Inkjet recording method, inkjet recording device, and aqueous ink

The inkjet recording method addresses the challenge of sedimentation in water-based inks by using small resin particles to create pores and enhance light scattering, achieving high hiding properties and sedimentation resistance, thereby improving image quality and concealment.

WO2024242036A1PCT designated stage expired Publication Date: 2024-11-28CANON KK
View PDF 9 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2024/018255
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2024-04-08
Filing Date
2024-05-17
Publication Date
2024-11-28

AI Technical Summary

Technical Problem

Inkjet recording methods face challenges in achieving excellent hiding properties while using water-based inks with high sedimentation resistance, particularly due to the settling of titanium oxide particles, which affects image quality and concealment rates.

Method used

An inkjet recording method that involves applying a water-based ink containing particles and resin particles with an average primary particle diameter of 150 nm or less, heating the recording medium to melt the resin particles and create pores, and controlling the heating temperature to form a binder with a low refractive index, enhancing light scattering and image hiding power without sedimentation.

Benefits of technology

The method effectively records images with high hiding properties and excellent sedimentation resistance, improving image quality by scattering light and preventing particle settling, thus maintaining image concealment without the need for high-settling titanium oxide.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JP2024018255_28112024_PF_FP_ABST
    Figure JP2024018255_28112024_PF_FP_ABST
Patent Text Reader

Abstract

Provided is an inkjet recording method for recording an image on a recording medium using aqueous ink containing particles and first resin particles. The present invention has an ink application step for applying an aqueous ink to a recording medium, and a heating step for heating the recording medium to which the aqueous ink has been applied to a temperature that is equal to or higher than the glass transition temperature Tg(°C) or melting point TM(°C) of the first resin particles and less than the glass transition temperature Tg(°C) or melting point TM(°C) of the particles, the average primary particle diameter DP0 (nm) of the particles being 150 nm or less, and the recording medium being heated in the heating step to melt the first resin particles and generate pores.
Need to check novelty before this filing date? Find Prior Art

Description

Inkjet recording method, inkjet recording apparatus, and water-based ink

[0001] The present invention relates to an inkjet recording method, an inkjet recording apparatus, and a water-based ink.

[0002] In recent years, in fields such as commercial printing, white images are sometimes recorded on recording media other than white, such as transparent film, semi-transparent film, and colored paper. From the viewpoints of material stability and cost, white pigments such as titanium oxide are used in inks for recording white images.

[0003] However, the specific gravity of titanium oxide is higher than that of materials used in inks of colors other than white. Therefore, the difference in specific gravity with the solvent is also large, resulting in the issue of titanium oxide being more likely to settle in the ink. In particular, if titanium oxide with a larger particle size is used or the titanium oxide content is increased in order to improve the hiding power and whiteness of the recorded image, the titanium oxide is more likely to settle. Furthermore, a white ink containing rutile-type titanium oxide with an average particle size of 300 nm or more and a urethane resin has been proposed as an ink that can record images with excellent whiteness and is easy to redisperse even if the pigment settles (Patent Document 1).

[0004] JP 2013-60513 A

[0005] The settling velocity V of particles in ink can be calculated by the following formula (A) (Stokes' equation): V={g(ρ S -ρ)d 2} / 18μ...(A) d: Particle diameter g: Gravitational acceleration ρ S : Density of particle ρ: Density of dispersion medium μ: Viscosity of dispersion medium

[0006] According to Stokes' equation, the sedimentation velocity V increases in proportion to the square of the particle diameter, i.e., the larger the particle diameter, the more easily the particles settle. The specific gravity of rutile titanium oxide is greater than that of other common materials used in inks, and the sedimentation velocity is faster. For this reason, the titanium oxide used as a pigment in the white ink proposed in Patent Document 1 settles relatively easily.

[0007] On the other hand, in images recorded with ink containing titanium oxide particles with small particle diameters, visible light tends to pass through without scattering. This causes a rapid decrease in scattering intensity, which tends to reduce the image's hiding power. In other words, there is a trade-off between the particle settling speed and the hiding power of the recorded image.

[0008] Therefore, an object of the present invention is to provide an inkjet recording method that can record images with excellent hiding power while using an aqueous ink with excellent sedimentation resistance. Another object of the present invention is to provide an inkjet recording apparatus and an aqueous ink for use in this inkjet recording method.

[0009] That is, according to the present invention, there is provided an inkjet recording method for recording an image on a recording medium using a water-based ink containing particles and first resin particles, the method comprising: an ink applying step of applying the water-based ink to the recording medium; and a step of measuring the temperature of the recording medium to which the water-based ink has been applied at a glass transition temperature Tg (°C) or a melting point T M (°C) or higher, and the glass transition temperature Tg (°C) or melting point T M and a heating step of heating the particles to a temperature of less than 100° C., P0 (nm) is 150 nm or less, and in the heating step, the recording medium is heated to melt the first resin particles and generate voids.

[0010] According to the present invention, it is possible to provide an inkjet recording method that can record images with excellent hiding power while using an aqueous ink that has excellent sedimentation resistance. Furthermore, according to the present invention, it is possible to provide an inkjet recording apparatus and an aqueous ink that can be used in this inkjet recording method.

[0011] It is a schematic diagram for explaining an example of an image forming process. It is a schematic diagram for explaining an example of an image forming process. It is a perspective view which shows an embodiment of an ink jet recording apparatus of the present invention. It is a side view which shows an embodiment of an ink jet recording apparatus of the present invention.

[0012] The present invention will be described in further detail below with reference to preferred embodiments. In the present invention, when the compound is a salt, the salt is present in the ink as dissociated ions, but for convenience, it will be expressed as "containing a salt." Furthermore, aqueous inkjet inks and aqueous reaction liquids may be simply referred to as "ink" and "reaction liquid." Physical property values ​​are values ​​at room temperature (25°C) unless otherwise specified.

[0013] The present inventors have investigated an inkjet recording method capable of recording an image with excellent hiding power even when using an ink with excellent sedimentation resistance. As a result, they have found that by satisfying the following requirements (i) to (iv), it is possible to record an image with excellent hiding power even when using an ink with excellent sedimentation resistance, and have arrived at the present invention. (i) An ink applying step of applying an ink to a recording medium, and a step of heating the recording medium to which the ink has been applied, at a temperature higher than the glass transition temperature Tg (°C) or the melting point T M (°C) or higher, and the glass transition temperature Tg (°C) or melting point T M (ii) the ink contains particles and first resin particles; and (iii) the average primary particle diameter D of the particles. P0 (iv) In the heating step, the recording medium is heated to melt the first resin particles and generate voids.

[0014] 1 and 2 are schematic diagrams illustrating an example of an image formation process. When ink is applied to a recording medium, as shown in FIG. 1, volatile components such as water and water-soluble organic solvents evaporate, causing the ink to dry, and an ink film is formed in which particles 1 and first resin particles 2 in the ink are densely packed. Thereafter, the temperature at which the first resin particles 2 melt (the glass transition temperature Tg (°C) or melting point T of the first resin particles) is reached. M When the recording medium is heated to a temperature equal to or higher than the glass transition temperature Tg (°C) of the particles, the resin generated by the melting of the first resin particles 2 penetrates into the gaps between the particles 1, as shown in FIG. 2. At the same time, voids 4 are formed in the locations where the first resin particles 2 were present. The heating temperature at this time is set to a temperature equal to or higher than the glass transition temperature Tg (°C) or the melting point T M(°C), the particles 1 are not melted. The resin penetrates into the gaps between the particles 1, forming a binder 3, which is a mixture of the particles 1 and the resin. Here, the average primary particle diameter D P0 Since the refractive index (nm) is 150 nm or less, visible light is hardly scattered by the particles 1. However, air with a low refractive index is present within the voids 4 formed by the melting of the first resin particles. Therefore, it is believed that the refractive index of the voids 4 is relatively low compared to the refractive index of the binder 3. Under these conditions, incident light can be scattered due to the difference in refractive index between the binder 3 and the voids 4. Therefore, images with high concealing properties can be recorded without using components that tend to settle, such as titanium oxide, which has a large particle size. As described above, it is necessary to melt the first resin particles through a heating process. Therefore, it is believed that the first resin particles do not melt if a drying process is simply performed after image recording to evaporate the solvent (liquid component) on the surface of the recording medium, or if the heating process is performed at a temperature lower than the melting temperature of the first resin particles. As a result, scattering due to the difference in refractive index between the binder 3 and the voids 4 does not occur, and images with high concealing properties cannot be recorded. Furthermore, if the heating process is performed at a temperature higher than the melting temperature of the particles, not only the first resin particles but also the particles themselves melt, preventing the formation of voids. As a result, the above-mentioned scattering does not occur, and an image with high concealability cannot be recorded.

[0015] Furthermore, as shown by Stokes' equation (Equation (A)), the smaller the particle diameter, the slower the settling velocity of the particles. P0 By using particles with a relatively small particle size of 150 nm or less (nm), the sedimentation rate is slowed, and an ink with excellent sedimentation resistance can be obtained. The average primary particle size will be described in detail later. P0 If the particle size (nm) exceeds 150 nm, scattering of visible light is likely to occur, improving the hiding power, but the sedimentation rate increases as shown by Stokes' equation, making it difficult to obtain sedimentation resistance. Furthermore, if the particles are large, it becomes difficult to achieve a state in which the first resin particles are uniformly distributed around the particles as shown in Figure 1 during image formation, making it impossible to record an image with high hiding power.

[0016] <Inkjet Recording Method, Inkjet Recording Apparatus, and Water-Based Ink> The inkjet recording method of the present invention is a method of ejecting water-based ink from an inkjet recording head and applying it to a recording medium to record an image. The inkjet recording method of the present invention includes an ink applying step of applying the water-based ink to the recording medium, and a heating step of heating the recording medium to which the water-based ink has been applied to a predetermined temperature. In the heating step, the glass transition temperature Tg (°C) or the melting point T M (°C) or higher, and the glass transition temperature Tg (°C) or melting point T M The recording medium is heated to a temperature of less than 100° C. The water-based ink contains particles and first resin particles, and the particles have an average primary particle diameter D P0 The average particle size (nm) is 150 nm or less. In the heating step, the recording medium is heated to melt the first resin particles, thereby generating pores.

[0017] The inkjet recording apparatus of the present invention is an apparatus used in an inkjet recording method in which an aqueous ink is ejected from an inkjet recording head and applied to a recording medium to record an image, and is an apparatus suitable for use in the above-mentioned recording method. In the present invention, it is not necessary to cure the image by irradiation with actinic energy rays or the like.

[0018] The water-based ink of the present invention is an ink used in an ink-jet recording method in which the water-based ink is ejected from an ink-jet recording head and applied to a recording medium to record an image, and is an ink suitable for use in the above-mentioned recording method.

[0019] The inkjet recording method and inkjet recording apparatus (hereinafter also simply referred to as "recording method and recording apparatus") of the present invention will be described in detail below.

[0020] FIG. 3 is a perspective view schematically illustrating an embodiment of an inkjet recording apparatus according to the present invention. FIG. 4 is a side view schematically illustrating an embodiment of an inkjet recording apparatus according to the present invention. The recording apparatus according to the embodiment shown in FIGS. 3 and 4 includes an inkjet recording head 22 that ejects ink. The recording head 22 ejects ink by the action of thermal energy. A recording head that ejects ink by the action of thermal energy is a thermal recording head that applies thermal energy to ink by applying electric pulses to electrothermal transducers, thereby ejecting ink from ejection openings. While a recording head that ejects ink by the action of thermal energy has been described as an example here, a recording head that ejects ink by the action of mechanical energy may also be used. The recording head may include a mechanism (temperature control mechanism) that heats the aqueous ink ejected from the recording head. If a temperature control mechanism is provided, the temperature of the ink ejected from the recording head is preferably set to 35° C. or higher and 70° C. or lower.

[0021] Multi-pass printing is preferred, in which ink application to a unit area on a recording medium is performed by dividing the application of ink into multiple relative scans of the recording head and the recording medium. It is particularly preferred that white ink and color ink are applied to a unit area by different relative scans. This increases the time until the inks come into contact, making it easier to suppress mixing. The unit area can be set to any area, such as one pixel or one band.

[0022] (Heating Step) The recording method of the present invention includes a heating step of heating (heat treatment) a recording medium to which ink has been applied. In the heating step, the recording medium to which ink has been applied is heated to melt the first resin particles in the ink. This allows an image containing voids created by the melting to be fixed on the recording medium. When the recording medium to which ink has been applied is heated, the volatile components (solvents) in the ink, such as water or water-soluble organic solvents, evaporate, forming an ink film densely packed with particles and first resin particles, which are solid components dispersed in the ink. The heated first resin particles then melt to form voids, and the resin generated by the melting of the first resin particles penetrates into the voids between the particles. This forms a binder, which is a mixture of particles and resin, allowing an image containing voids therein to be fixed on the recording medium.

[0023] In the heating step, in order to melt the first resin particles in the ink, the ink is heated to a temperature equal to or higher than the glass transition temperature or melting point of the first resin particles and equal to or lower than the glass transition temperature Tg (°C) or melting point T M (°C), that is, the recording medium is heated to a temperature less than the heating temperature T H is the glass transition temperature Tg or melting point T M , and the glass transition temperature Tg (°C) or melting point T M In this case, when the first resin particles are formed of a crystalline resin, the Tg and T M In this case, T M The crystalline resin is heated to a temperature T H The heating temperature T (°C) is preferably 70°C or higher, more preferably 80°C or higher, and particularly preferably 90°C or higher. There is no particular upper limit to the heating temperature, but it is preferably 200°C or lower in view of the heat resistance temperature of the recording medium. H The heating temperature T Hcan be measured using, for example, a contact thermometer in which a thermocouple or the like is brought into contact with the surface of the recording medium, a non-contact infrared thermometer, etc. In the examples of the present invention, the temperature on the surface of the recording medium was measured using a non-contact infrared thermometer digital radiation temperature sensor FT-H20 (manufactured by Keyence) from a position 10 cm vertically upward from the surface of the recording medium.

[0024] By performing the heating step, the first resin particles are melted, generating voids, thereby recording an image containing voids. The heating step may be performed alone or in combination. Examples of means for heating the recording medium include known heating means such as heaters, air blowing means using air blowers such as dryers, and combinations thereof. Examples of heating means include the heating means, air blowing means, and combinations thereof. Examples of heat treatment methods include applying heat from the side opposite the recording surface (ink application surface) of the recording medium (back side) using a heater, applying warm or hot air to the recording surface of the recording medium, and heating from the recording surface or back side using an infrared heater. A combination of these methods may also be used. Furthermore, heating may be performed by contacting a heated member with the recording surface or back side of the recording medium. The duration of the heating step is not particularly limited as long as it can melt the first resin particles. For example, when the heating step is performed by blowing air, the air temperature can be set to 80°C or higher and 120°C or lower.

[0025] In the recording device shown in Figures 3 and 4, a heater 25 supported by a frame (not shown) is disposed downstream in the sub-scanning direction A from the position where the recording head 22 reciprocates in the main scanning direction B. The recording medium 10 to which ink has been applied can be heated by the heater 25. Specific examples of the heater 25 include a sheath heater and a halogen heater. The heater 25 is covered by a heater cover 26. The heater cover 26 is a member for efficiently irradiating the heat generated by the heater 25 onto the recording medium 10. The heater cover 26 also serves as a member for protecting the heater 25. The recording medium 10 to which ink has been applied from the recording head 22 is taken up by a take-up spool 27 to form a roll-shaped taken-up medium 24.

[0026] It is preferable to further include a step of forming an ink film in which the particles and first resin particles are densely packed, as shown in FIG. 1, prior to the heating step. By including such a step, the molten first resin particles can more reliably penetrate the voids between the particles, making it easier to create an image containing voids, as shown in FIG. 2. That is, the inkjet recording method preferably further includes at least one step selected from the group consisting of a reaction liquid application step of applying an aqueous reaction liquid containing a reactant that reacts with the ink to a recording medium, and a drying step of drying the liquid component on the recording medium. It is also more preferable to use these steps (the reaction liquid application step and the drying step) in combination. When these steps are used in combination, it is particularly preferable to perform the drying step after the reaction liquid application step. In other words, it is preferable to perform the reaction liquid application step, the ink application step, the drying step, and the heating step in this order. The ink may be applied in parallel with the application of the reaction liquid. Applying the reaction liquid to the recording medium allows the particles and first resin particles in the ink to aggregate and become densely packed. Details of the reaction liquid will be described later. When blowing air onto the recording medium, it is preferable to blow air onto the surface (recording surface) of the recording medium from the perspective of drying efficiency.

[0027] The drying step can be carried out to dry the liquid component (solvent) on the surface of the recording medium. Here, the liquid component does not have to be completely dried in the drying step. Furthermore, the liquid component on the recording medium will gradually dry without going through the above steps, but carrying out the drying step promotes drying and can efficiently achieve the state shown in FIG. 1. The drying step may be a single step or multiple steps. The same heating means as in the heating step can be used in the drying step. Among these, blowing air is preferred from the viewpoint of efficiently drying the liquid component.

[0028] Since the drying step is carried out in a state where the solvent remains on the surface of the recording medium and the viscosity has not increased sufficiently, it is preferable not to apply too much heat energy to the recording medium in order to prevent the recording medium from becoming difficult to reach the state shown in FIG. 1. Specifically, it is preferable not to make the heating temperature or heating time too long. For example, when drying is performed by blowing air, the temperature of the air blowing means (hot air, etc.) can be set so that the recording medium reaches the desired temperature, taking into account the conveying speed and the ambient temperature. Specifically, the temperature of the air blown by the air blowing means (hot air, etc.) is preferably 60° C. or less, and more preferably 30° C. or less. The air temperature may be room temperature (25° C.). Here, in order to reduce the liquid component without melting the first resin particles and to achieve a state in which the particles and the first resin particles are dense, as shown in FIG. 1, the Tg or T M It is preferable to heat the recording medium at a temperature lower than the temperature at which the recording medium is heated. The wind speed is preferably 1 m / s or more and 100 m / s or less. The temperature of the hot air or other wind can be measured using a K-type thermocouple thermometer. A specific example of a measuring device is an AD-5605H (manufactured by A&D). If necessary, the wind may be blown against the backside of the recording medium, but it is preferable to blow the wind against the front side of the recording medium (the side to which the ink is applied). The distance from the air blowing device to the recording medium is preferably 5 mm or more and 50 mm or less.

[0029] (Recording Medium) The type of recording medium on which an image is recorded is not particularly limited, and any recording medium may be used. In particular, since an ink capable of recording an image in white or other color with excellent hiding power is used, it is preferable to use a recording medium other than white, such as a transparent film, a semi-transparent film, or colored paper. In other words, it is preferable to use a non-absorbent recording medium. Here, a non-absorbent recording medium (a low to non-absorbent recording medium) is a recording medium that is capable of recording an image in a Bristow method within 30 msec from the start of contact. 1/2 Water absorption up to 0 mL / m 2 10mL / m or more 2 The Bristow method is described in JAPAN TAPPI Paper and Pulp Test Method No. 51, "Test Method for Liquid Absorbency of Paper and Paperboard." Recording media for inkjet recording (glossy paper, matte paper, etc.) having a coating layer (ink receiving layer) formed of inorganic particles, and plain paper having no coating layer, have a water absorption capacity of 10 mL / m. 2 It is an "absorbent recording medium" that exceeds

[0030] Examples of low to non-absorbent recording media that can be used include plastic films; recording media in which a plastic film is adhered to the recording surface of a substrate; and recording media in which a resin coating layer is provided on the recording surface of a substrate containing cellulose pulp. Of these, plastic films are preferred, and recording media in which a resin coating layer is provided on the recording surface of a substrate containing cellulose pulp are also preferred. Note that the recording medium in this specification does not refer to a transfer medium, but rather to a recording medium on which an image is recorded as a recorded matter.

[0031] (Water-based ink) The ink used in the recording method of the present invention is a water-based ink for inkjet recording containing particles and first resin particles. In particular, a white ink is preferable. The white ink also includes inks that are capable of recording (forming) white images even if they do not exhibit white color in the ink state. The white color is defined as a color that is lighter than the lightness (L * ) and chromaticity (a * , b * ) are 70≦L * ≦100, −4.5≦a* ≦2, and −6≦b * The components constituting the ink will be described in detail below.

[0032] [Particles] The ink contains particles. These particles may be colorants or may be non-colored particles such as resin particles. In particular, since a white image is to be recorded, it is preferable to use colorless or white particles. The particle content (volume %) in the ink is preferably 1.5 volume % or more based on the total volume of the ink. If the particle content is less than 1.5 volume %, sufficient voids for penetration may not be formed when the first resin particles described below melt, and sufficient image hiding power may not be obtained. The particle content in the ink is preferably 5.0 volume % or less.

[0033] The particles are usually dispersed in the ink in the form of secondary aggregates formed by aggregation of two or more primary particles. P0 (nm) is 150 nm or less, preferably 50 nm or less. P0 The lower limit of the particle diameter (nm) is not particularly limited, but is preferably 5 nm or more. The particle diameter of the primary particles of the particles can be measured by observing the particles using a scanning electron microscope. The average primary particle diameter of the particles can be calculated as the average particle diameter of a plurality of primary particles (e.g., 100 particles).

[0034] Cumulative 50% particle diameter D based on particle volume P The particle diameter (nm) is preferably 150 nm or less, and more preferably 5 nm or more and 100 nm or less. By using particles having a volume-based cumulative 50% particle diameter within the above range, light scattering can be suppressed to allow for better light transmission, and the sedimentation rate can be further reduced.

[0035] In this specification, the term "volume-based cumulative 50% particle diameter (D 50")" is the diameter of a particle that is 50% of the total volume of measured particles in a particle size cumulative curve, calculated from the smallest particle diameter side, and can be measured using a particle size distribution measuring device based on the dynamic light scattering method. Measurement conditions can include, for example, Set Zero: 30 seconds, number of measurements: 3, measurement time: 180 seconds, shape: non-spherical, etc. Furthermore, as the particle size distribution measuring device, a particle size analyzer based on the dynamic light scattering method (for example, trade name "UPA-EX150", manufactured by Nikkiso) can be used. Of course, the particle size distribution measuring device used and the measurement conditions are not limited to those described above.

[0036] The particles must not melt during the heating process for melting the first resin particles. Specifically, the particles must not melt at a temperature higher than the glass transition temperature Tg or melting point T M is equal to or higher than the temperature of the recording medium in the heating step, and preferably equal to or higher than 200° C. The particles are preferably at least one selected from the group consisting of titanium oxide, calcium carbonate, calcium phosphate, barium sulfate, zirconium oxide, silicon dioxide, kaolin, clay, and second resin particles. Details of the second resin particles will be described later.

[0037] From the viewpoint of forming a binder with a high refractive index, it is preferable to use titanium oxide particles having a relatively high refractive index. The refractive index of titanium oxide is preferably 2.1 or more, and more preferably 2.5 to 2.8. The surface of titanium oxide may be coated with alumina or zirconia. The surface of titanium oxide may also be coated with an inorganic oxide such as silica, zinc oxide, or zirconia; or an organic substance such as polyol. The use of surface-coated titanium oxide is expected to suppress photocatalytic activity and improve dispersibility. Titanium oxide has three crystalline forms: rutile, anatase, and brookite. Of these, it is preferable to use rutile titanium oxide, which has low photocatalytic activity. Examples of industrial production methods for titanium oxide include a sulfuric acid method and a chlorine method. Titanium oxide produced by either production method can be used.

[0038] The content (mass %) of titanium oxide in the ink is preferably 5.0 mass % or more and 45.0 mass % or less, and more preferably 7.0 mass % or more and 38.0 mass % or less, based on the total mass of the ink. P0 The volume-based cumulative 50% particle diameter D (nm) of titanium oxide is preferably 50 nm or less, and more preferably 30 nm or less. P (nm) is preferably 100 nm or less, and more preferably 5 nm or more and 50 nm or less.

[0039] The particle shape of calcium carbonate can be cubic or spindle-shaped. Among them, it is preferable to use calcium carbonate with a uniform cubic shape. As calcium phosphate, monocalcium phosphate (Ca(H 2 P.O. 4 ) 2 ), dibasic calcium phosphate (CaHPO 4 ), and tricalcium phosphate (Ca 3 (PO) 2 Among them, apatite-type calcium phosphate is preferable, and hydroxyapatite (Ca 10 (P.O. 6 ) (OH) 2 ) is more preferred.

[0040] Barium sulfate is broadly divided into elutriated barium sulfate and precipitated barium sulfate. The particle size of precipitated barium sulfate can be controlled by adjusting the synthesis conditions, allowing for the production of barium sulfate with an appropriate particle size. Zirconium oxide, also known as zirconia, is known as a highly tough ceramic. Pure zirconia is prone to deterioration due to changes in its crystalline structure and volume caused by temperature changes. For this reason, stabilized zirconia, which has been modified by adding a stabilizer to suppress volume changes, can be used.

[0041] Silicon dioxide can be synthesized by, for example, the Stober method. The Stober method is a method in which a hydrolysis and polycondensation reaction of an alkoxysilane, which is a silica source, proceeds in a solution of water, ethanol, and aqueous ammonia. By changing the concentration of each reactant, it is possible to control the particle size of the resulting spherical particles.

[0042] Kaolin is a clay mineral containing multiple inorganic components. Specifically, it is a clay consisting of kaolinite, hydrated halloysite, and halloysite crystal structures. In addition to the kaolin component, clay also contains ilmenite, montmorillonite, vermiculite, and the like. When using the above particles, it is preferable to use particles with high whiteness in order to produce a white ink.

[0043] [Resin Particles] The ink contains first resin particles. When the solvent in the ink applied to the recording medium evaporates, the particles and the first resin particles become closely attached to each other. Then, the heating process melts the first resin particles, creating voids. The content (mass %) of the first resin particles in the ink is preferably 2.5% by mass or more and 17.0% by mass or less, and more preferably 2.5% by mass or more and 14.0% by mass or less, based on the total mass of the ink. Furthermore, the content (volume %) of the first resin particles in the ink is preferably 2.5% by volume or more and 17.0% by volume or less, and more preferably 2.5% by volume or more and 14.0% by volume or less, based on the total volume of the ink.

[0044] The size of the pores formed in the heating step is roughly the same as the size (particle diameter) of the first resin particles. The size of the pores formed significantly affects the light scattering efficiency. Therefore, from the viewpoint of further improving the light scattering efficiency, the volume-based cumulative 50% particle diameter D E is preferably 100 nm or more and 400 nm or less, and more preferably 150 nm or more and 250 nm or less.

[0045] Whether the first resin particles have melted during the heating process can be easily determined, for example, by cutting the recording medium on which images before and after the heating process are recorded and observing it with a scanning electron microscope, etc. Furthermore, by measuring the particle diameter of the first resin particles in the image before the heating process, if the difference between the size of the pores in the image after the heating process and the particle diameter of the first resin particles is small (for example, within 10%), it can be determined that the first resin particles have melted and pores have been formed.

[0046] From the viewpoint of forming a binder with a high refractive index, it is preferable to use first resin particles having a higher refractive index. Specifically, the refractive index of the first resin particles is preferably 1.5 or more, and more preferably 1.6 to 2.5.

[0047] The content (volume %) of the first resin particles in the ink is preferably 1.3 to 5.0 times, more preferably 2.0 to 4.0 times, in volume ratio relative to the particle content (volume %). If the volume ratio exceeds 5.0 times, the amount of fusion between the first resin particles tends to increase, making it difficult to form voids of the desired size. As a result, sufficient image hiding power may not be obtained. Furthermore, the refractive index of the molten first resin particles and the binder composed of the particles may decrease, which may lead to a decrease in light scattering efficiency and hiding power. On the other hand, if the mass ratio is less than 1.3 times, the amount of voids formed may decrease, and sufficient image hiding power may not be obtained.

[0048] When the particles are titanium oxide, the content (mass %) of the first resin particles in the ink is preferably 0.30 times or more and 1.0 times or less, and more preferably 0.40 times or more and 0.60 times or less, in mass ratio to the content (mass %) of titanium oxide.

[0049] The content (volume %) of the first resin particles in the ink corresponds to the volume occupied by the first resin particles in the ink. Therefore, if the first resin particles have pores or internal voids, the volume occupied by the first resin particles in the ink is a value including the pores and internal voids. Because the first resin particles are directly replaced by pores, the apparent density of the first resin particles is 0.8 g / cm. 3It is preferable that the apparent density is 0.8 g / cm or more. 3 If the binder content is less than 100%, it is difficult to generate enough resin to fill the gaps between the particles, which reduces the refractive index of the binder and may result in insufficient light scattering efficiency and hiding power.Furthermore, the amount of resin in the binder may be reduced, which may result in insufficient image strength.

[0050] The apparent density of the first resin particles can be measured, for example, according to the following procedure. 3 About 30 cm 3 The volumetric flask filled with the first resin particles is then filled with isopropanol up to the marked line. The mass of the isopropanol added to the volumetric flask is accurately weighed, and the apparent density (g / cm) of the first resin particles is calculated using the following formula (X): 3 In the examples described later, the apparent density of the first resin particles was measured and calculated by the above method. Alternatively, it can be measured using the Le Chatelier pycnometer method in accordance with JIS Z 8807. The apparent density (g / cm) of the first resin particles can be calculated by the Le Chatelier pycnometer method in accordance with JIS Z 8807. 3 )=A / (100-B) / C (X) A: mass (g) of the first resin particles B: mass (g) of isopropanol C: specific gravity of isopropanol at 25°C

[0051] Examples of resins that form the first resin particles include vinyl chloride resins, styrene resins, urethane resins, acrylic resins, and polyester resins. Among these, acrylic resins, polyester resins, and urethane resins are preferred from the viewpoint of inkjet characteristics. If first resin particles formed from a resin other than those mentioned above are used, ejection tends to become unstable, and as a result, sufficient image hiding power may not be obtained. Among these, acrylic resins are preferred, and acrylic resins having units derived from styrene are more preferred. Details of the resins that form the resin particles will be described later.

[0052] If the first resin particles melt before the heating step is performed, the mixing of the particles and the resin may not proceed quickly, or the first resin particles may fuse together, making it somewhat difficult to form the desired pores. If the desired pores are not formed, the light scattering efficiency may decrease, and the hiding power may be easily reduced. Therefore, it is preferable to use resin particles that do not substantially fuse under room temperature (25°C) conditions. Specifically, (i) the glass transition temperature Tg (°C) of the first resin particles is 25°C or higher; or (ii) the melting point T M It is preferable that the temperature (°C) is 25°C or higher, and the resin constituting the first resin particles is a crystalline resin.

[0053] Tg and T of the first resin particles M Although there is no particular upper limit to the Tg and Tc of the first resin particles, they are preferably 100° C. or less, and more preferably 80° C. or less. M can be measured using a differential scanning calorimeter (DSC).

[0054] In this specification, "resin particles" refers to a resin that is present in a state in which it is not dissolved in the aqueous medium of the ink, and more specifically refers to a resin that can be present in the aqueous medium in the form of particles whose particle diameter can be measured by dynamic light scattering. In contrast, "water-soluble resin" refers to a resin that is present in a state in which it is dissolved in the aqueous medium of the ink.

[0055] Whether a certain resin corresponds to "resin particles" can be determined according to the following method. First, a liquid containing the resin to be determined is prepared and diluted with pure water so that the resin content is approximately 1.0% to prepare a sample. Then, when the particle size of the resin in the sample is measured by dynamic light scattering, if particles having a particle size are measured, the resin is determined to be "resin particles" (i.e., a "water-dispersible resin"). On the other hand, if particles having a particle size are not measured, the resin is determined not to be "resin particles" (i.e., a "water-soluble resin"). The measurement conditions in this case can be, for example, Set Zero: 30 seconds, number of measurements: 10, measurement time: 120 seconds, shape: spherical, refractive index: 1.5, and density: 1.0.

[0056] As the particle size distribution measuring device, a particle size analyzer using a dynamic light scattering method (for example, trade name "UPA-EX150" manufactured by Nikkiso Co., Ltd.) can be used. Of course, the particle size distribution measuring device to be used and the measurement conditions are not limited to those described above.

[0057] Whether the resin constituting the resin particles is an amorphous resin or a crystalline resin can be determined by measuring the crystallinity using a differential scanning calorimeter. If no melting peak is observed using a differential scanning calorimeter, the resin can be determined to be an amorphous resin. On the other hand, if a melting peak is observed, the resin can be determined to be a crystalline resin. If the resin is a crystalline resin, the heat of fusion can be calculated from the peak area, and the crystallinity can be calculated from the ratio to the heat of fusion of a completely crystalline material with a crystallinity of 100% calculated by theoretical calculation.

[0058] The acid value of the resin constituting the first resin particles is preferably 5 mgKOH / g or more and 100 mgKOH / g or less. The weight average molecular weight of the resin constituting the first resin particles is preferably 1,000 or more and 3,000,000 or less, and more preferably 100,000 or more and 3,000,000 or less. The first resin particles do not need to contain a colorant.

[0059] As mentioned above, the first resin particles melt when heated, and the resin generated penetrates into the voids between the particles. As a result, voids are generated. For this reason, the properties of the first resin particles as a viscoelastic body, particularly the loss modulus related to viscosity, affect the ease with which voids are generated. The resin generated by melting penetrates into the voids between the particles, generating voids. For this reason, the properties of the first resin particles as a viscoelastic body, particularly the loss modulus related to viscosity, affect the ease with which the resin penetrates into the voids, that is, the ease with which the desired voids are generated. Therefore, the loss viscoelastic modulus of the resin at high temperatures becomes important. This loss modulus changes depending on the temperature. For example, the loss modulus of the first resin particles at 80°C is 1.0 x 10 7 Pa or less, and 5 It is more preferable that the viscosity is 0.05 Pa or less.

[0060] The particles are characterized by their glass transition temperature Tg (°C) or melting point T M(°C) is the glass transition temperature Tg (°C) or melting point T M The second resin particles may have a temperature higher than that of the first resin particles. The resin constituting the second resin particles may be the same as the resin constituting the first resin particles. In particular, the resin constituting the second resin particles is preferably a crosslinked resin, and more preferably a crosslinked acrylic resin.

[0061] [Resin] The ink may further contain a resin (other resin) other than the first resin particles. The content (mass %) of the resin (other resin) in the ink is preferably 0.1 mass % or more and 20.0 mass % or less, and more preferably 0.5 mass % or more and 15.0 mass % or less, based on the total mass of the ink.

[0062] Resins can be added to inks (i) to stabilize the dispersion state of pigments, i.e., as a resin dispersant or its auxiliary. Resins can also be added to inks (ii) to improve various properties of the recorded image. Examples of resin forms include block copolymers, random copolymers, graft copolymers, and combinations thereof. Furthermore, the resin is preferably a water-soluble resin that can be dissolved in an aqueous medium.

[0063] [Resin Composition] Examples of the resin include acrylic resins, urethane resins, olefin resins, etc. Among these, acrylic resins and urethane resins are preferred, and acrylic resins composed of units derived from (meth)acrylic acid or (meth)acrylate are more preferred.

[0064] The acrylic resin is preferably one having a hydrophilic unit and a hydrophobic unit as constituent units. Among these, a resin having a hydrophilic unit derived from (meth)acrylic acid and a hydrophobic unit derived from at least one monomer selected from the group consisting of a monomer having an aromatic ring and a (meth)acrylic acid ester-based monomer is preferred. A resin having a hydrophilic unit derived from (meth)acrylic acid and a hydrophobic unit derived from at least one monomer selected from the group consisting of styrene and α-methylstyrene is particularly preferred. These resins are prone to interact with pigments, and can therefore be suitably used as resin dispersants for dispersing pigments.

[0065] The hydrophilic unit is a unit having a hydrophilic group such as an anionic group. The hydrophilic unit can be formed, for example, by polymerizing a hydrophilic monomer having a hydrophilic group. Specific examples of hydrophilic monomers having a hydrophilic group include acidic monomers having a carboxylic acid group such as (meth)acrylic acid, itaconic acid, maleic acid, and fumaric acid, and anionic monomers such as anhydrides and salts of these acidic monomers. Examples of cations constituting the salts of acidic monomers include ions of lithium, sodium, potassium, ammonium, and organic ammonium. The hydrophobic unit is a unit that does not have a hydrophilic group such as an anionic group. The hydrophobic unit can be formed, for example, by polymerizing a hydrophobic monomer that does not have a hydrophilic group such as an anionic group. Specific examples of hydrophobic monomers include monomers having an aromatic ring such as styrene, α-methylstyrene, and benzyl (meth)acrylate; and (meth)acrylic acid ester monomers such as methyl (meth)acrylate, butyl (meth)acrylate, and 2-ethylhexyl (meth)acrylate.

[0066] The urethane resin can be obtained by reacting, for example, polyisocyanate with a polyol. Alternatively, a chain extender may be further added to the urethane resin. Examples of the olefin resin include polyethylene and polypropylene.

[0067] Polyester resins are typically composed of units derived from polyhydric alcohols and units derived from polycarboxylic acids. Examples of polyhydric alcohols that form the polyhydric alcohol-derived units that constitute polyester resins through reaction include dihydric, tetrahydric, and tetrahydric alcohols. Examples of polyhydric alcohols include polyhydric alcohols having aliphatic groups, polyhydric alcohols having aromatic groups, and sugar alcohols. Examples of polyhydric alcohols include dihydric alcohols such as ethylene glycol (1,2-ethanediol), neopentyl glycol (2,2-dimethyl-1,3-propanediol), 1,3-propanediol, 1,4-butanediol, benzenediol, and 2,2-bis(4-hydroxyphenyl)propane (bisphenol A); trihydric alcohols such as glycerin, trimethylolethane, and trimethylolpropane; and tetrahydric alcohols such as pentaerythritol. Furthermore, oligomers (low-molecular-weight polymers having a molecular weight of 1,000 or less) can also be used as polyhydric alcohols. It is preferable to use dihydric or trihydric polyhydric alcohols because it is easy to adjust the weight average molecular weight of the polyester resin.

[0068] Examples of polycarboxylic acids that form the polycarboxylic acid-derived units that constitute the polyester resin through reaction include divalent to tetravalent polycarboxylic acids. Examples of polycarboxylic acid structures include polycarboxylic acids having an aliphatic group, polycarboxylic acids having an aromatic group, and nitrogen-containing polycarboxylic acids. Examples of polycarboxylic acids include dicarboxylic acids such as glutaric acid, adipic acid, terephthalic acid, isophthalic acid, and 2,6-naphthalenedicarboxylic acid; tricarboxylic acids such as trimellitic acid; and tetracarboxylic acids such as ethylenediaminetetraacetic acid. Furthermore, oligomers (low-molecular polymers having a molecular weight of 1,000 or less) can also be used as polycarboxylic acids. Divalent or trivalent polycarboxylic acids are preferred because they allow for easy adjustment of the weight-average molecular weight and acid value of the polyester resin.

[0069] [Resin Properties] The water-soluble resin preferably has an acid value of 100 mgKOH / g or more and 250 mgKOH / g or less, and a weight-average molecular weight of 3,000 or more and 15,000 or less.

[0070] [Aqueous Medium] The ink used in the recording method of the present invention is an aqueous ink containing at least water as the aqueous medium. The ink may contain water or an aqueous medium that is a mixed solvent of water and a water-soluble organic solvent. Deionized water or ion-exchanged water is preferably used as the water. The water content (mass %) in the ink is preferably 50.0% to 95.0% by mass, based on the total mass of the ink. Furthermore, the water-soluble organic solvent content (mass %) in the ink is preferably 3.0% to 50.0% by mass, based on the total mass of the ink. As the water-soluble organic solvent, any of those usable in inkjet inks, such as alcohols, (poly)alkylene glycols, glycol ethers, nitrogen-containing compounds, and sulfur-containing compounds, can be used.

[0071] [Other Components] The ink may further contain water-soluble organic compounds that are solid at 25°C, such as urea or its derivatives, trimethylolpropane, and trimethylolethane. The content (mass %) of the water-soluble organic compounds in the ink is preferably 0.1 mass % or more and 10.0 mass % or less, based on the total mass of the ink. In addition to the above components, the ink may also contain various other components as needed. Examples of other components include various additives such as surfactants, antifoaming agents, pH adjusters, viscosity adjusters, rust inhibitors, preservatives, antifungal agents, antioxidants, and reduction inhibitors. However, it is preferable that the ink does not contain the reactant to be contained in the reaction liquid.

[0072] [Physical Properties of Ink] The ink is an aqueous ink applied to an inkjet system. Therefore, from the viewpoint of reliability, it is preferable to appropriately control its physical properties. Specifically, the surface tension of the ink at 25°C is preferably 20 mN / m or more and 60 mN / m or less. Furthermore, the viscosity of the ink at 25°C is preferably 1.0 mPa·s or more and 10.0 mPa·s or less. The pH of the ink at 25°C is preferably 7.0 or more and 9.5 or less, and more preferably 8.0 or more and 9.5 or less.

[0073] (Reaction Liquid) The recording method of the present invention preferably includes a reaction liquid application step of applying an aqueous reaction liquid containing a reactant that reacts with the aqueous ink to the recording medium. It is particularly preferred to include a reaction liquid application step before the ink application step, or to carry out the ink application step and the reaction liquid application step in parallel. Hereinafter, each component used in the reaction liquid will be described in detail.

[0074] [Reactant] The reaction liquid reacts with the ink upon contact with it to aggregate the components in the ink (resins and components having anionic groups, such as self-dispersible pigments), and contains a reactant. Examples of the reactant include organic acids, polyvalent metal salts, and cationic resins.

[0075] Examples of polyvalent metal ions include Ca 2+ , Cu 2+ , Ni 2+ , Mg 2+ , Sr 2+ , Ba 2+ , and Zn 2+ Divalent metal ions such as Fe 3+ , Cr 3+ , Y 3+ , and Al 3+ In order to incorporate polyvalent metal ions into the reaction solution, polyvalent metal salts (which may be hydrates) formed by combining polyvalent metal ions with anions can be used. Examples of anions include Cl. - ,Br - , I - , ClO - , ClO 2- , ClO 3 - , ClO 4 - , NO 2 - , NO 3 - , S.O. 4 2- , CO 3 2- , HCO 3 - , P.O. 4 3- , H.P.O. 4 2- , and H 2 P.O. 4 - Inorganic anions such as HCOO - , (COO - ) 2 , COOH (COO - ), C.H. 3 COO - , C 2 H 5 COO - , C.H. 3 CH(OH)COO - , C 2 H 4 (COO - ) 2 , C 6 H 5 COO - , C 6 H 4 (COO - ) 2 , and C.H. 3 SO 3 - Examples of organic anions include those mentioned above. When a polyvalent metal ion is used as the reactant, the content (% by mass) of the polyvalent metal salt in the reaction solution is preferably 1.0% by mass or more and 20.0% by mass or less, based on the total mass of the reaction solution. In this specification, when the polyvalent metal salt is a hydrate, the "content (% by mass) of the polyvalent metal salt" in the reaction solution means the "content (% by mass) of the anhydrous polyvalent metal salt" excluding water as the hydrate.

[0076] The organic acid-containing reaction solution has a buffering capacity in the acidic range (less than pH 7.0, preferably pH 2.0 to 5.0), thereby efficiently converting anionic groups present in the ink into the acid form and causing them to aggregate. Examples of organic acids include monocarboxylic acids and salts thereof, such as formic acid, acetic acid, propionic acid, butyric acid, benzoic acid, glycolic acid, lactic acid, salicylic acid, pyrrolecarboxylic acid, furancarboxylic acid, picolinic acid, nicotinic acid, thiophenecarboxylic acid, levulinic acid, and coumaric acid; dicarboxylic acids and salts thereof, such as oxalic acid, malonic acid, succinic acid, glutaric acid, adipic acid, maleic acid, fumaric acid, itaconic acid, sebacic acid, phthalic acid, malic acid, and tartaric acid; tricarboxylic acids and salts thereof, such as citric acid and trimellitic acid; and tetracarboxylic acids and salts thereof, such as pyromellitic acid. When an organic acid is used as a reactant, the content (mass %) of the organic acid in the reaction liquid is preferably 1.0 mass % or more and 50.0 mass % or less based on the total mass of the reaction liquid.

[0077] Examples of cationic resins include resins having a primary to tertiary amine structure and resins having a quaternary ammonium salt structure. Specific examples include resins having structures such as vinylamine, allylamine, vinylimidazole, vinylpyridine, dimethylaminoethyl methacrylate, ethyleneimine, guanidine, diallyldimethylammonium chloride, and alkylamine-epichlorohydrin condensates. To enhance solubility in the reaction solution, the cationic resin may be used in combination with an acidic compound or the cationic resin may be subjected to a quaternization treatment. When a cationic resin is used as a reactant, the content (mass %) of the cationic resin in the reaction solution is preferably 0.1% by mass or more and 10.0% by mass or less, based on the total mass of the reaction solution.

[0078] [Aqueous Medium] The reaction liquid is an aqueous reaction liquid containing at least water as the aqueous medium. The aqueous medium used in the reaction liquid may contain the water-soluble organic solvent that can be contained in the ink.

[0079] [Other Components] The reaction liquid may contain various other components as needed. Examples of other components include the same components as those that can be contained in the ink.

[0080] [Physical Properties of Reaction Liquid] The reaction liquid that can be suitably used in the recording method of the present invention is an aqueous reaction liquid that is applicable to inkjet printing. Therefore, from the viewpoint of reliability, it is preferable to appropriately control its physical properties. Specifically, the surface tension of the reaction liquid at 25°C is preferably 20 mN / m or more and 60 mN / m or less. Furthermore, the viscosity of the reaction liquid at 25°C is preferably 1.0 mPa·s or more and 10.0 mPa·s or less. The pH of the reaction liquid at 25°C is preferably 5.0 or more and 9.5 or less, more preferably 6.0 or more and 9.0 or less.

[0081] The present invention will be described in more detail below with reference to examples and comparative examples, but the present invention is not limited to these examples in any way as long as the gist of the invention is not exceeded. The terms "parts" and "%" used to describe component amounts are based on mass unless otherwise specified. Hereinafter, a particle dispersion will also be referred to as a pigment dispersion.

[0082] <Measurement of physical properties> (Average primary particle diameter of particles, cumulative 50% particle diameter on a volume basis) Using a scanning electron microscope (product name "S-4700", manufactured by Hitachi High-Technologies), the sample was photographed at a magnification of 100,000 times. Then, the diameters of 100 circles circumscribing the primary particles were measured, and the average value was calculated. The calculated average value was used as the average primary particle diameter D P0 In addition, a particle size measurement device using a dynamic light scattering method (trade name "UPA-EX150", manufactured by Nikkiso) was used to measure the cumulative 50% particle size D P The cumulative 50% particle diameter D of the resin particles based on the volume was measured. E was also measured using the particle size measuring device described above.

[0083] (Glass transition temperature and melting point of resin particles) The glass transition temperature Tg and melting point Tg of resin particles were measured using a differential scanning calorimeter (DSC). Mwas measured. Specifically, 2 mg of resin particles obtained by drying a liquid containing resin particles at 60°C was placed in an aluminum container and sealed to prepare a sample for measurement. The prepared sample was subjected to thermal analysis using a differential scanning calorimeter (trade name "DSC-2500", manufactured by TA Instruments) according to the temperature program shown below. The glass transition temperature of resin particles in this specification is defined as follows. That is, in the temperature rise curve of the following temperature program (3) (horizontal axis: temperature, vertical axis: heat quantity), the temperature at the intersection of a straight line extending from two points on the low-temperature side curve to the high-temperature side and a tangent drawn at the point where the gradient of the step-like change portion in the curve is maximum is determined. The temperature thus determined was defined as the "glass transition temperature Tg of the resin particles." Furthermore, for crystalline resins, the peak top of the endothermic peak in the above temperature rise curve was defined as the "melting point T M [Temperature program]: (1) Heat from 20°C to 200°C at 10°C / min. (2) Cool from 200°C to -50°C at 5°C / min. (3) Heat from -50°C to 200°C at 10°C / min.

[0084] (Loss Modulus of Resin Particles) The loss modulus of the resin particles was measured according to the following method. Approximately 10 g of an aqueous dispersion of resin particles was dropped onto a fluororesin plate and placed in a vacuum dryer (trade name "ADP300", manufactured by Yamato Scientific). The plate was dried under reduced pressure at 80°C for 30 minutes to prepare a sample for measurement. Using a viscoelasticity measuring device (trade name "Rheogel-E4000", manufactured by UBM), the prepared sample was compressed while heating to measure the loss modulus. The measurement conditions were: measurement jig: compression jig φ20; strain waveform: sine wave; vibration state: continuous vibration; fundamental frequency: 1 Hz; strain control: constant at 3 μm; start temperature: -20°C; step temperature: 2°C; end temperature: 80°C; and heating rate: 5°C / min.

[0085] (Particle Density) The density of the particles was measured by a Gay-Lussac type pycnometer method in accordance with JIS Z 8807. The density of the resin particles was also measured by the same method.

[0086] <Preparation of Particles (Pigment Dispersions)> The types of particles (particles 1 to 14) shown in Table 1 were prepared, and pigment dispersions 1 to 14 were prepared using the respective particles prepared.

[0087] For particles 1 to 3, 7, and 10, the particle content was adjusted to 30.0% by adding an appropriate amount of ion-exchanged water or evaporating the liquid component, thereby obtaining pigment dispersions 1 to 3, 7, and 10. For particles 4 to 6, 8, and 9, 10.0 parts of each particle, 0.8 parts of an acrylic dispersant (trade name "DISPERBYK-154", manufactured by BYK), and 100 parts of 0.1 mm zirconia beads were mixed and dispersed for 6 hours using a beads mill. The zirconia beads were filtered off, and an appropriate amount of ion-exchanged water was added as necessary to obtain pigment dispersions 4 to 6, 8, and 9.

[0088] A solution was obtained by dissolving 6.3 g of tetraethyl orthosilicate in a mixed solvent of 75.0 g of ethanol, 25.0 g of methanol, and 18.0 g of ion-exchanged water. 2.2 g of 28% aqueous ammonia was added to the resulting solution, and the mixture was stirred at 25°C for 24 hours to obtain pigment dispersion 11. Furthermore, D in Table 1 P Pigment Dispersion Liquid 12 was obtained in the same manner as in Pigment Dispersion Liquid 4, except that the dispersion treatment time was adjusted so that the particle diameter became (nm).

[0089] 30.0 parts of each titanium oxide (particles 13 and 14), 0.45 parts of potassium hydroxide, 69.55 parts of ion-exchanged water, and 100 parts of 0.1 mm zirconia beads were mixed and dispersed using a beads mill. The zirconia beads were filtered off, and an appropriate amount of ion-exchanged water was added as needed to obtain pigment dispersions 13 and 14. Note that D in Table 1 P The dispersion treatment time was adjusted appropriately so that the particle diameter was 100 nm.

[0090] Each pigment dispersion was appropriately adjusted so that the particle content was 30.0%. In Table 1, particles 4 and 12 are cubic calcium carbonate. Particle 5 is hydroxyapatite, a type of calcium phosphate. Particle 7 is stabilized zirconia with a stabilizer added. In Table 1, the refractive index of each titanium oxide was 2.5 or more and 2.8 or less. The refractive index of particles other than titanium oxide was 1.5 or more and 2.2 or less.

[0091]

[0092] <Preparation of Resin Particles> Aqueous dispersions of resin particles of the types shown in Table 2 were prepared. In Table 2, the content of resin particles in each aqueous dispersion of resin particles is shown in the column for "Resin Particle Content (%)." Aqueous dispersions of resin particles 2 and aqueous dispersions of resin particles 3 were each prepared according to the methods shown below.

[0093] (Aqueous Dispersion of Resin Particles 2) 300 g of sebacic acid and 170 g of 1,6-hexanediol were mixed and heated to 190°C over 1 hour while stirring. After adding 0.01 g of tetrabutyl orthotitanate, the internal temperature was raised to 240°C over 6 hours while distilling off the generated water, and polymerization was carried out to obtain a crystalline polyester resin. The melting point T M The temperature was 75°C. 50 g of the obtained polyester resin was placed in a 300 mL four-neck flask equipped with a nitrogen inlet tube, a stirrer, and a thermocouple. 50 g of methyl ethyl ketone was added, and the mixture was heated to 40°C under a nitrogen stream to dissolve the polyester resin. 1.2 g of triethylamine was further added and stirred for 1 hour, after which 106 g of ion-exchanged water was added dropwise at a rate of 7.5 g / min and stirred for 30 minutes. Next, the methyl ethyl ketone was removed under reduced pressure to obtain an aqueous dispersion of resin particles 2 with a resin particle content of 30.0%. The volume-based cumulative 50% particle diameter D of resin particles 2 measured using the above equipment was E was 190 nm.

[0094] (Aqueous Dispersion of Resin Particles 3) 300 g of sebacic acid and 170 g of 1,6-hexanediol were mixed and heated to 190°C over 1 hour while stirring. After adding 0.01 g of tetrabutyl orthotitanate, the internal temperature was raised to 240°C over 6 hours while distilling off the generated water, and polymerization was carried out to obtain a crystalline polyester resin. The melting point T M The temperature was 75°C. 50 g of the obtained polyester resin was placed in a 300 mL four-neck flask equipped with a nitrogen inlet tube, a stirrer, and a thermocouple. 50 g of methyl ethyl ketone was added, and the mixture was heated to 40°C under a nitrogen stream to dissolve the polyester resin. 1.0 g of triethylamine was further added and stirred for 1 hour, after which 106 g of ion-exchanged water was added dropwise at a rate of 7.5 g / min and stirred for 30 minutes. Next, the methyl ethyl ketone was removed under reduced pressure to obtain an aqueous dispersion of resin particles 3 with a resin particle content of 30.0%. The volume-based cumulative 50% particle diameter D of resin particles 3 measured using the above equipment was E was 230 nm.

[0095]

[0096] (Resin Particles 15 to 17) Resin particles 15 to 17 shown below were prepared. The density and apparent density of resin particles 15 to 17 were all 1.0 g / cm 3 Resin particles 15: styrene acrylic resin (trade name "Vinyblan 2685", manufactured by Nissin Chemical Industry Co., Ltd., amorphous, average particle size 210 nm, Tg 50°C, resin particle content 30.0%) Resin particles 16: styrene acrylic resin (trade name "Joncryl 450", manufactured by Johnson Polymer, amorphous, average particle size 90 nm, Tg 16°C, resin particle content 42.0%) Resin particles 17: styrene acrylic resin (trade name "WEM-3000", manufactured by Taisei Fine Chemical Co., Ltd., amorphous, average particle size 300 nm, Tg 98°C, resin particle content 33.0%)

[0097] <Preparation of Emulsion> (Emulsion 1) 0.3 parts of a fluorine-based nonionic surfactant (trade name "Capstone FS-31", manufactured by DuPont) was dissolved in 10.0 parts of ion-exchanged water. 4.0 parts of perfluorohexane was added, and the mixture was dispersed for 4 minutes using an ultrasonic disperser with a duty cycle of 50% to obtain Emulsion 1, an O / W emulsion.

[0098] <Ink Preparation> The components (unit: %) shown in the upper rows of Tables 3-1 to 3-3 were mixed. Potassium hydroxide was added to adjust the pH to within the range of 8 to 9. Each ink was prepared by pressure filtration using a 3.0 μm pore size microfilter (manufactured by Fujifilm). In Tables 3-1 to 3-3, "Acetylenol E100" is the trade name of a nonionic surfactant (acetylene glycol ethylene oxide adduct) manufactured by Kawaken Fine Chemicals. The properties of the prepared inks are shown in the lower rows of Tables 3-1 to 3-3. As shown in Table 3-3, 8.3 parts and 10.7 parts of resin particles 16 and 17, respectively, were used to prepare ink 38.

[0099]

[0100]

[0101]

[0102] <Preparation of Reaction Solution> (Reaction Solution 1) 10.0 parts of magnesium sulfate heptahydrate, 2.0 parts of glycerin, 7.0 parts of ethylene glycol, 0.5 parts of a nonionic surfactant (trade name "Acetylenol E100", manufactured by Kawaken Fine Chemicals), and ion-exchanged water were mixed to obtain reaction solution 1. The amount of ion-exchanged water was appropriately adjusted so that the total amount of the components was 100.0 parts.

[0103] (Reaction Solution 2) 37.0 parts of a cationic resin, 2.0 parts of glycerin, 7.0 parts of ethylene glycol, 0.5 parts of Acetylenol E100, and 53.5 parts of ion-exchanged water were mixed to obtain Reaction Solution 2. The cationic resin used was a product name "Unisense FPA100L" (manufactured by Senka, cationic resin content: 27.0%).

[0104] (Reaction Solution 3) Reaction solution 3 was obtained by mixing 10.0 parts of succinic acid, 2.0 parts of glycerin, 7.0 parts of ethylene glycol, 0.5 parts of Acetylenol E100, and 81.5 parts of ion-exchanged water.

[0105] <Evaluation> Each of the inks obtained above was evaluated for the following items. In the present invention, in the evaluation criteria for each item shown below, "AA", "A", and "B" were considered acceptable levels, and "C" was considered unacceptable. The evaluation results are shown on the right side of Table 4.

[0106] (Recording of Evaluation Image) An inkjet recording device (trade name "PIXUS PRO-10S", manufactured by Canon) equipped with a recording head that ejects liquid by the action of thermal energy was prepared. The types of ink shown on the left side of Table 4 were filled into ink cartridges and set in the prepared inkjet recording device. In this example, the recording duty of a solid image recorded at a resolution of 600 dpi x 600 dpi under conditions in which eight ink droplets, each with a mass of 3.5 ng, are applied to a unit area of ​​1 / 600 inch x 1 / 600 inch, is defined as 100%. Using this inkjet recording device, ink was ejected from the ejection ports in the lower half of the longitudinal direction of the recording head to record an image (50 mm x 50 mm) with a recording duty of 400% on the recording medium. The recording medium was a PET film (trade name "LLRPCF1372", manufactured by Sakurai, 30 msec from the start of contact in the Bristow method). 1/2 The water absorption rate is 0 mL / m 2 10mL / m or more 2 The material was cut into A4 size pieces (within the range below).

[0107] In Table 4, in examples where a reaction liquid application step is "included," the type of reaction liquid shown in Table 4 was filled into an ink cartridge, and the reaction liquid was applied to the recording medium in parallel with the application of the ink. The printing duty of the reaction liquid was 40%. The reaction liquid indicated by the number in the reaction liquid application step column was used. In examples where a drying step is "included" in Table 4, the recording medium was transported for half the length of the recording head in the longitudinal direction, and then hot air at 25°C was applied for 5 minutes to dry the image. The temperature of the hot air was measured at the hot air outlet using a molded surface sensor (product name "MF-O-K," manufactured by Toa Denki).

[0108] Thereafter, in the example of heating step "1" in Table 4, the recording medium on which the image was recorded was placed in a thermostatic chamber at 100°C for 5 minutes to perform a heat treatment, thereby fixing the image on the recording medium. H In the example of the heating step "2", the image was fixed on the recording medium in the same manner as in the heating step "1" except that the temperature of the thermostatic bath was set to 80°C. H The heating temperature was 70° C. or higher and lower than 80° C. Heating in a thermostatic chamber corresponds to heating of the recording surface and the back surface by an infrared heater. In Examples 21, 37, and 38, the reaction liquid was applied in parallel with the application of the ink, and the drying step and the heating step were carried out in this order.

[0109] In the example of the heating step "3", the recording medium was conveyed by half the length in the longitudinal direction of the recording head, and then hot air of 90°C was blown onto the recording medium at a speed of 11 m / s for 1 minute to dry the image. H In the example of heating step "4", the recording medium was conveyed by half the length in the longitudinal direction of the recording head, and then hot air of 110°C was blown onto the recording medium at a speed of 15 m / s for 10 seconds to dry the image. H The temperature was about 90°C.

[0110] (Formation of voids) Whether or not the resin particles had melted and voids had formed was determined using the following method. A portion of the recording medium to which the ink had been applied was cut before and after the heating process, and the cross section was observed using a scanning electron microscope. If resin particles were observed on the cross section before the heating process, the particle diameter was measured. If voids were observed on the cross section after the heating process, the void diameter was measured. If the difference between the measured void diameter and the particle diameter of the resin particles was 10% or less, it was determined that the resin particles had melted and voids had formed during the heating process. The evaluation results are shown in the "void formation" column in Table 4.

[0111] (Hiding ability) The hiding rate of the evaluation image recorded according to a method in accordance with ISO2471:2008 was measured and calculated, and the hiding rate of the image was evaluated. The ink prepared in each example was a white ink. In ISO2471:2008, the test paper is backed with a white board and a black board, respectively, to measure the reflectance, and the hiding rate is calculated using the following formula (B). Hiding rate = (R 0 / R ∞ )×100...(B) R 0 : Reflectance measured with a black board as backing R ∞ : Reflectance measured with a white board as the backing

[0112] In this example, the hiding rate of the recorded image was measured and calculated according to this method using a hiding rate test paper (manufactured by TP Giken, with inspection certificate from the Japan Paint Inspection Association). The hiding property of the image was evaluated according to the following evaluation criteria: AA: The hiding rate was 60% or more. A: The hiding rate was 55% or more and less than 60%. B: The hiding rate was 45% or more and less than 55%. C: The hiding rate was less than 45%.

[0113] (Sedimentation Resistance) The prepared ink was placed in a cylindrical sample container to a height of 24 mm and left in an environment of 25°C for one week. After leaving the container, the thickness (mm) of the transparent portion of the supernatant was measured, and the sedimentation resistance of the ink was evaluated according to the following evaluation criteria. A: The thickness of the transparent portion of the supernatant was 2 mm or less. B: The thickness of the transparent portion of the supernatant was more than 2 mm but not more than 10 mm. C: The thickness of the transparent portion of the supernatant was more than 10 mm.

[0114]

[0115] The evaluation results of the hiding power of the images of Examples 25 and 26 were "A", the same as Examples 4 to 6, but Examples 4 to 6 were superior. The evaluation result of the hiding power of the image of Example 29 was "B", the same as Examples 27 and 28, but Examples 27 and 28 were superior. The evaluation result of the hiding power of the image of Example 31 was "A", the same as the evaluation result of Example 32, but Example 32 was superior.

[0116] The present invention is not limited to the above-described embodiments, and various modifications and variations can be made without departing from the spirit and scope of the present invention. Therefore, the following claims are appended to apprise the public of the scope of the present invention.

[0117] This application claims priority based on Japanese Patent Application No. 2023-084008 filed on May 22, 2023 and Japanese Patent Application No. 2024-062310 filed on April 8, 2024, the entire contents of which are incorporated herein by reference.

[0118] 1 Particle 2 First resin particle 3 Binder 4 Hole

Claims

1. An inkjet recording method for recording an image on a recording medium using an aqueous ink containing particles and first resin particles, comprising: an ink application step of applying the aqueous ink to the recording medium; and measuring the temperature of the recording medium to which the aqueous ink has been applied at a glass transition temperature Tg (°C) or a melting point T of the first resin particles. M (°C) or higher, and the glass transition temperature Tg (°C) or melting point T M (° C.), and a heating step of heating the particles to a temperature of less than an average primary particle diameter D P0 (nm) is 150 nm or less, and in the heating step, the recording medium is heated to melt the first resin particles and generate voids.

2. The volume-based cumulative 50% particle diameter D of the first resin particles E 2. The ink jet recording method according to claim 1, wherein (nm) is 100 nm or more and 400 nm or less.

3. An inkjet recording method as described in claim 1, wherein the content (volume %) of the first resin particles in the aqueous ink is 1.3 times or more and 5.0 times or less in volume relative to the content (volume %) of the particles.

4. The ink-jet recording method according to claim 1, wherein the first resin particles have a glass transition temperature Tg (° C.) of 25° C. or higher.

5. The melting point T of the first resin particles M The ink-jet recording method according to claim 1, wherein the temperature (°C) is 25°C or higher, and the resin constituting the first resin particles is a crystalline resin.

6. The loss modulus of the first resin particles at 80° C. is 1.2×10 7 The ink-jet recording method according to claim 1, wherein the viscosity is 0.01 Pa or less.

7. The loss modulus of the first resin particles at 80° C. is 3.3×10 5 The ink-jet recording method according to claim 1, wherein the viscosity is 0.01 Pa or less.

8. The ink jet recording method according to claim 1, wherein the resin constituting the first resin particles is at least one type selected from the group consisting of acrylic resins, polyester resins, and urethane resins.

9. The apparent density of the first resin particles is 0.8 g / cm 3 The ink-jet recording method according to claim 1, 10. Cumulative 50% particle diameter D of the particles based on volume P 2. The ink jet recording method according to claim 1, wherein (nm) is 150 nm or less.

11. The ink jet recording method according to claim 1, wherein the particles are at least one type selected from the group consisting of titanium oxide, calcium carbonate, calcium phosphate, barium sulfate, zirconium oxide, silicon dioxide, kaolin, clay, and second resin particles.

12. An inkjet recording method as described in claim 1, wherein the particles are titanium oxide, and the content (mass %) of the first resin particles in the aqueous ink is 0.30 times or more and 1.0 times or less in mass ratio to the content (mass %) of the titanium oxide.

13. The volume-based cumulative 50% particle diameter D of the titanium oxide P The ink jet recording method according to claim 12, wherein (nm) is 100 nm or less.

14. The ink-jet recording method according to any one of claims 1 to 13, wherein the content (volume %) of the particles in the aqueous ink is 1.5 volume % or more based on the total volume of the ink.

15. Heating temperature T in the heating step H The ink-jet recording method according to any one of claims 1 to 13, wherein (°C) is 80°C or higher.

16. An inkjet recording method according to any one of claims 1 to 13, further comprising at least one step selected from the group consisting of a reaction liquid application step of applying an aqueous reaction liquid containing a reactant that reacts with the aqueous ink to the recording medium, and a drying step of drying the liquid component on the recording medium.

17. The ink-jet recording method according to any one of claims 1 to 13, wherein the water-based ink is a white ink.

18. An inkjet recording apparatus for use in an inkjet recording method for recording an image on a recording medium using an aqueous ink containing first resin particles and a first resin particle, comprising: an ink applying means for applying the aqueous ink to the recording medium; and a measuring means for measuring the glass transition temperature Tg (°C) or the melting point T of the first resin particles. M (°C) or higher, and the glass transition temperature Tg (°C) or melting point T M (° C.), and a heating means for heating the particles to a temperature less than an average primary particle diameter D P0 (nm) is 150 nm or less, and the heating means heats the recording medium to melt the first resin particles and generate voids.

19. An aqueous ink used in an inkjet recording method for recording an image on a recording medium using an aqueous ink containing first resin particles and first resin particles, the inkjet recording method comprising: an ink application step of applying the aqueous ink to the recording medium; and measuring the temperature of the recording medium to which the aqueous ink has been applied at a glass transition temperature Tg (°C) or a melting point T M (°C) or higher, and the glass transition temperature Tg (°C) or melting point T M (° C.), and a heating step of heating the particles to a temperature of less than an average primary particle diameter D P0 (nm) is 150 nm or less, and in the heating step, the recording medium is heated to melt the first resin particles and generate voids.

Citation Information

Patent Citations

  • White inkjet ink for textile printing

    JP2013060513A

  • Electronic apparatus

    JP2023084008A

  • Method for producing inorganic flocculant

    JP2024062310A

  • Ink set, inkjet recording method, inkjet recording device and recorded matter

    JP2017210528A

  • White ink, ink storage container, recording device, recording method, and recorded matter

    JP2020169232A