Method for manufacturing lead terminal for power storage device, and lead terminal for power storage device

The laser welding method addresses the limitations of conventional percussion arc welding by improving the reproducibility and quality of lead terminals for power storage devices, enhancing manufacturing efficiency and reducing defects in lead terminals made from aluminum or copper materials.

WO2024242162A1PCT designated stage expired Publication Date: 2024-11-28KOHOKU KOGYO CO LTD
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2024/018946
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-05-23
Filing Date
2024-05-23
Publication Date
2024-11-28

AI Technical Summary

Technical Problem

Conventional percussion arc welding methods for manufacturing lead terminals for power storage devices face issues with low reproducibility of weld shape, adhesion of dissimilar metals, and limited manufacturing speed, which affect the quality and yield of lead terminals made from aluminum or copper materials.

Method used

A laser welding method is employed, where a wire rod and lead wire are aligned and the wire rod end is irradiated with a laser beam to create a molten pool, followed by pushing the lead wire into the pool to form a welded connection, controlling the welded portion shape and preventing dissimilar metal adhesion, thus improving reproducibility and manufacturing speed.

Benefits of technology

The laser welding method enhances the reproducibility and quality of the welded portion, reduces the risk of dissimilar metal adhesion, and increases manufacturing speed, resulting in improved yield and performance of lead terminals for power storage devices.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JP2024018946_28112024_PF_FP_ABST
    Figure JP2024018946_28112024_PF_FP_ABST
Patent Text Reader

Abstract

A method for manufacturing a lead terminal for a power storage device comprising an electrode terminal 2 composed of a wire material 100 mainly containing aluminum or copper, and a lead wire 3 connected to the electrode terminal via a welding part 4, the method comprising: a first step for linearly aligning the wire material and the lead wire and holding the wire material and the lead wire in a state where a predetermined distance is maintained between an end surface 100b on the lead wire side of the wire material and an end surface 3b on the wire material side of the lead wire; a second step for irradiating the end part 100a on the lead wire side of the wire material with a laser beam using a laser irradiation machine 400 to melt the end part 100a; and a third step for pressing one of the wire material and the lead wire in the axial direction toward the other after a predetermined time has elapsed from the start of the laser beam irradiation in the second step, to form a welded part.
Need to check novelty before this filing date? Find Prior Art

Description

Manufacturing method for lead terminal for electric storage device and lead terminal for electric storage device

[0001] The present invention relates to a method for manufacturing a lead terminal for an electricity storage device, and a lead terminal for an electricity storage device.

[0002] Lead terminals for electricity storage devices have been known for some time. Each lead terminal for an electricity storage device includes a metal electrode terminal and a lead wire. The lead wire is connected to the electrode terminal via a weld. For example, in a lead terminal for an electrolytic capacitor (a type of electricity storage device), the electrode terminal is connected to an electrode foil that forms a capacitor element (a component of the electrolytic capacitor), and the lead wire is connected to an electric circuit.

[0003] A typical example of a lead terminal is a lead terminal having an electrode terminal made of aluminum or copper. The welds of such lead terminals have generally been formed by percussion arc welding (see, for example, Patent Document 1). This is because, among the welding methods under consideration at the time, percussion arc welding offered the highest yield, while other welding methods, such as brazing (a type of soldering), have drawbacks, such as the risk of foreign matter being mixed in, and resistance welding (a type of pressure welding) has drawbacks, such as the relatively slow melting rate of the welded material.

[0004] Patent No. 5461570

[0005] (Problem to be Solved by the Invention) However, the welding method using percussion arc welding cannot be said to be the best, and there is room for improvement in the manufacturing method of a lead terminal having an aluminum or copper electrode terminal and the lead terminal manufactured by this manufacturing method.

[0006] The present invention has been made to address the above-mentioned problems. That is, one object of the present invention is to provide a manufacturing method for appropriately manufacturing a lead terminal for an electricity storage device having an electrode terminal made of a wire material mainly containing aluminum or copper, and a lead terminal manufactured by the manufacturing method.

[0007] (Means for Solving the Problem) The method for manufacturing a lead terminal of the present invention is for an electricity storage device, the method comprising: an electrode terminal (2) made of a wire (100) containing mainly aluminum or copper; and a lead wire (3) connected to the electrode terminal via a weld (4). The method for manufacturing the lead terminal comprises: a first step of linearly aligning the wire (100) and the lead wire (3) and holding the wire and the lead wire in a state in which a predetermined distance is maintained between an end face (100b) of the wire on the lead wire side and an end face (3b) of the lead wire on the wire wire side; a second step of irradiating a laser beam onto an end face (100a) of the wire (100) on the lead wire side using a laser irradiator (400) to melt the end; and a third step of axially pushing one of the wire (100) and the lead wire (3) toward the other to form the weld (4) after a predetermined time has elapsed since the start of irradiation of the laser beam in the second step.

[0008] The lead terminal (101) of the present invention is a lead terminal for an electricity storage device, comprising an electrode terminal (102) made of a wire material mainly containing aluminum or copper, and a lead wire (103) connected to the electrode terminal via a welded portion (104). In this lead terminal, the ratio of the diameter of the lead wire to the diameter of the wire material is 83% or more and 100% or less.

[0009] (Effects of the Invention) According to the present invention, a manufacturing method for appropriately manufacturing a lead terminal for an electricity storage device having an electrode terminal made of a wire material mainly containing aluminum or copper, and a lead terminal manufactured by the manufacturing method can be provided.

[0010] 7A is a perspective view showing a lead terminal manufactured by a method for manufacturing a lead terminal for an electricity storage device according to an embodiment of the present invention. FIG. 7B is a view (first) for explaining a method for manufacturing the lead terminal of FIG. 1. FIG. 7C is a view (second) for explaining a method for manufacturing the lead terminal of FIG. 1. FIG. 7D is a view (fourth) for explaining a method for manufacturing the lead terminal of FIG. 1. FIG. 7E is a view (fourth) for explaining a method for manufacturing the lead terminal of FIG. 1. FIG. 7F is a view (fourth) for explaining a method for manufacturing the lead terminal of FIG. 1. FIG. 7G is a view (fourth) for explaining a method for manufacturing the lead terminal of FIG. 1. FIG. 7H is a view (fourth) for explaining a dent formed in a welded portion. FIG. 7I is a view (fourth) for explaining a method for manufacturing a lead terminal for an electricity storage device according to Modification 1. FIG. 7I is a partial enlarged view of a defective lead terminal manufactured using percussion arc welding. FIG. 7J is a partial enlarged view of another defective lead terminal manufactured using percussion arc welding. FIG. 7J is a partial enlarged view of yet another defective lead terminal manufactured using percussion arc welding. FIG. 7I is a perspective view showing a lead terminal manufactured by a method for manufacturing a lead terminal for an electricity storage device according to Modification 3. FIG. 7G is a partial enlarged view of a lead terminal having a wire diameter ratio of 83%. FIG. 7H is a schematic view of an X-ray image of the lead terminal of FIG. 7A. FIG. 7I is a schematic view of an EPMA image of a cross section of sample S having a wire diameter ratio of 83%. 8A is a partially enlarged view of a lead terminal having a wire diameter ratio of 83% manufactured by percussion arc welding, FIG. 8B is a schematic view of an X-ray image of the lead terminal of FIG. 8A, and FIG. 8C is a schematic view of an EPMA image of a cross section of sample Sc having a wire diameter ratio of 83%.

[0011] Hereinafter, a method for manufacturing a lead terminal for an electric storage device according to an embodiment of the present invention will be described with reference to the drawings, taking as an example a lead terminal for an electrolytic capacitor, which is one type of electric storage device. First, the configuration of the lead terminal will be described. As shown in Fig. 1, the lead terminal 1 includes an aluminum electrode terminal 2 and a lead wire 3 made of a CP wire.

[0012] The electrode terminal 2 is formed by radially pressing a portion of an axial direction of a wire material primarily containing aluminum (hereinafter simply referred to as "aluminum wire"), and has a rod-shaped portion 21 at one end and a rolled portion 22 at the other end. The rod-shaped portion 21 is the portion that remains unpressed (i.e., the other portion of the aluminum wire in the axial direction). The rolled portion 22 is formed by pressing the portion of the aluminum wire into a flat plate and then cutting the outer periphery along the thickness direction. The axis of the rolled portion 22 (a line passing through the center in the width direction and thickness direction) is coaxial with the axis of the rod-shaped portion 21. However, a configuration in which the rolled portion 22 is eccentric with respect to the rod-shaped portion 21 may also be adopted. The aluminum wire has been previously subjected to a well-known anodizing process, and an oxide coating is formed on its outer periphery. The diameter of the aluminum wire is approximately 2 mm. The electrode terminal 2 may also be formed using an aluminum wire that has not been anodized.

[0013] The lead wire 3 is connected to one end of the rod-shaped portion 21 via a welded portion 4. The diameter of the lead wire 3 is approximately 0.8 mm, which is smaller than the rod-shaped portion 21. The axis of the lead wire 3 is coaxial with the axis of the rod-shaped portion 21. In this embodiment, the CP wire constituting the lead wire 3 is a metal wire in which the outer surface of an iron wire is coated with a copper plating layer, and the copper plating layer is further coated with a tin plating layer. The thicknesses of the copper plating layer and the tin plating layer are both on the order of several tens of μm. However, instead of the tin plating layer, a CP wire coated with a nickel plating layer, a silver plating layer, or a lead-free solder plating layer may be used. Alternatively, the CP wire constituting the lead wire 3 may be a metal wire in which the outer surface of an iron wire is coated only with a copper plating layer.

[0014] 2A to 2D, a method for manufacturing the lead terminal 1 will be described. First, a long aluminum wire (strictly speaking, an anodized aluminum wire) that is the material for the electrode terminal 2 is cut to a predetermined length to form the wire material 100. Next, a long CP wire that is the material for the lead wire 3 is cut to a predetermined length to form the lead wire 3.

[0015] Next, as shown in FIG. 2A, the wire 100 is held in a jig 200, and the lead wire 3 is held in a jig 300, so that the wire 100 and the lead wire 3 are aligned in a straight line so that their axes are coaxial, and the distance between the end face 100b of one end 100a of the wire 100 and the end face 3b of the other end 3a of the lead wire 3 is maintained at a predetermined distance (2 mm in this embodiment) (first step).

[0016] Next, a laser beam is irradiated from a laser irradiator 400 to a predetermined position P on the end 100a of the wire 100 from a direction perpendicular to the axis of the wire 100 (hereinafter simply referred to as the "orthogonal direction"). The position P is located on the outer peripheral surface 100c of the end 100a, a predetermined distance L (0.10 mm in this embodiment) from the end surface 100b. When the wire 100 is viewed from above from the direction of irradiation of the laser beam, the position P is located at the radial center of the wire 100. That is, the laser beam is irradiated toward the axis of the wire 100. The irradiator 400 is a single-mode infrared laser (IR laser) with an output of 700 W. The laser beam is irradiated with a spot diameter of 30 μm for 0.030 s. The irradiator 400 irradiates the position P of the wire 100 with a laser beam, thereby melting the entire end 100a and forming a molten pool A, as shown in Fig. 2B (second step). Note that the distance L may be appropriately changed depending on the output, spot diameter, irradiation time, etc. of the irradiator 400.

[0017] The jig 300 is provided with a pushing mechanism (not shown). The pushing mechanism is configured to apply an external force in a predetermined direction. In this embodiment, the pushing mechanism applies an external force to the lead wire 3, pushing the lead wire 3 axially toward the wire 100, immediately after the laser beam irradiation by the irradiator 400 is completed (in other words, after the irradiation time has elapsed since the start of laser beam irradiation). This external force is applied so that the lead wire 3 moves a predetermined distance at a predetermined speed (200 mm / s in this embodiment). As a result, the end 3 a of the lead wire 3 is pushed into the molten pool A of the wire 100, as shown in FIG. 2C . Then, a portion of the molten pool A spreads to cover the outer peripheral surface 3 c of the end 3 a of the lead wire 3. Thereafter, when the molten pool A (or the molten portion of the molten pool A and the molten portion of the end 3a, if the end 3a is partially melted) solidifies, a conical weld 4 (strictly speaking, an approximately truncated cone shape whose diameter decreases from the wire 100 toward the lead wire 3) is formed between the wire 100 and the lead wire 3, as shown in Figure 2D, and the wire 100 and the lead wire 3 are connected (third step).

[0018] Thereafter, the other end of the wire 100 is pressed to form the rolled portion 22 shown in Fig. 1, and is then subjected to well-known anodizing and resin coating processes as necessary, thereby producing the lead terminal 1. Note that a strength test confirmed that the strength of the lead terminal 1 produced by laser welding was equivalent to that of a lead terminal produced by percussion arc welding.

[0019] The manufacturing method for a lead terminal according to the present embodiment enables more appropriate manufacturing of lead terminals than conventional manufacturing methods using percussion arc welding (hereinafter simply referred to as "arc welding"). The following specific explanations are provided below. Conventional arc welding methods have several problems. The first problem is poor reproducibility of the weld shape. In other words, arc welding has a problem in that the amount of heat input tends to vary from workpiece to workpiece depending on the environmental conditions at the time of arc generation (type and flow rate of shielding gas, shape and condition of each end face of the wire and lead wire). As a result, the shape of the lead terminal tends to vary. FIGS. 5A to 5C are partially enlarged views of a defective lead terminal 11 manufactured using arc welding. The lead terminal 11 includes an aluminum electrode terminal 12 and a lead wire 13 made of a CP wire connected to the electrode terminal 12 via a weld 14. In Fig. 5A, a portion 14a of the weld 14 covers the outer peripheral surface of the lead wire 13, while the other portion of the weld 14 does not, resulting in an irregular shape (so-called uneven buildup). In Fig. 5B, a protrusion (so-called weld thorn) 14b large enough to be visible to the naked eye is generated from the weld 14. In Fig. 5C, a portion 14c of the weld 14 in the circumferential direction protrudes radially, thereby locally increasing the diameter of the weld 14 (so-called protrusion). The low reproducibility of the weld shape exemplified in the lead terminal 11 of Figs. 5A to 5C has been a factor preventing improvement in yield.

[0020] The second problem is the deposition of dissimilar metals on the workpiece (especially the electrode terminals). In arc welding, an arc discharge generates an arc between the wire and the lead wire, melting the tips of both wires and the lead wire, resulting in spatter from both the wire and the lead wire. For example, if the lead wire is a CP wire coated with a copper and tin plating layer, the spatter generated from the lead wire contains copper and tin. Therefore, when spatter containing copper and tin generated from the lead wire adheres to an aluminum wire, dissimilar metals are deposited on the workpiece (specifically, the part that will become the electrode terminal after the product is completed). When a capacitor element (a component of an electrolytic capacitor) is manufactured using a lead terminal with a dissimilar metal attached to its electrode terminal, the dissimilar metal may react with the electrolyte inside the capacitor element, potentially resulting in a deterioration in quality characteristics. This problem is unavoidable as long as the lead wire contains materials other than aluminum. The deposition of dissimilar metals on the workpiece is another factor hindering yield improvement.

[0021] The third problem is the limited improvement in workpiece manufacturing speed. In arc welding, an arc is generated by first contacting a wire and a lead wire and then separating them. The tips of the wire and the lead wire are melted, and then the two are brought into contact again (strictly speaking, one is pushed into the other). This requires multiple reciprocating motions for one workpiece, complicating the manufacturing process. Furthermore, the performance of actuators capable of realizing such a series of reciprocating motions is limited, making it difficult to control the actuator at high speed. These problems have hindered efforts to increase workpiece manufacturing speed.

[0022] In contrast, the present embodiment employs laser welding as the welding method. This allows for relatively easy control of the shape of the weld 4 (in other words, once the environmental conditions for laser beam irradiation are determined, subsequent adjustments are essentially unnecessary). As a result, the reproducibility of the weld shape can be significantly improved. Furthermore, since the laser beam is irradiated only on the wire 100 during laser welding, even if spatter is generated from the wire 100 during laser welding, it is unlikely that dissimilar metals will adhere to the electrode terminal 2 (spatter generated from the wire 100 adhering to the lead wire 3 is not considered a particular problem). Furthermore, since the weld 4 is formed by forcing the end 3 a of the lead wire 3 into the molten pool A of the wire 100, the welding process can be performed by simply moving the lead wire 3 in one direction for one workpiece, simplifying the manufacturing process. Furthermore, because actuators capable of achieving such simple movements are readily available, the time required for actuator operation can be significantly reduced by introducing a high-speed actuator. As described above, by employing laser welding as the welding method, the above three problems associated with arc welding can be solved, and the yield and manufacturing speed of the lead terminals 1 can be improved.

[0023] Even when laser welding is used as the welding method, the following manufacturing method, i.e., "Manufacturing Method M, in which the end face 100b of the wire 100 and the end face 3b of the lead wire 3 are butted together (contacted) and a laser beam is irradiated onto the wire 100 while one of the wire 100 and the lead wire 3 is axially pressed toward the other," may not properly form the weld 4. This will be described in detail with reference to FIG. 3. FIG. 3 shows a partial enlarged view of the lead terminal 1 after the weld 4 has been formed by Manufacturing Method M. In this example, the laser beam is irradiated from an orthogonal direction. As shown in FIG. 3, a crater-like dent d is formed in the weld 4. The dent d is a depression formed by continuously irradiating the laser beam onto a single location on the outer peripheral surface 100c of the wire 100. It was found that the height hd of the weld 4 at the portion where the dent d is formed is greater than the height h of the weld 4 at the portion where the dent d is not formed, with the ratio (hd / h) tending to be approximately 1.5 to 2 times. A welded portion 4 with such a dent d formed therein significantly deviates from the general specifications for welded portions 4, and is therefore a factor that hinders improvement in yield. Furthermore, when an electrolytic capacitor is manufactured using a lead terminal 1 with a dent d in the welded portion 4, a gap may form between the resin sealing body and the lead terminal 1, causing the electrolyte (electrolytic solution held in the capacitor element) to leak from the gap, which may result in a deterioration in the quality characteristics of the electrolytic capacitor.

[0024] Therefore, in this embodiment, the laser beam irradiation is started while the distance between the end face 100b of the wire 100 and the end face 3b of the lead wire 3 is maintained at a predetermined distance, and one of the wire 100 and the lead wire 3 is pushed axially toward the other after a predetermined time T has elapsed from the start of irradiation. This configuration makes it difficult for a dent d to occur in the welded portion 4, thereby improving the yield of the lead terminal 1 and suppressing a deterioration in the quality characteristics of the electrolytic capacitor.

[0025] As described above, the manufacturing method for a lead terminal according to this embodiment makes it possible to appropriately manufacture a lead terminal having an electrode terminal made of a wire material containing mainly aluminum. The lead terminal 1 may be used as a component of other power storage devices, not limited to electrolytic capacitors. Examples of other power storage devices include lithium ion capacitors, electric double layer capacitors (EDLCs), and lithium ion batteries. The same effects can be achieved even when the lead terminal 1 is used as a component of other power storage devices.

[0026] The inventors of the present application investigated the incidence of dents d while varying the predetermined time T (the time from the start of laser beam irradiation to the time when the lead wire 3 is pressed toward the wire 100). The results showed that, when the laser beam is irradiated from the orthogonal direction, when the irradiation time is 0<T<, the incidence of dents d can be reduced compared to when T = 0, but the incidence is higher than when T = irradiation time. Furthermore, when the irradiation time is greater than T, the incidence of dents d can be suppressed to the same extent as when T = irradiation time. However, the temperature of the molten pool A decreases due to the delay in the timing of pressing the lead wire 3 toward the wire 100, which may result in an inadequate connection between the wire 100 and the lead wire 3 (i.e., a decrease in the strength of the lead terminal 1). Therefore, in this embodiment, when the laser beam is irradiated from the orthogonal direction, the lead wire 3 is pressed toward the wire 100 immediately after the end of laser beam irradiation (i.e., the predetermined time T = irradiation time). This configuration further reduces the incidence of dents d in the welded portion 4 while maintaining the strength of the lead terminal 1.

[0027] When the laser beam is irradiated from the orthogonal direction, the position of the irradiator 400 is adjusted by orthogonally ...

[0028] Furthermore, in this embodiment, an infrared laser is used for the irradiator 400. Therefore, the cost of the manufacturing equipment for the lead terminal 1 can be reduced compared to when a short-wavelength laser (typically, a blue laser or a green laser) is used for the irradiator 400. However, since the absorptivity of aluminum is equivalent across the entire wavelength band of infrared and visible light, from the viewpoints other than manufacturing cost, even when a short-wavelength laser is used, the same effects as those of this embodiment can be achieved. Note that the type of laser (for example, a fiber laser or a semiconductor laser) is not particularly limited.

[0029] The laser beam may be irradiated not only at position P on wire 100 but also in a linear or elliptical shape over a predetermined range on outer peripheral surface 100c of end 100a. Furthermore, wire 100 may be rotated around its axis at a predetermined speed during irradiation with the laser beam.

[0030] (Modification 1) Next, a manufacturing method of a lead terminal for an electricity storage device according to Modification 1 of the present invention will be described with reference to FIG. 4 . The same components as those in the embodiment are designated by the same reference numerals, and detailed description thereof will be omitted. This also applies to other modifications. As shown in FIG. 4 , the manufacturing method of Modification 1 differs from the manufacturing method of the embodiment in that the direction of irradiation of the laser beam is oblique to the axis of the wire 100. Specifically, in this modification, the irradiator 400 irradiates the center C of the end face 100b of the wire 100 with a laser beam from a direction intersecting the axis of the wire 100 at an angle of 45°. Immediately after the end of irradiation of the laser beam, the pushing mechanism applies an external force to the lead wire 3 to push the lead wire 3 axially toward the wire 100 (i.e., the predetermined time T = irradiation time). The spot diameter and irradiation time may be the same as or different from those in the embodiment.

[0031] This configuration also achieves the same effects as the embodiment. In particular, in this modification, the laser beam is irradiated not on the outer peripheral surface 100c of the wire 100 but on the end surface 100b (i.e., the portion inside the molten pool A). This prevents the formation of dents d in the welded portion 4, thereby more suitably improving the yield of the lead terminals 1 and further suppressing the deterioration of the quality characteristics of the electricity storage device.

[0032] As long as the laser beam is irradiated onto the end face 100b of the wire 100, the direction of irradiation of the laser beam is not limited to a direction intersecting the axis of the wire 100 at 45°. The irradiation position of the laser beam may be eccentric from the center C of the end face 100b, or the laser beam may be irradiated in a predetermined range on the end face 100b, for example, linearly or circularly. Furthermore, since no dent d is formed in the welded portion 4 in this modification, the timing at which the lead wire 3 is pressed toward the wire 100 may be earlier than the end of the irradiation of the laser beam (typically, it may be several tens of milliseconds earlier than the end of the irradiation). That is, the predetermined time T may be set to any value that satisfies 0<T≦irradiation time.

[0033] (Variation 2) Next, a description will be given of a manufacturing method of a lead terminal for an electricity storage device according to Variation 2 of the present invention. The manufacturing method of Variation 2 differs from the manufacturing methods of the embodiment and Variation 1 in that a wire material containing mainly copper is used instead of an aluminum wire as the wire material 100 constituting the electrode terminal 2, and a short-wavelength laser is used as the irradiator 400 instead of an infrared laser.

[0034] The wire 100 has been subjected to a known anodizing treatment in advance, and an oxide film is formed on its outer circumferential surface. The diameter of the wire 100 and the method for forming the electrode terminal 2 are the same as those in the embodiment. Note that the electrode terminal 2 may be formed using a wire that has not been subjected to an anodizing treatment.

[0035] The lead terminal 1 can basically be manufactured by the manufacturing method described in the embodiment or variant example 1. However, in the second step, a short-wavelength laser is used as the irradiator 400. The short-wavelength laser is a multi-mode blue laser with an output of 2 kW. The laser beam is irradiated for 70 μs with a spot diameter of 600 μm. By irradiating the position P of the wire 100 with the blue laser, the entire end portion 100 a is melted to form a molten pool A, as in the embodiment. Note that a green laser may be used as the short-wavelength laser instead of the blue laser. In this case, the spot diameter and irradiation time can be appropriately adjusted depending on the output of the green laser.

[0036] Here, when a wire containing mainly copper is used as the wire 100, no dent d occurs even if the predetermined time T (the time from the start of laser beam irradiation to the time when the lead wire 3 is pressed toward the wire 100) is 0 < T < irradiation time. Therefore, in this modified example, the predetermined time T does not necessarily have to satisfy T = irradiation time. The predetermined time T can be set appropriately based on the diameter ratio of the lead wire 3 to the wire 100, the output of the short-wavelength laser, the spot diameter, the irradiation time, etc.

[0037] As described above, the manufacturing method of the lead terminal for an electricity storage device according to the second modification can solve the three problems associated with arc welding described in the embodiment, and can improve the yield and manufacturing speed of the lead terminal 1. In other words, it becomes possible to appropriately manufacture the lead terminal 1 having an electrode terminal made of a wire material mainly containing copper.

[0038] Furthermore, when manufacturing the lead terminal 1 using a manufacturing method similar to that of the embodiment, it is easier to adjust the position of the short-wavelength laser compared to a configuration in which the laser beam is irradiated so as to intersect obliquely with the axis of the wire 100.

[0039] Furthermore, although the absorptivity of a laser beam to a metal generally varies depending on the wavelength of the laser beam and the type of metal, the absorptivity of a short-wavelength laser beam to copper is significantly higher than that of an infrared laser beam. Therefore, when the wire 100 is a wire that mainly contains copper, the end 100a of the wire 100 can be appropriately melted by using a short-wavelength laser.

[0040] 6 to 8C , a lead terminal for an electric storage device and a manufacturing method thereof according to Modification 3 of the present invention will be described using a lead terminal for an electrolytic capacitor as an example. The lead terminal of Modification 3 differs from the lead terminal 1 of the embodiment and Modifications 1 and 2 in that the ratio of the wire diameter of the lead wire to the wire material (described later) is relatively large.

[0041] As shown in FIG. 6 , the lead terminal 101 according to this modification includes an aluminum electrode terminal 102 and a lead wire 103 made of CP wire. The electrode terminal 102 has a rod-shaped portion 121 at one end and a rolled portion 122 at the other end. The lead wire 103 is connected to one end of the rod-shaped portion 121 via a welded portion 104. The diameter of the wire (aluminum wire) (i.e., the diameter of the rod-shaped portion 121) is, for example, 1.2 mm, and the diameter of the lead wire 103 is, for example, 1.0 mm. Hereinafter, the ratio of the diameter of the lead wire to the diameter of the wire (i.e., the diameter of the rod-shaped portion) is referred to as the "wire diameter ratio of the lead wire to the wire" or the "wire length ratio of the lead terminal." The wire diameter ratio is calculated as an integer value by rounding off decimal points. The upper limit of the wire diameter ratio is 100%. In the above example, the wire diameter ratio of the lead terminal 101 is 1.0 / 1.2=83%, which is larger than the wire diameter ratio of 40% (=0.8 / 2) of the lead terminal 1 according to the embodiment and modifications 1 and 2. The lead terminal according to this modification is characterized by a wire diameter ratio in the range of 83% or more and 100% or less. In other words, as long as the wire diameter ratio of the lead terminal 101 is within this range, the diameters of the wire material and the lead wire 103 are not limited to the above values.

[0042] The lead terminal 101 can be manufactured by using a wire rod having a wire diameter ratio of 83% or more and 100% or less and a lead wire 103 in the first step of the embodiment. The lead terminal 1 can also be manufactured by the manufacturing method of Modification 1.

[0043] FIG. 7A is a diagram showing the welded portion 104 of the lead terminal 101 and its vicinity. The diameter of the rod-shaped portion 121 is 1.2 mm, and the diameter of the lead wire 103 is 1.0 mm. FIG. 7B is a schematic diagram of an X-ray image of FIG. 7A. FIG. 7C is a schematic diagram of an EPMA (Electron Probe Micro Analyzer) image of a cross section including the axis of sample S. Sample S was manufactured by laser welding (strictly speaking, the manufacturing method according to the embodiment) using a material with the same dimensions as the lead terminal 101. On the other hand, FIG. 8A is a diagram showing the welded portion 114 of a lead terminal 111 as a comparative example manufactured by arc welding and its vicinity. The diameter of the rod-shaped portion 131 is 1.2 mm, and the diameter of the lead wire 113 is 1.0 mm. FIG. 8B is a schematic diagram of the X-ray image of FIG. 8A. FIG. 8C is a schematic diagram of an EPMA image of a cross section including the axis of sample Sc. Sample Sc was manufactured by arc welding using a material with the same dimensions as the lead terminal 111.

[0044] 7A and 8A, in Fig. 7A, the surface of weld 104 of lead terminal 101 is relatively smooth, whereas in Fig. 8A, numerous irregularities are formed on the surface of weld 114 of lead terminal 111. Furthermore, although weld 104 has slight bulges in some areas, its shape is nearly symmetrical about the axis. In contrast, weld 114 protrudes significantly in the radial direction, making its shape asymmetrical about the axis. Generally, when an electrolytic capacitor is manufactured using a lead terminal whose weld shape is asymmetrical about the axis, a gap may form between the sealing body and the lead terminal, causing electrolyte leakage through the gap. In such a case, the quality characteristics of the electrolytic capacitor may be degraded.

[0045] Therefore, in this modification, an upper limit dmu is set for the maximum diameter dm of the welded portion, and only lead terminals that satisfy dm < dmu are deemed to be non-defective. The upper limit dmu is a value that sufficiently suppresses electrolyte leakage and may be set, for example, to "wire diameter + 0.100 mm" (dmu = wire diameter + 0.100 mm). In the examples of FIGS. 7A and 8A , the maximum diameter dm of the welded portion 104 is less than the upper limit dmu, while the maximum diameter dm of the welded portion 114 significantly exceeds the upper limit dmu. Therefore, when manufacturing an electrolytic capacitor using lead terminals with a wire diameter ratio of 83%, laser welding can adequately suppress electrolyte leakage, but arc welding may result in electrolyte leakage, which may lead to a deterioration in the quality characteristics of the electrolytic capacitor.

[0046] The reason why the shape of the welded portion of lead terminal 101 can be more precisely controlled than that of lead terminal 111 is believed to be due to the difference in the welding method. Specifically, with laser welding, the environmental conditions during irradiation are preset to match the wire diameter ratio, allowing the shape of welded portion 104 to be appropriately controlled regardless of the wire diameter ratio. In contrast, with arc welding, the lead wire 113 made of CP wire becomes more difficult to melt as the wire diameter ratio increases (in other words, as the difference in wire diameter between the wire material and lead wire 113 decreases). Therefore, when the tip of the insufficiently molten lead wire 113 is forcefully inserted into the molten pool formed at the end of the wire material, the molten pool is pushed out radially while mixing with the small amount of molten metal at the tip of lead wire 113, resulting in the welded portion 114 having a shape that significantly protrudes radially.

[0047] Another factor that reduces the quality characteristics of electrolytic capacitors is the bending strength of the welded portion of the lead terminal. Bending strength is an index of the strength of the welded portion, and is expressed as the number of cycles (n) required for the lead wire to break, where one cycle is defined as bending the lead wire 90° to one side relative to the wire material, returning it, and then bending it 90° to the other side (the opposite direction). For example, if the lead wire breaks after two cycles, n = 2. The greater the number of cycles (n), the stronger the welded portion. Note that if the lead wire breaks after being bent 90° to one side relative to the wire material and then returned, the number of cycles (n) is defined as "the number of cycles up to that point + 0.5." When electrolytic capacitors are manufactured using lead terminals with low bending strength, the lead terminals may break due to vibration or slight impact during use, which may result in a reduction in the quality characteristics of the electrolytic capacitor.

[0048] Therefore, in this modification, a lower limit nl is set for the number of cycles n, and only lead terminals that satisfy n≧nl are deemed to be non-defective. The lower limit nl is a value that sufficiently prevents breakage of the lead terminal due to vibration or mild impact, and in the dimensional standard of this modification, it may be set to, for example, 1.0 cycle. Bending strength tests were conducted on lead terminals 101 and 111, and the number of cycles n for lead terminal 101 was 1.5 cycles, satisfying n≧nl, while the number of cycles n for lead terminal 111 was 0.5 cycles, satisfying n<nl. Therefore, when manufacturing an electrolytic capacitor using lead terminals with a wire diameter ratio of 83%, laser welding can adequately prevent breakage of the lead terminal, but arc welding may result in a deterioration in the quality characteristics of the electrolytic capacitor due to breakage of the lead terminal.

[0049] The higher bending strength of lead terminal 101 compared to lead terminal 111 is believed to be due to the difference in composition between welded portion 104 and welded portion 114. The following description will be made with reference to FIGS. 7B, 7C, 8B, and 8C. In FIG. 7B, portion p1 corresponds to rod-shaped portion 121, portions p2 and the upper end of portion p3 correspond to welded portion 104, and the remainder of portion p3 corresponds to lead wire 103. Portion p2 accounts for the majority of welded portion 104. The shades of color in portions p1 to p3 are due to the amount of X-ray penetration. Portion p1 exhibits a color derived from the main component of the wire (aluminum), while portion p3 exhibits a color derived from the main component of lead wire 103 (iron). Portion p2 exhibits a color intermediate between the two, suggesting that aluminum and iron (strictly speaking, iron, plus traces of copper and tin) melt and solidify in portion p2.

[0050] This is also supported by Figure 7C. In Figure 7C, portion p4 corresponds to the rod-shaped portion 121, portions p5 and the upper end of portion p6 correspond to the weld 104, and the remainder of portion p6 corresponds to the lead wire 103. Portion p5 accounts for the majority of the weld 104. The shades of color in portions p4 to p6 are due to the type and concentration of elements. Portion p4 exhibits a color derived from the main component of the wire (aluminum), while portion p6 exhibits a color derived from the main component of the lead wire 103 (iron). Portion p5, like portion p2, exhibits a color intermediate between the two. From the above, it can be seen that the majority of the weld 104 has a composition resulting from the melting and mixing of aluminum and iron (strictly speaking, iron, plus traces of copper and tin), which then solidified. Hereinafter, such a composition will be referred to as a "mixed composition."

[0051] 8B , the portion of portion p11 excluding its lower end corresponds to the rod-shaped portion 131, the lower end of portion p11, portion p12, and the upper end of portion p13 (in other words, the portion of portion p13 covered by portions p11 and p12) correspond to the welded portion 114, and the remainder of portion p13 corresponds to the lead wire 113. Portion p13 accounts for the majority of the welded portion 114. Portion p11 exhibits a color derived from the main component of the wire (aluminum), while portion p13 exhibits a color derived from the main component of the lead wire 103 (iron). Portion p12 exhibits a color intermediate between the two, and therefore it is believed that aluminum and iron (strictly speaking, iron, plus trace amounts of copper and tin) melt and solidify in portion p12.

[0052] This is also supported by Figure 8C. In Figure 8C, the portion of portion p14 excluding its lower end corresponds to the rod-shaped portion 131, the lower end of portion p14, portion p15, and the upper end of portion p16 (in other words, the portion of portion p16 covered by portions p14 and p15) correspond to the welded portion 114, and the remainder of portion p16 corresponds to the lead wire 113. Portion p16 accounts for the majority of the welded portion 114. Portion p14 exhibits a color derived from the main component of the wire (aluminum), while portion p16 exhibits a color derived from the main component of the lead wire 113 (iron). Portion p15, like portion p12, exhibits a color intermediate between the two. From the above, it can be seen that the majority of the weld 114 has an iron composition, and that a boundary between different metals (iron and aluminum) is formed between portions p13 and p11 (or between portions p16 and p14) within the weld 114. In addition, it can be seen that the mixed composition is formed only in the outer peripheral portion of the weld 114.

[0053] As described above, the welded portion 104 is mostly composed of a mixture of aluminum and iron. Therefore, when a bending load is applied to the lead terminal 101, the welded portion 104 acts as a buffer, preventing stress from concentrating at the welded portion 104, resulting in increased bending strength. In contrast, the welded portion 114 is mostly composed of iron, and a boundary between dissimilar metals (iron and aluminum) is formed within the welded portion 114. Therefore, when a bending load is applied to the lead terminal 111, stress concentrates at the welded portion 114 due to the difference in physical properties (typically, hardness and bendability) between the iron and aluminum. In particular, in the examples of Figures 8A to 8C, the wire diameter ratio is relatively large (in other words, the difference in wire diameter between the wire material and the lead wire 113 is small), which increases the area of ​​the boundary between the iron and aluminum, resulting in correspondingly large stress concentrations. As a result, the bending strength is likely to be reduced.

[0054] In order to verify the superiority of laser welding over arc welding in terms of wire diameter ratio, the inventors of the present application manufactured seven lead terminal samples (Samples 1 to 7) with different wire diameter ratios by laser welding and arc welding, respectively, and conducted tests to investigate the quality of the samples. Table 1 below shows the test results for Samples 1 to 7 of lead terminals in which the wire material is an aluminum wire and the lead wire is a CP wire.

[0055] In this test, the quality of the lead terminal was evaluated as good (○) when the maximum diameter dm of the welded portion satisfied dm < dmu and the number of cycles n in the bending strength test satisfied n ≥ nl. The quality of the lead terminal was evaluated as poor (×) when dm ≥ dmu or n < nl. The upper limit dmu is "diameter of the wire rod + 0.100 mm" regardless of the wire diameter ratio. Meanwhile, the lower limit nl is set to a predetermined value for each dimensional standard of the lead terminal. For example, nl = 1.5 when the wire diameter ratio is 33%, nl = 2.0 when the wire diameter ratio is 40%, nl = 2.0 when the wire diameter ratio is 53%, nl = 1.5 when the wire diameter ratio is 57%, nl = 1.0 when the wire diameter ratio is 67%, nl = 1.0 when the wire diameter ratio is 83%, and nl = 1.0 when the wire diameter ratio is 100%. It should be noted that different types of CP wires (for example, CP wires with different thicknesses of copper plating layers) may be used depending on the dimensional standards of the lead terminals.

[0056] With laser welding, the quality is good for all samples 1 to 7. In contrast, with arc welding, the quality is good for samples 1 to 5, but poor for samples 6 and 7.

[0057] The good quality of the laser-welded lead terminals for all Samples 1 to 7 is believed to be due to the following two reasons. First, in laser welding, the environmental conditions during irradiation are set in advance to match the wire diameter ratio, so the shape of the weld can be appropriately controlled regardless of the wire diameter ratio. Second, in laser welding, most of the weld is made of a mixed composition, so stress is less likely to concentrate on the weld, and high bending strength can be achieved.

[0058] In contrast, the poor quality of the arc-welded lead terminals for Samples 6 and 7 is believed to be due to the following two reasons. First, in arc welding, as the wire diameter ratio increases, the lead wire made of CP wire becomes more difficult to melt. Therefore, in lead terminals with a wire diameter ratio of 83% or more, the tip of the insufficiently molten lead wire is thrust forcefully into the molten pool formed at the end of the wire, causing the weld to protrude significantly in the radial direction. Second, in arc-welded lead terminals with a wire diameter ratio of 83% or more, the majority of the weld is composed of iron, and in lead terminals with a wire diameter ratio of 83% or more, the area of ​​the boundary between dissimilar metals (iron and aluminum) in the weld increases. Therefore, when a bending load is applied to the lead terminal, large stress tends to concentrate in the weld, reducing the bending strength of the lead terminal.

[0059] The good quality of the arc-welded lead terminals for Samples 1 to 5 is believed to be due to the following two reasons. First, in lead terminals with a wire diameter ratio of 67% or less, the lead wire made of CP wire melts sufficiently even when arc-welded, making it difficult for the weld to protrude significantly in the radial direction even when the tip of the lead wire is forcefully inserted into the molten pool formed at the end of the wire. Second, in lead terminals with a wire diameter ratio of 67% or less, the area of ​​the boundary between dissimilar metals in the weld is relatively small, so stress does not concentrate significantly in the weld even when a bending load is applied to the lead terminal.

[0060] According to Table 1, the quality of laser-welded lead terminals can be guaranteed regardless of the wire diameter ratio. However, in this modification, the invention targets lead terminals with a wire diameter ratio of 83% or more and 100% or less. This is because, with recent advances in the automotive and computer industries, the applications of electrolytic capacitors are expected to become increasingly diverse in the future, and as a result, there is a demand for the development of lead terminals with relatively large wire diameter ratios as one of the lead terminals with various dimensional standards. While most conventional lead terminals have been manufactured by arc welding, as is clear from Table 1, it has been difficult to ensure quality with arc welding when the wire diameter ratio is relatively large. In contrast, because the lead terminal according to this modification is manufactured by laser welding, the quality can be appropriately guaranteed even for lead terminals with wire diameter ratios (i.e., 83% to 100%) whose quality could not be guaranteed with arc welding.

[0061] In addition, because the wire diameter ratio is large, if the diameter of the wire material 100 is the same as that of a conventional wire, a thicker lead wire than that of a conventional wire can be used for the lead wire 103. As the diameter of the lead wire 103 increases, the thickness of the copper plating layer also increases accordingly. Since the conductivity of the lead wire 103 is mainly provided by copper, this configuration can reduce the electrical resistance of the lead terminal 101 and improve the electrical characteristics of the electrolytic capacitor.

[0062] Furthermore, the lead terminal 101 may be manufactured by a manufacturing method according to Modification 2. That is, a wire containing mainly copper may be used instead of an aluminum wire as the wire 100. In this case, the same results as those in Table 1 were obtained.

[0063] Furthermore, a metal wire containing mainly copper (hereinafter also referred to as a "copper lead wire") may be used as the lead wire 103 instead of a CP wire. Here, "metal wire containing mainly copper" means a metal wire whose outer surface is coated with a tin-plated layer or a silver-plated layer. In this case, the lead terminal 101 includes two types: "a lead terminal in which the wire material 100 is an aluminum wire and the lead wire 103 is a copper lead wire" and "a lead terminal in which the wire material 100 is a wire material containing mainly copper and the lead wire 103 is a copper lead wire." With both types of lead terminal 101, results similar to those in Table 1 were obtained.

[0064] As described above, the manufacturing method of the lead terminal 101 and the lead terminal 101 according to the third modification can provide a manufacturing method for appropriately manufacturing the lead terminal 101 having the electrode terminal 102 made of the wire 100 containing mainly aluminum or copper, and the lead terminal 101 manufactured by the manufacturing method. The lead terminal 101 is not limited to an electrolytic capacitor and may be used as a component of other power storage devices. Examples of other power storage devices include lithium ion capacitors, electric double layer capacitors, and lithium ion batteries. The same effects can be achieved even when the lead terminal 101 is used as a component of other power storage devices.

[0065] Although the embodiment and modifications 1 to 3 have been described above, the present invention is not limited to the above-described embodiment and modifications, and various modifications are possible without departing from the object of the present invention.

[0066] For example, as in Modification 3, in the embodiment, Modifications 1, and 2, the type of lead wire is not limited to a CP wire. The lead wire may be, for example, a copper lead wire (a metal wire mainly containing copper). When a copper lead wire is used in Modification 2 (i.e., when the main metal materials of the wire rod 100 and the lead wire 3 are both copper), the following effect is obtained in addition to the above-described effect. That is, when the main metal materials of the wire rod 100 and the lead wire 3 are both copper, there is a problem that, when attempting to melt the wire rod 100 by arc welding, the lead wire 3 melts excessively, making it impossible to properly connect the wire rod 100 and the lead wire 3 (in other words, making it impossible to properly form the welded portion 4). On the other hand, when the amount of discharge is suppressed in order to properly melt the lead wire 3, the wire rod 100 does not melt sufficiently, and in this case, there is also a problem that the wire rod 100 and the lead wire 3 cannot be properly connected. In contrast, in the manufacturing method according to Modification 2, only the end 100a of the wire 100 is melted by laser welding, and the lead wire 3 is pressed into the molten pool A and then melted by the heat of the molten pool A. The molten pool A at the end 100a and the molten copper at the end 3a of the lead wire 3 mix and solidify to form the weld 4. This manufacturing method can avoid excessive melting of the lead wire 3 or insufficient melting of the wire 100, thereby enabling the appropriate manufacturing of the lead terminal 101 in which the main metallic materials of both the wire 100 and the lead wire 3 are copper, which has been difficult to manufacture by arc welding. Note that the weld 4 is mostly a solidified copper structure, with a small amount of alloy of copper and other metals (e.g., tin).

[0067] The pushing mechanism may be provided in the jig 200 instead of the jig 300. That is, the pushing mechanism may be configured to apply an external force to the wire 100 that pushes the wire 100 axially toward the lead wire 3 by a predetermined distance at a predetermined speed.

[0068] Furthermore, in the above embodiment (and variants 1 to 3), the wire material 100 of the electrode terminal 2 is welded to the lead wire 3, and then the wire material 100 is pressed to form the electrode terminal 2. However, instead of this, the wire material 100 may first be pressed to form the electrode terminal 2, and then the lead wire 3 may be welded to one end of the rod-shaped portion 21.

[0069] Furthermore, in the above-described embodiment and modifications 1 to 3, a hybrid laser that combines an infrared laser and a short-wavelength laser may be used as the laser irradiator 400 .

[0070] Furthermore, as described in the above embodiment, the absorptivity of aluminum is equivalent across the entire wavelength bands of infrared and visible light. Therefore, when an aluminum wire is used for the wire rod 100, other inexpensive laser irradiators may be used in addition to the infrared laser or short wavelength laser.

[0071] 1, 101: lead terminal, 2, 102: electrode terminal, 3, 103: lead wire, 3a: end of lead wire, 3b: end face of lead wire, 3c: outer circumferential surface of lead wire, 4, 104: welded portion, 21, 121: rod-shaped portion, 22, 122: rolled portion, 100: wire rod, 100a: end of wire rod, 100b: end face of wire rod, 100c: outer circumferential surface of wire rod, 200: jig, 300: jig, 400: laser irradiator

Claims

1. A method for manufacturing a lead terminal for an electricity storage device, comprising an electrode terminal made of a wire containing mainly aluminum or copper, and a lead wire connected to the electrode terminal via a weld, comprising: a first step of linearly aligning the wire and the lead wire and holding the wire and the lead wire in a state in which a predetermined distance is maintained between the lead wire side end face of the wire and the wire wire side end face of the lead wire; a second step of irradiating the lead wire side end face of the wire with a laser beam using a laser irradiator to melt the end; and a third step of pushing one of the wire and the lead wire in the axial direction toward the other to form the weld, a predetermined time after the start of irradiation of the laser beam in the second step.

2. A method for manufacturing a lead terminal according to claim 1, wherein in the first step, a CP wire or a metal wire mainly containing copper is used as the lead wire.

3. A method for manufacturing a lead terminal as claimed in claim 1, wherein in the second step, the laser beam is irradiated onto the outer peripheral surface of the end of the wire in a direction perpendicular to the axial direction.

4. A method for manufacturing a lead terminal as claimed in claim 3, wherein in the second step, the laser beam is irradiated onto a predetermined position on the outer circumferential surface of the wire.

5. A method for manufacturing a lead terminal as described in claim 3, wherein in the first step, a wire material mainly containing aluminum is used as the electrode terminal, and the predetermined time in the third step is the irradiation time of the laser beam.

6. A method for manufacturing a lead terminal as described in claim 4, wherein in the first step, a wire material mainly containing aluminum is used as the electrode terminal, and the predetermined time in the third step is the irradiation time of the laser beam.

7. A method for manufacturing a lead terminal as claimed in claim 1, wherein in the second step, the end face of the end of the wire is irradiated with the laser beam from a direction obliquely intersecting the axial direction.

8. A method for manufacturing a lead terminal as described in claim 7, wherein in the first step, a wire material mainly containing aluminum is used as the electrode terminal, and the predetermined time in the third step is the irradiation time of the laser beam.

9. A method for manufacturing a lead terminal according to any one of claims 1 to 8, wherein in the first step, a wire material mainly containing aluminum is used as the electrode terminal, and the laser irradiation device is an infrared laser.

10. A method for manufacturing a lead terminal according to any one of claims 1 to 4 and claim 7, wherein in the first step, a wire material mainly containing copper is used as the electrode terminal, and the laser irradiator is a short-wavelength laser or a hybrid laser.

11. A method for manufacturing a lead terminal as claimed in any one of claims 1 to 8, wherein in the first step, a wire material and a lead wire are used in which a wire diameter ratio of the lead wire to the wire material is 83% or more and 100% or less.

12. A lead terminal for an electricity storage device, comprising an electrode terminal made of a wire material mainly containing aluminum or copper, and a lead wire connected to the electrode terminal via a welded portion, wherein the ratio of the diameter of the lead wire to the wire material is 83% or more and 100% or less.

13. The lead terminal according to claim 12, wherein the lead wire is a CP wire or a metal wire mainly containing copper.

Citation Information

Patent Citations

  • Method for manufacturing terminals for electronic components and terminals for electronic components obtained by the same manufacturing method

    JP5461570B2

  • Terminal structure of an electrolytic capacitor

    JP1982102125U

  • JP1986065741U

  • Terminal for electronic component and manufacturing method thereof

    JP2004335859A

  • Method for producing terminal for electronic component, and terminal for electronic component produced by the production method

    WO2011052091A1