The production process of nanoparticle zinc oxide
A low-temperature zinc oxide production process using acidic and basic solutions addresses inefficiencies in existing methods by achieving high-purity, small-particle-size zinc oxide with reduced waste and energy consumption, enhancing economic viability and market competitiveness.
Patent Information
- Application Number
- PCT/TH2023/050020
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-05-19
- Filing Date
- 2023-08-15
- Publication Date
- 2024-11-28
AI Technical Summary
Current zinc oxide production processes require high heat, generate industrial waste, and use excessive chemical agents, resulting in low-quality zinc oxide with large particle sizes and high energy consumption, making them inefficient and costly.
A low-temperature process involving leaching zinc ingot with an acidic solution and reacting it with a basic solution to produce nanoparticle zinc oxide, achieving high purity and controlled particle size without generating waste, using nitric acid, sulfuric acid, or other acids in combination with sodium hydroxide, and subsequent rinsing and drying.
The process achieves high-purity zinc oxide (>98%) with particle sizes less than 100 nanometers, reducing energy consumption and eliminating industrial waste, while enabling high-volume production with economic advantages for domestic and international markets.
Smart Images

Figure TH2023050020_28112024_PF_FP_ABST
Abstract
Description
[0001] THE PRODUCTION PROCESS OF NANOPARTICLE ZINC OXIDE
[0002] Field of the Invention
[0003] Science related to the production process of nanoparticle zinc oxide
[0004] Background of the Invention
[0005] For the most part, the process of producing zinc oxide in Thailand use a production technology that applies principles of time and temperature control (thermal oxidation) by using a high-purity zinc ingot as a starting substance. It is then burned at 1,000 degrees Celsius. The resulting gaseous zinc then enters into reaction with the oxygen in the atmosphere to become a microparticle zinc oxide. This process requires a high fuel and energy investment outlay, since the technology involved must be imported from abroad. Also, the particle size of the zinc oxide that is produced by this technology is in the micrometer range, which has a rather large size, resulting in a low-quality zinc oxide. So the value of this zinc oxide powder is low. It therefore cannot compete in a diverse and potential market, or in a market requiring high-value merchandise. Moreover, the aforementioned production process generates industrial waste in the form of zinc ash in each production batch, amounting to over 1,000 tons annually, none of which has any potential future application.
[0006] As per a patent search, some prior inventions relating to the zinc oxide production process were found. For example:
[0007] A Chinese patent, publication number CN109775746A, describes a method of preparing nano-zinc oxide that comprises the addition of a solution mixture of acetic acid and ammonium bicarbonate in the ratio of acetic acid to ammonium bicarbonate of 1-3 : 1 into a starting substrate (secondary zinc oxide) in order to cleanse the zinc of impurities. After cleansing, lead dioxide is added and stirred for a period of 10-20 minutes to generate the reaction. Filtration is then conducted. The zinc powder is added to the remaining mixture from the filtration and stirred for 25-30 minutes. Filtration is then repeated. The product obtained is heated at 50-60 degrees Celsius for 35-40 minutes and is then filtered. It is then heated again at 120-150 degrees Celsius for 2-3 hours. It is subsequently burned in an oven heated to 450-500 degrees Celsius for 1.5-2.0 hours to obtain a nano-zinc oxide.
[0008] A Taiwanese patent, publication number TWI309637B, describes a neutral zinc oxide nano-powder sol method that uses a crystalline salt containing molten zinc to adjust its pH value within 4.0-9.0 with sodium hydroxide (NaOH) solution in order to form a zinc-containing crystalline salt. It is then rinsed and filtered. The appropriate oxidants are then added, which may include hydrogen peroxide, chloric acid, perchloric acid or nitric acid, together with additives such as iron, copper, zinc, nickel and stannous oxide, or hydroxides, nitrates, carbonates, phosphates, sulfates, chlorides and surfactants like polyvinyl alcohol (PEG), polypropylene alcohol (PPG) and nonanol (NP). The selected ingredients are stirred at a rate of 30-1,200 revolutions per minute to generate a reaction lasting 4-24 hours at 70-100 degrees Celsius to form a nanoparticle zinc oxide (ZnO) of 2-100 nanometers.
[0009] A Chinese patent, publication number CN105197981B, describes a method of preparing high-potency nano-zinc oxide that comprises a process of inserting high-purity zinc material such as zinc oxide, zinc powder, zinc ingot into a 60%-concentration sulfuric acid solution in the ratio of n (Zn): n (SO4’2) = 1:1.2, creating a reaction lasting 1-3 hours. The zinc powder is then added, creating a reaction lasting 0.5-1 hour. It is then filtered to obtain the zinc-leaching water and is then brought into a reaction with a mixture of ammonium bicarbonate and ammonium carbonate with a molar concentration of 0.5-5 in a mixing ratio ranging from 10: 1 to 1 : 10. The reaction takes place in a reactor over a period of 1-5 hours at a controlled temperature of 30-70 degrees Celsius with a carbon-to-zinc ratio of n(C):n(Zn)=l:l-5:l. The obtained zinc-carbonate product (ZnCCh) is filtered and rinsed, and barium chloride (BaCh) is then used to test for the presence of any whitecolored settlings in the rinse water. Once the zinc carbonate is dry, it is inserted into an oven and burned at an elevated temperature of 400-850 degrees Celsius for a period of 5-10 hours to obtain a spherical nano-zinc oxide of 5-20 nanometers in size.
[0010] A Chinese patent, publication number CN109399693A, describes a preparation of high- purity nano-zinc oxide that comprises the purification of zinc sulfate by leaching a zinc substrate with sulfuric acid for a period of 1-2 hours to arrive at a zinc sulfate solution. It is then filtered and heated to within 70-90 degrees Celsius. Calcium carbonate and sulfuric acid are added to adjust the pH to 5. With the addition of potassium permanganate, metallic and manganese oxide sediments are filtered out to leave a purified zinc sulfate starter solution, which is then heated one additional time. Concentrated sulfuric acid is then added to adjust the pH of the solution. Heavy metallic-ion sediments are then filtered out, leaving a purified zinc sulfate solution. It is then mixed with ion-free water and stirred at high speed. Potassium carbonate is added to the mixture, which is then centrifuged to obtain zinc carbonate. A stabilizer, a silane coupling agent and methyl acrylate are then added to the mixture, which is placed in a vacuum environment where it comes under ultrasonic radiation. It is then cooled to room temperature and centrifuged into a dry condition. Following the addition of absolute ethanol, it is thoroughly mixed and centrifuged. The settlings will then be dried out to produce a high-purity nano-zinc oxide.
[0011] From the prior art above, it is readily apparent that the zinc oxide production process has been undergoing development. However, it is nonetheless a process requiring the use of high levels of heat, and even requires burning in an oven during the final step in order to derive the zinc oxide. In addition, devising this invention has required the use of additional raw materials, such as oxidation agents like hydrogen peroxide, chloric acid, perchloric acid and nitric acid, and additives like iron, copper, zinc, nickel, raw metallic oxides, hydroxides, nitrates, carbonates, phosphates, sulfates, chlorides and surfactants during the production process. However, there has yet to appear an invention that cites a high-quality zinc oxide production process using only low levels of heat and reducing the application of chemical agents to the level of the factory model as per this invention. As regards this invention, it is possible to control both the purity and particle size while obtaining a product consisting of zinc oxide with a high purity level of over 98% and not creating any industrial waste in the production process. In addition, it is also possible to control the zinc oxide particle size to less than 100 nanometers, with a zinc oxide production output as high as 16- 20 kilograms per production cycle.
[0012] Summary of the Invention
[0013] The nanoparticle zinc oxide production process consists of these steps: preparation of a zinc solution substrate by leaching zinc ingot with an acidic solution, which is selected from any one of nitric acid, hydrochloric acid, sulfuric acid, carbonic acid, acetic acid, citric acid or combination thereof. The ratio of zinc ingot to the acidic solution is between 1 : 3-5. When the specified time has elapsed, the specimen is then filtered in order to remove any non-reacting zinc ingot. The obtained zinc solution enters into a reaction with a basic solution, which is selected from any one of sodium hydroxide, potassium hydroxide, calcium hydroxide, magnesium hydroxide, lithium hydroxide, aluminum hydroxide, ammonium hydroxide or combination thereof. The ratio of the zinc solution to the basic solution in a reactor is 1 : 1-3, where it is heated. When the specified time has elapsed, it is filtered to obtain a nanoparticle zinc oxide (ZnO). The product is then rinsed in water and dried out by burning. It is then pulverized and stored in a packing bag.
[0014] The purpose of this invention is to provide a nanoparticle zinc oxide through an uncomplicated production process as an alternative to the importation of zinc oxide from abroad. Zinc oxide is useful as a component of high-value merchandise, such as cosmetics and rubber products, for example. Also, since the production process uses a low temperature and reduced energy consumption, the investment outlay is low. It thus provides an economic advantage for conducting business both within the country and abroad.
[0015] Brief Description of the Drawings
[0016] Figure 1 : The zinc oxide powder X-ray diffraction pattern
[0017] Detailed Description of the Invention
[0018] The production process of nanoparticle zinc oxide consists of the following steps.
[0019] A. Preparation of zinc oxide solution substrate B . Generating a reaction in a reactor to obtain zinc oxide (ZnO)
[0020] C. Rinsing the zinc oxide product with water
[0021] Details of each step in the production process of nanoparticle zinc oxide are as follows.
[0022] A. Preparation of zinc solution substrate by leaching zinc ingot with an acidic solution with molar concentration of 1-5 and constantly stirring this combination for a full 60-120 minutes. When the specified time has elapsed, it is then filtered to remove any non-reacting zinc ingot.
[0023] In one embodiment, the acidic solution is selected from any one of nitric acid, hydrochloric acid, sulfuric acid, carbonic acid, acetic acid, citric acid or combination thereof.
[0024] In another embodiment, the ratio of the zinc ingot to the acidic solution is 1 : 3-5.
[0025] In another embodiment, step A further comprises the addition of water during the leaching of the zinc ingot in that same step prior to the addition of the acidic solution, wherein the water used is either de-ionized (Dl-water) or water from the reverse osmosis process. The amount of water is preferably 1 / 4 of the volume of the container used in preparing the zinc solution substrate.
[0026] B . Generating a reaction in a reactor to obtain zinc oxide by bringing the zinc solution obtained from step A into a reaction with a basic solution with a molar concentration of 1-15 in a reactor. It is heated to a temperature of 50-120 degrees Celsius for a period of 4-24 hours. When the specified time has elapsed, it is then filtered to obtain a nanoparticle zinc oxide product.
[0027] In another embodiment, the basic solution is selected from any one of sodium hydroxide, potassium hydroxide, calcium hydroxide, magnesium hydroxide, lithium hydroxide, aluminum hydroxide, ammonium hydroxide or combination thereof.
[0028] In another embodiment, the ratio of the zinc solution to the basic solution is 1 : 1-3.
[0029] In yet another embodiment, the heat setting within the reactor is preferably at a temperature of 60-80 degrees Celsius.
[0030] C. Rinsing the zinc oxide product: The zinc oxide product is rinsed in water 3-5 times and then dried out by burning at 60-80 degrees Celsius for a period of 12-24 hours. It is then pulverized and stored in a packing bag.
[0031] In another embodiment, the water used is ion-free water or water from the reverse osmosis process.
[0032] In another embodiment, the step of rinsing the zinc oxide product further comprises rinsing the product with alcohol, which is selected from any one of methanol, ethanol, isopropanol, butanol, isobutanol or combination thereof.
[0033] In further embodiment, the step of rinsing the zinc oxide product requires rinsing with both water and ethanol from 3 to 5 times. The obtained zinc oxide has a purity level of more that 98% and a particle size less than 100 nanometers.
[0034] From this point on, descriptions of this invention will be made through invention examples that are intended to provide a clearer understanding. Nonetheless, the production process of nanoparticle zinc oxide and the relevant data that will be cited from this point on will only be examples for the purpose of making a greater understanding of the invention. They otherwise place no boundaries on the possible outcomes of the invention through these examples in any way whatsoever.
[0035] Example 1: The production process of nanoparticle zinc oxide
[0036] A. Prepare a zinc-nitrate (Zn(NOs)2) solution substrate by leaching zinc ingot. The zinc ingot is placed in a container. Then, add an amount of water equal to 1 / 4 of the volume of the container. Add a nitric acid solution of 1-5 molar concentration and stir constantly for 60-120 minutes. When the specified time has elapsed, filter it to remove any non-reacting zinc ingot.
[0037] B. Bring zinc nitrate obtained from step A into a reaction with a sodium hydroxide solution with a molar concentration of 1-15 in a reactor and heat this mixture to a temperature of 50-120 degrees Celsius for a period of 4-24 hours. When the specified time has elapsed, filter it to obtain a nanoparticle zinc oxide (ZnO).
[0038] C. Rinse the product obtained from step B with ion-free water and ethanol to remove any traces of sodium- nitrate solution (NaNCh) from the product. Then, dry it out by burning at 60- 80 degrees Celsius for a period of 12-24 hours. Finally, pulverize it and store in a packing bag. Example 2: Results of analyzing the specific characteristics of the synthesized zinc oxide obtained through the powder X-ray diffraction (XRD) technique
[0039] Analysis results by the powder X-ray diffraction technique indicate an X-ray diffraction pattern as shown in Figure 1, from which it was found that the obtained product was zinc oxide (ZnO). The X-ray diffraction pattern peaks of the product samples at positions 2theta = 31.7, 34.3, 36.2, 47.4, 56.5, 62.8, 66.3, 67.9 and 69.0 degrees corresponded to the structural formation of the zinc oxide (ZnO). By referring to the JCPDS Database no. 01-080-0074, after having analyzed the crystallite size from the Scherrer equation, it was found that the zinc oxide had a crystallite size of approximately 54.5 nanometers. Otherwise, the X-ray diffraction pattern of the sample was that of purified zinc oxide. No other intervening peaks were found, and there was a high level of crystallinity.
[0040] Example 3: Results of analyzing the specific characteristics of the elemental composition of the zinc oxide by use of quantitative analysis tools for the presence of elements and metals The analytical results of the elemental composition of the zinc oxide were obtained by use of quantitative analysis tools for the presence of elements and metals. An inductively coupled plasma-optical emission spectrometer was implemented in order to analyze and quantify the elemental composition of the synthetic products. It was found that there were elemental components of zinc (Zn), cadmium (Cd), iron (Fe) and lead (Pb) in the amounts of 0.902, 0.000, 0.130 and 0.000 milligrams per liter, respectively.
[0041] Example 4: Results of analyzing the specific characteristics of the zinc oxide by use of a transmission electron microscope (TEM)
[0042] Analysis of the specific characteristics of the zinc oxide was accomplished by use of a transmission electron microscope for analysis of size and shape, and a selected area electron diffraction (SAED) pattern of the zinc oxide. It was found that the zinc oxide had a hexagonal shape and a size of 100 nanometers. When the zinc oxide was analyzed by the selected area electron diffraction technique, it was found that the crystal planes of the zinc oxide appeared to be equal to (100), (110), (101) and (002), which corroborated the research results derived from the powder X-ray diffraction technique. It can therefore be confirmed that the synthesized product is indeed zinc oxide.
[0043] Example 5: Results of surface area analysis by use of the Brunauer-Emmett-Teller (BET) surface area analyzer
[0044] From the surface area analysis results obtained by use of the BET surface area analyzer, it was found that the zinc sample had a surface area = 13.34 square meter per gram.
[0045] Best Mode of the Invention
[0046] As described in the Detailed Description of the Invention
Claims
Claims1. A production process of nanoparticle zinc oxide comprises the following steps:A. Prepare a zinc solution substrate by leaching zinc ingot with an acidic solution of 1- 5 molar concentration and stirring steadily for a period of 60-120 minutes. When the specified time has elapsed, filter out any non-reacting zinc oxide.B . Bring the zinc solution obtained from step A into a reaction with a basic solution of 1-15 molar concentration in a reaction tank, holding it to a temperature of 50-120 degrees Celsius for a period of 4-24 hours. When the specified time has elapsed, filter it to obtain a nanoparticle zinc oxide (ZnO) product.C. Wash the product obtained from step B with water and dry it at a temperature of 60- 80 degrees Celsius for a period of 12-24 hours. Then, pulverize and store it in a packing bag.
2. The production process of nanoparticle zinc oxide according to claim 1, wherein from step A the acidic solution is selected from any one of nitric acid, hydrochloric acid, sulfuric acid, carbonic acid, acetic acid, citric acid or combination thereof.
3. The production process of nanoparticle zinc oxide according to claim 1, wherein from step A the ratio of zinc ingot to acid solution is within 1 : 3-5.
4. The production process of nanoparticle zinc oxide according to claim 1, wherein step A further comprises the addition of water during the zinc ingot leaching process prior to the addition of acidic solution.
5. The production process of nanoparticle zinc oxide according to claim 4, wherein the water is either deionized water (Dl-water) or water drawn from the reverse osmosis process (RO water).
6. The production process of nanoparticle zinc oxide according to claim 4, wherein the amount of water added during the zinc ingot leaching process is preferably 1 / 4 the volume of the container used for the zinc ingot leaching.
7. The production process of nanoparticle zinc oxide according to claim 1, wherein from step B the basic solution is selected from any one of sodium hydroxide, potassium hydroxide, calcium hydroxide, magnesium hydroxide, lithium hydroxide, aluminum hydroxide, ammonium hydroxide or combination thereof.
8. The production process of nanoparticle zinc oxide according to claim 1, wherein from step B the ratio of zinc solution to basic solution is 1 : 1-3.
9. The production process of nanoparticle zinc oxide according to claim 1, wherein the heating in the reaction tank is preferably at a temperature of 60-80 degrees Celsius.
10. The production process of nanoparticle zinc oxide according to claim 1, wherein from step C the water is deionized water or reverse osmosis water.
11. The production process of nanoparticle zinc oxide according to claim 1, wherein step C further comprises the wash of product with alcohol, which is selected from any one of methanol, ethanol, isopropanol, butanol, isobutanol or combination thereof.
12. The production process of nanoparticle zinc oxide according to claim 1, wherein from step C the obtained product is washed with water and alcohol.
13. The production process of nanoparticle zinc oxide according to claim 1, wherein from step C the obtained product is washed 3-5 times.
Citation Information
Patent Citations
Preparation process of secondary zinc oxide through leaching, calcination and purification
CN110078113A
Preparation method of zinc oxide desulfurizer
CN115448356A
Preparation of ZnO Powder by Pyrophoric SynthesisMethod
KR1020020083651A
Methods of Preparing P-type ZnO Nanoparticles and Ink Formulation Using the Same
KR1020130135539A
Method for producing single crystalline zinc oxide nanoparticles
US20170130358A1