Colloidal silica and method for producing same
Organopolysiloxane dispersants with acid anhydride structures in colloidal silica address viscosity issues and contamination concerns, ensuring effective long-term performance as a polishing abrasive for semiconductor processes.
Patent Information
- Application Number
- PCT/JP2024/018644
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-05-24
- Filing Date
- 2024-05-21
- Publication Date
- 2024-11-28
AI Technical Summary
Colloidal silica used in CMP processes experiences increased viscosity over time, leading to reduced effectiveness as an abrasive, and existing methods to prevent this often result in silica aggregation or contamination from metal impurities.
The use of an organopolysiloxane with an acid anhydride structure or its hydrolyzed form as a dispersant in colloidal silica, allowing for high concentration without significant viscosity increase during long-term storage without surface treatment of silica particles.
The colloidal silica maintains low viscosity at high concentrations and exhibits minimal viscosity increase over time, enhancing its performance as a polishing abrasive for semiconductor devices and silicon wafers.
Smart Images

Figure JPOXMLDOC01-APPB-C000001 
Figure JPOXMLDOC01-APPB-C000002 
Figure JPOXMLDOC01-APPB-C000003
Abstract
Description
Colloidal silica and its manufacturing method
[0001] The present invention relates to colloidal silica and a method for producing the same.
[0002] BACKGROUND ART With the recent remarkable miniaturization of semiconductor devices, colloidal silica, which has small silica particles, is used in processes such as silicon wafer polishing and chemical mechanical polishing (hereinafter referred to as "CMP") of semiconductor devices.
[0003] As colloidal silica for CMP processes, high-purity colloidal silica with extremely low metal impurities is required to prevent contamination of silicon wafers, etc. Patent Document 1 discloses a method for producing colloidal silica modified with a silane coupling agent having a cationic group, which has a low content of metal impurities. However, the presence of cationic groups on the silica surface can cause hydrogen bonding between the cationic groups and silanol groups, or the cationic groups can act as a condensation catalyst between silanol groups, causing aggregation of silica particles.
[0004] Furthermore, producing colloidal silica with a high silica concentration is desirable not only because it improves production efficiency but also because it improves storage and transportation efficiency and allows for free adjustment of the blending ratio of the abrasives used in polishing, thereby increasing the degree of blending freedom. On the other hand, when colloidal silica is used in a CMP process, there is a problem that if it is reused, the viscosity of the colloidal silica increases, preventing it from fully demonstrating its effectiveness as an abrasive. Therefore, there is a demand for colloidal silica that is high in concentration and exhibits little increase in viscosity over a long period of time.
[0005] Therefore, Patent Documents 2 and 3 disclose a method of adding an inorganic or organic acid dispersant, such as sulfuric acid, nitric acid, or citric acid, to colloidal silica in order to improve the dispersibility of high-concentration colloidal silica. While the use of these dispersants makes it possible to improve the dispersibility of colloidal silica while preventing the inclusion of metal impurities, there are cases in which the silica aggregates or the viscosity increases due to changes in the pH value during long-term storage.
[0006] Patent Document 4 discloses a method for producing a surface-treated water-dispersed colloidal silica that is free of metal impurities and dispersants, has a high concentration, and shows little increase in viscosity over a long period of time, by treating a portion of the surface of water-dispersed colloidal silica obtained by a sol-gel method in the presence of a hydrophilic organic solvent with a trifunctional silane compound or the like, and then replacing the dispersion medium with water. However, because this method requires surface treatment of the silica, a simpler method has been desired.
[0007] Japanese Patent Application Laid-Open No. 2005-162533 Japanese Patent No. 5270344 Japanese Patent Application Laid-Open No. 2019-172558 Japanese Patent Application Laid-Open No. 2023-5414
[0008] Therefore, an object of the present invention is to provide colloidal silica that has a low viscosity even at high concentrations and that does not increase in viscosity much during long-term storage.
[0009] As a result of extensive research conducted by the present inventors in order to achieve the above object, they discovered that by using an organopolysiloxane having a group with an acid anhydride structure, a group with a structure formed by hydrolysis of an acid anhydride, or both as a dispersant, it is possible to obtain colloidal silica that has a low viscosity even at high concentrations and that shows little increase in viscosity during long-term storage, even without surface treatment of the silica, and thus completed the present invention.
[0010] That is, the present invention provides the following colloidal silica and a method for producing colloidal silica. [1] Colloidal silica containing silica particles, a dispersant comprising an organopolysiloxane having a group having an acid anhydride structure, a group having a structure formed by hydrolysis of an acid anhydride, or both, and water. [2] Colloidal silica according to [1], wherein the silica particles are sol-gel silica particles surface-treated with a trifunctional silane compound represented by the following formula (II): R 2 Si(OR 3 )3 (II) (wherein, R 2 represents a substituted or unsubstituted monovalent hydrocarbon group having 1 to 20 carbon atoms, R 3each independently represents a monovalent hydrocarbon group having 1 to 6 carbon atoms.) [3] A colloidal silica according to [1] or [2], wherein the silica particles have a Z-average particle size of 5 to 300 nm as measured by a dynamic light scattering method. [4] A colloidal silica according to any one of [1] to [3], wherein the dispersant is at least one selected from the group consisting of organopolysiloxanes represented by the following general formula (1) and organopolysiloxanes represented by the following general formula (2): (In the formula, R 4 are independently a substituted or unsubstituted alkyl group having 1 to 4 carbon atoms or a group represented by the following formula (3) or (4), and R 4 At least two of the groups are groups represented by the following formula (3) or (4), and k is an integer of 0 to 150. (In the formula, R 6 each independently represents a substituted or unsubstituted alkyl group having 1 to 4 carbon atoms; R 5 are independently a group represented by the following formula (3) or (4), m is an integer of 2 to 5, n is an integer of 0 to 3, and the sum of m and n is 4 or 5. The order of arrangement of the siloxane units is arbitrary. (In the formula, the wavy line represents a bond.) [5] The colloidal silica according to any one of [1] to [4], wherein the amount of dispersant is 10 to 3,000 ppm by mass relative to the silica particles. [6] The colloidal silica according to any one of [1] to [5], wherein the concentration of metal impurities is 0 to 1 ppm by mass. [7] The colloidal silica according to any one of [1] to [6], wherein the concentration of the hydrophilic organic solvent is 0 to 1% by mass. [8] The colloidal silica according to any one of [1] to [7], wherein the solid content is 30 to 50% by mass. [9] The colloidal silica according to any one of [1] to [7], wherein the kinematic viscosity at 25°C is 1 to 100 mm 2
[10] A chemical mechanical polishing liquid containing the colloidal silica according to any one of [1] to [9].
[11] A method for producing the colloidal silica according to any one of [1] and [3] to [9], comprising the following steps (A1), (A3'), and (A4'): Step (A1): A step of hydrolyzing and condensing a tetrafunctional silane compound represented by the following formula (I), a partial hydrolysis condensate thereof, or a mixture thereof, in a mixed liquid containing a hydrophilic organic solvent and water in the presence of a basic substance, to obtain colloidal silica (A1): Si(OR 1 )4 (I) (wherein, R 1 each independently represents a monovalent hydrocarbon group having 1 to 6 carbon atoms.) Step (A3'): a step of adding a dispersant composed of an organopolysiloxane having a group having an acid anhydride structure, a group having a structure obtained by hydrolysis of an acid anhydride, or both, to the colloidal silica (A1) obtained in Step (A1), to obtain a dispersant-containing colloidal silica (A3'). Step (A4'): a step of replacing the hydrophilic organic solvent in the dispersion medium of the dispersant-containing colloidal silica (A3') obtained in Step (A3') with water.
[12] A method for producing colloidal silica according to any one of Items [2] to [9], which comprises the following steps (A1), (A2), (A3), and (A4): Step (A1): a step of hydrolyzing and condensing a tetrafunctional silane compound represented by the following formula (I), a partial hydrolysis condensate thereof, or a mixture thereof, in a mixed liquid containing a hydrophilic organic solvent and water in the presence of a basic substance, to obtain a colloidal silica: Si(OR 1 )4 (I) (wherein, R 1 each independently represents a monovalent hydrocarbon group having 1 to 6 carbon atoms. Step (A2): To the colloidal silica (A1) obtained in step (A1), a trifunctional silane compound represented by the following formula (II), a partial hydrolysis condensate thereof, or a mixture thereof is added, and R 2 SiO 3 / 2 Step R of introducing units to obtain surface-treated colloidal silica (A2) 2 Si(OR 3 )3 (II) (wherein, R 2represents a substituted or unsubstituted monovalent hydrocarbon group having 1 to 20 carbon atoms, R 3 each independently represents a monovalent hydrocarbon group having 1 to 6 carbon atoms.) Step (A3): a step of adding a dispersant composed of an organopolysiloxane having a group having an acid anhydride structure, a group having a structure obtained by hydrolysis of an acid anhydride, or both, to the surface-treated colloidal silica (A2) obtained in step (A2), to obtain a dispersant-containing surface-treated colloidal silica (A3). Step (A4): a step of replacing the hydrophilic organic solvent in the dispersion medium of the dispersant-containing surface-treated colloidal silica (A3) obtained in step (A3) with water.
[13] The method for producing colloidal silica according to
[12] , wherein in step (A2), the amount of the trifunctional silane compound represented by formula (II), its partial hydrolysis condensate, or a mixture thereof added is 0.001 to 1 mol per 1 mol of SiO units in the colloidal silica (A1) obtained in step (A1).
[14] The method for producing colloidal silica according to any one of
[11] to
[13] , wherein the dispersant is at least one selected from organopolysiloxanes represented by the following general formula (1) and organopolysiloxanes represented by the following general formula (2): (In the formula, R 4 are independently a substituted or unsubstituted alkyl group having 1 to 4 carbon atoms or a group represented by the following formula (3) or (4), and R 4 At least two of the groups are groups represented by the following formula (3) or (4), and k is an integer of 0 to 150. (In the formula, R 6 each independently represents a substituted or unsubstituted alkyl group having 1 to 4 carbon atoms; R 5 are independently a group represented by the following formula (3) or (4), m is an integer of 2 to 5, n is an integer of 0 to 3, and the sum of m and n is 4 or 5. The order of arrangement of the siloxane units is arbitrary. (In the formula, the wavy line represents a bond.)
[0011] The colloidal silica of the present invention has a low viscosity even at high concentrations and shows little increase in viscosity during long-term storage, making it extremely useful as abrasive grains for polishing silicon wafers and CMP processes for semiconductor devices.
[0012] The colloidal silica of the present invention contains silica particles, a dispersant comprising an organopolysiloxane having a group with an acid anhydride structure, a group with a structure formed by hydrolysis of an acid anhydride, or both, and water.
[0013] [Silica Particles] The silica particles contained in the colloidal silica of the present invention are not particularly limited as long as they are silica dispersible in water, but sol-gel silica is preferred, and sol-gel silica particles surface-treated with a trifunctional silane compound represented by the following formula (II) are more preferred. 2 Si(OR 3 )3 (II) (wherein, R 2 represents a substituted or unsubstituted monovalent hydrocarbon group having 1 to 20 carbon atoms, R 3 each independently represents a monovalent hydrocarbon group having 1 to 6 carbon atoms.
[0014] In the above formula (II), R 2 is a monovalent hydrocarbon group having 1 to 20 carbon atoms, preferably 1 to 10 carbon atoms, and particularly preferably 1 to 3 carbon atoms. 2 Examples of the monovalent hydrocarbon group represented by the formula (I) include alkyl groups such as methyl, ethyl, propyl, isopropyl, butyl, hexyl, octyl, and decyl, and particularly preferred are methyl, ethyl, and propyl. Some or all of the hydrogen atoms in these monovalent hydrocarbon groups may be substituted with halogen atoms such as fluorine, chlorine, and bromine, preferably fluorine atoms.
[0015] In the above formula (II), R 3 R is a monovalent hydrocarbon group having 1 to 6 carbon atoms, preferably having 1 to 4 carbon atoms, and particularly preferably having 1 or 2 carbon atoms. 3 Examples of the monovalent hydrocarbon group represented by the formula (I) include a methyl group, an ethyl group, a propyl group, a butyl group, and a phenyl group. Of these, a methyl group, an ethyl group, a propyl group, and a butyl group are preferred, and a methyl group and an ethyl group are particularly preferred.
[0016] Specific examples of the trifunctional silane compound represented by formula (II) above include methyltrimethoxysilane, methyltriethoxysilane, ethyltrimethoxysilane, ethyltriethoxysilane, n-propyltrimethoxysilane, n-propyltriethoxysilane, i-propyltrimethoxysilane, i-propyltriethoxysilane, butyltrimethoxysilane, butyltriethoxysilane, hexyltrimethoxysilane, 3,3,3-trifluoropropyltrimethoxysilane, and (heptadecafluoro-1,1,2,2-tetrahydrodecyl)trimethoxysilane.
[0017] The silica particles contained in the colloidal silica of the present invention preferably have a Z-average particle size of 5 to 300 nm, more preferably 10 to 150 nm, as measured by dynamic light scattering. The Z-average particle size as measured by dynamic light scattering can be measured using, for example, a Zetasizer Ultra (manufactured by Malvern Instruments).
[0018] [Dispersant] The colloidal silica of the present invention contains, as a dispersant, an organopolysiloxane having a group having an acid anhydride structure, a group having a structure formed by hydrolysis of an acid anhydride, or both.
[0019] Such organopolysiloxanes include linear, branched, cyclic, and three-dimensional network organopolysiloxanes, and particularly preferred are organopolysiloxanes represented by the following general formula (1) and organopolysiloxanes represented by the following general formula (2):
[0020] (In the formula, R 4 are independently a substituted or unsubstituted alkyl group having 1 to 4 carbon atoms or a group represented by the following formula (3) or (4), and R 4 At least two of the groups are groups represented by the following formula (3) or (4), and k is an integer of 0 to 150.
[0021] (In the formula, R 6 each independently represents a substituted or unsubstituted alkyl group having 1 to 4 carbon atoms; R 5are independently a group represented by the following formula (3) or (4), m is an integer of 2 to 5, n is an integer of 0 to 3, and the sum of m and n is 4 or 5. The order of arrangement of the siloxane units is arbitrary.
[0022] (In the formula, the wavy line represents a bond.)
[0023] In the above formulas (3) and (4), R 4 and R 6 Examples of the alkyl group having 1 to 4 carbon atoms include a methyl group, an ethyl group, an n-propyl group, an isopropyl group, an n-butyl group, a sec-butyl group, and a tert-butyl group, and particularly preferred are a methyl group, an ethyl group, and an n-propyl group. Some or all of the hydrogen atoms of these monovalent hydrocarbon groups may be substituted with halogen atoms such as fluorine atoms, chlorine atoms, and bromine atoms, and preferably fluorine atoms.
[0024] In the above formula (1), k is an integer of 0 to 150, and is preferably an integer of 1 to 30 from the viewpoints of viscosity and solubility in water.
[0025] In the above formula (2), m is an integer of 2 to 5, preferably an integer of 2 to 4. n is an integer of 0 to 3, preferably an integer of 0 to 2. m+n is 4 or 5, preferably 4.
[0026] Specific examples of preferred dispersants include organopolysiloxanes represented by the following formulas and organopolysiloxanes in which the acid anhydride structure contained therein has been partially or completely hydrolyzed.
[0027]
[0028]
[0029]
[0030]
[0031] These organopolysiloxanes can be produced, for example, by the hydrosilylation reaction of an organohydrogenpolysiloxane with allylsuccinic anhydride, using known hydrosilylation reaction conditions.
[0032] These dispersants may be used alone or in combination of two or more.
[0033] Generally, it is thought that as the concentration of silica particles in colloidal silica increases, the distance between silica particles decreases, hydrogen bonds are formed between the silanol groups between the silica particles, and viscosity increases. However, these dispersants act on the particles to block the hydrogen bonds between the silica particles, preventing aggregation even at high silica concentrations and suppressing the increase in viscosity of the colloidal silica.
[0034] The amount of the dispersant is preferably 10 to 3000 ppm by mass, more preferably 500 to 2000 ppm by mass, relative to the silica particles.
[0035] [Dispersion Medium] The colloidal silica of the present invention contains water as a dispersion medium. As a dispersion medium other than water, a hydrophilic organic solvent may be contained. Examples of the hydrophilic organic solvent include alcohols such as methanol, ethanol, 1-propanol, 2-propanol, and t-butanol; ethers such as tetrahydrofuran and dioxane; and glycols such as diethylene glycol and dipropylene glycol, with alcohols being preferred.
[0036] The concentration of the hydrophilic organic solvent in the colloidal silica of the present invention is preferably 0 to 1 mass %, more preferably 0 to 100 mass ppm, and particularly preferably 0 to 10 mass ppm.
[0037] The total concentration of metal impurities such as sodium, potassium, iron, calcium, magnesium, titanium, nickel, chromium, and copper in the colloidal silica of the present invention is preferably 0 to 1 ppm by mass, and more preferably 0 to 0.5 ppm by mass, relative to the total mass of the colloidal silica.
[0038] The solid content concentration (concentration of silica particles) of the colloidal silica of the present invention is preferably 30% by mass or more, and more preferably 30 to 50% by mass.
[0039] The kinematic viscosity of the colloidal silica of the present invention at 25°C is 1 to 100 mm 2 / s, and 5 to 20 mm 2 Within this range, the powder is suitable for use as an abrasive.
[0040] The colloidal silica of the present invention may contain other components as long as they do not impair the dispersion stability of the silica. For example, preservatives, bactericides, and biocides may be added to prevent bacterial growth. Examples of such compounds include hydrogen peroxide, ammonia, quaternary ammonium hydroxides, quaternary ammonium salts, ethylenediamine, glutaraldehyde, hydrogen peroxide, methyl p-hydroxybenzoate, isothiazoline compounds such as 2-methyl-4-isothiazolin-3-one, 5-chloro-2-methyl-4-isothiazolin-3-one, and 1,2-benzisothiazoline, and phenoxyethanol.
[0041] [Method for Producing Colloidal Silica] The colloidal silica of the present invention can be obtained by a production method including the following steps (A1), (A3'), and (A4'): Step (A1): A synthesis step for obtaining colloidal silica; Step (A3'): A step for adding a dispersant; and Step (A4'): A step for replacing the dispersion medium.
[0042] The method for producing colloidal silica of the present invention preferably includes the following steps (A1), (A2), (A3), and (A4): Step (A1): A synthesis step for obtaining colloidal silica; Step (A2): A surface treatment step using a trifunctional silane compound; Step (A3): A dispersant addition step; and Step (A4): A dispersion medium substitution step.
[0043] Step (A1): Synthesis Step for Obtaining Colloidal Silica This step is a step for obtaining colloidal silica (A1) by hydrolyzing and condensing a tetrafunctional silane compound represented by the following formula (I), its partial hydrolysis condensate, or a mixture thereof in a mixed liquid containing a hydrophilic organic solvent and water in the presence of a basic substance. Si(OR 1 )4 (I) (wherein, R 1 each independently represents a monovalent hydrocarbon group having 1 to 6 carbon atoms.
[0044] In the above formula (I), R1 R is a monovalent hydrocarbon group having 1 to 6 carbon atoms, preferably having 1 to 4 carbon atoms, and particularly preferably having 1 or 2 carbon atoms. 1 Examples of the monovalent hydrocarbon group represented by the formula (I) include a methyl group, an ethyl group, a propyl group, a butyl group, and a phenyl group. Of these, a methyl group, an ethyl group, a propyl group, and a butyl group are preferred, and a methyl group and an ethyl group are particularly preferred.
[0045] Examples of the tetrafunctional silane compound represented by the formula (I) include tetraalkoxysilanes such as tetramethoxysilane, tetraethoxysilane, tetrapropoxysilane, and tetrabutoxysilane, and tetraphenoxysilane, among which tetramethoxysilane, tetraethoxysilane, tetrapropoxysilane, and tetrabutoxysilane are preferred, and tetramethoxysilane and tetraethoxysilane are particularly preferred. Examples of the hydrolysis condensate of the tetrafunctional silane compound represented by the formula (I) include methyl silicate and ethyl silicate.
[0046] Examples of basic substances include ammonia, dimethylamine, diethylamine, etc., and ammonia and diethylamine are preferred, with ammonia being particularly preferred. These basic substances can be used by dissolving the required amount in water.
[0047] The hydrophilic organic solvent is not particularly limited as long as it dissolves the compound represented by formula (I) and / or its partial hydrolysis condensate, as well as water, and examples thereof include alcohols such as methanol, ethanol, 1-propanol, 2-propanol, and t-butanol; ethers such as tetrahydrofuran and dioxane; and glycols such as diethylene glycol and dipropylene glycol, with alcohols being preferred. Since the particle size of the produced silica particles increases as the number of carbon atoms in the alcohol increases, the type of alcohol can be selected depending on the desired particle size of the silica particles.
[0048] The amount of water used in this step is preferably 0.5 to 5 mol, more preferably 0.6 to 2 mol, and particularly preferably 0.7 to 1 mol, per mol of the total hydrocarbyloxy groups of the tetrafunctional silane compound represented by formula (I) above and / or its partial hydrolysis condensate. When the basic substance is dissolved in water, the water used to dissolve the basic substance is also included in the "water" used in this step. From the viewpoints of affinity between the silica particles and the mixed solvent and ease of production, the ratio of the hydrophilic organic solvent to water is preferably 0.2 to 10, more preferably 0.3 to 5, by mass. From the viewpoints of the size of the resulting silica particles, the amount of the basic substance is preferably 0.01 to 2 mol, more preferably 0.03 to 0.5 mol, per mol of the total hydrocarbyloxy groups of the tetrafunctional silane compound represented by formula (I) above and / or its partial hydrolysis condensate.
[0049] The reaction conditions for the hydrolysis condensation in this step are preferably a reaction temperature of 20 to 120°C and a reaction time of 1 to 8 hours, more preferably a reaction temperature of 20 to 100°C and a reaction time of 1 to 6 hours.
[0050] The concentration of silica particles in the colloidal silica (A1) obtained in step (A1) is preferably from 2 to 20% by mass, particularly preferably from 3 to 10% by mass.
[0051] Step (A2): Surface Treatment Step with Trifunctional Silane Compound This step is an optional step in which a trifunctional silane compound represented by the following formula (II), a partial hydrolysis condensate thereof, or a mixture thereof is added to the colloidal silica (A1) obtained in step (A1), and R is formed on the surface of the colloidal silica. 2 SiO 3 / 2 This is the step of introducing the unit to obtain surface-treated colloidal silica (A2). 2 Si(OR 3 )3 (II) (wherein, R 2 represents a substituted or unsubstituted monovalent hydrocarbon group having 1 to 20 carbon atoms, R 3 each independently represents a monovalent hydrocarbon group having 1 to 6 carbon atoms.
[0052] In the above formula (II), R2 is a monovalent hydrocarbon group having 1 to 20 carbon atoms, preferably 1 to 10 carbon atoms, and particularly preferably 1 to 3 carbon atoms. 2 Examples of the monovalent hydrocarbon group represented by the formula (I) include alkyl groups such as methyl, ethyl, propyl, isopropyl, butyl, hexyl, octyl, and decyl, and particularly preferred are methyl, ethyl, and propyl. Some or all of the hydrogen atoms in these monovalent hydrocarbon groups may be substituted with halogen atoms such as fluorine, chlorine, and bromine, preferably fluorine atoms.
[0053] In the above formula (II), R 3 R is a monovalent hydrocarbon group having 1 to 6 carbon atoms, preferably having 1 to 4 carbon atoms, and particularly preferably having 1 or 2 carbon atoms. 3 Examples of the monovalent hydrocarbon group represented by the formula (I) include a methyl group, an ethyl group, a propyl group, a butyl group, and a phenyl group. Of these, a methyl group, an ethyl group, a propyl group, and a butyl group are preferred, and a methyl group and an ethyl group are particularly preferred.
[0054] Specific examples of the trifunctional silane compound represented by formula (II) above include methyltrimethoxysilane, methyltriethoxysilane, ethyltrimethoxysilane, ethyltriethoxysilane, n-propyltrimethoxysilane, n-propyltriethoxysilane, i-propyltrimethoxysilane, i-propyltriethoxysilane, butyltrimethoxysilane, butyltriethoxysilane, hexyltrimethoxysilane, 3,3,3-trifluoropropyltrimethoxysilane, and (heptadecafluoro-1,1,2,2-tetrahydrodecyl)trimethoxysilane.
[0055] The amount of the trifunctional silane compound represented by formula (II) used is preferably 0.001 to 1 mol, more preferably 0.01 to 0.1 mol, and particularly preferably 0.01 to 0.05 mol, per mol of SiO units (Si atoms derived from formula (I)) in the colloidal silica obtained in step (A1).
[0056] In step (A2), a trifunctional silane compound represented by formula (II) is added to the colloidal silica (A1) obtained in step (A1), and a surface treatment reaction of the silica with the trifunctional silane compound is carried out under the following reaction conditions: The reaction conditions in step (A2) are preferably a reaction temperature of 40 to 60°C and a reaction time of 1 to 10 hours, more preferably a reaction temperature of 50 to 60°C and a reaction time of 1 to 8 hours.
[0057] The surface-treated colloidal silica (A2) obtained in this step preferably has a Z-average particle size, as measured by dynamic light scattering, of 5 to 300 nm, more preferably 10 to 150 nm.
[0058] Step (A3') and Step (A3): Step of Adding Dispersant This step is a step of adding one or more dispersants selected from organopolysiloxanes having acid anhydride groups and organopolysiloxanes having groups obtained by hydrolyzing at least a portion of the acid anhydride groups to the colloidal silica (A1) obtained in step (A1) or the surface-treated colloidal silica (A2) obtained in step (A2).
[0059] Such organopolysiloxanes include linear, branched, cyclic, and three-dimensional network organopolysiloxanes, and particularly preferred are organopolysiloxanes represented by the following general formula (1) and organopolysiloxanes represented by the following general formula (2):
[0060] (In the formula, R 4 are independently a substituted or unsubstituted alkyl group having 1 to 4 carbon atoms or a group represented by the following formula (3) or (4), and R 4 At least two of the groups are groups represented by the following formula (3) or (4), and k is an integer of 0 to 150.
[0061] (In the formula, R 6 each independently represents a substituted or unsubstituted alkyl group having 1 to 4 carbon atoms; R 5 are independently a group represented by the following formula (3) or (4), m is an integer of 2 to 5, n is an integer of 0 to 3, and the sum of m and n is 4 or 5. The order of arrangement of the siloxane units is arbitrary.
[0062] (In the formula, the wavy line represents a bond.)
[0063] In the above formulas (3) and (4), R 4 and R 6 Examples of the alkyl group having 1 to 4 carbon atoms include a methyl group, an ethyl group, an n-propyl group, an isopropyl group, an n-butyl group, a sec-butyl group, and a tert-butyl group, and particularly preferred are a methyl group, an ethyl group, and an n-propyl group. Some or all of the hydrogen atoms of these monovalent hydrocarbon groups may be substituted with halogen atoms such as fluorine atoms, chlorine atoms, and bromine atoms, and preferably fluorine atoms.
[0064] In the above formula (1), k is an integer of 0 to 150, and is preferably an integer of 1 to 30 from the viewpoints of viscosity and solubility in water.
[0065] In the above formula (2), m is an integer of 2 to 5, preferably an integer of 2 to 4. n is an integer of 0 to 3, preferably an integer of 0 to 2. The sum of m and n is 4 or 5, preferably 4.
[0066] These dispersants may be used alone or in combination of two or more.
[0067] The amount of the dispersant added is preferably 10 to 3000 ppm by mass, more preferably 500 to 2000 ppm by mass, based on the silica particles.
[0068] Step (A4') and Step (A4): Dispersion Medium Substitution Step This step is a step of substituting water for the hydrophilic organic solvent in the dispersion medium of the dispersant-containing colloidal silica (A3') obtained in step (A3') and the dispersant-containing, surface-treated colloidal silica (A3) obtained in step (A3). The hydrophilic organic solvent includes the hydrophilic organic solvent used in step (A1) and volatile by-products such as alcohol produced by condensation. Substitution methods that can be used include a heat concentration method in which the dispersant-containing colloidal silica (A3') obtained in step (A3') and the dispersant-containing, surface-treated colloidal silica (A3) obtained in step (A3) are heated and concentrated while adding water in an amount equal to or greater than the amount of distillate obtained by heating, and ultrafiltration using a filter.
[0069] From the viewpoint of the stability of colloidal silica, the amount of water added is preferably 0.5 to 4 times, more preferably 1.8 to 3.0 times by weight, the total amount of the hydrophilic organic solvent used and the alcohol produced. Furthermore, when the dispersion medium substitution step is carried out by a thermal concentration method, the amount of hydrophilic organic solvent distilled off may be adjusted, the amount of water added in the dispersion medium substitution step may be appropriately adjusted, or water may be added after the dispersion medium substitution step, so that the finally obtained colloidal silica satisfies the desired solid content concentration (silica particle concentration) or kinematic viscosity.
[0070] The present invention will be specifically described below using examples and comparative examples. Note that the following examples do not limit the present invention in any way. The colloidal silica obtained in each example and comparative example was evaluated as follows, and the results are shown in Tables 1 and 2.
[0071] [Particle size (Z-average particle size) and polydispersity index (PDI) measured by dynamic light scattering] Colloidal silica was diluted with ion-exchanged water to a silica particle concentration of 0.1% by mass, and the colloidal silica was irradiated with ultrasonic waves for 10 minutes. The particle size distribution was measured using a Zetasizer Ultra (manufactured by Malvern Panalytical), and the Z-average particle size and PDI measured by dynamic light scattering were calculated. A PDI value of 0.1 or less indicates high monodispersity.
[0072] [Solid Content Concentration] 1.5 g of colloidal silica was precisely weighed and placed in an aluminum dish, and dried at 105° C. for 3 hours. The residue (X) g was precisely weighed, and the silica solid content concentration was calculated using the following formula: Silica solid content concentration (mass%)=(X / 1.5)×100
[0073] [Measurement of Residual Methanol Amount] The amount of residual methanol in the water-dispersed colloidal silica was measured by analyzing the gas phase of the vial while heating at 60°C for 30 minutes using a headspace gas chromatography measurement device set (HP6890 Series GC system, 5975 Mass Selective Detector, G1888 Network headspace Sampler, all manufactured by Agilent Technologies, Inc.).
[0074] [Metal Impurity Amount Measurement] Metal elements were measured using an ICP optical emission spectrometer (Agilent 5110 ICP-OES, manufactured by Agilent Technologies Inc.), and the amount of metal impurities in the water-dispersed colloidal silica was calculated.
[0075] [Kinematic Viscosity] The kinematic viscosity of the colloidal silica was measured using a Cannon-Fenske viscometer. 80 g of colloidal silica was placed in a 100 ml polyethylene bottle, sealed, and stored at 60° C., and the kinematic viscosity at 25° C. was measured after 14 days, 30 days, and 60 days.
[0076] [Example 1] - Step (A1) 793.0 g of methanol, 32.1 g of ion-exchanged water, and 40.6 g of 28% aqueous ammonia were mixed in a 3-liter glass reactor equipped with a stirrer, a dropping funnel, and a thermometer. The solution was adjusted to 46°C, and while stirring, 646.5 g of tetramethoxysilane and 160.9 g of 5.5% aqueous ammonia were simultaneously added dropwise, the former over 6 hours and the latter over 4 hours. After the dropwise addition of tetramethoxysilane was completed, stirring was continued for an additional 0.5 hours to carry out hydrolysis and condensation, thereby obtaining colloidal silica (A1). The concentration of silica particles in this colloidal silica (A1) was 15.5% by mass.
[0077] Step (A2): 5.8 g of methyltrimethoxysilane (equivalent to 0.01 mole per mole of SiO units in the colloidal silica) was added to the colloidal silica (A1) obtained in the above step (A1) at 25° C., and the mixture was stirred at 55° C. for 1 hour to obtain surface-treated colloidal silica (A2). Step (A3): 0.46 g of an organopolysiloxane represented by the following formula (1a) (1,800 ppm by mass relative to the silica) was added to the surface-treated colloidal silica (A2) obtained in the above step (A2) with stirring at 25° C. to obtain dispersant-containing surface-treated colloidal silica (A3).
[0078]
[0079] Step (A4): 840 g of ion-exchanged water was added at 25° C. to the dispersant-containing surface-treated colloidal silica (A3) obtained in the step (A3), and then the methanol was distilled off so that the solid content was 35 mass% or more, thereby obtaining 662 g of colloidal silica (i).
[0080] Example 2 689 g of colloidal silica (ii) was obtained in the same manner as in Example 1, except that in step (A2) of Example 1, the amount of methyltrimethoxysilane added was changed to 28.9 g (equivalent to 0.05 moles per mole of SiO units of the colloidal silica), and in step (A3) of Example 1, the amount of organopolysiloxane represented by the above formula (1a) added was changed to 0.15 g (600 ppm by mass relative to silica).
[0081] Example 3 700 g of colloidal silica (iii) was obtained in the same manner as in Example 1, except that in step (A2) of Example 1, methyltrimethoxysilane was changed to 6.9 g of propyltrimethoxysilane (equivalent to 0.01 mole per mole of SiO units of the colloidal silica), and in step (A3) of Example 1, the organopolysiloxane represented by the above formula (1a) was changed to 0.46 g of an organopolysiloxane represented by the following formula (2a) (1,800 ppm by mass relative to silica):
[0082]
[0083] Example 4 705 g of colloidal silica (iv) was obtained in the same manner as in Example 1, except that in step (A2) of Example 1, methyltrimethoxysilane was changed to 9.2 g of 3,3,3-trifluoropropyltrimethoxysilane (equivalent to 0.01 mole per mole of SiO units of the colloidal silica), and in step (A3) of Example 1, the organopolysiloxane represented by the above formula (1a) was changed to 0.46 g of an organopolysiloxane represented by the following formula (2b) (1,800 ppm by mass relative to silica):
[0084] Example 5 660 g of colloidal silica (v) was obtained in the same manner as in Example 1, except that in step (A1) of Example 1, the reaction temperature was changed to 38° C., and in step (A3) of Example 1, the amount of organopolysiloxane represented by formula (1a) added was changed to 0.15 g, and 0.05 g of organopolysiloxane represented by formula (2a) was also added (total of both was 800 ppm by mass relative to the silica).
[0085] Example 6 690 g of colloidal silica (vi) was obtained in the same manner as in Example 1, except that in step (A1) of Example 1, the reaction temperature was changed to 30° C., and in step (A3) of Example 1, the organopolysiloxane represented by formula (1a) was changed to 0.51 g (2000 ppm by mass relative to silica) of an organopolysiloxane represented by formula (2a) below:
[0086] Example 7 690 g of colloidal silica (vii) was obtained in the same manner as in Example 1, except that in step (A1) of Example 1, the reaction temperature was changed to 20° C., and in step (A3) of Example 1, the organopolysiloxane represented by formula (1a) was changed to 0.51 g (2,000 ppm by mass relative to silica) of an organopolysiloxane represented by formula (1b) below:
[0087]
[0088] [Example 8] - Step (A1) 793.0 g of methanol, 32.1 g of ion-exchanged water, and 40.6 g of 28% aqueous ammonia were mixed in a 3-liter glass reactor equipped with a stirrer, a dropping funnel, and a thermometer. The solution was adjusted to 46°C, and while stirring, 646.5 g of tetramethoxysilane and 160.9 g of 5.5% aqueous ammonia were simultaneously added dropwise, the former over 6 hours and the latter over 4 hours. After the dropwise addition of tetramethoxysilane was completed, stirring was continued for an additional 0.5 hours to carry out hydrolysis and condensation, thereby obtaining colloidal silica (A1). The concentration of silica particles in this colloidal silica (A1) was 15.5% by mass.
[0089] Step (A3′): 0.46 g (1,800 ppm by mass relative to the silica) of the organopolysiloxane represented by the formula (1a) was added to the colloidal silica (A1) obtained in the step (A1) at 25° C. with stirring, thereby obtaining a dispersant-containing colloidal silica (A3′).
[0090] Step (A4′): 840 g of ion-exchanged water was added at 25° C. to the dispersant-containing surface-treated colloidal silica (A3′) obtained in the above step (A3′), and then the methanol was distilled off so that the solid content was 35 mass% or more, thereby obtaining 662 g of colloidal silica (viii).
[0091] Comparative Example 1 655 g of colloidal silica (ix) was obtained in the same manner as in Example 8, except that the step (A3′) was not carried out.
[0092] Comparative Example 2 675 g of colloidal silica (x) was obtained in the same manner as in Example 8, except that in step (A1) of Example 8, the reaction temperature was changed to 20° C. and step (A3′) of Example 8 was not performed.
[0093] Comparative Example 3 690 g of colloidal silica (xi) was obtained in the same manner as in Example 8, except that in step (A3′) of Example 8, the organopolysiloxane represented by the above formula (1a) was changed to 0.17 g of ammonium benzoate (600 ppm by mass relative to the silica).
[0094] Comparative Example 4 695 g of colloidal silica (xii) was obtained in the same manner as in Example 8, except that in step (A3′) of Example 8, the organopolysiloxane represented by the above formula (1a) was changed to 0.09 g of citric acid (300 ppm by mass relative to the silica).
[0095] Comparative Example 5 677 g of colloidal silica (xiii) was obtained in the same manner as in Example 1, except that in step (A3) of Example 1, the organopolysiloxane represented by the above formula (1a) was changed to 0.46 g (1,800 ppm by mass relative to silica) of an organopolysiloxane represented by the following formula (5):
[0096]
[0097]
[0098]
[0099] From the above results, it was found that the colloidal silica obtained by the production method of the present invention has a low viscosity even at a high concentration, and the increase in viscosity during long-term storage is small.
[0100] The colloidal silica of the present invention has a low viscosity even at high concentrations and shows little increase in viscosity during long-term storage, and therefore can be suitably used as abrasive grains in polishing silicon wafers, CMP processes for semiconductor devices, and the like.
Claims
1. A colloidal silica containing silica particles, a dispersant made of an organopolysiloxane having a group having an acid anhydride structure, a group having a structure formed by hydrolysis of an acid anhydride, or both, and water.
2. The colloidal silica according to claim 1, wherein the silica particles are sol-gel silica particles whose surfaces have been treated with a trifunctional silane compound represented by the following formula (II): 2 Si(OR 3 )3 (II) (wherein, R 2 represents a substituted or unsubstituted monovalent hydrocarbon group having 1 to 20 carbon atoms; R 3 each independently represents a monovalent hydrocarbon group having 1 to 6 carbon atoms.
3. The colloidal silica according to claim 1, wherein the Z-average particle size of the silica particles as measured by dynamic light scattering is 5 to 300 nm.
4. The colloidal silica according to claim 1, wherein the dispersing agent is at least one selected from the group consisting of organopolysiloxanes represented by the following general formula (1) and organopolysiloxanes represented by the following general formula (2): (In the formula, R 4 are independently a substituted or unsubstituted alkyl group having 1 to 4 carbon atoms or a group represented by the following formula (3) or (4), R 4 At least two of the groups are represented by the following formula (3) or (4). k is an integer of 0 to 150. (In the formula, R 6 each independently represents a substituted or unsubstituted alkyl group having 1 to 4 carbon atoms; R 5 are independently a group represented by the following formula (3) or (4), m is an integer of 2 to 5, n is an integer of 0 to 3, and the sum of m and n is 4 or 5. The order of arrangement of the siloxane units is arbitrary. (In the formula, the wavy line represents a bond.) 5. The colloidal silica according to claim 1, wherein the amount of the dispersant is 10 to 3,000 ppm by mass based on the silica particles.
6. The colloidal silica according to claim 1, wherein the concentration of metal impurities is 0 to 1 ppm by mass.
7. The colloidal silica according to claim 1, wherein the concentration of the hydrophilic organic solvent is 0 to 1% by mass.
8. The colloidal silica according to claim 1, having a solids concentration of 30 to 50 mass %.
9. Kinematic viscosity at 25°C is 1 to 100 mm 2 2. The colloidal silica according to claim 1, wherein 10. A chemical mechanical polishing liquid containing the colloidal silica according to any one of claims 1 to 9.
11. A method for producing colloidal silica according to claim 1, comprising the following steps (A1), (A3') and (A4'): Step (A1): A step of obtaining colloidal silica (A1) by hydrolyzing and condensing a tetrafunctional silane compound represented by the following formula (I), a partial hydrolysis condensate thereof or a mixture thereof in a mixed liquid containing a hydrophilic organic solvent and water in the presence of a basic substance: Si(OR 1 )4 (I) (wherein, R 1 each independently represents a monovalent hydrocarbon group having 1 to 6 carbon atoms.) Step (A3'): A step of adding a dispersant composed of an organopolysiloxane having a group having an acid anhydride structure, a group having a structure obtained by hydrolysis of an acid anhydride, or both, to the colloidal silica (A1) obtained in step (A1), to obtain a dispersant-containing colloidal silica (A3'). Step (A4'): A step of replacing the hydrophilic organic solvent in the dispersion medium of the dispersant-containing colloidal silica (A3') obtained in step (A3') with water.
12. A method for producing colloidal silica according to claim 2, comprising the following steps (A1), (A2), (A3) and (A4): Step (A1): A step of obtaining colloidal silica by hydrolyzing and condensing a tetrafunctional silane compound represented by the following formula (I), a partial hydrolysis condensate thereof or a mixture thereof in a mixed liquid containing a hydrophilic organic solvent and water in the presence of a basic substance: Si(OR 1 )4 (I) (wherein, R 1 each independently represents a monovalent hydrocarbon group having 1 to 6 carbon atoms. Step (A2): To the colloidal silica (A1) obtained in step (A1), a trifunctional silane compound represented by the following formula (II), a partial hydrolysis condensate thereof, or a mixture thereof is added, and R2 SiO 3 / 2 Step R of introducing units to obtain surface-treated colloidal silica (A2) 2 Si(OR 3 )3 (II) (wherein, R 2 represents a substituted or unsubstituted monovalent hydrocarbon group having 1 to 20 carbon atoms; R 3 each independently represents a monovalent hydrocarbon group having 1 to 6 carbon atoms.) Step (A3): A step of adding a dispersant composed of an organopolysiloxane having a group having an acid anhydride structure, a group having a structure obtained by hydrolysis of an acid anhydride, or both, to the surface-treated colloidal silica (A2) obtained in step (A2), to obtain a dispersant-containing surface-treated colloidal silica (A3). Step (A4): A step of replacing the hydrophilic organic solvent in the dispersion medium of the dispersant-containing surface-treated colloidal silica (A3) obtained in step (A3) with water.
13. The method for producing colloidal silica according to claim 11, wherein the amount of the trifunctional silane compound represented by formula (II), its partial hydrolysis condensate, or a mixture thereof added in step (A2) is 0.001 to 1 mol per 1 mol of SiO2 units in the colloidal silica (A1) obtained in step (A1).
14. The method for producing colloidal silica according to any one of claims 11 to 13, wherein the dispersant is at least one selected from the group consisting of organopolysiloxanes represented by the following general formula (1) and organopolysiloxanes represented by the following general formula (2): (In the formula, R 4 are independently a substituted or unsubstituted alkyl group having 1 to 4 carbon atoms or a group represented by the following formula (3) or (4), R 4 At least two of the groups are represented by the following formula (3) or (4). k is an integer of 0 to 150. (In the formula, R 6 each independently represents a substituted or unsubstituted alkyl group having 1 to 4 carbon atoms; R 5 are independently a group represented by the following formula (3) or (4), m is an integer of 2 to 5, n is an integer of 0 to 3, and the sum of m and n is 4 or 5. The order of arrangement of the siloxane units is arbitrary. (In the formula, the wavy line represents a bond.)
Citation Information
Patent Citations
Method for producing modified colloidal silica
JP2005162533A
Method for producing silica sol
JP2019172558A
Silica sol and method for producing the same
JP5270344B2
Method for producing water-dispersed surface-treated colloidal silica
JP2023005414A
Method for producing silica sol, polishing method, method for producing semiconductor wafer and method for producing semiconductor device
JP2023043024A