compound, an epoxy resin, a melamine resin, a urea resin, dialdehydes, a methylol polymer, etc., and preferably, a polyisocyanate compound.
[0077] The above solvent may include a typical solvent used in the field of resin compositions, and for example, alcohol compounds such as methanol, ethanol, isopropanol, butanol, and propylene glycol methoxy alcohol; ketone compounds such as methyl ethyl ketone, methyl butyl ketone, methyl isobutyl ketone, diethyl ketone, and dipropyl ketone; acetate compounds such as methyl acetate, ethyl acetate, butyl acetate, and propylene glycol methoxy acetate; cellosolve compounds such as methyl cellosolve, ethyl cellosolve, and propyl cellosolve; and hydrocarbon compounds such as hexane, heptane, benzene, toluene, and xylene. These solvents may be used alone or in combination of two or more.
[0078] The thickness of the adhesive film (150) may be appropriately determined depending on the type of resin that acts as the adhesive, the adhesive strength, the environment in which the adhesive film (150) is used, etc. In one embodiment, the adhesive film (150) may have a thickness of 5 to 25 μm, preferably 15 to 25 μm, and more preferably 20 to 25 μm, but is not limited thereto, in order to secure sufficient adhesive strength and minimize the thickness of the laminate.
[0079]
[0080] Functional Film
[0081] The present invention includes a functional film comprising the laminated body in addition to the laminated body. Furthermore, the present invention may be applied to sunroofs, left and right side windows, and rear windows for vehicles, or may be attached to glass for architectural windows, but is not limited thereto.
[0082] A functional film according to one embodiment of the present invention includes both an energy-reflecting type metal deposition layer (110) and an energy-absorbing type polymer coating layer (120), thereby preventing visual confusion due to reflection when recognizing an external environment through a reflective surface, and at the same time, ensuring energy efficiency.
[0083] Total solar energy transmittance (T) TS ) is 20% or less, preferably 15 to 20%, has a visible light transmittance of 25 to 30%, and has a visible light reflectance measured from the inside of 25% or less, preferably 15 to 25%.
[0084] Total solar energy transmittance (T) TS) is the sum of the solar radiation transmittance (Te), which is the energy of sunlight (energy) that directly penetrates the substrate and enters the room, and the re-radiated energy (qi), which is the energy that is absorbed by the substrate and then re-radiated into the room. According to one embodiment of the present invention, since the metal deposition layer (110) is located on the outer surface of the laminate, the outer reflectivity is high and an appropriate transmittance is secured, thereby ensuring T TS By lowering the price, we can secure energy efficiency for indoor heating and cooling.
[0085] The polymer coating layer (120) has a property of absorbing light energy, and thus absorbs energy passing through the metal deposition layer (110), thereby satisfying the visible light transmittance of the present invention while reducing the indoor reflectance, thereby obtaining a low-reflection characteristic, i.e., an effect of improving visibility. In addition, when the visible light transmittance is less than 25%, there is a problem that it is too low and it is difficult to secure a view.
[0086]
[0087] Therefore, when the conditions of the laminate according to the present invention and the functional film including the laminate are satisfied, the effect of improving visibility obstruction while increasing indoor energy efficiency can be obtained.
[0088]
[0089] Hereinafter, experimental examples including specific examples and comparative examples are presented to help understand the present invention, but these are only illustrative of the present invention and do not limit the scope of the appended claims. It will be apparent to those skilled in the art that various changes and modifications to the examples are possible within the scope and technical idea of the present invention, and it is natural that such changes and modifications fall within the scope of the appended claims. “%” and “parts” in the examples mean “mass%” and “mass parts”, respectively, unless otherwise specified.
[0090]
[0091] Manufacturing example: Manufacturing of polymer coating layer composition
[0092] The polymer coating layer was prepared by mixing coating solutions 1 and 2 in a 1:1 ratio. The coating solution 1 was prepared using a mixture of 60 wt% of an ethylene benzenesulfonic acid homopolymer compound with 2,3-dihydrothieno[3,4-b]-1,4-dioxin homopolymer (water based), 20 wt% of ethyl alcohol, and 20 wt% of deionized water, based on the total weight of the coating solution 1, and the coating solution 2 was prepared using a mixture of 1.0 wt% of a polyester resin (solid content 25%, water based), 75 wt% of ethyl alcohol, and 24 wt% of deionized water, based on the total weight of the coating solution 2.
[0093]
[0094] Manufacturing of laminates of Examples 1 to 3
[0095] As shown in Table 1 below, a laminate of the example was manufactured to include a metal deposition layer formed on the outer surface facing the light source; and a polymer coating layer on the lower surface of the metal deposition layer.
[0096] Specifically, using a heat-insulating film (product name: NABIL) from MSWAY, in which a metal deposition layer is coated on a polyethylene terephthalate (PET) having a thickness of 125 μm, a polymer coating layer composition according to the above manufacturing example is coated on the lower surface of the metal deposition layer to a thickness of 0.5 μm (Example 1), or a polymer coating layer composition according to the above manufacturing example is coated on the lower surface of the substrate film (PET) to a thickness of 0.5 μm (Example 2), or a polymer coating layer composition according to the above manufacturing example is coated on both surfaces of the substrate film (PET) to a thickness of 0.5 μm (Example 3), and dried in an oven for 5 to 10 minutes, and the resultant is dried according to the method of '1. Preparation of polymer (A)' and '2. An adhesive film manufactured to have a thickness of 25 μm after drying using a diluted solution of an adhesive composition manufactured according to the 'adhesive composition' was attached to the lowest surface to form a laminate of the present invention.
[0097]
[0098] Manufacturing of laminates of comparative examples 1 to 4
[0099] As shown in Table 2 below, a laminate of a comparative example was manufactured.
[0100] Specifically, Comparative Example 1 was manufactured by manufacturing a laminate by laminating the metal deposition layer on the lower surface of the polymer coating layer according to the lamination order of Table 2 below. In addition, compared to Example 1, a heat-insulating film (NABIL) from MSWAY (Comparative Example 4) in which a metal deposition layer is coated on polyethylene terephthalate (PET) having a thickness of 125 μm was used to coat the polymer coating layer composition according to the manufacturing example to a thickness of 0.3 μm (Comparative Example 2) or the polymer coating layer composition according to the manufacturing example to a thickness of 3.0 μm (Comparative Example 3) and dried in an oven for 5 to 10 minutes to form a laminate of the present invention.
[0101]
[0102] The lamination order of the above examples and comparative examples is shown in Tables 1 and 2 below, respectively.
[0103]
[0104]
[0105]
[0106]
[0107] Experimental example
[0108] Based on the test equipment, measuring equipment and measuring environment below, the total solar energy transmittance (%, Total solar energy transmittance: T TS ), visible light transmittance (%), outer visible light reflectance (%), and inner visible light reflectance (%) were measured and shown in Table 3 below.
[0109]
[0110] (1) Total solar energy transmittance (T TS , %)
[0111] The total solar energy transmittance value was calculated based on the ISO 13837:2021 standard by using the values of solar radiation transmittance, solar radiation reflectance, and re-radiated energy measured using UV-VIS-NIR Spectrophotometer, Perkin-Elmer, Lambda 950 & 1050, USA equipment.
[0112]
[0113] (2) Visible light transmittance, visible light reflectance (outer, inner)
[0114] Visible light transmittance and visible light reflectance from the outside and inside were measured using UV-VIS-NIR Spectrophotometer, Perkin-Elmer, Lambda 950 & 1050, USA.
[0115]
[0116] Comparative Example Example 1234123 Reflective Layer AgAgAgAgAgAgAgAg Substrate PETPETPETPETPETPETPET Polymer Coating Layer PEDOTPEDOTPEDOT-PEDOTPEDOTPEDOT Polymer Coating (Single-Sided / Double-Sided) Cross-Section Cross-Section Cross-Section Cross-Section Double-Sided Polymer Coating Layer Total Thickness (㎛) 0.5 0.3 3.0-0.5 0.5 1.0 T TS (%)30251035191915Visible light transmittance(%)42351045303025Visible light reflectance outside(%)25555555555555Visible light reflectance inside(%)55301055252015
[0117]
[0118] Referring to the experimental data in Table 3 above, the laminate according to the present invention and the functional film including the laminate have a total solar energy transmittance (T TS ) was measured to be 20% or less, the visible light transmittance was 25 to 30%, and the visible light reflectance measured from the inside was 25% or less. On the other hand, in Comparative Example 1 where the lamination order of the metal deposition layer and the polymer coating layer is not according to the present invention, in Comparative Example 2 where the thickness of the polymer coating layer is 0.3 ㎛, and in Comparative Example 4 where the polymer coating layer is not included, the total solar energy transmittance, the visible light transmittance, and the visible light reflectance measured from the inside are shown to be outside the above ranges. For reference, in Comparative Example 3 where the thickness of the polymer coating layer is 3.0 ㎛, it can be confirmed that the total solar energy transmittance and the visible light reflectance measured from the inside are lower than in the other Comparative Examples. This can be said to be the result of the polymer coating layer being excessively thick, absorbing light energy. In this case, it may be difficult to secure a field of vision.
[0119] Therefore, in the present invention, it can be confirmed that the stacking order of the metal deposition layer and the polymer coating layer included in the laminate, and the appropriate thickness of the polymer coating layer have a significant influence on the total solar energy transmittance, visible light transmittance, and visible light reflectance measured from the inside.
[0120]
[0121] According to the laminate according to the present invention and the functional film including the laminate, energy economy can be improved by effectively shielding total solar energy.
Claims
1. A metal deposition layer formed on the outer surface facing the light source; and Including a polymer coating layer formed on the lower surface of the metal deposition layer, A laminate having a thickness of the polymer coating layer exceeding 0.3 ㎛ and less than 3.0 ㎛.
2. In claim 1, The polymer coating layer is selected from the group consisting of polyaniline, polythiophene, polyethylenedioxythiophene (PEDOT), polyimide, polystyrenesulfonate (PSS), polypyrrole, polyacetylene, poly(p-phenylene), poly(p-phenylene sulfide), poly(p-phenylenevinylene), polythiophene poly(thienylenevinylene), poly(3,4-ethylenedioxythiophene) poly(styrenesulfonate), A laminate comprising at least one selected from (PEDOT:PSS) and combinations thereof.
3. In claim 1, A laminate, wherein the laminate further comprises a substrate, and the polymer coating layer is included on one or both sides of the substrate.
4. In claim 1, A laminate comprising at least one selected from the group consisting of Ag, Cu, Au, Al, Ce, Pr, Nd, Pm, Sm, Eu, Gd, Tb, Dy, Ho, Er, Tm, Yb, Lu, Sc, Ti, V, Cr, Mn, Fe, Co, Ni, Zn, Y, Zr, Nb, Mo, Tc, Ru, Rh, Pd, Cd, In, Sn, Hf, Ta, W, Re, Os, Ir, Pt, Tl, Pb, Bi, Ga, Ge, Sb, Ac, Th, and alloys thereof.
5. In claim 1, A laminate, wherein the laminate further comprises at least one selected from a protective film and an adhesive layer.
6. A functional film comprising a laminate according to any one of claims 1 to 5.
7. In claim 6, Total solar energy transmittance (T) of the above functional film TS ) is 20% or less.
8. In claim 7, Total solar energy transmittance (T) of the above functional film TS ) is 15 to 20%, a functional film.
9. In claim 6, A functional film, characterized in that the visible light transmittance of the functional film is 25 to 30%.
10. In claim 6, A functional film characterized in that the visible light reflectance measured from the inside of the functional film is 25% or less.
11. In claim 10, A functional film characterized in that the visible light reflectance measured from the inside of the functional film is 15 to 25%.
Citation Information
Patent Citations
Infrared blocking film
KR101067277B1
Manufacturing method for ultraviolet and infrared absorbable film of minimum heat deterioration
KR101391732B1
Insulating Glazing for Shield of Far Infrared and Near Infrared
KR101470356B1
Substrate having a multilayer with thermal properties and an absorbing layer
US20150247961A1
Low-Emissivity Coating for a Glass Substrate
US20190330101A1