Low-stress organosilicon double-component potting compound and preparation method therefor

By using single-ended vinyl silicone oil and silica-coated nano-copper particles as fillers, the problems of silicone potting compound penetration and device protection in micro-gaps were solved, achieving a balance between low stress, high flowability, and low adhesion performance.

WO2024239425A1PCT designated stage expired Publication Date: 2024-11-28GOLOHO POLYMER (JIANGXI) CO LTD
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
PCT/CN2023/104407
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-05-23
Filing Date
2023-06-30
Publication Date
2024-11-28

AI Technical Summary

Technical Problem

Existing silicone potting compounds struggle to achieve a balance between low stress, high flowability, and low adhesion, particularly in terms of penetration into tiny gaps and protection of micro-devices.

Method used

Single-ended vinyl silicone oil and nano-copper particles are used as thermally conductive fillers. By coating the surface of the nano-copper particles with a silica layer and using a filler treatment agent for surface modification, the reaction sites and viscosity are reduced, and the fluidity is improved. At the same time, methyl silicone oil is added to ensure the smoothness and low viscosity of the colloid.

Benefits of technology

It significantly reduces the internal stress of the potting compound, improves its flowability and permeability, ensures that small devices are not damaged during secondary repairs, and maintains good thermal conductivity.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure PCTCN2023104407-APPB-I100001
    Figure PCTCN2023104407-APPB-I100001
  • Figure PCTCN2023104407-APPB-I100002
    Figure PCTCN2023104407-APPB-I100002
  • Figure PCTCN2023104407-APPB-I100003
    Figure PCTCN2023104407-APPB-I100003
Patent Text Reader

Abstract

A low-stress organosilicon double-component potting compound and a preparation method therefor. The potting compound comprises a component A and a component B, wherein the component A comprises 80 parts of a base material, 15-20 parts of methyl silicone oil and 0.5-1 part of a platinum catalyst, and the component B comprises 80 parts of the base material, 15-20 parts of methyl silicone oil, 1.5-2 parts of hydrogen-containing silicone oil and 0.01-0.05 part of an inhibitor. The base material comprises 5-25 parts of mono-vinyl-terminated silicone oil, 5-15 parts of a first heat conduction filler, 20-40 parts of a second heat conduction filler, 5-15 parts of methyl silicone oil and 0.1-0.6 part of a filler treatment agent, the first heat conduction filler comprising nano-copper particles and a silicon dioxide layer coating the surfaces of the nano-copper particles. The present application uses the mono-vinyl-terminated silicone oil as a raw material, thereby effectively reducing reaction sites between the present application and hydrogen-containing silicone oil. In addition, the present application further reduces the dosages of the heat conduction fillers while ensuring the heat conduction performance of the heat conduction fillers, thereby reducing the internal stress of the organic silicon potting compound after curing of same, and further improving the fluidity thereof and reducing the hardness of same.
Need to check novelty before this filing date? Find Prior Art

Description

A low-stress organosilicon two-component potting compound and its preparation method Technical Field

[0001] The present invention relates to the field of organosilicon potting adhesives, and in particular to a low-stress organosilicon two-component potting adhesive and a preparation method thereof. Background Art

[0002] In recent years, the demand for greater integration and miniaturization of electronic components has increased, placing increasingly stringent demands on potting materials. Addition-type silicone potting compounds have been widely used in component packaging due to their resistance to small molecule release, lack of shrinkage, and elasticity within a temperature range of -50°C to 200°C.

[0003] However, due to the large amount of thermally conductive filler added, addition-type silicone encapsulants have a relatively high viscosity and poor fluidity, making them difficult to penetrate into tiny gaps, especially those less than 1mm. Furthermore, the hardness of the colloid gradually increases under high and low temperature conditions, which can cause internal stress in the device. Furthermore, because the colloid itself is relatively soft and viscous, secondary repairs can easily damage tiny devices.

[0004] Patent application number 201910675359.1 discloses a two-component silicone potting adhesive, which includes component A and component B of equal mass; the component A includes a base material, double-ended vinyl silicone oil, methyl silicone oil, and a platinum catalyst; the component B includes a base material, methyl silicone oil, hydrogen-containing silicone oil, hydrogen-terminated silicone oil, a tackifier, a black paste, and an inhibitor; the base material includes double-ended vinyl silicone oil, a thermally conductive filler, and a filler treatment agent, and the tackifier is a silane coupling agent with epoxy and vinyl groups. The adhesive has excellent flow properties and low stress, but its strong viscosity makes it difficult to apply to the potting of tiny devices that need to be repaired. Summary of the Invention

[0005] The present invention aims to overcome the defect that the prior art two-component silicone potting adhesive is difficult to achieve a balance between low stress, high flow performance and low adhesion performance, and provides a low-stress two-component silicone potting adhesive and a preparation method thereof to overcome the above-mentioned defect.

[0006] To achieve the above-mentioned purpose, the present invention is implemented through the following technical solutions:

[0007] In a first aspect, the present invention first provides a low-stress two-component silicone potting compound, comprising component A and component B;

[0008] The component A comprises 80 parts of base material, 15-20 parts of methyl silicone oil, and 0.5-1 part of platinum catalyst;

[0009] The B component includes 80 parts of base material, 15-20 parts of methyl silicone oil, 1.5-2 parts of hydrogenated silicone oil, and 0.01-0.05 parts of inhibitor;

[0010] The base material comprises 5-25 parts of single-end vinyl silicone oil, 5-15 parts of a first thermally conductive filler, 20-40 parts of a second thermally conductive filler, 5-15 parts of methyl silicone oil, and 0.1-0.6 parts of a filler treatment agent;

[0011] The first thermally conductive filler includes nano copper particles and a silicon dioxide layer coated on the surface of the nano copper particles.

[0012] Research by the applicants has revealed that stress in silicone potting compounds originates from the addition reaction between hydrogenated silicone oil and vinylated silicone oil, specifically the process by which hydrogen and double bonds are converted into saturated structures. The lower the vinyl content of the vinyl silicone oil and the hydrogen content of the hydrogenated silicone oil, the fewer reaction sites there are, and the lower the stress in the silicone potting compound.

[0013] Currently, existing silicone potting compounds typically use vinyl silicone oil containing vinyl groups at both ends as a raw material. However, since both ends participate in the addition reaction with the hydrogenated silicone oil, the ends of the main chain are pulled and fixed after the reaction, preventing free rotation. This causes resistance during the main chain's structural adjustment, generating internal stress within the potting compound.

[0014] In order to overcome the above phenomenon, the present application adopts a single-end containing vinyl silicone oil as raw material. Since only one end participates in the reaction while the other end can still rotate freely during the addition process with hydrogen silicone oil, the chain segment can still freely adjust the structure after the reaction is completed, significantly reducing the generation of internal stress. At the same time, due to the reduction of the connection site, its viscosity and bonding performance also show a relatively obvious decline, which is more easily separated from the micro device, thereby facilitating the repair of the micro device.

[0015] In addition, the present invention further reduces the viscosity of the potting compound to improve its fluidity by innovating the formulation of thermally conductive fillers. In this application, a method of compounding a first thermally conductive filler and a second thermally conductive filler is adopted, wherein the first thermally conductive filler is composed of nano-copper particles and a silicon dioxide layer. Because the thermal conductivity of metallic copper particles is far higher than that of conventional inorganic thermally conductive fillers (such as silicon micropowder and aluminum oxide powder), the addition of the first thermally conductive filler can significantly reduce the overall amount of thermally conductive filler added while maintaining the same thermal conductivity, effectively avoiding the impact of excessive thermally conductive filler on the viscosity of the potting compound and ensuring its better fluidity.

[0016] In addition, the surface of the nano-copper particles is coated with a layer of silicon dioxide, which has extremely low electrical conductivity, effectively avoiding the influence of nano-copper on the electrical conductivity of the overall potting compound, and can be applied to the packaging process of electronic components. The main chain of the silicon dioxide layer and the silicone potting compound is also a Si-O-Si structure, so the compatibility between them is relatively high. However, the silicon dioxide layer in the first thermally conductive filler and the surface of the second thermally conductive filler usually have more -OH hydrophilic structures. Therefore, the present application uses a filler treatment agent to modify the surface of the first and second thermally conductive fillers, so that the filler treatment agent can react with the -OH hydrophilic structure on the surface of the silicon dioxide to form an oleophilic structure, which is conducive to the mixing of the filler and the silicone oil.

[0017] Finally, under the premise of ensuring the performance of the colloid, sufficient methyl silicone oil is added to the formula to make the surface of the colloid smooth and flat after curing, with low viscosity, and will not cause damage to tiny devices during secondary repair.

[0018] Preferably, the preparation method of the first thermally conductive filler is as follows:

[0019] A copper precursor and a trialkoxysilane with a ligand group are dissolved and dispersed in water, an acidic reducing agent is added to reduce the copper precursor to obtain nano-copper particles, and the trialkoxysilane with a ligand group is hydrolyzed to form a silicon dioxide layer to coat the nano-copper particles, thereby obtaining nano-copper particles coated with the silicon dioxide layer. After filtering and washing, the particles are dried and heat-treated in a vacuum environment to obtain the first thermally conductive filler.

[0020] The nano-copper particles in the first thermally conductive filler of this application are formed by reducing a copper precursor with a reducing agent. After the nano-copper particles are prepared, the ligand groups in the trialkoxysilane with ligand groups attract and cooperate with the nano-copper particles, thereby encapsulating the nano-copper particles. Because the acidic reducing agent catalyzes the reduction of the copper precursor, the alkoxy groups in the trialkoxysilane with ligand groups form a cross-linked silica layer during the hydrolysis and condensation process, thereby tightly encapsulating the nano-copper particles and protecting them.

[0021] Preferably, the ligand group in the trialkoxysilane having a ligand group includes any one of a pyrrolidone group, an amide group, a pyridine group, and a carboxylic acid group.

[0022] Preferably, the copper precursor includes any one of copper chloride, copper sulfate and copper acetate.

[0023] Preferably, the acidic reducing agent includes any one of citric acid, ascorbic acid, oxalic acid, and oxalic acid.

[0024] Preferably, the reduction temperature is 70-85° C., and the reaction time is 3-5 h.

[0025] Preferably, the single-end vinyl silicone oil is a linear vinyl polydimethylsiloxane;

[0026] The single-end vinyl silicone oil has a vinyl content of 0.15-0.25% and a viscosity of 500-1000 mPa·s.

[0027] Preferably, the second thermally conductive filler is silicon powder and / or aluminum oxide;

[0028] The average particle size of the silicon powder and / or aluminum oxide is 5 to 20 μm.

[0029] Preferably, the viscosity of the methyl silicone oil is 100 mPa·s-1000 mPa·s.

[0030] Preferably, the hydrogen content of the hydrogen-containing silicone oil is 0.1-0.36%.

[0031] Preferably, the filler treating agent is a chlorosilane containing an alkyl group having 12 to 20 carbon atoms.

[0032] In a second aspect, the present invention further provides a method for preparing the low-stress two-component silicone potting compound, comprising the following steps:

[0033] 1) Preparing a base material: blending and dehydrating a single-end vinyl silicone oil, a first thermally conductive filler, a second thermally conductive filler, and a methyl silicone oil, then adding a filler treatment agent to treat the first thermally conductive filler and the second thermally conductive filler, and then continuing to blend and dehydrate to obtain the base material;

[0034] 2) Preparation of component A: Mix the base material, methyl silicone oil, and platinum catalyst evenly, and evacuate to remove bubbles to obtain component A;

[0035] 3) Preparation of component B: Mix the base material, methyl silicone oil, hydrogenated silicone oil, and inhibitor evenly, and evacuate to remove air bubbles to obtain component B;

[0036] 4) Preparing the organic silicone potting compound: uniformly mix the component A prepared in step 2) and the component B prepared in step 3) in a weight ratio of 1:1, and vacuum the mixture to remove air bubbles, thereby obtaining the organic silicone potting compound.

[0037] Preferably, the step (1) is specifically as follows:

[0038] Single-end vinyl silicone oil, a first thermally conductive filler, a second thermally conductive filler, and methyl silicone oil are blended and dehydrated at a temperature of 120-130°C and a vacuum degree of ≤-0.095MPa for 1-5 hours; the temperature is lowered to 70-90°C, a filler treatment agent is added, and the temperature is kept for 0.5-2 hours; the temperature is again raised to 120-130°C and a vacuum degree of ≤-0.095MPa, and the mixture is blended and dehydrated for 1-2 hours to obtain the base material.

[0039] Therefore, the present invention has the following beneficial effects:

[0040] (1) This application uses single-end vinyl silicone oil as a raw material, thereby effectively reducing the reaction sites between the silicone oil and the hydrogen-containing silicone oil, thereby reducing the internal stress of the silicone potting compound after curing, while improving its fluidity and reducing its hardness;

[0041] (2) This application has made certain improvements to the thermal conductive filler. On the basis of ensuring the thermal conductivity of the thermal conductive filler, the amount of thermal conductive filler added is further reduced, the viscosity of the organic potting compound is reduced, and its fluidity is improved;

[0042] (3) While ensuring the performance of the colloid, a relatively large amount of methyl silicone oil is added to the formula, so that the surface of the colloid after curing is relatively smooth and has low viscosity, which will not cause damage to tiny devices during secondary repair. Implementation Method

[0043] The present invention will be further described below with reference to specific embodiments. Those skilled in the art will be able to implement the present invention based on these descriptions. Furthermore, the embodiments of the present invention described below generally represent only a portion of the present invention, rather than all of the embodiments. Therefore, all other embodiments derived by those skilled in the art based on the embodiments of the present invention without inventive effort should fall within the scope of protection of the present invention.

[0044]

Preparation of trialkoxysilane with ligand group

[0045] Trialkoxysilane A1: Under nitrogen atmosphere, 16.4 (0.1 mol) of triethoxysilane and 11.1 (0.1 mol) of vinylpyrrolidone were dissolved in 200 ml of toluene, 3000 ppm of Custer catalyst was added, and the mixture was heated and refluxed for 3 h. The reaction was then stopped, and 1 g of activated carbon was added. The mixture was stirred at room temperature for 30 min and filtered. The toluene in the filtrate was evaporated to obtain trialkoxysilane A1. The reaction schematic is shown in the following formula (1):

[0046]

[0047] Formula (1).

[0048] Trialkoxysilane A2: Under nitrogen atmosphere, 16.4 (0.1 mol) of triethoxysilane and 10.5 (0.1 mol) of 4-vinylpyridine were dissolved in 200 ml of toluene, 3000 ppm of Custer catalyst was added, and the temperature was raised and refluxed for 3 h. The reaction was then stopped, and 1 g of activated carbon was added. The mixture was stirred at room temperature for 30 min and then filtered. The toluene in the filtrate was evaporated to obtain trialkoxysilane A2. The reaction schematic is shown in the following formula (2):

[0049]

[0050] Formula (2).

[0051] Trialkoxysilane A3: Under nitrogen atmosphere, 16.4 (0.1 mol) of triethoxysilane and 9.8 (0.1 mol) of maleic anhydride were dissolved in 200 ml of toluene, 3000 ppm of Custer catalyst was added, and the mixture was heated and refluxed for 3 h. The reaction was then stopped, and 1 g of activated carbon was added. The mixture was stirred at room temperature for 30 min and filtered. The toluene in the filtrate was evaporated to obtain trialkoxysilane A3. The reaction schematic is shown in the following formula (3):

[0052]

[0053] Formula (3).

[0054]

Preparation of the first thermally conductive filler

[0055] First thermally conductive filler B1: Dissolve 16g (0.1mol) of copper sulfate and 27.5g (0.1mol) of triethoxysilane A1 in 50g of water to form solution A. Dissolve 25g of ascorbic acid in 60g of water to form solution B. Add solution A dropwise to solution B, and stir at 75°C for 5h. The reaction reduces the copper precursor to produce nano-copper particles and hydrolyzes the triethoxysilane A1 to form a silica layer that coats the nano-copper particles, resulting in a precipitate of nano-copper particles coated with a silica layer. The precipitate is centrifuged at 4000r / min, the supernatant removed, and washed with ethanol for 5min. After further centrifugation, the supernatant removed, and the mixture was heated to 110°C and dried for 5h under vacuum to obtain the first thermally conductive filler B1.

[0056] First thermally conductive filler B2: Dissolve 16g (0.1mol) of copper sulfate and 27g (0.1mol) of triethoxysilane A2 in 50g of water to form solution A. Dissolve 25g of citric acid in 50g of water to form solution B. Add solution A dropwise to solution B, and stir at 75°C for 5h. The reaction reduces the copper precursor to produce nano-copper particles and hydrolyzes triethoxysilane A2 to form a silica layer, thereby coating the nano-copper particles. A nano-copper particle precipitate coated with a silica layer is obtained. The precipitate is centrifuged at 4000r / min, the supernatant is removed, and the precipitate is shaken and washed with ethanol for 5min. After further centrifugation, the supernatant is removed, and the temperature is raised to 110°C and dried for 5h under vacuum to obtain the first thermally conductive filler B2.

[0057] First thermally conductive filler B3: Dissolve 16g (0.1mol) of copper sulfate and 26g (0.1mol) of triethoxysilane A3 in 50g of water to form solution A. Dissolve 25g of ascorbic acid in 60g of water to form solution B. Add solution A dropwise to solution B, and stir at 75°C for 5h. The reaction reduces the copper precursor to form nano-copper particles, and hydrolyzes triethoxysilane A3 to form a silica layer, thereby coating the nano-copper particles. A nano-copper particle precipitate coated with a silica layer is obtained. The precipitate is centrifuged at 4000r / min, and the supernatant is removed. The precipitate is then washed with ethanol for 5min, centrifuged again, and the supernatant is removed. The temperature is raised to 110°C and dried for 5h under vacuum to obtain the first thermally conductive filler B3.

[0058] First thermally conductive filler B4: 16g (0.1mol) of copper sulfate and 21g (0.1mol) of tetraethoxysilane were dissolved in 50g of water to form solution A. 25g of ascorbic acid was dissolved in 60g of water to form solution B. Solution A was added dropwise to solution B, and the mixture was stirred and reacted at 75°C for 5h. The reaction reduced the copper precursor to obtain nano-copper particles, and hydrolyzed the tetraethoxysilane to form a silica layer, thereby coating the nano-copper particles. Nano-copper particles coated with a silica layer were precipitated. The precipitate was centrifuged at 4000r / min, and the supernatant was removed. The precipitate was then washed with ethanol by shaking for 5min, and the supernatant was removed after another centrifugation. The mixture was heated to 110°C and dried for 5h under vacuum to obtain the first thermally conductive filler B4.

[0059] Example 1

[0060] A low-stress two-component silicone potting compound, comprising component A and component B;

[0061] The component A includes 80 parts of base material, 18 parts of methyl silicone oil, and 0.8 parts of 3000ppm platinum catalyst;

[0062] The component B comprises 80 parts of base material, 15 parts of methyl silicone oil, 1.8 parts of hydrogenated silicone oil with a hydrogen content of 0.25%, and 0.03 parts of 1-hexynyl-1-cyclohexanol;

[0063] The base material includes 20 parts of single-end vinyl silicone oil with a vinyl content of 0.2% and a viscosity of 800 mPa·s, 10 parts of a first thermally conductive filler B1, 35 parts of a second thermally conductive filler (spherical aluminum oxide with an average particle size of 10 μm), 10 parts of methyl silicone oil, and 0.5 parts of dodecyldimethylchlorosilane.

[0064] The preparation method comprises the following steps:

[0065] (1) Preparation of base material: single-end vinyl silicone oil, first thermal conductive filler B1, second thermal conductive filler, and methyl silicone oil are blended and dehydrated at a temperature of 120-130°C and a vacuum degree of -0.095MPa for 2 hours; the temperature is lowered to 80°C, a filler treatment agent is added, and the temperature is kept for 1 hour; the temperature is then raised to 120-130°C and the vacuum degree is -0.095MPa, and the blending and dehydration are continued for 2 hours to obtain the base material;

[0066] (2) Preparation of component A: Mix the base material, methyl silicone oil, and platinum catalyst evenly, and evacuate to remove bubbles to obtain component A;

[0067] (3) Preparation of component B: Mix the base material, methyl silicone oil, hydrogenated silicone oil, and inhibitor evenly, and evacuate to remove air bubbles to obtain component B;

[0068] (4) Preparation of organic silicone potting compound: uniformly mix the component A prepared in step 2) and the component B prepared in step 3) in a weight ratio of 1:1, and vacuum the mixture to remove air bubbles to obtain the organic silicone potting compound.

[0069] Example 2

[0070] A low-stress two-component silicone potting compound, comprising component A and component B;

[0071] The component A includes 80 parts of base material, 18 parts of methyl silicone oil, and 0.8 parts of 3000ppm platinum catalyst;

[0072] The component B comprises 80 parts of base material, 15 parts of methyl silicone oil, 1.8 parts of hydrogenated silicone oil with a hydrogen content of 0.25%, and 0.03 parts of 1-hexynyl-1-cyclohexanol;

[0073] The base material includes 20 parts of single-end vinyl silicone oil with a vinyl content of 0.2% and a viscosity of 800 mPa·s, 10 parts of a first thermally conductive filler B2, 35 parts of a second thermally conductive filler (spherical aluminum oxide with an average particle size of 10 μm), 10 parts of methyl silicone oil, and 0.5 parts of dodecyldimethylchlorosilane.

[0074] The preparation method is shown in Example 1.

[0075] Example 3

[0076] A low-stress two-component silicone potting compound, comprising component A and component B;

[0077] The component A includes 80 parts of base material, 18 parts of methyl silicone oil, and 0.8 parts of 3000ppm platinum catalyst;

[0078] The component B comprises 80 parts of base material, 15 parts of methyl silicone oil, 1.8 parts of hydrogenated silicone oil with a hydrogen content of 0.25%, and 0.03 parts of 1-hexynyl-1-cyclohexanol;

[0079] The base material includes 20 parts of single-end vinyl silicone oil with a vinyl content of 0.2% and a viscosity of 800 mPa·s, 10 parts of a first thermally conductive filler B3, 35 parts of a second thermally conductive filler (spherical aluminum oxide with an average particle size of 10 μm), 10 parts of methyl silicone oil, and 0.5 parts of dodecyldimethylchlorosilane.

[0080] The preparation method is shown in Example 1.

[0081] Example 4

[0082] A low-stress two-component silicone potting compound, comprising component A and component B;

[0083] The component A includes 80 parts of base material, 18 parts of methyl silicone oil, and 0.5 parts of 3000ppm platinum catalyst;

[0084] The component B comprises 80 parts of base material, 15 parts of methyl silicone oil, 1.5 parts of hydrogenated silicone oil with a hydrogen content of 0.1%, and 0.01 parts of 1-hexynyl-1-cyclohexanol;

[0085] The base material includes 5 parts of single-end vinyl silicone oil with a vinyl content of 0.15% and a viscosity of 1000 mPa·s, 5 parts of a first thermally conductive filler B3, 20 parts of a second thermally conductive filler (spherical aluminum oxide with an average particle size of 10 μm), 15 parts of methyl silicone oil, and 0.1 part of dodecyldimethylchlorosilane.

[0086] The preparation method is shown in Example 1.

[0087] Example 5

[0088] A low-stress two-component silicone potting compound, comprising component A and component B;

[0089] The component A includes 80 parts of base material, 20 parts of methyl silicone oil, and 1 part of 3000ppm platinum catalyst;

[0090] The component B comprises 80 parts of base material, 20 parts of methyl silicone oil, 2 parts of hydrogenated silicone oil with a hydrogen content of 0.36%, and 0.05 parts of 1-hexynyl-1-cyclohexanol;

[0091] The base material includes 25 parts of single-end vinyl silicone oil with a vinyl content of 0.25% and a viscosity of 500 mPa·s, 15 parts of a first thermally conductive filler B3, 30 parts of a second thermally conductive filler (spherical aluminum oxide with an average particle size of 10 μm), and 0.6 parts of dodecyldimethylsilyl chloride.

[0092] The preparation method is shown in Example 1.

[0093] Example 6

[0094] A low-stress two-component silicone potting compound, comprising component A and component B;

[0095] The component A includes 80 parts of base material, 15 parts of methyl silicone oil, and 1 part of 3000ppm platinum catalyst;

[0096] The B component includes 80 parts of base material, 20 parts of methyl silicone oil, 2 parts of hydrogenated silicone oil with a hydrogen content of 0.36%, and 0.03 parts of 1-hexynyl-1-cyclohexanol;

[0097] The base material includes 25 parts of single-end vinyl silicone oil with a vinyl content of 0.25% and a viscosity of 500 mPa·s, 12 parts of a first thermally conductive filler B3, 36 parts of a second thermally conductive filler (spherical aluminum oxide with an average particle size of 10 μm), and 0.3 parts of octadecyldimethylsilyl chloride.

[0098] The preparation method is shown in Example 1.

[0099] Comparative Example 1

[0100] A low-stress two-component silicone potting compound, comprising component A and component B;

[0101] The component A includes 80 parts of base material, 18 parts of methyl silicone oil, and 0.8 parts of 3000ppm platinum catalyst;

[0102] The component B comprises 80 parts of base material, 15 parts of methyl silicone oil, 1.8 parts of hydrogenated silicone oil with a hydrogen content of 0.25%, and 0.03 parts of 1-hexynyl-1-cyclohexanol;

[0103] The base material includes 20 parts of single-end vinyl silicone oil with a vinyl content of 0.2% and a viscosity of 800 mPa·s, 65 parts of a second thermal conductive filler (spherical aluminum oxide with an average particle size of 10 μm), 10 parts of methyl silicone oil, and 0.5 parts of dodecyldimethylchlorosilane.

[0104] The preparation method is shown in Example 1.

[0105] Comparative Example 2

[0106] A low-stress two-component silicone potting compound, comprising component A and component B;

[0107] The component A includes 80 parts of base material, 18 parts of methyl silicone oil, and 0.8 parts of 3000ppm platinum catalyst;

[0108] The component B comprises 80 parts of base material, 15 parts of methyl silicone oil, 1.8 parts of hydrogenated silicone oil with a hydrogen content of 0.25%, and 0.03 parts of 1-hexynyl-1-cyclohexanol;

[0109] The base material includes 20 parts of double-ended vinyl silicone oil with a vinyl content of 0.2% and a viscosity of 800 mPa·s, 10 parts of a first thermally conductive filler B1, 35 parts of a second thermally conductive filler (spherical aluminum oxide with an average particle size of 10 μm), 10 parts of methyl silicone oil, and 0.5 parts of dodecyldimethylchlorosilane.

[0110] The preparation method is shown in Example 1.

[0111] Comparative Example 3

[0112] A low-stress two-component silicone potting compound, comprising component A and component B;

[0113] The component A includes 80 parts of base material, 18 parts of methyl silicone oil, and 0.8 parts of 3000ppm platinum catalyst;

[0114] The component B comprises 80 parts of base material, 15 parts of methyl silicone oil, 1.8 parts of hydrogenated silicone oil with a hydrogen content of 0.25%, and 0.03 parts of 1-hexynyl-1-cyclohexanol;

[0115] The base material includes 20 parts of single-end vinyl silicone oil with a vinyl content of 0.2% and a viscosity of 800 mPa·s, 10 parts of a first thermally conductive filler B4, 35 parts of a second thermally conductive filler (spherical aluminum oxide with an average particle size of 10 μm), 10 parts of methyl silicone oil, and 0.5 parts of dodecyldimethylchlorosilane.

[0116] The preparation method is shown in Example 1.

[0117] Examples 1 to 5 and Comparative Examples 1 to 3 were tested for leveling, thermal conductivity, electrical conductivity, and hardness, respectively.

[0118] in:

[0119] Leveling: Take 0.5 ml of glue and drop it into a polytetrafluoroethylene tank at a certain angle, and test the length of the glue after 3 minutes.

[0120] Thermal conductivity: Thermal conductivity is tested in accordance with GB / T10297-2015.

[0121] Hardness: The potting glue is cured to obtain a colloid, and its Shore hardness is tested.

[0122] The test results are shown in Table 1 below

[0123]

[0124] The results in the table above demonstrate that the two-component silicone potting compound in this application exhibits excellent leveling properties, allowing it to penetrate even tiny gaps, making it suitable for potting tiny electronic components. Furthermore, after curing, it exhibits low hardness, resulting in low internal stress, and exhibits excellent thermal conductivity and dielectric constant.

[0125] By comparing Example 1 with Comparative Example 1, it was found that the first thermally conductive filler was not added in Comparative Example 1. Therefore, in order to achieve a similar thermal conductivity coefficient, more second thermally conductive filler was added in Comparative Example 1, resulting in reduced leveling and increased hardness.

[0126] By comparing Example 1 with Comparative Example 2, it was found that after replacing the single-terminal vinyl silicone oil with the double-terminal vinyl silicone oil, the hardness after curing was significantly improved, indicating that the single-terminal vinyl silicone oil can effectively reduce the internal stress of the potting compound.

[0127] By comparing Example 1 with Comparative Example 3, it was found that after changing the type of the first thermally conductive filler, since no ligand was introduced during the preparation of the first thermally conductive filler B4, the silica could not completely cover the copper nanoparticles, resulting in a decrease in its dielectric constant, indicating that the introduction of the ligand has a significant effect on the electrical conductivity of the first thermally conductive filler.

Claims

1. A low-stress two-component silicone potting adhesive, characterized in that: It includes component A and component B; The component A comprises 80 parts of base material, 15-20 parts of methyl silicone oil, and 0.5-1 part of platinum catalyst; The component B comprises 80 parts of base material, 15-20 parts of methyl silicone oil, 1.5-2 parts of hydrogen-containing silicone oil, and 0.01-0.05 parts of inhibitor; The base material comprises 5-25 parts of single-end vinyl silicone oil, 5-15 parts of a first thermally conductive filler, 20-40 parts of a second thermally conductive filler, 5-15 parts of methyl silicone oil, and 0.1-0.6 parts of a filler treatment agent; The first thermally conductive filler includes nano copper particles and a silicon dioxide layer coated on the surface of the nano copper particles.

2. The low stress organic silicon two-component potting adhesive according to claim 1, characterized in that: The preparation method of the first thermally conductive filler is as follows: A copper precursor and a trialkoxysilane with a ligand group are dissolved and dispersed in water, an acidic reducing agent is added, and the copper precursor is reduced to obtain nano copper particles, and the trialkoxysilane with a ligand group is hydrolyzed to form a silicon dioxide layer to coat the nano copper particles, thereby obtaining nano copper particles coated with a silicon dioxide layer. After filtering and washing, the nano copper particles are dried and heat treated in a vacuum environment to obtain the first thermal conductive filler.

3. The low stress two-component silicone potting adhesive according to claim 2, characterized in that: The ligand group in the trialkoxysilane with a ligand group includes any one of a pyrrolidone group, an amide group, a pyridine group and a carboxylic acid group.

4. A low stress organosilicon two-component potting adhesive according to any one of claims 1 to 3, characterized in that: The single-terminated vinyl silicone oil is a linear vinyl polydimethylsiloxane; The single-terminated vinyl silicone oil has a vinyl content of 0.15-0.25% and a viscosity of 500-1000 mPa·s.

5. A low stress organosilicon two-component potting adhesive according to claims 1 to 3, characterized in that: The second thermally conductive filler is silicon powder and / or aluminum oxide; The average particle size of the silicon powder and / or alumina is 5-20 μm.

6. A low stress organosilicon two-component potting adhesive according to claims 1 to 3, characterized in that: The viscosity of the methyl silicone oil is 100 mPa·s-1000 mPa·s.

7. A low stress organosilicon two-component potting adhesive according to claims 1 to 3, characterized in that: The hydrogen content of the hydrogen-containing silicone oil is 0.1-0.36%.

8. The low stress organic silicon two-component potting adhesive according to claim 1 to 3, characterized in that: The filler treating agent is a chlorosilane containing an alkyl group having 12 to 20 carbon atoms.

9. A method for preparing the low stress organosilicon two-component potting adhesive according to any one of claims 1 to 8, characterized in that: The following steps are involved: 1) preparing a base material: blending and dehydrating a single-end vinyl silicone oil, a first thermally conductive filler, a second thermally conductive filler, and a methyl silicone oil, then adding a filler treatment agent to treat the first thermally conductive filler and the second thermally conductive filler, and then continuing to blend and dehydrate to obtain the base material; 2) Preparation of component A: uniformly mix the base material, methyl silicone oil and platinum catalyst, and evacuate to remove bubbles to obtain component A; 3) Preparation of component B: uniformly mix the base material, methyl silicone oil, hydrogen-containing silicone oil and inhibitor, and evacuate to remove bubbles to obtain component B; 4) Preparing the organic silicone potting adhesive: uniformly mixing the component A prepared in step 2) and the component B prepared in step 3) at a weight ratio of 1:1, and evacuating the mixture to remove air bubbles, thereby obtaining the organic silicone potting adhesive.

10. The method according to claim 9, characterized in that The step (1) is specifically as follows: The single-ended vinyl silicone oil, the first thermal conductive filler, the second thermal conductive filler and the methyl silicone oil are mixed and dehydrated at a temperature of 120-130°C and a vacuum degree of ≤-0.095MPa for 1-5 hours; the temperature is lowered to 70-90°C, a filler treatment agent is added and the mixture is kept warm for 0.5-2 hours; the temperature is raised to 120-130°C and the vacuum degree is ≤-0.095MPa and the mixture is mixed and dehydrated for 1-2 hours to obtain the base material.

Citation Information

Patent Citations

  • Organic silicon pouring sealant and preparation method thereof

    CN110819298A

  • Heat-conducting silica gel as well as preparation method and application thereof

    CN111004510A

  • Low-modulus heat-conducting organopolysiloxane composition as well as preparation method and application thereof

    CN111154269A

  • Low-dielectric-constant organic silicon pouring sealant and preparation method thereof

    CN111423842A

  • Bi-component addition type heat-conducting silica gel for heat dissipation of LED lighting chip

    CN113444487A