High mobility substrate having δ-doped layer and method for manufacturing high mobility substrate

The high mobility substrate, achieved by sandwiching a thin silicon layer between δ-doped layers with larger band gaps, addresses the challenge of achieving uniform mobility across large substrates, using oxygen δ-doping to enhance silicon-based substrates, resulting in mobility comparable to two-dimensional materials like MoS2 without the need for expensive materials.

WO2024241643A1PCT designated stage expired Publication Date: 2024-11-28SHIN ETSU HANDOTAI CO LTD
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2024/006739
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-05-25
Filing Date
2024-02-26
Publication Date
2024-11-28

AI Technical Summary

Technical Problem

Current methods struggle to achieve uniform high mobility across large-area substrates, particularly with silicon materials, due to challenges in forming and attaching two-dimensional materials like MoS2, and in-plane uniformity of oxide films, which limits the effectiveness of silicon-based substrates in achieving mobility comparable to two-dimensional materials.

Method used

A high mobility substrate is created by sandwiching a thin silicon layer between δ-doped layers with larger band gaps, using oxygen δ-doping to form silicon oxide films, which improves mobility by reducing interface roughness and maintaining high mobility across large areas without the need for expensive two-dimensional materials.

Benefits of technology

This approach enables the achievement of high mobility comparable to two-dimensional materials like MoS2, while ensuring uniformity and practicality on large-diameter substrates, using general semiconductor materials like silicon, thus overcoming the limitations of existing technologies.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JP2024006739_28112024_PF_FP_ABST
    Figure JP2024006739_28112024_PF_FP_ABST
Patent Text Reader

Abstract

The present invention is a high mobility substrate characterized by comprising a semiconductor substrate, a first δ-doped layer having a band gap larger than that of the semiconductor substrate on the semiconductor substrate, a thin film of the same material as the semiconductor substrate on the first δ-doped layer, and a second δ-doped layer having a band gap larger than that of the semiconductor substrate on the thin film, the high mobility substrate being structured such that the thin film is sandwiched between the first δ-doped layer and the second δ-doped layer. In this way, a high mobility substrate and a method for manufacturing a high mobility substrate are provided that are practical and make uniform creation on the entire surface of a substrate having a large area possible, while achieving high mobility.
Need to check novelty before this filing date? Find Prior Art

Description

High mobility substrate having δ-doped layer and method for manufacturing high mobility substrate

[0001] The present invention relates to a high mobility substrate having a δ-doped layer and a method for manufacturing the high mobility substrate.

[0002] MoS is being considered as the next-generation channel material for the currently mainstream FinFET (Fin Field Effect Transistor) and the partially commercialized GAAFET (Gate All Around Field Effect Transistor). 2 Two-dimensional materials such as these are being actively researched. This is because we are reaching the limit of performance improvement through the progress of miniaturization, and this technology aims to improve performance by using a material with high mobility as the channel material.

[0003] However, the proposed two-dimensional materials include the aforementioned MoS 2 Materials such as graphene and BN are known, and the significance of their properties has been demonstrated, but it is still difficult to obtain a film with a large diameter. Non-Patent Document 1 shows an example of BN, but it appears to be a film formation situation from the center to about halfway of a silicon substrate with a diameter of 100 mm.

[0004] In addition to the difficulty of film formation, it is easy to imagine that the characteristics of the material (which exists stably as a two-dimensional thin film) make it difficult to attach or fix to a substrate, and in devices where operation has been proven, the two-dimensional material appears to be fixed using source and drain electrode materials.

[0005] On the other hand, when we look at silicon materials, it has been known since the dawn of SOI (Silicon on Insulator) that mobility can be improved by sandwiching thin silicon of about 2 to 3 nm between silicon oxide films. 2 It is possible to achieve mobility comparable to that of two-dimensional materials such as those mentioned above (Non-Patent Documents 2 and 3).

[0006] As mentioned above, if silicon is covered (sandwiched) with an insulating film, the mobility is improved and the mobility can be equivalent to that of two-dimensional materials. However, it is difficult to achieve a uniform structure over the entire surface of a wafer, for example, the entire surface of a 300 mm diameter substrate. In the conventional method, first, a wafer with an oxide film is formed and H + By bonding and peeling the silicon-implanted substrates together, a silicon layer is transferred onto the oxide film, and then an oxide film is formed. However, it is difficult to achieve a uniform thickness of 2-3 nm over the entire surface of a 300 mm diameter due to the problem of in-plane uniformity of the oxide film. (The in-plane uniformity of the oxidation furnace must be kept to 0.1 nm or less over a 300 mm diameter.)

[0007] ISSCC2021.1.1, Mark Liu, “Unleashing the Future of Innovation” ISSCC2023.27.3, D. Verrreck et. al., “The promise of 2-D materials for scaled digital and analog applications” Sumida et al., “Optimal design of channel material and plane orientation for ultra-thin film nMOSFETs utilizing anisotropy of electron valleys to suppress surface roughness scattering” Proceedings of the 70th Spring Meeting of the Japan Society of Applied Physics, 2023, 16p-A403-2.

[0008] As mentioned above, although it was previously known that high mobility could be achieved by thinning silicon and covering (sandwiching) it with an oxide film, it was difficult to create it uniformly over the entire substrate, making it impractical.

[0009] The present invention has been made in consideration of the above-mentioned problems of the conventional technology, and aims to provide a practical high-mobility substrate and a method for manufacturing a high-mobility substrate that can be formed uniformly over the entire surface of a large-area substrate while realizing high mobility.

[0010] In order to solve the above problems, the high mobility substrate of the present invention has a semiconductor substrate, a first δ-doped layer on the semiconductor substrate and having a band gap larger than that of the semiconductor substrate, a thin film on the first δ-doped layer made of the same material as the semiconductor substrate, and a second δ-doped layer on the thin film and having a band gap larger than that of the semiconductor substrate, with the thin film sandwiched between the first δ-doped layer and the second δ-doped layer.

[0011] In such a high-mobility substrate, the first δ-doped layer and the second δ-doped layer have a larger band gap than the thin film. Therefore, at the interface between the thin film and each δ-doped layer, band curvature (also known as band bending) similar to that observed at the junction between a semiconductor and an insulator with a larger band gap than the semiconductor occurs, forming a low-potential groove and improving mobility. Furthermore, the use of δ-doped layers prevents interface roughness, preventing mobility degradation due to interface scattering and maintaining high mobility. Furthermore, δ-doped layers can be easily doped onto semiconductor substrates and thin films, and can be uniformly formed over the entire surface of large-area substrates, especially those with large diameters. The definition of δ-doping is that the doped layer is thin (e.g., 3 nm or less).

[0012] Preferably, the first δ-doped layer and the second δ-doped layer are oxygen δ-doped layers, the semiconductor substrate and the thin film are silicon, and the thickness of the thin film is 2 nm to 3 nm.

[0013] Such an oxygen δ-doped layer can be formed on a silicon substrate or a silicon thin film as an insulating film. 2 The structure is such that a thin silicon layer of 2 nm to 3 nm is sandwiched between silicon oxide films, which reliably improves mobility and 2 This makes it possible to achieve mobility comparable to that of two-dimensional materials such as silicon dioxide.

[0014] In addition, the method for producing a high-mobility substrate of the present invention is a method in which a first δ-doped layer having a band gap larger than that of the semiconductor substrate is formed on a semiconductor substrate, a thin film made of the same material as the semiconductor substrate is formed thereon, a second δ-doped layer having a band gap larger than that of the semiconductor substrate is formed thereon, and the thin film is sandwiched between the first δ-doped layer and the second δ-doped layer.

[0015] In this method for manufacturing a high-mobility substrate, the first δ-doped layer and the second δ-doped layer have a larger band gap than the thin film. Therefore, at the interface between the thin film and each δ-doped layer, band curvature (also known as band bending) similar to that observed at the interface between a semiconductor and an insulator with a larger band gap than the semiconductor occurs, forming a low-potential groove, thereby improving mobility. Furthermore, the use of the δ-doped layer prevents interface roughness from increasing, preventing a decrease in mobility due to interface scattering and maintaining high mobility. Furthermore, the δ-doped layer can be easily doped onto the semiconductor substrate and the thin film, and can be uniformly formed over the entire surface of a large-area substrate, especially a substrate with a large diameter.

[0016] It is also preferable that the first δ-doped layer and the second δ-doped layer are oxygen δ-doped layers, the semiconductor substrate and the thin film are silicon, and the thickness of the thin film is 2 nm to 3 nm.

[0017] If such an oxygen δ-doped layer is used, a silicon oxide film SiO 2 The structure is such that a thin silicon layer of 2 nm to 3 nm is sandwiched between silicon oxide films, which reliably improves mobility and 2 It is possible to achieve mobility comparable to that of two-dimensional materials such as silicon dioxide.

[0018] Furthermore, it is preferable that the thin film is formed to a thickness that takes into account the fact that it will be thinned by oxidation, and then the thin film is oxidized to form the second δ-doped layer.

[0019] This method prevents the thin film from becoming too thin and ensures that the film is formed to the desired thickness.

[0020] It is also preferable to form silicon on the first δ-doped layer to a thickness of 1 nm or more and 3 nm or less, and then form an oxygen δ-doped layer multiple times, and then form the thin silicon film on top of that to a thickness of 2 nm or more and 3 nm or less.

[0021] By using this method, a high mobility substrate can be reliably manufactured even if it has a laminated structure.

[0022] The high-mobility substrate and the method for manufacturing the high-mobility substrate of the present invention can be practically produced evenly over the entire surface of a large-area substrate, especially a large-diameter substrate, while realizing high mobility. Furthermore, by using a thin film layer simulating such a two-dimensional material, it becomes possible to form a high-mobility channel material over the entire surface of a large-area substrate, especially a large-diameter substrate. Furthermore, MoS 2 It is inexpensive because it can be realized using common semiconductor materials such as silicon, without using expensive two-dimensional materials such as silicon.

[0023] 1A to 1C are schematic diagrams of a high mobility substrate according to a first embodiment of the present invention, a high mobility substrate according to a second embodiment of the present invention, and a high mobility substrate according to a third embodiment of the present invention.

[0024] The present invention will be described in detail below, but the present invention is not limited thereto.

[0025] As a result of intensive research into the above-mentioned problems, the inventors have discovered a structure comprising a semiconductor substrate, a first δ-doped layer on the semiconductor substrate, the first δ-doped layer having a band gap larger than that of the semiconductor substrate, a thin film made of the same material as the semiconductor substrate on the first δ-doped layer, and a second δ-doped layer on the thin film, the thin film being sandwiched between the first δ-doped layer and the second δ-doped layer, thereby completing the present invention. Specifically, by combining lamination of δ-doped and thin-film silicon with oxidation treatment, an insulating oxide film (more specifically, SiO 2 , a material having a band gap larger than that of silicon) can be formed as the δ-doped layer. 2The inventors discovered that by sandwiching a thin film silicon of 2 nm to 3 nm in thickness between the two layers of the substrate, it is possible to obtain a cheaper, higher quality substrate without using expensive two-dimensional materials, and completed the present invention.

[0026] This can be achieved, for example, by delta-doping oxygen atoms onto a silicon substrate, stacking silicon thereon to a thickness of 2 nm to 3 nm to form a thin film of silicon, and then delta-doping oxygen atoms thereon.

[0027] Furthermore, it can also be provided by delta-doping oxygen atoms onto a silicon substrate, laminating silicon on top of that to a thickness that takes into account the thinning caused by oxidation, to form a thin film of silicon, and then oxidizing it.

[0028] Furthermore, the thin film can also be provided by repeating the process of delta-doping oxygen atoms onto a silicon substrate, laminating silicon to a thickness of 1 nm to 3 nm, preferably 1 nm, and further delta-doping oxygen atoms multiple times, and then laminating silicon to a thickness of 2 to 3 nm on top to form a thin film silicon, and further delta-doping oxygen atoms.

[0029] A first embodiment of the present invention will now be described with reference to the drawings. First, the configuration of a high-mobility substrate 1 will be described with reference to FIG. 1. As shown in FIG. 1, the high-mobility substrate 1 of this embodiment includes a semiconductor substrate (support substrate) 2, a first δ-doped layer (first oxide film layer) 3-1 on the semiconductor substrate 2, the first δ-doped layer 3-1 being made of the same material as the semiconductor substrate 2, and a second δ-doped layer (second oxide film layer) 3-2 on the thin film 4, the second δ-doped layer 3-1 being made of the same material as the semiconductor substrate 2, and the second δ-doped layer 3-2 being made of the same material as the semiconductor substrate 2. The thin film 4 is sandwiched between the first δ-doped layer 3-1 and the second δ-doped layer 3-2.

[0030] In a more preferred embodiment, the first δ-doped layer 3-1 and the second δ-doped layer 3-2 are oxygen δ-doped layers, each forming an oxide film. The semiconductor substrate 2 and thin film 4 are silicon, with a thickness of 2 nm to 3 nm to achieve high mobility. A thickness of 2 nm or greater makes the thin film (silicon) 4 layer more likely to become perfectly crystalline, improving mobility. On the other hand, a thickness of 3 nm or less results in characteristics different from those of ordinary bulk silicon, enabling more effective improvement in mobility. The following description focuses on a preferred embodiment in which the semiconductor substrate 2 is a silicon substrate and the δ-doped layer is an oxide film layer. In the case of oxygen doping, δ-doping can be achieved by thermal oxidation or natural oxidation.

[0031] In the high-mobility substrate 1 of this embodiment, the first δ-doped layer 3-1 and the second δ-doped layer 3-2 have a larger band gap than the thin film 4. Therefore, at the junction interface between the thin film 4 and each δ-doped layer, a band curvature (also called band bending) similar to that observed at the junction between a semiconductor and an insulator with a larger band gap than the semiconductor occurs, forming a low-potential groove and improving mobility. Furthermore, the use of a δ-doped layer prevents interface roughness from increasing, preventing a decrease in mobility due to interface scattering and maintaining high mobility. Furthermore, the δ-doped layer can be easily doped onto the semiconductor substrate and thin film, and can be formed uniformly over the entire surface of a large-area substrate, especially a substrate with a large diameter.

[0032] In the case of the oxygen δ-doped layer (first δ-doped layer 3-1 and second δ-doped layer 3-2) of this embodiment, a silicon oxide film SiO 2 is formed as an insulating film on a silicon substrate (semiconductor substrate 2) or a silicon thin film (thin film 4). 2 The structure is such that a thin silicon film (thin film 4) of 2 nm or more and 3 nm or less is sandwiched between silicon oxide films, which reliably improves the mobility and 2 This makes it possible to achieve mobility comparable to that of two-dimensional materials such as silicon dioxide.

[0033] Next, a specific manufacturing flow of the high-mobility substrate 1 of this embodiment will be described with reference to Fig. 1. A semiconductor substrate (support substrate) 2 is prepared, which can be a general silicon substrate. In the case of a silicon substrate, a (100) orientation is preferable from the viewpoint of electron mobility, but a (110) substrate may also be used in consideration of the balance with hole mobility, and the substrate surface orientation can be selected depending on the application.

[0034] Next, a first δ-doped layer (first oxide film layer) 3-1 of oxygen having a band gap larger than that of the semiconductor substrate 2 is formed on the semiconductor substrate (support substrate) 2. If this method is used to form a δ-doped layer on the semiconductor substrate 2, the δ-doped layer can be formed uniformly even on a large diameter substrate such as a substrate with a diameter of 300 mm.

[0035] There are no particular restrictions on the method for forming the δ-doped layer, but the oxygen concentration can be set to a concentration at which silicon single crystal can grow, in anticipation of further forming a thin film (silicon) 4 made of the same material as the semiconductor substrate on top of the δ-doped layer. In this case, the oxygen concentration is set to 1×10 15 atoms / cm 2 It is preferable to set it to around the same time.

[0036] Next, a thin film (silicon) 4 made of the same material as the semiconductor substrate 2 is grown on the first δ-doped layer 3-1. When growing a thin film having a thickness of 2 nm to 3 nm, there are no particular restrictions on the growth method, but growth can be easily achieved by using an apparatus that can set low temperature and reduced pressure conditions.

[0037] Next, a second δ-doped layer (second oxide film layer) 3-2 of oxygen having a band gap larger than that of the semiconductor substrate 2 is formed on the thin film 4. This method may be the same as the method for forming the first δ-doped layer (first oxide film layer) 3-1.

[0038] As a result of the above, the thin film 4 can be sandwiched between the first δ-doped layer 3-1 and the second δ-doped layer 3-2, and the high mobility substrate 1 as shown in FIG. 1 can be manufactured.

[0039] In the manufacturing method of the high-mobility substrate 1 of this embodiment, the first δ-doped layer 3-1 and the second δ-doped layer 3-2 have a larger band gap than the thin film 4. Therefore, at the junction interface between the thin film 4 and each δ-doped layer, a band curvature (also known as band bending) similar to that observed at the junction between a semiconductor and an insulator with a larger band gap than the semiconductor occurs, forming a low-potential groove, thereby improving mobility. Furthermore, the use of a δ-doped layer prevents increased interface roughness, preventing a decrease in mobility due to interface scattering and maintaining high mobility. Furthermore, the δ-doped layer can be easily doped onto the semiconductor substrate and thin film, and can be uniformly formed over the entire surface of a large-area substrate, especially a substrate with a large diameter.

[0040] In the case of the oxygen δ-doped layer (first δ-doped layer 3-1 and second δ-doped layer 3-2) of this embodiment, a silicon oxide film SiO 2 The structure is such that a thin silicon film (thin film 4) of 2 nm or more and 3 nm or less is sandwiched between silicon oxide films, which reliably improves the mobility and 2 It is possible to achieve mobility comparable to that of two-dimensional materials such as silicon dioxide.

[0041] A second embodiment will be described with reference to Fig. 2. In the method for manufacturing a high mobility substrate of this embodiment, a thin film is formed to a thickness that takes into account the fact that it will be thinned by oxidation, and then the thin film is oxidized to form a second δ-doped layer.

[0042] 2 shows the state of the thin film (silicon) 5 before oxidation, in which the thin film (silicon) 5 has a portion 5-1 that will be oxidized to form the second δ-doped layer and a portion 5-2 that will remain as the thin film (silicon) without being oxidized. To ensure that the portion 5-2 that will remain as the thin film (silicon) without being oxidized is 2 nm to 3 nm thick, the thin film (silicon) 5 is grown in advance to a thickness greater than 2 nm to 3 nm. The oxidation method may be a method of thermally oxidizing the thin film 5.

[0043] Here, the thickness can be determined by taking into account the expected thinning ratio, since when silicon is oxidized to form an oxide film, about half of the oxide film is silicon (for example, 44 Å of silicon is used in an oxide film of 100 Å). However, it is desirable to confirm the thickness more accurately through preliminary experiments, etc.

[0044] By using this method, the portion 5-2 of the thin film 5 that is not oxidized and remains as a thin film (silicon) can be prevented from becoming too thin, less than 2 nm or more and 3 nm or less, and can be reliably formed to the desired thickness.

[0045] A third embodiment will be described with reference to Fig. 3. The method for manufacturing a high-mobility substrate of this embodiment involves forming silicon to a thickness of 1 nm to 3 nm on a first δ-doped layer, and then forming an oxygen δ-doped layer, which is repeated multiple times, and then forming a thin silicon film to a thickness of 2 nm to 3 nm on the silicon film.

[0046] Referring to FIG. 3, silicon 7-1 is formed on a first oxygen delta-doped layer 6-1 to a thickness of 1 nm or more and 3 nm or less, and then an oxygen delta-doped layer 6-2 is formed, and then silicon 7-2 is formed to a thickness of 1 nm or more and 3 nm or less, and then an oxygen delta-doped layer 6-3 is formed, and then a thin film (silicon) 4 is formed thereon to a thickness of 2 nm or more and 3 nm or less.

[0047] By using this method, a high mobility substrate can be reliably manufactured even if it has a laminated structure.

[0048] Here, the repetition of silicon and δ-doped layers multiple times indicates that a stacked structure can be achieved by repeating the process. On the other hand, in the CFET (Complementary Field Effect Transistor) structure, which is expected to be realized in the 2030s as a next-generation transistor structure, a structure in which three or four layers of channels are stacked is expected to obtain a sufficient current value, and this embodiment can be applied to such a stacked structure.

[0049] The present invention will be specifically explained below with reference to examples, but the present invention is not limited to these examples.

[0050] Example 1 Example 1 is an example in which the first embodiment described above is implemented, and a high mobility substrate as shown in FIG. 1 is manufactured.

[0051] First, a 300 mm diameter, boron-doped p-type silicon (110) single crystal substrate with a resistivity of 10 Ω·cm was prepared as the semiconductor substrate (support substrate) 2. This was immersed in a 1% hydrofluoric acid solution for 3 minutes, and after removing the native oxide film, it was left in the atmosphere (temperature 23°C ± 1°C, humidity 39% ± 3%) for 3 hours to form a first oxygen delta-doped layer 3-1. It was then placed in a low-pressure epitaxial growth chamber, where a thin-film (silicon) layer 4 was grown for 60 seconds under conditions of a temperature of 700°C, a pressure of 100 Torr, and 1200 sccm of monosilane. It was then removed from the chamber and left in the atmosphere for 1 hour to form a second oxygen delta-doped layer 3-2 on the surface side, resulting in a high-mobility substrate 1.

[0052] In the high mobility substrate obtained here, the first δ-doped layer, the thin film (silicon) layer, and the second δ-doped layer all had a thickness of 3 nm, and the mobility was 100 cm 2 / V·s.

[0053] Example 2 Example 2 is an example that differs from Example 1 in that the steps of forming the δ-doped layer and the silicon layer are added.

[0054] A 300 mm diameter, boron-doped p-type silicon (110) single crystal substrate with a resistivity of 10 Ω·cm was prepared as a semiconductor substrate (support substrate). It was immersed in a 1% hydrofluoric acid solution for 3 minutes, and after removing the native oxide film, it was left in air (temperature 23°C ± 1°C, humidity 39% ± 3%) for 3 hours to form a first δ-doped layer of oxygen. It was then placed in a low-pressure epitaxial growth chamber and grown for 2 seconds at 700°C, 100 Torr, and 1200 sccm of monosilane. It was then removed from the chamber and left in air for 1 hour to form a third δ-doped layer of oxygen. It was then placed in a low-pressure epitaxial growth chamber and grown for 2 seconds at 700°C, 100 Torr, and 1200 sccm of monosilane. The substrate was then removed from the apparatus and left in the atmosphere for 1 hour to form a second δ-doped layer of oxygen on the surface side. The substrate was then placed in a reduced-pressure epitaxial apparatus, where a silicon layer was grown in 2 seconds under conditions of a temperature of 700°C, a pressure of 100 Torr, and monosilane of 1200 sccm, yielding a high-mobility substrate.

[0055] In the high mobility substrate obtained here, the first δ-doped layer, the silicon layer, the third δ-doped layer, the thin film (silicon) layer, and the second δ-doped layer all had a thickness of 3 nm, and the mobility was 100 cm 2 / V·s.

[0056] Example 3 Example 3 is different from Example 1 in that the steps of forming the δ-doped layer and the silicon layer are added, the film formation conditions are different, and the second δ-doped layer is formed by thermally oxidizing the thin film (silicon) in a heat treatment furnace.

[0057] A 300 mm diameter, boron-doped p-type silicon (110) single crystal substrate with a resistivity of 10 Ω·cm was prepared as a semiconductor substrate (support substrate). It was immersed in a 1% hydrofluoric acid solution for 3 minutes, and after removing the native oxide film, it was left in air (temperature 23°C ± 1°C, humidity 39% ± 3%) for 3 hours to form a first δ-doped layer of oxygen. It was then placed in a low-pressure epitaxial growth chamber and grown for 2 seconds at 700°C, 100 Torr, and 1200 sccm of monosilane. It was then removed from the chamber and left in air for 1 hour to form a third δ-doped layer of oxygen. It was then placed in a low-pressure epitaxial growth chamber and grown for 120 seconds at 700°C, 100 Torr, and 1200 sccm of monosilane. Thereafter, the substrate was taken out of the apparatus and placed in a heat treatment furnace where it was heat treated in an oxygen atmosphere at 600° C. for 5 minutes, thereby forming a second δ-doped layer of oxygen on the surface side and obtaining a high mobility substrate.

[0058] In the high mobility substrate obtained here, the first δ-doped layer, the silicon layer, the third δ-doped layer, the thin film (silicon) layer, and the second δ-doped layer all had a thickness of 3 nm, and the mobility was 100 cm 2 / V·s.

[0059] The above results will be discussed. In particular, regarding mobility, according to Non-Patent Document 3, the conventional two-dimensional material MoS 2 The mobility of is 50 to 100 cm 2 / V·s, and the mobility of the high mobility substrates obtained in Examples 1 to 3 was 100 cm 2 / V·s, Examples 1 to 3 were able to achieve mobilities that were comparable to or better than those of two-dimensional materials.

[0060] As described above, it has been demonstrated that the high mobility substrate and the method for manufacturing the high mobility substrate of the present invention can be uniformly formed over the entire surface of a large-area substrate (large-diameter substrate) while realizing high mobility, and are therefore practical. Furthermore, by using a thin film layer simulating such a two-dimensional material, it becomes possible to form a high mobility channel material over the entire surface of a large-area substrate. Furthermore, MoS 2 It is inexpensive because it can be realized using common semiconductor materials such as silicon, without using expensive two-dimensional materials such as silicon.

[0061] The present invention includes the following aspects: [1]: A high-mobility substrate comprising: a semiconductor substrate; a first δ-doped layer on the semiconductor substrate, the first δ-doped layer having a band gap larger than that of the semiconductor substrate; a thin film on the first δ-doped layer made of the same material as the semiconductor substrate; and a second δ-doped layer on the thin film, the thin film being sandwiched between the first δ-doped layer and the second δ-doped layer. [2]: The high-mobility substrate according to [1] above, wherein the first δ-doped layer and the second δ-doped layer are oxygen δ-doped layers, the semiconductor substrate and the thin film are silicon, and the thin film has a thickness of 2 nm to 3 nm. [3]: A method for manufacturing a high-mobility substrate, comprising: forming a first δ-doped layer on a semiconductor substrate, the first δ-doped layer having a band gap larger than that of the semiconductor substrate; forming a thin film on the first δ-doped layer made of the same material as the semiconductor substrate; forming a second δ-doped layer on the second δ-doped layer having a band gap larger than that of the semiconductor substrate; and sandwiching the thin film between the first δ-doped layer and the second δ-doped layer. [4]: ​​A method for manufacturing a high-mobility substrate as described in [3] above, wherein the first δ-doped layer and the second δ-doped layer are δ-doped layers of oxygen, the semiconductor substrate and the thin film are silicon, and the thin film has a thickness of 2 nm to 3 nm. [5]: A method for manufacturing a high-mobility substrate as described in [3] or [4] above, wherein the thin film is formed to a thickness that takes into account the thinning due to oxidation, and the thin film is oxidized to form the second δ-doped layer. [6]: A method for manufacturing a high mobility substrate according to any one of [3] to [5] above, characterized in that a silicon layer is formed on the first δ-doped layer to a thickness of 1 nm or more and 3 nm or less, and then a δ-doped layer of oxygen is formed, and this process is repeated multiple times, and then the thin silicon film is formed on the silicon layer to a thickness of 2 nm or more and 3 nm or less.

[0062] The present invention is not limited to the above-described embodiments. The above-described embodiments are merely examples, and any configuration that is substantially identical to the technical idea described in the claims of the present invention and that provides similar effects is included within the technical scope of the present invention.

Claims

1. A high mobility substrate comprising: a semiconductor substrate; a first δ-doped layer disposed on said semiconductor substrate and having a band gap larger than that of said semiconductor substrate; a thin film disposed on said first δ-doped layer and made of the same material as said semiconductor substrate; and a second δ-doped layer disposed on said thin film and having a band gap larger than that of said semiconductor substrate, said thin film being sandwiched between said first δ-doped layer and said second δ-doped layer.

2. The high mobility substrate according to claim 1, characterized in that the first δ-doped layer and the second δ-doped layer are oxygen δ-doped layers, the semiconductor substrate and the thin film are silicon, and the thickness of the thin film is 2 nm or more and 3 nm or less.

3. A method for manufacturing a high mobility substrate, comprising forming a first δ-doped layer on a semiconductor substrate, the first δ-doped layer having a band gap larger than that of the semiconductor substrate, forming a thin film on the first δ-doped layer made of the same material as the semiconductor substrate, the second δ-doped layer on the second δ-doped layer having a band gap larger than that of the semiconductor substrate, and sandwiching the thin film between the first δ-doped layer and the second δ-doped layer.

4. A method for manufacturing a high mobility substrate as described in claim 3, characterized in that the first δ-doped layer and the second δ-doped layer are oxygen δ-doped layers, the semiconductor substrate and the thin film are silicon, and the thickness of the thin film is 2 nm or more and 3 nm or less.

5. A method for manufacturing a high mobility substrate as described in claim 3, characterized in that, when forming the thin film, the thin film is formed to a thickness that takes into account that the thin film will become thinner due to oxidation, and the second δ-doped layer is formed by oxidizing the thin film.

6. A method for manufacturing a high mobility substrate as described in any one of claims 3 to 5, characterized in that a silicon layer is formed on the first δ-doped layer to a thickness of 1 nm or more and 3 nm or less, and then a δ-doped layer of oxygen is formed, and this process is repeated multiple times, and then the thin silicon layer is formed on the silicon layer to a thickness of 2 nm or more and 3 nm or less.

Citation Information

Patent Citations

  • Method of manufacturing semiconductor wafer

    JP2005005490A

  • Method of manufacturing semiconductor substrate

    JP2009016637A

  • Method for manufacturing laminated wafer

    JP2015177150A

  • Method for manufacturing SOI wafer having thin film SOI layer

    JP2019087617A

  • Manufacturing method for epitaxial wafer, and epitaxial wafer

    JP2021111696A