Method for evaluating adsorption property and reaction mechanism of rubber particles in rubber-modified asphalt

By dispersing rubber particles in asphalt and determining their adsorption characteristics and reaction mechanisms using multiple analytical means, the problem of restricted application of rubber particles in asphalt is solved, and effective formulation and mixing conditions design of rubber modified asphalt is realized.

WO2024239546A1PCT designated stage expired Publication Date: 2024-11-28SOUTH CHINA UNIV OF TECH

Patent Information

Application Number
PCT/CN2023/128603
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-05-22
Filing Date
2023-10-31
Publication Date
2024-11-28

AI Technical Summary

Technical Problem

In the prior art, the adsorption characteristics and reaction mechanism of rubber particles in asphalt are not yet clear, which limits their application in asphalt.

Method used

By dispersing rubber particles in asphalt, performing multiple tetrahydrofuran soaking, and using gel permeation chromatography, Fourier transform infrared spectroscopy and thermogravimetric analysis, the molecular weight adsorption preference of rubber particles to asphalt, as well as rubber, are determined by rubber permeation chromatography, Fourier transform infrared spectroscopy and thermogravimetric analysis. Changes in composition before and after reaction between particles and asphalt.

Benefits of technology

The adsorption characteristics and reaction mechanism of rubber particles in rubber modified asphalt are clarified, which will help optimize the formulation and design of mixing conditions of rubber modified asphalt.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN2023128603_28112024_PF_FP_ABST
    Figure CN2023128603_28112024_PF_FP_ABST
Patent Text Reader

Abstract

A method for evaluating the adsorption property and reaction mechanism of rubber particles in rubber-modified asphalt, comprising the following steps: 1) preparing rubber-modified asphalt; 2) separating in the rubber-modified asphalt rubber particles from an asphalt liquid phase; 3) according to a gel permeation chromatogram, determining the adsorption preference of the rubber particles with respect to the molecular weight of the asphalt and, according to a Fourier transform infrared spectrum, determining the adsorption preference of the rubber particles with respect to functional groups of the asphalt; and 4) according to thermogravimetric analysis data, determining the change of components of the rubber particles before and after a reaction between the rubber particles and the asphalt. The method can obtain the adsorption property of the rubber particles in the rubber-modified asphalt and the reaction mechanism between the rubber particles and the asphalt, being conducive to the formulation optimization and mixing condition design of the rubber-modified asphalt.
Need to check novelty before this filing date? Find Prior Art

Description

A method for evaluating the adsorption characteristics and reaction mechanism of rubber particles in rubber-modified asphalt Technical Field

[0001] The present invention relates to the technical field of modified asphalt, and in particular to a method for evaluating the adsorption characteristics and reaction mechanism of rubber particles in rubber-modified asphalt. Background Art

[0002] Currently, approximately 1.4 billion scrap tires are generated worldwide each year, and the annual production of scrap tires continues to grow at a rate of 6% to 8% year-on-year. The treatment and disposal of scrap tires has become an urgent issue that needs to be addressed. To transform scrap tires into useful materials, a common approach is to grind them into rubber pellets and use them as a modifier for asphalt paving materials. However, the adsorption characteristics and reaction mechanisms of rubber pellets in asphalt are still unclear, which greatly limits their application in asphalt.

[0003] Therefore, it is of great significance to develop a method to evaluate the adsorption characteristics and reaction mechanism of rubber particles in rubber-modified asphalt.

[0004] Summary of the Invention

[0005] The object of the present invention is to provide a method for evaluating the adsorption characteristics and reaction mechanism of rubber particles in rubber-modified asphalt.

[0006] The technical solution adopted by the present invention is:

[0007] A method for evaluating the adsorption characteristics and reaction mechanism of rubber particles in rubber-modified asphalt comprises the following steps:

[0008] 1) Dispersing rubber particles in asphalt to obtain rubber-modified asphalt;

[0009] 2) Separating the rubber particles and the asphalt liquid phase in the rubber-modified asphalt;

[0010] 3) soaking the rubber particles separated in step 2) in tetrahydrofuran multiple times in sequence, and then taking the leachate obtained from each soaking and the asphalt liquid phase separated in step 2) and testing them with gel permeation chromatography and Fourier transform infrared spectroscopy, and then determining the adsorption preference of the rubber particles for the molecular weight of the asphalt based on the gel permeation chromatography and the adsorption preference of the rubber particles for the functional groups in the asphalt based on the Fourier transform infrared spectroscopy;

[0011] 4) performing thermogravimetric analysis on the rubber particles obtained in step 1) and the rubber particles that have been soaked for the final time in step 3), and determining the compositional changes of the rubber particles before and after the reaction with the asphalt based on the thermogravimetric analysis data.

[0012] Preferably, the mass ratio of the rubber particles to asphalt in step 1) is (0.15-0.25):1.

[0013] Preferably, the rubber particles in step 1) are made from waste tires.

[0014] Preferably, the rubber-modified asphalt in step 1) is one of warm mix asphalt and hot mix asphalt.

[0015] Preferably, the specific operation of step 2) is: pouring the rubber-modified asphalt onto a sieve in a sealed container and then allowing the container to stand to separate the rubber particles and the asphalt liquid phase.

[0016] Preferably, the mesh size of the sieve is 70 μm to 80 μm.

[0017] Preferably, the standing is carried out at 160° C. to 170° C., and the standing time is 50 min to 70 min.

[0018] Preferably, in step 3), the ratio of the rubber particles to tetrahydrofuran is 1 g:(5 mL to 10 mL).

[0019] Preferably, the soaking time in step 3) is 3 min to 5 min.

[0020] Preferably, the soaking times in step 3) is 4 to 5 times.

[0021] The beneficial effects of the present invention are as follows: the present invention extracts components in the interaction area between asphalt and rubber particles by a layer-by-layer separation method, and then determines the molecular weight distribution of asphalt adsorbed by rubber particles and the absorption preference for asphalt functional groups through gel permeation chromatography and Fourier transform infrared spectroscopy, and performs thermogravimetric analysis on the original rubber particles and the rubber particles after reaction with asphalt to determine the composition changes of the rubber particles before and after the reaction, thereby knowing the adsorption characteristics of the rubber particles in the rubber-modified asphalt and the mutual reaction mechanism between the rubber particles and the asphalt, which is helpful for optimizing the formula of the rubber-modified asphalt and designing the mixing conditions. BRIEF DESCRIPTION OF THE DRAWINGS

[0022] FIG1 is an operational flow chart of step 3) in the embodiment.

[0023] FIG2 is a gel permeation chromatogram of the asphalt liquid phase and the leachate in the example.

[0024] FIG3 is a Fourier transform infrared spectrum of the asphalt liquid phase and the leachate in the embodiment.

[0025] FIG4A is a TG curve and a DSC curve of the original rubber particles in the embodiment; FIG4B is a TG curve and a DSC curve of the rubber particles soaked in tetrahydrofuran. DETAILED DESCRIPTION

[0026] The present invention will be further explained and illustrated below with reference to specific embodiments.

[0027] Example

[0028] A method for evaluating the adsorption characteristics and reaction mechanism of rubber particles in rubber-modified asphalt comprises the following steps:

[0029] 1) Rubber particles (made from waste tires and able to pass a 40-mesh sieve) and hot-mix asphalt with a penetration grade of 60 / 70 were mixed in a mass ratio of 0.2:1, and then high-speed sheared at 6000 rpm at 176°C for 60 minutes, followed by standing for 30 minutes for swelling development to obtain rubber-modified asphalt;

[0030] 2) Pour the rubber-modified asphalt onto a 200-mesh sieve in a sealed container and allow to stand at 165°C for 60 minutes to separate the rubber particles and the asphalt liquid phase;

[0031] 3) Wrap 12 g of the rubber particles separated in step 2) with a 200-mesh sieve and immerse them sequentially in four beakers containing 60 mL of tetrahydrofuran for 3 minutes each time to obtain leachates (named Cup 1, Cup 2, Cup 3, and Cup 4 in the order of immersion; the operation flow chart is shown in FIG1 );

[0032] 4) The asphalt liquid phase separated in step 2) and the leachate obtained from each immersion in step 3) were subjected to gel permeation chromatography using an Agilent liquid chromatograph 1260 (the asphalt liquid phase was first dissolved in tetrahydrofuran before testing, according to a ratio of 1 mg asphalt liquid phase: 1 mL tetrahydrofuran. Since the leachate was obtained by extraction with tetrahydrofuran, it was directly tested. All samples needed to be filtered through a 0.2 μm filter before injection). Tetrahydrofuran was used as the mobile phase, and PLgel 3 μm Mixed-E and PLgel 5 μm were used. 103 two chromatographic columns, the temperature of the two columns was set to 30℃, the flow rate was set to 1mL / min, and the injection volume was 20μL (only asphalt molecules with a diameter smaller than the pore diameter can enter the gel pore channel, and among the asphalt molecules that enter the channel, the larger asphalt molecules can pass through the gaps between the gel particles and exit the column earlier. Therefore, the order of asphalt molecules exiting the column is from large to small). The concentration of the discharged molecules was recorded as a chromatogram by a refractive index differential detector. The obtained gel permeation chromatogram is shown in Figure 2. As shown in Figure 2, compared with the leachate of cups 1 to 4, the asphalt liquid phase has a higher curve within 10min to 14min, but has a lower peak at 15.7min, indicating that mixing rubber particles with original asphalt will lead to a higher content of large molecules in the asphalt, but the rubber particles do not uniformly absorb the components in the asphalt. On the contrary, during the reaction process between rubber particles and asphalt, there is a certain absorption preference between components of different molecular sizes, and they tend to absorb components with smaller molecular sizes.

[0033] 5) 30 mL of the asphalt liquid phase separated in step 2) and the leachate obtained from each soaking in step 3) were placed in a 70°C water bath until the liquid became solid, and then placed in a vacuum oven at 80°C for 8 h (to completely remove THF and water). The Fourier transform infrared spectrum was then measured using a Bruker VERTEX 70 FTIR spectrometer with a resolution of 4 cm -1 , scan times 16 times, scanning range 4000cm -1 ~400cm -1 , the sample was evenly spread on a potassium bromide (KBr) plate, and then the KBr plate was placed in the sample chamber to start the spectrum scan. At the same time, the Fourier transform infrared spectrum of the asphalt liquid phase was drawn for comparison. The obtained Fourier transform infrared spectrum is shown in Figure 3. It can be seen from Figure 3 that (in the process of the reaction between rubber particles and asphalt, the CH bond is usually relatively stable, so the CH bond is used as the reference peak, and the wavelength range is 840cm -1 ~785cm -1 , the integral area is recorded as Aera 810 ; Using CO bond as the contrast peak, the wavelength range is 1290cm -1 ~1235cm -1 , the integral area is recorded as Aera1270 ): There is a more prominent CO bond peak in the asphalt liquid phase, while the CO bond peaks of the leachates of cups 1 to 4 are very vague, indicating that the polymer containing CO bonds is not completely absorbed into the asphalt-rubber particle interaction area; In addition, Aera 1270 With Aera 810 The ratio first decreases significantly from the asphalt liquid phase to the leachate of cup 1, and then gradually decreases from the leachate of cup 1 to the leachate of cup 4, indicating that the rubber particles are repellent to the absorption of polymers containing CO bonds.

[0034] 6) The rubber particles obtained in step 1) and the rubber particles obtained after the final soaking in step 3) were subjected to thermogravimetric analysis using a Netzch TGA / DSC analyzer. The operating temperature range was 25°C to 1500°C, the heating rate was controlled at 20°C / min, the maximum temperature was 600°C, and a high-purity nitrogen atmosphere was applied at a flow rate of 500 mL / min. 15 mg of sample was used for each test, and the sample was washed with clean water to remove impurities. The TG curve and DSC curve of the original rubber particles are shown in FIG4A ; the TG curve and DSC curve of the tetrahydrofuran-soaked rubber particles are shown in FIG4B . As shown in FIG4A and FIG4B , the TG curve of the original rubber particles shows two main regions of mass degradation at 100°C to 130°C and 300°C to 500°C, while the DSC curve shows three main endotherms and one exotherm. These thermal characteristics are caused by the rubber particles. The results show that the DSC curves at 329°C and 410°C are caused by the changes in the components of the samples, including natural rubber, synthetic rubber, and minor components such as oil and water. The first mass loss and endothermic peak are due to the evaporation of water, followed by the decomposition of oil and other additives in the lower temperature range (<300°C). As the temperature further increases to above 300°C, the two peaks in the DSC curves at 329°C and 410°C are due to the degradation of natural rubber and synthetic rubber, respectively. For the rubber particles soaked in tetrahydrofuran, the main weight loss still occurs at 300°C~500°C. However, the residual mass percentage of the rubber particles soaked in tetrahydrofuran (about 26%) is higher than the final remaining mass percentage of the original rubber particles (17%), indicating that the interaction between the rubber particles and the base asphalt may have consumed some of the decomposable polymers.

[0035] In summary, the present invention extracts the components in the interaction area between asphalt and rubber particles through a layer-by-layer separation method, and then determines the molecular weight distribution of the asphalt adsorbed by the rubber particles and the absorption preference for asphalt functional groups through gel permeation chromatography and Fourier transform infrared spectroscopy. Thermogravimetric analysis is performed on the original rubber particles and the rubber particles after reaction with asphalt to determine the composition changes of the rubber particles before and after the reaction, thereby understanding the adsorption characteristics of the rubber particles in the rubber-modified asphalt and the interaction mechanism between the rubber particles and the asphalt, which is helpful for optimizing the formulation of the rubber-modified asphalt and designing the mixing conditions.

[0036] The above embodiments are preferred implementation modes of the present invention, but the implementation modes of the present invention are not limited to the above embodiments. Any other changes, modifications, substitutions, combinations, and simplifications that do not deviate from the spirit and principles of the present invention should be considered as equivalent replacement methods and are included in the scope of protection of the present invention.

Claims

1. A method for evaluating the adsorption characteristics and reaction mechanism of rubber particles in rubber-modified asphalt, characterized in that: The following steps are involved: 1) dispersing rubber particles in asphalt to obtain rubber modified asphalt; 2) Separating the rubber particles and the asphalt liquid phase in the rubber-modified asphalt; 3) soaking the rubber particles separated in step 2) in tetrahydrofuran for multiple times in sequence, taking the leaching solution obtained from each soaking and the asphalt liquid phase separated in step 2) to test gel permeation chromatography and Fourier transform infrared spectroscopy, and then determining the adsorption preference of the rubber particles for the molecular weight of asphalt according to the gel permeation chromatography and determining the adsorption preference of the rubber particles for the functional groups in the asphalt according to the Fourier transform infrared spectroscopy; 4) taking the rubber particles in step 1) and the rubber particles that have completed the last immersion in step 3) for thermogravimetric analysis, and then determining the composition changes of the rubber particles before and after the reaction with asphalt based on the thermogravimetric analysis data.

2. The method according to claim 1, characterized in that: In step 1), the mass ratio of the rubber particles to the asphalt is (0.15-0.25):

1.

3. The method according to claim 1 or 2, characterized in that: Step 1) The rubber particles are made from waste tires.

4. The method according to claim 1 or 2, characterized in that: In step 1), the rubber modified asphalt is one of warm mix asphalt and hot mix asphalt.

5. The method according to claim 1, characterized in that: The specific operation of step 2) is: pouring the rubber-modified asphalt onto the screen in a closed container and then letting it stand to separate the rubber particles and the asphalt liquid phase.

6. The method according to claim 5, characterized in that: The mesh size of the sieve is 70 μm to 80 μm.

7. The method according to claim 5 or 6, characterized in that: The standing is performed at 160° C. to 170° C., and the standing time is 50 min to 70 min.

8. The method according to claim 1, characterized in that: Step 3) The usage ratio of the rubber particles and tetrahydrofuran is 1g:(5mL-10mL).

9. The method according to claim 1 or 8, characterized in that: The soaking time in step 3) is 3 to 5 minutes.

10. The method according to claim 1 or 8, characterized in that: The soaking times in step 3) is 4 to 5 times.

Citation Information

Patent Citations

  • Method for analysis and differentiation of asphalt by combining infrared chromatography with gel permeation chromatography

    CN104198429A

  • Method for evaluating selective adsorption of rubber powder to asphalt components and molecular groups

    CN112098581A

  • Method for testing selective adsorption of mineral to asphalt component

    CN115436216A

  • Method for evaluating adsorption characteristics and reaction mechanism of rubber particles in rubber modified asphalt

    CN116735522A

  • Methods for analyzing hydrocarbons and hydrocarbon blends for chemical compositions

    US20190091642A1

Cited By

  • Desulfurization degree evaluation method of biological desulfurization rubber powder for modified asphalt

    CN120121557A