Preparation method of structured catalytic articles

The method of mixing and calcining a catalyst precursor with support and shape-forming materials addresses the inefficiencies of conventional catalytic article production, enabling cost-effective and efficient creation of structured catalytic articles with enhanced catalytic performance.

WO2024243235A1PCT designated stage expired Publication Date: 2024-11-28WL GORE & ASSOC INC
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
PCT/US2024/030423
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-05-24
Filing Date
2024-05-21
Publication Date
2024-11-28

AI Technical Summary

Technical Problem

Conventional methods for producing catalytic articles are costly and inefficient due to multi-step procedures, including milling and calcination, which can result in undesired particle size distribution and shape, and require additional steps for specific forms like tri-lobe or honeycomb structures.

Method used

A method involving mixing a dry catalyst precursor, a dry support material, and a dry shape-forming material, followed by calcination, to form structured catalytic articles such as granular supported catalyst particles or catalytic tapes, using a combination of metals and ligands like vanadyl acetylacetonate or palladium acetylacetonate with support materials like TiO2 or Al2O3, and polymers like PTFE, under controlled conditions.

Benefits of technology

This method reduces production costs and complexity, allowing for the creation of catalytic articles with desired properties and structures, such as granular or tape forms, which exhibit efficient catalytic performance in reactions like DeNOx and NH3 oxidation.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure US2024030423_28112024_PF_FP_ABST
    Figure US2024030423_28112024_PF_FP_ABST
Patent Text Reader

Abstract

Various aspects of the present disclosure are directed towards apparatuses, systems, and methods of preparing supported catalytic articles by dry mixing and thermal treatment. The method for preparing a supported catalytic article may include mixing a dry catalyst precursor, a dry support material, and a dry shape forming material to form a mixture, and calcining the mixture. The dry catalyst precursor may include a metal and a ligand.
Need to check novelty before this filing date? Find Prior Art

Description

PREPARATION METHOD OF STRUCTURED CATALYTIC ARTICLESCROSS-REFERENCE TO RELATED APPLICATION

[0001] This application claims the benefit of Provisional Application No. 63 / 468,712, filed May 24, 2023, which is incorporated herein by reference in its entirety for all purposes.FIELD

[0002] The present disclosure relates generally to catalytic articles, and methods of preparing catalytic articles. More specifically, the present disclosure relates to structured catalytic articles and methods of preparing structured catalytic articles by mixing and thermal treatment.BACKGROUND

[0003] Conventional methods for producing a catalytic article include the use of active catalyst powders, and combining the active catalysts with binders to form catalytic articles. Preparing the active catalysts generally takes several steps including liquid impregnation process, drying process, and calcination process.

[0004] For example, structured catalytic articles may be prepared by either of two processes consisting of multiple steps: (1) preparation of a structured substate, like sphere, pellet, or honeycomb; impregnation of a metal catalyst on structured substrate; drying, and calcination, or (2) impregnation of metal catalyst on powder substrate; drying, calcination, and shape formation to make a sphere, pellet or monolith, where impregnation is a wet process.

[0005] These multiple-step procedures significantly increase the cost of catalyst as well as the catalytic article. For example, in certain cases, where the commercial catalyst is in the form of a pellet, the catalyst needs to be milled before processing to make a catalytic article. In other cases, the commercially available catalyst powder does not have the desired particle size distribution or shape, resulting in additional efforts for making articles with the desired properties. In yet other instances additional steps are required to obtain catalytic articles that are a tri lobe, a honeycomb or a tape.SUMMARY

[0006] The present disclosure relates to structured catalytic articles and methods of preparing structured catalytic articles by mixing and thermal treatment.

[0007] According to one Embodiment (Embodiment 1 ), provided is a method for preparing a catalytic article including: mixing a dry catalyst precursor, a dry support material, and a dry shape forming material to form a mixture; and calcining the mixture to form the catalytic article including granular supported catalyst particles; wherein the dry catalyst precursor includes a metal and a ligand.

[0008] According to another Embodiment (Embodiment 2), provided is a method for preparing a catalytic article including: mixing a dry catalyst precursor, a dry support material, and a dry shape forming material to form a mixture; compressing the mixture into a mixture of compressed solids; calcining the mixture pack; and forming the mixture pack into the catalytic article comprising a catalytic tape or a catalytic membrane; wherein the catalyst precursor comprises a metal and a ligand.

[0009] Embodiment 3 is the method of either of Embodiments 1 or 2, wherein the dry shape forming material comprises dry polymer.

[0010] Embodiment 4 is the method of Embodiment 3, wherein the polymer comprises polytetrafluoroethylene (PTFE), polypropylene (PP), polyvinylidene fluoride (PVDF), polybenzimidazole (PBI), polyether ether ketone (PEEK), polyether ketone ketone (PEKK) or polyethylene (PE).

[0011] Embodiment 5 is the method of Embodiment 1 , wherein the granular supported catalyst particles have an average particle size of 5 urn to 3000 urn.

[0012] Embodiment 6 is the method of Embodiment 1 , wherein the granular supported catalyst particles have an average specific area of 10-1500 m2 / g.

[0013] Embodiment 7 is the method of Embodiment 1 , wherein the mixing and the calcining are conducted simultaneously or consecutively.

[0014] Embodiment 8 is the method of Embodiment 2, wherein the calcining and the forming are conducted simultaneously or consecutively.

[0015] Embodiment 9 is the method of any of Embodiments 1-8, wherein the mixture includes from 25-95% of the dry catalyst precursor by weight and the dry support material, and from 5-75% of the dry shape forming material by weight.

[0016] Embodiment 10 is the method of any of Embodiments 1 -9, wherein the support material is a porous support material selected from the group consisting of metal oxides, zeolites, carbons, clays, metal organic frameworks, and combinations thereof.

[0017] Embodiment 11 is the method of any of Embodiments 1-9, wherein the porous support material is selected from one or more of TiO2, S iC>2, AI2O3, zeolite, aluminosilicate or activated carbon.

[0018] Embodiment 12 is the method of any of Embodiments 1-11 , wherein the metal is selected from one or more of transition metals, lanthanides, alkali or alkaline earth metals, or salts thereof.

[0019] Embodiment 13 is the method of any of Embodiments 1 -12, wherein the metal is selected from the group consisting of vanadium, copper, platinum, palladium, nickel, iron, cobalt, molybdenum, rhodium, ruthenium, rhenium, or mixtures thereof.

[0020] Embodiment 14 is the method of any of Embodiments 1 -13, wherein the ligand is a carbonyl, oxalate, ammonium, dimethylamino, bromide, chloride, cyclopentadienyl, diketonate or a ligand of formula I:wherein R1 and R2 are independently alkyl, substituted alkyl, aryl, substituted aryl, acyl and substituted acyl.

[0021] Embodiment 15 is the method of any of Embodiments 1 -15, wherein the catalyst precursor is selected from the group consisting of vanadyl acetylacetonate, vanadium (III) acetylacetonate, platinum (II) acetylacetonate, palladium^ I) acetylacetonate, bis(acetylacetonato)dioxomolybdenum (VI), and copper (II) acetylacetonate.

[0022] Embodiment 16 is the method of any of Embodiments 1 -15, wherein mixing comprises mixing in a vortex mixer, a shaking mixer, a double cone mixer, or a combination thereof for a period of time of from 30 seconds to 10 hours.

[0023] Embodiment 17 is the method of any of Embodiments 1 -16, wherein the mixing step is conducted under inert, dry or ambient conditions.

[0024] Embodiment 18 is the method of any of Embodiments 1 -17, wherein the mixture is calcined at a temperature of from 100°C to 350°C at a rate of 1 °C / min to 50°C / min.

[0025] Embodiment 19 is the method of any of Embodiments 1 -18, wherein the mixture is calcined in an atmosphere containing from 1 to 100 vol.% oxygen.

[0026] Embodiment 20 is the method for any of Embodiments 1-19, wherein the catalytic article has a content of the metal of from 0.1 wt.% to 50 wt.% based on a total weight of the catalytic article.

[0027] Embodiment 21 is the method for any of Embodiments 1-20, wherein the support material has a surface area from about 10 m2 / g to about 3000 m2 / g.

[0028] Embodiment 22 is the method for any of Embodiments 1-21 , wherein thesupport material comprises particles having a mean diameter of from 0.5 pm to 1000 pm.

[0029] Embodiment 23 is the method for any of Embodiments 1-22, wherein the catalyst precursor is vanadyl acetylacetonate or vanadium (III) acetylacetonate, the support material is TiO2, and calcining is conducted at a temperature from 200°C to 350°C.

[0030] Embodiment 24 is the method for any of Embodiments 1-22, wherein the catalyst precursor is palladium^ I) acetylacetonate, the support material is AI2O3, and calcining is conducted at a temperature from 200°C to 350°C.

[0031] Embodiment 25 is a catalytic article prepared by the method of any of Embodiments 1-22 is used in flow-through or flow-by configuration.

[0032] Embodiment 26 is a method for catalyzing a reaction including contacting a reactant stream with the catalytic article of Embodiment 24, wherein the reaction is selected from the group consisting of DeNOx, selective catalytic reduction (SCR), partial oxidation, oxidation, reduction, hydrogenation, dehydrogenation, isomerization, a coupling reaction, an intramolecular Heck reaction, conjugate addition, a nucleophilic addition, an a-substitution reaction, and a ring-opening reaction.

[0033] Embodiment 27 is the method of Embodiment 2, wherein forming the mixture pack is conducted prior to the calcining the mixture pack.

[0034] Embodiment 28 is the method of Embodiment 2, wherein forming comprises rolling, compressing or calendaring.

[0035] The foregoing Embodiments are just that, and should not be read to limit or otherwise narrow the scope of any of the inventive concepts otherwise provided by the instant disclosure. While multiple embodiments are disclosed, still other embodiments will become apparent to those skilled in the art from the following detailed description, which shows and describes illustrative embodiments. Accordingly, the drawings and detailed description are to be regarded as illustrative in nature rather than restrictive in nature.BRIEF DESCRIPTION OF THE DRAWINGS

[0036] The accompanying drawings are included to provide a further understanding of the disclosure and are incorporated in and constitute a part of this specification, illustrate embodiments, and together with the description serve to explain the principles of the disclosure.

[0037] FIG. 1 is a flowchart illustrating a method for preparing a supported catalytic article in accordance with an embodiment;

[0038] FIG. 2 is a flowchart illustrating a method for preparing a supported catalytic article in accordance with an embodiment;

[0039] FIG. 3 is an optical image of 3.9wt%vanadium-62%TiO2-34.1 %PTFE catalytic granular in accordance with an embodiment;

[0040] FIG. 4 is a bar chart showing the DeNOx efficiency for a catalytic article (catalytic granular) at various temperatures, in accordance with an embodiment;

[0041] FIG. 5 is an optical image of 3.0wt%palladium-83.6%AI2O3-13.4%PTFE catalytic tape in accordance with an embodiment;

[0042] FIG. 6 is an SEM image of 3.0wt%palladium-83.6%AI2O3-13.4%PTFE catalytic tape in accordance with an embodiment;

[0043] FIG. 7 is a bar chart showing the DeNHs efficiency of a catalytic article (catalytic tape) at various temperatures, in accordance with an embodiment;

[0044] FIG. 8 shows absorbance of the 1530 cm’1and 1499 cm’1peaks as a function of time for a solution including a catalytic tape made from a method according to the present disclosure, in accordance with an embodiment;

[0045] FIG. 9 is a line graph showing the consumption of nitrobenzene in a solution including 3.0wt%palladium-83.6% Al2O3-13.4%PTFE catalytic tape in accordance with an embodiment; and

[0046] FIG. 10 is a line graph showing the formation of aniline in a solution including 3.0wt%palladium-83.6%Al2O3-13.4%PTFE catalytic tape in accordance with an embodiment.DETAILED DESCRIPTIONDefinitions and Terminology

[0047] This disclosure is not meant to be read in a restrictive manner. For example, the terminology used in the application should be read broadly in the context of the meaning those in the field would attribute such terminology.

[0048] With respect to terminology of inexactitude, the terms “about” and “approximately” may be used, interchangeably, to refer to a measurement that includes the stated measurement and that also includes any measurements that are reasonably close to the stated measurement. Measurements that are reasonably close to the stated measurement deviate from the stated measurement by a reasonably small amount as understood and readily ascertained by individuals having ordinary skill in the relevantarts. Such deviations may be attributable to measurement error, differences in measurement and / or manufacturing equipment calibration, human error in reading and / or setting measurements, minor adjustments made to optimize performance and / or structural parameters in view of differences in measurements associated with other components, particular implementation scenarios, imprecise adjustment and / or manipulation of objects by a person or machine, and / or the like, for example. In the event it is determined that individuals having ordinary skill in the relevant arts would not readily ascertain values for such reasonably small differences, the terms “about” and “approximately” can be understood to mean plus or minus 10% of the stated value.

[0049] As used herein, the term “activated carbon” may include any carbon with a relatively high surface area such as from about 50 to about 3000 m2 / g or from about 100 to about 2000 m2 / g (e.g., from about 200 to about 1500 m2 / g or about 300 to about 1000 m2 / g). The activated carbon may be derived from any carbonaceous material, such as coal (e.g., charcoal), nutshells (e.g., coconut) and wood. Any form of activated carbon may be used, such as powdered, granulated, extruded and pelleted activated carbon.

[0050] As used herein, a “structured catalytic article” is a catalytic article formed into a specific shape (e.g., granular, tape, membrane, filter bag, honeycomb, monolith, or any other suitable geometrically structured forms).Description of Various Embodiments

[0051] Persons skilled in the art will readily appreciate that various aspects of the present disclosure can be realized by any number of methods and apparatuses configured to perform the intended functions. It should also be noted that the accompanying drawing figures referred to herein are not necessarily drawn to scale, but may be exaggerated to illustrate various aspects of the present disclosure, and in that regard, the drawing figures should not be construed as limiting.

[0052] FIG. 1 is a flowchart illustrating a method 100 for preparing a supported catalytic article in accordance with an embodiment. One or more steps of method 100 may be optional and / or may be modified by one or more steps of other embodiments described herein. Additionally, one or more steps of other embodiments described herein may be added to the method.

[0053] At step 102, the method 100 may include loading a dry catalyst precursor 104, a dry support material 106, and a dry shape forming material 108. In some embodiments, the catalyst precursor 104 is free from any aqueous liquid or any organic liquid, the support material 106 is free from any aqueous liquid or any organic liquid,and the shape forming material 108 is free from any aqueous liquid or any organic liquid.

[0054] In some embodiments, the dry catalyst precursor 104 may include a metal and a ligand. In some embodiments, the metal may be selected from one or more of transition metals, lanthanides, alkali or alkaline earth metals, or salts thereof. In some embodiments, the metal may be selected from Groups 3 to 14 of the Periodic Table of Elements (e.g., the 38 transition metals, or metals from Groups 13 to 14 such as B, Al, Ga, In, Tl, Nh, Si, Ge, Sn, or Pb). Examples of suitable metals include Na, K, Or, Mn, Au, Fe, Cu, Zn, Sn, Ta, Ti, Sb, Al, Co, Ni, Mo, Ru, Rh, Pd and / or Pt and / or a compound (e.g., a halide, hydroxide, carbonate) of one or more of these metals.

[0055] In an exemplary embodiment, the metal is selected from the group consisting of vanadium, copper, platinum, palladium, nickel, iron, cobalt, molybdenum, rhodium, ruthenium, rhenium, or mixtures thereof.

[0056] In some embodiments, the ligand may be a carbonyl, oxalate, ammonium, dimethylamino, bromide, chloride, cyclopentadienyl, diketonate or a ligand of Formula (I): o o . JL ,, R1Formula (I)

[0057] wherein R1 and R2 are independently alkyl, substituted alkyl, aryl, substituted aryl, acyl and substituted acyl.

[0058] In an exemplary embodiment, the catalyst precursor 104 may include a metal and an acetylacetonate group or a ketone group. For example, the precursor may be selected from exemplary catalyst precursors listed in Table 1 .Table 1

[0059] In some embodiments, the catalyst precursor 104 is selected from the group consisting of vanadyl acetylacetonate, vanadium (III) acetylacetonate, platinum (II) acetylacetonate, palladium^ I) acetylacetonate, bis(acetylacetonato)dioxomolybdenum (VI), and copper (II) acetylacetonate.

[0060] The support material 106 is not particularly limiting provided the support material does not affect the end use of the catalytic composite. In some embodiments,the support material 106 may be porous. Examples of the support material may include, but are not limited to, metals, metal oxides (e.g., titanium dioxide, aluminum oxide, etc.), zeolites, carbons, clays, and combinations thereof.

[0061] In some embodiments, the dry support material 106 may be selected from the group consisting of metal oxides, zeolites, carbons, clays, metal organic frameworks, and combinations thereof. In an exemplary embodiment, the dry support material 106 may be selected from one or more of TiO2, SiC>2, AI2O3, zeolite, aluminosilicate or activated carbon.

[0062] The support material 106 may have a surface area from about 10 m2 / g to about 3000 m2 / g, from about 15 m2 / g to about 2500 m2 / g, from about 20 m2 / g to about 2000 m2 / g, from about 25 m2 / g to about 1500 m2 / g, from about 30 m2 / g to about 1000 m2 / g, from about 35 m2 / g to about 800 m2 / g, from about 40 m2 / g to about 600 m2 / g, from about 45 m2 / g to about 500 m2 / g, from about 50 m2 / g to about 400 m2 / g, from about 55 m2 / g to about 350 m2 / g, or may have a surface area encompassed within these ranges. In some embodiments, the support material 106 may have a surface area from about 60 m2 / g to about 340 m2 / g, from about 65 m2 / g to about 330 m2 / g, from about 70 m2 / g to about 320 m2 / g, or from about 75 m2 / g to about 310 m2 / g. In an exemplary embodiment, the support material 106 may have a surface area from about 80 m2 / g to about 305 m2 / g.

[0063] The support material 106 may include particles having a mean diameter of from about 0.5 pm to about 1000 pm, from about 0.6 pm to about 900 pm, from about 0.7 pm to about 800 pm, from about 0.8 pm to about 700 pm, from about 0.9 pm to about 600 pm, from about 1 .0 pm to about 500 pm, from about 1.1 pm to about 400 pm, from about 1 .2 pm to about 300 pm, from about 1 .3 pm to about 200 pm, from about 1 .4 pm to about 100 pm, or may include particles having a mean diameter encompassed within these ranges. In some embodiments, the support material 106 may include particles having a mean diameter of from about 1 .5 pm to about 90 pm, from about 1 .6 pm to about 80 pm, from about 1 .7 pm to about 70 pm, from about 1 .8 pm to about 60 pm, from about 1 .9 pm to about 55 pm, or from about 1 .95 pm to about 54 pm. In an exemplary embodiment, the support material 106 may include particles having a mean diameter of from about 2.0 pm to about 52 pm.

[0064] In some embodiments, the dry shape forming material 108 may include a dry polymer powder. In some instances, the polymer powder may be derived from a thermoplastic. For example, thermoplastics include Polymethyl Methacrylate (PMMA or Acrylic), Polystyrene (PS), Acrylonitrile Butadiene Styrene (ABS), Polyvinyl Chloride(PVC), Modified Polyethylene Terephthalate Glycol (PETG), Cellulose Acetate Butyrate (CAB); Semi-Crystalline Commodity Plastics that include Polyethylene (PE), High Density Polyethylene (HDPE), Low Density Polyethylene (LDPE or LLDPE), Polypropylene (PP), Polymethylpentene (PMP); Amorphous EngineeringThermoplastics that include Polycarbonate (PC), Polyphenylene Oxide (PPO), Modified Polyphenylene Oxide (Mod PPO), Polyphenelyne Ether (PPE), Modified Polyphenelyne Ether (Mod PPE), Polyurethane (PU), Thermoplastic Polyurethane (TPU); SemiCrystalline Engineering Thermoplastics that include Polyamide (PA or Nylon), Polyoxymethylene (POM or Acetal), Polyethylene Terephthalate (PET, Thermoplastic Polyester), Polybutylene Terephthalate (PBT, Thermoplastic Polyester), Ultra High Molecular Weight Polyethylene (UHMW-PE); High Performance Thermoplastics that include Polyimide (PI, Imidized Plastic), Polyamide Imide (PAI, Imidized Plastic), Polybenzimidazole (PBI, Imidized Plastic); Amorphous High PerformanceThermoplastics that include Polysulfone (PSU), Polyetherimide (PEI), Polyether Sulfone (PES), Polyaryl Sulfone (PAS); Semi-Crystalline High Performance Thermoplastics that include Polyphenylene Sulfide (PPS), Polyetheretherketone (PEEK); and SemiCrystalline High Performance Thermoplastics, Fluoropolymers that include Fluorinated Ethylene Propylene (FEP), Ethylene Chlorotrifluroethylene (ECTFE), Ethylene, Ethylene Tetrafluoroethylene (ETFE), Polychlortrifluoroethylene (PCTFE), Polytetrafluoroethylene (PTFE), Expanded Polytetrafluoroethylene (ePTFE), Polyvinylidene Fluoride (PVDF), Perfluoroalkoxy (PFA).

[0065] For example, the some embodiments, the polymer may include dry polytetrafluoroethylene (PTFE), dry polyethylene (PE), dry polypropylene (PP), dry polyvinylidene fluoride (PVDF), dry polybenzimidazole (PBI) or dry polyether ether ketone (PEEK).

[0066] At step 110, the method 100 may include mixing the catalyst precursor 104, the support material 106, and the shape forming material 108 to form a dry mixture. In some embodiments, step 110 may be performed using a vortex mixer, a shaking mixer, a double cone mixer, or a combination thereof. In some embodiments, step 110 may be performed using hand shaking in a scintillation vial. It is readily apparent that other mixing devices are suitable. In some embodiments, step 102 may be conducted under inert, dry or ambient conditions that is, for example, in the absence of O2, with dry N2 present.

[0067] In some embodiments, step 110 may be performed for a period of time of from about 30 seconds to about 10 hours, from about 1 minute to about 9.5 hours, fromabout 1.5 minutes to about 9 hours, from about 2 minutes to about 8.5 hours, from about 2.5 minutes to about 8 hours, from about 3 minutes to about 7.5 hours, from about 3.5 minutes to about 7 hours, from about 4 minutes to about 6.5 hours, from about 4.5 minutes to about 6 hours, from about 5 minutes to about 5.5 hours, from about 5.5 minutes to about 5 hours, or may be performed for a period of time encompassed within these ranges. In certain embodiments, step 110 may be performed for a period of time of from about 6 minutes to about 4.5 hours, from about 7 minutes to about 4 hours, or from about 8 minutes to about 3.5 hours. In an exemplary embodiment, step 110 may be performed for a period of time of from about 10 minutes to about 3 hours.

[0068] In some embodiments, the dry mixture formed in step 110 includes from about 25wt.% to about 95wt.% of the dry catalyst precursor 104 and the dry support material 106, and from about 5wt.% to about 75wt.% of the dry shape forming material. In certain embodiments, the dry mixture formed in step 110 includes from about 60% to about 80% of the dry catalyst precursor 104 and the dry support material 106, and from about 20% to about 40% of the dry shape forming material. In yet other embodiments, the dry mixture formed in step 110 includes from about 1wt.% to about 20wt.% of the dry catalyst precursor 104 and from 80wt.% to 99wt.% of the dry support material 106.

[0069] At step 112, the method 100 may include a calcining step 112 for heat treating the dry mixture formed in step 110. The calcining step 112 may be performed using standard calcining equipment such as, for example, a rotary calciner. In some embodiments, the mixing step 110 and the calcining step 112 may be conducted simultaneously (i.e. , combined into one step). In some embodiments, the mixing step 110 and the calcining step 112 may be conducted consecutively as shown in FIG. 1 .

[0070] In some embodiments, the calcining step 112 may be performed using a fast-heating method (e.g., heating the dry mixture formed in step 110 in an aluminum pan placed on a pre-heated hot plate). In some embodiments, the calcining step 112 may be performed using a slowing-heating method (e.g., slowly heating the dry mixture formed in step 110 in a crucible placed in a muffle oven starting at room temperature). In some embodiments, the mixture may be heated by being placed in a preheated oven.

[0071] In some embodiments, the dry mixture may be calcined at a temperature of from about 100°C to about 500°C, from about 105°C to about 480°C, from about 110°C to about 460°C, from about 115°C to about 440°C, from about 120°C to about 430°C, from about 125°C to about 420°C, from about 130°C to about 410°C, from about 135°C to about 400°C, from about 140°C to about 390°C, from about 145°C to about380°C, or at a temperature encompassed within these ranges. In some embodiments, the dry mixture 108 may be calcined at a temperature of from about 146°C to about 375°C, from about 147°C to about 370°C, or from about 148°C to about 365°C. In an exemplary embodiment, the dry mixture 108 may be calcined at a temperature of from about 100°C to about 350°C.

[0072] In certain embodiments, for example when the support is a polymeric support material, the dry mixture may be calcined at a temperature of from about 100°C to about 350°C. The polymeric support material (e.g., a porous felt) may include polytetrafluorethylene (PTFE), poly(ethylene-co-tetrafluoroethylene) (ETFE), polyparaxylylene (PPX), polyester (PE), polypropylene (PP), polyphenylene sulfide (PPS), P-84, nylon, acrylic, aramid or any combination or blend thereof.

[0073] In some instances, for example when the porous substrate is PE, the dry mixture may be calcined at a temperature of from about 100°C to about 135°C. In some instances, for example when the porous substrate is polypropylene (PP), the dry mixture may be calcined at a temperature of from about 100°C to about 120°C. In some instances, for example when the porous substrate is polyphenylene sulfide (PPS), the dry mixture may be calcined at a temperature of from about 100°C to about 190°C. In some instances, for example when the porous substrate is nylon, the dry mixture may be calcined at a temperature of from about 100°C to about 121 °C. In some instances, for example when the porous substrate is acrylic, the dry mixture may be calcined at a temperature of from about 100°C to about 135°C. In some instances, for example when the porous substrate is aramid, the dry mixture may be calcined at a temperature of from about 100°C to about 220°C.

[0074] In yet certain embodiments, for example when the porous substrate is an inorganic support material, the dry mixture may be calcined at a temperature of from about 100°C to about 500°C.

[0075] In some embodiments, the dry mixture may be calcined at a rate of from about 1°C / min to about 50°C / min, from about 1.25°C / min to about 45°C / min, from about 1.5°C / min to about 40°C / min, from about 1.75°C / min to about 35°C / min, from about 2°C / min to about 30°C / min, from about 2.25°C / min to about 25°C / min, from about 2.5°C / min to about 20°C / min, from about 2.75°C / min to about 15°C / min, from about 3°C / min to about 10°C / min, or at a rate encompassed within these ranges. In some embodiments, the dry mixture 108 may be calcined at a rate of from about 3.2°C / min to about 9°C / min, from about 3.4°C / min to about 8°C / min, from about 3.6°C / min to about 7°C / min, or from about 3.8°C / min to about 6°C / min. In an exemplary embodiment, thedry mixture 108 may be calcined at a rate of from about 4°C / min to about 5°C / min.

[0076] In some embodiments, the dry mixture is calcined in an atmosphere containing from about 1 to about 100 vol.% oxygen, from about 2 to about 20 vol.% oxygen, from about 3 to about 15 vol.% oxygen, from about 3.5 to about 10 vol.% oxygen, from about 4 to about 9 vol.% oxygen, from about 4.5 to about 8 vol.% oxygen, from about 5 to about 7 vol.% oxygen, from about 5.5 to about 6.5 vol.% oxygen, or containing a vol.% oxygen encompassed within these ranges. In an exemplary embodiment, the dry mixture 108 is calcined in an atmosphere containing about 6 vol.% oxygen.

[0077] At step 114, the method 100 includes forming a catalytic article having a granular structure. In some embodiments, the catalytic article includes granular supported catalyst particles.

[0078] In some embodiments, the granular supported catalyst particles have an average particle size of from about 5 urn to about 3000 urn, or from about 10 urn to about 2900 urn, or from about 15 urn to about 2800 urn, or from about 20 urn to about 2700 urn, or from about 25 urn to about 2600 urn, or from about 30 urn to about 2500 urn, or from about 35 urn to about 2400 urn, or from about 40 urn to about 2300 urn, or from about 45 urn to about 2200 urn, or from about 50 urn to about 2100 urn.

[0079] In some embodiments, the granular supported catalyst particles have an average specific area of from about 10 to about 1500 m2 / g, or from about 15 to about 1400 m2 / g, or from about 20 to about 1300 m2 / g, or from about 25 to about 1200 m2 / g, or from about 30 to about 1100 m2 / g, or from about 35 to about 1000 m2 / g, or from about 40 to about 900 m2 / g, or from about 45 to about 800 m2 / g, or from about 50 to about 700 m2 / g, or from about 55 to about 600 m2 / g.

[0080] In some embodiments, the catalytic article including granular supported catalyst particles formed in step 114 has a content of the metal (wt.%) based on the total weight of the catalytic article. In some embodiments, the catalytic article has a content of the metal of from about 0.1 wt.% to about 50 wt.%, from about 0.25 wt.% to about 45 wt.%, from about 0.5 wt.% to about 40 wt.%, from about 1 wt.% to about 35 wt.%, from about 1 .5 wt.% to about 32.5 wt.%, from about 2.0 wt.% to about 30 wt.%, from about 2.25 wt.% to about 27.5 wt.%, from about 2.5 wt.% to about 25 wt.%, from about 2.75 wt.% to about 22.5 wt.%, from about 3.0 wt.% to about 20 wt.%, based on the total weight of the catalytic article or has a content of the metal (wt.%) encompassed within these ranges. In an exemplary embodiment, the catalytic article has a content of the metal of from about 3.9 wt.% to about 15 wt.% based on the total weight of thecatalytic article. In yet another exemplary embodiment, the catalytic article has a content of the metal of from about 0.1 wt.% to about 10 wt.% based on the total weight of the catalytic article.

[0081] The catalytic article formed may be in a form of a filter bag, a honeycomb, a monolith, or any other suitable geometrically structured forms. In certain embodiments, the catalytic article is used in a flow-through configuration, where gas or liquid is flowing transverse to (e.g., perpendicular to) a cross section of the catalytic article, such that the gas or liquid passes through the catalyst particle layer in the catalytic article. In yet certain embodiments, the catalytic article is used in a flow-by configuration, where gas or liquid is flowing parallel to the cross-section of the catalytic article, such that the gas or liquid is flowing parallel and diffuse to the catalyst particle in the catalytic layer, and does not pass through the cross section of the catalytic article.

[0082] In some embodiments, a method for catalyzing a reaction includes contacting a catalytic article with a reactant stream. The reaction may be selected from a group consisting of DeNOx, selective catalytic reduction (SCR), partial oxidation, oxidation, reduction, hydrogenation, dehydrogenation, isomerization, a coupling reaction, an intramolecular Heck reaction, conjugate addition, a nucleophilic addition, an a-substitution reaction, and a ring-opening reaction.

[0083] In some embodiments, the catalytic article may be utilized in multiphase catalyzed reactions, such as for example a two- or three- phase reaction. There are numerous categories of multiphase catalyzed reactions including those with gas plus liquid reactants, gas plus liquid plus a second immiscible liquid phase reactants, liquid plus immiscible / liquid phase reactants, or gas plus condensed liquid vapor phase reactants and various other combinations with at least two distinct phases of matter exist for such reactants that can be used with the catalytic article. These reactions may be carried out where the catalytic article is located, for example, in a stirred tank autoclave reactor system, a continuous loop reactor, or a Parr Shaker Reactor as described herein.

[0084] For example, the catalytic article may be used in the hydrogenation of a solvated compound in a liquid or a compound in a mixture of immiscible liquids. The hydrogen source could be gas phase hydrogen, or another hydrogen donor component (Catalytic Transfer Hydrogenation). Non-limiting examples of solvents that may be employed in reactions include lower alcohols (e.g., methanol and ethanol), tetrahydrofuran, and glycols (e.g., ethylene glycol and diethylene glycol). The solvent may be present in the hydrogenation reaction in an amount from about 1 % to about99%, from about 1 % to about 75%, or from about 1 % to about 50% by weight of the charge. Non-limiting examples of hydrogen donor compounds include, ethanol, isopropanol, butanol, glycerol, formic acid, ammonium formate, or others known to those skilled in the art.

[0085] In some embodiments, the catalytic article has an NOx removal efficiency of from about 1 % to about 99%, from about 5% to about 90%, from about 10% to about 80%, from about 15% to about 70%, from about 20% to about 60%, or has an NOx removal encompassed within these ranges.

[0086] In some embodiments, the catalytic article has an NH3 oxidation efficiency of from about 20% to about 99%, from about 25% to about 90%, from about 30% to about 80%, from about 35% to about 75%, from about 40% to about 70%, from about 40% to about 65%, or has an NH3 oxidation efficiency encompassed within these ranges.

[0087] FIG. 2 is a flowchart illustrating a method 200 for preparing a supported catalytic article in accordance with an embodiment. One or more steps of method 200 are optional and / or can be modified by one or more steps of other embodiments described herein. Additionally, one or more steps of other embodiments described herein may be added to the method.

[0088] At step 202, the method 200 may include loading a dry catalyst precursor 204, a dry support material 206, and a dry shape forming material 208. In some embodiments, the dry catalyst precursor 204 may include a metal and a ligand. At step 210, the method 200 may include mixing the dry catalyst precursor 204, dry support material 206, and dry shape forming material 208 to form a dry mixture.

[0089] At step 212, the method 200 may include forming a structure out of the dry mixture formed in step 210. In some embodiments, the structure formation may include compressing the dry mixture into a mixture pack.

[0090] At step 214, the method 200 may include a thermal treatment and / or activation step to form a catalytic article including a catalytic tape or a catalytic membrane. In some embodiments, at step 214, the method 200 includes calcining the mixture pack formed in step 212. In some embodiments, step 214 includes forming the mixture pack into the shape of a tape or a membrane. In certain embodiments, the calcining and the forming are conducted simultaneously. In certain embodiments, the calcining and the forming are conducted consecutively. In some embodiments, the forming the mixture pack is conducted prior to the calcining the mixture pack. In some embodiments, step 214 may be conducted in a “batch” or “continuous” roll-to-rollprocess. For example, in a batch set up, the entire roll (or certain pieces of tape), may be place in the oven and heated to a desired temperature, and subsequently cooled. In a continuous roll to roll process, a tape may move from a first storage roll to a second storage roll passing through a heated zone therebetween. Thus, step 212 may be conducted in a “batch” or “continuous” roll-to-roll process. Alternatively, step 212 and 214 may be conducted in a “batch” or “continuous” roll-to-roll process.

[0091] The forming step may include any process that increases the surface to volume ratio of the catalytic article. In exemplary embodiments, forming may include rolling, compressing, calendaring, or any combination of these processes.TEST METHODS

[0092] It should be understood that although certain methods and equipment are described below, other methods or equipment determined suitable by one of ordinary skill in the art may be alternatively utilized.Particle Size Analysis

[0093] Particle size of TiO2 support was measured by dispersing the powder in iso-propanol, and using a Microtac Sync Size & Shape Particle Analyzer. The mean diameter (“MV”) of TiO2 support (CristalACTiV™ DT-51 , ) is 2.05 urn, is shown in Tables 2.Table 2. Particle size distribution of CristalACTiV™ DT-51 .EXAMPLESExample 1 - NOx removal efficiency on catalytic granular (3.9wt%vanadium-62%TiO2- 34.1 %PTFE)

[0094] Sample preparation: 1 .2 gram of TiO2 powder (CristalACTiV™ DT-51 , with a surface area of about 89.1 m2 / g), 0.39 gram of vanadyl acetylacetonate (Sigma- Aldrich), and 0.66 gram of fibrillatable homopolymer polytetrafluoroethylene (PTFE) fine powder particles were added into an IKA MT-40 disposable grinding chamber. The grinding chamber was placed into an IKA Tube mill and was milled for 18 minutes (e.g., for 6 times at 3-minute intervals). 0.2 gram of this mixture were loaded in a 57 mm aluminum crinkle dish and then placed on a hot plate pre-heated to 350 °C for 3 minutes, then 310 °C for 30 minutes. After a few seconds, smoke was observed indicating the decomposition of acetylacetonate. During the calcination process, the aluminum pan was shaken periodically by hand for a few seconds and then put back on the hot plate. The product formed, as shown in FIG. 3, are yellowish catalytic granular with diameter from about 60 urn to about 400 urn. The optical image was measured with a Keyence optical microscope.

[0095] NOx removal reaction: The following procedure was used to test performance of the catalytic granular in Example 1 for NOx removal. The NOx removal reaction of as prepared catalytic granular was carried out in a fixed-bed quartz flow reactor at different temperatures. 0.15 gram catalytic granular was used during the test. The feed gas mixture contained 100 ppm NO, 20 ppm NO2, 105 ppm NH3, 6 vol% 02 and N2 as balance. The NOx removal reaction was measured with a total flowrate of 0.45 L / min. To determine NOx removal efficiency, the upstream (i.e., the concentration of NOx entering into the chamber before exposure to the catalytic granular) and downstream concentration of NOx were monitored with a MKS MULTI-GASTM 2030D FTIR analyzer (MKS Instruments, Andover, MA).

[0096] NOx removal efficiency (i.e., “DeNOx efficiency (%)”) was calculated based on the following equation:NOx in - NOx out DeNOx efficiency (%) = - x 100%NOx in where NOx = total concentration of NO and NO2 in the stream NOx in = upstream concentration of NOxNOx out = downstream concentration of NOx

[0097] Results for the NOx removal efficiency calculated by using the catalytic article having granular supported catalyst particles at various temperatures are included in Table 1 and shown in FIG. 4.Table 1 .Example 2 - NOx removal efficiency on catalytic tape (3.9wt%vanadium-62%TiO2- 34.1 %PTFE)

[0098] Sample preparation: 1 .2 gram of TiO2 powder (CristalACTiV™ DT-51 ), 0.39 gram of vanadyl acetylacetonate (Sigma-Aldrich), and 0.66 gram of fibrillatable homopolymer polytetrafluoroethylene (PTFE) fine powder particles were added into an IKA MT-40 disposable grinding chamber. The grinding chamber was placed into an IKA Tube mill and was milled for 18 minutes (e.g., for 6 times at 3-minute intervals). 1 .0 gram of this mixture was placed into a 40 mm diameter boric acid die and was compressed into a pack by applying about 10 tn of pressure, using a hand operated hydraulic press (PHI Press), for about 10 minutes. Afterwards, the pack was removed from the die and placed on a hot plate pre-heated to 330 °C. After a few seconds smoke was observed indicating the decomposition of acetylacetonate. At that point a metal rod was used to compress and spread the pack to a tape by rolling back and forth several times on the hot plate. The tape was left on the hot plate pre-heated to 330°C for another two hours before measuring the area density and catalytic activity.

[0099] Area density: The catalytic tape area density was measured by die cutting a 26 mm diameter circle from the as prepared catalytic tape. The measured weight of the 26 mm diameter sample is 0.2582 gram. The calculated area density is 486.5 gram / m2(sample weight / sample area). The vanadium area density in the as- prepared catalytic tape is 19.0 gram / m2, the vanadium plus TiO2 area density in the as- prepared catalytic tape is 320.6 gram / m2.[000100] NOx removal reaction: The following procedure was used to test performance of the catalytic tape in Example 2 for NOx removal. A catalytic tape with 26 mm diameter was placed in a sample holder. The catalytic tape was exposed to an N2 balanced simulated flue gas at 200 °C. The simulated flue gas flowing through the catalytic tape contained 100 ppm NO, 20 ppm NO2, 105 ppm NH3, 6 vol% O2 and N2 with a total flowrate of 0.45 L / min. To determine NOx removal efficiency, the upstream (i.e. , the concentration of NOx entering into the chamber before exposure to the catalytic tape) and downstream concentration of NOx were monitored with a MKS MULTI-GASTM 2030D FTIR analyzer (MKS Instruments, Andover, MA).[000101 ] NOx removal efficiency (i.e., “DeNOx efficiency (%)”) was calculated based on the following equation:NOx in - NOx outDeNOx efficiency (%) = - — — - x 100%J v 7NOx in where NOx = total concentration of NO and NO2 in the streamNOx in = upstream concentration of NOxNOx out = downstream concentration of NOxTable 2.Example 3 - NH3 oxidation efficiency on catalytic tape (3.0wt%palladium-83.6%AI2O3- 13.4%PTFE)[000102] Sample preparation: 0.9351 gram of AI2O3 powder (Sigma Aldrich-No.199966), 0.0950 gram of palladium acetylacetonate (Pd(acac)2) (STREM Chemical Inc.), and 0.1498 gram of fibrillatable homopolymer polytetrafluoroethylene (PTFE) fine powder particles were added into an IKA MT-40 disposable grinding chamber. The grinding chamber was placed into an IKA Tube mill and was milled for about 30 min (10 time of 3 min intervals). 1.1 gr of this mixture were placed into a 40 mm diameter boric acid die and were compressed into a pack by applying about 15 tn of pressure, using ahand operated hydraulic press, for about 15 minutes. Upon removal from the die the pack broke into many pieces. A couple of pieces were placed on a hot plate pre-heated to 325 °C. After a few seconds smoke was observed indicating the decomposition of acetylacetonate. At that point a metal rod was used to compress and spread the pieces by rolling back and forth several times (process resembles that of spreading Filo dough with a rolling pin).[000103] The catalytic tape pieces prepared in Example 3 are shown in FIG. 5, and FIG. 6 includes the SEM image of the catalytic tape. As shown in FIG. 6, the catalyst particles are held together by PTFE fibrils.[000104] NH3oxidation reaction: The following procedure was used to test performance of the catalytic tape prepared in Example 3 for NH3 oxidation. The NH3 oxidation reaction was carried out in a fixed-bed quartz flow reactor. 0.25 gram of catalytic tape was used during the test. The catalytic tape was first treated with 115 ppm NH3 in N2 with a total flowrate of 0.45 L / min for 2 hours at 200 °C. After 2 hours of treatment, 6 vol% of O2 was introduced to the gas mixture while maintaining the NH3 concentration and total flowrate constant. The NH3 oxidation reaction was measured with 115 ppm NH3, 6 vol% O2 in N2 with a total flowrate of 0.45 L / min at 175 and 200 °C. To determine NH3 oxidation efficiency, the upstream (i.e. , the concentration of NH3 entering into the chamber before exposure to the catalytic tape) and downstream concentration of NH3 were monitored with a MKS MULTI-GASTM 2030D FTIR analyzer (MKS Instruments, Andover, MA).[000105] NH3 oxidation efficiency (i.e., “NH3 oxidation efficiency (%)”) was calculated based on the following equation:NH-, in - NH-, out NH3oxidation efficiency (%) = . - x 100%NH3in where NH3 = concentration of NH3 in the respective streamNH3 in = upstream concentration of NH3NH3 out = downstream concentration of NH3[000106] Results for the NH3 removal efficiency calculated by using the catalytic tape at various temperatures are included in Table 3 and shown in FIG. 7.Table 3.Example 4 - Catalytic transfer hydrogenation of nitro-benzene to aniline on catalytic tape (3.0wt%palladium-83.6%AI2O3-13.4%PTFE)[000107] Sample preparation: The 3.0wt%palladium-83.6%AI2O3-13.4%PTFE catalytic tape as described in Example 3 was applied this Example.[000108] Nitrobenzene reduction using Catalytic Transfer Hydrogenation (CTH): 0.6148 gram of ammonium formate were mixed with 14.64 gram of ethanol (200 proof). Dissolution of the salt took a significant amount of time, and a lot of stirring. Even after few hours it was possible to see few speckles of salt. 3 ml of this solution were mixed with 51 .3 ul of Nitrobenzene in a 20 ml scintillation vial. The ATR / FTIR spectra of the solution was recorded. 0.0827 gram pieces of catalytic tape (3.0wt%palladium- 83.6%AI2O3-13.4%PTFE) were placed into this solution and the vial was capped. No stirrer was used but the vial was shaken periodically. Gas bubbles were initially observed. Small quantities (e.g., about 2 to 3 drops) of the solution mixed with tape were removed periodically and the ATR-FTIR (Attenuated Total Reflectance Fourier Transform Infra Red) spectra were recorded.[000109] As shown in FIG. 8, nitrobenzene consumption and aniline formation are monitored as by observing the absorbance of the 1530 cm’1and 1499 cm’1peaks as a function of time. Nitrobenzene consumption is estimated based on the absorbance of the peak at about 1530 cm’1. The formation of aniline is estimated by the absorbance of the peak at about 1499 cm’1. The height of the 1520 cm’1was estimated considering a straight baseline between about 1517 and 1542 cm’1. The height of the 1499 cm’1was estimated considering a straight baseline between 1507 cm’1and 1493 cm’1.[000110] FIG. 9 shows the nitrobenzene consumption as a function of time, with the seventh data point indicating when an additional amount of ammonium formate (HCOO-NH4) was added to the mixture. FIG. 10 shows the formation of aniline as a function of time, with the seventh data point indicating when an additional amount of ammonium formate (HCOO-NH4) was added to the mixture.Example 5: Catalytic transfer hydrogenation of nitro-benzene to aniline on catalytic tape (3.0wt%palladium-83.6%AI2O3-13.4%PTFE )[000111] Sample preparation: The 3.0wt%palladium-83.6%AI2O3-13.4%PTFE catalytic tape as described in Example 3 was applied this Example.[000112] Nitrobenzene reduction using Catalytic Transfer Hydrogenation(CTH): A ~3 wt% solution of nitrobenzene in ethanol was prepared by mixing appropriate amounts of nitrobenzene and ethanol (solution A). 6.71 gr of this solution were mixed with 1.15 gr of formic acid (solution B) in a 20 ml scintillation vial. The concentration of nitrobenzene in solution B was about 0.177 M (determined by analysis with HPLC). 0.14 gr of pieces of catalytic tape (3.0wt%palladium-83.6%AI2O3- 13.4%PTFE) were placed into this solution and the vial was capped. No stirrer was used but the vial was shaken periodically. Formation of bubbles was not observed immediately but after about 2.5 hrs.[000113] Samples were collected periodically for analysis with HPLC. The concentrations of Nitrobenzene and Aniline are shown in table 4. The reaction time denotes the time the sample was collected after the pieces of catalytic tape were added to solution B.Table 4[000114] The invention of this application has been described above both generically and with regard to specific embodiments. It will be apparent to those skilled in the art that various modifications and variations can be made in the embodiments without departing from the scope of the disclosure. Thus, it is intended that the embodiments cover the modifications and variations of this invention provided they come within the scope of the appended claims and their equivalents.

Claims

WHAT IS CLAIMED IS:

1. A method for preparing a catalytic article comprising: mixing a dry catalyst precursor, a dry support material, and a dry shape forming material to form a mixture; and calcining the mixture to form the catalytic article comprising granular supported catalyst particles; wherein the dry catalyst precursor comprises a metal and a ligand.

2. A method for preparing a catalytic article comprising: mixing a dry catalyst precursor, a dry support material, and a dry shape forming material to form a mixture; compressing the mixture into a mixture of compressed solids; calcining the mixture pack; and forming the mixture pack into the catalytic article comprising a catalytic tape or a catalytic membrane; wherein the catalyst precursor comprises a metal and a ligand.

3. The method of either of claims 1 or 2, wherein the dry shape forming material comprises dry polymer.

4. The method of claim 3, wherein the polymer comprises polytetrafluoroethylene (PTFE), polypropylene (PP), polyvinylidene fluoride (PVDF), polybenzimidazole (PBI), polyether ether ketone (PEEK), polyether ketone ketone (PEKK) or polyethylene (PE).

5. The method of claim 1 , wherein the granular supported catalyst particles have an average particle size of 5 urn to 3000 urn.

6. The method of claim 1 , wherein the granular supported catalyst particles have an average specific area of 10-1500 m2 / g.

7. The method of claim 1 , wherein the mixing and the calcining are conducted simultaneously or consecutively.

8. The method of claim 2, wherein the calcining and the forming are conducted simultaneously or consecutively.

9. The method of any of claims 1-8, wherein the mixture includes from 25-95% of the dry catalyst precursor by weight and the dry support material, and from 5-75% of the dry shape forming material by weight.

10. The method of any of claims 1-9, wherein the support material is a porous support material selected from the group consisting of metal oxides, zeolites, carbons, clays, metal organic frameworks, and combinations thereof.11 . The method of any of claims 1 -9, wherein the porous support material is selected from one or more of TiO2, SiC>2, AI2O3, zeolite, aluminosilicate or activated carbon.

12. The method of any of claims 1-11 , wherein the metal is selected from one or more of transition metals, lanthanides, alkali or alkaline earth metals, or salts thereof.

13. The method of any of claims 1-12, wherein the metal is selected from the group consisting of vanadium, copper, platinum, palladium, nickel, iron, cobalt, molybdenum, rhodium, ruthenium, rhenium, or mixtures thereof.

14. The method of any of claims 1-13, wherein the ligand is a carbonyl, oxalate, ammonium, dimethylamino, bromide, chloride, cyclopentadienyl, diketonate or a ligand of formula I:wherein R1 and R2 are independently alkyl, substituted alkyl, aryl, substituted aryl, acyl and substituted acyl.

15. The method of any of claims 1 -15, wherein the catalyst precursor is selected from the group consisting of vanadyl acetylacetonate, vanadium (III) acetylacetonate, platinum (II) acetylacetonate, palladium(ll) acetylacetonate, bis(acetylacetonato)dioxomolybdenum (VI), and copper (II) acetylacetonate.

16. The method of any of claims 1-15, wherein mixing comprises mixing in a vortex mixer, a shaking mixer, a double cone mixer, or a combination thereof for a period of time of from 30 seconds to 10 hours.

17. The method of any of claims 1-16, wherein the mixing step is conducted under inert, dry or ambient conditions.

18. The method of any of claims 1-17, wherein the mixture is calcined at a temperature of from 100°C to 350°C at a rate of 1 °C / min to 50°C / min.

19. The method of any of claims 1 -18, wherein the mixture is calcined in an atmosphere containing from 1 to 100 vol.% oxygen.

20. The method for any of claims 1 -19, wherein the catalytic article has a content of the metal of from 0.1 wt.% to 50 wt.% based on a total weight of the catalytic article.21 . The method for any of claims 1-20, wherein the support material has a surface area from about 10 m2 / g to about 3000 m2 / g.

22. The method for any of claims 1-21 , wherein the support material comprises particles having a mean diameter of from 0.5 pm to 1000 pm.

23. The method for any of claims 1-22, wherein the catalyst precursor is vanadyl acetylacetonate or vanadium (III) acetylacetonate, the support material is TiO2, and calcining is conducted at a temperature from 200°C to 350°C.

24. The method for any of claims 1-22, wherein the catalyst precursor is palladium^ I) acetylacetonate, the support material is AI2O3, and calcining is conducted at a temperature from 200°C to 350°C.

25. A catalytic article prepared by the method of any of claims 1 -22 is used in flow- through or flow-by configuration.

26. A method for catalyzing a reaction comprising contacting a reactant stream with the catalytic article of claim 24, wherein the reaction is selected from the group consisting of DeNOx, selective catalytic reduction (SCR), partial oxidation, oxidation, reduction, hydrogenation, dehydrogenation, isomerization, a coupling reaction, an intramolecular Heck reaction, conjugate addition, a nucleophilic addition, an a- substitution reaction, and a ring-opening reaction.

27. The method of claim 2, wherein forming the mixture pack is conducted prior to the calcining the mixture pack.

28. The method of claim 2, wherein forming comprises rolling, compressing or calendaring.

Citation Information

Patent Citations

  • Method for the depositon of metals on support oxides

    US20140112849A1

  • Solid state synthesis of oxidative dehydrogenation catalysts

    US20170246619A1

  • Chromium catalyst materials and methods for making and using the same from chromium(VI) free sources

    US20180214852A1

  • MULTIMETAL OXIDE COMPOSITIONS COMPRISING Mo, Bi, Fe AND Cu

    US20190224651A1