High-dispersity ruthenium catalyst for oxidizing hydrogen chloride to prepare chlorine and preparation method therefor
The surfactant disperses the ruthenium active components and combines titanium oxide and alumina support to prepare a high-dispersion ruthenium catalyst, which solves the problem of the decrease in activity of ruthenium-based catalysts at high temperatures, and achieves efficient chlorine-based reaction and cost reduction in hydrogen chloride oxidation. .
Patent Information
- Application Number
- PCT/CN2024/094092
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-05-22
- Filing Date
- 2024-05-18
- Publication Date
- 2024-11-28
AI Technical Summary
The existing ruthenium-based catalysts have decreased activity at high temperatures and have poor high temperature resistance, resulting in a decrease in Deacon reaction efficiency, and the high price of precious metals, which is not conducive to commercial application.
By dispersing the ruthenium active components using a surfactant, combining a composite support of titanium oxide and alumina, a high-dispersion ruthenium catalyst is prepared to improve the dispersion and thermal stability of ruthenium, reduce the metal loading, and enhance catalytic activity.
The catalytic activity of high conversion rate in the low temperature range and long-term use in the high temperature range is achieved, the catalyst cost is reduced, and the efficiency of oxidizing hydrogen chloride to chlorine gas and the service life of the catalyst is improved.
Smart Images

Figure CN2024094092_28112024_PF_FP_ABST
Abstract
Description
A high-dispersion ruthenium catalyst for producing chlorine from hydrogen chloride and its preparation method Technical Field
[0001] The present application relates to the field of catalysts, and in particular to a highly dispersed ruthenium catalyst for producing chlorine by oxidation of hydrogen chloride and a preparation method thereof. Background Art
[0002] Chlorine is an important basic chemical raw material, widely used in industries such as chemistry, metallurgy, papermaking, textiles, petrochemicals, drinking water disinfection, and environmental protection. The industrial production of organochlorine products produces a large amount of by-product hydrogen chloride, with an atomic utilization rate of up to 50%. Most of this hydrogen chloride gas is absorbed with water to make hydrochloric acid, but it contains organic impurities, which limits its use. As people's environmental awareness increases, the requirements for the transportation management and discharge of toxic and highly corrosive substances such as chlorine and hydrogen chloride are becoming increasingly stringent, and the by-product hydrogen chloride is becoming increasingly difficult to handle. Converting hydrogen chloride to produce chlorine gas can achieve closed-loop recycling of chlorine resources and is the most effective method for treating and recovering by-product hydrogen chloride, and has formed a high degree of consensus in the chlorine-related industry.
[0003] Catalytic oxidation is the most effective solution, particularly the Deacon reaction, which has the greatest potential for industrialization due to its simple operation and low equipment costs. In the catalytic oxidation of hydrogen chloride, developed by Deacon in 1868, hydrogen chloride is oxidized to chlorine through an exothermic equilibrium with oxygen. The conversion of hydrogen chloride to chlorine allows for the separation of chlorine production from sodium hydroxide production via chlor-alkali electrolysis. This separation is particularly attractive because global demand for chlorine is higher than that for sodium hydroxide.
[0004] The most important factor in the Deacon reaction is the catalyst. Since the copper-based catalyst (Deacon catalyst), transition metal catalysts such as iron and chromium have been introduced one after another. In recent years, highly active ruthenium-based (Ru), cerium-based (Ce) and composite oxide catalysts have been developed. Copper-based catalysts have attracted much attention due to their low cost. Tsinghua University's Chinese patent application, publication number: CN101125297A, titled "A Kind of Oxychlorination Catalyst and Its Application", uses copper and an oxide inert carrier. However, as the reaction time at high temperature passes, copper particles aggregate and bridges are formed between the particles, causing the catalyst specific surface area to drop significantly, resulting in a decrease in activity, thereby leading to deactivation. Copper-containing hydrogen chloride oxidation catalysts can be loaded with a carrier that is inert to the hydrogen chloride oxidation reaction system. For example, U.S. patent application US4123389A uses silica gel, aluminum oxide or titanium oxide as a carrier, with copper as the main active component. However, the preparation process requires organic solvent impregnation, which is highly environmentally polluting.
[0005] Although chromium catalysts are highly active, they are highly toxic, and their large-scale use has adverse environmental impacts. U.S. Patent No. 5,716,592A reports the use of a composite catalyst of chromium oxide and rare earth cerium. With a loading of 45g, an HCl flow rate of 0.3L / min, and an O2 flow rate of 0.225L / min, the catalytic oxidation of hydrogen chloride at 380°C achieved a maximum hydrogen chloride conversion rate of 85.2%. However, chromium is toxic and readily reacts with chlorine to form low-boiling chromium oxychloride, which can easily deactivate the catalyst.
[0006] Regarding the use of ruthenium catalysts in hydrogen chloride oxidation catalysis, Sumitomo Chemical Co., Ltd.'s Chinese patent applications CN1182717A, CN1150127C, and CN1272238C disclose the preparation of ruthenium-based catalysts by impregnating ruthenium oxide and calcining oxides such as TiO2 and ZrO2 as supports. Furthermore, Bayer Materialscience AG's WO2007 / 134772A1 discloses a ruthenium-based catalyst system containing tin dioxide.
[0007] Although ruthenium-based catalysts offer advantages over other catalysts, such as the ruthenium-based catalyst prepared by loading RuO2 and SiO2 onto TiO2 in CN1182717A, which exhibits superior low-temperature catalytic performance, the exothermic reaction can lead to sintering of the active RuO2 particles due to insufficient heat dissipation. Consequently, this catalyst still suffers from decreased reactivity after prolonged use.
[0008] Sumitomo Chemical's CN1272238C discloses a RuO2 catalyst supported on a composite support of rutile TiO2 and α-alumina, which reduces the reaction temperature of the Deacon process to around 300°C and increases the theoretical equilibrium conversion to 90%-95%. However, in actual use, the conversion rate dropped significantly to below 80% at temperatures above 360°C, particularly above 390°C. Ruthenium-based catalysts have two major advantages over other non-precious metal catalysts: first, they exhibit excellent low-temperature activity at 300-350°C, resulting in high equilibrium HCl conversion; second, the chlorination of their surface active phase is self-limiting, preventing the formation of volatile chlorides due to overchlorination. However, the high price of precious metals reduces the economic benefits of the process. Ruthenium also has poor high-temperature resistance and is susceptible to deactivation at temperatures between 360-390°C, especially above 400°C. Researchers in this field are currently working to improve ruthenium-based catalysts by further enhancing their activity and high-temperature thermal stability, while reducing costs and enabling wider commercialization. Sumitomo Chemical's CN101223104A uses a mixture of rutile titanium dioxide and α-alumina in varying proportions as a support to produce a supported RuO2 catalyst. The catalyst's activity decreases during the hydrogen chloride oxidation process, requiring a gradual increase in reaction temperature to improve hydrogen chloride conversion. High temperatures also accelerate the decrease in activity.
[0009] The Deacon reaction temperature is generally between 280-420℃, which is in a relatively high thermal environment. At the same time, since the reaction is exothermic, the catalyst needs to have not only good thermal conductivity and thermal stability, but also a low specific surface area, such as 10-50m 2 / g. Due to the thermal effect on materials, materials with large specific surface areas can experience a decrease in specific surface area as their crystals grow at high temperatures, leading to changes in their pore structure. This is highly detrimental to catalysts loaded with active components, causing decreased activity and accelerated deactivation.
[0010] The particle size and dispersion of the active components of the catalyst greatly affect the activity of the reaction. The smaller the metal particle size, the higher the dispersion of the metal can be. At the same time, it can have a better bond with the carrier, the grains are not easy to grow, and it has better thermal stability. Usually, when preparing catalysts, high specific surface area materials are selected as carriers, which is conducive to the loading of active metals and high dispersion. Due to the limitations of reaction conditions, the Deacon reaction requires a carrier with good thermal stability. Selecting a material with a smaller specific surface area as a carrier will make it difficult to achieve high dispersion of the active component ruthenium, which not only affects the activity of the catalyst, but also increases the amount of ruthenium used, which is not conducive to cost control.
[0011] Summary of the Invention
[0012] The purpose of the present application is to provide a catalyst for the oxidation of hydrogen chloride to produce chlorine, wherein the active component ruthenium is in a highly dispersed state; and to provide a ruthenium catalyst with a high carrier thermal conductivity; and a method for preparing the catalyst and using the catalyst to catalytically oxidize hydrogen chloride to chlorine by oxygen.
[0013] In one aspect, a method for preparing a highly dispersed ruthenium catalyst for producing chlorine by oxidation of hydrogen chloride in the present application comprises the following steps:
[0014] (1) dispersing the ruthenium-containing active component through a surfactant to prepare an impregnation solution;
[0015] (2) contacting and adhering the impregnation solution to a composite support of titanium oxide and aluminum oxide, drying and then calcining the solution, wherein the calcination temperature is 150-700° C. and the calcination time is 1-24 hours;
[0016] (3) Cooling, washing, and drying.
[0017] There have been relevant studies in this field on the composition of the ruthenium active component loading carrier, the carrier specific surface area, and parameters such as temperature and time during the production and preparation process, but there has been no exploration of the dispersibility of the ruthenium active component, the size of the ruthenium grains, or the pretreatment of the impregnation solution.
[0018] The surfactant is selected from any one or more combinations of hydrophilic nonionic surfactants including, but not limited to, polyoxyethylene nonionic surfactants, polyethylene glycol, and polysorbate. More specifically, the surfactant is selected from any one or more combinations of T-80 (Tween-80), OP-10 (alkylphenol polyoxyethylene ether), and PEG-400 (polyethylene glycol 400); more preferably, T-80 is used as the surfactant. By adding the surfactant, a coating and isolation is formed between the active component ruthenium particles, and the ruthenium component does not seriously agglomerate between the ruthenium particles during the impregnation adsorption or drying stages, so that the precious metal ruthenium (Ru) as the active component is in a highly dispersed state, thereby suppressing the agglomeration caused by the growth of the metal particles due to calcination.
[0019] Preferably, the amount of the surfactant is 1-10 times the mass of the metal element in the ruthenium active component, more preferably 1-5 times.
[0020] The ruthenium active component described in this application is derived from, but not limited to, any one or more combinations of the following components: RuCl3, RuCl3·xH2O, RuBr3, RuBr3·xH2O; chlororuthenates, such as K3RuCl6, (RuCl3) 3- 、K2RuCl6;Chlororuthenate hydrate, such as [RuCl5(H2O)4] 2- 、[RuCl2(H2O)4] +Ruthenates, such as K2RuO4 or Na2RuO4; ruthenium oxychloride, such as Ru2OCl4, Ru2OCl5, Ru2OCl6; ruthenium oxychloride salts, such as K2Ru2OCl 10 、Cs2Ru2OCl4;Ruthenium ammonia complexes, such as [Ru(NH3)6] 2+ 、[Ru(NH3)6] 3+ 、[Ru(NH3)5H2O] 2+ ; Ruthenium chloride amine complexes, such as [Ru(NH3)5Cl] 2+ , [Ru(NH3)6]Cl2, [Ru(NH3)6]Cl3; ruthenium bromide amine complexes, such as [Ru(NH3)6]Br3; ruthenium acetylacetonate; ruthenium carbonyl, such as Ru(CO)5 or Ru(CO) 12 ; organic acid salts of ruthenium, such as [Ru3O(OCOCH3)6(H2O)3]OCOCH3, Ru2(RCOO)4Cl (wherein R is a hydrocarbon group containing 1-3 carbon atoms); ruthenium nitrosyl nitrates, such as K2[RuCl6(NO)], [Ru(NH3)5(NO)]Cl3, [Ru(OH)(NH3)4(NO)](NO3)2, Ru(NO)(NO3)3; ruthenium-phosphorus complexes, etc. Preferably, the ruthenium active component is selected from ruthenium trichloride or a hydrate thereof, ruthenium tribromide or a hydrate thereof. More preferably, the compound is ruthenium trichloride hydrate.
[0021] In the present application, the active precious metal component ruthenium element accounts for 0.1-10wt% of the ruthenium catalyst, more preferably 0.5-5wt%, and most preferably 1-3wt%. A lower content of the active component will result in insufficient catalyst activity, while a higher content will increase the catalyst cost.
[0022] Preferably, the impregnation method in step (2) is any one of equal volume impregnation, excess impregnation, and spray impregnation.
[0023] Preferably, the titanium oxide is preferably rutile titanium dioxide. The aluminum oxide is selected as α-Al2O3 and has a thermal conductivity of not less than 23W / m·℃. By forming a composite carrier with rutile titanium dioxide and α-Al2O3 having a high thermal conductivity, the carrier prepared after molding has high thermal conductivity and more macropores, thereby improving the dissipation of heat generated during the reaction process, preventing the growth of ruthenium active component grains due to excessively high reaction temperature and the formation of agglomerates, and also helping to achieve a high dispersion state of ruthenium active components. Most carriers in the prior art still have a certain degree of reaction inertness, and the specific surface area is not easy to improve, which makes the adsorption of metallic ruthenium more difficult. The composite carrier provided in the present application has significantly improved adsorption of metallic ruthenium under the pretreatment of the above-mentioned surfactant.
[0024] The composite carrier is prepared through a molding process, and its shape includes any one or more combinations of powder, spherical, columnar, special-shaped, and honeycomb.
[0025] The catalyst prepared after carrier impregnation and molding has a 10-50m 2 / g specific surface area, ruthenium grains are 1-10nm, and the surface area of ruthenium metal is 120-410m 2 / (g·Ru), in a highly dispersed state, and the preparation process enhances thermal stability, which is beneficial to prolonging the service life and meeting the requirements of industrial catalysis and production.
[0026] This application improves the preparation process and prepares a catalyst with higher ruthenium dispersion than existing catalysts on a carrier with lower specific surface area. The test results show that the currently industrialized 1.5% Ru content catalyst has a metal ruthenium surface area of about 130-200m 2 / (g·Ru), while the surface area of the catalyst prepared by the present invention with the same content of 1.5% Ru can reach 200-340m 2 / (g·Ru). High dispersion increases the effective utilization of ruthenium atoms, significantly improves catalyst activity, and can achieve higher activity at lower metal loading conditions.
[0027] Preferably, the present application loads the ruthenium active component after the carrier forming process, and the calcination after loading does not cause obvious sintering, which can effectively prevent the growth of metal grains, thereby preparing a highly dispersed catalyst.
[0028] The carrier material selected in the present application has the characteristics of acid and alkali resistance and stable high-temperature performance. The selection of high thermal conductivity materials is conducive to the timely dissipation of reaction heat, and the appropriate specific surface area is conducive to the dispersion of active metals. The ruthenium catalyst provided in the present application is used for the oxidation of hydrogen chloride to prepare chlorine, has good catalytic activity, and also has high catalytic activity at low temperatures. The addition of ruthenium active components through a surfactant to form an impregnation solution is conducive to improving the adsorption of active metals by the carrier and improving the dispersion of metallic ruthenium. At the same time, the migration and agglomeration of ruthenium components can be prevented in subsequent processes such as drying and calcination. High dispersion means that the effective utilization rate of metal atoms is increased, with high activity, while maintaining a high conversion rate, reducing the metal content, which is conducive to reducing the cost of the catalyst.
[0029] On the other hand, the present application provides a ruthenium catalyst, comprising a porous support and a ruthenium active component impregnated in the porous support; the porous support is derived from a mixture of titanium oxide, high thermal conductivity ceramics and additives, and the high thermal conductivity ceramics are selected from any one or more combinations of Si3N4, BN, and SiC.
[0030] The high thermal conductivity ceramics described in this application are required to have good thermal conductivity and suitable specific surface area, including but not limited to any one or more combinations of Si3N4, BN, and SiC. More specifically, it refers to an inorganic ceramic material with a thermal conductivity of not less than 30W / m·℃, because the thermal conductivity of α-Al2O3 is only 23W / m·℃, and the thermal conductivity of other crystal forms of Al2O3 generally does not exceed 23W / m·℃. By improving the thermal conductivity and surface area of the carrier component, the conversion rate of the carrier in a high-temperature environment will be significantly improved. More preferably, the high thermal conductivity ceramics are selected from materials such as β-SiC, β-Si3N4, hexagonal BN, etc. that may have a high thermal conductivity greater than 50W / m·℃. Among them, β-SiC has a thermal conductivity of 146-270w / m·℃ and a specific surface area of 20m 2 / g or more specific surface area, β-Si3N4 has a thermal conductivity of 30-155w / m·℃ and a thermal conductivity of 40m 2 / g or more specific surface area, hexagonal BN has a thermal conductivity of more than 79.54w / m·℃ and a thermal conductivity of 50m 2 / g or more specific surface area.
[0031] In addition, the titanium oxide is preferably rutile titanium dioxide or titanium dioxide containing rutile. By compounding rutile titanium dioxide with a high thermal conductivity material, the carrier prepared after molding has high thermal conductivity and a large number of macropores, thereby improving the dissipation of heat generated during the reaction, preventing the growth of ruthenium active component grains and the formation of agglomerates due to excessively high reaction temperatures, and thus extending the service life of the catalyst.
[0032] The ruthenium active component described in this application is derived from, but not limited to, any one or more combinations of the following components: RuCl3, RuCl3·xH2O, RuBr3, RuBr3·xH2O; chlororuthenates, such as K3RuCl6, (RuCl3) 3- 、K2RuCl6;Chlororuthenate hydrate, such as [RuCl5(H2O)4] 2- 、[RuCl2(H2O)4] + Ruthenates, such as K2RuO4 or Na2RuO4; ruthenium oxychloride, such as Ru2OCl4, Ru2OCl5, Ru2OCl6; ruthenium oxychloride salts, such as K2Ru2OCl 10 、Cs2Ru2OCl4;Ruthenium ammonia complexes, such as [Ru(NH3)6] 2+ 、[Ru(NH3)6] 3+ 、[Ru(NH3)5H2O] 2+ ; Ruthenium chloride amine complexes, such as [Ru(NH3)5Cl] 2+, [Ru(NH3)6]Cl2, [Ru(NH3)6]Cl3; ruthenium bromide amine complexes, such as [Ru(NH3)6]Br3; ruthenium acetylacetonate; ruthenium carbonyl, such as Ru(CO)5 or Ru(CO) 12 ; organic acid salts of ruthenium, such as [Ru3O(OCOCH3)6(H2O)3]OCOCH3 and Ru2(RCOO)4Cl (wherein R is a hydrocarbon group containing 1-3 carbon atoms); ruthenium-nitrosyl complexes, such as K2[RuCl6(NO)], [Ru(NH3)5(NO)]Cl3, [Ru(OH)(NH3)4(NO)](NO3)2, and Ru(NO)(NO3)3; and ruthenium-phosphorus complexes. Preferably, the ruthenium active component is selected from ruthenium trichloride or a hydrate thereof, or ruthenium tribromide or a hydrate thereof. More preferably, the compound is ruthenium trichloride hydrate.
[0033] In the present application, the active precious metal component ruthenium element accounts for 0.1-10wt% of the ruthenium catalyst, preferably 0.5-5wt%, more preferably 1-3%. A lower content of the active component will lead to insufficient catalyst activity, while a higher content will increase the catalyst cost.
[0034] In order to obtain the ruthenium catalyst, the present application provides a corresponding preparation method, which specifically includes the following steps:
[0035] (1) mixing titanium oxide, a high thermal conductivity material, and an additive to obtain a mixed powder;
[0036] (2) the mixed powder is mixed with water, formed, dried, and calcined for the first time to obtain a high-strength carrier;
[0037] (3) preparing a ruthenium active component precursor solution into an impregnation solution;
[0038] (4) impregnating the impregnation solution onto a high-strength carrier, drying, and calcining for the second time to obtain the ruthenium catalyst;
[0039] The high thermal conductivity material is selected from any one or more combinations of Si3N4, BN, and SiC. More preferably, the high thermal conductivity ceramic is selected from materials with a high thermal conductivity greater than 50 W / m·°C, such as β-SiC, β-Si3N4, and hexagonal BN.
[0040] This application uses an impregnation solution made from a ruthenium active component precursor to load it onto a high-strength carrier. The acid resistance, alkali resistance, and high thermal stability of the carrier must be considered, and selecting a suitable specific surface area is conducive to the dispersion of the active metal.
[0041] The shape of the carrier is selected from, but not limited to, spherical, cylindrical, honeycomb, special-shaped structures, and the like.
[0042] A suitable molding process will provide a larger specific surface area for reaction. The molding method comprises subjecting a powder carrier to a molding process to obtain solid particles, and then subjecting the powder carrier to a drying and calcining process to obtain the molded carrier. The molding process is selected from, but not limited to, tableting, ball rolling, extrusion, spray molding, and oil column molding. Extrusion, tableting, and ball rolling molding processes are preferred, and extrusion molding is more preferred. As a preferred extrusion molding process, the high-strength carrier particles formed by extrusion are 1-3 mm in diameter and 2-7 mm in length.
[0043] Preferably, the additive in step (1) accounts for 1-10 wt% of the total weight of the mixed powder, and the titanium oxide in step (2) accounts for 20-80% of the total weight of the carrier after calcination. More preferably, the titanium oxide accounts for 30-60% of the total weight of the carrier, and the additive accounts for 1-10 wt% of the total weight of the mixed powder. The titanium oxide is preferably rutile titanium dioxide.
[0044] Preferably, the auxiliary agent is selected from any one or more combinations of polyvinyl alcohol, cellulose, starch, sesbania powder, and synthetic resin, with cellulose or sesbania powder being preferred. The cellulose is selected from any one or more combinations including, but not limited to, methyl cellulose, hydroxyethyl cellulose, and hydroxypropyl methyl cellulose. The auxiliary agent is an organic binder that helps improve the molding effect of the mixed powder during the molding process and forms pores after drying and calcining, thereby increasing the specific surface area.
[0045] Preferably, the amount of water added in step (2) is 20-50% of the mass of the mixed powder. The drying in step (2) is carried out at 60-120° C. for 3-24 hours.
[0046] Those skilled in the art can make adaptive adjustments based on the desired pore morphology and specific surface area of the selected additives and carriers, all of which are within the scope of protection of this application.
[0047] The first calcination is to obtain a high-strength carrier for loading the ruthenium active component, mainly to optimize the porous morphology and physical properties of the carrier, while the second calcination is after step (3), and the thermal stability of the ruthenium active component must be considered. To this end, the first calcination is calcined at 300-800°C for 1-24 hours, preferably calcined at 400-700°C for 3-6 hours. The second calcination is calcined at 200-700°C for 1-24 hours, preferably calcined at 250-600°C for 2-6 hours, and then naturally cooled to room temperature.
[0048] After step (4), the ash can be removed by further washing with water, and then dried at 60-120° C. to obtain the ruthenium catalyst product.
[0049] The ruthenium catalyst of this application should have a suitable specific surface area to maintain catalytic activity and stability. Too high a specific surface area will lead to insufficient stability. For this purpose, the specific surface area of the carrier in step (2) is controlled to be 10-50m 2 / g, this will cause the carrier to be comparatively difficult to absorb active component, especially metallic ruthenium, so that metal Ru is difficult to be evenly distributed on the carrier, causing dispersity to be lower. For this reason, also comprise surfactant in the described impregnation fluid, described surfactant is selected from and includes but not limited to any one in T-80 (Tween-80), OP-10 (alkylphenol polyoxyethylene ether), PEG-400 (Polyethylene Glycol 400). The consumption of described surfactant is 1-10 times, preferably 1-5 times, of the metallic element quality in the ruthenium active component. By surfactant, impregnation fluid is processed, can prevent the migration and reunion of ruthenium component in oven dry, calcining process, generate thinner ruthenium grains, be more conducive to improving the dispersity of ruthenium.
[0050] The ruthenium catalyst obtained after drying and calcining twice has a 10-50m 2 / g of specific surface area, pore size of 0.01-6um, strength of 120-200N / cm when the diameter is 1.5-3mm, and thermal conductivity of 0.6-2.0W / m·℃ at 350℃ based on the hot wire method.
[0051] The ruthenium catalyst provided in this application has high low-temperature activity. The industrial production of chlorine from hydrogen chloride requires a catalytic temperature between 300-420°C, with a conversion rate of 50-80% being essentially guaranteed at low temperatures of 300-330°C and a conversion rate of no less than 90% at high temperatures of 360-420°C. The ruthenium catalyst provided in this application can achieve a conversion rate of no less than 90% in this low-temperature range.
[0052] The catalyst of the present application does not need to be activated before use. The catalyst use conditions are: reaction pressure 0.1-0.5Mpa; reaction temperature 200-500°C, preferably 300-400°C; hydrogen chloride space velocity 1-5m 3 / kg-cat·h, with an oxygen to hydrogen chloride molar ratio of 1:(4-1). The resulting gas stream was passed through an aqueous potassium iodide solution, and samples were taken for measurement by iodine titration and neutralization titration to determine the amount of chlorine generated and the amount of unreacted hydrogen chloride, from which the conversion rate was calculated. BRIEF DESCRIPTION OF THE DRAWINGS
[0053] FIG1 is a TEM image of the ruthenium catalyst of Example 1-1.
[0054] FIG2 shows the particle size distribution of the ruthenium catalyst of Example 1-1.
[0055] FIG3 is a TEM image of the ruthenium catalyst of the control group 1-1.
[0056] FIG4 shows the particle size distribution of the ruthenium catalyst of the control group 1-1. DETAILED DESCRIPTION
[0057] The present application is described in detail below based on examples. It should be noted that the embodiments described below are illustrative for experienced people and are intended to be used to explain the present application, but the present application is not limited to these examples. Unless otherwise specified, all percentage units should be understood to be mass percentages.
[0058] The surface area test method of ruthenium metal adopts CO pulse adsorption method for testing: the specific operation is to use Micrometric Chemisorb type chemical adsorption instrument to perform CO pulse on the catalyst sample and adsorption characterization analysis. 50mg of sample is filled into a U-shaped quartz tube, and a certain amount of quartz wool is padded at the bottom; Ar gas containing H2 is introduced, and the temperature is raised to 350℃ at a rate of 5℃ / min, and pretreated at this temperature and atmosphere for 3h. Cool down to room temperature, and after the baseline is stable, adsorb with Ar pulse containing CO until CO is saturated. After obtaining the CO adsorption amount, the ruthenium metal surface area can be obtained by calculation based on the atomic ratio of Ru / CO=1:1. The ruthenium metal surface area in the embodiment is converted into the surface area per gram of metal ruthenium, and the unit is m 2 The ruthenium metal surface area test methods in all examples were carried out under the same conditions.
[0059] Thermal Conductivity Determination: There are different methods for determining thermal conductivity, and different test methods may yield different results. This is related to factors such as the particle size of the test material, loading speed, and loading method. Even with the same test protocol, different particle sizes of the same material can produce different results. To highlight the high thermal conductivity of the catalysts described herein and their comparability with the control group, the following examples and control groups were tested under the same conditions.
[0060] The thermal conductivity of catalysts is tested using the hot wire method, which assumes that there is an ideal infinitely thin and infinitely long linear heat source in the material. The temperature rise of the hot wire over time is a function of the heating power and the thermal conductivity of the material being tested. The temperature rise of the hot wire in the material being tested is measured using a thermocouple. The thermal conductivity of the test sample is calculated as follows:
[0061] Where k is the thermal conductivity of the material being tested; d(Inτ) / dθ is the logarithm of the time-temperature change rate; and Q is the heat flow rate transferred from the hot wire to the test sample. As the formula shows, knowing the heat flow rate Q transferred from the hot wire to the test sample and the rate of change of temperature at the selected point over time allows us to calculate the thermal conductivity of the test sample.
[0062] Example 1-1
[0063] Weigh 50 g of a strip composite carrier composed of rutile titanium dioxide and α-alumina (titanium dioxide accounts for 50%) with a diameter of 3 mm and a length of 5 mm, a strength of 120 N / cm, and a specific surface area of 30 m 2 / g.
[0064] A ruthenium chloride solution containing 0.75 g of Ru was added with 1.5 g of Tween-80 to prepare 25 ml for impregnation, and dried at 60° C. for 12 hours to obtain a dried catalyst.
[0065] The dried catalyst was dry-calcined in air at 200°C for 5 hours, washed with water, and dried at 80°C to obtain the catalyst product.
[0066] Theoretical calculations show that the catalyst component mass percentage is 1.5% Ru / (TiO2:Al2O3=50:50), and the surface area of ruthenium metal is 306.7m 2 / (g·Ru).
[0067] As shown in Figure 1, the metal particle size was observed using a transmission electron microscope (TEM). As shown in Figure 2, the average particle size of the ruthenium active component of the catalyst prepared by this method is about 1.21 nm.
[0068] Example 1-2
[0069] Weigh 50 g of a strip composite carrier composed of rutile titanium dioxide and α-alumina (titanium dioxide accounts for 30%) with a diameter of 3 mm and a length of 5 mm, a strength of 130 N / cm, and a specific surface area of 25 m 2 / g.
[0070] A ruthenium nitrosyl nitrate solution containing 0.5 g of Ru was added to 0.5 g of Tween-80 to make 25 ml for impregnation, and dried at 80° C. for 6 hours to obtain a dried catalyst;
[0071] The dried catalyst was dry-calcined in air at 250°C for 4 hours; the product was washed with water and dried at 90°C to obtain the catalyst product.
[0072] Theoretical calculations show that the catalyst component mass percentage is 1.0% Ru / (TiO2:Al2O3=30:70), and the surface area of ruthenium metal is 281.0m 2 / (g·Ru).
[0073] Examples 1-3
[0074] Weigh 50 g of a strip composite carrier composed of rutile titanium dioxide and α-alumina (titanium dioxide accounts for 70%) with a diameter of 3 mm and a length of 5 mm, a strength of 138 N / cm, and a specific surface area of 30 m 2 / g.
[0075] 3.8 g of OP-10 was added to a ruthenium chloride solution containing 1.5 g of Ru to prepare 25 ml for impregnation, and then dried at 80°C for 10 hours to obtain a dried catalyst.
[0076] The dried catalyst was dry-calcined in air at 350°C for 3 hours; the product was washed with water and dried at 100°C to obtain the catalyst product.
[0077] Theoretical calculations show that the catalyst component mass percentage is 3.0% Ru / (TiO2:Al2O3=70:30), and the surface area of ruthenium metal is 260.0m 2 / (g·Ru).
[0078] Examples 1-4
[0079] Weigh 50g of a strip composite carrier composed of rutile titanium dioxide and α-alumina (titanium oxide accounts for 34%) with a diameter of 3mm and a length of 5mm, a strength of 142N / cm, and a specific surface area of 50m 2 / g.
[0080] A ruthenium chloride solution containing 1.0 g of Ru was added with 2.0 g of Tween-80 to prepare 30 ml for impregnation, and then dried at 80° C. for 10 hours to obtain a dried catalyst.
[0081] The dried catalyst was dry-calcined in air at 350°C for 3 hours; the product was washed with water and dried at 110°C to obtain the catalyst product.
[0082] Theoretical calculations show that the mass percentage of the catalyst components is 2.0% Ru / (TiO2:Al2O3=34:66), and the surface area of ruthenium metal is 325.0 m 2 / (g·Ru).
[0083] Examples 1-5
[0084] Weigh 50 g of a strip composite carrier composed of rutile titanium dioxide and α-alumina (titanium dioxide accounts for 34%) with a diameter of 3 mm and a length of 5 mm, a strength of 130 N / cm, and a specific surface area of 29 m 2 / g.
[0085] 50 g of the calcined support was impregnated with 30 ml of a ruthenium nitrate solution containing 0.75 g of Ru and 4.0 g of PEG-400, and dried at 100° C. for 7 hours to obtain a dried catalyst.
[0086] The dried catalyst was dry-calcined in air at 400°C for 3 hours; the product was washed with water and dried at 120°C to obtain the catalyst product.
[0087] Theoretical calculations show that the catalyst component mass percentage is 1.5% Ru / (TiO2:Al2O3=34:66), and the surface area of ruthenium metal is 326.7m 2 / (g·Ru).
[0088] Examples 1-6
[0089] Weigh 50 g of a strip composite carrier composed of rutile titanium dioxide and α-alumina (titanium dioxide accounts for 80%) with a diameter of 3 mm and a length of 5 mm, a strength of 150 N / cm, and a specific surface area of 18 m 2 / g.
[0090] 50 g of the calcined support was impregnated with 30 ml of a ruthenium nitrate solution containing 0.4 g of Ru and 5.0 g of PEG-400, and dried at 110° C. for 6 hours to obtain a dried catalyst.
[0091] The dried catalyst was dry-calcined in air at 500°C for 3 hours; the product was washed with water and dried at 120°C to obtain the catalyst product.
[0092] Theoretical calculations show that the catalyst component mass percentage is 0.8% Ru / (TiO2:Al2O3=80:20), and the surface area of ruthenium metal is 297.5m 2 / (g·Ru).
[0093] Examples 1-7
[0094] Weigh 50 g of a strip composite carrier composed of rutile titanium dioxide and α-alumina (titanium dioxide accounts for 50%) with a diameter of 3 mm and a length of 5 mm, a strength of 150 N / cm, and a specific surface area of 18 m 2 / g.
[0095] 50 g of the calcined carrier was impregnated with 30 ml of a potassium oxyruthenate solution containing 0.5 g of Ru and 2.0 g of Tween-80, and dried at 110° C. for 6 hours to obtain a dried catalyst.
[0096] The dried catalyst was dry-calcined in air at 400°C for 3 hours; the product was washed with water and dried at 120°C to obtain the catalyst product.
[0097] Theoretical calculations show that the catalyst component mass percentage is 1.0% Ru / (TiO2:Al2O3=50:50), and the surface area of ruthenium metal is 300.0m 2 / (g·Ru).
[0098] Examples 1-8
[0099] Weigh 50 g of a strip composite carrier composed of rutile titanium dioxide and α-alumina (titanium dioxide accounts for 34%) with a diameter of 3 mm and a length of 5 mm, a strength of 150 N / cm, and a specific surface area of 29 m 2 / g.
[0100] 50 g of the calcined carrier was impregnated with 30 ml of a potassium chlororuthenate solution containing 0.75 g of Ru and 3.0 g of Tween-80, and dried at 110° C. for 6 hours to obtain a dried catalyst.
[0101] The dried catalyst was dry-calcined in air at 450°C for 3 hours; the product was washed with water and dried at 120°C to obtain the catalyst product.
[0102] Theoretical calculations show that the catalyst component mass percentage is 1.5% Ru / (TiO2:Al2O3=34:66), and the surface area of ruthenium metal is 286.7m 2 / (g·Ru).
[0103] Examples 1-9
[0104] Weigh 50 g of a strip composite carrier composed of rutile titanium dioxide and α-alumina (titanium dioxide accounts for 34%) with a diameter of 3 mm and a length of 5 mm, a strength of 150 N / cm, and a specific surface area of 29 m 2 / g.
[0105] 50 g of the calcined carrier was impregnated with 30 ml of a ruthenium-ammine complex solution containing 1.0 g of Ru and 3.0 g of OP-10, and dried at 110° C. for 6 hours to obtain a dried catalyst.
[0106] The dried catalyst was dry-calcined in air at 350°C for 3 hours; the product was washed with water and dried at 120°C to obtain the catalyst product.
[0107] Theoretical calculations show that the catalyst component mass percentage is 2% Ru / (TiO2:Al2O3=50:50), and the surface area of ruthenium metal is 305.0 m 2 / (g·Ru).
[0108] Examples 1-10
[0109] Weigh 50g of a strip composite carrier composed of rutile titanium dioxide and α-alumina (titanium oxide accounts for 34%) with a diameter of 3mm and a length of 5mm, a strength of 150N / cm, and a specific surface area of 27m 2 / g.
[0110] 50 g of the calcined carrier was impregnated with 30 ml of a ruthenium-ammine complex solution containing 0.5 g of Ru and 1.5 g of OP-10, and dried at 110° C. for 6 hours to obtain a dried catalyst.
[0111] The dried catalyst was dry-calcined in air at 300°C for 3 hours; the product was washed with water and dried at 120°C to obtain the catalyst product.
[0112] Theoretical calculations show that the catalyst component mass percentage is 1% Ru / (TiO2:Al2O3=50:50), and the surface area of ruthenium metal is 410.0 m 2 / (g·Ru).
[0113] Control group 1-1
[0114] A ruthenium catalyst was prepared according to the preparation method disclosed in Example 4 of Chinese invention patent CN1245773A, as control group 1. The specific steps are as follows: 3.23 grams of commercially available ruthenium oxide hydrate (RuCl3·nH2O, Ru content 37.3%) was dissolved in 21.9 grams of pure water and stirred to obtain a ruthenium chloride aqueous solution. The resulting aqueous solution was added dropwise to 40.0 grams of a titanium oxide support to impregnate the ruthenium chloride. The supported material was dried in air at 60°C for 2 hours to obtain titanium oxide-supported ruthenium chloride. Then, the obtained solid was heated from room temperature to 350°C in air over approximately 1 hour and calcined at this temperature for 3 hours to obtain a spherical solid. 0.5 L of pure water was added to the obtained solid, stirred, allowed to stand for 30 minutes, and washed by filtration. This operation was repeated 10 times. The washing time was approximately 7 hours. The washed material was dried in air at 60°C for 4 hours to obtain 41.1 grams of gray-black supported ruthenium oxide catalyst.
[0115] The calculated value of the ruthenium content of the control group 1-1 is 2.9% Ru / TiO2, and the measured value of the ruthenium metal surface area is 162.0m 2 / (g·Ru). The metal particle size was observed using a transmission electron microscope (TEM), as shown in Figure 3. Figure 4 shows that the average particle size of the ruthenium catalyst prepared by this technology is 2.09nm.
[0116] Control group 1-2
[0117] A ruthenium catalyst was prepared according to the preparation method disclosed in Example 18 of Chinese invention patent CN1245773A, as control group 2, with the following specific steps: 2.03 grams of commercially available ruthenium oxide hydrate (RuCl3·nH2O, Ru content 37.3%) was dissolved in 14.6 g of pure water and stirred to obtain an aqueous solution of ruthenium chloride. The resulting aqueous solution was added dropwise to 50.0 grams of a strip-shaped composite carrier composed of titanium oxide-α-alumina (titanium oxide accounts for 50%) to impregnate ruthenium chloride. The supported material was dried at 60°C in air for 2 hours to obtain titanium oxide-α-alumina supported ruthenium chloride. Then, the obtained solid was heated from room temperature to 350°C in air for about 1 hour, and calcined at this temperature for 3 hours to obtain a spherical solid. 0.5 L of pure water was added to the obtained solid, stirred, and allowed to stand for 30 minutes and washed by filtration. This operation was repeated 5 times. The washing time was about 4 hours. The washed material was dried in air at 60°C for 4 hours to obtain 50.0 g of a gray-black supported ruthenium oxide catalyst. The calculated value of the ruthenium metal content in the control group 1-2 was 1.5% Ru / (TiO2:Al2O3=50:50), and the measured value of the ruthenium metal surface area was 166.7 m 2 / (g·Ru).
[0118] Test Example 1-1
[0119] The catalyst activities of all examples and controls were tested in a fixed-bed catalytic reactor. The reactor type was a quartz tubular reactor with an inner diameter of 25 mm. The catalyst was granular and the dosage was 10 g. The main reaction conditions were: HCl was passed through the catalyst bed at a rate of 0.76 L / min and O2 at a rate of 0.64 L / min. The conversion rates at different temperatures are shown in Tables 1 and 2. Examples 1-1 to 1-10 were tested under the same conditions as Controls 1-1 and 1-2.
[0120] Table 1. Dispersion of different catalysts and hydrogen chloride conversion at different temperatures
[0121] Table 2. Hydrogen chloride conversion after 500 h of operation of different catalysts
[0122] As can be seen from Tables 1 and 2, the overall activity of the catalyst prepared in the present application in catalyzing the oxidation of hydrogen chloride to produce chlorine is significantly better than that of the control catalyst, especially the dispersion of the active components is much greater than that of the control group, indicating that the active components of the catalyst prepared in the present application have high dispersion, thus showing better activity. At the same time, the low metal loading is of great significance to cost reduction.
[0123] Example 2-1
[0124] Take 30 grams of rutile titanium dioxide, 70 grams of β-phase silicon carbide, and 2.0 grams of sesbania powder and knead them evenly. Add 30 grams of water and knead for 40 minutes. Extrude to form a 3 mm diameter strip. Dry in air at 60°C for 12 hours to obtain a dried strip carrier. Cut the carrier into approximately 5 mm lengths.
[0125] The dried carrier was dry-calcined in air at 400° C. for 6 hours to obtain a calcined strip-shaped carrier.
[0126] 50 g of the calcined carrier was impregnated with 25 ml of a RuCl3·3H2O solution containing 0.15 g of Ru and 0.15 g of Tween-80, and dried at 60°C for 12 hours to obtain a dried catalyst.
[0127] The dried catalyst was dry-calcined in air at 250°C for 6 hours, the product was washed with water, and dried at 80°C to obtain the catalyst product.
[0128] Theoretical calculations show that the mass percentage of the catalyst components is:
[0129] [RuO2 / (RuO2+TiO2+SiC)]*100=0.39%
[0130] The mass percentage of metallic ruthenium is:
[0131] [Ru / (RuO2+TiO2+SiC)]*100=0.3%
[0132] The final catalyst strength is 120N / cm and the specific surface area is 30m 2 / g, average pore size 0.02um, thermal conductivity tested at 350℃ is 1.60W / m·℃.
[0133] Example 2-2
[0134] Take 45 grams of rutile titanium dioxide, 55 grams of β-phase silicon carbide, and 5.0 grams of sesbania powder and knead them evenly. Add 25 grams of water and knead for 40 minutes. Extrude to form a 3 mm diameter strip. Dry in air at 60°C for 12 hours to obtain a dried strip carrier. Cut the carrier into approximately 5 mm lengths.
[0135] The dried carrier was dry-calcined in air at 500° C. for 4 hours to obtain a calcined strip-shaped carrier.
[0136] Take 50 g of the calcined carrier and impregnate it with 25 ml of RuCl3·3H2O solution containing 0.25 g of Ru and add 0.5 g of Tween-80, and dry it at 80°C for 6 hours to obtain a dried catalyst.
[0137] The dried catalyst was dry-calcined in air at 280°C for 5 hours; the product was washed with water and dried at 90°C to obtain the catalyst product.
[0138] Theoretical calculations show that the mass percentage of the catalyst components is:
[0139] [RuO2 / (RuO2+TiO2+SiC)]*100=0.65%
[0140] The mass percentage of metallic ruthenium is:
[0141] [Ru / (RuO2+TiO2+SiC)]*100=0.5%
[0142] The final catalyst strength was 130N / cm and the specific surface area was 25m 2 / g, average pore size 0.04um, and thermal conductivity tested at 350℃ is 1.21W / m·℃.
[0143] Example 2-3
[0144] 33 g of rutile titanium dioxide, 67 g of β-phase silicon nitride, and 5.0 g of hydroxyethyl cellulose were mixed uniformly; 28 g of water was added to the mixture, and the mixture was kneaded for 40 min. The mixture was extruded to obtain a 3 mm diameter strip, which was then dried in air at 90°C for 8 hours to obtain a dried strip carrier, which was cut into 5 mm lengths.
[0145] The dried carrier was dry-calcined in air at 550° C. for 4 hours to obtain a calcined strip-shaped carrier.
[0146] 50 g of the calcined carrier was impregnated with 25 ml of a RuCl3·3H2O solution containing 0.76 g of Ru and added with 2.0 g of OP-10, and dried at 80°C for 10 hours to obtain a dried catalyst.
[0147] The dried catalyst was dry-calcined in air at 300°C for 4 hours; the product was washed with water and dried at 100°C to obtain the catalyst product.
[0148] Theoretical calculations show that the mass percentage of the catalyst components is:
[0149] [RuO2 / (RuO2+TiO2+Si3N4)]*100=1.97%
[0150] The mass percentage of metallic ruthenium is:
[0151] [Ru / (RuO2+TiO2+Si3N4)]*100=1.5%
[0152] The final catalyst strength was 138 N / cm and the specific surface area was 28 m 2 / g, average pore size 0.06um, and thermal conductivity tested at 350℃ is 1.48W / m·℃.
[0153] Examples 2-4
[0154] 45 g of rutile titanium dioxide, 55 g of β-phase silicon nitride, and 4.0 g of methyl cellulose were mixed uniformly; 35 g of water was added to the mixture, and the mixture was kneaded for 40 min. The mixture was extruded to obtain a 3 mm diameter strip, which was then dried in air at 100°C for 5 hours to obtain a dried strip carrier, which was cut into 5 mm lengths.
[0155] The dried carrier was dry-calcined in air at 650° C. for 4 hours to obtain a calcined strip-shaped carrier.
[0156] 50 g of the calcined carrier was impregnated with 30 ml of a RuCl3·3H2O solution containing 1.56 g of Ru and 6.0 g of Tween-80, and dried at 80°C for 10 hours to obtain a dried catalyst.
[0157] The dried catalyst was dry-calcined in air at 400°C for 2 hours; the product was washed with water and dried at 110°C to obtain the catalyst product.
[0158] Theoretical calculations show that the mass percentage of the catalyst components is:
[0159] [RuO2 / (RuO2+TiO2+Si3N4)]*100=3.95%
[0160] The mass percentage of metallic ruthenium is:
[0161] [Ru / (RuO2+TiO2+Si3N4)]*100=3.0%
[0162] The final catalyst strength was 142N / cm and the specific surface area was 50m 2 / g, average pore size 0.1um, and thermal conductivity tested at 350℃ is 1.32W / m·℃.
[0163] Examples 2-5
[0164] 40 g of rutile titanium dioxide, 60 g of hexagonal boron nitride, and 4.0 g of hydroxypropyl methylcellulose were mixed uniformly; 28 g of water was added to the mixture, and the mixture was kneaded for 40 min. The mixture was extruded to obtain a 3 mm diameter strip, which was then dried in air at 120°C for 5 hours to obtain a dried strip carrier, which was cut into 5 mm lengths.
[0165] The dried carrier was dry-calcined in air at 700° C. for 4 hours to obtain a calcined strip-shaped carrier.
[0166] 50 g of the calcined support was impregnated with 30 ml of a ruthenium nitrosyl nitrate solution containing 2.11 g of Ru and 4.0 g of PEG-400, and dried at 100° C. for 7 hours to obtain a dried catalyst.
[0167] The dried catalyst was dry-calcined in air at 350°C for 4 hours to obtain the catalyst product.
[0168] Theoretical calculations show that the mass percentage of the catalyst components is:
[0169] [RuO2 / (RuO2+TiO2+BN)]*100=5.2%
[0170] The mass percentage of metallic ruthenium is:
[0171] [Ru / (RuO2+TiO2+BN)]*100=4.0%
[0172] The final catalyst strength was 118 N / cm and the specific surface area was 26 m 2 / g, average pore size 0.07um, thermal conductivity tested at 350℃ is 1.29W / m·℃.
[0173] Examples 2-6
[0174] Take 50 grams of rutile titanium dioxide, 50 grams of hexagonal boron nitride, and 4.0 grams of polyvinyl alcohol and mix them evenly; add 29 grams of water to the mixture and knead for 40 minutes. Extrusion molding gives a 3 mm diameter strip, which is then dried in air at 110°C for 5 hours to obtain a dried strip carrier, which is cut into 5 mm lengths.
[0175] The dried carrier was dry-calcined in air at 750° C. for 4 hours to obtain a calcined strip-shaped carrier.
[0176] 50 g of the calcined support was impregnated with 30 ml of a ruthenium nitrate solution containing 1.56 g of Ru and 7.5 g of PEG-400, and dried at 110° C. for 6 hours to obtain a dried catalyst.
[0177] The dried catalyst was dry-calcined in air at 500°C for 2 hours to obtain the catalyst product.
[0178] Theoretical calculations show that the mass percentage of the catalyst components is:
[0179] [RuO2 / (RuO2+TiO2+BN)]*100=3.95%
[0180] The mass percentage of metallic ruthenium is:
[0181] [Ru / (RuO2+TiO2+BN)]*100=3.0%
[0182] The final catalyst strength was 150N / cm and the specific surface area was 22m 2 / g, average pore size 3um, and thermal conductivity tested at 350℃ is 1.20W / m·℃.
[0183] Examples 2-7
[0184] 60 g of rutile titanium dioxide, 40 g of β-phase silicon nitride, and 5.0 g of starch were mixed uniformly; 25 g of water was added to the mixture, and the mixture was kneaded for 40 min. The mixture was extruded to obtain a 3 mm diameter strip, which was then dried in air at 110°C for 5 hours to obtain a dried strip carrier, which was cut into 5 mm lengths.
[0185] The dried carrier was dry-baked in air at 800℃ for 3 hours to obtain a strip carrier with a strength of 200N / cm and a specific surface area of 34m 2 / g, average pore size 6um.
[0186] Take 50 g of the calcined carrier and impregnate it with 30 ml of K2RuCl6 solution containing 0.51 g of Ru and adding 2.5 g of Tween-80, and dry it at 110°C for 6 hours to obtain a dried catalyst.
[0187] The dried catalyst was dry-calcined in air at 550°C for 5 hours; the product was washed with water and dried at 120°C to obtain the catalyst product.
[0188] Theoretical calculations show that the mass percentage of the catalyst components is:
[0189] [RuO2 / (RuO2+TiO2+Si3N4)]*100=1.3%
[0190] The mass percentage of metallic ruthenium is:
[0191] [Ru / (RuO2+TiO2+Si3N4)]*100=1.0%
[0192] The final catalyst strength was 200 N / cm and the specific surface area was 18 m 2 / g, average pore size 6um, and thermal conductivity tested at 350℃ is 1.22W / m·℃.
[0193] Examples 2-8
[0194] 50 g of rutile titanium dioxide, 50 g of hexagonal boron nitride, and 3.0 g of hydroxyethyl cellulose were mixed uniformly; 25 g of water was added to the mixture, and the mixture was kneaded for 40 min. The mixture was extruded to obtain a 3 mm diameter strip, which was then dried in air at 110°C for 5 hours to obtain a dried strip carrier, which was cut into 5 mm lengths.
[0195] The dried carrier was dry-calcined in air at 600° C. for 4 hours to obtain a calcined strip-shaped carrier.
[0196] 50 g of the calcined carrier was impregnated with 30 ml of a [Ru(NH3)6]Cl2 solution containing 0.25 g of Ru and 0.5 g of PEG-400, and dried at 110°C for 6 hours to obtain a dried catalyst.
[0197] The dried catalyst was dry-calcined in air at 400°C for 3 hours to obtain the catalyst product.
[0198] Theoretical calculations show that the mass percentage of the catalyst components is:
[0199] [RuO2 / (RuO2+TiO2+BN)]*100=0.66%
[0200] The mass percentage of metallic ruthenium is:
[0201] [Ru / (RuO2+TiO2+BN)]*100=0.5%
[0202] The final catalyst strength was 143 N / cm and the specific surface area was 24 m 2 / g, average pore size 1.0um, and thermal conductivity tested at 350℃ is 1.23W / m·℃.
[0203] Examples 2-9
[0204] 35 g of rutile titanium dioxide, 65 g of β-phase silicon carbide, and 10.0 g of sesbania powder were mixed uniformly; 30 g of water was added to the mixture, and the mixture was kneaded for 40 min. The mixture was extruded to obtain a 3 mm diameter strip, which was then dried in air at 110°C for 5 hours to obtain a dried strip carrier, which was cut into 5 mm lengths.
[0205] The dried carrier was dry-calcined in air at 650° C. for 4 hours to obtain a calcined strip-shaped carrier.
[0206] 50 g of the calcined carrier was impregnated with 30 ml of a RuBr3·3H2O solution containing 0.92 g of Ru and added with 2.7 g of OP-10, and dried at 110°C for 6 hours to obtain a dried catalyst.
[0207] The dried catalyst was dry-calcined in air at 350°C for 2 hours; the product was washed with water and dried at 120°C to obtain the catalyst product.
[0208] Theoretical calculations show that the mass percentage of the catalyst components is:
[0209] [RuO2 / (RuO2+TiO2+SiC)]*100=2.37%
[0210] The mass percentage of metallic ruthenium is:
[0211] [Ru / (RuO2+TiO2+SiC)]*100=1.8%
[0212] The final catalyst strength was 129N / cm and the specific surface area was 20m 2 / g, average pore size 0.6um, and thermal conductivity tested at 350℃ is 1.45W / m·℃.
[0213] Example 2-10
[0214] 60 g of rutile titanium dioxide, 40 g of β-phase silicon carbide, and 8.0 g of sesbania powder were mixed uniformly; 26 g of water was added to the mixture, and the mixture was kneaded for 40 min. The mixture was extruded to obtain a 3 mm diameter strip, which was then dried in air at 110°C for 5 hours to obtain a dried strip carrier, which was cut into 5 mm lengths.
[0215] The dried carrier was dry-calcined in air at 650° C. for 4 hours to obtain a calcined strip-shaped carrier.
[0216] 50 g of the calcined support was impregnated with 32 ml of a RuCl3·3H2O solution containing 0.4 g of Ru and 0.8 g of PEG-400, and dried at 110°C for 6 hours to obtain a dried catalyst.
[0217] The dried catalyst was dry-calcined in air at 300°C for 3 hours; the product was washed with water until there was no chloride ion, and dried at 120°C to obtain the catalyst product.
[0218] Theoretical calculations show that the mass percentage of the catalyst components is:
[0219] [RuO2 / (RuO2+TiO2+Si3N4)]*100=1.0%
[0220] The mass percentage of metallic ruthenium is:
[0221] [Ru / (RuO2+TiO2+Si3N4)]*100=0.8%
[0222] The final catalyst strength was 121N / cm and the specific surface area was 27m 2 / g, average pore size 0.09um, thermal conductivity tested at 350℃ is 1.28W / m·℃.
[0223] Example 2-11
[0224] 55 g of rutile titanium dioxide, 45 g of β-silicon nitride, and 3.0 g of sesbania powder were mixed uniformly; 28 g of water was added to the mixture, and the mixture was kneaded for 40 min. The mixture was extruded to obtain a 3 mm diameter strip, which was then dried in air at 120°C for 4 hours to obtain a dried strip carrier, which was cut into 5 mm lengths.
[0225] The dried carrier was dry-calcined in air at 750° C. for 4 hours to obtain a calcined strip-shaped carrier.
[0226] 50 g of the calcined carrier was impregnated with 28 ml of a RuCl3·3H2O solution containing 0.61 g of Ru and added with 1.8 g of OP-10, and dried at 120°C for 6 hours to obtain a dried catalyst.
[0227] The dried catalyst was dry-calcined in air at 350°C for 3 hours; the product was washed with water and dried at 120°C to obtain the catalyst product.
[0228] Theoretical calculations show that the mass percentage of the catalyst components is:
[0229] [RuO2 / (RuO2+TiO2+Si3N4)]*100=1.58%
[0230] The mass percentage of metallic ruthenium is:
[0231] [Ru / (RuO2+TiO2+Si3N4)]*100=1.2%
[0232] The final catalyst strength was 139 N / cm and the specific surface area was 42 m 2 / g, average pore size 0.04um, thermal conductivity tested at 350℃ is 1.22W / m·℃.
[0233] Example 2-12
[0234] 30 g of rutile titanium dioxide, 60 g of hexagonal boron nitride, and 3.0 g of sesbania powder were mixed uniformly; 30 g of water was added to the mixture, and the mixture was kneaded for 40 min. The mixture was extruded to obtain a 3 mm diameter strip, which was then dried in air at 120°C for 4 hours to obtain a dried strip carrier, which was cut into 5 mm lengths.
[0235] The dried carrier was dry-baked in air at 600℃ for 4 hours to obtain a strip carrier with a strength of 153N / cm and a specific surface area of 25m 2 / g, average pore size 0.9um.
[0236] 50 g of the calcined support was taken and impregnated with 28 ml of a RuCl3·3H2O solution containing 1.03 g of Ru and 1.0 g of PEG-400, and dried at 120°C for 6 hours to obtain a dried catalyst.
[0237] The dried catalyst was dry-calcined in air at 280°C for 3 hours; the product was washed with water and dried at 120°C to obtain the catalyst product.
[0238] Theoretical calculations show that the mass percentage of the catalyst components is:
[0239] [RuO2 / (RuO2+TiO2+BN)]*100=2.63%
[0240] The mass percentage of metallic ruthenium is:
[0241] [Ru / (RuO2+TiO2+BN)]*100=2.0%
[0242] The final catalyst strength was 151N / cm and the specific surface area was 25m 2 / g, average pore size 0.03um, thermal conductivity tested at 350℃ is 1.52W / m·℃.
[0243] Control group 2-1
[0244] This example is based on the technical solution disclosed in Example 18 of Sumitomo Chemical patent CN1272238C to prepare a supported ruthenium oxide catalyst:
[0245] 2.03 grams of commercially available ruthenium oxide hydrate (RuCl3·nH2O, Ru content 37.3wt%) was dissolved in 14.6 grams of pure water and stirred to obtain a ruthenium chloride aqueous solution. The resulting aqueous solution was dropwise added to a 50.0 gram strip composite support composed of titanium oxide-α-alumina (50% titanium oxide) to impregnate the ruthenium chloride. The supported material was dried in air at 60°C for 2 hours to obtain titanium oxide-α-alumina-supported ruthenium chloride. A mixed solution consisting of 10.5 grams of 2 mol / L potassium hydroxide aqueous solution, 300 grams of pure water, and 2.54 grams of hydrazine hydrate was added to the resulting titanium oxide-α-alumina-supported ruthenium chloride at room temperature. The solution was stirred every 15 minutes and impregnated for 1 hour. Foaming was observed in the solution during impregnation. After standing for about 15 minutes until the foaming disappeared, it was filtered, 0.5 liters of pure water was added, and the solution was stirred and allowed to stand for 30 minutes. It was then filtered and repeated 5 times. Afterwards, remove the supernatant by decantation. Then, add 100 g of a 0.5 mol / L potassium chloride aqueous solution, stir, and let stand for 30 minutes. Then, remove the supernatant by decantation. Repeat this process three times. Then, air dry the washed material at 60°C for 4 hours to obtain a gray spherical solid containing potassium chloride.
[0246] The resulting solid was then heated in air from room temperature to 350°C over approximately one hour and calcined at this temperature for three hours to obtain a spherical solid. 0.5 L of pure water was added to the resulting solid, stirred, allowed to stand for 30 minutes, and then washed by filtration. This operation was repeated five times. The washing time was approximately four hours. The washed material was dried in air at 60°C for four hours to obtain 50.0 g of a gray-black supported ruthenium oxide catalyst.
[0247] The calculated value of the metallic ruthenium content is 1.5% Ru / (TiO2:Al2O3=50:50), and the tested thermal conductivity at 350°C is 0.57 W / m·°C.
[0248] Test Example 2-1
[0249] The catalyst activities of all examples were tested in a fixed-bed catalytic reactor. The reactor type was a quartz tubular reactor with an inner diameter of 25 mm. The catalyst particle size was original, and the catalyst dosage was 10 g. The main reaction conditions were: 0.1 MPa, HCl at 0.76 L / min, and O2 at 0.64 L / min through the catalyst bed. The conversion rates at different temperatures are shown in Tables 3 and 4. Examples 2-1 to 2-12 were tested under similar conditions to Control 2-1.
[0250] Table 3. Thermal conductivity of catalysts from different examples and hydrogen chloride conversion at different temperatures
[0251] Table 4. Conversion rate of catalysts in different embodiments after 500 h of operation
[0252] As can be seen from Tables 3 and 4, the overall activity of the catalysts prepared in Examples 2-1 to 2-12 is higher than that of the control group, especially the conversion rate in the high temperature range and the life of the catalyst at high temperature are significantly improved.
[0253] The above is only a preferred embodiment of the present application. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principles of the present application. These improvements and modifications should also be regarded as the scope of protection of the present application.
Claims
1. A method for preparing a highly dispersed ruthenium catalyst for preparing chlorine by oxidation of hydrogen chloride, characterized in that include: (1) dispersing the ruthenium-containing active component through a surfactant to prepare an impregnation solution, (2) contacting and adhering the impregnation solution to a composite support of titanium oxide and aluminum oxide, drying and then calcining, (3) cooling, washing with water, and drying, Or (1) titanium oxide, high thermal conductivity ceramics and additives are mixed to obtain a mixed powder, the mixed powder is mixed with water, molded, dried, and subjected to a first calcination to obtain a high-strength carrier, wherein the high thermal conductivity ceramic is selected from any one or more of Si3N4, BN, and SiC; (2) a ruthenium active component precursor solution is prepared into an impregnation liquid, wherein the impregnation liquid also includes a surfactant; (3) the impregnation liquid is impregnated on the high-strength carrier, dried, and subjected to a second calcination to obtain the ruthenium catalyst; The surfactant is selected from any one or more of polyoxyethylene nonionic surfactants, polyethylene glycol, and polysorbate, and the amount of the surfactant is 1-10 times the mass of the metal element in the ruthenium-containing active component. The ruthenium catalyst has a specific surface area of 10-50 m 2 / g, and ruthenium element accounts for 0.1-10wt% of the ruthenium catalyst.
2. The method for preparing a highly dispersed ruthenium catalyst for preparing chlorine by oxidation of hydrogen chloride according to claim 1, characterized in that: The surfactant is selected from any one or more of T-80, OP-10, and PEG-400; and / or the ruthenium active component is selected from any one or more combinations of ruthenium trichloride or its hydrate, ruthenium tribromide or its hydrate, chlororuthenate or its hydrate, ruthenate, ruthenium oxychloride, ruthenium oxychloride salt, ruthenium ammine complex, ruthenium chloride amine complex, ruthenium bromide amine complex, ruthenium acetylacetonate, carbonyl ruthenium, organic acid salt of ruthenium, ruthenium nitrosyl nitrate, ruthenium-nitrosyl complex, ruthenium phosphorus complex; and / or the auxiliary agent is selected from any one or more of polyvinyl alcohol, cellulose, starch, sesbania powder, and synthetic resin; the auxiliary agent is 1-10wt% of the mixed powder; and / or the titanium oxide is rutile titanium dioxide; And / or the aluminum oxide is α-Al2O3.
3. The method for preparing a highly dispersed ruthenium catalyst for preparing chlorine by oxidation of hydrogen chloride according to claim 1, characterized in that: The impregnation method in the impregnation liquid contact attachment is any one of equal volume impregnation, excess impregnation and spray impregnation; and / or the impregnation liquid contact attachment is completed at a temperature of 30-60°C; and / or the calcination temperature in the calcination after drying is 150-700°C and the time is 1-24 hours.
4. The method for preparing a highly dispersed ruthenium catalyst for preparing chlorine by oxidation of hydrogen chloride according to claim 1, characterized in that: The composite carrier is prepared by a molding process and has any one or more shapes including powder, spherical, columnar, irregular, and honeycomb.
5. The method for preparing a highly dispersed ruthenium catalyst for preparing chlorine by oxidation of hydrogen chloride according to claim 1, characterized in that: The ruthenium element accounts for 0.3-5wt% of the ruthenium catalyst.
6. The method for preparing a highly dispersed ruthenium catalyst for preparing chlorine by oxidation of hydrogen chloride according to claim 1, characterized in that: The particle size of ruthenium is 1-10nm, and the surface area of ruthenium metal is 120-410m 2 / (g·Ru).
7. The method for preparing a highly dispersed ruthenium catalyst for preparing chlorine by oxidation of hydrogen chloride according to claim 1, characterized in that: The pore size of the ruthenium catalyst is 0.01-6um, and the strength is 120-200N / cm when the diameter is 1.5-3mm cylinder.
8. The method for preparing a highly dispersed ruthenium catalyst for preparing chlorine by oxidation of hydrogen chloride according to claim 1, characterized in that: The first calcination is calcined at 300-800° C. for 1-24 h; and / or the second calcination is calcined at 200-700° C. for 1-24 h, and then naturally cooled to room temperature.
9. The method for preparing a highly dispersed ruthenium catalyst for preparing chlorine by oxidation of hydrogen chloride according to claim 7, characterized in that: The thermal conductivity of the ruthenium catalyst at 350° C. based on the hot wire method is 0.6-2.0 W / m·° C.
10. A ruthenium catalyst, characterized in that: The ruthenium catalyst is prepared by the method according to any one of claims 1-9.
Citation Information
Patent Citations
Method for production of supported ruthenium and method for production of chlorine
CN101316656A
Ruthenium dioxide catalyst for producing chlorine by oxidizing hydrogen chloride and preparation method thereof
CN109453764A
Preparation method of hydrogen chloride oxidation catalyst
CN115155632A
High-dispersity ruthenium catalyst for preparing chlorine by oxidizing hydrogen chloride and preparation method of high-dispersity ruthenium catalyst
CN116550321A
High-thermal-conductivity ruthenium catalyst with thermal stability and preparation method thereof