Core-sheath composite monofilament for screen gauze

The core-sheath composite monofilament with reduced reflectance and strategically placed light absorbers addresses the environmental and technical issues of halation and thread breakage in screen printing, enabling high-definition and environmentally friendly screen printing without dyeing.

WO2024242012A1PCT designated stage expired Publication Date: 2024-11-28TORAY INDUSTRIES INC
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2024/018094
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-05-25
Filing Date
2024-05-16
Publication Date
2024-11-28

AI Technical Summary

Technical Problem

Conventional screen gauze dyeing processes for preventing halation in screen printing are environmentally harmful and result in thread breakage and defects due to high light absorber concentrations and organic pigment exposure, which affects the strength and spinning properties of monofilaments.

Method used

A core-sheath composite monofilament with a reflectance of 20.0% or less in the 300-450 nm wavelength range, containing two or more light absorbers with different absorption peaks only in the core, and a composite volume ratio of 50:50 to 95:5, using polyester as the primary resin for both core and sheath, to suppress halation and maintain strength for high-definition screen printing.

Benefits of technology

The solution eliminates the need for dyeing, provides excellent antihalation effects, and ensures high strength and precision in screen printing by evenly absorbing a wide range of light wavelengths while maintaining the monofilament's strength and abrasion resistance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JPOXMLDOC01-APPB-T000001
    Figure JPOXMLDOC01-APPB-T000001
  • Figure JPOXMLDOC01-APPB-T000002
    Figure JPOXMLDOC01-APPB-T000002
Patent Text Reader

Abstract

The problem to be solved by the invention is to provide a core-sheath composite monofilament for a screen gauze, the core-sheath composite monofilament having excellent abrasion resistance when woven into a high-definition mesh fabric and excellent anti-halation effects when forming a printing pattern on a screen without requiring a dyeing process. This core-sheath composite monofilament for a screen gauze satisfies requirements (a) to (c). (a) The reflectance in the entire region having an optical wavelength of 300 to 450 nm is 20.0% or less. (b) Only the core section contains a light-absorbing agent. (c) The breaking strength is between 7.0 cN / dtex and 9.0 cN / dtex.
Need to check novelty before this filing date? Find Prior Art

Description

Core-sheath composite monofilament for screen gauze

[0001] The present invention relates to a core-sheath composite monofilament for screen gauze, and more particularly to a core-sheath composite monofilament for screen gauze that has an excellent antihalation effect when a printing pattern is formed on the screen gauze by exposing it to light without dyeing the screen gauze.

[0002] Traditionally, mesh fabrics made from natural fibers such as silk or inorganic fibers such as stainless steel have been widely used as screen gauze for screen printing. In recent years, synthetic mesh has become popular due to its flexibility, durability, and cost performance. Among these, polyester monofilament is widely used due to its excellent dimensional stability and other suitability for screen applications.

[0003] Furthermore, in high-definition screen printing applications such as electrode and wiring printing for electronic components, against the backdrop of rising global demand for clean energy such as multilayer ceramic capacitors and solar cells, there has been remarkable growth and expansion, and the requirements for high-definition printing have become increasingly strict, calling for the development of more advanced monofilaments for screen gauze.

[0004] In a typical platemaking process, a screen made of monofilament is stretched and fixed on a frame, and then refined to remove unwanted materials such as oils adhering to the monofilament. After that, an ultraviolet-curable resin is applied and dried, and then a positive film with a black pattern to be printed is attached to the screen, and the screen is exposed to ultraviolet light with a wavelength of 300 to 450 nm.

[0005] The UV-curable resin that overlaps the image area of ​​the positive film does not harden, but the UV-curable resin in other areas hardens through a photochemical reaction when exposed to UV light. Therefore, by washing the plate after exposure with water, the UV-curable resin in the image area of ​​the positive film is washed away, creating a printing negative.

[0006] In screen printing, in order to achieve more precise and accurate printing, it is important to solidify the ultraviolet curable resin in accordance with the image on the positive film.

[0007] If the screen mesh has a high ultraviolet reflectance, ultraviolet light is diffused on the surface of the screen mesh, causing halation, which exposes areas of the pattern that do not need to be exposed, resulting in a significant decrease in printing accuracy.

[0008] To prevent this diffused reflection, a method is generally adopted in which monofilaments are woven into a screen gauze and then dyed.

[0009] However, the wavelength range of the ultraviolet curing resin and the ultraviolet irradiating lamp used in the plate making process differs depending on the plate maker in order to prevent diffused reflection.

[0010] Furthermore, the dyes and color settings used for dyeing vary depending on the plate maker, resulting in a huge variety of UV-curable resins and dyes.

[0011] Furthermore, the discharge of wastewater that places a heavy burden on the environment during the dyeing process is becoming a serious issue in many areas.

[0012] In this situation, various studies have been conducted on spun-dyed monofilaments for screen gauze that are colored by adding pigments during the spinning process in order to eliminate the dyeing process of screen gauze. For example, Patent Document 1 discloses an invention in which the fiber cross section of the monofilament has a core-sheath composite structure and the core component contains a light-absorbing substance.

[0013] Furthermore, Patent Document 2 discloses an invention of a polyester monofilament having a fineness and high strength, in which an organic compound pigment is contained in the entire cross section of the fiber, for high-definition screen printing.

[0014] International Publication No. 2005 / 118927 Japanese Patent Application Laid-Open No. 2022-144471

[0015] Patent Document 1 proposes that a core-sheath composite monofilament contain a light absorbent in the core component, but in order to prevent halation in a wide range of light wavelengths from various types of ultraviolet curable resins and ultraviolet irradiation lamps, it is necessary to contain a higher concentration of light absorbent.

[0016] Furthermore, high-magnification stretching was necessary to obtain the monofilament strength necessary for the dimensional stability of the screen gauze. However, the fiber surface of monofilament containing a high concentration of light absorbent and stretched at a high magnification is easily scraped due to the highly oriented crystal structure, which causes thread breakage during the spinning and weaving processes.

[0017] Furthermore, Patent Document 2 proposes that an organic compound pigment be contained in the entire fiber to suppress the reflectance at ultraviolet wavelengths. However, this causes problems such as the organic compound pigment being exposed on the fiber surface, which generates colored powdery scum during the spinning and weaving processes, which deteriorates spinnability and causes many defects in the screen gauze.

[0018] Therefore, an object of the present invention is to obtain a core-sheath composite monofilament for screen gauze that has the strength required for high-definition screen printing, by reducing the reflectance over the entire light wavelength range of 300 nm to 450 nm, thereby eliminating the need for a dyeing process for the screen gauze.

[0019] In order to solve the above problems, the present invention employs the following configurations: 1. A core-sheath composite monofilament for screen gauze satisfying requirements (a) to (c): (a) a reflectance of 20.0% or less over the entire light wavelength range of 300 nm to 450 nm, (b) a light-absorbing agent is contained only in the core, and (c) a breaking strength of 7.0 cN / dtex to 9.0 cN / dtex. 2. A core-sheath composite monofilament for screen gauze according to 1. above, in which the maximum reflectance over the light wavelength range of 300 nm to 450 nm is 1.3 times or less the average reflectance. 3. A core-sheath composite monofilament for screen gauze according to 1. or 2. above, in which two or more types of light-absorbing agents having different absorption peaks over the light wavelength range of 300 nm to 450 nm are contained only in the core, and the total content of the light-absorbing agents in the core is 0.1% by weight to 0.8% by weight. 4. A core-sheath composite monofilament for screen gauze according to 1. or 2. above, made of polyester. The core-sheath composite monofilament for screen gauze described above.

[0020] According to the present invention, it is possible to provide a core-sheath composite monofilament suitable for high-definition screen printing, which does not require a dyeing process for the screen gauze and has an excellent effect of preventing halation when a print pattern is formed by exposure to light.

[0021] The screen gauze monofilament of the present invention has a composite cross section consisting of a core and a sheath.

[0022] The resin constituting the core and sheath may be any melt-spinnable resin, and examples thereof include polyolefins such as polyethylene and polypropylene, modified polyolefins containing these as their main components, polyamides such as nylon 6 and nylon 66, modified polyamide copolymers containing these as their main components, aromatic polyesters such as polyethylene terephthalate, polypropylene terephthalate, polybutylene terephthalate, and polyethylene naphthalate, aliphatic polyesters such as polylactic acid and polybutylene succinate, and copolymer polyesters containing these as their main components, polyarylates, polybenzazoles, wholly aromatic polyesters, and wholly aromatic polyamides.

[0023] Among these, the resin used for the core is preferably a polyester mainly composed of polyethylene terephthalate (hereinafter referred to as PET) from the viewpoints of dimensional stability and production costs.

[0024] For PET, it is preferable to use a polyester having terephthalic acid as the main acid component and ethylene glycol as the main glycol component, with 90 mol % or more of repeating units being ethylene terephthalate.

[0025] Copolymerization components inhibit fiber orientation, and therefore, satisfactory raw yarn strength may not be obtained for high-definition screen printing applications, so it is preferable that the copolymerization components are not included.

[0026] Furthermore, titanium dioxide as a delustering agent, fine particles of silica or alumina as a lubricant, hindered phenol derivatives as an antioxidant, and further flame retardants, antistatic agents, etc. may be added to the resin as required.

[0027] Since the resin disposed in the core of the present invention is mainly responsible for the strength of the monofilament, the content of inorganic particle additives, typically titanium oxide, added as a delustering agent is preferably less than 0.6% by weight.

[0028] On the other hand, the resin used for the sheath is preferably a polyester mainly composed of PET.

[0029] For PET, it is preferable to use a polyester having terephthalic acid as the main acid component and ethylene glycol as the main glycol component, with 90 mol % or more of repeating units being ethylene terephthalate.

[0030] The resin disposed in the sheath is mainly responsible for the abrasion resistance of the monofilament, so it is preferable to add about 0.1 to 0.5% by weight of inorganic particles, typically titanium oxide.

[0031] The cross-sectional shape of the core-sheath composite monofilament of the present invention is preferably a round cross section from the viewpoint of uniformity of the mesh openings of the screen gauze.

[0032] Furthermore, it is preferable that the fiber has a core-sheath composite fiber structure in which the core is covered by the sheath in the cross section and is arranged so that the core is not exposed on the surface, and that the core and sheath are arranged concentrically.

[0033] In order to achieve both the scum suppression effect of the sheath and the high strength of the core, the composite volume ratio of the core to the sheath is 50:50 to 95:5.

[0034] When the same type of resin is used for the core and sheath, the composite volume ratio is preferably 70:30 to 90:10, since peeling at the composite interface is unlikely to occur.

[0035] When different types of resins are used for the core and sheath, the preferred composite volume ratio is 50:50 to 70:30 from the viewpoints of suppressing peeling at the composite interface and maintaining the strength of the monofilament.

[0036] The core-sheath composite monofilament of the present invention has a reflectance of 20.0% or less, more preferably 15.0% or less, over the entire range of light wavelengths from 300 nm to 450 nm. While there is no particular lower limit, lowering the reflectance generally requires the addition of a large amount of pigment, which impairs the strength of the yarn. Therefore, the reflectance must be set taking into account the desired yarn strength and reflectance. When curing a photosensitive resin with ultraviolet light during the platemaking process, light wavelengths of 300 nm to 450 nm are typically irradiated. The light wavelength range is selected by the platemaker based on compatibility with the UV-curable resin. To prevent halation, it is important to suppress reflection of light wavelengths in this range over the entire range. As described below, the reflectance is measured at 10-nm intervals between light wavelengths of 300 nm and 450 nm. If the maximum measured value is 20.0% or less, i.e., the reflectance over the entire range is 20.0%, reflection of ultraviolet light is suppressed, resulting in a clear printed pattern without halation.

[0037] Furthermore, by making the maximum reflectance, which is the maximum value of the measured reflectance values, 1.3 times or less the average reflectance, which is the average value of the measured reflectance values, the occurrence of halation can be suppressed.

[0038] In the present invention, the core-sheath composite monofilament contains a light absorber only in the core portion for the purpose of suppressing halation when forming a print pattern and reproducing the print pattern with high resolution using an ultraviolet-curable resin.

[0039] If a light absorbing agent is contained in the sheath, the light absorbing agent exposed on the fiber surface will fall off in powder form, which will manifest as colored powdery scum during the spinning and weaving processes and induce yarn breakage, so the sheath does not contain a light absorbing agent.

[0040] Light absorbers have specific absorption peaks for different light wavelengths, but by incorporating two or more types of light absorbers with different absorption peaks in the light wavelength range of 300 nm to 450 nm into the core, it becomes possible to absorb a wide range of light wavelengths evenly.

[0041] Furthermore, the total amount of light absorbent contained in order to achieve a reflectance of 20.0% or less over the entire light wavelength range of 300 nm to 450 nm is smaller than when a single type of light absorbent is contained, and this can suppress a decrease in strength of the core-sheath composite monofilament. More preferably, by combining light absorbents whose absorption peaks in the light wavelength range differ by 50 nm or more, it becomes possible to absorb a wide range of light wavelengths and the amount of light absorbent contained can be reduced.

[0042] The total content of the light absorbent in the core is preferably 0.1% by weight to 0.8% by weight. At 0.1% by weight or more, a sufficient anti-halation effect is obtained, and at 0.8% by weight or less, a core-sheath composite monofilament is obtained that has both sufficient strength and abrasion resistance to achieve precise and accurate screen printing. A more preferred total content of the light absorbent in the core is 0.2% by weight to 0.4% by weight.

[0043] As the light absorbing agent, a conventionally known light absorbing agent that disperses well in the molten resin and can be colored at the melt spinning stage can be used.

[0044] Generally, screen gauze is widely used when it is a warm color such as red or yellow because it has good absorption properties from the high wavelength side of visible light to ultraviolet light, and it is preferable that the light absorbent of the present invention also has a similar color.

[0045] Examples of warm color light absorbers include organic pigments such as benzene azo pigments (monoazo pigments, disazo pigments, etc.), heterocyclic azo pigments (thiazole azo pigments, benzothiazole azo pigments, quinoline azo pigments, pyridine azo pigments, imidazole azo pigments, thiophene azo pigments, etc.), anthraquinone pigments, and isoindoline pigments; inorganic pigments such as titanium oxide pigments having iron or aluminum as a ligand; and dyes such as indigoid dyes, triphenylmethane dyes, xanthene dyes, alizarin dyes, acridine dyes, and cyanine dyes.

[0046] In screen printing, a common method used to improve the accuracy of the printing pattern is to increase the tension of the screen and reduce the distance between the screen and the object to be printed.

[0047] In order to increase the tension during stretching, the strength of each monofilament is increased.

[0048] Furthermore, the printing industry has strict requirements, requiring finer fineness and higher mesh, i.e., screen gauze with a higher weaving density. However, the tension applied to the yarn during the weaving process is not necessarily proportional to the fineness, and it is important that each monofilament has high strength. The thinner the monofilament, the higher the breaking strength is required.

[0049] The core-sheath composite monofilament of the present invention has a breaking strength of 7.0 cN / dtex or more in order to prevent deterioration of weaving properties and occurrence of gauze elongation and to obtain high dimensional stability.

[0050] On the other hand, since it is necessary to suppress the orientation and crystallinity in terms of abrasion resistance, the breaking strength is set to 9.0 cN / dtex or less, and preferably 8.8 cN / dtex or less.

[0051] The fineness of the core-sheath composite monofilament of the present invention is preferably 2.0 dtex to 10.0 dtex.

[0052] In the case of high mesh screen gauze of #420 (420 threads per 2.54 cm) or more, which is suitable for precision printing, the mesh lattice spacing per thread is very small, so when monofilaments with a fineness of 10 dtex or thicker are used, the opening per lattice becomes very small.

[0053] This makes it easy for scum to be generated by the friction between the reed and the monofilament, and as a result, it becomes difficult to obtain a screen mesh of #420 or larger.

[0054] Furthermore, it is preferable that the screen mesh of #450 or larger is 8.0 dtex or less, and that the screen mesh of #500 or larger is 6.0 dtex or less.

[0055] The lower limit of the fineness is preferably 2.0 dtex or more in terms of weaving properties, particularly the ease of weft feeding in a sulzer loom.

[0056] In the present invention, the strength of the monofilament at 5% elongation is preferably 4.5 cN / dtex to 6.5 cN / dtex.

[0057] If the strength at 5% elongation is 4.5 cN / dtex or more, a decrease in elongation during weaving and gauze elongation during printing are unlikely to occur, and high dimensional stability is obtained, while if it is 6.5 cN / dtex or less, fibrillation of the crystalline orientation of the fibers is unlikely to occur, and abrasion resistance is likely to be improved.

[0058] As a method for melt-spinning the core-sheath composite monofilament for screen gauze of the present invention, any conventionally known melt-spinning method may be employed.

[0059] The melting method may be a pressure melter method or an extruder method, but from the viewpoint of uniform melting and preventing retention, the extruder method is preferred.

[0060] The resins of the core component and the sheath component are melted in separate melt extruders. The separately melted polymers pass through their respective pipes, are metered, and then flow into a spinneret pack. In this case, the time for passing through the pipes is preferably within 30 minutes from the viewpoint of suppressing thermal degradation. The two polymers flowing into the pack are joined by the spinneret, combined into a core-sheath configuration, and discharged from the spinneret.

[0061] Thereafter, the fiber is cooled and oiled, and then drawn without being taken up once, by a direct spinning drawing method, whereby the core-sheath composite monofilament for screen gauze of the present invention can be produced.

[0062] It is possible to take up the undrawn yarn in the spinning step and then subject it to the drawing step again, but a direct spinning and drawing method in which drawing is performed directly in connection with the spinning step is preferred from the viewpoint of reducing the number of guides through which the yarn passes in the production process and suppressing yarn wear.

[0063] The stretching step is preferably multi-stage stretching using three or more pairs of rollers.

[0064] The temperature of the stretching rollers before the final stretching roller in the multistage stretching is preferably 130°C or lower, more preferably 110°C or lower, to suppress crystallization during stretching. The temperature of the final stretching roller is preferably 130°C or higher, more preferably 180°C or higher. If the final stretching roller temperature is 130°C or lower, it becomes difficult to control the fiber surface orientation, and fiber crystallization does not proceed easily, making it impossible to obtain a high-strength polyester monofilament. On the other hand, if the final stretching roller temperature exceeds 230°C, fusion at the final stretching roller is likely to occur, deteriorating spinnability, which is not preferred.

[0065] In the winding step, the fiber is wound into a pirn or cheese shape to obtain the core-sheath composite monofilament for screen gauze of the present invention.

[0066] Although various types of resins as mentioned above can be used for the core component, polyester is preferred from the viewpoint of dimensional stability. Among these, PET is preferred from the viewpoint of cost and spinning operability. When the core component is PET, its intrinsic viscosity (IV) is preferably 0.90 to 1.50. By setting the IV to 0.90 or more, it becomes possible to produce a core-sheath composite monofilament that combines sufficient strength and elongation. A more preferred IV is 0.95 or more. Furthermore, the upper limit of the IV is preferably 1.50 or less from the viewpoint of ease of molding, such as melt extrusion, and more preferably 1.30 or less, taking into consideration the manufacturing cost and the effect of molecular weight reduction due to molecular chain scission caused by heat and shear force during the process.

[0067] The resin for the sheath component may be any of the various types of resins described above. However, in terms of peeling at the composite interface, it is preferable that the resin be similar to the resin for the core component. In terms of cost and spinning operability, polyester is preferable, and PET is more preferable.

[0068] When the resin components of the core and sheath are PET, from the viewpoint of obtaining good abrasion resistance and sufficient strength, it is preferable that the IV of the PET of the sheath component be lower than the IV of the PET of the core component, and that the difference in IV be 0.20 to 1.00.

[0069] By setting the IV difference to 0.20 or more, the degree of orientation and crystallinity of the PET molecular chains of the sheath component, i.e., the PET molecular chains on the fiber surface, can be suppressed, resulting in good abrasion resistance. Furthermore, the sheath component bears the shear stress on the inner wall surface of the nozzle hole during melt spinning, so the shear stress experienced by the core component is reduced. As a result, the core component has a low degree of molecular chain orientation and is spun out in a uniform state, improving the strength of the final monofilament.

[0070] On the other hand, since the sheath component must be oriented appropriately in order for the monofilament to have high strength, the original yarn strength can be obtained by making the IV difference 1.00 or less. A more preferable IV difference is 0.30 to 0.70.

[0071] As described above, the light absorbing agent is contained only in the core component.

[0072] Examples of methods for adding the light absorbent include a method of melt-spinning pellets obtained by adding the light absorbent to a meltable resin, and a method of melt-kneading a high-concentration master pellet having a concentration of about 2 to 20 times the predetermined content with a normal resin, and spinning the resulting mixture while diluting the pellets.

[0073] In the latter case, the master pellets and ordinary resin pellets may be mixed in a pellet state and kneaded in a melt extruder, or they may be melted in separate melt extruders and then kneaded in a molten polymer transport pipe or a spin pack. In either case, it is preferable to use a static kneader in order to ensure uniform dispersion of the light absorber.

[0074] The evaluations of the examples and comparative examples were carried out by the following methods.

[0075] (1) Fineness A 500 m length of monofilament was taken, and the mass (g) of the skein was multiplied by 20 to obtain the fineness.

[0076] (2) Breaking strength (cN / dtex), strength at 5% elongation (cN / dtex) Breaking strength and strength at 5% elongation were measured using Tensilon UCT-100 manufactured by Orientec in accordance with JIS L1013 (2010).

[0077] (3) Intrinsic Viscosity IV The intrinsic viscosity IV was calculated by dissolving 0.8 g of a sample in 10 mL of o-chlorophenol (hereinafter abbreviated as OCP) with a purity of 98% or higher at 25°C, and determining the relative viscosity ηr using an Ostwald viscometer at 25°C using the following formula: ηr = η / η0 = (t × d) / (t0 × d0) Intrinsic viscosity IV = 0.0242ηr + 0.2634 where η is the viscosity of the polymer solution, η0 is the viscosity of the OCP, t is the drop time of the solution (seconds), and d is the density of the solution (g / cm 3 ), t0: fall time of the OCP (seconds), d0: density of the OCP (g / cm 3 ).

[0078] (4) Abrasion Resistance A monofilament is fixed in the air with a tension of 5 g, and one SUS reed dent (thickness 65 μm) is pressed from above, fixed at an angle of 2° to the horizontal. The reed dent is moved back and forth in the direction of the fiber axis at a speed of 133 m / min for a distance of 3.2 cm, and stopped after 20 seconds. The area rubbed by the reed dent is observed using a Keyence VHX-D500, and the abrasion state is evaluated using SEM images as follows, with S and A being deemed acceptable. S... No deformation or fluff-like abrasion on the monofilament surface, no problem. A... Thin streaks on the monofilament surface in the fiber longitudinal direction, but no problem in terms of quality. B... Fluff-like abrasion on the monofilament surface.

[0079] (5) Weavability The presence or absence of problems in the process of obtaining a screen mesh having a warp density and a weft density of 460 mesh (460 threads / 2.54 cm) from monofilaments was evaluated as follows, with S and A being considered acceptable. S: Almost no fluff scraping or powdery residue generation, no problem. A: Some fluff scraping or powdery residue generation, but no problem in terms of quality. B: Significant fluff scraping or powdery residue generation.

[0080] (6) Reflectance 10,000 m of monofilament was tightly wound around a plate measuring 6 cm in length and 6 cm in width, and the reflectance was measured at 10 nm intervals in the light wavelength range of 300 nm to 450 nm using a V750 spectrophotometer manufactured by JASCO Corporation in accordance with photolithography (JIS Z8722:2009). The maximum value of the measured reflectance was defined as the maximum reflectance, and the average of the measured values ​​was defined as the average reflectance.

[0081] (7) Peak Absorption Wavelength of Pigment A 10,000 m length of monofilament containing only one type of pigment was tightly wound around a plate measuring 6 cm in length and 6 cm in width, and the reflectance was measured at 5 nm intervals between light wavelengths of 300 nm and 500 nm using a V750 spectrophotometer manufactured by JASCO Corporation in accordance with photolithography (JIS Z8722:2009). The wavelength at which the measured reflectance was minimum was determined to be the peak absorption wavelength.

[0082] (8) Halation A fine pattern was printed onto the screen mesh obtained in the same manner as described in (5) above, and the pattern was observed under an electron microscope for evaluation, with S and A being deemed acceptable. S: High anti-halation effect. Almost no bleeding of the fine pattern, no problem. A: Halation effect. Some bleeding of the fine pattern, but no problem in terms of quality. B: Halation occurs. Significant bleeding of the fine pattern.

[0083] (9) Printing accuracy: The screen mesh obtained in the same manner as described in (5) above was stretched over a 30 cm x 30 cm frame. A 50 μm line pattern was formed at 50 μm intervals on the obtained mesh fabric using a photosensitive emulsion, and the state after printing was observed and evaluated using the following index. S and A were judged to be acceptable. S: Good line reproduction; A: Irregularities were observed at the line boundaries, but no problems; B: The line boundaries were very irregular, causing partial breaks.

[0084] (Example 1) Polyethylene terephthalate having an intrinsic viscosity IV of 0.70 and 0.1% by weight of titanium oxide, polymerized and pelletized by a conventional method, was freeze-ground, and 10% by weight of Pigment Yellow 150 having an absorption peak at 450 nm and Pigment Brown 48 having an absorption peak at 300 nm were mixed in a ratio of 1:4, and the mixture was fed into a twin-screw extruder to obtain master pellets. Using a compounding device, the obtained master pellets were blended with polyethylene terephthalate pellets having an intrinsic viscosity IV of 1.19 and 0.5% by weight of titanium oxide in a ratio of 4:96, and 0.40% by weight of a light absorber was incorporated into the core component.

[0085] The component of the sheath was polyethylene terephthalate with an intrinsic viscosity IV of 0.50 and containing 0.4% by weight of titanium oxide.

[0086] The polyester core and sheath components were melted at 297°C using an extruder, and then pumped to a polymer temperature of 275-285°C with a core-sheath volume ratio of 80:20. The melt was then introduced into a melt spinning pack. The melt was then introduced into a known composite spinneret to form a core-sheath structure, where it was spun into a yarn. The polyester monofilament discharged from the spinneret was actively heated and maintained at 300°C so that the ambient temperature directly below the spinneret was kept at 300°C. It was then cooled with a yarn cooling fan, and while applying a spinning oil, it was taken up on an unheated first godet roll. Without being wound up, the polyester monofilament was drawn around a first hot roll heated to 90°C, a second hot roll heated to 90°C, and a third hot roll heated to 190°C, where it was stretched and heat-set. The stretch ratio between the second and third hot rolls was 4.90. The fiber was then drawn around two unheated godet rolls with a surface roughness of 0.8 S, and then wound onto a package while controlling the spindle rotation speed so that the winding tension was 0.417 g / dtex, to obtain a 6.0 dtex sheath-core composite monofilament. The properties of this sheath-core composite monofilament are shown in Table 1. The maximum reflectance in the light wavelength range of 300 nm to 450 nm was 10.2%, i.e., the reflectance over the entire range was 10.2% or less, and the fiber exhibited excellent abrasion resistance and halation suppression effects suitable for use as a screen gauze.

[0087] (Examples 2 and 3) Except for changing the draw ratio to 4.70 times and 5.90 times, the fibers were spun and wound in the same manner as in Example 1. The properties of the core-sheath composite monofilament are shown in Table 1. Although the printing accuracy was slightly reduced in Example 2 and the abrasion resistance was slightly reduced in Example 3, both of them achieved sufficient abrasion resistance and halation suppression effects for use in screen gauze.

[0088] (Examples 4 and 5) Core-sheath composite monofilaments having finenesses of 3.1 dtex and 13.0 dtex were obtained in the same manner as in Example 1, except that the extrusion rate was changed. The properties of these core-sheath composite monofilaments are shown in Table 1. Although the weaving ability was slightly reduced in Example 4 and the printing accuracy was slightly reduced in Example 5, both exhibited sufficient abrasion resistance and halation suppression effects for use in screen gauze.

[0089] Examples 6 and 7: Except for changing the intrinsic viscosity IV of the core component polyethylene terephthalate pellets to 1.50 and 0.90 and changing the draw ratio to 5.20, respectively, spinning and winding were performed in the same manner as in Example 1. The properties of the core-sheath composite monofilaments are shown in Table 1. Although the abrasion resistance and weaving properties of Example 7 were slightly reduced, all of the monofilaments had sufficient abrasion resistance and halation suppression effects for use in screen gauze.

[0090] (Example 8) The master pellets and polyethylene terephthalate pellets contained in the core component polyester were blended in a ratio of 1:99, and the light absorber was added at 0.10% by weight, but the fibers were spun and wound in the same manner as in Example 1. The properties of this core-sheath composite polyester monofilament are shown in Table 1. Although the antihalation effect and printing accuracy were slightly reduced, sufficient abrasion resistance and halation suppression effect were obtained for use in screen gauze.

[0091] (Example 9) The master pellets and polyethylene terephthalate pellets contained in the core component polyester were blended in a ratio of 7:93, and the light absorber was added at 0.70% by weight, but the fibers were spun and wound in the same manner as in Example 1. The properties of this core-sheath composite polyester monofilament are shown in Table 1. Although the abrasion resistance and weaving properties were slightly reduced, the abrasion resistance and halation suppression effect sufficient for use in screen gauze were obtained.

[0092] Example 10: Polyethylene terephthalate having an intrinsic viscosity IV of 0.70 and 0.1 wt% titanium oxide, polymerized and pelletized by conventional methods, was frozen and pulverized, mixed with 10 wt% of Pigment Yellow 150, and fed into a twin-screw extruder to obtain master pellets. The resulting master pellets were blended with polyethylene terephthalate pellets having an intrinsic viscosity IV of 1.19 and 0.5 wt% titanium oxide in a ratio of 8:92 using a blending machine. A core-sheath composite polyester monofilament having a fineness of 6.0 dtex was obtained by spinning in the same manner as in Example 1, except that 0.80 wt% of a light absorber was added to the core component. The properties of this core-sheath composite polyester monofilament are shown in Table 1. Although the abrasion resistance, weaving ability, and printing accuracy were all reduced, the abrasion resistance and halation suppression effect sufficient for use in screen gauze applications were obtained.

[0093] Example 11: Polyethylene terephthalate having an intrinsic viscosity IV of 0.70 and 0.1% by weight of titanium dioxide, polymerized and pelletized by a conventional method, was freeze-ground, and 20% by weight of Pigment Yellow 150 having an absorption peak at 450 nm, Pigment Brown 48 having an absorption peak at 300 nm, and Pigment Red 101 having an absorption peak at 390 nm were mixed in a ratio of 1:2:2, and the mixture was fed into a twin-screw extruder to obtain master pellets. The master pellets were blended with polyethylene terephthalate pellets having an intrinsic viscosity IV of 1.19 and 0.5% by weight of titanium dioxide in a ratio of 3:97 using a blending machine, and a core-sheath composite polyester monofilament having a fineness of 6.0 dtex was obtained by spinning in the same manner as in Example 1, except that 0.60% by weight of a light absorber was added to the core component and the draw ratio was 5.2 times. The properties of this core-sheath composite polyester monofilament are shown in Table 1, and it exhibited excellent abrasion resistance and halation suppression effects suitable for use in screen gauze.

[0094]

[0095] (Comparative Example 1) Polyethylene terephthalate having an intrinsic viscosity IV of 0.70 and 0.1% by weight of titanium oxide, polymerized and pelletized by a conventional method, was freeze-ground, mixed with 10% by weight of Pigment Yellow 150, and fed to a twin-screw extruder-type kneading extruder to obtain master pellets. Using a compounding device, the obtained master pellets were blended with polyethylene terephthalate pellets having an intrinsic viscosity IV of 0.96 and 0.5% by weight of titanium oxide in a ratio of 4:96, and 0.40% by weight of a light absorber was incorporated into the core component.

[0096] Furthermore, polyethylene terephthalate having an intrinsic viscosity IV of 0.50 and 0.4% by weight of titanium oxide, which had been polymerized and pelletized by a conventional method, was freeze-ground, mixed with 10% by weight of Pigment Yellow 150, and fed to a twin-screw extruder-type kneading extruder to obtain master pellets. Using a compounding device, the obtained master pellets and polyethylene terephthalate pellets having an intrinsic viscosity IV of 0.50 and 0.4% by weight of titanium oxide were compounded in a ratio of 4:96, and 0.40% by weight of a light absorber was incorporated into the sheath component.

[0097] The above-mentioned polyester core and sheath components were spun and wound in the same manner as in Example 1 to obtain a core-sheath composite monofilament having a fineness of 6.0 dtex. The properties of this core-sheath composite polyester monofilament are shown in Table 2, and the abrasion resistance was reduced, and colored powdery scum was generated during weaving, resulting in yarn breakage.

[0098] Comparative Example 2: Polyethylene terephthalate having an intrinsic viscosity IV of 0.70 and 0.1 wt% titanium oxide, polymerized and pelletized by conventional methods, was frozen and pulverized, mixed with 10 wt% of Pigment Yellow 150, and fed into a twin-screw extruder to obtain master pellets. Using a compounding device, the resulting master pellets were blended with polyethylene terephthalate pellets having an intrinsic viscosity IV of 0.96 and 0.5 wt% titanium oxide at a ratio of 10:90, and 1.00 wt% of a light absorber was incorporated into the core component. The yarn was spun and wound in the same manner as in Example 1, except that the draw ratio was 4.30 times, to obtain a sheath-core composite monofilament having a fineness of 6.0 dtex. The properties of this sheath-core composite polyester monofilament are shown in Table 2. It had low strength and did not achieve sufficient accuracy in screen printing.

[0099] Comparative Example 3: Polyethylene terephthalate having an intrinsic viscosity IV of 0.70 and 0.1 wt% titanium oxide, polymerized and pelletized by conventional methods, was frozen and pulverized, mixed with 10 wt% of Pigment Yellow 150, and fed into a twin-screw extruder to obtain master pellets. Using a compounding device, the obtained master pellets were blended with polyethylene terephthalate pellets having an intrinsic viscosity IV of 1.19 and 0.5 wt% titanium oxide at a ratio of 4:96, and 0.40 wt% of a light absorber was added to the core component. The yarn was spun and wound in the same manner as in Example 1, except that the draw ratio was 5.00 times, to obtain a core-sheath bicomponent polyester monofilament having a fineness of 6.0 dtex. The properties of this core-sheath bicomponent polyester monofilament are shown in Table 2. Halation occurred, and sufficient precision could not be obtained in screen printing.

[0100] Comparative Example 4: Polyethylene terephthalate having an intrinsic viscosity IV of 0.70 and 0.1 wt% titanium oxide, polymerized and pelletized by a conventional method, was freeze-ground, mixed with 5 wt% of Pigment Yellow 150 and Pigment Brown 48 at a ratio of 1:4, and fed to a twin-screw extruder to obtain master pellets. The resulting master pellets were blended with polyethylene terephthalate pellets having an intrinsic viscosity IV of 1.19 and 0.5 wt% titanium oxide at a ratio of 1:99 using a blending device. The yarn was spun and wound in the same manner as in Example 1, except that 0.05 wt% of a light absorber was added to the core component, to obtain a core-sheath composite polyester monofilament having a fineness of 6.0 dtex. The properties of this core-sheath composite polyester monofilament are shown in Table 2. halation occurred, and sufficient precision could not be obtained in screen printing.

[0101]

Claims

1. A core-sheath composite monofilament for screen gauze that satisfies the following requirements (a) to (c): (a) reflectance of 20.0% or less in the entire range of light wavelengths from 300 nm to 450 nm; (b) light absorbent contained only in the core; (c) breaking strength of 7.0 cN / dtex to 9.0 cN / dtex.

2. The core-sheath composite monofilament for screen gauze according to claim 1, wherein the maximum reflectance in the light wavelength region of 300 nm to 450 nm is 1.3 times or less the average reflectance.

3. A core-sheath composite monofilament for screen gauze according to claim 1 or 2, in which two or more types of light absorbing agents having different absorption peaks in the light wavelength range of 300 nm to 450 nm are contained only in the core, and the total content of the light absorbing agents in the core is 0.1% by weight to 0.8% by weight.

4. The core-sheath composite monofilament for screen gauze according to claim 1 or 2, which is made of polyester.

Citation Information

Patent Citations

  • Polyester monofilament for screen gauze

    JP2022144471A

  • Monofilament for screen gauze

    JP2007092233A

  • Core-sheath composite polyester monofilament for high-precision screen gauze

    JP2022028194A

  • Core-sheath composite polyester monofilament for high-definition screen printing

    JP2024053157A

  • Monofilament for screen gauze and screen gauze therefrom

    WO2005118927A1