Silicon carbide substrate, silicon carbide epitaxial substrate, and method for producing silicon carbide semiconductor device

By employing a flexible heat insulating material to manage gas flow and maintain a stable temperature, the method effectively reduces carbon-based impurity incorporation in silicon carbide substrates, enhancing their quality and purity.

WO2024241913A1PCT designated stage expired Publication Date: 2024-11-28SUMITOMO ELECTRIC INDUSTRIES LTD
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2024/017407
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-05-19
Filing Date
2024-05-10
Publication Date
2024-11-28

AI Technical Summary

Technical Problem

Existing methods for manufacturing silicon carbide substrates and semiconductor devices struggle to effectively suppress the incorporation of carbon-based impurities, which affects the quality and purity of the materials.

Method used

The method involves using a flexible heat insulating material with appropriate flexibility to reduce gas permeation and prevent the escape of raw material gas from the crucible, thereby minimizing the incorporation of carbon-based impurities during the growth of silicon carbide ingots and substrates. This is achieved by embedding the flexible heat insulating material between molded heat insulating materials to fill gaps and maintain a stable temperature environment.

Benefits of technology

The approach successfully suppresses the incorporation of carbon-based impurities, resulting in silicon carbide substrates with improved purity and quality, as evidenced by controlled Raman spectra and reduced impurity peaks.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JP2024017407_28112024_PF_FP_ABST
    Figure JP2024017407_28112024_PF_FP_ABST
Patent Text Reader

Abstract

In the present invention, if an intensity in a Raman spectrum at a Raman shift of 1300 cm-1 is taken to be a first intensity and the intensity of a maximum peak in a Raman spectrum at a Raman shift of 1300 cm-1 -1800 cm-1 is taken to be a second intensity, the ratio of the second intensity relative to the first intensity is 1.03-1.12.
Need to check novelty before this filing date? Find Prior Art

Description

Silicon carbide substrate, silicon carbide epitaxial substrate, and method for manufacturing silicon carbide semiconductor device

[0001] The present disclosure relates to a silicon carbide substrate, a silicon carbide epitaxial substrate, and a method for manufacturing a silicon carbide semiconductor device. This application claims priority to Japanese Patent Application No. 2023-083127, filed May 19, 2023. The entire contents of this Japanese patent application are incorporated herein by reference.

[0002] Japanese Patent Laid-Open Publication No. 2011-178622 (Patent Document 1) describes an apparatus for producing silicon carbide crystals that has a crucible and a heat insulating material.

[0003] JP 2011-178622 A

[0004] The silicon carbide substrate according to the present disclosure has a Raman shift of 1300 cm -1 The intensity of the Raman spectrum at -1 More than 1800cm -1 When the intensity of the maximum peak in the Raman spectrum in the following range is defined as the second intensity, the ratio of the second intensity to the first intensity is equal to or greater than 1.03 and equal to or less than 1.12.

[0005] FIG. 1 is a plan view schematic diagram showing the configuration of a silicon carbide substrate according to this embodiment. FIG. 2 is a cross-sectional view schematic diagram taken along line II-II in FIG. 1 . FIG. 3 is a cross-sectional view schematic diagram showing the configuration of a Raman spectroscopy apparatus. FIG. 4 is a cross-sectional view schematic diagram showing an example of a Raman spectrum of a silicon carbide substrate. FIG. 5 is a cross-sectional view schematic diagram showing the shape of a first peak in the Raman spectrum of a silicon carbide substrate according to this embodiment. FIG. 6 is a cross-sectional view schematic diagram showing the shape of a second peak and a third peak in the Raman spectrum of a silicon carbide substrate according to this embodiment. FIG. 7A is a cross-sectional view schematic diagram showing the shape of a Raman spectrum of a silicon carbide substrate according to a first modification of this embodiment. FIG. 7B is a cross-sectional view schematic diagram showing the shape of a Raman spectrum of a silicon carbide substrate according to a second modification of this embodiment. FIG. 8 is a cross-sectional view schematic diagram showing the configuration of a first example of an apparatus for producing a silicon carbide ingot. FIG. 9 is a cross-sectional view schematic diagram showing the configuration of a second example of an apparatus for producing a silicon carbide ingot. FIG. 10 is a cross-sectional view schematic diagram showing a step of chemical mechanical polishing a silicon carbide substrate. Fig. 11 is a flow diagram schematically showing a method for manufacturing a silicon carbide semiconductor device according to this embodiment. Fig. 12 is a cross-sectional view schematically showing the configuration of a silicon carbide epitaxial substrate according to this embodiment. Fig. 13 is a cross-sectional view schematically showing the step of forming a body region. Fig. 14 is a cross-sectional view schematically showing the step of forming a source region. Fig. 15 is a cross-sectional view schematically showing the step of forming a trench in a third main surface of a silicon carbide epitaxial layer. Fig. 16 is a cross-sectional view schematically showing the step of forming a gate insulating film. Fig. 17 is a cross-sectional view schematically showing the step of forming a gate electrode and an interlayer insulating film. Fig. 18 is a cross-sectional view schematically showing the configuration of a silicon carbide semiconductor device according to this embodiment.

[0006] [Problem to be Solved by the Present Disclosure] The problem to be solved by the present disclosure is to provide a silicon carbide substrate, a silicon carbide epitaxial substrate, and a method for manufacturing a silicon carbide semiconductor device, which are capable of suppressing the incorporation of carbon-based impurities. [Advantages of the Present Disclosure] According to one aspect of the present disclosure, it is possible to provide a silicon carbide substrate, a silicon carbide epitaxial substrate, and a method for manufacturing a silicon carbide semiconductor device, which are capable of suppressing the incorporation of carbon-based impurities. [Explanation of the Embodiments of the Present Disclosure] (1) The silicon carbide substrate 100 according to the present disclosure has a Raman shift of 1300 cm -1The intensity of the Raman spectrum at -1 More than 1800cm -1 When the intensity of the maximum peak in the Raman spectrum in the following range is defined as the second intensity, the ratio of the second intensity to the first intensity is equal to or greater than 1.03 and equal to or less than 1.12.

[0007] (2) The silicon carbide substrate 100 according to the present disclosure has a Raman shift of 1300 cm -1 More than 1800cm -1 In the following range, the Raman shift at which the intensity of the Raman spectrum is maximum is defined as the first wavenumber, and the Raman shift 30 cm to the wavenumber lower than the first wavenumber is defined as the -1 The separated Raman shift is defined as a second wavenumber, the intensity ratio of the Raman spectrum at the first wavenumber is defined as a first intensity ratio, the intensity ratio of the Raman spectrum at the second wavenumber is defined as a second intensity ratio, the value obtained by subtracting the second intensity ratio from the first intensity ratio is defined as a first intensity ratio difference, and the value obtained by subtracting 1 from the first intensity ratio is defined as a second intensity ratio difference, where the first intensity ratio is less than 1.03 or the first intensity ratio difference is less than 50% of the second intensity ratio difference.

[0008] (3) According to the silicon carbide substrate 100 according to (1) or (2), the Raman shift is 964 cm -1 ±50cm -1 The half-width of the peak in the Raman spectrum within the range of 50 cm -1 It may be the following:

[0009] (4) According to the silicon carbide substrate 100 according to any one of (1) to (3), the Raman shift is 964 cm -1 ±50cm -1 The peak of the Raman spectrum within the range of 1000 to 15000 is defined as the first peak, the Raman shift of the first peak is defined as the third wavenumber, and the Raman shift of the Raman spectrum having half the intensity of the first peak and positioned on the wavenumber side higher than the third wavenumber is defined as the fourth wavenumber. The value obtained by subtracting the third wavenumber from the fourth wavenumber is 20 cm. -1 It may be the following:

[0010] (5) According to silicon carbide substrate 100 according to any one of (1) to (4) above, silicon carbide substrate 100 may have a maximum diameter of 150 mm or more.

[0011] (6) A silicon carbide epitaxial substrate 200 according to the present disclosure includes a silicon carbide substrate 100 according to any one of (1) to (5) above, and a silicon carbide epitaxial layer 20 provided on the silicon carbide substrate 100.

[0012] (7) A method for manufacturing silicon carbide semiconductor device 400 according to the present disclosure includes the steps of preparing silicon carbide epitaxial substrate 200 as described in (6) above, and forming an electrode on silicon carbide epitaxial layer 20. [Details of the Embodiments of the Present Disclosure] Hereinafter, embodiments of the present disclosure will be described with reference to the drawings. Note that identical or corresponding parts in the following drawings are designated by the same reference numerals, and descriptions thereof will not be repeated. In the crystallographic descriptions in this specification, individual orientations are indicated by [ ], collective orientations by < >, individual planes by ( ), and collective planes by {}. Furthermore, for negative indices, a "-" (bar) is placed before the number in crystallography, but in this specification, a negative sign is placed before the number.

[0013] First, the configuration of silicon carbide substrate 100 according to this embodiment will be described. Fig. 1 is a plan view schematically showing the configuration of silicon carbide substrate 100 according to this embodiment. Fig. 2 is a cross-sectional view schematically showing the configuration of silicon carbide substrate 100 along line II-II in Fig. 1.

[0014] 1 and 2 , silicon carbide substrate 100 according to the present embodiment mainly has a first main surface 1, a second main surface 2, and an outer peripheral surface 9. As shown in Fig. 2 , second main surface 2 is located opposite first main surface 1. Outer peripheral surface 9 is continuous with each of the first main surface and the second main surface.

[0015] The polytype of silicon carbide constituting silicon carbide substrate 100 is, for example, 4H. The polytype of silicon carbide constituting silicon carbide substrate 100 may be, for example, 6H. Silicon carbide substrate 100 contains an n-type impurity such as nitrogen (N). The conductivity type of silicon carbide substrate 100 is, for example, n-type. The concentration of the n-type impurity in silicon carbide substrate 100 is, for example, 1×10 17 cm -3 1x10 or more 20 cm -3 The following is the result.

[0016] Maximum diameter W1 of silicon carbide substrate 100 is, for example, 150 mm or more. Maximum diameter W1 of silicon carbide substrate 100 may be, for example, 200 mm or more, or 250 mm or more. Maximum diameter W1 of silicon carbide substrate 100 may be, for example, 300 mm or less. Maximum diameter W1 of silicon carbide substrate 100 is the longest linear distance between two different points on outer peripheral surface 9 when viewed along a line perpendicular to first main surface 1.

[0017] First main surface 1 is, for example, a {0001} plane or a plane inclined at an off angle greater than 0° and equal to or less than 8° with respect to the {0001} plane. The off angle may be, for example, 1° or greater, or 2° or greater. The off angle may be 7° or less, or 6° or less. Specifically, first main surface 1 may be a plane inclined at an off angle greater than 0° and equal to or less than 8° with respect to the (0001) plane or the (0001) plane. First main surface 1 may be a plane inclined at an off angle greater than 0° and equal to or less than 8° with respect to the (000-1) plane or the (000-1) plane. The inclination direction of first main surface 1 is, for example, the <11-20> direction.

[0018] 1 , the outer peripheral surface 9 may have, for example, an orientation flat 7 and an arc-shaped portion 8. The orientation flat 7 extends, for example, along the first direction 101. The arc-shaped portion 8 is continuous with the orientation flat 7.

[0019] The first direction 101 is parallel to the first main surface 1. The first direction 101 is, for example, the <11-20> direction. The first direction 101 may be a direction including a component in the <11-20> direction. The second direction 102 is a direction perpendicular to the first direction 101. The second direction 102 is parallel to the first main surface 1. The second direction 102 is, for example, the <1-100> direction. The second direction 102 may be a direction including a component in the <1-100> direction. The third direction 103 is a direction perpendicular to both the first direction 101 and the second direction 102.

[0020] Next, the configuration of a Raman spectrometer for measuring Raman spectra will be described with reference to Fig. 3, which is a schematic diagram showing the configuration of the Raman spectrometer.

[0021] As shown in FIG. 3 , the Raman spectrometer 30 mainly includes a light source 32, an objective lens 31, a spectrometer 33, a stage 34, a beam splitter 35, and a detector 38. A LabRAM HR-800 manufactured by HORIBA JOBIN YVON can be used as the Raman spectrometer 30. The light source 32 is a YAG (Yttrium Aluminum Garnet) laser. The excitation wavelength of the light source 32 is 532 nm. The laser irradiation intensity is 0.5 mW. The measurement method is backscattering measurement. The magnification of the objective lens 31 is 100x. The diameter of the measurement area is 1 μm. The laser irradiation time is 20 to 180 seconds. The number of integrations is 2. The filter is D1. The grating is 300 gr / mm. The hole is 100.

[0022] Next, a method for measuring a Raman spectrum will be described. First, incident light 36 is emitted from a YAG laser of light source 32. As indicated by a first arrow F1 in FIG. 3 , incident light 36 is reflected by beam splitter 35 and directed toward first main surface 1 of silicon carbide substrate 100. Raman spectroscopy device 30 employs, for example, a confocal optical system. In the confocal optical system, a confocal aperture (not shown) having a circular opening is disposed at a position conjugate to the focal point of objective lens 31. This allows light only at the focused position to be detected.

[0023] As shown by the second arrow F2 in FIG. 3 , the Raman scattered light scattered by the silicon carbide substrate 100 passes through the beam splitter 35 and is introduced into the spectrometer 33. In the spectrometer 33, the Raman scattered light is resolved into wavenumbers. The resolved Raman scattered light is detected by the detector 38. This results in a Raman spectrum with the horizontal axis representing the Raman shift (wavenumber) and the vertical axis representing the intensity of the Raman scattered light. The stage 34 can be moved in a direction parallel to the first main surface 1 of the silicon carbide substrate 100 (in the direction of the third arrow F3). As shown in FIG. 3 , the Raman spectrum is measured at the center of the first main surface 1.

[0024] Fig. 4 is a schematic diagram showing an example of a Raman spectrum of silicon carbide substrate 100. The horizontal axis of Fig. 4 represents the Raman shift (wave number). The vertical axis of Fig. 4 represents the intensity of Raman scattered light (Raman intensity). The Raman shift is the difference between the wave number of the excitation light and the wave number of the Raman scattered light of the object to be measured. As shown in Fig. 4, multiple peaks are observed in Raman spectrum 5.

[0025] The first peak P1 is Raman scattered light due to the folded mode of the longitudinal optical (LO) branch. The first peak P1 is, for example, a Raman shift of 964 cm -1 Specifically, the first peak P1 appears around the Raman shift of 964 cm -1 ±50cm -1 The first peak P1 appears within a range of 964 cm -1 ±40cm -1 It may appear within a range of 964 cm -1 ±30cm -1 It may appear within a range of 964 cm -1 ±20cm -1 It may appear within the range.

[0026] The fourth peak P4 is Raman scattered light caused by the folded mode of the transverse optical (TO) branch. The fourth peak P4 is, for example, at 776 cm -1 The fifth peak P5 is Raman scattered light caused by the folded mode of the longitudinal acoustic (LA) branch. The fifth peak P5 appears, for example, at 610 cm -1 appears nearby.

[0027] When silicon carbide substrate 100 contains carbon-based impurities such as graphite, peaks in the Raman spectrum due to the carbon-based impurities are observed. Specifically, the Raman spectrum of silicon carbide substrate 100 may have a second peak P2 and a third peak P3. As the amount of graphite mixed in silicon carbide substrate 100 increases, the intensities of each of second peak P2 and third peak P3 increase.

[0028] The second peak P2 is Raman scattered light caused by graphite. For example, the second peak P2 has a Raman shift of 1500 cm -1 Specifically, the second peak P2 appears around the Raman shift of 1500 cm -1 ±30cm -1 The second peak P2 appears within a range of 1500 cm -1 ±20cm -1 The Raman shift may appear within a range of 1500 cm -1 ±10cm -1 It may appear within the range.

[0029] The third peak P3 is Raman scattered light caused by graphite. The third peak P3 is, for example, at 1700 cm -1 Specifically, the third peak P3 appears around the Raman shift of 1700 cm -1 ±30cm -1 The third peak P3 appears within a range of 1700 cm -1 ±20cm -1 The Raman shift may appear within a range of 1700 cm -1 ±10cm -1 It may appear within the range.

[0030] The intensity of the first peak P1 is referred to as the first peak intensity A1. The intensity of the second peak P2 is referred to as the second peak intensity A2. The intensity of the third peak P3 is referred to as the third peak intensity A3. As shown in FIG. 4 , the second peak intensity A2 may be higher than the third peak intensity A3. The first peak intensity A1 may be lower than the second peak intensity A2 and higher than the third peak intensity A3. The intensity of the fifth peak may be higher than the intensity of the first peak P1. The intensity of the fourth peak may be higher than the intensity of the fifth peak.

[0031] Fig. 5 is a schematic diagram showing the shape of the vicinity of first peak P1 in the Raman spectrum of silicon carbide substrate 100 according to this embodiment. The horizontal axis of Fig. 5 represents the Raman shift. The vertical axis of Fig. 5 represents the Raman intensity.

[0032] The first peak broadens as the amount of carbon-based impurities contained in silicon carbide substrate 100 increases. In particular, the length of first peak P1 on the high wavenumber side tends to be longer than the length of first peak P1 on the low wavenumber side.

[0033] 5, the intensity of the first peak P1 in the Raman spectrum 5 may increase sharply from the low wavenumber side to the maximum value and then decrease gradually from the maximum value to the high wavenumber side. From another perspective, the length of the tail on the high wavenumber side of the first peak P1 may be longer than the length of the tail on the low wavenumber side of the first peak P1.

[0034] The Raman shift of the first peak P1 is the third wavenumber B3. The intensity of the first peak P1 is the first peak intensity A1. Half the intensity of the first peak P1 is the fourth intensity A4. The Raman shift of a Raman spectrum having the fourth intensity A4 and located at a higher wavenumber than the third wavenumber B3 is the fourth wavenumber B4. The Raman shift of a Raman spectrum having the fourth intensity A4 and located at a lower wavenumber than the third wavenumber B3 is the fifth wavenumber B5.

[0035] The value obtained by subtracting the fifth wave number B5 from the fourth wave number B4 is the half-value width D3 of the first peak P1. The half-value width D3 of the first peak P1 is, for example, 50 cm -1 The half width D3 of the first peak P1 is, for example, 45 cm -1 The half width D3 of the first peak P1 may be, for example, 40 cm -1 It may be less than 35 cm -1 It may be less than 30 cm -1 It may be less than 25 cm -1 It may be less than 20 cm -1 The half width D3 of the first peak P1 may be, for example, 10 cm -1 It may be more than 15 cm -1 It may be more than that.

[0036] The value obtained by subtracting the third wave number B3 from the fourth wave number B4 is the length of the tail on the high wave number side of the first peak P1 (first length D1). The first length D1 is, for example, 20 cm -1The first length D1 is, for example, 15 cm. -1 It may be less than 10 cm -1 The first length D1 may be, for example, 2 cm or less. -1 It may be more than 5 cm -1 It may be more than that.

[0037] The value obtained by subtracting the fifth wave number B5 from the third wave number B3 is the length of the tail on the low wave number side of the first peak P1 (second length D2). The second length D2 is smaller than the first length D1. The value obtained by subtracting the second length D2 from the first length D1 is, for example, 1 cm. -1 It may be more than 3 cm -1 The value obtained by subtracting the second length D2 from the first length D1 is, for example, 15 cm. -1 It may be less than 10 cm -1 It may be the following:

[0038] 6 is a schematic diagram showing the shape of the vicinity of the second peak P2 and the third peak P3 in the Raman spectrum of silicon carbide substrate 100 according to the present embodiment. The horizontal axis of FIG. 6 represents the Raman shift. The vertical axis of FIG. 6 represents the intensity ratio of the Raman spectrum. Specifically, the intensity ratio of the Raman spectrum is calculated by dividing the intensity of the Raman spectrum by the Raman shift of 1300 cm -1 In other words, the Raman shift is 1300 cm -1 The intensity of the Raman spectrum is normalized so that the intensity of the Raman spectrum at

[0039] 6, the intensity ratio of the Raman spectrum of the second peak P2 may be greater than the intensity ratio of the Raman spectrum of the third peak P3. The intensity ratio of the Raman spectrum of the second peak P2 is, for example, greater than 1 and less than or equal to 1.12. The intensity ratio of the Raman spectrum of the second peak P2 may be less than or equal to 1.10, less than or equal to 1.08, or less than or equal to 1.06. The intensity ratio of the Raman spectrum of the second peak P2 may be greater than or equal to 1.04, or greater than or equal to 1.05.

[0040] According to the silicon carbide substrate 100 according to this embodiment, the Raman shift is 1300 cm -1 The intensity of the Raman spectrum at -1 More than 1800cm -1 When the intensity of the maximum peak in the Raman spectrum in the following range is defined as the second intensity, the ratio of the second intensity to the first intensity is greater than 1 and not more than 1.12. -1 More than 1800cm -1 The maximum peak in the Raman spectrum in the following range corresponds to the second peak P2. When the intensity of the third peak P3 is higher than that of the second peak P2, the Raman shift is 1300 cm -1 More than 1800cm -1 The maximum peak of the Raman spectrum in the following range is the third peak P3.

[0041] As shown in FIG. 6, the Raman shift is 1300 cm -1 More than 1800cm -1 In the following range, the Raman shift at which the intensity of the Raman spectrum is maximized is the first wavenumber B1. -1 The distant Raman shift is the second wavenumber B2. The intensity ratio of the Raman spectrum at the first wavenumber B1 is the first intensity ratio C1. The intensity ratio of the Raman spectrum at the second wavenumber B2 is the second intensity ratio C2. The value obtained by subtracting the second intensity ratio C2 from the first intensity ratio C1 is the first intensity ratio difference E1. The value obtained by subtracting 1 from the first intensity ratio C1 is the second intensity ratio difference E2.

[0042] Raman shift is 1300 cm -1 More than 1800cm -1 In the following range, when the first intensity ratio C1 is 1.03 or more and the first intensity ratio difference E1 is 50% or more of the second intensity ratio difference E2, it is determined that the Raman spectrum has a peak. In other words, when the first intensity ratio C1 is less than 1.03, it is determined that the Raman spectrum does not have a peak. Even if the first intensity ratio C1 is 1.03 or more, when the first intensity ratio difference E1 is less than 50% of the second intensity ratio difference E2, the Raman shift is 1300 cm-1 More than 1800cm -1 The Raman spectrum is considered to have no peaks in the following ranges:

[0043] 7A is a schematic diagram showing the shape of a Raman spectrum of silicon carbide substrate 100 according to a first modified example of the present embodiment. The horizontal axis of Fig. 7A represents the Raman shift. The vertical axis of Fig. 7A represents the intensity ratio of the Raman spectrum.

[0044] As shown in FIG. 7A, the Raman shift is 1300 cm -1 More than 1800cm -1 In the following range, the Raman shift is 1300 cm -1 The ratio of the intensity of the Raman spectrum at a Raman shift of 1300 cm to the intensity of the Raman spectrum at a Raman shift of 1300 cm may be less than 1.03. -1 More than 1800cm -1 In the following range, the first intensity ratio C1 is less than 1.03. In this case, the Raman shift is 1300 cm -1 More than 1800cm -1 The Raman spectrum is considered to have no peaks in the following ranges:

[0045] 7B is a schematic diagram showing the shape of the Raman spectrum of silicon carbide substrate 100 according to the second modified example of the present embodiment. The horizontal axis of FIG. 7B represents the Raman shift. The vertical axis of FIG. 7B represents the intensity ratio of the Raman spectrum.

[0046] As shown in FIG. 7B, the Raman shift is 1300 cm -1 The intensity ratio of the Raman spectrum at 1300 cm to the intensity of the Raman spectrum at 1300 cm may oscillate and increase as the wavenumber increases. -1 More than 1800cm -1 In the following range, the first wave number B1, which is the Raman shift at which the intensity of the Raman spectrum is maximum, is 1800 cm -1 7B, a first intensity ratio C1, which is the intensity ratio of the Raman spectrum at a first wave number B1, may be 1.03 or more.

[0047] 30 cm to the lower wavenumber side than the first wavenumber B1 -1 The distant Raman shift is the second wavenumber B2. The intensity ratio of the Raman spectrum at the first wavenumber B1 is the first intensity ratio C1. The intensity ratio of the Raman spectrum at the second wavenumber B2 is the second intensity ratio C2. The value obtained by subtracting the second intensity ratio C2 from the first intensity ratio C1 is the first intensity ratio difference E1. The value obtained by subtracting 1 from the first intensity ratio C1 is the second intensity ratio difference E2.

[0048] 7B, the first intensity ratio difference E1 is less than 50% of the second intensity ratio difference E2. Thus, even if the first intensity ratio C1 is 1.03 or more, when the first intensity ratio difference E1 is less than 50% of the second intensity ratio difference E2, the Raman shift is 1300 cm -1 More than 1800cm -1 The Raman spectrum is considered to have no peaks in the following ranges:

[0049] Next, an apparatus for manufacturing silicon carbide ingot 110 according to this embodiment will be described. Fig. 8 is a partial cross-sectional schematic diagram showing the configuration of a first example of an apparatus for manufacturing silicon carbide ingot 110. As shown in Fig. 8, apparatus 500 for manufacturing silicon carbide ingot 110 mainly includes crucible 90, first resistive heater 61, second resistive heater 62, third resistive heater 63, molded insulating material 80, and flexible insulating material 70.

[0050] Crucible 90 has a raw material storage section 92 and a lid 91. Lid 91 is disposed on raw material storage section 92. First resistive heater 61 is disposed above lid 91. Second resistive heater 62 is disposed to surround the outer periphery of raw material storage section 92. Third resistive heater 63 is disposed below the bottom surface of raw material storage section 92.

[0051] The molded insulation material 80 has a first molded insulation material portion 81, a second molded insulation material portion 82, and a third molded insulation material portion 83. The first molded insulation material portion 81 is disposed above the first resistive heater 61. A through-hole is provided in the center of the first molded insulation material portion 81. The second molded insulation material portion 82 is disposed so as to surround each of the first resistive heater 61, the second resistive heater 62, and the third resistive heater 63. The third molded insulation material portion 83 is disposed below the third resistive heater 63. A through-hole is provided in the center of the third molded insulation material portion 83.

[0052] Flexible insulation 70 has first flexible insulation portion 71, second flexible insulation portion 72, and third flexible insulation portion 73. First flexible insulation portion 71 is disposed on the bottom surface of first molded insulation portion 81. In the growth direction of silicon carbide ingot 110, first flexible insulation portion 71 is located between first resistive heater 61 and first molded insulation portion 81.

[0053] Second flexible insulating portion 72 is disposed on the inner peripheral surface of second molded insulating portion 82. In the radial direction of silicon carbide ingot 110, second flexible insulating portion 72 is located between second resistive heater 62 and second molded insulating portion 82. Third flexible insulating portion 73 is disposed on the upper surface of third molded insulating portion 83. In the growth direction of silicon carbide ingot 110, third flexible insulating portion 73 is located between third resistive heater 63 and third molded insulating portion 83.

[0054] As the molded heat insulating material 80, for example, a product manufactured by Osaka Gas Chemicals (DON-2011) or a product manufactured by Nippon Carbon Co., Ltd. (FGL-203GH) is used. As the flexible heat insulating material 70, for example, a product manufactured by Osaka Gas Chemicals (LFP-105) or a product manufactured by Shin-Nihon Techno Carbon Co., Ltd. (GF-20-5FH) is used.

[0055] The flexible insulation 70 has higher flexibility than the molded insulation 80. Specifically, the value of the actual density relative to the compacted bulk density of the flexible insulation 70 is smaller than the value of the actual density relative to the compacted bulk density of the molded insulation 80. Note that the actual density is the weight relative to the actual volume. The compacted bulk density is the weight relative to the volume when the material is filled without gaps. As the flexibility increases, the gaps increase, so the actual density is smaller than the compacted bulk density.

[0056] Furthermore, the amount of sinking per unit pressure of the flexible insulating material 70 is greater than the amount of sinking per unit pressure of the molded insulating material 80. The amount of sinking per unit pressure is the amount of sinking of the pressing part of the pressing machine when the insulating material is pressed with a constant pressure by the pressing part. The amount of sinking per unit pressure can be measured using a Mitutoyo Digimatic Indicator (ID-H0530).

[0057] 9 is a partial cross-sectional schematic diagram showing the configuration of a second example of an apparatus for manufacturing silicon carbide ingot 110. The second example of the apparatus for manufacturing silicon carbide ingot 110 differs from the first example of the apparatus for manufacturing silicon carbide ingot 110 mainly in that a fourth flexible insulating material section 74 is disposed between first molded insulating material section 81 and second molded insulating material section 82, but other configurations are substantially the same as those of the first example of the apparatus for manufacturing silicon carbide ingot 110. The following description will focus on the configurations that differ from those of the first example of the apparatus for manufacturing silicon carbide ingot 110.

[0058] 9 , manufacturing apparatus 500 for silicon carbide ingot 110 may have fourth flexible insulating material portion 74. Fourth flexible insulating material portion 74 is disposed between first molded insulating material portion 81 and second molded insulating material portion 82. Fourth flexible insulating material portion 74 is continuous with first flexible insulating material portion 71. In the growth direction of silicon carbide ingot 110, the thickness of fourth flexible insulating material portion 74 may be the same as the thickness of first flexible insulating material portion 71.

[0059] Next, a method for manufacturing silicon carbide substrate 100 according to this embodiment will be described. First, a pre-firing step is performed. Specifically, crucible 90 is heated without silicon carbide source material 94 and seed substrate 93 placed in crucible 90. Specifically, crucible 90 is heated by applying power to first resistive heater 61, second resistive heater 62, and third resistive heater 63. The temperature of crucible 90 is set to, for example, 2200°C or higher and 2400°C or lower. The pressure of crucible 90 is set to, for example, 0.1 kPa or higher and 3 kPa or lower. The atmospheric gas contains argon gas or nitrogen gas. The time for the pre-firing step is, for example, 5 hours or higher and 20 hours or lower.

[0060] Next, a growth step is performed. As shown in FIGS. 8 and 9 , silicon carbide source material 94 is placed in source material storage unit 92. Seed substrate 93 is fixed to lid 91 using, for example, an adhesive (not shown). Seed substrate 93 is placed so as to face silicon carbide source material 94. Seed substrate 93 is, for example, silicon carbide substrate 100 having a polytype of 4H. The diameter of the main surface of seed substrate 93 is, for example, 150 mm. The main surface of seed substrate 93 is, for example, a {0001} plane or a plane inclined at an off-angle of approximately 8° or less with respect to the {0001} plane.

[0061] Next, crucible 90 is maintained in a state where no power is applied to first resistive heater 61, second resistive heater 62, and third resistive heater 63 and the pressure in crucible 90 is maintained at 1.0 Pa or less for approximately 30 minutes. Next, crucible 90 is heated by applying power to first resistive heater 61, second resistive heater 62, and third resistive heater 63. Specifically, crucible 90 is heated under high vacuum without flowing argon gas or nitrogen gas until the temperature of the bottom surface of crucible 90 reaches 1300°C. This significantly removes impurities (e.g., aluminum, titanium, iron, vanadium, boron, calcium, etc.) contained in flexible insulating material 70. After the temperature of the bottom surface of crucible 90 reaches 1300°C, atmospheric gas is introduced into crucible 90 so that the pressure in crucible 90 becomes 0.3 kPa or more and 1.0 kPa or less. Next, the temperature of crucible 90 is raised to the growth temperature of silicon carbide ingot 110. This starts the growth of silicon carbide ingot 110.

[0062] The pressure in crucible 90 is set to, for example, not less than 0.1 kPa and not more than 3 kPa. The temperature in crucible 90 is set to, for example, not less than 2200°C and not more than 2400°C. As a result, silicon carbide source material 94 sublimes, and silicon carbide gas (source gas) is generated. The silicon carbide gas is recrystallized on the surface of seed substrate 93. As a result, silicon carbide ingot 110 grows on the surface of seed substrate 93.

[0063] After the growth of silicon carbide ingot 110 is completed, the pressure in crucible 90 is adjusted to about 80 kPa. The atmospheric gas is argon gas only. With the temperature of crucible 90 set to, for example, 2200° C. or higher and 2400° C. or lower, silicon carbide ingot 110 is annealed for about 5 hours.

[0064] After the annealing is completed, silicon carbide ingot 110 is cooled to room temperature. Next, silicon carbide ingot 110 is removed from crucible 90. Next, silicon carbide ingot 110 is sliced ​​using a wire saw device (not shown). As a result, a plurality of silicon carbide substrates 100 are cut out from silicon carbide ingot 110.

[0065] Silicon carbide substrate 100 is made of, for example, hexagonal silicon carbide of polytype 4H. Silicon carbide substrate 100 has a first main surface 1 and a second main surface 2 opposite to first main surface 1. First main surface 1 is a plane that is off-axis, for example, by 4° or less in the <11-20> direction with respect to the {0001} plane.

[0066] Next, a step of mechanically polishing silicon carbide substrate 100 is carried out. Specifically, first main surface 1 is arranged to face a surface plate (not shown). Next, a slurry is introduced between first main surface 1 and the surface plate. The slurry contains, for example, diamond abrasive grains. The diameter of the diamond abrasive grains is, for example, not less than 1 μm and not more than 3 μm. A load is applied to first main surface 1 by the surface plate. As a result, silicon carbide substrate 100 is mechanically polished at first main surface 1.

[0067] Next, a step of chemically mechanically polishing silicon carbide substrate 100 is performed. Fig. 10 is a schematic diagram showing the step of chemically mechanically polishing silicon carbide substrate 100. As shown in Fig. 10, chemical mechanical polishing apparatus 300 has polishing cloth 301, polishing head 302, vacuum pump 304, and pressure unit 305. Polishing cloth 301 is, for example, a suede polishing cloth (SUPREME) manufactured by Nitta Haas.

[0068] 9, chemical mechanical polishing is performed on silicon carbide substrate 100 using polishing liquid 310. Polishing liquid 310 contains abrasive grains 312 and an oxidizing agent 311. Abrasive grains 312 are, for example, colloidal silica. The oxidizing agent is, for example, hydrogen peroxide, permanganate, nitrate, or hypochlorite. The polishing liquid is, for example, DSC-0902 manufactured by Fujimi Incorporated.

[0069] Silicon carbide substrate 100 is attached to polishing head 302. Silicon carbide substrate 100 is arranged to face polishing cloth 301. Polishing liquid 310 is supplied between silicon carbide substrate 100 and polishing cloth 301. The rotation speed of polishing head 302 is, for example, 60 rpm. The rotation speed of a surface plate on which polishing cloth 301 is provided is, for example, 60 rpm. The average processing surface pressure is, for example, 450 g / cm 2 The flow rate of polishing liquid 310 is, for example, 2 liters per minute. In this manner, silicon carbide substrate 100 (FIG. 1) in accordance with this embodiment is obtained.

[0070] <Method of Manufacturing Silicon Carbide Semiconductor Device> Next, a method of manufacturing the silicon carbide semiconductor device 400 according to this embodiment will be described. Fig. 11 is a flow diagram that schematically shows the method of manufacturing the silicon carbide semiconductor device 400 according to this embodiment. As shown in Fig. 11, the method of manufacturing the silicon carbide semiconductor device 400 according to this embodiment mainly includes the step (S5) of preparing a silicon carbide epitaxial substrate, the step (S3) of processing the silicon carbide epitaxial layer, and the step (S4) of forming an electrode on the silicon carbide epitaxial layer.

[0071] First, the step (S5) of preparing a silicon carbide epitaxial substrate is performed. The step (S5) of preparing a silicon carbide epitaxial substrate includes the step (S1) of preparing a silicon carbide substrate and the step (S2) of forming a silicon carbide epitaxial layer on the silicon carbide substrate. In the step (S1) of preparing a silicon carbide substrate, a silicon carbide substrate 100 according to the present embodiment is prepared (see FIG. 1 ).

[0072] Next, a step (S2) of forming silicon carbide epitaxial layer 20 on silicon carbide substrate 100 is performed. Specifically, silicon carbide epitaxial layer 20 is formed by epitaxial growth on first main surface 1 of silicon carbide substrate 100. In the epitaxial growth, for example, silane (SiH4) and propane (C3H8) are used as source gases, and hydrogen (H2) is used as a carrier gas. The temperature of the epitaxial growth is, for example, approximately 1400°C or higher and 1700°C or lower. In the epitaxial growth, an n-type impurity such as nitrogen is introduced into silicon carbide epitaxial layer 20. In this way, silicon carbide epitaxial substrate 200 according to this embodiment is prepared.

[0073] Fig. 12 is a cross-sectional schematic view showing the configuration of a silicon carbide epitaxial substrate 200 according to this embodiment. As shown in Fig. 12, the silicon carbide epitaxial substrate 200 according to this embodiment has a silicon carbide substrate 100 and a silicon carbide epitaxial layer 20. The silicon carbide epitaxial layer 20 is provided on the silicon carbide substrate 100.

[0074] Silicon carbide epitaxial layer 20 may have a buffer layer 41, a drift layer 42, and a third main surface 3. Buffer layer 41 is in contact with first main surface 1 of silicon carbide substrate 100. Drift layer 42 is provided on buffer layer 41. The nitrogen concentration contained in drift layer 42 may be lower than the nitrogen concentration contained in buffer layer 41. Third main surface 3 is formed of drift layer 42.

[0075] Next, the step (S3) of processing the silicon carbide epitaxial layer is performed. Specifically, the following processing is performed on silicon carbide epitaxial layer 20. First, ions are implanted into silicon carbide epitaxial layer 20.

[0076] 13 is a schematic cross-sectional view showing a step of forming a body region. In the step of forming the body region, p-type impurities such as aluminum are ion-implanted into third main surface 3 of silicon carbide epitaxial layer 20. This forms body region 113 having p-type conductivity. Portions where body region 113 is not formed become drift layer 42 and buffer layer 41. The thickness of body region 113 is, for example, 0.9 μm. Silicon carbide epitaxial layer 20 includes buffer layer 41, drift layer 42, and body region 113.

[0077] Next, a step of forming a source region is performed. FIG. 14 is a schematic cross-sectional view showing the step of forming the source region. Specifically, n-type impurities such as phosphorus are ion-implanted into the body region 113. This forms a source region 114 having n-type conductivity. The thickness of the source region 114 is, for example, 0.4 μm. The concentration of the n-type impurity contained in the source region 114 is higher than the concentration of the p-type impurity contained in the body region 113.

[0078] Next, a p-type impurity such as aluminum is ion-implanted into the source region 114 to form a contact region 118. The contact region 118 is formed to penetrate the source region 114 and the body region 113 and to be in contact with the drift layer 42. The concentration of the p-type impurity contained in the contact region 118 is higher than the concentration of the n-type impurity contained in the source region 114.

[0079] Next, activation annealing is performed to activate the implanted impurities. The temperature of the activation annealing is, for example, 1500° C. or higher and 1900° C. or lower. The activation annealing time is, for example, about 30 minutes. The atmosphere of the activation annealing is, for example, an argon atmosphere.

[0080] Next, a step of forming trenches in the third main surface 3 of the silicon carbide epitaxial layer 20 is performed. FIG. 15 is a cross-sectional schematic diagram showing the step of forming trenches in the third main surface 3 of the silicon carbide epitaxial layer 20. A mask 117 having openings is formed on the third main surface 3 including the source region 114 and the contact region 118. The source region 114, the body region 113, and a portion of the drift layer 42 are removed by etching using the mask 117. For example, inductively coupled plasma reactive ion etching can be used as the etching method. Specifically, for example, inductively coupled plasma reactive ion etching using SF or a mixed gas of SF and O as the reactive gas is used. Recesses are formed in the third main surface 3 by etching.

[0081] Next, thermal etching is performed on the recesses. Thermal etching can be performed, for example, by heating the mask 117 formed on the third main surface 3 in an atmosphere containing a reactive gas having at least one type of halogen atom. The at least one type of halogen atom includes at least one of chlorine (Cl) atoms and fluorine (F) atoms. The atmosphere can include, for example, Cl2, BCl3, SF6, or CF4. For example, thermal etching is performed using a mixed gas of chlorine gas and oxygen gas as the reactive gas, and setting the heat treatment temperature to, for example, 700°C or higher and 1000°C or lower. The reactive gas may contain a carrier gas in addition to the above-mentioned chlorine gas and oxygen gas. Examples of the carrier gas that can be used include nitrogen gas, argon gas, and helium gas.

[0082] 15 , a trench 56 is formed in the third main surface 3 by thermal etching. The trench 56 is defined by a sidewall surface 53 and a bottom wall surface 54. The sidewall surface 53 is formed by the source region 114, the body region 113, and the drift layer 42. The bottom wall surface 54 is formed by the drift layer 42. Next, the mask 117 is removed from the third main surface 3.

[0083] Next, a step of forming a gate insulating film is performed. FIG. 16 is a schematic cross-sectional view showing the step of forming a gate insulating film. Specifically, silicon carbide epitaxial substrate 200 having trench 56 formed in third main surface 3 is heated in an oxygen-containing atmosphere at a temperature of, for example, 1300° C. or higher and 1400° C. or lower. This forms gate insulating film 115 that is in contact with drift layer 42 at bottom wall surface 54, in contact with drift layer 42, body region 113, and source region 114 at sidewall surface 53, and in contact with source region 114 and contact region 118 at third main surface 3.

[0084] Next, a step of forming a gate electrode is performed. FIG. 17 is a cross-sectional view showing a step of forming a gate electrode and an interlayer insulating film. The gate electrode 127 is formed inside the trench 56 so as to contact the gate insulating film 115. The gate electrode 127 is disposed inside the trench 56 and is formed on the gate insulating film 115 so as to face each of the sidewall surface 53 and the bottom wall surface 54 of the trench 56. The gate electrode 127 is formed by, for example, a low pressure chemical vapor deposition (LPCVD) method.

[0085] Next, an interlayer insulating film 126 is formed. The interlayer insulating film 126 is formed so as to cover the gate electrode 127 and to be in contact with the gate insulating film 115. The interlayer insulating film 126 is formed by, for example, chemical vapor deposition. The interlayer insulating film 126 is made of, for example, a material containing silicon dioxide. Next, the interlayer insulating film 126 and part of the gate insulating film 115 are etched so as to form openings over the source region 114 and the contact region 118. As a result, the contact region 118 and the source region 114 are exposed from the gate insulating film 115.

[0086] Next, a step of forming a source electrode is performed. The source electrode 116 is formed so as to be in contact with each of the source region 114 and the contact region 118. The source electrode 116 is formed by, for example, a sputtering method. The source electrode 116 is made of, for example, a material containing Ti (titanium), Al (aluminum), and Si (silicon).

[0087] Next, alloying annealing is performed. Specifically, the source electrode 116 in contact with each of the source region 114 and the contact region 118 is maintained at a temperature of, for example, 900° C. or higher and 1100° C. or lower for about 5 minutes. As a result, at least a portion of the source electrode 116 is silicided. This forms the source electrode 116 in ohmic contact with the source region 114. The source electrode 116 may also form an ohmic contact with the contact region 118.

[0088] Next, the source wiring 119 is formed. The source wiring 119 is electrically connected to the source electrode 116. The source wiring 119 is formed so as to cover the source electrode 116 and the interlayer insulating film 126.

[0089] Next, a step of forming a drain electrode is carried out. First, silicon carbide substrate 100 is polished at second main surface 2. This reduces the thickness of silicon carbide substrate 100. Next, drain electrode 123 is formed. Drain electrode 123 is formed so as to be in contact with second main surface 2. In this manner, silicon carbide semiconductor device 400 according to this embodiment is manufactured.

[0090] 18 is a cross-sectional schematic diagram showing the configuration of a silicon carbide semiconductor device according to this embodiment. The silicon carbide semiconductor device 400 is, for example, a MOSFET (Metal Oxide Semiconductor Field Effect Transistor). The silicon carbide semiconductor device 400 mainly includes a silicon carbide epitaxial substrate 200, a gate electrode 127, a gate insulating film 115, a source electrode 116, a drain electrode 123, a source wiring 119, and an interlayer insulating film 126. The silicon carbide epitaxial substrate 200 includes a buffer layer 41, a drift layer 42, a body region 113, a source region 114, and a contact region 118. The silicon carbide semiconductor device 400 may be, for example, an IGBT (Insulated Gate Bipolar Transistor) or the like.

[0091] Next, the effects of silicon carbide substrate 100 according to this embodiment will be described. In the production of silicon carbide ingot 110, deterioration of molded insulating material 80 may occur due to the influence of raw material gas leaking from crucible 90. As deterioration of molded insulating material 80 progresses, gaps are formed in molded insulating material 80, creating a path for the raw material gas to escape to the outside. In this case, the temperature at the top of crucible 90 drops excessively, increasing the temperature difference between the top and bottom of crucible 90. Therefore, compared to when no gaps are formed in molded insulating material 80, an excessive upward flow of the raw material gas occurs.

[0092] 8 and 9 show an example of the flow of the source gas (silicon carbide gas). The source gas passes through the crucible 90 and tends to flow toward the molded insulating material 80 located above the crucible 90.

[0093] Furthermore, since molded insulating material 80 is used multiple times, gaps in molded insulating material 80 widen over time. This reduces the insulating performance and causes pressure fluctuations within crucible 90. This reduces the stability of the temperature environment during crystal growth of silicon carbide ingot 110, making it difficult to achieve a desired temperature distribution within crucible 90. As a result, the crystal quality of silicon carbide ingot 110 may be affected.

[0094] In particular, deterioration of molded insulating material 80 located above crucible 90 increases the temperature difference between the top and bottom of crucible 90. As a result, an excessive upward flow of the raw material gas occurs, which makes it easier for carbon-based impurities to float up from the carbon members constituting crucible 90, the carbonized raw material, etc. As a result, carbon-based impurities are taken into grown silicon carbide ingot 110.

[0095] The inventors have conducted extensive research into measures to prevent the generation of an excessive upward flow of the source gas, and have come to the following findings.

[0096] First, a flexible insulating material 70 with appropriate flexibility was placed near the molded insulating material 80. If the flexible insulating material 70 has high flexibility, it can be embedded in the joint between two molded insulating materials 80. This makes it possible to fill gaps between the two molded insulating materials 80 that occur due to assembly variations, design errors, etc. By sandwiching the flexible insulating material 70 between the molded insulating materials 80 arranged above and below, the weight of the molded insulating material 80 arranged above can further fill the gaps between the two molded insulating materials 80.

[0097] On the other hand, if the flexibility is too high, the raw material gas will easily permeate the flexible insulating material 70. As a result, it will be impossible to sufficiently suppress deterioration of the molded insulating material 80. The degree of flexibility of the molded insulating material 80 is evaluated by the ratio of the actual density to the compacted bulk density and the amount of sinking per unit pressure.

[0098] According to the present disclosure, by arranging flexible insulating material 70 having appropriate flexibility near molded insulating material 80, it is possible to prevent the formation of a path through which the source gas escapes to the outside in molded insulating material 80. As a result, it is possible to prevent the source gas from excessively flowing upward. Therefore, it is possible to obtain silicon carbide substrate 100 in which the incorporation of carbon-based impurities is suppressed.

[0099] (Sample Preparation) First, silicon carbide substrates 100 according to Samples 1 to 3 were prepared. Silicon carbide substrate 100 according to Sample 1 was used as a comparative example. Silicon carbide substrates 100 according to Samples 2 and 3 were used as examples. Silicon carbide substrates 100 according to Samples 1, 2 and 3 were manufactured using apparatus A, apparatus B and apparatus C, respectively. Apparatus B is the manufacturing apparatus shown in FIG. 8. Apparatus C is the apparatus shown in FIG. 9. Apparatus A has molded insulating material 80 but does not have flexible insulating material 70.

[0100] The properties of the molded insulation 80 and the flexible insulation 70 are shown in Table 1. In Device A, the density ratio of the molded insulation 80 was 0.99. In Device B, the density ratio of the molded insulation 80 was 0.98. In Device C, the density ratio of the molded insulation 80 was 0.99. In Table 1, density ratio is the ratio of the actual density to the compacted bulk density.

[0101]

[0102] Device A did not have flexible insulation 70. In Device B, the density ratio of the flexible insulation 70 was 0.95. In Device C, the density ratio of the flexible insulation 70 was 0.91. In Device B, the density ratio of the flexible insulation 70 to the density ratio of the molded insulation 80 (B / A) was 97%. In Device C, the density ratio of the flexible insulation 70 to the density ratio of the molded insulation 80 (B / A) was 92%.

[0103] In Table 1, the sinking amount is the amount of sinking per unit pressure. In device A, the sinking amount of the molded insulating material 80 was set to 0.58 mm / N. In device B, the sinking amount of the molded insulating material 80 was set to 0.53 mm / N. In device C, the sinking amount of the molded insulating material 80 was set to 0.60 mm / N. In device B, the sinking amount of the flexible insulating material 70 was set to 2.04 mm / N. In device C, the sinking amount of the flexible insulating material 70 was set to 1.72 mm / N.

[0104] As shown in Table 1, the pre-firing step was not performed in the apparatus A. The pre-firing step was performed in the apparatus B and the apparatus C. In the pre-firing step, the temperature of the crucible 90 was set to 2300°C. The pressure of the crucible 90 was set to 0.5 kPa. The atmospheric gas was a mixed gas of argon gas and nitrogen gas. The time for the pre-firing step was 18 hours.

[0105] (Evaluation Method) Next, Raman spectra of silicon carbide substrates 100 according to Sample 1, Sample 2, and Sample 3 were measured. A LabRAM HR-800 manufactured by HORIBA JOBIN YVON was used as the Raman spectrometer 30. A YAG laser was used as the light source 32. The excitation wavelength of the light source 32 was 532 nm. The laser irradiation intensity was 0.5 mW. The measurement method was backscattering measurement. The magnification of the objective lens 31 was 100 times. The diameter of the measurement area was 1 μm. The laser irradiation time was 20 to 180 seconds. The number of accumulations was 2. The filter was D1. The grating was 300 gr / mm. The hole was 100.

[0106] (Evaluation Results) When the concentration of carbon-based impurities in the silicon carbide substrate 100 increases, the Raman shift decreases from 1300 cm -1 More than 1800cm -1 The intensity of the maximum peak in the Raman spectrum tends to increase in the following range: Furthermore, the half-value width D3 of the first peak P1 increases; in particular, the length of the tail of the first peak P1 on the high wavenumber side increases.

[0107] As shown in Table 1, the 1300 cm measured on first main surface 1 of silicon carbide substrate 100 according to Samples 1 to 3 -1 From 1800 cm -1 The intensity ratios of the maximum peaks in the range of 1300 cm were 1.13, 1.08 and 1.01, respectively. -1 From 1800 cm -1 The intensity ratio of the maximum peak in the range of the Raman shift of 1300 cm -1 More than 1800cm -1 The intensity of the maximum peak in the Raman spectrum in the following range is calculated as the Raman shift of 1300 cm -1 The Raman spectrum intensity is calculated by dividing the Raman spectrum intensity by the Raman spectrum intensity at 1000 MHz.

[0108] The half width D3 of the first peak P1 measured on the first main surface 1 of the silicon carbide substrate 100 according to Samples 1 to 3 was 120 cm -1 , 40 cm -1 and 20 cm -1The length of the tail on the high wavenumber side of first peak P1 measured on first main surface 1 of silicon carbide substrate 100 according to samples 1 to 3 was 100 cm -1 , 20 cm -1 and 10 cm -1 It was.

[0109] From the above results, it was confirmed that silicon carbide substrate 100 according to each of Samples 2 and 3 was able to suppress the incorporation of carbon-based impurities compared to silicon carbide substrate 100 according to Sample 1.

[0110] The embodiments and examples disclosed herein are illustrative in all respects and should not be considered limiting. The scope of the present invention is defined by the claims, not the above description, and is intended to include meanings equivalent to the claims and all modifications within the scope thereof.

[0111] 1 First main surface, 2 Second main surface, 3 Third main surface, 5 Raman spectrum, 7 Orientation flat, 8 Arc-shaped portion, 9 Outer circumferential surface, 20 Silicon carbide epitaxial layer, 30 Raman spectroscopy device, 31 Objective lens, 32 Light source, 33 Spectrometer, 34 Stage, 35 Beam splitter, 36 Incident light, 38 Detector, 41 Buffer layer, 42 Drift layer, 53 Side wall surface, 54 Bottom wall surface, 56 Trench, 61 First resistive heater, 62 Second resistive heater, 63 Third resistive heater, 70 Flexible insulation, 71 First flexible insulation portion, 72 Second flexible insulation portion, 73 Third flexible insulation portion, 74 Fourth flexible insulation portion, 80 Molded insulation, 81 First molded insulation portion, 82 Second molded insulation portion, 83 Third molded insulation portion, 90 Crucible, 91 Lid, 92 Raw material container, 93 Seed substrate, 94 Silicon carbide raw material, 100 Silicon carbide substrate, 101 First direction, 102 Second direction, 103 Third direction, 110 Silicon carbide ingot, 113 Body region, 114 Source region, 115 Gate insulating film, 116 Source electrode, 117 Mask, 118 Contact region, 119 Source wiring, 123 Drain electrode, 126 Interlayer insulating film, 127 Gate electrode, 200 Silicon carbide epitaxial substrate, 300 Chemical mechanical polishing apparatus, 301 Polishing cloth, 302 Polishing head, 304 Vacuum pump, 305 Pressurizing unit, 310 Polishing liquid, 311 Oxidizing agent, 312 Abrasive grains, 400 Silicon carbide semiconductor device, 500 Manufacturing apparatus, A1 First peak intensity, A2 Second peak intensity, A3 Third peak intensity, A4 Fourth intensity, B1 First wavenumber, B2 Second wavenumber, B3 Third wavenumber, B4 Fourth wavenumber, B5 Fifth wavenumber, C1 First intensity ratio, C2 Second intensity ratio, D1 First length, D2 Second length, D3 Half width, E1 First intensity ratio difference, E2 Second intensity ratio difference, F1 First arrow, F2 Second arrow, F3 Third arrow, P1 First peak, P2 Second peak, P3 Third peak, P4 Fourth peak, P5 Fifth peak, W1 Maximum diameter.

Claims

1. Raman shift is 1300 cm -1 The intensity of the Raman spectrum at the Raman shift of 1300 cm is defined as the first intensity. -1 More than 1800cm -1 A silicon carbide substrate, wherein, when a maximum peak intensity in a Raman spectrum in the following range is defined as a second intensity, a ratio of the second intensity to the first intensity is equal to or greater than 1.03 and equal to or less than 1.

12.

2. Raman shift is 1300 cm -1 More than 1800cm -1 In the following range, the Raman shift at which the intensity of the Raman spectrum is maximum is defined as the first wavenumber, and the Raman shift 30 cm to the lower wavenumber side from the first wavenumber is defined as the -1 The distant Raman shift is the second wave number, and the Raman shift is 1300 cm -1 The ratio of the intensity of the Raman spectrum at the first wave number to the intensity of the Raman spectrum at the Raman shift of 1300 cm is defined as a first intensity ratio. -1 a second intensity ratio is an intensity ratio of the Raman spectrum at the second wavenumber to an intensity of the Raman spectrum at the second wavenumber, a first intensity ratio difference is a value obtained by subtracting the second intensity ratio from the first intensity ratio, and a second intensity ratio difference is a value obtained by subtracting 1 from the first intensity ratio, wherein the first intensity ratio is less than 1.03 or the first intensity ratio difference is less than 50% of the second intensity ratio difference.

3. Raman shift is 964 cm -1 ±50cm -1 The half-width of the peak in the Raman spectrum within the range of 50 cm -1 3. The silicon carbide substrate according to claim 1, wherein:

4. Raman shift is 964 cm -1 ±50cm -1 A peak in the Raman spectrum within a range of 10 cm to 30 cm is defined as a first peak, a Raman shift of the first peak is defined as a third wavenumber, and a Raman shift of a Raman spectrum having half the intensity of the first peak and located on the higher wavenumber side than the third wavenumber is defined as a fourth wavenumber, -1 The silicon carbide substrate according to claim 1 , wherein:

5. The silicon carbide substrate according to claim 1, wherein the silicon carbide substrate has a maximum diameter of 150 mm or more.

6. A silicon carbide epitaxial substrate comprising: a silicon carbide substrate according to any one of claims 1 to 5; and a silicon carbide epitaxial layer provided on the silicon carbide substrate.

7. A method for manufacturing a silicon carbide semiconductor device, comprising the steps of: preparing a silicon carbide epitaxial substrate according to claim 6; and forming an electrode on the silicon carbide epitaxial layer.

Citation Information

Patent Citations

  • Internal stress evaluation method of silicon carbide single crystal wafer, and prediction method of warp of silicon carbide single crystal wafer

    JP2015059073A

  • POLYCRYSTALLINE SiC COMPACT

    JP2021054667A

  • Silicon carbide substrate

    WO2017064897A1

  • Silicon carbide substrate

    WO2019111507A1

  • Silicon carbide substrate

    WO2019167337A1