Method for manufacturing gallium oxide layer
The alternating use of ALD and CVD techniques in forming multiple gallium oxide layers, with plasma and specific precursors, addresses the issues of uneven quality and long processing times in existing methods, resulting in improved film quality and efficiency in gallium oxide layer deposition.
Patent Information
- Application Number
- PCT/KR2024/006429
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-05-15
- Filing Date
- 2024-05-13
- Publication Date
- 2024-11-21
AI Technical Summary
Existing methods for depositing gallium oxide layers using a single technique, such as atomic layer deposition (ALD) or chemical vapor deposition (CVD), often result in uneven film quality and prolonged processing times, with potential impurities from source and reactant materials affecting the quality of the oxide semiconductor layer.
A method involving alternating steps of atomic layer deposition (ALD) and chemical vapor deposition (CVD) to form multiple gallium oxide layers, with the use of plasma and specific precursors like trimethyl gallium, oxygen, and nitrous oxide, and incorporating purge gases to enhance film quality and reduce impurities.
This approach improves the film quality of the gallium oxide layer while reducing deposition time and minimizing impurities, achieving a more efficient and effective manufacturing process for gallium oxide layers.
Smart Images

Figure KR2024006429_21112024_PF_FP_ABST
Abstract
Description
Method for manufacturing a gallium oxide layer
[0001] The present invention relates to a method for manufacturing a gallium oxide layer.
[0002] Oxide semiconductors possess high mobility and can exhibit significant resistance changes depending on the oxygen content, making it easy to obtain desired properties. Furthermore, because the oxides that make up the oxide semiconductor layer can be formed at relatively low temperatures during the manufacturing process, manufacturing costs are low.
[0003] There may be various methods for depositing oxide semiconductors. For example, the oxide semiconductor may be deposited using atomic layer deposition (ALD), chemical vapor deposition (CVD), etc. However, when depositing the oxide semiconductor using only one method, there are problems such as the film quality of the oxide semiconductor being uneven or taking a long time to form the oxide semiconductor.
[0004] Furthermore, when, for example, atomic layer deposition (ALD) is used as a method for depositing an oxide semiconductor, the oxide semiconductor layer can be formed by depositing a source material and a reactant material. At this time, after completing the step of spraying the source material and the step of spraying the reactant material, unnecessary source material or reactant material may remain in the chamber, which may become a factor that hinders the film quality of the oxide semiconductor.
[0005] The present invention is designed to overcome the shortcomings of the aforementioned method for manufacturing a gallium oxide layer, and aims to provide a method for manufacturing a gallium oxide layer that can reduce the time required to deposit the gallium oxide layer while forming an excellent film quality of the gallium oxide layer.
[0006] In order to achieve the above object, the present invention provides a method for forming a gallium oxide (GaO) layer on a substrate, comprising: forming a first gallium oxide layer; and forming a second gallium oxide layer on the first gallium oxide layer, wherein the step of forming one of the first gallium oxide layer and the second gallium oxide layer uses atomic layer deposition (ALD), and the step of forming the other gallium oxide layer uses chemical vapor deposition (CVD).
[0007] In the present invention, the step of forming the first gallium oxide layer may use atomic layer deposition (ALD), and the step of forming the second gallium oxide layer may use chemical vapor deposition (CVD).
[0008] The present invention includes a step of forming a third gallium oxide layer containing gallium oxide on the second gallium oxide layer, and the step of forming the third gallium oxide layer may use an atomic layer deposition (ALD) method.
[0009] In the present invention, the step of forming the first gallium oxide layer may use a chemical vapor deposition method, and the step of forming the second gallium oxide layer may use an atomic layer deposition method.
[0010] The present invention includes a step of forming a third gallium oxide layer containing gallium oxide on the second gallium oxide layer, and the step of forming the third gallium oxide layer may use a chemical vapor deposition method.
[0011] In the present invention, the step of forming the single gallium oxide layer using the atomic layer deposition (ALD) method may include the step of injecting a first source material containing gallium, the step of injecting a first purge gas, the step of injecting a first reactant material containing oxygen, and the step of injecting a second purge gas.
[0012] In the present invention, the first source material may contain trimethyl gallium (TMGa), and the first reactant material may contain either oxygen (O2) or nitrous oxide (N2O).
[0013] The present invention may further include a step of forming a plasma containing hydrogen (H2) gas or argon (Ar) gas between the step of injecting the first source material and the step of injecting the first reactant material.
[0014] The present invention may further include a step of forming a plasma containing hydrogen (H2) gas or argon (Ar) gas after the step of injecting the first reactant material.
[0015] The present invention can form a plasma containing oxygen during the step of injecting the first reactant material.
[0016] In the present invention, the step of forming the remaining gallium oxide layer using the chemical vapor deposition (CVD) method may include the step of spraying a first source material containing gallium and the step of spraying a first reactant material containing oxygen.
[0017] In the present invention, the first source material may contain trimethyl gallium (TMGa), and the first reactant material may contain either oxygen (O2) or nitrous oxide (N2O).
[0018] The present invention may further include a step of forming a plasma containing hydrogen (H2) gas or argon (Ar) gas after the step of injecting the first source material and the step of injecting the first reactant material.
[0019] The present invention can form a plasma containing oxygen during the step of injecting the first source material and the step of injecting the first reactant material.
[0020] According to the present invention with the above configuration, the following effects are achieved.
[0021] According to the present invention, the first gallium oxide layer is formed by atomic layer deposition (ALD), and the second gallium oxide layer is formed by chemical vapor deposition (CVD), so that the film quality of the gallium oxide layer including the first gallium oxide layer and the second gallium oxide layer can be improved while also increasing the speed at which the gallium oxide layer is formed.
[0022] According to the present invention, the first gallium oxide layer is formed by atomic layer deposition (ALD), the second gallium oxide layer is formed by chemical vapor deposition (CVD), and the third gallium oxide layer is formed by atomic layer deposition (ALD), thereby making it possible to improve the film quality of the gallium oxide layer including the first gallium oxide layer to the third gallium oxide layer while also increasing the speed at which the gallium oxide layer is formed.
[0023] According to the present invention, when depositing the first gallium oxide layer using an atomic layer deposition (ALD) method, by applying plasma after spraying the first source material and applying plasma after spraying the first reactant material, it is possible to prevent impurities from being generated by the first source material and the first reactant material.
[0024] According to the present invention, when depositing the third gallium oxide layer using an atomic layer deposition (ALD) method, by applying plasma after spraying the third source material and applying plasma after spraying the third reactant material, it is possible to prevent impurities from being generated by the third source material and the third reactant material.
[0025] FIG. 1 is a schematic cross-sectional view of a gallium oxide layer according to one embodiment of the present invention.
[0026] FIG. 2 is a schematic cross-sectional view of a gallium oxide layer according to another embodiment of the present invention.
[0027] Figure 3 is a schematic flowchart of a method for manufacturing a gallium oxide layer according to one embodiment of the present invention.
[0028] Figure 4 is a schematic flowchart of a method for manufacturing a gallium oxide layer according to another embodiment of the present invention.
[0029] Figure 5 is a schematic flowchart of a method for manufacturing a gallium oxide layer according to another embodiment of the present invention.
[0030] Figure 6 is a schematic flowchart of a method for manufacturing a gallium oxide layer according to another embodiment of the present invention.
[0031] FIG. 7 is a schematic cross-sectional view of a gallium oxide layer according to another embodiment of the present invention.
[0032] FIG. 8 is a schematic cross-sectional view of a gallium oxide layer according to another embodiment of the present invention.
[0033] Figure 9 is a schematic flowchart of a method for manufacturing a gallium oxide layer according to another embodiment of the present invention.
[0034] Figure 10 is a schematic flowchart of a method for manufacturing a gallium oxide layer according to another embodiment of the present invention.
[0035] Figure 11 is a schematic flowchart of a method for manufacturing a gallium oxide layer according to another embodiment of the present invention.
[0036] Figure 12 is a schematic flowchart of a method for manufacturing a gallium oxide layer according to another embodiment of the present invention.
[0037] FIG. 13 is a drawing showing a device for manufacturing a gallium oxide layer according to another embodiment of the present invention.
[0038] The advantages and features of the present invention, and the methods for achieving them, will become clearer with reference to the embodiments described in detail below together with the accompanying drawings. However, the present invention is not limited to the embodiments disclosed below, but may be implemented in various different forms. These embodiments are provided solely to ensure that the disclosure of the present invention is complete and to fully inform those skilled in the art of the scope of the invention, and the present invention is defined solely by the scope of the claims.
[0039] The shapes, sizes, ratios, angles, numbers, etc. disclosed in the drawings for explaining embodiments of the present invention are illustrative and are not limited to the matters illustrated in the drawings. Like reference numerals refer to like components throughout the specification. In addition, in describing the present invention, if a detailed description of a related known technology is judged to unnecessarily obscure the gist of the present invention, the detailed description thereof will be omitted. When the terms “includes,” “has,” and “consists of” are used in this specification, other parts may be added unless “only” is used. When a component is expressed in the singular, it includes a case where the plural is included unless there is a specifically explicit description.
[0040] When interpreting a component, it is interpreted as including the error range even if there is no separate explicit description.
[0041] When describing a positional relationship, for example, when the positional relationship between two parts is described as 'on top of', 'upper part of', 'lower part of', 'next to', etc., one or more other parts may be located between the two parts, unless 'right away' or 'directly' is used.
[0042] When describing a temporal relationship, for example, when the temporal continuity is described as 'after', 'following', 'next to', 'before', etc., it can also include cases where it is not continuous, as long as 'right away' or 'directly' is not used.
[0043] While terms like "first" and "second" are used to describe various components, these components are not limited by these terms. These terms are merely used to distinguish one component from another. Therefore, a "first" component referred to below may also be a "second" component within the technical scope of the present invention.
[0044] The individual features of the various embodiments of the present invention can be partially or wholly combined or combined with each other, and various technical linkages and operations are possible, and each embodiment can be implemented independently of each other or implemented together in a related relationship.
[0045] Hereinafter, a preferred embodiment of the present invention will be described in detail with reference to the drawings.
[0046] FIG. 1 is a schematic cross-sectional view of a gallium oxide layer according to one embodiment of the present invention.
[0047] As can be seen in Fig. 1, the gallium oxide layer according to one embodiment of the present invention comprises a first gallium oxide layer (121) and a second gallium oxide layer (122). At this time, the first gallium oxide layer may be formed through atomic layer deposition (ALD), and the second gallium oxide layer may be formed through chemical vapor deposition (CVD).
[0048] The first gallium oxide layer (121) may be formed on a substrate (100). The first gallium oxide layer (121) may include an oxide semiconductor, and for example, the first gallium oxide layer (121) may include a GaO series oxide semiconductor containing gallium.
[0049] The first gallium oxide layer (121) can be formed using atomic layer deposition (ALD). Since the first gallium oxide layer (121) is formed using the atomic layer deposition method, the film quality of the first gallium oxide layer (121) is excellent.
[0050] Meanwhile, the first gallium oxide layer (121) may be formed using plasma enhanced atomic layer deposition (PEALD).
[0051] The second gallium oxide layer (122) is formed on the first gallium oxide layer (121).
[0052] The second gallium oxide layer (121) is formed by including an oxide semiconductor, and for example, the second gallium oxide layer (122) may be formed by including a GaO series oxide semiconductor containing gallium.
[0053] The second gallium oxide layer (122) can be formed using a chemical vapor deposition method (CVD). When the second gallium oxide layer (122) is formed using the chemical vapor deposition method, the second gallium oxide layer (122) can be formed more quickly than when the atomic layer deposition method is used.
[0054] Meanwhile, the second gallium oxide layer (122) may be formed using plasma enhanced chemical vapor deposition (PECVD).
[0055] FIG. 2 is a schematic cross-sectional view of a gallium oxide layer according to another embodiment of the present invention.
[0056] As can be seen in FIG. 2, the gallium oxide layer according to another embodiment of the present invention comprises a first gallium oxide layer (121), a second gallium oxide layer (122), and a third gallium oxide layer (123). Meanwhile, the gallium oxide layer according to the embodiment of FIG. 2 is identical to the gallium oxide layer according to the embodiment of FIG. 1 except for the third gallium oxide layer (123), and therefore, the following description will focus on the different configurations.
[0057] The first gallium oxide layer (121) is formed using an atomic layer deposition method, and the second gallium oxide layer (122) is formed using a chemical vapor deposition method.
[0058] The third gallium oxide layer (123) is formed on the second gallium oxide layer (122).
[0059] The third gallium oxide layer (123) is formed by including an oxide semiconductor, and for example, the third gallium oxide layer (123) may be formed by including a GaO series oxide semiconductor containing gallium.
[0060] The third gallium oxide layer (123) can be formed using atomic layer deposition (ALD). Since the first gallium oxide layer (123) is formed using the atomic layer deposition method, the film quality of the first gallium oxide layer (123) is improved.
[0061] Meanwhile, the third gallium oxide layer (123) may be formed using plasma enhanced atomic layer deposition (PEALD).
[0062] Figure 3 is a schematic flowchart of a method for manufacturing a gallium oxide layer according to one embodiment of the present invention.
[0063] As can be seen from FIG. 3, a method for manufacturing a gallium oxide layer according to one embodiment of the present invention comprises a step of spraying a first source material (S110), a step of spraying a first reactant material (S120), and a step of spraying a second source material and a second reactant material (S130).
[0064] At this time, the step of spraying the first source material (S110) and the step of spraying the first reactant material (S120) can use atomic layer deposition (ALD).
[0065] Accordingly, the step of spraying the first source material (S110) and the step of spraying the first reactant material (S120) can be performed in a vacuum chamber, and specifically, the substrate is placed on a susceptor provided at the bottom of the vacuum chamber, and the first source material and the first reactant material are sprayed through a gas injection port provided at the top of the vacuum chamber to form the first gallium oxide layer (see 121 of FIGS. 1 and 2) on the substrate.
[0066] When using the above atomic layer deposition method, the steps of spraying the first source material on the substrate and then spraying the first reactant material can be repeated in one cycle.
[0067] In the step (S110) of spraying the first source material, the first source material may include a material containing gallium (Ga). At this time, the material may be a precursor material or a gas material.
[0068] The material containing the gallium (Ga) may be, for example, trimethylgallium (TriMethyl Gallium, TMGa). Meanwhile, the material containing the gallium (Ga) is not limited thereto and may vary depending on knowledge in the art.
[0069] After the step (S110) of spraying the first source material is performed, the step (S120) of spraying the first reactant material may be performed.
[0070] When the first source material includes a material including gallium (Ga), the first reactant material may include either oxygen (O2) or nitrous oxide (N2O), in which case gallium oxide (GaO) may be obtained as the first gallium oxide layer (see 121 in FIGS. 1 and 2).
[0071] When performing the step (S120) of spraying the first reactant material, the first reactant material (S120) can be sprayed with or without forming plasma.
[0072] At this time, if plasma is not formed in the step (S120) of spraying the first reactant material, the first gallium oxide layer may be formed using atomic layer deposition (ALD), and if plasma is formed in the step (S120) of spraying the first reactant material, the first gallium oxide layer may be formed using plasma-enhanced atomic layer deposition (PEALD).
[0073] When the step (S120) of injecting the first reactant is formed using the plasma-enhanced atomic layer deposition method, the plasma may include oxygen (O2).
[0074] The first gallium oxide layer can be formed by atomic layer deposition (ALD or PEALD) to improve film quality.
[0075] After the step (S120) of injecting the first reactant material is performed, the step (S130) of injecting the second source material and the second reactant material may be performed.
[0076] The step (S130) of spraying the second source material and the second reactant material may utilize a chemical vapor deposition (CVD) method. At this time, in the chamber in which the first gallium oxide layer is formed through the step (S110) of spraying the first source material and the step (S120) of spraying the first reactant material, the second source material and the second reactant material are simultaneously sprayed onto the first gallium oxide layer (see 121 of FIGS. 1 and 2) through the gas injection port, thereby forming the second gallium oxide layer (see 122 of FIGS. 1 and 2) on the first gallium oxide layer (see 121 of FIGS. 1 and 2) by a chemical vapor deposition method.
[0077] The second source material may be a material containing gallium (Ga). In this case, the second source material may contain, for example, trimethylgallium (TriMethyl Gallium, TMGa).
[0078] The second reactant may include either oxygen (O2) or nitrous oxide (N2O).
[0079] When the second source material includes a material including gallium (Ga) and the second reactant material includes either oxygen (O2) or nitrous oxide (N2O), gallium oxide (GaO) can be obtained as the second gallium oxide layer (see 121 in FIGS. 1 and 2).
[0080] When performing the step (S130) of spraying the second source material and the second reactant material, the second source material and the second reactant material may be sprayed with or without forming plasma.
[0081] At this time, if plasma is not formed in the step (S130) of spraying the second source material and the second reactant material, the second gallium oxide layer (see 121 of FIGS. 1 and 2) may be formed using a chemical vapor deposition method (CVD), and if plasma is formed in the step (S130) of spraying the second source material and the second reactant material, the second gallium oxide layer (see 121 of FIGS. 1 and 2) may be formed using a plasma-enhanced chemical vapor deposition method (PECVD). At this time, the plasma may include oxygen (O2).
[0082] The above second gallium oxide layer (see 121 in FIGS. 1 and 2) can be formed by chemical vapor deposition (CVD or PECVD), so that the deposition time can be shortened.
[0083] Although not illustrated, a step of injecting a purge gas may be added between each of the steps (S110, S120, S130). For example, a step of injecting a purge gas may be added between the step of injecting the first source material (S110) and the step of injecting the first reactant material (S120), and a step of injecting a purge gas may be added between the step of injecting the first reactant material (S120) and the step of injecting the second source material and the second reactant material (S130).
[0084] Figure 4 is a schematic flowchart of a method for manufacturing a gallium oxide layer according to another embodiment of the present invention.
[0085] As can be seen in FIG. 4, a method for manufacturing a gallium oxide layer according to another embodiment of the present invention includes a step of spraying a first source material (S110), a step of spraying a first reactant material (S120), a step of spraying a second source material and a second reactant material (S130), a step of spraying a third source material (S140), and a step of spraying a third reactant material (S150). At this time, the method for manufacturing a gallium oxide layer according to FIG. 4 is the same as the method for manufacturing a gallium oxide layer according to FIG. 3 except for the step of spraying the third source material (S140) and the step of spraying the third reactant material (S150), so the following description will focus on different configurations.
[0086] The step of spraying the third source material (S140) and the step of spraying the third reactant material (S150) may use atomic layer deposition (ALD).
[0087] Accordingly, the step of spraying the third source material (S140) and the step of spraying the third reactant material (S150) can be performed in a vacuum chamber, and specifically, the substrate on which the first gallium oxide layer and the second gallium oxide layer are formed is placed on a susceptor provided at the bottom of the vacuum chamber, and the third source material and the third reactant material are sprayed through a gas injection port provided at the top of the vacuum chamber to form the third gallium oxide layer (see 123 of FIG. 2) on the second gallium oxide layer.
[0088] When using the above atomic layer deposition method, the steps of spraying the third source material on the substrate and then spraying the third reactant material can be repeated in one cycle.
[0089] The step (S140) of injecting the third source material may be performed after the step (S130) of injecting the second source material and the second reactant material.
[0090] In the step (S140) of spraying the third source material, the third source material may include a material containing gallium (Ga). At this time, the material may be a precursor material or a gas material.
[0091] The material containing the gallium (Ga) may be, for example, trimethylgallium (TriMethyl Gallium, TMGa). Meanwhile, the material containing the gallium (Ga) is not limited thereto and may vary depending on knowledge in the art.
[0092] After the step (S140) of spraying the third source material is performed, the step (S150) of spraying the third reactant material may be performed.
[0093] When the third source material includes a material including gallium (Ga), the third reactant material may include either oxygen (O2) or nitrous oxide (N2O), in which case gallium oxide (GaO) may be obtained as the third gallium oxide layer (see 123 in FIG. 2).
[0094] When performing the step (S150) of spraying the third reactant material, the third reactant material can be sprayed with or without forming plasma.
[0095] At this time, if plasma is not formed in the step (S150) of spraying the third reactant material, the third gallium oxide layer (see 123 in FIG. 2) is formed using atomic layer deposition (ALD), and if plasma is formed in the step (S150) of spraying the third reactant material, the third gallium oxide layer (see 123 in FIG. 2) can be formed using plasma-enhanced atomic layer deposition (PEALD).
[0096] When the step (S150) of injecting the third reactant is formed using the plasma-enhanced atomic layer deposition method, the plasma may include oxygen (O2).
[0097] The third gallium oxide layer (see 123 in Fig. 2) can be formed by atomic layer deposition (ALD or PEALD) to improve film quality.
[0098] Although not shown, a step of injecting purge gas may be added between each of the steps (S110, S120, S130, S140, S150). For example, a step of injecting a purge gas may be added between the step of injecting the first source material (S110) and the step of injecting the first reactant material (S120), a step of injecting a purge gas may be added between the step of injecting the first reactant material (S120) and the step of injecting the second source material and the second reactant material (S130), a step of injecting a purge gas may be added between the step of injecting the second source material and the second reactant material (S130) and the step of injecting the third source material (S140), and a step of injecting a purge gas may be added between the step of injecting the third source material (S140) and the step of injecting the third reactant material (S150).
[0099] Figure 5 is a schematic flowchart of a method for manufacturing a gallium oxide layer according to another embodiment of the present invention.
[0100] As can be seen in FIG. 5, a method for manufacturing a gallium oxide layer according to another embodiment of the present invention includes a step of injecting a first source material (S110), a step of applying plasma containing hydrogen gas or argon gas (S115), a step of injecting a first reactant material (S120), a step of applying plasma containing hydrogen gas or argon gas (S125), and a step of injecting a second source material and a second reactant material (S130). At this time, the method for manufacturing a gallium oxide layer according to FIG. 5 is the same as the method for manufacturing a gallium oxide layer according to FIG. 3 except for the steps of applying plasma containing hydrogen gas or argon gas (S115, S125), so the following description will focus on different configurations.
[0101] The step (S115, S125) of applying plasma containing the hydrogen or argon gas may be performed after the step (S110) of injecting the first source material or after the step (S120) of injecting the first reactant material.
[0102] In the step of applying plasma containing hydrogen or argon gas (S115, S125), plasma containing hydrogen gas (H2) or argon (Ar) gas may be applied into the chamber. Specifically, the step of spraying the first source material (S110) may be performed so that plasma containing hydrogen or argon gas may be applied onto the substrate on which the first source material is adsorbed, and in this case, impurities remaining on the substrate without being adsorbed may be removed.
[0103] Alternatively, the step of spraying the first reactant material (S125) may be performed so that plasma including hydrogen or argon gas is applied to the substrate on which the first source material and the first reactant material react to form the first gallium oxide layer, and in this case, impurities remaining on the substrate without reacting can be removed.
[0104] Therefore, when the step of spraying the first source material (S110) and the step of spraying the first reactant material (S120) are performed using an atomic layer deposition method, the content of impurities on the surface or inside of the first gallium oxide layer formed can be minimized.
[0105] Although not shown, a step of applying plasma containing hydrogen gas or argon gas may be additionally included after the step (S130) of injecting the second source material and the second reactant material.
[0106] Although not shown, a step of injecting purge gas may be added between each of the steps (S110, S115, S120, S125, S130).
[0107] Figure 6 is a schematic flowchart of a method for manufacturing a gallium oxide layer according to another embodiment of the present invention.
[0108] As can be seen in FIG. 6, a method for manufacturing a gallium oxide layer according to another embodiment of the present invention comprises a step of injecting a first source material (S110), a step of applying plasma containing hydrogen gas or argon gas (S115), a step of injecting a first reactant material (S120), a step of applying plasma containing hydrogen gas or argon gas (S125), a step of injecting a second source material and a second reactant material (S130), a step of injecting a third source material (S140), a step of applying plasma containing hydrogen gas or argon gas (S145), a step of injecting a third reactant material, and a step of applying plasma containing hydrogen gas or argon gas.
[0109] At this time, the method for manufacturing a gallium oxide layer according to FIG. 6 is the same as the method for manufacturing a gallium oxide layer according to FIG. 5 except for the step of spraying the third source material (S140) and the step of applying plasma containing hydrogen gas or argon gas (S155), so the following description will focus on different configurations.
[0110] The step of spraying the third source material (S140) and the step of spraying the third reactant material (S150) are the same as the step of spraying the third source material and the step of spraying the third reactant material according to FIG. 4. Therefore, the step of spraying the third source material (S140) and the step of spraying the third reactant material (S150) may utilize an atomic layer deposition method, and at this time, the third gallium oxide layer may be formed.
[0111] The step (S145, S155) of applying plasma containing the hydrogen or argon gas may be performed after the step (S140) of injecting the third source material or after the step (S150) of injecting the third reactant material.
[0112] In the step of applying plasma containing hydrogen or argon gas (S145, S155), plasma containing hydrogen gas (H2) or argon (Ar) gas may be applied into the chamber. Specifically, the step of spraying the third source material (S140) may be performed so that plasma containing hydrogen or argon gas may be applied onto the second gallium oxide layer on which the third source material is adsorbed, and in this case, impurities remaining on the substrate without being adsorbed may be removed.
[0113] Alternatively, the step of spraying the third reactant material (S155) may be performed so that plasma including hydrogen or argon gas is applied to the substrate on which the third source material and the third reactant material react to form a third gallium oxide layer, and in this case, impurities remaining on the substrate without reacting can be removed.
[0114] Therefore, when the step of spraying the third source material (S140) and the step of spraying the third reactant material (S150) are performed using an atomic layer deposition method, the content of impurities on the surface or inside of the third gallium oxide layer formed can be minimized.
[0115] Although not shown, a step of applying plasma containing hydrogen gas or argon gas may be additionally included between the step of injecting the second source material and the second reactant material (S130) and the step of injecting the third source material (S140).
[0116] Although not shown, a step of injecting purge gas may be added between each of the steps (S110, S115, S120, S125, S130, S140, S145, S150, S155).
[0117] FIG. 7 is a schematic cross-sectional view of a gallium oxide layer according to another embodiment of the present invention.
[0118] As can be seen in Fig. 7, a gallium oxide layer according to another embodiment of the present invention comprises a first gallium oxide layer (221) and a second gallium oxide layer (222). At this time, the first gallium oxide layer may be formed through chemical vapor deposition (CVD), and the second gallium oxide layer may be formed through atomic layer deposition (ALD).
[0119] The first gallium oxide layer (221) is formed by including an oxide semiconductor, and for example, the first gallium oxide layer (221) may be formed by including a GaO series oxide semiconductor containing gallium.
[0120] The first gallium oxide layer (221) may be formed on a substrate (200). The first gallium oxide layer (221) may be formed using a chemical vapor deposition method (CVD). When the first gallium oxide layer (221) is formed using the chemical vapor deposition method, the first gallium oxide layer (221) may be formed more quickly than when the atomic layer deposition method is used.
[0121] Meanwhile, the first gallium oxide layer (221) may be formed using plasma enhanced chemical vapor deposition (PECVD).
[0122] The second gallium oxide layer (222) is formed on the first gallium oxide layer (221).
[0123] The second gallium oxide layer (222) is formed by including an oxide semiconductor, and for example, the second gallium oxide layer (222) may be formed by including a GaO series oxide semiconductor containing gallium.
[0124] The second gallium oxide layer (222) can be formed using atomic layer deposition (ALD). Since the second gallium oxide layer (222) is formed using the atomic layer deposition method, the film quality of the second gallium oxide layer (222) is improved.
[0125] Meanwhile, the second gallium oxide layer (222) may be formed using plasma enhanced atomic layer deposition (PEALD).
[0126] Figure 8 is a schematic cross-sectional view of a gallium oxide layer according to another embodiment of the present invention.
[0127] As can be seen in Fig. 8, the gallium oxide layer according to another embodiment of the present invention comprises a first gallium oxide layer (221), a second gallium oxide layer (222), and a third gallium oxide layer (223). Meanwhile, the gallium oxide layer according to the embodiment of Fig. 8 is identical to the gallium oxide layer according to the embodiment of Fig. 7, except for the third gallium oxide layer (223), and therefore, the following description will focus on the different configurations.
[0128] The first gallium oxide layer (221) is formed using a chemical vapor deposition method, and the second gallium oxide layer (222) is formed using an atomic layer deposition method.
[0129] The third gallium oxide layer (223) is formed on the second gallium oxide layer (222).
[0130] The third gallium oxide layer (223) is formed by including an oxide semiconductor, and for example, the third gallium oxide layer (223) may be formed by including a GaO series oxide semiconductor containing gallium.
[0131] The third gallium oxide layer (223) can be formed using a chemical vapor deposition method (CVD). When the third gallium oxide layer (223) is formed using the chemical vapor deposition method, the third gallium oxide layer (223) can be formed more quickly than when the atomic layer deposition method is used.
[0132] Meanwhile, the third gallium oxide layer (223) may be formed using plasma enhanced atomic layer deposition (PEALD).
[0133] Figure 9 is a schematic flowchart of a method for manufacturing a gallium oxide layer according to another embodiment of the present invention.
[0134] As can be seen from FIG. 9, a method for manufacturing a gallium oxide layer according to one embodiment of the present invention comprises a step of spraying a first source material and a first reactant material (S210), a step of spraying a second source material (S220), and a step of spraying a second reactant material (S230).
[0135] The step (S210) of spraying the first source material and the second reactant material may utilize a chemical vapor deposition (CVD) method. The step (S210) of spraying the first source material and the first reactant material may be performed in a vacuum chamber, and specifically, a substrate may be placed on a susceptor provided at the bottom of the vacuum chamber, and the first source material and the first reactant material may be simultaneously sprayed onto the substrate through a gas injection port provided at the top of the vacuum chamber, thereby forming a first gallium oxide layer (see 221 of FIGS. 7 and 8) on the substrate by a chemical vapor deposition method.
[0136] The first source material may be a material containing gallium (Ga). In this case, the first source material may contain, for example, trimethylgallium (TriMethyl Gallium, TMGa).
[0137] The first reactant may include either oxygen (O2) or nitrous oxide (N2O).
[0138] When the first source material includes a material including gallium (Ga) and the first reactant material includes either oxygen (O2) or nitrous oxide (N2O), gallium oxide (GaO) can be obtained as the first gallium oxide layer (see 221 of FIGS. 7 and 8).
[0139] When performing the step (S210) of spraying the first source material and the first reactant material, the first source material and the first reactant material can be sprayed with or without forming plasma.
[0140] At this time, if plasma is not formed in the step (S210) of spraying the first source material and the first reactant material, the first gallium oxide layer (see 221 of FIGS. 7 and 8) may be formed using a chemical vapor deposition method (CVD), and if plasma is formed in the step (S210) of spraying the first source material and the first reactant material, the first gallium oxide layer (see 221 of FIGS. 7 and 8) may be formed using a plasma-enhanced chemical vapor deposition method (PECVD). At this time, the plasma may include oxygen (O2).
[0141] The first gallium oxide layer (see 221 in FIGS. 7 and 8) can be formed by chemical vapor deposition, thereby shortening the deposition time.
[0142] After the step (S210) of injecting the first source material and the first reactant material is performed, the step (S220) of injecting the second source material and the step (S230) of injecting the second reactant material may be performed.
[0143] The step of spraying the second source material (S220) and the step of spraying the second reactant material (S230) may use atomic layer deposition (ALD).
[0144] In the chamber where the first gallium oxide layer is formed through the step (S210) of injecting the first source material and the first reactant material, the second source material and the second reactant material are injected through the gas injection port onto the first gallium oxide layer (see 221 of FIGS. 7 and 8), thereby forming the second gallium oxide layer (see 222 of FIGS. 7 and 8) on the first gallium oxide layer (see 221 of FIGS. 7 and 8) by atomic layer deposition.
[0145] When using the above atomic layer deposition method, the steps of spraying the second source material on the first gallium oxide layer (see 221 in FIGS. 7 and 8) and then spraying the second reactant material can be repeated in one cycle.
[0146] In the step (S210) of spraying the second source material, the second source material may include a material containing gallium (Ga). At this time, the material may be a precursor material or a gas material.
[0147] The material containing the gallium (Ga) may be, for example, trimethylgallium (TriMethyl Gallium, TMGa). Meanwhile, the material containing the gallium (Ga) is not limited thereto and may vary depending on knowledge in the art.
[0148] After the step of spraying the second source material (S220) is performed, the step of spraying the second reactant material (S230) may be performed.
[0149] When the second source material includes a material including gallium (Ga), the second reactant material may include either oxygen (O2) or nitrous oxide (N2O), in which case gallium oxide (GaO) may be obtained as the second gallium oxide layer (see 222 of FIGS. 7 and 8).
[0150] When performing the step (S230) of spraying the second reactant material, the second reactant material (S230) can be sprayed with or without forming plasma.
[0151] At this time, if plasma is not formed in the step (S230) of spraying the second reactant material, the second gallium oxide layer (see 222 of FIGS. 7 and 8) is formed using atomic layer deposition (ALD), and if plasma is formed in the step (S230) of spraying the second reactant material, the second gallium oxide layer can be formed using plasma-enhanced atomic layer deposition (PEALD).
[0152] When the step (S230) of injecting the second reactant is formed using the plasma-enhanced atomic layer deposition method, the plasma may include oxygen (O2).
[0153] The above second gallium oxide layer (see 222 in FIGS. 7 and 8) can be formed by atomic layer deposition (ALD or PEALD) to improve film quality.
[0154] Although not shown, a step of injecting purge gas may be added between each of the steps (S210, S220, S230).
[0155] Figure 10 is a schematic flowchart of a method for manufacturing a gallium oxide layer according to another embodiment of the present invention.
[0156] As can be seen in Fig. 10, a method for manufacturing a gallium oxide layer according to another embodiment of the present invention includes a step of spraying a first source material and a first reactant material (S210), a step of spraying a second source material (S220), a step of spraying a second reactant material (S230), and a step of spraying a third source material and a third reactant material (S240). At this time, the method for manufacturing a gallium oxide layer according to Fig. 10 is the same as the method for manufacturing a gallium oxide layer according to Fig. 9 except for the step of spraying the third source material and the third reactant material (S240), so the following description will focus on different configurations.
[0157] The step (S230) of spraying the third source material and the third reactant material may use a chemical vapor deposition method (Chemical Vaporization Deposition; CVD).
[0158] Accordingly, the step (S230) of spraying the third source material and the third reactant material can be performed in a vacuum chamber, and specifically, the substrate on which the first gallium oxide layer and the second gallium oxide layer are formed is placed on a susceptor provided at the bottom of the vacuum chamber, and the third source material and the third reactant material are simultaneously sprayed through a gas injection port provided at the top of the vacuum chamber to form the third gallium oxide layer (see 223 of FIG. 8) on the second gallium oxide layer.
[0159] The step (S230) of injecting the third source material and the third reactant material may be performed after the step (S220) of injecting the second source material.
[0160] The third source material may be a material containing gallium (Ga). In this case, the third source material may contain, for example, trimethylgallium (TriMethyl Gallium, TMGa).
[0161] The third reactant may include either oxygen (O2) or nitrous oxide (N2O).
[0162] When the third source material includes a material including gallium (Ga) and the third reactant material includes either oxygen (O2) or nitrous oxide (N2O), gallium oxide (GaO) can be obtained as the third gallium oxide layer.
[0163] In the step (S240) of spraying the third source material and the third reactant material, the third source material and the third reactant material can be sprayed with or without forming plasma.
[0164] At this time, if plasma is not formed in the step (S240) of spraying the third source material and the third reactant material, the third gallium oxide layer (see 223 of FIG. 8) may be formed using a chemical vapor deposition method (CVD), and if plasma is formed in the step (S240) of spraying the third source material and the third reactant material, the third gallium oxide layer (see 223 of FIG. 8) may be formed using a plasma-enhanced chemical vapor deposition method (PECVD). At this time, the plasma may include oxygen (O2).
[0165] The third gallium oxide layer (see 223 in FIG. 8) can be formed by chemical vapor deposition (CVD or PECVD), so that the deposition time can be shortened.
[0166] Although not shown, a step of injecting purge gas may be added between each of the steps (S210, S220, S230, S240).
[0167] Figure 11 is a schematic flowchart of a method for manufacturing a gallium oxide layer according to another embodiment of the present invention.
[0168] As can be seen in Fig. 11, a method for manufacturing a gallium oxide layer according to another embodiment of the present invention includes a step of injecting a first source material and a first reactant material (S210), a step of applying plasma containing hydrogen gas or argon gas (S215), a step of injecting a second source material (S220), and a step of injecting a second reactant material (S230). At this time, the method for manufacturing a gallium oxide layer according to Fig. 11 is the same as the method for manufacturing a gallium oxide layer according to Fig. 9 except for the step of applying plasma containing hydrogen gas or argon gas (S215), so the following description will focus on different configurations.
[0169] The step (S215) of applying plasma containing the hydrogen or argon gas may be performed after the step (S210) of injecting the first source material and the first reactant material.
[0170] In the step (S215) of applying plasma containing hydrogen or argon gas, plasma containing hydrogen gas (H2) or argon (Ar) gas may be applied into the chamber. Specifically, the step (S210) of spraying the first source material and the first reactant material may be performed so that the plasma containing hydrogen or argon gas may be applied onto the substrate on which the first source material and the first reactant material react to form a first gallium oxide layer. In this case, impurities remaining on the substrate without reacting may be removed.
[0171] Therefore, the content of impurities on the surface or inside of the first gallium oxide layer formed through the step (S210) of spraying the first source material and the first reactant material can be minimized.
[0172] Although not shown, a step of applying plasma containing hydrogen gas or argon gas may be additionally included between the step of injecting the second source material (S220) and the step of injecting the second reactant material (S230). In addition, a step of applying plasma containing hydrogen gas or argon gas may be additionally included after the step of injecting the second reactant material (S230).
[0173] Although not shown, a step of injecting purge gas may be added between each of the steps (S210, S215, S220, S230).
[0174] Figure 12 is a schematic flowchart of a method for manufacturing a gallium oxide layer according to another embodiment of the present invention.
[0175] As can be seen from FIG. 12, a method for manufacturing a gallium oxide layer according to another embodiment of the present invention comprises a step of injecting a first source material and a first reactant material (S210), a step of applying plasma containing hydrogen gas or argon gas (S215), a step of injecting a second source material (S220), a step of injecting a second reactant material (S230), a step of injecting a third source material and a third reactant material (S240), and a step of applying plasma containing hydrogen gas or argon gas (S245).
[0176] At this time, the method for manufacturing a gallium oxide layer according to FIG. 12 is the same as the method for manufacturing a gallium oxide layer according to FIG. 11 except for the step of spraying the third source material (S240) and the step of applying plasma containing hydrogen gas or argon gas (S245), so the following description will focus on different configurations.
[0177] The step (S240) of spraying the third source material and the third reactant material is the same as the step of spraying the third source material and the third reactant material according to Fig. 10. Therefore, the step (S240) of spraying the third source material and the third reactant material may use a chemical vapor deposition method, and at this time, the third gallium oxide layer may be formed.
[0178] The step (S245) of applying plasma containing the hydrogen or argon gas may be performed after the step (S240) of injecting the third source material and the third reactant material.
[0179] In the step (S245) of applying plasma containing hydrogen or argon gas, plasma containing hydrogen gas (H2) or argon (Ar) gas may be applied into the chamber. Specifically, the plasma containing hydrogen or argon gas may be applied onto the third gallium oxide layer formed after the step (S240) of spraying the third source material and the third reactant material is performed.
[0180] When plasma containing the hydrogen or argon gas is applied, impurities generated after the step (S240) of spraying the third source material and the third reactant material can be removed. Therefore, when the step (S240) of spraying the third source material and the third reactant material and the step (S150) of spraying the third reactant material are performed using a chemical vapor deposition method, the content of impurities on the surface or inside of the third gallium oxide layer formed can be minimized.
[0181] Although not shown, a step of applying plasma containing hydrogen gas or argon gas may be additionally included between the step of injecting the second source material (S220) and the step of injecting the second reactant material (S230). In addition, a step of applying plasma containing hydrogen gas or argon gas may be additionally included between the step of injecting the second reactant material (S230) and the step of injecting the third source material and the third reactant material (S240).
[0182] Although not shown, a step of injecting purge gas may be added between each of the steps (S210, S215, S220, S230, S240, S250).
[0183] FIG. 13 is a drawing showing a device for manufacturing a gallium oxide layer according to another embodiment of the present invention.
[0184] Referring to FIG. 13, a gallium oxide layer manufacturing apparatus according to an embodiment of the present invention is an apparatus for depositing a gallium oxide layer, and includes an upper dome (352) and a lower dome (358). A step gas, i.e., a source material and a reactant material, can be injected into the upper dome (352), and the step gas, i.e., the source material and the reactant material, can be exhausted from the upper dome (352). The source material and the reactant material can be injected through a gas injection unit. The gas injection unit has one or more injectors, and the step gas can be injected into the step space by one or more injectors. The step space can be located below the upper dome (352). By supplying a purge gas to the lower dome (358) and supplying a step gas to the upper dome (352), the step gas can be prevented from flowing into the lower dome (358), thereby suppressing the deposition of an abnormal layer on the lower dome (358). In addition, by forming a uniform plasma, a uniform layer can be formed without rotating the substrate (374).
[0185] Additionally, the gallium oxide (GaO) of this step can also be formed using a plasma enhanced ALD (PEALD) device employing an inductively coupled plasma source.
[0186] The gallium oxide layer manufacturing apparatus having the upper dome (352) and the lower dome (358) above has a liner (354, 356) to prevent deposition of an unnecessary layer on the inner wall of the chamber (360). The liner (354, 356) may be periodically replaced or cleaned.
[0187] The lamp heater (366) positioned at the bottom of the lower dome (358) is a ring-shaped lamp heater, and a plurality of lamp heaters may be provided. The plurality of lamp heaters (366) can independently control power to uniformly heat the substrate (374).
[0188] A high vacuum pump (390) consisting of a turbomolecular pump (TMP) connected to the exhaust of the chamber (360) maintains a base vacuum inside the chamber (360), thereby forming a stable plasma at a pressure of several Torr or less even during the step.
[0189] The gallium oxide layer manufacturing device of the present invention can form a uniform layer on the substrate (374) at high speed by providing infrared rays reflected from the electromagnetic shielding housing (330) back to the substrate (374) while reducing the performance degradation caused by infrared heating of the antenna (310) forming the inductively coupled plasma disposed on the upper part of the upper dome (352).
[0190] Referring to FIG. 17, a gallium oxide layer manufacturing device (300) according to one embodiment of the present invention includes a chamber (360) having a side wall; a substrate support member (372) provided inside the chamber and supporting a substrate; an upper dome (352) formed of a transparent dielectric material and covering an upper surface of the chamber (360); an antenna (310) disposed on an upper portion of the upper dome (352) and forming an inductively coupled plasma; and an electromagnetic shielding housing (330) disposed to surround the antenna (310). The electromagnetic shielding housing (330) can be heated by a heater.
[0191] The above antenna (310) includes two one-turn unit antennas, and the two one-turn unit antennas can be connected in parallel to an RF power source (340).
[0192] The plasma of the step of generating hydrogen plasma performed after the step of injecting the reactant material and the step of generating plasma performed between the step of injecting the source material and the step of injecting the reactant material can be formed by the antenna (310).
[0193] The source material and the reactant material can be injected into the step space within the upper dome (352) and the lower dome (358) by an injector (not shown). The source material and the reactant material can be injected into the chamber (360) by the injector in the direction of the upper dome (352) or in a horizontal direction.
[0194] The chamber (360) is formed of a conductor, the internal space of the chamber (360) may have a cylindrical shape, and the external shape of the chamber (360) may have a rectangular parallelepiped shape. The chamber (360) may be cooled by cooling water. The chamber (360), the upper dome (352), and the lower dome (358) are combined to provide a sealed space.
[0195] A substrate entrance (360a) may be provided on one side of the chamber (360), and an exhaust port (360b) may be provided on the other side of the chamber (360) facing the substrate entrance (360a). The exhaust port (360b) may be connected to a high vacuum pump (390). The high vacuum pump (390) may be a turbomolecular pump. The high vacuum pump (390) maintains a low base pressure and may maintain a pressure of several torr or less even when the step is performed. The upper surface of the exhaust port (360b) may be equal to or lower than the upper surface of the substrate entrance (360a).
[0196] The upper dome (352) may be made of a transparent dielectric such as quartz, sapphire, or ceramic. The upper dome (352) may be made of a ceramic material. Ceramic materials have better corrosion resistance and erosion resistance than quartz.
[0197] The upper dome (352) can be inserted into a protrusion formed on the upper surface of the chamber (360) and coupled with the chamber (360). The coupling portion of the upper dome (352) coupled with the chamber (360) for vacuum sealing may have a washer shape. The upper dome (352) may be arc-shaped or oval-shaped. The upper dome (352) can transmit infrared rays incident from below.
[0198] Infrared rays reflected from the electromagnetic shielding housing (330) can pass through the upper dome (352) and enter the substrate (374).
[0199] The lower dome (358) may be made of quartz or sapphire as a transparent dielectric. The lower dome (358) may include a washer-shaped joining portion that joins to a ledge formed on the lower surface of the chamber (360), a funnel-shaped lower dome body that extends downward from the joining portion, and a cylindrical pipe that extends downward from the center of the lower dome body. The lower dome (358) may be inserted into the ledge formed on the lower surface of the chamber (360) and joined to the chamber (360). The joining portion of the lower dome (358) that joins to the chamber (360) for vacuum sealing may be washer-shaped.
[0200] The drive shaft of the first lifter (384) and the drive shaft of the second lifter (382) may be inserted and placed within the cylindrical pipe of the lower dome (358). The purge gas supplied through the lower dome (358) may be supplied through a passage. The passage may be the cylindrical pipe of the lower dome (358). The purge gas may be an inert gas such as argon.
[0201] The upper liner (354) may be made of a transparent dielectric material. For example, the upper lighter (354) may be made of quartz, alumina, sapphire, or aluminum nitride. The upper liner (354) may be made of a material that inhibits the deposition of an abnormal layer.
[0202] The insulating member (362) is disposed between the lower surface of the chamber (360) and the reflector (361) and may be ring-shaped. The insulating member (362) may reduce heat transfer from the heated reflector (361) to the chamber (360). The insulating member (362) may be made of a ceramic material. The upper surface of the insulating member (362) may have a protrusion. The protrusion of the insulating member (362) and the protrusion of the lower surface of the chamber (360) may accommodate and vacuum-seal the washer-shaped joint portion of the lower dome (358).
[0203] The concentric ring-shaped lamp heater (366) may include a plurality of concentric ring-shaped lamp heaters and be connected to a power source (364). The concentric ring-shaped lamp heaters (366) are arranged at regular intervals along the inclined surface of the lower dome (358), and the concentric ring-shaped lamp heaters (366) may be divided into three groups and may be supplied with power independently of each other. The concentric ring-shaped lamp heaters (366) may be inserted and aligned into a ring-shaped groove formed on the inclined surface of the reflector (360).
[0204] For example, the concentric lamp heaters (366) may be halogen lamp heaters, and there may be eight of them. The three lamp heaters at the bottom may form a first group, the two lamp heaters in the middle may form a second group, and the three lamp heaters at the top may form a third group. The first group may be connected to a first power source (364a), the second group may be connected to a second power source (364b), and the third group may be connected to a third power source (364c). The first to third power sources (364a to 364c) may be independently controlled to uniformly heat the substrate.
[0205] The RF power source (340) can supply RF power to the antenna (310) through an impedance matching box (342) and a power supply line (343). The antenna (310) through which RF current flows must have a sufficient cross-sectional area for high current, and preferably forms a closed loop to form sufficient magnetic flux. The antenna (310) can use a vertically erected strip line to absorb infrared rays incident from above or below and minimize resistance increase due to heating. The antenna (310) provides high transmittance to infrared rays.
[0206] Additionally, the antenna (310) may be coated with gold (Au) or silver (Ag) to increase infrared reflection. Furthermore, a two-layer antenna (310) may be used to secure sufficient magnetic flux. The circular unit antenna may be positioned on the upper surface to receive RF power, thereby reducing power loss due to capacitive coupling.
[0207] The lower dome (358) covers the lower surface of the chamber (360), is formed of a transparent dielectric material, and may have the same curvature as the upper dome (352). The lamp heater (366) may be disposed on the lower surface of the lower dome (358). The reflector (361) may be disposed on the lower surface of the lamp heater (366).
[0208] In addition, a control unit (not shown) for controlling the RF power source (340) may be further included. Here, for example, a source material supply path (not shown) for supplying a raw material gas and a reactant material supply path (not shown) may be formed separately.
[0209] Meanwhile, a substrate can be placed into the chamber (360) on the substrate support (372) for a layer formation step. The substrate (374) can include various substrates for forming a gallium oxide (GaO) layer.
[0210] The substrate support member (372) may be provided with, for example, an electrostatic chuck or the like so that the substrate (374) can be fixedly supported, and the substrate (374) can be held in place by electrostatic force, or the substrate (374) can be supported by vacuum suction or mechanical force.
[0211] The clamp (350) may be arranged to cover the edge of the upper dome (352). The clamp (350) may be formed of a conductor and may be cooled by cooling water. The lower surface of the clamp (350) may have a protrusion to engage with a washer-shaped engaging portion of the upper dome (352) and may include a curved portion (150a) to cover a portion of the curved portion of the upper dome (352). The curved portion (150a) of the clamp (350) may be gold-plated to reflect infrared rays. The inner diameter of the clamp (350) may be substantially the same as the inner diameter of the upper liner (354). In addition, the inner diameter of the clamp (350) may be the same as the diameter of the antenna housing (330).
[0212] The chamber housing (332) can be placed on the clamp (350) and arranged to cover the antenna housing (330).
[0213] Meanwhile, it may be configured to supply a gas containing gallium (Ga) as a source material, and a gas containing oxygen (O) as a reactant material. Here, the gas containing gallium, for example, the source material, may include trimethyl gallium (TMGa) gas, and the gas containing oxygen, for example, the reactant material, may include oxygen (O2) gas or nitrous oxide (N2O) gas.
[0214] Although the embodiments of the present invention have been described in more detail with reference to the attached drawings, the present invention is not necessarily limited to these embodiments, and various modifications may be implemented without departing from the technical spirit of the present invention. Therefore, the embodiments disclosed in the present invention are not intended to limit the technical spirit of the present invention, but to explain it, and the scope of the technical spirit of the present invention is not limited by these embodiments. Therefore, it should be understood that the embodiments described above are illustrative in all aspects and not restrictive. The protection scope of the present invention should be interpreted by the claims, and all technical ideas within a scope equivalent thereto should be interpreted as being included in the scope of the rights of the present invention.
Claims
1. A method for forming a gallium oxide (GaO) layer on a substrate, a step of forming a first gallium oxide layer; and A step of forming a second gallium oxide layer on the first gallium oxide layer is included, A method for manufacturing a gallium oxide layer, wherein the step of forming one of the first gallium oxide layer and the second gallium oxide layer uses an atomic layer deposition (ALD) method, and the step of forming the other gallium oxide layer uses a chemical vapor deposition (CVD) method.
2. In paragraph 1, A method for manufacturing a gallium oxide layer, wherein the step of forming the first gallium oxide layer uses atomic layer deposition (ALD), and the step of forming the second gallium oxide layer uses chemical vapor deposition (CVD).
3. In paragraph 2, A step of forming a third gallium oxide layer containing gallium oxide on the second gallium oxide layer, The step of forming the third gallium oxide layer is a method for manufacturing a gallium oxide layer using an atomic layer deposition (ALD) method.
4. In paragraph 1, A method for manufacturing a gallium oxide layer, wherein the step of forming the first gallium oxide layer uses a chemical vapor deposition method, and the step of forming the second gallium oxide layer uses an atomic layer deposition method.
5. In paragraph 4, A step of forming a third gallium oxide layer containing gallium oxide on the second gallium oxide layer, The step of forming the third gallium oxide layer is a method for manufacturing a gallium oxide layer using a chemical vapor deposition method.
6. In any one of paragraphs 1 to 5, The step of forming the single gallium oxide layer using the above atomic layer deposition (ALD) method includes the steps of spraying a first source material containing gallium; Step of injecting the first purge gas; a step of injecting a first reactant material containing oxygen; and A method for manufacturing a gallium oxide layer, comprising a step of injecting a second purge gas.
7. In paragraph 6, The above first source material contains trimethyl gallium (TMGa), A method for producing a gallium oxide layer, wherein the first reactant material contains either oxygen (O2) or nitrous oxide (N2O).
8. In paragraph 6, A method for manufacturing a gallium oxide layer, further comprising a step of forming a plasma containing hydrogen (H2) gas or argon (Ar) gas between the step of injecting the first source material and the step of injecting the first reactant material.
9. In paragraph 6, A method for manufacturing a gallium oxide layer, further comprising a step of forming a plasma containing hydrogen (H2) gas or argon (Ar) gas after the step of injecting the first reactant material.
10. In paragraph 6, A method for manufacturing a gallium oxide layer, wherein a plasma containing oxygen is formed during the step of injecting the first reactant material.
11. In any one of paragraphs 1 to 5, The step of forming the remaining gallium oxide layer using the chemical vapor deposition (CVD) method includes the steps of spraying a first source material containing gallium; and A method for producing a gallium oxide layer, comprising the step of spraying a first reactant material containing oxygen.
12. In paragraph 11, The above first source material contains trimethyl gallium (TMGa), A method for producing a gallium oxide layer, wherein the first reactant material contains either oxygen (O2) or nitrous oxide (N2O).
13. In paragraph 11, A method for manufacturing a gallium oxide layer, further comprising a step of forming a plasma containing hydrogen (H2) gas or argon (Ar) gas after the step of injecting the first source material and the step of injecting the first reactant material.
14. In paragraph 11, A method for manufacturing a gallium oxide layer, wherein a plasma containing oxygen is formed during the step of injecting the first source material and the step of injecting the first reactant material.
Citation Information
Patent Citations
Multilayer semiconductor material structure and preparation method thereof
CN114628229A
Semiconductor device and manufacturing method thereof
JP2020021828A
Semiconductor device and manufacturing method for the same
JP2022039096A
Thin film transistor and manufacturing method thereof
KR1020160099346A
Crystallizer for extracting powder from sludge or liquid using centrifugal force
KR1020210122748A