Adhesive composition, adhesive, adhesive sheet, and optical member with adhesive layer

The adhesive composition with specific antistatic agents and (meth)acrylic acid ester polymers addresses static electricity and corrosion issues in electronic devices, providing a cost-effective solution with enhanced antistatic and corrosion-resistant properties.

WO2024241809A1PCT designated stage expired Publication Date: 2024-11-28LINTEC CORP
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2024/015758
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-05-23
Filing Date
2024-04-22
Publication Date
2024-11-28

AI Technical Summary

Technical Problem

Conventional adhesive compositions used in contact with metal members in electronic devices, such as touch panels, often suffer from static electricity issues, which can disturb liquid crystal molecule orientation and lead to corrosion, requiring separate antistatic and corrosion-resistant materials, increasing production costs.

Method used

An adhesive composition containing an antistatic agent with a hydroxyl group or a chain hydrocarbon with 1 to 7 carbon atoms, improving compatibility with polymers to prevent segregation and enhance antistatic and corrosion-resistant properties, including nitrogen-containing onium salts and (meth)acrylic acid ester polymers for crosslinking.

Benefits of technology

The adhesive composition achieves excellent antistatic properties and metal corrosion resistance, reducing the need for separate materials and lowering production costs by ensuring effective compatibility and performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JP2024015758_28112024_PF_FP_ABST
    Figure JP2024015758_28112024_PF_FP_ABST
Patent Text Reader

Abstract

Provided are: an adhesive composition containing an antistatic agent for constituting an adhesive used in contact with a metal member, wherein the antistatic agent is a compound having a hydroxyl group or the antistatic agent is a compound having a chain hydrocarbon and the number of carbons in the chain hydrocarbon is 1-7; an adhesive obtained by crosslinking the adhesive composition; and an adhesive sheet 1 provided with an adhesive layer 11 comprising the adhesive. The adhesive composition, the adhesive, and the adhesive sheet 1 have excellent antistatic properties and metal corrosion resistance.
Need to check novelty before this filing date? Find Prior Art

Description

Adhesive composition, adhesive, adhesive sheet, and optical member with adhesive layer

[0001] The present invention relates to a pressure-sensitive adhesive used in contact with a metal member, a pressure-sensitive adhesive sheet, an optical member with a pressure-sensitive adhesive layer, and a pressure-sensitive adhesive composition for constituting the pressure-sensitive adhesive.

[0002] In recent years, touch panels that serve as both a display device and an input device have come into widespread use in various electronic devices. Touch panels are primarily classified into resistive, capacitive, optical, and ultrasonic types. Resistive types include analog resistive and matrix resistive types, while capacitive types include surface and projected types.

[0003] Recently, projected capacitive touch panels have become widely used in mobile electronic devices such as smartphones and tablet terminals. For example, a known projected capacitive touch panel for such mobile electronic devices is one that includes, from bottom to top, a liquid crystal display (LCD), an adhesive layer, a transparent conductive film, a glass substrate, a transparent conductive film, and a protective layer such as tempered glass, laminated with an adhesive layer interposed therebetween. While tin-doped indium oxide (ITO) is primarily used as the material for the transparent conductive film, the use of other metals is also being considered.

[0004] A liquid crystal cell is generally used as an optical component constituting the liquid crystal display device. A liquid crystal cell generally comprises two transparent electrode substrates each having an alignment layer formed thereon, arranged with the alignment layer facing inward at a predetermined distance by a spacer, and sealed at their peripheries, with a liquid crystal material sandwiched between the two transparent electrode substrates. Typically, polarizing plates or the like are adhered to the outer surfaces of the two transparent electrode substrates in the liquid crystal cell via adhesive layers.

[0005] Here, the release sheet or optical film such as a polarizing plate laminated on the pressure-sensitive adhesive layer is usually made of a plastic material, which has high electrical insulation properties and is prone to generating static electricity when the release sheet is peeled off. If a polarizing plate or the like is attached to a liquid crystal cell while static electricity remains, the orientation of the liquid crystal molecules may be disturbed, and the static electricity may also damage the touch sensor. Furthermore, the presence of static electricity can cause problems such as the attraction of dust and dirt. To solve these problems, it is possible to impart antistatic properties to the pressure-sensitive adhesive layer.

[0006] Therefore, in order to obtain effective antistatic performance, it has been proposed to add an antistatic agent to a pressure-sensitive adhesive composition (for example, Patent Document 1).

[0007] Japanese Patent Application Laid-Open No. 2005-290357

[0008] On the other hand, the adhesive of the adhesive layer that contacts with metal members such as the transparent conductive film preferably has the performance of making these metal members less corroded, that is, metal corrosion resistance.Conventionally, the adhesive sheet that is used for laminating optical members such as polarizing plates and the adhesive sheet that is used in contact with metal members have been used separately as having different performances, but if the adhesive sheet has both antistatic and metal corrosion resistance performances, there is no need to distinguish them according to the place of use, and it is possible to reduce the production cost of electronic devices.

[0009] The present invention has been made in consideration of the above circumstances, and aims to provide an adhesive composition, an adhesive, an adhesive sheet, and an optical component with an adhesive layer, which have excellent antistatic properties and metal corrosion resistance.

[0010] In order to achieve the above object, firstly, the present invention provides an adhesive composition containing an antistatic agent for constituting an adhesive used in contact with a metal member, characterized in that the antistatic agent is a compound having a hydroxyl group or a compound having a chain hydrocarbon, and the number of carbon atoms in the chain hydrocarbon is 1 or more and 7 or less (Invention 1).

[0011] In the above invention (Invention 1), the inclusion of the specific antistatic agent improves the compatibility between the antistatic agent and the polymer contained in the adhesive. Therefore, the antistatic agent is less likely to segregate on the surface of the adhesive layer, thereby reducing the likelihood of a localized potential difference occurring between the adhesive layer and a metal member in contact with the adhesive layer, thereby providing excellent metal corrosion resistance. Furthermore, the good compatibility of the antistatic agent with the polymer contained in the adhesive makes it easier to obtain an adhesive that meets the required physical properties, thereby providing excellent antistatic properties.

[0012] In the above invention (Invention 1), it is preferable that the compound having a hydroxyl group has two or more hydroxyl groups in one molecule (Invention 2).

[0013] In the above inventions (Inventions 1 and 2), the antistatic agent is preferably an ionic compound (Invention 3).

[0014] In the above invention (invention 3), the ionic compound is preferably a nitrogen-containing onium salt (invention 4).

[0015] In the above invention (Invention 4), the cation constituting the nitrogen-containing onium salt is preferably a quaternary ammonium cation, a pyridinium cation or an imidazolium cation (Invention 5).

[0016] In the above inventions (Inventions 4 and 5), the anion constituting the nitrogen-containing onium salt is preferably a sulfonylimide anion (Invention 6).

[0017] In the above inventions (Inventions 5 and 6), it is preferable that the quaternary ammonium cation has a hydroxyl group (Invention 7).

[0018] In the above inventions (Inventions 5 and 6), it is preferable that the chain hydrocarbon is bonded to the nitrogen cation of the pyridinium-based cation or imidazolium-based cation (Invention 8).

[0019] In the above inventions (Inventions 1 to 8), it is preferable that the pressure-sensitive adhesive composition contains a (meth)acrylic acid ester polymer as a main adhesive agent (Invention 9).

[0020] Secondly, the present invention provides a pressure-sensitive adhesive (Invention 10) obtained by crosslinking the pressure-sensitive adhesive composition (Inventions 1 to 9).

[0021] Thirdly, the present invention provides a pressure-sensitive adhesive sheet (Invention 11) having a pressure-sensitive adhesive layer made of the pressure-sensitive adhesive (Invention 10).

[0022] In the above invention (Invention 11), it is preferable that the adhesive sheet has two release sheets, and the adhesive layer is sandwiched between the release sheets so as to contact the release surfaces of the two release sheets (Invention 12).

[0023] In the above inventions (Inventions 11 and 12), when a voltage of 100 V is applied to the exposed surface of the pressure-sensitive adhesive layer laminated on a release sheet for 30 seconds in an environment of 23°C and a relative humidity of 50%, the surface resistivity of the exposed surface of the pressure-sensitive adhesive layer is 1.2 × 10 12 It is preferably Ω / sq or less (Invention 13).

[0024] Fourthly, the present invention provides an optical member with a pressure-sensitive adhesive layer, characterized by comprising an optical member and a pressure-sensitive adhesive layer made of the pressure-sensitive adhesive (Invention 10) laminated on at least one surface of the optical member (Invention 14).

[0025] The pressure-sensitive adhesive composition, pressure-sensitive adhesive, pressure-sensitive adhesive sheet and pressure-sensitive adhesive layer-attached optical member according to the present invention have excellent antistatic properties and metal corrosion resistance.

[0026] 1 is a cross-sectional view of a pressure-sensitive adhesive sheet according to one embodiment of the present invention, and FIG. 2 is a cross-sectional view of a pressure-sensitive adhesive layer-attached optical member according to one embodiment of the present invention.

[0027] Hereinafter, embodiments of the present invention will be described. [Adhesive Composition] An adhesive composition according to one embodiment of the present invention is intended to constitute an adhesive used in contact with a metal member. The adhesive composition according to this embodiment contains an antistatic agent. The antistatic agent is (1) a compound having a hydroxyl group, or (2) a compound having a chain hydrocarbon, and the chain hydrocarbon has 1 to 7 carbon atoms.

[0028] Conventional antistatic agents that do not have a hydroxyl group or that have a long-chain hydrocarbon have poor compatibility with the polymer contained in the adhesive and tend to segregate on the surface of the adhesive layer. This creates a local potential difference between the adhesive layer and a metal member in contact with the adhesive, ionizing the metal and, as a result, facilitating corrosion of the metal member. In contrast, the antistatic agent contained in the adhesive composition according to the present embodiment is a compound having a hydroxyl group or a compound having a relatively short-chain hydrocarbon having 1 to 7 carbon atoms, thereby achieving good compatibility with the polymer contained in the adhesive. Therefore, the antistatic agent is less likely to segregate on the surface of the adhesive layer, thereby less likely to create a local potential difference between the adhesive layer and a metal member in contact with the adhesive layer, thereby exhibiting excellent metal corrosion resistance. Furthermore, due to the antistatic agent's good compatibility with the polymer contained in the adhesive, an adhesive that easily satisfies the physical properties described below can be easily obtained, thereby exhibiting excellent antistatic properties.

[0029] The metal member is not particularly limited, but a preferred example is an electrode in a capacitive touch panel. Examples of the electrode include transparent conductive films and mesh electrodes made of metals such as platinum, gold, silver, copper, and aluminum, oxides such as tin oxide, indium oxide, cadmium oxide, zinc oxide, and zinc dioxide, complex oxides such as tin-doped indium oxide (ITO), zinc oxide-doped indium oxide, fluorine-doped indium oxide, antimony-doped tin oxide, fluorine-doped tin oxide, and aluminum-doped zinc oxide, and non-oxide compounds such as chalcogenides, lanthanum hexaboride, titanium nitride, and titanium carbide.

[0030] The first antistatic agent in this embodiment (hereinafter sometimes referred to as "antistatic agent (C1)") is a compound having a hydroxyl group. The compound may have one hydroxyl group per molecule, but preferably has two or more, more preferably has two to six, particularly preferably has two to four, and even more preferably has two. This improves the compatibility of the antistatic agent (C1) with the polymer contained in the pressure-sensitive adhesive. As a result, a pressure-sensitive adhesive that easily satisfies the physical properties described below can be easily obtained, and the pressure-sensitive adhesive has better antistatic properties and metal corrosion resistance.

[0031] Examples of the antistatic agent (C1) include ionic compounds and nonionic compounds, with ionic compounds being preferred. The ionic compound may be a liquid (ionic liquid) or a solid (ionic solid) at room temperature. Here, the ionic compound in this specification refers to a compound in which a cation and an anion are bonded together primarily by electrostatic attraction. The antistatic agent may be used alone or in combination of two or more.

[0032] The ionic compound is preferably a nitrogen-containing onium salt, a sulfur-containing onium salt, a phosphorus-containing onium salt, an alkali metal salt, or an alkaline earth metal salt, and from the viewpoint of antistatic properties and metal corrosion resistance, a nitrogen-containing onium salt is particularly preferred. The nitrogen-containing onium salt is preferably an ionic compound composed of a nitrogen-containing cation and its counter anion, and particularly preferably an ionic compound composed of a nitrogen-containing cation having a hydroxyl group and its counter anion.

[0033] Examples of nitrogen-containing cations having a hydroxyl group include quaternary ammonium cations. Examples of quaternary ammonium cations having a hydroxyl group include hydroxyalkyl-trialkylammonium, bishydroxyalkyl-bisalkylammonium, and alkyl-bishydroxyalkyl-alkylammonium. The alkyl group in the above compound preferably has 1 to 15 carbon atoms, more preferably 1 to 12 carbon atoms, particularly preferably 1 to 8 carbon atoms, and even more preferably 1 to 4 carbon atoms. The hydroxyalkyl group in the above compound preferably has 1 to 5 carbon atoms, particularly preferably 1 to 4 carbon atoms, more preferably 2 to 3 carbon atoms, and most preferably 2 carbon atoms. Of the above compounds, butyl-bishydroxyethyl-methylammonium is particularly preferred.

[0034] On the other hand, as the anion constituting the ionic compound, sulfonylimide anions or halogenated phosphate anions are preferred, with sulfonylimide anions being particularly preferred. Preferred examples of sulfonylimide anions include bis(fluorosulfonyl)imide and bis(fluoroalkylsulfonyl)imide. The bis(fluoroalkylsulfonyl)imide may be bis(perfluoroalkylsulfonyl)imide, with bis(trifluoromethanesulfonyl)imide being a preferred example. Preferred examples of halogenated phosphate anions include hexafluorophosphate. Among the above, bis(fluorosulfonyl)imide is particularly preferred from the viewpoint of antistatic properties.

[0035] Examples of nitrogen-containing onium salts comprising a quaternary ammonium cation having a hydroxyl group and a sulfonylimide anion include butyl-bishydroxyethyl-methylammonium bis(fluorosulfonyl)imide and butyl-bishydroxyethyl-ethylammonium bis(fluorosulfonyl)imide, with butyl-bishydroxyethyl-methylammonium bis(fluorosulfonyl)imide being particularly preferred. Butyl-bishydroxyethyl-methylammonium bis(fluorosulfonyl)imide makes it easy to obtain a PSA that easily satisfies the physical properties described below, and can exhibit better antistatic properties and metal corrosion resistance.

[0036] The second antistatic agent in this embodiment (hereinafter sometimes referred to as "antistatic agent (C2)") is a compound having a chain hydrocarbon, and the chain hydrocarbon has 1 to 7 carbon atoms. The number of carbon atoms is preferably 1 to 6, particularly preferably 1 to 5, and even more preferably 1 to 4. This improves the compatibility of the antistatic agent (C2) with the polymer contained in the PSA. As a result, a PSA that easily satisfies the physical properties described below is easily obtained, and the PSA has better antistatic properties and metal corrosion resistance.

[0037] Examples of the antistatic agent (C2) include ionic compounds and nonionic compounds, with ionic compounds being preferred. Preferred ionic compounds include nitrogen-containing onium salts, sulfur-containing onium salts, phosphorus-containing onium salts, alkali metal salts, and alkaline earth metal salts, with nitrogen-containing onium salts being particularly preferred from the viewpoints of antistatic properties and metal corrosion resistance. The nitrogen-containing onium salt is preferably an ionic compound composed of a nitrogen-containing cation and its counteranion, and particularly preferably an ionic compound composed of a nitrogen-containing cation having a chain hydrocarbon and its counteranion.

[0038] The nitrogen-containing cation having a chain hydrocarbon is preferably one having a heterocyclic structure containing a nitrogen cation, specifically, pyridinium-based cation, imidazolium-based cation, pyrrolidinium-based cation, etc. Among them, from the viewpoint of antistatic property and metal corrosion resistance, pyridinium-based cation or imidazolium-based cation is particularly preferred. In this case, it is preferable that a chain hydrocarbon is bonded to the nitrogen cation of the heterocyclic structure. This makes it easy to obtain a pressure-sensitive adhesive that easily satisfies the physical properties described below, and the antistatic property and metal corrosion resistance are more excellent.

[0039] Examples of pyridinium cations include 1-alkylpyridinium cations, 1-alkyl-2-alkylpyridinium cations, 1-alkyl-3-alkylpyridinium cations, and 1-alkyl-4-alkylpyridinium cations, with 1-alkyl-3-alkylpyridinium cations being preferred.

[0040] The alkyl group bonded to position 1 of the pyridinium-based cation preferably has 1 to 7 carbon atoms, more preferably 1 to 6 carbon atoms, particularly preferably 1 to 5 carbon atoms, and even more preferably 1 to 4 carbon atoms. Furthermore, the alkyl group bonded to positions other than position 1 of the pyridinium-based cation preferably has 1 to 3 carbon atoms, particularly preferably 1 to 2 carbon atoms, and even more preferably 1 carbon atom. This facilitates the production of a pressure-sensitive adhesive that readily satisfies the physical properties described below, and provides superior antistatic properties and metal corrosion resistance. Among the above compounds, the 1-butyl-3-methylpyridinium cation is particularly preferred.

[0041] Examples of imidazolium cations include 1-alkyl-3-alkylimidazolium cations, 1,2-dialkyl-3-alkylimidazolium cations, and 1-alkyl-2,3-dialkylimidazolium cations, and among these, 1-alkyl-3-alkylimidazolium cations are preferred.

[0042] The alkyl group bonded to the 1-position of the imidazolium-based cation preferably has 1 to 7 carbon atoms, more preferably 1 to 6 carbon atoms, particularly preferably 1 to 5 carbon atoms, and even more preferably 1 to 4 carbon atoms. The alkyl group bonded to the 3-position of the imidazolium-based cation preferably has 1 to 4 carbon atoms, particularly preferably 1 to 3 carbon atoms, and even more preferably 1 to 2 carbon atoms. Furthermore, when an alkyl group is bonded to the 2-position of the imidazolium-based cation, the alkyl group preferably has 1 to 3 carbon atoms, particularly preferably 1 to 2 carbon atoms, and even more preferably 1 carbon atom. As a result, a pressure-sensitive adhesive that easily satisfies the physical properties described below can be easily obtained, and the pressure-sensitive adhesive exhibits even better antistatic properties and metal corrosion resistance. Of the above compounds, the 1-methyl-3-ethylimidazolium cation is particularly preferred.

[0043] The content of the antistatic agent in the pressure-sensitive adhesive composition (pressure-sensitive adhesive) according to the present embodiment is preferably 0.1 to 20% by mass, more preferably 0.3 to 15% by mass, particularly preferably 0.6 to 10% by mass, even more preferably 0.8 to 5% by mass, and even more preferably 1 to 4% by mass, most preferably 1.2 to 3% by mass. This makes it easier to obtain a pressure-sensitive adhesive that easily satisfies the physical properties described below, and provides better antistatic properties and metal corrosion resistance.

[0044] The pressure-sensitive adhesive obtained from the pressure-sensitive adhesive composition according to this embodiment may be any of an acrylic pressure-sensitive adhesive, a polyester pressure-sensitive adhesive, a polyurethane pressure-sensitive adhesive, a rubber pressure-sensitive adhesive, a silicone pressure-sensitive adhesive, etc. The pressure-sensitive adhesive may be any of an emulsion type, a solvent type, or a solventless type, and may be any of a cross-linked type or a non-cross-linked type. Among these, an acrylic pressure-sensitive adhesive is preferred because of its excellent adhesive properties, optical properties, etc.

[0045] The acrylic pressure-sensitive adhesive may be an active energy ray-curable one, an active energy ray-non-curable one, a crosslinkable one, a non-crosslinkable one, or a combination thereof. Among them, from the viewpoint of antistatic property development, an active energy ray-non-curable acrylic pressure-sensitive adhesive is preferred, and a crosslinkable active energy ray-non-curable acrylic pressure-sensitive adhesive is particularly preferred.

[0046] The adhesive composition (adhesive) according to this embodiment preferably contains a (meth)acrylic acid ester polymer as the adhesive base in addition to the antistatic agent described above, and preferably further contains a crosslinking agent capable of crosslinking the (meth)acrylic acid ester polymer. Specifically, the adhesive composition according to this embodiment preferably contains a (meth)acrylic acid ester polymer (A), a crosslinking agent (B), and an antistatic agent (C). Hereinafter, this adhesive composition may be referred to as "adhesive composition P." In this specification, "(meth)acrylic acid" refers to both acrylic acid and methacrylic acid. The same applies to other similar terms. Furthermore, "polymer" also includes the concept of "copolymer."

[0047] (1) Components (1-1) (Meth)acrylic Acid Ester Polymer (A) The (meth)acrylic acid ester polymer (A) preferably contains, as monomer units constituting the polymer, a (meth)acrylic acid alkyl ester for exhibiting good adhesiveness and a monomer having a reactive functional group that serves as a crosslinking point (reactive functional group-containing monomer).

[0048] The (meth)acrylic acid alkyl ester preferably includes a (meth)acrylic acid alkyl ester in which the carbon number of the alkyl group is 1 to 20. The alkyl group is preferably linear or branched.

[0049] Examples of (meth)acrylic acid alkyl esters having an alkyl group containing 1 to 20 carbon atoms include methyl (meth)acrylate, ethyl (meth)acrylate, propyl (meth)acrylate, n-butyl (meth)acrylate, n-pentyl (meth)acrylate, n-hexyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, isooctyl (meth)acrylate, n-decyl (meth)acrylate, n-dodecyl (meth)acrylate, myristyl (meth)acrylate, palmityl (meth)acrylate, and stearyl (meth)acrylate. Among these, from the viewpoint of adhesive strength, (meth)acrylic acid esters having an alkyl group containing 1 to 10 carbon atoms are preferred, and (meth)acrylic acid esters having an alkyl group containing 1 to 8 carbon atoms are particularly preferred. Specifically, methyl (meth)acrylate, n-butyl (meth)acrylate, isooctyl (meth)acrylate, or 2-ethylhexyl (meth)acrylate are preferred, with methyl acrylate or n-butyl acrylate being particularly preferred. These may be used alone or in combination of two or more.

[0050] The (meth)acrylic acid alkyl ester is also preferably a biomass monomer produced from a biomass-derived material, which allows the resulting PSA to contain a biomass-derived material and is therefore environmentally friendly.

[0051] The (meth)acrylic acid ester polymer (A) preferably contains 50 to 99 mass %, more preferably 60 to 98 mass %, and particularly preferably 70 to 97 mass %, of (meth)acrylic acid alkyl esters having an alkyl group containing 1 to 20 carbon atoms as monomer units constituting the polymer. When a carboxy group-containing monomer is used as the reactive functional group-containing monomer, the (meth)acrylic acid alkyl ester is preferably contained in an amount of 80 to 95 mass %. This facilitates the production of a pressure-sensitive adhesive that readily satisfies the physical properties described below, and allows the antistatic properties and metal corrosion resistance provided by the antistatic agent (C) to be effectively exhibited.

[0052] The (meth)acrylic acid ester polymer (A) contains a reactive functional group-containing monomer as a monomer unit constituting the polymer, and thus reacts with the crosslinking agent (B) described below via the reactive functional group derived from the reactive functional group-containing monomer, thereby forming a crosslinked structure (three-dimensional network structure), and a pressure-sensitive adhesive having the desired cohesive strength is obtained.

[0053] Preferred examples of the reactive functional group-containing monomer contained in the (meth)acrylic acid ester polymer (A) as a monomer unit constituting the polymer include a monomer having a hydroxyl group in the molecule (hydroxyl group-containing monomer), a monomer having a carboxyl group in the molecule (carboxyl group-containing monomer), a monomer having an amino group in the molecule (amino group-containing monomer), etc. These reactive functional group-containing monomers may be used alone or in combination of two or more.

[0054] Among the reactive functional group-containing monomers, hydroxyl group-containing monomers are preferred from the viewpoint of metal corrosion resistance, but since the pressure-sensitive adhesive composition according to the present embodiment contains the antistatic agent described above, good metal corrosion resistance can be obtained even when a carboxyl group-containing monomer is used. The carboxyl group-containing monomer can be used alone, and is also preferably used in combination with a hydroxyl group-containing monomer.

[0055] Examples of hydroxyl group-containing monomers include (meth)acrylic acid hydroxyalkyl esters such as 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, 3-hydroxypropyl (meth)acrylate, 2-hydroxybutyl (meth)acrylate, 3-hydroxybutyl (meth)acrylate, and 4-hydroxybutyl (meth)acrylate. Among these, (meth)acrylic acid hydroxyalkyl esters having a hydroxyalkyl group having 1 to 4 carbon atoms are preferred. Specifically, for example, 2-hydroxyethyl acrylate or 4-hydroxybutyl acrylate are preferred. These may be used alone or in combination of two or more.

[0056] Examples of carboxyl group-containing monomers include ethylenically unsaturated carboxylic acids such as acrylic acid, methacrylic acid, crotonic acid, maleic acid, itaconic acid, and citraconic acid. Among these, acrylic acid or methacrylic acid is preferred from the viewpoint of the adhesive strength of the resulting (meth)acrylic acid ester polymer (A), and acrylic acid is particularly preferred. These may be used alone or in combination of two or more.

[0057] From the viewpoint of cohesive strength, the (meth)acrylic acid ester polymer (A) preferably contains 0.1 to 25% by mass, more preferably 0.4 to 20% by mass, particularly preferably 0.8 to 15% by mass, and even more preferably 1 to 12% by mass of reactive functional group-containing monomers as monomer units constituting the polymer. When only a hydroxyl group-containing monomer is used as the reactive functional group-containing monomer, the content is preferably 1.2 to 10% by mass, more preferably 1.4 to 7% by mass, particularly preferably 1.6 to 4% by mass, and even more preferably 1.8 to 3.5% by mass. When only a carboxyl group-containing monomer is used as the reactive functional group-containing monomer, the content is preferably 2 to 10% by mass, more preferably 3 to 9% by mass, particularly preferably 4 to 8% by mass, and even more preferably 5 to 7% by mass. When a carboxyl group-containing monomer and a hydroxyl group-containing monomer are used in combination as the reactive functional group-containing monomer, the content of the carboxyl group-containing monomer is preferably 0.5 to 10 mass%, particularly preferably 2 to 7 mass%, and the content of the hydroxyl group-containing monomer is preferably 0.01 to 5 mass%, particularly preferably 0.1 to 2 mass%. As a result, a pressure-sensitive adhesive that easily satisfies the physical properties described below can be easily obtained, and the desired cohesive strength can be obtained without deteriorating metal corrosion resistance.

[0058] From the viewpoint of metal corrosion resistance, it is also preferable that the (meth)acrylic acid ester polymer (A) does not contain a carboxy group-containing monomer as a monomer unit constituting the polymer. Here, "containing no carboxy group-containing monomer" means that the polymer does not substantially contain a carboxy group-containing monomer, and in addition to not containing any carboxy group-containing monomer at all, it is acceptable to contain a carboxy group-containing monomer to an extent that does not affect metal corrosion resistance. Specifically, it is acceptable that the (meth)acrylic acid ester polymer (A) contains a carboxy group-containing monomer as a monomer unit in an amount of 0.1 mass% or less, preferably 0.01 mass% or less, and more preferably 0.001 mass% or less.

[0059] It is also preferable that the (meth)acrylic acid ester polymer (A) contains a monomer having an alicyclic structure in the molecule (alicyclic structure-containing monomer) as a monomer unit constituting the polymer. Since the alicyclic structure-containing monomer is bulky, its presence in the polymer is presumed to increase the spacing between polymers, thereby making the resulting adhesive excellent in flexibility. It is also preferable that the alicyclic structure-containing monomer is a biomass monomer produced from a biomass-derived material. Biomass monomers can be preferably used from an environmental perspective.

[0060] The carbon ring of the alicyclic structure in the alicyclic structure-containing monomer may be a saturated structure or may partially contain an unsaturated bond. The alicyclic structure may be a monocyclic alicyclic structure or a polycyclic alicyclic structure (polycyclic structure) such as a bicyclic or tricyclic structure. From the viewpoint of optimizing the distance between the resulting (meth)acrylic acid ester polymer (A) and imparting high stress relaxation properties to the PSA, the alicyclic structure is preferably a polycyclic structure. Furthermore, in consideration of the compatibility of the (meth)acrylic acid ester polymer (A) with other components, the polycyclic structure is particularly preferably a bicyclic to tetracyclic structure. Similarly, from the viewpoint of imparting stress relaxation properties and compatibility, the number of carbon atoms in the alicyclic structure (meaning the total number of carbon atoms in the ring, or the total number of carbon atoms in the case where multiple rings are present independently) is preferably 5 to 15, and particularly preferably 7 to 10.

[0061] Specific examples of the alicyclic structure-containing monomer include cyclohexyl (meth)acrylate, dicyclopentanyl (meth)acrylate, adamantyl (meth)acrylate, isobornyl (meth)acrylate, dicyclopentenyl (meth)acrylate, and dicyclopentenyloxyethyl (meth)acrylate. Among these, dicyclopentanyl (meth)acrylate (alicyclic structure carbon number: 10), adamantyl (meth)acrylate (alicyclic structure carbon number: 10), or isobornyl (meth)acrylate (alicyclic structure carbon number: 7) are preferred, as they exhibit superior conformability to uneven surfaces. Isobornyl (meth)acrylate is particularly preferred, and isobornyl acrylate is even more preferred. These may be used alone or in combination of two or more.

[0062] When the (meth)acrylic acid ester polymer (A) contains an alicyclic structure-containing monomer as a monomer unit constituting the polymer, the content thereof is preferably 0.1 to 24 mass%, more preferably 0.5 to 18 mass%, particularly preferably 1 to 12 mass%, and even more preferably 3 to 8 mass%. This makes it easy to obtain a PSA that easily satisfies the physical properties described below, and can obtain a PSA that exhibits desired cohesion and adhesiveness while exhibiting metal corrosion resistance.

[0063] The (meth)acrylic acid ester polymer (A) preferably contains a monomer having an aromatic ring in the molecule (aromatic ring-containing monomer) as a monomer unit constituting the polymer. This allows the pressure-sensitive adhesive to relieve stress when stress is generated due to shrinkage of an optical component such as a polarizing plate under heat-resistant conditions or moist heat-resistant conditions, thereby suppressing light leakage. It is also preferable that the aromatic ring-containing monomer is a biomass monomer produced from a biomass-derived material. Biomass monomers can be used preferably from an environmental perspective.

[0064] Examples of aromatic ring-containing monomers include monomers containing one or more aromatic rings, monomers having a polycyclic aromatic skeleton, etc. Among them, aromatic ring-containing monomers containing one aromatic ring are preferred from the viewpoint of being able to obtain a high molecular weight substance without gelation and being able to easily obtain a pressure-sensitive adhesive that easily exhibits desired cohesive strength and optical properties.

[0065] Examples of aromatic ring-containing monomers containing one aromatic ring include phenyl (meth)acrylate, 2-phenylethyl (meth)acrylate, benzyl (meth)acrylate, 2-phenoxyethyl (meth)acrylate, phenoxybutyl (meth)acrylate, styryl (meth)acrylate, phenoxydiethylene glycol (meth)acrylate, and phenoxypolyethylene glycol (meth)acrylate. Among these, 2-phenylethyl (meth)acrylate is preferred, and 2-phenylethyl acrylate is particularly preferred. These may be used alone or in combination of two or more.

[0066] When the (meth)acrylic acid ester polymer (A) contains an aromatic ring-containing monomer as a monomer unit constituting the polymer, the content thereof is preferably 1 to 35 mass%, more preferably 6 to 30 mass%, particularly preferably 12 to 26 mass%, and even more preferably 16 to 22 mass%. This makes it easy to obtain a PSA that easily satisfies the physical properties described below, and can obtain a PSA that exhibits desired cohesion and adhesion while exhibiting metal corrosion resistance.

[0067] The (meth)acrylic acid ester polymer (A) may contain other monomers as monomer units constituting the polymer, if desired. As the other monomer, a monomer not containing a reactive functional group is preferred so as not to inhibit the above-described action of the reactive functional group-containing monomer. Examples of such monomers include non-reactive nitrogen atom-containing monomers such as N-acryloylmorpholine and N-vinyl-2-pyrrolidone, (meth)acrylic acid alkoxyalkyl esters such as methoxyethyl (meth)acrylate and ethoxyethyl (meth)acrylate, vinyl acetate, and styrene. These may be used alone or in combination of two or more.

[0068] The polymerization mode of the (meth)acrylic acid ester polymer (A) may be a random copolymer or a block copolymer.

[0069] The weight-average molecular weight of the (meth)acrylic acid ester polymer (A) is preferably 500,000 to 3,000,000, more preferably 700,000 to 2,800,000, particularly preferably 1,000,000 to 2,500,000, even more preferably 1,300,000 to 2,200,000, and most preferably 1,450,000 to 2,100,000. This improves the compatibility between the (meth)acrylic acid ester polymer (A) (or its crosslinked form) and the antistatic agent (C), resulting in superior antistatic properties and metal corrosion resistance. Furthermore, even if stress is generated due to the shrinkage of optical components such as polarizing plates when placed under heat-resistant or moist heat-resistant conditions, the polymer exhibits cohesive strength sufficient to withstand the stress and suppress light leakage. The weight-average molecular weight of the polymer in this specification is a value measured by gel permeation chromatography (GPC) in terms of standard polystyrene.

[0070] In the pressure-sensitive adhesive composition P, the (meth)acrylic acid ester polymer (A) may be used alone or in combination of two or more.

[0071] The content of the (meth)acrylic acid ester polymer (A) in the pressure-sensitive adhesive composition P according to this embodiment is preferably 80 to 99.9 mass%, more preferably 85 to 99.8 mass%, particularly preferably 90 to 99.5 mass%, even more preferably 93 to 99.2 mass%, and most preferably 95 to 99 mass%, which provides good adhesive strength and allows the antistatic property and metal corrosion resistance provided by the antistatic agent (C) to be effectively exhibited.

[0072] (1-2) Crosslinking Agent (B) The crosslinking agent (B) crosslinks the (meth)acrylic acid ester polymer (A) by heating the pressure-sensitive adhesive composition P, and can satisfactorily form a crosslinked structure of a three-dimensional network structure. This allows a pressure-sensitive adhesive having a predetermined cohesive strength to be obtained.

[0073] The crosslinking agent (B) may be any agent that reacts with the reactive functional groups (hydroxyl groups, carboxyl groups, etc.) of the (meth)acrylic acid ester polymer (A), and examples thereof include isocyanate-based crosslinking agents, epoxy-based crosslinking agents, amine-based crosslinking agents, melamine-based crosslinking agents, aziridine-based crosslinking agents, hydrazine-based crosslinking agents, aldehyde-based crosslinking agents, oxazoline-based crosslinking agents, metal alkoxide-based crosslinking agents, metal chelate-based crosslinking agents, metal salt-based crosslinking agents, and ammonium salt-based crosslinking agents. When the (meth)acrylic acid ester polymer (A) contains a hydroxyl group-containing monomer as a monomer unit constituting the polymer, it is preferable to use an isocyanate-based crosslinking agent that has excellent reactivity with hydroxyl groups as the crosslinking agent (B). The crosslinking agent (B) may be used alone or in combination of two or more.

[0074] The isocyanate-based crosslinking agent contains at least a polyisocyanate compound. Examples of polyisocyanate compounds include aromatic polyisocyanates such as tolylene diisocyanate, diphenylmethane diisocyanate, and xylylene diisocyanate; aliphatic polyisocyanates such as hexamethylene diisocyanate; alicyclic polyisocyanates such as isophorone diisocyanate and hydrogenated diphenylmethane diisocyanate; and biuret and isocyanurate forms thereof, as well as adducts thereof that are reaction products with low-molecular-weight active hydrogen-containing compounds such as ethylene glycol, propylene glycol, neopentyl glycol, trimethylolpropane, and castor oil. Among these, trimethylolpropane-modified aromatic polyisocyanates, particularly trimethylolpropane-modified tolylene diisocyanate or trimethylolpropane-modified xylylene diisocyanate, are preferred from the viewpoint of reactivity with hydroxyl groups.

[0075] The content of the crosslinking agent (B) in the pressure-sensitive adhesive composition P is preferably 0.01 to 3.0 parts by mass, more preferably 0.02 to 2.5 parts by mass, particularly preferably 0.04 to 2.0 parts by mass, even more preferably 0.06 to 1.5 parts by mass, and of these, preferably 0.08 to 1 part by mass, and most preferably 0.1 to 0.5 parts by mass, relative to 100 parts by mass of the (meth)acrylic acid ester polymer (A), from the viewpoint of cohesive strength. This makes it easier to obtain a pressure-sensitive adhesive that easily satisfies the physical properties described below.

[0076] (1-3) Antistatic Agent (C) Preferred examples of the antistatic agent (C) include the antistatic agent (C1) and the antistatic agent (C2) described above. The content (% by mass) of the antistatic agent (C) in the pressure-sensitive adhesive composition P is as described above. The amount of the antistatic agent (C) blended per 100 parts by mass of the (meth)acrylic acid ester polymer (A) is preferably 0.1 to 20 parts by mass, more preferably 0.3 to 15 parts by mass, particularly preferably 0.6 to 10 parts by mass, and even more preferably 0.8 to 5 parts by mass, with 1 to 4 parts by mass being preferred and 1.2 to 3 parts by mass being most preferred. This makes it easier to obtain a pressure-sensitive adhesive that easily satisfies the physical properties described below, and can exhibit better antistatic properties and metal corrosion resistance.

[0077] (1-4) Silane Coupling Agent (D) The pressure-sensitive adhesive composition P preferably further contains a silane coupling agent (D). This improves the adhesion of the resulting pressure-sensitive adhesive to a glass member when the adherend is a glass member. Even when the adherend is a plastic plate, the resulting pressure-sensitive adhesive improves the adhesion to the plastic plate. Furthermore, the pressure-sensitive adhesive also has excellent adhesion to metal members, which tends to contribute to metal corrosion resistance.

[0078] The silane coupling agent (D) is preferably an organosilicon compound having at least one alkoxysilyl group in the molecule, which has good compatibility with the (meth)acrylic acid ester polymer (A) and the antistatic agent (C), and has optical transparency.

[0079] Examples of the silane coupling agent (D) include polymerizable unsaturated group-containing silicon compounds such as vinyltrimethoxysilane, vinyltriethoxysilane, and methacryloxypropyltrimethoxysilane; silicon compounds having an epoxy structure such as 3-glycidoxypropyltrimethoxysilane, 3-glycidoxypropylmethyldiethoxysilane, and 2-(3,4-epoxycyclohexyl)ethyltrimethoxysilane; mercaptopropyltrimethoxysilane, 3-mercaptopropyltriethoxysilane, and 3-mercaptopropyldimethoxymethylsilane; Examples of such compounds include capryl group-containing silicon compounds, amino group-containing silicon compounds such as 3-aminopropyltrimethoxysilane, N-(2-aminoethyl)-3-aminopropyltrimethoxysilane and N-(2-aminoethyl)-3-aminopropylmethyldimethoxysilane, 3-chloropropyltrimethoxysilane and 3-isocyanatepropyltriethoxysilane, and condensates of at least one of these compounds with alkyl group-containing silicon compounds such as methyltriethoxysilane, ethyltriethoxysilane, methyltrimethoxysilane and ethyltrimethoxysilane. These compounds may be used alone or in combination of two or more.

[0080] The silane coupling agent (D) is particularly preferably one having an acid anhydride group as an organic functional group. When a silane coupling agent having an acid anhydride group as an organic functional group is used, a high adhesive strength can be obtained even when the pressure-sensitive adhesive layer is thin. This adhesive strength increasing effect is particularly exhibited more effectively when combined with an antistatic agent (C2).

[0081] The silane coupling agent (D) having an acid anhydride group as an organic functional group is preferably a silane compound represented by the following general formula (I). (In the formula, R represents a hydrocarbon group having 1 to 6 carbon atoms, n represents an integer of 2 to 8, m represents an integer of 1 to 3, l represents an integer of 1 to 3, k represents an integer of 0 to 2, and k + l + m = 4.)

[0082] The hydrocarbon group of R is preferably an alkyl group, a vinyl group, or an aryl group, and particularly preferably an alkyl group. The number of carbon atoms in the hydrocarbon group of R is preferably 1 to 5, more preferably 1 to 4, particularly preferably 1 to 3, further preferably 1 to 2, and most preferably 1. n is preferably 1 to 6, more preferably 2 to 5, particularly preferably 2 to 4, further preferably 2 to 3, and most preferably 3. m is preferably 1 to 2, and most preferably 1. l is preferably 1 to 3, more preferably 2 to 3, and most preferably 3. k is preferably 0 to 2, more preferably 0 to 1, and most preferably 0.

[0083] Specific examples of the silane coupling agent represented by general formula (I) include 3-trimethoxysilylethyl succinate anhydride represented by the following formula (II) and 3-trimethoxysilylpropyl succinate anhydride represented by the following formula (III). (III)

[0084] The content of the silane coupling agent (D) in the pressure-sensitive adhesive composition P is preferably 0.01 to 3 parts by mass, more preferably 0.04 to 2 parts by mass, particularly preferably 0.08 to 1 part by mass, even more preferably 0.12 to 0.7 parts by mass, and especially preferably 0.15 to 0.4 parts by mass, relative to 100 parts by mass of the (meth)acrylic acid ester polymer (A). This makes the effect of the silane coupling agent (D) even more excellent.

[0085] (1-5) Various Additives The pressure-sensitive adhesive composition P may contain, if desired, various additives commonly used in acrylic pressure-sensitive adhesives, such as ultraviolet absorbers, tackifiers, antioxidants, colorants, light diffusing agents, infrared absorbers, rust inhibitors, light stabilizers, softeners, fillers, and refractive index adjusters.

[0086] (2) Production of adhesive composition The adhesive composition P can be produced by producing a (meth)acrylic acid ester polymer (A), mixing the obtained (meth)acrylic acid ester polymer (A) with a crosslinking agent (B) and an antistatic agent (C), and, if desired, adding a silane coupling agent (D), an additive, etc.

[0087] The (meth)acrylic acid ester polymer (A) can be produced by polymerizing a mixture of monomers constituting the polymer by a conventional radical polymerization method. The polymerization of the (meth)acrylic acid ester polymer (A) is preferably carried out by a solution polymerization method, using a polymerization initiator as desired. However, the present invention is not limited to this, and the polymerization may be carried out without a solvent. Examples of polymerization solvents include ethyl acetate, n-butyl acetate, isobutyl acetate, toluene, acetone, hexane, and methyl ethyl ketone, and two or more of them may be used in combination.

[0088] Examples of the polymerization initiator include azo compounds, organic peroxides, etc., and two or more of them may be used in combination. In the polymerization step, the weight average molecular weight of the resulting polymer can be adjusted by adding a chain transfer agent such as 2-mercaptoethanol.

[0089] Once the (meth)acrylic acid ester polymer (A) is obtained, a crosslinking agent (B), an antistatic agent (C), and, if desired, a silane coupling agent (D), an additive, a dilution solvent, etc. are added to the solution of the (meth)acrylic acid ester polymer (A) and mixed thoroughly to obtain a solvent-diluted adhesive composition P (coating solution). Note that, when a solid component is used for any of the above components, or when precipitation occurs when the component is mixed with other components in an undiluted state, the component may be dissolved or diluted alone in a dilution solvent before being mixed with other components.

[0090] Examples of the dilution solvent include aliphatic hydrocarbons such as hexane, heptane, and cyclohexane; aromatic hydrocarbons such as toluene and xylene; halogenated hydrocarbons such as methylene chloride and ethylene chloride; alcohols such as methanol, ethanol, propanol, butanol, and 1-methoxy-2-propanol; ketones such as acetone, methyl ethyl ketone, 2-pentanone, isophorone, and cyclohexanone; esters such as ethyl acetate and butyl acetate; and cellosolve-based solvents such as ethyl cellosolve.

[0091] The concentration and viscosity of the coating solution prepared in this manner are not particularly limited as long as they are within a range that allows coating, and can be appropriately selected depending on the situation. For example, the pressure-sensitive adhesive composition P is diluted so that the concentration is 10 to 60 mass %. Note that the addition of a dilution solvent or the like is not a necessary condition for obtaining the coating solution, and as long as the pressure-sensitive adhesive composition P has a viscosity that allows coating, the addition of a dilution solvent is not necessary. In this case, the pressure-sensitive adhesive composition P becomes a coating solution in which the polymerization solvent for the (meth)acrylic acid ester polymer (A) is used as the dilution solvent.

[0092] [Adhesive] An adhesive according to one embodiment of the present invention is obtained by crosslinking the above-mentioned adhesive composition, preferably the adhesive composition P. Crosslinking of the adhesive composition P can be carried out by a heat treatment. This heat treatment can also serve as a drying treatment for volatilizing the diluent solvent of the adhesive composition P.

[0093] When heat treatment is performed, the heating temperature is preferably 50 to 150°C, and particularly preferably 70 to 120°C. The heating time is preferably 30 seconds to 10 minutes, and particularly preferably 50 seconds to 2 minutes. After the heat treatment, a curing period of about 1 to 2 weeks may be provided at room temperature (e.g., 23°C, 50% RH), if necessary. If this curing period is required, the pressure-sensitive adhesive layer is formed after the curing period has elapsed; if no curing period is required, the pressure-sensitive adhesive layer is formed after the heat treatment has ended.

[0094] The pressure-sensitive adhesive obtained by crosslinking the pressure-sensitive adhesive composition P exhibits excellent antistatic properties due to the action of the antistatic agent (C), and can also inhibit corrosion of metal members that come into contact with it.

[0095] The gel fraction of the pressure-sensitive adhesive according to this embodiment is preferably 40 to 99%, more preferably 50 to 95%, particularly preferably 60 to 92%, and even more preferably 65 to 90%. This allows for good cohesive strength to be exhibited. Note that when the pressure-sensitive adhesive according to this embodiment is an acrylic pressure-sensitive adhesive containing a (meth)acrylic acid ester polymer (A) and contains an aromatic ring-containing monomer or an alicyclic structure-containing monomer as a monomer unit constituting the polymer, the gel fraction tends to be preferably 66 to 80%, more preferably 67 to 75%, and particularly preferably 68 to 73%. On the other hand, when the pressure-sensitive adhesive according to the present embodiment is an acrylic pressure-sensitive adhesive containing a (meth)acrylic acid ester polymer (A) and does not contain an aromatic ring-containing monomer or an alicyclic structure-containing monomer as a monomer unit constituting the polymer, the gel fraction is preferably 70 to 88%, particularly preferably 75 to 87%; further, when a hydroxyl group-containing monomer is contained, a gel fraction of 80 to 86% tends to be preferable, and when a carboxy group-containing monomer is contained, a gel fraction of 76 to 80% tends to be preferable.

[0096] [Adhesive Sheet] An adhesive sheet according to one embodiment of the present invention comprises an adhesive layer made of the adhesive according to the embodiment described above.

[0097] (1) Physical Properties (1-1) Thickness The thickness of the pressure-sensitive adhesive layer of the pressure-sensitive adhesive sheet according to this embodiment (measured in accordance with JIS K7130) is preferably 1 to 50 μm, more preferably 3 to 40 μm, particularly preferably 5 to 30 μm, even more preferably 8 to 25 μm, and of these, preferably 10 to 20 μm, from the viewpoint of antistatic properties and metal corrosion resistance.

[0098] (1-2) Haze Value The haze value of the pressure-sensitive adhesive layer of the pressure-sensitive adhesive sheet according to this embodiment is preferably 2.0% or less, more preferably 1.8% or less, particularly preferably 1.5% or less, even more preferably 1.2% or less, and most preferably 1.0% or less. This provides very high transparency and makes the sheet suitable for optical applications (displays). In this embodiment, the compatibility between the (meth)acrylic acid ester polymer (A) (or its crosslinked form) and the antistatic agent (C) is good, so that the above-mentioned low haze value can be achieved. The lower limit of the haze value of the pressure-sensitive adhesive layer is not particularly limited. The lower limit may be 0%. Here, the haze value in this specification is a value measured in accordance with JIS K7136:2000.

[0099] (1-3) Total Light Transmittance The total light transmittance of the pressure-sensitive adhesive layer of the pressure-sensitive adhesive sheet according to this embodiment is preferably 80% or more, and particularly preferably 90% or more. This provides very high transparency and makes the sheet suitable for optical applications (displays). In this embodiment, the compatibility between the (meth)acrylic acid ester polymer (A) (or a crosslinked product thereof) and the antistatic agent (C) is good, so that the high total light transmittance described above can be achieved. The upper limit of the total light transmittance of the pressure-sensitive adhesive layer is not particularly limited and may be 100%. Here, the total light transmittance in this specification is a value measured in accordance with JIS K7361-1:1997.

[0100] (1-4) Surface Resistivity When a voltage of 100 V is applied to the exposed surface of the pressure-sensitive adhesive layer of the pressure-sensitive adhesive sheet according to this embodiment (pressure-sensitive adhesive layer / release sheet) for 30 seconds in an environment of 23°C and 50% RH, the surface resistivity of the exposed surface of the pressure-sensitive adhesive layer is 1.2 × 10 as the upper limit. 12 It is preferably Ω / sq or less, and 1×10 12 More preferably, it is 5×10 Ω / sq or less. 11 It is more preferable that the resistance is Ω / sq or less, and particularly 3×10 11 It is preferable that the resistance is Ω / sq or less, and more preferably 1.3×10 11 It is preferably Ω / sq or less, and more preferably 1×10 11The surface resistivity is preferably Ω / sq or less. This allows the resulting display to exhibit excellent antistatic properties. The lower limit of the surface resistivity is not particularly limited, but is usually 1×10 7 It is preferably Ω / sq or more, and particularly 1×10 8 It is preferable that the resistance is Ω / sq or more, and more preferably 1×10 9 The surface resistivity of the pressure-sensitive adhesive layer is preferably Ω / sq or more. The surface resistivity of the pressure-sensitive adhesive layer is measured in accordance with JIS K6911:2006, specifically as shown in the test examples described later.

[0101] (1-5) Peeling Electrostatic Potential When the release sheet of the pressure-sensitive adhesive sheet according to this embodiment is manually peeled from the pressure-sensitive adhesive layer at a peeling speed of 10 m / min and a peeling angle of 180° under an environment of 23°C and 50% RH, the electrostatic potential (peeling electrostatic potential) measured 5 seconds after peeling at a position 2.0 cm from the exposed surface of the pressure-sensitive adhesive layer is preferably 0.3 kV or less, more preferably 0.2 kV or less, particularly preferably 0.1 kV or less, and even more preferably 0.05 kV or less, and even more preferably 0.04 kV or less, and most preferably 0.03 kV or less. This makes it difficult for static electricity to be generated when the release sheet is peeled from the pressure-sensitive adhesive layer, effectively preventing dust and dirt in the air from adhering to the adherend or substrate due to static electricity. The lower limit of the peeling electrostatic potential is not particularly limited, but is preferably 0 kV. Details of the method for measuring the peeling electrostatic potential are as shown in the test examples described below.

[0102] (1-6) Adhesive Strength The adhesive strength of the pressure-sensitive adhesive sheet according to this embodiment to alkali-free glass is preferably 1 to 40 N / 25 mm, more preferably 1.5 to 35 N / 25 mm, particularly preferably 2 to 30 N / 25 mm, and even more preferably 2.5 to 25 N / 25 mm. This allows for good fixation to metal members and other optical members, and provides excellent reworkability. From this perspective, when the pressure-sensitive adhesive according to this embodiment is an acrylic pressure-sensitive adhesive containing a (meth)acrylic acid ester polymer (A), and the polymer contains a reactive group-containing monomer as a monomer unit, and the reactive group-containing monomer is a hydroxyl group-containing monomer, the adhesive strength tends to be preferably 2.5 to 20 N / 25 mm, particularly preferably 5 to 18 N / 25 mm. When the pressure-sensitive adhesive sheet does not contain an aromatic ring-containing monomer or an alicyclic structure-containing monomer, the adhesive strength tends to be preferably 8 to 16 N / 25 mm. On the other hand, when the reactive group-containing monomer is a carboxy group-containing monomer, the strength tends to be preferably 6 to 8 N / 25 mm.

[0103] Here, the adhesive strength basically refers to the adhesive strength measured by the 180-degree peeling method in accordance with JIS Z0237:2009, and the specific test method is as shown in the test examples described below.

[0104] (1-7) Haze Value Change When measuring the adhesive strength of the pressure-sensitive adhesive sheet according to this embodiment to alkali-free glass, the haze value of the alkali-free glass after measuring the adhesive strength (after peeling off the pressure-sensitive adhesive sheet) minus the haze value of the alkali-free glass before laminating the pressure-sensitive adhesive sheet (haze value change) is preferably 2.2 points or less, more preferably 1.8 points or less, particularly preferably 1.2 points or less, and even more preferably 0.8 points or less. This indicates that there is little component migration or residue from the pressure-sensitive adhesive to the adherend, and can serve as an indicator for finding an antistatic agent (C) that will produce a pressure-sensitive adhesive with little component migration or residue to the adherend. Using a pressure-sensitive adhesive with little component migration or residue not only effectively suppresses changes in the properties of the adherend surface during rework, but also tends to effectively suppress metal corrosion due to the components. The lower limit of the haze value change is most preferably 0 points, but may be 0.05 points or more, preferably 0.1 points or more. The method for calculating the amount of change in haze value will be described later.

[0105] (1-8) Change in Total Light Transmittance An aluminum-deposited polyethylene terephthalate film (total thickness: 25 μm, aluminum layer thickness: 50 nm) fixed to a glass plate with a transparent, general-purpose acrylic adhesive layer (with the aluminum-deposited surface exposed) was used as an adherend, and a laminate of the adhesive layer of this embodiment and a polyethylene terephthalate film (thickness: 50 μm) was attached to the aluminum-deposited surface of the adherend with the adhesive layer to form a sample. This sample was placed in a high-temperature, high-humidity environment of 85°C and 85% RH for 250 hours or 500 hours, and the total light transmittance (%) was measured before and after the exposure. The total light transmittance (%) before the exposure to the high-temperature, high-humidity environment was subtracted from the total light transmittance (%) after the exposure to the high-temperature, high-humidity environment to form the change in total light transmittance (points). In this specification, "relative humidity α%" may also be referred to as "α% RH" (RH; Relative humidity).

[0106] The change in total light transmittance of the pressure-sensitive adhesive sheet according to this embodiment is preferably 10 points or less, more preferably 6 points or less, particularly preferably 3 points or less, and even more preferably 1 point or less. This means that metal corrosion is effectively suppressed. On the other hand, the lower limit of the change in total light transmittance is most preferably 0 points, but may be 0.05 points or more, preferably 0.1 points or more.

[0107] Based on the change in total light transmittance measured by the above test method, it is possible to judge the metal corrosion resistance not only of aluminum but also of other metals such as ITO, copper, silver, etc.

[0108] (2) Specific Configuration of the Pressure-Sensitive Adhesive Sheet A specific configuration as an example of the pressure-sensitive adhesive sheet according to the present embodiment is shown in Figure 1. As shown in Figure 1, the pressure-sensitive adhesive sheet 1 according to one embodiment is composed of two release sheets 12a, 12b and a pressure-sensitive adhesive layer 11 sandwiched between the two release sheets 12a, 12b so as to be in contact with the release surfaces of the two release sheets 12a, 12b. Note that the release surface of the release sheet in this specification refers to the surface of the release sheet that has releasability, and includes both a surface that has been subjected to a release treatment and a surface that exhibits releasability even without being subjected to a release treatment.

[0109] The pressure-sensitive adhesive layer 11 is the pressure-sensitive adhesive layer in the pressure-sensitive adhesive sheet according to the above-described embodiment.

[0110] The release sheets 12a and 12b protect the adhesive layer until the adhesive sheet is used, and are peeled off when the adhesive sheet (adhesive layer) is to be used. In the adhesive sheet 1 according to this embodiment, one or both of the release sheets 12a and 12b are not necessarily required.

[0111] Examples of materials that can be used as the release sheets 12a and 12b include polyethylene films, polypropylene films, polybutene films, polybutadiene films, polymethylpentene films, polyvinyl chloride films, vinyl chloride copolymer films, polyethylene terephthalate films, polyethylene naphthalate films, polybutylene terephthalate films, polyurethane films, ethylene vinyl acetate films, ionomer resin films, ethylene-(meth)acrylic acid copolymer films, ethylene-(meth)acrylic acid ester polymer films, polystyrene films, polycarbonate films, polyimide films, and fluororesin films. Crosslinked films of these materials can also be used. Furthermore, laminated films of these materials may also be used. From the perspective of the SDGs, the material constituting the release sheets may be a material with a high biomass content, a recyclable or reusable material, or a recycled or reused material.

[0112] It is preferable that a release treatment be performed on the release surfaces of the release sheets 12a and 12b (particularly the surfaces that come into contact with the pressure-sensitive adhesive layer 11). Examples of release agents used for the release treatment include alkyd-based, silicone-based, fluorine-based, unsaturated polyester-based, polyolefin-based, and wax-based release agents.

[0113] There is no particular limitation on the thickness of the release sheets 12a and 12b, but it is usually about 20 to 150 μm.

[0114] From the viewpoint of handling, it is preferable that one of the two release sheets 12a, 12b be a heavy release type release sheet with a large release force and the other be a light release type release sheet with a small release force.

[0115] (3) Production of Pressure-Sensitive Adhesive Sheet In one example of producing the pressure-sensitive adhesive sheet 1, a coating solution of the pressure-sensitive adhesive composition P is applied to the release surface of one release sheet 12a (or 12b), a heat treatment is performed to thermally crosslink the pressure-sensitive adhesive composition P, and a coating layer is formed. After that, the release surface of the other release sheet 12b (or 12a) is superimposed on the coating layer. If a curing period is required, a curing period is allowed, but if no curing period is required, the coating layer becomes the pressure-sensitive adhesive layer 11 as is. The pressure-sensitive adhesive sheet 1 is obtained by the above steps. The conditions for the heat treatment and curing are as described above.

[0116] The coating solution of the adhesive composition P can be applied by, for example, bar coating, knife coating, roll coating, blade coating, die coating, gravure coating, or the like.

[0117] (4) Use of the adhesive sheet The adhesive sheet 1 according to this embodiment can be used to bond a metal member to a non-metal member, a metal member to a metal part, or a non-metal member to a non-metal member. The metal member and the non-metal member are preferably optical members, and particularly preferably members constituting a display (display member components). Specifically, the adhesive sheet 1 according to this embodiment can be preferably used to bond an optical member such as a polarizing plate to a transparent conductive film, a transparent conductive film to a desired optical member, or an optical member such as a polarizing plate to a desired optical member.

[0118] The pressure-sensitive adhesive sheet 1 according to this embodiment has both antistatic properties and metal corrosion resistance, and therefore can be used as a pressure-sensitive adhesive sheet that is used in contact with metal members, or as a pressure-sensitive adhesive sheet that is used to laminate optical members such as polarizing plates, etc. Therefore, according to the pressure-sensitive adhesive sheet 1 according to this embodiment, a common pressure-sensitive adhesive sheet can be used even if the application location is different, and the production cost of the target product (for example, an electronic device such as a display) can be reduced.

[0119] [Optical member with pressure-sensitive adhesive layer] An optical member with a pressure-sensitive adhesive layer according to one embodiment of the present invention comprises an optical member and a pressure-sensitive adhesive layer laminated on at least one side of the optical member. A specific configuration of an optical laminate according to this embodiment is shown in FIG. 2. As shown in FIG. 2, an optical member with a pressure-sensitive adhesive layer 2 according to this embodiment comprises an optical member 21, a pressure-sensitive adhesive layer 11 laminated on one side of the optical member 21, and a release sheet 11b laminated on the pressure-sensitive adhesive layer 11 on the side opposite to the optical member 21. This pressure-sensitive adhesive layer 11 is the pressure-sensitive adhesive layer 11 of the pressure-sensitive adhesive sheet 1 described above, and the release sheet 11b is the release sheet 11b of the pressure-sensitive adhesive sheet 1 described above.

[0120] Examples of the optical member 21 include optical films such as polarizing plates, retardation films, brightness enhancement films, viewing angle compensation films, contrast enhancement films, liquid crystal polymer films, diffusion films, semi-transparent reflective films, shatterproof films, transparent conductive films, and electrode-equipped sensor films. A preferred example of a transparent conductive film is an ITO-PET film in which a tin-doped indium oxide (ITO) layer is formed on one side of a polyethylene terephthalate film. Among the above optical members, transparent conductive films and electrode-equipped sensor films are considered to be metal members.

[0121] Examples of polarizing plates include a polarizing plate in which triacetyl cellulose (TAC) films are bonded to both sides of a polyvinyl alcohol (PVA) polarizer as protective films, a polarizing plate in which one of the TAC films is replaced with a cycloolefin polymer film (COP polarizing plate), or a polarizing plate in which a TAC film is bonded to one side of a PVA polarizer as a protective film. The TAC film may or may not be saponified.

[0122] To manufacture the optical element 2 with the adhesive layer, as an example, one of the release sheets 12a of the adhesive sheet 1 described above is peeled off, and the exposed adhesive layer 11 of the adhesive sheet 1 is bonded to one side of the optical element 21.

[0123] The optical element 2 with the adhesive layer according to this embodiment can be used by peeling off the release sheet 12b and attaching the exposed adhesive layer 11 to a desired substrate (optical element, display component, etc.).

[0124] The pressure-sensitive adhesive layer-attached optical member 2 according to this embodiment can be preferably used for manufacturing a display such as a touch panel, for example. Examples of the display include a liquid crystal (LCD) display, a light-emitting diode (LED) display, an organic electroluminescence (organic EL) display, and electronic paper.

[0125] Since the pressure-sensitive adhesive layer 11 has excellent resistance to metal corrosion, when the pressure-sensitive adhesive layer 11 of the optical element 2 with a pressure-sensitive adhesive layer according to this embodiment is attached to a metal element, or when the optical element 2 is a metal element, corrosion of the metal element can be suppressed.

[0126] Furthermore, because the pressure-sensitive adhesive layer 11 has excellent antistatic properties, it can effectively prevent static electricity from being generated, for example, when the release sheet 11b is peeled off from the pressure-sensitive adhesive layer-attached optical member 2 according to this embodiment. This prevents problems caused by static electricity from occurring in internal components such as a display. Specific examples include preventing problems such as deterioration or destruction of electrodes and poor touch panel responsiveness (delays or no response, etc.). Furthermore, there is no risk of disturbances in the alignment of liquid crystal molecules in the liquid crystal cell. Furthermore, it is possible to prevent dust and dirt caused by static electricity from entering the display.

[0127] The above-described embodiments have been described to facilitate understanding of the present invention, and are not intended to limit the present invention. Therefore, each element disclosed in the above embodiments is intended to include all design modifications and equivalents that fall within the technical scope of the present invention.

[0128] For example, one or both of the release sheets 12a and 12b in the pressure-sensitive adhesive sheet 1 may be omitted.

[0129] In this specification, when it is stated that "X to Y" (X and Y are any numbers), it means "X or more and Y or less" unless otherwise specified, and also means "preferably greater than X" or "preferably smaller than Y". Furthermore, when it is stated that "X or more" (X is any number), it means "preferably greater than X" unless otherwise specified, and when it is stated that "Y or less" (Y is any number), it also means "preferably smaller than Y" unless otherwise specified.

[0130] The present invention will be explained in more detail below with reference to examples, but the scope of the present invention is not limited to these examples.

[0131] Example 1 1. Preparation of (meth)acrylic acid ester polymer 77 parts by mass of n-butyl acrylate, 20 parts by mass of methyl acrylate, and 3 parts by mass of 4-hydroxybutyl acrylate were copolymerized by solution polymerization to prepare a (meth)acrylic acid ester polymer (A). The molecular weight of this (meth)acrylic acid ester polymer (A) was measured by the following method, and the weight average molecular weight (Mw) was found to be 1,500,000.

[0132] 2. Preparation of adhesive composition 100 parts by mass (solids equivalent value; the same applies hereinafter) of the (meth)acrylic acid ester polymer (A) obtained in the above step 1, 0.3 parts by mass of an isocyanate-based crosslinking agent (B1; manufactured by Mitsui Chemicals, Inc., product name "Takenate D-110N") as the crosslinking agent (B), 1.5 parts by mass of 1-butyl-3-methylpyridinium bis(fluorosulfonyl)imide (C2-1) as the antistatic agent (C), and 0.2 parts by mass of 2-trimethoxysilylethyl succinate (D1) as the silane coupling agent (D) were mixed, thoroughly stirred, and diluted with methyl ethyl ketone to obtain a coating solution of the adhesive composition P.

[0133] Here, the formulations (solid content equivalent) of the pressure-sensitive adhesive compositions when the (meth)acrylic acid ester polymer (A) is taken as 100 parts by mass (solid content equivalent) are shown in Table 1. Details of the abbreviations and the like shown in Table 1 are as follows. [(Meth)acrylic acid ester polymer (A)] BA: n-butyl acrylate MA: methyl acrylate 4HBA: 4-hydroxybutyl acrylate IBXA: isobornyl acrylate PhEA: 2-phenylethyl acrylate HEA: 2-hydroxyethyl acrylate AA: acrylic acid [Crosslinking agent (B)] B1: isocyanate-based crosslinking agent (manufactured by Mitsui Chemicals, Inc., product name "Takenate D-110N") B2: isocyanate-based crosslinking agent (manufactured by Mitsui Chemicals, Inc., product name "Takenate D-101E") [Antistatic agent (C)] C1: butyl-bishydroxyethyl-methylammonium bis(fluorosulfonyl)imide C2-1: 1-butyl-3-methylpyridinium bis(fluorosulfonyl)imide C2-2: 1-methyl-3-ethylimidazolium bis(fluorosulfonyl)imide C3: 1-decyl-pyridinium bis(fluorosulfonyl)imide C4: 1-octyl-4-methylpyridinium bis(fluorosulfonyl)imide C5: lithium bis(fluorosulfonyl)imide [Silane coupling agent (D)] D1: 3-trimethoxysilylpropyl succinate anhydride D2: mercapto group-containing oligomeric silane coupling agent D3: 3-glycidoxypropylmethyldiethoxysilane

[0134] 3. Production of Pressure-Sensitive Adhesive Sheet The coating solution of the pressure-sensitive adhesive composition obtained in step 2 above was applied using a knife coater to the release-treated surface of a heavy-release type release sheet R1, which was a polyethylene terephthalate film with one side treated with a silicone-based release agent. The coating layer was then heat-treated at 90°C for 1 minute to form a coating layer.

[0135] Next, the coating layer on the release sheet R1 obtained above was bonded to a light-release type release sheet R2, which was a polyethylene terephthalate film with one side treated with a silicone-based release agent, so that the release-treated surface of the release sheet R2 was in contact with the coating layer, and the resulting sheet was cured for 7 days under conditions of 23°C and 50% RH to produce an adhesive sheet consisting of release sheet R2 / adhesive layer (thickness: 15 μm) / release sheet R1.

[0136] The thickness of the pressure-sensitive adhesive layer was measured using a constant pressure thickness measuring device (manufactured by Teclock Corporation, product name "PG-02") in accordance with JIS K 7130. It was also confirmed that the release strength of release sheet R1 was greater than that of release sheet R2 in the obtained pressure-sensitive adhesive sheet.

[0137] Examples 2 to 13, Comparative Examples 1 to 9 Pressure-sensitive adhesive sheets were produced in the same manner as in Example 1, except that the types and amounts of each monomer constituting the (meth)acrylic acid ester polymer (A), the weight average molecular weight (Mw) of the (meth)acrylic acid ester polymer (A), the type and amount of the crosslinking agent (B), the type and amount of the antistatic agent (C), and the type of the silane coupling agent (D) were changed as shown in Table 1.

[0138] The weight average molecular weight (Mw) is a polystyrene-equivalent weight average molecular weight measured by gel permeation chromatography (GPC) under the following conditions (GPC measurement). <Measurement conditions> Measurement device: HLC-8320, manufactured by Tosoh Corporation GPC columns (passed in the following order): TSK gel super H-H, TSK gel super HM-H, TSK gel super H2000, manufactured by Tosoh Corporation Measurement solvent: tetrahydrofuran Measurement temperature: 40°C

[0139] [Test Example 1] (Measurement of gel fraction) The pressure-sensitive adhesive sheets produced in the Examples and Comparative Examples were cut to a size of 80 mm x 80 mm, the pressure-sensitive adhesive layer was wrapped in a polyester mesh (mesh size 200), and the mass was weighed using a precision balance. The mass of the mesh alone was subtracted to calculate the mass of the pressure-sensitive adhesive alone. This mass was designated M1.

[0140] Next, the adhesive wrapped in the polyester mesh was immersed in ethyl acetate at room temperature (23°C) for 24 hours. The adhesive was then removed and dried in an oven at 100°C for 6 hours, and then left in an environment of 23°C and 50% RH for 24 hours. The mass of the adhesive wrapped in the mesh was then weighed using a precision balance, and the mass of the mesh alone was subtracted to calculate the mass of the adhesive alone. This mass was designated M2. The gel fraction (%) was expressed as (M2 / M1) x 100. The results are shown in Table 2.

[0141] [Test Example 2] (Measurement of Surface Resistivity) The release sheet R2 was peeled off from the pressure-sensitive adhesive sheets produced in the Examples and Comparative Examples, and the surface resistivity of the exposed surface of the pressure-sensitive adhesive layer was measured in accordance with JIS K6911:2006. Specifically, using a resistivity meter (manufactured by Mitsubishi Analytech Co., Ltd., product name "Hiresta UP MCP-HT450 type") in an environment of 23°C and 50% RH, a voltage of 100 V was applied for 30 seconds to the pressure-sensitive adhesive sheet (100 mm x 100 mm) from which the release sheet R2 had been peeled off, and the surface resistivity (Ω / sq) of the exposed surface of the pressure-sensitive adhesive layer was then measured. The results are shown in Table 2. Note that the surface resistivity values ​​for Comparative Examples 1, 6, and 9 were too high to be measured (over).

[0142] [Test Example 3] (Measurement of peeling electrification voltage) In an environment of 23°C and 50% RH, the release sheet R2 was manually peeled from the pressure-sensitive adhesive sheets produced in the Examples and Comparative Examples at a peeling speed of 10 m / min and a peeling angle of 180°, and 5 seconds after peeling, the electrostatic potential (peeling electrification voltage; kV) was measured at a position 2.0 cm from the exposed surface of the pressure-sensitive adhesive layer using a static electricity meter (manufactured by Simco Japan, product name "FMX-003"). The results are shown in Table 2.

[0143] [Test Example 4] (Measurement of adhesive strength) The release sheet R2 was peeled off from the pressure-sensitive adhesive sheets produced in the Examples and Comparative Examples, and the exposed pressure-sensitive adhesive layer was attached to an easy-adhesion layer of a polyethylene terephthalate (PET) film (manufactured by Toyobo Co., Ltd., product name "Cosmoshine A4160", thickness: 100 μm) having an easy-adhesion layer, to obtain a release sheet R1 / adhesive layer / PET film laminate. The obtained laminate was cut into a width of 25 mm and a length of 100 mm, and this was used as a sample.

[0144] In an environment of 23°C and 50% RH, the release sheet R1 was peeled off from the above sample, and the exposed adhesive layer was attached to alkali-free glass (manufactured by Corning Incorporated, product name "Eagle XG"), and then pressurized in an autoclave manufactured by Kurihara Manufacturing Co., Ltd. at 0.5 MPa and 50°C for 20 minutes.

[0145] After that, the adhesive strength (N / 25 mm) was measured using a tensile tester (Tensilon, manufactured by Orientec Co., Ltd.) at a peel speed of 300 mm / min and a peel angle of 180 degrees. The measurement was conducted under conditions other than those described here in accordance with JIS Z0237:2009. The results are shown in Table 2.

[0146] [Test Example 5] (Measurement of Haze Value Change) The haze value (%) of the alkali-free glass before the adhesive sheet was attached in the adhesive strength measurement of Test Example 4, and the alkali-free glass after the adhesive strength measurement (after the adhesive sheet was peeled off) was measured using a haze meter (manufactured by Nippon Denshoku Industries Co., Ltd., product name "SH-7000") in accordance with JIS K7136:2000. The haze value change (points) was calculated by subtracting the haze value of the alkali-free glass before the adhesive sheet was attached from the haze value of the alkali-free glass after the adhesive strength measurement. The results are shown in Table 2.

[0147] [Test Example 6] (Measurement of change in total light transmittance / evaluation of metal corrosion resistance) An aluminum-vapor-deposited polyethylene terephthalate (PET) film (manufactured by VDI, total thickness: 25 μm, aluminum layer thickness: 50 nm) was fixed to a soda-lime glass plate (manufactured by AGC) with a transparent general-purpose acrylic adhesive layer (manufactured by Lintec Corporation, product name "NCF-F619", thickness: 25 μm) to serve as an adherend. At this time, the aluminum-vapor-deposited PET film was fixed to the glass plate so that the aluminum-vapor-deposited surface was exposed.

[0148] On the other hand, the release sheet R2 was peeled off from the pressure-sensitive adhesive sheets produced in the Examples and Comparative Examples, and the exposed pressure-sensitive adhesive layer was attached to a PET film (manufactured by Toyobo Co., Ltd., product name "Cosmoshine A4360", thickness: 50 μm) to obtain a laminate consisting of release sheet R1 / pressure-sensitive adhesive layer / PET film. The release sheet R1 was peeled off from this laminate, and the exposed pressure-sensitive adhesive layer was attached to the aluminum-deposited surface of the adherend, to obtain a sample consisting of PET film / pressure-sensitive adhesive layer / aluminum-deposited PET film / general-purpose acrylic pressure-sensitive adhesive layer / glass plate.

[0149] The obtained sample was placed in a high-temperature, high-humidity environment of 85°C and 85% RH for 250 hours and 500 hours, and the total light transmittance (%) was measured before and after. The total light transmittance was measured using a haze meter (manufactured by Nippon Denshoku Industries Co., Ltd., product name "SH-7000") in accordance with JIS K7361-1:1997. The total light transmittance (%) after placement in the high-temperature, high-humidity environment was subtracted from the total light transmittance (%) before placement in the high-temperature, high-humidity environment, and the difference was taken as the change in total light transmittance (points). The results are shown in Table 2.

[0150] The condition of the sample after exposure to the high temperature, high humidity environment was visually inspected, and the metal corrosion resistance was evaluated according to the following criteria. The results are shown in Table 2. ⊚: No change was observed compared to before exposure to the high temperature, high humidity environment. ◯: Metal corrosion was observed only in some areas compared to before exposure to the high temperature, high humidity environment. ×: Metal corrosion was observed overall compared to before exposure to the high temperature, high humidity environment.

[0151]

[0152]

[0153] As can be seen from Table 2, the pressure-sensitive adhesive sheets produced in the examples were excellent in antistatic properties and metal corrosion resistance. Furthermore, pressure-sensitive adhesive sheets using a silane coupling agent (D1) having an acid anhydride group as an organic functional group exhibited high adhesive strength even when the pressure-sensitive adhesive layer was thin, and particularly exhibited even greater adhesive strength when combined with an antistatic agent (C2).

[0154] The pressure-sensitive adhesive sheet of the present invention can be suitably used, for example, in the production of a display, for bonding a transparent conductive film to a desired display component, and for bonding an optical member such as a polarizing plate to a desired display component.

[0155] DESCRIPTION OF SYMBOLS 1... Adhesive sheet 11... Adhesive layer 12a, 12b... Release sheets 2... Optical member with adhesive layer 21... Optical member

Claims

1. An adhesive composition containing an antistatic agent for forming an adhesive used in contact with metal members, characterized in that the antistatic agent is a compound having a hydroxyl group, or the antistatic agent is a compound having a chain hydrocarbon, and the number of carbon atoms in the chain hydrocarbon is 1 or more and 7 or less.

2. The adhesive composition according to claim 1, characterized in that the compound having a hydroxyl group has two or more hydroxyl groups in one molecule.

3. The adhesive composition according to claim 1, wherein the antistatic agent is an ionic compound.

4. The adhesive composition according to claim 3, wherein the ionic compound is a nitrogen-containing onium salt.

5. The adhesive composition according to claim 4, characterized in that the cation constituting the nitrogen-containing onium salt is a quaternary ammonium cation, a pyridinium cation or an imidazolium cation.

6. The adhesive composition according to claim 4, characterized in that the anion constituting the nitrogen-containing onium salt is a sulfonylimide anion.

7. The adhesive composition according to claim 5, characterized in that the quaternary ammonium cation has a hydroxyl group.

8. The adhesive composition according to claim 5, characterized in that the chain hydrocarbon is bonded to a nitrogen cation of the pyridinium-based cation or the imidazolium-based cation.

9. The adhesive composition according to claim 1, characterized in that the adhesive composition contains a (meth)acrylic acid ester polymer as an adhesive base.

10. A pressure-sensitive adhesive obtained by crosslinking the pressure-sensitive adhesive composition according to any one of claims 1 to 9.

11. An adhesive sheet having an adhesive layer made of the adhesive according to claim 10.

12. The adhesive sheet according to claim 11, characterized in that the adhesive sheet comprises two release sheets, and the adhesive layer is sandwiched between the release sheets so as to be in contact with the release surfaces of the two release sheets.

13. When a voltage of 100 V is applied to the exposed surface of the pressure-sensitive adhesive layer laminated on a release sheet for 30 seconds in an environment of 23° C. and relative humidity of 50%, the surface resistivity of the exposed surface of the pressure-sensitive adhesive layer is 1.2×10 12 The pressure-sensitive adhesive sheet according to claim 11, characterized in that it has a resistance of Ω / sq or less.

14. An optical member with an adhesive layer, comprising: an optical member; and an adhesive layer made of the adhesive according to claim 10 and laminated on at least one surface of the optical member.

Citation Information

Patent Citations

  • Pressure-sensitive adhesive composition, pressure-sensitive adhesive sheets, and surface protection film

    JP2005290357A

  • Acrylic adhesive composition

    JP2010525098A

  • Adhesive, adhesive sheet and optical film with adhesive layer

    JP2017014407A